Laminated barrier having a silicone foam layer defining voids containing a heat-absorbing material

A multilayer laminate with a silicone foam sheet and heat-absorbing voids addresses the insufficiencies of silicone foam sheets by providing enhanced thermal and flame barrier properties in EV battery packs.

JP7955358B2Active Publication Date: 2026-11-24DOW SILICONES CORP +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024533021
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-12-16
Filing Date
2022-11-04
Publication Date
2026-11-24
Estimated Expiration
2042-11-04

AI Technical Summary

Technical Problem

Existing silicone foam sheets used as insulating layers in EV battery packs are insufficient to prevent heat transfer and thermal runaway, necessitating a material that provides both flame-retardant and high thermal insulation properties.

Method used

A multilayer laminate comprising a silicone foam sheet with voids containing a heat-absorbing material, sandwiched between two silicone layers with flame-retardant additives, enhancing thermal and flame barrier properties.

Benefits of technology

The laminate achieves thermal insulation of 20 seconds or more to 180°C per millimeter and is flame-resistant at 650°C, effectively preventing thermal runaway in battery packs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955358000001
    Figure 0007955358000001
  • Figure 0007955358000002
    Figure 0007955358000002
Patent Text Reader

Abstract

The article includes a multi-layer laminate having: (a) a first surface layer having opposing major surfaces, the first surface layer comprising a crosslinked polysiloxane matrix having a flame retardant additive dispersed therein; (b) a central layer having opposing major surfaces, one major surface adhered to a major surface of the first surface layer, the central layer being a silicone foam sheet having a flame retardant filler dispersed therein; and (c) a second surface layer having opposing major surfaces, one major surface adhered to a major surface of the central layer opposite the major surface adhered to the first surface layer, the second surface layer having a composition as described for the first surface layer, although the first and second surface layers need not have the same composition, the article comprising a heat sink occupying a void defined by the central layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a laminated article comprising a central layer of silicone foam material defining voids containing an endothermic material. This article is useful as a barrier material for battery packs in electric vehicles. Background Art

[0002] Electric vehicle (EV) technology is becoming increasingly prevalent. EV technology utilizes battery packs to store energy and power the vehicle. The energy demand of vehicles is increasing, especially as the desire and demand for EVs capable of traveling longer distances on a single charge grows. Uncontrolled energy release from EV battery packs can lead to catastrophic consequences due to the enormous heat release. Therefore, it is desirable to design battery packs with protection against uncontrolled energy release from the battery pack.

[0003] EV battery packs typically comprise a plurality of battery cells that are electrically connected to each other and assembled to either directly form the battery pack or form modules, which are then stacked to create the battery pack. EVs can contain up to several thousand battery cells. If a single cell fails, it can release enough energy to heat adjacent cells, leading to thermal runaway and thermal propagation, which in turn causes these adjacent cells to fail and release even more energy. Therefore, it is desirable to identify a barrier material that can be placed between the cells and modules of a battery pack and insulate adjacent cells from thermal energy release in the event of a cell failure.

[0004] Silicone foam sheets are one material considered for use as an insulating layer between cells in battery packs for electric vehicles (EVs). However, silicone foam sheets alone or in laminated form are often insufficient to prevent heat transfer and thermal runaway in battery packs. Therefore, it is desirable to identify articles that are flame-retardant and offer higher insulation properties than simple silicone foam sheets. [Overview of the Initiative]

[0005] The present invention provides an article that is flame-retardant and offers higher thermal insulation than a simple silicone foam sheet. The present invention is the result of discovering a multilayer laminate comprising a silicone foam sheet between two silicone layers, wherein the silicone foam sheet defines voids containing a heat absorbent. The silicone layers contain flame-retardant additives and provide thermal insulation and flame-retardant barrier properties. The silicone foam sheet provides further flame retardancy and thermal insulation, while the heat absorbent pockets provide even higher thermal barrier properties by absorbing heat and, in at least some cases, releasing heat from the heated gas to remove heat from the area of ​​the battery pack that is experiencing thermal failure. Surprisingly, this combination of elements works together to provide particularly desirable thermal and flame barrier properties to the laminated structure that can exist between the cells of a battery pack.

[0006] The multilayer laminate can achieve the "time to 180°C per millimeter of thickness" result of 20 seconds or more, more precisely 25 seconds or more, and more precisely 30 seconds or more, in the thermal insulation test described herein. At the same time, the multilayer laminate is flame-retardant as indicated by the absence of flame when directly compressed against a hot plate at a temperature of at least 650°C, in the flame resistance test method described herein. The multilayer laminate can achieve these properties even with a thickness of 10 millimeters (millimeters, mm) or less, and even 5 mm or less. Therefore, the multilayer laminate achieves the desired properties to function as a barrier material for use in EV battery packs.

[0007] In a first aspect, the present invention relates to an article comprising a multilayer laminate, the multilayer laminate comprising: (a) a first surface layer having opposing main surfaces, comprising a crosslinked polysiloxane matrix having a flame retardant additive dispersed internally at a concentration in the range of 5 to 95 weight percent based on the weight of the first surface layer; and (b) a core layer having opposing main surfaces, one of which is bonded to the main surface of the first surface layer, the core layer being a silicone foam sheet, the silicone foam sheet comprising a flame retardant filler dispersed internally at a concentration in the range of 5 to 80 weight percent based on the weight of the silicone foam sheet. The article comprises a central layer which is a silicone foam matrix, and (c) a second surface layer having opposing main surfaces, wherein one main surface is bonded to the main surface of the central layer opposite to the main surface bonded to the first surface layer, and the second surface layer has the composition described for the first surface layer, but the first and second surface layers do not need to have the same composition, wherein the central layer defines one or more voids such that the total volume of voids defined within the central layer is in the range of 5 to 95 volume percent of the volume defined by the central layer, and the article contains a heat absorbent that occupies the voids within the central layer. The article may further include battery cells, wherein multilayer laminates are electrically connected to each other with a multilayer laminate present between the battery cells.

[0008] The laminate of the present invention is useful as a heat and flame barrier material in battery packs, such as battery packs for electric vehicles. [Modes for carrying out the invention]

[0009] Unless a date is indicated along with the test method number, the test method refers to the test method most recent to the priority date of this document. References to test methods include both references to the testing association and the test method number. The following abbreviations and identifiers for test methods apply in this specification: ASTM refers to the ASTM International Method, END refers to the European Norm, DIN refers to the German Institute for Standardization (Deutsches Institut für Normung), ISO refers to the International Organization for Standardization (International Organization for Standardization), and UL refers to the Underwriters Laboratory.

[0010] Products identified by trade names refer to compositions available under those trade names as of the priority date of this document.

[0011] "Multiple" means two or more. "And / or" means "and, or alternatively." All ranges include the endpoint unless otherwise specified.

[0012] "Sheet" refers to an article having opposing main surfaces separated by a thickness that is less than 1 / 10 of the length or width size defining the main surface.

[0013] Width, length, and thickness are dimensions of an object that are perpendicular to each other.

[0014] The "primary surface" refers to the surface of an object that has the largest planar surface area, as well as the surface opposite to that surface. Planar surface area refers to the surface area projected onto a plane to eliminate the contribution of the surface contour to the surface area. Opposite primary surfaces are separated by the thickness dimension of the object.

[0015] The present invention relates to an article comprising a multilayer laminate. The article may consist of a multilayer laminate or may include components in addition to the multilayer laminate. For example, the article may comprise a battery cell having a multilayer laminate present between the battery cells.

[0016] A multilayer laminate comprises a first surface layer, a core layer, and a second surface layer in that order relative to each other. “Laminate” means that the layers are on top of each other and bonded together. Typically, the main surfaces of bonded layers are bonded to each other. “Bonded to” means either directly attached by direct contact between the bonded layers, or attached via an adhesive, with an adhesive present between the bonded layers. The adhesive may be a layer covering the entire bonded surface, or it may be present only over a portion of the bonded surface.

[0017] The first and second surface layers may have the same or different composition and / or dimensions, but each is selected from materials having similar compositional and dimensional descriptions. The first and second surface layers each have opposing main surfaces and contain a crosslinked polysiloxane matrix and a flame retardant.

[0018] The cross-linked polysiloxane matrix preferably has a 10 percent strain modulus of at least 100 Pascals (Pa), and more preferably has a 10 percent strain modulus of 200 Pa or more, 300 Pa or more, 400 Pa or more, 500 Pa or more, 600 Pa or more, 700 Pa or more, 800 Pa or more, 850 Pa or more, 900 Pa or more, 1000 Pa or more, 2000 Pa or more, 4000 Pa or more, 6000 Pa or more, 8000 Pa or more, 10 kilopascals (kPa) or more, 100 kPa or more, 500 kPa or more, 800 kPa or more, and more preferably 870 kPa or more. While there is no technical upper limit to the 10 percent strain modulus of a crosslinked polysiloxane matrix, crosslinked polysiloxane matrices often have the lower limits mentioned above, as well as upper limits to their 10 percent strain modulus of less than 1 gigapascal (GPa), less than 0.5 GPa, less than 100 megapascals (MPa), less than 50 MPa, less than 25 MPa, less than 15 MPa, less than 100 MPa, less than 5 MPa, less than 1 MPa, or even less than 900 kPa. The 10 percent strain modulus is the tensile stress of the material at 10 percent elongation, as determined according to ASTM D412. Preferably, the crosslinked polysiloxane matrix is ​​flexible.

[0019] The crosslinked polysiloxane matrix can be a crosslinked liquid polysiloxane elastomer or a crosslinked polysiloxane gum. A "crosslinked liquid polysiloxane elastomer" is a polysiloxane elastomer created by crosslinking liquid polysiloxane. Crosslinked liquid polysiloxane elastomers and crosslinked gums are well known and can be created by any known process. Preferably, the crosslinked liquid polysiloxane elastomer consists of 50 mol% or more, 60 mol% or more, 70 mol% or more, 80 mol% or more, or 90 mol% or more based on total siloxane units, and RSiO 3 / 2 and R2SiO 2 / 2 It may contain 95 mol% or more of polysiloxane units selected from the units. Polysiloxane units include R3SiO 1 / 2(M type unit), R2SiO 2 / 2 (Type D unit), RSiO 3 / 2 (Type T unit), and SiO 4 / 2 (The "Q" type unit) is where each R is independently selected from hydrocarbyl groups and substituted hydrocarbyl groups, the oxygen atoms listed in the unit refer to oxygen bonded to silicon atoms of two different siloxane units, the subscript in oxygen refers to the number of shared oxygen atoms in the molecule, and dividing the molecule by 2 indicates that an oxygen atom is shared with another siloxane unit. Examples of polysiloxane elastomers suitable for use as polysiloxane matrices include, for example, crosslinked dimethylvinyl-terminated dimethyl, methylvinylsiloxane gum, and / or crosslinked dimethylvinyl-terminated dimethylsiloxane gum, each having a Williams plasticity of 154–155 mm / 100 mm (Williams plasticity determined according to ASTM D926).

[0020] The curing of liquid siloxanes and / or polysiloxane gums can be achieved, for example, by free radical, hydrosilylation, and / or condensation reactions. Free radical polymerization can be catalyzed, for example, by peroxides. Hydrosilylated curable silicone compositions comprise one or more vinyl-containing siloxane polymers and one or more silicon hydride-functionalized siloxanes. At least one of the vinyl-containing siloxane polymers and silicon hydride-functionalized siloxanes contains two or more of a specific functional group to act as a crosslinking agent. Typically, a hydrosilylation catalyst, such as a platinum compound, is present to facilitate the hydrosilylation reaction. Condensation reaction curable silicone compositions comprise siloxanes having condensation-curable functional groups, such as any one or more hydroxyl functional groups and hydrolyzable functional groups selected from alkoxy, carboxy, amide, enoxy, amino, oxymo, and amioxy groups. Condensation-curable silicone compositions typically further include crosslinking agents such as silanes having hydrolyzable groups, water scavengers such as vinyltrimethoxysilane and methyltrimethoxysilane, and curing catalysts such as titanium and tin compounds, and may be formulated to adjust curing behavior, shelf life, and other post-curing properties. Condensation-curable silicone compositions can be cured at room temperature or high temperatures with or without artificially added moisture in addition to that available from the atmosphere during curing.

[0021] Preferably, the polysiloxane matrix is ​​a non-porous continuous sheet.

[0022] The first and second surface layers further comprise flame retardant additives dispersed within a crosslinked polysiloxane matrix. Suitable flame retardant additives include any one or any combination of two or more selected from the group consisting of metal hydroxides, mixed metal hydroxides, hydrated metal salts, and combinations thereof. Preferably, the flame retardant additive is any one additive, any combination of any additives, or two or more additives from the group consisting of aluminum trihydrate and magnesium hydroxide, calcium hydroxide, magnesium carbonate hydroxide, aluminum carbonate hydroxide, boehmite, hydrated magnesium sulfate, magnesium carbonate trihydrate, and magnesium carbonate tetrahydrate. Optionally, the polysiloxane layer may further comprise metal carbonates and bicarbonates in combination with metal hydroxides, mixed metal hydroxides, and / or hydrated metal salts to further improve flame retardancy. Examples of metal carbonates and bicarbonates include magnesium carbonate, calcium magnesium carbonate (e.g., commercially available as Hantite), and sodium bicarbonate.

[0023] The flame retardant additives are present in each of the first and second surface layers at concentrations of 5% by weight or more, 10% by weight or more, 15% by weight or more, 20% by weight or more, 25% by weight or more, and 30% by weight or more, relative to the weight of the surface layer containing them, and may be present at concentrations of 35% by weight or more, 40% by weight or more, 45% by weight or more, 50% by weight or more, 55% by weight or more, 60% by weight or more, 65% by weight or more, 70% by weight or more, 75% by weight or more, and even 80% by weight or more, while at the same time, they are typically present at concentrations of 95% by weight or less, and may be present at concentrations of 90% by weight or less, 85% by weight or less, 80% by weight or less, 75% by weight or less, 70% by weight or less, 65% by weight or less, 60% by weight or less, 55% by weight or less, and even 50% by weight or less, 45% by weight or less, 40% by weight or less, or 35% by weight or less.

[0024] The first and / or second surface layer may or may not contain any one additional additive or any combination of two or more additional additives. An "additional additive" is an additive included in addition to the flame retardant additives already mentioned. For example, the polysiloxane layer may contain silica, calcium silicate, calcium metasilicate, fumed silica, precipitated silica, ground quartz, precipitated and ground calcium carbonate, calcium sulfate, magnesium sulfate, barium sulfate, zeolites, TiO2, ZnO, magnesium oxide, iron oxide, boron oxide, wollastonite, perlite, vermiculite, mica, kaolin, glass, glass bubbles, aerogel particles, diatomaceous earth, halloysite, magnetite, hematite; benzotriazole, ammonium polyphosphate, ammonium or aluminum alkyl phosphinates, melamine polyphosphate, organophosphates, halogenated organophosphates, other halogen-containing flame retardants with or without antimony oxide, dihydrooxaphosphaphenanthrene, zinc stannate, zinc hydroxystannate, platinum metals and platinum metal compositions, colorants such as carbon black and pigments (e.g., ultramarine blue pigment and / or Yellow 109), stabilizers such as cerium hydroxide, and other flame retardant additives; curing catalysts such as peroxides, organic stannates or titanates, and platinum; accelerators or retarders for curing reactions such as amines, acetylenic alcohols, and organic phosphines; rheology modifiers such as diluents and thickeners; and / or any one additional additive selected from the group consisting of density-reducing additives such as hollow glass or ceramic additives, or any combination of two or more additional additives.

[0025] The combined concentration of flame retardant additives and additional additives in the surface layer is 95 wt% or less, based on the weight of the surface layer, provided that the amount of flame retardant additives is within the range specified above for flame retardant additives, and may be 90 wt% or less, 85 wt% or less, 80 wt% or less, 75 wt% or less, 70 wt% or less, 65 wt% or less, 60 wt% or less, 55 wt% or less, or even 50 wt% or less, 45 wt% or less, 40 wt% or less, or 35 wt% or less.

[0026] Typically, each surface layer has a thickness of 0.1 millimeter (mm) or more, typically 0.2 mm or more, 0.3 mm or more, 0.4 mm or more, 0.5 mm or more, 0.6 mm or more, 0.7 mm or more, 0.8 mm or more, 0.9 mm or more, 1.0 mm or more, 1.2 mm or more, 1.4 mm or more, 1.6 mm or more, 1.8 mm or more, and even 2.0 mm or more. There is no technical limitation on the upper limit of how thick the polysiloxane layer can be. However, typically, in combination with any of the lower limits, the polysiloxane has a thickness of 10 mm or less, 5.0 mm or less, 3.0 mm or less, 1.0 mm or less, 0.8 mm or less, 0.7 mm or less, 0.6 mm or less, and may have a thickness of 0.5 mm or less, 0.4 mm or less, or even 0.2 mm or less.

[0027] The central layer has opposing major surfaces, one major surface is adhered to the major surface of the first surface layer, and the opposing major surface is adhered to the major surface of the second surface layer. The central layer is a silicone foam sheet.

[0028] The silicone foam sheet is a polysiloxane matrix that defines numerous cells. The polysiloxane matrix contains cross-linked polysiloxanes and / or polysiloxane hybrids. Each cell is a void space having a volume of less than 0.5 volume percent (vol%) of the silicone foam sheet volume. Typically, cells in a silicone foam sheet have an average size of 10 mm or less, and can have average sizes of 5 mm or less, 4 mm or less, 3 mm or less, 2 mm or less, 1 mm or less, 900 micrometers or less, 800 micrometers or less, 700 micrometers or less, 600 micrometers or less, 500 micrometers or less, 400 micrometers or less, 300 micrometers or less, 200 micrometers or less, 100 micrometers or less, 50 micrometers or less, and even 10 micrometers or less. At the same time, typically, they have an average size of 5 nanometers (nm) or more, preferably 10 nm or more, 25 nm or more, 50 nm or more, 100 nm or more, 500 nm or more, 1 micrometer or more, 50 micrometers or more, 100 micrometers or more, 500 micrometers or more, or even 1 mm or more. The cell structure can be an "open-cell" structure with interconnected cellular void spaces, an "closed-cell" structure where a polysiloxane matrix material surrounds each cell, separating the void space of each cell from the void space of other cells, or a combination of open-cell and closed-cell structures.

[0029] The silicone foam sheet may contain, and preferably contains, a flame retardant compound dispersed within its polysiloxane matrix. Examples of suitable flame retardants include metal hydroxides, mixed metal hydroxides, metal salts, hydrated metal salts, halogenated polymers, organophosphates, halogenated organophosphates, and any combination thereof.

[0030] Silicone foam sheets generally have an average density of 0.05 grams per cubic centimeter (g / cc) or higher, and can have densities of 0.1 g / cc or higher, 0.2 g / cc or higher, 0.3 g / cc or higher, 0.4 g / cc or higher, 0.5 g / cc or higher, and even 0.6 g / cc or higher. At the same time, they typically have a density of 0.9 g / cc or lower, and can have densities of 0.8 g / cc or lower, or even 0.7 g / cc or lower. The density can be uniform or non-uniform within the silicone foam sheet. For example, a silicone foam sheet may have low porosity and a higher density on its surface than in its core.

[0031] Silicone foam sheets can be prepared by any of the following methods. For example, a foam sheet can be prepared by crosslinking siloxane gum with a peroxide at the crosslinking temperature in the presence of a blowing agent, where the blowing agent generates or becomes a gas at or near the crosslinking temperature. Some free radical initiators generate nitrogen gas upon decomposition and can be used as blowing agents and as initiators for crosslinking reactions. Silicone foams can be prepared by crosslinking siloxane gum and / or liquids using hydrosilylation or condensation reactions in the presence of a blowing agent. Instead of including a blowing agent, gas can be mixed with the siloxane gum and / or liquid before or during curing. A silicone foam sheet may be a syntactic foam containing multiple hollow filler components that provide foam "cells". Suitable hollow filler components include hollow glass or ceramic microparticles, such as spheres.

[0032] Suitable silicone foam materials that can be used as silicone foam sheets include materials available under the trade names DOWSIL® 3-8235 Silicone Foam, DOWSIL® 3-8209 Silicone Foam, Norseal® R10400M, Norseal® R10450, Norseal® R10490, and Norseal® R10480S. DOWSIL is a trademark of The Dow Chemical Company. Norseal is a trademark of Saint-Gobain Performance Plastics Corporation.

[0033] The central layer typically has an average thickness of 0.5 mm or more, and can have thicknesses of 1.0 mm or more, 1.5 mm or more, 2.0 mm or more, 2.5 mm or more, 3.0 mm or more, 4.0 mm or more, 5.0 mm or more, 10 mm or more, 20 mm or more, 30 mm or more, and even 40 mm or more, while at the same time, it generally has a thickness of 50 mm or less, and can have thicknesses of 40 mm or less, 30 mm or less, 20 mm or less, 10 mm or less, 5.0 mm or less, 4 mm or less, or even 3.0 mm or less.

[0034] The core layer defines one or more voids that can extend partially or entirely through the thickness of the core layer. These voids are distinct from cells in the silicone foam sheet due to their much larger volume. Each void may have a volume of 5 volume percent or more, more than 10 volume percent or more, or more than 20 volume percent or more of the total volume of the core layer. The total volume of the void space defined by the central layer is 5 volume percent (volume %) or more of the total volume of the central layer, and can be 10 volume percent or more, 15 volume percent or more, 20 volume percent or more, 25 volume percent or more, 30 volume percent or more, 35 volume percent or more, 40 volume percent or more, 45 volume percent or more, 50 volume percent or more, 55 volume percent or more, 60 volume percent or more, 65 volume percent or more, 70 volume percent or more, 75 volume percent or more, 80 volume percent or more, 85 volume percent or more, and even 90 volume percent or more. At the same time, it is typically 95 volume percent or less, and can be 90 volume percent or less, 85 volume percent or less, 80 volume percent or less, 75 volume percent or less, 70 volume percent or less, 65 volume percent or less, 60 volume percent or less, 55 volume percent or less, 50 volume percent or less, 47 volume percent or less, 45 volume percent or less, 40 volume percent or less, 35 volume percent or less, 30 volume percent or less, or even 25 volume percent or less.

[0035] A multilayer laminate further includes a heat absorber occupying the voids defined by the central layer. The heat absorber is typically in particulate form, with a large number of particles occupying a given void. The heat absorber is a material that absorbs heat when it decomposes at temperatures in the range of 80°C to 550°C to produce carbon dioxide and / or water. The heat absorbers may all be the same or a combination of several different heat absorbers. Examples of heat absorbers that absorb heat and produce water when they decompose include metal hydroxides, metal salts, hydrates of metal salts, e.g., aluminum hydroxide, magnesium hydroxide, calcium hydroxide, calcium magnesium hydroxide, hydrotalcite, boehmite, talc, calcium sulfate hydrate, magnesium hydroxide, and zinc borate. Specific examples include hydrated magnesium sulfate minerals (e.g., epsomite), aluminum trihydrate, and magnesium hydroxide. Examples of heat-absorbing materials that produce carbon dioxide when they absorb heat and decompose include magnesium carbonate, calcium carbonate, magnesium calcium carbonate, sodium bicarbonate, lithium bicarbonate, potassium bicarbonate, and magnesium bicarbonate. Examples of heat-absorbing materials that release both water and carbon dioxide while absorbing heat and decomposing include hydrated magnesium carbonate minerals such as hydromagnesite. The heat-absorbing material can completely or partially occupy the void spaces defined within the core layer. Preferably, the void spaces and the heat-absorbing material are located throughout the core layer rather than concentrated in a small part of it. The role of the heat-absorbing material is to reduce heat transfer through the multilayer laminate by absorbing heat and releasing that heat as water vapor or carbon dioxide; therefore, it is optimal to widely distribute the heat-absorbing material throughout the core layer. In this regard, it is desirable that the core layer defines voids that are widely distributed throughout the core layer and that the heat-absorbing material occupies these voids.

[0036] The heat absorber occupies a defined void volume within the central layer and can therefore occupy any of the volumes defined by the central layer, ranging from 5 to 95%. Preferably, the heat absorber occupies 40% or more of the volume defined by the central layer, more preferably 45% or more, 50% or more, and even more than 55% or more, while simultaneously typically occupying 95% or less, 90% or less, 85% or less, 80% or less, 75% or less, 70% or less, 65% or less, 60% or less, or even more than 55% or less, 50% or less, or even more than 45% or less.

[0037] One example of a desirable void orientation in the central layer is having one large void space defined by the outer periphery of the central layer material, such that the heat-absorbing material within the void space continuously occupies most of the volume of the central layer space. Another example of a desirable void orientation is having multiple void spaces defined throughout the central layer and occupied by the heat-absorbing material, so as to effectively provide a broad distribution of the heat-absorbing material throughout the central layer.

[0038] The heat-absorbing materials are typically sealed within the voids they occupy by a central layer and first and second surface layers.

[0039] The multilayer laminate can be fabricated by any conceivable means. For example, a first surface layer can be bonded to a core layer, then a heat absorbent can be placed in the void defined by the core layer, and then a second surface layer can be bonded onto the core layer, sandwiching the core layer and the heat absorbent between the first and second surface layers.

[0040] One or both of the surface layers can be directly bonded to the core layer, or neither can be directly bonded to the core layer. To achieve direct bonding between the surface layer and the core layer, the surface layer can be cured to form a cross-linked polysiloxane matrix while in contact with the core layer.

[0041] One or both of the surface layers may be bonded to the core layer using an adhesive, or neither may be bonded. The adhesive may be present between the surface layer and the core layer, bonding the two layers together. The adhesive may completely cover the bonded surfaces so as to form a film between the two layers. Alternatively, the adhesive may cover only a portion of the bonded surfaces. The adhesive may be continuous, like a film or bead, or discontinuous, like a series of dots, unconnected beads, or a combination of beads and dots. The adhesive may form any pattern that bonds the surface layer to the core layer.

[0042] The adhesive, if used, may be a silicone adhesive. The adhesive may be a one-component or two-component adhesive. Preferably, the adhesive contains a flame retardant additive. For example, the adhesive may be a silicone foam adhesive, such as the one commercially available from The Dow Chemical Company under the name DOWSIL (trademark) 3-8235 Silicone Parts A and B. DOWSIL is a trademark of The Dow Chemical Company. Preferably, the adhesive is suitable for high-temperature applications.

[0043] Multilayer laminates are particularly useful as insulators between cells in battery modules for electric vehicles. In this regard, the article of the present invention may further include a plurality of battery cells having multilayer laminates present between the battery cells. The article may be a battery module that may be in a vehicle, and the battery module includes a housing that contains a plurality of battery cells having multilayer laminates present between the battery cells. [Examples]

[0044] Table 1 lists the materials to be used in the following examples.

[0045] [Table 1-1]

[0046] [Table 1-2] XIAMETER, SILASTIC, and SYL-OFF are trademarks of Dow Corning Corporation. DOWSIL is a trademark of The Dow Chemical Company. HALTEX is a trademark of TOR Minerals International. ZEROGEN, HYMOD, and MICRAL are trademarks of JMHuber Corporation. WOLLASTOCOAT is a trademark of NYCO Minerals, Inc. CAB-O-SIL is a trademark of Cabot Corporation.

[0047] Preparation of additive A2. Prepare A2 as described in International Publication No. 2020131985 using the standard mixing procedure described in ASTM D3182. A2 consists of 7 wt% magnesium ferrite, 23 wt% ultramarine pigment, 23 wt% titanium dioxide, 6 wt% chromium oxide green, and 41 wt% G1.

[0048] Preparation of the polysiloxane layer. The polysiloxane layer is prepared as described in International Publication No. 2020131985 using the standard mixing procedure described in ASTM D3182. The polysiloxane layer consists of 17.19 wt% B1, 13.45 wt% G1, 33.52 wt% alumina trihydrate, 20.12 wt% magnesium hydroxide, 0.8 wt% magnesium silicate, 8.05 wt% calcium metasilicate, 2.68 wt% A1, 1.07 wt% P1, 0.24 wt% F1, and 2.88 wt% A2. The polysiloxane layer is prepared to a thickness of 0.6 mm by calendering the composition using a two-roll mill. The sheet was cured at 120 degrees Celsius (°C) for 15 minutes in a hot press under 30 tons of pressure on a 0.6 mm thick, 30.5 cm x 30.5 cm metal chase to form a sample with dimensions of 30.5 cm x 30.5 cm x 0.6 mm. The polysiloxane layer has a 10 percent modulus of elasticity of 0.87 megapascals as measured according to ASTM D412.

[0049] Preparation of polysiloxane foam 1. The components of the silicone adhesive are mixed in a 1:1 weight ratio in a speed mixer at 2000 revolutions per minute for 30 seconds. A polysiloxane foam sheet is produced using a nib roller with a thickness control of 3 mm. The sheet is cured at 25°C for 24 hours. Polysiloxane foam 1 has a density of 0.23 grams per cubic centimeter.

[0050] Preparation of polysiloxane foam 2. The following components are mixed together in a speed mixer at 2000 revolutions per minute for 30 seconds, and then a polysiloxane foam sheet is produced using a nib roller with a thickness control of 3 mm. The sheet is cured at 25°C for 24 hours. The components for producing polysiloxane foam 2 are 0.42 parts C1, 2.88 parts F5, 12.64 parts F6, 2.16 parts F2, 1.39 parts benzyl alcohol, 1.09 parts butanediol, 26.91 parts alumina trihydrate 2, 2.88 parts F3, 15.48 parts alumina trihydrate 3, and 34.17 parts F4, where parts are by weight. Polysiloxane foam 2 has a density of 0.54 grams per cubic centimeter.

[0051] Characterization of the sample The following thermal insulation and flame resistance tests will be used to characterize the sample.

[0052] Thermal insulation test. The hot plate is placed in a hydraulic environment surrounded by a vented space on one side, with the vent port directly adjacent to the sample. A porous ceramic refractory insulator is placed on the top surface of the hot plate, and the hot plate is heated to 710°C. Four thermocouple probes are attached to an aluminum heat sink using Kapton tape. The sample is placed on the aluminum heat sink and secured to the aluminum heat sink using Kapton tape. Another thermocouple is secured to the sample surface using Kapton tape. The insulator is removed from the heated surface of the hot plate, and the sample is quickly placed on the heated surface of the hot plate with the aluminum heat sink on the opposite side of the hot plate from the sample. A pressure of 355 kilopascals is rapidly applied to compress the sample against the hot plate. The temperature of the hot plate surface and the sample is monitored using a data logger. When the temperature on the sample side opposite the hot plate reaches 180°C, the pressure is released and the test is terminated. The time required for the sample side opposite the hot plate to reach 180°C is recorded in seconds as the adiabatic time. The adiabatic time is divided by the thickness of the sample to provide the "time to reach 180°C per millimeter" in seconds per millimeter (s / mm). Longer times correspond to higher adiabatic performance.

[0053] Flame resistance test. During the heat insulation test, observe the sample to see if it ignites. If flames are observed, note whether they self-extinguish within the test time (the time required to reach 180°C). General observation indicates that a sample that ignites will generally ignite within the first 5 seconds after contact with the hot plate. If a sample ignites during the test time, it fails the flame resistance test.

[0054] Sample having polysiloxane foam 1 Comparative Example (Comp Ex) A. Comp Ex A is a 10 cm x 10 cm square piece of polysiloxane foam 1. Characterization results: Sample thickness: 3 mm. Thermal insulation test: Time to 180°C per 1 mm thickness: 0.63 s / mm. Flame resistance test: No flame.

[0055] Comp Ex B. Comp Ex B is prepared as a laminate using two 10cm × 10cm square pieces of polysiloxane layer and one 10cm × 10cm square piece of polysiloxane foam 1. Two grams (g) of silicone adhesive are applied to both opposing main surfaces of polysiloxane foam 1 by distributing parts A and B of the silicone adhesive through a static mixture and mixing them together as these parts are distributed. The silicone adhesive is applied as a bead (approximately 3 mm in diameter) to the main surface of polysiloxane foam 1 around the void. The polysiloxane layer sheets are bonded to each side of polysiloxane foam 1 to form a pre-laminate. The pre-laminate is placed in a chaise that is 25.4cm × 25.4cm × 4mm and a weight of 10 tons is applied to the laminated layers to press them together. The compressed laminate layers are cured at 25°C for 24 hours or at 60°C for 10 minutes to achieve Comp Ex B. Comp Ex B has a final thickness of 4.5 mm. Characterization results: Sample thickness: 4.5 mm. Thermal insulation test: Time to 180°C per 1 mm thickness: 19 s / mm. Flame resistance test: No flame.

[0056] Example (Ex) 1. Ex1 is prepared in the same manner as Comp Ex B, except that nine circular voids with a diameter of 2.54 cm are defined within the polysiloxane foam 1, uniformly distributed throughout the entire thickness of the polysiloxane foam 1. Before forming the laminate, 3 grams of hydrated magnesium carbonate mineral are evenly distributed into the nine voids to provide 44 volume% of the heat absorber in the polysiloxane foam 1 (the central layer of the laminate). Characterization results: Sample thickness: 4.5 mm. Thermal insulation test: Time to 180°C per 1 mm thickness: 26 s / mm. Flame resistance test: No flame.

[0057] Ex2. Ex2 is prepared in the same manner as Comp Ex B, except that a single square void with dimensions of 7.62 cm × 7.62 cm is defined in the center of polysiloxane foam 1, extending across the entire thickness of polysiloxane foam 1. Before forming the laminate, 5 grams of sodium bicarbonate are distributed into the void to provide 56 volume% of the heat absorber in the ceramic sheet layer (the central layer of the laminate). Characterization results: Sample thickness: 4.5 mm. Thermal insulation test: Time to 180°C per 1 mm thickness: 24 s / mm. Flame resistance test: No flame.

[0058] The results for Comp Ex A and B, and Ex1 and Ex2 illustrate a significant increase in the thermal insulation of the claimed laminate of the present invention, which contains a heat absorbent in the core layer, compared to either the core layer alone (Comp Ex A) or a similar laminate without a heat absorbent (Comp Ex B).

[0059] A sample containing polysiloxane foam 2. Comp Ex C. Comp Ex C is a 10 cm x 10 cm square piece of polysiloxane foam 2. Characterization results: Sample thickness: 3 mm. Thermal insulation test: Time to 180°C per 1 mm thickness: 22 s / mm. Flame resistance test: No flame.

[0060] Comp Ex D. Comp Ex D is prepared in the same manner as Comp Ex B, except that polysiloxane foam 2 is used instead of polysiloxane foam 1. Characterization results: Sample thickness: 4.5 mm. Thermal insulation test: Time to 180°C per 1 mm thickness: 24 s / mm. Flame resistance test: No flame.

[0061] Ex3. Ex3 is prepared in the same manner as Ex1, except that polysiloxane foam 2 is used instead of polysiloxane foam 1. Characterization results: Sample thickness: 4.5 mm. Thermal insulation test: Time to 180°C per 1 mm thickness: 37 s / mm. Flame resistance test: No flame.

[0062] The results for Comp Ex C, D, and Ex3 illustrate a significant increase in thermal insulation of the claimed laminate of the present invention, which contains a heat absorbent in the core layer, compared to either a core layer only (Comp Ex C) or a similar laminate without a heat absorbent (Comp Ex D). The present invention includes the following embodiments. [Aspect 1] An article comprising a multilayer laminate, wherein the multilayer laminate is (a) A first surface layer having opposing main surfaces, comprising a crosslinked polysiloxane matrix having a flame retardant additive dispersed internally at a concentration ranging from 5 to 95 weight percent based on the weight of the first surface layer, (b) A central layer having opposing main surfaces, one of which is bonded to the main surface of the first surface layer, wherein the central layer is a silicone foam sheet, and the silicone foam sheet is a silicone foam matrix having a flame retardant filler dispersed internally at a concentration in the range of 5 to 80% by weight based on the weight of the silicone foam sheet, (c) A second surface layer having opposing main surfaces, wherein one main surface is bonded to the main surface of the central layer opposite to the main surface bonded to the first surface layer, and the second surface layer has the composition described for the first surface layer, but the first and second surface layers do not need to have the same composition. The central layer defines one or more voids such that the total volume of voids defined within the central layer is within the range of 5 to 95 volume percent of the volume defined by the central layer, and the article comprises a heat-absorbing agent occupying the voids within the central layer. [Aspect 2] The article according to embodiment 1, wherein each of the first and second surface layers has a 10 percent strain modulus of at least 100 Pascals as determined by ASTM D412. [Aspect 3] The article according to embodiment 1 or 2, wherein each of the first and second surface layers has an average thickness in the range of 0.1 to 3.0 millimeters. [Aspect 4] The article according to any one of embodiments 1 to 3, wherein the central layer has an average thickness of 0.5 to 50 millimeters. [Aspect 5] The article according to any one of embodiments 1 to 4, wherein each of the first and second surface layers contains a flame retardant at a concentration ranging from 50 to 85 weight percent based on the weight of the layer containing it. [Aspect 6] The article according to any one of embodiments 1 to 5, wherein the heat-absorbing agent is present at a concentration in the range of 40 to 60 volume percent of the volume defined by the central layer. [Aspect 7] The article according to any one of embodiments 1 to 6, wherein the heat-absorbing agent is one or more selected from the group consisting of hydrated magnesium carbonate mineral, hydrated magnesium sulfate mineral, sodium bicarbonate, aluminum trihydrate, and magnesium hydroxide. [Aspect 8] The article according to any one of embodiments 1 to 7, wherein the multilayer laminate further includes an adhesive between the central layer and each of the first and second surface layers. [Aspect 9] The article according to embodiment 8, wherein the adhesive is a silicone adhesive. [Aspect 10] The article according to any one of embodiments 1 to 9, wherein the article further comprises battery cells, the battery cells being electrically connected to one another with the multilayer laminate present between them.

Claims

1. An article comprising a multilayer laminate, wherein the multilayer laminate is (a) A first surface layer having opposing main surfaces, comprising a crosslinked polysiloxane matrix having a flame retardant additive dispersed internally at a concentration in the range of 5 to 95 weight percent based on the weight of the first surface layer, (b) A central layer having opposing main surfaces, one of which is bonded to the main surface of the first surface layer, wherein the central layer is a silicone foam sheet, and the silicone foam sheet is a silicone foam matrix having a flame retardant filler dispersed inside at a concentration in the range of 5 to 80% by weight based on the weight of the silicone foam sheet, (c) A second surface layer having opposing main surfaces, wherein one main surface is bonded to the main surface of the central layer opposite to the main surface bonded to the first surface layer, and the second surface layer has the composition described for the first surface layer, but the first and second surface layers do not need to have the same composition. The central layer defines one or more voids such that the total volume of voids defined within the central layer is within the range of 5 to 95 volume percent of the volume defined by the central layer, and the article comprises a heat-absorbing agent occupying the voids within the central layer.

2. The article according to claim 1, wherein each of the first and second surface layers has a 10 percent strain modulus of at least 100 Pascals as determined by ASTM D412.

3. The article according to claim 1, wherein each of the first and second surface layers has an average thickness in the range of 0.1 to 3.0 millimeters.

4. The article according to claim 1, wherein the central layer has an average thickness of 0.5 to 50 millimeters.

5. The article according to claim 1, wherein each of the first and second surface layers contains a flame retardant at a concentration ranging from 50 to 85 weight percent based on the weight of the layer containing it.

6. The article according to claim 1, wherein the heat-absorbing agent is present in a concentration in the range of 40 to 60 volume percent of the volume defined by the central layer.

7. The article according to claim 1, wherein the heat-absorbing agent is one or more selected from the group consisting of hydrated magnesium carbonate mineral, hydrated magnesium sulfate mineral, sodium bicarbonate, aluminum trihydrate, and magnesium hydroxide.

8. The article according to claim 1, wherein the multilayer laminate further includes an adhesive between the central layer and each of the first and second surface layers.

9. The article according to claim 8, wherein the adhesive is a silicone adhesive.

10. The article according to any one of claims 1 to 9, wherein the article further comprises battery cells, the battery cells being electrically connected to one another with the multilayer laminate present between them.

Citation Information

Patent Citations

  • Fireproof structure

    CN103753927A

  • Foamed silicone rubber core material and foamed heat-insulating buffer composite material

    CN112480686A

  • POLYMER MATRIX COMPOSITES CONTAINING THERMALLY ENDOTHERMIC PARTICLES AND METHODS FOR MANUFACTURING SAME (CROSS-REFERENCE TO RELATED APPLICATIONS) This application claims the benefit of U.S. Provisional Patent Application No. 62 / 587,054, filed November 16, 2017, the entire disclosure of which is incorporated herein by reference.

    JP2021503531A

  • Multilayer sheet for preventing thermal runaway

    US20220181715A1