Polyester-polyurethane-poly(meth)acrylic hybrid dispersion

The polyester-polyurethane-poly(meth)acrylic hybrid dispersion addresses compatibility issues in automotive coatings by enhancing layer compatibility and eliminating the need for a final stripping process, resulting in improved appearance and weather resistance.

JP7955376B2Active Publication Date: 2026-11-24SURVENTIS GMBH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024552692
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-03-04
Filing Date
2023-03-02
Publication Date
2026-11-24
Estimated Expiration
2043-03-02

AI Technical Summary

Technical Problem

Existing automotive coating compositions lack good compatibility between different layers, leading to inferior appearance and weather resistance, and require a final stripping process, which increases time and cost.

Method used

A polyester-polyurethane-poly(meth)acrylic hybrid dispersion is prepared by esterifying carboxyl group-containing polyurethane with hydroxyl group-containing polyester, followed by radical polymerization of ethylenically unsaturated monomers, including (meth)acrylic monomers, to achieve a high solids content and eliminate the need for a final stripping process.

Benefits of technology

The hybrid dispersion ensures excellent compatibility and appearance of multilayer coatings, reducing time and cost by eliminating the need for a final stripping process and improving weather resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955376000001
    Figure 0007955376000001
  • Figure 0007955376000002
    Figure 0007955376000002
  • Figure 0007955376000003
    Figure 0007955376000003
Patent Text Reader

Abstract

The present invention relates to a polyester-polyurethane-poly(meth)acrylic hybrid dispersion, which can be obtained by esterifying at least one carboxyl-containing polyurethane, which has an acid value of more than 200 mgKOH / g to 400 mgKOH / g and at least one or more terminal carboxyl groups, with at least one hydroxyl-containing polyester, which has a hydroxyl value of 50 mgKOH / g to 300 mgKOH / g, to obtain a polyester-polyurethane, followed by a step of polymerizing ethylenically unsaturated monomers, including at least a (meth)acrylic monomer, by radical polymerization in the presence of the polyester-polyurethane in step (a), wherein one or more solvents are present and / or used during steps (a) and / or (b) and / or are added after step (b).Furthermore, the present invention relates to a coating composition comprising the polyester-polyurethane-poly(meth)acrylic hybrid dispersion, a coating layer formed from the composition, and a substrate thus coated. Furthermore, the present invention relates to a method for using a coating composition comprising the polyester-polyurethane-poly(meth)acrylic hybrid dispersion in automotive coatings, and to a method for producing a multi-layer coating, wherein at least one coating layer is formed from a coating composition comprising the polyester-polyurethane-poly(meth)acrylic hybrid dispersion.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a polyester-polyurethane-poly(meth)acrylic hybrid dispersion and a method for producing a polyester-polyurethane-poly(meth)acrylic hybrid dispersion. Furthermore, the present invention relates to a coating composition comprising a polyester-polyurethane-poly(meth)acrylic hybrid dispersion, a coating layer formed from the composition, and a substrate thus coated. Furthermore, the present invention relates to a method for using a coating composition comprising a polyester-polyurethane-poly(meth)acrylic hybrid dispersion in an automotive coating, and a method for producing a multilayer coating, wherein at least one coating layer is formed from a coating composition comprising a polyester-polyurethane-poly(meth)acrylic hybrid dispersion. [Background technology]

[0002] Automotive body painting is performed using multi-layer coating. A multi-layer coating system typically includes, among other things, a primer-surfacer layer formed on a pre-coated substrate, followed by one or more base coat layers, and an uppermost clear coat layer. Each layer can be baked separately or applied in a wet-on-wet process, in which case the coating layer is formed on the previous coating layer without an intermediate curing step. A flash-off or drying step is required between the two coating steps, in which the subsequent coating layer is applied after the solvent of the coating composition has evaporated. Thus, it is essential to achieve rapid drying during the flash-off or drying step to prevent mixing of the coating compositions after the application of the subsequent coating composition. Rapid drying can be achieved, for example, by a high solids content in the coating composition.

[0003] Today, it is common to use an integrated wet-on-wet-on-wet application for painting automotive bodies, in which at least three coating layers are applied in a wet-on-wet-on-wet process. Two integrated paint processes (IPPs) are particularly preferred, and integrated paint process 1 (IPP1) includes forming a primer-surfacer layer by applying a primer-surfacer composition to a preferably electrocoated metal substrate and a subsequent flash-off or drying step. Then, one or two basecoat compositions are applied on top of the primer-surfacer layer to form one or two basecoat layers, followed by a flash-off or drying step. Then, a clearcoat composition may be applied on top of the basecoat layer(s) to form a clearcoat layer, followed by a flash-off or drying step. Finally, all layers are cured simultaneously in a single curing step.

[0004] In the Integrated Paint Process 2 (IPP2), preferably, the electrocoated metal substrate is not coated with a primer-surfacer layer. Instead, two basecoat compositions are applied using a wet-on-wet application method to form two basecoat layers, followed by a flash-off or drying process, after which the first basecoat has primer-surfacer functionality. Subsequently, a clearcoat composition is applied to form a clearcoat layer, followed by a curing process that simultaneously cures all coating layers. By simultaneously curing all coating layers, the energy and material costs of the coating process are reduced.

[0005] Regarding environmental issues, compatibility of individual coating layers, good appearance, and weather resistance, there are high demands not only for individual coating layers but also for multilayer coatings. Excellent appearance requires good compatibility between different coating layers in a multilayer coating.

[0006] Furthermore, the manufacturing of multi-layer coating systems must be simple and inexpensive.

[0007] EP1199342A1 describes increasing the solids content of each binder combination by using binder combinations containing water-miscible hydroxyurethane.

[0008] Polyester-polyurethane-poly(meth)acrylic hybrid dispersions are known from US10,233,353B2. However, there is still a need to improve the base coat composition to achieve good compatibility between different coating layers. Good compatibility between different coating compositions forming the coating layers of a multilayer coating results in a superior appearance of the multilayer coating. [Prior art documents] [Patent Documents]

[0009] [Patent Document 1] EP1199342A1 [Patent Document 2] US10,233,353B2 [Overview of the Initiative] [Problems that the invention aims to solve]

[0010] The objective was to provide a coating composition having a high solids content, thereby offering good compatibility with other coating compositions in a multilayer coating and usable in an integrated paint process. Therefore, the objective was to prepare a coating composition comprising a polyester-polyurethane-poly(meth)acrylic hybrid dispersion having a high solids content. A further objective was to provide a polyester-polyurethane-poly(meth)acrylic hybrid dispersion that eliminates the need for a final stripping process, thus reducing the time and cost of preparing this hybrid dispersion. Furthermore, the multilayer coating obtained from the coating composition exhibits excellent appearance, particularly excellent leveling. [Means for solving the problem]

[0011] This object has been solved by the subject of the present application and the preferred embodiments thereof disclosed herein.

[0012] A first subject of the present invention is a polyester-polyurethane-poly(meth)acrylic hybrid dispersion obtainable by the following steps: a. esterifying at least one carboxyl group-containing polyurethane having an acid number of greater than 200 mg KOH / g to 400 mg KOH / g and at least one terminal carboxyl group, with at least one hydroxyl group-containing polyester having a hydroxyl number of 50 mg KOH / g to 300 mg KOH / g to obtain a polyester-polyurethane, followed by b. polymerizing ethylenically unsaturated monomers comprising at least (meth)acrylic monomers by radical polymerization in the presence of the polyester-polyurethane of step (a) to obtain a poly(meth)acrylate wherein one or more solvents are present and / or used during steps (a) and / or (b) and / or are added after step (b).

[0013] The present invention further relates to a process for preparing the polyester-polyurethane-poly(meth)acrylic hybrid dispersion of the present invention, comprising the following steps: a. esterifying at least one carboxyl group-containing polyurethane having an acid number of greater than 200 mg KOH / g to 400 mg KOH / g and at least one terminal carboxyl group, with at least one hydroxyl group-containing polyester having a hydroxyl number of 50 mg KOH / g to 300 mg KOH / g to obtain a polyester-polyurethane, followed by b. polymerizing ethylenically unsaturated monomers comprising at least (meth)acrylic monomers by radical polymerization in the presence of the polyester-polyurethane of step (a) to obtain a poly(meth)acrylate This is due to, The present invention provides a method in which one or more solvents are present and / or used between steps (a) and / or (b), and / or added after step (b).

[0014] Another object of the present invention is a coating composition comprising the polyester-polyurethane-poly(meth)acrylic hybrid dispersion of the present invention.

[0015] A further object of the present invention is a coating layer formed from a coating composition comprising the polyester-polyurethane-poly(meth)acrylic hybrid dispersion of the present invention, and a substrate thus coated.

[0016] Another object of the present invention is a method for using a coating composition comprising the polyester-polyurethane-poly(meth)acrylic hybrid dispersion of the present invention in automotive coatings.

[0017] Another object of the present invention is a method for manufacturing a multilayer coating, comprising the following steps: a. A step of applying one or more base coat compositions to form one or more base coat layers on a substrate, wherein at least one base coat composition comprises the polyester-polyurethane-poly(meth)acrylic hybrid dispersion of the present invention. b. A step of applying a clear coat composition onto one or more base coat layers to form a clear coat layer. c. A process in which one or more base coat layers and clear coat layers are cured simultaneously, or one or more layers obtained in steps (a) and (b) are cured individually and then a subsequent coating layer is applied, or all layers obtained in steps (a) and (b) are cured individually. This method includes [something].

[0018] Preferred embodiments of the polyester-polyurethane-poly(meth)acrylic hybrid dispersion and coating composition of the present invention will become clear from the following description and from the dependent claims. [Modes for carrying out the invention]

[0019] definition First, let's explain the terminology used in the context of this invention.

[0020] The term "hybrid dispersion" according to the present invention refers to a dispersion comprising polyester-polyurethane and poly(meth)acrylate. Polyester-polyurethane can be physically mixed with poly(meth)acrylate and / or covalently bonded with poly(meth)acrylate.

[0021] The expression "aqueous coating composition" is known to those skilled in the art. This refers to a coating composition in which the volatile portion of the coating composition is essentially water-based. Therefore, in the context of the present invention, "aqueous" is understood to mean that the coating composition preferably contains at least 40% by mass, more preferably at least 50% by mass, and most preferably at least 60% by mass of water fraction with respect to the total amount of solvent present (i.e., water and organic solvents) in each case.

[0022] The term "aliphatic" is used according to the IUPAC definition, and thereby includes all acyclic or cyclic, saturated or unsaturated carbon compounds except aromatic compounds.

[0023] The term "polymeric" refers to a substance composed of multiple monomeric entities with different degrees of polymerization, molar mass, and chain length. These monomeric entities may be identical or different. In the context of this invention, "polymeric" substances also include oligomeric substances.

[0024] In the context of the present invention, a polyfunctional alcohol or isocyanate refers to a molecule having at least two functional groups, and by extension, a bifunctional alcohol or isocyanate.

[0025] The term "(meth)acrylic" refers to a substance containing methacrylate and / or methacrylic acid and / or acrylate and / or acrylic acid.

[0026] Polyester-polyurethane-poly(meth)acrylic hybrid dispersion The polyester-polyurethane-poly(meth)acrylic hybrid dispersion is produced through the following process: a. A polyurethane containing at least one carboxyl group, having an acid value of more than 200 mg KOH / g and more than 400 mg KOH / g, and having at least one terminal carboxyl group. Esterilization with a polyester containing at least one hydroxyl group having a hydroxyl value of 50 mg KOH / g to 300 mg KOH / g The process of obtaining polyester-polyurethane, followed by b. A step to obtain poly(meth)acrylate by polymerizing an ethylenically unsaturated monomer containing at least a (meth)acrylic monomer by radical polymerization in the presence of the polyester-polyurethane of step (a). It can be obtained by Here, one or more solvents are present and / or used between steps (a) and / or (b), and / or added after step (b).

[0027] The ethylenically unsaturated monomer in step (b) is polymerized to obtain poly(meth)acrylate in the presence of the polyester-polyurethane obtained in step (a). Thus, the polyester-polyurethane of step (a) can be physically mixed with and / or covalently bonded with the poly(meth)acrylate of step (b). The poly(meth)acrylate of step (b) can be covalently bonded with the polyester-polyurethane of step (a), for example, if the polyester-polyurethane of step (a) contains ethylenically unsaturated groups, and / or if radical formation in the polyester-polyurethane of step (a) occurs by hydrogen detachment, resulting in the attachment of ethylenically unsaturated (meth)acrylic monomers to the polyester-polyurethane. In this way, there is no better way to represent the polyester-polyurethane-poly(meth)acrylic hybrid dispersion of the present invention than by the method by which it is obtained.

[0028] A polyester-polyurethane-poly(meth)acrylic hybrid dispersion can be obtained by the following reaction steps (a) and (b).

[0029] Process a Polyester-polyurethane is obtained by esterifying a polyurethane containing at least one carboxyl group, having an acid value of more than 200 mg KOH / g and 400 mg KOH / g and at least one terminal carboxyl group, with a polyester containing at least one hydroxyl group, having a hydroxyl value of 50 mg KOH / g to 300 mg KOH / g.

[0030] i. Polyurethane synthesis At least one polyurethane is synthesized by reacting one or more diisocyanates, one or more diols, and one or more carboxyl group-containing and / or carboxyl group-forming monomers.

[0031] The diol can be saturated or ethylenically unsaturated, more preferably saturated, and the saturated or ethylenically unsaturated diol can be substituted or unsubstituted. The diol can be aromatic or aliphatic, more preferably aliphatic. The aliphatic diol can be linear, branched, or cyclic, preferably having 2 to 40 carbon atoms, more preferably 2 to 20 carbon atoms, even more preferably 2 to 16 carbon atoms, and most preferably 4 to 10 carbon atoms. Preferably, at least one diol is substituted, and more preferably, the substituted diol contains one or more carboxyl groups.

[0032] Suitable examples of saturated monomer diols include ethylene glycol, neopentyl glycol, tripropylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,3-butanediol, 1,2-butanediol, 1,5-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, 1,2-cyclohexanedimethanol, 2,2-bis(4-hydroxycyclohexyl)-propane, dimethylolpropionic acid, and dimethylolbutyric acid. The saturated monomer diol is preferably ethylene glycol and / or dimethylolpropionic acid.

[0033] Ethylene-unsaturated diols preferably contain at least one allyl group, vinyl group, acrylic group, or methacrylic group. Examples of ethylenically unsaturated monomer diols are trimethylolpropane monoallyl ether and pentaerythritol diallyl ether.

[0034] Preferably, one or more diols are ethylene glycol and / or dimethylolpropionic acid.

[0035] Polyurethanes are synthesized by reacting at least one diol with one or more diisocyanates. The one or more diisocyanates can be aromatic or aliphatic, more preferably aliphatic. The aliphatic diisocyanates can be linear or cyclic, more preferably cyclic.

[0036] Preferred examples of alicyclic diisocyanates include isophorone diisocyanate (= 5-isocyanato-1-isocyanatomethyl-1,3,3-trimethylcyclohexane), 5-isocyanato-1-(2-isocyanatoetho-1-yl)-1,3,3-trimethylcyclohexane, 5-isocyanato-1-(3-isocyanatoprop-1-yl)-1,3,3-trimethylcyclohexane, 5-isocyanato-(4-isocyanatobuto-1-yl)-1,3,3-trimethylcyclohexane, 1-isocyanato-2-(3-isocyanatoprop-1-yl)cyclohexane, and 1-I These are socyanato-2-(2-isocyanatoetho-1-yl)cyclohexane, 1-isocyanato-2-(4-isocyanatobuto-1-yl)cyclohexane, 1,2-diisocyanatocyclobutane, 1,3-diisocyanatocyclobutane, 1,2-diisocyanatocyclopentane, 1,3-diisocyanatocyclopentane, 1,2-diisocyanatocyclohexane, 1,3-diisocyanatocyclohexane, 1,4-diisocyanatocyclohexane, dicyclohexylmethane 2,4'-diisocyanate, and 4,4'-methylenebis(cyclohexyl isocyanate).

[0037] Preferred examples of aromatic diisocyanates include 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, diphenylmethane-4,4'-diisocyanate, p-phenylenediisocyanate, biphenyl diisocyanate, 3,3'-dimethyl-4,4'-diphenylenediisocyanate, and tetramethylxylene diisocyanate.

[0038] Examples of linear aliphatic diisocyanates include ethylene diisocyanate, trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, 2,2,4-trimethylhexane-1,6-diisocyanate, heptamethylene diisocyanate, and 1,12-dodecane diisocyanate.

[0039] One or more diisocyanates are preferably isophorone diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), and / or tetramethylxylene diisocyanate.

[0040] One or more diisocyanates are reacted, preferably with one or more diols, in a solvent. The solvent is preferably an organic solvent. Examples of organic solvents suitable for the present invention include heterocyclic, aliphatic or aromatic hydrocarbons, monofunctional or polyfunctional alcohols, ethers, esters, ketones and amides, such as N-methylpyrrolidone, N-ethylpyrrolidone, dimethylformamide, toluene, xylene, butanol, ethyl glycol and butyl glycol and their acetates, butyl diglycol, diethylene glycol dimethyl ether, cyclohexanone, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), acetone, isophorone, or mixtures thereof. Preferably, the organic solvent is methyl ethyl ketone (MEK).

[0041] The hydroxy-terminated polyurethanes obtained in this way can be synthesized in a one-step or two-step process. In the one-step process, one or more diisocyanates are reacted with one or more diols, and the hydroxy-terminated polyurethane is prepared using an excess of the diols. In the two-step process, one or more diisocyanates are first reacted with one or more diols. Subsequently, one or more diols are added to react with the terminal NCO group and prepare the hydroxy-terminated polyurethane. In the two-step process, the one or more diols that react with the free isocyanate group are preferably ethylene glycols.

[0042] The reaction of one or more diisocyanates with one or more diols is carried out until, preferably less than 2% by mass, and most preferably less than 1% by mass, of NCO- groups are converted relative to the mass of the polyurethane. As a result, the polyurethane is substantially free of free NCO- groups, and the isocyanate content (NCO content) is measured by adding an excess of a 2% N,N-dibutylamine solution in xylene to a homogeneous solution of the sample in acetone / N-ethylpyrrolidone (1:1 vol%), and then potentiometric back titrating the excess amine with 0.1N hydrochloric acid according to DIN EN ISO 3251, DIN EN ISO 11909, and DIN EN ISO 14886.

[0043] The hydroxy-terminated polyurethane thus obtained is reacted with one or more carboxyl group-containing monomers and / or carboxyl group-forming group-containing monomers. These monomers are preferably polycarboxylic acids and their anhydrides, preferably dicarboxylic acids, tricarboxylic acids and / or their anhydrides. The term "carboxyl group-forming group" preferably refers to the ability of a functional group to form a carboxyl group by hydrolysis of the corresponding anhydride group or ester group.

[0044] Polycarboxylic acids and their anhydrides can be aromatic or aliphatic, preferably having 2 to 20 carbon atoms, more preferably 2 to 16 carbon atoms, even more preferably 4 to 12 carbon atoms, and most preferably 6 to 10 carbon atoms.

[0045] Suitable examples of aliphatic dicarboxylic acids include ethanedioic acid (oxalic acid), propanedioic acid (malonic acid), butanedioic acid (succinic acid), pentanedioic acid (glutaric acid), hexanedioic acid (adipic acid), heptanedioic acid (pimelic acid), octanodioic acid (suberic acid), nonanedioic acid (azelaic acid), decanedioic acid (sebacic acid), maleic acid, hexahydrophthalic acid, and their respective anhydrides.

[0046] Suitable examples of aromatic dicarboxylic acids include 1,2-benzenedicarboxylic acid (phthalic acid), 1,3-benzenedicarboxylic acid (isophthalic acid), and 1,4-benzenedicarboxylic acid (terephthalic acid), and their respective anhydrides.

[0047] Suitable tricarboxylic acids include citric acid, isocitric acid, aconitic acid, propane-1,2,3-tricarboxylic acid, agaric acid, trimesic acid, trimellitic acid, and their respective anhydrides.

[0048] Preferably, the hydroxy-terminated polyurethane is reacted with trimellitic anhydride.

[0049] The reaction is stopped at a certain acid value. The resulting polyurethane has at least one terminal carboxyl group, preferably the polyurethane has one or more terminal carboxyl groups and one or more carboxyl groups in the backbone, more preferably the polyurethane has at least two carboxyl groups per terminal, and most preferably the polyurethane has at least two carboxyl groups per terminal and contains one or more carboxyl groups in the backbone.

[0050] The resulting polyurethane can be linear or branched, preferably linear.

[0051] The resulting polyurethane has an acid value of more than 200 mg KOH / g and up to 400 mg KOH / g, preferably more than 205 mg KOH / g and up to 350 mg KOH / g, more preferably more than 210 mg KOH / g and up to 300 mg KOH / g, even more preferably more than 220 mg KOH / g and up to 300 mg KOH / g, and most preferably more than 240 mg KOH / g and up to 300 mg KOH / g, which is measured according to DIN EN ISO2114.

[0052] Preferably, the resulting polyurethane has a hydroxyl value in the range of 0 mg KOH / g to 50 mg KOH / g, more preferably 0 mg KOH / g to 46 mg KOH / g, even more preferably 0 mg KOH / g to 42 mg KOH / g, and most preferably 0 mg KOH / g to 40 mg KOH / g, which is measured at room temperature in a tetrahydrofuran (THF) / dimethylformamide (DMF) solution in the presence of 4-dimethylaminopyridine as a catalyst, using acetic anhydride, according to R.-P. Krueger, R. Gnauck and R. Algeier (Plaste und Kautschuk, 20, 274 (1982)).

[0053] Subsequently, the obtained polyurethane is diluted with a solvent, preferably an organic solvent, to a solid content of preferably 60% to 80% by mass, more preferably 65% ​​to 75% by mass. This solid content is measured using a 1.0 g weighing unit at 130°C for 60 minutes according to DIN EN ISO 3251.

[0054] ii. Synthesis of polyester At least one polyester is synthesized by reacting one or more polyols with one or more monomers selected from the group consisting of dicarboxylic acids and cyclic acid anhydrides. At least one polyester can be saturated or ethylenically unsaturated.

[0055] Polyols can be saturated or ethylenically unsaturated, more preferably saturated, and saturated or ethylenically unsaturated polyols can be substituted or unsubstituted. Polyols can be aromatic or aliphatic, more preferably aliphatic. Aliphatic polyols can be linear, branched, or cyclic, preferably having 2 to 40 carbon atoms, more preferably 2 to 20 carbon atoms, even more preferably 2 to 16 carbon atoms, and most preferably 4 to 10 carbon atoms.

[0056] Suitable examples of saturated monomer polyols include ethylene glycol, neopentyl glycol, tripropylene glycol, 1,2-propanediol, 1,4-butanediol, 1,3-butanediol, 1,5-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, 1,2-cyclohexanedimethanol, 2,2-bis(4-hydroxycyclohexyl)propane, trimethylolpropane, trimethylolethane, trimethylolhexane, glycerol, 1,2,4-butanetriol, ditrimethylolpropane, pentaerythritol, and dipentaerythritol.

[0057] Ethylene-unsaturated polyols preferably contain at least one allyl group, vinyl group, acrylic group, or methacrylic group. Examples of ethylenically unsaturated monomer polyols are trimethylolpropane monoallyl ether and pentaerythritol diallyl ether.

[0058] Preferably, one or more polyols are neopentyl glycol, tripropylene glycol, 1,6-hexanediol and / or trimethylolpropane.

[0059] A polyester is synthesized by reacting at least one polyol with one or more monomers selected from the group consisting of dicarboxylic acids, tricarboxylic acids, and cyclic acid anhydrides.

[0060] The dicarboxylic acid can be an aromatic or aliphatic compound having preferably 2 to 50 carbon atoms, more preferably 2 to 44 carbon atoms, even more preferably 4 to 44 carbon atoms, and most preferably 6 to 44 carbon atoms.

[0061] Suitable examples of aliphatic dicarboxylic acids include ethanedioic acid (oxalic acid), propanedioic acid (malonic acid), butanedioic acid (succinic acid), pentanedioic acid (glutaric acid), hexanedioic acid (adipic acid), heptanedioic acid (pimelic acid), octanodioic acid (suberic acid), nonanodioic acid (azelaic acid), decandioic acid (sebacic acid), maleic acid, and hexahydrophthalic acid. Preferably, hexanedioic acid (adipic acid) is used as the aliphatic dicarboxylic acid. Suitable examples of aromatic dicarboxylic acids include 1,2-benzenedicarboxylic acid (phthalic acid), 1,3-benzenedicarboxylic acid (isophthalic acid), and 1,4-benzenedicarboxylic acid (terephthalic acid).

[0062] A further possibility is to use dimer fatty acids as polycarboxylic acids. Dimer fatty acids are mixtures produced by the oligomerization of unsaturated fatty acids. 12 ~C 22 Fatty acids are used as starting materials. Suitable dimer fatty acids include, for example, Radiacid0970, Radiacid0971, Radiacid0972, Radiacid0975, Radiacid0976, Radiacid0977, Pripol1006, Pripol1009, Pripol1012 and Pripol1013, Empol1008, Empol1061 and Empol1062 (WO2015 / 028201A1).

[0063] Preferably, the dicarboxylic acid is aromatic, and more preferably is an isophthalic acid.

[0064] Suitable tricarboxylic acids include citric acid, isocitric acid, aconitic acid, propane-1,2,3-tricarboxylic acid, agaric acid, trimesic acid, and trimellitic acid.

[0065] The cyclic acid anhydride preferably has 2 to 40 carbon atoms, more preferably 2 to 30 carbon atoms, even more preferably 4 to 20 carbon atoms, and most preferably 6 to 18 carbon atoms. The cyclic acid anhydride can be saturated or ethylenically unsaturated.

[0066] Suitable examples of cyclic acid anhydrides include phthalic anhydride, trimellitic anhydride, maleic anhydride and its derivatives, and alkenyl succinic anhydrides, such as tetrapropenyl succinic anhydride. Preferably, one or more cyclic acid anhydrides are phthalic anhydride, trimellitic anhydride and / or tetrapropenyl succinic anhydride.

[0067] One or more polyols are reacted with one or more monomers selected from the group consisting of dicarboxylic acids and cyclic acid anhydrides at a temperature preferably of 200°C to 250°C, more preferably of 210°C to 240°C.

[0068] The hydroxyl value of the resulting polyester is 50 mg KOH / g to 300 mg KOH / g, preferably 60 to 280 mg KOH / g, more preferably 70 to 250 mg KOH / g, even more preferably 100 to 250 mg KOH / g, and most preferably 120 to 250 mg KOH / g, which is measured at room temperature in a tetrahydrofuran (THF) / dimethylformamide (DMF) solution in the presence of 4-dimethylaminopyridine as a catalyst, using acetic anhydride, according to R.-P. Krueger, R. Gnauck and R. Algeier (Plaste und Kautschuk, 20, 274 (1982)).

[0069] Preferably, the acid value of the resulting polyester is less than 20 mgKOH / g, more preferably less than 18 mgKOH / g, even more preferably less than 15 mgKOH / g, and most preferably less than 12 mgKOH / g, which is measured according to DIN EN ISO2114.

[0070] The resulting polyester can be linear or branched, preferably branched.

[0071] iii. Synthesis of polyester-polyurethane (PEU) or polyester-polyurethane dispersion (PEUD) The polyester and polyurethane are mixed, and the temperature is carefully raised, preferably to 120°C to 180°C, more preferably to 130°C to 170°C, under reduced pressure. Preferably, the pressure is 15 mbar to 80 mbar, more preferably to 15 mbar to 70 mbar. The process can be monitored by titration and viscosity measurement at 140°C. The reaction is stopped when the acid value reaches preferably 10 mg KOH / g to 50 mg KOH / g, more preferably 15 mg KOH / g to 45 mg KOH / g, most preferably 20 mg KOH / g to 40 mg KOH / g, and / or when the viscosity reaches preferably 1000 mPa*s to 2400 mPa*s, more preferably 1200 mPa*s to 2200 mPa*s, most preferably 1300 mPa*s to 2000 mPa*s, which is measured at a temperature of 140°C for 1250 seconds using a CAP2000H viscometer with spindle 03. -1 The shear rate is used and measured according to DIN EN ISO2884-1. The temperature is lowered to preferably 60°C to 120°C, more preferably 70°C to 115°C.

[0072] The polyester-polyurethane can be reacted with at least one ethylenically unsaturated monomer as outlined in step b, either by adding one or more solvents after neutralization with a neutralizing agent, or without adding one or more solvents.

[0073] Suitable examples of neutralizing agents include alkyl alkanolamines, such as dimethylethanolamine (DMEA), diethylethanolamine (DEEA), methyldiethanolamine (MDEA), or methylethanolamine (NMEA). Preferably, dimethylethanolamine is used as the neutralizing agent.

[0074] One or more solvents may be present and / or used between steps (a) and / or (b), and / or added after step (b), and the solvent may be present during the preparation of the polyester and / or polyurethane, and / or during step (a), and / or during the esterification of the polyester and polyurethane in step (b), and the solvent may be present before, during, and / or after the addition of the (meth)acrylic monomer and / or radical initiator. At least one polyurethane and at least one polyester in step (a) may be esterified in the presence of one or more solvents to obtain a polyester-polyurethane dispersion.

[0075] The solvent can be water or an organic solvent. Preferably, water is added to adjust the solid content and produce an aqueous polyester-polyurethane dispersion.

[0076] Preferably, the synthesized polyester-polyurethane dispersion has a solids content of ≥40% by mass, more preferably ≥42% by mass, even more preferably ≥45% by mass, and most preferably ≥48% by mass, which is measured using a 1.0 g weighing unit at 130°C for 60 minutes according to DIN EN ISO3251.

[0077] Preferably, the polyester-polyurethane dispersion is heated for 1000 seconds at a temperature of 23°C using a Rheolab QC rotational rheometer equipped with cylinder cc27. -1 Using the shear rate, the viscosity is measured according to DIN53019-1 and is 100 mPa*s to 300 mPa*s, more preferably 110 mPa*s to 290 mPa*s, even more preferably 120 mPa*s to 280 mPa*s, and most preferably 130 mPa*s to 260 mPa*s.

[0078] Preferably, the polyester-polyurethane has an acid value in the range of 10 mg KOH / g to 50 mg KOH / g, more preferably 15 mg KOH / g to 45 mg KOH / g, even more preferably 20 mg KOH / g to 40 mg KOH / g, and most preferably 25 mg KOH / g to 35 mg KOH / g, which is measured according to DIN EN ISO 2114.

[0079] Preferably, the polyester-polyurethane has a particle size of 50 nm to 200 nm, more preferably 70 nm to 180 nm, even more preferably 80 nm to 150 nm, and most preferably 90 nm to 130 nm, which is measured by measuring the hydrodynamic volume / hydrodynamic radius of the dispersed particles using photon correlation spectroscopy (PCS).

[0080] Preferably, the polyester-polyurethane has a number-average molecular weight (M) of 1,000 g / mol to 3,500 g / mol, more preferably 1,200 g / mol to 3,200 g / mol, even more preferably 1,500 g / mol to 3,000 g / mol, and most preferably 1,800 g / mol to 2,800 g / mol. n ) is present, which is measured by gel permeation chromatography using a poly(meth)acrylate standard and a tetrahydrofuran / acetic acid mixture (1 mole of acetic acid per liter of tetrahydrofuran).

[0081] Preferably, the polyester-polyurethane has a mass-average molecular weight (M) of 6,000 g / mol to 50,000 g / mol, more preferably 7,000 g / mol to 48,000 g / mol, even more preferably 8,000 g / mol to 46,000 g / mol, and most preferably 9,000 g / mol to 43,000 g / mol. w ) is present, which is measured by gel permeation chromatography using a poly(meth)acrylate standard and a tetrahydrofuran / acetic acid mixture (1 mole of acetic acid per liter of tetrahydrofuran).

[0082] Process b In the presence of the polyester-polyurethane of step (a), an ethylenically unsaturated monomer containing at least a (meth)acrylic monomer is polymerized by radical polymerization to obtain a poly(meth)acrylate.

[0083] The ethylenically unsaturated monomer of step (b) is added to the polyester-polyurethane dispersion or undiluted polyester-polyurethane of step (a) before the addition of the radical initiator, simultaneously with the radical initiator, and / or after the radical initiator. If the ethylenically unsaturated monomer is added to the polyester-polyurethane of step (a) before the addition of the radical initiator, the ethylenically unsaturated monomer and the polyester-polyurethane of step (a) are incubated preferably for at least 10 minutes, more preferably at least 30 minutes, even more preferably at least 60 minutes, most preferably at least 2 hours, for example at least 4 hours, preferably at a temperature of 20°C to 30°C.

[0084] A polyester-polyurethane dispersion containing a (meth)acrylic monomer can be obtained by adding a solvent to the polyester-polyurethane before or after the addition of a (meth)acrylic monomer or a radical initiator. The solvent can be water or an organic solvent. Preferably, water is added to adjust the solids content and produce an aqueous polyester-polyurethane dispersion.

[0085] The ethylenically unsaturated monomer can be a cyclic, linear, or branched alkyl (meth)acrylate, a hydroxyalkyl ester of (meth)acrylic acid, (meth)acrylic acid, and / or vinyl aromatic hydrocarbon. The ethylenically unsaturated monomer can be monoethylenically unsaturated or polyethylenically unsaturated, and the functional value of the polyethylenically unsaturated monomer can be in the range of 2 to 5. Preferably, the polyethylenically unsaturated monomer is diethylenically unsaturated or triethylenically unsaturated, and most preferably diethylenically unsaturated. Preferably, the ethylenically unsaturated monomer is a monoethylenically unsaturated monomer or a mixture of a monoethylenically unsaturated monomer and a diethylenically unsaturated monomer.

[0086] Preferred cyclic, linear, or branched alkyl (meth)acrylates are cyclohexyl (meth)acrylates and alkyl (meth)acrylates having 20 or fewer carbon atoms. Preferred monoethylenically unsaturated alkyl (meth)acrylates are t-butyl acrylate, n-butyl acrylate, n-butyl methacrylate, methyl methacrylate, ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate, with t-butyl acrylate, n-butyl acrylate, n-butyl methacrylate, and ethylhexyl methacrylate being the most preferred.

[0087] Suitable hydroxyalkyl esters of (meth)acrylic acid are hydroxyalkyl esters of (meth)acrylic acid containing 6 or fewer carbon atoms in the hydroxyalkyl group, preferably 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate.

[0088] Suitable diethylenically unsaturated monomers are ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, 1,2-propanediol di(meth)acrylate, 1,3-propanediol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,5-pentanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, tricyclodecanedimethanol di(meth)acrylate, allyl(meth)acrylate, and divinylbenzene. Suitable polyethylenically unsaturated monomers are trimethylolpropane tri(meth)acrylate, pentaerythritol tri- and tetraacrylate, tris(2-hydroxyethyl) isocyanurate triacrylate, and ethoxylated 3-trimethylolpropane triacrylate.

[0089] Suitable vinyl aromatic hydrocarbons include styrene, α-alkylstyrene, vinyltoluene, (meth)acrylamide, and (meth)acrylonitrile.

[0090] Preferably, the ethylenically unsaturated monomer in step (b) is an alkyl (meth)acrylate, more preferably t-butyl acrylate, n-butyl acrylate, n-butyl methacrylate, and ethylhexyl methacrylate.

[0091] The ethylenically unsaturated monomer in step (b) is added to the polyester-polyurethane in step (a) before or simultaneously with the addition of the radical initiator.

[0092] To initiate radical polymerization, water-soluble or water-insoluble initiators can be used. Examples of water-soluble initiators include hydrogen peroxide, peroxydisulfates such as sodium, potassium, and ammonium peroxydisulfates, ammonium salts of 4,4'-azobis(4-cyanopentanoic acid), 2,2'-azobis(2-methyl-N-1,1-bis(hydroxymethyl)ethyl)propionamide, and 2,2'-azobis(2-methyl-N-2-hydroxyethyl)propionamide). Preferably, ammonium peroxydisulfate (APS) is used as a water-soluble initiator.

[0093] Examples of water-insoluble initiators include tert.butyl-peroxy-2-ethylhexanol, tert.butyl-peroxypivalate, and dibenzoyl peroxide. Preferably, tert.butyl-peroxy-2-ethylhexanol is used as the water-insoluble initiator. Preferably, radical polymerization is initiated by a water-insoluble initiator, more preferably by tert.butyl-peroxy-2-ethylhexanol.

[0094] The radical initiator generates radicals within the ethylenically unsaturated polyester-polyurethane polymer and / or within the ethylenically unsaturated monomer. This yields a poly(meth)acrylate, which can be physically mixed with the polyester-polyurethane of step (a) or covalently bonded with the polyester-polyurethane of step (a). For example, the poly(meth)acrylate can be covalently bonded with the polyester-polyurethane of step (a) by forming a graft polymer formed by radical copolymerization of the ethylenically unsaturated monomer with the ethylenically unsaturated groups in the backbone of the polyester-polyurethane of step (a), and / or by abstracting H on the backbone of the polyester-polyurethane of step (a).

[0095] Preferably, the solids content of the resulting polyester-polyurethane-poly(meth)acrylic hybrid dispersion is ≥40% by mass, more preferably ≥42% by mass, even more preferably ≥43% by mass, even more preferably ≥44% by mass, even more preferably ≥48% by mass, and most preferably ≥50% by mass, which is measured using a 1.0 g weighing unit at 130°C for 60 minutes according to DIN EN ISO3251.

[0096] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid has a glass transition temperature of -50°C to +50°C, more preferably -48°C to 40°C, even more preferably -45°C to 35°C, and most preferably -45°C to 30°C, which is measured according to DIN-EN-ISO11357-1 and -2.

[0097] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid prepared using one or more monoethylenically unsaturated monomers has a number average molecular weight (M) of 2,500 g / mol to 5,000 g / mol, more preferably 2,700 g / mol to 4,800 g / mol, and most preferably 3,000 g / mol to 4,500 g / mol. n ) is present, which is measured by gel permeation chromatography using a poly(meth)acrylate standard and a tetrahydrofuran / acetic acid mixture (1 mole of acetic acid per liter of tetrahydrofuran).

[0098] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid prepared using one or more monoethylenically unsaturated monomers has a mass-average molecular weight (M) of 25,000 g / mol to 550,000 g / mol, more preferably 30,000 g / mol to 500,000 g / mol, even more preferably 50,000 g / mol to 450,000 g / mol, and most preferably 100,000 g / mol to 400,000 g / mol. w) as determined by gel permeation chromatography using poly(meth)acrylate standards and a tetrahydrofuran / acetic acid mixture (1 mol acetic acid per liter of tetrahydrofuran).

[0099] The number average molecular weight (M n ) and weight average molecular weight (M w ) of the polyester-polyurethane-poly(meth)acrylic hybrid prepared using at least one polyethylenically unsaturated monomer, preferably at least one diethylenically unsaturated monomer, may be even higher than the number average molecular weight (M n ) and weight average molecular weight (M w ) described in the two preceding paragraphs of this specification.

[0100] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid has an acid value of 5 mg KOH / g to 50 mg KOH / g, more preferably 10 mg KOH / g to 45 mg KOH / g, even more preferably 15 mg KOH / g to 40 mg KOH / g, even more preferably 15 mg KOH / g to 35 mg KOH / g, most preferably 15 mg KOH / g to 30 mg KOH / g, as determined in accordance with DIN EN ISO 2114.

[0101] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid dispersion has a viscosity of 5 mPa·s to 3000 mPa·s, more preferably 10 mPa·s to 2500 mPa·s, even more preferably 10 mPa·s to 1000 mPa·s, even more preferably 10 mPa·s to 500 mPa·s, even more preferably 10 mPa·s to 200 mPa·s, as measured in accordance with DIN 53019-1 using a Rheolab QC rotational rheometer at a temperature of 23° C. and a shear rate of 1000 s -1 .

[0102] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid dispersion has a particle size of 50 nm to 400 nm, more preferably 70 nm to 300 nm, even more preferably 100 nm to 250 nm, and most preferably 120 nm to 220 nm, which is measured by measuring the hydrodynamic volume / hydrodynamic radius of the dispersed particles using photon correlation spectroscopy (PCS).

[0103] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid dispersion comprises 45-90% by mass of polyester-polyurethane in step (a) and 10-55% by mass of poly(meth)acrylate obtained in step (b), more preferably 50-90% by mass of polyester-polyurethane in step (a) and 10-50% by mass of poly(meth)acrylate obtained in step (b), and even more preferably 55-90% by mass of polyester-polyurethane in step (a) and 10-45% by mass of step (b) The mixture comprises poly(meth)acrylate obtained by step (a), more preferably 60-90% by mass of polyester-polyurethane from step (a) and 10-40% by mass of poly(meth)acrylate obtained by step (b), most preferably 65-90% by mass of polyester-polyurethane from step (a) and 10-35% by mass of poly(meth)acrylate obtained by step (b), where these mass percent are relative to the solid content of the polyester-polyurethane-poly(meth)acrylic hybrid dispersion.

[0104] Method for manufacturing a polyester-polyurethane-poly(meth)acrylic hybrid dispersion The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention can be obtained by first step (a) esterifying a polyurethane containing at least one carboxyl group having an acid value of more than 200 mg KOH / g to 400 mg KOH / g and at least one terminal carboxyl group with a polyester containing at least one hydroxyl group having a hydroxyl value of 50 mg KOH / g to 300 mg KOH / g to obtain polyester-polyurethane, and then in the subsequent second step (b) polymerizing an ethylenically unsaturated monomer containing at least a (meth)acrylic monomer by radical polymerization in the presence of the polyester-polyurethane from step (a) to obtain poly(meth)acrylate, wherein one or more solvents are present and / or used between steps (a) and / or (b) and / or added after step (b).

[0105] Step (a): Preparation of polyester-polyurethane (PEU) or polyester-polyurethane dispersion (PEUD) The polyester-polyurethane in the polyester-polyurethane-poly(meth)acrylic dispersion is produced by esterifying a polyurethane containing at least one carboxyl group (at least one polyurethane having an acid value greater than 200 mg KOH / g and between 400 mg KOH / g and at least one terminal carboxyl group) with a polyester containing at least one hydroxyl group (the polyester having a hydroxyl value between 50 mg KOH / g and 300 mg KOH / g).

[0106] Polyurethanes are synthesized by reacting one or more diisocyanates, one or more diols, and one or more carboxyl group-containing and / or carboxyl group-forming monomers. The diols, diisocyanates, and carboxyl group-containing and / or carboxyl group-forming monomers are the same as those described above in item i. Synthesis of Polyurethanes.

[0107] The reaction between one or more diisocyanates and one or more diols is carried out until, preferably less than 2% by mass, and most preferably less than 1% by mass, of the NCO- groups are converted relative to the mass of the polyurethane. This results in the polyurethane being substantially free of free NCO- groups.

[0108] The hydroxy-terminated polyurethane thus obtained is reacted with one or more monomers containing a carboxyl group and / or a carboxyl group forming group. This monomer is preferably a polycarboxylic acid and its anhydride, preferably a dicarboxylic acid, tricarboxylic acid, and / or its anhydride. Suitable dicarboxylic acids, tricarboxylic acids, and their anhydrides are shown above.

[0109] Preferably, the hydroxy-terminated polyurethane is reacted with trimellitic anhydride.

[0110] The reaction is stopped at a certain acid value. The resulting polyurethane has at least one terminal carboxyl group, preferably the polyurethane has one or more terminal carboxyl groups and one or more carboxyl groups in its skeleton, more preferably the polyurethane has at least two carboxyl groups per terminal, and most preferably the polyurethane has at least two carboxyl groups per terminal and contains one or more carboxyl groups in its skeleton.

[0111] The resulting polyurethane can be linear or branched, preferably linear.

[0112] The resulting polyurethane has an acid value of more than 200 mg KOH / g and up to 400 mg KOH / g, preferably more than 205 mg KOH / g and up to 350 mg KOH / g, more preferably more than 210 mg KOH / g and up to 300 mg KOH / g, even more preferably more than 220 mg KOH / g and up to 300 mg KOH / g, and most preferably more than 240 mg KOH / g and up to 300 mg KOH / g, which is measured according to DIN EN ISO2114.

[0113] Subsequently, the obtained polyurethane is diluted with a solvent, preferably an organic solvent, to a solid content of preferably 60% to 80% by mass, more preferably 65% ​​to 75% by mass. This solid content is measured using a 1.0 g weighing unit at 130°C for 60 minutes according to DIN EN ISO 3251.

[0114] At least one polyester is synthesized by reacting one or more polyols with one or more monomers selected from the group consisting of dicarboxylic acids and cyclic acid anhydrides. The polyols and one or more monomers selected from the group consisting of dicarboxylic acids and cyclic acid anhydrides are the same as those described above in item ii. Synthesis of Polyesters.

[0115] One or more polyols are reacted with one or more monomers selected from the group consisting of dicarboxylic acids and cyclic acid anhydrides at a temperature preferably of 200°C to 250°C, more preferably of 210°C to 240°C.

[0116] The resulting polyester can be linear or branched, preferably branched.

[0117] The hydroxyl value of the resulting polyester is 50 mg KOH / g to 300 mg KOH / g, preferably 60 to 280 mg KOH / g, more preferably 70 to 250 mg KOH / g, even more preferably 100 to 250 mg KOH / g, and most preferably 120 to 250 mg KOH / g, which is measured at room temperature in a tetrahydrofuran (THF) / dimethylformamide (DMF) solution in the presence of 4-dimethylaminopyridine as a catalyst, using acetic anhydride, according to R.-P. Krueger, R. Gnauck and R. Algeier (Plaste und Kautschuk, 20, 274 (1982)).

[0118] The acid value of the resulting polyester is less than 20 mgKOH / g, preferably less than 18 mgKOH / g, more preferably less than 15 mgKOH / g, and most preferably less than 12 mgKOH / g, which is measured according to DIN EN ISO2114.

[0119] The polyester and polyurethane are mixed, and the temperature is carefully raised, preferably to 120°C to 180°C, more preferably to 130°C to 170°C, under reduced pressure. Preferably, the pressure is 15 mbar to 80 mbar, more preferably to 15 mbar to 70 mbar. The process is monitored by titration and viscosity measurement at 140°C. Preferably, the reaction is stopped when the acid value reaches preferably 10 to 50 mg KOH / g, more preferably 15 to 45 mg KOH / g, most preferably 20 mg KOH / g to 40 mg KOH / g, and / or when the viscosity reaches preferably 1000 mPa*s to 2400 mPa*s, more preferably 1200 mPa*s to 2200 mPa*s, most preferably 1300 mPa*s to 2000 mPa*s, measured at a temperature of 140°C for 1250 seconds using a CAP2000H viscometer with spindle 03. -1 The shear rate is used and measured according to DIN EN ISO2884-1.

[0120] The temperature is preferably lowered to 60°C to 120°C, more preferably to 70°C to 115°C.

[0121] The polyester-polyurethane can be reacted with at least one ethylenically unsaturated monomer as outlined in step (b), either by adding one or more solvents after neutralization with a neutralizing agent, or without adding one or more solvents.

[0122] Suitable examples of neutralizing agents include alkyl alkanolamines, such as dimethylethanolamine (DMEA), diethylethanolamine (DEEA), methyldiethanolamine (MDEA), or methylethanolamine (NMEA). Preferably, dimethylethanolamine is used as the neutralizing agent.

[0123] One or more solvents may be present and / or used between steps (a) and / or (b), and / or added after step (b), and the solvent may be present during the preparation of the polyester and / or polyurethane, and / or during step (a), and / or during the esterification of the polyester and polyurethane in step (b), and the solvent may be present before, during, and / or after the addition of the (meth)acrylic monomer and / or radical initiator. At least one polyurethane and at least one polyester in step (a) may be esterified in the presence of one or more solvents to obtain a polyester-polyurethane dispersion.

[0124] Preferably, a solvent is added to adjust the solid content of the polyester-polyurethane dispersion. The solvent can be water or an organic solvent. Preferably, water is added to adjust the solid content and produce an aqueous polyester-polyurethane dispersion.

[0125] Preferably, the synthesized polyester-polyurethane dispersion has a solids content of ≥40% by mass, more preferably ≥42% by mass, and most preferably ≥45% by mass, which is measured using a 1.0 g weighing unit at 130°C for 60 minutes according to DIN EN ISO 3251.

[0126] Preferably, the polyester-polyurethane dispersion is heated for 1000 seconds at a temperature of 23°C using a Rheolab QC rotational rheometer equipped with cylinder cc27. -1 Using the shear rate, the viscosity is measured according to DIN53019-1 and is 100 mPa*s to 300 mPa*s, more preferably 110 mPa*s to 290 mPa*s, even more preferably 120 mPa*s to 280 mPa*s, and most preferably 130 mPa*s to 260 mPa*s.

[0127] Preferably, the polyester-polyurethane has an acid value in the range of 10 mg KOH / g to 50 mg KOH / g, more preferably 15 mg KOH / g to 45 mg KOH / g, even more preferably 20 mg KOH / g to 40 mg KOH / g, and most preferably 25 mg KOH / g to 35 mg KOH / g, which is measured according to DIN EN ISO 2114.

[0128] Preferably, the polyester-polyurethane has a particle size of 50 nm to 200 nm, more preferably 70 nm to 180 nm, even more preferably 80 nm to 150 nm, and most preferably 90 nm to 130 nm, which is measured by measuring the hydrodynamic volume / hydrodynamic radius of the dispersed particles using photon correlation spectroscopy (PCS).

[0129] Preferably, the polyester-polyurethane has a number-average molecular weight (M) of 1,000 g / mol to 3,500 g / mol, more preferably 1,200 g / mol to 3,200 g / mol, even more preferably 1,500 g / mol to 3,000 g / mol, and most preferably 1,800 g / mol to 2,800 g / mol. n ) is present, which is measured by gel permeation chromatography using a poly(meth)acrylate standard and a tetrahydrofuran / acetic acid mixture (1 mole of acetic acid per liter of tetrahydrofuran).

[0130] Preferably, the polyester-polyurethane has a mass-average molecular weight (M) of 6,000 g / mol to 50,000 g / mol, more preferably 7,000 g / mol to 48,000 g / mol, even more preferably 8,000 g / mol to 46,000 g / mol, and most preferably 9,000 g / mol to 43,000 g / mol. w ) is present, which is measured by gel permeation chromatography using a poly(meth)acrylate standard and a tetrahydrofuran / acetic acid mixture (1 mole of acetic acid per liter of tetrahydrofuran).

[0131] Step (b): Preparation of poly(meth)acrylate In the presence of the polyester-polyurethane of step (a), an ethylenically unsaturated monomer containing at least a (meth)acrylic monomer is polymerized by radical polymerization to obtain a poly(meth)acrylate.

[0132] Ethylene-unsaturated monomers can be added to a neutralized and / or diluted polyester-polyurethane dispersion or an undiluted polyester-polyurethane. The ethylenically unsaturated monomer of step (b) is added to the polyester-polyurethane of step (a) before or simultaneously with the addition of the radical initiator. If the ethylenically unsaturated monomer is added to the polyester-polyurethane of step (a) before the addition of the radical initiator, the ethylenically unsaturated monomer and the polyester-polyurethane of step (a) are incubated preferably for at least 10 minutes, more preferably at least 30 minutes, even more preferably at least 60 minutes, most preferably at least 2 hours, for example at least 4 hours, preferably at a temperature of 20°C to 30°C.

[0133] A polyester-polyurethane dispersion containing a (meth)acrylic monomer can be obtained by adding a solvent to the polyester-polyurethane before or after the addition of a (meth)acrylic monomer or a radical initiator. The solvent can be water or an organic solvent. Preferably, water is added to adjust the solids content and produce an aqueous polyester-polyurethane dispersion.

[0134] Suitable ethylenically unsaturated monomers are shown above. Preferably, monoethylenically unsaturated alkyl (meth)acrylate monomers, more preferably t-butyl acrylate, n-butyl acrylate, n-butyl methacrylate and ethylhexyl methacrylate, are polymerized in step (b).

[0135] To initiate radical polymerization, water-soluble or water-insoluble initiators can be used. Examples of water-soluble initiators include hydrogen peroxide, peroxydisulfates such as sodium, potassium, and ammonium peroxydisulfates, ammonium salts of 4,4'-azobis(4-cyanopentanoic acid), 2,2'-azobis(2-methyl-N-1,1-bis(hydroxymethyl)ethyl)propionamide, and 2,2'-azobis(2-methyl-N-(2-hydroxyethyl)propionamide). Preferably, ammonium peroxydisulfate (APS) is used as a water-soluble initiator.

[0136] Examples of water-insoluble initiators include tert.butyl-peroxy-2-ethylhexanol, tert.butyl-peroxypivalate, and dibenzoyl peroxide. Preferably, tert.butyl-peroxy-2-ethylhexanol is used as the water-insoluble initiator.

[0137] Preferably, radical polymerization is initiated by a water-insoluble initiator, more preferably by tert.butyl-peroxy-2-ethylhexanol.

[0138] Radical initiators generate radicals within the ethylenically unsaturated polyester-polyurethane polymer and / or within the ethylenically unsaturated monomer.

[0139] This yields a poly(meth)acrylate, which can be physically mixed with the polyester-polyurethane of step (a) or covalently bonded with the polyester-polyurethane of step (a). For example, the poly(meth)acrylate can be covalently bonded with the polyester-polyurethane of step (a) by forming a graft polymer by radical copolymerization of an ethylenically unsaturated monomer with an ethylenically unsaturated group in the backbone of the polyester-polyurethane of step (a), and / or by abstracting H on the backbone of the polyester-polyurethane of step (a).

[0140] Preferably, the solids content of the resulting polyester-polyurethane-poly(meth)acrylic hybrid dispersion is ≥40% by mass, more preferably ≥42% by mass, even more preferably ≥43% by mass, even more preferably ≥44% by mass, even more preferably ≥48% by mass, and most preferably ≥50% by mass, which is measured using a 1.0 g weighing unit at 130°C for 60 minutes according to DIN EN ISO3251.

[0141] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid has a glass transition temperature of -50°C to +50°C, more preferably -48°C to 40°C, even more preferably -45°C to 35°C, and most preferably -45°C to 30°C, which is measured according to DIN-EN-ISO11357-1 and -2.

[0142] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid prepared using one or more monoethylenically unsaturated monomers has a number average molecular weight (M) of 2,500 g / mol to 5,000 g / mol, more preferably 2,700 g / mol to 4,800 g / mol, and most preferably 3,000 g / mol to 4,500 g / mol. n ) is present, which is measured by gel permeation chromatography using a poly(meth)acrylate standard and a tetrahydrofuran / acetic acid mixture (1 mole of acetic acid per liter of tetrahydrofuran).

[0143] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid prepared using one or more monoethylenically unsaturated monomers has a mass-average molecular weight (M) of 25,000 g / mol to 550,000 g / mol, more preferably 30,000 g / mol to 500,000 g / mol, even more preferably 50,000 g / mol to 450,000 g / mol, and most preferably 100,000 g / mol to 400,000 g / mol. w) is present, which is measured by gel permeation chromatography using a poly(meth)acrylate standard and a tetrahydrofuran / acetic acid mixture (1 mole of acetic acid per liter of tetrahydrofuran).

[0144] The number average molecular weight (M) of a polyester-polyurethane-poly(meth)acrylic hybrid prepared using at least one polyethylene unsaturated monomer, preferably at least one diethylene unsaturated monomer. n ) and mass average molecular weight (M w ) is the number average molecular weight (M) as described in the two preceding paragraphs of this specification. n ) and mass average molecular weight (M w It can be even higher than that.

[0145] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid has an acid value of 5 mg KOH / g to 50 mg KOH / g, more preferably 10 mg KOH / g to 45 mg KOH / g, even more preferably 15 mg KOH / g to 40 mg KOH / g, even more preferably 15 mg KOH / g to 35 mg KOH / g, and most preferably 15 mg KOH / g to 30 mg KOH / g, which is measured according to DIN EN ISO 2114.

[0146] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid dispersion is heated for 1000 seconds at a temperature of 23°C using a Rheolab QC rotational rheometer equipped with cylinder cc27. -1 Using the shear rate, and measured according to DIN53019-1, it has a viscosity of 5 mPa*s to 3000 mPa*s, more preferably 10 mPa*s to 2500 mPa*s, even more preferably 10 mPa*s to 1000 mPa*s, even more preferably 10 mPa*s to 500 mPa*s, and even more preferably 10 mPa*s to 200 mPa*s.

[0147] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid dispersion has a particle size of 50 nm to 400 nm, more preferably 70 nm to 300 nm, even more preferably 100 nm to 250 nm, and most preferably 120 nm to 220 nm, which is measured by measuring the hydrodynamic volume / hydrodynamic radius of the dispersed particles using photon correlation spectroscopy (PCS).

[0148] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid dispersion contains 45-90% by mass of polyester-polyurethane from step (a) and 10-55% by mass of poly(meth)acrylate from step (b), more preferably 50-90% by mass of polyester-polyurethane from step (a) and 10-50% by mass of poly(meth)acrylate from step (b), even more preferably 55-90% by mass of polyester-polyurethane from step (a) and 10-45% by mass of poly(meth)acrylate from step (b), even more preferably 60-90% by mass of polyester-polyurethane from step (a) and 10-40% by mass of poly(meth)acrylate from step (b), most preferably 65-90% by mass of polyester-polyurethane from step (a) and 10-35% by mass of poly(meth)acrylate from step (b), where these mass percentages are relative to the solid content of the polyester-polyurethane-poly(meth)acrylic hybrid dispersion.

[0149] Method of using the polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention is suitable for several applications. In particular, the polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention can be used in many fields of coatings, especially in automotive coatings.

[0150] In particular, the polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention can be used in base coat compositions or filler coating compositions, more preferably in base coat compositions or filler coating compositions in automotive coatings. A coating composition containing the polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention can be used to form a base coat layer on an untreated or pretreated substrate. Furthermore, a coating composition containing the polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention can be used to form a second base coat layer on a first base coat layer.

[0151] Coating composition comprising polyester-polyurethane-poly(meth)acrylic hybrid dispersion of the present invention Another object of the present invention is a coating composition comprising a polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention.

[0152] The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention can be used as a binder in any coating composition, particularly in a base coat composition.

[0153] The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention can be used in any liquid coating composition, preferably an aqueous coating composition, which may be aqueous or solvent-based.

[0154] The coating composition comprising the polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention can be used to form one or more layers in multilayer coatings, preferably on untreated or pretreated substrates, particularly on the body of an automobile or its parts.

[0155] The coating composition is preferably thermosetting. In addition to the polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention, the thermosetting coating composition includes further materials, such as one or more further binders (A1) and / or one or more commonly used coating additives (A2) and / or one or more pigments and / or fillers (A3) and / or one or more solvents (A4), as additional components (A).

[0156] Further binders (A1) In addition to the polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention, further polymers selected from the group consisting of polyurethane, polyurea, polyester, polyamide, poly(meth)acrylate and / or copolymers of the structural units of the said polymers can be used as binders. The term "poly(meth)acrylate" refers not only to polyacrylate but also to polymethacrylate, and even polymers containing both methacrylate and / or methacrylic acid and / or acrylate and / or acrylic acid.

[0157] Preferred polyurethanes are described, for example, in German Patent Application DE19948004A1, pp. 4, line 19 to pp. 11, line 29 (Polyurethane Prepolymer B1), European Patent Application EP0228003A1, pp. 3, line 24 to pp. 5, line 40, European Patent Application EP0634431A1, pp. 3, line 38 to pp. 8, line 9, and International Patent Application WO92 / 15405, pp. 2, line 35 to pp. 10, line 32.

[0158] Preferred polyesters are described, for example, in DE4009858A1, columns 6, line 53 to 7, line 61 and 10, line 24 to 13, line 3 and Example D, or in WO2014 / 033135A2, pages 2, line 24 to 7, line 10 and 28, line 13 to 29, line 13. Similarly, polyesters may have a dendritic structure, as described, for example, in WO2008 / 148555A1.

[0159] Preferred polyurethane-poly(meth)acrylate copolymers (e.g., (meth)acrylic polyurethanes) and their preparations are described, for example, in WO91 / 15528A1, page 3, line 21 to page 20, line 33, and DE4437535A1, page 2, line 27 to page 6, line 22.

[0160] Preferred poly(meth)acrylates can be prepared by multi-step free-radical emulsion polymerization of olefinic unsaturated monomers in water and / or organic solvents. Seed-core-shell polymers (SCS polymers) are particularly preferred, for example. Such polymers or aqueous dispersions containing such polymers are known, for example, from WO2016 / 116299A1.

[0161] Preferred polyurethane-polyurea copolymers are polyurethane-polyurea particles, preferably having an average particle size of 40 to 2000 nm, where each reacted form of polyurethane-polyurea particles contains at least one isocyanate group-containing polyurethane prepolymer containing an anionic group and / or a group that can be converted to an anionic group, and at least one polyamine containing two primary amino groups and one or two secondary amino groups. Preferably, such copolymers are used in the form of aqueous dispersions. Such polymers can, in principle, be prepared, for example, by the conventional polyaddition of polyisocyanates with polyols and polyamines.

[0162] To crosslink the polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention, at least one further binder is included in the coating composition containing the polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention. Suitable crosslinking binders are amino resins, such as urea-formaldehyde resins or melamine-formaldehyde resins, or isocyanate-terminated polyurethanes having free or blocked isocyanate groups, or isocyanates that can be converted to free or blocked isocyanates. A blocked isocyanate refers to a reaction product of an isocyanate in which the isocyanate functional group reacts with a "blocking agent". Blocking of the isocyanate occurs by the reaction of the isocyanate with a compound containing active hydrogen. Suitable blocking agents are oximes, lactams, phenols, activated methylene, pyrazoles, mercaptans, imidazoles, amines, imines, triazoles, hydroxylamines, and derivatives from aliphatic or alicyclic alkyl monoalcohols. The blocked isocyanate component does not react at room temperature. The crosslinking reaction between blocked isocyanates and hydroxy-functional compounds is achieved at high temperatures.

[0163] Additives are binders, typically used in minimal amounts to impart specific properties to a coating composition.

[0164] Coating additive (A2) The coating composition may contain at least one additive selected from the group consisting of reactive diluents, light stabilizers, antioxidants, defoamers, emulsifiers, surfactants, slip additives, polymerization inhibitors, free radical polymerization initiators, catalysts, adhesion promoters, film-forming aids, wetting agents, dispersants, leveling agents, rheology regulators, sagging regulators (SCAs), flame retardants, corrosion inhibitors, drying agents, biocides, matting agents, and dyes (colorants that are soluble in the coating composition). Further examples of suitable coating additives are described, for example, in the textbook "Lackadditive" ("Additives for Coatings" by Johan Bieleman, Wiley-VCH, Weinheim, 1998). Additives may be used in known and conventional amounts.

[0165] Preferred coating additives are rheology control agents, wetting agents, or leveling agents.

[0166] Pigments and fillers (A3) The coating composition according to the present invention may contain a pigment, especially if the coating composition is a base coat composition or a filler composition. The terms "coloring pigment" and "color pigment" are interchangeable and include colored pigments, black pigments, and white pigments. Inorganic pigments and organic pigments can be used as color pigments.

[0167] Examples of white pigments include titanium dioxide, zinc white, zinc sulfide, and lithopone. Examples of black pigments include carbon black, iron-manganese black, and spinel black. Examples of other colored pigments include chromium oxide, chromium oxide hydrate green, cobalt green, ultramarine green, cobalt blue, ultramarine blue, manganese blue, ultramarine violet, cobalt and manganese violet, iron oxide red, cadmium sulfoselenide, molybdate red, and ultramarine red, iron oxide brown, mixed brown, spinel and corundum phases, and chromium orange, iron oxide yellow, nickel titanium yellow, chromium titanium yellow, cadmium sulfide, cadmium zinc sulfide, chromium yellow, and bismuth vanadate.

[0168] Possible organic pigments include azo pigments, polycyclic pigments, and anthraquinone pigments.

[0169] The term "filler" is known to those skilled in the art, for example, from DIN 55943 (dated October 2001). Examples of suitable fillers include kaolin, dolomite, calcite, chalk, calcium sulfate, barium sulfate, talc, silica, especially pyrogenated silica, and hydroxides, such as aluminum hydroxide or magnesium hydroxide. See also Roempp Lexikon Lacke und Druckfarben, Georg Thieme Verlag, 1998, pp. 250 onwards, for more information on "fillers".

[0170] Solvent (A4) In particular, the coating composition may contain a solvent. The solvent can be water or an organic solvent. Preferably, water is used as the solvent. Suitable examples of organic solvents include heterocyclic, aliphatic or aromatic hydrocarbons, monofunctional or polyfunctional alcohols, ethers, esters, ketones and amides, such as N-methylpyrrolidone, N-ethylpyrrolidone, dimethylformamide, toluene, xylene, butanol, ethyl glycol and butyl glycol and their acetates, butyl diglycol, diethylene glycol dimethyl ether, cyclohexanone, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), acetone, isophorone, or mixtures thereof. Organic solvents can be used in combination with water and in combination with water in aqueous coating compositions.

[0171] The content of the polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention in the total coating composition is preferably 2% to 30% by mass, more preferably 5% to 25% by mass, and most preferably 7% to 20% by mass.

[0172] A coating layer formed from a coating composition containing a polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention, and a substrate coated in the same manner. The coating composition for forming the coating layer is applied to the substrate by conventional painting methods well known to those skilled in the art. The substrate material is selected from the group consisting of metals, polymers, wood, glass, mineral-based materials, and any composite materials of the aforementioned materials. Untreated or pretreated substrates can be used, and the pretreatment usually depends on the chemical properties of the substrate.

[0173] The coating composition comprising the polyester-polyurethane-poly(meth)acrylate hybrid dispersion according to the present invention is preferably applied by spraying, pneumatic pressure, and / or electrostatic discharge. The coating composition is thermosetting at high temperatures, preferably between 60°C and 180°C, and most preferably between 80°C and 160°C, depending on the reactivity of the crosslinking agent and the duration.

[0174] The present invention further provides a substrate coated with a coating layer formed from a coating composition comprising a polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention.

[0175] Multilayer coating and multilayer coated substrates Another object of the present invention is a method for manufacturing a multilayer coating, comprising the following steps: a) A step of applying one or more base coat compositions to form one or more base coat layers on a substrate, wherein at least one base coat composition comprises the polyester-polyurethane-poly(meth)acrylic hybrid dispersion of the present invention, b) A step of applying a clear coat composition onto one or more base coat layers to form a clear coat layer, c) A process in which one or more base coat layers and a clear coat layer are cured simultaneously, or one or more layers obtained in steps (a) and (b) are cured individually and then a subsequent coating layer is applied, or all layers obtained in steps (a) and (b) are cured individually. This method includes [something].

[0176] The multilayer coated substrate can be a pre-treated or untreated substrate, which may be uncoated or pre-coated. Each coating layer is applied by conventional coating methods well known to those skilled in the art. The coating composition is preferably applied by spraying, pneumatic and / or electrostatic, and at least one coating composition may be a base coat composition or a filler coating composition comprising the polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention.

[0177] The application of the base coat composition onto the substrate to form the base coat layer and the application of the clear coat composition onto the base coat layer(s) are preferably carried out by wet-on-wet application, i.e., application while the preceding layer is not cured or not completely cured before the application of the next coating composition. Therefore, before the application of the clear coat composition, the base coat composition may be flashed off at room temperature (25°C) and / or, instead, dried at a high temperature.

[0178] The coating composition is thermosetting at high temperatures, preferably between 60°C and 180°C, and most preferably between 80°C and 160°C, depending on the reactivity of the crosslinking agent and the curing period. The coating composition is preferably cured for 15 to 50 minutes, most preferably for 20 to 40 minutes.

[0179] Furthermore, the present invention provides a substrate coated with the multilayer coating of the present invention. The substrate is selected from the group consisting of metals, polymers, wood, glass, mineral-based materials, and any composite materials of the aforementioned materials. Untreated or pretreated substrates can be used, and the pretreatment usually depends on the chemical properties of the substrate. Pretreatment of a metal substrate is, for example, a zinc phosphate treatment step.

[0180] The multilayer coating of the present invention, including the coating composition according to the present invention, exhibited excellent appearance in terms of low long-wavelength values. This was achieved using a polyester-polyurethane-poly(meth)acrylic hybrid dispersion having a high solids content, which was surprising because dispersions with such high solids content usually undergo solidification. Furthermore, if at least one of the base coat compositions contains the polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention, good compatibility of the base coat compositions is achieved. [Examples]

[0181] method solids content Unless otherwise stated, the solids content was measured according to DIN EN ISO 3251, using a 1.0 g weighing unit at 130°C for 60 minutes.

[0182] Isocyanate content The isocyanate content (NCO content) was measured by adding an excess of 2% N,N-dibutylamine solution in xylene to a homogeneous solution of the sample in acetone / N-ethylpyrrolidone (1:1 vol%), and then potentiometric back titrating the excess amine with 0.1N hydrochloric acid according to DIN EN ISO 3251, DIN EN ISO 11909, and DIN EN ISO 14886. The polymer content in the solution (solids content) is used to refer to the NCO content of the polymer relative to the solids content.

[0183] Hydroxyl value The hydroxyl value was measured at room temperature using acetic anhydride in a tetrahydrofuran (THF) / dimethylformamide (DMF) solution in the presence of 4-dimethylaminopyridine as a catalyst, according to R.-P. Krueger, R. Gnauck, and R. Algeier (Plaste und Kautschuk, 20, 274 (1982)). The excess acetic anhydride remaining after acetylation was completely hydrolyzed, and the acetic acid was back titrated potentiometrically with an alcoholic potassium hydroxide solution.

[0184] Acid value The acid value was measured according to DIN EN ISO 2114 using a homogeneous solution of tetrahydrofuran (THF) / water (9 parts by volume of THF and 1 part by volume of distilled water) with an ethanolic potassium hydroxide solution.

[0185] Number-average molecular weight and mass-average molecular weight Number average molecular weight (M n ) and mass average molecular weight (M w The values ​​were measured by gel permeation chromatography using poly(meth)acrylate standards and a tetrahydrofuran / acetic acid mixture (1 mole of acetic acid per liter of tetrahydrofuran).

[0186] Average particle size In this application, the average particle size (z-mean) of the polyester-polyurethane-poly(meth)acrylic hybrid dispersion was measured by measuring the hydrodynamic volume / hydrodynamic radius of the dispersion particles using photon correlation spectroscopy (PCS).

[0187] A Malvern Nano S90 (Malvern Instruments) was used for the measurements at 25±1℃. This instrument covered a size range of 3nm to 3000nm and was equipped with a 633nm 4mW He-Ne laser. A polyester-polyurethane-poly(meth)acrylic hybrid dispersion was diluted with deionized water free of particles as the dispersion medium, and the polymer hybrid dispersion in 1 ml of polystyrene cuvette was measured at a suitable scattering intensity. The measurement was performed five times, and the second measurement was repeated using a freshly prepared sample. The average particle size (z-mean) described is the arithmetic mean of the average particle size (intensity-weighted) of each preparation. For validation, polystyrene standards with certified particle sizes of 50 to 3000nm were used.

[0188] viscosity The viscosity of the polyester-polyurethane during synthesis was measured using a CAP2000H viscometer with a 03 spindle at a temperature of 140°C for 1250 seconds. -1 ~2500s -1The shear rate was used and measured according to DIN EN ISO2884-1.

[0189] The viscosity of the final polyester-polyurethane dispersion and the final polyester-polyurethane-poly(meth)acrylic hybrid dispersion was measured using a Rheolab QC rotational rheometer with a cc27 cylinder at a temperature of 23°C for 1000 seconds. -1 The shear rate was used and measured according to DIN53019-1.

[0190] glass transition temperature The glass transition temperature was measured according to DIN-EN-ISO11357-1 and -2. The liquid dispersion was applied to a glass substrate by drawdown (50 μm) and dried at 130°C for 60 minutes. A predetermined atmosphere was obtained using nitrogen gas. The dried sample was placed in a crucible. When the starting temperature reached -90°C, the temperature was raised at 10 K / min to a selected limit, and then cooled at the same rate to a selected limit (-90°C to 100°C). A second measurement was then performed at the same temperature limit, and the glass transition temperature was measured during the heating step of the second measurement.

[0191] Appearance evaluation The appearance of the coated substrate was evaluated using a wave scan measurement system from Byk / Gardner. A laser beam was shone at a 60° angle onto the surface of a substrate coated with a multilayer coating, and the reflected light in the short wavelength range (0.3~1.2 mm) and the long wavelength range (1.2~12 mm) was measured. Smaller values ​​for both the short wavelength (LW) and long wavelength (LW) indicate a better appearance. Furthermore, the clarity of the image reflected from the surface of the multilayer structure was measured using a wave scan measurement device. This parameter is called "Image Clarity" (DOI), and a higher value indicates a better appearance.

[0192] All quantities listed are in parts by mass or grams, and percentages are by mass unless otherwise specified.

[0193] Comparative example: Synthesis of polyester-polyurethane-poly(meth)acrylic hybrid dispersions C1-C3 Preparation of carboxyl-rich polyurethane and polyester is described in Example 3 of US10,233,353B2 (COOH-rich polyurethane: 23.3 g dimethylolpropionic acid, 53.4 g H 12 The synthesis was carried out according to MDI, 23.3 g of 12-hydroxystearic acid (acid value 141 mg KOH / g) and Example 4 (polyester: 375 g of 1,6-hexanediol, 118 g of trimethylolpropane, 389 g of isophthalic acid, 118 g of adipic acid (acid value 10 mg KOH / g)). The synthesis of the polyester-polyurethane dispersion was carried out similarly to Example 5 of US10,233,353B2, using comparative examples polyester-polyurethane-poly(meth)acrylic hybrid dispersions C1 and C3 as the basis. Comparative example dispersion C1 is a reproduction of Example 6 of the aforementioned patent. The amounts in Table 1 are shown in grams.

[0194] [Table 1]

[0195] As shown in Table 1, polymerization at a solids content of 42% by mass caused coagulation, and a polyester-polyurethane-poly(meth)acrylic hybrid dispersion could not be obtained.

[0196] Synthesis of the polyester-polyurethane-poly(meth)acrylic hybrid dispersion of the present invention Synthesis of polyester PE1 and PE2 The compounds listed in Table 2 were mixed in a reactor equipped with a stirrer and a Dean-Stark apparatus. The temperature was raised to 220°C and carefully controlled to minimize monomer loss. Reaction monitoring was performed by titration. Polyester PE2 with the indicated properties was obtained. The condensation process of PE1 was carried out until the acid value reached less than 10 mg KOH / g. After cooling, polyester PE1 was prepared with methyl ethyl ketone (MEK) to obtain a solids content of 74% by mass.

[0197] [Table 2]

[0198] Polyurethane PU1-PU7 synthesis The compounds listed in Table 3 were reacted in an N2 purge reactor equipped with a stirrer and reflux condenser to obtain polyurethanes PU1 to PU7 having the characteristics shown.

[0199] Dimethylolpropionic acid (DMPA), isophorone diisocyanate (IPDI), and methyl ethyl ketone (MEK) were mixed for the synthesis of PU1, and the temperature was carefully raised to 77°C. The reaction was monitored by titration. After the theoretical NCO content reached 14.9%, the mixture was cooled and ethylene glycol was added. The temperature was maintained at 77°C until complete conversion of the NCO group was detected by titration. Then, trimellitic anhydride was added, and the reaction was stopped at a certain acid value.

[0200] Dimethylolpropionic acid, methyl ethyl ketone, ethylene glycol, and 4,4'-methylenebis(cyclohexyl isocyanate) were mixed for the synthesis of PU2, and the temperature was maintained at 77°C after the exothermic reaction. The reaction was monitored by titration. After complete conversion of the NCO group was achieved, MEK was added to adjust the solid content to 60% by mass. Subsequently, trimellitic anhydride was added, and the reaction was stopped at a certain acid value.

[0201] PU1 and PU2 were diluted with MEK to a solid content of approximately 70% by mass. PU3, PU4, and PU7 were synthesized in a similar manner to PU1. Following the preparation of PU2, PU5 and PU6 were obtained and diluted to a solid content of 55% or 57%, respectively.

[0202] [Table 3]

[0203] Synthesis of polyester-polyurethane dispersions PEUD1, PEUD2, PEUD4 and polyester-polyurethane PEU3 Synthesis of polyester-polyurethane dispersion PEUD1 To prepare polyester-polyurethane dispersion 1, 7814.0 g of PE1 and 2218.0 g of PU2 were mixed in a reactor equipped with a stirrer. The temperature was carefully raised to a maximum of 160°C while applying reduced pressure (20 mbar). The process was monitored by titration and viscosity measurement at 140°C. The acid value was 29 mg KOH / g and the viscosity was approximately 1800 mPa*s (CAP2000H, spindle 03, 140°C, shear rate 1250 s). -1 After reaching ), the temperature was lowered to 115°C, and 160g of dimethylethanolamine was added over 10 minutes. Water was added at 90°C to adjust the solid content of PEUD1 to 55% by mass. Further properties are shown in Table 4.

[0204] Synthesis of polyester-polyurethane dispersion PEUD2 To prepare polyester-polyurethane dispersion 2, 1084.0 g of PE2 and 415.8 g of PU2 were mixed in a reactor equipped with a stirrer. The temperature was carefully raised to a maximum of 140°C under reduced pressure (40-60 mbar). The process was monitored by titration and viscosity measurement at 140°C. Acid value of 32 mg KOH / g and viscosity of approximately 1400 mPa*s (CAP2000H, spindle 03, 140°C, shear rate 2500 s) were obtained. -1 After reaching ), the temperature was lowered to 80°C, and 46.0 g of dimethylethanolamine was added over 10 minutes. Water was added at 80°C to adjust the solid content of PEUD2 to 45% by mass.

[0205] The characteristics of PEUD1 and PEUD2 are shown in Table 4.

[0206] [Table 4]

[0207] 1 Viscosity was measured using a Rheolab QC rotational rheometer with a cc27 cylinder at a temperature of 23°C for 1000 seconds. -1 The measurement was performed using the shear rate.

[0208] Polyester polyurethane PEU3 synthesis To prepare polyester-polyurethane 3, 2441.8 g of PE1 and 693.1 g of PU2 were mixed in a reactor equipped with a stirrer. The temperature was carefully raised to a maximum of 140°C while applying reduced pressure (50-120 mbar). The process was monitored by titration and viscosity measurement at 140°C. Acid value of 26 mg KOH / g and viscosity of approximately 2000 mPa*s (CAP2000H, spindle 03, 140°C, shear rate 1250 s) -1 After reaching 0°C, the temperature was lowered to 82°C, and 203.0 g of n-butyl acrylate was added. A polyester-polyurethane 3 with a solid content of approximately 90% by mass was obtained.

[0209] Synthesis of polyester-polyurethane dispersion PEUD4 To prepare polyester-polyurethane dispersion 4, 2168.3 g of PE1 and 831.7 g of PU2 were mixed in a reactor equipped with a stirrer. The temperature was carefully raised to a maximum of 140°C while applying reduced pressure (50-120 mbar). The process was monitored by titration and viscosity measurement at 140°C. Acid value of 28 mg KOH / g and viscosity of approximately 1800 mPa*s (CAP2000H, spindle 03, 140°C, shear rate 1250 s) -1 After reaching 0°C, the temperature was lowered to 100°C and 187.3 g of butyl diglycol was added. 60.0 g of dimethylethanolamine was added over 10 minutes. Then, 1925.0 g of water was slowly added at 95°C. A polyester-polyurethane dispersion 4 with a solids content of 48.2% by mass was obtained.

[0210] Synthesis of polyester-polyurethane-poly(meth)acrylic hybrid dispersions B1-B17 of the present invention by emulsion polymerization Examples B1-B11 The synthesis was carried out in a 3.5 L steel reactor using an anchor stirrer for B1-B11. The stirrer was set to a low setting (50-100 rpm). For Examples B9 and B10, a glass reactor with a 150 rpm stirrer was used. Heat transfer oil was used to control the reactor temperature. Undiluted PEUD1 was used for the synthesis of B1-B3, B5, B7 and B10, and undiluted PEUD2 was used for the synthesis of B9. For the synthesis of B4 and B6, PEUD1 was diluted with 569 g of deionized water. For the synthesis of B8, PEUD1 was neutralized with 17.2 g of dimethylethanolamine (DMEA), diluted with 26.9 g of butyl diglycol and 792.2 g of deionized water to obtain a dispersion with a solid content of 40% by mass and a degree of neutralization of approximately 70%. Undiluted or diluted PEUD1 or PEUD2 was heated to 80°C. The amounts in Table 5 are shown in grams.

[0211] In Examples B1 to B7, a (meth)acrylic monomer or monomer was mixed with 2 g of tert-butyl-peroxy-2-ethylhexanol. Each mixture was slowly added over 3 hours at 80°C. Then, 0.4 g of tert-butyl-peroxy-2-ethylhexanol was added and the mixture was stirred for a further 2 hours at 80°C.

[0212] In Example B8, (meth)acrylic monomer and 2.4 g of tert-butyl-peroxy-2-ethylhexanol were slowly added over 2.5 hours at 80°C. Then, 0.4 g of tert-butyl-peroxy-2-ethylhexanol was added and the mixture was stirred for a further 2 hours at 80°C.

[0213] In Example B9, (meth)acrylic monomer was mixed with 0.3 g of tert-butyl-peroxy-2-ethylhexanol. Each mixture was slowly added over 3 hours at 80°C. The mixture was then stirred for a further 2 hours at 80°C.

[0214] In Example B10, (meth)acrylic monomer was mixed with 0.2 g of tert-butyl-peroxy-2-ethylhexanol. Each mixture was slowly added over 3 hours at 80°C. The mixture was then stirred at 80°C for 1 hour. Next, 0.1 g of tert-butyl-peroxy-2-ethylhexanol was added, and the mixture was stirred for another hour at 80°C.

[0215] For the synthesis of B11, PEUD1 was diluted with 79.9 g of butyl diglycol and 257.8 g of deionized water. Then, (meth)acrylic monomer and 1.3 g of tert-butylperoxy-2-ethylhexanol were slowly added over 3 hours at 80°C. The dispersion was then stirred at 80°C for a further 2 hours.

[0216] After the reaction, during the cooling period, dispersions B1-B3, B5, and B10 were diluted with 230 g (B1, B2), 105 g (B3, B5), or 21 g (B10) of deionized water. Dispersions B4, B6-B9, and B11 were not further diluted.

[0217] [Table 5]

[0218] The properties of dispersions B1 to B11 are shown in Table 6.

[0219] [Table 6]

[0220] Examples B12-B14 The same apparatus as in Examples B1-B6 and B8 was used for the synthesis of dispersions B12-B14. The stirring speed was set to 150 rpm. According to Table 7, 509.7 g of polyester-polyurethane 3 was diluted with 62.9 g of (meth)acrylate, and then 13.5 g of dimethylethanolamine was added. Over 15 minutes, 463.4 g of water was added at 80°C to obtain a monomer-swollen polyester-polyurethane dispersion with a theoretical solids content of approximately 43.7% by mass. Subsequently, 0.6 g of tert-butylperoxy-2-ethylhexanol was added over 2 hours, and the temperature was maintained at 80°C for 2 hours. A further 0.3 g of tert-butylperoxy-2-ethylhexanol was added, and stirring was continued for 1 hour.

[0221] Example B15 The same apparatus as in Examples B1-B6 and B8 was used for the synthesis of dispersion B15. The stirring speed was set to 150 rpm. 1456.0 g of polyester-polyurethane 3 was diluted at 110°C with 316.0 g of t-butyl acrylate, 197.5 g of styrene, and 323.9 g of n-butyl acrylate. The temperature was lowered to 95°C, and 220.0 g of butyl diglycol was added, followed by 63.2 g of dimethylethanolamine. After 10 minutes, 3100.0 g of water was added at 80°C to obtain a monomer-swollen polyester-polyurethane dispersion with a theoretical solids content of approximately 23.1% by mass. 2500.0 g of this monomer-swollen polyester-polyurethane dispersion was heated to 80°C, and 8.2 g of tert-butyl-peroxy-2-ethylhexanol was added over 2.5 hours, maintaining the reaction temperature at 80°C for a further 2 hours. 2.0 g of tert-butyl-peroxy-2-ethylhexanol was added, and stirring was continued for 1 hour.

[0222] Examples B16 and B17 The same apparatus used in Examples B1-B6 and B8 was used for the synthesis of dispersions B16 and B17. The stirring speed was set to 150 rpm. According to Table 7, 1065.1 g of PEUD4 was diluted with 185.7 g of water and heated to 80°C. 127.3 g of n-butyl acrylate, 73.5 g of t-butyl acrylate, and 46.0 g of styrene were added over 3 hours. In parallel with the monomer addition, 2.4 g of tert-butyl-peroxy-2-ethylhexanol (B16) or a mixture of 52.5 g of water and 4.8 g of ammonium peroxydisulfate (B17) was added to the reactor. For the synthesis of dispersion B16, 1.0 g of tert-butyl-peroxy-2-ethylhexanol was used, and the reaction was carried out for a further 2 hours while maintaining the reaction temperature at 80°C.

[0223] [Table 7]

[0224] The acid values ​​of dispersions B12 to B17 are shown in Table 8.

[0225] [Table 8]

[0226] As is clear from Tables 5 and 7, the polyester-polyurethane-poly(meth)acrylic hybrid dispersion of the present invention exhibited a solids content much higher than 40% by mass, and no coagulation was observed. In the comparative example polyester-polyurethane-poly(meth)acrylic hybrid dispersion C3, coagulation already occurred at a solids content of 42% by mass, but the polyester-polyurethane-poly(meth)acrylic hybrid dispersion did not coagulate even at a high solids content of approximately 60% by mass (B3), which was surprising.

[0227] Preparation of a base coat composition comprising polyester-polyurethane-poly(meth)acrylic hybrid dispersions B1-B6 and B11 of the present invention. Preparation of milling base MB1 A milling base was prepared using 19.1 parts by mass of deionized water, 0.9 parts by mass of a 10% dimethylethanolamine solution, 8.3 parts by mass of a water-based polyester having a solid content of 60.0 ± 1.0% by mass (measured at 130°C for 1 hour) and an acid value of 29-34 mg KOH / g solids, 15 parts by mass of titanium dioxide, 0.5 parts by mass of 2-ethylhexanol, 34.4 parts by mass of barium sulfate, 1.8 parts by mass of an additive, 2.6 parts by mass of carbon black, and 17.4 parts by mass of a polyurethane dispersion having a solid content of 33.0 ± 1.0% by mass (measured at 130°C for 1 hour) and an acid value of 19-23 mg KOH / g solids.

[0228] Preparation of base coat composition The base coat compositions were prepared by mixing the components listed in Table 9. The base coat compositions BC-I1 to BC-I7 of the present invention contained the polyester-polyurethane-poly(meth)acrylic hybrid dispersions B1 to B6 and B11 of the present invention, while the comparative base coat compositions BC-C1, BC-C2, and BC-C3 contained the comparative aliphatic polycarbonate ester polyether polyurethane dispersion (Impranil® DLU) (BC-C1), the polyurethane dispersion PEUD-1 (BC-C2), which is an intermediate product with added ethylenically unsaturated monomers and not polymerized, or the comparative polyester-polyurethane-poly(meth)acrylic hybrid dispersion C2 (see Table 1) (BC-C3), which was prepared similarly to Example 5 of US10,233,353B2. Typical polyurethane, polyester, and polyacrylate dispersions were used as the main resins in all base coat compositions. Since the base coat compositions were one-component compositions, a melamine-formaldehyde crosslinking agent was used as a typical crosslinking agent for such compositions. The base coat composition of the present invention or a comparative example was prepared with water to obtain a base coat composition with a solid content of 27.5%.

[0229] [Table 9]

[0230] 1Polyurethane dispersion: Solids content: 32-34%; Acid value: 19-23 mgKOH / g solids; Hydroxyl value: 17 mgKOH / g solids. The polyurethane dispersion is known from WO2016000947A1. 2 Polyester aqueous solution: Solid content: 60±1.0% (measured at 130°C for 1 hour); Acid value: 29~34 mgKOH / g solids. Polyester aqueous solutions are known from DE4009858 and Example D. 3 Polyacrylate dispersion: Solids content: 25.5-27.5%, Acid value: 16.6-17.6 mgKOH / g solids, Hydroxyl value: 16.5-17.5 mgKOH / g solids. The polyacrylate dispersion is known from WO2017148796A1. 4 Applicable viscosity: 85±25mPa*s (RheolabQC, cc27, shear rate 1000s -1 (Use) Preparation of base coat composition 2 (BC2) The BC2 formulation consists of 26.5 parts by mass of deionized water, 3.1 parts by mass of 10% dimethylethanolamine solution, 4.5 parts by mass of water-based polyester having a solid content of 60.0 ± 1.0% by mass (measured at 130°C for 1 hour) and an acid value of 29-34 mg KOH / g solids, 6.8 parts by mass of rheological agent, 2.0 parts by mass of 2-ethylhexanol, 9.2 parts by mass of butoxypropanol, 1.0 part by mass of dipropylene glycol methyl ether, 4.1 parts by mass of additives, 14.0 parts by mass of carbon black, and 7.5 parts by mass of melamine resin, with a solid content of 35.5 ± 1.0% by mass. The preparation involved a first polyurethane polyacrylate dispersion having an acid value of 32-35 mgKOH / g solids (measured at 130°C for 1 hour), a second polyurethane polyacrylate dispersion having a solids content of 36.0±1.0% by mass (measured at 130°C for 1 hour), a third polyurethane polyacrylate dispersion having a solids content of 44.0±1.0% by mass (measured at 130°C for 1 hour) and an acid value of 30-32 mgKOH / g solids, and 3.0 parts by mass of OH-functional aqueous polyacrylate having a solids content of 46.5±1.0% by mass (measured at 130°C for 1 hour).

[0231] Application of coating composition The spray booth was maintained at 25°C and 70% humidity. Base coats BC-C1 to BC-C3 and BC-I1 to BC-I7 were applied to panels with an electron immersion coating (BASF Coatings GmbH, Cathoguard) by electrostatic spray coating (ESTA) to a thickness of approximately 25 μm. After a flash-off time of 3.5 minutes at 80°C, base coat BC2 was applied to a thickness of approximately 12 μm (BC-C1, BC-C2, and BC-I1 to BC-I6) or approximately 24 μm (BC-C3 and BC-I7). After a flash-off time of 3.5 minutes at 80°C, a clear coat (BASF Coatings GmbH, UniGloss) was applied to a thickness of approximately 40 μm. The coating was then cured at 140°C for 30 minutes.

[0232] Testing of the coating layer The obtained multilayer coatings were evaluated according to DIN EN ISO 2813 using an orange peel meter (BYK 4840 wave scan dual, BYK-Gardner GmbH) for appearance in terms of long wavelength (LW) and short wavelength (SW), and gloss in terms of DOI (image clarity).

[0233] [Table 10]

[0234] Multilayer coatings containing a polyester-polyurethane-poly(meth)acrylic hybrid dispersion as base coat 1 exhibit superior appearance in terms of low long-wavelength values, which is lower compared to conventional multilayer coatings containing a base coat 1 containing an aliphatic polycarbonate ester polyether polyurethane dispersion (Impranil® DLU). Comparison with multilayer coatings containing PEUD-1 as base coat 1 demonstrates that the presence of PEUD-1 in dispersions B1-B7 of the present invention allows for further emulsion polymerization with acrylate monomers to improve the appearance of the multilayer coating. It was surprising that emulsion polymerization of polyester-polyurethane using ethylenically unsaturated monomers as described above improved the appearance in terms of low long-wavelength values. Furthermore, multilayer coatings containing a polyester-polyurethane-poly(meth)acrylic hybrid dispersion as base coat 1 exhibit superior appearance in terms of low long-wavelength values, combined with low short-wavelength values ​​and high DOI values.

[0235] Furthermore, the compatibility of the base coat composition containing the polyester-polyurethane-poly(meth)acrylic hybrid dispersion of the present invention with respect to the second base coat composition was improved compared to the base coat composition of the comparative example.

Claims

1. A polyester-polyurethane-poly(meth)acrylic hybrid dispersion, comprising the following steps: (a) A polyurethane containing at least one carboxyl group, having an acid value of 205 mg KOH / g to 400 mg KOH / g and at least one terminal carboxyl group, A step of obtaining polyester-polyurethane by esterifying a polyester containing at least one hydroxyl group having a hydroxyl value of 50 mg KOH / g to 300 mg KOH / g, and the following (b) A step of polymerizing an ethylenically unsaturated monomer containing at least a (meth)acrylic monomer by radical polymerization in the presence of the polyester-polyurethane of step (a). It can be obtained by One or more solvents are present and / or used between steps (a) and / or (b), and / or added after step (b), and A polyester-polyurethane-poly(meth)acrylic hybrid dispersion in which the solids content of the polyester-polyurethane dispersion obtained in step (a) is ≥ 40% by mass.

2. The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to claim 1, characterized in that the at least one polyurethane in step (a) has at least two carboxyl groups at each of its ends, and / or the at least one polyurethane and the at least one polyester in step (a) are esterified in the presence of one or more solvents to obtain a polyester-polyurethane dispersion.

3. The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to claim 1 or 2, characterized in that the polyester-polyurethane obtained in step (a) has an acid value in the range of 10 to 50 mg KOH / g solids.

4. The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to claim 1 or 2, characterized in that the polyester-polyurethane dispersion obtained in step (a) is aqueous.

5. The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to claim 1 or 2, characterized in that the ethylenically unsaturated monomer in step (b) is added to the polyester-polyurethane in step (a) before or simultaneously with the addition of the radical initiator.

6. The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to claim 1 or 2, characterized in that the radical polymerization of the ethylenically unsaturated monomer in step (b) is initiated by a water-soluble initiator or a water-insoluble initiator.

7. The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to claim 1 or 2, characterized in that the (meth)acrylic monomer in step (b) comprises an alkyl (meth)acrylate monomer.

8. The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to claim 1 or 2, characterized in that the polyester-polyurethane-poly(meth)acrylic hybrid has a glass transition temperature of -50°C to +50°C.

9. The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to claim 1 or 2, characterized in that the solid content of the polyester-polyurethane-poly(meth)acrylic hybrid dispersion is ≥ 40% by mass.

10. The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to claim 1 or 2, wherein the polyester-polyurethane-poly(meth)acrylic hybrid dispersion comprises 45 to 90% by mass of polyester-polyurethane and 10 to 55% by mass of poly(meth)acrylic, and these mass percentages are relative to the solid content of the polyester-polyurethane-poly(meth)acrylic hybrid.

11. A polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to claim 1 or 2, wherein the polyester-polyurethane of step (a) is physically mixed with the poly(meth)acrylate of step (b), and / or covalently bonded with the poly(meth)acrylate of step (b).

12. The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to claim 1 or 2, wherein the polyester-polyurethane-poly(meth)acrylic hybrid prepared using one or more monoethylenically unsaturated monomers has a number-average molecular weight (Mn) of 2,500 g / mol to 5,000 g / mol and / or a mass-average molecular weight (Mw) of 25,000 g / mol to 550,000 g / mol.

13. The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to claim 1 or 2, wherein the carboxyl group-containing polyurethane has an acid value of more than 210 mg KOH / g to 400 mg KOH / g.

14. A method for producing a polyester-polyurethane-poly(meth)acrylic hybrid dispersion as defined in claim 1 or 2, comprising the following steps: (a) A polyurethane containing at least one carboxyl group, having an acid value of 205 mg KOH / g to 400 mg KOH / g and at least one terminal carboxyl group, Esterilization with a polyester containing at least one hydroxyl group having a hydroxyl value of 50 mg KOH / g to 300 mg KOH / g The process of obtaining polyester-polyurethane, followed by (b) A step of polymerizing an ethylenically unsaturated monomer containing at least a (meth)acrylic monomer by radical polymerization in the presence of the polyester-polyurethane of step (a). Includes, One or more solvents are present and / or used during steps (a) and / or (b), and / or added after step (b), In this way, the polyester-polyurethane-poly(meth)acrylic hybrid dispersion is obtained, and A method wherein the solid content of the polyester-polyurethane dispersion obtained in step (a) is ≥ 40% by mass.

15. The method according to claim 14, wherein the carboxyl group-containing polyurethane has an acid value of more than 210 mg KOH / g to 400 mg KOH / g.

16. A coating composition comprising a polyester-polyurethane-poly(meth)acrylic hybrid dispersion as defined in claim 1 or 2.

17. A coating layer formed from the coating composition described in claim 16.

18. A substrate coated with the coating layer described in claim 17.

19. A method of using the coating composition according to claim 16 in automotive coatings.

20. A method for manufacturing a multilayer coating, comprising the following steps: a. A step of forming one or more base coat layers on a substrate by applying one or more base coat compositions, wherein at least one base coat composition comprises a polyester-polyurethane-poly(meth)acrylic hybrid dispersion as defined in claim 1 or 2. b. A step of applying a clear coat composition onto one or more base coat layers to form a clear coat layer. c. A process in which one or more base coat layers and clear coat layers are cured simultaneously, or one or more layers obtained in steps a. and b. are cured individually and then a subsequent coating layer is applied, or all layers obtained in steps a. and b. are cured individually. A method that includes this.

Citation Information

Patent Citations

  • Waterdilutable lacquer compositions with high solids level

    EP1199342A1

  • Water-based 2-component clear paint composition and method for forming multi-layer coating film

    JP2007084801A

  • Aqueous dispersion of copolymer

    JP2016531169A

  • US10,233,353B2

  • Waterborne base coat compositions and processes for preparing waterborne base coat compositions

    US20150315414A1