Thin film modification composition and method for forming a thin film using the same

A thin film modification composition with a shielding and diffusion improving material addresses the challenge of achieving uniform film thickness and step coverage on complex substrates, improving film quality and reducing impurities.

JP7955380B2Active Publication Date: 2026-11-24SOULBRAIN CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024556815
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-10-25
Filing Date
2023-03-17
Publication Date
2026-11-24
Estimated Expiration
2043-03-17

AI Technical Summary

Technical Problem

Existing thin film deposition methods struggle to achieve 100% step coverage and uniform film thickness on substrates with complex microstructures, particularly at high temperatures, leading to poor electrical characteristics and increased impurity levels.

Method used

A thin film modification composition comprising a shielding material with lone pairs of electrons from oxygen, sulfur, or phosphorus, and a diffusion improving material, applied in a specific ratio, is used to shield the substrate surface, improving reaction rates and reducing film growth rates, thereby enhancing step coverage and uniformity.

Benefits of technology

The composition effectively improves step coverage and film uniformity on complex substrates, reduces impurities, and enhances film quality by minimizing process by-products and corrosion, even at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955380000034
    Figure 0007955380000034
  • Figure 0007955380000035
    Figure 0007955380000035
  • Figure 0007955380000036
    Figure 0007955380000036
Patent Text Reader

Abstract

The present invention relates to a thin film modification composition, a thin film formation method using the same, and a semiconductor substrate and a semiconductor device manufactured thereby. The present invention has the effect of improving the step coverage and the uniformity of the thin film thickness even when a thin film is formed under high temperature conditions on a substrate having a complex structure by improving the reaction rate and appropriately reducing the thin film growth rate by using a shielding material and a diffusion improving material in combination, and improving the film quality by reducing impurities.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a thin film modification composition, a method for forming a thin film using the same, and a semiconductor substrate and a semiconductor device manufactured thereby, and more particularly, to a thin film modification composition composed of a shielding material and a diffusion improving material, which is provided to effectively shield a substrate even under high temperature conditions to improve a reaction rate and appropriately reduce a thin film growth rate, so that even when a thin film is formed on a substrate having a complicated structure, step coverage and film thickness uniformity of the thin film can be significantly improved, impurities can be greatly reduced, and film quality can be improved, a method for forming a thin film using the same, and a semiconductor substrate manufactured thereby. Background Art

[0002] As the degree of integration of memory and non-memory semiconductor devices increases, the microstructure of substrates is becoming more and more complex.

[0003] As an example, the ratio of the width to the depth of the microstructure (hereinafter, also referred to as "aspect ratio (vertical / horizontal ratio)") has increased to 20:1 or more, 100:1 or more, and there is a problem that as the aspect ratio increases, it becomes difficult to form a deposition layer having a uniform layer thickness along a complicated microstructure surface.

[0004] As a result, step coverage, which limits the thickness ratio of the deposition layer formed on the upper and lower portions in the depth direction of the microstructure, remains at a level of 90%, and as a result, electrical characteristics of the device are gradually difficult to be expressed, and thus its importance is increasing more and more. Since the step coverage of 100% means that the thickness of the deposition layer formed on the upper and lower portions of the microstructure is the same, it is necessary to develop a technique so that the step coverage is as close to 100% as possible.

[0005] In other words, for a thin film deposited on a substrate to obtain excellent uniform physical properties, high step-level coverage of the thin film is essential. Atomic layer deposition (ALD), which utilizes surface reactions, is used more than chemical vapor deposition (CVD), which mainly utilizes gas-phase reactions. However, there are still problems in achieving 100% step-level coverage.

[0006] It is difficult to raise the deposition temperature to achieve 100% step coverage. First, in a deposition process consisting of a precursor and reactants, raising the deposition temperature not only leads to a rapid increase in the growth rate per particle size (GPC), but even if the ALD process is performed at 300°C to mitigate the increase in GPC associated with the rising deposition temperature, this does not solve the problem because the deposition temperature rises during the process.

[0007] Furthermore, high-temperature processes are necessary to achieve high-quality metal oxide films in semiconductor devices. Research has shown that increasing the atomic layer deposition temperature to 400°C reduces the concentration of residual carbon and hydrogen in the thin film (see paper J.Vac.Sci.Technol.A,35(2017)01B130).

[0008] However, as the deposition temperature increases, it becomes more difficult to ensure sufficient step coverage. First, in a deposition process consisting of a precursor and a reactant, an increase in deposition temperature can lead to a rapid increase in GPC (growth rate of film). Furthermore, even if known shielding agents are applied to mitigate the increase in GPC associated with rising deposition temperature, it has been confirmed that GPC increases by approximately 10% at 300°C. In other words, when deposition is performed at temperatures above 360°C, the GPC reduction effect of conventionally known shielding agents is unlikely to be significant.

[0009] Therefore, there is a need for the development of a thin film formation method that can effectively form thin films with complex structures even at high temperatures, has a low amount of residual impurities, and significantly improves step coverage and thickness uniformity of the thin film, as well as semiconductor substrates manufactured by this method. [Overview of the Initiative] [Problems that the invention aims to solve]

[0010] The present invention has been made to solve the problems of the prior art described above, and aims to provide a thin film modification composition that improves film quality by reducing impurities while significantly improving step coverage and uniformity of film thickness, even when forming a thin film on a substrate having a complex structure, by effectively shielding the substrate by using a shielding material and a diffusion improving material in combination to improve the reaction rate and appropriately reduce the thin film growth rate, a thin film modification composition that uses the same to form a thin film, a method for forming a thin film using the same, and a semiconductor substrate manufactured therefrom.

[0011] The present invention aims to improve the density, electrical properties, and dielectric properties of a thin film by improving its crystallinity and oxidation fraction.

[0012] All of the above-mentioned and other objectives of the present invention can be achieved by the present invention as described below. [Means for solving the problem]

[0013] To achieve the above objective, the present invention comprises 50 to 99 parts by weight of a shielding material having one or more lone pairs of electrons selected from oxygen (O), sulfur (S), and phosphorus (P), and 1 to 50 parts by weight of a diffusion improving material.

[0014] The diffusion-improving substance provides a thin-film modification composition characterized by having a boiling point in the range of 5 to 200°C.

[0015] The shielding material may include linear or cyclic saturated or unsaturated hydrocarbons having two or more oxygen (O), phosphorus (P), or sulfur (S) atoms, and having 3 to 15 carbon atoms.

[0016] The aforementioned shielding material may include compounds having a structure in which oxygen (O), phosphorus (P), or sulfur (S) are present at both ends of a central carbon atom linked to oxygen by a double bond.

[0017] The shielding material may include a compound having a structure in which one end of a central carbon atom linked to oxygen by a double bond contains oxygen (O), phosphorus (P), or sulfur (S), and the other end contains carbon (C).

[0018] The aforementioned shielding material may be one or more compounds selected from the compounds represented by chemical formula 1 to chemical formula 2 below.

[0019] [Chemical formula 1]

[0020] [ka]

[0021] [Chemical formula 2]

[0022] [ka]

[0023] (In the above chemical formulas 1 and 2, the above R' and R ” These are, independently, hydrogen, a C1-C5 alkyl group, a C1-C5 alkene group, or a C1-C5 alkoxy group.

[0024] A is oxygen (O), sulfur (S), phosphorus (P), nitrogen (N), -CH, or -CH2.

[0025] The aforementioned B is -OH, -OCH3, -OCH2CH3, -CH2CH3, -SH, -SCH3, or -SCH2CH3,

[0026] m is an integer between 0 and 3.

[0027] The shielding material may contain one or more compounds selected from the compounds represented by the following chemical formulas 1-1 to 1-4 and 2-1 to 2-4.

[0028] [Chemical formula 1-1~1-6]

[0029] [ka]

[0030] [Chemical formula 2-1~2-4]

[0031] [ka]

[0032] The shielding material may have a refractive index (measured at 20-25°C) of 1.30 or higher, 1.3-1.5, 1.35-1.48, or 1.36-1.46.

[0033]

[0034] The diffusion-improving substance may have a boiling point in the range of 5 to 200°C, specifically 10 to 150°C, preferably 25 to 140°C.

[0035] The diffusion-improving substance may preferably be a liquid at room temperature in order to improve the diffusivity and uniformity of the aforementioned shielding substance.

[0036] The diffusion-improving substance may be one or more selected from octane, diethyl ether, methylene chloride, toluene, hexane, and ethanol.

[0037] The diffusion-improving material may have a refractive index of 1.30 or higher, 1.30 to 1.70, 1.35 to 1.60, or 1.36 to 1.50.

[0038]

[0039] The thin film modification composition may have a deposition rate reduction rate of 30% or more, as shown in the following formula 1.

[0040] [Formula 1]

[0041] TIFF0007955380000005.tif9138

[0042] (In the above formula, DR (Deposition rate, Å / cycle) is the rate at which the thin film is deposited. When a thin film formed by a precursor and reactants is deposited, DR i The (initial deposition rate) is the deposition rate of a thin film formed without the addition of a diffusion-improving material. DR f The (final deposition rate) is the deposition rate of the thin film formed by adding a diffusion-improving material during the process described above. Here, the deposition rate (DR) is measured using an ellipsometer for thin films with a thickness of 3-30 nm under normal temperature and pressure conditions, and its unit is Å / cycle.

[0043] The thin film may be one or more laminated films selected from the group consisting of Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce, and Nd.

[0044] The thin film may be used as a diffusion prevention film, etching stop film, electrode film, dielectric film, gate insulating film, block oxide film, or charge trap.

[0045]

[0046] Furthermore, the present invention is

[0047] A thin film modification composition comprising 50 to 99 parts by weight of a shielding material having at least one lone pair of electrons selected from oxygen (O), sulfur (S), and phosphorus (P), and 1 to 50 parts by weight of a diffusion improving material is injected into a chamber to shield a surface of a loaded substrate, wherein the diffusion improving material is at least one selected from the group consisting of an alkylamine having a boiling point in the range of 5 to 200° C. and an arylamine having a boiling point in the range of 50 to 260° C.

[0048] A precursor compound used in the thin film forming method may be a compound represented by the following Chemical Formula 3.

[0049] [Chemical Formula 3]

[0050] [Chemical Formula]

[0051] (In Chemical Formula 3, M is at least one selected from the group consisting of Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce, and Nd, and L 1 , L 2 , L 3 , and L4 are each -H, -X, -R, -OR, -NR, or Cp (cyclopentadiene)2, and may be the same as or different from each other, wherein -X is F, Cl, Br, or I, and -R is C1 to C 10 alkyl, C1 to C 10 alkene, or C1 to C 10 alkane, and may be linear or cyclic, wherein the L 1 , L 2 , L 3 , and L 4 may be formed in 2 to 6 depending on an oxidation value of the central metal.)

[0052] As an example, when the central metal is divalent, L 1 and L 2It can attach to the central metal as a ligand, and if the central metal is hexavalent, L 1 , L 2 , L 3 , L 4 , L 5 , L 6 It can be attached to the central metal, L 1 ~L 6 The ligands corresponding to these may be the same or different from each other.

[0053] In the aforementioned chemical formula 3, L 1 , L 2 , L 3 and L 4 -H, -X, or -R, which may be the same or different from each other, where -R is C1~C 10 Alkyl, C1~C 10 Alkenes of the C1-C 10 It is an alkane and can be linear or cyclic.

[0054] In the aforementioned chemical formula 3, L 1 , L 2 , L 3 and L 4 is -H, -OR, -NR, or Cp(cyclopentadiene)2, which may be the same or different from each other, where -R is H, C1~C 10 Alkyl, C1~C 10 Alkenes, C1~C 10 It may be an alkane, iPr, or TBu.

[0055] In the aforementioned chemical formula 3, L 1 , L 2 , L 3 and L 4 is -H or -X, which may be the same or different from each other, where -X may be F, Cl, Br, or I.

[0056]

[0057] Furthermore, the present invention is

[0058] i) A step of vaporizing the aforementioned thin film modification composition to shield the surface of the substrate loaded into the chamber,

[0059] ii) A step of primary purging the inside of the chamber with a purge gas,

[0060] iii) A step of vaporizing the precursor compound and adsorbing it onto a region outside the shielding region,

[0061] iv) The step of secondary purging the inside of the chamber with purge gas,

[0062] v) The step of supplying a reaction gas to the inside of the chamber,

[0063] vi) A thin film formation method is provided, which includes the step of tertiarily purging the inside of the chamber with a purge gas.

[0064] The precursor compound may be a molecule consisting of one or more elements selected from the group consisting of Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce, and Nd, and having a vapor pressure at 25°C greater than 0.01 mTorr and less than or equal to 100 Torr.

[0065] The chamber may be an atomic layer deposition (ALD) chamber, a chemical vapor deposition (CVD) chamber, a plasma-enhanced atomic layer deposition (PEALD) chamber, or a plasma-enhanced chemical vapor deposition (PECVD) chamber.

[0066] The process may include a step of vaporizing and injecting the thin-film modification composition or precursor compound, followed by plasma post-treatment.

[0067] The amount of purge gas introduced into the chamber in step i) and step iv) can be 10 to 100,000 times the volume of the introduced thin-film modification composition.

[0068] The reaction gas is an oxidizing agent, a nitriding agent, or a reducing agent, and the reaction gas, thin-film modifying composition, and precursor compound can be transported into the chamber by a vapor flow control (VFC), direct liquid introduction (DLI), or liquid delivery system (LDS).

[0069] The thin film may be a silicon nitride film, a silicon oxide film, a titanium nitride film, a titanium oxide film, a tungsten nitride film, a molybdenum nitride film, a hafnium oxide film, a zirconium oxide film, a tungsten oxide film, or an aluminum oxide film.

[0070] The substrate loaded into the chamber is heated to 100-800°C, and the ratio of the amount (mg / cycle) of the thin-film modification composition to the precursor compound introduced into the chamber can be 1:1-1:20.

[0071] Furthermore, the present invention provides a semiconductor substrate characterized by being manufactured by the thin-film formation method described above.

[0072] The thin film may have a multilayer structure consisting of two or three or more layers.

[0073]

[0074] Furthermore, the present invention provides a semiconductor device including the aforementioned semiconductor substrate.

[0075] The semiconductor substrate may be a low-resistive metal gate interconnect, a high-aspect-ratio 3D metal-insulator-metal (MIM) capacitor, a DRAM trench capacitor, a 3D gate-all-around (GAA) capacitor, or a 3D NAND flash memory. [Effects of the Invention]

[0076] According to the present invention, by effectively shielding adsorption to the substrate surface to improve the reaction rate and appropriately reducing the thin film growth rate, it is possible to provide a thin film modification composition that improves step coverage even when forming a thin film on a substrate having a complex structure under high-temperature conditions.

[0077] Furthermore, the process by-products during thin film formation are more effectively reduced, preventing corrosion and degradation, and improving the crystallinity of the thin film by modifying its properties, thereby improving its electrical properties.

[0078] Furthermore, it is possible to improve the step coverage and density of the thin film, and it is also possible to provide a thin film formation method using this method and a semiconductor substrate manufactured therefrom. [Brief explanation of the drawing]

[0079] [Figure 1] This diagram schematically shows the deposition process sequence according to the present invention, focusing on one cycle.

[0080] [Figure 2] This figure shows a comparison of the calculated non-uniformity for each thin film obtained in Examples 1-2 and Comparative Examples 2-3, which will be described later.

[0081] [Figure 3] This is a TEM image showing the step coverage at the upper and lower edges of the thin film obtained in Example 1, which will be described later. [Figure 4] This is a TEM image showing the step coverage at the upper and lower edges of the thin film obtained in Example 2, which will be described later. [Figure 5] This is a TEM image showing the step coverage at the upper and lower edges of the thin film obtained in Example 3, which will be described later. [Modes for carrying out the invention]

[0082]

[0083] The thin-film modification composition described herein, the thin-film formation method using the same, and the semiconductor substrate manufactured therefrom will be described in detail below.

[0084] In this description, unless otherwise specified, the term "shielding" means not only reducing, preventing, or blocking the adsorption of precursor compounds for forming thin films onto the substrate, but also reducing, preventing, or blocking the adsorption of process by-products onto the substrate.

[0085] In this description, unless otherwise specified, the term "diffusion-improving substance" refers to a substance that can assist in the diffusion of a shielding substance and improve its uniformity.

[0086] The inventors have found that by using a shielding material that can block the adsorption of the precursor compound to be supplied for forming a thin film on the surface of a substrate loaded inside a chamber, and a diffusion improving material that can modify the uniformity of the resulting thin film, the reaction rate under high-temperature conditions can be improved. Even when applied to substrates with complex structures, the film quality is improved, ensuring the uniformity of the thin film and significantly improving step coverage. In particular, it is possible to deposit thin films, and it is possible to improve residual O, Si, metals, metal oxides, and even carbon residues that were previously difficult to reduce as process by-products. Based on this finding, the inventors incorporated research on thin film modification compositions and completed the present invention.

[0087]

[0088] The thin film can be provided, for example, as one or more precursors selected from the group consisting of Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce, and Nd, and can provide an oxide film, a nitride film, or a metal film, in which case the effects to be achieved in the present invention can be fully obtained.

[0089] The thin film may, in specific examples, have a film composition of silicon nitride, silicon oxide, titanium nitride, titanium oxide, tungsten nitride, molybdenum nitride, hafnium oxide, zirconium oxide, tungsten oxide, or aluminum oxide.

[0090] The aforementioned thin film means that the aforementioned film composition also includes SiH and SiOH.

[0091] The thin film can be used in semiconductor devices not only as a diffusion-blocking film for general use, but also as an etching stop film, electrode film, dielectric film, gate insulating film, block oxide film, or charge trap.

[0092]

[0093] In the present invention, the precursor compound used to form a thin film is a molecule having Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce, and Nd as the central metal atom (M), and containing one or more ligands consisting of C, N, O, H, and X (halogens). The film quality improvement effect described later can be maximized when the precursor has a vapor pressure of 1 mTorr to 100 Torr at 25°C.

[0094] As an example of the precursor compound, a compound represented by the following chemical formula 3 can be used.

[0095] [Chemical formula 3]

[0096] [ka]

[0097] (In the above chemical formula 3, M is one or more selected from Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce, and Nd, L 1 , L 2 , L 3 and L 4 -H, -X, -R, -OR, -NR, or Cp(cyclopentadiene)2, which may be the same or different from each other, where -X is F, Cl, Br, or I, and -R is C1~C 10 Alkyl, C1~C 10 Alkenes of the C1-C 10 (An alkane, which may be linear or cyclic.)

[0098] In the aforementioned chemical formula 3, M is hafnium (Hf), silicon (Si), zirconium (Zr), or aluminum (Al), preferably hafnium (Hf) or silicon (Si). In this case, there is a significant reduction in process by-products, excellent step coverage, and further advantages in thin film density improvement, electrical properties, insulation, and dielectric properties of the thin film.

[0099] Said L 1 , L 2 , L 3 and L 4 -H, -X, or -R, which may be the same or different from each other, where -R is C1~C 10 Alkyl, C1~C 10 Alkenes of the C1-C 10 It is an alkane, which may have a linear or cyclic structure.

[0100] Furthermore, the L1 , L 2 , L 3 and L 4 is -H, -OR, -NR, or Cp(cyclopentadiene)2, which may be the same or different from each other, where -R is H, C1~C 10 Alkyl, C1~C 10 Alkenes, C1~C 10 It may be an alkane, iPr, or tBu.

[0101] Furthermore, in the above chemical formula 3, L 1 , L 2 , L 3 and L 4 is -H or -X, which may be the same or different from each other, where -X may be F, Cl, Br, or I.

[0102] Specifically, examples of silicon precursor compounds include SiH4, SiHCl3, SiH2Cl2, SiCl4, Si2Cl6, Si3Cl8, and Si4Cl 10 One or more of the following can be used: SiH2[NH(C4H9)]2, Si2(NHC2H5)4, Si3NH4(CH3)3, and SiH3[N(CH3)2], SiH2[N(CH3)2]2, SiH[N(CH3)2]3, and Si[N(CH3)2]4.

[0103] Furthermore, examples of hafnium precursor compounds that can be used include tris(dimethylamide)cyclopentadienylhafnium (CpHf(NMe2)3) and (methyl-3-cyclopentadienylpropylamino)bis(dimethylamino)hafnium (Cp(CH2)3NM3Hf(NMe2)2).

[0104] Examples of aluminum precursor compounds include trimethylaluminum (TMA), tris(dimethylamido)aluminum (TDMAA), and aluminum chloride (AlCl3).

[0105] These can be used.

[0106]

[0107] The thin film modification composition may consist of a shielding substance and a diffusion-improving substance.

[0108] Here, the shielding material is characterized by containing a compound having one or more lone pairs of electrons selected from oxygen (O), sulfur (S), and phosphorus (P), preferably two or more oxygen (O), phosphorus (P), or sulfur (S), and containing linear or cyclic saturated or unsaturated hydrocarbons having 3 to 15 carbon atoms. In this case, when forming a thin film, a shielding region that does not remain in the thin film is formed, creating a relatively sparse thin film, while suppressing side reactions, adjusting the thin film growth rate, reducing process by-products in the thin film, reducing corrosion and degradation, improving the crystallinity of the thin film, and enabling the formation of a stoichiometric oxidation state during the formation of a metal oxide film. This has the effect of significantly improving step coverage and the uniformity of the thin film thickness, even when forming a thin film under high-temperature conditions on a substrate with a complex structure.

[0109] As a specific example, the shielding material contains a compound having a structure in which oxygen (O), phosphorus (P), or sulfur (S) are present at both ends of a central carbon atom linked to oxygen by a double bond. This significantly reduces process by-products, provides excellent step coverage, and further improves thin film density and the electrical properties of the thin film.

[0110] Here, structures in which oxygen (O), phosphorus (P), or sulfur (S) are present at both ends of a central carbon atom linked to oxygen by a double bond, as described above, are defined as follows, unless otherwise specified. [ka] It refers to.

[0111] As a specific example, the shielding material has a structure in which one end of a central carbon atom linked to oxygen by a double bond contains oxygen (O), phosphorus (P), or sulfur (S), and the other end contains carbon (C). This significantly reduces process by-products, provides excellent step coverage, and offers superior thin film density improvement and electrical properties.

[0112] Here, a structure containing oxygen (O), phosphorus (P), or sulfur (S) at one end of a central carbon atom linked to oxygen by a double bond, and carbon (C) at the other end, is defined as follows, unless otherwise specified. [ka] It refers to.

[0113] The shielding material can be, as a specific example, one or more compounds selected from the compounds represented by chemical formula 1 to chemical formula 2 below. In this case, when forming a thin film, a shielding region that does not remain in the thin film is formed, creating a relatively sparse thin film. Side reactions are suppressed, the thin film growth rate is adjusted, process by-products within the thin film are reduced, corrosion and degradation are reduced, the crystallinity of the thin film is improved, and even when forming a thin film on a substrate with a complex structure, step coverage and thickness uniformity of the thin film can be significantly improved.

[0114] [Chemical formula 1]

[0115] [ka]

[0116] [Chemical formula 2]

[0117] [ka]

[0118] (In the above chemical formulas 1 and 2, the above R' and R ”These are, independently, hydrogen, a C1-C5 alkyl group, a C1-C5 alkene group, or a C1-C5 alkoxy group.

[0119] A is oxygen (O), sulfur (S), phosphorus (P), nitrogen (N), -CH, or -CH2.

[0120] The aforementioned B is -OH, -OCH3, -OCH2CH3, -CH2CH3, -SH, -SCH3, or -SCH2CH3.

[0121] m is an integer between 0 and 3.

[0122] In the aforementioned chemical formula 1, A is oxygen (O) or sulfur (S), preferably oxygen (O). In this case, there are advantages such as a significant reduction in process by-products, excellent step coverage, improved thin film density, and even better electrical, insulating, and dielectric properties of the thin film.

[0123] The R' is an alkyl group having 1 to 3 carbon atoms, preferably an alkyl group having 1 to 2 carbon atoms. In this case, there is a significant effect in reducing process by-products, excellent step coverage, and further advantages in improving thin film density, electrical properties, insulation, and dielectric properties of the thin film.

[0124] The aforementioned m is an integer between 1 and 2, preferably an integer of 1.

[0125] In the aforementioned chemical formula 2, B is -OH, -OCH3, -OCH2CH3, -CH2CH3, -SH, -SCH3, or -SCH2CH3. In this case, there are advantages such as a significant reduction in process by-products, excellent step coverage, improved thin film density, and even better electrical properties of the thin film.

[0126] The R'' is an alkyl group having 1 to 3 carbon atoms, preferably an alkyl group having 1 to 2 carbon atoms. In this case, there are advantages such as a significant reduction in process by-products, excellent step coverage, improved thin film density, and even better electrical properties of the thin film.

[0127]

[0128] As an example, if the shielding material is a compound represented by chemical formula 1, it may be a compound with a refractive index in the range of 1.4 to 1.5, more specifically 1.4 to 1.48, preferably 1.4 to 1.46.

[0129] For example, if the shielding material is a compound represented by chemical formula 2, it may be a compound with a refractive index in the range of 1.3 to 1.4, specifically 1.33 to 1.39, preferably 1.35 to 1.39.

[0130]

[0131] In this case, by forming a uniform layer thickness on the substrate as a shielding region that does not remain on the thin film, due to the difference in the degree of adsorption distribution of the shielding agent having the aforementioned structure, the deposition rate of the thin film is reduced and the thin film growth rate is appropriately lowered. This has the advantage of significantly improving step coverage and the uniformity of the thin film thickness, even when forming a thin film on a substrate with a complex structure under high-temperature conditions, effectively protecting the substrate surface by preventing the adsorption of not only thin film precursors but also process by-products, and effectively removing process by-products.

[0132] In particular, because it forms a relatively sparse thin film and significantly reduces the growth rate of the formed thin film, even when applied to substrates with complex structures, it ensures the uniformity of the thin film and greatly improves step coverage. Moreover, it enables deposition at very thin thicknesses and can improve the amount of residual O, Si, metals, metal oxides, and even carbon residues that were previously difficult to reduce as process by-products.

[0133]

[0134] The shielding material may include one or more compounds selected from the compounds represented by the following chemical formulas 1-1 to 1-4 and 2-1 to 2-4. In this case, the effect of providing a thin film shielding region and adjusting the thin film growth rate is significant, the effect of removing process by-products is also significant, and not only are there excellent effects in improving step coverage and film quality, but the uniformity of the resulting thin film can also be significantly improved.

[0135] [Chemical formula 1-1~1-4]

[0136] [ka]

[0137] [Chemical formula 2-1~2-4]

[0138] [ka]

[0139] The aforementioned diffusion-improving material is characterized by having a boiling point in the range of 5 to 200°C, 5 to 190°C, or 6 to 190°C. In such cases, it improves the diffusivity of the shielding material, suppresses side reactions during thin film formation, adjusts the thin film growth rate, reduces process by-products within the thin film, reduces corrosion and degradation, and improves the quality of the film, such as improving the crystallinity of the thin film. Furthermore, it enables the formation of a metal oxide film to reach a stoichiometric oxidation state, and even when forming a thin film under high-temperature conditions on a substrate with a complex structure, it has the effect of significantly improving step coverage and the uniformity of the film thickness.

[0140] The aforementioned diffusion-improving substance, as an example, has a solubility in water (at 25°C) of 200 mg / L or less, preferably 50 to 400 mg / L, and more preferably 135 to 175 mg / L. Within this range, it has the advantage of low reactivity to the precursor compound and easy moisture management.

[0141] In this description, solubility is not particularly limited to measurement methods or standards commonly used in the art to which the present invention pertains. For example, a saturated solution can be measured by high-performance liquid chromatography (HPLC).

[0142] The aforementioned diffusion-improving substance, preferably one or more selected from octane, diethyl ether, and methylene chloride, can reduce the deposition rate represented by the following formula 1 by 30% or more, specifically 40% or more, and preferably 50% or more. In this case, a uniform layer thickness deposition layer is formed as a shielding region that does not remain in the thin film due to the difference in the degree of adsorption distribution of the activator having the aforementioned structure, thereby forming a relatively sparse thin film. Furthermore, the growth rate of the formed thin film is significantly reduced. As a result, even when applied to substrates with complex structures, the uniformity of the thin film is ensured, and step coverage is greatly improved. In particular, it is possible to deposit thin films, and it is possible to improve the amount of O, Si, metals, metal oxides, and even carbon residues that were previously difficult to reduce as process by-products.

[0143] [Formula 1]

[0144] TIFF0007955380000014.tif13148

[0145] (In the above formula, DR (Deposition rate, Å / cycle) is the rate at which the thin film is deposited. When a thin film formed by a precursor and reactants is deposited, DR i (Initial deposition rate) is the deposition rate of a thin film formed without the addition of a diffusion-improving agent. f The (final deposition rate) is the deposition rate of the thin film formed by adding a diffusion-improving material during the process described above. Here, the deposition rate (DR) is measured using an ellipsometer for thin films with a thickness of 3-30 nm under normal temperature and pressure conditions, and its unit is Å / cycle.

[0146] In the above formula 1, the thin film growth rate per cycle when the thin film modification composition is used and when it is not used refers to the deposition thickness of the thin film per cycle (Å / cycle), i.e., the deposition rate. As an example, the deposition rate can be determined by measuring the final thickness of a thin film with a thickness of 3 to 30 nm under room temperature and atmospheric pressure conditions using ellipsometry, and then dividing by the total number of cycles to obtain the average deposition rate.

[0147] In the aforementioned formula 1, "when the thin film modification composition is not used" means the case in which only the precursor compound is adsorbed onto the substrate during the thin film deposition process to produce a thin film. A specific example is the case in the thin film formation method in which the steps of adsorbing the thin film modification composition and purging the unadsorbed thin film modification composition are omitted to form a thin film.

[0148] The diffusion-improving substance may, for example, be a compound having a refractive index in the range of 1.30 or higher, 1.30 to 1.70, 1.35 to 1.60, or 1.36 to 1.50.

[0149] In this case, by appropriately shielding the adsorption of the precursor compound onto the substrate, the reaction rate is improved, and even when forming a thin film on a substrate with a complex structure, the step coverage and uniformity of the thin film thickness are greatly improved. This has the advantage of effectively protecting the substrate surface by preventing the adsorption of not only the thin film precursor but also process by-products, and effectively removing process by-products.

[0150]

[0151] The thin film modification composition may contain the shielding substance and the diffusion improving substance in a weight ratio of 50:50 to 99:1, more preferably 60:40 to 95:5, more preferably 70:30 to 92:8, and even more preferably 80:20 to 90:10. In this case, a relatively sparse thin film is formed, and the growth rate of the formed thin film is significantly reduced. Therefore, even when applied to substrates with complex structures, the uniformity of the thin film is ensured, the step coverage is greatly improved, and in particular, it is possible to deposit thin films, and it is possible to improve residual O, Si, metals, metal oxides, and even carbon residues that were previously difficult to reduce as process by-products.

[0152] For reference, examples of diffusion-improving substances include octane with a boiling point of approximately 125.6°C, methylene chloride with a boiling point of approximately 39.6°C, and diethyl ether with a boiling point of approximately 34.6°C.

[0153]

[0154] The thin film modification composition may have a deposition rate reduction rate of 30% or more, as shown in the following formula 1.

[0155] [Formula 1]

[0156] TIFF0007955380000015.tif13169

[0157] (In the above formula, DR (Deposition rate, Å / cycle) is the rate at which the thin film is deposited. When a thin film formed by a precursor and reactants is deposited, DR i (Initial deposition rate) is the deposition rate of a thin film formed without the addition of a diffusion-improving agent. fThe (final deposition rate) is the deposition rate of the thin film formed by adding a diffusion-improving material during the process described above. Here, the deposition rate (DR) is measured using an ellipsometer for thin films with a thickness of 3-30 nm under normal temperature and pressure conditions, and its unit is Å / cycle.

[0158] The aforementioned shielding region for the thin film is characterized by not remaining in the thin film.

[0159] Here, "no residue" means, unless otherwise specified, the presence of C, Si, N, and halogen elements in amounts less than 0.1 atoms (atom%) during component analysis by XPS. More preferably, in a measurement method using secondary-ion mass spectrometry (SIMS) or X-ray photoelectron spectroscopy (XPS) while measuring while excavating the substrate in the depth direction, it is preferable that the increase or decrease in signal intensity for each element species does not exceed 5%, considering the increase or decrease in C, N, Si, and halogen impurities before and after using the activator under the same deposition conditions.

[0160]

[0161] In the aforementioned thin film formation method, for example, when using the thin film modification composition, the non-uniformity shown in the following formula 2 may be 1.2% or less, specifically 1.1% or less, preferably 0.01 to 1.1%. In this case, a uniform layer thickness is formed as a replacement region that does not remain in the thin film due to the difference in the degree of adsorption distribution of the step coverage improving agent having the aforementioned structure, thereby forming a relatively sparse thin film. Furthermore, the growth rate of the formed thin film is significantly reduced. As a result, even when applied to substrates with complex structures, the uniformity of the thin film is ensured, and step coverage is significantly improved. In particular, it is possible to deposit thin films, and it is possible to improve the amount of O, Si, metals, metal oxides, and even carbon residues that were previously difficult to reduce as process by-products.

[0162] [Formula 2]

[0163] TIFF0007955380000016.tif11146

[0164] The maximum and minimum film thicknesses were determined by measuring the thin films using the ellipsometer device used to determine the reduction rate of the deposition rate, as described above.

[0165] For example, the film thickness can be measured and selected at 10 arbitrarily chosen locations. Preferably, the film thickness can be measured and selected at four locations on the east, west, north, and south edges of a 300 mm wafer, and at one location in the central part.

[0166]

[0167] The aforementioned thin film may, for example, contain a halogen compound at a concentration of 100 ppm or less. For reference, if halogens remain in excess, it is undesirable when using a nitride agent under the experimental conditions described later, such as a temperature of 200-300°C, because it generates byproducts such as NH4Cl that remain in the thin film.

[0168] The thin film can be used, but is not limited to, as an etching stop film, electrode film, dielectric film, gate insulating film, block oxide film, or charge trap.

[0169] The thin-film modification composition may preferably be a compound with a purity of 99.9% or higher, a compound with a purity of 99.95% or higher, or a compound with a purity of 99.99% or higher. For reference, if a compound with a purity of less than 99% is used, impurities may remain in the thin film or cause side reactions with precursors or reactants, so it is preferable to use a substance with a purity of 99% or higher.

[0170]

[0171] The thin-film modification composition is preferably used in an atomic layer deposition (ALD) process. In this case, it has the advantage of effectively protecting the substrate surface and effectively removing process by-products without hindering the adsorption of precursor compounds.

[0172] The thin film modification composition preferably has a density of 0.8 to 2.5 g / cm³. 3 Or 0.8~1.5 g / cm³ 3 The vapor pressure (at 20°C) can be between 0.1 and 300 mmHg or between 1 and 300 mmHg, and within this range, it exhibits excellent step coverage, thin film thickness uniformity, and film quality improvement.

[0173] More preferably, the thin film modification composition has a density of 0.75 to 2.0 g / cm³ 3 Or 0.8-1.3 g / cm³ 3 Therefore, the vapor pressure (at 20°C) can be between 1 and 260 mmHg, and within this range, it exhibits excellent step coverage, thin film thickness uniformity, and film quality improvement.

[0174]

[0175] In particular, because it forms a relatively sparse thin film and significantly reduces the growth rate of the formed thin film, even when applied to substrates with complex structures, it ensures the uniformity of the thin film and greatly improves step coverage. Moreover, it enables deposition at very thin thicknesses and can improve the amount of residual O, Si, metals, metal oxides, and even carbon residues that were previously difficult to reduce as process by-products.

[0176]

[0177] The present invention provides a thin film formation method that includes the step of injecting the aforementioned thin film modification composition into a chamber to replace the ligand of the precursor compound adsorbed on the surface of the loaded substrate. In this case, by effectively replacing the ligand of the precursor adsorbed on the substrate, the reaction rate is improved and the thin film growth rate is appropriately reduced, thereby significantly improving step coverage and the uniformity of the thin film thickness, even when forming a thin film on a substrate with a complex structure.

[0178]

[0179] The step of shielding the surface of the substrate using the thin film modification composition is characterized in that the feeding time (seconds (sec)) of the thin film modification composition to the surface of the substrate is preferably 0.01 to 10 seconds, more preferably 0.02 to 8 seconds, even more preferably 0.04 to 6 seconds, and even more preferably 0.05 to 5 seconds per cycle. Within this range, there are advantages such as a low thin film growth rate, excellent step coverage, and economic efficiency.

[0180] In this description, the feeding time of the precursor compound is based on a flow rate of 0.1 to 500 mg / cycle at a chamber volume of 15 to 20 L, and more specifically, on a flow rate of 0.8 to 200 mg / cycle at a chamber volume of 18 L.

[0181]

[0182] As a preferred embodiment, the thin film formation method may include: i) vaporizing the thin film modification composition to shield the surface of the substrate loaded into the chamber; ii) primary purging the inside of the chamber with a purge gas; iii) vaporizing the precursor compound and adsorbing it to the area outside the shielded region; iv) secondary purging the inside of the chamber with a purge gas; v) supplying a reaction gas to the inside of the chamber; and vi) tertiary purging the inside of the chamber with a purge gas. In this case, steps i) to vi) can be considered as a unit cycle and repeated until a thin film of the desired thickness is obtained (see Figure 1 below). When the thin film modification composition of the present invention is introduced before the precursor compound within one cycle to improve the film quality, even if deposition is performed at high temperatures, the thin film growth rate can be appropriately reduced, the process by-products generated are effectively removed, the resistivity of the thin film decreases, and the step coverage is greatly improved.

[0183] In a preferred example, the thin film formation method of the present invention allows the thin film modification composition of the present invention to be introduced before the precursor compound within a single cycle and adsorbed onto the substrate. In this case, even if the thin film is deposited at high temperatures, the thin film growth rate can be appropriately reduced, significantly reducing process by-products, greatly improving step coverage, increasing the crystallinity of the thin film, and reducing the resistivity of the thin film. Furthermore, even when applied to semiconductor devices with a large aspect ratio, the uniformity of the thin film thickness can be greatly improved, ensuring the reliability of the semiconductor device.

[0184]

[0185] As an example, in the thin film formation method, when the thin film modification composition is deposited before or after the deposition of the precursor compound, the unit cycle can be repeated 1 to 99,999 times as needed, preferably 10 to 10,000 times, more preferably 50 to 5,000 times, and even more preferably 100 to 2,000 times. Within this range, the desired thin film thickness can be obtained while fully achieving the effects to be achieved in the present invention.

[0186]

[0187] In the present invention, the chamber may, for example, be an ALD chamber, a CVD chamber, a PEALD chamber, or a PECVD chamber.

[0188] In the present invention, the thin film modification composition or precursor compound may be vaporized and injected, followed by a plasma post-treatment step, in which case the growth rate of the thin film can be improved while reducing process by-products.

[0189]

[0190] When the precursor compound is adsorbed while the thin film modification composition is injected onto the substrate, the amount of purge gas introduced into the chamber in the step of purging the unadsorbed thin film modification composition is not particularly limited as long as it is sufficient to remove the unadsorbed thin film modification composition. For example, it may be 10 to 100,000 times, preferably 50 to 50,000 times, and more preferably 100 to 10,000 times. Within this range, the unadsorbed thin film modification composition can be sufficiently removed to form a uniform thin film and prevent deterioration of the film quality. Here, the amounts of purge gas and thin film modification composition introduced are based on one cycle, and the volume of the thin film modification composition refers to the volume of vaporized thin film modification composition vapor.

[0191] As a specific example, in the step of injecting the thin film modification composition at a flow rate of 1.66 mL / s and an injection time of 0.5 seconds (per cycle), and purging the unadsorbed thin film modification composition, if the purge gas is injected at a flow rate of 166.6 mL / s and an injection time of 3 seconds (per cycle), the amount of purge gas injected is 602 times the amount of thin film modification composition injected.

[0192]

[0193] The amount of purge gas introduced into the chamber in the step of purging the unadsorbed precursor compound is not particularly limited as long as it is sufficient to remove the unadsorbed precursor compound. For example, it may be 10 to 10,000 times the volume of the precursor compound introduced into the chamber, preferably 50 to 50,000 times, and more preferably 100 to 10,000 times. Within this range, the unadsorbed precursor compound can be sufficiently removed to form a thin film uniformly and prevent deterioration of the film quality. Here, the amounts of purge gas and precursor compound introduced are based on one cycle, and the volume of the precursor compound refers to the volume of vaporized precursor compound vapor.

[0194]

[0195] Furthermore, in the purging step performed immediately after the reaction gas supply step, the amount of purge gas introduced into the chamber may, for example, be 10 to 10,000 times the volume of reaction gas introduced into the chamber, preferably 50 to 50,000 times, and more preferably 100 to 10,000 times, and the desired effect can be sufficiently obtained within this range. Here, the amounts of purge gas and reaction gas introduced are based on one cycle each.

[0196]

[0197] The thin-film modification composition and precursor compound can preferably be transported into the chamber by VFC, DLI, or LDS, and more preferably by LDS.

[0198] The substrate loaded into the chamber may be heated to, for example, 50 to 400°C, specifically 50 to 400°C. The thin-film modification composition or precursor compound may be injected onto the substrate either unheated or heated. Depending on the deposition efficiency, the injection may be performed unheated first, and then the heating conditions may be adjusted during the deposition process. For example, it may be injected onto the substrate at 50 to 400°C for 1 to 20 seconds.

[0199]

[0200] The ratio of the amount (mg / cycle) of the thin film modification composition to the amount of the precursor compound to be introduced into the chamber is preferably 1:1.5 to 1:20, more preferably 1:2 to 1:15, even more preferably 1:2 to 1:12, and even more preferably 1:2.5 to 1:10. Within this range, the effect of improving step coverage and reducing process by-products is significant.

[0201]

[0202] The aforementioned precursor material can be used in combination with a nonpolar solvent.

[0203] As the nonpolar solvent, an alkane having 1 to 5 carbon atoms or a cycloalkane can be used, and specifically, it may be present in an amount of 5 to 95% by weight, more preferably 10 to 90% by weight, even more preferably 40 to 90% by weight, and most preferably 70 to 90% by weight, relative to the total weight of the precursor compound and the nonpolar solvent combined.

[0204] Even if the aforementioned types of nonpolar solvents are used, if the amount used exceeds the upper limit, it induces impurities, increasing resistance and the value of impurities in the thin film. Conversely, if the amount of the organic solvent added is below the lower limit, there is a disadvantage in that the effect of improving step coverage due to the addition of the solvent and the effect of reducing impurities such as chloride (Cl) ions are not obtained to a great extent.

[0205]

[0206] In the aforementioned thin film formation method, for example, when using the thin film modification composition, the reduction rate of the deposition rate, represented by the following formula 1, can be 30% or more, and in specific cases, 35% or more. In this case, a deposition layer of uniform thickness is formed as a substitution region that does not remain in the thin film due to the difference in the degree of adsorption distribution of the activator having the aforementioned structure, thereby forming a relatively sparse thin film. Furthermore, the growth rate of the formed thin film is significantly reduced. As a result, even when applied to substrates with complex structures, the uniformity of the thin film is ensured, the step coverage is greatly improved, and in particular, deposition is possible at a thin thickness. Moreover, it is possible to improve the amount of O, Si, metals, metal oxides, and even carbon residues that were previously difficult to reduce as process by-products.

[0207] [Formula 1]

[0208] TIFF0007955380000017.tif10135

[0209] (In the above formula, DR (Deposition rate, Å / cycle) is the rate at which the thin film is deposited. When a thin film formed by a precursor and reactants is deposited, DR i (Initial deposition rate) is the deposition rate of a thin film formed without the addition of a diffusion-improving agent. fThe (final deposition rate) is the deposition rate of the thin film formed by adding a diffusion-improving material during the process described above. Here, the deposition rate (DR) is measured using an ellipsometer for thin films with a thickness of 3-30 nm under normal temperature and pressure conditions, and its unit is Å / cycle.

[0210]

[0211] The thin film formation method described above allows the residual halogen intensity (c / s) within the thin film, measured based on SIMS and based on a film thickness of 100 Å, to be preferably 100,000 or less, more preferably 70,000 or less, even more preferably 50,000 or less, and even more preferably 10,000 or less. In a preferred embodiment, it may be 5,000 or less, more preferably 1,000 to 4,000, and even more preferably 1,000 to 3,800, and within this range, the effect of preventing corrosion and deterioration is outstanding.

[0212] In this description, the purging is preferably 1,000 to 50,000 sccm (Standard Cubic Centimeters per Minute), more preferably 2,000 to 30,000 sccm, and even more preferably 2,500 to 15,000 sccm. Within this range, the thin film growth rate per cycle is appropriately controlled, and deposition is performed as a single atomic layer (atomic mono-layer) or approximately thereof, which has the advantage of being advantageous in terms of film quality.

[0213]

[0214] The aforementioned ALD (atomic layer deposition process) is highly advantageous for the fabrication of integrated circuits (ICs) that require a high aspect ratio. In particular, its self-limiting thin film growth mechanism offers advantages such as excellent conformality, uniformity, and precise thickness control.

[0215] The aforementioned thin film formation method can be carried out, for example, at a deposition temperature in the range of 50 to 800°C, preferably in the range of 100 to 700°C, more preferably in the range of 200 to 650°C, and even more preferably in the range of 220 to 400°C. Within this range, it is possible to grow a thin film with excellent film quality while achieving the ALD process characteristics.

[0216] The aforementioned thin film formation method can be carried out, for example, at a deposition pressure in the range of 0.01 to 20 Torr, preferably in the range of 0.1 to 20 Torr, more preferably in the range of 0.1 to 10 Torr, and most preferably in the range of 0.3 to 7 Torr. Within this range, a thin film with a uniform thickness can be obtained.

[0217] In this description, the deposition temperature and deposition pressure may be measured as the temperature and pressure formed within the deposition chamber, or as the temperature and pressure applied to the substrate within the deposition chamber.

[0218] The thin film formation method may preferably include the steps of raising the temperature inside the chamber to the deposition temperature before introducing the thin film modification composition into the chamber, and / or purging the chamber by injecting an inert gas before introducing the thin film modification composition into the chamber.

[0219] Furthermore, the present invention may include a thin film manufacturing apparatus capable of realizing the thin film manufacturing method, comprising: an ALD chamber; a first vaporizer for vaporizing a thin film modification composition; a first transport means for transporting the vaporized thin film modification composition into the ALD chamber; a second vaporizer for vaporizing a thin film precursor; and a second transport means for transporting the vaporized thin film precursor into the ALD chamber. Here, the vaporizer and transport means are not particularly limited as long as they are vaporizers and transport means commonly used in the art to which the present invention belongs.

[0220] The first vaporizer for vaporizing the thin film modification composition may be configured as at least two separate vaporizers, such as a vaporizer for vaporizing a shielding substance and a vaporizer for vaporizing a diffusion-improving substance, as needed.

[0221] As a specific example, the thin film formation method described above is first positioned in a deposition chamber capable of depositing atomic layers, on which a substrate on which a thin film is to be formed is placed.

[0222] Examples of the aforementioned substrates include semiconductor substrates such as silicon substrates and silicon oxide.

[0223] The substrate may have a conductive layer or an insulating layer further formed on its upper surface.

[0224] To deposit a thin film onto a substrate located in the aforementioned deposition chamber, the thin film modification composition described above and a precursor compound or a mixture thereof with a nonpolar solvent are prepared.

[0225] Subsequently, the prepared thin-film modification composition (e.g., a shielding substance) is injected into the vaporizer, converted into a vapor phase, and transferred to the deposition chamber where it is adsorbed onto the substrate. The unadsorbed thin-film modification composition is then removed by purging.

[0226] Next, the prepared precursor compound or a mixture thereof with a nonpolar solvent (a composition for thin film formation) is injected into the vaporizer, converted into a vapor phase, and transferred to the deposition chamber where it is adsorbed onto the substrate. This is then shielded by a pre-injected shielding material, and any unadsorbed precursor compound or mixture thereof with a nonpolar solvent is purged.

[0227] In this description, as a method for transferring the thin film modification composition and precursor compound (composition for thin film formation) to the deposition chamber, one example is to use a method that utilizes a gas flow control (MFC: Mass Flow Controller) to transport volatile gas (VFC: Vapor Flow Control), or a method that utilizes a liquid flow control (LMFC: Liquid Mass Flow Controller) to transport liquid (LDS: Liquid Delivery System), and preferably the LDS method is used.

[0228] In this case, one or more gases selected from the group consisting of argon (Ar), nitrogen (N2), and helium (He) can be used as the carrier gas or diluent gas for moving the thin film modification composition and precursor compounds onto the substrate, but are not limited to these.

[0229] In this description, an inert gas can be used as the purge gas, and preferably the carrier gas or diluent gas can be used.

[0230]

[0231] Next, a reaction gas is supplied. The reaction gas is not particularly limited, and may preferably contain a nitride agent, as long as it is a reaction gas commonly used in the art to which the present invention belongs. The nitride agent reacts with the precursor compound adsorbed on the substrate to form a nitride film.

[0232] Preferably, the nitriding agent may be nitrogen gas (N2), hydrazine gas (N2H4), or a mixture of nitrogen gas and hydrogen gas.

[0233] Next, an inert gas is used to purge any unreacted residual reaction gas. This removes not only excess reaction gas but also any by-products that have been generated.

[0234] As described above, the thin film formation method, as an example, can be performed as a unit cycle comprising the steps of supplying a shielding material onto a substrate, purging unadsorbed shielding material, adsorbing a precursor compound / thin film formation composition onto the substrate, purging unadsorbed precursor compound, adsorbing a diffusion improving material onto the substrate, purging unadsorbed diffusion improving material, supplying a reaction gas, and purging residual reaction gas. This unit cycle can be repeated to form a thin film of a desired thickness.

[0235] The aforementioned unit cycle can be repeated, for example, 1 to 99,999 times, preferably 10 to 1,000 times, more preferably 50 to 5,000 times, and even more preferably 100 to 2,000 times, and within this range, the desired thin film characteristics are well expressed.

[0236]

[0237] The present invention also provides a semiconductor substrate, characterized in that the semiconductor substrate is manufactured by the thin film formation method described herein, and in this case, the step coverage and uniformity of the thin film thickness are significantly superior, and the density and electrical properties of the thin film are also excellent.

[0238]

[0239] Preferably, the manufactured thin film has a thickness of 20 nm or less, a resistivity of 50 to 400 μΩ·cm based on a thin film thickness of 10 nm, a halogen content of 10,000 ppm or less, and a step coverage rate of 90% or more. Within this range, it exhibits excellent performance as a diffusion-blocking film and has the effect of reducing corrosion of metal wiring materials, but is not limited to this.

[0240] As an example, the thin film may have a thickness of 0.1 to 20 nm, preferably 1 to 20 nm, more preferably 3 to 25 nm, and even more preferably 5 to 20 nm, and within this range, there is an effect of excellent thin film properties.

[0241] As an example, the thin film may have a specific resistance value of 0.1 to 400 μΩ·cm, preferably 15 to 300 μΩ·cm, more preferably 20 to 290 μΩ·cm, and even more preferably 25 to 280 μΩ·cm, based on a thin film thickness of 10 nm, and within this range, there is an effect of excellent thin film properties.

[0242] The thin film may have a halogen content of preferably 10,000 ppm or less or 1 to 9,000 ppm, more preferably 5 to 8,500 ppm, and even more preferably 100 to 1,000 ppm, and within this range, there is an effect that the thin film growth rate is reduced while having excellent thin film properties. Here, the halogen remaining in the thin film may be, for example, Cl2, Cl, or Cl - and the lower the residual amount of halogen in the thin film, the better the film quality, which is preferable.

[0243] As an example, the thin film has step coverage of 90% or more, preferably 92% or more, more preferably 95% or more, and within this range, even if the thin film has a complex structure, it can be easily deposited on a substrate, and there is an advantage that it can be applied to next-generation semiconductor devices.

[0244] The manufactured thin film preferably has a thickness of 20 nm or less, a carbon, nitrogen, and halogen content of 10,000 ppm or less based on a thin film thickness of 10 nm, and a step coverage of 90% or more, and within this range, there is an effect of excellent performance as a dielectric film or a blocking film, but is not limited thereto.

[0245]

[0246] As an example, the thin film may have a two-layer or three-layer multilayer structure, preferably a two-layer or three-layer multilayer structure, as necessary. As a specific example, the multilayer film having a two-layer structure may have a structure of a lower film - an intermediate film, and as a specific example, the multilayer film having a three-layer structure may have a structure of a lower film - an intermediate film - an upper film.

[0247] As an example, the lower film may comprise at least one selected from the group consisting of Si, SiO2, MgO, Al2O3, CaO, ZrSiO4, ZrO2, HfSiO4, Y2O3, HfO2, LaLuO2, Si3N4, SrO, La2O3, Ta2O5, BaO, and TiO2.

[0248] As an example, the intermediate film is Ti x N y , preferably comprising TN.

[0249] As an example, the upper film may comprise at least one selected from the group consisting of W and Mo.

[0250]

[0251] Hereinafter, preferred embodiments and drawings are presented to help understand the present invention. However, the following embodiments and drawings are merely illustrative of the present invention, and various changes and modifications may be made within the scope and spirit of the present invention. It will be apparent to those skilled in the art that such variations and modifications naturally fall within the scope of the appended claims.

[0252]

[0253] [Example]

[0254] Examples 1-3, Comparative Examples 1-2

[0255] Using the components shown in Table 1 below, an ALD deposition process was performed according to Figure 1 below.

[0256] FIG. 1 is a diagram schematically illustrating a deposition process sequence according to the present invention, focusing on one cycle.

[0257] Specifically, a compound represented by the following Chemical Formula 2-1 was prepared as a shielding material, and a compound represented by the following Chemical Formula 4-1, a compound represented by the following Chemical Formula 4-2, and a compound represented by the following Chemical Formula 4-3 were prepared as diffusion improving materials, respectively.

[0258] [Chemical Formula 2-1]

[0259] [Chemical Formula]

[0260] [Chemical Formula 4-1]

[0261] [Chemical Formula]

[0262] [Chemical Formula 4-2]

[0263] [Chemical Formula]

[0264] [Chemical Formula 4-3]

[0265] [Chemical Formula]

[0266] As a thin film modifying composition, 90 parts by weight of the compound represented by Chemical Formula 2-1 and 10 parts by weight of the compound represented by Chemical Formula 4-1 were mixed, and shown as Composition 1 in Table 1 below.

[0267] As a thin film modifying composition, 90 parts by weight of the compound represented by Chemical Formula 2-1 and 10 parts by weight of the compound represented by Chemical Formula 4-2 were mixed, and shown as Composition 2 in Table 1 below.

[0268] As a thin-film modification composition, 80 parts by weight of the compound represented by 2-1 and 20 parts by weight of the compound represented by chemical formula 4-3 were mixed and are shown as composition 3 in Table 1 below.

[0269]

[0270] In addition, trimethylaluminum (indicated as "TMA" in the table below) was prepared as a precursor.

[0271] As shown in Figure 1 below, the prepared thin-film modification composition, or shielding or diffusion-improving material, was placed in a canister and supplied at room temperature to a vaporizer heated to 150°C at a flow rate of 0.05 g / min using a Liquid Mass Flow Controller (LMFC). The shielding material vaporized into the vapor phase in the vaporizer was introduced into a deposition chamber with a substrate loaded for 1 second, and then an argon purge was performed by supplying argon gas at 5000 sccm for 2 seconds. At this time, the pressure in the reaction chamber was controlled to 2.5 Torr.

[0272] Next, the precursor was placed in a canister and introduced into the deposition chamber using a vapor flow controller (VFC) as shown in Table 1. After that, argon gas was supplied at 5000 sccm for 2 seconds to perform an argon purge. At this time, the pressure inside the reaction chamber was controlled to 2.5 Torr.

[0273] Next, 1000 sccm of ozone was introduced into the reaction chamber as a reactive gas for 3 seconds, followed by argon purging for 3 seconds. At this time, the substrate on which the metal thin film was to be formed was heated under the temperature conditions shown in Table 1 below.

[0274] This process was repeated 200 to 400 times to form a self-limiting atomic layer thin film with a thickness of 10 nm.

[0275] For each of the thin films obtained in Examples 1-3 and Comparative Examples 1-2, the deposition rate reduction rate (D / R reduction rate), secondary ion mass spectrometry (SIMS) C impurities, and step coverage rate were measured using the following method.

[0276] * The reduction rate of deposition rate (D / R (dep.rate) reduction rate) refers to the ratio of the reduction in deposition rate after the introduction of the thin film modification composition compared to the D / R before the introduction of the thin film modification composition, and was calculated as a percentage using the measured Å / cycle values.

[0277] Specifically, the film thickness of the manufactured thin film was measured using an ellipsometer, a device capable of measuring optical properties such as film thickness and refractive index using the polarization characteristics of light. This measurement was divided by the number of cycles to calculate the film thickness deposited per cycle, and the rate of decrease in the thin film growth rate was then calculated. Specifically, the calculation was performed using Equation 1 below.

[0278] [Formula 1]

[0279] TIFF0007955380000022.tif11135

[0280] (In the above formula, DR (Deposition rate, Å / cycle) is the rate at which the thin film is deposited. When a thin film formed by a precursor and reactants is deposited, DR i (Initial deposition rate) is the deposition rate of a thin film formed without the addition of a diffusion-improving agent. f The (final deposition rate) is the deposition rate of the thin film formed by adding a diffusion-improving material during the process described above. Here, the deposition rate (DR) is measured using an ellipsometer for thin films with a thickness of 3-30 nm under normal temperature and pressure conditions, and its unit is Å / cycle.

[0281] *The degree of non-uniformity was calculated by selecting the maximum and minimum film thicknesses from the thin films measured using the ellipsometer device, and using the following formula 2. The results are shown in Table 1 and Figure 2 below. Specifically, the film thickness was measured at four locations on the east, west, north, and south edges of a 300 mm wafer, and at one location in the central part.

[0282] [Formula 2]

[0283] TIFF0007955380000023.tif9147

[0284] * SIMS (Secondary-ion mass spectrometry) C impurities: While ion sputtering to engrave a thin film axially, the C impurity content (counts) in the surface layer of the substrate was considered when the sputtering time for minimal contamination was 50 seconds, and the C impurity value in the SIMS graph was confirmed.

[0285] * Step Coverage (%): Thin films deposited on substrates with a complex structure and aspect ratio of 22:1 according to Examples 1-3 and Comparative Examples 1-2 were horizontally cut at a position of 100 nm from the top to the bottom (left figure) and a position of 100 nm from the bottom to the top (right figure). These samples were measured using a transmission electron microscope (TEM), and the step coverage (%) was calculated according to the following formula 3.

[0286] [Formula 3]

[0287] TIFF0007955380000024.tif10164

[0288] Specifically, a deposition process was carried out on a substrate with a complex structure having an aspect ratio of 22:1, with an upper diameter of 90 nm, a lower diameter of 65 nm, and a via hole depth of approximately 2000 nm, under conditions of applying a diffusion-improving material. To confirm the uniformity of the thickness and step coverage of the deposited material inside the vertically formed via holes, specimens were prepared by horizontally cutting them at positions 100 nm from the top to the bottom and 100 nm from the bottom to the top. These specimens were measured using a transmission electron microscope (TEM), and the results are shown in Table 1 and Figures 3 to 5 below.

[0289] [Table 1]

[0290] As shown in Table 1 above, in Examples 1 to 3, which used the thin film modification composition according to the present invention, it was confirmed that the reduction rate of the deposition rate and the uniformity were significantly improved compared to Comparative Example 1, which did not use the composition. Furthermore, in Examples 1 to 3, which used the thin film modification composition according to the present invention, it was confirmed that the reduction rate of the deposition rate was equivalent to or similar to that of Comparative Example 2, which used another type that was not considered a suitable type, while the uniformity was superior.

[0291] In particular, in Examples 1 to 3, which used the thin-film modification composition according to the present invention, it was confirmed that the uniformity was 20% or more better than in Comparative Example 1, which did not use this composition, and in Comparative Example 2, which used a shielding material alone (see Figure 2 below).

[0292] Furthermore, as shown in Figures 3 to 5 below, in Examples 1 to 3 using the thin-film modification composition according to the present invention, the step coverage was 99.1 to 100.2%, which was significantly improved compared to Comparative Example 1, which did not use the composition and had a step coverage of 95.0%.

Claims

1. It comprises 50 to 99 parts by weight of a shielding material having one or more lone pairs of electrons selected from oxygen (O), sulfur (S), and phosphorus (P), and 1 to 50 parts by weight of a diffusion improving material. The diffusion-improving material has a boiling point in the range of 5 to 200°C. The aforementioned shielding material is a substance that contributes to improving the crystallinity of the thin film while shielding against the adsorption of precursor compounds onto the substrate surface. The shielding material is a compound represented by the following chemical formulas 1 to 2, and the shielding material includes one or more compounds selected from the compounds represented by the following chemical formulas 1-1 to 1-4 and 2-1 to 2-4. The precursor compound is characterized by containing one or more elements selected from the group consisting of Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce, and Nd as a central metal, in a thin film modification composition. [Chemical formula 1] 【Chemistry 1】 [Chemical formula 2] 【Chemistry 2】 (In the above chemical formulas 1 to 2, R' and R'' are each independently hydrogen, a C1-C5 alkyl group, a C1-C5 alkene group, or a C1-C5 alkoxy group, The above A is oxygen (O), sulfur (S), phosphorus (P), nitrogen (N), -CH, or -CH2, The aforementioned B is -OH, -OCH3, -OCH2CH3, -CH2CH3, -SH, -SCH3, or -SCH2CH3, m is an integer between 0 and 3. [Chemical formulas 1-1 to 1-4] 【Transformation 3】 [Chemical formulas 2-1 to 2-4] 【Chemistry 4】

2. The thin film modification composition according to claim 1, characterized in that the diffusion improving substance is one or more selected from octane, diethyl ether, methylene chloride, toluene, hexane, and ethanol.

3. The process includes the steps of: injecting a thin film modification composition into a chamber to shield the loaded substrate surface; and injecting a precursor compound into the chamber and depositing it to form a thin film. The thin film modification composition comprises 50 to 99 parts by weight of a shielding material having one or more lone pairs of electrons selected from oxygen (O), sulfur (S), and phosphorus (P), and 1 to 50 parts by weight of a diffusion improving material. The shielding material is a substance that contributes to improving the crystallinity of the thin film while shielding the adsorption of the precursor compound onto the substrate surface. The shielding material is a compound represented by the following chemical formulas 1 to 2, and the shielding material includes one or more compounds selected from the compounds represented by the following chemical formulas 1-1 to 1-4 and 2-1 to 2-4. The diffusion-improving material has a boiling point in the range of 5 to 200°C. The precursor compound contains one or more elements selected from the group consisting of Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce, and Nd as a central metal. The substrate loaded into the chamber is heated to 100-800°C. The supply time (seconds) of the thin film modification composition to the substrate surface is 0.01 to 10 seconds per cycle, and the supply time of the precursor compound is based on a flow rate of 0.1 to 500 mg / cycle per chamber volume of 15 to 20 L. The ratio of the injection amounts (mg / cycle) of the thin-film modification composition to the precursor compound injected into the chamber is 1:1 to 1:

20. A method for forming a thin film, characterized in that the deposition is carried out at a deposition pressure in the range of 0.01 to 20 Torr and a deposition temperature in the range of 50 to 800°C. [Chemical formula 1] 【Transformation 5】 [Chemical formula 2] 【Transformation 6】 (In the above chemical formulas 1 to 2, R' and R'' are each independently hydrogen, a C1-C5 alkyl group, a C1-C5 alkene group, or a C1-C5 alkoxy group, The above A is oxygen (O), sulfur (S), phosphorus (P), nitrogen (N), -CH, or -CH2, The aforementioned B is -OH, -OCH3, -OCH2CH3, -CH2CH3, -SH, -SCH3, or -SCH2CH3, m is an integer between 0 and 3. [Chemical formulas 1-1 to 1-4] 【Transformation 7】 [Chemical formulas 2-1 to 2-4] 【Transformation 8】

4. The thin film formation method according to claim 3, characterized in that the chamber is an atomic layer deposition (ALD) chamber, a chemical vapor deposition (CVD) chamber, a plasma-enhanced atomic layer deposition (PEALD) chamber, or a plasma-enhanced chemical vapor deposition (PECVD) chamber.

5. The thin film forming method according to claim 3, characterized in that the thin film modification composition is transported into the chamber by a VFC (vapor flow control) method, a DLI (direct liquid introduction) method, or an LDS (liquid delivery system) method, and the thin film is a silicon nitride film, a silicon oxide film, a titanium nitride film, a titanium oxide film, a tungsten nitride film, a molybdenum nitride film, a hafnium oxide film, a zirconium oxide film, a tungsten oxide film, or an aluminum oxide film.

Citation Information

Patent Citations

  • Composition for Forming Thin Film and Method for Forming Thin Film Using The same

    KR1020190036794A

  • Method of depositing thin films using protective material

    KR1020210059332A