Filtration laminate and method for manufacturing a filtration laminate
The laminate of spunbond and meltblown nonwoven fabrics with controlled embossing addresses filtration and water pressure resistance issues, enhancing performance and durability for filtration applications.
Patent Information
- Application Number
- JP2024567716
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-12-28
- Filing Date
- 2023-12-21
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-12-21
AI Technical Summary
Existing nonwoven fabric laminates, such as those described in Patent Document 1, do not adequately address filtration performance and water pressure resistance, limiting their use in applications requiring these properties.
A filtration laminate is created by laminating spunbond and meltblown nonwoven fabric layers with specific fiber diameters and embossing fusion rates, using thermoplastic resins like propylene homopolymers, and employing controlled embossing conditions to enhance filtration performance and water pressure resistance.
The resulting laminate exhibits excellent filtration performance and water pressure durability, suitable for applications involving liquid and gas filtration.
Smart Images

Figure 0007955389000005 
Figure 0007955389000006 
Figure 0007955389000007
Abstract
Description
[Technical Field]
[0001] This disclosure relates to a filtration laminate and a method for manufacturing a filtration laminate. [Background technology]
[0002] In recent years, nonwoven fabrics made from thermoplastic resin fibers have been widely used in various applications due to their excellent breathability, flexibility, and lightweight properties. Therefore, nonwoven fabrics require various properties tailored to their specific applications, and there is a growing demand for improvements in these properties.
[0003] For example, nonwoven fabrics made of thermoplastic resin fibers are used as adhesive sheet substrates for bandages, surgical tapes, and other medical adhesive materials. For example, Patent Document 1 describes a laminated nonwoven fabric consisting of one or more layers each of a surface layer, an intermediate layer, and a back layer, which are integrated by heat bonding, wherein the nonwoven fabric of the surface layer is made of thermoplastic synthetic long fibers obtained by the spunbond method with a fiber diameter of 30 μm or less, the nonwoven fabric of the intermediate layer is made of meltblown fibers with a fiber diameter of 10 μm or less, and the nonwoven fabric of the back layer is made of thermoplastic synthetic long fibers with a fiber diameter of 10 μm or more and 30 μm or less, and has a basis weight of 3 g / m². 2 A medical adhesive tape base material characterized by having the above features has been proposed. [Patent Document 1] Patent No. 4799097 [Overview of the Initiative] [Problems that the invention aims to solve]
[0004] Patent Document 1 discloses a nonwoven fabric laminate formed by heat-sealing a spunbond nonwoven fabric and a meltblown nonwoven fabric together, and describes its use as an adhesive sheet base material for bandages, surgical tapes, and other medical adhesive materials. However, Patent Document 1 does not describe the use of a laminate comprising spunbond nonwoven fabric and meltblown nonwoven fabric for filtration, nor does it describe a laminate having a configuration suitable for filtration due to its excellent filter performance and water pressure resistance.
[0005] This disclosure has been made in view of the above, and aims to provide a filtration laminate that is excellent in filter performance and water pressure resistance, and a method for manufacturing a filtration laminate that is capable of producing a filtration laminate that is excellent in filter performance and water pressure resistance. [Means for solving the problem]
[0006] The following embodiments are included as means to solve the above problems. <1> A spunbond nonwoven fabric layer containing spunbond nonwoven fabric, A meltblown nonwoven fabric layer containing a meltblown nonwoven fabric, The average fiber diameter of the fibers contained in the meltblown nonwoven fabric is 1.0 μm or less. An embossed filtration laminate. <2> The embossing fusion rate is less than 100%. <1> The filtration laminate described above. <3> The embossing fusion rate is between 60% and 90%. <1> The filtration laminate described above. <4> The spunbond nonwoven fabric and the meltblown nonwoven fabric each independently contain an olefin polymer. <1> ~ <3> A filtration laminate as described in any one of the following. <5> The spunbond nonwoven fabric and the meltblown nonwoven fabric each independently contain a propylene homopolymer. <1> ~ <3> A filtration laminate as described in any one of the following. <6> The average fiber diameter of the fibers contained in the spunbond nonwoven fabric is 15 μm to 40 μm, and the basis weight of the spunbond nonwoven fabric layer is 10 g / m². 2 ~40g / m 2 That is <1> ~ <5> A filtration laminate as described in any one of the following. <7> The tensile strength is 10 N / 25 mm or more. <1> ~ <6> A filtration laminate as described in any one of the following. <8> The spunbond nonwoven fabric layer is laminated on both sides of the meltblown nonwoven fabric layer. <1> ~ <7> A filtration laminate as described in any one of the following. <9> A step of melt-spinning a first thermoplastic resin or a first resin composition containing the first thermoplastic resin by a spunbond method, and depositing the fibers obtained by melt-spinning onto a moving collection surface to obtain a first spunbond nonwoven fabric layer containing a spunbond nonwoven fabric, A step of obtaining a meltblown nonwoven fabric layer containing a meltblown nonwoven fabric by depositing fibers obtained by the meltblown method onto a moving collection surface using a second thermoplastic resin or a second resin composition containing the second thermoplastic resin, A step of heat-sealing the first spunbond nonwoven fabric layer and the meltblown nonwoven fabric layer by embossing, Includes, A method for manufacturing a laminate for filtration, wherein in the heat-sealing step, the embossing temperature is less than 130°C and the embossing linear pressure is 10.0 kgf / cm or less. <10> The embossing temperature is 100°C or higher. <9> A method for manufacturing a filtration laminate as described above. <11> A step of melt-spinning a third thermoplastic resin or a third resin composition containing the third thermoplastic resin by a spunbond method, and depositing the fibers obtained by melt-spinning onto a moving collection surface to obtain a spunbond nonwoven fabric layer containing a second spunbond nonwoven fabric, The process involves heat-sealing the first spunbond nonwoven fabric layer, the meltblown nonwoven fabric layer, and the second spunbond nonwoven fabric layer in this order by embossing, including <9> or <10> A method for manufacturing a filtration laminate as described above. <12> In the heat-sealing process, the embossing speed is 15 m / min or more. <9> ~ <11> A method for manufacturing a filtration laminate as described in any one of the following. <13> The embossing fusion rate of the aforementioned filtration laminate is less than 100%. <9> ~ <12> A method for manufacturing a filtration laminate as described in any one of the following. <14> The embossing fusion rate of the aforementioned filtration laminate is 60% or more and 90% or less. <9> ~ <12> A method for manufacturing a filtration laminate as described in any one of the following. [Effects of the Invention]
[0007] According to the present disclosure, it is possible to provide a filtration laminate having excellent filtration performance and water pressure durability, and a method for producing a filtration laminate capable of producing the filtration laminate having excellent filtration performance and water pressure durability. [Brief Description of Drawings]
[0008] [Figure 1] It is a figure which shows an example of the manufacturing method of a spunbond nonwoven fabric. [Figure 2] It is a figure which shows an example of the manufacturing method of a meltblown nonwoven fabric. [Figure 3] It is the image of the embossed part of Experimental Examples 1 and 9 to 11. [Figure 4] It is the image of the embossed part of Experimental Examples 12 to 15. [Figure 5] It is the image of the embossed part of Experimental Examples 16 to 19. [Figure 6] It is the image of the embossed part of Experimental Examples 20 to 23. [Figure 7] It is the image of the embossed part of Experimental Examples 24 to 27. [Figure 8] It is the image of the embossed part of Experimental Examples 28 to 31. [Figure 9] It is the image of the embossed part of Experimental Examples 32 and 33. [Modes for Carrying Out the Invention]
[0009] In the present disclosure, numerical ranges indicated using "to" indicate ranges including the numerical values described before and after "to" as the minimum and maximum values, respectively. In the numerical ranges described stepwise in the present specification, the upper limit value or lower limit value described in a certain numerical range may be replaced with the upper limit value or lower limit value of another stepwise numerical range. In addition, in the numerical ranges described in the present specification, the upper limit value or lower limit value described in a certain numerical range may be replaced with the values shown in Examples. In the present disclosure, the amount of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified, when a plurality of substances corresponding to each component are present in the composition. In this disclosure, a combination of two or more preferred embodiments is a more preferred embodiment.
[0010] <Filtration laminate> The filtration laminate of this disclosure comprises a spunbond nonwoven fabric layer containing a spunbond nonwoven fabric and a meltblown nonwoven fabric layer containing a meltblown nonwoven fabric, wherein the average fiber diameter of the fibers contained in the meltblown nonwoven fabric is 1.0 μm or less, and the laminate is embossed.
[0011] In the filtration laminate of this disclosure, a spunbond nonwoven fabric layer and a meltblown nonwoven fabric layer containing a meltblown nonwoven fabric with an average fiber diameter of 1.0 μm or less are bonded together by embossing. As a result, the filtration laminate has excellent filter performance and water pressure resistance.
[0012] Filtration laminates are used, for example, to remove solids from liquids, gases, etc.
[0013] [Spunbond nonwoven fabric layer] The filtration laminate of this disclosure comprises a spunbond nonwoven fabric layer including a spunbond nonwoven fabric. The filtration laminate may comprise one spunbond nonwoven fabric layer or two or more spunbond nonwoven fabric layers. When comprising one spunbond nonwoven fabric layer, it is preferable that the spunbond nonwoven fabric layer is provided downstream of the meltblown nonwoven fabric layer in the filtration direction, from the viewpoint of preventing deformation of the meltblown nonwoven fabric layer due to filtration pressure and improving water pressure resistance. When comprising two or more spunbond nonwoven fabric layers, it is preferable to provide one or more spunbond nonwoven fabric layers on each side of the meltblown nonwoven fabric layer, from the viewpoint of preventing the embossing roll from directly contacting the meltblown nonwoven fabric layer during the embossing process described later. This prevents porosity due to thermal damage to the meltblown fibers and improves water pressure resistance. It also prevents clogging of the meltblown nonwoven fabric layer in the non-embossed portion, described later, and ensures the liquid flow rate during filtration.
[0014] The fibers contained in the spunbond nonwoven fabric preferably contain a thermoplastic resin. Examples of thermoplastic resins are not particularly limited and include olefin-based polymers which are homopolymers or copolymers of olefins such as ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, and 4-methyl-1-hexene; polyesters such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polyamides such as nylon-6, nylon-66, and polymetaxylene adipamide; polyvinyl chloride; polyimide; ethylene-vinyl acetate copolymer; polyacrylonitrile; polycarbonate; polystyrene; and ionomers. The thermoplastic resin may consist of one type or a mixture of two or more types.
[0015] Spunbond nonwoven fabrics preferably contain olefin polymers. Examples of olefin polymers include ethylene polymers such as ethylene-propylene random copolymers, high-pressure low-density polyethylene, linear low-density polyethylene (LLDPE), high-density polyethylene, and ethylene-1-butene random copolymers; propylene polymers such as polypropylene (propylene homopolymer), propylene-ethylene random copolymers, and propylene-1-butene random copolymers; and poly-1-butene and poly-4-methyl-1-pentene. Thermoplastic resins preferably contain propylene polymers from the viewpoint of excellent spinnability and stretchability.
[0016] Examples of propylene polymers include propylene homopolymers and propylene random copolymers, which are copolymers of propylene as the main component and one or more olefins as minor components. Among these, propylene homopolymers are preferred from the viewpoint of tensile strength and hydrostatic resistance. In propylene random copolymers, the content of constituent units derived from olefins is preferably 1 mol% to 10 mol% of the total, and more preferably 1 mol% to 6 mol% of the total.
[0017] For copolymerization of propylene random copolymers, ethylene or α-olefins having 4 or more carbon atoms are preferred, and ethylene or α-olefins having 4 to 8 carbon atoms are more preferred. Specifically, preferred α-olefins include 1-butene, 1-pentene, 1-hexene, 1-octene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, and 4-methyl-1-hexene.
[0018] The melting point (Tm) of the propylene polymer is not particularly limited and may be, for example, 125°C or higher, or 125°C to 165°C.
[0019] In this disclosure, the melting point can be measured using differential scanning calorimetry (DSC) as follows. Using a differential scanning calorimeter (DSC) such as the PerkinElmer DSC Pyris1 or the SII Nanotechnology DSC7020, the sample (approximately 5 mg) is heated under a nitrogen atmosphere (20 mL / min) to the target temperature set for each thermoplastic resin (230°C for propylene polymers), held at that temperature for 3 minutes, then cooled to 30°C at 10°C / min and held at 30°C for 1 minute, before being heated back up to the target temperature at 10°C / min. The melting point (Tm) is calculated from the peak of the crystal melting peak observed during the heating process. If multiple crystal melting peaks are observed, the peak on the higher temperature side is considered the melting point (Tm).
[0020] When a propylene-olefin random copolymer is used as the propylene polymer, its melting point (Tm) is preferably 153°C or lower, and more preferably 125°C to 150°C. When a propylene homopolymer is used as the propylene polymer, its melting point (Tm) is preferably 155°C or higher, and more preferably 157°C to 165°C.
[0021] The melt flow rate (MFR) (ASTM D-1238, 230°C, load 2160g) of the propylene polymer is not particularly limited as long as it can be used to produce a nonwoven fabric. For example, it is preferably 10g / 10min to 100g / 10min, and more preferably 20g / 10min to 70g / 10min. When a propylene polymer with an MFR of 10g / 10min or higher is used, the melt viscosity tends to be low and spinnability tends to be improved. On the other hand, when a propylene polymer with an MFR of 100g / 10min or lower is used, the tensile strength of the resulting nonwoven fabric tends to be improved.
[0022] Propylene polymers are typically obtained by slurry polymerization, gas-phase polymerization, or bulk polymerization, using a Ziegler-Natta type catalyst that combines a so-called titanium-containing solid transition metal component with an organometallic component, or a metallocene catalyst consisting of a transition metal compound from Group 4 to 6 of the periodic table having at least one cyclopentadienyl skeleton and a co-catalyst component, to homopolymerize propylene or copolymerize propylene with a small amount of α-olefin.
[0023] The content of thermoplastic resin (preferably an olefin polymer, more preferably a propylene homopolymer) in the spunbond nonwoven fabric may be 50% by mass or more, 70% by mass or more, 90% by mass or more, or 95% by mass or more, based on the total amount of the spunbond nonwoven fabric. The content of thermoplastic resin (preferably an olefin polymer, more preferably a propylene homopolymer) in the spunbond nonwoven fabric may be 100% by mass or less, or 99% by mass or less, based on the total amount of the spunbond nonwoven fabric.
[0024] The average fiber diameter of the fibers contained in the spunbond nonwoven fabric is not particularly limited, and is preferably 15 μm to 40 μm, more preferably 15 μm to 30 μm, and even more preferably 15 μm to 20 μm, from the viewpoints of lightness and tensile strength. When the average fiber diameter is 30 μm or less, the structure of the spunbond nonwoven fabric becomes dense, which is advantageous from the viewpoint of water pressure durability. When the average fiber diameter is 15 μm or more, the liquid permeation resistance is reduced, which is advantageous from the viewpoint of filtration rate.
[0025] In the present disclosure, the average fiber diameter of fibers can be determined as follows. The nonwoven fabric to be measured is observed with an optical microscope (for example, ECLIPSE E-400 manufactured by Nikon Corporation), 100 fibers are selected from the fibers forming the nonwoven fabric on the screen, the fiber diameters thereof are measured, and the average value thereof is taken as the average fiber diameter of the fibers.
[0026] The basis weight of the spunbond nonwoven fabric layer is 10 g / m 2 to 40 g / m 2 . The basis weight of the spunbond nonwoven fabric layer is, from the viewpoint of tensile strength, preferably 12 g / m 2 or more, more preferably 15 g / m 2 or more. The basis weight of the spunbond nonwoven fabric layer is, from the viewpoint of weight reduction, preferably 30 g / m 2 or less, more preferably 20 g / m 2 or less. In the present disclosure, the basis weight of the nonwoven fabric layer means the basis weight of a single layer.
[0027] [Meltblown nonwoven fabric layer] The filtration laminate of this disclosure comprises a meltblown nonwoven fabric layer containing a meltblown nonwoven fabric. The average fiber diameter of the fibers contained in the meltblown nonwoven fabric is 1.0 μm or less. The filtration laminate may comprise one meltblown nonwoven fabric layer, or it may comprise two or more meltblown nonwoven fabric layers. If it comprises two or more meltblown nonwoven fabric layers, the two or more meltblown nonwoven fabric layers may be directly laminated, or other layers (e.g., spunbond nonwoven fabric layers) may be interposed between the meltblown nonwoven fabric layers.
[0028] The filtration laminate of this disclosure may include a meltblown nonwoven fabric layer having an average fiber diameter of 1.0 μm or less, as well as a meltblown nonwoven fabric layer having an average fiber diameter of more than 1.0 μm. Alternatively, the filtration laminate of this disclosure may not include a meltblown nonwoven fabric layer having an average fiber diameter of more than 1.0 μm. Hereinafter, meltblown nonwoven fabric layers with an average fiber diameter of 1.0 μm or less and meltblown nonwoven fabric layers with an average fiber diameter exceeding 1.0 μm will be collectively referred to as meltblown nonwoven fabric layers. Meltblown nonwoven fabric layers with an average fiber diameter of 1.0 μm or less will be referred to as specific meltblown nonwoven fabric layers.
[0029] In a filtration laminate, it is preferable that spunbond nonwoven fabric layers are laminated on both sides of a specific meltblown nonwoven fabric layer, and it is more preferable that the spunbond nonwoven fabric layer, the meltblown nonwoven fabric layer, and the spunbond nonwoven fabric layer are laminated in this order, forming a three-layer structure of SMS.
[0030] The fibers contained in the meltblown nonwoven fabric preferably contain a thermoplastic resin. The thermoplastic resin is not particularly limited and can have the same configuration as exemplified in the section on the spunbond nonwoven fabric layer described above.
[0031] Meltblown nonwoven fabrics preferably contain olefin polymers. Examples of olefin polymers include ethylene polymers such as ethylene-propylene random copolymers, high-pressure low-density polyethylene, linear low-density polyethylene (LLDPE), high-density polyethylene, and ethylene-1-butene random copolymers; propylene polymers such as polypropylene (propylene homopolymer), propylene-ethylene random copolymers, and propylene-1-butene random copolymers; and poly-1-butene and poly-4-methyl-1-pentene. Thermoplastic resins preferably contain propylene polymers from the viewpoint of excellent spinnability and stretchability.
[0032] Examples of propylene polymers include propylene homopolymers and propylene random copolymers, which are copolymers of propylene as the main component and one or more olefins as minor components. Among these, propylene homopolymers are preferred from the viewpoint of water pressure resistance. In propylene random copolymers, the content of constituent units derived from olefins is preferably 1 mol% to 10 mol%, and more preferably 1 mol% to 6 mol%.
[0033] For copolymerization of propylene random copolymers, ethylene or α-olefins having 4 or more carbon atoms are preferred, and ethylene or α-olefins having 4 to 8 carbon atoms are more preferred. Specifically, preferred α-olefins include 1-butene, 1-pentene, 1-hexene, 1-octene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, and 4-methyl-1-hexene.
[0034] When the meltblown nonwoven fabric contains a propylene-based polymer, the preferred conditions for the propylene-based polymer, such as its melting point, are the same as those described in the section on the spunbond nonwoven fabric layer.
[0035] The melt flow rate (MFR) (ASTM D-1238, 230°C, load 2160g) of the propylene polymer contained in the meltblown nonwoven fabric is not particularly limited as long as it is possible to manufacture the nonwoven fabric. For example, it is preferably 100g / 10min to 3000g / 10min, and more preferably 500g / 10min to 2000g / 10min. When a propylene polymer with an MFR of 100g / 10min or higher is used, the melt viscosity tends to be low and the fiber diameter can be made smaller. On the other hand, when a propylene polymer with an MFR of 3000g / 10min or lower is used, molding defects due to fusion of fibers during spinning tend to be suppressed.
[0036] The content of thermoplastic resin (preferably an olefin polymer, more preferably a propylene homopolymer) in the meltblown nonwoven fabric may be 50% by mass or more, 70% by mass or more, 90% by mass or more, or 95% by mass or more, based on the total amount of the meltblown nonwoven fabric. The content of thermoplastic resin (preferably an olefin polymer, more preferably a propylene homopolymer) in the meltblown nonwoven fabric may be 100% by mass or less, or 99% by mass or less, based on the total amount of the meltblown nonwoven fabric.
[0037] In a specific meltblown nonwoven fabric layer, the average fiber diameter of the fibers contained in the meltblown nonwoven fabric is not particularly limited as long as it is 1 μm or less. From the viewpoint of tensile strength and filter efficiency, it is preferably 0.1 μm to 1 μm, more preferably 0.2 μm to 0.9 μm, and even more preferably 0.4 μm to 0.8 μm. When the average fiber diameter is 1.0 μm or less, the structure of the meltblown nonwoven fabric becomes denser, and finer solid particles can be captured. When the average fiber diameter is 0.1 μm or more, the liquid flow resistance is reduced, which is advantageous from the viewpoint of filtration speed.
[0038] The basis weight of the meltblown nonwoven fabric layer is 10 g / m². 2 ~40g / m 2 Preferably, it is 10 g / m 2 ~20g / m 2It is more preferable that the basis weight of the meltblown nonwoven fabric be 12 g / m², from the viewpoint of tensile strength. 2 Preferably, it is 15 g / m 2 It is more preferable that the above conditions are met. The basis weight of the meltblown nonwoven fabric should be 30 g / m² from the viewpoint of weight reduction. 2 Preferably, it is 20 g / m 2 The following is more preferable:
[0039] Since the filtration laminate is embossed, it may have both embossed and non-embossed areas. The area ratio of the embossed area is preferably 10% to 20%, and more preferably 12% to 19%. An area ratio of 10% or more of the embossed area is advantageous in terms of tensile strength and water pressure resistance. An area ratio of 20% or less of the embossed area increases the area through which liquid can pass, which is advantageous in terms of filtration speed. The area ratio of the embossed portion is determined by taking a 10 mm x 10 mm test piece from the filtration laminate, observing the contact surface of the test piece with the embossing roll using an electron microscope (magnification: 100x), and defining it as the ratio of the area of the heat-pressed portion to the observed area of the filtration laminate. The area of the embossed portion is approximately the same as the area of the protrusions formed on the embossing roll, and the area of the region corresponding to the protrusions on the embossing roll is called the area of the embossed portion. Therefore, there may be areas in the embossed portion that are not embossed. The area ratio of the protrusions formed on the embossing roll that can form the embossed portion is also called the "embossed area ratio."
[0040] The total basis weight of the filtration laminate is 30 g / m². 2 ~100g / m 2 Preferably, it is 36 g / m 2 ~95g / m 2 It is more preferable that it be 40g / m 2 ~80g / m 2 It is even more preferable that this be the case.
[0041] The embossing fusion rate of the filtration laminate may be less than 100%, 60% to 90%, 60% to less than 90%, 70% to less than 90%, or 80% to less than 90%. The embossing fusion rate can be determined as follows: First, place the black drawing paper and the filter laminate on a table in that order. Next, select any part of the filter laminate and take a photograph from directly above using a digital camera, ensuring that at least 15 embossed fusion areas are visible without being cut off. Repeat the above photography operation, changing the position of the part being photographed, until at least 100 embossed fusion areas are visible without being cut off. Using the photographs of the embossed fused areas taken in this manner, count the number of embossed fused areas E1 and E2 as follows. E1: Total number of embossed fused areas that are not cut off in the image. E2: The number of areas within the embossed fused section that are not cut off, where the black drawing paper is obscured by unfused fibers. The embossing fusion rate (%) is calculated by rounding the value obtained using the following formula to the first decimal place. Embossing fusion rate (%) = [1 - (E2 / E1)] × 100
[0042] From the viewpoint of automatic handling in the filtration process, the tensile strength of the filtration laminate is preferably 10 N / 25 mm or more, more preferably 15 N / 25 mm or more, and even more preferably 18 N / 25 mm or more. There is no particular upper limit to the tensile strength of the filtration laminate, and it may be 30 N / 25 mm or less. The tensile strength of the filtration laminate can be measured by the method described in the examples below.
[0043] The filtration laminate of this disclosure may be laminated with materials such as knitted fabrics, woven fabrics, or nonwoven fabrics other than the aforementioned spunbond nonwoven fabrics or meltblown nonwoven fabrics (also referred to as other nonwoven fabrics), depending on the purpose. Other nonwoven fabrics are not particularly limited and include various known short-fiber nonwoven fabrics and long-fiber nonwoven fabrics (e.g., long-fiber cellulose nonwoven fabrics), such as wet-laid nonwoven fabrics, spunlace nonwoven fabrics, dry-laid nonwoven fabrics, dry-pulp nonwoven fabrics, airlaid nonwoven fabrics, waterjet nonwoven fabrics, flash-spun nonwoven fabrics, open-fiber nonwoven fabrics, and needle-punched nonwoven fabrics.
[0044] The filtration laminates of this disclosure may contain additives such as commonly used antioxidants, weather stabilizers, light stabilizers, antistatic agents, hydrophilic agents, antifogging agents, antiblocking agents, lubricants, nucleating agents, and pigments, to the extent that they do not impair the purpose of the present invention. For example, the spunbond nonwoven fabric layer and the meltblown nonwoven fabric layer may or may not independently contain additives. These additives may be incorporated as needed into thermoplastic resins that can be used when manufacturing spunbond nonwoven fabrics or meltblown nonwoven fabrics.
[0045] <Method for manufacturing a filter laminate> A method for manufacturing a filtration laminate according to the present disclosure includes the steps of melt-spinning a first thermoplastic resin or a first resin composition containing the first thermoplastic resin by a spunbond method, depositing the fibers obtained by melt-spinning onto a moving collection surface to obtain a spunbond nonwoven fabric layer containing a first spunbond nonwoven fabric, A step of obtaining a meltblown nonwoven fabric layer containing a meltblown nonwoven fabric by depositing fibers obtained by the meltblown method onto a moving collection surface using a second thermoplastic resin or a second resin composition containing the second thermoplastic resin, A step of heat-sealing the first spunbond nonwoven fabric and the meltblown nonwoven fabric by embossing, Includes, In the aforementioned heat-sealing process, the embossing temperature is less than 130°C, and the embossing linear pressure is 10.0 kgf / cm or less. These conditions prevent excessive heat transfer to the meltblown nonwoven fabric layer, and consequently, prevent punctures caused by thermal damage to the meltblown fibers, thereby improving water pressure resistance.
[0046] The aforementioned filtration laminate can be manufactured by the method for manufacturing the filtration laminate of this disclosure.
[0047] A preferred example of the first thermoplastic resin is the same as the thermoplastic resin described in the section on spunbond nonwoven fabrics above. A preferred example of the first resin composition is a resin composition containing the thermoplastic resin described in the section on spunbond nonwoven fabrics above and the additives described above.
[0048] A preferred example of the second thermoplastic resin is the same as the thermoplastic resin described in the section on meltblown nonwoven fabrics above. A preferred example of the second resin composition is a resin composition containing the thermoplastic resin described in the section on meltblown nonwoven fabrics above and the additives mentioned above.
[0049] The first spunbond nonwoven fabric layer and the second spunbond nonwoven fabric layer described later (hereinafter collectively referred to as "spunbond nonwoven fabric layers") can be manufactured by a closed-type spunbond process as shown in Japanese Patent Publication No. 60-155765, Japanese Patent No. 3442896, and Japanese Patent No. 3883818, etc.
[0050] Referring to Figure 1, an example of a method for manufacturing spunbond nonwoven fabric will be described. In the method for manufacturing spunbond nonwoven fabric, as an example, a manufacturing apparatus equipped with a spinning section 11 having a closed cooling chamber structure as shown in Figure 1 can be used. In one embodiment, the cooling chamber may be open.
[0051] The nonwoven fabric manufacturing apparatus comprises a spinning unit 11 for melt-spinning a molten first thermoplastic resin or first resin composition, and for cooling and stretching the melt-spun continuous fiber group 22; a movable collection member 51 for collecting the stretched continuous fiber group 22; and a suction unit 39 for efficiently collecting the continuous fiber group 22 on the movable collection member 51.
[0052] The spinning unit 11 includes an extruder 32 for extruding a first thermoplastic resin or a first resin composition, a spinneret 34 for discharging molten first thermoplastic resin or a first resin composition from a spinning nozzle, a cooling chamber 38C for cooling the continuous fiber group 22 discharged from the spinning nozzle of the spinneret 34, cooling air supply units 38A and 38B for supplying cooling air 36, and a stretching unit 38D for stretching the continuous fiber group 22.
[0053] In the spinning section 11, the first thermoplastic resin or the first resin composition is extruded and introduced into the spinneret 34. Next, the molten first thermoplastic resin or the first resin composition is discharged from the spinning nozzle of the spinneret 34 and melt-spun. The melting temperature of the first thermoplastic resin, etc., is not particularly limited as long as it is possible to melt the first thermoplastic resin, etc.
[0054] The melt-spun continuous fiber group 22 is introduced into the cooling chamber 38C. The continuous fiber group 22 is cooled by cooling air 36 supplied from either or both of the cooling air supply unit 38A and the cooling air supply unit 38B. The cooled continuous fiber group 22 is introduced into the stretching unit 38D located downstream of the cooling chamber 38C. The stretching unit 38D is provided in a narrow passage shape. As the velocity of the cooling air increases in the narrow passage, the continuous fiber group 22 introduced into the stretching unit 38D is stretched.
[0055] The stretched continuous fiber group 22 is collected by the movable collection member 51, and the nonwoven web 43 consisting of the collected continuous fiber group 22 corresponds to the spunbond nonwoven fabric layer before heat fusion.
[0056] The meltblown nonwoven fabric layer can be manufactured by a meltblown process using an ultrafine fiber nonwoven fabric manufacturing apparatus as shown in Japanese Patent No. 6339124, etc.
[0057] Referring to Figure 2, an example of a method for manufacturing meltblown nonwoven fabric will be described.
[0058] Figure 2 is a schematic diagram showing an example of the configuration of a meltblown nonwoven fabric manufacturing apparatus 10. As shown in Figure 2, the nonwoven fabric manufacturing apparatus 10 comprises an extruder 20, a die (spinning end cap) 23, and a movable collection member 51.
[0059] The extruder 20 includes a hopper 21 and a compression section 22. The extruder 20 melts the solid second thermoplastic resin or solid second resin composition that is fed into the hopper 21 in the compression section 22. The extruder 20 may be a single-screw extruder or a multi-screw extruder.
[0060] The die (spinning nozzle) 23 is positioned connected to the tip of the extruder 20. The die 23 has a plurality of spinning nozzles 24 and two gas nozzles 25.
[0061] Multiple spinning nozzles 24 are typically arranged in a row. Molten second thermoplastic resin or second resin composition P, transported from the extruder 20, is introduced into the spinning nozzles 24, and the second thermoplastic resin, etc., is extruded in fibrous form from the nozzle opening. The diameter of the spinning nozzles can be, for example, 0.05 mm to 0.80 mm. The melting temperature of the second thermoplastic resin, etc., can be adjusted by the set temperature of the die 23.
[0062] The two gas nozzles (air nozzles) 25 are positioned near the nozzle opening of the spinning nozzle 24, specifically on both sides of the row of spinning nozzles 24. The gas nozzles 25 inject heated gas (heated compressed gas) near the opening of the spinning nozzle 24. As shown in Figure 2, the gas nozzles 25 inject heated gas onto the second thermoplastic resin, etc., immediately after it is discharged from the opening of the spinning nozzle 24.
[0063] The heated gas supplied to the gas nozzle 25 is supplied from the gas heating device 50. The temperature of the heated gas can be adjusted by a heating temperature adjustment means (not shown) attached to the gas heating device 50.
[0064] The fibrous material obtained by stretching and thinning the second thermoplastic resin, etc., discharged from the opening of the spinning nozzle 24 with a heated gas is collected on the movable collection member 51. An air suction unit 44 is positioned on the back side of the collection surface of the movable collection member 51, and rollers (not shown) are positioned to support and transport the movable collection member 51. The air suction unit 44 is connected to a blower (not shown). A nonwoven web 41 made of fibrous material is collected on the movable collection member 51. The nonwoven web 41 corresponds to the meltblown nonwoven fabric layer before heat fusion.
[0065] In the manufacturing method of the present disclosure, the first spunbond nonwoven fabric layer and the meltblown nonwoven fabric layer obtained as described above are heat-fused by embossing. Nonwoven webs corresponding to the first spunbond nonwoven fabric layer and nonwoven webs corresponding to the meltblown nonwoven fabric may be collected on separate moving collection members, and then these nonwoven webs may be laminated and heat-fused. Alternatively, nonwoven webs corresponding to the first spunbond nonwoven fabric layer and nonwoven webs corresponding to the meltblown nonwoven fabric may be laminated sequentially on the same moving collection member, and then these nonwoven webs may be heat-fused.
[0066] In the manufacturing method of the present disclosure, a third thermoplastic resin or a third resin composition containing the third thermoplastic resin may be melt-spun by a spunbond method, and the fibers obtained by melt-spinning may be deposited on a moving collection surface to form a second spunbond nonwoven fabric layer containing a spunbond nonwoven fabric. The second spunbond nonwoven fabric layer may be made separately from the first spunbond nonwoven fabric layer and the meltblown nonwoven fabric layer, and then these layers may be laminated together, or the nonwoven fabric layers may be laminated by sequentially making nonwoven webs corresponding to each nonwoven fabric layer on the same moving collection member. This yields a laminate before heat fusion in which the first spunbond nonwoven fabric layer, the meltblown nonwoven fabric layer and the second spunbond nonwoven fabric layer are laminated in this order. This laminate may be heat-fused by embossing. This yields a filtration laminate in which spunbond nonwoven fabric layers are laminated on both sides of the meltblown nonwoven fabric layer. The method for melt spinning the third thermoplastic resin or the third resin composition by the spunbond method is the same as the method for melt spinning the first thermoplastic resin or the first resin composition by the spunbond method.
[0067] In the heat-sealing process, the embossing method is not particularly limited, as long as the embossing temperature is less than 130°C and the embossing linear pressure is 10.0 kgf / cm or less.
[0068] The embossing temperature does not need to be 130°C, and from the viewpoint of improving filter efficiency and water pressure resistance, it may be 128°C or lower, or even 126°C or lower. The embossing temperature may be 110°C or higher, or 120°C or higher, from the viewpoint of ensuring embossing strength and thereby improving water pressure resistance.
[0069] The embossed wire pressure should be 10.0 kgf / cm or less, but from the viewpoint of improving filter efficiency and water pressure durability, it may be 9.0 kgf / cm or less, or even 8.2 kgf / cm or less. The embossing line pressure may be 6.0 kgf / cm or higher, or 7.1 kgf / cm or higher, from the viewpoint of ensuring embossing strength and thereby improving water pressure resistance.
[0070] The embossing speed may be 15 m / min or more, or 20 m / min or more, from the viewpoint of improving filter efficiency and water pressure resistance. The embossing speed may be 30 m / min or less, or 25 m / min or less, from the viewpoint of ensuring embossing strength and thereby improving water pressure resistance.
[0071] The embossing fusion rate of the filtration laminate can be adjusted by adjusting the embossing conditions in the heat-sealing process. For example, increasing the embossing temperature and embossing linear pressure tends to increase the embossing fusion rate, while increasing the embossing speed tends to decrease the embossing fusion rate. [Examples]
[0072] The embodiments of the present invention will be described in more detail below based on the examples, but the present invention is not limited to these embodiments, which are one embodiment of the present invention. The physical properties and other values in the examples and comparative examples were measured by the following method. In Table 1, "-" indicates that physical properties were not measured, the process was not performed, or resin was not used, etc.
[0073] (1) Weight [g / m 2 ] Ten test specimens measuring 100 mm (flow direction: MD) × 100 mm (direction perpendicular to the flow direction: CD) were taken from spunbond nonwoven or meltblown nonwoven fabric. The test specimens were taken at 10 locations along the CD direction. Next, under conditions of 20°C and 50% RH relative humidity, the mass [g] of each test specimen was measured using a top-loading electronic balance (manufactured by Kensei Kogyo Co., Ltd.). The average mass of each test specimen was calculated. From the calculated average value, 1 m 2 Convert to mass per unit [g], round to the first decimal place, and obtain the weight [g / m²] of each sample. 2]
[0074] (2) Average fiber diameter [μm] The average fiber diameter of the fibers was determined as follows: The spunbond nonwoven or meltblown nonwoven fabric to be measured was observed using an optical microscope (Nikon ECLIPSE E-400). 100 fibers were selected from those forming the spunbond or meltblown nonwoven fabric on the screen, and their diameters were measured. The average value of these measurements was taken as the average fiber diameter of the fiber in question.
[0075] (3) Tensile strength The tensile strength of the filtration laminate or nonwoven fabric was measured in accordance with JIS L 1906. A test specimen measuring 25 mm wide x 200 mm long was taken from the filtration laminate, and the tensile strength (N / 25 mm) was determined by measuring five points in the MD (fiber direction) using a tensile testing machine with a chuck distance of 100 mm and a head speed of 100 mm / min, and calculating the average value. The evaluation criteria for tensile strength are as follows. Rating A: 15N / 25mm or more Rating B: 10N / 25mm or more and less than 15 Rating C: 10N / less than 25mm
[0076] (4) Filter efficiency The filter efficiency of the filtration laminate or nonwoven fabric was measured using the following method. Three 15cm x 15cm samples were taken from any part of the filtration laminate or nonwoven fabric, and the filter efficiency of each sample was measured using a filter performance measuring device (TSI AFT8130A). To measure the filter efficiency, NaCl particulate dust with a median diameter of 0.07 μm was generated using an atomizer, then the sample was placed in a holder, and the airflow was adjusted using a flow control valve so that the filter passage velocity was 31.8 L / min. The number of dust particles D2 upstream and D1 downstream of the sample were detected using a laser particle detector, and the filter efficiency (%) was calculated by rounding the value obtained using the following formula to the first decimal place. Filter efficiency (%) = [1 - (D1 / D2)] × 100 Here, D1 is the number of dust particles downstream, and D2 is the number of dust particles upstream. The criteria for evaluating filter efficiency are as follows: Rating A: 60% or higher Rating B: 40% to less than 60% Rating C: Less than 40%
[0077] (5) Water pressure resistance The water pressure resistance of the filtration laminate or nonwoven fabric was evaluated as follows. First, a water pressure of 0.2 MPa was applied to the filtration laminate for 5 minutes, and then the presence or absence of tears in the filtration laminate, holes in the embossed areas, etc., was checked. The evaluation criteria for water pressure resistance are as follows. Evaluation A: No tears were observed in the filtration laminate, nor were any punctures found in the embossed areas. Evaluation B: Perforation was observed in the embossed area. Evaluation C: Tear in the filtration layer was observed.
[0078] (6) Embossing fusion rate The embossing fusion rate of the filtration laminate was determined as follows. First, black drawing paper and the filtration laminate were placed on a table in that order. Next, an arbitrary part of the filtration laminate was selected, and a photograph was taken from directly above using a digital camera, ensuring that at least 15 embossed fusion areas were visible without being cut off. The above photography operation was repeated, changing the position of the arbitrary part being photographed, until at least 100 embossed fusion areas were visible without being cut off. Using the photographs of the embossed fused areas taken in this manner, the number of embossed fused areas E1 and E2 were counted as follows. E1: Total number of embossed fused areas that are not cut off in the image. E2: The number of areas within the embossed fused section that are not cut off, where the black drawing paper is obscured by unfused fibers. The embossing fusion rate (%) was calculated by rounding the value obtained using the following formula to the first decimal place. Embossing fusion rate (%) = [1 - (E2 / E1)] × 100 Figures 3 to 9 show images of the embossed areas in experimental examples 1 and 9-33, each with different embossing conditions.
[0079] [Experimental Example 1] A filtration laminate (SMS in Table 1) consisting of a spunbond nonwoven fabric layer, a meltblown nonwoven fabric layer, and a spunbond nonwoven fabric layer in the following order was prepared. The physical properties of each layer, the physical properties of the fibers constituting each layer, and the physical properties of the filtration laminate are shown in Table 1.
[0080] (Layer 1: Spunbond nonwoven fabric layer) Using component I listed below, melt spinning was performed by the spunbond method, and the nonwoven web formed from the fibers was deposited on a moving collection surface to create the first layer. Component I: Propylene homopolymer (hPP) with a melting point of 162°C and a MFR of 60 g / 10 min (measured at 230°C and 2160 g load according to ASTM D1238; the same applies hereafter unless otherwise specified).
[0081] (Layer 2: Meltblown nonwoven fabric layer) The following component II was supplied to the die of a meltblown nonwoven fabric manufacturing apparatus. From the heated die, it was discharged using a meltblown nozzle along with high-temperature, high-speed air blown from both sides of the nozzle, depositing a nonwoven web formed from fibers onto the first layer to create the second layer. Component II: Propylene homopolymer (hPP) with a melting point of 159°C and a MFR of 850 g / 10 min.
[0082] (Third layer: Spunbond nonwoven fabric layer) Using component I described above, melt spinning was performed by the spunbond method, and the nonwoven web formed from the fibers was deposited on the second layer to create a third layer, thereby producing a laminated nonwoven web structure.
[0083] Next, a laminated nonwoven web was heat-fused using the embossing roll described below under the embossing conditions to produce a filtration laminate (SMS in Table 1). The fabricated filtration laminate was then used for the evaluations shown in Table 1. -Embossing Roll- Embossing area ratio: 18% - Embossing conditions - Embossing temperature: 125℃ Embossing pressure: 7.1 kgf / cm Embossing speed: 20 m / min
[0084] [Experimental Examples 2-4] The above component II was supplied to the die of a meltblown nonwoven fabric manufacturing apparatus. From the heated die, it was discharged using a meltblown nozzle along with high-temperature, high-speed air blown from both sides of the nozzle, and the nonwoven web formed from the fibers was deposited on a moving collection surface to produce a meltblown nonwoven fabric. The meltblown nonwoven fabric produced (MB in Table 1) was used for the evaluations shown in Table 1.
[0085] [Experimental Example 5] Meltblown nonwoven fabric was prepared in the same manner as in Comparative Example 1, except that polybutylene terephthalate (product name: Juranex 200FP, PBT) was supplied to the die of the meltblown nonwoven fabric manufacturing apparatus instead of component II. The prepared meltblown nonwoven fabric (MB in Table 1) was used for the evaluations shown in Table 1.
[0086] [Experimental Example 6] Using component I described above, melt spinning was performed using the spunbond method in the same manner as in the preparation of the first layer in Experimental Example 1. The nonwoven web formed from the fibers was deposited onto a moving collection surface to produce a spunbond nonwoven fabric. The prepared spunbond nonwoven fabric (SB in Table 1) was used for the evaluations shown in Table 1.
[0087] [Experimental Example 7] In Experimental Example 6, spunbond nonwoven fabric was prepared in the same manner as in Experimental Example 6, except that the average fiber diameter and the basis weight of the spunbond nonwoven fabric were changed as shown in Table 1. The prepared spunbond nonwoven fabric (SB in Table 1) was used for the evaluations shown in Table 1.
[0088] [Experimental Example 8] A laminated nonwoven web consisting of a spunbond nonwoven layer, a meltblown nonwoven layer, and a spunbond nonwoven layer was prepared in the same manner as in Experimental Example 1. Without embossing the laminated nonwoven web, the evaluations shown in Table 1 were performed using the laminated nonwoven web (SMS in Table 1).
[0089] [Experimental Example 9] A laminated nonwoven web consisting of a spunbond nonwoven layer, a meltblown nonwoven layer, and a spunbond nonwoven layer was prepared in the same manner as in Experimental Example 1. A filtration laminate (SMS in Table 1) was prepared in the same manner as in Experimental Example 1, except that the embossing conditions for the laminated nonwoven web were changed as shown in Table 1.
[0090] [Experimental Examples 10-33] For Experimental Example 1, a laminated nonwoven web consisting of a spunbond nonwoven layer, a meltblown nonwoven layer, and a spunbond nonwoven layer was prepared by changing each nonwoven layer as shown in Tables 2 to 4. Furthermore, a filtration laminate (SMS in Table 1) was prepared in the same manner as in Experimental Example 1, except that the embossing conditions for the laminated nonwoven web were changed as shown in Tables 2 to 4.
[0091] [Table 1]
[0092] [Table 2]
[0093] [Table 3]
[0094] [Table 4]
[0095] In Experimental Example 1, samples 10-25 demonstrated excellent tensile strength, filter efficiency, and water pressure resistance. On the other hand, in experimental examples 2-9 and 26-33, at least one of the evaluations of tensile strength, filter efficiency, and water pressure resistance was inferior to that of Example 1.
[0096] The disclosure of Japanese Patent Application No. 2022-212321, filed on 28 December 2022, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated by reference to the same extent as if each individual document, patent application, and technical standard were specifically and individually noted to be incorporated by reference.
Claims
1. A spunbond nonwoven fabric layer containing spunbond nonwoven fabric, A meltblown nonwoven fabric layer containing a meltblown nonwoven fabric, The average fiber diameter of the fibers contained in the meltblown nonwoven fabric is 1.0 μm or less. Embossed, A filtration laminate with an embossing fusion rate of 60% to 90%.
2. The filtration laminate according to claim 1, wherein the spunbond nonwoven fabric and the meltblown nonwoven fabric each independently contain an olefin polymer.
3. The filtration laminate according to claim 1, wherein the spunbond nonwoven fabric and the meltblown nonwoven fabric each independently contain a propylene homopolymer.
4. The average fiber diameter of the fibers contained in the spunbond nonwoven fabric is 15 μm to 40 μm, and the basis weight of the spunbond nonwoven fabric layer is 10 g / m². 2 ~40g / m 2 The filtration laminate according to claim 1.
5. The filtration laminate according to claim 1, wherein the tensile strength is 10 N / 25 mm or more.
6. The filtration laminate according to claim 1, wherein the spunbond nonwoven fabric layer is laminated on both sides of the meltblown nonwoven fabric layer.
7. A step of melt-spinning a first thermoplastic resin or a first resin composition containing the first thermoplastic resin by a spunbond method, and depositing the fibers obtained by melt-spinning onto a moving collection surface to obtain a first spunbond nonwoven fabric layer containing a spunbond nonwoven fabric, A step of obtaining a meltblown nonwoven fabric layer containing a meltblown nonwoven fabric by depositing fibers obtained by the meltblown method onto a moving collection surface using a second thermoplastic resin or a second resin composition containing the second thermoplastic resin, A step of heat-sealing the first spunbond nonwoven fabric layer and the meltblown nonwoven fabric layer by embossing, Includes, The method for manufacturing a filtration laminate according to claim 1, wherein in the heat-sealing step, the embossing temperature is less than 130°C and the embossing linear pressure is 10.0 kgf / cm or less.
8. The method for manufacturing a filtration laminate according to claim 7, wherein the embossing temperature is 110°C or higher.
9. A step of melt-spinning a third thermoplastic resin or a third resin composition containing the third thermoplastic resin by a spunbond method, and depositing the fibers obtained by melt-spinning onto a moving collection surface to obtain a spunbond nonwoven fabric layer containing a second spunbond nonwoven fabric, The process involves heat-sealing the first spunbond nonwoven fabric layer, the meltblown nonwoven fabric layer, and the second spunbond nonwoven fabric layer in this order by embossing, A method for manufacturing a filter laminate according to claim 7 or claim 8, including the following:
10. The method for manufacturing a filter laminate according to claim 7 or claim 8, wherein the embossing speed in the heat-sealing step is 15 m / min or more.
11. The method for manufacturing a filter laminate according to claim 7 or claim 8, wherein the embossing fusion rate of the filter laminate is less than 100%.
12. The method for manufacturing a filter laminate according to claim 7 or claim 8, wherein the embossing fusion rate of the filter laminate is 60% or more and 90% or less.
Citation Information
Patent Citations
Laminated non-woven fabric
JP1998251960A
Laminated non-woven fabric
WO2019167852A1