Steel plates with excellent bending anisotropy and high-strength press-hardened steel parts, and methods for manufacturing the same.
By controlling the chemical composition and inclusion clustering in steel sheets, the anisotropic bending issue is addressed, resulting in high-strength steel parts with uniform mechanical properties and enhanced safety.
Patent Information
- Application Number
- JP2025072071
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-06-30
- Filing Date
- 2025-04-24
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-04-26
AI Technical Summary
Producing high-strength steel with uniform bending behavior in all directions is challenging due to anisotropic bending properties, which can lead to premature cracking and reduced impact resistance, complicating design and safety in applications like automotive components.
A steel sheet with a specific chemical composition and controlled inclusion clustering, combined with a manufacturing process that limits bending anisotropy to 7° or less, achieving uniform mechanical properties across directions.
The solution results in high-strength steel parts with tensile strength over 1300 MPa and minimal bending anisotropy, ensuring stable performance and improved safety through uniform impact resistance and energy absorption.
Smart Images

Figure 0007955420000007 
Figure 0007955420000001 
Figure 0007955420000002
Abstract
Description
[Technical Field]
[0001] This invention relates to steel plates and high-strength press-hardened steel parts. [Background technology]
[0002] High-strength press-hardened parts can be used as structural elements in automobile vehicles for intrusion prevention or energy absorption functions.
[0003] For such applications, it is desirable to produce steel components that combine high mechanical strength with high impact resistance. Furthermore, one of the major challenges in the automotive industry is to reduce vehicle weight to improve fuel efficiency from an environmental perspective, without neglecting safety requirements.
[0004] This weight reduction can be achieved, in particular, thanks to the use of steel components that primarily have a martensitic microstructure.
[0005] Producing extremely high-strength steel that also possesses good and uniform resistance to crack formation under bending is difficult. In fact, extremely high-strength steel tends to crack prematurely when subjected to bending loads. This is detrimental to the impact resistance of parts produced from such high-strength steel, because even though the material can withstand extremely high loads thanks to its high tensile strength, once cracks begin to appear in the part, these cracks propagate rapidly under continuous load, causing the part to fail prematurely.
[0006] In particular, producing very high-strength press-hardened steel with isotropic bending behavior is difficult. In fact, generally speaking, it is well known that the bending behavior of steel sheets is better in the rolling direction than in the transverse direction. This anisotropic behavior imposes constraints when designing steel components and when considering hot stamping processes. Therefore, providing steel sheets and methods for producing such steel that enable very similar bending behavior in all directions is of great interest. [Overview of the Initiative] [Problems that the invention aims to solve]
[0007] The object of the present invention is to address the above-mentioned problems and provide a press-hardened steel part that has a combination of high mechanical properties, a tensile strength of 1300 MPa or more after hot stamping, and an anisotropy of a very small bending angle between the rolling direction and the transverse direction.
[0008] Another object of the present invention is to provide a steel sheet that can be deformed into such press-hardened steel parts by hot forming, and a method for manufacturing such a steel sheet.
[0009] An object of the present invention is achieved by providing a steel sheet according to claim 1 having any of the features of claims 2 to 4. Another object of the present invention is achieved by providing a press-hardened steel part according to claim 5. The steel part may also have the features of claims 6 to 7. A further object of the present invention is a method for manufacturing the hot-stamped part according to claim 8, which optionally includes the features of claim 9.
[0010] Here, the present invention will be described and illustrated in detail by examples, without introducing any limitations, with reference to Figure 1, which shows a schematic cross-sectional view of a steel plate according to the present invention. [Brief explanation of the drawing]
[0011] [Figure 1] Figure 1 shows a steel sheet 1 according to the present invention, comprising a bulk portion 3 and upper and lower skin layers 2. [Modes for carrying out the invention]
[0012] A steel blank refers to a flat sheet of steel cut into any shape suitable for its use. The blank has a top and a bottom surface, also referred to as the top and bottom surfaces or upper and lower surfaces. The distance between these surfaces is specified as the thickness of the blank. The thickness can be measured, for example, using a micrometer, with its spindle and anvil positioned on the top and bottom surfaces. Similarly, the thickness can also be measured on a molded part.
[0013] Hot stamping is a forming technique that involves heating a blank to a temperature at which the steel microstructure transforms at least partially into austenite, shaping the blank at high temperatures by stamping it, and quenching the formed part to obtain a microstructure with very high strength. Hot stamping makes it possible to obtain very high-strength parts with complex shapes and presents many technical advantages. It should be understood that the heat treatment the part undergoes includes not only the thermal cycle of the hot stamping process itself as described above, but also, in some cases, other subsequent heat treatment cycles performed after the part has been painted to cure the paint, such as a paint curing step. The mechanical properties of the hot-stamped parts below were measured after the complete thermal cycle, and optionally include, for example, a paint curing step if paint curing was actually performed.
[0014] The ultimate tensile strength is measured according to the ISO standard ISO 6892-1, published in October 2009. Tensile test specimens are cut from the flat areas of the hot-stamped parts. Smaller tensile test samples are taken as needed to cover the entire available flat area on the part.
[0015] The bending angle is measured according to the VDA-238-100 bending standard, version published in June 2017. The bending angle was measured using a laser measuring device. When performing bending tests on hot-stamped parts, samples are cut from the flat areas of the part. If necessary, small-sized samples are taken to cover the entire available flat area on the part.
[0016] The bending angle of a part represents its ability to withstand deformation without forming cracks.
[0017] The bending angle is measured in the rolling direction (RD), i.e., the direction in which the steel sheet moved during the hot rolling step, and in the transverse direction (TD), i.e., at an orientation of 90° compared to the rolling direction. Bending anisotropy is defined as the absolute value of the difference between the bending angles measured in the rolling direction and the transverse direction for a given sample.
[0018] If the rolling direction on a hot-stamped part is unknown, it can be determined using electron backscatter diffraction (EBSD) analysis across a cross-section of the sample with a scanning electron microscope (SEM). The rolling direction is determined according to the intensity of the orientation density function (ODF) representing the principal fiber at φ2 = 45°, where φ2 is the Euler angle as defined in "H.-J. Bunge: Texture Analysis in Materials Science - Mathematical Methods. 1st English Edition by Butterworth Co (Publ.) 1982" (see Figures 2.2 and 2.3 for the definition of φ2).
[0019] Next, the composition of the steel according to the present invention will be described, with the content expressed in weight percent. The chemical composition is given with respect to the lower and upper limits of the composition range, and the said limits are included within the possible composition range according to the present invention. Where a preferred range for a given element is disclosed, the present invention also discloses all possible combinations of these preferred ranges for each individual element.
[0020] According to the present invention, carbon is in the range of 0.2% to 0.4% to ensure satisfactory strength. When carbon exceeds 0.4%, the weldability and bendability of the steel sheet may deteriorate. When the carbon content is less than 0.2%, the tensile strength does not reach the target value. In certain embodiments, carbon is in the range of 0.2% to 0.3% to ensure sufficient strength while further controlling excellent weldability and bendability. In certain embodiments, carbon is in the range of 0.2% to 0.25% to ensure sufficient strength while further controlling excellent weldability and bendability.
[0021] The manganese content is in the range of 0.8% to 2.0%. When the addition amount exceeds 2.0%, the risk of MnS formation increases, and bendability is impaired. When it is less than 0.8%, the hardenability of the steel sheet during the hot stamping process deteriorates.
[0022] In certain embodiments, the manganese content is in the range of 1.0% to 1.4% to further improve the hardenability of steel, further limit the formation of MnS, and thus improve bendability.
[0023] The silicon content is in the range of 0.1% to 0.5%. Silicon is an element involved in hardening in solid solution. Silicon is added to limit the formation of carbides. When it exceeds 0.5%, silicon oxide is formed on the surface, which impairs the coatability of steel. Furthermore, the weldability of parts produced from the steel sheet may deteriorate. In certain embodiments, the silicon content is in the range of 0.1% to 0.4% to further improve coatability and weldability. In certain embodiments, the silicon content is in the range of 0.15% to 0.35% to further harden the steel and further improve coatability and weldability.
[0024] According to the present invention, the aluminum content is in the range of 0.01% to 0.1%, since aluminum is a very effective element for deoxidizing steel in the liquid phase during smelting. If the titanium content is insufficient, aluminum can protect boron. The aluminum content is less than 0.1% to avoid oxidation problems and ferrite formation during press hardening. Preferably, the aluminum content is in the range of 0.02% to 0.06% to further ensure good deoxidation of steel in the liquid phase while further avoiding oxidation problems and ferrite formation during press hardening.
[0025] According to the present invention, the titanium content is in the range of 0.01% to 0.1% to protect boron that would otherwise be trapped in the BN precipitate. The titanium content is limited to 0.1% to avoid excessive TiN formation. In certain embodiments, the Ti content is in the range of 0.02% to 0.06% to further protect boron while further avoiding excessive TiN formation.
[0026] According to the present invention, the boron content is in the range of 0.0005% to 0.005%. Boron improves the hardenability of steel. The boron content is 0.005% or less to avoid the problem of slab fracture during continuous casting. In certain embodiments, the boron content is in the range of 0.002% to 0.004% to further ensure the hardenability of steel and further avoid the problem of slab fracture.
[0027] Phosphorus is controlled to 0.040% or less because it causes brittleness and weldability problems. In certain embodiments, the P content is controlled to 0.020% or less to further avoid brittleness and weldability problems.
[0028] The presence of calcium in molten steel can lead to the formation of coarse inclusions that are detrimental to flexibility; therefore, calcium content is controlled to 0.01% or less. In certain embodiments, the Ca content is controlled to 0.005% or less to further avoid the problems associated with coarse inclusions.
[0029] The presence of sulfur in molten steel can lead to the formation of MnS precipitates, which are detrimental to bendability; therefore, sulfur content is controlled to 0.006% or less. In certain embodiments, the sulfur content is controlled to 0.005% or less to further avoid the formation of MnS precipitates.
[0030] Nitrogen levels should be controlled to less than 0.01%, preferably less than 0.008%, and even more preferably less than 0.005%. The presence of nitrogen can lead to the formation of precipitates such as TiN or TiNbCN, which are detrimental to flexibility.
[0031] Chromium may be added optionally, up to a maximum of 0.4%. Chromium can be used to provide strength through solid solution hardening and to improve the hardenability of steel sheets during hot stamping. Chromium is limited to 0.4% to limit costs and avoid processing problems.
[0032] Molybdenum may be added optionally, up to a maximum of 0.3%. Molybdenum improves the hardenability of steel. The amount of molybdenum is limited to 0.3% to limit costs and avoid processing problems.
[0033] Niobium is optionally added, up to a maximum of 0.1%. Niobium improves the ductility of steel. Niobium is limited to 0.1% to limit costs and avoid processing problems.
[0034] Vanadium is optionally added, up to a maximum of 0.3%. Vanadium improves the hardenability of steel. Vanadium is limited to 0.3% to limit costs and avoid processing problems.
[0035] If one or more of the above elements are added, the following formula is further examined to limit costs and avoid processing problems: Cr + Mo + Nb + V ≤ 0.5%.
[0036] In certain embodiments, the chemical composition is further controlled so that the following conditions are verified.
[0037] (S-Ca*32 / 40)+(30*Ti*N)≦0.0045
[0038] The inventors have found that this allows for further control of the inclusion cluster in the steel sheet, and therefore further improvement in bendability and bending anisotropy.
[0039] The remainder of steel composition consists of iron and impurities arising from the smelting process. The level of impurities arising from the smelting process depends on the production route used and the level of scrap used in the molten steel. For example, when using a basic oxygen furnace route with low-level steel scrap (recycled steel), the level of impurities remains very low. However, it is also possible to add a large amount of scrap in the converter to the pig iron produced in the basic oxygen furnace, which increases the level of impurities. Furthermore, for example, when smelting steel using an electric furnace with a very high proportion of recycled scrap steel, the level of impurities increases significantly. When using high-level scrap, the level of Cu can rise to 0.25%, Ni to 0.25%, Sn to 0.05%, As to 0.03%, Sb to 0.03%, and Pb to 0.03%.
[0040] Next, the microstructure of the steel sheet according to the present invention will be described.
[0041] The steel sheet has a microstructure in which the surface fraction of any analytical cross-section includes the following: -75%~90% ferrite, - The remaining portion consists of carbide Fe3C and hard phases such as martensite and bainite.
[0042] Referring to Figure 1, the steel sheet 1 according to the present invention comprises a bulk portion 3 and upper and lower skin layers 2. The total thickness of the steel sheet 1 is t0, and the thickness ts of the skin layer 2 is such that ts = t0 * 10%. In other words, the skin layer 2 accounts for the outermost 10% of the thickness on both sides of the bulk, and the bulk of the steel sheet corresponds to 80% of the thickness of the steel sheet.
[0043] The inventors have found a correlation between bending anisotropy and the clustering of inclusions in the bulk portion of steel sheets. In particular, the sum of the clustering indices of MnS and TiN / Ti(C,N) inclusions in the bulk portion of steel was 300 μm / mm². 2 By controlling the following, it is possible to limit the bending anisotropy to 7° or less.
[0044] The following is a description of the methodology used to characterize inclusions in steel plates and steel components. Please understand that this is only one possible methodology, and other protocols can also be implemented.
[0045] The cross-section of the steel plate in which the inclusions are observed is taken in the direction of the steel's rolling. In other words, the plane of the observed cross-section has a transverse direction as its normal direction.
[0046] Inclusions present in the steel plates were characterized using a scanning electron microscope (SEM) equipped with a field effect gun (FEG). A Tescan Mira 3 SEM was used with a power setting of 14 kV. This allows for the detection of small particles of approximately 0.5 μm. Using the FEGSEM setting allows for obtaining stable images with excellent resolution over long periods, which may be necessary to complete extensive image analysis. The FEGSEM setting allows for acquiring image fields over periods of up to 48 hours, which may be necessary for the analysis of multiple samples. Furthermore, the inclusions were analyzed using energy-dispersive spectroscopy (EDS). A 120 mm SEM with a large active surface was used to detect light elements (O, N), obtain high counting rates, and thus enable precise quantification. 2A Bruker EDS probe was used. Accurate quantification was obtained using the phi-rho-Z method.
[0047] Using the RJ Lee Group's Automated Steel Cleanliness Analysis Tool (ASCAT), we will pilot SEM and associated EDS based on computer-controlled scanning electron microscopy technology. Six individual samples can be analyzed in the same batch. The sample surface is divided into three regions (upper skin, lower skin, and bulk, as previously mentioned). Each region is divided into fields. In each field, inclusions are detected. To detect fine particles, the scanning pixel size is set to a very low value of 0.11 μm. This is to reduce matrix noise in the SEM image. As you would expect, only objects with a diameter greater than 0.5 μm are actually considered. The initial selection of objects referred to as particles is done by selecting objects that form a solid and have a gray level that is either less than 150 or greater than 220 on a scale of 0 to 255 (extreme values are excluded).
[0048] Next, each individual particle is zoomed in on to capture its morphological features, and EDS analysis is performed. A database of all particles is created using ASCAT, taking into account the chemical and morphological characteristics of all analyzed particles for all acquired images.
[0049] Of the entire set of particles analyzed, only those with a size greater than 0.5 μm and an iron content of less than 80% are retained for subsequent analysis and are called inclusions, while the other particles are considered to be part of the matrix and are not relevant to subsequent analysis.
[0050] Next, using information from the EDS probe, each inclusion is classified into one of the following families: TiN, alumina, complex oxides, oxysulfide particles, MnS, etc. For example, Table 1 details the strict rules used by the inventors to classify MnS and TiN / Ti(C,N) inclusions. Oxygen quantification is made possible by a high-performance EDS detector. Oxygen levels are checked to separate TiN from TiO2 and MnS from complex oxysulfide inclusions.
[0051] Table 1 - Criteria for classifying inclusions by weight percentage of Ti, M, SO, and Nb
[0052] [Table 1]
[0053] Next, the following characteristics are calculated for each inclusion family: -Average diameter in microns, -mm 2 The density of the number of inclusions per unit.
[0054] The method for calculating the clustering index is based on the DBSCAN (Density-Based Spatial Clustering in Noisy Applications) algorithm, as detailed in the paper "A density-based algorithm for discovering clusters in large spatial databases with noise", Ester, Martin; Kriegel, Hans-Peter; Sander, Jorg; Xu, Xiaowei (1996), Proceedings of the Second International Conference on Knowledge Discovery and Data Mining (KDD-96). AAAI Press. pp.226-231.
[0055] The clustering index is determined using two parameters: Max_distance and Min_points. Clusters are characterized by the following features: -It contains only particles of the same type, -In a given cluster, all inclusions are at a distance less than Max_distance from at least one other inclusion. -It contains more than Min_point individual inclusions.
[0056] With respect to the present invention, the inventors have found that good detection of clusters can be obtained when the maximum distance Max_distance is 30 μm and the minimum number of inclusions per cluster Min_points is 4.
[0057] The length L of a given cluster is calculated as follows: - First, determine the convex hull of the cluster using a known algorithm (see, for example, the chapter "Convex Hulls: Basic Algorithms" in *In: Computational Geometry, Preparata, FP, Shamos, MI, 1985, Texts and Monographs in Computer Science, Springer, New York, NY*). Next, the maximum ferret diameter of the convex hull, called Dmax, is determined, and the ferret diameter taken perpendicular to Dmax, called Dperp, is also determined. Information on ferret diameter measurement is available, for example, in "Particle Size Measurements: Fundamentals, Practice, Quality" Springer, Henk G. Merkus (January 1, 2009).
[0058] - The length L of the cluster is calculated as follows:
[0059]
number
[0060] For each type of inclusion, the average length L_average of all clusters is calculated.
[0061] The cluster density C_density of a given type of inclusion is given by mm 2 This is the number of clusters per match.
[0062] The cluster index C_index of a given type of inclusion is defined as the product of the average length of the clusters and their density, C_index = L_average * C_density. The cluster index is expressed in μm / mm². 2 It is represented as follows. The inventors have found that the cluster index allows for the comparison of samples having different characteristics using a unique number, and that it correlates well with the bending behavior of the samples.
[0063] The steel sheet according to the present invention can be produced by any suitable manufacturing method, which can be defined by those skilled in the art. However, it is preferable to use the method according to the present invention, which includes the steps described below.
[0064] In the following description, the term ladle refers to the vessel used to hold molten steel during the refining process. The refining process is referred to as the step of adjusting the final chemical composition and temperature of the molten steel before casting it into its first solidified form (for example, before casting it into a slab that will later be hot-rolled).
[0065] To successfully control the aggregation of inclusions in steel, for example, the following steps can be implemented: - Molten steel is tapped into a ladle from the previous steelmaking process step. For example, in the case of an electric arc furnace production route, the previous process step is the electric arc furnace process itself. For example, in the case of a blast furnace and converter process (or a direct reduced iron and converter process), the previous process step is the converter.
[0066] - The sulfur content of the molten steel before the smelting step is measured, for example, by taking a sample of the molten steel and analyzing it using a spark spectrometer. The sulfur content is measured, for example, by directly sampling the molten steel in the ladle, or by taking a sample while the molten steel is being tapped into the ladle. The sulfur content before the smelting step is measured in weight percent and is referred to as S_start in the following description.
[0067] - To deoxygenate the molten steel, aluminum is added to the ladle at the start of the refining process. The addition of Al is carried out, for example, at the same time that the steel is poured into the ladle, which is advantageous as it saves time, thus improving productivity and allowing the molten steel to remain at a sufficiently high temperature. The amount of Al added to the molten steel at the start of the refining process is expressed in kilograms of aluminum per ton of molten steel (kg / ton), and is referred to as Al_added in the following description.
[0068] -In a subsequent optional step, for example, if the molten steel temperature is too low, or if the waiting time between the end of the refining step and the subsequent process (e.g., continuous casting) is expected to ensure it is heated, the molten steel is reheated by aluminosermic heating. This is done by adding a determined amount of aluminum and blowing a determined amount of oxygen into the molten steel, corresponding to the stoichiometric ratio required to form Al2O3 with the added aluminum. The strong exothermic reaction between Al and O2 allows the temperature of the molten steel to rise. The amount of O2 injected during this optional step is called O2_inj, and is the standard cubic meter (Nm³) of O2 per ton of molten steel. 3 It is expressed as ( / ton). Since there is a direct stoichiometric relationship between O2_inj and the associated Al injection for aluminothermic reheating, the amount of Al injected for aluminothermy is not considered separately in this explanation. Note that the Al injected for aluminothermy is different from the Al_added mentioned above.
[0069] - The slag ratio (%CaO / %Al2O3) is greater than 1, the amount of slag per ton of molten steel is at least 10 kg / ton of molten steel, and the slag composition on top of the molten metal is adjusted by adding an appropriate amount of minerals to ensure that the slag remains liquid so that the steel beneath the slag can be accessed and the steel and / or slag can be tapped separately, thereby promoting chemical exchange with the steel. (The liquid state of the slag is confirmed using visual and / or thermodynamic rules based on its composition and temperature.) -In a subsequent step, the molten steel is stirred by blowing in an inert gas, for example, by blowing in Ar. This is done to promote exchange between the molten steel and the slag, and to reduce the sulfur content of the molten steel.
[0070] -In a further step, Ca is added to the ladle to spheroidize inclusions present in the molten steel. For example, Ca may be added in the form of silicon calcium (SiCa), or ferrocalcium (FeCa), or as pure calcium. For example, the addition may be carried out by adding SiCa or FeCa to the ladle in the form of a cored wire, which advantageously allows for easy control of the amount of Ca added by controlling the length of the cored wire inserted into the molten metal and the injection rate. The amount of Ca added to the molten steel is measured in weight percent of the molten steel and will be referred to as Ca_added in the following description.
[0071] Taking the above process into consideration, the inventors have found that by controlling the above-mentioned level of sulfur measured at the start of the refining process (S_start measured in wt%), the amount of Al added at the start of the refining process (Al_added measured in kg / ton), the amount of Ca added during the refining process (Ca-added measured in kg / ton), and the amount of O2 injected (O2_inj measured in Nm3 / ton), in order to verify that the following combination (referred to as C1 in the remainder of this specification) remains below a given cutoff value, a satisfactory level of inclusions can be obtained to achieve the desired bending anisotropy after hot stamping.
[0072] Al_added+0.1953*(S_start*1000+O2_inj)-9.367*Ca_added(C1) In practice, the specific cutoff value that needs to be controlled for combination C1 depends on the specific industrial equipment used to produce the steel. It depends on the manufacturing process in the steelworks, the geometric configuration of the ladle used to process the molten steel, the equipment used to add different additives, the oxygen blowing configuration, and so on.
[0073] To determine the relationships between these parameters for a given industrial machine and production route, it is recommended to apply the following method: - Perform several heating processes using the aforementioned chemical composition range.
[0074] - The heat is processed using different refining process parameters, particularly different levels of measured sulfur at the start of the refining process, the amount of Al added at the start of the refining process, the amount of Ca added during the refining process, and the amount of O2 injected. The range of refining process parameters tested is selected to represent the industrial variation of these parameters. For example, six different sets of heat are selected, each having six different sets of refining process parameters. For example, eight different sets of heat are selected, each having eight different sets of refining process parameters.
[0075] -The heat is treated according to the industrial route described below, and the inclusion clusters in the steel are characterized using the method described above.
[0076] Next, the sum of the clustering indices of MnS and TiN / Ti(C,N) inclusions in the bulk portion of the steel sheet, as well as the associated refining process parameters, are recorded. The combination C1 of the aforementioned refining process parameters is calculated. As a general trend, it can be seen that the higher the combination C1, the higher the sum of the clustering indices.
[0077] - Using the above dataset which correlates clustering indices with refining process parameters, the sum of the clustering indices of MnS and TiN / Ti(C,N) inclusions in the bulk portion of the steel sheet is 300 μm / mm². 2 A cutoff value is determined as follows. The cutoff value of combination C1 determines how to control the refining process for the specific industrial equipment under consideration. By controlling C1 to less than the cutoff value, 300 μm / mm 2 It becomes possible to produce steel sheets having the following combined clustering indices of MnS and TiN / Ti(C,N) inclusions in the bulk portion, and thus achieve the relevant excellent bending anisotropy of 7° or less.
[0078] For example, in the case of a specific industrial equipment in which the inventors conducted experiments, the cutoff value is equal to 1.80.
[0079] After the molten steel refining step, the method for producing steel sheets according to the present invention preferably includes the following steps.
[0080] - Continuous casting of molten steel into semi-finished products suitable for hot rolling. During the casting step, particular care should be taken to avoid oxygen pickup and therefore higher inclusion levels in the semi-finished products. For example, in a continuous casting process where the semi-finished products are slabs produced in a continuous sequence by casting products of multiple heats in a mold into a tundish, certain refractories and linings can be used in the tundish, and certain assignment rules can be used for sequence slabs and transient slabs between two different heats.
[0081] Next, the semi-finished product is optionally reheated at a temperature including 1150°C to 1300°C.
[0082] Next, the steel sheet is hot-rolled at a finishing hot-rolling temperature range of 800°C to 950°C.
[0083] Next, the hot-rolled steel is cooled, wound up in a Tcoil at a temperature of less than 670°C, and optionally pickled to remove oxidation.
[0084] Next, the coiled steel sheet is optionally cold-rolled to obtain a cold-rolled steel sheet. The cold-rolling reduction ratio is preferably in the range of 20% to 80%. If it is less than 20%, recrystallization during subsequent heat treatment is undesirable and may impair the ductility of the steel sheet. If it exceeds 80%, there is a risk of edge cracking during cold rolling.
[0085] -In an embodiment of the present invention, the steel plate is heated in an annealing furnace to a soaking temperature including 700°C to 850°C and maintained at the soaking temperature for a soaking time including 10 seconds to 20 minutes.
[0086] -In embodiments of the present invention, the annealed steel sheet is cooled to a temperature range of 400°C to 700°C and further coated with a metal coating. The metal coating is, for example, an aluminum-based metal coating containing at least 50% by weight of aluminum. The metal coating is, for example, a zinc-based metal coating containing at least 50% by weight of zinc.
[0087] -In this embodiment of the present invention, the steel plate is then cooled to room temperature.
[0088] In summary, the method described above preferably includes the following sequence of steps:
[0089] - A step of producing molten steel having the above chemical composition, wherein during the molten steel refining stage, the sulfur level measured at the start of the refining process, the amount of Al added at the start of the refining process, the amount of Ca added during the refining process, and the amount of O2 injected are controlled to verify that the combination Al_added+0.1953*(S_start*1000+O2_inj)-9.367*Ca_added(C1) remains below a predetermined cutoff value. The cutoff value is such that if C1 is below the cutoff value, the sum of the clustering indices of MnS and TiN / Ti(C,N) inclusions in the bulk portion of the steel is 300 μm / mm².2 It is determined for the specific industrial equipment used to achieve the following.
[0090] - casting said molten steel to obtain a semi-finished product that can be hot-rolled, - optionally, reheating said semi-finished product to a temperature T reheat comprised between 1100°C and 1300°C, - hot rolling the semi-finished product at a finishing hot rolling temperature comprised between 800°C and 950°C, - coiling the hot-rolled steel sheet at a coiling temperature T coil of less than 670°C to obtain a coiled steel sheet, - optionally, pickling the coiled steel sheet, - optionally, cold rolling the coiled steel sheet with a reduction ratio ranging from 20% to 80% to obtain a cold-rolled steel sheet, - optionally, heating the hot-rolled steel sheet or cold-rolled steel sheet to a soaking temperature comprised between 700°C and 850°C, maintaining the steel sheet at said temperature for a soaking time comprised between 10 seconds and 20 minutes to obtain an annealed steel sheet, - optionally, cooling said annealed steel sheet to a temperature range of 400°C to 700°C, - optionally, coating the annealed steel sheet with a metallic coating, - optionally, cooling the coated steel sheet to room temperature.
[0091] Next, the manufacturing process of pressed parts and the subsequent assurance of the properties of the pressed parts will be described in detail.
[0092] A steel blank is cut from the steel sheet according to the present invention and heated in an austenitizing furnace. Preferably, the steel blank is heated to a temperature comprised between 880°C and 950°C for 10 seconds to 15 minutes to obtain a heated steel blank. The heated blank is then transferred to a forming press, hot formed, and die quenched to obtain a pressed part.
[0093] Optionally, the hot-stamped parts are further subjected to a paint curing step in which the parts are heated to a temperature of 150°C to 250°C for a duration of 10 minutes to 2 hours.
[0094] The microstructure of the pressed part contains more than 95% martensite and less than 5% bainite + ferrite in surface fraction on any analyzed cross-section. Furthermore, the pressed part according to the present invention comprises a bulk portion and upper and lower skin layers, the skin layers occupying the outermost 10% of the thickness on both sides of the bulk. The bulk portion is 300 μm / mm 2 The following clustering indices are found in the sum of the clustering indices of MnS and TiN / Ti(C,N) inclusions.
[0095] The pressed part according to the present invention has a tensile strength of over 1300 MPa, preferably over 1350 MPa, preferably over 1400 MPa, and a bending angle anisotropy of 7° or less. Such high tensile strength and low bending anisotropy provide the part with very good mechanical resistance, especially in the event of a collision, and further enable very predictable and uniform behavior in all directions. These characteristics provide very good energy absorption and penetration resistance in all directions, thereby enhancing vehicle safety. [Examples]
[0096] The present invention will be explained by the following examples, but these are by no means limiting.
[0097] Eight different samples were tested, derived from eight different heats A, B, C, D, E, F, G, and H of steel produced using industrial production routes. Samples I1, I2, I3, and I4 are according to the present invention, while samples R1, R2, R3, and R4 are reference samples.
[0098] All produced samples followed the same industrial production process at the steelworks. All samples were coated after annealing using an AlSi-based coating containing 8–12 wt% Si, 2–4 wt% Fe, and the remainder being Al.
[0099] Table 2 - Sample Composition The tested compositions are summarized in the table below, with elemental content expressed as weight percentage. The remainder of the composition consists of iron and unavoidable impurities resulting from the smelting process.
[0100] [Table 2]
[0101] Table 3 - Steelmaking process parameters and the sum of clustering indices of MnS and TiN / Ti(C,N) inclusions in the bulk portion of steel. The following process parameters were applied in the steel mill, and the following sums of clustering indices for MnS and TiN / Ti(C,N) inclusions in the bulk portion of the steel were observed - the underlined values are not according to the present invention.
[0102] [Table 3]
[0103] As can be seen, under the tested industrial conditions, the sum of the clustering indices of MnS and TiN / Ti(C,N) inclusions in the bulk portion of the steel was 300 μm / mm², provided that the refining process parameters were appropriately controlled to keep C1 below 1.80. 2 The following can be controlled. As mentioned above, this cutoff value of 1.80 is specific to the industrial equipment on which the trial was conducted, and it is necessary to determine an appropriate cutoff coefficient for a given industrial equipment, for example, by following the methodology described above.
[0104] Table 4 - Further process conditions The following process parameters were applied along the production route.
[0105] [Table 4]
[0106] Table 5 - Microstructure, bending angle, and tensile strength The following microstructure (surface fraction), bending angle, bending angle anisotropy, and tensile strength were measured on the sample, but the underlined values are not according to the present invention.
[0107] [Table 5]
[0108] Table 5 shows that the sample according to the present invention has a tensile strength exceeding 1300 MPa (both RD and TD) while having a bending anisotropy of less than 7°. On the other hand, the reference sample has a comparable tensile strength level exceeding 1300 MPa but has a bending anisotropy greater than 7°.
[0109] The inventors found that this excellent bending anisotropy correlates with the sum of the clustering indices of MnS and TiN / Ti(C,N) inclusions in the bulk portion of the steel, as shown in Table 3. The higher the sum of the clustering indices of MnS and TiN / Ti(C,N) inclusions in the bulk portion of the steel, the higher the bending anisotropy. Cutoff value: 300 μm / mm 2 This makes it possible to control the bending anisotropy to 7° or less. This very low level of bending anisotropy results in very uniform behavior of the hot-stamped part when subjected to loads coming from any direction. This extremely stable behavior of the hot-stamped part under load allows for simplified part design, for example in the case of automotive parts, and ensures very good, robust, and stable impact resistance of the hot-stamped part.
Claims
1. A press-hardened steel part, wherein the steel part is, by weight percentage, C: 0.2-0.3% Mn: 0.8-2.0% Si: 0.1-0.5% Al: 0.01~0.1% Ti: 0.01~0.1% B: 0.0005-0.005% P ≤ 0.040% 0 < Ca ≤ 0.01% S ≤ 0.006% N ≤ 0.01% 0 < Cr ≤ 0.4% Mo ≤ 0.3% Nb ≤ 0.1% V ≤ 0.3% It has a composition containing (Cr + Mo + Nb + V ≤ 0.5%), The remainder of the aforementioned composition consists of iron and unavoidable impurities arising from the smelting process. The above composition is subject to the following conditions: (S - Ca*32 / 40) + (30*Ti*N) ≤ 0.0045, where all elements are expressed in weight percent, and further adherence to this, The steel part has a microstructure that, in terms of surface fraction, contains more than 95% martensite and up to 5% bainite or ferrite. The steel component extends from the bulk to the surface of the steel component. - Equipped with bulk, - Such a bulk is covered by an upper skin layer and a lower skin layer that make up the outermost 10% of the thickness on both sides of the bulk. The bulk material has a combined clustering index of 300 μm / mm² for MnS and TiN / Ti(C,N) inclusions. 2 A press-hardened steel part containing the following inclusion clusters.
2. C: 0.2–0.25%, and / or Mn: 1.0–1.4%, and / or Si: 0.1–0.4%, and / or Al: 0.02–0.06%, and / or Ti: 0.02–0.06%, and / or B: 0.002–0.004%, and / or P ≤ 0.020%, and / or 0 < Ca ≤ 0.005%, and / or S ≤ 0.005%, and / or The press-hardened steel part according to claim 1, wherein N ≤ 0.008%.
3. Si: 0.15 to 0.35%, and / or The press-hardened steel part according to claim 2, wherein N ≤ 0.005%.
4. The press-hardened steel part according to claim 1 or 2, wherein the press-hardened steel part has a tensile strength TS of at least 1300 MPa and a bending angle anisotropy of 7° or less.
5. A method for manufacturing steel plates, comprising the following series of steps: - A step of providing molten steel, wherein the molten steel is, by weight percentage, C: 0.2-0.3% Mn: 0.8-2.0% Si: 0.1-0.5% Al: 0.01~0.1% Ti: 0.01~0.1% B: 0.0005-0.005% P ≤ 0.040% 0 < Ca ≤ 0.01% S ≤ 0.006% N ≤ 0.01% 0 < Cr ≤ 0.4% Mo ≤ 0.3% Nb ≤ 0.1% V ≤ 0.3% It has a composition containing (Cr + Mo + Nb + V ≤ 0.5%), The remainder of the aforementioned composition is iron and unavoidable impurities. The above composition is subject to the following conditions: (S - Ca*32 / 40) + (30*Ti*N) ≤ 0.0045, where all elements are expressed in weight percent, further adhering to the following steps, - A step of casting the molten steel to obtain a semi-finished product that can be hot-rolled, - The step of hot-rolling the aforementioned semi-finished product at a finish hot-rolling temperature included in 800°C to 950°C, - The hot-rolled steel sheet is wound at a temperature T of less than 670°C. coil The steps include winding the steel sheet to obtain a coiled steel sheet, The resulting steel sheet has a microstructure containing 75% to 90% ferrite in surface fraction, with the remainder being Fe 3 It is composed of C and a hard phase consisting of martensite and bainite. The steel plate extends from the bulk to the surface of the steel plate. - Equipped with bulk equivalent to 80% of the thickness of the steel plate, - Such a bulk is covered by an upper skin layer and a lower skin layer that occupy the outermost 10% of the thickness on both sides of the bulk, and the bulk has a combined clustering index of 300 μm / mm² for MnS and TiN / Ti(C,N) inclusions. 2 The following group of inclusions is included: method.
6. C: 0.2–0.25%, and / or Mn: 1.0–1.4%, and / or Si: 0.1–0.4%, and / or Al: 0.02–0.06%, and / or Ti: 0.02–0.06%, and / or B: 0.002–0.004%, and / or P ≤ 0.020%, and / or 0 < Ca ≤ 0.005%, and / or S ≤ 0.005%, and / or The method according to claim 5, wherein N ≤ 0.008%.
7. Si: 0.15 to 0.35%, and / or The method according to claim 6, wherein N ≤ 0.005%.
8. The step of providing molten steel includes a step of refining the molten steel, during which the level of sulfur measured at the start of the refining, the amount of Al added at the start of the refining, the amount of Ca added during the refining, and O 2 The amount blown in is, combination C1 = Al_added + 0.1953 * (S_start * 1000 + O 2 Controlled to verify that _inj)-9.367*Ca_added remains below a predetermined cutoff value. Al_added is the amount of Al added at the start of the refining process, in terms of kg of aluminum per ton of molten steel. S_start is the sulfur content before refining, in weight percent. O 2 _inj, expressed in standard cubic meters of O per tonne of molten steel 2 , is the amount of O injected during an optional aluminothermic heating step 2 , The method according to claim 5 or 6, wherein Ca_added is the amount of Ca added to the molten steel, measured in weight percent within the molten steel.
9. The method according to claim 5 or 6, wherein the steel plate is coated with a metal coating containing at least 50% Al by weight.
10. The method according to claim 5 or 6, wherein the steel plate is coated with a metal coating containing at least 50% Zn by weight.
11. A method for manufacturing a press-hardened steel part according to claim 1 or 2, comprising the following consecutive steps: - A step of providing a steel plate made of steel, Here, the steel is, in weight percentage, C: 0.2-0.3% Mn: 0.8-2.0% Si: 0.1-0.5% Al: 0.01~0.1% Ti: 0.01~0.1% B: 0.0005-0.005% P ≤ 0.040% 0 < Ca ≤ 0.01% S ≤ 0.006% N ≤ 0.01% 0 < Cr ≤ 0.4% Mo ≤ 0.3% Nb ≤ 0.1% V ≤ 0.3% It has a composition containing (Cr + Mo + Nb + V ≤ 0.5%), The remainder of the aforementioned composition consists of iron and unavoidable impurities arising from the smelting process. The above composition is subject to the following conditions: (S - Ca*32 / 40) + (30*Ti*N) ≤ 0.0045, where all elements are expressed in weight percent, and further adherence to this, The steel sheet has a microstructure containing 75% to 90% ferrite in surface fraction, with the remaining portion being Fe 3 It is composed of C and a hard phase consisting of martensite and bainite. The steel plate extends from the bulk to the surface of the steel plate. - Equipped with bulk equivalent to 80% of the thickness of the steel plate, - Such a bulk is covered by an upper skin layer and a lower skin layer that occupy the outermost 10% of the thickness on both sides of the bulk, and the bulk has a combined clustering index of 300 μm / mm² for MnS and TiN / Ti(C,N) inclusions. 2 The following group of inclusions is included: - In order to obtain a steel blank, the steps include cutting the steel plate into a predetermined shape, - The step of heating the steel blank to a temperature of 880°C to 950°C for 10 seconds to 15 minutes to obtain a heated steel blank, - The step of transferring the heated blank to a forming press, - The step of hot-forming the heated blank in the molding press to obtain a molded part, A method comprising the step of die-quenching the molded part.
12. The method according to claim 11, further comprising a paint baking step in which the molded part is heated to a temperature of 150°C to 250°C for a duration of 10 minutes to 2 hours.
Citation Information
Patent Citations
Niobium and vanadium composite microalloying thermoforming steel and production and hot stamping forming method thereof
CN111235483A
Steel plate for hot-stamping component and method for manufacturing the same
JP2021155787A
Coated steel sheet and high-strength press-hardened steel part, and manufacturing method thereof
JP2023554400A
Hot stamping product and method of manufacturing the same
KR1020210050806A
Coated steel sheet and high strength press hardened steel part and method of manufacturing the same
WO2022129994A1