Urea group-containing polyurethane acrylate resin composition and composite material

By integrating urea groups into polyurethane acrylate resins through a specific reaction, the resins achieve enhanced properties and broader applicability, outperforming unmodified counterparts in composite materials.

JP7955427B2Active Publication Date: 2026-11-24SWANCOR INNOVATION & INCUBATION CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2025088599
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2025-02-25
Filing Date
2025-05-28
Publication Date
2026-11-24
Estimated Expiration
2045-05-28

AI Technical Summary

Technical Problem

Existing polyurethane acrylate resins lack versatility and desirable qualities for broader applications.

Method used

A method is developed to modify polyurethane acrylate resins by incorporating urea groups through a reaction with isocyanate, polyol, hydroxyl-containing acrylate, and amine compounds, forming a urea group-containing polyurethane acrylate resin with enhanced properties.

Benefits of technology

The modified resin exhibits superior quality and wider applicability, particularly in composite materials, demonstrating equivalent or superior mechanical properties compared to unmodified resins.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955427000001
    Figure 0007955427000001
  • Figure 0007955427000002
    Figure 0007955427000002
  • Figure 0007955427000003
    Figure 0007955427000003
Patent Text Reader

Abstract

The present invention provides a method for preparing a urea group-containing polyurethane acrylate resin, a resin composition, and a composite material that can replace unmodified polyurethane acrylate and have superior quality or applicability. [Solution] A method for preparing a urea group-containing polyurethane acrylate resin is provided. The method comprises providing a polyurethane acrylate polymer, adding an amine compound, and heating to modify the polyurethane acrylate polymer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a method for preparing resins, resin compositions, and composite materials, and more particularly to a method for preparing urea group-containing polyurethane acrylate resins, resin compositions, and composite materials. [Background technology]

[0002] Polyurethane acrylate (PUA) resins are widely used in electronic devices, building materials, coatings, and paints. However, research challenges include how to modify them to allow for broader applications and / or to achieve more desirable qualities. [Overview of the Initiative] [Problems that the invention aims to solve]

[0003] The present invention provides a method for preparing a urea group-containing polyurethane acrylate resin, a resin composition, and a composite material that can replace unmodified polyurethane acrylate and have superior quality or applicability. [Means for solving the problem]

[0004] The present invention provides a method for preparing a urea group-containing polyurethane acrylate resin, a resin composition, and a composite material that are widely applicable and possess superior quality.

[0005] The present invention provides a method for preparing a urea group-containing polyurethane acrylate resin, comprising providing a polyurethane acrylate polymer, adding an amine-based compound, and heating to modify the polyurethane acrylate polymer.

[0006] The resin composition of the present invention includes a urea group-containing polyurethane acrylate resin represented by Formula 1, which will be described later.

[0007] The composite material of the present invention comprises the aforementioned resin composition and fiber material. The total amount of the resin composition is 100 parts by weight, and the total amount of the fiber material is 67 to 240 parts by weight. [Effects of the Invention]

[0008] Based on the above, the polyurethane acrylate resin used in the resin composition and composite material of the present invention is a modified urea group-containing polyurethane acrylate resin, and therefore is widely applicable and has superior quality. [Modes for carrying out the invention]

[0009] In this specification, unless otherwise specified, when the prefix "approximately" is used to represent a numerical value, the specific numerical value may be represented directly. Furthermore, when the prefix "approximately" is used to represent a numerical value, it may include the measurement error range that is typically included in a general measurement method, or the error propagation range after deriving or calculating it.

[0010] In this specification, when representing a numerical value or a range of numerical values, possible embodiments include one specific value, another specific value, and a range between the two specific values. For example, when representing the range from 1 to 10, and separately representing specific values ​​3 and 7, one embodiment may include specific value 1, specific value 3, specific value 7, specific value 10, the range from 1 to 3, the range from 1 to 7, the range from 3 to 7, the range from 3 to 10, and the range from 7 to 10. For example, when representing specific values ​​2, 5, and 8, one embodiment may include specific value 2, specific value 5, specific value 8, the range from 2 to 5, the range from 2 to 8, and the range from 5 to 8.

[0011] <1. Urea group-containing polyurethane acrylate resin> Urea group-containing polyurethane acrylate resins may be obtained by reaction with isocyanate compounds, polyol compounds, hydroxyl-containing (meth)acrylate compounds, and amine compounds.

[0012] <1.1 Isocyanate Compounds> An isocyanate compound is a difunctionalized (i.e., at least bifunctionalized) isocyanate compound. For example, an isocyanate compound containing two isocyanate groups (NCO). Commercially available difunctionalized isocyanate compounds include, but are not limited to, Tosoh Corporation's MR200 and NM, Wanhua Chemical's PM200 and MDI-50, BASF SE's M20S, Covestro AG's 44V20, and Huntsman Corporation's 5005.

[0013] The present invention is not limited to isocyanate compounds in the form of a single compound. Taking a bifunctionalized isocyanate compound in polymer form as an example, it may be a polymer of a single monomer, for example, toluene diisocyanate (TDI) or isoholodiisocyanate (IPDI). Alternatively, it may be a mixture of polymers of multiple monomers. Alternatively, it may be a copolymer, for example, diphenylmethane diisocyanate (MDI-50).

[0014] <1.2 Polyol Compounds> The polyol compound is a difunctionalized polyol compound. For example, it is a difunctionalized polyether polyol compound, which may be, but is not limited to, polyoxyethylene ether, polyoxyethylene alkyl ether, polyoxypropylene ether, polyoxypropylene alkyl ether, or polytetrahydrofuran. In the embodiments described above, the polyol compound is given as a polymer as an example, but this application is not limited to these, and the polyol compound may be in a non-polymeric form.

[0015] The present invention does not limit polyol compounds to the form of a single compound. Taking a bifunctional polyol compound in polymer form as an example, it may be a polymer of a single monomer, or a mixture of polymers of multiple monomers, or a copolymer.

[0016] In one embodiment, when the difunctional polyol compound is in a polymer form, its number average molecular weight is preferably about 2000 g / mol or less.

[0017] <1.3 Hydroxyl-Containing (Meth)Acrylate Compound> In the present invention, hydroxyl-containing (meth)acrylate is an abbreviation for "hydroxyl-containing acrylate" or "hydroxyl-containing methacrylate". Multiple types of hydroxyl-containing (meth)acrylates may be mixed for use. Specifically, the hydroxyl-containing (meth)acrylate compound may include, but is not limited to, at least one or more of hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, and hydroxypropyl methacrylate.

[0018] <1.4 Amine Compound> The amine compound may include an amine polymer, a monoamine compound, a diamine compound, or a mixture thereof. The amine polymer is, for example, a polyetheramine with a number average molecular weight of about 400 g / mol or less. The monoamine compound may include an aliphatic primary amine, an aliphatic secondary amine, an alicyclic primary amine, an alicyclic secondary amine, or a mixture thereof. The aliphatic secondary amine is, for example, dibutylamine. The diamine compound may include an aliphatic primary amine, an alicyclic primary amine, an alicyclic secondary amine, or a mixture thereof. The aliphatic primary amine is, for example, polyetheramine (D230). The alicyclic primary amine is, for example, isophoronediamine (IPDA) or 4,4'-diaminodicyclohexylmethane (PACM). The alicyclic secondary amine is, for example, piperazine.

[0019] <1.5 Diluting Monomer> Diluting monomers have functional groups suitable for the reaction, or can form corresponding free radicals. In this way, viscosity / fluidity can be adjusted by forming polymer chains with the corresponding reactants by a continuous addition method. For this reason, diluting monomers can also be called viscosity-adjusting monomers. In selection, the type of isocyanate compound, polyol compound, hydroxyl-containing (meth)acrylate compound, or amine compound described above may be used. To facilitate the continuous addition polymerization reaction, it is appropriate to select and use diluting monomers that are structurally similar to or have the same functional groups as the isocyanate compounds, polyol compounds, hydroxyl-containing (meth)acrylate compounds, or amine compounds described above. For example, the diluting monomer may be one or more mixtures selected from methyl (meth)acrylate, ethyl (meth)acrylate, hydroxyethyl (meth)acrylate, propyl (meth)acrylate, hydroxypropyl (meth)acrylate, tetrahydrofuran (meth)acrylate, isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, styrene, methylstyrene, or vinyltoluene.

[0020] In one embodiment, the total amount of urea group-containing polyurethane acrylate resin ultimately produced in the subsequent reaction is 100 parts by weight, and the total amount of diluting monomer is 30 to 45 parts by weight.

[0021] <1.6 Inhibitors> The addition of inhibitors can enhance the stability of the resin composition. In one embodiment, the inhibitor may include a phenolic compound, such as 2,5-dihydroxytoluene or 2,6-di-tert-butylhydroxytoluene.

[0022] In one embodiment, the total amount of the urea group-containing polyurethane acrylate resin composition ultimately produced in the subsequent reaction is 100 parts by weight, and the total amount of the inhibitor is 0.01 to 0.03 parts by weight.

[0023] <1.7 Ratio Relationships Between Reactants> From the perspective of reagent formulation, the amounts of each component in a composition can be directly described in terms of weight or weight ratio. However, from the perspective of reactivity between each composition, it may be more accurate to describe the amounts in terms of molar ratio or molar equivalent ratio (abbreviated as equivalent ratio) of the compound or its functional groups, taking into account the number and / or types of functional groups in the compound (especially compounds with specific reaction purposes, e.g., bifunctional compounds), the actual composition ratio in commercially available reagents, etc. The relationship between the molar ratio or equivalent ratio of functional groups and the weight or weight ratio of each component in the composition may be derived and calculated by an appropriate measurement method. For example, titration, infrared spectroscopy (IR spectroscopy), or nuclear magnetic resonance spectroscopy (NMR spectroscopy), but the present invention is not limited to these.

[0024] In one embodiment, the equivalent ratio of the isocyanate group of the isocyanate compound to the hydroxyl group of the polyol compound is 15:1 to 1:1, and preferably 9:1 to 3:1.

[0025] In one embodiment, the equivalent ratio of the hydroxyl group of the polyol compound to the amino group of the amine compound is 9:1 to 7:3.

[0026] In one embodiment, the equivalent ratio of the hydroxyl group of the hydroxyl-containing (meth)acrylate compound to the isocyanate group of the isocyanate compound is 1:1.1 to 1:1.5.

[0027] <2. Synthesis method for urea group-containing polyurethane acrylate resin>

[0028] <2.1 Prepolymerization Reaction> First, the isocyanate compound and the diluted monomer are mixed and heated for later use to prepare the subsequent first reaction reagent. The appropriate heating temperature may be 40°C to 70°C, for example, 45°C to 60°C.

[0029] Then, the polyol compound is added to the first reaction reagent at an appropriate temperature to carry out a polymerization reaction and obtain the corresponding urethane prepolymer.

[0030] In one embodiment, the prepolymerization reaction described above may be further modified by adding a catalyst. The catalyst may include an organometallic (e.g., tin, zinc, bismuth, or titanium) catalyst or an organobase catalyst. An organometallic catalyst may include, for example, dibutyltin dilaurate (DBTDL). An organobase catalyst may include, for example, 1,4-diazabicyclo[2.2.2]octane (DABCO).

[0031] In one embodiment, the total amount of urea group-containing polyurethane acrylate resin ultimately produced in the subsequent reaction is 1 kilogram, and the amount of catalyst added is 50 milligrams (mg) to 200 milligrams.

[0032] In one embodiment, the aforementioned prepolymerization reaction may be further modified by adding an inhibitor to reduce or delay the occurrence of unwanted polymerization reactions. The inhibitor may include, for example, dibutylhydroxytoluene (BHT) or 2,5-dihydroxytoluene.

[0033] In one embodiment, after the addition of the polyol compound is complete, the mixture may be allowed to react thoroughly for a certain period of time, for example, 1 to 4 hours, in an environment where the appropriate temperature described above is maintained. In one embodiment, it may be determined whether a sufficient ratio or amount of urethane prepolymer has already been produced by an appropriate detection method (e.g., viscosity measurement, spectral analysis, sample titration, or thermal analysis).

[0034] <2.2 Polymerization Reaction> Subsequently, after obtaining a sufficient ratio or amount of urethane prepolymer, a hydroxyl-containing (meth)acrylate compound is added to the urethane prepolymer, which has been maintained at the aforementioned appropriate temperature, and a polymerization reaction is carried out to obtain a polyurethane acrylate polymer.

[0035] In one embodiment, based on the total amount of urethane prepolymer and hydroxyl-containing (meth)acrylate compound added, the total number of moles of isocyanate groups in the urethane prepolymer is higher than the total number of moles of hydroxyl groups in the hydroxyl-containing (meth)acrylate compound. In other words, the resulting polyurethane acrylate polymer also contains isocyanate groups.

[0036] In one embodiment, after the addition of the hydroxyl-containing (meth)acrylate compound is complete, the mixture may be allowed to react thoroughly for a certain period of time, for example, 1 to 4 hours, in an environment at a suitable temperature. In one embodiment, it may be determined by the appropriate measurement method described above whether a sufficient ratio or amount of polyurethane acrylate polymer has already been produced.

[0037] <2.3 Denaturation Reaction> Next, an amine compound is added to the polyurethane acrylate polymer while maintaining the appropriate temperature as described above to induce a modification reaction. The modification reaction is essentially to amidate the isocyanate groups remaining in the polyurethane acrylate polymer to urea groups using the amine compound.

[0038] In one embodiment, based on the total amount of the urethane prepolymer, the total amount of the hydroxyl-containing (meth)acrylate compound, and the total amount of the amine compound added, the sum of the moles of hydroxyl groups in the hydroxyl-containing (meth)acrylate compound and the total amount of amino groups in the amine compound is higher than the total number of moles of isocyanate groups in the urethane prepolymer. In other words, after the modification reaction described above is complete, any isocyanate groups remaining in the polyurethane acrylate polymer can essentially be amidated. This is defined as the percentage ratio of the total weight of isocyanate groups to the total weight of the polyurethane acrylate polymer (i.e., the weight percentage of isocyanate groups (hereinafter referred to as the NCO value)) being less than 0.5%. The NCO value may be measured based on a standard method (e.g., ISO 14896:2009 Plastics - Polyurethane raw materials - Determination of isocyanate content).

[0039] In one embodiment, the amine compound may be added continuously / evenly (for example, by dropwise addition) over a period of 5 to 40 minutes (preferably 10 to 30 minutes).

[0040] Appropriate reaction temperature and appropriate rate of addition of amine compounds can lead to the amidation of isocyanate groups. However, if the local instantaneous concentration of the entire reactant of the added amine compound is excessively high, it may result in unexpected reactions (e.g., excessive or unforeseen crosslinking), potentially altering subsequent reactivity or physical properties (e.g., viscosity, glass transition temperature (Tg), tensile strength, or impact strength). For this reason, amine compounds must be added continuously and uniformly.

[0041] In one embodiment, after the addition of the amine compound is complete, the mixture may be allowed to react thoroughly for a certain period of time, for example, 1 to 2 hours, in an environment at a suitable temperature. In one embodiment, the NCO value may be measured by the standard method described above to determine whether the remaining isocyanate groups have been largely amidated to urea groups.

[0042] <3. Urea group-containing polyurethane acrylate resin> The urea group-containing polyurethane acrylate resin synthesized by the method described above may, for example, contain a polymer represented by the following formula 1.

[0043] [ka]

[0044] In Equation 1, R 1 R is either hydrogen or methyl. 2 R is an organic group containing an alkyl group, for example, a linked alkyl group containing 1 to 3 carbon atoms (i.e., -CH2-, -C2H4-, the group represented by formula 1-a below, or -C3H6-). 3 R is an organic group containing an aromatic group, such as a phenyl group, a group represented by formula 1-b below, a group represented by formula 1-c below, a group represented by formula 1-d below, or a group represented by formula 1-e below. 4 is an organic group, such as an alkyl group, an alkenyl group, or an alkyl ether group. The alkyl group mentioned above is, for example, a linked alkyl group containing 1 to 3 carbon atoms. The alkenyl group mentioned above is, for example, an allyl group. The alkyl ether group mentioned above is, for example, an ether group bonded to two alkyl groups each having 1 to 4 carbon atoms, and includes, but is not limited to, a dimethyl ether group (i.e., -CH2-O-CH2-), a methyl ethyl ether group (i.e., -CH2-O-C2H4-), a diethyl ether group (-C2H4-O-C2H4-), a dipropyl ether group (-C3H6-O-C3H6-), or a dibutyl ether group (-C4H8-O-C4H8-). [ka]

[0045] In Formula 1, R 5 is a linking group represented by the following Formula 2.

[0046] [Chemical formula]

[0047] In Formula 2, T 21 is an organic group, including, for example, an alkyl group, an alkenyl group, or an alkyl ether group. The definition thereof is the same as R 4 in the previous paragraph.

[0048] In Formula 2, T 2 is an organic group containing an aromatic group, for example, a phenyl group, a group represented by the following Formula 2-a, a group represented by the following Formula 2-b, a group represented by the following Formula 2-c, or a group represented by the following Formula 2-d. [Chemical formula]

[0049] In Formula 2, T 22 is hydrogen or a methyl group.

[0050] In Formula 1, R 6 is an organic group, for example, an organic group containing nitrogen. R 7 is hydrogen or a cyclic organic substance that is co-constructed with R 6 .

[0051] In Formula 1, m and n are integers of 1 or more. Based on consideration of physical properties, m is preferably less than 100, and n is preferably less than 100.

[0052] In one embodiment, the urea group-containing polyurethane acrylate resin of the present invention may be represented by the following Formula 1-1, Formula 1-2, Formula 1-3, Formula 1-4, or Formula 1-5.

[0053] [ka]

[0054] In equations 1-1, 1-2, 1-3, 1-4, and 1-5, R 1 , R 2 , R 3 , R 4 , R 5 The definitions of m and n are the same as in Equation 1.

[0055] In equations 1-1, 1-2, 1-3, 1-4, and 1-5, R 81 , R 82 , R 83 , R 84 Each of these is an independent organic group, for example, hydrogen, and the group represented by formula 1-f below. [ka]

[0056] In one embodiment, the formation of urea groups in the urea-containing polyurethane acrylate resin may be further detected by nuclear magnetic resonance spectroscopy. In one embodiment, when the aforementioned urea-containing polyurethane acrylate resin is measured by solution nuclear magnetic resonance spectroscopy, two signal peaks with a separation distance greater than 0.5 ppm are observed in the hydrogen spectrum, located in the range of 8 to 10 ppm, suggesting that active hydrogens of the amide group and the urea group are being generated, respectively. Since the urea-containing polyurethane acrylate resin molecule contains polar groups, the active hydrogens of the amide group and the urea group are affected by intramolecular and / or intermolecular hydrogen bonding, causing the detected signal peaks to be positioned at a downfield shift position.

[0057] <4. Resin composition>

[0058] The resin composition contains at least the urea group-containing polyurethane acrylate resin described above. In other words, the resin composition contains at least a resin obtained by the reaction of an isocyanate compound, a polyol compound, a hydroxyl-containing (meth)acrylate compound, and an amine compound.

[0059] In one embodiment, the resin composition may further contain one or more additives. The additives may be added appropriately during and / or after the synthesis of the urea group-containing polyurethane acrylate resin. In other words, the additives may be part of the resin composition.

[0060] The additives may include, but are not limited to, diluting monomers, flame retardants, inhibitors, mold release agents, curing agents, viscosity modifiers, wetting and dispersing agents, or low-shrinkage agents.

[0061] <5. Applications of Resin Compositions> In one embodiment, the mechanical properties of cast plates manufactured from the resin composition were compared, and the urea-containing polyurethane acrylate resin of the present invention and the unmodified polyurethane acrylate resin (i.e., polyurethane acrylate resin without urea) were found to be at least equivalent in basic performance. They are even superior in specific applications (e.g., composite material applications).

[0062] In one embodiment, the resin composition containing the urea group-containing polyurethane acrylate resin described above can be mixed with other materials to form a composite material. For example, the resin composition of the above embodiment (the resin composition containing the urea group-containing polyurethane acrylate resin) may be mixed with a fibrous material to form a fiber-reinforced polymer (FRP). The fibrous material described above may include glass fibers, carbon fibers, polymer fibers (e.g., synthetic fibers), or other fibers. Fiber-reinforced polymers can have high strength and lightweight properties and are widely applied in fields such as aerospace, automotive, and construction.

[0063] In one embodiment, the total amount of the resin composition is 100 parts by weight, and the total amount of the fiber material is 67 to 240 parts by weight.

[0064] In one embodiment, the fibers contained in the composite material are carbon fibers, and the composite material may be a carbon fiber reinforced polymer (CFRP). Since the urea group-containing polyurethane acrylate resin of the present invention forms urea groups by modifying the polyurethane acrylate resin structure, in the carbon fiber reinforced polymer, the modified urea groups can form polar interactions (e.g., hydrogen bonds) or bonds with the carbon fiber surface, giving the composite material a desirable interlaminar shear strength (ILSS) that is equivalent to or better than that of commercially available epoxy resins. For this reason, the urea group-containing polyurethane acrylate resin and / or resin composition thereof of the present invention can be given a wider range of applications and even better quality.

[0065] In one embodiment, the resin composition of the urea group-containing polyurethane acrylate resin described above may be dissolved in a suitable solvent or liquid curing agent (e.g., methyl ethyl ketone peroxide) and then impregnated into a fiber material before use.

[0066] <6. Examples and Comparative Examples>

[0067] <6.1 Preparation of Resin Composition>

[0068] <Example 1> Resin composition 1 280.0 grams of poly(methylenephenyl isocyanate) (manufacturer: Wanhua, model number: PM200, isocyanate group content: 2.083 equivalents), 0.106 grams of dibutylhydroxytoluene (inhibitor), and 0.148 grams of dibutyltin dilaurate (catalyst) were dispersed in 363 grams of methyl methacrylate (diluted monomer), uniformly mixed in a reaction vessel, and heated to 45°C to 60°C for later use. Subsequently, 125.0 grams of propylene glycol (manufacturer: Oriental Union Chemical, average molecular weight 400, hydroxyl group content: 0.625 equivalents) were added dropwise to the reaction vessel. The addition time was 40 to 60 minutes, during which the temperature was controlled to be below 60°C. After the addition was complete, the temperature was maintained for 2 to 4 hours. Next, 180.75 grams of 2-hydroxyethyl methacrylate (HEMA, hydroxyl group content 1.389 equivalents) was added dropwise. The addition time was 40 to 60 minutes, during which the temperature was controlled to below 60°C. After the addition was complete, the temperature was maintained for 1 to 2 hours. Finally, 7.99 grams of polyetheramine (D230, average molecular weight 230 g / mol, amino group content 0.069 equivalents) was added dropwise to the reaction vessel described above. The addition time was 10 to 30 minutes, during which the temperature was controlled to below 60°C. After the addition was complete, the temperature was maintained for 1 to 2 hours. After confirming that the NCO value was less than 0.5%, 90.75 grams of methyl methacrylate was added to dilute the mixture, and the finished product was designated as resin composition 1. Its viscosity was approximately 151 centipoise (cps).

[0069] <Example 2> Resin composition 2 The difference between Example 2 and Example 1 is that 7.99 grams of polyetheramine was replaced with 7.30 grams of 4,4'-diaminodicyclohexylmethane (containing 0.069 equivalents of amino groups). The resulting product after the reaction was designated as resin composition 2, and its viscosity was approximately 213 cps.

[0070] <Example 3> Resin composition 3 The difference between Example 3 and Example 1 is that 7.99 grams of polyetheramine was replaced with 5.92 grams of isophoronediamine (containing 0.069 equivalents of amino groups). The resulting product after the reaction was designated as resin composition 3, and its viscosity was approximately 128 cps.

[0071] <Example 4> Resin composition 4 The difference between Example 4 and Example 1 is that 7.99 grams of polyetheramine was replaced with 3.00 grams of piperazine (containing 0.069 equivalents of amino groups). The resulting product after the reaction was designated as resin composition 4, and its viscosity was approximately 133 cps.

[0072] <Example 5> Resin composition 5 The difference between Example 5 and Example 1 is that 7.99 grams of polyetheramine was replaced with 15.97 grams of polyetheramine (containing 0.139 equivalents of amino groups). The final product after the reaction was designated as resin composition 5, and its viscosity was approximately 190 cps.

[0073] <Example 6> Resin composition 6 The difference between Example 6 and Example 1 is that 7.99 grams of polyetheramine was replaced with 23.96 grams of polyetheramine (containing 0.208 equivalents of amino groups). The resulting product after the reaction was designated as resin composition 6, and its viscosity was approximately 239 cps.

[0074] <Comparative Example 1> Resin composition 7 The difference between Comparative Example 1 and Example 1 is that 125.0 grams of propylene glycol was replaced with 138.9 grams of propylene glycol (containing 0.694 equivalents of hydroxyl groups), and no amine compound was added. The final product after the reaction was designated as resin composition 7, and its viscosity was approximately 121 cps.

[0075] <6.2 Manufacturing of Composite Materials>

[0076] <Example 7> Composite Material 1 Based on parts by weight, 100 parts by weight of the aforementioned resin composition 1 was obtained, and 0.2 parts of a 6% cobalt salt accelerator and 1 part by weight of methyl ethyl ketone peroxide (MEKP) were added. After thorough mixing, it was impregnated into commercially available carbon fiber woven fabric (manufacturer: SHENG PENG APPLIED MATERIALS CO., LTD., model number: carbon fiber woven-3K). After molding by vacuum-assisted resin injection molding (VARTM), it was cured at room temperature for 24 hours, and then cured at 105°C for 2 hours to obtain the finished product of Example 7.

[0077] <Example 8> Composite Material 2 The difference between Example 8 and Example 7 is that resin composition 1 is replaced with resin composition 2.

[0078] <Example 9> Composite Material 3 The difference between Example 9 and Example 7 is that resin composition 1 is replaced with resin composition 3.

[0079] <Example 10> Composite Material 4 The difference between Example 10 and Example 7 is that resin composition 1 is replaced with resin composition 4.

[0080] <Example 11> Composite Material 5 The difference between Example 11 and Example 7 is that resin composition 1 is replaced with resin composition 5.

[0081] <Example 12> Composite Material 6 The difference between Example 12 and Example 7 is that resin composition 1 is replaced with resin composition 6.

[0082] <Comparative Example 2> Composite Material 7 The difference between Comparative Example 2 and Example 7 lies in the fact that resin composition 1 is replaced with resin composition 7.

[0083] <Comparative Example 3> Composite Material 8 Based on parts by weight, 31 parts of a commercially available aliphatic polyetheramine curing agent (manufacturer: Huntsman Corporation) were added to 100 parts of bisphenol F type epoxy resin mixed with bisphenol A (manufacturer: Nanya Plastics), and after thorough mixing, the mixture was impregnated into a commercially available carbon fiber woven fabric. After molding using the technique described above, the material was cured at 40°C for 8 hours, and then cured at 70°C for 8 hours to achieve complete curing, resulting in the finished product of Comparative Example 3.

[0084] <Comparative Example 4> Composite Material 9 Based on parts by weight, 100 parts of commercially available bisphenol A type vinyl resin (manufacturer: SWANCOR) were mixed with 0.2 parts of a 6% cobalt salt accelerator, 0.05 parts of an accelerator N,N-dimethylaniline (DMA), and 1 part of methyl ethyl ketone peroxide. After thorough mixing, the mixture was impregnated into a commercially available carbon fiber woven fabric. After molding using the technique described above, the mixture was cured at room temperature for 24 hours, and then cured at 105°C for 2 hours to achieve complete curing, resulting in the finished product of Comparative Example 4.

[0085] <6.3 Evaluation Items>

[0086] <Measurement of average interlaminar shear strength (unit: MPa)> Based on the ISO 14130 specification, five samples measuring 20mm x 10mm x 2mm were cut from each of the composite material products from Examples 7 to 12 and Comparative Examples 2 to 4. The interlaminar shear strength was then measured on these samples using a universal material testing machine (manufacturer: Instron, model number: 5892), and the average interlaminar shear strength was calculated. The measurement results are shown in Tables 1 to 3.

[0087] <Mechanical properties testing of cast plates> Mechanical properties tests were performed on each of the resin compositions 1 to 7 described above (the curing method was the same as the conditions for manufacturing the composite materials described above, with 0.2 parts of 6% cobalt salt accelerator and 1 part of methyl ethyl ketone peroxide, cured at room temperature for 24 hours, and then cured at 105°C for 2 hours). The tensile test standard was ASTM D638, the bending test standard was ASTM D790, and the heat distortion temperature test standard was ASTM D648. The specific test results are shown in Table 4.

[0088] Comparison of interlaminar shear strength of urea group-containing polyurethane acrylate resin composite materials modified with different amine compounds and unmodified polyurethane acrylate resin composite materials.

[0089] [Table 1]

[0090] As shown in Table 1, urea-containing polyurethane acrylate resin composites exhibit superior interlaminar shear strength compared to unmodified polyurethane acrylate resin composites.

[0091] Comparison of interlaminar shear strength of urea group-containing polyurethane acrylate resin composites and epoxy resin composites modified with different amine compounds

[0092] [Table 2]

[0093] As shown in Table 2, epoxy resin structures have high polarity and good interlaminar adhesion with carbon fibers, and therefore it is well known that epoxy resin composite materials generally have excellent interlaminar shear strength. Urea group-containing polyurethane acrylate resin composite materials can achieve interlaminar shear strength close to that of epoxy resin composite materials.

[0094] Comparison of interlaminar shear strength of urea group-containing polyurethane acrylate resin composites, epoxy resin composites, and vinyl resin composites modified with different ratios of polyetheramine.

[0095] [Table 3]

[0096] As shown in Table 3, increasing the reaction equivalent number of polyetheramine (i.e., increasing the urea group equivalent number of the polyurethane acrylate resin) can effectively increase the adhesion between the carbon fiber and the resin, and can also provide better interlaminar shear strength than epoxy resin composite materials.

[0097] Mechanical Properties Test

[0098] [Table 4]

[0099] As shown in Table 4, the modified urea group-containing polyurethane acrylate resin has equivalent mechanical properties to the unmodified polyurethane acrylate resin. [Industrial applicability]

[0100] The modified urea group-containing polyurethane acrylate resin composite material of the above-described embodiment of the present invention can be applied directly or indirectly to fields such as aerospace, automotive, and construction. The modified urea group-containing polyurethane acrylate resin can also be used to replace unmodified polyurethane acrylate resin and may have superior quality or applicability.

Claims

1. A resin composition comprising a urea group-containing polyurethane acrylate resin represented by the following formula 1, 【Transformation 7】 【Transformation 8】 Resin composition.

2. Diluted monomer It further includes, The total amount of the urea group-containing polyurethane acrylate resin is 100 parts by weight, and the total amount of the diluting monomer is 30 to 45 parts by weight. The resin composition according to claim 1.

3. Inhibitors It further includes, The total amount of the urea group-containing polyurethane acrylate resin is 100 parts by weight, and the total amount of the inhibitor is 0.01 to 0.03 parts by weight. The resin composition according to claim 1.

4. A resin composition according to any one of claims 1 to 3, Textile materials and Includes, The total amount of the resin composition is 100 parts by weight, and the total amount of the fiber material is 67 to 240 parts by weight. Composite material.

Citation Information

Patent Citations

  • Hyperbranched water-based polyurea acrylic resin, carbon-coated slurry, carbon-coated aluminum foil and preparation method and application of hyperbranched water-based polyurea acrylic resin

    CN119978299A

  • Composition for producing polyurethane elastomer and production of polyurethane elastomer using the same composition

    JP1992008717A

  • Tin-free polyurethane aqueous dispersion

    JP2011094141A

  • Laminate film for decorating molded article, paint composition and decorative molded article

    JP2015145103A

  • Water dispersion of polyurethane urea-acrylic composite resin

    JP2016204571A