Method for evaluating the corrosion resistance of separators

The method addresses the inefficiencies of existing corrosion resistance evaluation by using an acid treatment and potential measurement process to quickly and economically assess the corrosion resistance of fuel cell separators, ensuring their reliability.

JP7955429B1Active Publication Date: 2026-11-24HONDA MOTOR CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2025094716
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2025-06-06
Publication Date
2026-11-24
Estimated Expiration
2045-06-06

AI Technical Summary

Technical Problem

Existing methods for evaluating the corrosion resistance of fuel cell separators are time-consuming and costly, and the coating layers on metal substrates have weak points that lead to insufficient corrosion resistance.

Method used

A method involving an acid treatment step followed by a potential measurement step to assess the natural potential of the separator, using specific acidic solutions and electrochemical measurement circuits to determine the corrosion resistance of separators with coating layers.

Benefits of technology

This method allows for rapid and cost-effective evaluation of corrosion resistance, identifying potential corrosion issues in separators, thereby ensuring their suitability for fuel cell operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955429000001_ABST
    Figure 0007955429000001_ABST
Patent Text Reader

Abstract

Time reduction and cost reduction in the corrosion resistance evaluation method for separators. [Solution] The separator for fuel cells comprises a metal substrate and a coating layer formed on the surface of the metal substrate. The corrosion resistance of the separator can be evaluated by a corrosion resistance evaluation method having an acid treatment step and a potential measurement step. Specifically, in the acid treatment step, the separator is immersed in an acidic solution. In the potential measurement step, the natural potential of the separator after the acid treatment step is measured.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present disclosure relates to a method for evaluating the corrosion resistance of a separator. [Background Art]

[0002] A unit cell of a fuel cell stack is configured by sandwiching a membrane electrode assembly between a pair of separators for a fuel cell. During operation of the fuel cell stack, a reaction gas containing moisture and a cooling medium such as cooling water come into contact with the separators for a fuel cell. Therefore, corrosion resistance is required for the separators for a fuel cell. Accordingly, conventionally, it has been proposed to configure a separator for a fuel cell by forming a coating layer exhibiting corrosion resistance on a metal base material.

[0003] The coating layer inevitably has weak portions such as cracks and pinholes. Ions may elute from such weak portions. That is, despite the coating layer being provided on the metal base material, the corrosion resistance of the separators for a fuel cell becomes insufficient.

[0004] Japanese Patent Application Publication No. 2004-31256 (Patent Document 1), Japanese Patent Application Publication No. 2012-59485 (Patent Document 2), and Japanese Patent Application Publication No. 2022-110360 (Patent Document 3) disclose methods for evaluating the corrosion resistance of a separator. In addition, "NEDO PEFC Cell Evaluation and Analysis Protocol 2023 Edition", New Energy and Industrial Technology Development Organization (NEDO), issued in July 2023, URL: https: / / www.nedo.go.jp / content / 100963953.pdf (Non-Patent Document 1), pages 42 to 43, describes evaluating the amount of metal elution as a corrosion resistance test method for a separator. [Prior Art Documents] [Patent Documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 2004-31256 [Patent Document 2] Japanese Patent Publication No. 2012-59485 [Patent Document 3] Japanese Patent Publication No. 2022-110360 [Non-patent literature]

[0006] [Non-Patent Document 1] "NEDO PEFC Cell Evaluation and Analysis Protocol 2023 Edition," New Energy and Industrial Technology Development Organization (NEDO), published July 2023, URL: https: / / www.nedo.go.jp / content / 100963953.pdf [Overview of the Initiative] [Problems that the invention aims to solve]

[0007] In particular, the evaluation method described on pages 42-43 of the NEDO PEFC Cell Evaluation and Analysis Protocol 2023 edition requires a long time (approximately one month) to obtain evaluation results. Furthermore, it is costly.

[0008] This disclosure aims to solve the problems described above. [Means for solving the problem]

[0009] Aspects of the present disclosure are methods for evaluating the corrosion resistance of a separator for a fuel cell, comprising a metal substrate and a coating layer formed on the surface of the metal substrate, the methods comprising: an acid treatment step of immersing the separator in an acidic solution; and a potential measurement step of measuring the natural potential of the separator after the acid treatment step. [Effects of the Invention]

[0010] According to this disclosure, it is possible to evaluate whether or not a separator has excellent corrosion resistance in a short time and at low cost. [Brief explanation of the drawing]

[0011] [Figure 1]Figure 1 is a cross-sectional view of the main part of a unit cell that makes up a fuel cell stack. [Figure 2] Figure 2 is a cross-sectional view of the separator along the thickness direction. [Figure 3] Figure 3 is a schematic diagram showing the situation under which the acid treatment process is carried out. [Figure 4] Figure 4 is a schematic diagram of a potential measurement system including an electrochemical measurement circuit. [Figure 5] Figure 5 is a graph showing the correlation between the spontaneous potential of the sample separated from the separator and the amount of metal ions (iron ions) eluted. [Modes for carrying out the invention]

[0012] Figure 1 is a cross-sectional view of the main part of a unit cell 10 that constitutes a fuel cell stack (not shown). Note that the dimensions of each component shown in Figure 1 do not necessarily reflect the actual dimensions. The same applies to Figures 2 to 4.

[0013] The unit cell 10 comprises a membrane electrode assembly (MEA) 12 and two fuel cell separators 20. The MEA 12 has an electrolyte membrane 14, an anode electrode 16 provided on one end face of the electrolyte membrane 14, and a cathode electrode 18 provided on the other end face of the electrolyte membrane 14. The anode electrode 16 has a first gas diffusion layer 161 and a first electrode catalyst layer 162, and the cathode electrode 18 has a second gas diffusion layer 181 and a second electrode catalyst layer 182. The electrolyte membrane 14 is interposed between the first electrode catalyst layer 162 and the second electrode catalyst layer 182.

[0014] One of the two separators 20 is an anode-side separator 22, and the other of the two separators 20 is a cathode-side separator 24. The anode-side separator 22 has a fuel gas flow channel 221 and a first cooling medium flow channel 222. The cathode-side separator 24 has an oxidant gas flow channel 241 and a second cooling medium flow channel 242. In the fuel cell stack configured by stacking the unit cells 10, the first cooling medium flow channel 222 of the anode-side separator 22 and the second cooling medium flow channel 242 of the cathode-side separator 24 communicate with each other to form a single cooling medium flow channel.

[0015] Hereinafter, the anode-side separator 22 will be described as an example. The anode-side separator 22 includes a metal base material 30 and a coating layer 32 covering both surfaces of the metal base material 30. In the illustrated example, the coating layer 32 includes an intermediate layer 321 formed on the metal base material 30, and a conductive layer 322 formed on the intermediate layer 321 and made of a conductive material. It should be noted that it is not essential to cover both surfaces of the metal base material 30 with the coating layer 32 as in the illustrated example, and the coating layer 32 may be formed only on the surface of the metal base material 30 facing the first gas diffusion layer 161.

[0016] The material of the metal base material 30 is preferably a metal that exhibits sufficient corrosion resistance and has low electrical resistance. A specific example of such a metal is stainless steel. Since stainless steel is inexpensive, the material cost can also be reduced. However, the material of the metal base material 30 is not limited to stainless steel.

[0017] As the material of the intermediate layer 321, a substance with excellent corrosion resistance is selected. Preferable examples of such materials include metals or metal compounds. When the material of the metal base 30 is the above stainless steel and the material of the conductive layer 322 is carbon described later, preferable specific examples of the material of the intermediate layer 321 include Ti (titanium), titanium carbide (titanium carbide; TiC or titanium carbonitride; TiCN), and titanium nitride (titanium nitride; TiN). In this combination, the intermediate layer 321 is favorably bonded to both the metal base 30 and the conductive layer 322. However, the material of the intermediate layer 321 is not limited to titanium, titanium carbide, or titanium nitride. Examples of other materials include Cr (chromium), Nb (niobium), Sn (tin), and CrN (chromium nitride).

[0018] A preferable example of the material of the conductive layer 322 is carbon. Typical examples of carbon include amorphous carbon such as diamond-like carbon (DLC). However, the carbon may be polycrystalline graphite or graphite-like carbon (GLC).

[0019] The cathode-side separator 24 is configured similarly to the anode-side separator 22. Therefore, a detailed description of the configuration of the cathode-side separator 24 is omitted. In the following description, when the anode-side separator 22 and the cathode-side separator 24 are not distinguished, they are referred to as "separator 20".

[0020] In the separator 20, the thickness of the coating layer 32 is about several hundred nm. That is, the coating layer 32 is a thin layer. Therefore, as shown in FIG. 2, fine defects 40 are inevitably generated in the coating layer 32. The fine defects 40 are defects such as pinholes or cracks. When operating the fuel cell stack, the reaction gas can penetrate into the fine defects 40. Therefore, when the fine defects 40 extend to the surface of the metal base 30, moisture contained in the reaction gas may come into contact with the surface of the metal base 30 and contribute to corrosion of the metal base 30.

[0021] Therefore, in this embodiment, after manufacturing the separator 20, the corrosion resistance of the separator 20 is evaluated. That is, whether or not the metal substrate 30 is susceptible to corrosion is determined by the corrosion resistance evaluation method described below. It is preferable to perform the corrosion resistance evaluation method before assembling the unit cell 10.

[0022] The corrosion resistance evaluation method comprises an acid treatment step and a potential measurement step. As shown in Figure 3, in the acid treatment step, the sample 21 is subjected to acid treatment. Here, the sample 21 is a cut piece formed by cutting out a part of the separator 20.

[0023] Specifically, the tester places the sample 21 inside a sealed container 50 containing the acidic solution AS1, and then seals the container 50. This prevents the acidic solution AS1 from evaporating.

[0024] Acidic solution AS1 can be obtained, for example, by dissolving NaF in deionized water. As additives such as NaF dissolve, fluoride ions (F) are released. - This occurs. The concentration of fluoride ions is preferably 5 ppm to 20 ppm. At concentrations below 5 ppm, the variation in spontaneous potential is large in the potential measurement process described later. Furthermore, the variation in spontaneous potential saturates at a fluoride ion concentration of 20 ppm. Therefore, if the concentration of fluoride ions in the acidic solution AS1 is greater than 20 ppm, the material cost related to the additive will increase significantly.

[0025] Furthermore, the pH of the acidic solution AS1 is adjusted by adding an acid, such as dilute sulfuric acid. The pH of the acidic solution AS1 is preferably between 2 and 4.

[0026] Next, the tester activates the temperature controller 54 and heater 56 to raise the water in the constant temperature bath 52 to a predetermined temperature. This heating process turns the water in the constant temperature bath 52 into a hot water bath HB1. The predetermined temperature is preferably in the range of 60°C to 90°C, and more preferably 70°C.

[0027] The temperature of the water bath HB1 is kept approximately constant by the temperature controller 54 and the heater 56. As a result, the heat from the water bath HB1 is transferred to the acidic solution AS1 via the sealed container 50, and the temperature of the acidic solution AS1 becomes approximately equal to the temperature of the water bath HB1. That is, the temperature of the acidic solution AS1 is adjusted to, for example, a range of 60°C to 90°C, preferably to 70°C.

[0028] Immersing the sample 21 in the acidic solution AS1 stabilizes the surface of the conductive layer 322. In other words, foreign matter adhering to the surface of the conductive layer 322 can be removed. Furthermore, the functional groups in the conductive layer 322 become chemically stable under the operating environment of the fuel cell stack. In addition, the surface of the intermediate layer 321 (e.g., a metal surface) exposed to the micro-defects 40 of the conductive layer 322 also becomes chemically stable under the operating environment of the fuel cell stack.

[0029] Furthermore, it is preferable that the time for which the sealed container 50 is immersed in the water bath HB1 is at least 72 hours (3 days). This ensures that the surface state of the conductive layer 322 is reliably stabilized. By immersing multiple samples 21 in the acidic solution AS1 in multiple sealed containers 50 and simultaneously immersing multiple sealed containers 50 in the water bath HB1 in the constant temperature bath 52, multiple samples 21 can be treated with acid simultaneously.

[0030] After a predetermined time has elapsed since the sealed container 50 was immersed in the constant temperature bath 52, the sealed container 50 was removed from the constant temperature bath 52, and then the sample 21 was removed from the sealed container 50. Next, the sample 21 was washed with pure water and then dried. Next, the potential measurement process was carried out using this sample 21 under predetermined conditions. The predetermined conditions are, for example, those conforming to the "Corrosion Resistance Test Method (Anode Corrosion)" on page 42 of Non-Patent Document 1 mentioned above.

[0031] To perform the potential measurement process, an electrochemical measurement circuit 60, as shown in Figure 4, is configured. The potential measurement system 61, including this electrochemical measurement circuit 60, will be briefly described below. The potential measurement system 61 comprises a constant temperature bath 62, a measurement cell 65, a potentiostat 67, and an information processing computer 68. Hereinafter, the computer may be referred to as "PC". Note that a galvanostat or a potentio-galvanostat may be used instead of the potentiostat 67.

[0032] The measuring cell 65 has a measuring container 70. The measuring container 70 has a first container 72 and a second container 74. An acidic solution AS2 is stored in the container body 721 of the first container 72, and a saturated potassium chloride aqueous solution KS is stored in the second container 74. The first container 72 and the second container 74 are connected via a salt bridge 76. The salt bridge 76 forms an electrical path between the acidic solution AS2 and the saturated potassium chloride aqueous solution KS.

[0033] A bubbling tube 78 is provided in the first container 72. One end of the bubbling tube 78 is located outside the lid 722 of the first container 72. One end of the bubbling tube 78 is connected to a source of inert gas such as argon (e.g., a gas cylinder). The other end of the bubbling tube 78 is immersed in the acidic solution AS2. Therefore, it is possible to supply inert gas to the acidic solution AS2 inside the container body 721.

[0034] The counter electrode 80 and sample 21 are further immersed in the acidic solution AS2. The material of the counter electrode 80 is, for example, platinum. The counter electrode 80 is electrically connected to the potentiostat 67 via a first wire 82. The sample 21 is electrically connected to the potentiostat 67 via a second wire 84 and functions as the working electrode. A reference electrode 86, held in a second container 74, is further electrically connected to the potentiostat 67 via a third wire 88. The reference electrode 86 is, for example, a silver / silver chloride electrode (SSCE). Depending on the type of reference electrode 86, it is also possible to immerse the reference electrode 86 in the acidic solution AS2 within the first container 72. In this case, the second container 74 is not necessary.

[0035] The lid 722 of the first container 72 has first insertion tube sections 723 to fourth insertion tube sections 726. A bubbling tube 78 is inserted through the first insertion tube section 723, and a first conductor 82 is inserted through the second insertion tube section 724. A second conductor 84 is inserted through the third insertion tube section 725, and a salt bridge 76 is inserted through the fourth insertion tube section 726. A sealing material 73 is filled between the first insertion tube section 723 and the bubbling tube 78. The same applies to the second insertion tube sections 724 to fourth insertion tube sections 726.

[0036] The lid portion 722 further includes a cooling section 727. In the illustrated example, the cooling section 727 includes a Diemroth condenser 728. Since the Diemroth condenser 728 is well known, a detailed explanation is omitted.

[0037] The acidic solution AS2 is preferably prepared in accordance with the "test solution" shown in the "corrosion resistance test method (anodic corrosion)" on page 42 of Non-Patent Document 1 mentioned above. That is, the pH of the acidic solution AS2 is preferably 2.95 to 3.05 (3 ± 0.05), and more preferably 3. The pH of the acidic solution AS2 is prepared, for example, with an acid such as dilute sulfuric acid.

[0038] Furthermore, the acidic solution AS2 can be obtained, for example, by dissolving NaF in deionized water, similar to the acidic solution AS1 described above. The concentration of fluoride ions is preferably 3 ppm. In addition, the temperature of the acidic solution AS2 is preferably in the range of 78°C to 82°C (80±2°C), and more preferably 80°C.

[0039] The information processing PC 68 collects information about the potential (the natural potential of sample 21) obtained by the potentiostat 67 according to a program stored in its memory. The information about the natural potential is displayed on the monitor 681 of the information processing PC 68.

[0040] The potential measurement process is carried out using the potential measurement system 61 configured in this manner, as follows.

[0041] First, the tester prepares the acidic solution AS2, and immerses the bubbling tube 78, counter electrode 80, sample 21, and salt bridge 76 in the acidic solution AS2. Furthermore, the first container 72, which is sealed by attaching the lid 722 to the container body 721, is immersed in water in the constant temperature bath 62. Subsequently, the tester electrically connects the counter electrode 80, sample 21, and reference electrode 86 to the potentiostat 67, and connects one end of the bubbling tube 78 to the inert gas supply source.

[0042] The tester then supplies a cooling medium such as cooling water to the Diebroth condenser 728, which constitutes the cooling unit 727. The tester also supplies an inert gas such as argon to the acidic solution AS2 via the bubbling tube 78. This causes bubbling in the acidic solution AS2. The tester then activates the temperature controller 64 and heater 66 to raise the water in the constant temperature bath 62 to a predetermined temperature (78°C to 82°C). This heating causes the water in the constant temperature bath 62 to become the hot water bath HB2.

[0043] The heat from the water bath HB2 is transferred to the acidic solution AS2 via the first container 72, so the temperature of the acidic solution AS2 becomes approximately equal to the temperature of the water bath HB2. That is, the temperature of the acidic solution AS2 becomes 78°C to 82°C (80±2°C). Furthermore, since an inert gas is supplied to the acidic solution AS2, a portion of the acidic solution AS2 evaporates easily. The vapor of the acidic solution AS2 is cooled in the cooling unit 727 (Diebroth condenser 728), causing it to condense and return to the liquid phase. The liquid phase of the acidic solution AS2 flows down from the cooling unit 727 to the container body 721. The inert gas is also discharged into the atmosphere from the cooling unit 727.

[0044] After the temperature of the water bath HB2 reaches approximately 80±2℃ and stabilizes, it is left to stand for 30 minutes to 1 hour. This stabilizes the temperature of the acidic solution AS2. After that, the tester starts the potentiostat 67 and the information processing PC 68. Note that the potentiostat 67 and the information processing PC 68 may be started before or after starting the temperature controller 64 and the heater 66. The potentiostat 67 measures the potential, and the information processing PC 68 records the potential. The tester continues measuring and recording the potential for approximately 5 to 60 minutes. Here, as described above, since the surface state of the conductive layer 322 is stabilized, it is presumed that the variation in potential is suppressed.

[0045] The potential is the natural potential of sample 21 with respect to the reference electrode 86. If no corrosion has occurred in sample 21, in other words, if no metal ions have leached from the metal substrate 30 (see Figure 2) of sample 21, the natural potential is approximately constant. In contrast, if metal ions have leached from the metal substrate 30 of sample 21, the natural potential will decrease (become larger on the negative side). Note that if the material of the metal substrate 30 is stainless steel, the metal ions will mainly be iron ions. The following explanation will use this case as an example.

[0046] As shown in Figure 5, a correlation is observed between the level of the natural potential (nobility) and the amount of iron ions eluted as measured by the "corrosion resistance test method (anodic corrosion)" described above. The program stored in the memory of the information processing PC68 contains the correlation shown in Figure 5. Note that Figure 5 shows the correlation when the material of the metal substrate 30 is stainless steel, the material of the intermediate layer 321 is titanium, and the material of the conductive layer 322 is DLC.

[0047] As can be seen from Figure 5, when the natural potential is lower than 0.09V, the amount of iron ions eluted exceeds the acceptable range. In other words, when the measured value of the natural potential is 0.09V or higher, the amount of iron ions eluted is sufficiently low and below the acceptable range. Therefore, in this embodiment, the control value for the natural potential is set to, for example, 0.1V. In this case, the information processing PC 68 shown in Figure 4 determines that the sample is "acceptable" when the measured value of the natural potential is 0.1V or higher, and displays this on the monitor 681. Thus, the tester can ascertain that the sample 21 is an acceptable product via the monitor 681.

[0048] Furthermore, according to the "Corrosion Resistance Test Method (Anode Corrosion)" described above, the passing standard (amount of iron ions eluted) when the voltage is applied for 60 hours is 1.0 μg / cm³. 2 The following is the result. On the other hand, according to Figure 5, the amount of iron ions eluted was 1.0 μg / cm³. 2 The natural potential at which this occurs is 0.08V. Therefore, the control value for the natural potential may be set to a predetermined value between 0.08V and less than 0.1V.

[0049] If the material of the metal substrate 30 shown in Figure 2 is a metal other than stainless steel, the tester investigates the correlation between the natural potential and the amount of mainly eluted metal ions, as described above. The same procedure applies if the material of the intermediate layer 321 is other than titanium, or if the material of the conductive layer 322 is other than DLC. The tester creates a program that includes this correlation and stores it in the storage device of the information processing PC 68 shown in Figure 5.

[0050] Since sample 21 is deemed acceptable, the separator 20 (see Figure 1), which is the base material of sample 21, is also judged to be acceptable. In other words, this separator 20 is evaluated to have good corrosion resistance. Therefore, it is expected that corrosion will be less likely to occur in the unit cell 10 using this separator 20 when the fuel cell stack is in operation.

[0051] As described above, with the corrosion resistance evaluation method according to this embodiment, evaluation results can be obtained for one sample 21 (see Figures 3 and 4) in approximately 73 to 75 hours, including the time required for the acid treatment process and the time required for the potential measurement process. In other words, the time required to obtain evaluation results can be shortened compared to quantitative analysis using inductively coupled plasma (ICP). In other words, it is possible to efficiently determine whether or not the separator 20 (see Figure 1) has excellent corrosion resistance. Moreover, since an ICP analyzer is not required, the analysis cost can be reduced.

[0052] Furthermore, if the coating layer 32 is formed on only one of the two surfaces of the metal substrate 30, masking is applied to the other surface where the coating layer 32 is not formed before carrying out the acid treatment process. Masking prevents metal ions from eluting from the other surface where the coating layer 32 is not formed.

[0053] This embodiment provides the following effects.

[0054] According to the above corrosion resistance evaluation method, even if the separator 20 has a coating layer 32 (see Figures 1 and 2) with excellent corrosion resistance, which tends to result in large variations in its natural potential, it is possible to evaluate whether or not the separator 20 has excellent corrosion resistance based on the natural potential of a sample 21, which is a part of the separator 20. Therefore, the pass / fail status of the separator 20 can be determined in a short time and at low cost.

[0055] In the separator 20, the material of the metal substrate 30 is stainless steel, the material of the intermediate layer 321 of the coating layer 32 is a metal such as Ti or a metal compound such as TiC, and the material of the conductive layer 322 of the coating layer 32 is carbon. According to the above corrosion resistance evaluation method, it is easy to evaluate whether or not microscopic defects 40 (see Figure 2) exist in the coating layer 32 of such a separator 20, and it is easy to determine whether or not the separator 20 is suitable for actual use in a unit cell 10 (fuel cell stack).

[0056] The acidic solution AS1 (see Figure 3) used in the acid treatment process has a pH of 2 to 4 and a temperature of 60°C to 90°C. By treating sample 21 with such an acidic solution AS1, the surface of sample 21 can be stabilized.

[0057] Acidic solution AS1 contains 5 ppm to 20 ppm of fluoride ions. In this case, variations in the spontaneous potential of sample 21 can be suppressed during the potential measurement process.

[0058] As shown in Figure 5, in the above corrosion resistance evaluation method, if the measured natural potential of sample 21 is above a predetermined value, typically 0.1V or higher, sample 21 is judged to be a satisfactory product. This is because, based on the correlation between the natural potential and the amount of metal ions eluted from the metal substrate 30, it can be evaluated that the amount of metal ions eluted is sufficiently small and that the separator 20 has excellent corrosion resistance.

[0059] As shown in Figure 4, an electrochemical measurement circuit 60 is configured during the potential measurement process. This allows for easy and highly accurate measurement of the natural potential of the sample 21.

[0060] The acidic solution AS2 used in the potential measurement process has a pH of 2.95 to 3.05 and a temperature of 78°C to 82°C. Furthermore, the acidic solution AS2 contains 3 ppm of fluoride ions. Therefore, it is possible to obtain the spontaneous potential of sample 21 under conditions similar to those described in the "Corrosion Resistance Test Method (Anode Corrosion)" in Non-Patent Document 1.

[0061] The following additional information is disclosed regarding the above embodiments.

[0062] (Note 1) The corrosion resistance evaluation method for a separator (20) according to the present disclosure is a method for evaluating the corrosion resistance of a separator for a fuel cell, comprising a metal substrate (30) and a coating layer (32) formed on the surface of the metal substrate, comprising an acid treatment step of immersing the separator in an acidic solution (AS1) and a potential measurement step of measuring the natural potential of the separator after the acid treatment step.

[0063] This process allows for the evaluation of whether a separator has excellent corrosion resistance in a short time and at low cost. Therefore, even when dealing with large quantities of separators, the pass / fail status of the separators can be determined efficiently.

[0064] (Note 2) In the method for evaluating the corrosion resistance of the separator described in Appendix 1, the acidic solution used in the acid treatment step may contain 5 ppm to 20 ppm of fluoride ions.

[0065] When such an acidic solution is used, variations in the spontaneous potential can be suppressed in the potential measurement step after the acid treatment step.

[0066] (Note 3) In the method for evaluating the corrosion resistance of a separator as described in Appendix 1 or 2, the acidic solution used in the acid treatment step may have a pH of 2 to 4 and a temperature of 60°C to 90°C.

[0067] The surface of the separator can be stabilized by acid treatment using such an acidic solution.

[0068] (Note 4) In the method for evaluating the corrosion resistance of a separator described in any one of the appendices 1 to 3, the coating layer may have an intermediate layer (321) formed on the metal substrate and made of a metal or metal compound, and a conductive layer (322) formed on the intermediate layer and made of a conductor.

[0069] It is easy to evaluate whether or not defects exist in the coating layer, and it is also easy to determine whether or not the separator is suitable for actual use in fuel cells.

[0070] (Note 5) In the method for evaluating the corrosion resistance of the separator described in Appendix 4, the material of the metal substrate may be stainless steel, the material of the intermediate layer may be titanium, titanium carbide, or titanium nitride, and the material of the conductive layer may be carbon.

[0071] In this case, the coating layer exhibits excellent corrosion resistance. Therefore, even with separators that tend to have large variations in their natural potential, the above acid treatment allows for evaluation of whether or not the separator has excellent corrosion resistance based on its natural potential.

[0072] (Note 6) In the method for evaluating the corrosion resistance of a separator described in any one of the appendices 1 to 5, the separator may be judged as acceptable if the measured value of the natural potential is 0.1V or higher.

[0073] This allows us to evaluate the separator as having low metal ion elution from the metal substrate and excellent corrosion resistance.

[0074] (Note 7) In the method for evaluating the corrosion resistance of a separator described in any one of the appendices 1 to 6, in the potential measurement step, an electrochemical measurement circuit (60) including the separator, a counter electrode (80), and a reference electrode (86) may be configured, and at least the separator and the counter electrode may be immersed in an acidic solution (AS2) stored in a measuring container (70) to measure the natural potential.

[0075] This configuration allows for easy and highly accurate measurement of the natural potential.

[0076] (Note 8) In the method for evaluating the corrosion resistance of a separator as described in Appendix 7, the acidic solution used in the potential measurement step may have a pH of 2.95 to 3.05 and a temperature of 78°C to 82°C.

[0077] (Note 9) In the method for evaluating the corrosion resistance of a separator as described in Appendix 7 or 8, the acidic solution used in the potential measurement step may contain 3 ppm of fluoride ions.

[0078] Based on the above, it is possible to obtain a natural potential under conditions similar to the "corrosion resistance test method (anodic corrosion)" shown in Non-Patent Document 1 above.

[0079] While this disclosure has been described in detail, it is not limited to the individual embodiments described above. These embodiments can be added, replaced, modified, partially deleted, etc., in any way that does not depart from the gist of this disclosure or from the intent of this disclosure derived from the claims and their equivalents. These embodiments can also be implemented in combination. For example, the order of operations and processes in the embodiments described above are given as examples only and are not limited thereto. The same applies when numerical values ​​or mathematical formulas are used in the description of the embodiments described above. [Explanation of Symbols]

[0080] 10... Unit cell 20... Separator 21...Sample 30...Metal substrate 32...Coating layer 40...Micro-defects 60... Electrochemical measurement circuit 61... Potential measurement system 70... Measuring container 78... Bubbling tube 80... Counter electrode 86... Reference electrode 321...Intermediate layer 322...Conductive layer AS1, AS2…Acidic solution HB1, HB2…Water bath

Claims

1. A method for evaluating the corrosion resistance of a separator for a fuel cell, comprising a metal substrate and a coating layer formed on the surface of the metal substrate, The acid treatment step involves immersing the separator in an acidic solution, A potential measurement step for measuring the natural potential of the separator after the acid treatment step, It has, A method for evaluating the corrosion resistance of a separator, wherein the acidic solution used in the acid treatment step contains 5 ppm to 20 ppm of fluoride ions.

2. A method for evaluating the corrosion resistance of a separator according to claim 1, wherein the acidic solution used in the acid treatment step has a pH of 2 to 4 and a temperature of 60°C to 90°C.

3. A method for evaluating the corrosion resistance of a separator according to claim 1, wherein the coating layer comprises an intermediate layer formed on the metal substrate and made of a metal or metal compound, and a conductive layer formed on the intermediate layer and made of a conductor.

4. A method for evaluating the corrosion resistance of a separator according to claim 3, wherein the material of the metal substrate is stainless steel, the material of the intermediate layer is titanium, titanium carbide, or titanium nitride, and the material of the conductive layer is carbon.

5. A method for evaluating the corrosion resistance of a separator according to claim 1, wherein the method determines that the separator is acceptable if the measured value of the natural potential is 0.1V or higher.

6. A method for evaluating the corrosion resistance of a separator for a fuel cell, comprising a metal substrate and a coating layer formed on the surface of the metal substrate, The acid treatment step involves immersing the separator in an acidic solution, A potential measurement step for measuring the natural potential of the separator after the acid treatment step, It has, In the potential measurement step, an electrochemical measurement circuit including the separator, counter electrode, and reference electrode is configured, and at least the separator and the counter electrode are immersed in an acidic solution stored in a measuring container to measure the natural potential, A method for evaluating the corrosion resistance of a separator, wherein the acidic solution used in the potential measurement step has a pH of 2.95 to 3.05 and a temperature of 78°C to 82°C.

7. A method for evaluating the corrosion resistance of a separator according to claim 6, wherein the acidic solution used in the potential measurement step contains 3 ppm of fluoride ions.

Citation Information

Patent Citations

  • Cover inspecting method

    JP1992329349A

  • Electrode potential measuring equipment

    JP1995092132A

  • Inspection method for polymer electrolyte fuel cell, and polymer electrolyte fuel cell by the method

    JP2004031256A

  • Separator of fuel cell, fuel cell stack, fuel cell vehicle, and method of manufacturing separator of fuel cell

    JP2007073440A

  • Inspection method of metal separator for fuel cell

    JP2012059485A