Catalytic systems in the form of supported catalysts
The catalyst system with granular or spherical activated carbon and optimized pore structure addresses inefficiencies in conventional systems, enhancing catalytic performance and mechanical stability for improved conversion rates and reduced pressure loss.
Patent Information
- Application Number
- JP2025112063
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-01-29
- Filing Date
- 2025-07-02
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2041-06-01
AI Technical Summary
Conventional activated carbon-supported catalysts face issues with suboptimal pore systems, leading to inefficient catalytic performance, high catalyst loss, and poor mechanical stability, particularly in continuous and discontinuous catalytic processes, resulting in reduced conversion rates and increased pressure loss.
A catalyst system using granular or spherical activated carbon with a high ratio of mesopores and macropores, surface-oxidized to enhance hydrophilicity, and loaded with catalytically active components, providing improved diffusion and mechanical stability.
The catalyst system achieves high catalytic activity, durability, and recyclability, with reduced pressure loss and sludge formation, suitable for both continuous and discontinuous applications.
Smart Images

Figure 0007955439000009 
Figure 0007955439000010 
Figure 0007955439000011
Abstract
Description
[Technical Field]
[0001] The present invention relates to the art of catalytic active systems, or to the art of catalysts or catalytic active components applied to carrier materials, and therefore, in particular to the art of supported catalysts that can be used in heterogeneous system catalysts.
[0002] In particular, the present invention relates to a method for producing a catalyst system comprising at least one catalytically active component, in particular a supported catalyst.
[0003] Furthermore, the present invention relates to a catalyst system obtained based on the method according to the present invention, and more particularly to a catalyst system comprising at least one catalytically active component applied to a catalyst support, and more particularly to at least one catalytically active component immobilized on the catalyst support.
[0004] Furthermore, the present invention relates to the use of the catalytic system according to the present invention as a catalyst or as a catalyst support. Moreover, the present invention relates to the use of the catalytic system according to the present invention for chemical catalysts. Furthermore, the present invention also relates to the use of the catalytic system according to the present invention for catalyzing chemical methods and reactions such as hydrogenation reactions.
[0005] Furthermore, the present invention relates to the manufacture of filters and filter materials, as well as the use of the catalyst system according to the present invention as adsorption storage for gases or liquids, and also to its use in or as a gas sensor or in fuel cells. Furthermore, the present invention relates to the use of the catalyst system according to the present invention for gas purification or gas treatment, and further for the removal of contaminants or substances or gases that are harmful to the environment, health or toxicity. The present invention also relates to the use of the catalyst system according to the present invention for the preparation or provision of cleanroom atmospheres and the like.
[0006] The present invention also relates to protective materials manufactured using or having a catalyst system according to the present invention. The present invention further relates to filters and filter materials manufactured using or having a catalyst system according to the present invention. [Background technology]
[0007] A catalyst is generally understood to be a material or substance that can increase the reaction rate of a chemical reaction by lowering the activation energy without being consumed itself.
[0008] In conventional technology, catalysts currently hold great technical and commercial importance in key catalytic processes, such as the so-called catalytic process for the production of sulfuric acid, the catalytic process for the production of methanol, the so-called Haber-Bosch process for the industrial production of ammonia, and the so-called Ostwald process for the large-scale production of nitric acid by oxidation of ammonia. Catalysts are also used in the synthesis of in-chemicals (generated chemical products) and specialty chemicals, in the synthesis of natural substances, and in the production of active pharmaceutical ingredients. In particular, catalysts are also used in catalytic hydrogenation processes.
[0009] Furthermore, given this background, the targeted use of catalysts, particularly in situations where chemical reactions are carried out rapidly or at lower energy, creates a high technical demand for specific and efficient catalysts for use in chemical catalysts. In this regard, the use of catalysts in chemical reactions has great commercial importance; for example, approximately 80% of all chemical products have a catalytic step in their potential manufacturing or price chain. Furthermore, catalysts play an important role in environmental protection, particularly in exhaust gas aftertreatment in industries such as industrial power production, as well as in exhaust gas treatment from the (passenger) automobile transport sector.
[0010] In principle, catalysts can be used in the form of homogeneous system catalysts or heterogeneous system catalysts. In the case of homogeneous system catalysts or catalysts used in homogeneous system catalysts, the reactants or reactants that form the basis of the catalyzed reaction and the catalyst exist in the same phase, whereas in the case of heterogeneous system catalysts or catalysts used in heterogeneous system catalysts, the reactants to be reacted and the catalyst exist in different phases, for example, as a solid with respect to the catalyst and as a liquid or gas with respect to the reactants.
[0011] In principle, the advantages associated with the use of heterogeneous system catalysts lie in the fact that they allow for improved separation or isolation of the catalyst from the reaction mixture, along with the basic possibility of recycling used catalysts or processing deactivated or inactive catalysts. Particularly in industrial processes, heterogeneous system catalysts exist as solids or as so-called contact (catalysts), while the reaction partners or reactants are used in gaseous or liquid form. For example, the industrially established method described above is one in which the catalyst is used as a solid.
[0012] For heterogeneous system catalysts and solid catalysts, metals and metal-containing compounds such as metal salts and metal oxides are commonly used as catalysts. Such catalysts are used, for example, in large quantities, or in a form where the catalyst or underlying catalytically active component is present in a support system, or bound to or immobilized on it. Such catalyst systems in which the catalytically active component is on a support are generally called supported catalysts.
[0013] The use of supported catalysts is associated with the fundamental advantage of being able to react a larger surface area or larger contact area, which generally leads to improved efficiency or reduced catalyst usage, resulting in associated cost advantages.
[0014] Furthermore, the use of supported systems or supported catalysts generally has the advantage that the underlying catalyst can be better removed or separated from the reaction medium and is generally easier to reuse. In particular, for catalysts used in large quantities or in phase with the reactants, separation of the reactants after reaction or transformation is difficult or involves high catalyst mass loss, which generally leads to poor economic efficiency and makes recycling of the used catalyst fundamentally difficult.
[0015] In general, for supported catalyst systems or supported catalysts, the use of compact or porous support structures is considered in the technical context. The use of so-called compact catalysts is associated with the disadvantage that efficient surface expansion cannot be achieved, and as a result, catalytic activity can only be obtained on a relatively small geometric surface. In contrast, porous solids used as catalyst supports have a large surface area (inside), and as mentioned above, efficiency can be increased even with a small amount of supported active components (so-called noble metals or other catalytically active metals), and high catalytic activity can be exhibited.
[0016] For example, crystalline porous solids of zeolite systems are used as catalyst supports, particularly in the fields of petrochemicals and refining technologies for processing or upgrading crude oil and petroleum. Zeolites generally have uniform pore sizes, and a degree of selective reaction control is possible through size matching with the reacting substances. Furthermore, the use of silica, molecular sieves, metal oxides such as aluminum oxide, ceramics, and activated carbon as catalyst supports is generally known as prior art.
[0017] In principle, such carrier systems are used to reduce associated losses during application, particularly in order to enable the permanent or elution-stable immobilization of costly catalysts, or to enable the corresponding recyclability or recovery of the entire catalyst system, as mentioned above.
[0018] In the prior art, to obtain activated carbon as a catalyst support material, particularly so-called activated carbon-supported catalysts, especially activated carbon-supported precious metal catalysts, the corresponding activated carbon is generally used in the form of finely divided (pulverized) or finely ground powder, with the corresponding particle size in the low μm range. The use of finely divided activated carbon as a support system generally aims to reduce the limitations on fundamental mass transfer related to the catalyzed target reaction, particularly by shortening the diffusion or penetration distance into the pore structure of the activated carbon-based support material. However, using finely powdered activated carbon with small particle sizes as a catalyst support has a central drawback: optimal coating properties cannot be obtained overall. For example, when finely divided activated carbon is used, particularly in discontinuous applications, the low porosity of the filtration cake or the high density of the substrate leads to degradation of properties, for example, in the separation of the catalyst or catalyst system after use. In this regard, it is also emphasized that the separation or filtration of the catalyst or catalyst system is an essential or absolutely necessary method step in discontinuous catalysis.
[0019] Furthermore, such activated carbons often have pore systems that are not optimally formed in terms of catalyst binding and the movement of reactants and products, which can impair the overall catalytic performance.
[0020] Under certain operating conditions, particularly in continuous catalytic processes (i.e., catalytic reaction processes) using powdered activated carbon or pulverized coal in the reaction chamber, there is a high pressure loss due to excessive compression in the catalyst system. This often results in a decrease in the flow rate of the reaction mixture containing the corresponding reactants supplied to the catalyst system. Furthermore, excessive compression can occur if the abrasive hardness of the catalyst or corresponding support material is too low.
[0021] Furthermore, the application characteristics of catalyst systems supported on activated carbon are often suboptimal, particularly in that the finely fragmented catalyst system in the liquid medium containing the reactants tends to form sludge and excessive compression, posing a risk of clogging of the reactor and excessive reduction in flow rate or filtration rate, which is detrimental to the overall catalytic conversion. In addition, excessive compression of the catalyst system can create a "dead zone" in the underlying equipment, significantly reducing the conversion of reactants.
[0022] In this regard, the formation of sludge-like regions is particularly relevant in discontinuous applications. In continuous catalytic applications, for example, the catalytic system is filled into a corresponding reaction chamber, such as one based on a cartridge system, followed by a particularly continuous flow of reactants or a medium containing reactants, but high pressure losses occur at the corresponding low flow rates of the catalytic system. Furthermore, complex filtration and retention systems that are prone to clogging are often required to prevent the catalyst from being discharged or washed away from the continuously flowing reaction system.
[0023] As a result, catalyst systems using powdered or finely powdered activated carbon as a carrier material cannot necessarily be said to possess sufficient or satisfactory properties overall for their intended use.
[0024] To mitigate the drawbacks associated with small particle sizes, prior art has attempted to use catalyst carriers based on particulate activated carbon, thereby considering activated carbon starting materials based on coconut shells, charcoal, and wood (e.g., wood chips, peat, hard charcoal, etc.). These activated carbons used as catalyst carriers can generally be in the form of splinters (fragments) or grains (particles), and in principle, they bring about certain improvements in application characteristics, particularly separation time in discontinuous applications. However, these activated carbons used as catalyst carriers often have too low mechanical stability, which leads to high wear of the carrier due to application conditions, such as sometimes vigorous stirring methods during catalytic conversion. The low wear resistance of such activated carbon results in finely divided particles via corresponding crushing or grinding methods, leading to high loss of catalytically active material and the aforementioned disadvantages regarding system sedimentation or compression. Furthermore, such activated carbons often lack an optimally formed pore system.
[0025] Furthermore, known concepts of prior art for providing catalyst systems based on activated carbon as a support material often fail to optimally support or immobilize the catalyst on the support material. As a result, there are disadvantages such as, on the one hand, a small amount of catalyst being applied to the support, and on the other hand, frequent release or elution of the catalyst from the support material under application conditions. On the other hand, under application conditions, release or elution of the catalyst from the support material is often observed, and the amount of catalyst washed away may be lost, which is disadvantageous from a method engineering standpoint, and at least from a cost standpoint.
[0026] In particular, activated carbon used in prior art, such as coconut shell-based activated carbon, often has low affinity for the catalyst to which it is applied or immobilized. This is partly because—and we do not wish to be limited to this theory—the underlying activated carbon is often hydrophobic on its pore surface, or often lacks sufficient amounts of polar functional groups to bind the catalyst (this is especially true for polymer-based activated carbon, particularly PBSAC). However, this is disadvantageous overall for catalyst packing and mounting, and also for permanent immobilization of the catalyst to the support system. High catalyst loss in the underlying catalyst system, along with a decrease in the conversion rate of reactants in the underlying catalytic reaction, worsens the economic viability of the catalyst system used.
[0027] Conventional activated carbon has a nonpolar or hydrophobic surface, which means it lacks sufficient affinity for coating or immobilizing catalysts or catalytically active components used in activated carbon reactors or catalytic devices. Therefore, to ensure a constant load on the activated carbon, it is necessary to use a large excess of catalyst material during the production of activated carbon or in the production of the device. To achieve a perfectly constant load on the activated carbon, it is necessary to use a large excess of catalyst material during the production process or the installation of the catalyst, or to create surface centers (centers for the attachment of catalytically active components) in advance. In particular, since catalysts generally adhere only through purely physical interactions, they can be at least partially removed or re-washed (e.g., by elution methods), especially when in contact with liquids.
[0028] In principle, heterogeneous system catalysts using activated carbon as a support material, based on known concepts of prior art, have drawbacks, particularly in that the pore system of the support material is not optimally formed, resulting in inoptimal methods of movement or diffusion of reactants or products, especially with respect to the underlying pore size and their distribution, or rather, their proportion to the total pore volume. When the movement or diffusion of reactants or products is inoptimal, for example, reactants may not be optimally moved to the underlying catalyst center, or the resulting products may not be optimally removed from the catalyst system, leading to a decrease in conversion rate and inoptimal spatial / time yield.
[0029] In this regard, heterogeneous catalytic reactions using porous structures such as activated carbon as catalyst supports can be basically divided into seven sub-steps, each of which involves a corresponding migration step of reactants or products, and the rate of each step can be determined. In this regard, please also refer to Figure 4 and the related explanation below.
[0030] If the pore system of the support material is not optimally formed, the means of transport within the system will be insufficient, limiting catalytic activity overall, which will lead to a deterioration in conversion rates and spatial / temporal yields over the long term.
[0031] Furthermore, the conversion rate or space / time yield may also be reduced due to the insufficient formation of such catalytic active centers, or the inadequate supply of catalytic active components by the supporting material, which in this respect can also be caused by an insufficiently formed pore system of the catalytic support.
[0032] Furthermore, catalyst systems known from prior art may have the drawback of generating high pressure loss during application, particularly in fixed beds, and high levels of dust formation, accompanied by associated material loss, often occur, especially as a result of insufficient hardness or wear resistance of the underlying catalyst system.
[0033] DE 29 36 362 C2 relates to a method for producing a palladium-carbon catalyst, in which palladium is precipitated by reduction on carbon suspended in an organic solvent as a catalyst support. In this regard, it is assumed that the palladium is precipitated as a metal on a suspended support. Powdered activated carbon, carbon black, or graphite are used as the carbon support. However, the described catalyst may have the aforementioned drawbacks, particularly with respect to catalyst separation or recovery in discontinuous catalytic methods, and to its applicability characteristics in continuous catalytic methods, especially with respect to pressure drop or flow rate.
[0034] In summary, catalyst systems known from prior art that use conventional activated carbon or powdered activated carbon as the carrier material have production-specific and application-specific disadvantages, particularly in terms of loading and immobilizing the catalytically active component onto the material, and in terms of using the basic system in continuous and discontinuous catalytic action. [Prior art documents] [Patent Documents]
[0035] [Patent Document 1] DE 29 36 362 C2 [Overview of the Initiative] [Problems that the invention aims to solve]
[0036] Against this backdrop, the object of the present invention is to provide a catalyst system or supported catalyst having at least one catalytically active component, and a corresponding manufacturing method, thereby avoiding or significantly mitigating the drawbacks of the prior art described above.
[0037] In particular, the present invention aims to provide a catalyst system having at least one catalytically active component or a supported catalyst having at least one catalytically active component, the catalyst system or catalyst having production-specific and application-specific advantages. In this regard, a corresponding method for manufacturing the catalyst system is also provided.
[0038] The fundamental objective of the present invention can be found, in particular, in the fact that, within the scope of the invention, a high-performance catalyst system is provided that enables high conversion and associated high space / time yield due to high durability or stability, while simultaneously providing high recyclability and stability of the system.
[0039] In particular, the present invention provides a catalyst system that enables high or efficient loading by a catalyst component or catalytically active component, while simultaneously ensuring permanent and consistent loading or attachment by the catalyst component.
[0040] Furthermore, according to the present invention, within its scope of application, particularly in chemical catalysts, preferably on an industrial scale, in both discontinuous and continuous catalytic applications, such catalyst systems should be provided that also have improved characteristics, particularly with respect to their catalytic performance and the separation, recovery, or recycling of the system (particularly in discontinuous methods), and also with respect to ensuring low or adjustable pressure drop and high or adjustable flow rate (particularly in discontinuous methods). The chemical catalyst should preferably have improved characteristics, particularly with respect to its catalytic performance and the separation, recovery, or recycling of the system (particularly in discontinuous methods), and also have improved characteristics with respect to ensuring low or adjustable pressure drop and high or adjustable flow rate (particularly in continuous catalytic methods), thereby also providing an overall optimized method time or increased catalytic activity.
[0041] In particular, the present invention aims to provide a catalyst system that, in addition to high catalytic activity, also exhibits excellent mechanical properties, especially the wear resistance or burst pressure of the underlying particulate structure.
[0042] Similarly, it is desirable that the systems according to the present invention be custom-made or individually designed or equipped for each application or use case.
[0043] Furthermore, the present invention is intended to provide an efficient method for obtaining a catalyst system according to the present invention having at least one catalytically active component. [Means for solving the problem]
[0044] As the applicant has discovered in a completely unexpected way, the aforementioned problem on which the present invention is based can be solved in an unexpected way, within the scope of the present invention, by providing a special method for manufacturing a special catalyst system and a corresponding catalyst system as such.
[0045] In this regard, according to the present invention, in addition to granular or spherical design or shape, a specially designed pore system, i.e., activated carbon with a high ratio of mesopores and macropores in the total pore volume of the activated carbon, is used as a catalyst support. Therefore, according to the present invention, activated carbon having high mesopores and macropores (while simultaneously having a predetermined ratio of micropores) is used. Furthermore, the activated carbon used in accordance with the present invention has a specific BET surface area, and at the same time, the ratio of total pore volume to specific BET surface area is special.
[0046] Furthermore, in the method according to the present invention, the targeted oxidation of the activated carbon subsequently used as a catalyst support, particularly surface oxidation (i.e., oxidation of the inner surface of the catalyst support in particular), is intended or aimed at adjusting a specific oxygen content, particularly surface oxygen content, and accompanied by the formation of a specific hydrophilicity, such a specific activated carbon subsequently contains a catalytically active component or its precursor, and is subsequently reduced to obtain the catalyst system according to the present invention.
[0047] In other words, according to the present invention, a supported catalyst having at least one catalytically active component applied to a special catalyst system or catalyst support is provided, wherein the catalyst support is in the form of very specially formed granular or spherical activated carbon having special porosity particularly with respect to the formation of high mesopores and macropores (i.e., having a high proportion of mesopores and macropores in the total pore volume with a predetermined proportion of micropores simultaneously), and the application of the catalytically active component to the activated carbon is carried out in an oxidized form of the activated carbon (i.e., to oxidized activated carbon), and then, in this embodiment, the catalyst system according to the present invention is obtained by further reduction of the underlying system (i.e., the active center or active component). In addition to high mesopores and macropores, the activated carbon used as the catalyst support generally exhibits a limited microporosity (i.e., a limited proportion of micropores in the total pore volume) sufficient for catalytic reactions, although this is generally dependent on the mesopores and macropores.
[0048] Remarkably, the catalyst system or supported catalyst according to the present invention exhibits excellent catalytic properties due to improved movement or diffusion characteristics of reactants or products and improved loading with catalytically active components resulting from a special pore system, providing catalysts based thereon that, when used in catalytic processes, result in high catalytic conversion rates and high space / time yields. In this regard, the catalyst system according to the present invention also exhibits a high degree of dispersibility of catalytically active components and optimized microcrystalline size, which can be used as parameters or measures of catalytic performance.
[0049] Furthermore, the catalyst systems provided according to the present invention are particularly suitable for use in the field of chemical catalysts, especially on a (large-scale) industrial scale. In addition, the catalyst systems according to the present invention are particularly suitable for corresponding filter applications for removing contaminants and hazardous substances from media containing these substances. In particular, the catalyst systems according to the present invention are particularly suitable for use in protective materials, especially in civilian or military fields, and especially in protective materials for NBC (nuclear, biological, and chemical) applications.
[0050] In particular, due to its spherical design or shape, the excellent mechanical properties of the catalyst support, and its controllable or specially designed meso- and macroporosity (with simultaneously defined microporosity), the catalyst system according to the present invention is especially important for continuous catalysts, thereby overcoming the shortcomings of the prior art, for example, with respect to discontinuous catalysts such as conventional powder catalysts, as described above.
[0051] To solve the above-mentioned objectives, the present invention, according to a first aspect of the present invention, proposes a method according to the present invention for producing a catalyst system having at least one catalytically active component according to the invention of claim 1. Furthermore, particularly advantageous embodiments of the method according to the present invention are the subject matter of the dependent claims of the relevant method.
[0052] A further object of the present invention, according to a second aspect of the present invention, is a catalyst system or supported catalyst according to the present invention, wherein the catalyst system or supported catalyst comprises at least one catalytically active component, and special granular activated carbon is used as a catalyst support according to the independent claims of the claims relating thereto and relating to the catalyst system of the present invention. Furthermore, particularly advantageous embodiments of the catalyst system according to the present invention are the subject matter of the dependent claims relating thereto.
[0053] Furthermore, a further subject of the present invention is, according to a third aspect of the present invention, the uses of the present invention described in the claims relating to each independent use.
[0054] Furthermore, a further subject of the present invention, according to a fourth aspect of the present invention, is a protective material according to the present invention, particularly for protective clothing, particularly for the civil or military field, as per the related independent claims.
[0055] Furthermore, a further subject of the present invention, according to a fifth aspect of the present invention, is a filter and filter material for removing all kinds of pollutants, odors and hazardous substances, as per the relevant independent claims. Furthermore, particularly advantageous embodiments of the filter and filter material according to the present invention are the subject of the relevant dependent claims.
[0056] It goes without saying that, in the following description of the present invention, for the purpose of avoiding unnecessary repetition, such embodiments, advantages, and examples described only in relation to one aspect of the present invention will naturally apply mutatis mutandis to the remaining aspects of the present invention without the need for explicit mention.
[0057] Furthermore, it will be obvious to those skilled in the art that, in the following description, any relevant descriptions of values, numbers, and ranges are not to be understood as limiting, and that, depending on the individual case or application, deviations from the described range or description may occur without departing from the scope of the present invention.
[0058] Furthermore, it is assumed that all values and parameters described below can be determined using standardized or explicitly defined determination methods, or methods and measurements well known to experts in this field.
[0059] Furthermore, it should be noted that, in the case of all relative or proportional quantitative data, particularly those relating to weight, listed below, these data must be selected or combined within the scope of the invention, as necessary, including further components or components as defined below, so as to always yield a result of 100% or 100% by weight. However, this is obvious to those skilled in the art.
[0060] The present invention will now be described in more detail.
[0061] Accordingly, according to a first aspect of the present invention, the present invention relates to a process for preparing a catalyst system comprising at least one catalytically active component, in particular a supported catalyst, preferably for use in heterogeneous catalysis, wherein at least one catalytically active component is applied to and / or fixed to a catalyst support, said catalytically active component comprising and / or consisting of at least one metal, wherein the process comprises the following successive steps (a) to (d) specified below: (a) providing and / or producing granular, preferably spherical activated carbon (= starting activated carbon) for use as catalyst support, wherein said activated carbon (so-called starting activated carbon) (i) has a total pore volume (V 3 ) in the range from 0.8 cm 3 / g to 3.9 cm / g, in particular the total pore volume according to Gurvich, in particular wherein at least 50% of the total pore volume of the activated carbon, in particular the total pore volume according to Gurvich, is formed by pores having a pore size of at least 2 nm, in particular by pores having a pore size in the range from 2 nm to 500 nm, preferably by meso- and macropores, and total (ii) has a specific BET surface area (S ) in the range from 1,000 m 2 / g to 3,000 m 2 / g, provided that the ratio (quotient; Q) of total pore volume (V BET ), in particular total pore volume according to Gurvich, to specific BET surface area (S total ), in particular Q = V BET / S total is at least 0.5 × 10 BET -9 m; thereafter, (b) Oxidation, particularly surface oxidation, of the activated carbon prepared and / or produced in step (a) of the method, wherein the oxidized, particularly surface-oxidized, activated carbon has an oxygen content of at least 4% (atomic%) based on the total elemental composition of the oxidized activated carbon, particularly a surface oxygen content measured by X-ray photoelectron spectroscopy (XPS or ESCA), and / or the oxidized, particularly surface-oxidized, activated carbon has hydrophilicity measured as water vapor adsorption behavior, wherein at least 30% of the maximum water vapor saturation load of the activated carbon reaches a partial pressure of 0.6 p / p0; after that, (c) Equipment, particularly loading and / or coating and / or impregnation, of the activated carbon oxidized in step (b) of the method, particularly surface-oxidized, with a catalytic active component, particularly with at least one precursor of a catalytic active component; after that, (d) Reduction of the activated carbon obtained in step (c) of an oxidized, particularly surface-oxidized, activated carbon, particularly the catalyst, particularly the catalyst, for transferring the catalyst precursor to the catalyst, in particular (i.e., on the one hand, surface reduction of the activated carbon, particularly previously oxidized, and / or on the other hand, reduction of the catalyst, particularly the catalyst, or its precursor, preferably reduction of a metal or metal compound containing the catalyst), in particular by which a catalyst system having at least one catalyst, particularly a supported catalyst, is obtained.
[0062] Therefore, the fundamental idea of the present invention lies, as described above, in the fact that a very special activated carbon is used as a catalyst support for containing or equipping catalytically active components. The present invention is, on the one hand, in a granular or spherical form, and on the other hand, has defined porosity with respect to particularly high mesoporosity and macroporosity, and simultaneously has a defined proportion of micropores (i.e., dependent on mesopores and macropores, but sufficient for catalytic activity), and furthermore, the activated carbon is oxidized or surface-oxidized in a specific manner before being equipped with catalytically active components. In this regard, the applicant has found quite astonishing that by using activated carbon having the defined porosity described above, the overall improved catalytic properties of the resulting catalyst system are provided, in particular with respect to high conversion with high catalytic activity and correspondingly high space / time yield in the underlying catalytic conversion or reaction.
[0063] Without being limited to this theory, the use of special activated carbon with a high ratio of mesopores to macropores, and in which the macropore ratio is defined, particularly improves the transfer and diffusion methods of reactants and products based on catalytic reactions, while also providing high accessibility and optimal formation of catalytically active components incorporated into the catalyst support.
[0064] In this regard, the kinetics of the underlying catalytic reaction are improved overall, particularly in terms of the methods of movement and diffusion within the pore system and the boundary layer of the catalyst support, while the reactants to be reacted have high accessibility to the catalytically active component or the catalyst center.
[0065] According to the present invention, a catalyst system is also provided that is improved overall by special adjustment and formation of the pore system of the activated carbon used as a catalyst support, exhibiting excellent efficiency in terms of catalytic activity. In this regard, the purpose-appropriate (surface) oxidation of the activated carbon used as a catalyst support before loading the catalytic active component is very important, which improves the binding or loading with the catalytic active component or related precursor, as well as the formation of catalyst centers having defined (metal) dispersion and microcrystalline size, as will be described in detail below.
[0066] A further central advantage of the present invention is the fact that the activated carbon used in accordance with the present invention has high mechanical stability or resistance with low wear during use in catalytic methods, and thus the catalyst system according to the present invention is given a reasonably high durability, along with high recyclability.
[0067] The specific use of granular or spherical activated carbon, i.e., activated carbon with special shapes, further improves the applicability of the catalyst system according to the present invention, that is, it improves the use of the catalyst system provided according to the present invention not only in continuous catalyst applications but also in discontinuous catalyst applications. This is because, on the one hand, special molding, particularly based on discontinuous spheres, achieves improved bulk porosity for discontinuous applications, preventing sludge formation in the reaction system while significantly improving the separation or recovery of the catalyst from the reaction system. On the other hand, the improved bulk properties of the catalyst system according to the present invention result in low pressure loss accompanied by high accessibility of the catalyst system to the reactants or reactants to be reacted, so that high flow rates can also be achieved with respect to the medium containing the reactants or reactants to be reacted using the catalyst system according to the present invention.
[0068] Granular, and especially spherical, activated carbon (spherical carbon) used according to the present invention offers many advantages over other forms of activated carbon, such as powdered carbon, crushed carbon, and carbon from coal, in terms of improved fluidity, wear resistance, and dust-free operation. This also leads to at least high mechanical resistance and durability, resulting in a longer service life for the underlying system. As a result, clogging during use is reduced, leading to a longer lifespan.
[0069] As shown below, by specifically adjusting the particle size or diameter of the underlying spherical activated carbon, particularly with respect to the recovery rate, flow behavior, or pressure drop of the catalyst system, it is possible to provide a generally customized catalyst system with optimized application characteristics for each case, while simultaneously further improving the catalytic activity of the catalyst system according to the present invention. In particular, by specifying the particle size, the pressure drop or flow rate can be adjusted or changed, so it is also possible to provide a system optimized for the background of each use or application.
[0070] In relation to the present invention, particularly highly wear-resistant or mechanically stable spherical activated carbon is used as appropriate for the catalyst support employed, provided, for example, by special activated carbon based on organic polymers, particularly sulfonated organic polymers, as defined below. In this regard, it is quite surprising in relation to the present invention that the sulfur content that may be present in the activated carbon, for example up to 0.1% by weight relative to the activated carbon, is not detrimental to the catalytic function of the catalyst system according to the present invention, does not cause harmful impairment of catalytic activity, and in particular does not lead to so-called catalyst poisoning.
[0071] Furthermore, as a result of the (surface) oxidation of the activated carbon used before supporting the catalytically active component, the present invention has succeeded in a remarkable manner in supporting the catalytically active component on the activated carbon used as a support at a high level, and simultaneously permanently or stably. This significantly improves the catalytic activity of the catalyst system according to the present invention, and at the same time improves its durability. In particular, the washing or peeling of the catalytically active component from the support material during application is reduced or avoided, thus improving the durability of the catalyst system according to the present invention.
[0072] While we do not wish to commit to this theory, targeted oxidation or surface oxidation of activated carbon results in the formation of special oxygen-containing functional groups on or within the pore system of the activated carbon used according to the present invention, in both micropore, mesopore, and macropore regions, thereby increasing the affinity of the activated carbon for the catalytic active ingredient used according to the present invention. As a result of the oxidation or surface oxidation treatment of the activated carbon carried out according to the present invention before loading the catalytic active ingredient, a less hydrophobic or hydrophilic surface of the activated carbon, or special functional groups, are generated or provided on the surface or pore system of the activated carbon, and the loading of the catalytic active ingredient is significantly improved in a truly remarkable way.
[0073] In this regard, it is equally astonishing that the catalyst system according to the present invention, based on spherical activated carbon with a defined particle shape or particle size that undergoes oxidation before supporting the catalytically active component, exhibits significantly improved catalytic activity compared to powdered activated carbon. In this regard, it is quite astonishing that, with respect to the catalyst system according to the present invention, there are no major limitations or restrictions on mass transfer in the pore system of the activated carbon, particularly with respect to the underlying reactants or reactants, and this is also particularly attributable to the defined pore structure of the activated carbon used in accordance with the present invention, as shown below. In this regard, it has been found that the present invention is particularly advantageous when a particularly defined proportion of dependent macropores is used as a catalyst support for the catalyst system according to the present invention.
[0074] In particular, it is quite remarkable that the catalyst systems provided according to the present invention exhibit high catalytic activity even with relatively large or fine particle sizes, especially compared to powdered carbon. In this regard, the degree of interaction according to the present invention—without intending to limit ourselves to this theory—makes it possible, on the one hand, to achieve particularly uniform and high loading of activated carbon by the catalytically active component, and on the other hand, to reduce mass transfer or diffusion limitations in the catalyst system that are detrimental to catalytic activity.
[0075] With respect to the ideas of the present invention, in particular, due to the special matching of one support system and the other catalytically active component, clogging of the pore system beneath the activated carbon by the catalytically active component—for example, due to excessive microcrystalline size with respect to the crystallization of the metal salt—is prevented at least substantially, thereby further improving the performance of the catalytic system provided according to the present invention.
[0076] According to the present invention, it is possible for the first time to provide a very special catalyst system having a very special activated carbon as a support material based on the method according to the present invention, which comprises a target method with at least one catalytically active component, and which has significant advantages and improved properties compared to prior art systems and is suitable for both discontinuous and continuous catalytic applications.
[0077] The catalyst system according to the present invention, provided by the method according to the present invention, exhibits both improved mechanical and improved catalytic properties, resulting in reduced method time and high recovery rates, and enabling excellent recycling of the underlying catalyst or catalytically active component. Furthermore, as previously stated, the catalyst system according to the present invention exhibits improved flow properties with low pressure loss, particularly when used or applied in (loose) bulk form.
[0078] Furthermore, the catalyst system according to the present invention, provided based on the method according to the present invention, is also suitable for use in filters or filter materials, particularly for detoxifying harmful or toxic substances.
[0079] Thus, the catalyst system provided based on the method according to the present invention possesses both excellent mechanical properties and excellent catalytic properties.
[0080] Based on the method according to the present invention, the results are an effective apparatus for using activated carbon as a carrier material and at least one catalytically active component to obtain the catalyst system according to the present invention.
[0081] The term “catalytic system,” as used synonymously with “supported catalyst” in accordance with the present invention, is understood very broadly in accordance with the present invention and, in particular, refers to a functional unit based on at least one catalytically active component on the one hand and a supporting material on the other, wherein the catalytic properties can be substantially attributed for this purpose to at least one metal or a catalytically active component made of metal. In this regard, a catalytic system according to the present invention can be obtained by having a catalytically active component based on the immobilization of the catalytically active component of a catalytic support particularly contained in the activated carbon used, in particular in the form of equipment or filling or coating or impregnation.
[0082] Furthermore, the terms “equipped,” “filled,” “coated,” or “impregnated” refer to “impregnation” as used in the present invention, and refer to the equipped activated carbon used in the present invention as to carrier materials having catalytically active components, thereby the outer and / or inner surface structure of the activated carbon, used with appropriate pores, particularly micropores and / or macropores, comes into contact with, or is provided with or filled with, the catalytically active component at least partially and / or cross-sectionally. In this regard, the catalytically active component, though not wishing to limit itself to this theory, forms a catalytic structure or chemisorption properties on the surface of the activated carbon that functionally complements the physicoadsorption properties of the activated carbon, so to speak, so the catalytic system provided based on the method according to the present invention essentially combines both chemisorption and physicoadsorption properties in the same material. In particular, the catalytically active component can be bonded to the surface of the activated carbon by physical and / or chemical means, and in particular, the properties of the catalytically active center or catalytically active component may depend particularly on the surface properties of the activated carbon, the catalytically active component itself, and / or the reduction conditions.
[0083] Furthermore, with respect to the term "spherical," which is also synonymously referred to as "spherical" as used in the activated carbon used as a carrier material according to the present invention, this term is understood very broadly and, according to preferred embodiments of the present invention, particularly relates to at least substantially ideal spherical or spherical shapes of activated carbon, but also relates to the formation or physical design of activated carbon used in deviation from spherical, such as the formation of (spherical) ellipsoidal activated carbon. Moreover, the term "spherical" also includes spherical or elliptical forms of activated carbon in which the activated carbon has protrusions or recesses, indentations, depressions, cracks, etc. According to the present invention, the use of spherical activated carbon or spherical carbon or spherical activated carbon is therefore decisive.
[0084] With regard to the term "surface oxidation" as used in accordance with the present invention, this specifically refers to the oxidation of the surface of activated carbon used as a starting material that is in contact with an environment containing an oxidizing agent, or that is, so to speak, externally accessible to the oxidizing agent used in accordance with the present invention. In particular, this refers to the pore system of activated carbon in the form of macropores, mesopores, and micropores.
[0085] Furthermore, the specific BET surface area (S BET Total pore volume (V) total ), in particular the ratio of total pore volumes (quotient; Q) by Gulvitch, especially the equation Q=V total ×S BETAccordingly, the value based on this helps to further characterize the pore system of the activated carbon used as a catalyst support according to the present invention, and in particular, helps to demonstrate that the porosity or pore system of the activated carbon is characterized and defined based on the quotient Q, that is, in particular for activated carbon used according to the present invention as a catalyst support, there is a defined proportion of micropores simultaneously with a high proportion of mesopores and macropores in the total pore volume. In particular, the underlying quotient explains the high mesoporosity and macroporosity of the activated carbon used according to the present invention. In this regard, the quotient Q can further be used as a measure of improved kinetics or improved catalytic activity in heterogeneous catalytic reactions when using the catalyst system according to the present invention as a result of the specially formed activated carbon. Thus, as a result of the specially formed pore system of the activated carbon further characterized by the quotient, an overall improvement is observed with respect to the rate determination step of the kinetics underlying heterogeneous catalytic reactions, for example, with respect to improved diffusion behavior of reactants or products and accessibility of catalytically active components. Accordingly, the quotient Q further reflects the properties of the catalyst system according to the present invention provided in the method according to the present invention, in particular its properties with respect to improved catalytic performance.
[0086] With respect to activated carbon or such related activated carbon particles used as catalyst supports, the parameter data enumerated in this regard are determined using standardized or explicitly defined determination methods, or using determination methods that are well known to those skilled in the art. In particular, parameter data relating to the characterization of porosity or pore size distribution and other adsorption properties are generally obtained from the corresponding nitrogen adsorption isotherms of the respective activated carbon or the product being measured, unless otherwise specified.
[0087] In relation to the present invention, the term "micropore" refers to a pore having a diameter of less than 2 nm, while the term "mesopore" refers to a pore having a diameter in the range of 2 nm (i.e., including 2 nm) to 50 nm, and the term "macropore" refers to a pore having a diameter greater than 50 nm (i.e., >50 nm), and more particularly, a pore up to a value including 500 nm.
[0088] The following describes in more detail the production of activated carbon used as a catalyst support, as described in step (a):
[0089] Thus, according to the present invention, the activated carbon prepared or manufactured in step (a) (so-called initial activated carbon) is 0.9 cm 3 / g~3.4cm 3 Within the range of / g, especially 1cm 3 / g~2.9cm 3 Within the range of / g, preferably 1.1cm 3 / g~2.4cm 3 Within the range of / g, more preferably 1.2cm 3 / g~1.9cm 3 / g, particularly preferably 1.5cm 3 / g~1.9cm 3 Total pore volume within the range of / g (V total ), in particular, it is provided that it has total pore capacity according to Gulvitch's method.
[0090] As previously shown, according to the present invention, the activated carbon used as a catalyst support is, in particular, activated carbon having high overall mesoporosity and macroporosity. The present invention provides that the total pore capacity of the activated carbon prepared and / or manufactured in step (a) in the range of 50% to 90%, particularly in the range of 52.5% to 87.5%, preferably in the range of 55% to 85%, more preferably in the range of 57.5% to 82.5%, and even more preferably in the range of 60% to 80%, particularly the total pore capacity according to Gulvitch, passes through the catalyst support (so-called initial activated carbon) and is formed by pores having a pore diameter of at least 2 nm, particularly by pores having a pore diameter in the range of 2 nm to 500 nm, and preferably by mesopores and macropores.
[0091] Furthermore, the activated carbon provided or produced in step (a) can also be sufficiently microporous, though limited and dependent, for catalytic activity, so that a relatively small proportion of the total pore volume is generally associated with micropores (and, in particular, to a degree sufficient for catalytic activity): Thus, according to the present invention, it is particularly provided that the total pore volume of the activated carbon provided and / or produced in step (a) (i.e., the starting activated carbon), in particular 2.5% to 50%, especially 5% to 50%, preferably 10% to 50%, particularly preferably 12.5% to 47.5%, more preferably 15% to 45%, very preferably 17.5% to 423.5%, and even more preferably 20% to 40% of the total pore volume according to Gulvitch, is formed by pores having wp with a pore diameter of less than 2 nm, preferably by micropores.
[0092] Furthermore, the activated carbon prepared or manufactured in step (a) (so-called initial activated carbon) is 0.8 cm 3 / g~3.9cm 3 Within the range of / g, especially 0.9cm 3 / g~3.4cm 3 Within the range of / g, preferably 1cm 3 / g~2.9cm 3 Within the range of / g, more preferably 1.1cm 3 / g~2.4cm 3 Within the range of / g, particularly preferably 1.2cm 3 / g~1.9cm 3 Within the range of / g, particularly more preferably 1.5cm 3 / g~1.9cm 3 Total pore volume (V) within the range of / g total The present invention provides that the activated carbon has a total pore volume determined by Gurvitch, and that 50% to 90%, particularly 52.5% to 87.5%, preferably 55% to 85%, more preferably 57.5% to 82.5%, and especially preferably 60% to 80% of the total pore volume determined by Gurvitch, is formed by pores having a diameter of at least less than 2 nm, particularly by pores having a diameter in the range of 2 nm to 500 nm, preferably by mesopores or macropores.
[0093] Furthermore, the activated carbon prepared or manufactured in step (a) (so-called initial activated carbon) is 0.8 cm 3 / g~3.9cm 3 Within the range of / g, especially 0.9cm 3 / g~3.4cm 3 Within the range of / g, preferably 1cm 3 / g~2.9cm 3 Within the range of / g, more preferably 1.1cm 3 / g~2.4cm 3 Within the range of / g, particularly preferably 1.2cm 3 / g~1.9cm 3 Within the range of / g, particularly more preferably 1.5cm 3 / g~1.9cm 3 Total pore volume (V) within the range of / g total), in particular having a total pore volume according to Gurvitch, the present invention provides that the total pore volume of the activated carbon (initial activated carbon) prepared or manufactured in step (a), in particular 2.5% to 50%, especially 5% to 50%, preferably 10% to 50%, more preferably 15% to 45%, particularly preferably 12.5% to 47.5%, particularly more preferably 17.5% to 42.5%, and even more preferably 20% to 40% of the total pore volume according to Gurvitch, is formed by pores having a pore diameter of less than 2 nm, particularly by micropores.
[0094] As far as Gurvitch's method for determining total pore volume is concerned, this is a well-known measurement / determination method among experts in this field. For further details on Gurvitch's method for determining total pore volume, see, for example, L. Gurvitch (1915), Russian Journal, Physical Chemistry Society. 47 See, 805 and Lowell et al., "Characterization of Porous Solids and Powders: Surface Area, Pore Size, and Density," Kruwer Academic Press, Article Technology Series, page 111ff. In particular, the pore volume of activated carbon is given by equation V P =W a / ρ l It is determined based on the Gurvitch rule, which follows W a ρ represents the amount of adsorbed material that forms the basis of the adsorbent, l represents the density of the adsorbed material used (see also equation (8.20) on page 111 by S. Lowell et al.).
[0095] Furthermore, the activated carbon prepared or manufactured in step (a) (i.e., initial activated carbon) is 1,100 m 2 / g~2,600m 2 Within the range of / g, especially 1,200m 2 / g~2,400m 2 Within the range of / g, preferably 1,300m 2 / g~2,200m 2 Within the range of / g, more preferably 1,350m 2 / g~1,950m 2 Within the range of / g, a particularly preferred 1,375m2 / g~1,900m 2 / g range specific BET surface area (S BET ).
[0096] The determination of specific surface area by BET is basically known to those skilled in the art as such, so no further details need to be elaborated in this regard. All BET surface area data refer to determinations made in accordance with ASTM D6556-04. Within the scope of the present invention, the so-called multi-point BET determination method (MP-BET) is generally used for the determination of BET surface area in the partial pressure range of 0.05 to 0.1 p / p0, unless explicitly stated otherwise below.
[0097] For further details regarding the determination of BET surface area or the BET method, reference is made to the above-mentioned ASTM D6556-04, as well as Rompp Chemie Lexikon, 10th Edition, Georg Thieme Verlag, Stuttgart / New York, keyword: "BET method", and also including the cited literature, Winnacker-Küchler (3rd Edition), Volume 7, pages 93 et seq., and Z. Anal. Chem., 238, pages 187 to 193 (1968).
[0098] As mentioned above, the formation of a defined pore system with a high mesopore and macropore volume or fraction leads, as mentioned above, in particular as a result of the high mesopore and macropore fraction, to an improvement in the transport and diffusion properties of the reactants or products on which the catalytic reaction is based. At the same time, with regard to the catalyst system provided, improved catalytic properties also result from the fact that catalytically active centers or active centers are formed in smaller pores, in particular micropores.
[0099] As a result of a balanced, tailored pore size distribution with an underlying defined hierarchical pore system that has sufficiently high mesopore and macropore volumes and micropore volume for catalytic action or catalytic activity, overall improved properties with respect to the reaction kinetics of heterogeneous system catalysts are thus provided. In this regard, the aforementioned properties of the activated carbon used in method step (a) (i.e., the starting activated carbon) are directly reflected in the catalyst system according to the invention obtained in method step (d).
[0100] In this regard, particularly according to the invention, for the activated carbon prepared or produced in method step (a) (i.e., initial activated carbon), the total pore volume (V total ) and, in particular, the ratio BET surface area (S BET ) to the total pore volume according to Gurvich (quotient; Q), in particular according to the formula Q = V total / S BET , is in the range of 0.5×10 9 m to 1.9×10 9 m, in particular in the range of 0.55×10 9 m to 1.9×10 9 m, preferably in the range of 0.6×10 9 m to 1.8×10 9 m, preferably in the range of 0.65×10 9 m to 1.7×10 9 m, particularly preferably in the range of 0.65×10 9 m to 1.6×10 9 m, most preferably in the range of 0.7×10 9 m to 1.5×10 9 m, more preferably in the range of 0.75×10 9 m to 1.4×10 9 m, even more preferably in the range of 0.8×10 9 m to 1.3×10 9 m.
[0101] The aforementioned lower limit value ensures a good occupancy rate of the activated carbon and the catalytically active component, while also ensuring good mass transfer, and thus a high conversion rate in the underlying catalytic reaction. Furthermore, the aforementioned upper limit value still ensures a sufficient micropore volume, which is associated with the formation of a correspondingly large number of active sites or centers, particularly with respect to the catalytic activity involving the catalytically active component.
[0102] According to the invention, it is particularly provided that the activated carbon prepared or produced in process step (a) (i.e. the initial activated carbon) has a specific BET surface area (S 2 / g to 3,000 m 2 / g, in particular in the range from 1,100 m 2 / g to 2,600 m 2 / g, preferably in the range from 1,200 m 2 / g to 2,400 m 2 / g, more preferably in the range from 1,300 m 2 / g to 2,200 m 2 / g, particularly preferably in the range from 1,350 m 2 / g to 1,950 m 2 / g, most preferably in the range from 1,375 m 2 / g to 1,900 m 2 / g, whereby BET ) the ratio (quotient; Q) of the total pore volume (V total ), in particular the total pore volume according to Gurvich, to the specific BET surface area (S BET ) is particularly in the range from 0.5×10 total / S BET according to the formula Q=V 9 m to 1.9×10 9 m, in particular in the range from 0.55×10 9 m to 1.9×10 9 m, preferably in the range from 0.6×10 9 m to 1.8×10 9 m, preferably in the range from 0.65×10 9 m to 1.7×10 9 m, particularly preferably in the range from 0.65×10 9 m to 1.6×10 9 m, most preferably in the range from 0.7×10 9m~1.5×10 9 Within the range of m, more preferably 0.75 × 10 9 m~1.4×10 9 Within the range of m, particularly more preferably 0.8 × 10 9 m~1.3×10 9 It is within the range of m.
[0103] Furthermore, it has been found to be advantageous with respect to the present invention if the activated carbon prepared and / or manufactured in step (a) (i.e., the starting activated carbon) has an average pore size of at least 15 nm, or if the activated carbon has an average pore size of up to 100 nm.
[0104] In particular, it is preferable that the activated carbon prepared and / or manufactured in step (a) (so-called initial activated carbon) has an average pore size in the range of 15 nm to 100 nm, particularly in the range of 16 nm to 90 nm, preferably in the range of 17 nm to 85 nm, more preferably in the range of 18 nm to 80 nm, even more preferably in the range of 20 nm to 70 nm, most preferably in the range of 22 nm to 60 nm, and even more preferably in the range of 25 nm to 50 nm.
[0105] The determination of the texture characteristics of mesoporous and macroporous activated carbon used in accordance with the present invention, or the determination of the texture characteristics in the mesoporous or macroporous region, can be carried out particularly with respect to the average pore diameter by mercury intrusion. According to this method, an evaluation range of 0.01 μm to 20 μm is recorded with respect to the pore diameter.
[0106] Generally, the average pore size is four times the volume of the liquid (adsorbent) absorbed or adsorbed into the activated carbon with completely filled pores (V total ) and on the other hand, the quotient of the BET surface area (BET) (pore diameter d = 4 × V total This can be calculated from (BET). For further details, see the corresponding explanation by RW Magee (loc.cit.), particularly the mathematical expression (15) on page 71 of that document.
[0107] Furthermore, the present invention is advantageous when the activated carbon prepared and / or manufactured in step (a) (i.e., initial activated carbon) is spherical, or when the activated carbon prepared and / or manufactured in step (a) is used in the form of spherical activated carbon.
[0108] Regarding catalytic applications based on the catalyst system according to the present invention, the special shape of the activated carbon also provides better inflow characteristics, further improving the transport of reactants and products.
[0109] Regarding spherical activated carbon, for example, it is particularly relevant to improving properties when the catalyst system according to the present invention is used in a fixed-bed reactor or the like.
[0110] According to the present invention, the activated carbon prepared and / or produced in step (a) (i.e., initial activated carbon) may have a particle size, particularly particle size, in the range of 60 μm to 1000 μm, particularly in the range of 70 μm to 800 μm, preferably in the range of 80 μm to 600 μm, more preferably in the range of 100 μm to 400 μm, particularly preferably in the range of 150 μm to 375 μm, and most preferably in the range of 175 μm to 250 μm. In this regard, at least 80% by weight, particularly at least 90% by weight, preferably at least 95% by weight, of the activated carbon particles, particularly the activated carbon particles, may have a particle size, particularly particle size, in the aforementioned range.
[0111] Generally, the activated carbon prepared or manufactured in step (a) (i.e., initial activated carbon) preferably has an average particle size (D50) in the range of 60 μm to 900 μm, particularly in the range of 75 μm to 750 μm, preferably in the range of 85 μm to 550 μm, more preferably in the range of 110 μm to 375 μm, even more preferably in the range of 175 μm to 350 μm, and most preferably in the range of 185 μm to 225 μm, particularly an average particle diameter (D50).
[0112] The corresponding particle size or particle size can be determined based on methods in particular in accordance with ASTM D2862-97 / 04. Furthermore, the above size can also be determined using measurement methods such as sieve analysis, X-ray diffraction, and laser diffraction. Since each of these determination methods is well known to those skilled in the art, no further explanation is necessary.
[0113] Furthermore, the activated carbon prepared and / or manufactured in step (a) (i.e., the starting activated carbon) has a ball-pan hardness and / or abrasion hardness of at least 90%, particularly at least 95%, preferably at least 97%, more preferably at least 98%, most preferably at least 99%, and even more preferably at least 99.5%. Abrasion resistance can generally be measured according to ASTM D3802-05. Thus, the activated carbon used according to the present invention is further characterized by excellent mechanical properties, which are also expressed in high abrasion resistance. The high mechanical strength of the activated carbon used according to the present invention results in low abrasion with respect to the application of the catalyst system obtained according to the present invention, which is particularly advantageous with respect to application or service life. In addition, the excellent mechanical properties with low abrasion provide further advantages with respect to the manufacture of the catalyst system by the method of the present invention, particularly with respect to avoiding abrasion when carrying out each step of the method. The high mechanical strength of the activated carbon, and therefore also of the catalyst system according to the present invention, results in only low abrasion with respect to its use in catalytic reactions, which is particularly advantageous with respect to service life and is advantageous in avoiding sludge formation due to abrasion.
[0114] The high mechanical stability of the activated carbon used in accordance with the present invention is also reflected in its high compressive strength and / or bursting strength (weight-loading capacity per activated carbon particle). In this regard, it is preferable that the activated carbon prepared or manufactured in step (a) (i.e., the starting activated carbon) has a compressive and / or bursting strength (weight-loading capacity) of at least 5 Newtons, particularly at least 10 Newtons, preferably at least 15 Newtons, preferably at least 20 Newtons, and particularly preferably at least 22.5 Newtons per activated carbon particle, particularly per activated carbon bead. In particular, it is preferable that the activated carbon prepared or manufactured in step (a) (i.e., the starting activated carbon) has a compressive and / or bursting strength (weight-loading capacity) of 5 to 50 Newtons, particularly 10 to 45 Newtons, preferably 15 to 40 Newtons, and particularly 17.5 to 35 Newtons per activated carbon particle, particularly per activated carbon pellet. The determination of compressive strength or bursting strength can be carried out by methods known to those skilled in the art, in particular by determining the compressive strength or bursting strength of individual particles by applying force to each particle using a punch until the particle bursts.
[0115] The activated carbon prepared or manufactured in step (a) (i.e., the starting activated carbon) preferably has a vibration or tamp density in the range of 100 g / L to 1,500 g / L, particularly in the range of 125 g / L to 1,000 g / L, preferably in the range of 150 g / L to 800 g / L, more preferably in the range of 200 g / L to 600 g / L, particularly preferably in the range of 225 g / L to 500 g / L, most preferably in the range of 250 g / L to 400 g / L, and even more preferably in the range of 255 g / L to 395 g / L. In particular, the activated carbon prepared or manufactured in step (a) (i.e., the starting activated carbon) preferably has a bulk density in the range of 150 g / L to 1,000 g / L, particularly in the range of 250 g / L to 700 g / L, preferably in the range of 300 g / L to 600 g / L, and more preferably in the range of 300 g / L to 550 g / L. Bulk density is measured in particular according to ASTM B527-93 / 00.
[0116] Furthermore, the activated carbon prepared or manufactured in step (a) (i.e., the starting activated carbon) preferably has at least 35%, particularly at least 40%, preferably at least 45%, and preferably at least 47.5% butane adsorption, and / or preferably has butane adsorption in the range of 35% to 90%, particularly in the range of 40% to 85%, preferably in the range of 45% to 80%, and more preferably in the range of 47.5% to 75%. The amount of butane adsorption is measured in particular according to ASTM D5742-95 / 00.
[0117] Furthermore, the activated carbon prepared and / or manufactured in step (a) of the method (i.e., the starting activated carbon) preferably has an iodine value of at least 1,250 mg / g, particularly at least 1,300 mg / g, preferably at least 1,400 mg / g, more preferably at least 1,425 mg / g, and / or the activated carbon prepared and / or manufactured in step (a) of the method preferably has an iodine value in the range of 1,250 mg / g to 2,100 mg / g, particularly in the range of 1,300 mg / g to 2,000 mg / g, preferably in the range of 1,400 mg / g to 1,900 mg / g, and preferably in the range of 1,425 mg / g to 1,850 mg / g. In particular, the iodine value can be determined according to ASTM D4607-94 / 99. The iodine value can be evaluated as a measure of the available surface area, which is mainly provided by small mesopores, and the above values of the iodine value indicate that the activated carbon used according to the present invention can have particularly high mesoporosity.
[0118] Furthermore, it is preferable that the activated carbon prepared and / or manufactured in step (a) (i.e., the starting activated carbon) has a methylene blue value of at least 17 mL, particularly at least 18 mL, preferably at least 19 mL, more preferably at least 19.5 mL, and / or that the activated carbon prepared and / or manufactured in step (a) has a methylene blue value in the range of 17 mL to 65 mL, particularly in the range of 18 mL to 55 mL, preferably in the range of 19 mL to 50 mL, more preferably in the range of 19.5 mL to 47.5 mL.
[0119] In particular, the activated carbon prepared and / or manufactured in step (a) of the method (i.e., the starting activated carbon) preferably has a molasses count of at least 255, particularly at least 310, preferably at least 375, and more preferably at least 510, and / or the activated carbon prepared and / or manufactured in step (a) of the method preferably has a molasses count in the range of 255 to 1,500, particularly in the range of 310 to 1,400, preferably in the range of 375 to 1,300, and more preferably in the range of 510 to 1,250.
[0120] Due to its high mesoporosity and macroporosity, the activated carbon according to the present invention likewise exhibits a high methylene blue value and molasses adsorption number, which together can be evaluated as a measure of the available surface area primarily provided by mesopores and macropores. Therefore, under defined conditions, the methylene blue number or methylene blue adsorption amount, which refers to the adsorption amount of methylene blue per defined amount of adsorbent (i.e., the volume or number of milliliters (mL) of a methylene blue standard solution decolorized by a defined amount of dry powdered adsorbent), can serve as an indicator of the adsorption capacity of the activated carbon of the present invention for molecules having a size comparable to that of methylene blue, since mesopores tend to be small. Furthermore, the molasses number, which is considered as a measure of mesoporosity and macroporosity and indicates the amount of adsorbent required to decolorize a standard molasses solution, serves as an indicator of the adsorption capacity of the activated carbon according to the present invention for molecules having a size comparable to that of molasses (generally beet molasses). Therefore, the combined values of methylene blue and molasses can be regarded as a measure of the mesoporosity and macroporosity, particularly the mesoporosity, of the activated carbon according to the present invention.
[0121] The dimensionless molasses number can basically be determined by the Norit method (Norit N.V. Amersfoort, the Netherlands, Norit Standard Method NSTM2.19 "Density (Europe)") or by PACS = Professional Analytical and Consulting Services Inc, Collaropolis, Pennsylvania, USA). For the purposes of the present invention, the value of the molasses number is determined according to the PACS method. In the determination of the molasses number by the Norit method or the PACS method, the amount of powdered activated carbon required to decolorize a standard molasses solution is determined. The determination is carried out by preparing a standard molasses solution against a standard activated carbon with molasses number 245 and / or 350 and using a photometer. For details in this regard, reference can be made to the two aforementioned regulations.
[0122] The methylene blue value can be determined according to the method of CEFIC (European Chemical Industry Council, 250 Louis Street, Bte 71, B-1050 Brussels, November 1986, European Chemical Industry Council, Test Methods for Activated Carbon, Section 2.4 "Methylene Blue Value", pp. 27 / 28).
[0123] Therefore, the methylene blue value obtained by the CEFIC method described above is defined by the number of mL of methylene blue standard solution decolorized with 0.1 g of dry activated carbon powder. This method requires a glass container with a glass stopper, a filter, and methylene blue standard solution, which is prepared as follows: Dissolve 1200 mg of pure methylene blue dye (equivalent to approximately 1.5 g of methylene blue from DAB VI [German Pharmacopoeia 6th Edition] or an equivalent) in water in a 1000 mL volumetric flask and let the solution stand for several hours or overnight; for confirmation, place 5.0 mL into the volumetric flask, dilute to 1.0 L with 0.25% (volume fraction) acetic acid, and measure the absorbance at 620 nm, path length 1 cm, and set to (0.840 ± 0.010). If the absorbance is high, dilute with the calculated amount of water; if it is low, discard the solution and prepare it again. To prepare the sample, crush the activated carbon (<0.1 mm) and dry it at 150 °C to a constant weight. An exact 0.1 g of spherical carbon is combined with 25 mL (5 mL) of methylene blue standard solution in a ground glass flask (a preliminary test is performed to determine whether an initial addition of 5 mL of 25 mL of methylene blue standard solution or 1 mL of 5 mL of methylene blue standard solution is usable). Shake until decolorization occurs. Then, add another 5 mL (1 mL) of methylene blue standard solution and shake until decolorization occurs. Repeat the addition of methylene blue standard solution in 5 mL (1 mL) volumes as long as decolorization occurs within 5 minutes. Record the total volume of test solution decolorized by the sample. Repeat the test to confirm the obtained results. The volume (mL) of methylene blue standard solution that is decolorized is taken as the methylene blue value of the activated carbon. Note that since the dye methylene blue is sensitive to heat, it is necessary to correct for the water content by calculation without drying.
[0124] According to the present invention, the activated carbon prepared and / or manufactured in step (a) above (i.e., the starting activated carbon) has a gravimetrically adsorbed amount of N2 V determined at a partial pressure p / p0 of 0.25. ads(wt) However, at least 250cm 3 / g, especially at least 300cm 3 / g, preferably at least 350cm 3 / g, more preferably at least 375cm² 3 It is further possible that it is / g. In this regard, the activated carbon prepared and / or manufactured in step (a) of the method is 250 cm 3 / g~850cm 3 Within the range of / g, especially 300cm 3 / g~700cm 3 Within the range of / g, preferably 350cm 3 / g~650cm 3 Within the range of / g, more preferably 375cm 3 / g~625cm 3 Gravimetric adsorption amount V is determined by the partial pressure p / p0 of 0.25 within the range of / g. ads(wt) It is preferable that it has
[0125] Generally, the activated carbon purified and / or produced in step (a) of the method (i.e., initial activated carbon) is at least 50 cm³. 3 / cm 3 , especially at least 100cm 3 / cm 3 Preferably at least 110 cm 3 / cm 3 The volume-based amount of adsorbed N2 V is determined by the partial pressure p / p0 of 0.25. ads(vol.) It can have the following characteristics. In this regard, the activated carbon purified or produced in step (a) of the method is determined at a partial pressure of 0.25 p / p0, at 50 cm 3 / cm 3 ~300cm 3 / cm 3 Within the range, especially 80cm 3 / cm 3 ~275cm 3 / cm 3 Within the range, preferably 90 cm 3 / cm3 ~250cm 3 / cm 3 Within the range, more preferably 95 cm 3 / cm 3 ~225cm 3 / cm 3 Capacity-based adsorption amount of N2 within the range V ads(vol.) It can be specifically defined that it possesses [this characteristic].
[0126] Similarly, the activated carbon purified or produced in step (a) of the method (i.e., the starting activated carbon) is at least 300 cm³. 3 / g, especially at least 450cm 3 / g, preferably at least 475cm 3 Gravimetric adsorbed N2 amount V is determined by the partial pressure p / p0 of 0.995 / g. ads(wt.) It is preferable that the present invention provides having the following characteristics. In particular, the activated carbon purified or produced in step (a) of the method is 300 cm². 3 / g~2,300cm 3 Within the range of / g, especially 400cm 3 / g~2,200cm 3 Within the range of / g, preferably 450cm 3 / g~2,100cm 3 Within the range of / g, more preferably 475cm 3 / g~2,100cm 3 Gravimetric adsorption N2 capacity V is determined by a partial pressure p / p0 of 0.995 within the range of / g. ads(wt.) It is preferable that it has
[0127] Furthermore, the activated carbon refined or produced in step (a) of the method (i.e., initial activated carbon) should be subjected to at least 200 cm³ of evaporation. 3 / cm 3 , especially at least 250cm 3 / cm 3 Preferably at least 275 cm 3 / cm 3 , more preferably at least 295 cm 3 / cm 3 The volume-related amount of adsorbed N2 V is determined by the partial pressure p / p0 of 0.995.ads(vol.) It is preferable to have the above. According to the present invention, the activated carbon purified or produced in step (a) (i.e., initial activated carbon) is 200 cm 3 / cm 3 ~500cm 3 / cm 3 Within the range, especially 250cm 3 / cm 3 ~400cm 3 / cm 3 Within the range, preferably 275 cm 3 / cm 3 ~380cm 3 / cm 3 Within the range, more preferably at least 295 cm 3 / cm 3 ~375cm 3 / cm 3 Volume-related adsorbed N2 amount V is determined by a partial pressure p / p0 of 0.995 within the range. ads(vol.) It is preferable that it has
[0128] As a result, the amount V related to the weight and volume of activated carbon according to the present invention ads (N2) is very large at different partial pressures p / p0, which can be seen as evidence of the excellent adsorption properties and superior suitability as a catalyst support of the activated carbon used according to the present invention.
[0129] According to the present invention, the activated carbon prepared or manufactured in step (a) (i.e., the starting activated carbon) preferably has a fractal dimension of open porosity in the range of 2.6 to 2.99, particularly in the range of 2.7 to 2.95, and / or preferably has a fractal dimension of open porosity of at least 2.7, particularly at least 2.8, preferably at least 2.85, and more preferably at least 2.9. The fractal dimension of open porosity serves as an indicator of the fine irregularities on the inner surface of the activated carbon. Further details in this regard, in particular for determining the fractal dimension of the activated carbon used according to the present invention, can be found in publications DE 102 54 241 A1, WO2004 / 046033A1, EP 1 562 855 B1 and US2006 / 148645A1, which belong to the same patent family, in particular by reference to Embodiment 4 cited in each publication. The contents of each cited publication are thus fully included by reference. The aforementioned fractal dimension leads to further improvement of the catalytic properties of the catalyst system produced by the method according to the present invention.
[0130] According to the present invention, the activated carbon purified and / or produced in step (a) above (i.e., the starting activated carbon) is preferably activated carbon obtained by carbonization and subsequent activation of an organic polymer-based starting material, particularly in the form of polymer-based, preferably spherical activated carbon (PBSAC or polymer-based spherical activated carbon).
[0131] Activated carbon in the form of PBSAC is particularly associated with its defined pore properties, defined shape, and high mechanical stability.
[0132] In particular, the starting material for activated carbon refined and / or produced in step (a) above (i.e., starting activated carbon) can be used in the form of granular and / or spherical, preferably spherical, starting material, and / or the starting material for activated carbon refined and / or produced in step (a) above is used in the form of granular and / or spherical, preferably spherical, starting material.
[0133] Furthermore, the starting material for the activated carbon purified or produced in step (a) of the method (i.e., the starting activated carbon) preferably has a particle size, particularly a particle diameter, within the range of 60 μm to 1,000 μm, particularly within the range of 70 μm to 800 μm, preferably within the range of 80 μm to 600 μm, more preferably within the range of 100 μm to 400 μm, particularly more preferably within the range of 150 μm to 375 μm, and most preferably within the range of 175 μm to 250 μm. In this regard, at least 80% by weight, particularly at least 90% by weight, and preferably at least 95% by weight of the particles of the starting material may have a particle size, particularly a particle diameter, within the above range.
[0134] Furthermore, the starting material for the activated carbon prepared or manufactured in step (a) of the method (i.e., the starting activated carbon) preferably has an average particle size (D50) in the range of 60 μm to 900 μm, particularly in the range of 75 μm to 750 μm, preferably in the range of 85 μm to 550 μm, more preferably in the range of 110 μm to 375 μm, even more preferably in the range of 175 μm to 350 μm, and most preferably in the range of 185 μm to 225 μm, particularly an average particle diameter (D50).
[0135] In particular, the starting material for the activated carbon prepared and / or manufactured in step (a) above (i.e., the starting activated carbon) is preferably a starting material based on an ion exchange resin precursor.
[0136] Furthermore, the starting material for the activated carbon prepared and / or produced in step (a) above (i.e., the starting activated carbon) is preferably an organic polymer-based starting material, particularly based on divinylbenzene-crosslinked polystyrene, and more preferably based on a styrene / divinylbenzene copolymer. In this regard, the content of divinylbenzene in the starting material is preferably in the range of 0.1% to 25% by weight, particularly in the range of 0.5% to 20% by weight, preferably in the range of 1% to 15% by weight, and more preferably in the range of 2% to 10% by weight, based on the starting material. For specific starting materials to be used, please refer to the detailed description of the embodiments.
[0137] According to the present invention, the activated carbon prepared and / or manufactured in step (a) of the method (i.e., initial activated carbon) is: (i) Carbonization of polymeric organic sulfonation starting materials (containing sulfonic acid groups), particularly particulate, preferably spherical polymeric organic sulfonation starting materials; then, (ii) It is particularly preferable that activated carbon, as defined in any of the preceding claims, can be obtained by activating the carbide (carbonized starting material) obtained in step (i).
[0138] Furthermore, it is provided that the method step of sulfonating polymerizable organic starting materials is carried out, in particular by contacting the starting materials with at least one sulfonating agent, prior to the method step (i) of carbonization. In this regard, the sulfonating agent is used in liquid form.
[0139] In particular, sulfur trioxide (SO3), especially in the form of oleum and / or preferably concentrated sulfuric acid, is used as a sulfonating agent. However, according to the present invention, it is also possible to start from already sulfonated materials.
[0140] In general, with respect to the present invention, in step (i) above, carbonization is carried out at a temperature in the range of 100°C to 1,200°C, particularly in the range of 120°C to 1,100°C, preferably in the range of 140°C to 1,000°C, and more preferably in the range of 150°C to 950°C.
[0141] In this regard, the present invention provides that in step (i) of the method, carbonization is carried out in multiple steps, particularly two steps, preferably using a temperature gradient and / or temperature profile. In this regard, in the first step, the method is carried out at a temperature in the range of 100°C to 600°C, particularly in the range of 120°C to 590°C, preferably in the range of 140°C to 570°C, more preferably in the range of 150°C to 550°C. Furthermore, in the second step, the method can be carried out at a temperature in the range of 500°C to 1,200°C, particularly in the range of 510°C to 1,100°C, preferably in the range of 530°C to 1,000°C, more preferably in the range of 550°C to 950°C.
[0142] According to the present invention, in step (i) of the method, carbonization is carried out for a period of time in the range of 0.1 hours to 20 hours, particularly in the range of 0.5 hours to 15 hours, preferably in the range of 1 hour to 10 hours, more preferably in the range of 1.5 hours to 8 hours, and most preferably in the range of 2 hours to 6 hours.
[0143] Within the scope of the method according to the present invention, in step (i) the carbonization is carried out such that chemical groups, particularly strongly acidic chemical groups, preferably sulfonic acid groups, are thermally decomposed or separated from the sulfonated starting material, particularly in connection with the formation of free radicals or crosslinks, preferably the initiation of carbonization or thermal decomposition of the starting material occurs in connection with the crosslinking of the polymer of the starting material and / or the formation of carbon.
[0144] Furthermore, in step (i) of the method, carbonization is carried out such that, in particular, after the thermal decomposition or removal of chemical groups, especially strongly acidic chemical groups, preferably sulfonic acid groups, more extensive or especially complete carbonization of the starting material occurs.
[0145] For example, step (i) of the method is carried out such that the thermal decomposition or removal of chemical groups, particularly strongly acidic chemical groups, preferably sulfonic acid groups, is carried out in the first step of carbonization. Furthermore, step (i) of the method is carried out such that further and / or complete carbonization of the starting material is carried out in the second step.
[0146] Generally, step (i) is preferably carried out in an inert atmosphere, particularly a nitrogen atmosphere, or at most a slightly oxidizing atmosphere. The present invention optionally provides that, in step (i), water in particular in the form of water vapor and / or an inert gas / water vapor mixture, preferably a nitrogen / water vapor mixture, is added to the carbonization atmosphere, particularly an inert atmosphere, during carbonization.
[0147] Furthermore, with respect to step (ii) of the method, the activation is carried out at a temperature in the range of 500°C to 1,200°C, particularly in the range of 800°C to 1,100°C, preferably in the range of 850°C to 1,000°C, and more preferably in the range of 900°C to 975°C. Furthermore, in step (ii) of the method, the activation is carried out over a period of time in the range of 0.5 hours to 20 hours, particularly in the range of 1 hour to 15 hours, and preferably in the range of 2 hours to 10 hours.
[0148] Generally, in step (ii) of the method, the activation is carried out in the form of at least one activating gas, particularly oxygen, preferably air, water vapor and / or carbon dioxide or a mixture of these activating gases, and / or in the presence of an inert gas / water vapor mixture, preferably a nitrogen / water vapor mixture, and / or in the presence of pure carbon dioxide or an inert gas / carbon dioxide mixture, particularly nitrogen / carbon dioxide.
[0149] The basic principle of activation provided in step (ii) of the present invention is, in particular, to selectively and specifically decompose or burn a portion of the carbon generated during carbonization under appropriate conditions, thereby further forming or specifically adjusting and, so to speak, finalizing the pore system.
[0150] The activated carbon provided or manufactured in step (a) above is, in principle, commercially available in the specific details shown herein, particularly from Blüchergemweh, as far as is relevant in general. Further details relating to the activated carbon provided or manufactured in accordance with the present invention in step (a) above, particularly with respect to the carbonization and activation steps, can be referenced to international patent application WO98 / 07655A1 and patent applications DE 196 53 238 A1, DE 196 50 414 A1, EP 0 952 960 A1 and US6300276B1, which belong to the same patent family, and the disclosures thereof are fully incorporated herein by reference. Furthermore, DE 4304 026 A1 and US6184177B1, which belong to the same patent family, can also be referenced, and the disclosures thereof are fully incorporated herein by reference. Furthermore, reference can also be made to international patent application WO2017 / 097447A1 and parallel patent applications DE 10 2016 101 215 A1, EP3362407A1 and US2019 / 177170A1, the disclosures of each of these are equally incorporated herein by reference.
[0151] The following describes step (b) of the method, which involves the oxidation of activated carbon, in more detail:
[0152] In general, the activated carbon oxidized in step (b) of the method, particularly the oxidized surface, has an oxygen content, particularly surface oxidation content, in the range of 4% (atomic%) to 20%, particularly in the range of 5% to 20%, preferably in the range of 5.5% to 18%, more preferably in the range of 6% to 15%, and even more preferably in the range of 7% to 12.5%, based on the total elemental composition of the oxidized activated carbon as measured by X-ray photoelectron spectroscopy [XPS (=X-Ray Phtoelectron Spectroscopy), ESCA (=Electron Spectroscopy for Chemical Analysis)].
[0153] According to the present invention, the activated carbon oxidized in step (b) of the method, particularly the oxidized surface, has an oxygen content of at least 5% (atomic percent), preferably at least 5.5%, preferably at least 6%, and particularly preferably at least 7%, particularly surface oxygen content, based on the total elemental composition of the oxidized activated carbon, which is determined in particular using XPS or ESCA.
[0154] According to the present invention, it is possible to provide that the activated carbon oxidized in step (b) above, particularly the oxidized surface, has an oxygen content, particularly the surface oxygen content, determined in particular by X-ray photoelectron spectroscopy (XPS or ESCA), which is up to 20% (atomic%), preferably up to 18%, preferably up to 15%, and particularly preferably up to 12.5%, based on the total elemental composition of the oxidized activated carbon.
[0155] In this regard, the present invention prefers that the activated carbon oxidized in step (b) above, particularly the oxidized surface, is formed of at least essentially carbon. In this regard, it is preferable that the activated carbon oxidized in step (b) above, particularly the oxidized surface, has traces of elements other than oxygen and carbon, particularly nitrogen, sulfur and / or chlorine, in amounts of up to 2% (atomic percent), particularly up to 1.5%, preferably up to 1%, calculated as the sum of elements other than oxygen and carbon based on the total elemental composition of the oxidized activated carbon.
[0156] Without wishing to be limited to this theory, the method according to the present invention generates an oxide layer on the (pore) surface of activated carbon, which generally has oxygen-containing functional groups as described below. Subsequently, the surface oxidation is finished with a catalytically active component, particularly in the region of the oxide layer (boundary layer), without limiting or clarifying this theory, thereby increasing the affinity of the oxygen-containing functional groups, particularly their interaction with the catalytically active component, or, in a sense, acting as a binding or fixing point for the catalytically active component used according to the present invention.
[0157] Therefore, the method according to the present invention provides a catalyst system having a catalytic or reactive surface by equipping activated carbon with a catalytically active component following oxidation.
[0158] With respect to the range of oxygen content of the activated carbon oxidized in step (b) of the method, the stated lower limit ensures that there is still a region that is sufficiently capable of binding for catalytically active components or their precursors. The upper limit ensures that the carbon content in the oxidized activated carbon is high enough to form a stable framework, accompanied by the presence of a pore system that continues to be defined in terms of corresponding mechanical stability and, in particular, the corresponding total pore volume and specific BET surface area by Gulvitch.
[0159] As shown above, a relatively hydrophilic activated carbon is obtained as a result of the target and purpose-oriented oxidation treatment in step (b) of the method, and based on this, the finishing with catalytic active components or their precursors is improved.
[0160] Given this background, the hydrophilicity of activated carbon can be described as follows: In particular, the activated carbon oxidized in step (b) of the method, especially the oxidized surface, has hydrophilicity determined as water vapor adsorption behavior such that at a partial pressure p / p0 of 0.6, at least 35%, particularly at least 40%, preferably at least 50%, and more preferably at least 60% of the maximum water vapor saturation load of the activated carbon is achieved. Furthermore, the activated carbon oxidized in step (b) of the method, particularly the oxidized surface, has hydrophilicity determined as water vapor absorption behavior such that, at a partial pressure of 0.6 p / p0, a maximum of 100%, particularly 99%, preferably 98%, more preferably 95%, and most preferably 90% of the activated carbon's maximum water vapor saturation load is achieved. Furthermore, the activated carbon oxidized in step (b) of the method, particularly the oxidized surface, has hydrophilicity determined as water vapor adsorption behavior such that at a partial pressure p / p0 of 0.6, 30% to 100%, particularly 35% to 99%, preferably 40% to 98%, more preferably 50% to 95%, and most preferably 60% to 90% of the maximum water vapor saturation load of the activated carbon is achieved. In particular, the activated carbon oxidized in step (b) of the method, especially the oxidized surface, has hydrophilicity determined as water vapor absorption behavior such that at least 30%, particularly at least 35%, preferably at least 40%, more preferably at least 50%, and especially preferably at least 60% of the maximum water vapor saturation load of the activated carbon is achieved in the partial pressure range p / p0 of 0.1 to 0.6. In particular, the activated carbon oxidized in step (b) of the method, especially the oxidized surface, has hydrophilicity determined as water vapor absorption behavior such that a maximum of 100%, particularly a maximum of 99%, preferably a maximum of 98%, more preferably a maximum of 95%, and especially preferably a maximum of 90% of the maximum water vapor saturation load of the activated carbon is achieved in the partial pressure range p / p0 of 0.1 to 0.6. Furthermore, the activated carbon oxidized in step (b) of the method, particularly the oxidized surface, has hydrophilicity determined as a water vapor adsorption behavior such that at a partial pressure p / p0 of 0.1 to 0.6, 30% to 100%, particularly 35% to 99%, preferably 40% to 98%, more preferably 50% to 95%, and most preferably 60% to 90% of the maximum water vapor saturation load of the activated carbon is achieved.
[0161] In addition to the hydrophilicity of the activated carbon oxidized in step (b) of the method described above, the following can be noted: Therefore, with respect to the activated carbon oxidized in step (b), the oxidation, particularly surface oxidation, of the activated carbon prepared or manufactured in step (a) is carried out within the scope of the present invention, such that the oxidation, particularly surface oxidation, is carried out under conditions that the oxidized, particularly surface-oxidized, activated carbon has hydrophilicity determined as water vapor adsorption behavior, and is carried out under conditions that the oxidized, particularly surface-oxidized, activated carbon has hydrophilicity determined as water vapor adsorption behavior, and is carried out under conditions that 30% of the maximum water vapor adsorption capacity of the activated carbon is consumed or utilized at a partial pressure of 0.6 p / p0. In particular, the activated carbon oxidized in step (b) of the method, especially the oxidized surface, has hydrophilicity such that, at a partial pressure of 0.6 p / p0, at least 30%, particularly at least 35%, preferably at least 40%, more preferably at least 50%, and especially preferably at least 60% of the maximum water vapor adsorption capacity of the activated carbon is consumed and / or utilized. Furthermore, the activated carbon oxidized in step (b) of the method, particularly the oxidized surface, has hydrophilicity such that, at a partial pressure of 0.6 p / p0, up to 100%, particularly up to 99%, preferably up to 98%, more preferably up to 95%, and most preferably up to 90% of the activated carbon's maximum water vapor adsorption capacity is consumed and / or utilized. Similarly, the activated carbon oxidized in step (b) of the method, particularly the oxidized surface, has hydrophilicity such that, at a partial pressure of 0.6 p / p0, 30% to 100%, particularly 35% to 99%, preferably 40% to 98%, more preferably 50% to 95%, and especially preferably 60% to 90% of the activated carbon's maximum water vapor adsorption capacity is consumed and / or utilized. Furthermore, the activated carbon oxidized in step (b) of the method, particularly the oxidized surface, has hydrophilicity such that, at a partial pressure of 0.1 to 0.6 p / p0, at least 30%, particularly at least 35%, preferably at least 40%, more preferably at least 50%, and especially preferably at least 60% of the maximum water vapor adsorption capacity of the activated carbon is consumed and / or utilized. In particular, the activated carbon oxidized in step (b) of the method, especially the oxidized surface, has hydrophilicity such that, at partial pressures p / p0 of 0.1 to 0.6, up to 100%, particularly up to 99%, preferably up to 98%, more preferably up to 95%, and especially preferably up to 90% of the activated carbon's maximum water vapor adsorption capacity is consumed and / or utilized. According to the present invention, the activated carbon oxidized in step (b) above, particularly the oxidized surface, has hydrophilicity such that, at a partial pressure of 0.1 to 0.6 p / p0, 30% to 100%, particularly 35% to 99%, preferably 40% to 98%, more preferably 50% to 95%, and especially preferably 60% to 90% of the maximum water vapor adsorption capacity of the activated carbon is consumed and / or utilized.
[0162] Furthermore, the activated carbon oxidized in step (b) of the method may also have the following properties with respect to hydrophilicity: Furthermore, the activated carbon oxidized in step (b) above, particularly the oxidized surface, at a partial pressure of 0.6 p / p0, is used to determine the amount of water vapor (H2O) adsorbed by the activated carbon based on the weight of the activated carbon (Vads). (H2O) However, at least 200cm 3 / g, especially at least 250cm 3 / g, preferably at least 300cm 3 / g, more preferably at least 325cm 3 / g, preferably at least 350cm 3 It possesses hydrophilicity determined by its water vapor adsorption behavior, such that the ratio is / g. Furthermore, the activated carbon oxidized in step (b) above, particularly the oxidized surface, at a partial pressure of 0.6 p / p0, is used to determine the amount of water vapor (H2O) adsorbed by the activated carbon based on the weight of the activated carbon (Vads). (H2O) However, up to 1,000cm 3 / g, especially up to 900cm 3 / g, preferably up to 800cm 3 / g, more preferably up to 700cm 3 / g, particularly preferably up to 600cm 3 It possesses hydrophilicity determined by its water vapor adsorption behavior, such that the ratio is / g. According to the present invention, the activated carbon oxidized in step (b) above, particularly the oxidized surface, is used to determine the amount of water vapor (H2O) adsorbed by the activated carbon, based on the weight of the activated carbon, at a partial pressure of 0.6 p / p0, in Vads. (H2O) However, 200cm 3 / g~1,000cm 3 Within the range of / g, especially 250cm 3 / g~900cm 3 Within the range of / g, preferably 300cm 3 / g~800cm 3 Within the range of / g, more preferably 325cm 3 / g~700cm 3 Within the range of / g, particularly preferably 350cm 3 / g~600cm 3 It possesses hydrophilicity determined by its water vapor adsorption behavior, such that it falls within the range of / g.
[0163] The above values for water vapor adsorption behavior refer, in particular, to the water vapor adsorption isotherm that forms the basis of the activated carbon obtained according to the present invention in step (b) of the method described above.
[0164] With regard to the determination of water vapor adsorption behavior, within the scope of the present invention, this is carried out by using water or water vapor as the underlying adsorbent or adsorbent, in accordance with DIN 66135-1. In this regard, the determination of water vapor adsorption behavior is performed statically and volumetrically at a temperature of 25°C (298 Kelvin). The pressure-dependent volume (Vads) of the adsorbed water or adsorbed water vapor that forms the basis of the water vapor adsorption behavior. (STP) The measurement is performed at varying or variable ambient pressures p / p0 in the range of 0.0 to 1.0, where p0 represents the pressure under standard conditions (1,013.25 hPa). The water vapor adsorption behavior used in accordance with the present invention relates to the adsorption isotherm of the underlying activated carbon.
[0165] For further information and explanations regarding water vapor adsorption, one can also refer to the doctoral dissertation by M. Neutsche, "Adsorption of Water Vapor and n-Butane in Activated Carbon: Mechanisms, Equilibrium, and Dynamics of Monoadsorption and Coadsorption," Faculty of Mechanical, Methods and Energy Engineering, Freiberg University of Mining Technology. The entire content on this subject, particularly the explanation of water vapor or water adsorption on activated carbon, is included here by full reference.
[0166] The water vapor adsorption behavior defined above serves as a measure of the hydrophilicity or hydrophobicity of the activated carbon used in accordance with the present invention, and based on the value defined above, the activated carbon obtained in step (b) and used in subsequent step steps is polar or hydrophilic as a whole (i.e., compared to the starting activated carbon used), and therefore has an effect that can be described as hydrophilic as a whole under normal use.
[0167] According to the present invention, the oxidation of activated carbon in step (b) above, particularly surface oxidation, is further such that the oxidized, particularly surface-oxidized, activated carbon thus obtained has an oxygen-containing group content calculated and / or expressed as a volatile component content ("fB") in the range of 1% by weight to 30% by weight, particularly in the range of 1.5% to 25% by weight, preferably in the range of 2% to 20% by weight, more preferably in the range of 3% to 15% by weight, based on the dry weight of the oxidized activated carbon. In this case, the oxygen-containing functional group content can be adjusted by temperature and / or time and / or the type and / or concentration of the oxidizing agent.
[0168] In this regard, the method according to the present invention can be used to control the oxidation of activated carbon, also from the viewpoint of optimizing the subsequent finishing by the catalytically active component.
[0169] Within the scope of the method according to the present invention, the oxygen content of activated carbon oxidized on its surface, expressed as the starting activated carbon-volatile component content ("fB"), can be increased significantly compared to generally having an oxygen content of less than 1% by weight, based on the dry weight of the starting activated carbon. The oxygen content described refers in particular to the activated carbon oxidized in method step (b) before carrying out the reduction subsequently provided by method step (d). The volatile component content ("fB") generally functions as a measure of oxidation and in particular indicates the surface oxides formed by oxidation. In particular, the volatile component content can be measured in accordance with ISO 562:1981. In particular, the volatile component content (fB) can be measured by appropriately heating pre-dried activated carbon at 900°C for 7 minutes under inert conditions to oxidize the surface.
[0170] By forming and adjusting the content of oxygen-containing functional groups as needed, the amount of catalytically active components or related precursors used thereafter, particularly in step (c), can be predetermined or influenced. In this regard, those skilled in the art can at any time select relevant properties and adapt them to each other so that a desired load with the catalytically active components is achieved in the sense of the present invention.
[0171] Generally, oxidation can be carried out in a gaseous atmosphere or wet chemically (especially when using acids).
[0172] According to the present invention, in step (b), the oxidation of activated carbon, particularly surface oxidation, can be carried out using at least one oxidizing agent. The oxidizing agent can be selected from the group consisting of oxygen, ozone, inorganic or organic oxides and peroxides, particularly hydrogen peroxide, inorganic or organic acids and peracids, particularly mineral acids, and combinations thereof.
[0173] In particular, the oxidizing agent can be selected from the group consisting of oxygen, hydrogen peroxide (H2O2), nitrogen oxides (preferably NO and / or NO2), hydrochloric acid (HCl), nitric acid (HNO3), sulfuric acid (H2SO4), perchloric acid (HClO4), phosphoric acid (H3PO4), and combinations thereof.
[0174] More preferably, the oxidizing agent is selected from the group consisting of oxygen (O2), hydrochloric acid (HCl), nitric acid (HNO3), sulfuric acid (H2SO4), perchloric acid (HClO4), phosphoric acid (H3PO4), hydrogen peroxide (H2O2), and combinations thereof; particularly preferably from the group consisting of oxygen (O2), hydrochloric acid (HCl), nitric acid (HNO3), and combinations thereof; and more preferably from the group consisting of oxygen (O2), nitric acid (HNO3), and combinations thereof.
[0175] Regarding the use of oxygen, it is possible to utilize oxygen from the atmosphere or synthetic air.
[0176] In general, with respect to the present invention, in step (b) of the method, the oxidation of activated carbon, particularly surface oxidation, can be carried out by heating, and in particular, surface oxidation can be carried out at a temperature such that the reaction between the oxidizing agent and the activated carbon takes place, resulting in the formation of oxygen-containing functional groups on the surface of the activated carbon. Thus, the oxidation of activated carbon, particularly surface oxidation, can be carried out at a temperature in the range of -20°C to 1000°C, particularly in the range of 0°C to 800°C, preferably in the range of 5°C to 700°C, more preferably in the range of 10°C to 600°C, and most preferably in the range of 20°C to 550°C. In this regard, the oxidation of activated carbon, particularly surface oxidation, is carried out over a period of up to 48 hours, particularly up to 24 hours, preferably up to 12 hours. According to the present invention, the oxidation of activated carbon, particularly surface oxidation, is carried out for a time in the range of, for example, 1 minute to 1000 minutes, particularly in the range of 5 minutes to 800 minutes, preferably in the range of 10 minutes to 600 minutes.
[0177] According to the present invention, oxidation of activated carbon, particularly surface oxidation, is carried out in conjunction with the formation of a hydrophilic surface of the activated carbon. In this respect, oxidation of activated carbon, particularly surface oxidation, is carried out by forming oxygen-containing functional groups on the surface of the activated carbon. Furthermore, oxidation of activated carbon, particularly surface oxidation, results in the formation of oxygen-containing functional groups, particularly on the surface of the activated carbon. In this respect, the oxygen-containing functional group is preferably selected from acidic and basic oxygen-containing functional groups and combinations thereof, particularly acidic and basic surface oxides. In particular, the oxygen-containing functional group is preferably selected from the group consisting of hydroxyl groups, carboxyl groups, carbonyl groups, anhydrides, lactones, quinones, pyrones, chromenes, and ether groups and combinations thereof, particularly from the group consisting of hydroxyl groups, carboxyl groups, and ether groups and combinations thereof.
[0178] According to the first embodiment of the present invention, in step (b), the oxidation of activated carbon, particularly surface oxidation, is carried out using an oxidizing agent in the form of oxygen (O2). Therefore, in step (b), the oxidation, particularly surface oxidation, is carried out using oxygen (O2) as the oxidizing agent. In this regard, the oxidation of activated carbon, particularly surface oxidation, is carried out at a temperature in the range of 100°C to 1000°C, particularly in the range of 200°C to 800°C, preferably in the range of 300°C to 700°C, more preferably in the range of 350°C to 600°C, and particularly preferably in the range of 400°C to 550°C. In particular, the oxidation of activated carbon, particularly surface oxidation, is carried out for a period of up to 10 hours, particularly in the range of up to 8 hours, preferably in the range of up to 6 hours, and the oxidation of activated carbon, particularly surface oxidation, is carried out for a time in the range of 30 minutes to 1000 minutes, particularly in the range of 60 minutes to 800 minutes, preferably in the range of 100 minutes to 600 minutes. In this regard, it is possible to proceed in the framework of air oxidation or oxidation in a gas atmosphere.
[0179] In contrast, according to further embodiments of the present invention, the oxidation of activated carbon, particularly surface oxidation, may also be carried out in step (b) using an oxidizing agent, which is a mineral acid such as nitric acid (HNO3). In this regard, a wet chemical method can be used in particular. In this regard, it is therefore preferable according to the present invention that in step (b), the oxidation, particularly surface oxidation, is carried out using a mineral acid, particularly nitric acid (HNO3), as the oxidizing agent. In this regard, the oxidation of activated carbon, particularly surface oxidation, is preferably carried out at a temperature in the range of -20°C to 250°C, particularly in the range of 0°C to 200°C, preferably in the range of 5°C to 175°C, more preferably in the range of 10°C to 150°C, and particularly preferably in the range of 15°C to 125°C. Furthermore, the oxidation of activated carbon, particularly surface oxidation, is carried out over a period of up to 6 hours, particularly up to 5 hours, and preferably up to 4 hours. Similarly, the oxidation of activated carbon, particularly surface oxidation, is preferably carried out within a time range of 5 to 500 minutes, especially within a range of 10 to 400 minutes, and more preferably within a range of 20 to 300 minutes.
[0180] According to this embodiment of the present invention, the mineral acid, particularly nitric acid (HNO3), is present in an amount of 10% (vol.%) to 75%, particularly 15% to 60%, preferably 20% to 55%, more preferably about 25%, and more preferably about 50%.
[0181] Furthermore, according to the present invention, step (b) is provided to purify and / or dry the oxidized activated carbon, following oxidation, particularly surface oxidation, and particularly before step (c). In this case, purification is carried out by at least one washing method in a liquid, particularly in water. Furthermore, drying is carried out while heating the oxidized, particularly surface-oxidized, activated carbon to a temperature in the range of 40°C to 200°C, particularly 50°C to 150°C, preferably 60°C to 120°C. In particular, drying is preferably carried out under reduced pressure and / or in a vacuum, and / or, in particular, drying is preferably carried out at an (air) pressure in the range of 0.01 Pa to 100 Pa, particularly 0.1 Pa to 10 Pa.
[0182] The following describes in more detail step (c) of the method using an apparatus with previously oxidized activated carbon having a catalytically active component or related precursor: Generally, in step (c), the apparatus for the activated carbon oxidized in step (b), particularly the oxidized surface or catalyst support, is carried out by coating and / or contacting the catalyst active component onto the catalyst support, and preferably fixing it.
[0183] Generally, the catalytically active component preferably comprises or consists of at least one metal, particularly in the form of a metal compound, preferably in the form of an ionic metal compound, and / or particularly in the form of an element.
[0184] Generally, catalytically active components may include at least one metal in a positive oxidation state, particularly at least one metal cation, where the oxidation state of the metal is in the range of +I to +VII, particularly in the range of +I to +IV, preferably in the range of +I to +III, and especially preferably in the range of +1 or +II, and / or the catalytically active component includes at least one metal in an oxidation state of zero. For simple ions, the oxidation number corresponds to the charge number, whereas in the case of multinuclear ions, particularly so-called clusters, the oxidation number can deviate from the charge number, which is well known to those skilled in the art.
[0185] In particular, the catalytically active component may include at least one metal or at least one lanthanide selected from the main or subgroups of the periodic table of elements. Preferably, the catalytically active component includes at least one metal selected from the elements of main group IV or subgroups I, II, III, IV, V, VI, VII, and VIII of the periodic table, and especially from the elements of main group IV or subgroups I and II of the periodic table. The present invention provides that the catalytically active component comprises at least one metal selected from the group consisting of Cu, Ag, Au, Zn, Hg, Sn, Ce, Ti, Zr, V, Nb, Cr, Mo, W, Mn, Fe, Bi, Ru, Os, Co, Rh, Re, Ir, Ni, Pd, and Pt, particularly the group consisting of Fe, Bi, V, Cu, Pb, Zn, Ag, Sn, Pd, Pt, Ru, and Ni, preferably the group consisting of Fe, Bi, V, Cu, Pt, Ru, and Pb, more preferably the group consisting of Pd, Pt, and Ru, and particularly preferably the group consisting of Pd and Pt. The catalytically active component is used in step (c), particularly in the form of a precursor.
[0186] In particular, the present invention provides that a precursor of the catalytically active component is formed or configured such that the precursor is converted into the catalytically active component by the reduction performed in step (d) of the method. In particular, the precursor of the catalytically active component may be an oxidized form of the catalytically active component, or may be formed therefrom.
[0187] Generally, the precursor of the catalytically active component may include at least one metal compound, preferably based on at least one of the previously defined metals, which is particularly soluble and / or dissociable in aqueous and / or particularly aqueous-based solvents and / or dispersion media.
[0188] Furthermore, the precursor of the catalytically active component may include at least one inorganic or organometallic compound, preferably at least one previously defined metal, in particular a metal salt or metal oxide, preferably based on a metal salt.
[0189] In particular, the precursor of the catalytically active component may include at least one organic or inorganic metal salt, preferably at least one based on the previously defined metal, and the salt is preferably selected from the group consisting of halide salts, hydroxides, amines, sulfates, sulfites, nitrates, phosphates, phosphides, carbamates, alkoxides, and carboxylates, in particular halide salts, nitrates, hydroxides, and carboxylates.
[0190] Furthermore, the precursor of the catalytically active component preferably comprises at least one metal halide based on at least one of the metals defined above, particularly fluorides, chlorides, bromides or iodides, preferably chlorides, and / or preferably at least one carboxylate, particularly acetate, of a metal based on at least one previously defined metal.
[0191] Generally, the precursor of the catalytically active component preferably contains at least one metal compound selected from the group consisting of palladium chloride, palladium nitrate, hexachloroplatinic acid, platinum nitrate, tetraaminoplatinum dihydrate, ruthenium chloride, copper chloride, iron chloride, vanadium chloride, and lead chloride, and particularly from the group consisting of palladium chloride, palladium nitrate, hexachloroplatinic acid, platinum nitrate, and tetraaminoplatinum dihydrate.
[0192] In particular, the precursor preferably comprises or consists of palladium chloride, palladium nitrate, hexachloroplatinic acid, platinum nitrate, and / or tetraamineplatinum dihydrate.
[0193] According to the present invention, H2PdCl4 and / or Pd(NO3)2 are used as precursors (palladium precursors). According to the present invention, H2(PtCl6), (NH3)4Pt(OH)2 and / or Pt(NO3)2 are similarly preferred to be used as precursors (platinum precursors).
[0194] In particular, catalyst-active component precursors are used, especially in the form of aqueous and / or particularly aqueous-based solutions and / or dispersions (dispersions), for the purpose of finishing and / or loading and / or coating and / or impregnating oxidized, particularly surface-oxidized, activated carbon.
[0195] In this regard, the solution or dispersion (dispersion) may contain water as a solvent or dispersion medium. Furthermore, the solution or dispersion (dispersion) may contain at least one organic or inorganic acid or base, preferably hydrochloric acid.
[0196] Furthermore, the precursor of the catalytically active component may exist in solution or dispersion form (dispersion) in a state that is at least substantially free of crystals and / or crystallites. In particular, the precursor of the catalytically active component in solution or dispersion form (dispersion) may be at least substantially dissolved, and in particular may be at least substantially dissociated.
[0197] Generally, the solution and / or dispersion form (dispersion) may contain a precursor of a catalytically active component calculated as a metal in an amount ranging from 0.01% to 80% by weight, particularly 0.1% to 60% by weight, preferably 1% to 50% by weight, and more preferably 2% to 40% by weight, based on the solution and / or dispersion form (dispersion).
[0198] The terms “solution” or “dispersion form” as used in relation to the present invention are understood, in particular, to mean that the precursor of the catalytically active component is present in the underlying solvent or dispersion medium at least substantially completely dissolved, dissociated, or dispersed in the underlying amount or concentration. For example, within the scope of the present invention, for the purpose of equipping or loading the activated carbon with a catalytically active component, the activated carbon used according to the present invention is provided to be immersed or submerged in the corresponding solution or dispersion of the catalytically active component (precursor). In this way, according to the present invention, in particular, it is ensured that the underlying solution or dispersion form fills at least substantially the entire pore system of the activated carbon, thereby resulting in homogeneous filling of the activated carbon with the catalytically active component.
[0199] Generally, according to the present invention, in step (c), the apparatus for oxidized, particularly surface-oxidized, activated carbon having a catalytically active component, particularly a precursor of a catalytically active component, comprises application and / or contact, preferably fixation, of the oxidized, particularly surface-oxidized activated carbon having a catalytically active component, particularly a precursor of a catalytically active component. In particular, application and / or contact, preferably fixation, is carried out by immersion and / or impregnation, wetting, covering, coating and / or spraying the oxidized, particularly surface-oxidized activated carbon with the catalytically active component, particularly a precursor of a catalytically active component. Thus, application and / or contact is carried out by energy input, particularly vibration and / or ultrasonic input. In this regard, the catalytically active component, particularly a precursor of a catalytically active component, is used in the form of a solution and / or dispersion (dispersion), as previously described.
[0200] In particular, for the purpose of equipping activated carbon that has been oxidized, particularly surface-oxidized, with a catalytically active component, particularly a precursor of a catalytically active component, or in the form of a solution and / or dispersion of the catalytically active component (dispersion), preferably in the form of a solution and / or dispersion of the precursor of a catalytically active component (dispersion), after coating and / or contact, it is provided that an excess amount of the catalytically active component, particularly an excess amount of the precursor of a catalytically active component, or in the form of a solution and / or dispersion of the catalytically active component (dispersion), is removed and / or separated from the activated carbon or catalyst system, particularly from the catalyst system.
[0201] In this regard, after coating or contact, the activated carbon obtained is purified and / or dried, particularly for the purpose of finishing the oxidized, particularly surface-oxidized, activated carbon with catalytic active components, particularly precursors of catalytic active components. In this regard, the purification and / or drying is carried out by at least one washing step in a liquid, particularly water. Furthermore, the purification and / or drying can be carried out by heating the activated carbon with catalytic components to a temperature in the range of 40°C to 200°C, particularly 50°C to 150°C, preferably 60°C to 120°C. Furthermore, the purification and / or drying can be carried out under reduced (air) pressure and / or vacuum. Furthermore, the purification and / or drying is carried out under (air) pressure in the range of 100 Pa to 0.01 Pa, particularly 10 Pa to 0.1 Pa. The removal of solvents and dispersion media and the drying of the activated carbon result in the drying or particulate formation of precursors of catalytic active components, which are present in crystalline form on or on the surface of the activated carbon used particularly as a catalyst support.
[0202] Generally, the method according to the present invention provides that in step (c), both the outer and inner surfaces of the oxidized activated carbon, particularly the micropore, mesopore and / or macropore surface oxidized carbon, are equipped with, particularly supported and / or coated and / or impregnated with, a catalytically active component, especially in the form of a corresponding precursor. This makes it possible to achieve a high load of the catalytically active component.
[0203] In the following, step (d) describes in more detail the reduction of oxidized, particularly surface-oxidized, activated carbon obtained in step (c) and equipped with the catalytically active component, and especially the precursor of the catalytically active component:
[0204] The oxidized, particularly surface-oxidized, activated carbon obtained in step (c) containing the catalytically active component, in particular the precursor of the catalytically active component, leads to the reduction of at least a portion of the catalytically active component or its associated precursor, particularly incorporated into or applied to the activated carbon, as far as the reduction carried out in step (d) according to the present invention, although this is not intended to be limited to this theory. In particular, the catalytically active component or its associated precursor or the underlying metal compound or underlying metal can be reduced in this manner, particularly when the catalytically active component or its associated precursor exists in an oxidized form, or in the form of a salt, ion, etc. Therefore, the reduction treatment can also generally be carried out against the background of catalyst activation and / or conversion of the catalyst or catalytically active component or its associated precursor to an active form, particularly a change and / or decrease in the oxidation number of the metal of the catalytically active component. Therefore, the reduction treatment can, in particular, be carried out against the background of activation of the catalytically active component or its associated precursor.
[0205] The reduction treatment in step (d) is carried out such that, with respect to metals, particularly noble metals, of catalytically active components or related precursors that are not used in a zero-oxidation state or are not present in compound form, particularly in salt form, in step (c) the activated carbon is equipped with the catalytically active component or related precursor, and the corresponding conversion of the metal or noble metal to its elemental form or to a zero-oxidation state is carried out in compound form, particularly in salt form, thereby achieving or carrying out the activation of the catalyst or conversion to a catalytically active form.
[0206] Furthermore, the reduction treatment by step (d), although not intended to be limited to this theory, results in the removal or reduction (surface reduction) of at least some of the functional groups, particularly oxygen-containing functional groups, on the surface of the activated carbon or the related pore system of the activated carbon. In step (d), surface reduction of oxidized activated carbon with a catalytic active component or related precursor can be carried out in this manner. In this way, the catalyst support or the activated carbon in question, and consequently the catalyst system, can be neutralized or neutralized.
[0207] The catalyst system according to the present invention, or activated carbon in this respect, processed in this manner, also exhibits a reduction in self-reaction, particularly as a result of the decrease in the content of functional groups on the surface accompanying the reduction treatment, which is beneficial to the catalytic properties as a whole.
[0208] Similarly, although we do not wish to be limited to this theory, based on the reduction treatment performed, the hydrophilicity of the activated carbon, and therefore the entire catalyst system, is reduced, or the content of polar groups is reduced, thereby improving the overall permeation or diffusion behavior of hydrophobic or nonpolar reactants or products resulting from the catalytic reaction.
[0209] Generally, in step (d), reduction can be carried out as gas-phase reduction or liquid-phase reduction.
[0210] In particular, it is preferable that, in step (d) of the method, the reduction is carried out at a temperature in the range of 20°C to 400°C, particularly in the range of 50°C to 300°C, preferably in the range of 100°C to 250°C, more preferably in the range of 110°C to 200°C, particularly preferably in the range of 115°C to 160°C, most preferably in the range of 120°C to 150°C, and even more preferably in the range of 130°C to 145°C. Furthermore, in step (d) of the method, the reduction is generally carried out at a temperature in the range of 0°C to 750°C, particularly in the range of 10°C to 600°C.
[0211] According to the present invention, in step (d), the reduction is carried out for a period of time ranging from 0.05 hours to 48 hours, particularly ranging from 0.1 hours to 36 hours, preferably ranging from 0.5 hours to 24 hours, and more preferably ranging from 1 hour to 12 hours.
[0212] Next, the reduction treatment using a gaseous reducing agent will be described in detail below, and this embodiment is preferred according to the present invention. In this regard, the present invention may provide that in step (d) the reduction of the catalytic system is carried out using at least one gaseous reducing agent, particularly a gaseous reducing agent, preferably hydrogen. In this regard, in step (d) of the method, the reduction is carried out in an atmosphere containing a reducing agent, particularly hydrogen, in particular an inert atmosphere, preferably a nitrogen atmosphere. In this regard, the atmosphere contains a reducing agent, particularly hydrogen, in an amount ranging from 0.1% to 20% by volume, particularly from 0.5% to 10% by volume, preferably from 2% to 8% by volume, based on the volume of the atmosphere. Furthermore, in step (d) of the method, the reduction is carried out at a temperature in the range of 50°C to 300°C, particularly in the range of 100°C to 250°C, preferably in the range of 110°C to 200°C, more preferably in the range of 115°C to 160°C, even more preferably in the range of 120°C to 150°C, and most preferably in the range of 130°C to 145°C. Furthermore, in step (d), the reduction is carried out at a volumetric flow rate of an atmosphere containing a reducing agent in the range of 5 L / h to 1,000 L / h, particularly in the range of 10 L / h to 500 L / h, preferably in the range of 50 L to 300 L / h. In relation to the present invention, it is preferable to provide that in step (d) of the method, the reduction is carried out using a gaseous reducing agent for a period of time in the range of 0.1 hours to 36 hours, particularly in the range of 0.2 hours to 24 hours, preferably in the range of 0.5 hours to 12 hours.
[0213] A reduction treatment using a liquid reducing agent, according to another embodiment of the present invention, will be described further below: Accordingly, according to the present invention, in step (d), the reduction of the catalytic system is carried out using at least one liquid reducing agent, particularly a liquid alkaline reducing agent, which is preferably based on at least one alkali metal hydroxide, preferably potassium hydroxide, and especially based on a combination of at least one alkali metal formate, preferably potassium formate. In this regard, in step (d) of the method, the reduction is carried out using a liquid reducing agent at a temperature in the range of 10°C to 250°C, particularly in the range of 20°C to 200°C, preferably in the range of 30°C to 150°C, preferably in the range of 40°C to 125°C, and particularly preferably in the range of 50°C to 120°C. In this regard, in step (d) of the method, the reduction is carried out for a period of time ranging from 0.05 hours to 24 hours, particularly ranging from 0.1 hours to 12 hours, preferably ranging from 0.5 hours to 8 hours.
[0214] With respect to the present invention, the reduction carried out in step (d) may therefore be carried out using at least one gaseous and / or liquid reducing agent. In addition to the reducing agents mentioned above, formalin, hydrazine, and complex hydrides such as LiAlH4 and / or NaBH4 and / or formic acid can also be considered as reducing agents in principle.
[0215] Overall, in the implementation of method step (d), or after the implementation, and especially in a second aspect of the present invention, such catalyst systems are obtained as described or defined below, so the description therein will apply as appropriate to this aspect.
[0216] Overall, in step (d) of the method, a catalyst system according to the present invention can be obtained, wherein the catalyst system has at least one catalytically active component applied to and / or immobilized on a catalyst support, the catalytically active component comprises and / or consists of at least one metal, the catalyst support is formed in the form of activated carbon and / or based on activated carbon, the catalyst support exists in the form of granular, preferably spherical, activated carbon, and the activated carbon (i.e., the activated carbon forming the catalyst support) (i) 0.8cm 3 / g~3.9cm 3The total pore volume is within the range of / g, particularly the total pore volume according to Gurvitch, and at least 50% of the total pore volume, particularly the total pore volume according to Gurvitch, is formed by pores having a diameter of at least 2 nm, particularly by pores having a diameter of 2 nm to 500 nm, preferably by mesopores and macropores, and (ii) is 1,000m 2 / g~3,000m 2 Specific BET surface area (S) within the range of / g BET ) has, however, the total pore volume (V total ), in particular the ratio of total pore volume to surface area (S) by Gulvitch BET The ratio (quotient: Q) that corresponds to the equation Q = V total / S BET The ratio (quotient; Q) is at least 0.5 × 10 -9 This is conditional on the condition being m.
[0217] With respect to the present invention, in step (d) of the method, in particular, a catalyst system can be obtained, wherein the catalyst system has at least one catalytically active component coated or fixed to a catalyst support, the catalytically active component having and / or comprising at least one metal, the catalyst support is formed in the form of activated carbon or based on activated carbon, and the catalyst support is in the form of granular, preferably spherical activated carbon.
[0218] According to the present invention, the catalyst system can have activity measured as the percentage of metal dispersion of the catalytically active component on the catalyst support, preferably measured by chemiadsorption using the (dynamic) flow method according to DIN66136-3:2007-01, in particular at least 15%, particularly at least 20%, preferably at least 25%, more preferably at least 28%, and / or in the range of 15% to 90%, particularly in the range of 20% to 80%, preferably in the range of 25% to 70%, most preferably in the range of 28% to 60%.
[0219] In particular, the catalyst system preferably has a maximum wavelength of 80 angstroms (8 nm), especially 70 angstroms (7 nm), preferably 60 angstroms (6 nm), more preferably 58 angstroms (5.8 nm), even more preferably 45 angstroms (4.5 nm), even more preferably 40 angstroms (4 nm), most preferably 38 angstroms (3.8 nm) and / or in the range of 5 angstroms (0.5 nm) to 80 angstroms (8 nm), especially 7 angstroms (0.7 nm) to 70 angstroms (7 nm) as measured by DIN66136. The average crystallite size (average crystallite size d) is preferably measured by DIN66136, within the range of m), preferably 10 angstroms (1 nm) to 60 angstroms (6 nm), more preferably 15 angstroms (1.5 nm) to 58 angstroms (5.8 nm), particularly preferably 17 angstroms (1.7 nm) to 45 angstroms (4.5 nm), particularly more preferably 18 angstroms (1.8 nm) to 40 angstroms (4 nm), and most preferably 20 angstroms (2 nm) to 38 angstroms (3.8 nm). Me A catalytically active component having ) is particularly a catalytically active component having a metal.
[0220] In this regard, it is generally provided by the present invention that the catalyst system obtained in step (d) has activity measured as the percentage of dispersion of the catalytically active components on the catalyst support, preferably measured as the percentage of dispersion of the metal of the catalytically active components, measured by chemical adsorption by (dynamic) flow method according to DIN66136:2007-01, in particular at least 15%, particularly at least 20%, preferably at least 25%, preferably at least 28%, and / or in the range of 15% to 90%, particularly in the range of 20% to 80%, preferably in the range of 25% to 70%, more preferably in the range of 28% to 60%.
[0221] Furthermore, in this regard, the catalyst system obtained in step (d) may have a maximum wavelength of 80 angstroms (8 nm), particularly 70 angstroms (7 nm), preferably 60 angstroms (6 nm), more preferably 58 angstroms (5.8 nm), most preferably 38 angstroms (3.8 nm), and / or in the range of 5 angstroms (0.5 nm) to 80 angstroms (8 nm), in the range of 7 angstroms (0.7 nm) to 70 angstroms (7 nm), preferably in the range of 10 angstroms (1 nm) to 60 angstroms (6 nm), more preferably It is also preferable within the scope of the present invention that the catalytically active component, particularly the metal of the catalytically active component, has an average crystallite size preferably determined according to DIN66136, in the range of 15 angstroms (1.5 nm) to 58 angstroms (5.8 nm), particularly preferably in the range of 17 angstroms (1.7 nm) to 45 angstroms (4.5 nm), even more preferably in the range of 18 angstroms (1.8 nm) to 40 angstroms (4 nm), and most preferably in the range of 20 angstroms (2 nm) to 38 angstroms (3.8 nm).
[0222] Therefore, according to the present invention, it is possible to obtain a catalyst system according to the present invention having the above-mentioned properties of the metal, a special percentage dispersion, and a specific crystallite size, which characterize the excellent catalytic properties of the catalyst system according to the present invention, particularly with respect to the defined percentage dispersion of the catalytically active component or the metal, as well as a large catalytically active surface due to the optimal equipment or occupancy of the pore system of the activated carbon having the catalytically active component.
[0223] The degree of dispersion of the catalytically active component or metal dispersion also describes the catalytic activity of the catalyst system or supported catalyst according to the present invention. Therefore, catalytic activity is characterized by the dispersion of the catalytically active component or the metal of the catalytically active component on the catalyst support material, given that a sufficient number of surface atoms of the catalytically active component contribute to or enable the catalytic conversion. According to the present invention, the term “degree of dispersion” (also referred to as “degree of dispersion D”) is used synonymously with the terms “metallic dispersion” or “metallic dispersion D”. Percentage dispersion is, in particular, based on the ratio of the atoms or molecules of the catalytically active component actually present on the surface to the theoretically possible size of atoms or molecules of the catalytically active component present on the surface. In other words, the percentage dispersion describes, in particular, the ratio of the number of atoms or molecules on the surface of the catalytically active component to the total number of atoms or molecules of the catalytically active component (which can be determined, for example, by chemisorption of the sample gas with atoms or molecules of the catalytically active component accessible to the sample gas) (i.e., with respect to the total number of atoms or molecules of the catalytically active component that are theoretically available or used or the total number of atoms or molecules of the catalytically active component present on the catalyst support). In particular, the measurement can be carried out by chemisorption. In particular, carbon monoxide (CO) can be used as the measurement gas. Thus, the dispersion or metallic dispersion can be measured, in particular, by chemisorption of carbon monoxide.
[0224] The degree of percentage dispersion (D) of catalytically active components, particularly metal catalytically active components, on the catalyst support or activated carbon can be calculated based on the following formula (I):
number
[0225] In particular, the average crystallite size (synonymously, average crystallite size d) Me ) can be calculated based on the following formula (II):
number
[0226] The following formula symbols apply to formulas (I) and (II) above: [Table 1]
[0227] As far as the average crystallite size of the present invention is concerned, this also characterizes the catalytic activity, particularly against the backdrop of improved accessibility of the catalytically active component to the reactants to be reacted. In particular, the average crystallite size of the present invention is optimized in terms of the ratio of the surface area to the corresponding volume of the catalytically active component that forms the crystallites, which also leads to improved catalytic activity.
[0228] In particular, according to the present invention, the average dispersion and the average crystallite size of one are linked with respect to the overall improved catalytic activity provided, and mutually reinforce each other beyond the sum of their individual effects. In this respect, there is a synergistic effect with respect to the improved catalytic activity of the catalyst system according to the present invention, particularly with respect to high conversion rates or improved space / time yields.
[0229] Based on the method according to the present invention, the amount or content of the catalytically active component can be specifically adjusted or controlled with respect to the catalyst system according to the present invention, so the catalytic activity of the catalyst system obtained according to the present invention can also be specifically predetermined from this viewpoint.
[0230] Accordingly, the present invention provides that the catalyst system obtained in step (d) contains the catalytically active component in an amount calculated as metal, particularly at least 0.05% by weight, especially at least 0.1% by weight, preferably at least 0.2% by weight, more preferably at least 0.5% by weight, particularly preferably at least 0.6% by weight, most preferably at least 1% by weight, and even more preferably at least 1.5% by weight, based on the total weight of the catalyst system. By setting a lower limit, a predetermined catalytic activity can be ensured.
[0231] Furthermore, according to the present invention, it is particularly provided that the catalyst system obtained in step (d) contains the catalytically active component in an amount calculated as a metal, up to 25% by weight, particularly up to 20% by weight, preferably up to 15% by weight, more preferably up to 10% by weight, particularly preferably up to 8% by weight, and very particularly preferably up to 7% by weight, based on the total weight of the catalyst system. The upper limit ensures good access to the catalytically active component in particular and avoids pore clogging in particular.
[0232] In this regard, it is particularly possible in the present invention that the catalyst system obtained in step (d) contains a catalytically active component in an amount calculated as metal, based on the total weight of the catalyst system, in the range of 0.05% to 25% by weight, particularly 0.1% to 25% by weight, preferably 0.2% to 20% by weight, more preferably 0.5% to 15% by weight, especially preferably 0.6% to 10% by weight, even more preferably 1% to 8% by weight, and most preferably 1.5% to 7% by weight.
[0233] Furthermore, the catalytically active components of the catalyst system obtained in step (d) of the present invention are preferably as follows:
[0234] In particular, the catalytically active components of the catalyst system obtained in step (d) comprise or consist of at least one metal, particularly in the form of a metal compound, preferably in the form of an ionic metal compound, and / or particularly in the form of an element.
[0235] In particular, the catalytically active component of the catalyst system obtained in step (d) preferably includes at least one metal in a positive oxidation state, and more preferably at least one metal cation. In this regard, the oxidation state of the metal is preferably in the range of +I to +VII, particularly in the range of +I to +IV, preferably in the range of +I to +III, or particularly preferably +I or +II. According to the present invention, it is also preferable that the catalytically active component includes at least one metal in an oxidation state of zero.
[0236] In particular, during the reduction process carried out in step (d), the catalytically active component or related metal used according to step (c) can be appropriately reduced so that the metal exists in an oxidation state of zero, especially in step (d). With respect to the present invention, it is particularly preferred that the catalytically active component of the catalyst system obtained in step 8d) (and therefore the final product obtained from this method) contains at least one metal in an oxidation state of zero.
[0237] In particular, the catalytically active components of the catalyst system obtained in step (d) may include at least one metal from the main or subgroup of the periodic table of elements, or at least one lanthanide.
[0238] Generally, the catalytically active components of the catalyst system obtained in step (d) preferably include at least one metal selected from the elements of main group IV or subgroups I, II, III, IV, V, VI, VII, and VIII of the periodic table, particularly from the elements of main group IV or subgroups I and II of the periodic table.
[0239] In particular, the catalytically active component of the catalyst system obtained in step (d) preferably contains at least one metal selected from the group consisting of Cu, Ag, Au, Zn, Hg, Sn, Ce, Ti, Zr, V, Nb, Cr, Mo, W, Mn, Fe, Bi, Ru, Os, Rh, Re, Ir, Ni, Pd, and Pt, especially the group consisting of Fe, Bi, V, Cu, Pb, Zn, Ag, Sn, Pd, Pt, Ru, and Ni, preferably the group consisting of Fe, Bi, V, Cu, Pt, Ru, and Pb, more preferably the group consisting of Pd, Pt, and Ru, and even more preferably the group consisting of Pd and Pt. This is because particularly high catalytic activity can be obtained with these metals for catalytic methods that form the basis of hydrogenation reactions and the like.
[0240] With respect to the activated carbon present in the catalyst system, it may be based on or derived from the following types of activated carbon, and the properties relating thereto will equally lead to improvements in the performance of the catalyst system according to the present invention (e.g., by improvements or formation of the apparatus with respect to the catalytic active component): Therefore, the (surface-)reduced) activated carbon (i.e., the activated carbon forming the catalyst support) of the catalyst system obtained in step (d) may be oxidized if oxidation of the activated carbon, particularly surface oxidation, was carried out using and / or in the presence of at least one oxidizing agent, especially on its surface, before the application and / or immobilization of the catalytically active components. In this regard, it is also possible to refer to the above description, in particular step (c). Similarly, within the scope of the present invention, it is preferable that, after the catalytically active component is provided, the activated carbon behaves in such a way that it is reduced, particularly at its surface, and in particular, the reduction of the activated carbon is carried out using and / or in the presence of at least one reducing agent. In particular, after the catalytically active component is provided and / or after the reduction is performed, the activated carbon behaves in such a way that it is reduced, and in particular, its surface is reduced. In particular, according to the present invention, during the reduction process, the precursor of the catalytically active component behaves in such a way that it is converted into an active form or into the catalytically active component, and in particular, the underlying metal component is converted into an elemental form. Furthermore, it is preferable that the activated carbon (i.e., the activated carbon that forms the catalyst support) is obtained by carbonizing the starting material based on an organic polymer, followed by activation, and then oxidation (where the oxidation is performed before the catalytically active component is provided), and then reduction (where the reduction is performed after the catalytically active component is provided). The above explanation can also be used as a reference in this regard. Similarly, the activated carbon (i.e., the activated carbon forming the catalyst support) may be activated carbon based on activated carbon obtained by carbonization and subsequent activation of an organic polymer-based starting material, and / or activated carbon based on polymer-based activated carbon, preferably in the form of spherical activated carbon (PBSAC or polymer-based spherical activated carbon). Furthermore, the activated carbon of the catalyst system obtained in step (d) (i.e., the activated carbon forming the catalyst support) may be activated carbon based on or derived from the starting materials described herein (see also claim 21). In particular, the activated carbon of the catalyst system obtained in step (d) may be returned to or based on activated carbon obtained according to the method for producing activated carbon described herein (see also claims 22-25) or according to the oxidation method described herein (see also claims 30-34) in step (b).
[0241] Furthermore, the catalytically active component of the catalyst system obtained according to the present invention can be based in particular on the precursor of the catalytically active component reduced in step (d).
[0242] In particular, with respect to the present invention, it is preferable that the catalyst system obtained in step (d) is a catalyst system that is reduced particularly on its surface (particularly including the oxidation of the catalyst support, and thus the associated activated carbon, and the associated catalytically active components or precursors).
[0243] Furthermore, for a further explanation of the catalyst system according to the present invention obtained in step (d), one can refer to the following description of a second aspect of the present invention comprising the catalyst system, the description relating thereto shall apply mutatis mutandis.
[0244] Turning to a first aspect of the present invention, the present invention also relates to a method for producing a catalyst system comprising at least one catalytically active component, in particular a supported catalyst, preferably a method for use in heterogeneous system catalysts, in particular by a method as defined herein, At least one catalytically active component is coated and / or immobilized on a catalyst support, wherein the catalytically active component comprises and / or consists of at least one metal. Herein, the method includes the following steps in the order (a) to (d) specified below. (a) Providing and / or manufacturing granular, preferably spherical, activated carbon (=initial activated carbon) to be used as a catalyst support, Activated carbon (so-called initial activated carbon) (i) 0.8cm 3 / g~3.9cm 3 Total pore volume (V) within the range of / g total ), in particular having a total pore volume according to Gurvitch, and at least 50% of the total pore volume of the activated carbon, in particular the total pore volume according to Gurvitch, being formed by pores having a pore diameter of at least 2 nm, in particular by pores having a pore diameter in the range of 2 nm to 500 nm, preferably by mesopores and macropores, (ii) Specific BET surface area (S) within the range of 1,000 m² / g to 3,000 m² / g BET ) having, however in particular equation Q=V total / S BET Total pore volume (V) total ) In particular, the specific BET surface area (S) of the total pore volume according to Gulvitch BET The ratio (quotient; Q) to ) is at least 0.5 × 10 -9 The condition is that it is m, and (iii) Having an average pore diameter in the range of 15 nm to 100 nm, particularly in the range of 16 nm to 90 nm, preferably in the range of 17 nm to 85 nm, more preferably in the range of 18 nm to 80 nm, particularly preferably in the range of 20 nm to 70 nm, most preferably in the range of 22 nm to 60 nm, and even more preferably in the range of 25 nm to 50 nm; after that, (b) Oxidation of the activated carbon prepared and / or manufactured in step (a) above, particularly surface oxidation, However, oxidized, especially surface-oxidized activated carbon, is provided that it has an oxygen content of at least 4% (atomic%) based on the total elemental composition of the oxidized activated carbon, particularly a surface oxygen content measured by X-ray photoelectron spectroscopy (XPS or ESCA), and / or, oxidized, especially surface-oxidized activated carbon, is provided that it has hydrophilicity as determined by its water vapor adsorption behavior, and that at least 30% of the maximum water vapor saturation load of the activated carbon reaches a partial pressure of 0.6 p / p0; after that, (c) Equip, in particular load and / or coat and / or impregnate the activated carbon oxidized in step (b) with a catalytic active component, in particular at least one precursor of a catalytic active component; after that, (d) Method: The oxidized, particularly surface-oxidized, activated carbon obtained in step (c) is reduced using a catalytic active component, particularly a precursor of a catalytic active component, to convert the precursor of a catalytic active component into a catalytic active component, particularly to obtain a catalytic system having at least one catalytic active component, particularly a supported catalyst.
[0245] In this regard, according to a first aspect of the present invention, the present invention also relates to a method for preparing a catalytic system comprising at least one catalytically active component, particularly a supported catalyst, for the use of a heterogeneous system catalyst, as defined above, preferably: In a catalyst, at least one catalytically active component is applied to and / or immobilized on a catalyst support, wherein the catalytically active component comprises and / or consists of at least one metal. Here, the method includes the following steps in the order (a) to (d) specified below: (a) Providing and / or manufacturing granular, preferably spherical, activated carbon (=initial activated carbon) to be used as a catalyst support, Activated carbon (so-called initial activated carbon) (i) 0.8cm 3 / g~3.9cm 3 Total pore volume (V) within the range of / g total ), in particular having a total pore volume according to Gurvitch, and at least 50% of the total pore volume of the activated carbon, in particular the total pore volume according to Gurvitch, being formed by pores having a pore diameter of at least 2 nm, in particular by pores having a pore diameter in the range of 2 nm to 500 nm, preferably by mesopores and macropores, (ii) Specific BET surface area (S) within the range of 1,000 m² / g to 3,000 m² / g BET ) having, however in particular equation Q=V total / SBET Total pore volume (V) total ) In particular, the specific BET surface area (S) of the total pore volume according to Gulvitch BET The ratio (quotient; Q) to ) is at least 0.5 × 10 -9 The condition is that it is m, and (iii) Having an average pore diameter in the range of 15 nm to 100 nm, particularly in the range of 16 nm to 90 nm, preferably in the range of 17 nm to 85 nm, more preferably in the range of 18 nm to 80 nm, particularly preferably in the range of 20 nm to 70 nm, most preferably in the range of 22 nm to 60 nm, and even more preferably in the range of 25 nm to 50 nm; and (iv) Having a particle size, particularly particle size, in the range of 60 μm to 1,000 μm, particularly in the range of 70 μm to 800 μm, preferably in the range of 80 μm to 600 μm; and / or having an average particle size (D50), particularly average particle diameter (D50), in the range of 60 μm to 900 μm, particularly in the range of 75 μm to 750 μm, preferably in the range of 85 μm to 550 μm, more preferably in the range of 110 μm to 375 μm, particularly preferably in the range of 175 μm to 350 μm, and very preferably in the range of 185 μm to 225 μm; after that, (b) Oxidation, particularly surface oxidation, of the activated carbon prepared and / or manufactured in step (a) of the method, provided that the oxidized, particularly surface-oxidized, activated carbon has an oxygen content of at least 4% (atomic%) based on the total elemental composition of the oxidized activated carbon, particularly a surface oxygen content measured by X-ray photoelectron spectroscopy (XPS or ESCA), and / or, provided that the oxidized, particularly surface-oxidized, activated carbon has hydrophilicity determined as water vapor adsorption behavior, and that at least 30% of the maximum water vapor saturation load of the activated carbon reaches a partial pressure of 0.6 p / p0; after that, (c) Equip, in particular load and / or coat and / or impregnate the activated carbon oxidized in step (b) with a catalytic active component, in particular at least one precursor of a catalytic active component; after that, (d) Method: The oxidized, particularly surface-oxidized, activated carbon obtained in step (c) is reduced using a catalytic active component, particularly a precursor of a catalytic active component, to convert the precursor of a catalytic active component into a catalytic active component, particularly to obtain a catalytic system having at least one catalytic active component, particularly a supported catalyst.
[0246] More specifically, according to a first aspect of the present invention, the present invention also relates to a method for preparing a catalytic system comprising at least one catalytically active component, in particular a supported catalyst, preferably for use in heterogeneous system catalysts, in particular by a method as defined herein, At least one catalytically active component is applied to and / or immobilized on a catalyst support, and the catalytically active component comprises and / or consists of at least one metal. The method described above comprises the following steps in the order specified below (a) to (d): (a) The activated carbon (so-called initial activated carbon) (i) 0.8cm 3 / g~3.9cm 3 Total pore volume (V) within the range of / g total ), in particular having a total pore volume according to Gurvitch, and at least 50% of the total pore volume of the activated carbon, in particular the total pore volume according to Gurvitch, being formed by pores having a pore diameter of at least 2 nm, in particular by pores having a pore diameter in the range of 2 nm to 500 nm, preferably by mesopores and macropores, (ii) Specific BET surface area (S) within the range of 1,000 m² / g to 3,000 m² / g BET ) having, however in particular equation Q=V total / S BET Total pore volume (V) total) In particular, the specific BET surface area (S) of the total pore volume according to Gulvitch BET The ratio (quotient; Q) to ) is at least 0.5 × 10 -9 The condition is that it is m, and (iii) Having an average pore diameter in the range of 15 nm to 100 nm, particularly in the range of 16 nm to 90 nm, preferably in the range of 17 nm to 85 nm, more preferably in the range of 18 nm to 80 nm, particularly preferably in the range of 20 nm to 70 nm, most preferably in the range of 22 nm to 60 nm, and even more preferably in the range of 25 nm to 50 nm; (iv) Having a particle size, particularly particle size, in the range of 60 μm to 1,000 μm, particularly in the range of 70 μm to 800 μm, preferably in the range of 80 μm to 600 μm; and / or having an average particle size (D50), particularly average particle diameter (D50), in the range of 60 μm to 900 μm, particularly in the range of 75 μm to 750 μm, preferably in the range of 85 μm to 550 μm, more preferably in the range of 110 μm to 375 μm, particularly preferably in the range of 175 μm to 350 μm, and very preferably in the range of 185 μm to 225 μm; (v) Optionally, having a ballpan hardness of at least 90%, particularly at least 95%, preferably at least 97%, preferably at least 98%, particularly preferably at least 99%, very particularly preferably at least 99.5%, and even more preferably at least 99.8%. (vi) Optionally, having a vibration density or tamping density in the range of 100 g / L to 1,500 g / L, particularly in the range of 125 g / L to 1,000 g / L, preferably in the range of 150 g / L to 800 g / L, more preferably in the range of 200 g / L to 600 g / L, particularly preferably in the range of 225 g / L to 500 g / L, most preferably in the range of 250 g / L to 400 g / L, even more preferably in the range of 255 g / L to 395 g / L, and / or having a bulk density in the range of 150 g / L to 1,000 g / L, particularly in the range of 250 g / L to 700 g / L, preferably in the range of 300 g / L to 600 g / L, more preferably in the range of 300 g / L to 550 g / L. (vii) Optionally, having butane adsorption capacity in the range of 35% to 90%, particularly in the range of 40% to 85%, preferably in the range of 45% to 80%, more preferably in the range of 47.5% to 75%. (viii) Optionally, having an iodine value within the range of 1,250 mg / g to 2,100 mg / g, particularly within the range of 1,300 mg / g to 2,000 mg / g, 1,400 mg / g to 1,900 mg / g, or 1,425 mg / g to 1,850 mg / g. (ix) The methylene blue value is optionally in the range of 17 mL to 65 mL, particularly in the range of 18 mL to 55 mL, preferably in the range of 19 mL to 50 mL, more preferably in the range of 19.5 mL to 47.5 mL. (x) The number of molasses is optionally in the range of 255 to 1,500, particularly in the range of 310 to 1,400, preferably in the range of 375 to 1,300, and more preferably in the range of 510 to 1,250. (xi) Optional, 250cm 3 / g~850cm 3 Within the range of / g, especially 300cm 3 / g~700cm 3 Within the range of / g, preferably 350cm 3 / g~650cm 3 Within the range of / g, more preferably 375cm 3 / g~625cm 3 Gravimetric absorption amount of N2 V measured at a partial pressure p / p0 of 0.25 within the range of / g ads(wt.)Having (xii) Optionally, 50cm 3 / cm 3 ~300cm 3 / cm 3 Within the range, especially 80cm 3 / cm 3 ~275cm 3 / cm 3 Within the range, preferably 90 cm 3 / cm 3 ~250cm 3 / cm 3 Within the range, more preferably 95 cm 3 / cm 3 ~225cm 3 / cm 3 Volume-based adsorbed N2 amount V measured at a partial pressure p / p0 of 0.25 within the range ads(vol.) Having (xiii) Optionally, 300cm 3 / g~2,300cm 3 Within the range of / g, especially 400cm 3 / g~2,200cm 3 Within the range of / g, preferably 450cm 3 / g~2,100cm 3 Within the range of / g, more preferably 475cm 3 / g~2,100cm 3 Gravimetric N2 absorption amount V measured at a partial pressure p / p0 of 0.995 within the range of / g ads(wt.) Having (xiv) Optional, 200cm 3 / cm 3 ~500cm 3 / cm 3 Within the range, especially 250cm 3 / cm 3 ~400cm 3 / cm 3 Within the range, preferably 275 cm 3 / cm 3 ~380cm 3 / cm 3 Within the range, more preferably 295 cm 3 / cm 3 ~375cm 3 / cm 3Volume-based adsorbed N2 amount V measured at a partial pressure p / p0 of 0.995 within the range ads(vol.) Having, (xv) Optionally, the activated carbon has a fractal dimension of porosity in the range of 2.6 to 2.99, particularly in the range of 2.7 to 2.95, preferably in the range of 2.8 to 2.95, and / or the activated carbon has a fractal dimension of porosity of at least 2.7, particularly at least 2.8, preferably 2.85, more preferably at least 2.9. after that, (b) Oxidation, particularly surface oxidation, of the activated carbon prepared and / or manufactured in step (a) of the method, provided that the oxidized, particularly surface-oxidized, activated carbon has an oxygen content of at least 4% (atomic%) based on the total elemental composition of the oxidized activated carbon, particularly a surface oxygen content measured by X-ray photoelectron spectroscopy (XPS or ESCA), and / or, provided that the oxidized, particularly surface-oxidized, activated carbon has hydrophilicity determined as water vapor adsorption behavior, and that at least 30% of the maximum water vapor saturation load of the activated carbon reaches a partial pressure of 0.6 p / p0; after that, (c) Equip, in particular load and / or coat and / or impregnate the activated carbon oxidized in step (b) with a catalytic active component, in particular at least one precursor of a catalytic active component; after that, (d) Method: The oxidized, particularly surface-oxidized, activated carbon obtained in step (c) is reduced using a catalytic active component, particularly a precursor of a catalytic active component, to convert the precursor of a catalytic active component into a catalytic active component, particularly to obtain a catalytic system having at least one catalytic active component, particularly a supported catalyst.
[0247] Furthermore, according to a first aspect of the present invention, the present invention relates to a method for preparing a catalyst system further comprising at least one catalytically active component, particularly a supported catalyst, preferably for use in heterogeneous system catalysts, and more particularly to a method as defined herein, At least one catalytically active component is applied to and / or immobilized on a catalyst support, and the catalytically active component comprises and / or consists of at least one metal. The method described above comprises the following steps in the order specified below (a) to (d): (a) The activated carbon (so-called initial activated carbon) (i) 0.8cm 3 / g~3.9cm 3 Total pore volume (V) within the range of / g total ), in particular having a total pore volume according to Gurvitch, and at least 50% of the total pore volume of the activated carbon, in particular the total pore volume according to Gurvitch, being formed by pores having a pore diameter of at least 2 nm, in particular by pores having a pore diameter in the range of 2 nm to 500 nm, preferably by mesopores and macropores, (ii) Specific BET surface area (S) within the range of 1,000 m² / g to 3,000 m² / g BET ) having, however in particular equation Q=V total / S BET Total pore volume (V) total ) In particular, the specific BET surface area (S) of the total pore volume according to Gulvitch BET The ratio (quotient; Q) to ) is at least 0.5 × 10 -9 The condition is that it is m, and (iii) Having an average pore diameter in the range of 15 nm to 100 nm, particularly in the range of 16 nm to 90 nm, preferably in the range of 17 nm to 85 nm, more preferably in the range of 18 nm to 80 nm, particularly preferably in the range of 20 nm to 70 nm, most preferably in the range of 22 nm to 60 nm, and even more preferably in the range of 25 nm to 50 nm; (iv) Particle size, particularly particle size, within the range of 60 μm to 1,000 μm, particularly within the range of 70 μm to 800 μm, preferably within the range of 80 μm to 600 μm; and / or within the range of 60 μm to 900 μm, particularly within the range of 75 μm to Having an average particle size (D50), particularly an average particle diameter (D50), within the range of 750 μm, preferably within the range of 85 μm to 550 μm, more preferably within the range of 110 μm to 375 μm, especially preferably within the range of 175 μm to 350 μm, and very especially preferably within the range of 185 μm to 225 μm; (v) Having a ballpan hardness of at least 90%, particularly at least 95%, preferably at least 97%, preferably at least 98%, particularly preferably at least 99%, very particularly preferably at least 99.5%, and even more preferably at least 99.8%, (vi) Having a vibration density or tamping density in the range of 100 g / L to 1,500 g / L, particularly in the range of 125 g / L to 1,000 g / L, preferably in the range of 150 g / L to 800 g / L, more preferably in the range of 200 g / L to 600 g / L, particularly preferably in the range of 225 g / L to 500 g / L, most preferably in the range of 250 g / L to 400 g / L, even more preferably in the range of 255 g / L to 395 g / L, and / or having a bulk density in the range of 150 g / L to 1,000 g / L, particularly in the range of 250 g / L to 700 g / L, preferably in the range of 300 g / L to 600 g / L, more preferably in the range of 300 g / L to 550 g / L. (vii) Having butane adsorption capacity in the range of 35% to 90%, particularly in the range of 40% to 85%, preferably in the range of 45% to 80%, more preferably in the range of 47.5% to 75%. (viii) Having an iodine value within the range of 1,250 mg / g to 2,100 mg / g, particularly within the range of 1,300 mg / g to 2,000 mg / g, 1,400 mg / g to 1,900 mg / g, and 1,425 mg / g to 1,850 mg / g. (ix) Having a methylene blue value in the range of 17 mL to 65 mL, particularly in the range of 18 mL to 55 mL, preferably in the range of 19 mL to 50 mL, more preferably in the range of 19.5 mL to 47.5 mL. (x) Having a molasses count in the range of 255 to 1,500, particularly in the range of 310 to 1,400, preferably in the range of 375 to 1,300, more preferably in the range of 510 to 1,250. (xi) 250cm 3 / g~850cm 3 Within the range of / g, especially 300cm 3 / g~700cm 3 Within the range of / g, preferably 350cm 3 / g~650cm 3 Within the range of / g, more preferably 375cm 3 / g~625cm 3 Gravimetric absorption amount of N2 V measured at a partial pressure p / p0 of 0.25 within the range of / g ads(wt.) Having (xii) 50cm 3 / cm 3 ~300cm 3 / cm 3 Within the range, especially 80cm 3 / cm 3 ~275cm 3 / cm 3 Within the range, preferably 90 cm 3 / cm 3 ~250cm 3 / cm 3 Within the range, more preferably 95 cm 3 / cm 3 ~225cm 3 / cm 3 Volume-based adsorbed N2 amount V measured at a partial pressure p / p0 of 0.25 within the range ads(vol.) Having (xiii) 300cm 3 / g~2,300cm 3 Within the range of / g, especially 400cm 3 / g~2,200cm 3 Within the range of / g, preferably 450cm 3 / g~2,100cm 3 Within the range of / g, more preferably 475cm 3 / g~2,100cm 3 Gravimetric N2 absorption amount V measured at a partial pressure p / p0 of 0.995 within the range of / g ads(wt.) Having (xiv) 200cm 3 / cm 3 ~500cm 3 / cm 3 Within the range, especially 250cm 3 / cm 3 ~400cm 3 / cm 3 Within the range, preferably 275 cm 3 / cm 3 ~380cm 3 / cm 3 Within the range, more preferably 295 cm 3 / cm 3 ~375cm 3 / cm 3 Volume-based adsorbed N2 amount V measured at a partial pressure p / p0 of 0.995 within the range ads(vol.) Having, (xv) Having a fractal dimension of porosity in the range of 2.6 to 2.99, particularly in the range of 2.7 to 2.95, preferably in the range of 2.8 to 2.95, and / or having a fractal dimension of porosity of at least 2.7, particularly at least 2.8, preferably 2.85, more preferably at least 2.9. after that, (b) Oxidation, particularly surface oxidation, of the activated carbon prepared and / or manufactured in step (a) of the method, provided that the oxidized, particularly surface-oxidized, activated carbon has an oxygen content of at least 4% (atomic%) based on the total elemental composition of the oxidized activated carbon, particularly a surface oxygen content measured by X-ray photoelectron spectroscopy (XPS or ESCA), and / or, provided that the oxidized, particularly surface-oxidized, activated carbon has hydrophilicity determined as water vapor adsorption behavior, and that at least 30% of the maximum water vapor saturation load of the activated carbon reaches a partial pressure of 0.6 p / p0; after that, (c) Equip, in particular load and / or coat and / or impregnate the activated carbon oxidized in step (b) with a catalytic active component, in particular at least one precursor of a catalytic active component; after that, (d) Method: The oxidized, particularly surface-oxidized, activated carbon obtained in step (c) is reduced using a catalytic active component, particularly a precursor of a catalytic active component, to convert the precursor of a catalytic active component into a catalytic active component, particularly to obtain a catalytic system having at least one catalytic active component, particularly a supported catalyst.
[0248] Overall, the present invention provides an efficient method for producing a catalyst system according to the present invention having high catalytic performance, thereby providing a catalyst system that can be specifically tuned or tailored, particularly with respect to its catalytic activity, while simultaneously simplifying the method, and the catalyst system having high catalytic activity overall, as also indicated, particularly based on the average dispersion and average crystallite size of the catalytically active components.
[0249] The provision of a high-performance catalyst system according to the present invention is thereby ensured by a specific sequence and adjustment of each method step as defined above. In this regard, the use of special activated carbon as a catalyst support having a defined pore system or the execution of special oxidation is also very important, in particular with respect to providing a high load of catalytically active components and better access for reactants and products.
[0250] Therefore, the method and catalyst system obtained by the present invention have numerous advantages and special properties, as already shown above. Due to the excellent catalytic properties of the catalyst system obtained by the method, a wide range of applications or uses are possible, thereby ensuring reasonably high catalytic conversion and high space / time yields within the scope of use for catalytic applications.
[0251] With regard to the methods according to the present invention, in addition to the description of further embodiments of the invention, references as appropriate in this case are also possible.
[0252] A further object of the present invention, according to a second aspect of the present invention, is a catalyst system according to the present invention, in particular a catalyst system for use in a supported catalyst according to the present invention, preferably a heterogeneous system catalyst, wherein the catalyst system according to the present invention or a supported catalyst associated therewith is obtainable or can be obtained by following the methods according to the present invention described above.
[0253] Similarly, according to this aspect of the present invention, the present invention relates preferably to heterogeneous system catalysts, in particular to catalyst systems according to the present invention for use in the catalyst systems defined above, and especially to supported catalysts according to the present invention. The catalyst system comprises at least one catalytically active component applied to and / or immobilized on a catalyst carrier, the catalytically active component comprising and / or consisting of at least one metal, the catalyst carrier being in the form of activated carbon and / or based on activated carbon, and the catalyst carrier being in the form of granular, preferably spherical, activated carbon. The activated carbon (the activated carbon that forms the so-called catalyst support) (i) 0.8cm 3 / g~3.9cm 3 Total pore volume (V) within the range of / g total ), in particular having a total pore volume according to Gurvitch, and at least 50% of the total pore volume, in particular the total pore volume according to Gurvitch, being formed by pores having a diameter of at least 2 nm, in particular pores having a diameter in the range of 2 nm to 500 nm, preferably mesopores and macropores, and (ii) 1,000m 2 / g~3,000m 2 Specific BET surface area (S) within the range of / g BET ) having, however, total pore volume (V total ), in particular the ratio of total pore volume to surface area (S) by Gulvitch BET The ratio (quotient: Q) to ) in particular, the equation Q = V total / S BET The ratio shown is at least 0.5 × 10 -9 The condition is that m is the value.
[0254] In this regard, the invention according to the second aspect relates to a catalyst system, preferably for use in heterogeneous system catalysts, more particularly to a supported catalyst, and more particularly to a catalyst system as defined above. Here, the catalyst system has at least one catalytically active component coated and / or immobilized on a catalyst carrier, wherein the catalytically active component comprises and / or consists of at least one metal, and the catalyst carrier is in the form of activated carbon and / or based on activated carbon, wherein the catalyst carrier is in the form of granular, preferably spherical, activated carbon. The activated carbon (i.e., the activated carbon that forms the catalyst support) (i) 0.8cm 3 / g~3.9cm 3 Total pore volume (V) within the range of / g total ), in particular having a total pore volume according to Gurvitch, wherein at least 50% of the total pore volume, in particular the total pore volume according to Gurvitch, is formed by pores having a diameter of at least 2 nm, particularly in the range of 2 nm to 500 nm, preferably mesopores and macropores. (ii) 1,000m 2 / g~3,000m 2 Specific BET surface area (S) within the range of / g BET ) has the following characteristics, however in particular, equation Q = V total / S BET According to this, the specific BET surface area (S BET Total pore volume (V) total ), in particular, the ratio of total pore volume by Gulvitch (quotient; Q) is at least 0.5 × 10 -9 It is conditional on m being the case; and The catalyst system has activity measured as a percentage of the dispersion of catalytically active components on a catalyst support, particularly metal dispersion of catalytically active components, measured by chemical adsorption by (dynamic) flow method according to DIN66136-3:2007-01, in the range of 15% to 90%, particularly 20% to 80%, preferably 25% to 70%, more preferably 28% to 60%, and / or the catalyst system has activity measured as a percentage of the dispersion of catalytically active components of metal on a catalyst support, in the range of 15% to 90%, particularly 20% to 80%, preferably 25% to 70%, more preferably 28% to 60%, and / or the catalyst system has activity measured as a percentage of the dispersion of metal on a catalyst support, particularly metal dispersion of catalytically active components, in the range of 80 angstroms (8 nm), particularly 70 angstroms (7 nm), preferably 60 angstroms (6 nm), more preferably 58 angstroms (5.8 nm), even more preferably 45 angstroms (4.5 nm), particularly preferably 40 angstroms (4 nm). The catalytic active component has an average crystallite size, most preferably 38 angstroms (3.8 nm), and / or in the range of 5 angstroms (0.5 nm) to 80 angstroms (80 nm), particularly in the range of 7 angstroms (0.7 nm) to 70 angstroms (7 nm), preferably in the range of 10 angstroms (1 nm) to 60 angstroms (6 nm), more preferably in the range of 15 angstroms (1.5 nm) to 58 angstroms (5.8 nm), particularly preferably in the range of 17 angstroms (1.7 nm) to 45 angstroms (4.5 nm), even more preferably in the range of 18 angstroms (1.8 nm) to 40 angstroms (4 nm), and most preferably in the range of 20 angstroms (2 nm) to 38 angstroms (3.8 nm), preferably measured by DIN66136.
[0255] Similarly, according to this embodiment, the present invention also relates to catalyst systems, in particular to supported catalysts, preferably heterogeneous system catalysts, and more particularly to catalyst systems as defined above. The catalyst system comprises at least one catalytically active component applied to and / or immobilized on a catalyst support, wherein the catalytically active component comprises and / or consists of at least one metal, the catalyst support is in the form of activated carbon and / or based on activated carbon, and the catalyst support is in the form of granular, preferably spherical, activated carbon; and The catalyst system has activity measured as a percentage of the dispersion of catalytically active components on a catalyst support, preferably measured by chemical adsorption by (dynamic) flow method according to DIN66136-3:2007-01, in the range of at least 15%, particularly at least 20%, preferably at least 28%, and / or in the range of 15% to 90%, particularly in the range of 20% to 80%, preferably in the range of 25% to 70%, more preferably in the range of 28% to 60%, and / or the catalyst system has activity measured as a percentage of the dispersion of metals of catalytically active components on a catalyst support, preferably in the range of chemiadsorption by (dynamic) flow method according to DIN66136-3:2007-01, and / or the catalyst system has activity measured as a percentage of the dispersion of metals of catalytically active components on a catalyst support, in the range of at least 15%, particularly at least 20%, preferably at least 28%, and / or in the range of 15% to 90%, particularly in the range of 20% to 80%, preferably in the range of 25% to 70%, more preferably in the range of 28% to 60%, and / or the catalyst system has activity measured as a percentage of the dispersion of metals of catalytically active components on a catalyst support, in the range of at least 15%, particularly at least 20%, preferably at least 28%, and / or in the range of 15% to 90%, particularly in the range of 20% to 80%, more preferably in the range of 25% to 70%, more preferably in the range of 28% to 60%, and / or the catalyst system has activity measured as a percentage of the dispersion of metals of catalytically active components on a maximum of 80 angstroms (8 nm), particularly at least 70 angstroms (7 nm), most preferably The catalytic active component has an average crystallite size of 38 angstroms (3.8 nm), and / or in the range of 5 angstroms (0.5 nm) to 80 angstroms (80 nm), particularly in the range of 7 angstroms (0.7 nm) to 70 angstroms (7 nm), preferably in the range of 10 angstroms (1 nm) to 60 angstroms (6 nm), more preferably in the range of 15 angstroms (1.5 nm) to 58 angstroms (5.8 nm), particularly preferably in the range of 17 angstroms (1.7 nm) to 45 angstroms (4.5 nm), even more preferably in the range of 18 angstroms (1.8 nm) to 40 angstroms (4 nm), and most preferably in the range of 20 angstroms (2 nm) to 38 angstroms (3.8 nm), preferably measured by DIN66136.
[0256] Therefore, the catalyst system according to the present invention is characterized by a defined percentage dispersion and a defined average crystallite size of the underlying catalytically active component, so that excellent catalytic properties are obtained overall. Furthermore, by using a special activated carbon with a defined pore system as the catalyst support, the transport characteristics of reactants and products in the catalytic reaction are improved, resulting in a highly efficient catalyst system overall that achieves high conversion efficiency and high space / time yield as a heterogeneous system catalyst.
[0257] The present invention provides that the catalyst system according to the present invention has activity determined as the percentage dispersion of catalytically active components, particularly metals of catalytically active components, on a catalyst support, preferably measured by chemiadsorption by (dynamic) flow method, in the range of at least 15%, particularly at least 20%, preferably at least 25%, more preferably at least 28%, and / or in the range of 15% to 90%, particularly in the range of 20% to 80%, preferably in the range of 25% to 70%, preferably in the range of 28% to 60%, preferably according to DIN66136-3:2007-01.
[0258] Furthermore, according to the present invention, the catalyst system has a wavelength of up to 80 angstroms (8 nm), particularly up to 70 angstroms (7 nm), preferably up to 60 angstroms (6 nm), more preferably up to 58 angstroms (5.8 nm), particularly preferably up to 45 angstroms (4.5 nm), particularly more preferably up to 40 angstroms (4 nm), even more preferably up to 38 angstroms (3.8 nm), and / or in the range of 5 angstroms (0.5 nm) to 80 angstroms (8 nm), particularly in the range of 7 angstroms (0.7 nm) to 70 angstroms (7 nm), preferably 10 angstroms It is provided that the catalytic active component has an average crystallite size preferably determined according to DIN66136, in the range of 1 angstrom (1 nm) to 60 angstroms (6 nm), more preferably in the range of 15 angstroms (1.5 nm) to 58 angstroms (5.8 nm), particularly more preferably in the range of 17 angstroms (1.7 nm) to 45 angstroms (4.5 nm), particularly more preferably in the range of 18 angstroms (1.8 nm) to 40 angstroms (4 nm), and even more preferably in the range of 20 angstroms (2 nm) to 38 angstroms (3.8 nm), and particularly especially includes a metal of the catalytic active component.
[0259] Furthermore, since the catalyst system according to the present invention has a defined amount of catalytically active components, the catalytic activity can be specifically determined from this point of view as well. In particular, it is possible to ensure high overall catalytic activity while simultaneously providing good accessibility to the catalytically active components.
[0260] Therefore, according to the present invention, it is preferable that the catalyst system contains a catalytically active component in an amount calculated as a metal and based on the total weight of the catalyst system, in an amount of at least 0.05% by weight, particularly at least 0.1% by weight, preferably at least 0.2% by weight, more preferably at least 0.5% by weight, particularly more preferably at least 0.6% by weight, most preferably at least 1% by weight, and even more preferably at least 1.5% by weight.
[0261] In particular, the catalyst system preferably contains a catalytically active component in an amount of 25% by weight or less, especially 20% by weight or less, preferably 15% by weight or less, more preferably 10% by weight or less, even more preferably 8% by weight or less, and most preferably 7% by weight or less, calculated as metal and based on the total weight of the catalyst system.
[0262] Therefore, according to the present invention as a whole, it is preferable that the catalyst system contains catalytically active components in a range of 0.05% to 25% by weight, particularly 0.1% to 25% by weight, preferably 0.2% to 20% by weight, more preferably 0.5% to 15% by weight, particularly more preferably 0.6% to 10% by weight, most preferably 1% to 8% by weight, and even more preferably 1.5% to 7% by weight, calculated as metal and based on the total weight of the catalyst system.
[0263] Furthermore, with respect to the catalyst system according to the present invention, the catalytic active component preferably consists of or comprises at least one metal, particularly in the form of a metal compound, preferably in the form of an ionic metal compound, and / or particularly in the form of an element.
[0264] In particular, the catalytically active component preferably has at least one metal cation, and more preferably at least one metal cation, in which the oxidation state of the metal is in the range of +I to +VII, particularly in the range of +I to +IV, preferably in the range of +I to +III, and especially preferably in the range of +I or +II. According to the present invention, it is particularly preferable that the catalytically active component consists of at least one metal with an oxidation state of zero.
[0265] In particular, the catalytically active component preferably includes at least one metal from the main or subgroup of the periodic table of elements, or at least one lanthanide.
[0266] Furthermore, it is preferable according to the present invention that the catalytically active component includes at least one metal selected from the elements of main group IV or subgroups I, II, III, IV, V, VI, VII, and VIII of the periodic table, particularly from the elements of main group IV or subgroups I and II of the periodic table.
[0267] In this regard, according to the present invention, it is preferable that the catalytically active component contains at least one metal selected from the group consisting of Cu, Ag, Au, Zn, Hg, Sn, Ce, Ti, Zr, V, Nb, Cr, Mo, W, Mn, Fe, Bi, Ru, Os, Co, Rh, Re, Ir, Ni, Pd, and Pt, particularly Fe, Bi, V, Cu, Pb, Zn, Ag, Sn, Pd, Pt, Ru, and Ni, preferably Fe, Bi, V, Cu, Pt, Ru, and Pb, more preferably Pd, Pt, and Ru, and particularly preferably Pd and Pt. Particularly high catalytic activity is observed in components containing the aforementioned metals.
[0268] In the catalyst system according to the present invention, in particular, both the outer and inner surfaces of the activated carbon, especially both micropores, mesopores and / or macropores, behave in such a way that they contain catalytically active components.
[0269] As previously stated, it is particularly preferable with respect to the present invention that the catalyst system has activity measured as the percentage dispersion of the catalytically active components on the catalyst support, especially the metal of the catalytically active components, measured in the range of at least 15%, particularly at least 20%, preferably at least 25%, more preferably at least 28%, and / or in the range of 15% to 90%, particularly in the range of 20% to 80%, preferably in the range of 25% to 70%, more preferably in the range of 28% to 60%, preferably according to DIN66136-3:2007-01, particularly by chemiadsorption by (dynamic) flow method.
[0270] According to the present invention, the catalyst system has a wavelength of up to 80 angstroms (8 nm), particularly up to 70 angstroms (7 nm), preferably up to 60 angstroms (6 nm), more preferably up to 58 angstroms (5.8 nm), even more preferably up to 45 angstroms (4.5 nm), even more preferably 40 angstroms (4 nm), and / or in the range of 5 angstroms (0.5 nm) to 80 angstroms (8 nm), particularly in the range of 7 angstroms (0.7 nm) to 70 angstroms (7 nm), preferably 10 angstroms (1 nm) to 60 angstroms. The invention particularly provides a catalytically active component having an average crystallite size, preferably measured by DIN66136, in the range of angstroms (6 nm), more preferably in the range of 15 angstroms (1.5 nm) to 58 angstroms (5.8 nm), even more preferably in the range of 17 angstroms (1.7 nm) to 45 angstroms (4.5 nm), even more preferably in the range of 18 angstroms (1.8 nm) to 40 angstroms (4 nm), and most preferably in the range of 20 angstroms (2 nm) to 38 angstroms (3.8 nm).
[0271] The present invention provides that the activated carbon (i.e., the activated carbon forming the catalyst support) is based on activated carbon that has been oxidized, particularly surface-oxidized, before the application and / or immobilization of the catalytic active component, and reduced, particularly on its surface, after the application and / or immobilization of the catalytic active component. This allows for particularly good engagement with the catalytic active component, as previously shown, with respect to the catalyst system according to the present invention. In particular, such activated carbon contributes to improved properties of the product obtained in the form of the catalyst system according to the present invention, as good dispersion is achieved, as well as crystallite size. As similarly shown above, the reduction performed can also reduce the oxygen-containing functional group content and the hydrophilicity of the activated carbon, which is particularly advantageous with respect to the transport properties of reactants or products in the activated carbon system as a catalyst support.
[0272] Generally, the present invention further provides that the activated carbon (i.e., the activated carbon forming the catalyst support) is based on activated carbon obtained by carbonization and subsequent activation of an organic polymer-based starting material, and thereafter oxidation (treatment) is performed, which is performed before coating and / or fixing of the catalytic active component, and thereafter reduction (treatment) is performed, which is performed after coating and / or fixing of the catalytic active component.
[0273] In particular, the activated carbon (i.e., the activated carbon that forms the catalyst support) can be based on activated carbon obtained by carbonizing and subsequently activating an organic polymer-based starting material, or it may be in the form of polymer-based, preferably spherical activated carbon (PBSAC or polymer-based spherical activated carbon).
[0274] Such activated carbons possess properties that are particularly defined with respect to their pore systems. Furthermore, they exhibit high mechanical stability, such as high wear resistance.
[0275] Generally, activated carbon is activated carbon based on the starting materials described above (see Claim 21). In particular, activated carbon is activated carbon that is derived from or based on activated carbon obtained according to the manufacturing method described above (see Claims 22-25 and 30-34).
[0276] Furthermore, the catalyst system is preferably a surface reduction type catalyst system.
[0277] Further properties of the activated carbon forming the catalyst support in the catalyst system according to the present invention are shown below:
[0278] In particular, activated carbon can have a defined total pore volume: Therefore, the activated carbon (i.e., the activated carbon that forms the catalyst support) is 0.9 cm 3 / g~3.4cm 3 Within the range of / g, especially 1cm 3 / g~2.9cm 3 Within the range of / g, preferably 1.1cm3 / g~2.4cm 3 Within the range of / g, preferably 1.2cm 3 / g~1.9cm 3 Within the range of / g, more preferably 1.5cm 3 / g~1.9cm 3 Total pore volume (V) within the range of / g total ), in particular those having the total pore volume according to Gulvitch. Furthermore, in this regard, the activated carbon (i.e., the activated carbon forming the catalyst support) behaves such that 50% to 90%, particularly 52.5% to 87.5%, preferably 55% to 85%, more preferably 57.5% to 82.5%, and especially preferably 60% to 80% of the total pore volume of the activated carbon (i.e., the activated carbon forming the catalyst support), in particular 52.5% to 87.5%, preferably 55% to 85%, more preferably 57.5% to 82.5%, and especially preferably 60% to 80%, is formed by pores having a pore diameter of at least 2 nm, particularly pores having a pore diameter in the range of 2 nm to 500 nm, preferably by mesopores and macropores. Furthermore, the activated carbon (i.e., the activated carbon that forms the catalyst support) is 0.8 cm 3 / g~3.9cm 3 Within the range of / g, especially 0.9cm 3 / g~3.4cm 3 Within the range of / g, preferably 1cm 3 / g~2.9cm 3 Within the range of / g, more preferably 1.1cm 3 / g~2.4cm 3 Within the range of / g, particularly more preferably 1.2cm 3 / g~1.9cm 3 Within the range of / g, most preferably 1.5cm 3 / g~1.9cm 3 Total pore volume (V) within the range of / g total), in particular having a total pore volume according to Gurvitch, wherein 50% to 90%, particularly 52.5% to 87.5%, preferably 55% to 85%, more preferably 57.5% to 82.5%, and especially more preferably 60% to 80% of the total pore volume of the activated carbon according to Gurvitch is formed by pores having a pore diameter of at least 2 nm, particularly by pores having a pore diameter in the range of 2 nm to 500 nm, preferably by mesopores and macropores.
[0279] Furthermore, the activated carbon forming the catalyst support may also have the following properties: In particular, activated carbon (i.e., activated carbon that forms the catalyst support) is 1,100 m 2 / g~2,600m 2 Within the range of / g, especially 1,200m 2 / g~2,400m 2 Within the range of / g, preferably 1,300m 2 / g~2,200m 2 Within the range of / g, more preferably 1,350m 2 / g~1,950m 2 Within the range of / g, more preferably 1,375m 2 / g~1,900m 2 Specific BET surface area (S) within the range of / g BET It has the following characteristics: Furthermore, regarding activated carbon (i.e., activated carbon that forms the catalyst support), the total pore volume (V total ), in particular, the formula Q=V for the pore volume according to Gulvitch total / S BET Specific BET surface area (S BET The ratio (Q) to ) is 0.5 × 10 -9 m~1.9×10 -9 Within the range of m, especially 0.55 × 10 -9 m~1.9×10 -9 Within the range of m, preferably 0.6 × 10 -9 m~1.8×10 -9 Within the range of m, more preferably 0.65 × 10 -9 m~1.7×10 -9 Within the range of m, more preferably 0.65 × 10 -9m~1.6×10 -9 Within the range of m, particularly preferably 0.7 × 10 -9 m~1.5×10 -9 Within the range of m, particularly more preferably 0.75 × 10 -9 m~1.4×10 -9 Within the range of m, most preferably 0.8 × 10 -9 m~1.3×10 -9 It is within the range of m. Furthermore, the activated carbon (i.e., the activated carbon that forms the catalyst support) is 1,000 m 2 / g~3,000m 2 Within the range of / g, especially 1,100m 2 / g~2,600m 2 Within the range of / g, preferably 1,200m 2 / g~2,400m 2 Within the range of / g, more preferably 1,300m 2 / g~2,200m 2 Within the range of / g, more preferably 1,350m 2 / g~1,950m 2 Within the range of / g, particularly more preferably 1,375m 2 / g~1,900m 2 Specific BET surface area (S) within the range of / g BET ) has a total pore volume (V total ), in particular, the formula Q=V for the pore volume according to Gulvitch total / S BET Specific BET surface area (S BET The ratio (Q) to ) is 0.5 × 10 -9 m~1.9×10 -9 Within the range of m, especially 0.55 × 10 -9 m~1.9×10 -9 Within the range of m, preferably 0.6 × 10 -9 m~1.8×10 -9 Within the range of m, more preferably 0.65 × 10 -9 m~1.7×10 -9 Within the range of m, more preferably 0.65 × 10 -9 m~1.6×10 -9 Within the range of m, particularly preferably 0.7 × 10 -9 m~1.5×10 -9Within the range of m, particularly more preferably 0.75 × 10 -9 m~1.4×10 -9 Within the range of m, most preferably 0.8 × 10 -9 m~1.3×10 -9 It is within the range of m.
[0280] Furthermore, activated carbon used as a catalyst support can also have the following properties: Therefore, it is preferable that the activated carbon (i.e., the activated carbon forming the catalyst support) has an average pore size of at least 15 nm and / or a maximum average pore size of 100 nm. In this regard, it is preferable that the activated carbon (i.e., the activated carbon forming the catalyst support) has an average pore size in the range of 15 nm to 100 nm, particularly in the range of 16 nm to 90 nm, preferably in the range of 17 nm to 85 nm, more preferably in the range of 18 nm to 80 nm, particularly more preferably in the range of 20 nm to 70 nm, even more preferably in the range of 22 nm to 60 nm, and most preferably in the range of 25 nm to 50 nm. With regard to the present invention, the activated carbon (i.e., the activated carbon that forms the catalyst support) is preferably spherical. In particular, the activated carbon is preferably in the form of spherical activated carbon. Furthermore, it is preferable that the activated carbon (i.e., the activated carbon forming the catalyst support) has a particle size, particularly a particle diameter, within the range of 60 μm to 1,000 μm, particularly 70 μm to 800 μm, preferably 80 μm to 600 μm, more preferably 100 μm to 400 μm, particularly preferably 150 μm to 375 μm, and most preferably 175 μm to 250 μm. In particular, it is preferable that the activated carbon particles, particularly at least 80% by weight, particularly at least 90% by weight, and preferably at least 95% by weight, have a particle size, particularly a particle diameter, within the aforementioned range. In particular, the activated carbon (i.e., the activated carbon forming the catalyst support) preferably has an average particle size (D50) in the range of 60 μm to 900 μm, particularly in the range of 75 μm to 750 μm, preferably in the range of 85 μm to 550 μm, more preferably in the range of 110 μm to 375 μm, particularly preferably in the range of 175 μm to 350 μm, and most preferably in the range of 185 μm to 225 μm, and especially an average particle diameter (D50). Furthermore, it is preferable that the activated carbon (i.e., the activated carbon forming the catalyst support) has a ball-pan hardness and / or wear hardness of at least 90%, particularly at least 95%, preferably at least 97%, more preferably at least 98%, particularly preferably at least 99%, most preferably at least 99.5%, and even more preferably at least 99.8%. Furthermore, it is preferable that the activated carbon (i.e., the activated carbon forming the catalyst support) has a compressive strength and / or burst strength (weight load capacity) of at least 5 Newtons, particularly at least 10 Newtons, preferably at least 15 Newtons, preferably at least 20 Newtons, and especially preferably at least 22.5 Newtons per activated carbon grain, particularly per activated carbon sphere. In particular, activated carbon (i.e., activated carbon forming the catalyst support) may have a compressive and / or bursting strength (weight-bearing capacity) per activated carbon particle, especially per activated carbon sphere, in the range of 5 to 50 Newtons, particularly 10 to 50 Newtons, preferably 15 to 40 Newtons, and more preferably 17.5 to 35 Newtons. Similarly, the activated carbon (i.e., the activated carbon that forms the catalyst support) preferably has a distribution density or compaction density within the range of 100 g / L to 1,500 g / L, particularly 125 g / L to 1,000 g / L, preferably 150 g / L to 800 g / L, more preferably 200 g / L to 600 g / L, even more preferably 225 g / L to 500 g / L, particularly preferably 250 g / L to 400 g / L, and even more preferably 255 g / L to 395 g / L. Furthermore, the activated carbon (i.e., the activated carbon that forms the catalyst support) preferably has a bulk density in the range of 150 g / L to 1,000 g / L, particularly 250 g / L to 700 g / L, preferably 300 g / L to 600 g / L, and more preferably 300 g / L to 550 g / L.
[0281] Furthermore, the activated carbon forming the catalyst support can have the following properties: Therefore, the activated carbon (i.e., the activated carbon forming the catalyst support) can have at least 35%, particularly at least 40%, preferably at least 45%, preferably at least 47.5% butane adsorption, and / or it is preferable that the activated carbon has butane adsorption in the range of 35% to 90%, particularly in the range of 40% to 85%, preferably in the range of 45% to 80%, and more preferably in the range of 47.5% to 75%. Furthermore, the activated carbon (i.e., the activated carbon forming the catalyst support) preferably has an iodine value of at least 1,350 mg / g, particularly at least 1,300 mg / g, preferably at least 1,400 mg / g, preferably at least 1,425 mg / g, and / or the activated carbon preferably has an iodine value in the range of 1,250 mg / g to 2,100 mg / g, particularly in the range of 1,300 mg / g to 2,000 mg / g, preferably in the range of 1,400 mg / g to 1,900 mg / g, and more preferably in the range of 1,425 mg / g to 1,850 mg / g. Furthermore, the activated carbon (i.e., the activated carbon forming the catalyst support) preferably has a methylene blue value of at least 17 mL, particularly at least 18 mL, preferably at least 19 mL, preferably at least 19.5 mL, and / or the activated carbon preferably has a methylene blue value in the range of 17 mL to 65 mL, particularly in the range of 18 mL to 55 mL, preferably in the range of 19 mL to 50 mL, more preferably in the range of 19.5 mL to 47.5 mL. Furthermore, the activated carbon (i.e., the activated carbon forming the catalyst support) preferably has a molasses count of at least 255, particularly at least 310, preferably at least 375, preferably at least 510, and / or the activated carbon preferably has a molasses count in the range of 255 to 1,500, particularly in the range of 310 to 1,400, preferably in the range of 375 to 1,300, more preferably in the range of 510 to 1,250. Furthermore, it is preferable that the activated carbon (i.e., the activated carbon forming the catalyst support) has a methylene blue value of at least 17 mL, particularly at least 18 mL, preferably at least 19 mL, and more preferably at least 20 mL. Furthermore, the activated carbon preferably has a methylene blue value in the range of 17 mL to 65 mL, particularly in the range of 18 mL to 55 mL, preferably in the range of 19 mL to 50 mL, and more preferably in the range of 20 mL to 47.5 mL. Furthermore, the activated carbon (i.e., the activated carbon that forms the catalyst support) must be at least 250 cm². 3 / g, especially at least 300cm 3 / g, preferably at least 350cm 3 / g, preferably at least 375cm 3 Gravimetric N2 adsorbed amount calculated using a partial pressure of 0.25 p / p0 per g Vads(wt) It is preferable that the activated carbon has 250 cm³. 3 / g~850cm 3 / g, especially 300cm 3 / g~700cm 3 / g, preferably 350cm 3 / g~650cm 3 / g, more preferably 375cm 3 / g~625cm 3 Gravimetric N2 amount V measured at a partial pressure p / p0 of 0.25 / g ads(wt) It is preferable that it has Similarly, the activated carbon (i.e., the activated carbon that forms the catalyst support) should be at least 50 cm². 3 / cm 3 , especially at least 100cm 3 / cm 3Preferably at least 110 cm 3 / cm 3 The volume-based amount of adsorbed N2 V is measured at a partial pressure of 0.25 p / p0. ads(vol.) It is preferable to have the following. In this regard, the activated carbon is 50 cm 3 / cm 3 ~300cm 3 / cm 3 , especially 80cm 3 / cm 3 ~275cm 3 / cm 3 Preferably 90cm 3 / cm 3 ~250cm 3 / cm 3 , more preferably 95cm 3 / cm 3 ~225cm 3 / cm 3 The volume-based amount of adsorbed N2 V is measured at a partial pressure of 0.25 p / p0. ads(vol.) It is preferable that it has Furthermore, the activated carbon (i.e., the activated carbon that forms the catalyst support) must be at least 300 cm². 3 / g, especially at least 450cm 3 / g, preferably at least 475cm 3 Gravimetric adsorbed N2 amount V measured at a partial pressure p / p0 of 0.995 / g ads(wt.) It is preferable to have this. In this regard, activated carbon is 300 cm 3 / g~2,300cm 3 / g, especially 400cm 3 / g~2,200cm 3 / g, preferably 450cm 3 / g~2,100cm 3 / g, more preferably 475cm 3 / g~2,100cm 3 Gravimetric N2 amount V measured at a partial pressure p / p0 of 0.995 / g ads(wt) It is preferable that it has Similarly, the activated carbon (i.e., the activated carbon that forms the catalyst support) must be at least 200 cm². 3 / cm 3 , especially at least 250cm 3 / cm 3 Preferably at least 275 cm 3 / cm 3 , more preferably 295cm 3 / cm 3 The volume-based amount of adsorbed N2 V is measured at a partial pressure of 0.995 p / p0. ads(vol.) It is preferable that it has 200 cm². In this regard, activated carbon is 200 cm². 3 / cm 3 ~500cm 3 / cm 3 , especially 250cm 3 / cm 3 ~400cm 3 / cm 3 Preferably 275cm 3 / cm 3 ~380cm 3 / cm 3 , more preferably 295cm 3 / cm 3 ~375cm 3 / cm 3 The volume-based amount of adsorbed N2 V is measured at a partial pressure of 0.995 p / p0. ads(vol.) It is preferable that it has With respect to the activated carbon further used in the present invention, the activated carbon (i.e., the activated carbon forming the catalyst support) preferably has a fractal dimension of open porosity in the range of 2.6 to 2.99, particularly 2.7 to 2.95, and / or preferably has a fractal dimension of open porosity of at least 2.7, particularly at least 2.8, preferably at least 2.85, and more preferably at least 2.9.
[0282] Within the scope of the present invention, an efficient catalyst system is provided that thus has the overall improved catalytic properties described above. From this viewpoint, the catalyst system according to the present invention leads to a considerable reduction in the method time underlying the catalytic reaction, for example, particularly in the case of discontinuous catalytic methods, and correspondingly, high resting or operating times can be utilized, which is also due to the excellent mechanical stability of the catalyst system according to the present invention. Furthermore, the use of the catalyst system according to the present invention is closely related to simplified dosing, significantly lower cleaning effort of the underlying equipment, minimized material loss, and generally simplified handling. Moreover, the catalyst system according to the present invention can be reused or recycled in a simple manner after appropriate reactivation of the catalyst. In particular, the defined pore system of activated carbon used as a support according to the present invention results in a significant improvement in activity with respect to improved methods of transporting reactants or products, and with respect to equipment having catalytically active components. Overall, the characteristics of the catalyst system according to the present invention are very important, even in the context of catalyst cost intensification, as its properties can result in considerable cost reductions.
[0283] In addition to use in discontinuous methods, the catalyst system according to the present invention is also highly suitable for use in continuous catalytic applications, thereby enabling the catalyst system to be, for example, filled into a corresponding reaction vessel or reactor and to allow a continuous flow of reactants or a medium containing reactants, thereby achieving reasonably high flow rates with only low pressure loss within the operating range.
[0284] The catalyst system according to the present invention has a wide range of applications: In addition to its use in catalytic reactions on a (large) industrial scale, the catalyst system according to the present invention is particularly suitable for adsorption applications, such as removing harmful substances like pollutants and toxins, due to its combined properties of chemical adsorption on the one hand and physical adsorption on the other.
[0285] In particular, with regard to the spherical shape, the excellent mechanical properties of the activated carbon material in the lower layer of the PBSAC form, and the current adjustable setting of porosity, especially the provision of high mesoporosity and macroporosity, the catalytic system according to the present invention is of high importance, especially for continuous catalytic reactions (i.e., continuous reaction control in catalytic reactions).
[0286] The catalyst system according to the present invention is, in particular, a supported noble metal catalyst or a metal catalyst supported on activated carbon. In particular, as mentioned above, a polymer system spherical high-performance adsorbent containing 99% by weight or more carbon forms the basis, and activated carbon functions as the catalyst support. As previously described with respect to the method according to the present invention, the catalyst support is pretreated by an oxidative method (before being equipped with the catalytically active component). In this method, the proportion of the volatile component can be varied in the range of 0.1% by weight to 15% by weight. With respect to the method according to the present invention described above, in a further method step, the catalyst support can be equipped with a noble metal, preferably as the catalytically active component, particularly by various impregnation techniques. Thereafter, the impregnation level can be varied, for example, in the range of 0.05% by weight to 20% by weight. After immobilizing the catalytically active component or the associated noble metal ions on the surface of the catalyst support, the metal ions can be converted in a reductive step. This reduction, which also leads to surface reduction of the activated carbon, can be carried out particularly in the liquid phase or gas phase. Based on this, the catalyst system according to the present invention described above can be obtained in this way.
[0287] With respect to embodiments of catalyst systems according to this embodiment, further descriptions of the present invention, as applicable as appropriate, may also be referenced.
[0288] A further object of the present invention, according to a third aspect of the present invention, is to provide applications for the catalyst system according to the present invention:
[0289] Therefore, the catalyst system according to the present invention can be used particularly as a catalyst or a catalyst support. Furthermore, the catalyst system according to the present invention can be used particularly for chemical catalysts, particularly heterogeneous catalysts and / or discontinuous catalysts, or continuous catalysts (i.e., continuous reaction control in catalysts).
[0290] Similarly, the catalyst system according to the present invention can be used as a catalyst for chemical methods and reactions, particularly hydrogenation reactions or oligomerization and polymerization reactions, preferably for olefins. Preferably, the catalyst system according to the present invention can be used as a catalyst for hydrogenation reactions. In particular, the catalyst system according to the present invention can be used for the hydrogenation of various functional groups. For example, the catalyst system according to the present invention can be used for the catalytic conversion or conversion of nitro groups to amine groups. Furthermore, the catalyst system according to the present invention can be used for deprotection.
[0291] Furthermore, the catalyst system according to this embodiment can also be used in the manufacture of filters and filter materials, particularly for the removal of contaminants, odors and toxins from air and / or gas streams, such as NBC protective mask filters, odor filters, surface filters, air filters, especially indoor air purification filters, adsorption support structures and filters in the medical field.
[0292] Furthermore, the catalyst system according to the present invention can be used as an adsorption reservoir for gases or liquids.
[0293] Similarly, catalytic systems can be used in gas sensors and fuel cells.
[0294] Furthermore, the catalyst system according to the present invention can be used as an adsorbent, particularly an adsorbent or chemioadsorbent, preferably a chemioadsorbent, and especially preferably a reactive and / or catalytic adsorbent.
[0295] Furthermore, the catalyst system according to the present invention can be used for gas purification and / or gas treatment.
[0296] Furthermore, the catalyst system according to the present invention can be used for the removal of contaminants, particularly gaseous contaminants, or substances or gases that are harmful to the environment, health, or toxicity.
[0297] Furthermore, the catalyst system according to the present invention can be used for the production and / or provision of a cleanroom atmosphere, particularly for the electrical industry, and especially for semiconductor or chip manufacturing.
[0298] Furthermore, according to a fourth aspect of the present invention, the present invention relates to protective materials, particularly for civilian or military use, particularly protective clothing, such as protective suits, protective gloves, protective socks, protective hoods and protective covers, preferably all of the aforementioned protective materials for NBC use manufactured using or having a catalyst system according to the present invention.
[0299] Furthermore, a further object of the present invention, according to a fifth aspect of the present invention, is a filter and filter material for removing all kinds of contaminants, odors and toxic substances from air or gas streams, particularly NBC protective mask filters, odor filters, surface filters, air filters, filters for purifying room air in particular, adsorbable and / or chemisorbable carrier structures and filters for the medical field, etc., manufactured using or comprising the catalyst system defined in the present invention.
[0300] With respect to filters and filter materials according to the present invention, the catalyst system used in this respect is preferably self-supporting and preferably in the form of a bulk material, particularly a loose bulk material. Furthermore, the catalyst system can also be applied to a support material.
[0301] With regard to descriptions relating to the third to fifth aspects of the present invention, further descriptions according to the first and second aspects of the present invention can also be referenced, and those descriptions may be applied as appropriate.
[0302] The present invention will be further described with reference to the drawings and / or graphic representations, thereby the description in this regard will apply to all aspects of the present invention and will not be limiting in any way. With reference to the drawings or graphic representations, the following description in the embodiments may also be seen. [Brief explanation of the drawing]
[0303] [Figure 1] Figure 1 shows the nitrogen isotherms of various catalyst supports or activated carbons used to determine porosity. [Figure 2] Figure 2 shows the mercury intrusion curves of various catalyst supports or activated carbons used to determine porosity. [Figure 3] Figure 3 shows a diagram illustrating the crystallite size and dispersion of the catalytically active component or metal, as determined for different catalyst systems (5% by weight of palladium catalyst). [Figure 4] Figure 4 is a schematic diagram of the underlying dynamics of a heterogeneous catalytic reaction based on substeps, including a first step (1) of diffusion of reactants (E) onto the surface of catalyst (K) via a fixed boundary layer (G); a second step (2) of dispersion of reactants (E) into the pores of catalyst (K) relative to the catalytic active center or catalytic active components; a third step (3) of adsorption of reactants (E) on the active center; a fourth step (4) of reacting reactants (E) on the active center to obtain the product (P); a fifth step (5) of desorption of the product (P) from the active center; a sixth step (6) of diffusion of the product (P) through the pore system of catalyst (K); and a seventh step (7) of diffusing the product (P) to the external region via the boundary layer (G) and removing the product (P). [Figure 5] Figure 5 is a schematic diagram of the method sequence according to one embodiment of the present invention [EP = precious metal precursor, TR = PBSAC carrier, TV = carrier pretreatment (e.g., oxidation with mineral acid or air oxidation), I = impregnation (e.g., immersion impregnation or spray impregnation), W = washing, T = drying, R = reduction (e.g., gas-phase or liquid-phase reduction), Cat = catalyst, CatR = catalyst reactivation, MR = metal recovery]. [Figure 6]Figure 6 is a schematic diagram of an apparatus based on a fixed-bed reactor used in heterogeneous catalytic reactions, particularly hydrogenation reactions. [Figure 7] Figure 7A is an explanatory diagram showing the basic reaction of the hydrogenation reaction of cinnamic acid using the catalyst system according to the present invention. Figure 7B is a diagram showing the time course of catalytic conversion (hydrogenation) of cinnamic acid as a reactant by various catalyst systems according to the present invention using activated carbon (mesoporous and macroporous activated carbon) with a high proportion of mesopores and macropores in the total pore volume of the activated carbon as a catalyst support. Figure 7C is a diagram showing the time course of catalytic conversion (hydrogenation) of cinnamic acid using a catalyst system (microporous activated carbon) that uses activated carbon as a catalyst support and has a high proportion of micropores in the total pore volume of the activated carbon. [Modes for carrying out the invention]
[0304] Further embodiments, modifications, and variations of the present invention, as well as their advantages, will be readily apparent and feasible to those skilled in the art by reading this specification without departing from the scope of the invention.
[0305] The following embodiments are merely illustrative of the present invention and do not limit it thereto. [Examples]
[0306] 1. Introduction: The use of special polymer-based spherical activated carbon (spherical or spherical PBSAC) having defined porosity, particularly high mesoporosity or macroporosity, and simultaneously defined microporosity, as a catalyst support material offers advantages related to the concept of the present invention, namely, an optimal method for transporting reactants / products and optimal mounting of the activated carbon with catalytically active components. As a result, the catalyst system according to the present invention can achieve overall high catalytic activity, particularly high conversion rates and high space / time yields. Furthermore, its preferred spherical shape allows for the lowest pressure drop compared to adsorbents of the same size but different shapes. Additionally, PBSAC has a low dust content and high mechanical load capacity, minimizing the possibility of metal-containing dust and fragments being discharged into the product flow during fixed-bed bulk applications.
[0307] 2. Catalyst support manufacturing a) Highly microporous catalyst support (not according to the present invention) Polymer-based spherical activated carbon (PBSAC) is produced by a three-step batch process. This process includes a sulfonation step for thermal stabilization of the polymer raw materials used, a carbonization step to remove volatile components, and an activation step to form an internal pore system using water as an oxidizing agent. A rotary tube reactor is used for the necessary process steps. The reactor is indirectly electrically heated within a rotary kiln.
[0308] Cross-linked styrene-divinylbenzene polymer (H) manufactured by Lancel. + The gel-type polymer is used as a raw material or starting material for the production of highly porous PBSAC (Lewapol D60). It is polystyrene with 4% by weight of divinylbenzene as a crosslinking agent. The polymer raw material already has a spherical morphology, which is transferred to the resulting PBSAC. The raw material exhibits a particle size distribution in the range of 0.08 mm to 0.7 mm.
[0309] Sulfonation is a step that stabilizes the polymer for subsequent carbonization. For this purpose, a mixture of oleum (sulfuric acid fumes, 25% free SO3) and sulfuric acid (96% by volume) is added to polystyrene in a 2:1 mass ratio at room temperature and heated to the sulfonation temperature of 423 K. This mixture is then reacted with sulfuric acid.
[0310] In the second stage of activated carbon production, known as carbonization, volatile components are released in a temperature range of 423K to 1223K. The carbonization process is divided into two stages. In the temperature range up to 823K, water and sulfur compounds are released in addition to other volatile components. In the temperature range up to 1223K, mainly hydrocarbons and hydrogen are released (activation time of 390 minutes). The particle shape and particle size after carbonization remain unchanged and are consistent with the particle shape of the resulting PBSAC.
[0311] In the third stage of activated carbon production, known as activation, the carbon is activated at approximately 1223 K in a steam atmosphere (120 kg of liquid water and 2 standard cubic meters of nitrogen per hour).
[0312] b) Mesoporous and macroporous catalyst supports (according to the present invention) For the production of mesoporous and macroporous PBSAC, the method steps described in Section 2.a) above are followed. Similarly, Rewapol D60 from Lances is used as a raw material or starting material for the production of mesoporous / macroporous PBSAC. However, the sulfonation of the cross-linked styrene-divinylbenzene polymer is carried out exclusively with sulfuric acid (96% by volume). The ratio of polymer to sulfonating agent is kept constant. The catalyst support is activated for 450 minutes. The resulting PBSAC exhibits an increased mesoporation content of 25% or more. Texture data is taken from Table 2.
[0313] c) Mesoporous and macroporous catalyst supports based on sulfonated ion exchange resins having high macroporous properties (according to the present invention) For the production of PBSAC based on macroporous ion exchange resin, the method steps described in Section 2.a) above are followed. As a raw material or starting material for the production of PBSAC based on macroporous ion exchanger (Finex CS16GC), a sulfonated crosslinked styrene-divinylbenzene polymer (H) of Finex Oy is used. + The form is used. Since the acidic macroporous ion exchanger is already protected, the sulfonation step can be omitted (activation time of 150 minutes). The resulting PBSAC exhibits a high mesopore content and a defined ratio of macropores. Texture data can be obtained from Table 2. Alternatively, the corresponding unsulfonated raw material or starting material can be assumed. In this case, for example, a crosslinked styrene-divinylbenzene polymer from Phenex Oy can be used (Phenex PS08G). Sulfonation can be carried out as in section 2.a).
[0314] 3. Characterization of catalyst supports or catalyst systems a) Nitrogen isotherms for determining texture data in micropore regions To determine the texture data of the catalyst support, nitrogen isotherms are recorded for various catalyst supports. This is performed using Quantachrome's "Quantrosolve" system. Specific internal surface area is measured using the Brunauer-Emmett Teller (BET) mathematical model. Total pore volume is calculated using the Gulvitch rule, and micropore volume is measured using the carbon black method.
[0315] Regarding measurement and manufacturing, the catalyst support is pre-treated in a vacuum at 200°C, particularly with the aim of removing adsorbed molecules.
[0316] b) Mercury immersion for measuring texture data in mesopore and macropore regions The samples are dried in a drying oven at 150°C for 2 hours and measured using a Quantachrom PoreMaster 60GT. To convert pressure to pore size, the literature value for the contact angle of mercury to carbon is calculated (155°).
[0317] c) Measurement of the elemental composition of catalyst supports by photoelectron spectroscopy (XPS) Samples are analyzed by photoelectron spectroscopy (ESCA / XPS) without pretreatment. For XPS analysis, measurements are performed using a ThermoVG Scientific K-α instrument. Monochromatic AlKα X-rays are used for excitation (usually up to 75W, 400μm spot size). For copper, silver, and gold standard samples, the transmission function and energy position are measured according to ISO 15472:2001 and ISO 21270:2004. The settings described below are used for measuring the spectrum: survey spectrum with a pass energy of 80 eV and high-resolution spectrum with a pass energy of 30 eV. Quantitative information on surface composition is calculated using the Schofield coefficient for survey measurements assuming the analyte is homogeneous. The error is estimated to be around 10%.
[0318] d) Determination of the dispersion and size of active sites by CO chemiadsorption (determination of the dispersion of catalytic active components on special metal surfaces and crystallite size). Measurement of monolayer capacity, dispersion, and active surface according to DIN66136-1 and DIN66136-3: flow method (dynamic), measurement gas, e.g., H2, CO, CO2; planned experimental program: H2 treatment, isothermal up to 80°C at 10K / min for 4 hours; CO titration at 50°C; then TPR 5K / min up to 250°C with 5% H2 / Ar; finally, CO titration at 50°C.
[0319] Specifically, proceed as follows: Standard basis: DIN 66136-1 (Basic) and DIN 66136-2 (Volumetric Method)
[0320] The following steps are recommended or performed for sample preparation and reduction of the sample surface: (i) Evaporate at 100°C for 30 minutes; (ii) Flow oxygen at 100°C for 5 minutes; (iii) Flow oxygen and raise the temperature to 350°C at a rate of 10°C / min; (iv) Flow oxygen at 350°C for 30 minutes; (v) Evaporate at 350°C for 15 minutes; (vi) Evaporate at 100°C for 15 minutes; (vii) Flow hydrogen at 100°C for 5 minutes; (viii) Flow hydrogen and raise the temperature to 350°C at a rate of 10°C / min; (ix) Flow hydrogen at 350°C for 120 minutes; (x) Evaporate at 350°C for 30 minutes; (xi) Evaporate at 100°C for 15 minutes.
[0321] Subsequently, to determine the active metal surface or metal dispersion, the CO isotherm at 40°C is measured using the static volume method.
[0322] The first isotherm measured after step (xi) may represent a superposition of strongly chemisorbed and weakly chemisorbed gas fractions (composite chemisorption). If it is necessary to distinguish between the two fractions, the following procedure is recommended or performed: After measuring the last isotherm, the measurement cell is vacuumed at the analysis temperature (40°C) for 60 minutes. This removes the weakly bound portion, leaving the strongly chemisorbed portion on the sample surface. The weakly chemisorbed fraction is then measured by repeating the isotherm measurement (weak chemisorption). The difference between the two isotherms gives the amount of strongly chemisorbed CO.
[0323] Assuming that CO molecules are chemically adsorbed onto one exposed metal atom (palladium atom) on the surface of the catalytically active component (stoichiometry = 1), the number of exposed palladium or metal atoms on the surface can be estimated from the amount of chemically adsorbed CO.
[0324] This is the area per gram (m²) 2 This provides an indication of the size of the active metal surface area per g (sample mass).
[0325] Further properties and characteristics are calculated using the metal load of the sample, known as the mass of palladium in g / g samples: ·m 2 / g (metal) active metal surface; • Degree of dispersion of metals (%); and • Average crystallite size of a metal cluster. A similar procedure is followed for other metals.
[0326] 4. Characteristics of catalyst supports The characteristics of each catalyst support are as different as possible in terms of their texture. To measure the texture data, nitrogen isotherms of each PBSAC are recorded. The results obtained are shown in Figure 1. In the legend, "200 μm" indicates the average particle size of the activated carbon investigated in each case. Figure 1 shows the nitrogen adsorption amount Vads as a function of the relative pressure p / p0 of the investigated activated carbon.
[0327] A characteristic of highly microporous materials is the rapid rise in isotherms at low relative pressures, accompanied by large nitrogen uptake. As shown in Figure 1, the isotherms run almost flat in the region of even lower relative pressures and do not show a significant hysteresis loop. The isotherm of "200 μm_Micro I" (a catalyst support or activated carbon A1 not according to the present invention) shows this progression, and therefore this material is described as having strong microporosity. Furthermore, the ratio of microporous volume to the total volume is very high at 89%.
[0328] The isotherm of "200μm_meso / macro I" (catalyst support or activated carbon B1 according to the present invention) shows a strong increase at a relative pressure of 0.75, as shown in Figure 1. Furthermore, the isotherm exhibits a prominent hysteresis loop. These two characteristics, along with the micropore content of 61%, demonstrate a high content of mesopores or macropores.
[0329] When using macroporous ion exchange resins in the production of PBSAC, some of the macroporosity of the polymer is transferred to the resulting activated carbon. This can be seen from the nitrogen isotherm of "200 μm Meso / Macro II" (catalyst support or activated carbon B2 according to the present invention). Only at a relative pressure of 0.85 does the isotherm and the resulting nitrogen uptake increase sharply (Figure 1). The prominent hysteresis loop and the micropore capacity of only 25% demonstrate the presence of pores larger than 2 nm, and the presence of mesopores and macropores.
[0330] Pore characteristics of 2 nm or larger can be achieved by mercury intrusion. Figure 2 shows the mercury intrusion curve of the catalyst support. The graphical representation in Figure 2 shows the mercury intrusion dVp / dlog(dp) as a function of the underlying pore diameter dp of the investigated activated carbon.
[0331] Here, it is clear that the microporous catalyst support or activated carbon A1 ("200 μm_micro I") does not have a pore volume greater than 2 nm. The meso / macroporous catalyst support or activated carbon B1 ("200 μm_meso / macro I") shows a significant pore volume in the range of 10 nm to 20 nm. The further meso / macroporous catalyst support or activated carbon B2 ("200 μm_meso / macro II") also shows a very large proportion of mesopores and a considerable proportion of macropores. Texture data can be found in Table 3.
[0332] The chemical composition and high purity of activated carbon in the PBSAC form are maintained and comparable in all cases. Similarly, the high mechanical stability of activated carbon in the PBSAC form is maintained, which is also maintained with high porosity and a high proportion of pores larger than 2 nm (see: "200 μm Meso / Macro I" (B1) and "200 μm Meso / Macro II" (B2)). High mechanical stability is demonstrated by high wear resistance of over 98% (see Table 2).
[0333] Table 2 below shows the corresponding properties of the activated carbon or catalyst support that was investigated.
[0334] [Table 2] * A1: Not based on the present invention ** C1, C2: Commercially available coconut shell activated carbon system; (not related to the present invention)
[0335] [Table 3]
[0336] In the corresponding method, further catalyst supports or activated carbons are provided. That is, catalyst supports or activated carbons A2 (200 μm micro II; average particle size 200 μm) and A3 (370 μm micro III; average particle size 370 μm) that do not conform to the present invention are essentially equivalent to catalyst support A1 in terms of their respective properties in the form of the parameters listed in Tables 2 and 2. Furthermore, further catalyst supports or activated carbons are provided, namely, catalyst supports B3 ("370 μm meso / macro III"; average particle transmittance 370 μm) and B4 ("470 μm meso / macro III"; average particle transmittance 470 μm) used according to the present invention are essentially comparable to catalyst supports B1 and B2 in terms of their other properties in the form of the parameters listed in Tables 2 and 2.
[0337] 5. Oxidative pretreatment of catalyst supports Oxidative pretreatment of materials in the form of catalyst supports or activated carbon helps create oxygen centers on the surface of each PBSAC. These then interact with metal ions in the salt solution. Due to the electrostatic interaction between the surface oxide and the metal ions, the metal ions become immobilized on the surface and preferentially migrate into the pores of the PBSAC rather than remaining in the supernatant.
[0338] a) For the oxidation of PBSAC, synthetic air is passed through a gas-sealed fused silica reactor capable of heating. For surface modification, typically 250g of PBSAC is placed in a fused silica tube, which is then placed in the furnace and all gas connections are attached. Typically, the furnace is set to 10Kmin. -1 The mixture is heated to the reaction temperature using a lamp. The reaction temperature is within the range of 350°C to 550°C. The reaction time varies within the range of 120 minutes to 600 minutes.
[0339] b) Oxidation treatment with mineral acids or hydrogen peroxide Oxidation with mineral acids is carried out by wet chemical means. The mineral acids are mainly hydrochloric acid (HCl), nitric acid (HNO3), and sulfuric acid (H2SO4). Perchloric acid (HClO4), phosphoric acid (H3PO4), and hydrogen peroxide (H2O2) are also used. These acids are used across the entire concentration range at temperatures from 20°C to 100°C.
[0340] Typically, 500g of polymer system spherical adsorbent is stirred with 1000g of mineral acid for 30 to 240 minutes. After that, the excess mineral acid is decanted, the oxidized base adsorbent is washed with distilled water, and dried.
[0341] c) Characteristics of oxidized catalyst supports As a result of surface modification, the structural properties remain unchanged or change only within a very small range. The properties of the oxidation catalyst supports used or analyzed in this invention can be obtained from Table 4. The mechanical stability of the oxidation catalyst supports is maintained by very high wear hardness. Measurement of volatile components is used to characterize the surface oxides. In this case, the material is left at 900°C for 7 minutes according to ISO 562-1981, and the weight loss is then measured gravimetrically.
[0342] However, this method still doesn't reveal anything about the properties of the oxygen species present on the surface of PBSAC. To determine these, the photoelectron spectra of each catalyst support are recorded. From these spectra, the elemental composition can be determined. These can be read from Table 5. The measured values of volatile components show a correlation with the atomic composition determined by photoelectron spectroscopy. The lowest oxygen content was observed in the sample oxidized with hydrochloric acid (90 minutes), at 4.0 atomic percent. When the catalyst support was oxidized with 50% by volume nitric acid, the surface oxygen content was highest at 11.8 atomic percent.
[0343] [Table 4]
[0344] [Table 5]
[0345] Furthermore, to understand the characteristics of the oxygen species, the bonded fractions are measured from high-resolution oxygen spectra. These can be obtained from Table 6. It can be seen that more than half of the oxygen species are in the form of surface alcohol oxygen. Approximately 35% to 40% of the oxygen atoms are bonded to the surface in the form of carbonyl oxygen. Different oxidized catalyst supports differ only slightly in the proportion of oxygen species.
[0346] [Table 6] O1: Carbonyl oxygen (RC=0 / R-CO=O) * ) O2: Alcohol Oxygen (R-OH / ROR / R-CO-O) * O3:pi-pi *
[0347] 6. Impregnation treatment of catalyst support Since the oxidized catalyst support or activated carbon has catalytically active components or related precursors, the corresponding impregnation catalyst system is obtained as described below.
[0348] a) Palladium load of PBSAC Add water and an acid solution (HCl, HNO3) to a round-bottom flask. Then add a palladium precursor (usually H2PdCl4, Pd(NO3) 32 ) is added. The turbid suspension is vigorously stirred in a magnetic stirrer for at least 30 minutes until a clear, brownish solution is obtained. The oxidation catalyst support is rapidly added as previously shown while vigorously stirring. The system is stirred at low speed (50 rpm) for 24 hours. The solution is then removed. The solid is then separated using a Büchner funnel and a suction flask. The catalyst is then thoroughly washed with ultrapure water. For drying, the material is transferred to a drying oven and dried at 80°C for 12 hours. The material is then dried in an oven.
[0349] b) Amount of platinum loaded onto spherical adsorbent Water and an acid solution (HCl, HNO3) are placed in a round-bottom flask. Subsequently, a platinum precursor (usually H2[PtCl6], (NH3)4Pt(OH)2, Pt[NO3)2) is added. The turbid suspension is vigorously stirred in a magnetic stirrer for at least 30 minutes until a clear, brownish solution is obtained. The oxidation catalyst support is rapidly added while vigorously stirring. The system is stirred at low speed (50 rpm) for 24 hours. The solid is then separated using a Büchner funnel and suction flask. The catalyst is then thoroughly washed with ultrapure water. For drying, the material is transferred to a drying oven and dried at 80°C for 12 hours. The material is then dried in an oven.
[0350] 7. Reduction of a catalyst or reduction to obtain a catalytic system By subjecting the above impregnation catalyst system to reduction treatment, the corresponding catalyst system can be obtained as follows. a) Gas-phase reduction The gas-phase reduction of the catalyst material is carried out in a horizontal, heatable flow tube containing 5% by volume of hydrogen in nitrogen, at a temperature of 50°C to 300°C for a period of 1 to 10 hours. The catalyst material is then heated to a temperature of 1°C. b) Liquid-phase reduction Liquid-phase reduction is preceded by the fixation of the active ingredient with potassium hydroxide (KOH). The base is added stoichiometrically to the impregnation solution at room temperature. Subsequently, potassium formate (COO) is added in a 10-fold stoichiometric excess, and the solution is left to stand at 50°C to 120°C for 1 to 5 hours. After that, the solution is fixed with potassium hydroxide (KOH).
[0351] 8. Properties of palladium catalysts The size and distribution of metal active centers can be controlled by the selected reduction method and reaction parameters. The degree of dispersion can be set in the range of 15% to 35%. The cluster diameter of the metal centers varies in the range of 33 angstroms (3.3 nm) to 76 angstroms (7.6 nm). In this regard, see Figure 3, which shows the measured values for metal dispersion (MD) and metal crystallite size (KG) of 5 wt% palladium catalyst (based on catalyst supports B1 and B4, respectively). Figure 3 also shows the optimized reduction temperature T according to the present invention. red2 (Here, at 140°C) the reduction temperature T, which is designated as the so-called standard temperature according to the present invention in Figure 3. red1 Compared to (here at 80°C) (and therefore explicitly belonging to the present invention), further improved properties are obtained in terms of metal dispersion and average crystallite size, which in turn leads to further improvements in the catalytic performance of catalyst systems according to the present invention. The same applies to platinum catalysts and ruthenium catalysts.
[0352] 9. General principles regarding hydrogenation in fixed-bed reactors The catalyst system according to the present invention can be used particularly on a large scale, for example, as a catalyst for hydrogenation reactions. Hydrogenation is one of the standard reactions in technical chemistry and is used in large-scale methods such as petrochemicals, for example, in the desulfurization of petroleum fractions and in the synthesis of fine chemicals. In addition to unsaturated compounds, other groups of substances are also hydrogenated, such as aldehydes and ketones to alcohols, and nitro compounds and nitriles to amines. In most hydrogenation reactions, the reactants are in the liquid phase; only low-boiling point substances such as butyraldehyde from hydroformylation are hydrogenated in the gas phase.
[0353] Precious metals such as nickel, platinum, ruthenium, and palladium function as hydrogenation catalysts, mostly in the form of supported catalysts. They are either suspended in the reaction mixture as particulate material or used as a fixed bed. In the latter case, trickle-bed reactors are used for three-phase reactions (reaction mixture, gaseous hydrogen, and solid catalyst). That is, fixed-bed reactors are used in which the catalyst packing is dispersed into the reaction mixture. The size of the catalyst packing (spheres, cylinders, extruded parts, etc.) is, for example, between 1 and 7 mm.
[0354] A corresponding hydrogenation apparatus is shown in Figure 6, and this will be used as an example to explain the method control: Reactant A is supplied from above to a tubular reactor (a) and flows through the reactor, which has a catalyst bed, in co-flow or counter-flow with hydrogen H2. In terms of volume, the gas phase is the dominant phase compared to the liquid phase and flows around the catalyst bed wetted by the liquid phase. However, only reactors operating in co-flow are widely applied in technology. The flow is driven by gravity or external pressure. For temperature control, the reactor is equipped with a double jacket. At its lower end, the hydrogenation product B is removed and finally degassed in a separator (b). The residual gas RG is discharged through apparatus (c).
[0355] In trickle-bed reactors, conversion rate and selectivity depend not only on reaction kinetics, pressure, and temperature, but also on the reactor's fluid dynamics. Fluid dynamics significantly affect the liquid distribution within the reactor, and the catalyst's fluid dynamics have a major impact on the liquid distribution within the reactor, directly affecting catalyst utilization. Non-uniform fluid distribution results in incomplete wetting of the catalyst bed, which can negatively impact catalyst utilization.
[0356] Furthermore, catalyst bed wetting can be disrupted by unoptimized technical sizing, such as the ratio of height to diameter of the reactor and the ratio of reactor inner diameter to catalyst particle diameter. To prevent these effects on the unwetted reactor interior and / or catalyst areas, the design of the liquid partition and the maintenance of the corresponding size ratio are crucial.
[0357] Therefore, the design of trickle bed reactors is based on parameters such as liquid hold-up (the amount of liquid present in the entire catalyst bed), pressure loss across the bed, gas-liquid phase distribution, or mass and heat transfer coefficients. Industrially used reactors are 5-30 m tall, and in these, the catalyst bed exists in multiple beds or a single bed. The diameter of the reactor is limited by the uniform distribution of liquid across the cross-section of the reactor and usually does not exceed a value of 4-5 m. Therefore, the ratio of the reactor height to diameter (Hr / Di) is generally between 5 and 25. Trickle bed reactors used on a laboratory scale have a diameter of 0.03 m to 0.2 m and can reach several m in length. At these scales, the ratio of the reactor inner diameter to the catalyst diameter (Di / dk) cannot be ignored and must be greater than or equal to Di / dk = 10 (usually Di / dk > 15). Otherwise, differences in the structure of the packing near the furnace wall and the packing core can limit fluid flow, which can be reflected in a decrease in conversion efficiency. In industrially used reactors, the ratio of the reactor bore to the catalyst diameter is usually between 100 and 1000 to ensure that the influence of liquid moving along the edges is eliminated.
[0358] Conventional trickle bed reactors with a diameter of 0.2m or more are generally not well-suited for the production of fine chemicals due to their minimal processing capacity. However, advancements in miniplant technology have made continuous operation possible even at very low processing capacities (less than 1kg / h). Miniplants have primarily been used in method development until now. However, miniplants are also suitable for production, particularly for the small-scale production of products requiring consistent quality, such as fine chemicals and active ingredients for pharmaceuticals and agrochemicals.
[0359] For more detailed explanations, please refer in particular to the following: Industrial Chemistry, Manfred Burns et al., 2nd edition, Willey-VCH Press Ltd., 2013; Chapter “Three-Phase Trickle Bed Reactors,” Ullmans Encyclopedia of Industrial Chemistry, Vol. 7, Online Education 2008; and Chapter “Types of Reactors and Their Industrial Applications,” Ullmans Encyclopedia of Industrial Chemistry, Vol. 7, Online Education 2008.
[0360] 10. Catalysis test (hydrogenation reaction of cinnamic acid) The catalytic performance of the catalyst system according to the present invention can also be investigated in comparison with a system not according to the present invention by examining hydrogenation reactions or catalytically controlled hydrogenation reactions, such as the hydrogenation of cinnamic acid as a reactant to hydrocinnamic acid as a product. For this purpose, please also refer to Figure 7A.
[0361] A 100 mL three-necked flask equipped with a stirring rod, an N2 inlet, and an H2 outlet is charged with cinnamic acid (1) (2 g, 13.5 mmol) and 144 mg of catalyst. The three-necked flask is sealed with a rubber septum, evacuated, and refilled with nitrogen (3 times). Ethyl acetate (14 mL) is added, and the mixture is stirred (700 rpm) until the reactants are completely dissolved. The flask is evacuated and hydrogen is replenished (3 times). Samples are taken periodically at 1, 2, 3, 5, 7, 10, and 16 hours and analyzed by gas chromatography combined with a mass spectrometer. Catalyst systems based on catalyst supports A1, A2, and A3 (not according to the present invention) and catalyst systems based on catalyst supports B1, B2, and B3 (according to the present invention) were investigated.
[0362] The results are shown in Figures 7B and 7C. These figures show the catalytic transformation (hydrogenation) of cinnamic acid as a reactant and starting material, respectively, by the amount of cinnamic acid over time (measured by GC-MS; area %), assuming that 100% of the unreacted cinnamic acid is present as a starting material at time t=0.
[0363] Figure 7B shows the results for catalyst systems according to the present invention based on catalyst supports B1, B2, and B3 (where, at t=4 hours, the upper line represents catalyst system B3, the middle line represents catalyst system B1, and the lower line represents catalyst system B2). Figure 7C shows the results for catalyst systems not according to the present invention based on catalyst supports A1, A2, and A3 (where, at t=7 hours, the upper line represents catalyst system A3, and the lower lines represent catalyst systems A1 and A2, respectively).
[0364] The comparison of the linear curves shown in Figures 7B and 7C demonstrates that the catalytic performance of the catalyst system according to the present invention, based on catalyst supports B1, B2, and B3, is significantly higher than that of a system not according to the present invention, based on catalyst supports A1, A2, and A3. Therefore, the conversion or hydrogenation of the starting material in the form of cinnamic acid is completed significantly faster in the system according to the present invention than in the system not according to the present invention, thus enabling the use of a higher conversion rate in the system according to the present invention.
[0365] Therefore, the catalyst systems based on catalyst supports B1, B2, and B3 according to the present invention exhibit high overall catalytic performance, particularly with high conversion rates and improved space / time yields. The same applies to the corresponding platinum catalyst systems and ruthenium catalyst systems.
[0366] As mentioned above, the special pore system of activated carbon used as a catalyst support, which has high mesoporosity and macroporosity, is particularly important in relation to improving the methods of transporting reactants and products.
[0367] Furthermore, the catalyst system according to the present invention features an overall improvement in the apparatus using the catalytically active component. This improvement is due to a special method of manufacturing the catalyst system according to the present invention, in which activated carbon is oxidized according to the target and purpose before supporting the catalytically active component or related precursor, and then reduced to obtain the catalyst system. In particular, the special pore structure of the activated carbon, as also described in the form of a special ratio (quotient Q) of total pore volume to a specific BET surface area, results in improved properties with respect to the catalytic activity of the catalyst system according to the present invention.
[0368] In this regard, in particular, as previously shown, the totality of measures according to the present invention in those specific combinations, the target and purpose-oriented combinations, lead to the advantages and characteristics of the catalyst system according to the present invention.
[0369] As a result, the basic investigations as a whole indicate that the catalyst system according to the present invention, obtained by the method of the present invention, has significantly improved properties compared to prior art systems.
Claims
1. A catalytic system in the form of a supported catalyst, The catalyst system comprises at least one catalytically active component immobilized on a catalyst support, the catalytically active component comprises at least one metal, the metal is selected from the group consisting of Ru, Pd, and Pt, and The catalyst support is in the form of spherical activated carbon. The spherical activated carbon forming the catalyst support is (i) 1.1 cm 3 / g ~ 2.4cm 3 Total pore volume V by Gulvitch within the range of / g total Having, 50% to 90% of the total pore volume of the spherical activated carbon by Gulvitch is formed by pores having a pore size in the range of 2 nm to 500 nm, and (ii) 1,300m 2 / g ~ 2,200m 2 Specific BET surface area S within the range of / g BET Having; Provided that the formula Q = V total / S BET the ratio Q of the Gurvich total pore volume V total to the specific BET surface area S BET is within the range of 0.6×10 -9 m to 1.8×10 -9 m; And, The catalyst system has an activity within the range of 15% to 90%, which is measured as the percentage dispersion of the catalytically active components on the catalyst support and measured by chemiadsorption using the dynamic flow method according to DIN 66136-3:2007-01; And, A catalyst system in the form of a supported catalyst, characterized in that the catalyst system comprises at least one catalytically active component having an average crystallite size in the range of 0.5 nm to 8 nm as measured by DIN 66136.
2. The catalyst system according to claim 1, characterized in that the catalyst system has an activity in the range of 20% to 80%, which is measured as the percentage dispersion of catalytically active components on a catalyst support and measured by chemiadsorption using the dynamic flow method according to DIN 66136-3:2007-01.
3. The catalyst system according to claim 1, characterized in that the catalyst system has an activity in the range of 25% to 70%, which is measured as the percentage dispersion of catalytically active components on a catalyst support and measured by chemiadsorption using the dynamic flow method according to DIN 66136-3:2007-01.
4. The catalyst system according to claim 1, characterized in that the catalyst system includes at least one catalytically active component having an average crystallite size in the range of 0.7 nm to 7 nm, as measured by DIN 66136.
5. The catalyst system according to claim 1, characterized in that it includes at least one catalytically active component having an average crystallite size in the range of 1 nm to 6 nm, as measured by DIN 66136.
6. The catalyst system according to claim 1, characterized in that the catalyst system includes at least one catalytically active component having an average crystallite size in the range of 1.5 nm to 5.8 nm, as measured by DIN 66136.
7. The catalyst system according to claim 1, characterized in that the catalytically active component is Pd.
8. A method for catalyzing a chemical reaction via a heterogeneous catalyst, the method comprising using the catalyst system described in claim 1.
9. The method according to claim 8, characterized in that the chemical reaction is selected from among a hydrogenation reaction, an oligomerization reaction, and a polymerization reaction.
10. A protective suit comprising the catalyst system described in claim 1.
11. The protective suit according to claim 10, characterized in that the protective suit is selected from the group consisting of protective suits for the civilian sector, protective suits for the military sector, protective suits, protective gloves, protective boots, protective socks, protective hoods and protective covers.
12. A filter for removing pollutants, odors and harmful substances, characterized in that the filter has the catalyst system described in claim 1.
13. The filter according to claim 12, characterized in that the filter is selected from the group consisting of NBC protective mask filters, odor filters, surface filters, air filters, indoor air purification filters, adsorption-capable support structures, chemical adsorption-capable support structures, and medical filters.
Citation Information
Patent Citations
Process for preparing a palladium-carbon catalyst
DE2936362C2
filter material for processing and purifying gas
JP2014529490A
Catalyst system based on spherical activated carbon as a carrier and use thereof
US20160296911A1