Pipe internal coating method
By applying water-based paint during the curing reaction of the powder coating film, the method addresses the adhesion issue between powder and water-based films, enabling the use of water-based paints and reducing VOC emissions.
Patent Information
- Application Number
- JP2025162243
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2025-09-29
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2045-09-29
AI Technical Summary
Existing methods struggle to ensure adhesion between powder coating films and water-based paint films on the inner surfaces of pipe sockets, which is necessary for replacing solvent-based paints with environmentally friendly water-based paints.
A method involving a powder coating step followed by applying water-based paint during the curing reaction of the powder coating film, ensuring sufficient adhesion by utilizing functional groups capable of bonding with resin molecules in the water-based paint.
Ensures sufficient adhesion between the powder coating film and water-based paint film, allowing for the replacement of solvent-based paints with water-based paints, reducing VOC emissions and providing an environmentally friendly coating method.
Smart Images

Figure 0007955458000001_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for coating the inner surface of a pipe.
Background Art
[0002] Various types of coating are applied to the inner peripheral surface of metal pipes used for water supply and sewage systems to protect the inner surface. In particular, cast iron pipes used for water supply pipes are often coated with powder coating on the inner surface of the straight portion. As for the powder coating on the inner surface of the socket, unevenness present on the inner surface of the socket may cause coating defects. In order to prevent such coating defects from occurring, there is a technique disclosed in Patent Document 1.
Prior Art Documents
Patent Documents
[0003]
Patent Document 1
Summary of the Invention
Problems to be Solved by the Invention
[0004] In recent years, from the perspective of environmental consideration, there is a demand to switch from solvent-based paints used for coating the inner surface of sockets to water-based paints in order to reduce VOC (volatile organic compounds). The technique described in Patent Document 1 involves applying a solvent-based liquid paint on top of a powder coating, and in this case, it is possible to ensure adhesion between the powder coating film and the solvent-based paint film.
[0005] However, Patent Document 1 does not envision the use of water-based paints for coating the inner surface of sockets. On the other hand, when water-based paints are used instead of solvent-based liquid paints, it has been difficult to ensure adhesion between the powder coating film and the water-based paint film.
[0006] Therefore, one aspect of the present invention aims to provide a coating method, etc., for ensuring sufficient adhesion between a powder coating film and a water-based coating film when water-based paint is used to coat the inner surface of a socket. [Means for solving the problem]
[0007] The present inventors, after diligent study to solve the aforementioned problems, have completed the present invention. That is, one embodiment of the present invention includes the following configuration.
[0008] A method for painting the inner surface of a pipe having a straight section and a socket, A powder coating step is performed to paint the inner surfaces of the straight portion and the socket by applying powder coating to the inner surfaces of the straight portion and the socket and curing the coating film formed thereon, A method for coating the inside surface of a pipe, comprising a step of coating the coating formed on the inner surface of the socket with a water-based paint during the curing reaction of the coating film. [Effects of the Invention]
[0009] According to one aspect of the present invention, when water-based paint is used for coating the inner surface of a pipe socket, sufficient adhesion between the powder coating film and the water-based paint film can be ensured. Furthermore, this allows for the replacement of solvent-based paints used for coating the inner surface of pipe sockets with water-based paints, thereby reducing VOCs and providing an environmentally friendly method for coating the inner surface of pipes. [Brief explanation of the drawing]
[0010] [Figure 1] This is a cross-sectional view illustrating a pipe inner surface coating apparatus according to an embodiment of the present invention, which processes the coating of the inner surface of a pipe with powder coating. [Figure 2] This is a cross-sectional view illustrating a process in which a pipe internal coating apparatus applies a water-based paint to a coating film formed by applying powder coating while the coating film is undergoing a curing reaction. [Figure 3] This figure shows the results of the cross-cut test on the specimens from Test Section 1 and Test Section 2 in Example 1. [Figure 4] This figure shows the results of the cross-cut test on the specimens from test section 3 in Example 1. [Figure 5] This figure shows the results of the solvent friction test performed on the specimens from Test Section A and Test Section B in Example 2, as specified in ASTM D4752. [Modes for carrying out the invention]
[0011] One embodiment of the present invention is described below, but the present invention is not limited thereto. The present invention is not limited to the configurations described below, and various modifications are possible within the scope of the claims. Furthermore, embodiments or examples obtained by combining the technical means disclosed in different embodiments or examples are also included in the technical scope of the present invention. Moreover, new technical features can be formed by combining the technical means disclosed in each embodiment. All academic and patent documents mentioned herein are incorporated herein by reference. Furthermore, unless otherwise specified herein, "A to B" representing a numerical range means "A or greater (including A and greater than A) and B or less (including B and less than B)."
[0012] [1. Method for coating the inside of pipes] A pipe interior coating method according to one embodiment of the present invention (hereinafter also referred to as "this method") is a pipe interior coating method for coating the inner surface of a pipe having a straight section and a socket, and comprises: a powder coating step of coating the inner surface of the straight section and the socket by applying powder coating to the inner surface of the straight section and the socket and curing the coating film formed thereon; and a water-based paint coating step of coating the coating film formed on the inner surface of the socket with water-based paint during the curing reaction of the coating film.
[0013] (1) Technical concept of this method Conventionally, the inner surface of a socket has been coated by applying powder coating to the socket and then applying a solvent-based paint onto the cured powder coating film. At this time, the solvent-based paint adheres to the coating film by dissolving the surface of the powder coating film. As a result, the coating film composed of the powder coating and the solvent-based paint can ensure adhesion to the socket.
[0014] However, when the present inventors replaced the solvent-based paint with a water-based paint, they found that adhesion between the water-based paint and the coating film could not be ensured. This is considered to be because the water-based paint cannot dissolve the surface of the fully cured powder coating film.
[0015] Accordingly, the present inventors conducted intensive studies and considered that, before the curing of the powder coating is completed, functional groups capable of bonding with resin molecules in the water-based paint remain in the resin of the powder coating film. Furthermore, the present inventors considered that, by bonding the functional groups to the resin molecules in the water-based paint, sufficient adhesion between the powder coating film and the water-based paint film can be achieved, and thus sufficient adhesion between the coating film containing the powder coating and the water-based paint and the socket can be ensured.
[0016] Then, the present inventors conducted further studies and found that, by applying the water-based paint onto the powder coating film during the curing reaction of the powder coating film, sufficient adhesion between the powder coating film and the water-based paint film can be ensured, thereby completing the present invention. The mechanism for ensuring the adhesion described above is merely speculative, and the present invention is not limited by such speculation.
[0017] (2) Powder coating step FIG. 1 is a cross-sectional view for explaining a process in which a pipe inner surface coating apparatus 100 according to an embodiment of the present invention applies a powder coating to an inner surface of a pipe 1 having a straight portion and a socket to form a coating film.
[0018] In Figure 1, the axial direction of the pipe 1 is defined as the X-axis direction, the direction opposite to the gravity direction is defined as the positive Z-axis direction, and the direction orthogonal to both the X-axis direction and the Z-axis direction is defined as the Y-axis direction. Furthermore, it is assumed that the unillustrated spigot of the pipe 1 faces the positive X-axis direction, and the socket 2 of the pipe 1 faces the negative X-axis direction. The following description primarily explains the processes performed by the pipe inner surface coating apparatus 100, but also serves as an explanation of the pipe inner surface coating method for coating the inner surface of the pipe 1.
[0019] (2-1) Configuration of Pipe 1 The pipe 1 has a substantially cylindrical shape and includes a socket 2 and a straight portion 3, as shown in Figure 1. The pipe 1 is, for example, a ductile cast iron pipe mainly used as a water supply pipe. The inner surface of the pipe 1 needs to be coated to prevent rusting and adverse effects on water quality. The pipe inner surface coating apparatus 100 is an apparatus for coating the inner surface of the pipe 1.
[0020] On the negative X-axis direction side of the inner surface 21 of the socket 2, unevenness 211 for connecting the pipe 1 to another pipe is formed. The inner surface 21 includes a portion where the unevenness 211 is formed and an intermediate portion R1. The intermediate portion R1 is the portion between the portion where the unevenness 211 is formed and the inner surface 31 of the straight portion 3. The inner surface 31 of the straight portion 3 is formed to be substantially flat. The inner surface of the pipe 1 is composed of the inner surface 21 and the inner surface 31.
[0021] (2-2) Application and Curing Reaction of Powder Coating Material The pipe inner surface coating apparatus 100 includes a first coating mechanism 11 and a pipe holding unit 4. The first coating mechanism 11 includes a nozzle 12 and a robot arm 13. The nozzle 12 is provided at the tip of the robot arm 13 and discharges a powder coating material. An unillustrated control unit (hereinafter simply referred to as the control unit) included in the pipe inner surface coating apparatus 100 controls the operation of the robot arm 13, and can change the position of the nozzle 12 in the X-axis direction, Y-axis direction, and Z-axis direction.
[0022] The temperature of the inner surfaces 21 and 31 is set to a temperature at which the powder coating can cure. Preferably, this temperature is 160°C to 230°C, and more preferably 200°C ± 10°C. This allows the powder coating to cure smoothly. The temperature can be set by appropriately heating the tube 1, and it can be confirmed that the inner surfaces 21 and 31 have been set to the desired temperature by, for example, installing sensors on the inner surfaces 21 and 31.
[0023] The control unit controls the movement of the robot arm 13 to position the nozzle 12 within the inner surface 31 of the straight section 3. With the nozzle 12 positioned within the inner surface 31 of the straight section 3, the first coating mechanism 11 dispenses powder coating from the nozzle 12, thereby applying the powder coating to the inner surface 31 of the straight section 3 and the inner surface 21 of the receiving opening 2.
[0024] The pipe holder 4 rotates the pipe 1 by holding it so that its axis is horizontal and rotating it around the X-axis. While the pipe holder 4 rotates the pipe 1, the first coating mechanism 11 discharges powder paint from the nozzle 12. The control unit also moves the nozzle 12 by a predetermined distance in the X-axis direction while the first coating mechanism 11 discharges powder paint from the nozzle 12.
[0025] Here, as the nozzle 12 discharges the powder coating, the powder coating adheres to the intermediate portion R1 of the inner surface 21 that is close to the inner surface 31. Simultaneously with the adhesion of the powder coating, the powder coating melts and the hardening reaction begins, forming a coating film C1 of the powder coating on the inner surface 31 and the intermediate portion R1. The coating film C1 formed on the intermediate portion R1 is thinner than the coating film C1 formed on the inner surface 31.
[0026] The thickness of the coating film C1 in the intermediate portion R1 is preferably 100 μm to 300 μm. Furthermore, the thickness of the coating film C1 formed on the inner surface 31 is preferably 300 μm or more. Having the thickness of the coating film C1 within these ranges is preferable because it allows the curing reaction to proceed to a degree that ensures the quality of the coating film C1 described later.
[0027] After the first coating mechanism 11 has finished discharging the powder coating, the control unit moves the nozzle 12 in the negative X-axis direction to retract the nozzle 12 from the tube 1. After the powder coating has finished discharging, it is preferable to allow the tube 1 to cool in the atmosphere. At this time, the curing reaction of the coating film C1 is continued by residual heat.
[0028] The cooling time in the atmosphere is preferably 5 to 10 minutes, as this allows the curing reaction to progress to a degree that ensures the quality of the coating film C1. The temperature of the inner surfaces 21 and 31 after the cooling is preferably 150 to 200°C.
[0029] The aforementioned qualities include not adversely affecting water quality; having excellent rust prevention capabilities; having excellent adhesion to the inner surface 31 and the intermediate portion R1; being resistant to damage to the coating film; and even if localized damage occurs, this does not lead to a decrease in the adhesion of the coating film.
[0030] Examples of the aforementioned powder coatings include epoxy resin powder coatings. Epoxy resin powder coatings have advantages over mortar linings in terms of life cycle cost and have a low residual chlorine concentration consumption rate constant. Epoxy resin powder coatings contain epoxy resin, a curing agent, a pigment, and additives, but do not contain solvents. The epoxy resin is not particularly limited, but it is preferably an epoxy resin synthesized from bisphenol F and epichlorohydrin because of its excellent safety.
[0031] After application, the powder coating undergoes a curing reaction (curing reaction of epoxy resin) of the coating film C1 formed by the application, and the coating film is completed upon completion of the curing reaction.
[0032] The inventors investigated whether it was possible to ensure adhesion between the coating film, which includes the powder coating and the water coating, and the socket by applying an aqueous coating to the inner surface 31 and the intermediate portion R1 of the tube 1, which had been reheated after the completion of the curing reaction and allowed to return to room temperature. However, this method did not ensure sufficient adhesion. Therefore, the inventors diligently investigated the timing of applying the aqueous coating to the coating film formed by applying the powder coating, and succeeded in finding a process that can sufficiently ensure the aforementioned adhesion. The process will now be described.
[0033] (3) Water-based paint application process (3-1) Details of the process This process involves coating the coating film formed on the inner surface of the socket with a water-based paint while the coating film formed by applying powder coating to the inner surface of the socket is curing.
[0034] As explained in (2-2) above, the curing reaction of the powder coating starts simultaneously with the adhesion of the powder coating, and a coating film C1 of the powder coating is formed on the inner surface 31 and the intermediate portion R1. This coating film C1 is still in the process of curing. In this step, this coating film C1, which is in the process of curing, is painted with water-based paint. This ensures sufficient adhesion between the coating film, which includes the powder coating and water-based paint, and the socket.
[0035] Water-based paints are paints that contain resin, hardener, pigment, additives, and water, and are uniformly dispersed in water by the solvation (hydration) of hydrophilic groups in the resin and / or surfactants surrounding the resin. Examples of the resin include water-based acrylic resin, water-based polyester resin, water-based epoxy resin, water-based urethane resin, and silicone acrylic resin.
[0036] The water-based paint coating process is preferably carried out when the inner surface temperature of the pipe is 60°C or higher, more preferably between 60 and 90°C, and even more preferably between 70 and 90°C. This is because this temperature is preferable for continuing the curing reaction of the coating film formed by applying powder coating to the inner surface of the socket, and because the rapid evaporation of water contained in the water-based paint is preferable for the stable formation of the coating film. Based on Figure 1, the inner surface temperature of the pipe is the temperature of inner surface 21 and inner surface 31, and this temperature is approximately the same as the temperature of the coating film C1.
[0037] The inner surface temperature of the pipe can be raised to 60°C or higher after the cooling in the atmosphere described in (2-2) has been completed, by, for example, spraying water on the outer surface of the pipe 1, and / or cooling the pipe 1 in combination with spraying water and air blowing.
[0038] The time between the start of the powder coating process and the start of the water-based paint coating process is preferably 5 to 30 minutes in order to ensure the quality of the aforementioned coating film C1 and to maintain the state in which the coating film C1 is undergoing a curing reaction.
[0039] The water-based paint coating process can be carried out during the curing reaction of the paint film, for example, using the pipe interior coating apparatus 100 shown in Figure 2. As shown in Figure 2, the pipe interior coating apparatus 100 includes a second coating mechanism 14. The second coating mechanism 14 has a nozzle 15 and a robot arm 16. The nozzle 15 is provided at the tip of the robot arm 16 and dispenses liquid water-based paint. The control unit controls the movement of the robot arm 16 and can change the position of the nozzle 15 in the X-axis, Y-axis, and Z-axis directions.
[0040] The control unit controls the movement of the robot arm 16 to position the nozzle 15 within the inner surface 21 of the socket 2. With the nozzle 15 positioned within the inner surface 21 of the socket 2, the second painting mechanism 14 discharges water-based paint from the nozzle 15, thereby coating the inner surface 21 of the socket 2 with water-based paint. In other words, the second painting mechanism 14 coats the coating film C1 formed on the inner surface 21 by the powder coating process with water-based paint. As a result, a coating film C2 made of water-based paint is formed on a portion of the coating film C1 that is in the process of curing.
[0041] The thickness of coating film C2 is preferably 100 μm to 150 μm, from the viewpoint of ensuring sufficient adhesion with coating film C1 and guaranteeing the aforementioned quality for both coating film C1 and coating film C2.
[0042] While the pipe holder 4 rotates the pipe 1, the second painting mechanism 14 discharges water-based paint from the nozzle 15. Furthermore, while the control unit moves the nozzle 15 a predetermined distance in the X-axis direction, the second painting mechanism 14 discharges water-based paint from the nozzle 15.
[0043] The control unit moves the nozzle 15 in the X-axis direction within the region enclosed by the area where the irregularities 211 are formed on the inner surface 21 and the intermediate portion R1 of the inner surface 21. As a result, the coating film C2 is formed over the area where the irregularities 211 are formed on the inner surface 21 and the intermediate portion R1 of the inner surface 21.
[0044] Alternatively, the coating film C1 formed on the inner surface 31 side of the intermediate portion R1, that is, on the rising portion of the intermediate portion R1, may be manually painted with water-based paint using a brush to form a coating film C3. After painting by the second painting mechanism 14 is completed, the control unit moves the nozzle 15 in the negative X-axis direction to retract the nozzle 15 from the pipe 1. Note that the straight section does not need to be painted with water-based paint.
[0045] As described above, when powder coating is applied to the inner surfaces of the straight section and the socket in the powder coating process, the pipe 1 is heated, so the curing reaction of the powder coating starts immediately upon application, a coating film C1 is formed, and the curing reaction of the coating film C1 proceeds. If the coating film C1 is coated with water-based paint during the curing reaction of the coating film C1 to form a coating film C2, sufficient adhesion between the powder coating film C1 and the water-based paint film C2 can be ensured, as described above. As a result, sufficient adhesion between the coating film containing the powder coating and water-based paint and the socket can be ensured. At this time, since water-based paint is used instead of solvent-based paint which was used in conventional methods, VOCs can be reduced.
[0046] As mentioned above, the effect of reducing VOCs contributes to achieving, for example, Goal 12 of the United Nations' Sustainable Development Goals (SDGs), "Ensure sustainable consumption and production patterns."
[0047] (3-2) The state of the coating film of powder paint during the curing reaction. The coating film of the powder coating during the curing reaction is preferably in a gel-like or liquid state. Once the curing reaction of the powder coating is complete, a three-dimensional network structure is formed, and the coating film becomes solid. If the coating film is in a gel-like or liquid state, the curing reaction is not yet complete and is still ongoing. In this case, performing the water-based paint coating process ensures sufficient adhesion between the powder coating film and the water-based paint film. As a result, sufficient adhesion between the coating film containing the powder coating and water-based paint and the socket can be ensured.
[0048] The coating film of the powder coating undergoing the curing reaction is preferably in a touch-dry or semi-cured state as specified in JIS K 5600-1-1:1999.
[0049] JIS K 5600-1-1:1999 is a standard that deals with sampling methods and testing for paints and related products. In the section on "drying time," this standard states that the drying time from the time the paint is applied until it loses its tackiness and forms a paint film should be determined to assess the rate of drying. The evaluation method states that when the drying time specified in the product standard has elapsed, the degree of drying should be checked by one of the following methods. a) Touch dry: The painted surface is dry to the touch when you lightly touch the center with your fingertip and your fingertip does not get dirty. b) Semi-hardened: The paint surface is dry when you gently rub the center with your fingertip and no scratches are left on the surface. c) Curing and drying: When the center of the painted surface is firmly pinched between the thumb and index finger, no indentations from fingerprints are left on the painted surface, no movement of the paint film can be felt, and when the center of the painted surface is rapidly and repeatedly rubbed with the fingertip, no scratches are left on the painted surface.
[0050] If the coating film of the powder coating, which is undergoing the curing reaction, is in a touch-dry or semi-cured state, the curing reaction is considered to be ongoing. Therefore, by performing the water-based paint coating process in this case, sufficient adhesion between the powder coating film and the water-based paint film can be ensured. As a result, sufficient adhesion between the coating film, which includes the powder coating and the water-based paint, and the socket can be ensured.
[0051] It is preferable that the coating film of the powder coating undergoing the curing reaction has a gel fraction, as evaluated by a solvent friction test specified in ASTM D4752, that is below a predetermined standard value.
[0052] ASTM D4752 is a method for evaluating the curability of a coating film by rubbing the film a specific number of times with a cloth coated with methyl ethyl ketone while applying constant pressure. If the gel fraction of the powder coating film, which is undergoing the curing reaction, is below a predetermined standard value, it can be said that the curing reaction is continuing. In this case, by performing the water-based paint coating process, sufficient adhesion between the powder coating film and the water-based paint film can be ensured. As a result, sufficient adhesion between the coating film containing the powder coating and water-based paint and the socket can be ensured.
[0053] The aforementioned standard value may be set appropriately depending on the paint being evaluated. For example, the gel fraction is preferably less than 97% from the viewpoint of easily ensuring the adhesion.
[0054] The gel fraction can be determined by performing a solvent friction test as specified in ASTM D4752 using the method described in the examples below.
[0055] The present invention is not limited to the embodiments described above, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention.
[0056] [2. Summary] The present invention includes the following embodiments.
[0057] [1] A method for painting the inner surface of a pipe having a straight section and a socket, A powder coating step is performed to paint the inner surfaces of the straight portion and the socket by applying powder coating to the inner surfaces of the straight portion and the socket and curing the coating film formed thereon, A method for coating the inside surface of a pipe, comprising a step of coating the coating formed on the inner surface of the socket with a water-based paint during the curing reaction of the coating film.
[0058] [2] The pipe inner surface coating method according to [1], wherein the water-based paint coating step is performed when the inner surface temperature of the pipe is 60°C or higher.
[0059] [3] The method for coating the inner surface of a pipe according to [1] or [2], wherein the coating film of the powder coating during the curing reaction is gel-like or liquid.
[0060] [4] The method for coating the inside surface of a pipe according to any one of [1] to [3], wherein the coating film of the powder coating that is undergoing the curing reaction is in a state of touch-dry or semi-cured dryness as specified in JIS K 5600-1-1:1999.
[0061] [5] The method for coating the inside surface of a pipe according to any one of [1] to [4], wherein the coating film of the powder coating that is undergoing the curing reaction is in a state in which the gel fraction evaluated by a solvent friction test specified in ASTM D4752 is below a predetermined standard value. [Examples]
[0062] The following are specific embodiments of the present invention. However, the present invention is not limited to the embodiments described below.
[0063] [Example 1] <Applying water-based paint to a powder coating> (1) Test method A 150mm x 70mm blasted steel plate (test specimen) was heated to 200°C ± 10°C, and then epoxy resin powder coating was sprayed onto one surface of the specimen using an electrostatic coating gun, thereby coating the entire surface with the powder coating. The thickness of the powder coating film was 300 μm or more (powder coating process).
[0064] Next, the test specimens were allowed to cool in the atmosphere, and the surface temperature of the specimens was adjusted 600 seconds after the completion of the powder coating. Two test sections were established, one with a surface temperature of 60°C to 70°C (hereinafter referred to as Test Section 1) and another with a surface temperature of 80°C to 90°C (hereinafter referred to as Test Section 2). In both Test Section 1 and Test Section 2, n=10. The 600 seconds mentioned above will be referred to as the "coating interval" in Table 1, which will be described later.
[0065] Next, while maintaining the surface temperature, the water-based acrylic resin paint was sprayed onto the test piece using an air spray gun, thereby coating the entire surface with the water-based paint (water-based paint coating step). The film thickness of the water-based paint was approximately 100 μm. The above method corresponds to the present method.
[0066] After the application of the water-based paint was completed, the test specimens were allowed to air dry at room temperature for one week. Next, the test specimens were immersed in tap water, and 28 days after the start of immersion, a cross-cut test as specified in JIS K 5600 5-6 (1999) was performed. The cut interval was 2 mm.
[0067] As a control, a 150 mm x 70 mm blasted steel plate (test specimen) was used, which was allowed to cool for 24 hours in the atmosphere at room temperature after the powder coating was completed, allowing the surface temperature to reach room temperature, and then heated to a surface temperature of 60°C to 90°C. Subsequently, while maintaining a surface temperature of 60°C to 90°C, the entire powder coating film was coated with the water-based acrylic resin paint by spraying it onto the specimen using an air spray gun (water-based paint coating process). The film thickness of the water-based paint was approximately 100 μm. Other processes were the same as in test sections 1 and 2. The obtained specimen was subjected to the cross-cut test (test section 3).
[0068] Table 1 shows the painting conditions for test sections 1 to 3 described above.
[0069] [Table 1]
[0070] Figure 3 shows the results of the cross-cut test on the specimens from Test Section 1 and Test Section 2. Since n=10 in both Test Section 1 and Test Section 2, for example, "1-1" in the figure refers to the first sample from Test Section 1, and "2-1" refers to the first sample from Test Section 2.
[0071] Figure 4 shows the results of the cross-cut test on the specimens from test section 3. Although only the results for two specimens are shown in Figure 4, similar results were obtained for all 10 specimens.
[0072] Both Test Section 1 and Test Section 2 showed adhesion levels corresponding to Class 2 or lower on the six-level classification system described in JIS K 5600 5-6 (1999) 8.3.
[0073] Furthermore, "Category 2 or lower" is defined as follows: "Category 0: The edges of the cuts are perfectly smooth, and there is no peeling at any of the grid lines"; "Category 1: Small peeling of the coating at the intersections of the cuts. The affected area in the cross-cuts does not clearly exceed 5%"; "Category 2: The coating is peeling along the edges of the cuts and / or at the intersections. The affected area in the cross-cuts is clearly more than 5%, but does not exceed 15%."
[0074] On the other hand, in test section 3, as shown in Figure 4, the coating film was significantly peeled off. This corresponds to "Category 5: Any degree of peeling that cannot be classified even under Category 4" in the six-level classification described in JIS K 5600 5-6 (1999) 8.3. Unlike test sections 1 and 2, test section 3 failed to ensure adhesion between the powder coating film and the water-based coating film.
[0075] Thus, according to this method, even when water-based paint is used for coating the inside of the socket, sufficient adhesion between the powder coating film and the water-based paint film can be ensured. As a result, sufficient adhesion between the coating film, which includes the powder coating and water-based paint, and the socket can be ensured. Furthermore, this allows for the replacement of solvent-based paints, which were conventionally used for coating the inside of sockets, with water-based paints, thus providing an environmentally friendly method for coating the inside of pipes.
[0076] [Example 2] <Confirmation of the state of the coating film of powder paint undergoing curing reaction> A 150mm x 70mm blasted steel plate (test specimen) was heated to 200°C to 220°C, and then epoxy resin powder coating was sprayed onto one surface of the specimen using an electrostatic coating gun, thereby coating the entire surface with the epoxy resin powder coating. The thickness of the epoxy resin powder coating film was approximately 500 μm.
[0077] Next, the test specimens were allowed to cool in the atmosphere, and the surface temperature of the test specimens was set to 60°C to 80°C 600 seconds after the completion of the powder coating. At this point, the test specimens were subjected to the solvent friction test specified in ASTM D4752 (Test Section A). The powder coating film in Test Section A was a coating film in the process of curing.
[0078] As a control, the aforementioned test specimens were used, which were allowed to cool in the atmosphere at room temperature after the completion of the powder coating application, allowing the surface temperature to reach room temperature. These specimens were subjected to the solvent friction test specified in ASTM D4752 (Test Section B). The powder coating film in Test Section B was a coating film that had completed the curing reaction.
[0079] The results are shown in Figure 5. In the figure, the results for two test pieces are shown for each of Test Section A and Test Section B. The gel fraction of the powder coating film in Test Section A was 94% to 96%. In contrast, the gel fraction of the powder coating film in Test Section B was 97% or higher. Test Section A used a coating film that was undergoing curing, while Test Section B used a coating film that had completed curing. Since the gel fraction of the coating film undergoing curing is lower than that of the coating film that has completed curing, it is thought that the coating film undergoing curing still contains functional groups that have not yet been used in the curing reaction. Example 1 was obtained by coating the test piece from Test Section A of Example 2 with water-based paint, so it is thought that the powder coating film and the water-based paint film showed sufficient adhesion, and as a result showed good results in the cross-cut test.
[0080] In the example shown in Figure 5, the standard value for evaluating pass / fail status in the solvent friction test is set at 97%, but this standard value can be appropriately changed depending on the paint being evaluated. [Explanation of Symbols]
[0081] 1 tube 2 socket 21, 31 Inner self 3 Straight section 11. First Painting Mechanism 14. Second Painting Mechanism 100 Pipe Inner Surface Coating Apparatus C1 and C2 coatings
Claims
1. A method for painting the inner surface of a pipe having a straight section and a socket, A powder coating step is performed to paint the inner surfaces of the straight portion and the socket by applying powder coating to the inner surfaces of the straight portion and the socket and curing the coating film formed thereon, The process includes a step of applying a water-based paint to the coating film formed on the inner surface of the socket during the curing reaction of the coating film, A method for coating the inside surface of a pipe, wherein the coating film of the powder coating undergoing the curing reaction has a gel fraction of less than 97%, as evaluated by a solvent friction test specified in ASTM D4752.
2. The method for coating the inner surface of a pipe according to claim 1, wherein the water-based paint coating step is performed when the inner surface temperature of the pipe is 60°C or higher.
3. The method for coating the inner surface of a pipe according to claim 1, wherein the coating film of the powder coating during the curing reaction is in a gel-like or liquid state.
4. The method for coating the inside surface of a pipe according to claim 1, wherein the coating film of the powder coating that is undergoing the curing reaction is in a touch-dry or semi-cured state as defined in JIS K 5600-1-1:1999.
Citation Information
Patent Citations
Cast iron pipe applied with water-based coating on socket inner face, and method of coating the same
JP2013204689A
Cast iron pipe having coated film at inner surface of socket and its coating method
JP2019158113A
Metal pipe and coating method for socket inner surface of metal pipe
JP2022072310A