Alkali-resistant spherical silica slurry for package substrates and method for manufacturing the same
By blending micron-sized and submicron-sized spherical silica and using silane coupling agents, the silica slurry achieves enhanced alkali resistance and reduced surface roughness, addressing the alkali resistance issues in existing silica slurries for package substrates.
Patent Information
- Application Number
- JP2025501326
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-12-22
- Filing Date
- 2024-10-21
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-10-21
AI Technical Summary
Existing silica slurries for package substrates lack sufficient alkali resistance, leading to increased surface roughness after Desmear treatment, which compromises long-term interlayer insulation reliability.
A method involving the blending of micron-sized and submicron-sized spherical silica, followed by wet and secondary modifications using silane coupling agents and non-polar short-chain silane coupling agents, to enhance alkali resistance and dispersibility, resulting in a stable and fluid silica slurry.
The method improves alkali resistance and reduces surface roughness, ensuring better interlayer insulation reliability and suitability for mass production.
Smart Images

Figure 0007955470000001 
Figure 0007955470000002
Abstract
Description
[Technical Field]
[0001] This application claims priority to a Chinese patent application filed with the China National Intellectual Property Office on December 22, 2023, with application number CN202311782512.3, titled "Alkali-resistant spherical silica slurry for package substrates and method for manufacturing the same," the entire contents of which are incorporated into this application by reference.
[0002] This application belongs to the technical field of inorganic fillers and relates to alkali-resistant spherical silica slurry for package substrates and a method for producing the same. [Background technology]
[0003] Package substrates, also known as IC substrates, are crucial materials for connecting chips to the PCB motherboard in IC packages, and have now replaced traditional lead frames in the mid-to-high-end packaging sector. The main functions of IC substrates include protecting the chip, providing secure support, and heat dissipation. IC substrates are similar to PCBs in terms of structure and function, and have evolved from HDI substrates, but the technical hurdles for IC substrates are far higher than those for HDI or ordinary PCBs. They feature high density, high precision, a large number of pins, high performance, miniaturization, and thinning, and have higher requirements for various technical parameters such as line width / line spacing.
[0004] Package substrates have high requirements for CTE (coefficient of thermal expansion) and are required to have high fluidity, as well as good bonding strength between filler and resin, good alkali resistance, and low surface roughness after Desmear (removal of glue residue during drilling). If alkali resistance is poor, the roughness after Desmear will be large, which may cause potential problems with long-term interlayer insulation reliability.
[0005] Patent Document 1 discloses a silica slurry composition obtained by coating the surface of silica fine powder with nanoscale silica and dispersing it in an organic solvent. This product is used in laminates and has excellent dispersibility and fluidity. However, adding nanospherical silicon dioxide does not improve alkali resistance.
[0006] Patent Document 2 discloses a slurry composition, a technique for producing a silica slurry composition by coating the surface of silica with a single layer of weakly polar or nonpolar monomer using a plasma modification method and dispersing it in an organic solvent. This composition has good dispersibility, fluidity, and dielectric properties, as well as good settling stability due to the uniform coating of the modifier. However, the plasma modification used in this method is difficult to manufacture industrially. [Prior art documents] [Patent Documents]
[0007] [Patent Document 1] Chinese Patent No. 106700132 Specification [Patent Document 2] Chinese Patent Application Publication No. 109021292 Specification [Overview of the project] [Problems that the invention aims to solve]
[0008] The object of the present invention is to provide an alkali-resistant spherical silica slurry for package substrates and a method for producing the same. [Means for solving the problem]
[0009] The following are technical proposals for achieving the objectives of this invention. A method for manufacturing alkali-resistant spherical silica slurry for package substrates is provided, and the specific steps are as follows. (1) Raw material composition: D50=0.3~0.8μm, D100≦5.0μm, SSA=4.0~12.0m2 Submicron spherical silica at / g, with D50 = 1.0~3.0 μm, D100 ≤ 5.0 μm, SSA = 0.5~4.0 μm 2 Micron-sized spherical silica ( / g) is mixed in a mass ratio of 1:3 to 3:1, with D50 = 0.4 to 2.0 μm, D100 ≤ 5.0 μm, and SSA = 1.5 to 9.0 μm. 2 Obtain spherical silica A in a quantity of / g. (2) Wet modification: The spherical silica A and water are uniformly mixed in a mass ratio of 3:7 to 6:4 and pre-dispersed to obtain a submicron slurry, then a modifier is added, and moisture is added. formula change After conducting the quality check, Wet method The modified slurry is dried and modified at 120-300°C until the moisture content is 0.3% or less, then kept warm at 60-120°C, and finally the material after warming is heated until its particle size matches that of spherical silica A. Crushing Then, spherical silica B is obtained after wet modification, and the modifier is selected from epoxy group silane coupling agents, anilino group silane coupling agents, isocyanate group silane coupling agents, or ureido group silane coupling agents. (3) Secondary modification: The spherical silica B obtained after the wet modification is subjected to secondary modification using a nonpolar short-chain silane coupling agent to obtain the spherical silica C obtained after secondary modification, and the nonpolar short-chain silane coupling agent is a short-chain alkylsilane coupling agent or a silazane. (4) Slurry formation: The spherical silica C after secondary modification is pre-dispersed in an organic solvent while stirring, then dispersed using a disperser, and subsequently, particles larger than a predetermined particle size are removed by classification to obtain an alkali-resistant spherical silica slurry for package substrates. The organic solvent is acetone, butanone, methyl isobutyl ketone (MIBK), or cyclohexanone.
[0010] Preferably, in step (2), the pre-dispersion is performed using a sand mill, and the temperature of the pre-dispersion is 50 to 90°C.
[0011] Preferably, in step (2), the time for keeping warm is 20 to 60 minutes.
[0012] Preferably, in step (2), a jet mill is used to perform the said Crushing , and the pressure of the said Crushing is 1.0 MPa or higher.
[0013] Preferably, in step (2), the mass ratio of the modifier to spherical silica A is 0.1-2.0:100.
[0014] Preferably, in step (2), the epoxy group-containing silane coupling agent is 3-glycidoxypropyltrimethoxysilane, the anilino group-containing silane coupling agent is N-phenyl-3-aminopropyltrimethoxysilane, the isocyanate group-containing silane coupling agent is 3-isocyanatopropyltriethoxysilane, and the ureido group-containing silane coupling agent is 3-ureidopropyltriethoxysilane.
[0015] Preferably, in step (3), the short-chain alkyl silane coupling agent is selected from methyltrimethoxysilane, methyltriethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, dimethyldimethoxysilane or trimethylmethoxysilane, and the silazane is hexamethyldisilazane or tetramethyldisilazane.
[0016] Preferably, in step (3), the mass ratio of the non-polar short-chain silane coupling agent to spherical silica B is 0.1-1.0:100.
[0017] Preferably, in step (3), the apparatus used for the secondary modification is a high-speed stirrer, the temperature in the secondary modification is 80-150°C, and the time in the secondary modification is 10-40 min.
[0018] Preferably, in step (4), the mass ratio of the spherical silica C to the organic solvent is 25:75-50:50.
[0019] Preferably, in step (4), a high-pressure homogenizer is used as the disperser, the dispersion pressure is 10,000 psi to 20,000 psi, the apparatus used for classification is a wet vibrating screen, the mesh size of the wet vibrating screen is 10 μm or less, and the apparatus used for drying modification is a flash dryer.
[0020] This is an alkali-resistant spherical silica slurry for package substrates, manufactured by the manufacturing method described in the above technical proposal. [Effects of the Invention]
[0021] Compared to conventional technology, the present invention offers the following advantages. (1) In the method according to the present invention, micron-sized spherical silica with a small specific surface area and narrow particle size distribution is blended with submicron-sized spherical silica. Because the specific surface area of the micron-sized spherical silica is small, there is less interfacial contact with the resin during use. Furthermore, by combining spheres of different sizes, alkali resistance can be improved, and the surface roughness after Desmear treatment is also reduced.
[0022] (2) In the method according to the present invention, wet modification is performed using a polar silane coupling agent to ensure uniform coating of the modifier, and then secondary modification is performed using a short-chain silane. Due to the presence of polar groups, the compatibility between the filler (silica) and the resin is improved, and due to the presence of non-polar groups, the dispersibility of the filler (silica) is improved. As a result, good alkali resistance is observed during use, and the surface roughness after Desmear treatment is reduced. Furthermore, by utilizing the synergistic effect of the silane coupling agent and the non-polar short-chain silane, the stability and fluidity of the product can be further improved.
[0023] (3) The spherical silica slurry product manufactured in this application has good stability, and when applied to a package substrate, it has good alkali resistance, low surface roughness after Desmear treatment, and the manufacturing process is easy to control, resulting in good product stability and suitability for mass production. [Modes for carrying out the invention]
[0024] The present application will be described in more detail below, incorporating specific examples. The methods for measuring D50, D100, pH, TGA (thermogravimetric analysis) weight loss, viscosity, and flow time of silica fine powder in the following examples and comparative examples are as follows. (1) Measurement of D50 and D100: Measurements are taken using the LS13320 laser particle size distribution analyzer from Beckman Coulter, Inc. in the United States. (2) Settling stability: Pour the slurry into a 100 ml stoppered test tube up to the 100 ml mark, seal it, and store it at room temperature. After one month, observe the layer separation of the slurry, record the height of the separated clear liquid, and invert the test tube to observe whether there is any sediment at the bottom. The less layer separation and the less sediment at the bottom, the better the stability of the product. (3) Measurement of melt viscosity: When the product is used in the formulation of a carrier substrate, the rheology curve of the resin powder of the semi-cured sheet is measured in the range of 80°C to 190°C to determine the minimum melt viscosity (η). A lower minimum melt viscosity indicates better fluidity.
[0025] [Example 1] (1) Raw material composition D50=0.50μm, D100=2.6μm, SSA=6.6m 2 Submicron spherical silica at / g, with D50=1.5μm, D100=2.2μm, SSA=2.6m 2 Micron-sized spherical silica particles were mixed in a mass ratio of 1:1, resulting in D50=0.93μm, D100=2.6μm, and SSA=4.6m. 2 Spherical silica A was obtained in a quantity of / g. (2) Wet modification After uniformly mixing spherical silica A and deionized water in a mass ratio of 1:1, the mixture is sent to a sand mill for pre-dispersion, the pre-dispersion temperature is controlled to 80°C, and after uniform dispersion, a submicron slurry is obtained. Subsequently, 0.6% of N-phenyl-3-aminopropyltrimethoxysilane KBM-573 (Shin-Etsu Chemical) relative to the mass of spherical silica A is added, and the mixture is then humidified. formula change After conducting the quality check, Wet methodThe modified slurry is sent to a flash dryer for drying and modification, with a blast temperature of 250°C. After drying until the moisture content is below 0.3%, it is sent to a collector for heat preservation at 110°C for 30 minutes. Next, the material after heat preservation is processed by an air flow pulverizer Crushing and Crushing setting the pressure to 1.0 MPa, to obtain wet-modified spherical silica B. (3) Secondary modification Spherical silica B is placed in a high-speed stirrer, and methyltrimethoxysilane KBM-13 (Shin-Etsu Chemical) is added simultaneously. Modification is performed at 100°C for 20 minutes to obtain secondary-modified spherical silica C. The mass ratio of methyltrimethoxysilane KBM-13 to spherical silica B is 0.3:100. (4) Slurry preparation Spherical silica C and acetone (an organic solvent) are placed in a stirring tank at a mass ratio of 7:3 for preliminary dispersion. Then, dispersion is performed using a homogenizer under a pressure condition of 10,000 psi. Next, large particles are sieved out and removed using a sieve mesh with an aperture of 5 μm, to obtain an alkali-resistant spherical silica slurry for package substrates.
[0026] [Example 2] (1) Raw material blending Submicron spherical silica with D50=0.78 μm, D100=3.5 μm, and SSA=5.2 m 2 / g is mixed with micron spherical silica with D50=2.0 μm, D100=3.5 μm, and SSA=1.8 m 2 / g at a mass ratio of 1:2, to obtain spherical silica A with D50=1.2 μm, D100=3.5 μm, and SSA=4.8 m 2 / g. (2) Wet modification Spherical silica A and deionized water are uniformly mixed at a mass ratio of 6:4, then sent to a sand mill for preliminary dispersion. The temperature of preliminary dispersion is controlled at 60°C. After uniform dispersion, a submicron slurry is obtained. Then, 0.8% (relative to the mass of spherical silica A) of 3-glycidoxypropyltrimethoxysilane KBM-403 (Shin-Etsu Chemical) is added for wet formula change modification, and then Wet methodThe modified slurry is sent to a flash dryer for drying and modification at an air temperature of 150°C until the moisture content is 0.3% or less. Then it is sent to a collector for heating at a temperature of 100°C for 60 minutes. Next, the heated material is processed in an air jet pulverizer. Crushing death, Crushing By setting the pressure to 1.0 MPa, wet-modified spherical silica B was obtained. (3) Secondary modification Spherical silica B was placed in a high-speed stirrer, and dimethyldimethoxysilane KBM-22 (Shin-Etsu Chemical) was added simultaneously. The mixture was modified at 100°C for 20 minutes to obtain spherical silica C after secondary modification. The mass ratio of dimethyldimethoxysilane KBM-22 to spherical silica B was 0.3:100. (4) Slurry formation Spherical silica C and the organic solvent butanone were placed in a stirring tank in a mass ratio of 7:3 for preliminary dispersion. Then, the mixture was dispersed under a pressure of 10,000 psi using a homogenizer. Next, large particles were sieved off using a sieve with a pore size of 10 μm to obtain an alkali-resistant spherical silica slurry for package substrates.
[0027] [Example 3] (1) Raw material composition D50=0.36μm, D100=0.87μm, SSA=11.6m 2 Submicron spherical silica at / g, with D50=1.1μm, D100=2.0μm, SSA=3.2m 2 Micron-sized spherical silica particles were mixed in a mass ratio of 1:2, resulting in D50=0.59μm, D100=2.0μm, and SSA=6.0m². 2 Spherical silica A was obtained in a quantity of / g. (2) Wet modification After uniformly mixing spherical silica A and deionized water in a mass ratio of 4:6, the mixture is sent to a sand mill for pre-dispersion. The pre-dispersion temperature is controlled to 60°C, and after uniform dispersion, a submicron slurry is obtained. Subsequently, 2.0% of 3-ureidopropyltriethoxysilane KBE-585 (Shin-Etsu Chemical) relative to the mass of spherical silica A is added, and the mixture is then humidified. formula change After conducting the quality check, Wet methodThe modified slurry is sent to a flash dryer for drying and modification at an air temperature of 220°C until the moisture content is 0.3% or less. Then it is sent to a collector for heating at a temperature of 120°C for 30 minutes. Next, the heated material is processed in an air jet pulverizer. Crushing death, Crushing By setting the pressure to 1.0 MPa, wet-modified spherical silica B was obtained. (3) Secondary modification Spherical silica B was placed in a high-speed stirrer, and hexamethyldisilazane SZ-13 (Shin-Etsu Chemical) was added simultaneously. The mixture was modified at 110°C for 20 minutes to obtain spherical silica C after secondary modification. The mass ratio of hexamethyldisilazane SZ-13 to spherical silica B was 0.8:100. (4) Slurry formation Spherical silica C and the organic solvent butanone were placed in a stirring tank in a mass ratio of 7:3 for preliminary dispersion. After dispersion under a pressure of 10,000 psi using a homogenizer, large particles were sieved off using a sieve with a pore size of 5 μm to obtain an alkali-resistant spherical silica slurry for package substrates.
[0028] [Example 4] (1) Raw material composition D50=0.50μm, D100=2.6μm, SSA=6.6m 2 Submicron spherical silica at / g, with D50=1.5μm, D100=2.2μm, SSA=2.6m 2 Micron-sized spherical silica particles were mixed in a mass ratio of 1:1, resulting in D50=0.93μm, D100=2.6μm, and SSA=4.6m. 2 Spherical silica A was obtained in a quantity of / g. (2) Wet modification After uniformly mixing spherical silica A and deionized water in a mass ratio of 3:7, the mixture is sent to a sand mill for pre-dispersion. The pre-dispersion temperature is controlled to 70°C, and after uniform dispersion, a submicron slurry is obtained. Subsequently, 1.0% of 3-isocyanatopropyltriethoxysilane KBE-9007N (Shin-Etsu Chemical) relative to the mass of spherical silica A is added, and then... formula change Conduct a quality check, Wet method After completing the modification, next Wet methodThe modified slurry is sent to a flash dryer for drying and modification at an air temperature of 180°C until the moisture content is 0.3% or less. Then it is sent to a collector for heating at a temperature of 100°C for 60 minutes. Next, the heated material is processed in an air jet pulverizer. Crushing death, Crushing By setting the pressure to 1.0 MPa, wet-modified spherical silica B was obtained. (3) Secondary modification Spherical silica B was placed in a high-speed stirrer, and methyltrimethoxysilane KBM-13 (Shin-Etsu Chemical) was added simultaneously. The mixture was modified at 100°C for 20 minutes to obtain spherical silica C after secondary modification. The mass ratio of methyltrimethoxysilane KBM-13 to spherical silica B was 0.5:100. (4) Slurry formation Spherical silica C and the organic solvent methyl isobutyl ketone (MIBK) were placed in a stirring tank in a mass ratio of 7:3 for preliminary dispersion. After dispersion under a pressure of 10,000 psi using a homogenizer, large particles were sieved off using a sieve with a pore size of 5 μm to obtain an alkali-resistant spherical silica slurry for package substrates.
[0029] [Comparative Example 1] This comparative example is substantially the same as Example 1, but differs in that dry modification is employed in step (2). Specifically, spherical silica A was placed in a high-speed mixer and stirred, and at the same time, 0.6% of KBM-573 (Shin-Etsu Chemical), an anilino group silane coupling agent, was added, and modification was carried out at 110°C for 30 minutes to obtain spherical silica B.
[0030] [Comparative Example 2] This comparative example is substantially the same as Example 1, but differs in that micron-sized spherical silica is not added in step (1).
[0031] [Comparative Example 3] This comparative example is substantially the same as Example 1, except that the silane coupling agent in step (2) is vinyltrimethoxysilane KBM-1003.
[0032] [Comparative Example 4] This comparative example is substantially the same as Example 1, but differs in that step (3) is omitted.
[0033] [Comparative Example 5] This comparative example is substantially the same as Example 1, except that the silane coupling agent in step (3) is decyltrimethoxysilane KBM-3103 (Shin-Etsu Chemical).
[0034] The results of detecting the stability of silica slurries produced by the examples and comparative examples are shown in Table 1.
[0035] Sedimentation results of silica slurries produced by the examples and comparative examples. [Table 1]
[0036] As can be seen from Table 1, after leaving Examples 1-4 for one month, the height of the layer separation was low and there was no sediment at the bottom even when inverted, indicating that the slurry products of the Examples have good stability. Comparative Example 1 differs from Example 1 in the modification process in step (2). Example 1 uses wet modification, while Comparative Example 1 uses dry modification. Comparative Example 1 has a higher height of layer separation and sediment at the bottom, indicating that wet modification helps improve sedimentation stability. Comparative Example 2 does not contain micron-spherical silica added to the raw material compared to Example 1. Comparative Example 2 has a slightly lower height of layer separation and no sediment at the bottom, and the slurry product also has good stability. This indicates that although the addition of micron-spherical silica is detrimental to sedimentation stability, its effect is not significant. Comparative Example 3 differs from Example 1 in the type of modifier used in step (2). However, the layer separation height of Comparative Example 3 is close to that of Example 1, there is no sediment at the bottom, and the stability of the slurry product is still good. This indicates that the type of modifier used in step (2) does not have a significant effect on the stability of the slurry product. Comparative Example 4 does not include step (3) compared to Example 1, but the layer separation height of the slurry product is high, and there is sediment at the bottom. This indicates that step (3) can improve sedimentation stability. Comparative Example 5 differs from Example 1 in that it uses a different modifier, and a long-chain alkylsilane KBM-3103 is used. The layer separation height of the slurry product in Comparative Example 5 is high, and there is sediment at the bottom. This indicates that the chain length of the alkylsilane in step (3) affects the stability of the product.
[0037] SC2050MT*, a slurry product from an advanced overseas competitor, and the slurry products of the examples and comparative examples were used in the formulation of BT resin package substrates. The filler ratio was set to 65%, and the melt viscosity of the product and the weight loss rate of the sheet material after desmearing were measured. It was shown that a smaller weight loss rate after desmearing indicated less surface roughness of the sheet material after desmearing and better alkali resistance. The melt viscosity of the product and the weight loss rate of the sheet material after desmearing are shown in Table 2.
[0038] Melt viscosity of package substrates manufactured by the examples and comparative examples, and weight loss rate of the plate material after desmearing. [Table 2]
[0039] As can be seen from Table 2, the minimum melt viscosity for all of the examples is SC2050MT. * It is close to the weight reduction rate after Desmear is SC2050MT * This is lower than the above, indicating that the fluidity of the product of this application is close to that of overseas competitors' products, and that its alkali resistance is better than that of overseas competitors' products. Comparative Example 1 differs from Example 1 in the modification process in step (2). Example 1 employs wet modification, while Comparative Example 1 employs dry modification. Comparative Example 1 has a larger weight loss rate and higher melt viscosity after Desmear, indicating that the wet modification adopted in this application has good alkali resistance and low melt viscosity. Comparative Example 1 does not have micron-spherical silica added to the raw material compared to Example 2. Comparative Example 2 has a larger weight loss rate and higher melt viscosity after Desmear, indicating that the addition of micron-spherical silica can improve alkali resistance and melt viscosity. Comparative Example 3 differs from Example 1 in the type of modifier in step (2). Comparative Example 3 has a larger weight loss rate and higher melt viscosity after Desmear, indicating that the type of modifier in step (2) affects the alkali resistance and melt viscosity of the slurry product. Comparative Example 4 does not include step (3) compared to Example 1, but the weight loss rate after desmearing of the product in Comparative Example 4 is larger and the melt viscosity is also larger, indicating that step (3) can improve alkali resistance and melt viscosity. Comparative Example 5 uses a different modifier compared to Example 1, and in Comparative Example 5 a long-chain alkylsilane KBM-3103 is used, but the weight loss rate after desmearing of the slurry product in Comparative Example 5 is slightly larger and the melt viscosity is also larger, indicating that the chain length of the alkylsilane in step (3) affects the alkali resistance and melt viscosity of the product.
[0040] While the above embodiments provide a detailed description of this application, they represent only a portion of the embodiments and do not encompass all of them. Based on these embodiments, people can derive other embodiments without requiring creativity, and all of these embodiments fall within the scope of protection of the present invention.
Claims
1. A method for manufacturing alkali-resistant spherical silica slurry for package substrates, comprising the following steps: (1) Raw material composition: D50=0.3~0.8μm, D100≦5.0μm, SSA=4.0~12.0m 2 Submicron spherical silica at a density of / g, with D50 = 1.0–3.0 μm, D100 ≤ 5.0 μm, and SSA = 0.5–4.0 μm. 2 Mix micron-sized spherical silica at a mass ratio of 1:3 to 3:1, with D50 = 0.4 to 2.0 μm, D100 ≤ 5.0 μm, and SSA = 1.5 to 9.0 μm. 2 Obtain spherical silica A in / g, (2) Wet modification: The spherical silica A and water are uniformly mixed in a mass ratio of 3:7 to 6:4 and pre-dispersed to obtain a submicron slurry. Next, a modifier is added and wet modification is performed. Then, the wet-modified slurry is dried at 120 to 300°C until the moisture content is 0.3% or less, and then kept warm at 60 to 120°C. Finally, the material after warming is pulverized until the particle size matches that of spherical silica A to obtain wet-modified spherical silica B. The modifier is selected from epoxy-based silane coupling agents, anilino-based silane coupling agents, isocyanate-based silane coupling agents, or ureido-based silane coupling agents. (3) Secondary modification: The spherical silica B, which has undergone the wet modification, is subjected to secondary modification using a nonpolar short-chain silane coupling agent to obtain the spherical silica C that has undergone secondary modification. The nonpolar short-chain silane coupling agent is a short-chain alkylsilane coupling agent or a silazane. The short-chain alkylsilane coupling agent is selected from methyltrimethoxysilane, methyltriethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, dimethyldimethoxysilane, or trimethylmethoxysilane. (4) Slurry formation: The spherical silica C, after secondary modification, is pre-dispersed in an organic solvent while stirring, then dispersed using a disperser, and subsequently, particles larger than a predetermined particle size are removed by classification to obtain an alkali-resistant spherical silica slurry for package substrates. The organic solvent is acetone, butanone, methyl isobutyl ketone, or cyclohexanone. A manufacturing method characterized by including the following.
2. The manufacturing method according to claim 1, characterized in that in step (2), the preliminary dispersion is performed using a sand mill, the temperature of the preliminary dispersion is 50 to 90°C, the holding time is 20 to 60 minutes, the pulverization is performed using an air jet pulverizer, and the pulverization pressure is 1.0 MPa or higher.
3. The manufacturing method according to claim 1, characterized in that in step (2), the mass ratio of the modifier to spherical silica A is 0.1 to 2.0:
100.
4. The manufacturing method according to claim 1, characterized in that in step (2), the epoxy group silane coupling agent is 3-glycidylpropyltrimethoxysilane, the anilino group silane coupling agent is N-phenyl-3-aminopropyltrimethoxysilane, the isocyanate group silane coupling agent is 3-isocyanatopropyltriethoxysilane, and the ureido group silane coupling agent is 3-ureidopropyltriethoxysilane.
5. The manufacturing method according to claim 1, characterized in that the silazane is hexamethyldisilazane or tetramethyldisilazane.
6. The manufacturing method according to claim 1, characterized in that in step (3), the mass ratio of the nonpolar short-chain silane coupling agent to spherical silica B is 0.1 to 1.0:
100.
7. The manufacturing method according to claim 1, characterized in that, in step (3), the apparatus used for the secondary modification is a high-speed agitator, the temperature during the secondary modification is 80 to 150°C, and the time during the secondary modification is 10 to 40 minutes.
8. The manufacturing method according to claim 1, characterized in that in step (4), the mass ratio of the spherical silica C to the organic solvent is 25:75 to 50:
50.
9. In step (4), a high-pressure homogenizer is used as the disperser, the dispersion pressure is 10,000 psi to 20,000 psi, the device used for classification is a wet vibrating screen, and the mesh size of the sieve of the wet vibrating screen is 10 μm or less. The manufacturing method according to claim 1, characterized in that, in step (2), the apparatus used for drying and modifying is a flash dryer.
Citation Information
Patent Citations
Silicon dioxide slurry composition as well as preparation method and application thereof
CN106700132A
Slurry composition, thermosetting resin composition, prepreg, laminated board, and printed circuit board
CN109021292A
High-strength surface modified silica powder for vinyl silica gel and preparation method of high-strength surface modified silica powder
CN115477859A
Silica particle and method for producing the same
JP2015013788A
Surface-modified silica powder and slurry composition
JP2015189638A