Manufacturing method for substrate laminates
The method addresses contamination and foreign matter issues in substrate laminates by using a surface protection layer and specific resin layers for precise lamination and bonding, enhancing the manufacturing process's reliability and quality.
Patent Information
- Application Number
- JP2025502747
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-02-20
- Filing Date
- 2024-02-20
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-02-20
AI Technical Summary
The challenges of manufacturing substrate laminates include contamination, scratches, and foreign matter inclusion during the lamination process of semiconductor chips, especially when using dicing tapes and handling semiconductor chips.
A method involving a surface protection layer on the second laminate, dicing with a tape attached to this layer, peeling and laminating chips with the protection layer intact, followed by cleaning and removal steps to suppress contamination and foreign matter, and using a resin layer with specific functional groups for temporary fixing and bonding.
This method effectively suppresses defects, contamination, and foreign matter inclusion in substrate laminates, ensuring precise alignment and strong bonding between layers.
Smart Images

Figure 0007955473000009 
Figure 0007955473000010 
Figure 0007955473000011
Abstract
Description
[Technical Field]
[0001] This disclosure relates to a method for manufacturing a substrate laminate. [Background technology]
[0002] As electronic devices become smaller, lighter, and more powerful, there is a growing demand for higher integration of semiconductor chips and other components. However, as circuits become more miniaturized, it becomes increasingly difficult to meet these demands. Therefore, in recent years, a method has been proposed to achieve high integration by stacking multiple semiconductor substrates (wafers) and semiconductor chips vertically (in the thickness direction) to create a multilayer three-dimensional structure. One method for stacking and joining semiconductor substrates (wafers), semiconductor chips, etc. (hereinafter sometimes referred to as "semiconductor substrates, etc.") is to join them by soldering between the electrodes of the stacked semiconductor substrates, etc. However, as circuits become more miniaturized, problems arise such as fusion of adjacent solders, cracking due to alloying, and malfunction of devices due to heat generated from the solder.
[0003] On the other hand, methods have been proposed for directly joining electrodes of stacked semiconductor substrates without using solder, and for using adhesives (for example, Patent Documents 1 to 3). Furthermore, methods for manufacturing laminates that bond substrates such as semiconductor substrates with high bonding strength via a resin layer with a low coefficient of thermal expansion have been proposed (for example, Patent Documents 4 and 5).
[0004] Patent document 1: Japanese Patent Application Laid-Open No. 4-132258 Patent Document 2: Japanese Unexamined Patent Publication No. 2010-226060 Patent Document 3: Japanese Unexamined Patent Publication No. 2016-47895 Patent Document 4: Japanese Unexamined Patent Publication No. 2021-182621 Patent Document 5: International Publication No. 2022 / 054839 [Overview of the Initiative] [Problems that the invention aims to solve]
[0005] For example, when a substrate laminate is produced by laminating semiconductor chips obtained by dicing on a semiconductor substrate or the like, contamination of the semiconductor chips due to contact with a dicing tape, scratches on the semiconductor chips when the semiconductor chips are peeled from the dicing tape, contamination of the semiconductor chips due to contact with an apparatus when handling the semiconductor chips, and voids due to mixing of foreign matters such as particles when laminating the semiconductor chips are likely to occur.
[0006] One aspect of the present disclosure has been made in view of the above problem, and an object of the present disclosure is to provide a method for manufacturing a substrate laminate, in which scratches, contamination, and mixing of foreign matters on a chip are suppressed when a chip including a substrate obtained by dicing is laminated on another substrate to manufacture a substrate laminate. [Means for Solving the Problems]
[0007] Specific means for solving the above problems are as follows. <1> A laminate preparation step of preparing a first laminate in which a first surface layer, a first substrate, and a first back surface layer are laminated in this order, and a second laminate in which a second surface layer, a second substrate, and a second back surface layer are laminated in this order; A surface protection step of providing a surface protection layer on the second surface layer of the second laminate; A dicing step of attaching a dicing tape to the surface protection layer side of the second laminate provided with the surface protection layer, performing dicing, and singulating the second laminate into chips with a surface protection layer including the divided second laminate and the surface protection layer; A lamination step of peeling the chip with a surface protection layer from the dicing tape, and laminating the chip with a surface protection layer on the first laminate such that the first surface layer and the second back surface layer are in contact with each other; A cleaning and removing step of cleaning the laminated first laminate and the chip with a surface protection layer and removing the surface protection layer; A bonding step of heating the first laminate and the chip of the second laminate from which the surface protection layer has been removed to obtain a substrate laminate in which the chip of the second laminate is bonded onto the first laminate; A method for manufacturing a substrate laminate containing [the specified material]. <2> The first laminate comprises a first electrode exposed from the first surface layer and the first back layer, The second laminate comprises a second electrode exposed from the second surface layer and the second back layer, In the lamination process, the chip with the surface protective layer is laminated on the first laminate such that the first electrode exposed from the first surface layer and the second electrode exposed from the second back surface layer are in contact with each other. <1> A method for manufacturing a substrate laminate as described above. <3> The aforementioned first surface layer is an inorganic material layer formed of an inorganic material, The second back layer is a resin layer formed of resin, The lamination process includes a temporary fixing step of temporarily fixing the laminated first laminate and the chip with the surface protection layer at a first temperature. The bonding step is a step of heating the temporarily fixed first laminate and the chip of the second laminate at a second temperature higher than the first temperature. <1> or <2> A method for manufacturing a substrate laminate as described above. <4> After the temporary fixing step, the chips of the second laminate before the joining step are considered to be the first laminate in the laminate preparation step, and the process from the laminate preparation step to the temporary fixing step is repeated one or more times before the joining step so that the chips of the second laminate are stacked in two or more layers and temporarily fixed, and after the last temporary fixing step, the joining step is performed. <3> A method for manufacturing a substrate laminate as described above. <5> The surface of the resin layer has at least one functional group selected from the group consisting of silanol groups, amino groups, epoxy groups, hydroxyl groups, and functional groups having unsaturated bonds. <3> A method for manufacturing a substrate laminate as described above. <6> The resin layer comprises a siloxane bond and at least one selected from the group consisting of an ester bond, an ether bond, an amide bond, and an imide bond. <3> A method for manufacturing a substrate laminate as described above. [Effects of the Invention]
[0008] According to one aspect of this disclosure, when manufacturing a substrate laminate by stacking chips, including a substrate obtained by dicing, onto another substrate, it is possible to provide a method for manufacturing a substrate laminate in which defects, contamination, and foreign matter inclusion of the chips are suppressed. [Brief explanation of the drawing]
[0009] [Figure 1] This diagram shows a schematic configuration of an example of a first laminate and a second laminate that can be used in the manufacturing method of the substrate laminate of this disclosure. [Figure 2] This is a schematic diagram showing a part of the process included in an example of a method for manufacturing a substrate laminate according to the present disclosure. [Figure 3] This is a schematic diagram showing a part of the process included in an example of a method for manufacturing a substrate laminate according to the present disclosure. [Figure 4] This is a schematic diagram showing a part of the process included in an example of a method for manufacturing a substrate laminate according to the present disclosure. [Figure 5] This is a schematic diagram showing a part of the process included in an example of a method for manufacturing a substrate laminate according to the present disclosure. [Figure 6] This is a schematic diagram showing a part of the process included in an example of a method for manufacturing a substrate laminate according to the present disclosure. [Figure 7] This is a schematic diagram showing an example of a substrate laminate manufactured by the substrate laminate manufacturing method of this disclosure. [Modes for carrying out the invention]
[0010] In this disclosure, a numerical range represented by "~" means a range that includes the numbers written before and after "~" as the lower and upper limits, respectively. In numerical ranges described in stages within this disclosure, the upper limit of one numerical range may be replaced with the upper limit of another numerical range described in stages, and the lower limit may be replaced with the lower limit of another numerical range described in stages. Furthermore, in numerical ranges described within this disclosure, the upper or lower limit of that range may be replaced with the values shown in the examples. In this disclosure, “substrate laminate” means a laminate having a structure in which two substrates, namely a first substrate and a second substrate, are laminated or joined via a first surface layer and a second back layer. The substrate laminate may have three or more substrates, and two of the three or more substrates may have a structure in which they are laminated or joined via a first surface layer and a second back layer. In this disclosure, “substrate” means “at least one of the first substrate and the second substrate.” In this disclosure, “at least one of the first laminate and the second laminate” may be simply referred to as “laminated structure.”
[0011] [Method for manufacturing a substrate laminate] A method for manufacturing a substrate laminate according to the present disclosure comprises a laminate preparation step of preparing a first laminate in which a first surface layer, a first substrate, and a first back layer are laminated in that order, and a second laminate in which a second surface layer, a second substrate, and a second back layer are laminated in that order. A surface protection step of providing a surface protection layer on the second surface layer of the second laminate, A dicing process is performed by attaching a dicing tape to the surface protection layer side of the second laminate having the surface protection layer, thereby dividing it into individual chips with a surface protection layer, each chip containing the divided second laminate and the surface protection layer. A lamination step of peeling the chip with the surface protection layer from the dicing tape and laminating the chip with the surface protection layer onto the first laminate such that the first surface layer and the second back surface layer are in contact, A cleaning and removal step involves cleaning the stacked first laminate and the chip with the surface protective layer, and removing the surface protective layer. The method includes a bonding step of heating the first laminate and the chip of the second laminate from which the surface protective layer has been removed to obtain a substrate laminate in which the chip of the second laminate is bonded onto the first laminate.
[0012] In the method for manufacturing a substrate laminate according to this disclosure, a surface protection layer is provided on the second laminate and dicing is performed, and the chipped second laminate is laminated onto the first laminate without peeling off the surface protection layer. This makes it possible to suppress contamination by the dicing tape, scratches on the second surface layer when peeling from the dicing tape, contamination of the semiconductor chip due to contact with equipment when handling the semiconductor chip, and contamination of foreign matter such as particles when the chip of the second laminate is laminated onto the first laminate after dicing.
[0013] The first and second laminates used in the manufacturing method of the substrate laminate of this disclosure may include other elements such as electrodes. For example, the first laminate comprises a first surface layer and a first electrode exposed from the first back layer, and the second laminate comprises a second surface layer and a second electrode exposed from the second back layer, and in the lamination process, a chip with a surface protection layer can be laminated on the first laminate such that the first electrode exposed from the first surface layer and the second electrode exposed from the second back layer are in contact.
[0014] Furthermore, the method for manufacturing the substrate laminate according to this disclosure may include other steps such as a cleaning step and a temporary fixing step before the bonding step. For example, the first surface layer may be an inorganic material layer formed of an inorganic material, the second back surface layer may be a resin layer formed of a resin, the lamination step may include a temporary fixing step of temporarily fixing the laminated first laminate and the chip with a surface protection layer at a first temperature, and the bonding step may be a step of heating the temporarily fixed first laminate and the chip of the second laminate at a second temperature higher than the first temperature.
[0015] In the manufacturing method of the substrate laminate described herein, a second laminate (chip) formed into chips by dicing is laminated onto a first laminate while the surface protective layer is still attached. This suppresses the adhesion and mixing of foreign matter when handling the chips during the lamination process. Furthermore, if the surface protective layer is removed by a cleaning and removal process after the second laminate (chip) laminated onto the first laminate is temporarily fixed, the occurrence of misalignment between the first laminate and the second laminate (chip) during the cleaning and removal process is suppressed.
[0016] Furthermore, in the method for manufacturing a substrate laminate according to the present disclosure, after the temporary fixing step, the chips of the second laminate before the bonding step are considered as the first laminate in the laminate preparation step, and the process from the laminate preparation step to the temporary fixing step is repeated one or more times before the bonding step, so that two or more layers of chips of the second laminate are stacked and temporarily fixed, and the bonding step can be performed after the final temporary fixing step. When manufacturing a substrate laminate by stacking two or more layers of chips from a second laminate, applying the manufacturing method for substrate laminates of this disclosure can suppress the inclusion of foreign matter such as particles between the chips of the stacked second laminates.
[0017] The resin layer may be, for example, a resin layer having at least one functional group selected from the group consisting of silanol groups, amino groups, epoxy groups, hydroxyl groups, and functional groups having unsaturated bonds on its surface, or a resin layer containing a siloxane bond and at least one bond selected from the group consisting of ester bonds, ether bonds, amide bonds, and imide bonds (hereinafter, these resin layers may be collectively referred to as "specific resin layers"). For example, when joining an inorganic material layer of a first laminate to a resin layer of a second laminate, if a cleaning and removal process is performed to remove the surface protective layer after the lamination process, the positions of the first laminate and the second laminate (chip) may easily shift. On the other hand, the above-mentioned specific resin layer is easily temporarily fixed even at room temperature (e.g., 23°C) when laminated on the inorganic material layer. Therefore, by laminating a second laminate (chip) equipped with the specific resin layer onto the first laminate and temporarily fixing it, and then removing the surface protective layer by a cleaning and removal process, the occurrence of positional shift between the first laminate and the second laminate (chip) during the cleaning and removal process is suppressed.
[0018] Before describing the details of each step in the manufacturing method of the substrate laminate according to this disclosure, an example of the manufacturing method of the substrate laminate according to this disclosure will be described with reference to the attached drawings. Note that this disclosure is not limited to the configurations shown in the drawings. Furthermore, the size, shape, and other configurations of the components in each figure are conceptual, and the relative relationships between the components are not limited thereto. Also, in each drawing, components having substantially the same function are assigned the same reference numeral, and the reference numerals and descriptions of redundant components may be omitted.
[0019] Figure 1 shows examples of the configurations of the first laminate 10 and the second laminate 20 that can be used in the manufacturing method of the substrate laminate according to this disclosure.
[0020] The first laminate 10 has a first surface layer, a first surface inorganic material layer 12 made of an inorganic material, on one side of the silicon substrate 11, which is the first substrate, and a first back surface inorganic material layer 13 made of an inorganic material, on the other side. A first surface electrode 14 surrounded by the first surface inorganic material layer 12 is placed on one side of the silicon substrate 11, and a first back surface electrode 15 surrounded by the first back surface inorganic material layer 13 is placed on the other side. Furthermore, a first through electrode 16 is provided that penetrates the silicon substrate 11 in the thickness direction and electrically connects the first surface electrode 14 and the first back surface electrode 15.
[0021] The second laminate 20 has a second surface layer, a second inorganic surface layer 22 made of an inorganic material, on one side of the silicon substrate 21, which is the second substrate, and a second resin back layer 23 made of resin, on the other side. A second surface electrode 24 surrounded by the second inorganic surface layer 22 is placed on one side of the silicon substrate 21, and a second back electrode 25 surrounded by the second resin back layer 23 is placed on the other side. Furthermore, a second through electrode 26 is provided that penetrates the silicon substrate 21 in the thickness direction and electrically connects the second surface electrode 24 and the second back electrode 25.
[0022] Figures 2 to 6 schematically show an example of a method for manufacturing a substrate laminate according to this disclosure using the first laminate 10 and the second laminate 20 shown in Figure 1.
[0023] (1) On the silicon substrate 21, which has an internal electrode that will become a second through electrode 26 and a second back electrode 25 connected to the internal electrode, a resin composition is spin-coated onto the side on which the second back electrode 25 is formed, and then cured to form a second back resin layer 23. After that, it is highly flattened by CMP (chemical mechanical polishing) and the back electrode 25 is exposed (Figure 2(1)).
[0024] (2) The second back surface resin layer 23 side of the silicon substrate 21 is temporarily supported on the temporary support 31 via the temporary support layer 32. For example, an adhesive layer is used as the temporary support layer 32, and a glass substrate, silicon substrate, ceramic substrate, etc. is used as the temporary support 31 (Figure 2(2)).
[0025] (3) The surface (front) of the silicon substrate 21, which is temporarily supported on the temporary support 31, opposite to the second back resin layer 23 is flattened to a high degree by CMP (chemical mechanical polishing), and the internal electrodes are exposed to form the second through-electrode 26 (Figure 2(3)).
[0026] (4) A second surface electrode 24 is formed to connect with the second through electrode 26 exposed from the surface of the silicon substrate 21 (Figure 3(4)).
[0027] (5) A second surface layer, a second inorganic surface layer 22, is formed on the surface side of the silicon substrate 21, and then it is highly planarized by CMP, exposing the surface electrodes 24 (Figure 3(5)). This gives the second laminate 20.
[0028] (6) A surface protective layer 27 is provided on the second surface inorganic material layer 22 and the back surface electrode 24 of the second laminate 20 (Figure 3(6)).
[0029] (7) The dicing tape 42 is attached to the surface protection layer 27 side of the second laminate 20 which has the surface protection layer 27, and the second laminate 20 is peeled off from the temporary support layer 32. After bonding, cleaning is performed (Figure 4(7)).
[0030] (8) Dicing is performed on the second back surface resin layer 23 side of the second laminate 20, cutting the surface protective layer 27 together with the second laminate 20 to form chips 28A with surface protective layer (chips 20A of the second laminate 20 with the surface protective layer 27A attached to the cut second surface inorganic material layer 22A) (Figure 4(8)).
[0031] (9) After dicing, the area is washed to remove any foreign matter such as particles (Figure 4(9)).
[0032] (10) The dicing tape 42 is peeled off the chip 28A with the surface protective layer by pushing up from the back side with the needle 51 (Figure 5(10)).
[0033] (11) The head 52 of the handling device adsorbs the surface protection layer 27A side of the surface protection layer chip 28A and laminates it onto the first laminate 10. At this time, the first surface inorganic material layer 12 of the first laminate 10 and the second back surface resin layer 23A of the surface protection layer chip 28A are in contact, and the first surface electrode 14 of the first laminate 10 and the second back surface electrode 25 of the second laminate 20 (surface protection layer chip 28A) are in contact (Figure 5(11)).
[0034] The stacked first laminate 10 and the chip 28A with a surface protection layer are temporarily fixed together at a first temperature, for example, room temperature. In this case, the chip 28A with a surface protection layer is temporarily fixed by stacking it on the first laminate 10 without heating. If necessary, temporary fixing may be performed by heating to a temperature below 100°C.
[0035] (12) Clean the temporarily fixed first laminate 10 and the chip 28A with the surface protection layer, and the surface protection layer 2 7Remove it (Figure 6(12)).
[0036] Surface protective layer 2 in a temporarily fixed state 7 The chip 20A of the second laminate 20 (which may be referred to as "second laminate chip 20A" in this disclosure) from which the coating has been removed, and the first laminate 10 are heated to a second temperature higher than the first temperature, for example, 100°C or higher. This results in a substrate laminate 100 in which the chip 20A of the second laminate 20 is bonded to the first laminate 10.
[0037] The steps shown in Figures 1 to 6 above are examples of methods for manufacturing a substrate laminate according to this disclosure, and are not limited thereto. The steps for manufacturing a substrate laminate according to this disclosure will be described in detail below. While the drawings may be referenced in the following description, reference numerals will be omitted as appropriate.
[0038] [Laminate preparation process] The manufacturing method of the substrate laminate according to this disclosure includes a laminate preparation step of preparing a first laminate 10 and a second laminate 20 (Figure 1). The first laminate has a first surface layer, a first substrate, and a first back layer stacked in this order in the thickness direction. The first surface layer is located on one side, and the first back layer is located on the other side (opposite side). Similarly, the second laminate has a second surface layer, a second substrate, and a second back layer stacked in this order in the thickness direction. The second surface layer is located on one side, and the second back layer is located on the other side (opposite side).
[0039] (First substrate and second substrate) The material of the circuit board is not particularly limited and can be any commonly used material. The materials of the first circuit board and the second circuit board may be the same or different. The substrate preferably contains at least one element selected from the group consisting of Si, Al, Ti, Zr, Hf, Fe, Ni, Cu, Ag, Au, Ga, Ge, Sn, Pd, As, Pt, Mg, In, Ta, and Nb. Examples of substrate materials include semiconductors: Si, InP, GaN, GaAs, InGaAs, InGaAlAs, SiC; oxides, carbides, nitrides: borosilicate glass (Pyrex®), quartz glass (SiO2), sapphire, ZrO2, Si3N4, AlN; piezoelectrics, dielectrics: BaTiO3, LiN Examples include bO3, SrTiO3, diamond, and metals such as Al, Ti, Fe, Cu, Ag, Au, Pt, Pd, Ta, and Nb.
[0040] Other materials that may be used for the substrate include resins such as polydimethylsiloxane (PDMS), epoxy resin, phenolic resin, polyimide, benzocyclobutene resin, and polybenzoxazole.
[0041] The substrate may have a multilayer structure. Examples include a structure in which an inorganic layer such as silicon oxide, silicon nitride, or SiCN (silicon carbonitride) is formed on the surface of a silicon substrate, a structure in which an organic layer such as polyimide resin, polybenzoxazole resin, epoxy resin, cyclotene (Dow Chem), imide-crosslinked siloxane resin, epoxy-modified siloxane, porous silica, organic-crosslinked siloxane, or organic-inorganic composite low-k such as black diamond (Applied Materials) is formed on the surface of a silicon substrate, and a structure in which a composite of inorganic and organic materials is formed on a silicon substrate.
[0042] Each material is primarily used for the following purposes: Si is used in semiconductor memory, LSI stacking, CMOS image sensors, MEMS encapsulation, optical devices, LEDs, etc. SiO2 is used in semiconductor memory, LSI stacking, MEMS encapsulation, microfluidics, CMOS image sensors, optical devices, LEDs, etc. PDMS is a microfluidic; InGaAlAs, InGaAs, and InP are optical devices; InGaAlAs, GaAs, and GaN are used in LEDs, etc.
[0043] The thickness of the substrate is not particularly limited, but is preferably 0.5 μm to 1 mm, more preferably 1 μm to 900 μm, and even more preferably 2 μm to 900 μm.
[0044] The shape of the substrate is not particularly limited. For example, if the substrate is a silicon substrate, it may be a silicon substrate on which an interlayer insulating layer (low-k film) is formed, and the silicon substrate may have fine grooves (recesses), fine through holes, etc.
[0045] In the method for manufacturing a substrate laminate according to this disclosure, surface treatment may be performed on the side of the substrate that comes into contact with the resin layer, from the viewpoint of bonding strength. By surface treatment of the substrate, at least one functional group selected from the group consisting of hydroxyl groups, epoxy groups, carboxyl groups, amino groups, and mercapto groups may be formed.
[0046] Examples of surface treatments include plasma treatment, chemical treatment, and ozone treatment such as ultraviolet (UV) ozone treatment.
[0047] Hydroxyl groups can be provided on the surface of a substrate by performing surface treatments such as plasma treatment, chemical treatment, or ozone treatment including UV ozone treatment. It is preferable that the hydroxyl group exists in a state of being bonded to at least one element selected from the group consisting of Si, Al, Ti, Zr, Hf, Fe, Ni, Cu, Ag, Au, Ga, Ge, Sn, Pd, As, Pt, Mg, In, Ta, and Nb, which is contained in the substrate. It is preferable that the surface of the substrate that is in contact with the resin layer has silanol groups containing hydroxyl groups.
[0048] Epoxy groups can be provided on the surfaces of substrates by performing surface treatments such as silane coupling with epoxysilane.
[0049] Carboxylic groups can be provided on the substrate surface by performing surface treatments such as silane coupling with carboxysilane.
[0050] Amino groups can be provided on the surfaces of substrates by performing surface treatments such as silane coupling with aminosilane.
[0051] Mercapto groups can be provided on the surface of a substrate by performing surface treatments such as silane coupling with mercaptosilane.
[0052] Furthermore, to enhance bonding strength, a primer such as a silane coupling agent may be formed on the surface of the substrate to which the resin material is applied.
[0053] (First surface layer and second surface layer) The first surface layer is a layer located on one side of the first substrate and is in contact with the second back surface layer of the second laminate during the lamination process. The second surface layer is the second substrate one This is a layer located on one side, and it is the layer on which a surface protection layer is provided during the surface protection process.
[0054] The first surface layer and the second surface layer may be composed of an inorganic material or a resin. From the viewpoint of resistance to cleaning and removal in the cleaning and removal process, it is preferable that the first surface layer and the second surface layer are inorganic material layers composed of inorganic materials.
[0055] (First back layer and second back layer) The first back layer is a layer located on the other side of the first substrate, that is, on the side opposite to the first front layer, and the second back layer is a layer located on the other side of the second substrate, that is, on the side opposite to the second front layer.
[0056] The first back layer and the second back layer may be made of an inorganic material or a resin. The first back surface layer located at the bottom of the substrate laminate manufactured by the substrate laminate manufacturing method of this disclosure is preferably an inorganic material layer from the viewpoint of cleaning resistance and other factors. On the other hand, from the viewpoint of suppressing void generation during the temporary fixing process between the first laminate and the second laminate, and during the bonding process between the first laminate and the second laminate, it is preferable that the second back surface layer is a resin layer made of resin.
[0057] Hereinafter, the first surface layer, the first back layer, the second surface layer, and / or the second back The inorganic material layer and resin layer that may constitute the surface layer will be described separately. In this disclosure, for example, the first surface layer and the second surface layer, which are composed of an inorganic material, may be referred to as the first surface inorganic material layer and the second surface inorganic material layer, respectively. Also, the second back surface layer, which is composed of resin, may be referred to as the second back surface resin layer.
[0058] (Inorganic layer) The material of the inorganic layer is not particularly limited and may be any inorganic material used when joining inorganic materials together in a semiconductor substrate. Specifically, the inorganic layer may contain at least one element selected from the group consisting of Si, Al, Ti, Zr, Hf, Fe, Ni, Cu, Ag, Au, Ga, Ge, Sn, Pd, As, Pt, Mg, In, Ta, and Nb, and preferably contains at least one element selected from the group consisting of Si, Ga, Ge, and As. The inorganic layer may also contain oxides, carbides, nitrides, etc., of the aforementioned elements. The materials of each inorganic layer may be the same or different.
[0059] The method for forming an inorganic material layer on at least one surface of a substrate is not particularly limited, and conventionally known methods for forming inorganic material layers can be used. Examples include CVD, sputtering, AGD (aerosolized gas deposition), sol-gel method, anodic oxidation, and thermal decomposition.
[0060] (Resin layer) The resin layer is formed by applying a resin composition containing a resin material to one side of the substrate and then curing the resulting resin composition layer.
[0061] The resin material included in the resin composition is not particularly limited and includes, for example, polyimide, polyamide, polyamideimide, parylene, polyalylene ether, tetrahydronaphthalene, octahydroanthracene, and other materials in which the bonds or structure are formed by crosslinking, and polybenzox Zo Examples include materials that form nitrogen ring-containing structures such as polybenzoxazine, materials in which bonds or structures such as Si-O are formed by crosslinking, and organic materials such as siloxane-modified compounds. The resin materials used to form each resin layer may be the same or different.
[0062] Examples of structures containing Si-O bonds (siloxane bonds) include those represented by the following formulas (1) to (3).
[0063] [ka]
[0064] In a structure having a Si-O bond (siloxane bond), the group that bonds to Si ga a It may be substituted with a lukilen group, a phenylene group, etc. For example, (-O-) x (R1) y Si-(R 2)-Si(R1) y (-O-) x The structure may also have such a configuration (R1 represents a methyl group, etc., and R2 represents an alkylene group, phenylene group, etc., and x and y are each independent integers of 0 or more, and x + y is 3).
[0065] Examples of materials in which Si-O bonds are formed by crosslinking include the compounds represented by formulas (4) and (5) shown below. Furthermore, the structures represented by formulas (1) and (2) can be produced, for example, by heating and reacting the compounds represented by formulas (4) and (5).
[0066] [ka]
[0067] For example, if the resin material includes materials such as polyimides, polyamides, and polyamide-imides in which the bonds or structure are formed by crosslinking, it is preferable to include a compound (A) having a cationic functional group containing at least one primary nitrogen atom and a secondary nitrogen atom, and having a weight-average molecular weight of 90 to 400,000, and a crosslinking agent (B) having three or more -C(=O)OX groups (where X is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms) in the molecule, with one to six of the three or more -C(=O)OX groups being -C(=O)OH groups, and having a weight-average molecular weight of 200 to 2000.
[0068] (Compound (A)) Compound (A) is a compound having a cationic functional group containing at least one primary nitrogen atom and a secondary nitrogen atom, and having a weight-average molecular weight of 90 to 400,000. The cationic functional group is not particularly limited as long as it can carry a positive charge and contains at least one primary nitrogen atom and a secondary nitrogen atom.
[0069] Furthermore, compound (A) may contain tertiary nitrogen atoms in addition to primary and secondary nitrogen atoms.
[0070] In this disclosure, "primary nitrogen atom" refers to a nitrogen atom bonded to only two hydrogen atoms and one non-hydrogen atom (for example, a nitrogen atom contained in a primary amino group (-NH2 group)), or a nitrogen atom (cation) bonded to only three hydrogen atoms and one non-hydrogen atom. In addition, the term "secondary nitrogen atom" refers to a nitrogen atom bonded to only one hydrogen atom and two atoms other than hydrogen (i.e., a nitrogen atom contained in the functional group represented by formula (a) below), or a nitrogen atom (cation) bonded to only two hydrogen atoms and two atoms other than hydrogen. In addition, the term "tertiary nitrogen atom" refers to a nitrogen atom bonded to only three atoms other than hydrogen (i.e., a nitrogen atom that is the functional group represented by formula (b) below), or a nitrogen atom (cation) bonded to only one hydrogen atom and three atoms other than hydrogen.
[0071] [Chemical Formula]
[0072] In formula (a) and formula (b), * indicates the bonding position with an atom other than a hydrogen atom. Here, the functional group represented by formula (a) may be a functional group constituting a part of a secondary amino group (-NHR a group; here, R a represents an alkyl group), or may be a divalent linking group contained in the polymer backbone. In addition, the functional group represented by formula (b) (i.e., tertiary nitrogen atom) may be a functional group constituting a part of a tertiary amino group (-NR b R c group; here, R b and R c each independently represent an alkyl group), or may be a trivalent linking group contained in the polymer backbone.
[0073] The weight-average molecular weight of compound (A) is between 90 and 400,000. Examples of compound (A) include aliphatic amines, compounds having a siloxane bond (Si-O bond) and an amino group, and amine compounds that do not have a Si-O bond in the molecule and have a ring structure. When compound (A) is an aliphatic amine, the weight-average molecular weight is preferably between 10,000 and 200,000. When compound (A) is a compound having a siloxane bond (Si-O bond) and an amino group, the weight-average molecular weight is preferably between 130 and 10,000, more preferably between 130 and 5,000, and even more preferably between 130 and 2,000. When compound (A) is an amine compound that does not have a Si-O bond in the molecule and has a ring structure, the weight-average molecular weight is preferably between 90 and 600.
[0074] In this disclosure, weight-average molecular weight refers to the weight-average molecular weight in terms of polyethylene glycol, measured by GPC (Gel Permeation Chromatography) for substances other than monomers. Specifically, the weight-average molecular weight is calculated using polyethylene glycol / polyethylene oxide as a standard. The refractive index is detected at a flow rate of 1.0 mL / min using a Shodex DET RI-101 analyzer and two types of analytical columns (TSKgel G6000PWXL-CP and TSKgel G3000PWXL-CP from Tosoh Corporation) with an aqueous solution of sodium nitrate concentration of 0.1 mol / L as the developing solvent. The calculation is performed using analytical software (Empower3 from Waters Corporation).
[0075] Furthermore, compound (A) may optionally have anionic functional groups, nonionic functional groups, etc. The nonionic functional group may be either a hydrogen bond acceptor or a hydrogen bond donor. Examples of the nonionic functional group include a hydroxyl group, a carbonyl group, an ether group (-O-), and the like. The anionic functional group is not particularly limited as long as it is a functional group capable of carrying a negative charge. Examples of the anionic functional group include carboxylic acid groups, sulfonic acid groups, and sulfate groups.
[0076] Examples of compound (A) include aliphatic amines, but more specifically, polyalkyleneimines, polyallylamines, and polyacrylamides, which are polymers of alkyleneimines such as ethyleneimine, propyleneimine, butyleneimine, pentyleneimine, hexyleneimine, heptyleneimine, octyleneimine, trimethyleneimine, tetramethyleneimine, pentamethyleneimine, hexamethyleneimine, and octamethyleneimine.
[0077] Polyethyleneimine (PEI) can be produced by known methods described in Japanese Patent Publication No. 43-8828, Japanese Patent Publication No. 49-33120, Japanese Patent Application Publication No. 2001-213958, and International Publication No. 2010 / 137711, etc. Other polyalkyleneimines can be produced by the same methods as polyethyleneimine.
[0078] Compound (A) is also preferably a derivative of the polyalkyleneimine described above (polyalkyleneimine derivative; particularly preferably polyethyleneimine derivative). There are no particular restrictions on the polyalkyleneimine derivative as long as it is a compound that can be produced using the above polyalkyleneimine. Specifically, examples include polyalkyleneimine derivatives obtained by introducing an alkyl group (preferably an alkyl group having 1 to 10 carbon atoms), an aryl group, etc., into polyalkyleneimine, and polyalkyleneimine derivatives obtained by introducing a crosslinking group such as a hydroxyl group into polyalkyleneimine. These polyalkylene imine derivatives can be produced by methods commonly used with the above-mentioned polyalkylene imines. Specifically, they can be produced, for example, in accordance with the method described in Japanese Patent Application Publication No. 6-016809.
[0079] Furthermore, as a polyalkyleneimine derivative, highly branched polyalkyleneimines obtained by reacting polyalkyleneimine with a monomer containing a cationic functional group to improve the degree of branching of the polyalkyleneimine are also preferred. Methods for obtaining highly branched polyalkyleneimines include, for example, a method in which a polyalkyleneimine having multiple secondary nitrogen atoms in its skeleton is reacted with a monomer containing a cationic functional group, thereby substituting at least one of the multiple secondary nitrogen atoms with the monomer containing a cationic functional group; and a method in which a polyalkyleneimine having multiple primary nitrogen atoms at its terminals is reacted with a monomer containing a cationic functional group, thereby substituting at least one of the multiple primary nitrogen atoms with the monomer containing a cationic functional group. Cationic functional groups that can be introduced to improve the degree of branching include aminoethyl group, aminopropyl group, diaminopropyl group, aminobutyl group, diaminobutyl group, and triaminobutyl group. However, the aminoethyl group is preferred because it reduces the equivalent amount of cationic functional groups and increases the density of cationic functional groups.
[0080] Furthermore, the polyethyleneimine and its derivatives may be commercially available. For example, polyethyleneimine and its derivatives can be appropriately selected and used from those commercially available from companies such as Nippon Shokubai Co., Ltd., BASF, MP-Biomedicals, etc.
[0081] Compound (A) can include, in addition to the aliphatic amines mentioned above, compounds having a Si-O bond and an amino group. Examples of compounds having a Si-O bond and an amino group include siloxanediamines, silane coupling agents having an amino group, and siloxane polymers of silane coupling agents having an amino group. Examples of silane coupling agents containing an amino group include compounds represented by the following formula (A-3).
[0082] [ka]
[0083] In formula (A-3), R 1 R represents an alkyl group having 1 to 4 carbon atoms, which may be substituted. 2 and R 3 Each of these independently represents an alkylene group, ether group, or carbonyl group having 1 to 12 carbon atoms, which may be substituted (the skeleton may contain carbonyl groups, ether groups, etc.). 4 and R 5 Each of these independently represents an alkylene group or single bond having 1 to 4 carbon atoms, which may be substituted. Ar represents a divalent or trivalent aromatic ring. X 1 X represents hydrogen or an alkyl group having 1 to 5 carbon atoms, which may be substituted. 2 R represents hydrogen, a cycloalkyl group, a heterocyclic group, an aryl group, or a C1-C5 alkyl group which may be substituted (may contain a carbonyl group, ether group, etc. in its skeleton). 1 , R 2 , R 3 , R 4 , R 5 , X 1 They may be the same or different. R 1 , R 2 , R 3 , R 4 , R 5 , X 1 , X 2 Examples of substituents on the alkyl group and alkylene group in the compound include, independently, amino groups, hydroxyl groups, alkoxy groups, cyano groups, carboxylic acid groups, sulfonic acid groups, halogens, and the like. Examples of divalent or trivalent aromatic rings in Ar include divalent or trivalent benzene rings. 2 Examples of aryl groups in this context include phenyl groups, methylbenzyl groups, and vinylbenzyl groups.
[0084] Specific examples of silane coupling agents represented by formula (A-3) include, for example, N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminoisobutyldimethylmethoxysilane, N-(2-aminoethyl)-3-aminoisobutylmethyldimethoxysilane, N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, (aminoethylaminoethyl)phenyltriethoxysilane, methylbenzylaminoethylaminopropyltrimethoxysilane, benzylaminoethylaminopropyltriethoxysilane, 3-ureidopropyltriethoxysilane, (aminoethylaminoethyl)phenyltriethoxysilane, Examples include (Tylaminoethyl)phenethyltrimethoxysilane, (aminoethylaminomethyl)phenethyltrimethoxysilane, N-[2-[3-(trimethoxysilyl)propylamino]ethyl]ethylenediamine, 3-aminopropyldiethoxymethylsilane, 3-aminopropyldimethoxymethylsilane, 3-aminopropyldimethylethoxysilane, 3-aminopropyldimethylmethoxysilane, trimethoxy[2-(2-aminoethyl)-3-aminopropyl]silane, diaminomethylmethyldiethoxysilane, methylaminomethylmethyldiethoxysilane, p-aminophenyltrimethoxysilane, N-methylaminopropyltriethoxysilane, N-methylaminopropylmethyldiethoxysilane, (phenylaminomethyl)methyldiethoxysilane, acetamidopropyltrimethoxysilane, and hydrolysates thereof.
[0085] Examples of silane coupling agents containing amino groups other than formula (A-3) include N,N-bis[3-(trimethoxysilyl)propyl]ethylenediamine, N,N'-bis[3-(trimethoxysilyl)propyl]ethylenediamine, bis[(3-triethoxysilyl)propyl]amine, piperazinylpropylmethyldimethoxysilane, bis[3-(triethoxysilyl)propyl]urea, bis(methyldiethoxysilylpropyl)amine, 2,2-dimethoxy-1,6-diaza-2-silacyclooctane, 3,5-diamino-N-(4-(methoxydimethylsilyl)phenyl)benzamide, 3,5-diamino-N-(4-(triethoxysilyl)phenyl)benzamide, 5-(ethoxydimethylsilyl)benzene-1,3-diamine, and their hydrolysates.
[0086] The aforementioned silane coupling agents having amino groups may be used individually or in combination of two or more. Furthermore, a silane coupling agent having amino groups may be used in combination with a silane coupling agent without amino groups. For example, a silane coupling agent having mercapto groups may be used to improve adhesion to metals.
[0087] Alternatively, polymers formed via siloxane bonds (Si-O-Si) from these silane coupling agents (siloxane polymers) may be used. For example, from the hydrolysis product of 3-aminopropyltrimethoxysilane, polymers having a linear siloxane structure, a branched siloxane structure, a cyclic siloxane structure, a cage-like siloxane structure, and the like can be obtained. The cage-like siloxane structure can be represented, for example, by the following formula (A-1).
[0088] [ka]
[0089] Examples of siloxanediamines include compounds represented by the following formula (A-2). In formula (A-2), i is an integer from 0 to 4, j is an integer from 1 to 3, and Me is a methyl group.
[0090] [ka]
[0091] Examples of siloxanediamines include 1,3-bis(3-aminopropyl)tetramethyldisiloxane (in formula (A-2), i=0, j=1) and 1,3-bis(2-aminoethylamino)propyltetramethyldisiloxane (in formula (A-2), i=1, j=1).
[0092] Compound (A) includes the aforementioned aliphatic amines and compounds having a Si-O bond and an amino group, as well as amine compounds that do not have a Si-O bond in the molecule and have a ring structure. Among these, amine compounds with a weight-average molecular weight of 90 to 600 that do not have a Si-O bond in the molecule and have a ring structure are preferred. Examples of amine compounds with a weight-average molecular weight of 90 to 600 that do not have a Si-O bond in the molecule and have a ring structure include alicyclic amines, aromatic ring amines, and heterocyclic amines. The molecule may have multiple ring structures, and these multiple ring structures may be the same or different. Among amine compounds with ring structures, compounds having an aromatic ring are more preferred because they are more likely to be thermally stable. Furthermore, as amine compounds having a weight-average molecular weight of 90 to 600 that do not have Si-O bonds in the molecule and have a ring structure, compounds having primary amino groups are preferred because they readily form thermal crosslinked structures such as amides, amide-imides, and imides together with the crosslinking agent (B), thereby increasing heat resistance. Moreover, as the aforementioned amine compounds, diamine compounds having two primary amino groups and triamine compounds having three primary amino groups are preferred because they readily form a large number of thermal crosslinked structures such as amides, amide-imides, and imides together with the crosslinking agent (B), thereby further increasing heat resistance.
[0093] Examples of alicyclic amines include cyclohexylamine and dimethylaminocyclohexane. Examples of aromatic ring amines include diaminodiphenyl ether, xylenediamine (preferably paraxylenediamine), diaminobenzene, diaminotoluene, methylenedianiline, dimethyldiaminobiphenyl, bis(trifluoromethyl)diaminobiphenyl, diaminobenzophenone, diaminobenzanilide, bis(aminophenyl)fluorene, bis(aminophenoxy)benzene, bis(aminophenoxy)biphenyl, dicarboxydiaminodiphenylmethane, diaminoresorcinol, dihydroxybenzidine, diaminobenzidine, 1,3,5-triaminophenoxybenzene, 2,2'-dimethylbenzidine, tris(4-aminophenyl)amine, 2,7-diaminofluorene, 1,9-diaminofluorene, and dibenzylamine. Examples of heterocyclic amines include heterocyclic rings containing a sulfur atom as a heteroatom (e.g., thiophene rings), or heterocyclic rings containing a nitrogen atom as a heteroatom (e.g., five-membered rings such as pyrrole rings, pyrrolidine rings, pyrazole rings, imidazole rings, and triazole rings; six-membered rings such as isocyanuric rings, pyridine rings, pyridazine rings, pyrimidine rings, pyrazine rings, piperidine rings, piperazine rings, and triazine rings; and condensed rings such as indole rings, indoline rings, quinoline rings, acridine rings, naphthyridine rings, quinazoline rings, purine rings, and quinoxaline rings). For example, heterocyclic amines having a nitrogen-containing heterocycle include melamine and ammeline. Examples include melam, melem, and tris(4-aminophenyl)amine. Furthermore, examples of amine compounds that have both heterocyclic and aromatic rings include N2,N4,N6-tris(4-aminophenyl)-1,3,5-triazine-2,4,6-triamine.
[0094] Since compound (A) has primary or secondary amino groups, it can strongly bond the substrates together through electrostatic interactions with functional groups such as hydroxyl groups, epoxy groups, carboxyl groups, amino groups, and mercapto groups that may be present on the surfaces of the first and second substrates, or by forming dense covalent bonds with such functional groups. Furthermore, since compound (A) has a primary or secondary amino group, it readily dissolves in the polar solvent (D) described later. By using compound (A), which readily dissolves in the polar solvent (D), the affinity with the hydrophilic surface of the substrate, such as a silicon substrate, is increased, making it easier to form a smooth film and allowing the resin layer to be made thinner.
[0095] As for compound (A), aliphatic amines or compounds having a Si-O bond and an amino group are preferred from the viewpoint of forming a smooth thin film, and compounds having a Si-O bond and an amino group are more preferred from the viewpoint of heat resistance.
[0096] If compound (A) contains a compound having a Si-O bond and an amino group, it is preferable from the viewpoint of forming a smooth thin film if the ratio of the total number of primary and secondary nitrogen atoms in compound (A) to the number of silicon atoms (total number of primary and secondary nitrogen atoms / number of silicon atoms) is 0.2 or more and 5 or less.
[0097] When compound (A) contains a compound having a Si-O bond and an amino group, it is preferable that, from the viewpoint of adhesion between substrates, the non-crosslinking group, such as a methyl group bonded to Si in the compound having the Si-O bond and amino group satisfies the relationship (non-crosslinking group) / Si < 2 in molar ratio. It is presumed that by satisfying this relationship, the crosslinking density of the formed film (crosslinking between Si-O-Si bonds and amide bonds, imide bonds, etc.) is improved, the substrates have sufficient adhesion to each other, and substrate delamination can be suppressed.
[0098] As described above, compound (A) has a cationic functional group containing at least one primary nitrogen atom and a secondary nitrogen atom. Here, if compound (A) contains a primary nitrogen atom, it is preferable that the proportion of primary nitrogen atoms to the total nitrogen atoms in compound (A) is 20 mol% or more, more preferably 25 mol% or more, and even more preferably 30 mol% or more. Furthermore, compound (A) may have a cationic functional group that contains a primary nitrogen atom but does not contain nitrogen atoms other than primary nitrogen atoms (e.g., secondary nitrogen atoms, tertiary nitrogen atoms).
[0099] Furthermore, if compound (A) contains secondary nitrogen atoms, it is preferable that the proportion of secondary nitrogen atoms in compound (A) is 5 mol% or more and 50 mol% or less, and more preferably 10 mol% or more and 45 mol% or less.
[0100] Furthermore, compound (A) may contain tertiary nitrogen atoms in addition to primary and secondary nitrogen atoms. If compound (A) contains tertiary nitrogen atoms, it is preferable that the proportion of tertiary nitrogen atoms to the total nitrogen atoms in compound (A) is 20 mol% or more and 50 mol% or less, and more preferably 25 mol% or more and 45 mol% or less.
[0101] In this disclosure, the content of the component derived from compound (A) in the resin layer is not particularly limited, and for example, it can be 1% by mass or more and 82% by mass or less of the total resin layer, preferably 5% by mass or more and 82% by mass or less, and more preferably 13% by mass or more and 82% by mass or less.
[0102] (Crosslinking agent (B)) The crosslinking agent (B) is a compound having three or more -C(=O)OX groups (where X is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms) in its molecule, with one to six of the three or more -C(=O)OX groups (hereinafter also referred to as "COOX") being -C(=O)OH groups (hereinafter also referred to as "COOH"), and having a weight-average molecular weight of 200 to 2000.
[0103] The crosslinking agent (B) is a compound having three or more -C(=O)OX groups (where X is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms) in its molecule, preferably a compound having three to six -C(=O)OX groups in its molecule, and more preferably a compound having three or four -C(=O)OX groups in its molecule.
[0104] In the crosslinking agent (B), X in the -C(=O)OX group can be a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, with hydrogen atoms, methyl groups, ethyl groups, and propyl groups being preferred. The X in the -C(=O)OX group may be the same or different from each other.
[0105] The crosslinking agent (B) is a compound having one to six -C(=O)OH groups in its molecule where X is a hydrogen atom, preferably a compound having one to four -C(=O)OH groups in its molecule, more preferably a compound having two to four -C(=O)OH groups in its molecule, and even more preferably a compound having two or three -C(=O)OH groups in its molecule.
[0106] The crosslinking agent (B) is a compound having a weight-average molecular weight of 200 or more and 2000 or less. The weight-average molecular weight of the crosslinking agent (B) is preferably 200 or more and 1000 or less, more preferably 200 or more and 600 or less, and even more preferably 200 or more and 400 or less.
[0107] The crosslinking agent (B) preferably has a ring structure within its molecule. Examples of ring structures include alicyclic structures and aromatic ring structures. Furthermore, the crosslinking agent (B) may have multiple ring structures within its molecule, and these multiple ring structures may be the same or different.
[0108] Examples of alicyclic structures include alicyclic structures having 3 to 8 carbon atoms, preferably alicyclic structures having 4 to 6 carbon atoms, and the ring structure may be saturated or unsaturated. More specifically, examples of alicyclic structures include saturated alicyclic structures such as cyclopropane rings, cyclobutane rings, cyclopentane rings, cyclohexane rings, cycloheptane rings, and cyclooctane rings; and unsaturated alicyclic structures such as cyclopropene rings, cyclobutene rings, cyclopentene rings, cyclohexene rings, cycloheptene rings, and cyclooctene rings.
[0109] The aromatic ring structure is not particularly limited as long as it is an aromatic ring structure, and examples include benzene-based aromatic rings such as benzene rings, naphthalene rings, anthracene rings, and perylene rings; aromatic heterocycles such as pyridine rings and thiophene rings; and non-benzene-based aromatic rings such as indene rings and azulene rings.
[0110] The ring structure that the crosslinking agent (B) has within the molecule is preferably at least one selected from the group consisting of a cyclobutane ring, a cyclopentane ring, a cyclohexane ring, a benzene ring, and a naphthalene ring, and at least one of the benzene ring and the naphthalene ring is more preferred from the viewpoint of further improving the heat resistance of the resin layer.
[0111] As mentioned above, the crosslinking agent (B) may have multiple ring structures within its molecule, and if the ring structure is benzene, it may have a biphenyl structure, a benzophenone structure, a diphenyl ether structure, etc.
[0112] The crosslinking agent (B) preferably has fluorine atoms in its molecule, more preferably has one to six fluorine atoms in its molecule, and even more preferably has three to six fluorine atoms in its molecule. For example, the crosslinking agent (B) may have a fluoroalkyl group in its molecule, specifically a trifluoroalkyl group or a hexafluoroisopropyl group.
[0113] Furthermore, examples of crosslinking agents (B) include carboxylic acid compounds such as alicyclic carboxylic acids, benzenecarboxylic acids, naphthalenecarboxylic acids, diphthalic acids, and fluorinated aromatic carboxylic acids; and carboxylic acid ester compounds such as alicyclic carboxylic acid esters, benzenecarboxylic acid esters, naphthalenecarboxylic acid esters, diphthalic acid esters, and fluorinated aromatic carboxylic acid esters. Carboxylic acid ester compounds are compounds that have a carboxyl group (-C(=O)OH group) in their molecule, and in three or more -C(=O)OX groups, at least one X is an alkyl group having 1 to 6 carbon atoms (i.e., having an ester bond). In this disclosure, because the crosslinking agent (B) is a carboxylic acid ester compound, aggregation due to association between compound (A) and crosslinking agent (B) is suppressed, resulting in fewer aggregates and pits, and making it easier to adjust the film thickness.
[0114] The carboxylic acid compound is preferably a tetravalent or less carboxylic acid compound containing four or fewer -C(=O)OH groups, and more preferably a trivalent or tetravalent carboxylic acid compound containing three or four -C(=O)OH groups.
[0115] The carboxylic acid ester compound is preferably a compound that contains three or fewer carboxyl groups (-C(=O)OH groups) and three or fewer ester bonds in its molecule, and more preferably a compound that contains two or fewer carboxyl groups and two or fewer ester bonds in its molecule.
[0116] Furthermore, in the carboxylic acid ester compound, if X is an alkyl group having 1 to 6 carbon atoms in three or more -C(=O)OX groups, X is preferably a methyl group, ethyl group, propyl group, butyl group, etc., but it is preferable that X be an ethyl group or a propyl group in order to further suppress aggregation due to association between compound (A) and crosslinking agent (B).
[0117] Specific examples of the carboxylic acid compounds mentioned above are, but are not limited to, alicyclic carboxylic acids such as 1,2,3,4-cyclobutanetetracarboxylic acid, 1,2,3,4-cyclopentanetetracarboxylic acid, 1,3,5-cyclohexanetricarboxylic acid, 1,2,4-cyclohexanetricarboxylic acid, 1,2,4,5-cyclohexanetetracarboxylic acid, and 1,2,3,4,5,6-cyclohexanehexacarboxylic acid; benzenecarboxylic acids such as 1,2,4-benzenetricarboxylic acid, 1,3,5-benzenetricarboxylic acid, pyromellitic acid, 3,4'-biphthalic acid, p-phenylenebis(trimellitate acid), benzenepentacarboxylic acid, and mellitic acid; 1,4 Naphthalene carboxylic acids such as ,5,8-naphthalenetetracarboxylic acid and 2,3,6,7-naphthalenetetracarboxylic acid; 3,3',5,5'-tetracarboxydiphenylmethane, biphenyl-3,3',5,5'-tetracarboxylic acid, biphenyl-3,4',5-tricarboxylic acid, biphenyl-3,3',4,4'-tetracarboxylic acid, benzophenone-3,3',4,4'-tetracarboxylic acid, 4,4'-oxydiphthalic acid, 3,4'-oxydiphthalic acid, 1,3-bis(phthalic acid)tetramethyldisiloxane, 4,4'-(ethyn-1,2-diyl)diphthalic acid 4,4'-(1,4-phenylenebis(oxy))diphthalic acid, 4,4'-([1,1'-biphenyl]-4,4'-diylbis(oxy))diphthalic acid, 4,4'-((oxybis(4,1-phenylene))bis(oxy))diphthalic acid, 4,4'-((oxybis(4,1-phenylene))bis(oxy))diphthalic acid, 4,4'-((oxybis(4,1-phenylene))bis(oxy))diphthalic acid, 4,4'-([1,1'-biphenyl]-4,4'-diylbis(oxy))diphthalic acid, 4,4'-((oxybis(4,1-phenylene))bis(oxy))diphthalic acid, 4,4'-(1,4-phenylenebis(oxy))diphthalic acid, 4,4'-([1,1'-biphenyl]-4,4'-diylbis(oxy))diphthalic acid, 4,4'-([1,1'-biphenyl]-4,4'-diylbis(oxy))diphthalic acid, 4,4'-((oxybis(4,1-phenylene) Examples include diphthalic acids such as 4,4'-((oxybis(4,1-phenylene))bis(oxy))diphthalic acid; perylene carboxylic acids such as perylene-3,4,9,10-tetracarboxylic acid; anthracene carboxylic acids such as anthracene-2,3,6,7-tetracarboxylic acid; and fluorinated aromatic ring carboxylic acids such as 4,4'-(hexafluoroisopropylidene)diphthalic acid, 9,9-bis(trifluoromethyl)-9H-xanthene-2,3,6,7-tetracarboxylic acid, and 1,4-ditrifluoromethylpyromellitic acid.
[0118] Specific examples of the carboxylic acid ester compounds include compounds in which at least one carboxyl group in the above-mentioned specific examples of carboxylic acid compounds is substituted with an ester group. Examples of carboxylic acid ester compounds include half-esterified compounds represented by the following general formulas (B-1) to (B-5).
[0119] [ka]
[0120] In general formulas (B-1) to (B-5), R is independently an alkyl group having 1 to 6 carbon atoms, with methyl, ethyl, propyl, and butyl groups being preferred, and ethyl and propyl groups being more preferred. In general formula (B-2), Y is a single bond, O, C=O, or C(CF3)2.
[0121] Half-esterified compounds can be produced, for example, by mixing a carboxylic acid anhydride (the anhydride of the aforementioned carboxylic acid compound) with an alcohol solvent and opening the ring of the carboxylic acid anhydride.
[0122] In this disclosure, the content of components derived from the crosslinking agent (B) in the resin layer is not particularly limited. For example, the ratio of the number of carbonyl groups (-(C=O)-Y) in the substance derived from the crosslinking agent (B) to the total number of nitrogen atoms in the substance derived from compound (A) ((-(C=O)-Y) / N) is preferably 0.1 to 3.0, more preferably 0.3 to 2.5, and even more preferably 0.4 to 2.2, respectively. Here, in -(C=O)-Y, Y represents an imide-crosslinked or amide-crosslinked nitrogen atom, OH, or ester group. By having (-(C=O)-Y) / N be 0.1 to 3.0, the resin layer preferably has a crosslinked structure such as an amide, amide-imide, or imide, and exhibits superior heat resistance.
[0123] (Polar solvent (D)) The laminate preparation step may involve applying a resin composition containing a resin material to at least one surface of the substrate. In this case, the resin composition containing the resin material preferably contains a polar solvent (D) along with the aforementioned compound (A), crosslinking agent (B), and other resin materials. Here, polar solvent (D) refers to a solvent having a relative permittivity of 5 or more at room temperature. Examples of polar solvents (D) include protic inorganic compounds such as water and heavy water; alcohols such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, isobutyl alcohol, isopentyl alcohol, cyclohexanol, ethylene glycol, propylene glycol, 2-methoxyethanol, 2-ethoxyethanol, benzyl alcohol, diethylene glycol, triethylene glycol, and glycerin; ethers such as tetrahydrofuran and dimethoxyethane; aldehydes and ketones such as furfural, acetone, ethyl methyl ketone, and cyclohexane; acid derivatives such as acetic anhydride, ethyl acetate, butyl acetate, ethylene carbonate, propylene carbonate, formaldehyde, N-methylformamide, N,N-dimethylformamide, N-methylacetamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, and hexamethylphosphate; nitriles such as acetonitrile and propionitrile; nitro compounds such as nitromethane and nitrobenzene; and sulfur compounds such as dimethyl sulfoxide. The polar solvent (D) preferably contains a protic solvent, more preferably contains water, and even more preferably contains ultrapure water. The content of the polar solvent (D) in the resin composition is not particularly limited, but is preferably 1.0% by mass or more and 99.99896% by mass or less, relative to the entire resin composition, and preferably 40% by mass or more and 99.99896% by mass or less. The boiling point of the polar solvent (D) is preferably 150°C or lower, and more preferably 120°C or lower, in order to volatilize the polar solvent (D) by heating when forming the resin layer and reduce the amount of residual solvent in the resin layer.
[0124] (Additive (C)) The resin composition containing the resin material may also contain an additive (C) in addition to the aforementioned compound (A), crosslinking agent (B), polar solvent (D), etc. Examples of additive (C) include an acid (C-1) having a carboxyl group and a weight-average molecular weight of 46 to 195, and a base (C-2) having a nitrogen atom and a weight-average molecular weight of 17 to 120, without a ring structure. Although the additive (C) volatilizes when heated during the formation of the resin layer, the resin layer in the substrate laminate of this disclosure may contain the additive (C).
[0125] Acid (C-1) is an acid with a carboxyl group and a weight-average molecular weight of 46 to 195. It is presumed that by including acid (C-1) as additive (C), aggregation due to association between compound (A) and crosslinking agent (B) is suppressed because an ionic bond is formed between the amino group in compound (A) and the carboxyl group in acid (C-1). More specifically, it is presumed that aggregation is suppressed because the interaction (e.g., electrostatic interaction) between the ammonium ion derived from the amino group in compound (A) and the carboxylate ion derived from the carboxyl group in acid (C-1) is stronger than the interaction between the ammonium ion derived from the amino group in compound (A) and the carboxylate ion derived from the carboxyl group in crosslinking agent (B). This disclosure is not limited in any way by the above presumption.
[0126] The acid (C-1) is not particularly limited as long as it has a carboxyl group and a weight-average molecular weight of 46 or more and 195 or less, and examples include monocarboxylic acid compounds, dicarboxylic acid compounds, and oxydicarboxylic acid compounds. More specifically, examples of acid (C-1) include formic acid, acetic acid, malonic acid, oxalic acid, citric acid, benzoic acid, lactic acid, glycolic acid, glyceric acid, butyric acid, methoxyacetic acid, ethoxyacetic acid, phthalic acid, terephthalic acid, picolinic acid, salicylic acid, and 3,4,5-trihydroxybenzoic acid.
[0127] In this disclosure, the content of acid (C-1) in the resin composition including the resin material is not particularly limited. For example, the ratio of the number of carboxyl groups in acid (C-1) to the total number of nitrogen atoms in compound (A) (COOH / N) is preferably 0.01 or more and 10 or less, more preferably 0.02 or more and 6 or less, and even more preferably 0.5 or more and 3 or less.
[0128] The base (C-2) is a base having a nitrogen atom and a weight-average molecular weight of 17 to 120. It is hypothesized that by including the base (C-2) as additive (C) in a resin composition containing a resin material, aggregation due to association between compound (A) and the crosslinking agent (B) is suppressed because the carboxyl group in the crosslinking agent (B) and the amino group in the base (C-2) form an ionic bond. More specifically, it is hypothesized that aggregation is suppressed because the interaction between the carboxylate ion derived from the carboxyl group in the crosslinking agent (B) and the ammonium ion derived from the amino group in the base (C-2) is stronger than the interaction between the ammonium ion derived from the amino group in compound (A) and the carboxylate ion derived from the carboxyl group in the crosslinking agent (B). This disclosure is not limited in any way by the above hypothetical.
[0129] The base (C-2) is not particularly limited as long as it has a nitrogen atom and does not have a ring structure with a weight-average molecular weight of 17 or more and 120 or less, and examples include monoamine compounds and diamine compounds. More specifically, examples of base (C-2) include ammonia, ethylamine, ethanolamine, diethylamine, triethylamine, ethylenediamine, N-acetylethylenediamine, N-(2-aminoethyl)ethanolamine, and N-(2-aminoethyl)glycine.
[0130] In this disclosure, the content of the base (C-2) in the resin composition including the resin material is not particularly limited. For example, the ratio of the number of nitrogen atoms in the base (C-2) to the number of carboxyl groups in the crosslinking agent (B) (N / COOH) is preferably 0.5 or more and 5 or less, and more preferably 0.9 or more and 3 or less.
[0131] When insulation is required for the resin layer of the substrate laminate of this disclosure, tetraethoxysilane, tetramethoxysilane, bistriethoxysilylethane, bistriethoxysilylmethane, bis(methyldiethoxysilyl)ethane, 1,1,3,3,5,5-hexaethoxy-1,3,5-trisilacyclohexane, 1,3,5,7-tetramethyl-1,3,5,7-tetrahydroxylcyclosiloxane, 1,1,4,4-tetramethyl-1,4-diethoxydisylethylene, and 1,3,5-trimethyl-1,3,5-trimethyl-1,3,5-triethoxy-1,3,5-trisilacyclohexane may be mixed in to improve insulation or mechanical strength. Furthermore, methyltriethoxysilane, dimethyldiethoxysilane, trimethylethoxysilane, etc. may be mixed in to improve the hydrophobicity of the insulating resin layer. These compounds may be mixed to control etching selectivity.
[0132] The resin composition containing the resin material may also contain a solvent other than the polar solvent (D), such as n-hexane.
[0133] Furthermore, the resin composition containing the resin material may also contain, for example, phthalic acid, benzoic acid, or derivatives thereof, to improve electrical properties. Furthermore, the resin composition containing the resin material may also contain benzotriazole or a derivative thereof, for example, to suppress the corrosion of copper.
[0134] The pH of the resin composition containing the resin material is not particularly limited, but is preferably 2.0 or higher and 12.0 or lower.
[0135] Furthermore, when using an acid (C-1) as additive (C), it is preferable to mix the mixture of acid (C-1) and compound (A) with the crosslinking agent (B). That is, it is preferable to pre-mix compound (A) and acid (C-1) before mixing compound (A) and crosslinking agent (B). This effectively suppresses clouding and gelation of the resin composition containing the resin material when compound (A) and crosslinking agent (B) are mixed (gelation can cause delays in the transparency of the resin composition, which is undesirable).
[0136] Furthermore, when using a base (C-2) as additive (C), it is preferable to mix the mixture of the base (C-2) and the crosslinking agent (B) with compound (A). In other words, it is preferable to pre-mix the crosslinking agent (B) and the base (C-2) before mixing compound (A) and the crosslinking agent (B). This effectively suppresses clouding and gelation of the resin composition containing the resin material when compound (A) and the crosslinking agent (B) are mixed (gelation can cause delays in the transparency of the resin composition, which is undesirable).
[0137] Methods for applying a resin material to at least one surface of a substrate include vapor deposition methods such as vapor deposition polymerization, CVD (chemical vapor deposition), and ALD (atomic layer deposition), as well as coating methods such as dipping, spraying, spin coating, and bar coating. When applying a resin material by coating, it is preferable to apply a resin composition containing the aforementioned resin material. For example, when forming a film with a thickness of micron size, it is preferable to use the bar coating method, and when forming a film with a thickness of nano size (several nanometers to several hundred nanometers), it is preferable to use the spin coating method. The thickness of the resin material can be appropriately adjusted according to the intended thickness of the resin layer.
[0138] For example, the method of applying the resin material by the spin coating method is not particularly limited. For instance, a method can be used in which a resin composition containing the resin material is dropped onto the surface of a first substrate while the substrate is rotated in a spin coater, and then the rotation speed of the substrate is increased to dry it. In a method of applying resin material by spin coating, there are no particular restrictions on conditions such as the rotation speed of the substrate, the amount and duration of the resin composition containing the resin material, and the rotation speed of the substrate during drying. These conditions can be adjusted as appropriate while considering the thickness of the resin material to be formed.
[0139] A substrate coated with resin material may be cleaned to remove any excess resin material. Cleaning methods include wet cleaning with a rinsing solution such as a polar solvent, and plasma cleaning.
[0140] In the method for manufacturing a substrate laminate according to the present disclosure, the laminate preparation step may include a step of curing a resin material applied to one side of a substrate to form a resin layer. For example, the resin material is cured by heating or the like to form a resin layer. In this case, if the resin material contains a thermosetting compound, it is cured by heating the resin material at a temperature above the curing temperature.
[0141] It is preferable to heat and cure the resin material applied to one side of the substrate at 100°C to 450°C. The aforementioned temperature refers to the surface temperature of the resin material applied to the surface. By heating the resin material, the solvent in the resin composition containing the resin material is removed. Furthermore, the components in the resin material react to obtain a cured product, forming a resin layer containing this cured product. From the viewpoint of suppressing thermal damage to devices such as semiconductor memory, the aforementioned temperature is preferably 150°C to 450°C, more preferably 180°C to 400°C, even more preferably 180°C to 250°C, and particularly preferably 180°C to 200°C.
[0142] Furthermore, there are no particular restrictions on the pressure when the resin material applied to the surface is heated, but an absolute pressure of 17 Pa or less is preferred. The absolute pressure is more preferably 1000 Pa or more and atmospheric pressure or less, even more preferably 5000 Pa or more and atmospheric pressure or less, and particularly preferably 10000 Pa or more and atmospheric pressure or less.
[0143] The resin material applied to the surface can be heated by a conventional method using a furnace or hot plate. Examples of furnaces that can be used include the SPX-1120 manufactured by Apex Corporation and the VF-1000LP manufactured by Koyo Thermo Systems Co., Ltd. Furthermore, the heating of the resin material applied to the surface may be carried out in an atmospheric environment or in an inert gas (nitrogen gas, argon gas, helium gas, etc.) atmosphere.
[0144] There are no particular restrictions on the heating time of the resin material applied to the surface, for example, it may be 3 hours or less, and preferably 1 hour or less. There are no particular restrictions on the lower limit of the heating time, and it may be 5 minutes, for example.
[0145] To shorten the curing time of the resin material applied to the surface, the resin material applied to the surface may be irradiated with ultraviolet (UV) light. Preferred UV light includes ultraviolet light with wavelengths of 170 nm to 230 nm, excimer light with a wavelength of 222 nm, and excimer light with a wavelength of 172 nm. It is also preferable to perform UV irradiation in an inert gas atmosphere.
[0146] Whether a resin material has hardened can be confirmed, for example, by measuring the peak intensity of specific bonds and structures using FT-IR (Fourier Transform Infrared Spectroscopy). Examples of specific bonds and structures include those generated by crosslinking reactions. For example, if amide bonds, imide bonds, siloxane bonds, tetrahydronaphthalene structures, oxazole ring structures, etc., are formed, it can be determined that the resin material has hardened, and this can be confirmed by measuring the peak intensities derived from these bonds, structures, etc., using FT-IR. The amide bond is approximately 1650 cm². -1 and approximately 1520cm -1 This can be confirmed by the presence of vibration peaks. The imide bond is approximately 1770 cm -1 and approximately 1720cm -1 This can be confirmed by the presence of vibration peaks. Siloxane bonds are 1000 cm-1 ~1080cm -1 This can be confirmed by the presence of vibration peaks between them. The tetrahydronaphthalene structure is 1500 cm -1 This can be confirmed by the presence of vibration peaks between them. The oxazole ring structure is approximately 1625 cm². -1 and approximately 1460cm -1 This can be confirmed by the presence of vibration peaks.
[0147] The resin layer obtained by curing the resin material preferably has a siloxane bond and at least one bond selected from the group consisting of ester bonds, ether bonds, amide bonds, and imide bonds, and more preferably has a siloxane bond and an imide bond.
[0148] The resin layer formed by curing the resin material preferably contains 10 ppb by mass or less of sodium and potassium on an elemental basis. If the sodium or potassium content is 10 ppb by mass or less on an elemental basis, it is possible to suppress problems with the electrical characteristics of the semiconductor device, such as transistor malfunctions.
[0149] The amount of silicon on the surface of the resin layer is preferably 20 atomic% or less, more preferably 15 atomic% or less, and even more preferably 10 atomic% or less, independently of each other. The amount of silicon on the surface of the resin layer can be evaluated by measuring the atomic ratio using X-ray photoelectron spectroscopy (XPS). Specifically, using an XPS instrument such as AXIS-NOVA (manufactured by KRATOS), the atomic ratio can be measured from the peak intensity of the narrow spectrum when the total amount of each element detected in the wide spectrum is set to 100%.
[0150] The thickness of the resin layer is preferably 0.001 μm to 8.0 μm, more preferably 0.01 μm to 6.0 μm, and even more preferably 0.03 μm to 5.0 μm. A resin layer thickness of 0.001 μm or more can increase the bonding strength with inorganic material layers, other layers, etc. A resin layer thickness of 8.0 μm or less can suppress variations in the thickness of the resin layer when forming a resin layer on a large-area substrate.
[0151] When electrodes are provided on a portion of the surface of the resin layer, the thickness of the resin layer is preferably 0.01 μm to 8.0 μm, more preferably 0.03 μm to 6.0 μm, and even more preferably 0.05 μm to 5.0 μm, from the viewpoint of improving bonding strength with inorganic material layers, other layers, etc., and suppressing variations in the thickness of the resin layer.
[0152] When electrodes are not provided on the surface of the resin layer, the thickness of the resin layer is preferably 0.001 μm or more and less than 1.0 μm, more preferably 0.01 μm to 0.8 μm, and even more preferably 0.03 μm to 0.6 μm, from the viewpoint of improving bonding strength with inorganic material layers, other layers, etc., and suppressing variations in the thickness of the resin layer.
[0153] The resin layer preferably has functional groups on its surface that can form chemical bonds, in order to increase the bonding strength between the first and second laminates in the substrate laminate. More preferably, it has at least one functional group selected from the group consisting of silanol groups (Si-OH groups), amino groups, epoxy groups, hydroxyl groups, and functional groups having unsaturated bonds. In terms of heat resistance, it is even more preferable to have silanol groups. These functional groups may be formed by surface treatment after the formation of the resin layer, or by treatment with a silane coupling agent, etc. Alternatively, compounds containing these functional groups may be mixed into the resin composition. Examples of functional groups containing unsaturated bonds include vinyl groups, allyl groups, acrylic groups, methacrylic groups, and styryl groups.
[0154] Whether or not the surface of a resin layer contains Si-OH groups can be evaluated by surface analysis of the resin layer using time-of-flight secondary ion mass spectrometry (TOF-SIMS). Specifically, using the TOF-SIMS PHI nanoTOFII (ULVAC-PHI, Inc.), the presence or absence of a peak with a mass-to-charge ratio (m / Z) of 45 can be used to evaluate whether or not the surface of the resin layer contains Si-OH groups.
[0155] After forming the resin layer, the resin layer may be planarized. Methods for planarization include fly-cutting and chemical mechanical polishing (CMP). One planarization method may be used alone, or two or more methods may be used in combination.
[0156] After forming the resin layer, the resin layer may be cleaned. Cleaning methods include wet cleaning with a rinsing solution and dry cleaning using plasma, etc. Examples of wet cleaning include ultrasonic cleaning using pure water and spin cleaning using solvents such as NMP.
[0157] (electrode) The first laminate and the second laminate may each have electrodes exposed on one or part of both sides. In the lamination process, it is preferable that the electrodes are arranged so that the electrode provided on the first surface layer side of the first laminate and the electrode provided on the second back surface layer side of the second laminate are in contact with each other.
[0158] The first laminate may have through-holes that penetrate from the surface on the first surface layer side to the surface on the first back layer side, and electrodes that penetrate the first laminate may be provided in these through-holes. Similarly, the second laminate may have through-holes that penetrate from the surface on the second surface layer side to the surface on the second back layer side, and electrodes that penetrate the second laminate may be provided in these through-holes.
[0159] The electrode material is not particularly limited and can be any conventionally known electrode material. Specifically, it can be copper, solder, tin, gold, silver, aluminum, indium, cobalt, tungsten, etc.
[0160] The method for providing electrodes to the laminate is not particularly limited, and conventionally known methods can be employed. For example, electrodes may be formed on the surface to which the resin material is applied before the resin layer of the laminate is formed, or electrodes may be formed on the surface to which the resin layer is formed after the resin layer has been formed. Furthermore, electrodes may be formed on the surface on which the inorganic material layer is formed before the inorganic material layer of the laminate is formed, or electrodes may be formed on the surface on which the inorganic material layer is formed after the inorganic material layer has been formed.
[0161] The electrodes may be formed as convex shapes on the surface of the substrate, may be formed in a manner that penetrates the substrate, or may be formed in a manner that is embedded in the substrate.
[0162] Furthermore, when forming a resin layer on one side of a substrate and an inorganic material layer on the other side, the order in which the resin layer and the inorganic material layer are formed is not particularly limited. For example, the resin layer may be formed on one side of the substrate first, and then the inorganic material layer on the other side, or conversely, the inorganic material layer may be formed first, and then the resin layer may be formed.
[0163] If the electrode is formed before the resin layer or inorganic material layer is formed, the electrode is provided on a portion of the surface of the resin layer or inorganic material layer by removing the resin layer or inorganic material layer from the electrode after the resin layer or inorganic material layer has been formed. Methods for removing the resin layer or inorganic material layer from the electrode include fly cutting, chemical mechanical polishing (CMP), and plasma dry etching. One removal method may be used alone, or two or more methods may be used in combination. For example, in the fly cutting method, a surface planer (DFS8910 (manufactured by DISCO Corporation)) can be used. When using CMP, the slurry may be, for example, a slurry containing silica or alumina, which is commonly used for polishing resins, or a slurry containing hydrogen peroxide and silica, which is commonly used for polishing metals. When using plasma dry etching, fluorocarbon plasma, oxygen plasma, etc., may be used.
[0164] If the resin or inorganic material layer on the electrode is removed and the electrode is exposed, the oxide on the electrode surface may be reduced as needed. Methods for reduction include heating the substrate in an acidic atmosphere such as formic acid at 100°C to 300°C, or heating the substrate in a hydrogen atmosphere. These treatments may be performed simultaneously with the bonding process described later.
[0165] When electrodes are formed after the resin layer or inorganic material layer has been formed, for example, holes for electrode formation may be formed in the surface of the substrate where the resin layer or inorganic material layer has been formed using a known method, and electrodes may be formed in the formed holes. Methods for forming holes include dry etching using gas and laser ablation.
[0166] Methods for forming electrodes include electroplating, electroless plating, sputtering, and inkjet methods.
[0167] If the resin material is photosensitive, holes may be formed in the resin material applied to at least one surface of the substrate by photolithography to form electrodes. After curing the resin material to form a resin layer, electrodes may be formed in the formed holes.
[0168] [Surface protection process] The method for manufacturing the substrate laminate of this disclosure includes a surface protection step of providing a surface protection layer 27 on the second surface layer 22 (Figure 3(6)).
[0169] By applying a surface protection layer on the second surface layer before the dicing process, contamination of the second surface layer by the dicing tape and damage to the second surface layer when peeling the chips of the second laminate from the dicing tape after the dicing process can be prevented.
[0170] The surface protection layer is not particularly limited as long as it protects the second surface layer and does not dissolve the resin or inorganic material layers constituting the first and second laminates during the cleaning and removal process, and the surface protection layer can be selectively removed. Examples include water-soluble resins, or photoresists that can be cleaned with organic solvents such as TMAH (tetramethylammonium hydroxide) or NMP (N-methyl-2-pyrrolidone). As a water-soluble resin, Hogomax from Disco may be used. The method for forming the surface protective layer 27 is not particularly limited. For example, a method may be used in which a composition for forming the surface protective layer 27 is spin-coated onto the second surface layer 22, and then cured by drying, heating, etc. The thickness of the surface protective layer 27 can be, for example, in the range of 0.1 μm to 1 mm.
[0171] Examples of cleaning and removal methods for each layer of the laminate, the surface protective layer, and the surface protective layer include the following combinations. Inorganic layer: SiO2 Resin layer: Resin layer containing imide bonds Surface protective layer: Sumitomo Chemical Co., Ltd. Positive-type photoresist Sumiresist PFI-58A7MS Washing and removal method: TMAH (Formation of surface protective layer) After spin-coating a positive-type photoresist onto the substrate surface, the entire surface was exposed to UV light to form a surface protective layer. The thickness of the surface protective layer was 1 μm. (Cleaning and removal of the surface protective layer) The surface protective layer was removed by dropping a positive-type photoresist developer (Tokuyama Corporation SD-1) onto the substrate surface for 65 seconds, followed by washing with pure water.
[0172] [Dicing process] The manufacturing method of the substrate laminate of this disclosure includes a dicing step in which a dicing tape 42 is attached to the surface protection layer side of a second laminate 20 provided with a surface protection layer 27, and dicing is performed to separate the second laminate 20A into individual chips 28A with a surface protection layer, each chip including the divided second laminate 20A and the surface protection layer 27A (Figures 4(7), (8)).
[0173] After applying a surface protection layer 27 to the first surface layer 22, the second laminate 20 is peeled off from the temporary support 31, and as shown in Figure 4(7), the surface protection layer side is bonded to the dicing tape 42, and cleaned as necessary. Next, as shown in Figure 4(8), dicing is performed from the back surface layer 23 side of the second laminate 20, and the second laminate 20, including the surface protection layer 27, is broken down into individual chips 28A. As the dicing tape 42, for example, a dicing tape 42 can be used in which an adhesive layer is provided on one side of a resin film, the adhesive strength of which decreases when exposed to ultraviolet (UV) light. Through dicing, the second back resin layer 23, the silicon substrate 21, the second surface inorganic material layer 22, and the surface protective layer 27 are separated into the second back resin layer 23A, the silicon substrate 21A, the second surface inorganic material layer 22A, and the surface protective layer 27A, respectively. For dicing, for example, a dicer (DAD6340 (manufactured by DISCO Corporation)) can be used. Alternatively, dicing may be performed using stealth dicing or plasma dicing.
[0174] The method for manufacturing a substrate laminate according to this disclosure may include a step of cleaning the diced second laminate, etc., after the dicing step and before the lamination step, in order to remove particles, etc. Furthermore, the first surface layer of the first laminate may be cleaned, and in particular, the first surface layer may be cleaned before it comes into contact with other layers (e.g., resin layers) during the lamination process.
[0175] The cleaning method is not particularly limited and may include wet cleaning using solvents such as alkaline cleaning solutions, acidic cleaning solutions, hydrofluoric acid-containing cleaning solutions, and manganese-containing solutions (desmear solutions); wet cleaning using pure water; and dry cleaning using UV ozone, plasma, etc.
[0176] [Lamination process] The manufacturing method of the substrate laminate of this disclosure includes a lamination step of peeling a chip 28A with a surface protection layer, which includes a chipped second laminate and a surface protection layer, from a dicing tape 42, and laminating the chip 28A with a surface protection layer on the first laminate 10 such that the first surface layer 12 and the second back surface layer 23A are in contact (Figure 5(10), (11)).
[0177] The lamination process is a process of bringing the first surface layer and the second back layer into contact with each other before joining the first laminate and the second laminate via the first surface layer and the second back layer (for example, the first surface inorganic material layer and the second back resin layer) in the bonding process described later. For example, after reducing the adhesive strength of the dicing tape 42 by ultraviolet irradiation, the chip 28A with the surface protective layer is peeled off the dicing tape 42 by pushing it up from the back side with a needle 51. The chip 28A with the surface protective layer is laminated on the first laminate 10 so that the desired positional relationship is achieved when the first laminate 10 and the second laminate chip 28A are joined.
[0178] For example, if the aforementioned electrodes are provided on the first laminate and the second laminate respectively, a chip 28A with a surface protection layer is laminated on the first laminate 10 such that the electrode 14 provided on the first surface layer side contacts the electrode 25 provided on the second back surface layer side.
[0179] When bringing an inorganic material layer and a resin layer into contact during the lamination process, it is preferable that the curing rate of the resin layer before contact is between 70% and 100%. This ensures that the first laminate and the second laminate chip are firmly bonded in the temporary fixing process and the bonding process described later, and that misalignment of the bonded parts is less likely to occur.
[0180] The curing rate of the resin layer is more preferably 80% or higher, even more preferably 85% or higher, particularly preferably 90% or higher, and even more preferably 93% or higher. Furthermore, the curing rate of the resin layer may be 100%, 99% or lower, 95% or lower, or 90% or lower. The curing rate of the resin layer may be the curing rate before contact with other layers (for example, other inorganic material layers).
[0181] The curing rate of a resin layer containing at least one selected from the group consisting of amide bonds, imide bonds, siloxane bonds, tetrahydronaphthalene structures, oxazole ring structures, ester bonds, and ether bonds is more preferably 80% or higher, even more preferably 85% or higher, particularly preferably 90% or higher, and even more preferably 93% or higher. The curing rate of a resin layer containing a siloxane bond and at least one selected from the group consisting of ester bonds, ether bonds, amide bonds, and imide bonds is more preferably 80% or higher, even more preferably 85% or higher, particularly preferably 90% or higher, and even more preferably 93% or higher.
[0182] The curing rate of a resin layer formed by curing a resin material may be determined by measuring the peak intensity of specific bonds and structures (the sum of the peak intensities if there are multiple peaks, such as imides and amides) using FT-IR (Fourier transform infrared spectroscopy) in the resin material before it is applied to the substrate, the resin layer before contact with the inorganic material layer during the lamination process, and the resin layer after the bonding process, and then determining the rate of increase or decrease in the peak intensity. In cases where there are band-shaped peaks that are difficult to separate, such as siloxane bonds, the maximum peak intensity should be adopted.
[0183] Specifically, if a particular bond and structure are generated by the curing reaction, the rate of increase in peak intensity may be calculated using the following formula, and the calculated value may be used as the curing rate of the resin layer. Increase rate of peak intensity (curing rate of resin layer) = [(Peak intensity of specific bonds and structure of the resin layer before contact between the resin layer and the inorganic material layer in the lamination process) / (Peak intensity of specific bonds and structure of the resin layer after heating at 300°C for 1 hour in the bonding process)] × 100 Background signal rejection can be performed using standard methods. Furthermore, FT-IR measurements can be performed using either the transmission or reflection method as needed.
[0184] In the aforementioned rate of increase in peak intensity, if there are multiple bonds and structures that cause an increase in peak intensity, the peak intensity may be interpreted as the sum of the multiple peak intensities.
[0185] Before the resin layer and the inorganic material layer come into contact during the lamination process, the composite modulus of the resin layer at 23°C is preferably 0.1 GPa or more and 20 GPa or less, and more preferably 0.1 GPa or more and 10 GPa or less. This tends to suppress the generation of voids, as the voids formed when the resin layer and the inorganic material layer come into contact during the lamination process are absorbed by the resin layer during the bonding process.
[0186] The composite modulus of the aforementioned resin layer at 23°C is preferably 8 GPa or less, and more preferably 6 GPa or less, from the viewpoint of effectively suppressing the generation of voids. Furthermore, the composite modulus of the aforementioned resin layer at 23°C is preferably 0.1 GPa or more, and more preferably 1 GPa or more, from the viewpoint of effectively suppressing alignment misalignment. Furthermore, the preferred range for the composite modulus of the resin layer at 23°C is the same as the preferred range for the composite modulus of the resin layer at 23°C. The composite modulus of the resin layer at 23°C may also be the composite modulus at 23°C before contact with other layers (e.g., other inorganic material layers).
[0187] The composite modulus of the resin layer at 23°C can be measured by the method described below. A resin composition containing resin material is prepared, spin-coated onto a silicon substrate, and then heated at 400°C for 10 minutes to prepare a measurement sample. For the prepared measurement sample, the unloading-displacement curve at 23°C is measured using a nanoindenter (product name TI-950 Tribo Indenter, Hysitron, Berkovich type indenter) at a test depth of 20 nm. The composite modulus at 23°C is calculated from the maximum load and maximum displacement according to the calculation method described in the reference (Handbook of Micro / nano Tribology (second Edition), edited by Bharat Bhushan, CRC Press). Here, the composite modulus of elasticity is defined by the following equation (1). In equation (1), E r represents the composite modulus, E i ν represents the Young's modulus of the indenter, which is 1140 GPa. i This represents the Poisson's ratio of the indenter, which is 0.07, and E s and ν s These represent the Young's modulus and Poisson's ratio of the sample, respectively.
[0188]
number
[0189] Before bringing the first surface layer and the second back layer into contact during the lamination process, the surface roughness (Ra) of the first surface layer is preferably 0.01 nm to 1.2 nm, and more preferably 0.1 nm to 1.0 nm. This facilitates the temporary fixing of the first surface layer and the second back layer, as described later, at low temperatures. Furthermore, the preferred range for the surface roughness (Ra) of the second back layer is the same as the preferred range for the surface roughness (Ra) of the first front layer. The surface roughness (Ra) of each layer may be the same as the surface roughness (Ra) of each layer before they come into contact with each other. The surface roughness of each layer can be evaluated by morphological observation using a scanning probe microscope (SPM). Specifically, using the SPA400 SPM (manufactured by Hitachi High-Technologies), surface roughness can be determined by measuring a 3 μm × 3 μm square area in dynamic force microscope mode.
[0190] The method for manufacturing a substrate laminate according to this disclosure may include the following steps prior to the lamination step described above. The following steps are preferably performed after the laminate preparation step and before the lamination step.
[0191] The manufacturing method of the substrate laminate according to this disclosure may include a step of applying a surface activation treatment to the second back layer before the lamination process. By applying the surface activation treatment, the bonding strength between the first surface layer and the second back layer can be increased. In particular, when electrodes are provided on the bonding surface of the first laminate and the second laminate and the electrodes are bonded together, it is preferable to apply the surface activation treatment from the viewpoint of promoting the diffusion of metals such as copper contained in the electrodes to increase the bonding strength between the electrodes, and from the viewpoint of reducing the heating temperature during metal diffusion. Furthermore, the first surface layer on the first substrate may also be subjected to a surface activation treatment, and in particular, the first surface layer may be subjected to a surface activation treatment before it comes into contact with other layers (for example, other resin layers).
[0192] Specific examples of surface activation treatments include plasma treatment and FAB (Fast Atom Bombardment) treatment.
[0193] [Temporary fixing process] The manufacturing method for the substrate laminate of this disclosure includes a temporary fixing step in which the stacked first laminate 10 and the chip 28A with a surface protection layer are temporarily fixed at a first temperature (Figure 5(11)). Depending on the resin layer 23A, temporary fixing to the inorganic material layer 12 may occur even at room temperature, so the temporary fixing step is a part of the lamination process and can be considered to be included in the lamination process.
[0194] The temporary fixation of the first laminate and the chip with the surface protective layer is performed at a first temperature, for example, a low temperature of room temperature (e.g., 23°C) or higher but less than 100°C. Preferably, it is performed at a low temperature of room temperature or higher but 50°C or lower, and more preferably at room temperature. When the first and second substrates include silicon substrates, the surface energy of the bonding interface between the two laminates in a temporarily fixed state is 0.05 J / m², considering ease of handling during the bonding process, suppression of alignment misalignment (bonding position misalignment), and suppression of foreign matter contamination. 2 Preferably, it is 0.1 J / m 2 It is more preferable that the value be greater than or equal to 0.15 J / m 2 It is even more preferable that the above conditions are met. The surface energy (bonding strength) of the aforementioned bonding interface can be determined by a blade insertion test according to the method described in the non-patent document "MPMaszara, G.Goetz, A.Cavigila, and JBMckitterick, Journal of Applied Physics, 64 (1988) 4943-4950." A blade with a thickness of 0.1 mm to 0.3 mm is inserted into the bonding interface of a temporarily fixed laminate, and the distance from the blade tip to the delamination of the laminate is measured using an infrared light source and an infrared camera. The surface energy can then be determined based on the following formula. γ = 3 × 10 9 ×t b 2 ×E 2 ×t 6 / (32×L 4 ×E×t 3 ) Here, γ is the surface energy (J / m 2 ), t b θ represents the blade thickness (m), E represents the Young's modulus (GPa) of the silicon substrate contained in the first and second substrates, t represents the thickness of the first and second substrates (m), and L represents the delamination distance from the blade tip (m).
[0195] [Cleaning and Removal Process] The manufacturing method of the substrate laminate according to the present disclosure includes a cleaning and removal step after the lamination step, or, if a temporary fixing step is performed after the lamination step (including when the temporary fixing step is performed as part of the lamination step), after the temporary fixing step, in which the first laminate 10 and the chip 28A with a surface protection layer are cleaned and the surface protection layer 27A is removed (Figure 6(12)). As a cleaning and removal method for removing the surface protective layer, a cleaning and removal means is used that can remove the surface protective layer without causing misalignment between the laminated first laminate 10 and the chip 28A with the surface protective layer, and that can maintain the lamination (temporary fixing) of the first laminate and the second laminate chip without dissolving the second back surface resin layer, for example. Such cleaning and removal methods can be selected according to the materials of the surface protective layer, the first surface layer, the second back layer, etc. Specifically, examples include a developer containing TMAH and an organic solvent such as NMP (N-methyl-2-pyrrolidone).
[0196] [Joining process] The manufacturing method of the substrate laminate according to the present disclosure includes a bonding step of heating a first laminate 10 and a second laminate chip 20A from which the surface protective layer 27A has been removed to obtain a substrate laminate 100 in which the second laminate chip 20A is bonded onto the first laminate 10. In the bonding step, heating is performed at a second temperature higher than the first temperature in the temporary fixing step, for example, 100°C or higher. The bonding step yields a substrate laminate 100 in which the first laminate and the second laminate chip are bonded via a first surface layer and a second back surface layer.
[0197] There are no particular restrictions on the pressure used when joining the first laminate and the second laminate chip, with an absolute pressure of 10 -4 A pressure of less than or equal to Pa (superatmospheric pressure) is preferable. The aforementioned absolute pressure is 10 -3 A pressure of Pa or higher and below atmospheric pressure is more preferable, a pressure of 100 Pa or higher and below atmospheric pressure is even more preferable, and a pressure of 1000 Pa or higher and below atmospheric pressure is particularly preferable. When joining the first laminate and the second laminate chip, the process may be carried out in an atmospheric environment or in an inert gas (nitrogen gas, argon gas, helium gas, etc.) atmosphere.
[0198] In the bonding process, it is preferable to heat the temporarily fixed first laminate and second laminate chip at 100°C to 450°C with the first surface inorganic material layer and the second back surface resin layer in contact. The aforementioned heating temperature refers to the surface temperature of the second surface layer. The heating temperature is preferably 100°C to 400°C, more preferably 130°C to 350°C, even more preferably 150°C to 300°C, even more preferably 150°C to 250°C, and particularly preferably 150°C to 200°C.
[0199] When the electrodes are arranged in the lamination process such that the first surface electrode provided on the first surface layer side is in contact with the second back electrode provided on the second back layer side, the aforementioned temperature is preferably 130°C or higher, more preferably 150°C or higher, and even more preferably 200°C or higher. This causes the components (e.g., copper) contained in the first surface electrode provided on the first surface layer side and the second back electrode provided on the second back layer side to diffuse, and the bonding strength between the electrodes tends to increase.
[0200] Heating during the joining process can be carried out by conventional methods using a furnace or hot plate. Furthermore, the heating in the joining process may be carried out in an atmospheric environment or in an inert gas (nitrogen gas, argon gas, helium gas, etc.) atmosphere. There are no particular restrictions on the heating time in the joining process; for example, it may be 3 hours or less, and preferably 1 hour or less. There are no particular restrictions on the lower limit of the heating time; for example, it may be 5 minutes.
[0201] In the bonding process, to increase the bonding strength between the first laminate and the second laminate, the first laminate and the second laminate chip may be pressurized while the first surface layer and the second back layer are in contact. Pressurization may be performed simultaneously with heating. The pressure applied when pressurizing the temporarily fixed first laminate and second laminate chip is not particularly limited, but is preferably 0.1 MPa to 10 MPa, and more preferably 0.1 MPa to 5 MPa. As a pressurizing device, for example, a TEST MINI PRESS manufactured by Toyo Seiki Seisakusho Co., Ltd. can be used.
[0202] The manufacturing method of the substrate laminate according to this disclosure may include, after the bonding step, a step of providing through holes in the thickness direction of the first laminate and the second laminate, and forming electrodes in the through holes that penetrate the first laminate and the second laminate. Preferably, if electrodes are not formed in the substrate laminate obtained in the bonding step, this electrode formation step is performed so that electrodes that penetrate the first laminate and the second laminate are formed in the through holes.
[0203] For example, through holes penetrating the first and second laminates may be formed by known methods, and electrodes may be formed in the formed holes. Methods for forming the holes include dry etching using gas and laser ablation.
[0204] Methods for forming electrodes that penetrate the first and second laminates include electroplating, electroless plating, sputtering, and inkjet methods.
[0205] The material for the electrodes penetrating the first and second laminates is not particularly limited and includes conventionally known electrode materials. Specifically, examples include copper, solder, tin, gold, silver, aluminum, indium, cobalt, tungsten, and the like.
[0206] In the method for manufacturing a substrate laminate according to the present disclosure, after the temporary fixing step, the second laminate chip before the bonding step may be considered as the first laminate in the laminate preparation step, and the process from the laminate preparation step to the temporary fixing step may be repeated one or more times before the bonding step so that two or more layers of chips of the second laminate are stacked and temporarily fixed, and the bonding step may be performed after the final temporary fixing step.
[0207] For example, by repeating the steps from the laminate preparation step to the temporary fixing step three times and then performing the bonding step, as shown in FIG. 7, a substrate laminate 200 in which second laminate chips 20A, 20B, and 20C are stacked in three tiers on the first laminate 10 can be manufactured. According to such a method, the substrate laminate 200 in which the second laminate chips 20A, 20B, and 20C are bonded in multiple stages can be manufactured through a single bonding step. Therefore, damage to each laminate caused by heating can be suppressed, and the manufacturing cost associated with the bonding step can also be kept low. The second laminate chips 20A, 20B, and 20C bonded to each other at each tier may have the same configuration or may have different configurations. The number of tiers of the stacked second laminate chips is not particularly limited and can be set as needed.
[0208] In the method for manufacturing a substrate laminate of the present disclosure, after the bonding step, a thinning process (back grinding) may be performed on the surface of the substrate laminate as necessary.
[0209] (Example of laminated structure of substrate laminate) Examples of the laminated structure of the substrate laminate for each application are shown below. Note that the bonding layer means a layer in a bonded state composed of an inorganic material layer / a resin layer. For MEMS packaging; Si / bonding layer / Si, SiO2 / bonding layer / Si, SiO2 / bonding layer / SiO2, Cu / bonding layer / Cu, For microchannels; PDMS / bonding layer / PDMS, PDMS / bonding layer / SiO2, For CMOS image sensors; SiO2 / bonding layer / SiO2, Si / bonding layer / Si, SiO2 / bonding layer / Si, For through-silicon vias (TSV); SiO2 (with Cu electrode) / bonding layer / SiO2 (with Cu electrode), Si (with Cu electrode) / bonding layer / Si (with Cu electrode), For optical devices; (InGaAlAs, InGaAs, InP, GaAs) / bonding layer / Si, For LEDs; (InGaAlAs, GaAs, GaN) / bonding layer / Si, (InGaAlAs, GaAs, GaN) / bonding layer / SiO2, (InGaAlAs, GaAs, GaN) / bonding layer / (Au, Ag, Al), (InGaAlAs, GaAs, GaN) / bonding layer / Sapphire.
[0210] The disclosure of Japanese Patent Application No. 2023-024730, filed on 20 February 2023, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated by reference to the same extent as if each individual document, patent application, and technical standard were specifically and individually noted to be incorporated by reference. [Explanation of Symbols]
[0211] 10. First Laminate 11. First substrate 12 First surface layer 13. First back layer 20 Second Laminate 21 Second substrate 22 Second surface layer 23. Second back layer 42 Dicing Tapes 100 substrate stack 200 substrate stack
Claims
1. A laminate preparation step for preparing a first laminate in which a first surface layer, a first substrate, and a first back layer are stacked in that order, and a second laminate in which a second surface layer, a second substrate, and a second back layer are stacked in that order, A surface protection step of providing a surface protection layer on the second surface layer of the second laminate, A dicing process is performed by attaching a dicing tape to the surface protection layer side of the second laminate having the surface protection layer, thereby dividing it into individual chips with a surface protection layer, each chip containing the divided second laminate and the surface protection layer. A lamination step of peeling the chip with the surface protection layer from the dicing tape and laminating the chip with the surface protection layer on the first laminate such that the first surface layer and the second back surface layer are in contact, A cleaning and removal step involves cleaning the stacked first laminate and the chip with the surface protective layer, and removing the surface protective layer. A bonding step of heating the first laminate and the chip of the second laminate from which the surface protective layer has been removed to obtain a substrate laminate in which the chip of the second laminate is bonded onto the first laminate, A method for manufacturing a substrate laminate containing [the specified material].
2. The first laminate comprises a first electrode exposed from the first surface layer and the first back layer, The second laminate comprises a second electrode exposed from the second surface layer and the second back layer, The method for manufacturing a substrate laminate according to claim 1, wherein in the lamination step, the chip with the surface protective layer is laminated on the first laminate such that the first electrode exposed from the first surface layer and the second electrode exposed from the second back surface layer are in contact with each other.
3. The aforementioned first surface layer is an inorganic material layer formed of an inorganic material, The second back surface layer is a resin layer formed of resin, The lamination process includes a temporary fixing step of temporarily fixing the laminated first laminate and the chip with the surface protection layer at a first temperature. The method for manufacturing a substrate laminate according to claim 1 or claim 2, wherein the bonding step is a step of heating the temporarily fixed first laminate and the chip of the second laminate at a second temperature higher than the first temperature.
4. The method for manufacturing a substrate laminate according to claim 3, wherein, after the temporary fixing step, the chips of the second laminate before the bonding step are considered to be the first laminate in the laminate preparation step, and the process from the laminate preparation step to the temporary fixing step is repeated one or more times before the bonding step so that the chips of the second laminate are stacked in two or more layers and temporarily fixed, and after the last temporary fixing step, the bonding step is performed.
5. The method for producing a substrate laminate according to claim 3, wherein the surface of the resin layer has at least one functional group selected from the group consisting of silanol groups, amino groups, epoxy groups, hydroxyl groups, and functional groups having unsaturated bonds.
6. The method for manufacturing a substrate laminate according to claim 3, wherein the resin layer comprises a siloxane bond and at least one selected from the group consisting of an ester bond, an ether bond, an amide bond, and an imide bond.
Citation Information
Patent Citations
Dicing method and adhesive tape for dicing used therefor
JP1994310598A
Processing method of wafer
JP2020161618A
Method for manufacturing semiconductor device, and mounting device
WO2018062482A1