Polythiol compositions and optical resin materials

The polythiol composition with pentaerythritol tetra(3-mercaptopropionate) disulfide substitution addresses issues of reactivity and steric hindrance in lens curing, enhancing lens durability and reducing yellowing and fatigue through uniform polymerization and reduced active group exposure.

JP7955474B2Active Publication Date: 2026-11-24EFIRM NEW MATERIAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2025504153
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-06-30
Filing Date
2024-03-28
Publication Date
2026-11-24
Estimated Expiration
2044-03-28

AI Technical Summary

Technical Problem

Current lens curing methods using polythiol compounds result in low reactivity, steric hindrance, and gel polymerization inhibition, leading to incomplete crosslinking, active group degradation, yellowing, and visual fatigue due to oxidation and water/oxygen penetration, particularly in rimless glasses.

Method used

A polythiol composition with a specific proportion of pentaerythritol tetra(3-mercaptopropionate) disulfide substitution, which reduces steric hindrance and activates thiol groups for uniform polymerization, minimizing active group presence and oxygen/water intrusion.

Benefits of technology

The solution effectively prevents gel polymerization inhibition, reduces lens yellowing and degradation, and alleviates visual fatigue by ensuring uniform crosslinking and improved lens durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955474000005
    Figure 0007955474000005
  • Figure 0007955474000006
    Figure 0007955474000006
  • Figure 0007955474000007
    Figure 0007955474000007
Patent Text Reader

Abstract

The present invention relates to the field of polymer materials, and in particular to a polythiol composition containing pentaerythritol tetra(3-mercaptopropionate) and a pentaerythritol tetra(3-mercaptopropionate) disulfide-substituted compound, and an optical resin material. The mass ratio of the pentaerythritol tetra(3-mercaptopropionate) disulfide-substituted compound to pentaerythritol tetra(3-mercaptopropionate) is 1:181 to 10,000. By controlling the specific proportion of the pentaerythritol tetra(3-mercaptopropionate) disulfide-substituted compound in the polythiol composition, the present invention effectively avoids gel polymerization inhibition, reduces the presence of active groups in resin lenses, and reduces the penetration of water and oxygen. This significantly reduces the deterioration and yellowing of resin lenses, reduces the occurrence of prism effects, and alleviates visual fatigue.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention belongs to the technical field of optical materials, and particularly relates to a polythiol composition and an optical resin material. [Background Art]

[0002] With the rapid development of the information society, the myopia rate has been increasing year by year and gradually becoming younger. According to relevant statistics, the myopia rate is 14.3% among 6-year-old children, 35.6% among primary school students, 71.7% among junior high school students, and 80.5% among high school students. Properly wearing glasses to correct vision at the right time can avoid continuous vision decline caused by the fatigue of the human eye's crystalline lens.

[0003] Polythiol compounds are used in lenses with a refractive index of 1.56 to 1.61. The produced lenses have excellent refractive index, toughness, and light transmittance characteristics, and are also superior in terms of cost, occupying a larger market share. The current lens curing method involves uniformly mixing reactant materials, pouring them into a mold, placing the mold in an oven for heating, and reacting to solidify. As the temperature and crosslinking degree increase, the reaction rate increases. However, the reaction is carried out by standing in an oven, and the polythiol compound has low reactivity and large steric hindrance. At this time, self-crosslinking of isocyanate groups and inhibition of gel polymerization occur. Furthermore, the viscosity of the reactant increases, and partial curing occurs, resulting in insufficient contact of active groups. Uncrosslinked thiol groups and isocyanate groups exist during crosslinking. These reactive groups have high activity and are prone to degradation and yellowing. In addition, the current usage period of glasses is as long as 1 to 2 years. During use, active groups are denatured by light and oxygen, causing the lens to turn yellow and its transparency to decrease. In addition, ester groups are present in polythiol compounds. The secretion and penetration of human fat and sweat damage the molecular chains of the lens, accelerating the degradation rate. This phenomenon is particularly prominent in rimless glasses. The edges of the lens generate heat and are not protected by a film layer, so they are prone to oxidation and yellowing, causing a prism effect for the wearer, worsening visual fatigue, and accelerating the decline of vision in young people. [Summary of the Invention] [Problems that the invention aims to solve]

[0004] In view of the current problems, the present invention provides a polythiol composition and an optical resin material. By using a specific proportion of pentaerythritol tetra(3-mercaptopropionate) disulfide substitution in the polythiol composition, the gel polymerization inhibition phenomenon is effectively avoided, the presence of active groups in the resin lens and the penetration of water and oxygen are reduced, the deterioration and yellowing of the resin lens is greatly reduced, the occurrence of the prism effect is reduced, and visual fatigue is alleviated. [Means for solving the problem]

[0005] The technical solution of the present invention is as follows: A polythiol composition characterized by comprising pentaerythritol tetra(3-mercaptopropionate) and a pentaerythritol tetra(3-mercaptopropionate) disulfide substitution, wherein the mass ratio of the pentaerythritol tetra(3-mercaptopropionate) disulfide substitution to pentaerythritol tetra(3-mercaptopropionate) is 1:181 to 10000. The structural formula of the pentaerythritol tetra(3-mercaptopropionate) disulfide substitution is shown in Formula 1.

[0006] [ka]

[0007] Preferably, the polythiol composition is a mixture of 50-90 parts pentaerythritol tetra(3-mercaptopropionate) and pentaerythritol tetra(3-mercaptopropionate) disulfide substitution, 10-20 parts pentaerythritol tris(3-mercaptopropionate), and 2-15 parts 3-Sulfanylpropanoate [2,2-Bis(3-sulfanylpropanoyloxymethyl)-3-[3-(3-sulfanylpropanoylsulfanyl)propanoyloxy]propyl] ester , 50-145 copies 2,3-Bis(2-mercaptoethylthio)-1-propanthol Includes.

[0008] More preferably, the polythiol composition is 1 to 5 parts pentaerythritol bis(3-mercaptopropionate), 0 to 3 parts pentaerythritol-3-mercaptopropionate, 0 to 5 parts 3-Sulfanylpropanoate [2-(hydroxymethyl)-2-(3-sulfanylpropanoyloxymethyl)-3-[3-(3-sulfanylpropanoylsulfanyl)propanoyloxy]propyl] ester Includes.

[0009] An optical resin material made from the above-mentioned polythiol composition and isocyanate as raw materials.

[0010] When manufacturing the corresponding optical resin materials, the practicality of the resulting optical materials can be further improved by adding additives to the raw materials mentioned above. The raw materials may also include additives such as catalysts, UV absorbers, mold release agents, blue pigments, and red pigments.

[0011] Preferably, the isocyanate is one or more of m-xylylene diisocyanate, cyclohexanedimethylene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, and norbornane diisocyanate selected in any proportion.

[0012] Preferably, the raw materials are cured to obtain an optical resin material.

[0013] The pentaerythritol tetra(3-mercaptopropionate) disulfide-substituted compound (referred to as disulfide-substituted compound) of the present invention contains six thiol groups compared to the structure of other polythiol compounds, and can significantly improve the relationship between the polythiol compound and the isocyanate. Steric hindrance to the reaction is reduced, an active site is formed upon reaction with the isocyanate, and as a result the thiol groups of the polythiol are activated, expanding the molecular chain upon reaction with the isocyanate, reducing steric hindrance, and the polymerization reaction becomes a point-line-plane reaction, meaning a uniform polymerization reaction occurs, avoiding steric hindrance and gel inhibition, increasing the crosslinking density and uniformity of the resin network, reducing the presence of active groups and the intrusion of water and oxygen, and significantly reducing the progression of degradation. At the same time, because the structure of the disulfide-substituted compound is similar to that of the polythiol compound, lenses polymerized with isocyanate still have excellent refractive index, toughness, and light transmittance properties. If an excess of disulfide substitution is added to the polythiol composition, the reaction during the degassing stage is too rapid, resulting in excessive viscosity that prevents injection into the mold. On the other hand, if too little is added, the desired effect cannot be obtained.

[0014] The following describes the synthesis method for the pentaerythritol tetra(3-mercaptopropionate) disulfide-substituted product shown in Equation 1, but the method is not limited to this one. Specifically, the synthesis method involves placing pentaerythritol tetra(3-mercaptopropionate) and toluene in a water bath and stirring uniformly. An oxidizing agent is added, and the mixture is prepared by catalytic action of neutral and alkaline reagents. After removing the solvent, the mixture is separated by chromatography to obtain the disulfide-substituted product.

[0015] Preferably, the mass ratio of pentaerythritol tetra(3-mercaptopropionate) to toluene is 1:5 to 10.

[0016] Preferably, the oxidizing agent is selected in any proportion from one or more of the following: air, oxygen, ozone, sulfur trioxide, hydrogen peroxide, metachloroperoxybenzoic acid, peroxybenzoic acid, and I2. When a gaseous oxidizing agent is used, the reaction rate is slower and the selectivity of the product is higher. Liquid oxidizing agents have a faster reaction rate but are less selective because they readily produce polymer compounds. Therefore, gaseous oxidizing agents are more preferable.

[0017] Preferably, the molar ratio of the oxidizing agent to pentaerythritol tetra(3-mercaptopropionate) is 10-30:1, more preferably 15-20:1. If the amount of oxidizing agent is too small, the formation of disulfide substitutions will be insufficient. If the amount of oxidizing agent is too large, excessive crosslinking will occur, leaving a small amount of gel-like substance after the solvent is removed.

[0018] Preferably, the catalyst selected during the reaction is one or more of the following in any proportion: aqueous ammonia, sodium hydroxide, potassium hydroxide, calcium hydroxide, sodium bicarbonate, sodium carbonate, potassium carbonate, sodium dihydrogen phosphate, sodium phosphate, diethylamine, triethylamine, diethylamine, triethylamine, triethylenediamine, bisdimethylaminoethyl ether, bismorpholine diethyl ether, dimethylaminoethoxyethanol, N,N-dimethylcyclohexylamine, bis(2-dimethylaminoethyl) ether, N,N,N′,N′-tetramethylalkylenediamine, N,N-dimethylbenzylamine, triethanolamine, DMEA, pyridine, and N,N′-lutidine. More preferably, it is aqueous ammonia, triethylamine, or N,N-dimethylcyclohexylamine.

[0019] The molar ratio of catalyst to pentaerythritol tetra(3-mercaptopropionate) is 0.005 to 0.05:1, with a more preferable molar ratio of 0.01 to 0.03:1. If the amount of catalyst is too small, the amount of disulfide substitution is too small; if the amount of catalyst is too large, excessive crosslinking occurs, and after solvent removal, a small amount of gel-like substance remains.

[0020] The reaction temperature is preferably 10 to 60°C, more preferably 20 to 40°C. If the reaction temperature is too low, the substrate conversion rate will be excessively low; if the reaction temperature is too high, excessive crosslinking will occur. When the solvent is removed, a slightly gel-like substance will appear.

[0021] Preferably, the height of the chromatography column is 40 to 80 cm, the ratio of the column diameter to height is 15 to 20:1, the optimal column height is 60 cm, the water absorbing agent is anhydrous sodium sulfate, the eluent is petroleum ether and ethyl acetate, and the mass ratio of petroleum ether to ethyl acetate is 3 to 10:1, more preferably 5 to 7:1.

Effects of the Invention

[0022] The polythiol composition and optical resin material provided by the present invention can effectively avoid gel polymerization inhibition phenomenon and reduce the presence of active groups by controlling the specific proportion of pentaerythritol tetrakis(3-mercaptopropionate) disulfide substituent in the polythiol composition. The penetration of water and oxygen into the resin lens can greatly reduce the degradation and yellowing of the resin lens, reduce the occurrence of the prism effect, and alleviate visual fatigue.

Brief Description of the Drawings

[0023] [Figure 1] It is a secondary mass spectrum of pentaerythritol tetrakis(3-mercaptopropionate) disulfide substituent. [Figure 2] It is an infrared spectrum of pentaerythritol tetrakis(3-mercaptopropionate) disulfide substituent. [Figure 3] It is a 1H NMR spectrum of pentaerythritol tetrakis(3-mercaptopropionate) disulfide substituent.

Modes for Carrying Out the Invention

[0024] The present invention will be further described below with reference to examples, but these descriptions will not further limit the scope of the invention. Those skilled in the art should understand that equivalent substitutions or corresponding improvements made to the technical features of the invention are still within the scope of protection of the invention. Transmittance and yellowness (YI313) were measured using an UltraScan VIS spectrophotometer manufactured by HunterLab Company, USA. The operating temperature was 25–30°C, the light source was D65, and the spectral range was 360–780 nm. The following parts are based on mass percentages.

[0025] (Example 1) One method for synthesizing pentaerythritol tetra(3-mercaptopropionate) disulfide substitutions: 20 g of pentaerythritol tetra(3-mercaptopropionate) and 100 g of toluene were stirred and dissolved in a 30°C water bath. Then, 0.13 g of triethylamine was added, and 0.82 mol of ozone was slowly passed through the solution. The reaction was incubated at 25°C for 48 hours. After removing toluene under vacuum, a bright yellow liquid was obtained. A 60 cm high chromatography column with a diameter-to-height ratio of 20:1 was used, and the eluents were petroleum ether and ethyl acetate in a mass ratio of 6:1. The product was obtained by chromatography-column separation. ¹H NMR (400 MHz, CDCl3) δ 4.16 (s, ¹H, OCH), 2.76-2.74 (m, ¹H, SCH), 2.67-2.66 (m, ¹H, O=CC) -H), 1.60-1.64(m, 1H, SH).

[0026] All of the following disulfide substitutions refer to pentaerythritol tetra(3-mercaptopropionate) disulfide substitutions, as shown in Equation 1.

[0027] [ka]

[0028] (Example 2) Optical resin material: (1) Polythiol composition: 5.3 g pentaerythritol tris(3-mercaptopropionate), 0.02 g disulfide substitution, 40 g pentaerythritol tetra(3-mercaptopropionate), 4.5 g 3-Sulfanylpropanoate [2,2-Bis(3-sulfanylpropanoyloxymethyl)-3-[3-(3-sulfanylpropanoylsulfanyl)propanoyloxy]propyl] ester 51.9g 2,3-Bis(2-mercaptoethylthio)-1-propanthol ;

[0029] (2) Mix 55 parts norbornane diisocyanate, 45 parts polythiol composition, 0.05 parts dibutyltin dichloride, 0.6 parts UV absorber 329, and 0.1 parts mold release agent (dibutyl phosphate), mix well, filter through a 1 μm filter, and degas under vacuum at 30°C for 30 minutes. Inject into a mold, gradually increase the temperature from 30°C to 120°C within 8 hours, maintain temperature for 2 hours, and then cool to 60°C over 3 hours to obtain the optical resin material. After coating, the obtained optical lens is left at 50°C and 95% RH for 200 hours to verify accelerated aging, and then a performance test is performed.

[0030] (Example 3) Optical resin material: (1) Polythiol composition: 5.3 g pentaerythritol tris(3-mercaptopropionate), 0.095 g disulfide substitution, 40 g pentaerythritol tetra(3-mercaptopropionate), 4.5 g 3-Sulfanylpropanoate [2,2-Bis(3-sulfanylpropanoyloxymethyl)-3-[3-(3-sulfanylpropanoylsulfanyl)propanoyloxy]propyl] ester 51.9g 2,3-Bis(2-mercaptoethylthio)-1-propanthol ;

[0031] (2) Mix 55 parts norbornane diisocyanate, 45 parts polythiol composition, 0.05 parts dibutyltin dichloride, 0.6 parts UV absorber 329, and 0.1 parts mold release agent (dibutyl phosphate), mix well, filter through a 1 μm filter, and degas under vacuum at 30°C for 30 minutes. Inject into a mold, gradually increase the temperature from 30°C to 120°C within 8 hours, maintain temperature for 2 hours, and then cool to 60°C over 3 hours to obtain the optical resin material. After coating, the obtained optical lens is left at 50°C and 95% RH for 200 hours to verify accelerated aging, and then a performance test is performed.

[0032] (Example 4) Optical resin material: (1) Polythiol composition: 5.3 g pentaerythritol tris(3-mercaptopropionate), 0.15 g disulfide substitution, 40 g pentaerythritol tetra(3-mercaptopropionate), 4.5 g 3-Sulfanylpropanoate [2,2-Bis(3-sulfanylpropanoyloxymethyl)-3-[3-(3-sulfanylpropanoylsulfanyl)propanoyloxy]propyl] ester 51.9g 2,3-Bis(2-mercaptoethylthio)-1-propanthol ;

[0033] (2) Mix 55 parts norbornane diisocyanate, 45 parts polythiol composition, 0.05 parts dibutyltin dichloride, 0.6 parts UV absorber 329, and 0.1 parts mold release agent (dibutyl phosphate), mix well, filter through a 1 μm filter, and degas under vacuum at 30°C for 30 minutes. Inject into a mold, gradually increase the temperature from 30°C to 120°C within 8 hours, maintain temperature for 2 hours, and then cool to 60°C over 3 hours to obtain the optical resin material. After coating, the obtained optical lens is left at 50°C and 95% RH for 200 hours to verify accelerated aging, and then a performance test is performed.

[0034] (Example 5) Optical resin material: (1) Polythiol composition: 5.3 g pentaerythritol tris(3-mercaptopropionate), 0.216 g disulfide substitution, 40 g pentaerythritol tetra(3-mercaptopropionate), 4.5 g 3-Sulfanylpropanoate [2,2-Bis(3-sulfanylpropanoyloxymethyl)-3-[3-(3-sulfanylpropanoylsulfanyl)propanoyloxy]propyl] ester 51.9g 2,3-Bis(2-mercaptoethylthio)-1-propanthol ;

[0035] (2) Mix 55 parts norbornane diisocyanate, 45 parts polythiol composition, 0.05 parts dibutyltin dichloride, 0.6 parts UV absorber 329, and 0.1 parts mold release agent (dibutyl phosphate), mix well, filter through a 1 μm filter, and degas under vacuum at 30°C for 30 minutes. Inject into a mold, gradually increase the temperature from 30°C to 120°C within 8 hours, maintain temperature for 2 hours, and then cool to 60°C over 3 hours to obtain the optical resin material. After coating, the obtained optical lens is left at 50°C and 95% RH for 200 hours to verify accelerated aging, and then a performance test is performed.

[0036] (Example 6) Optical resin material: (1) Polythiol composition: 0.6 g pentaerythritol bis(3-mercaptopropionate), 5.3 g pentaerythritol tris(3-mercaptopropionate), 0.15 g disulfide substitution, 1.7 g 3-Sulfanylpropanoate [2-(hydroxymethyl)-2-(3-sulfanylpropanoyloxymethyl)-3-[3-(3-sulfanylpropanoylsulfanyl)propanoyloxy]propyl] ester 40g of pentaerythritol tetra (3-mercaptopropionate), 4.5g of 3-Sulfanylpropanoate [2,2-Bis(3-sulfanylpropanoyloxymethyl)-3-[3-(3-sulfanylpropanoylsulfanyl)propanoyloxy]propyl] ester 51.9g 2,3-Bis(2-mercaptoethylthio)-1-propanthol ;

[0037] (2) Mix 55 parts norbornane diisocyanate, 45 parts polythiol composition, 0.05 parts dibutyltin dichloride, 0.6 parts UV absorber 329, and 0.1 parts mold release agent (dibutyl phosphate), mix well, filter through a 1 μm filter, and degas under vacuum at 30°C for 30 minutes. Inject into a mold, gradually increase the temperature from 30°C to 120°C within 8 hours, maintain temperature for 2 hours, and then cool to 60°C over 3 hours to obtain the optical resin material. After coating, the obtained optical lens is left at 50°C and 95% RH for 200 hours to verify accelerated aging, and then a performance test is performed.

[0038] (Comparative Example 1) Optical resin material: (1) Polythiol composition: 5.3 g pentaerythritol tris(3-mercaptopropionate), 0.3 g disulfide substitution, 40 g pentaerythritol tetra(3-mercaptopropionate), 4.5 g 3-Sulfanylpropanoate [2,2-Bis(3-sulfanylpropanoyloxymethyl)-3-[3-(3-sulfanylpropanoylsulfanyl)propanoyloxy]propyl] ester 51.9g 2,3-Bis(2-mercaptoethylthio)-1-propanthol ;

[0039] (2) 55 parts norbornane diisocyanate, 45 parts polythiol composition, 0.05 parts dibutyltin dichloride, 0.6 parts UV absorber 329, and 0.1 parts mold release agent (dibutyl phosphate) were mixed and thoroughly combined, filtered through a 1 μm filter, and degassed under vacuum at 30°C for 30 minutes. Subsequently, when attempting to inject the mixture into the mold, the gel clogged the tip of the gun and injection was not possible.

[0040] (Comparative Example 2) Optical resin material: (1) Polythiol composition: 5.3 g of pentaerythritol tris(3-mercaptopropionate), 40 g of pentaerythritol tetra(3-mercaptopropionate), 4.5 g 3-Sulfanylpropanoate [2,2-Bis(3-sulfanylpropanoyloxymethyl)-3-[3-(3-sulfanylpropanoylsulfanyl)propanoyloxy]propyl] ester 51.9g 2,3-Bis(2-mercaptoethylthio)-1-propanthol ;

[0041] (2) Mix 55 parts norbornane diisocyanate, 45 parts polythiol composition, 0.05 parts dibutyltin dichloride, 0.6 parts UV absorber 329, and 0.1 parts mold release agent (dibutyl phosphate), mix well, filter through a 1 μm filter, and degas under vacuum at 30°C for 30 minutes. Inject into a mold, gradually increase the temperature from 30°C to 120°C within 8 hours, maintain temperature for 2 hours, and then cool to 60°C over 3 hours to obtain the optical resin material. After coating, the obtained optical lens is left at 50°C and 95% RH for 200 hours to verify accelerated aging, and then a performance test is performed.

[0042] (Comparative Example 3) Optical resin material: (1) Polythiol composition: 5.3 g of pentaerythritol tris(3-mercaptopropionate), 40 g of pentaerythritol tetra(3-mercaptopropionate), 4.5 g 3-Sulfanylpropanoate [2,2-Bis(3-sulfanylpropanoyloxymethyl)-3-[3-(3-sulfanylpropanoylsulfanyl)propanoyloxy]propyl] ester 51.9g 2,3-Bis(2-mercaptoethylthio)-1-propanthol ;

[0043] (2) 55 parts norbornane diisocyanate, 45 parts polythiol composition, 0.1 0.6 parts dibutyltin dichloride, 0.6 parts UV absorber 329, and 0.1 parts mold release agent (dibutyl phosphate) were mixed and thoroughly combined. The mixture was filtered through a 1 μm filter and degassed under vacuum at 30°C for 30 minutes. The mixture was poured into a mold, and the temperature was gradually increased from 30°C to 120°C within 8 hours. After holding the temperature for 2 hours, the temperature was lowered to 60°C over 3 hours to obtain the optical resin material. After coating, the obtained optical lens was left at 50°C and 95% RH for 200 hours to verify accelerated aging, and then a performance test was conducted. (Test example)

[0044] [Table 1]

[0045] The above mass ratio is the mass ratio of pentaerythritol tetra(3-mercaptopropionate) disulfide substitution to pentaerythritol tetra(3-mercaptopropionate).

[0046] From the data in Table 1 above, in Comparative Example 1, the content of pentaerythritol tetra(3-mercaptopropionate) disulfide substitution was too high, resulting in high viscosity. When poured into the mold, gelation occurred at the tip of the gun, making it impossible to pour. The products of Examples 2-4 of the present invention, after aging over time, had higher front light transmittance than the products of Comparative Examples 2-3, and their yellowness was far lower than that of the comparative examples. Furthermore, the light transmittance at the edges of the products of Examples 2-4 of the present invention was even higher than that of the products of Comparative Examples 2-3, and their yellowness was far lower than that of the products of Comparative Examples 2-3. Through the verification of the above test examples, it is possible to effectively avoid the gel polymerization inhibition phenomenon by using a specific proportion of pentaerythritol tetra(3-mercaptopropionate) disulfide substitution in the polythiol composition, reduce the presence of active groups in the resin lens and the penetration of water and oxygen, significantly reduce the deterioration and yellowing of the resin lens, reduce the occurrence of the prism effect, and alleviate visual fatigue. The lifespan of eyeglasses can be extended.

Claims

1. A polythiol composition comprising an isocyanate, The polythiol composition comprises pentaerythritol tetra(3-mercaptopropionate) and pentaerythritol tetra(3-mercaptopropionate) disulfide substituted products. The structural formula of the aforementioned pentaerythritol tetra(3-mercaptopropionate) disulfide substitution is shown in Formula 1. 【Chemistry 1】 The mass ratio of the pentaerythritol tetra(3-mercaptopropionate) disulfide substitution to pentaerythritol tetra(3-mercaptopropionate) is 1:181 to 1:10000. An optical resin material characterized by the following features.

2. The optical resin material according to claim 1, characterized in that the polythiol composition comprises 50 to 90 parts by mass of a mixture of pentaerythritol tetra(3-mercaptopropionate) and a pentaerythritol tetra(3-mercaptopropionate) disulfide substituted product, 10 to 20 parts by mass of pentaerythritol tris(3-mercaptopropionate), 2 to 15 parts by mass of 3-sulfanylpropanoic acid [2,2-bis(3-sulfanylpropanoyloxymethyl)-3-[3-(3-sulfanylpropanoylsulfanyl)propanoyloxy]propyl] ester, and 50 to 145 parts by mass of 2,3-bis(2-mercaptoethylthio)-1-propanthol.

3. The optical resin material according to claim 2, characterized in that the polythiol composition further comprises 1 to 5 parts by mass of pentaerythritol bis(3-mercaptopropionate), 0 to 3 parts by mass of pentaerythritol-3-mercaptopropionate, and 0 to 5 parts by mass of 3-sulfanylpropanoic acid [2-(hydroxymethyl)-2-(3-sulfanylpropanoyloxymethyl)-3-[3-(3-sulfanylpropanoylsulfanyl)propanoyloxy]propyl] ester.

4. The optical resin material according to claim 1, characterized in that the isocyanate is any one of metaxylylene diisocyanate, cyclohexanedimethylene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, norbornane diisocyanate, or a combination of any number thereof in any proportion.

5. The optical resin material according to claim 1, characterized in that it is obtained by curing the polythiol composition and the isocyanate as raw materials.

Citation Information

Patent Citations

  • Polymerizable composition

    CN103547608A

  • Method for manufacturing polymer for optical material

    JP2002348349A

  • Polymerizable composition for optical material

    JP2020139085A

  • Optical material and use thereof

    US20160216407A1

  • Method for producing polythiourethane resin

    WO2008026727A1