Degradable crosslinking agent

A degradable crosslinking agent with enhanced solubility addresses the solubility and decomposition challenges of diacylhydrazine compounds, enabling efficient use in solvent-based processes and reducing environmental burden.

JP7955479B2Active Publication Date: 2026-11-24NAGASE CHEMTEX CORPORATION
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2025508372
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-03-20
Filing Date
2024-03-14
Publication Date
2026-11-24
Estimated Expiration
2044-03-14

AI Technical Summary

Technical Problem

Diacylhydrazine compounds used in polymers have low solubility in solvents, limiting their application in processes like paints and causing environmental burden due to high-boiling-point solvents, and they are difficult to decompose after use.

Method used

A degradable crosslinking agent with enhanced solubility in solvents is developed, incorporating specific structures and functional groups, allowing for improved solubility and decomposition with oxidizing agents.

Benefits of technology

The agent exhibits excellent solubility in various solvents and can be easily decomposed, reducing environmental impact and expanding applications such as paints.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955479000001
    Figure 0007955479000001
  • Figure 0007955479000002
    Figure 0007955479000002
  • Figure 0007955479000003
    Figure 0007955479000003
Patent Text Reader

Abstract

The present invention provides a degradable crosslinking agent having high solubility in a solvent. The present invention pertains to a degradable crosslinking agent comprising a compound represented by formula (1). In formula (1), ∙ n≥0, k≥0, m≥0, p1≥1, p2≥1, and p3≥1. ∙ R1, R2, and R3 are each independently a single bond or a C1-C500 hydrocarbon which may have a substituent or a heteroatom. ∙ Q1, Q2, and Q3 are each independently at least one reactive functional group selected from the group consisting of a hydroxyl group, an amino group, a thiol group, a hydrazide group, a carboxylic acid group, an acid anhydride group, a vinyl group, an allyl group, an acrylate group a methacrylate group, a crotonate group, an isoprenyl group, an acrylamide group, a methacrylamide group, a crotonamide group, an epoxy group, an oxetane group, an oxazoline group, an isocyanate group, a carbodiimide group, a methylol group, a silanol group, a hydroxysilyl group, and an alkoxysilyl group. ∙ X1a, X1b, X2a, X2b, X3a, X3b, X4a, and X4b are each independently an oxygen atom, a sulfur atom, a single bond, a C1-C20 hydrocarbon group which may have a substituent, or –NB- (B is a hydrogen atom or a hydrocarbon group), where at least one among X1a, X1b, X2a, X2b, X3a, X3b, X4a, and X4b is an oxygen atom, a sulfur atom, or –NB- (B is a hydrogen atom or a hydrocarbon group). ∙ A1-A8 are carbonyl groups or single bonds, at least one among A1 and A2 is a carbonyl group, at least one among A3 and A4 is a carbonyl group, at least one among A5 and A6 is a carbonyl group, and at least one among A7 and A8 is a carbonyl group. ∙ Zs are each independently a di- or higher-valent group containing a siloxane structure or a C1-C500 hydrocarbon group which may have a heteroatom.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to a biodegradable crosslinking agent. [Background technology]

[0002] Plastic products are used in a variety of fields, including daily necessities, automobiles, and electronic devices, due to their moldability, durability, and lightweight properties. However, they have the problem of not being easily decomposed after disposal. In recent years, the development of easily biodegradable polymers has been progressing in order to protect the global environment.

[0003] As one example of a biodegradable polymer, polymers having a diacylhydrazine structure have been disclosed (see Patent Documents 1, 2, and 3). These polymers, due to their diacylhydrazine structure, are stable in air but are rapidly decomposed by reaction with oxidizing agents such as sodium hypochlorite. [Prior art documents] [Patent Documents]

[0004] [Patent Document 1] Japanese Patent Publication No. 2011-236381 [Patent Document 2] International Publication No. 2021 / 131003 [Patent Document 3] Japanese Patent Publication No. 2011-052075 [Overview of the Initiative] [Problems that the invention aims to solve]

[0005] The diacylhydrazine compounds used as raw materials for polymers described in Patent Documents 1 and 2, and the diacylhydrazine-containing polymers described in Patent Document 3, have low solubility in solvents, which severely limits the composition when combined with resins, polymerization initiators, etc. Furthermore, even those with relatively high solubility in solvents only dissolve in high-boiling-point aprotic polar solvents or strong acids, resulting in a significant environmental burden and difficulty of application in applications such as paints that involve processes to dry and remove the solvent. The present invention aims to provide a degradable crosslinking agent with high solubility in solvents. [Means for solving the problem]

[0006] The inventors of the present invention have discovered that the solubility in solvents can be enhanced in hydrazine derivatives by incorporating a specific structure, and have completed the present invention.

[0007] In other words, the present disclosure (1) is a degradable crosslinking agent comprising a compound represented by the following formula (1). [ka] (In formula (1), n≧0, k≧0, m≧0, p1≧1, p2≧1, p3≧1. ·R 1 , R 2 , R 3 These are hydrocarbons having 1 to 500 carbon atoms, which may independently have single bonds, substituents, or heteroatoms. Q 1 Q 2 Q 3 These are one or more reactive functional groups independently selected from the group consisting of hydroxyl groups, amino groups, thiol groups, hydrazide groups, carboxylic acid groups, acid anhydride groups, vinyl groups, allyl groups, acrylate groups, methacrylate groups, crotonate groups, isoprenyl groups, acrylamide groups, methacrylamide groups, crotonamide groups, epoxy groups, oxetane groups, oxazoline groups, isocyanate groups, carbodiimide groups, methylol groups, silanol groups, hydroxysilyl groups, and alkoxysilyl groups. ·X 1a , X1b , X 2a , X 2b , X 3a , X 3b , X 4a , X 4b are each independently an oxygen atom, a sulfur atom, a single bond, a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, or -NB- (B is a hydrogen atom or a hydrocarbon group), and X 1a , X 1b , X 2a , X 2b , X 3a , X 3b , X 4a , X 4b one or more of them are an oxygen atom, a sulfur atom, or -NB- (B is a hydrogen atom or a hydrocarbon group). ·A 1 to A 8 are a carbonyl group or a single bond, and A 1 and A 2 at least one of them is a carbonyl group, and A 3 and A 4 at least one of them is a carbonyl group, and A 5 and A 6 at least one of them is a carbonyl group, and A 7 and A 8 at least one of them is a carbonyl group. ·Z are each independently a divalent or higher-valent group containing a siloxane structure, or a hydrocarbon group having 1 to 500 carbon atoms which may have a hetero atom.)

[0008] The present disclosure (2) is p1 ≧ 2, p2 ≧ 2, or p3 ≧ 2, and a plurality of Q 1 each other, Q 2 each other or Q 3 The degradable cross-linking agent according to the present disclosure (1), wherein the two are different reactive functional groups.

[0009] The present disclosure (3) is the degradable cross-linking agent according to the present disclosure (1) or (2), wherein p1 = 1, p2 = 1, or p3 = 1.

[0010] Disclosure (4) is a degradable crosslinking agent according to Disclosure (1) or (2), having at least one degradation site represented by the following formula (2). -X 5 -C 1 -NH-NH-C 2 -X 6 - (2) (In formula (2), X 5 , X 6 These are all different from each other and are an oxygen atom, a sulfur atom, a single bond, a C1-C20 hydrocarbon group which may have substituents, or -NB- (where B is a hydrogen atom or a hydrocarbon group). 1 , C 2 is a carbonyl group or single bond, C 1 and C 2 At least one of them is a carbonyl group.

[0011] This disclosure (5) is X 1a or X 1b The degradable crosslinking agent described in (1) or (2) of this disclosure is wherein is an oxygen atom.

[0012] Disclosure (6) is a degradable crosslinking agent as described in Disclosure (1) or (2), wherein n≧1.

[0013] This disclosure (7) is for n≧1, X 1a , X 1b , X 2a , X 2b , X 3a , X 3b , X 4a , X 4b among At least one is an oxygen atom, At least one of them is a single bond or a hydrocarbon group having 1 to 20 carbon atoms which may have substituents, At least one is -NB- (where B is a hydrogen atom or a hydrocarbon group). The degradable crosslinking agent described in (1) or (2) of this disclosure.

[0014] The present disclosure (8) is a degradable crosslinking agent according to the present disclosure (1) or (2), having a molecular weight of 2000 or less.

[0015] Disclosure (9) is a degradable crosslinking agent as described in Disclosure (1) or (2), wherein k ≥ 1.

[0016] Disclosure (10) is a composition comprising a degradable crosslinking agent as described in Disclosure (1) or (2) and one or more selected from the group consisting of a curable resin, a polymerization initiator, and a solvent.

[0017] Disclosure (11) is the composition described in Disclosure (10), which substantially does not contain a solvent with a boiling point above 150°C.

[0018] Disclosure (12) is a degradable crosslinked product comprising the composition described in Disclosure (10).

[0019] This disclosure (13) is a degradable crosslinked product as described in this disclosure (12) that can be degraded with an oxidizing agent.

[0020] This disclosure (14) is a method for decomposing a decomposable crosslinked product, comprising the step of bringing the decomposable crosslinked product described in this disclosure (12) into contact with an aqueous solution containing an oxidizing agent at a temperature of 100°C or lower. [Effects of the Invention]

[0021] The degradable crosslinking agent of the present invention exhibits excellent solubility in solvents. [Modes for carrying out the invention]

[0022] <<Degradable Crosslinking Agent>> The degradable crosslinking agent of the present invention is a degradable crosslinking agent comprising a compound represented by the following formula (1). [ka] In formula (1), n≧0, k≧0, m≧0, p1≧1, p2≧1, p3≧1. ·R 1 , R 2 , R 3These are hydrocarbons having 1 to 500 carbon atoms, which may independently have single bonds, substituents, or heteroatoms. Q 1 Q 2 Q 3 These are one or more reactive functional groups independently selected from the group consisting of hydroxyl groups, amino groups, thiol groups, hydrazide groups, carboxylic acid groups, acid anhydride groups, vinyl groups, allyl groups, acrylate groups, methacrylate groups, crotonate groups, isoprenyl groups, acrylamide groups, methacrylamide groups, crotonamide groups, epoxy groups, oxetane groups, oxazoline groups, isocyanate groups, carbodiimide groups, methylol groups, silanol groups, hydroxysilyl groups, and alkoxysilyl groups. ·X 1a , X 1b , X 2a , X 2b , X 3a , X 3b , X 4a , X 4b Each is independently an oxygen atom, a sulfur atom, a single bond, a hydrocarbon group having 1 to 20 carbon atoms which may have substituents, or -NB- (where B is a hydrogen atom or a hydrocarbon group), but X 1a , X 1b , X 2a , X 2b , X 3a , X 3b , X 4a , X 4b One or more of these atoms are an oxygen atom, a sulfur atom, or an -NB- group (where B is a hydrogen atom or a hydrocarbon group). ·A 1 ~A 8 is a carbonyl group or a single bond, A 1 and A 2 At least one of them is a carbonyl group, A 3 and A 4 At least one of them is a carbonyl group, A 5 and A 6 At least one of them is a carbonyl group, A 7 and A 8 At least one of them is a carbonyl group. ·Z each independently represent a divalent or higher-valent group containing a siloxane structure, or a hydrocarbon group having 1 to 500 carbon atoms that may have a heteroatom. The degradable crosslinking agent of the present invention is characterized in that, among a plurality of X present in formula (1), at least one is an oxygen atom or -NB- (B is a hydrogen atom or a hydrocarbon group). This gives the degradable crosslinking agent high solubility in solvents.

[0023] In a narrow sense, the term "crosslinking agent" may mean a chemical substance that forms chemical bonds between polymers or within a polymer, but in the present specification, in addition to chemical substances that form chemical bonds between polymers or within a polymer, it also means chemical substances that can form chemical bonds between their own molecules.

[0024] <n, m, k in Formula (1)> In Formula (1), n and m are both 0 or more, but each independently, 1 to 50 is preferable, and 1 to 5 is more preferable. When n is 1 or more, since it has two or more hydrazine structures (-A-NH-NH-A-), the degradability of the degradable crosslinking agent is improved, and X 1a , X 1b In addition to the selection of X 2a , X 2b The solubility in a solvent can be finely adjusted by selecting the type. The upper limits of n and m are not particularly limited, but if they exceed 50, the solubility in solvents tends to decrease.

[0025] In Formula (1), k is 0 or more, but is preferably 1 or more, and more preferably 2 or more. When k is 1 or more, three-dimensional crosslinking can be performed with the degradable crosslinking agent of the present invention. The upper limit of k is not particularly limited, but can be 200 or less. If it exceeds 200, the solubility in solvents tends to decrease.

[0026] <p1, p2, p3 in Formula (1)> In formula (1), p1, p2, and p3 are all 1 or greater, but are each independently preferably 1 to 4, more preferably 1 to 2. When p1≧2, p2≧2, or p3≧2, three-dimensional crosslinking is facilitated by the degradable crosslinking agent of the present invention, and the strength and reliability of the crosslinked product are improved. When p1≧2, p2≧2, or p3≧2, and a plurality of Q 1 s, Q 2 s, or Q 3 s are reactive functional groups different from each other, it becomes easy to select various types of curable resins and crosslinking processes as the crosslinking agent. Furthermore, when only a specific reactive functional group is crosslinked, the reactive functional group not used in the crosslinking reaction can contribute to improvement of other physical properties such as adhesion improvement or solubility improvement. When p1=1, p2=1, or p3=1, the solubility in a solvent and the decomposition rate are further improved.

[0027] <R in formula (1) 1 , R 2 , R 3 > In formula (1), R 1 , R 2 , R 3 are each independently a single bond or a hydrocarbon group having 1 to 500 carbon atoms which may have a substituent or a hetero atom. In the case of a hydrocarbon group, the number of carbon atoms is 1 to 500, but is preferably 1 to 100, more preferably 1 to 10 from the viewpoint of decomposition rate. Examples of the substituent include an alkoxy group, a phenoxy group, a halogen atom, a tertiary amino group, and a sulfo group.

[0028] The hydrocarbon group has a saturated or unsaturated hydrocarbon group as its main skeleton and may have either a branched or linear structure. The hydrocarbon group skeleton may also have a cyclic structure. The hydrocarbon group may have heteroatoms such as N, S, and O. These heteroatoms may be present in the main chain or side chains of the hydrocarbon group. Examples of structures with heteroatoms include ether bonds, urethane bonds, urea bonds, -NH- bonds (where hydrogen atoms may be substituted), silicone bonds, ester bonds, thioether bonds, and carbonate bonds. Methylene groups other than terminals in the hydrocarbon group may be replaced by 1 to 4 heteroatoms selected from N, S, O, etc., or by an arylene group or heteroarylene group. Hydrogen atoms in the hydrocarbon group may be substituted with cyano, nitro, halogen, or phenyl atoms. However, R 1 , R 2 , R 3 It is preferable that the structure does not contain disulfide bonds, because disulfide bonds can generate sulfonic acid when oxidized by an oxidizing agent.

[0029] Examples of hydrocarbon groups include linear hydrocarbons such as methylene, ethylene, propylene, butylene, pentylene, hexylene, heptylene, octylene, and nonylene; branched hydrocarbons such as isopropylene, isobutylene, 2,2-dimethylpropylene, and 2-ethyl-2-methylpropylene; cyclic hydrocarbons such as cyclohexylene, cyclopentylene, norbornenylene, phenylene, and naphthylene; PEG chains; and groups in which these groups are trivalent or tetravalent.

[0030] <Q in equation (1) 1 Q 2 Q 3 > In formula (1), Q 1 Q 2 Q 3Each of these is independently one or more reactive functional groups selected from the group consisting of hydroxyl groups, amino groups, thiol groups, hydrazide groups, carboxylic acid groups, acid anhydride groups, vinyl groups, allyl groups, acrylate groups, methacrylate groups, crotonate groups, isoprenyl groups, acrylamide groups, methacrylamide groups, crotonamide groups, epoxy groups, oxetane groups, oxazoline groups, isocyanate groups, carbodiimide groups, methylol groups, silanol groups, hydroxysilyl groups, and alkoxysilyl groups. The type of reactive functional group can be selected to be optimal depending on the application and process.

[0031] <X in equation (1)> In formula (1), X 1a , X 1b , X 2a , X 2b , X 3a , X 3b , X 4a , X 4b These are, independently of each other, an oxygen atom, a sulfur atom, a single bond, a C1-C20 hydrocarbon group which may have substituents, or -NB- (where B is a hydrogen atom or a hydrocarbon group). Hereinafter, X 1a , X 1b , X 2a , X 2b , X 3a , X 3b , X 4a , X 4b Let's call this X.

[0032] When X is a hydrocarbon group, its carbon number is 1 to 20, but from the viewpoint of ease of handling and ease of crosslinking reaction, 1 to 10 is preferred, and 1 to 6 is more preferred.

[0033] The hydrocarbon group has a saturated or unsaturated hydrocarbon group as its main backbone. The hydrocarbon group may have either a branched or linear structure. Furthermore, the backbone formed by the hydrocarbon group may have a cyclic structure.

[0034] Furthermore, the hydrocarbon group may have heteroatoms such as N, S, and O in its molecular chain. Methylene groups other than terminal methylene groups in the hydrocarbon group may be replaced with 1 to 4 heteroatoms selected from N, S, and O, or with an arylene group or a heteroarylene group. Hydrogen atoms in the hydrocarbon group may be substituted with cyano, nitro, halogen, or phenyl atoms.

[0035] Specific examples of hydrocarbon groups include linear hydrocarbons such as methylene, ethylene, propylene, butylene, pentylene, hexylene, heptylene, octylene, and nonylene; branched hydrocarbons such as 2,2-dimethylpropylene and 2-ethyl-2-methylpropylene; and cyclic hydrocarbons such as 1,4-cyclohexylene, cyclopentylene, norbornenylene, phenylene, and naphthylene. Among these, methylene and phenylene are preferred.

[0036] If X is -NB-, then B is a hydrogen atom or a hydrocarbon group. When B is a hydrocarbon group, from the viewpoint of decomposition rate, its carbon number is preferably 1 to 10, and more preferably 1 to 5. The hydrocarbon group B has a saturated or unsaturated hydrocarbon group as its main skeleton and may have either a branched chain or a linear structure. The hydrocarbon group skeleton may also have a cyclic structure.

[0037] Furthermore, the hydrocarbon group B may have heteroatoms such as N, S, and O in its molecular chain. The methylene groups other than the terminals in the hydrocarbon group may be replaced with 1 to 4 heteroatoms selected from N, S, and O, or with an arylene group or a heteroarylene group. The hydrogen atoms in the hydrocarbon group may be substituted with cyano, nitro, halogen, or phenyl atoms.

[0038] Specific examples of hydrocarbon group B include linear hydrocarbons such as methylene, ethylene, propylene, butylene, pentylene, hexylene, heptylene, octylene, and nonylene; branched hydrocarbons such as 2,2-dimethylpropylene and 2-ethyl-2-methylpropylene; cyclic hydrocarbons such as 1,4-cyclohexylene, cyclopentylene, norbornenylene, phenylene, and naphthylene; PEG chains; and groups in which these groups are trivalent or tetravalent. Among these, linear hydrocarbons are preferred.

[0039] In formula (1), if one or more of X are oxygen atoms, sulfur atoms, or -NB- (where B is a hydrogen atom or a hydrocarbon group), the overall solubility in the solvent is improved. Furthermore, the solubility in the solvent can be finely adjusted by selecting from multiple types of X. In terms of excellent solubility in the solvent, X 1a , X 1b , X 2a , X 2b , X 3a , X 3b , X 4a , X 4b Preferably, one of them is an oxygen atom, X 1a , or X 1b It is more preferable that it is an oxygen atom.

[0040] Furthermore, in equation (1), n≧1, and X 1a , X 1b , X 2a , X 2b , X 3a , X 3b , X 4a , X 4b Preferably, at least one of them is an oxygen atom, at least one is a single bond or a hydrocarbon group having 1 to 20 carbon atoms which may have substituents, and at least one is -NB- (where B is a hydrogen atom or a hydrocarbon group). Also, in formula (1), n≧1, X 1a , X 1b , X 2a , X 2b , X 3a , X 3b , X 4a , and X 4bIt is preferable that at least three elements selected from the group consisting of an oxygen atom, a sulfur atom, a C1-C20 hydrocarbon group which may have a single bond or substituent, and -NB- (where B is a hydrogen atom or a hydrocarbon group) are present within the X. By making the three or more X elements have different structures from each other in this way, solubility in solvents can be improved.

[0041] The degradable crosslinking agent is preferably one in which the structures at both ends of the hydrazine structure (-A-NH-NH-A-) are different. This structure is represented by the following formula (2). -X 5 -C 1 -NH-NH-C 2 -X 6 - (2) In formula (2), X 5 , X 6 These are all different from each other and are an oxygen atom, a sulfur atom, a single bond, a C1-C20 hydrocarbon group which may have substituents, or -NB- (where B is a hydrogen atom or a hydrocarbon group). 1 , C 2 is a carbonyl group or single bond, C 1 and C 2 At least one of them is a carbonyl group. 5 , X 6 Preferred combinations include an oxygen atom with a hydrocarbon group having 1 to 20 carbon atoms, which may have a single bond or substituents, and an oxygen atom with -NB- (where B is a hydrogen atom or a hydrocarbon group).

[0042] Also, the combination of X at both ends of the hydrazine structure (-A-NH-NH-A-), namely X 1a , X 1b The combination, X 2a , X 2b The combination, X 3a , X 3b The combination, X 4a , X 4b The combinations may be the same or different. The design of these combinations allows for fine-tuning of solubility in solvents. An example of a different combination is X 1a X is an oxygen atom.1b A hydrocarbon group having 1 to 20 carbon atoms, which may have single bonds or substituents, X 2a X is an oxygen atom. 2b One example is to use -NB- (where B is a hydrogen atom or a hydrocarbon group).

[0043] <A in equation (1) 1 ~A 8 > In formula (1), A 1 ~A 8 is a carbonyl group or a single bond, A 1 and A 2 At least one of them is a carbonyl group, A 3 and A 4 At least one of them is a carbonyl group, A 5 and A 6 At least one of them is a carbonyl group, A 7 and A 8 At least one of them is a carbonyl group. When one of the two A groups on either side of the -NH-NH- is a carbonyl group, the rate of decomposition by an oxidizing agent tends to increase. When both A groups are carbonyl groups, the decomposition product tends to dissolve more easily in a solution containing an oxidizing agent.

[0044] <Z in equation (1)> In formula (1), the multiple Zs are, independently of each other, divalent or greater groups containing a siloxane structure, or hydrocarbon groups having 1 to 500 carbon atoms that may have heteroatoms.

[0045] If Z is a group with a siloxane structure and is divalent or higher, the group containing the siloxane structure contains a -Si-O- bond as its main skeleton. The main skeleton may be a linear, branched, or cyclic structure. The number of silicon atoms in the group containing the siloxane structure is preferably 2 to 400, more preferably 4 to 200, and even more preferably 8 to 150.

[0046] In a siloxane structure, hydrogen atoms bonded to silicon atoms may be substituted. Specific examples of substituents include alkyl groups, alkoxy groups, phenoxy groups, halogen atoms, amino groups, sulfo groups, cyano groups, and nitro groups.

[0047] Specific examples of groups containing a siloxane structure include dimethyl silicone, diethyl silicone, ethylmethyl silicone, polymethylsilsesquioxane, or modified silicones in which the hydrocarbon groups at the terminals and / or side chains of these structures are modified to include heteroatoms such as N, S, O, and P.

[0048] When Z is a hydrocarbon group having 1 to 500 carbon atoms, which may contain heteroatoms, the number of carbon atoms is more preferably 1 to 200, and even more preferably 2 to 30, from the viewpoint of decomposition rate and crosslinking density. The hydrocarbon group has a saturated or unsaturated hydrocarbon group as its main skeleton and may have either a branched or linear structure. The skeleton of the hydrocarbon group may also have a cyclic structure. The hydrocarbon group may contain heteroatoms such as N, S, and O. The heteroatoms may be present in the main chain of the hydrocarbon group or in the side chains. Examples of structures containing heteroatoms include ether bonds, urethane bonds, urea bonds, -NH- bonds (which may have hydrogen atoms substituted), silicone bonds, ester bonds, thioether bonds, and carbonate bonds. Methylene groups other than terminals in the hydrocarbon group may be replaced with 1 to 4 heteroatoms selected from N, S, O, etc., or with arylene groups or heteroarylene groups. Hydrogen atoms in the hydrocarbon group may be substituted with hydroxyl, cyano, amino, nitro, halogen, or phenyl. However, it is preferable that the structure of Z does not contain disulfide bonds. This is because disulfide bonds can produce sulfonic acids when exposed to oxidizing agents.

[0049] Examples of hydrocarbon groups include linear hydrocarbons such as methylene, ethylene, propylene, butylene, pentylene, hexylene, heptylene, octylene, and nonylene; branched hydrocarbons such as isopropylene, isobutylene, 2,2-dimethylpropylene, and 2-ethyl-2-methylpropylene; cyclic hydrocarbons such as cyclohexylene, cyclopentylene, norbornenylene, phenylene, naphthylene, and pyridylene; PEG chains; and groups in which these groups are trivalent or tetravalent.

[0050] <Molecular weight> The molecular weight of the degradable crosslinking agent is not particularly limited, but is preferably 20,000 or less, more preferably 400 to 2,000, and even more preferably 700 to 2,000. When the molecular weight is within these ranges, the balance between degradability and crosslinking density tends to improve, while when the molecular weight exceeds 20,000, solubility in solvents tends to decrease.

[0051] <Method for synthesizing biodegradable crosslinking agents> The method for synthesizing the degradable crosslinking agent is not particularly limited and includes, for example, the reaction of a hydrazide compound, semicarbazide compound, or carbazate compound with a carbonate compound, isocyanate compound, acid anhydride, acid halide, or cyclic ester compound; the reaction of hydrazine with a carboxylic acid ester; the reaction of hydrazine with a carbonate compound; and the reaction of hydrazine with an isocyanate compound.

[0052] Examples of hydrazide compounds used in the above synthesis method include lactate hydrazide, methacrylate hydrazide, sebacate dihydrazide, adipic acid dihydrazide, phthalate dihydrazide, salicylic acid dihydrazide, and trimellitic acid trihydrazide. Examples of carbonate compounds include allyl N-succinimidyl carbonate and C,C'-(oxydi-2,1-ethanediyl)bis-N-succinimidyl carbonate. Examples of isocyanate compounds include 2-isocyanatoethyl methacrylate, hexamethylene diisocyanate, toluene diisocyanate, and polymethylene polyphenyl polyisocyanate. Examples of semicarbazide compounds include N-allylhydrazinecarboxamide, N,N'-1,6-hexanediylbis[hydrazinecarboxamide], 4,4'-isophoronebis(semicarbazide), and 4,4'-(1,3-phenylenebismethylene)bis(semicarbazide). Examples of carbazate compounds include allylcarbazate and C,C'-(oxydi-2,1-ethanediyl)biscarbazate. Examples of acid anhydrides include methacrylic anhydride, succinic anhydride, and pyromellitic dianhydride. Examples of acid halides include acrylate chloride, sebacate dichloride, adipic acid dichloride, phthalate dichloride, salicylic acid dichloride, and trimesic acid trichloride. Examples of cyclic ester compounds include propiolactone, butyrolactone, and valerolactone. Examples of carboxylic acid esters include ethyl lactate, methylparaben, monomethyl succinate, diethyl adipate, and trimethyl trimellitate.

[0053] <Composition> The composition of the present invention comprises the degradable crosslinking agent and one or more selected from the group consisting of a curable resin, a polymerization initiator, and a solvent. The amount of degradable crosslinking agent in the composition is preferably 0.1 to 99% by weight, and more preferably 1 to 50% by weight.

[0054] <Curable resin> The curable resin is not particularly limited as long as it has a structure that reacts with the reactive functional groups of the degradable crosslinking agent and crosslinks, and examples include acrylic resins, phenolic resins, epoxy resins, melamine resins, urea resins, unsaturated polyester resins, alkyd resins, silicone resins, isocyanate compounds, and polyimides. The curable resin may be a thermosetting resin or a photocurable resin. The amount of curable resin in the composition is preferably 0.1 to 95% by weight, and more preferably 1 to 50% by weight.

[0055] <Polymerization initiator> The polymerization initiator is not particularly limited as long as it is a compound that can catalyze the polymerization of the curable resin, and either a thermal polymerization initiator or a photopolymerization initiator can be used. Polymerization initiators include radical generators such as alkylphenone compounds, benzoin compounds, benzophenone compounds, oxime ester compounds, and phosphine compounds; base generators such as oxime ester compounds, ammonium compounds, benzoin compounds, dimethoxybenzyl urethane compounds, and orthonitrobenzyl urethane compounds; acid generators such as onium salts, halogen-containing compounds, diazomethane compounds, sulfone compounds, and sulfonic acid compounds; tin compounds such as dibutyltin dilaurate and dibutyltin diacetate; bismuth compounds such as bismuth octyl octate; titanium compounds such as tetraoctyl titanate and titanium ethyl acetate; zirconium compounds such as zirconium monoacetyl acetate and zirconium tetraacetyl acetate; amines such as triethylenediamine and 1,4-diazabicyclo[2,2,2]octane (DABCO); platinum compounds such as chloroplatinic acid and alkenylsiloxane platinum complexes; iron complexes; cobalt complexes; and nickel complexes. The amount of polymerization initiator in the composition is preferably 0.1 to 10 parts by weight, and more preferably 1 to 5 parts by weight, per 100 parts by weight of the curable resin.

[0056] <Solvent> Examples of solvents include water and organic solvents. Examples of organic solvents include ether-based solvents, amide-based solvents, hydrocarbon-based solvents, alcohol-based solvents, ester-based solvents, aldehyde-based solvents, ketone-based solvents, and solvents containing carbon atoms and heteroatoms.

[0057] Examples of ether-based solvents include propylene glycol monomethyl ether, anisole, 4-methylanisole, diisopropyl ether, diethyl ether, dibutyl ether, tetrahydrofuran, dimethoxyethane, cyclopentyl methyl ether, and tert-butyl methyl ether. Examples of amide-based solvents include dimethylformamide, dimethylacetamide, and N-methylpyrrolidone. Examples of hydrocarbon-based solvents include aliphatic hydrocarbon solvents such as pentane, hexane, heptane, octane, nonane, decane, undecane, dodecane, and cyclohexane, and aromatic hydrocarbon solvents such as benzene, toluene, xylene, mesitylene, ethylbenzene, tert-butylbenzene, trifluoromethylbenzene, nitrobenzene, and chlorobenzene. Examples of alcohol-based solvents include ethanol, propanol, butanol, ethylene glycol, and propylene glycol monomethyl ether. Examples of ester-based solvents include ethyl acetate, butyl acetate, and propylene glycol monomethyl ether acetate. Examples of aldehyde-based solvents include formaldehyde and acetaldehyde. Examples of ketone solvents include acetone, methyl ethyl ketone, and methyl isobutyl ketone. Examples of solvents containing carbon atoms and heteroatoms include acetonitrile and dimethyl sulfoxide. The amount of solvent in the composition is preferably 1 to 99% by weight, and more preferably 20 to 80% by weight.

[0058] The solvents listed above may be used individually or in combination of two or more. Furthermore, the solvents preferably have a boiling point of 150°C or lower, more preferably 130°C or lower, and even more preferably 110°C or lower. When the boiling point is within these ranges, the solvent can be removed by heating for a relatively short time. It is preferable that the composition substantially contains no solvents with a boiling point exceeding 150°C. Here, "substantially containing no solvents with a boiling point exceeding 150°C" means that the amount in the composition is less than 1% by weight.

[0059] <Degradable crosslinked product> The biodegradable crosslinked product of the present invention is obtained by curing a composition comprising a biodegradable crosslinking agent and one or more selected from the group consisting of a curable resin, a polymerization initiator, and a solvent. The method for producing the biodegradable crosslinked product from the composition only needs to promote polymerization and crosslinking of the curable resin, and a person skilled in the art can appropriately select light irradiation conditions, heating conditions, etc., depending on the types of biodegradable crosslinking agent, curable resin, and polymerization initiator contained in the composition. For example, when the biodegradable crosslinked product is made into a three-dimensional molded body, methods such as injection molding, compression molding, transfer molding, three-dimensional printing, and photolithography can be used.

[0060] Furthermore, when forming a coating film made of a biodegradable crosslinked material, the composition can be applied to a substrate to form a coating film, and the coating film can then be subjected to light irradiation or heating. The material and shape of the substrate are not particularly limited and include resins, inorganic materials, paper, and cloth. Examples of resins include polyesters such as polyethylene terephthalate, polyethylene naphthalate, polylactic acid, polyhydroxybutyric acid, and polybutylene succinate; polyolefins such as polyethylene, polypropylene, and polymethylpentene; cycloolefins; polystyrene; polytetrafluoroethylene; polyamides such as PMMA, nylon 6, and nylon 66; polycarbonate; polyvinyl acetate; polyvinyl alcohol; polyimide; ABS resin; cellulose; cellulose acetate; fibroin; and keratin. Examples of inorganic materials include glass, metals such as Ni, Cu, Cr, Fe, and Si, and their oxides and composite materials.

[0061] Methods for applying the composition to a substrate include, for example, bar coating, spin coating, spray coating, dip coating, nozzle coating, gravure coating, reverse roll coating, die coating, air doctor coating, blade coating, rod coating, curtain coating, knife coating, transfer roll coating, squeeze coating, impregnation coating, kiss coating, calender coating, and ejection coating.

[0062] The curing conditions for a composition applied to a substrate are not particularly limited, but when curing by light irradiation, 100-2000 mJ / cm² is recommended.2 The amount of light irradiation is an example. When curing by heating, the heating temperature is preferably 40 to 300°C, and more preferably 80 to 120°C. The heating time is preferably 0.5 to 180 minutes, and more preferably 0.5 to 10 minutes.

[0063] The thickness of the cured coating film is not particularly limited, but is preferably 0.01 to 900 μm, more preferably 0.02 to 100 μm, and even more preferably 0.05 to 10 μm. Within this range, the strength of the coating film and its adhesion to the substrate can be maintained.

[0064] <Method for decomposing biodegradable crosslinked materials> The present invention provides a method for decomposing a degradable crosslinked product, which includes the step of bringing the degradable crosslinked product into contact with an aqueous solution containing an oxidizing agent at a temperature of 100°C or lower.

[0065] <Oxidizing agent> The oxidizing agent is not particularly limited as long as it is an oxidizing agent other than molecular oxygen. Examples include sodium hypochlorite, potassium hypochlorite, calcium hypochlorite, ammonium hypochlorite, hydrogen peroxide, peracetic acid, m-chloroperbenzoic acid, perbenzoic acid, ammonium hypobromite, calcium hypobromite, potassium hypobromite, sodium hypobromite, and ozone. These may be used individually or in combination of two or more. Among these, water-soluble salts of sodium hypochlorite and sodium hypobromite, and ozonated water are preferred. These oxidizing agents are preferably reacted as a decomposition solution mixed with an alkaline aqueous solution such as an aqueous sodium hydroxide solution, an organic solvent, or a surfactant. The concentration of the oxidizing agent in the aqueous solution is preferably 0.001 to 50% by weight, and more preferably 0.01 to 3% by weight.

[0066] The temperature for contacting the degradable crosslinked material with an aqueous solution containing an oxidizing agent is 100°C or lower, but 15 to 50°C is preferred. The time is preferably 60 minutes or less, and more preferably 10 minutes or less. If necessary, the crosslinked material may be shaken or stirred during the reaction with the oxidizing agent. The specific method for contacting the degradable crosslinked material with an aqueous solution containing an oxidizing agent is not particularly limited and includes methods such as immersing the degradable crosslinked material in an aqueous solution containing an oxidizing agent, or spraying or dropping the aqueous solution containing an oxidizing agent onto the degradable crosslinked material.

[0067] <Degraded products> When n≧1 in equation (1) above, the reaction between the degradable crosslinking product and the oxidizing agent yields the following equation: XZ(X) k -X This yields a decomposition product represented by the following equation. Here, Z and k are the same as in equation (1), and X is the same as X in equation (1). 1a , X 1b , X 2a , X 2b , X 3a , X 3b , X 4a , X 4b This is the same as above. When X is a hydrocarbon group or a single bond, the decomposition product is a carboxylic acid group; when X is an oxygen atom, the decomposition product is an alcohol; when X is -NB- (where B is a hydrogen atom or a hydrocarbon group), the decomposition product is an amine; and when X is a sulfur atom, the decomposition product is a thiol. In a decomposable crosslinking agent, if there are multiple X's that are different from each other, the decomposition product may have two or more selected from the group consisting of carboxylic acid groups, hydroxyl groups, amino groups, and thiol groups.

[0068] The decomposition products preferably have a water solubility of 30 g / L or more, and more preferably 60 g / L or more. The water solubility is measured at 20°C. When decomposition products with high water solubility are produced, the decomposition rate of the crosslinking material is excellent. This is thought to be because the decomposition products dissolve more easily in the aqueous solution containing the oxidizing agent, preventing the reaction between the oxidizing agent and the crosslinking agent from being inhibited by the accumulation of decomposition products, and promoting the penetration of the aqueous solution of the oxidizing agent into the interior of the crosslinking material. However, the present invention is not limited to this mechanism.

[0069] The decomposition products include carboxylic acids, alcohols, amines, or thiols containing Z, and may include sparingly water-soluble decomposition products with low solubility in water. Sparingly water-soluble decomposition products, as used herein, include substances with low solubility in water and substances that do not dissolve in water at all. Specific examples of sparingly water-soluble decomposition products include terephthalic acid, 1,10-decanediol, 4,4'-methylenedianiline, and 1,2-ethanedithiol.

[0070] <Uses of biodegradable crosslinking agents> The biodegradable crosslinking agent of the present invention has excellent solubility in solvents and can therefore be used for crosslinking various resins. Applications of crosslinked products using the biodegradable crosslinking agent of the present invention include adhesives, tacks, superabsorbent resins, resins for 3D modeling, photoresists, release agents, cell culture media, wound fixation materials, and imprinted molded products. [Examples]

[0071] The present invention will be described below with reference to examples, but the present invention is not limited to the following examples. Hereinafter, unless otherwise specified, "parts" or "%" means "parts by weight" or "weight percent," respectively.

[0072] (Comparative Example 1) In a 30 ml two-necked flask, 1.4 g of pyridine, 10.3 g of acetonitrile, and 0.86 g of allyl acetohydrazide were mixed. 0.82 g of sebacate dichloride, dissolved in 6.2 g of acetonitrile, was added dropwise at a temperature below 5°C, and the mixture was stirred at room temperature for 3 hours. The resulting white solid was washed with 30 g of acetonitrile and dried in a vacuum dryer at 40°C to obtain the compound of formula (A) in 95% yield. [ka]

[0073] 1 H-NMR (DMSO, δppm) 1.25 (8H, S, C8H16), 1.50 (4H, t, C8H16), 2.09 (4H, t, C8H16), 2.17~2.18 (8H, m, C2H4), 4 .96(2H, d, CH=CH2), 5.05(2H, d, CH=CH2), 5.76~5.87(2H, m, CH=CH2), 9.66(2H, S, NHNH), 9.69(2H, S, NHNH)

[0074] The solvent solubility of the compound of formula (A) was evaluated, and the results are shown in Table 1. When a 3% sodium hypochlorite aqueous solution was added to the powdered compound of formula (A), foaming and decomposition were observed.

[0075] A thermosetting composition solution was obtained by adding 0.3 g of the compound of formula (A), 0.1 g of poly(methylhydrosiloxane), and 4.0 mg of a platinum-based catalyst (product name: CAT-PL-50T, manufactured by Shin-Etsu Chemical Co., Ltd.) to 40 g of dimethyl sulfoxide. After coating the solution onto a glass substrate to a film thickness of 0.1 μm, it was dried and cured at 150°C for 10 minutes to obtain a degradable crosslinked product. The degradable crosslinked product was insoluble in water, but when immersed in a 3% sodium hypochlorite aqueous solution, it was observed to foam and be removed from the substrate.

[0076] (Example 1) 15.7 g of dimethyl sulfoxide and 0.50 g of sebacate dihydrazide were mixed in a Schlenk tube at 80°C, and 0.46 g of allyl isocyanate was added dropwise, followed by stirring for 4 hours. The reaction mixture, which had been returned to room temperature, was added dropwise to 150 g of acetone to obtain a white solid. This solid was then washed with acetone and dried in a vacuum dryer at room temperature to obtain the compound of formula (B) in 84% yield. [ka]

[0077] 1 H-NMR (DMSO, δppm) 1.24 (8H, S, C8H16), 1.49 (4H, t, C8H16), 2.08 (4H, t, C8H16), 3.61~3.64 (4H, m, CH2), 5.01 (2H, d d, CH=CH2), 5.11(2H, dd, CH=CH2), 5.73~5.83(2H, m, CH=CH2), 6.41(2H, t, NH), 7.69(2H, S, NHNH), 9.39(2H, S, NHNH)

[0078] The solvent solubility of the compound of formula (B) was evaluated, and the results are shown in Table 1. When a 3% sodium hypochlorite aqueous solution was added to the powdered compound of formula (B), foaming and decomposition were observed.

[0079] A thermosetting composition solution was obtained by adding 0.3 g of the compound of formula (B), 0.1 g of poly(methylhydrosiloxane), and 4.0 mg of a platinum-based catalyst (product name: CAT-PL-50T, manufactured by Shin-Etsu Chemical Co., Ltd.) to 40 g of dimethyl sulfoxide. After coating a glass substrate with a curing thickness of 0.1 μm, the solution was dried and cured at 150°C for 10 minutes to obtain a degradable crosslinked product. The degradable crosslinked product was insoluble in water, but when immersed in a 3% sodium hypochlorite aqueous solution, it was observed to foam and be removed from the substrate.

[0080] (Example 2) 22.2 g of dimethyl sulfoxide and 1.00 g of 4,4'-hexyl disemicarbazide were mixed in a 50 ml round-bottom flask at 40°C, and 1.89 g of N-(allyloxycarbonyloxy)succinimide was added dropwise. The mixture was then stirred at room temperature for 4 hours. The reaction mixture was added dropwise to 300 g of acetonitrile to obtain a white solid. This solid was further washed with acetonitrile and dried in a vacuum dryer at room temperature to obtain the compound of formula (C) in 89% yield. [ka]

[0081] 1 H-NMR (DMSO, δppm) 1.22 (4H, S, C6H12), 1.36 (4H, t, C6H12), 2.95~3.00 (4H, m, C6H12), 4.49~4.51 (4H, m, CH2), 5.19 (2H, d, CH=CH2), 5.28~5.33(2H, m, CH=CH2), 5.85~5.94(2H, m, CH=CH2), 6.30(2H, s, NH), 7.65(2H, S, NHNH), 8.83(2H, S, NHNH)

[0082] The solvent solubility of the compound of formula (C) was evaluated, and the results are shown in Table 1. When a 3% sodium hypochlorite aqueous solution was added to the powdered compound of formula (C), foaming and decomposition were observed.

[0083] A thermosetting composition solution was obtained by adding 0.3 g of the compound of formula (C), 0.1 g of poly(methylhydrosiloxane), and 4.0 mg of a platinum-based catalyst (product name: CAT-PL-50T, manufactured by Shin-Etsu Chemical Co., Ltd.) to 40 g of propylene glycol monomethyl ether. The solution was applied to a glass substrate to a curing thickness of 0.1 μm, and then dried and cured at 130°C for 1 minute to obtain a degradable crosslinked product. The degradable crosslinked product was insoluble in water, but when immersed in a 3% sodium hypochlorite aqueous solution, it was observed to foam and be removed from the substrate.

[0084] (Example 3) 22.4 g of dimethyl sulfoxide and 1.00 g of sebacate dihydrazide were mixed in a 50 ml round-bottom flask at room temperature, and 1.90 g of N-(allyloxycarbonyloxy)succinimide was added dropwise, followed by stirring for 20 hours. The reaction mixture was added dropwise to 230 g of deionized water to obtain a white solid, which was then washed with deionized water and dried in a vacuum dryer at 40°C to obtain the compound of formula (D) in 88% yield. [ka]

[0085] 1 H-NMR (DMSO, δppm) 1.24 (8H, S, C8H16), 1.49 (4H, t, C8H16), 2.07 (4H, t, C8H16), 4.51 (4H, d, CH2), 5.19 (2H, d, CH=CH2), 5.30(2H, d, CH=CH2), 5.86~5.95(2H, m, CH=CH2), 9.04(2H, S, NHNH), 9.58(2H, S, NHNH)

[0086] The solvent solubility of the compound of formula (D) was evaluated, and the results are shown in Table 1. When a 3% sodium hypochlorite aqueous solution was added to the powdered compound of formula (D), foaming and decomposition were observed.

[0087] The compound of formula (D) and poly(methylhydrosiloxane) were mixed in a weight ratio of 3:1, dissolved in isopropanol to a concentration of 2% by weight, then diluted with ethyl acetate to a concentration of 1% by weight, and 1 part by weight of a platinum-based catalyst (product name: CAT-PL-50T, manufactured by Shin-Etsu Chemical Co., Ltd.) was added to obtain a thermosetting composition solution. After curing, the solution was applied to a glass substrate to a film thickness of 0.1 μm, dried and cured at 130°C for 1 minute to obtain a degradable crosslinked product. The degradable crosslinked product was insoluble in water, but when immersed in a 3% sodium hypochlorite aqueous solution, it was observed to foam and be removed from the substrate.

[0088] The compound of formula (D), pentaerythritol tetrakis(3-mercaptobutyrate), and N-methylpyrrolidone were mixed in a weight ratio of 3:2:5. The mixture was then diluted with a mixed solvent of isopropanol and propylene glycol monomethyl ether (weight ratio 1:1) to a concentration of 15% by weight. 0.2 parts by weight of a photopolymerization initiator (Omnirad 907, IGM RESINS) and 0.2 parts by weight of another photopolymerization initiator (Omnirad TPO-H, IGM RESINS) were added to obtain a photocurable composition solution. The composition was applied to a glass substrate to a curing thickness of 2.5 μm, dried at 120°C for 3 minutes, and then treated with an ultraviolet irradiation device (UniCure UVH-1500M, Ushio Inc.) at a rate of 500 mJ / cm². 2A biodegradable crosslinked material was obtained by irradiating it with ultraviolet light. The biodegradable crosslinked material was insoluble in water, but when immersed in a 3% sodium hypochlorite aqueous solution, it was observed to foam and be removed from the substrate.

[0089] (Example 4) In a 100 ml round-bottom flask, 10 g of carbinol-modified polydimethylsiloxane (KF-6000, Shin-Etsu Chemical Co., Ltd.), with a molecular weight of approximately 1000, was mixed with 16 g of acetone and 6.5 g of triethylamine. 6.0 g of di(N-succinimidyl) carbonate was added, and the mixture was stirred overnight at room temperature. 47 g of chloroform and 3.1 g of 4-pentenoic acid hydrazide were added to the reaction mixture, and the mixture was stirred again overnight at room temperature. The reaction mixture was transferred to a separatory funnel, 140 g of chloroform was added, and the organic layer was washed three times with 140 g of pure water. After washing, the organic layer was removed by distillation to obtain a compound having the structure of formula (E) in 98% yield. The obtained compound of formula (E) was liquid at 30°C. [ka] In the formula, R represents a hydrocarbon group.

[0090] 1 H-NMR (CDCl3, δppm) 0.06 (76H, br, CH3), 2.29~2.46 (8H, m, CH2CH2), 4.96~5.10 (4H, m, CH=CH2), 5.76~5.94 (2H, m, CH=CH2), 7.74 (2H, br, NHNH), 8.41 (2H, br, NHNH)

[0091] The solvent solubility of the compound of formula (E) was evaluated, and the results are shown in Table 1. When a 3% sodium hypochlorite aqueous solution was added to the compound of formula (E), foaming and decomposition were observed.

[0092] To a mixed solvent of 10 g of toluene and 8 g of isopropanol, 1.61 g of the compound of formula (E), 0.27 g of pentaerythritol tetrakis (mercaptoacetate), 60 mg of polymerization initiator (Omnirad 907, IGM RESINS), and 60 mg of polymerization initiator (Omnirad TPO-H, IGM RESINS) were added and mixed to obtain a photocurable composition solution. After coating a PET film substrate to a curing thickness of 0.9 μm, the solution was dried at 120°C for 2 minutes and then irradiated with ultraviolet light at 500 mJ / cm² using a UV irradiation device (UniCure UVH-1500M, Ushio Inc.). 2 The material was irradiated with ultraviolet light to obtain a degradable crosslinked product. The degradable crosslinked product was insoluble in ethanol and water, but when it was immersed in a solution of Kao Kitchen Hyter containing sodium hypochlorite diluted five times with Solmix AP-1, manufactured by Nippon Alcohol Sales Co., Ltd., whose main component is ethanol, it was observed to foam and be removed from the substrate.

[0093] (Example 5) In a 100 ml round-bottom flask, 3.30 g of 1,12-bis(2,5-dioxy-1-pyrrolidinyl)2,5,8,11-tetraoxadodecanedioic acid, 26 g of dimethylformamide, and 1.6 g of triethylamine were mixed. 0.88 g of succinic acid dihydrazide was added, and the mixture was stirred overnight at room temperature. Next, 0.31 g of 4-hydroxybenzohydrazide was added, and the mixture was stirred for a further 6 hours at room temperature. 37 g of ethyl acetate was added to the reaction mixture, and the mixture was allowed to stand overnight at -10°C to form a precipitate. After removing the organic solvent by decanting, the precipitate was washed twice with 35 g of ethyl acetate. Finally, the solvent was removed by distillation, and a compound having the structure of formula (F) was obtained as a white solid in 79% yield. [ka]

[0094] 1 H-NMR (DMSO, δppm) 2.34 (36H, br, CH2CO), 3.54 (40H, br, CH2O), 3.59 (40H, br, CH2O), 4.10 (40H, br, CH2OC) O), 6.81 (4H, d, benzene ring), 7.72 (4H, d, benzene ring), 9.07 (20H, br, NHNH), 9.67 (20H, br, NHNH), 10.02 (2H, br, OH)

[0095] The molecular weight, calculated from the proton ratio of 1H-NMR, was 3,030.

[0096] The solvent solubility of the compound of formula (F) was evaluated, and the results are shown in Table 1. When a 3% sodium hypochlorite aqueous solution was added to the compound of formula (F), foaming and decomposition were observed.

[0097] To 10 g of deionized water, 1.0 g of the compound of formula (F), 0.14 g of polyglycerol polyglycidyl ether (GEX-521, manufactured by Nagase ChemteX), 0.06 g of benzyltriethylammonium chloride, 2 g of methanol, and 0.06 g of a leveling agent (BYK-348, manufactured by Bic Chemie) were added to obtain a cured composition solution. After curing, the solution was applied to a glass petri dish to a film thickness of 5 μm, and then dried and cured at 120°C for 3 hours to obtain a degradable crosslinked product. The degradable crosslinked product was insoluble in ethanol and water, but when immersed in a solution of Kao Kitchen Hyter containing sodium hypochlorite diluted twice with Solmix AP-1, manufactured by Nippon Alcohol Sales Co., Ltd., whose main component is ethanol, it was observed to foam and be removed from the substrate.

[0098] (Example 6) In a 200 ml round-bottom flask, 2.0 g of 4-hydroxybutyrate hydrazide was dissolved in 170 g of acetonitrile at 50°C. 3.4 g of N-allyloxycarbonyloxysuccinimide was added, and the mixture was stirred at 40°C for 1 hour, followed by stirring at room temperature overnight. After concentrating the reaction mixture using an evaporator, 30 g of chloroform was added, causing N-hydroxysuccinimide to precipitate as a white solid. The N-hydroxysuccinimide was removed by filtration, and the solvent was again removed by distillation to obtain the compound of formula (G) in 90% yield. The obtained compound of formula (G) was liquid at 50°C. [ka]

[0099] 1 H-NMR (DMSO, δppm) 1.61~1.68 (2H, m, CH2), 2.12 (2H, t, C=OCH2), 3.89 (2H, q, OCH2), 4.45 (1H, t, OH), 4.51 (2H, q, C=OOCH2), 5.20(1H, d, C=CH2), 5.30(1H, d, C=CH2), 5.85~5.96(1H, m, CH=C), 9.04(1H, s, NHNH), 9.59(1H, s, NHNH)

[0100] The solvent solubility of the compound of formula (G) was evaluated, and the results are shown in Table 1. When a 3% sodium hypochlorite aqueous solution was added to the compound of formula (G), foaming and decomposition were observed.

[0101] 0.9 g of hexamethylene diisocyanate nurate modified (DIC Corporation, Barnock DN-901S), 1.0 g of compound (G), and 0.9 g of bis(3-mercaptopropionic acid)tetraethylene glycol were dissolved in 20 g of a mixed solvent of propylene glycol monomethyl ether and butyl acetate (weight ratio 1:1). 70 mg of dibutyltin-based curing catalyst (Nitto Chemical Industries, Ltd., Neostan U-810), 40 mg of photopolymerization initiator (IGM Resins, Ltd., Omnirad 907), and 40 mg of photopolymerization initiator (IGM Resins, Ltd., Omnirad TPO-H) were added to obtain a cured composition solution. The above composition was coated onto a glass plate to a dry film thickness of 10 μm, dried and cured at 100°C for 120 minutes, and then further cured with ultraviolet irradiation at 500 mJ / cm² using a UV irradiation device (Ushio Inc., UniCure UVH-1500M). 2 A biodegradable crosslinked material was obtained by irradiating it with ultraviolet light. The biodegradable crosslinked material did not dissolve in water, but when it was immersed in a 3% sodium hypochlorite aqueous solution, it was observed to foam and be removed from the substrate.

[0102] (Example 7) In a 200 ml round-bottom flask, 10.0 g of 2-hydroxyethyl carbazate was added to 38.7 g of glycerol 1,2-carbonate and stirred at 80°C for 6 days. After returning to room temperature, the mixture was added dropwise to 300 g of acetonitrile. The upper layer was removed, and the remaining viscous liquid was dried overnight in a vacuum dryer at 50°C to obtain the compound of formula (H) in 46% yield. The obtained compound of formula (H) was liquid at 40°C. [ka]

[0103] 1H-NMR (DMSO, δppm) 3.49~3.58 (2H, m, CH2), 4.00 (2H, t, CH2), 4.35~4.84 (7H, m), 9.04 (2H, br, NHNH)

[0104] The solvent solubility of the compound of formula (H) was evaluated, and the results are shown in Table 1. When a 3% sodium hypochlorite aqueous solution was added to the compound of formula (H), foaming and decomposition were observed.

[0105] A curing composition solution was obtained by mixing 4.0 g of polymethylene polyphenyl polyisocyanate (Millionate MR-200, manufactured by Tosoh Corporation), 2.0 g of compound (H), 0.2 g of trimethylolpropane, and 50 mg of dibutyltin-based curing catalyst (Neostan U-810, manufactured by Nitto Chemical Industries, Ltd.). The above composition was coated onto a glass plate to a dry film thickness of 10 μm and cured at 70°C for 150 minutes to obtain a degradable crosslinked product. The degradable crosslinked product did not dissolve in THF or water, but when immersed in a solution of 3% sodium hypochlorite aqueous solution diluted three times with THF, it was observed to foam and be removed from the substrate.

[0106] (Example 8) In a 100 ml round-bottom flask, 2.5 g of 3,5-dihydroxybenzoic acid hydrazide was dissolved in 27.3 g of DMSO at room temperature. 2.3 g of 2-isocyanatoethyl methacrylate (Karenz MOI, Resonaq) was added, and the mixture was stirred for 1 day. The reaction mixture was then mixed with 300 g of toluene, and the upper layer was removed. 280 g of methyl isobutyl ketone was added to the remaining lower layer, and a solid precipitated. After filtering the solid, it was washed with 150 g of methyl isobutyl ketone and dried overnight in a vacuum dryer at 30°C to obtain the compound of formula (I) in 82% yield. [ka]

[0107] 1 H-NMR (DMSO, δppm) 1.88 (3H, s, CH3), 3.33 (2H, q, CH2), 4.08 (2H, t, CH2), 5.67 (1H, br, C=CH2), 6.07 (1H, br, C=CH2) , 6.38 (1H, t, benzene ring), 6.55 (1H, t, NH) 6.72 (2H, d, benzene ring), 7.89 (1H, br, NHNH), 9.47 (2H, br, OH), 9.88 (1H, br, NHNH)

[0108] The solvent solubility of the compound of formula (I) was evaluated, and the results are shown in Table 2. When a 3% sodium hypochlorite aqueous solution was added to the compound of formula (I), foaming and decomposition were observed.

[0109] 2.0 g of polyethylene glycol diglycidyl ether (EX-830, manufactured by Nagase ChemteX), 1.0 g of compound (I), and 0.06 g of benzyltriethylammonium chloride were mixed with 20 g of methanol. 4 g of N-methylpyrrolidone and 0.05 g of a photopolymerization initiator (Omnirad 907, manufactured by IGM Resins) were added to obtain a cured composition solution. The above composition was coated onto a glass petri dish to a dry film thickness of 5 μm, dried and cured at 120°C for 2 minutes, and then treated with an ultraviolet irradiation device (UniCure UVH-1500M, manufactured by Ushio Inc.) at a rate of 500 mJ / cm². 2 The material was then irradiated with ultraviolet light. Further curing at 120°C for 2 hours yielded a biodegradable crosslinked material. The biodegradable crosslinked material did not dissolve in isopropanol or water, but when immersed in a solution of 3% sodium hypochlorite aqueous solution diluted twice with isopropanol, it was observed to foam and be removed from the substrate.

[0110] (Example 9) 2.0 g of 3-mercaptopropanehydrazide was dissolved in 26 g of THF in a 100 ml round-bottom flask, and 3.0 g of poly(hexamethylene diisocyanate) (Sigma Aldrich) was added dropwise. The mixture was stirred overnight at room temperature. The precipitated white solid was collected by decantation and dried in a vacuum dryer to obtain a crosslinking agent having the structure of formula (J) in 94% yield. [ka]

[0111] 1 H-NMR (DMSO, δppm) 1.24~1.50 (24H, m, CH2), 2.41 (6H, t, C=OCH2), 2.67 (6H, t, SCH2), 2.9 7~3.10(12H, m, NCH2), 6.26(3H, s, NH), 7.67(3H, s, NH), 8.21(2H, br, NH), 9.50(3H, s, NH)

[0112] The solvent solubility of the compound of formula (J) was evaluated, and the results are shown in Table 2. When a 3% sodium hypochlorite aqueous solution was added to the compound of formula (J), foaming and decomposition were observed.

[0113] 1.2 g of compound (J) and 2.3 g of reactive silicone oil having acrylate groups at both ends (X-22-2445, Shin-Etsu Silicone Co., Ltd.) were dissolved in a mixed solvent of 20 g of N-methylpyrrolidone, 4 g of toluene, and 10 g of methyl ethyl ketone. 0.3 g of leveling agent (BYK-307, BIC Chemie Co., Ltd.), 0.2 g of photopolymerization initiator (Omnirad 907, IGM Resins Co., Ltd.), and 0.2 g of photopolymerization initiator (Omnirad TPO-H, IGM Resins Co., Ltd.) were added to obtain a cured composition solution. The above composition was applied to a PET film to a dry film thickness of 0.8 μm, dried at 120°C for 10 minutes, and then subjected to a curing agent of 2000 mJ / cm². 2 A biodegradable crosslinked material was obtained by curing it with UV light. The biodegradable crosslinked material was insoluble in water, but when immersed in a 3% sodium hypochlorite aqueous solution, it was observed to foam and be removed from the substrate.

[0114] (Example 10) In a 100 ml round-bottom flask, 10 g of methyl polyacrylate (UMM-1001, manufactured by Soken Chemical Co., Ltd.), with a molecular weight of approximately 1000 and a hydroxyl group at one end, 13 g of acetonitrile, and 5.1 g of triethylamine were mixed. 4.7 g of di(N-succinimidyl) carbonate was added, and the mixture was stirred overnight at room temperature. Next, 1.4 g of trihydrazide trimesic acid and 80 g of dimethyl sulfoxide were added, and the mixture was stirred at 60°C for 4 hours. The reaction mixture was transferred to a separatory funnel, and 210 g of ethyl acetate and 210 g of pure water were added to remove the aqueous layer. The organic layer was then washed four times with 90 g of pure water, and the organic solvent was removed by distillation. 4 g of the residue was taken, dissolved in 30 g of acetonitrile, and then 10 g of ethanol was added. This process of concentration using an evaporator was repeated twice. The purified residue was transferred to a 500 ml round-bottom flask and dissolved in 168 g of ethanol and 100 g of acetonitrile. 38 g of hydrazine monohydrate was added in four portions, and the mixture was stirred at room temperature for four days. The reaction mixture was added dropwise to 140 g of ice-cooled isopropanol to precipitate a solid. The obtained solid was washed with 40 g of acetonitrile and then dried in a vacuum dryer at 50°C for 3 hours. 1.0 g of the dried solid was transferred to a 30 ml round-bottom flask, dissolved in 11.1 g of DMSO, and 2.3 g of N-allyloxycarbonyloxysuccinimide was added. The mixture was stirred overnight at room temperature. The reaction mixture was added dropwise to 87 g of deionized water to precipitate the solid. The obtained solid was dissolved in 6 g of ethanol and added dropwise to 60 g of methyl isobutyl ketone to precipitate the solid again. The obtained solid was dried overnight in a vacuum dryer at 30°C to obtain 0.5 g of the compound of formula (K). [ka] In the formula, R represents a hydrocarbon group.

[0115] 1 H-NMR (DMSO, δppm) 1.4~1.9 (75H, m, CH2), 1.95~2.41 (37H, m, CH), 4.55 (71H, d, OCH2), 5.21 (35H, t, C=CH2) , 5.32 (35H, d, C=CH2), 5.91 (35H, br, C=CH), 8.48 (3H, s, benzene ring), 9.30 (72H, br, NHNH), 10.61 (3H, br, NHNH)

[0116] The solvent solubility of the compound of formula (K) was evaluated, and the results are shown in Table 2. When a 3% sodium hypochlorite aqueous solution was added to the compound of formula (K), foaming and decomposition were observed.

[0117] The compound of formula (K), pentaerythritol tetrakis (mercaptoacetate), and the compound of formula (I) were mixed in a weight ratio of 3:2:2. The mixture was diluted with methanol to a concentration of 15% by weight. Then, 0.2 parts by weight of a photopolymerization initiator (Omnirad 907, IGM RESINS) and 0.2 parts by weight of another photopolymerization initiator (Omnirad TPO-H, IGM RESINS) were added to obtain a photocurable composition solution. The composition was applied to a glass substrate to a curing thickness of 4 μm, dried at 120°C for 1 minute, and then treated with an ultraviolet irradiation device (UniCure UVH-1500M, Ushio Inc.) at a rate of 500 mJ / cm². 2 A biodegradable crosslinked material was obtained by irradiating it with ultraviolet light. The biodegradable crosslinked material was insoluble in water, but when immersed in a 3% sodium hypochlorite aqueous solution, it was observed to foam and be removed from the substrate.

[0118] (Example 11) In a 100 mL three-necked flask, 5.0 g of succinate dihydrazide was dissolved in 30 g of methyl sulfoxide, and 15.7 g of diethyl 2-isocyanatoglutarate was added. The mixture was stirred at room temperature for 1 day, then 24.7 g of hydrazine monohydrate was added and the mixture was stirred for another day. This reaction mixture was added dropwise to 900 g of methanol to precipitate a solid. The obtained solid was washed with 300 g of methanol and dried in a vacuum dryer at 40 °C for 3 hours. 5 g of the dried solid was transferred to a 100 mL round-bottom flask, dissolved in 23 g of DMSO, and 7.3 g of N-allyloxycarbonyloxysuccinimide was added. The mixture was stirred at room temperature for 1 day. This reaction mixture was added dropwise to 550 g of acetonitrile to precipitate a solid. The precipitated solid was washed with 250 g of acetonitrile and dried in a vacuum dryer at 50 °C for 3 hours to obtain 2.6 g of compound (L). [ka]

[0119] 1 H-NMR (DMSO, δppm) 1.68~1.91 (4H, m, CH2), 2.04~2.17 (4H, m, C=OCH2), 2.37 (4H, br, C= OCH2), 4.07~4.13(2H, m, C=OCH), 4.51(8H, br, OCH2), 5.19(4H, d, C=CH2), 5.30(4H, d, C=CH2), 5.89(4H, br, CH=C), 6.52(2H, br, NC=ONHC), 7.90(2H, s, NHNH), 9.03(2H, br, N HNH), 9.19(2H, br, NHNH), 9.57(2H, br, NHNH), 9.64(2H, br, NHNH), 9.81(2H, br, NHNH)

[0120] The solvent solubility of the compound of formula (L) was evaluated, and the results are shown in Table 2. When a 3% sodium hypochlorite aqueous solution was added to the compound of formula (L), foaming and decomposition were observed.

[0121] 0.26 g of compound (L) and 0.22 g of bis(3-mercaptopropionic acid)tetraethylene glycol were dissolved in 4 g of a mixed solvent of methanol and N-methylpyrrolidone (weight ratio 3:1). 8 mg of photopolymerization initiator (Omnirad 907, IGM RESINS) and 8 mg of photopolymerization initiator (Omnirad TPO, IGM RESINS) were added to obtain a curable composition. The above composition was coated onto a glass plate to a dry film thickness of 2 μm and irradiated with ultraviolet light at 500 mJ / cm² using a UV irradiation device (UniCure UVH-1500M, Ushio Inc.). 2 The material was irradiated with ultraviolet light to obtain a biodegradable molded product. The biodegradable crosslinked product did not dissolve in water, but when it was immersed in a 3% sodium hypochlorite aqueous solution, it was observed to foam and be removed from the substrate.

[0122] (Example 12) In a 1 L round-bottom flask, 14.5 g of N-hydroxysuccinimide was dissolved in 377 g of THF, and 9.5 g of isophthalic acid and 24.3 g of 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride were added and the mixture was stirred overnight at room temperature. After concentration using an evaporator, 310 g of chloroform was added and the mixture was transferred to a separatory funnel. The organic layer was washed four times with 200 g of deionized water. The organic layer was dried over 5.8 g of magnesium sulfate and then concentrated using an evaporator. The concentrate was added dropwise to 150 g of isopropanol to precipitate the solid. The obtained solid was dried overnight in a vacuum dryer at 25°C. 13.6 g of 6-hydroxyhexanoic acid hydrazide, 18 g of triethylamine, and 40 g of DMF were mixed in a 100 mL round-bottom flask. 15.3 g of the above-mentioned dried solid was added to the mixture and stirred overnight at room temperature. This reaction solution was then added dropwise to 800 g of acetonitrile to precipitate a white powder. This white powder was filtered, washed with 200 g of acetonitrile, and dried in a vacuum dryer at 50°C for 3 hours. 6 g of the dried white powder was transferred to a 100 mL round-bottom flask and dissolved in 36 g of DMF. Then, 8.7 g of triethylamine and 7.3 g of di(N-succinimidyl) carbonate were added and stirred for 90 minutes at room temperature. Finally, 3.4 g of 2-hydroxyethyl carbazate was added and the mixture was stirred overnight. The reaction solution was added dropwise to 800 g of acetonitrile to precipitate a solid, which was then washed with 200 g of acetonitrile and dried in a vacuum dryer at 50°C for 3 hours to obtain 6.7 g of compound (M). [ka]

[0123] 1 H-NMR (DMSO, δppm) 1.31~1.63 (12H, m, CH2), 2.17~2.24 (4H, m, O=CCH2), 3.55 (4H, q, OCH2), 3.99~4.023 (8H, q, O=COCH2), 4.77 (2H, br, OH), 7. 62 (1H, t, benzene ring), 8.03 (2H, dd, benzene ring), 8.37 (1H, s, benzene ring), 9.00 (2H, br, NHNH), 9.03 (2H, br, NHNH), 9.99 (2H, br, NHNH), 10.40 (2H, br, NHNH)

[0124] The solvent solubility of the compound of formula (M) was evaluated, and the results are shown in Table 2. When a 3% sodium hypochlorite aqueous solution was added to the compound of formula (M), foaming and decomposition were observed.

[0125] A curing composition solution was obtained by mixing 1.5 g of polymethylene polyphenyl polyisocyanate (Millionate MR-200, manufactured by Tosoh Corporation), 4.0 g of compound (M), 50 mg of dibutyltin-based curing catalyst (Neostan U-810, manufactured by Nitto Chemical Industries, Ltd.), and 5 g of N-methylpyrrolidone. The above composition was coated onto a glass plate to a dry film thickness of 2 μm, and dried and cured at 120°C for 150 minutes to obtain a degradable crosslinked product. The degradable crosslinked product did not dissolve in THF or water, but when immersed in a solution of 3% sodium hypochlorite aqueous solution diluted three times with THF, it was observed to foam and be removed from the substrate.

[0126] (Example 13) In a 100 ml round-bottom flask, 10 g of triol-type polypropylene glycol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) with a molecular weight of approximately 1500, 40 g of acetonitrile, and 18.2 g of triethylamine were mixed. 15.3 g of di(N-succinimidyl) carbonate was added, and the mixture was stirred overnight at room temperature. After removing the precipitated solid by filtration, 54 g of chloroform and 100 g of pure water were added to the filtrate, and liquid-liquid extraction was performed. After removing the aqueous layer, the solvent was removed by distillation to a concentration of 80%. 11 g of acetonitrile and 2.8 g of triethylamine were added, followed by the addition of 0.22 g of 2-hydroxyethyl carbazate, and the mixture was stirred at room temperature for 4 hours. The completion of the reaction was confirmed by NMR, and then 1.9 g of α-resorcinol hydrazide was added and the mixture was stirred at room temperature for 4 hours. After concentrating the reaction mixture in an evaporator, 103 g of chloroform was added, and the mixture was transferred back to a separatory funnel. The organic layer was washed twice with 70 g of deionized water, and the solvent was removed by evaporation using an evaporator to obtain a degradable compound having the structure of formula (N) in 61% yield. [ka]

[0127] 1 H-NMR (DMSO, δppm) 1.05 (77H, d, CH3), 3.32~3.67 (80H, m, CH, CH2), 4.00 (6H, t, O=COCH2), 4.75 (3H, t, OH), 8.97 (3H, br, NHNH), 8.99 (3H, br, NHNH)

[0128] The solvent solubility of the compound of formula (N) was evaluated, and the results are shown in Table 2. When a 3% sodium hypochlorite aqueous solution was added to the compound of formula (N), foaming and decomposition were observed.

[0129] A curing composition solution was obtained by mixing 1.0 g of polymethylene polyphenyl polyisocyanate (Millionate MR-200, manufactured by Tosoh Corporation), 5.0 g of compound (N), 60 mg of dibutyltin-based curing catalyst (Neostan U-810, manufactured by Nitto Chemical Industries, Ltd.), and 0.5 g of methyl isobutyl ketone. The above composition was coated onto a polyester nonwoven fabric to a dry film thickness of 200 μm, heated at 60°C for 10 minutes, and then heated at 40°C for 6 hours to obtain a degradable crosslinked product. The degradable crosslinked product did not dissolve in isopropanol or water, but when immersed in a solution of 3 wt% aqueous solution of sodium dichloroisocyanurate diluted twice with isopropanol, it was observed to foam and be removed from the substrate.

[0130] (Evaluation of solvent solubility) 2 mg of the degradable crosslinking agent from Examples 1-13 and Comparative Example 1 was mixed with 0.5 ml of the solvents listed in Tables 1-2 and stirred, and dissolution was visually confirmed. Any undissolved material at room temperature was thoroughly heated with a heat gun and visually checked again. Three samples were assigned to samples that were completely dissolved at room temperature, two samples were assigned to samples that were undissolved at room temperature but completely dissolved after heating, one sample was assigned to samples with a small amount of undissolved material after heating, and zero samples were assigned to samples with a large amount of undissolved material after heating. For the degradable crosslinking agents in liquid form, the compatibility with the solvents was evaluated. The results are shown in Tables 1-2.

[0131] [Table 1]

[0132] [Table 2]

[0133] The compound of formula (A) in Comparative Example 1 had low solubility in all solvents. The compounds of Examples 1 to 13 showed solubility in multiple solvents. In particular, the compounds of Examples 1 to 7 and Examples 10 to 13, which have an -NHNHCOO- structure, showed high solubility. The compound of Example 9, having a branched structure, showed usable solubility, although slightly inferior to that of the compound of Example 3. The compounds of Examples 5 and 10, having high molecular weights, showed usable solubility, although slightly inferior to that of the compound of Example 3. The compounds of Examples 7 to 8 showed usable solubility, although slightly inferior to that of the compound of Example 3, due to the localization of reactive functional groups.

[0134] This disclosure (1) is a degradable crosslinking agent comprising a compound represented by the following formula (1). [ka] (In formula (1), n≧0, k≧0, m≧0, p1≧1, p2≧1, p3≧1. ·R 1 , R 2 , R 3 These are hydrocarbons having 1 to 500 carbon atoms, which may independently have single bonds, substituents, or heteroatoms. Q 1 Q 2 Q 3 These are one or more reactive functional groups independently selected from the group consisting of hydroxyl groups, amino groups, thiol groups, hydrazide groups, carboxylic acid groups, acid anhydride groups, vinyl groups, allyl groups, acrylate groups, methacrylate groups, crotonate groups, isoprenyl groups, acrylamide groups, methacrylamide groups, crotonamide groups, epoxy groups, oxetane groups, oxazoline groups, isocyanate groups, carbodiimide groups, methylol groups, silanol groups, hydroxysilyl groups, and alkoxysilyl groups. ·X 1a , X 1b , X 2a , X 2b , X 3a , X 3b , X 4a , X 4b Each is independently an oxygen atom, a sulfur atom, a single bond, a hydrocarbon group having 1 to 20 carbon atoms which may have substituents, or -NB- (where B is a hydrogen atom or a hydrocarbon group), but X 1a , X 1b , X 2a , X 2b , X 3a , X 3b , X 4a , X 4b One or more of these atoms are an oxygen atom, a sulfur atom, or an -NB- group (where B is a hydrogen atom or a hydrocarbon group). ·A 1 ~A 8 is a carbonyl group or a single bond, A 1 and A 2 At least one of them is a carbonyl group, A 3 and A 4 At least one of them is a carbonyl group, A 5 and A 6 At least one of them is a carbonyl group, A 7 and A 8 At least one of them is a carbonyl group. Z is a hydrocarbon group having 1 to 500 carbon atoms, which may independently contain a siloxane structure, a divalent or greater group, or a heteroatom.

[0135] (2) This disclosure is p1≧2, p2≧2, or p3≧2, and there are multiple Q 1 Allies, Q 2 Both or Q 3 This is a degradable crosslinking agent according to disclosure (1), wherein each of the reactive functional groups is different from the others.

[0136] Disclosure (3) is the degradable crosslinking agent described in Disclosure (1), wherein p1=1, p2=1, or p3=1.

[0137] Disclosure (4) is a degradable crosslinking agent according to any one of Disclosures (1) to (3), having at least one degradation site represented by the following formula (2). -X 5 -CO 1 -NH-NH-CO 2 -X 6 - (2) (In formula (2), X 5 , X 6 These are all different from each other and are an oxygen atom, a sulfur atom, a single bond, a C1-C20 hydrocarbon group which may have substituents, or -NB- (where B is a hydrogen atom or a hydrocarbon group). 1 , C 2 is a carbonyl group or single bond, C 1 and C 2 At least one of them is a carbonyl group.

[0138] This disclosure (5) is X 1a or X 1b The degradable crosslinking agent is one of the descriptions (1) to (4) of this disclosure, wherein the atom is an oxygen atom.

[0139] Disclosure (6) is a degradable crosslinking agent according to any of Disclosures (1) to (5), wherein n ≥ 1.

[0140] This disclosure (7) is for n≧1, X 1a , X 1b , X 2a , X 2b , X 3a , X 3b , X 4a , X 4b among At least one is an oxygen atom, At least one of them is a single bond or a hydrocarbon group having 1 to 20 carbon atoms which may have substituents, At least one is -NB- (where B is a hydrogen atom or a hydrocarbon group). The degradable crosslinking agent is one of the descriptions in (1) to (6) of this disclosure.

[0141] Disclosure (8) is a degradable crosslinking agent according to any of Disclosures (1) to (7), having a molecular weight of 2000 or less.

[0142] Disclosure (9) is a degradable crosslinking agent according to any of Disclosures (1) to (8), wherein k ≥ 1.

[0143] Disclosure (10) is a composition comprising a degradable crosslinking agent described in any of Disclosures (1) to (9) and one or more selected from the group consisting of a curable resin, a polymerization initiator, and a solvent.

[0144] Disclosure (11) is the composition described in Disclosure (10), which substantially does not contain a solvent with a boiling point above 150°C.

[0145] Disclosure (12) is a degradable crosslinked product comprising the composition described in Disclosure (10) or (11).

[0146] This disclosure (13) is a degradable crosslinked product as described in this disclosure (12) that can be degraded with an oxidizing agent.

[0147] The present disclosure (14) is a method for decomposing a decomposable crosslinked product, comprising the step of bringing the decomposable crosslinked product described in the present disclosure (12) or (13) into contact with an aqueous solution containing an oxidizing agent at a temperature of 100°C or lower.

Claims

1. A degradable crosslinking agent comprising a compound represented by the following formula (1). 【Chemistry 1】 (In formula (1), n≧0, k≧0, m≧0, p1≧1, p2≧1, p3≧1. ・R 1 , R 2 , R 3 These are hydrocarbons having 1 to 500 carbon atoms, which may independently have single bonds, substituents, or heteroatoms. Q 1 Q 2 Q 3 These are one or more reactive functional groups independently selected from the group consisting of hydroxyl groups, amino groups, thiol groups, hydrazide groups, carboxylic acid groups, acid anhydride groups, vinyl groups, allyl groups, acrylate groups, methacrylate groups, crotonate groups, isoprenyl groups, acrylamide groups, methacrylamide groups, crotonamide groups, epoxy groups, oxetane groups, oxazoline groups, isocyanate groups, carbodiimide groups, methylol groups, silanol groups, hydroxysilyl groups, and alkoxysilyl groups. ·X 1a , X 1b , X 2a , X 2b , X 3a , X 3b , X 4a , X 4b are each independently an oxygen atom, a sulfur atom, a single bond, an optionally substituted hydrocarbon group having 1 to 20 carbon atoms, or -NB- (B is a hydrogen atom or a hydrocarbon group), provided that X 1a , X 1b , X 2a , X 2b , X 3a , X 3b , X 4a , X 4b One or more of these atoms are an oxygen atom, a sulfur atom, or -NB- (where B is a hydrogen atom or a hydrocarbon group). A 1 ~A 8 A is a carbonyl group or a single bond. 1 and A 2 At least one of them is a carbonyl group, A 3 and A 4 At least one of them is a carbonyl group, A 5 and A 6 At least one of them is a carbonyl group, A 7 and A 8 At least one of them is a carbonyl group. Z is a hydrocarbon group having 1 to 500 carbon atoms, which may independently contain a siloxane structure, a divalent or higher group, or a heteroatom.

2. Q such that p1 ≥ 2, p2 ≥ 2, or p3 ≥ 2, and there are multiple such Qs. 1 Comrades, Q 2 Fellow or Q 3 The degradable crosslinking agent according to claim 1, wherein each of the reactive functional groups is different from the others.

3. A degradable crosslinking agent according to claim 1 or 2, wherein p1 = 1, p2 = 1, or p3 = 1.

4. A degradable crosslinking agent according to claim 1 or 2, having at least one decomposition site represented by the following formula (2). -X 5 -C 1 -NH-NH-C 2 -X 6 - (2) (In formula (2), X 5 , X 6 These are all different from each other and are an oxygen atom, a sulfur atom, a single bond, a hydrocarbon group having 1 to 20 carbon atoms which may have substituents, or -NB- (where B is a hydrogen atom or a hydrocarbon group). 1 , C 2 is a carbonyl group or single bond, C 1 and C 2 At least one of them is a carbonyl group.

5. X 1a or X 1b A degradable crosslinking agent according to claim 1 or 2, wherein is an oxygen atom.

6. A degradable crosslinking agent according to claim 1 or 2, wherein n ≥ 1.

7. n ≥ 1, X 1a , X 1b , X 2a , X 2b , X 3a , X 3b , X 4a , X 4b among At least one is an oxygen atom, At least one of them is a single bond or a hydrocarbon group having 1 to 20 carbon atoms which may have substituents, At least one is -NB- (where B is a hydrogen atom or a hydrocarbon group). A degradable crosslinking agent according to claim 1 or 2.

8. A degradable crosslinking agent according to claim 1 or 2, wherein the molecular weight is 2000 or less.

9. A degradable crosslinking agent according to claim 1 or 2, wherein k ≥ 1.

10. A composition comprising a degradable crosslinking agent according to claim 1 or 2, and one or more selected from the group consisting of a curable resin, a polymerization initiator, and a solvent.

11. The composition according to claim 10, which substantially does not contain solvents with a boiling point above 150°C.

12. A degradable crosslinked product comprising the composition described in claim 10.

13. A degradable crosslinked product according to claim 12, which can be decomposed by an oxidizing agent.

14. A method for decomposing a decomposable crosslinked product, comprising the step of bringing the decomposable crosslinked product described in claim 12 into contact with an aqueous solution containing an oxidizing agent at a temperature of 100°C or lower.

Citation Information

Patent Citations

  • Method for producing poly(diacylhydrazine) and poly(diacylhydrazine)

    JP2011052075A

  • Epoxy curing agent, epoxy resin composition, semiconductor device, and repairing method therefor

    JP2011236381A

  • Curable composition, cured product and polymer compound

    JP2024001645A

  • Sealant for liquid crystal display element, vertical conduction material, and liquid crystal display element

    WO2019225376A1

  • Crosslinked polymer compound and method for producing same, absorbent article, paper diaper, sanitary article, disposal container, and disposal method

    WO2021131003A1