Photosensitive resin compositions, dry films, cured products, printed circuit boards, and laminates

A photosensitive resin composition with a carboxyl group-containing resin and trimethylbenzoylphosphine oxide initiator addresses outgassing issues, maintaining high reflectivity and reducing process complexity and power consumption in solder resist layers.

JP7955485B2Active Publication Date: 2026-11-24TAIYO INK MFG CO KOREALTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2025515601
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2024-03-27
Filing Date
2024-03-28
Publication Date
2026-11-24
Estimated Expiration
2044-03-28

Smart Images

  • Figure 0007955485000020
    Figure 0007955485000020
  • Figure 0007955485000021
    Figure 0007955485000021
  • Figure 0007955485000001
    Figure 0007955485000001
Patent Text Reader

Abstract

One embodiment of the present invention relates to a photosensitive resin composition comprising (A) a carboxyl group-containing resin not containing an aromatic ring, (B) an inorganic filler, and (E) a photopolymerization initiator that is a trimethylbenzoylphosphine oxide group-containing compound containing one or more P-O bonds. The combination of these four components significantly reduces outgassing of the photopolymerization initiator, thereby improving the yellowing and uncured state of silicone encapsulants and improving the reactivity of silicone encapsulants. Furthermore, the composition can prevent transfer of outgassing of the photopolymerization initiator to the protective film, eliminating the need for a baking process after the reflow process. Furthermore, the composition can improve power consumption by increasing reflectivity. Furthermore, the composition exhibits high HAST resistance and reflectivity after the HAST test, and the decrease in reflectivity under high temperature / high humidity conditions is suppressed. These characteristics enable the photosensitive resin composition of the present invention to exhibit excellent effectiveness as a solder resist. Therefore, the photosensitive resin composition of the present invention can efficiently open many holes in the solder resist, and the solder resist has high reflectivity, making it possible to realize an efficient backlight unit.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a photosensitive resin composition, a dry film, a cured product, a printed circuit board, and a laminate. More specifically, the dry film has a photosensitive resin layer obtained by coating and drying the photosensitive resin composition on a first film, the cured product is obtained by curing the photosensitive resin layer of the dry film, and the printed circuit board and laminate include the cured product. [Background technology]

[0002] Generally, in printed circuit boards used in electronic devices and the like, a solder resist layer is formed in areas other than the connection holes on the board where the circuit pattern is formed, in order to prevent solder from adhering to unnecessary parts when mounting electronic components on the printed circuit board, and to prevent the circuit conductors from being exposed and corroded by oxidation and humidity.

[0003] With the recent trend towards miniaturization and lighter electronic devices, and the resulting increase in the precision and density of printed circuit boards, the solder resist layer is now predominantly formed using so-called photosolder resist. This involves applying a photosensitive resin composition to the substrate, forming a pattern through exposure and development, and then curing the patterned resin by heating or light irradiation.

[0004] As described above, liquid photosensitive resin compositions contain solvents and require repeated printing and drying processes during manufacturing, resulting in long working times and environmentally unfriendly issues.

[0005] Therefore, it has been proposed to form the solder resist layer using a so-called photosensitive dry film, which eliminates the drying step after coating the composition, instead of a liquid photosensitive resin composition. Laminating with a dry film shortens the working time, greatly reduces the manufacturing process, and offers excellent productivity, as well as enabling the efficient use of the solder resist layer even on thin-film substrates.

[0006] Such dry films generally include a laminated structure in which a solder resist layer, which is a photosensitive resin layer, is formed on a first film that serves as a substrate, and a second film for purposes such as protection is bonded to this layer. When used, the second film is peeled off and heat-pressed onto a wiring board, and after exposure from above the first film, the first film is peeled off and developed to form a patterned solder resist layer. When forming a solder resist layer using a dry film, compared to using a liquid photosensitive resin composition as described above, not only is the drying process of the composition omitted, but because the dry film is pressed onto the circuit board, it is difficult for air bubbles to be mixed between the substrate and the solder resist layer, and the ability to fill pores in recesses on the substrate surface is also improved. Furthermore, when forming a solder resist layer using a dry film, the flatness of the film is excellent, so chips can be mounted efficiently and have high resolution.

[0007] However, because the white solder resist layer has a higher reflectivity than the colored solder resist layer, when forming a solder resist layer using a dry film in the manner described above, light is reflected from the surface of the solder resist layer during exposure, making it difficult for light to penetrate to the bottom. This results in a phenomenon called halation, where the upper part of the surface is larger than the lower part, making it difficult to realize the pattern (see, for example, Patent Document 1).

[0008] On the other hand, since the solder resist layer also functions as a permanent protective film for the circuit board, the solder resist composition is required to possess various properties such as alkali developability and solder heat resistance.

[0009] Furthermore, in addition to the properties required for general solder resist layers, the white solder resist layer also possesses high reflectivity, exhibits minimal decrease in reflectivity during the manufacturing process, and does not yellow even when exposed to heat or light.

[0010] There is a need for a photosensitive resin composition that satisfies the basic properties required for a solder resist layer, as well as additional properties required for a white solder resist layer, has a higher reflectivity than conventional materials, and exhibits excellent resistance to yellowing, and for a method of manufacturing a dry film and printed circuit board containing a solder resist layer that can solve the specific problems that arise during the manufacturing process of the solder resist layer. [Prior art documents] [Patent Documents]

[0011] [Patent Document 1] Detailed description of the invention of Korean Published Patent No. 10-2022-0086524

[0012] [Technical issues] Conventionally, photopolymerization initiators (e.g., 2,4,6-trimethylbenzoyldiphenyl phosphine oxide (TPO)) contained in photosensitive resin compositions that form solder resists generate a large amount of outgassing. If this outgassing spreads to the adjacent silicon encapsulant, the transparent silicon encapsulant may yellow, reducing its reflectivity and making it difficult for the silicon encapsulant to cure. These problems have led to issues with the long-term reliability of the substrate. In addition, the photopolymerization initiator can be transferred not only to the silicon encapsulant but also to adjacent substrates.

[0013] Therefore, to remove outgassing of the photopolymerization initiator, it was considered to add a curing step (e.g., curing at 150°C for 6 hours) after the reflow step (e.g., 10 seconds at 260°C). However, such a curing step significantly reduces reflectivity, leading to the problem of increased power consumption to increase reflectivity after the chip is mounted when used in backlight units, etc. In other words, the number of steps increases, and reflectivity may also decrease.

[0014] Furthermore, before performing such a firing process, a protective film (PF) can be placed on the solder resist layer to remove the photoinitiator. The protective film is used to remove as much outgassing of the photoinitiator as possible after the solder resist has been prepared and before the subsequent firing process. It is peeled off and removed before the firing process, and because it has a high affinity for the photoinitiator, it can efficiently remove the photoinitiator and was used for the purpose of removing the photoinitiator. However, ultimately, the use of such a protective film and the firing process are required, and the problem of reduced reflectivity still remains.

[0015] The present invention aims to solve the above-mentioned problems and provides a technology for a photosensitive resin composition comprising (A) a carboxyl group-containing resin that does not contain an aromatic ring, (B) an inorganic filler or (C) a mercapto-modified (meth)acrylate, and (E) a photopolymerization initiator which is a trimethylbenzoylphosphine oxide group-containing compound containing one or more PO bonds.

[0016] The photosensitive resin composition of the present invention significantly reduces outgassing of the photopolymerization initiator, thereby improving the problems of yellowing and incurability of the silicone encapsulant and improving the reaction rate of the silicone encapsulant. Furthermore, it suppresses the amount of outgassing generated by the photopolymerization initiator, reduces the amount of outgass transferred to the protective film, eliminates the need for a firing process after the reflow process, and improves the problem of power consumption by increasing reflectivity. In addition, it exhibits high reflectivity, excellent HAST resistance, and suppresses the decrease in reflectivity under high temperature / high humidity conditions after HAST (Highly Accelerated Stress Test) resistance, reflow, UV test, or HAST test. Due to these characteristics, the solder resist produced using the photosensitive resin composition of the present invention exhibits excellent effects.

[0017] Furthermore, the present invention provides dry films, cured products, printed circuit boards, and laminates using the photosensitive resin composition described above. [Technical solution]

[0018] One embodiment of the present invention relates to a photosensitive resin composition.

[0019] In one aspect, the photosensitive resin composition may include (A) a carboxyl group-containing resin that does not contain an aromatic ring, (B) an inorganic filler, and (E) a photopolymerization initiator that is a trimethylbenzoylphosphine oxide group-containing compound including one or more P-O bonds.

[0020] In one aspect, the photopolymerization initiator that is the (E) trimethylbenzoylphosphine oxide group-containing compound including one or more P-O bonds may include a *-C(=O)-P(=O)R1-O-*' moiety (wherein R1 is an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, or a cyclic group having 5 to 20 carbon atoms).

[0021] In one aspect, the photopolymerization initiator that is the (E) trimethylbenzoylphosphine oxide group-containing compound including one or more P-O bonds may be a trimethylbenzoylphosphine oxide group-containing polymer.

[0022] In one aspect, the trimethylbenzoylphosphine oxide group-containing polymer may have a weight average molecular weight (Mn) of 900 g / mol or more.

[0023] In one aspect, the trimethylbenzoylphosphine oxide group-containing polymer may be represented by the following Chemical Formula 1.

[0024] [Chemical Formula] a=0~100, b=0~100, c=0~100

[0025] In one aspect, the photopolymerization initiator that is the (E) trimethylbenzoylphosphine oxide group-containing compound including one or more P-O bonds may include an alkoxy group.

[0026] In one aspect, the photopolymerization initiator, which is a trimethylbenzoylphosphine oxide group-containing compound having one or more PO bonds, may contain an ethoxy group.

[0027] In one aspect, the photopolymerization initiator that is a trimethylbenzoylphosphine oxide group-containing compound having one or more PO bonds (E) may be represented by the following chemical formula 2.

[0028] [ka]

[0029] In one aspect, the content of the photopolymerization initiator, which is a trimethylbenzoylphosphine oxide group-containing compound having one or more PO bonds, may be 0.01 to 10% by weight relative to the total weight of the composition.

[0030] In one respect, the carboxyl group-containing resin that does not contain the aromatic ring (A) may contain an unsaturated double bond.

[0031] In one aspect, the photosensitive resin composition may further contain a resin containing (D) an aromatic ring.

[0032] In one aspect, the resin containing the (D) aromatic ring may be a melamine resin, a silicone resin, or a resin having a styrene skeleton.

[0033] In one aspect, the photosensitive resin composition may further contain (C) mercapto-modified (meth)acrylate.

[0034] In one aspect, the photosensitive resin composition may further contain (F) a silane coupling agent.

[0035] In one aspect, the photosensitive resin composition may further contain (G) a resin having a urethane bond.

[0036] In one aspect, the outgassing content of the photosensitive resin composition, as measured by thermal desorption spectroscopy (TDS) and gas chromatography-mass spectrometry (GC-MS), may be 1,000 ppm or less relative to the content of the photopolymerization initiator, which is a trimethylbenzoylphosphine oxide group-containing compound having one or more PO bonds.

[0037] In one aspect, the photosensitive resin composition may have a phosphorus content of 500 to 5000 ppm.

[0038] Another embodiment of the present invention relates to a photosensitive resin composition comprising (A) a carboxyl group-containing resin that does not contain an aromatic ring, (C) a mercapto-modified (meth)acrylate, and (E) a photopolymerization initiator which is a trimethylbenzoylphosphine oxide group-containing compound containing one or more PO bonds.

[0039] In one aspect, the photosensitive resin composition may further contain a resin containing (D) an aromatic ring.

[0040] In one aspect, the photosensitive resin composition may further contain (F) a silane coupling agent.

[0041] In one aspect, the photosensitive resin composition may further contain (G) a resin having a urethane bond.

[0042] Another embodiment of the present invention relates to a dry film having a photosensitive resin layer obtained by coating and drying the above-described photosensitive resin composition on a first film.

[0043] Another embodiment of the present invention relates to a cured product obtained by curing the photosensitive resin layer of the photosensitive resin composition or a dry film obtained thereby.

[0044] Another embodiment of the present invention relates to a printed wiring substrate containing the above-described cured material as a solder resist.

[0045] On one side, the printed circuit board may further include a silicon encapsulant layer disposed on the solder resist.

[0046] In one aspect, the silicon encapsulant layer includes an upper encapsulant region and a lower encapsulant region, and the content of (E) photopolymerization initiator contained in at least one of the upper encapsulant region or the lower encapsulant region may be 1,000 ppm or less relative to the content of (E) photopolymerization initiator contained in the solder resist.

[0047] Yet another embodiment of the present invention relates to a laminate comprising the cured product described above and a protective film.

[0048] On one side, the content of the (E) photopolymerization initiator contained in the protective film may be 1,000 ppm or less relative to the content of the (E) photopolymerization initiator contained in the solder resist. [Effects of the invention]

[0049] A photosensitive resin composition according to one embodiment of the present invention significantly reduces outgassing of the photopolymerization initiator, thereby improving the problems of yellowing and incurability of the silicone encapsulant and improving the reaction rate of the silicone encapsulant. Furthermore, it can reduce the amount of outgassing of the photopolymerization initiator transferred to the protective film, making it possible to omit the firing process after the reflow process, and improving the problem of power consumption by increasing reflectivity. In addition, it exhibits high HAST resistance and reflectivity after HAST testing, and the decrease in reflectivity under high temperature / high humidity conditions can be suppressed. Due to these characteristics, the solder resist produced by the photosensitive resin composition of the present invention can exhibit excellent effects.

[0050] For example, a photosensitive resin composition according to one aspect of the present invention further contains titanium oxide as an inorganic filler, and can obtain an excellent reflectivity maintenance effect.

[0051] Furthermore, the present invention can provide a dry film, a cured product, and a printed circuit board using the photosensitive resin composition. [Brief explanation of the drawing]

[0052] Figures 1A and 1B are images showing the BHAST test results of dry films using the photosensitive resin compositions of Comparative Example 1 and Example 3, respectively. Embodiments for the Invention

[0053] Various embodiments of the present invention will be described below.

[0054] [Photosensitive resin composition]

[0055] One embodiment of the present invention relates to a photosensitive resin composition comprising (A) a carboxyl group-containing resin that does not contain an aromatic ring, (B) an inorganic filler, and (E) one or more photopolymerization initiators selected from trimethylbenzoylphosphine oxide group-containing compounds containing one or more PO bonds.

[0056] Another embodiment of the present invention relates to a photosensitive resin composition comprising (A) a carboxyl group-containing resin that does not contain an aromatic ring, (C) a mercapto-modified (meth)acrylate, and (E) a photopolymerization initiator which is a trimethylbenzoylphosphine oxide group-containing compound containing one or more PO bonds.

[0057] The aforementioned photosensitive resin composition can suppress outgassing and exhibit excellent silicone encapsulant reaction rate, reflectivity, and HAST resistance.

[0058] For example, the photosensitive resin composition may be a composition for curing to form a solder resist.

[0059] The following describes in detail each component of the photosensitive resin composition.

[0060] [(A) Carboxyl group-containing resin that does not contain aromatic rings]

[0061] The present invention relates to a photosensitive resin composition, wherein (A) a carboxyl group-containing resin that does not contain an aromatic ring (hereinafter referred to as "resin (A)") may be a resin that hardens upon irradiation with active energy rays and exhibits electrical insulation properties. For example, the aromatic ring can be a benzene ring, a pyridine ring, a pyrimidine ring, a triazine ring, and the like.

[0062] Resin (A) is alkali-developable due to the presence of carboxyl groups and, because it does not contain aromatic rings, exhibits excellent resistance to discoloration and yellowing when exposed to heat and UV energy. Furthermore, high reflectivity can be achieved through combination with the inorganic filler (B) described later, with minimal decrease in reflectivity after the reflow process and after a 3000-hour blue light test. Therefore, compositions containing resin (A) exhibit less reduction in reflectivity due to discoloration and yellowing compared to other white ink compositions, and have superior yellowing resistance. For example, carboxyl group-containing resins containing aromatic rings have a relatively lower initial reflectivity of the cured product compared to resin (A) that does not contain aromatic rings, and the decrease in reflectivity can be very large when subjected to heat, UV, BHAST, and 85°C / 85% tests. This is because the aromatic rings deform due to heat, UV, BHAST, and 85°C / 85% tests, significantly affecting the decrease in reflectivity.

[0063] For example, resin (A) may contain unsaturated double bonds. By containing unsaturated double bonds, resin (A) can be radical-cured by ultraviolet light, electron beams, or heat.

[0064] The resin (A) is not particularly limited as long as it does not contain an aromatic ring and contains a carboxyl group, but may be, for example, a photosensitive carboxyl group-containing resin having one or more photosensitive unsaturated double bonds of its own, or a carboxyl group-containing resin that does not have a photosensitive unsaturated double bond.

[0065] For example, as resin (A), any resin that does not have an aromatic ring (either oligomer or polymer) can be used as appropriate from the list below:

[0066] (1) Carboxyl group-containing resin obtained by copolymerization of unsaturated carboxylic acid and compounds having unsaturated double bonds,

[0067] (2) A photosensitive carboxyl group-containing resin obtained by reacting a carboxyl group-containing (meth)acrylic copolymer resin with a compound having an oxirane ring and an ethylenically unsaturated group in one molecule.

[0068] (3) A photosensitive carboxyl group-containing resin obtained by reacting a copolymer of a compound having one epoxy group and one unsaturated double bond in each molecule with an unsaturated monocarboxylic acid, and then reacting the resulting secondary hydroxyl group-saturated or unsaturated polybasic acid anhydride.

[0069] (4) A resin containing photosensitive hydroxyl groups and carboxyl groups, obtained by reacting a hydroxyl group-containing polymer with a saturated or unsaturated polybasic acid anhydride, and then reacting each molecule of the carboxylic acid produced by this reaction with a compound having one epoxy group and one unsaturated double bond.

[0070] For example, resin (A) may be a carboxyl group copolymer resin obtained by the reaction of (a) a carboxyl group-containing (meth)acrylic copolymer resin and (b) a compound having a carboxyl group obtained by the reaction of a compound having an oxirane ring and an ethylenically unsaturated group in one molecule.

[0071] For example, (a) a carboxyl group-containing (meth)acrylic copolymer resin can be obtained by copolymerizing a (meth)acrylic acid ester with a compound having one unsaturated group and at least one carboxyl group in one molecule, but is not limited to this. Examples of (meth)acrylic acid esters constituting the copolymer resin (a) include alkyl (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, and hexyl (meth)acrylate; hydroxyl group-containing (meth)acrylic acid esters such as 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and caprolactone-modified 2-hydroxyethyl (meth)acrylate; and glycol-modified (meth)acrylates such as methoxydiethylene glycol (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, isooctyloxyethylene glycol (meth)acrylate, phenoxytriethylene glycol (meth)acrylate, methoxytriethylene glycol (meth)acrylate, and methoxypolyethylene glycol (meth)acrylate. These may be used individually or in combination of two or more. Furthermore, in this specification, (meth)acrylate is a general term encompassing acrylate and methacrylate, and the same applies to other similar expressions.

[0072] Furthermore, examples of compounds having one unsaturated group and at least one carboxyl group in one molecule include acrylic acid, methacrylic acid, modified unsaturated monocarboxylic acids in which the chain between the unsaturated group and the carboxylic acid is extended, such as β-carboxyethyl (meth)acrylate, 2-acryloyloxyethyl succinic acid, 2-acryloyloxyethyl hexahydrophthalic acid, unsaturated monocarboxylic acids having an ester bond due to lactone modification, modified unsaturated monocarboxylic acids having an ether bond, and compounds containing two or more carboxyl groups in the molecule, such as maleic acid. These may be used individually or in combination of two or more.

[0073] (b) The compound having an oxirane ring and an ethylenically unsaturated group in one molecule can be any compound having an oxirane ring and an ethylenically unsaturated group in one molecule, for example, glycidyl (meth)acrylate, α-methylglycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, 3,4-epoxycyclohexylethyl (meth)acrylate, 3,4-epoxycyclohexylbutyl (meth)acrylate, 3,4-epoxycyclohexylmethylaminoacrylate, etc. These may be used individually or in combination of two or more. For example, (b) the compound having an oxirane ring and an ethylenically unsaturated group in one molecule may be 3,4-epoxycyclohexylmethyl (meth)acrylate.

[0074] For example, resin (A) may have an acid value of 30 to 200 mg KOH / g. If the acid value of resin (A) is 30 mg KOH / g or higher, unexposed portions of the solder resist composition coating can be easily removed with a weakly alkaline aqueous solution. If the acid value of resin (A) is 200 mg KOH / g or lower, the water resistance and electrical properties of the cured film can be improved.

[0075] For example, the weight-average molecular weight of resin (A) may be 5,000 to 100,000 g / mol. If the weight-average molecular weight of resin (A) is 5,000 g / mol or more, the decrease in the touch-drying properties of the solder resist composition coating can be suppressed. If the weight-average molecular weight of resin (A) is 100,000 g / mol or less, the decrease in the developability and storage stability of the solder resist composition can be suppressed.

[0076] In the photosensitive resin composition of the present invention, the content of resin (A) may be 5 to 40% by weight, 10 to 35% by weight, or 12 to 33% by weight of the whole composition. The composition contains solids and a solvent. The content of resin (A) may be calculated on a solids basis.

[0077] If the content of resin (A) is within the above range, it is possible to achieve excellent yellowing resistance, high reflectivity, good formation of solder resist coating film, excellent pencil hardness and adhesion, and suppression of the decrease in touch-dryness and undercut of the coating film.

[0078] [(B) Inorganic fillers]

[0079] A photosensitive resin composition according to one embodiment of the present invention can obtain high reflectivity by including an inorganic filler.

[0080] Examples of inorganic fillers include titanium oxide, zinc oxide, basic carbonates, basic sulfates, sulfates, zinc sulfide, antimony oxide, aluminum hydroxide, silica, and barium sulfate. For example, when a composition is created using a mixture of barium sulfate and silica as inorganic fillers, the L value is 80 or higher, the a value is -5 or higher, and the b value is -5 or higher. The L value may be measured by Hunter 1948. For example, when a composition is created using high-content titanium oxide and silica as inorganic fillers, the L value of the cured composition is 90 or higher, the a value is -3 or higher, and the b value is -3 or higher, resulting in high whiteness and reflectance. For example, when a composition is created using one or more of titanium oxide or silica as inorganic fillers, the L value is 95 or higher, the a value is -2 or higher, and the b value is -1 or higher, resulting in the highest possible whiteness and reflectance.

[0081] For example, the method for producing titanium oxide may be either the sulfuric acid method or the chlorine method, for example, the chlorine method. For example, sulfuric acid does not need to be used in the manufacturing process. Also, the surface treatment of titanium oxide is not particularly limited, but titanium oxide may be treated with an acid other than sulfuric acid, such as hydrochloric acid, nitric acid, phosphoric acid, or acetic acid, during neutralization.

[0082] The titanium oxide can be any structure of rutile, anatase, or ramsdellite titanium oxide, and may be used alone or in combination of two or more types. Of these, ramsdellite titanium oxide is ramsdellite Li 0.5 It can be obtained by subjecting TiO2 to a chemical lithium oxide removal treatment.

[0083] In particular, using rutile-type titanium oxide can further improve heat resistance, making it less susceptible to discoloration due to light irradiation and preventing quality degradation even in harsh operating environments. Specifically, using rutile-type titanium oxide surface-treated with aluminum oxide such as alumina can improve heat resistance. The content of rutile-type titanium oxide surface-treated with aluminum oxide in the total titanium oxide is, for example, 35% by mass or more, for example, 55% by mass or more, with an upper limit of 100% by mass or less; that is, the entire amount of titanium oxide may be rutile-type titanium oxide surface-treated with the aforementioned aluminum oxide. Furthermore, since anatase-type titanium oxide has lower hardness than rutile-type titanium oxide, using anatase-type titanium oxide is more advantageous in terms of the moldability of the composition.

[0084] In the photosensitive resin composition of the present invention, the amount of (B) inorganic filler may be in the range of 30 to 70% by mass of the entire resin composition, for example, in the range of 40 to 70% by mass, or for example, in the range of 45 to 70% by mass. The content of (B) inorganic filler may be calculated on a solid content basis. If the content of (B) inorganic filler is within the above range, it is advantageous for high reflectivity; if it is less than the above range, the reflectivity decreases; and if it exceeds the above range, cracks may occur.

[0085] (B) Among the inorganic fillers, titanium oxide may have a sulfur concentration of 100 ppm or less, or 50 ppm or less. Alternatively, commercially available titanium oxide with a sulfur concentration of 100 ppm or less may be used, or commercially available titanium oxide with a sulfur concentration of 100 ppm or more may be mixed after reducing the sulfur concentration by heat treatment, chemical treatment, or purification treatment such as washing or calcination. Here, the sulfur contained in the titanium oxide refers to all sulfur detected by analysis, including sulfur adsorbed on the titanium oxide and sulfur coated on the titanium oxide as an impurity. Furthermore, the sodium concentration of the titanium oxide may be 100 ppm or less, or 50 ppm or less. The lower the sodium concentration, the better. If the sodium concentration is too high, corrosion and oxidation of the copper substrate may be accelerated when exposed to moisture due to sodium ions. For this reason, the sodium ion concentration may be 100 ppm or less.

[0086] Furthermore, the photosensitive resin composition of the present invention may contain titanium oxide with a sulfur concentration of 100 ppm or more, to the extent that it does not impair the effects of the present invention. Examples of titanium oxide with a sulfur concentration of 100 ppm or more include CR-58, CR-90, and R-630 from Ishihara Sangyo Co., Ltd., and R-21 from Sakai-chem Co., Ltd.

[0087] Additionally, rutile-type chlorinated titanium oxides such as T-550, T-580, R-630, R-820, CR-50, CR-60, R-90, and CR-97 from Ishihara Industries Co., Ltd., as well as DuPont's Ti PURE R-706, R-902+, and R931, Fuji Titanium Industries Co., Ltd.'s TR-600, TR-700, and TR-840, and Titanium Industries Co., Ltd.'s KR-270, KR-310, and KR-380 can be used.

[0088] If the particle size of titanium oxide is too small, its fluidity will be poor, and conversely, if it is too large, its insertion into small-diameter substrates may be poor. Therefore, the median particle size of titanium oxide is in the range of 0.1 to 5 μm, for example, 0.1 to 1 μm, for example, 0.1 to 0.5 μm, and may be 0.36 μm. If the particle size of titanium oxide is within this range, high reflectivity can be achieved. The above particle size was measured using a laser diffraction method.

[0089] (B) Among inorganic fillers, barium sulfate can be found in the following forms: precipitated barium sulfate #100, precipitated barium sulfate #300, precipitated barium sulfate SS-50, BARIACE B-30, BARIACE B-31, BARIACE B-32, BARIACE B-33, BARIACE B-34, BARIFINE BF-1, BARIFINE BF-10, BARIFINE BF-20, BARIFINE BF-40 (manufactured by Sakai Chemical Industry Co., Ltd.), W-1, W-6, W-10, C300 (manufactured by Takehara Chemical Industry Co., Ltd.).

[0090] (B) Among the inorganic fillers, silica particles are not particularly limited and may be obtained by methods known to ordinary technicians. For example, they can be produced by burning silicon powder using the VMC (Vap-erized Metal Combustion) method. The VMC method is a method in which a chemical flame is formed by a burner in an oxygen-containing atmosphere, and a metal powder that constitutes part of the target oxide particles is introduced into this chemical flame in an amount that forms a dust cloud, causing knocking to occur in order to obtain oxide particles. Examples of commercially available silica include the SO series from Admatex Corporation and the HPS series from Towa Synthetic Co., Ltd. (HPS-0500, HPS-1000, HPS3500, etc.).

[0091] [(C) Mercapto-modified (meth)acrylate]

[0092] A photosensitive resin composition according to one embodiment of the present invention may have enhanced surface hardening, improved gloss, and enable the realization of high reflectivity by using (C) mercapto-modified (meth)acrylate.

[0093] Furthermore, if (C) mercapto-modified (meth)acrylate of the present invention is used together with the above-mentioned (B) inorganic filler in a photosensitive resin composition, the surface hardening of the photosensitive resin layer is improved, and this improvement in surface hardening may enable the realization of higher reflectivity and higher gloss.

[0094] The (C) mercapto-modified (meth)acrylate of the present invention is a compound modified by introducing a mercapto group into an acrylate compound, and the acrylate compound may be a single or polyfunctional acrylate compound, and may be an aliphatic compound having 1 to 15 carbon atoms substituted with one or more functional groups selected from the group consisting of acryloyl groups, acryloyloxy groups, and acryloyloxyalkyl groups, for example, pentane triacrylate.

[0095] The (C) mercapto-modified (meth)acrylate of the present invention may be curable or active energy ray curable, and the (C) mercapto-modified (meth)acrylate of the present invention is a mercapto-modified (meth)acrylate that can be obtained by Michael addition reaction of a polyfunctional thiol compound and a stoichiometrically excessive amount of two or more polyfunctional (meth)acrylate compounds. Examples of polyfunctional thiol compounds include polyisocyanates such as pentaerythritol tetrakis(3-mercaptopropionate) (molecular weight 489 g / mol), trimethylolpropantris(3-mercaptopropionate) (molecular weight 399 g / mol), and 1,3-bis(2-isocyanato-2-propyl)benzenetetrathiol (thiol) and polyfunctional thiol compounds such as trimethylolpropantris(3-mercaptopropionate), as well as polyisocyanates such as isophorone diisocyanate and polyfunctional thiol compounds such as trimethylolpropantris(3-mercaptopropionate). Examples of polyfunctional thiol compounds resulting from the reaction of polyisocyanates such as hexamethylene diisocyanate with polyfunctional thiol compounds such as trimethylolpropanetris (3-mercaptopropionate) include 1,6-hexanedithiol (molecular weight 150 g / mol), ethylene glycol di-2-mercaptoacetate (molecular weight 210 g / mol), pentaerythritol tetrakis (2-mercaptoacetate) (molecular weight 433 g / mol), trimethylolpropanetris (2-mercaptoacetate), and ethylene glycol bis(3-mercaptopropionate) (molecular weight 238 g / mol). For example, the (C) mercapto-modified (meth)acrylate may contain two or more mercapto groups, or three or more mercapto groups.

[0096] The (C) mercapto-modified (meth)acrylate may have a weight-average molecular weight of 5,000 g / mol or less, 3,000 g / mol or less, or 2,000 g / mol or less. If the weight-average molecular weight is 5,000 g / mol or less, the mobility of the mercapto-modified (meth)acrylate molecules decreases, which can suppress the decrease in reactivity of the active energy ray curable coating film formation of the present invention. For example, if the reactivity decreases, when the coating film is cured with a UV-LED, the tackiness of the cured coating film surface increases, which increases the possibility of problems such as the printed material sticking to the printed material when it is placed on top.

[0097] In the photosensitive resin composition of the present invention, the content of (C) mercapto-modified (meth)acrylate may be 1 to 20 parts by weight, 1 to 10 parts by weight, or 1 to 7 parts by weight per 100 parts by weight of the entire composition.

[0098] (C) If the content of mercapto-modified (meth)acrylate is within the above range, surface hardening is enhanced, gloss is improved, high reflectivity is possible, reflectivity decreases little even after the manufacturing process, and excellent crack resistance can be obtained. In addition, gloss reduction due to decreased surface hardening is suppressed, high reflectivity can be achieved, the surface is properly hardened to reduce cracking of the coating film, and resolution can be improved.

[0099] [(D) Resins containing aromatic rings]

[0100] The photosensitive resin composition of the present invention includes (A) a carboxyl group-containing resin (A) that does not contain an aromatic ring, but in addition to the resin (A), it may further include (D) a resin containing an aromatic ring.

[0101] (D) The resin containing the aromatic ring can exhibit excellent yellowing resistance when combined with resin (A). A photosensitive resin composition according to one embodiment of the present invention can exhibit excellent yellowing resistance by containing resin (D) containing the aromatic ring in a smaller amount than resin (A).

[0102] The resin containing the aromatic ring (D) of the present invention may be, for example, a resin that hardens upon heating and exhibits electrical insulation properties.

[0103] The aromatic ring may be a benzene ring, a pyridine ring, a pyrimidine ring, a triazine ring, etc., and as the resin containing the (D) aromatic ring of the present invention, for example, a melamine resin, a silicone resin, a resin having a styrene skeleton, etc., for example, a resin having a styrene skeleton can be used.

[0104] Furthermore, the resin containing the aromatic ring (D) may contain carboxyl groups, and may, for example, be a carboxyl group-containing resin having a styrene skeleton. For example, the resin containing the aromatic ring (D) may be a mixture of a carboxyl group-containing resin having a styrene skeleton and a carboxyl group-containing resin other than a carboxyl group-containing resin having a styrene skeleton.

[0105] For example, if the resin containing (D) an aromatic ring is a carboxyl group-containing resin having a styrene skeleton, it may not have photosensitive groups such as ethylenically unsaturated bonds with carboxyl groups in the molecule, have a styrene skeleton in the molecule, have an average molecular weight of 10,000 to 50,000 g / mol, and have an acid value of 80 to 200 mg KOH / g. Such a carboxyl group-containing resin having a styrene skeleton can be synthesized by copolymerization with styrene as the essential monomer. By using a carboxyl group-containing resin having the above-mentioned physical properties, it is possible to obtain a cured film with excellent touch-drying properties and a flow-preventing effect.

[0106] Examples of carboxyl group-containing resins having a styrene skeleton include carboxyl group-containing resins (both oligomers and polymers are possible) obtained by copolymerizing an unsaturated carboxylic acid such as (meth)acrylic acid with a compound containing an unsaturated group that can be selected from styrene, α-methylstyrene, lower alkyl (meth)acrylate, isobutylene, etc. Here, lower alkyl can mean an alkyl group having 1 to 5 carbon atoms.

[0107] In the photosensitive resin composition of the present invention, the average molecular weight per unit weight of the carboxyl group-containing resin having a styrene skeleton varies depending on the resin skeleton, but may be 10,000 g / mol to 50,000 g / mol, 10,000 g / mol to 25,000 g / mol, 10,000 g / mol to 20,000 g / mol, or 10,000 g / mol to 17,000 g / mol. By setting the weight-average molecular weight to 10,000 g / mol or more, not only is the effect of preventing flow improved, but the touch-drying properties (tackiness) are further improved, the moisture resistance of the exposed coating film is enhanced, and film reduction during development is suppressed, thus suppressing a decrease in resolution. Furthermore, by setting the weight-average molecular weight to 50,000 g / mol or less, not only is the effect of preventing flow improved, but developability is also improved, and storage stability may also be enhanced.

[0108] In the photosensitive resin composition of the present invention, the acid value of the carboxyl group-containing resin having a styrene skeleton may be 80 to 200 mg KOH / g, or 100 to 180 mg KOH / g. By setting the acid value of the carboxyl group-containing resin having a styrene skeleton to 80 mg KOH / g or higher, the softening point is increased, thereby improving tackiness and developability. On the other hand, by setting the acid value of the carboxyl group-containing resin having a styrene skeleton to 200 mg KOH / g or lower, stress is not generated during curing due to an appropriate crosslinking density, and a good coating film can be obtained.

[0109] In the photosensitive resin composition of the present invention, the carboxyl group-containing resin having a styrene skeleton, despite having aromatic rings, suppresses the decrease in reflectivity and discoloration of the cured product due to light irradiation and heat, and exhibits excellent developability and touch-dryness. The ratio of the styrene skeleton may be 10 to 80 mol%, 10 to 60 mol%, or 10 to 50 mol% in the molecule. That is, when synthesizing the carboxyl group-containing resin having a styrene skeleton, 30 to 60 mol% of styrene can be used relative to the total amount of monomer. If the ratio of the styrene skeleton in the carboxyl group-containing resin having a styrene skeleton is 10 mol% or more in the molecule, compatibility with other components is good, and if it is 80 mol% or less in the molecule, developability may be good.

[0110] Carboxyl group-containing resins with a styrene skeleton can be produced by suspension polymerization to achieve high molecular weight. As a result, photosensitive resin compositions using such resins may exhibit excellent tackiness. Generally, producing carboxyl group-containing resins with a styrene skeleton by suspension polymerization results in high molecular weight resins, but considering properties such as screen printing suitability, tackiness, and developability, the weight-average molecular weight may be limited to the range of 10,000 to 50,000 g / mol. Therefore, in controlling the molecular weight, chain transfer agents can be used during the synthesis of carboxyl group-containing resins with a styrene skeleton.

[0111] Furthermore, a polymerization initiator can be used during the synthesis of a carboxyl group-containing resin having a styrene skeleton to promote polymerization. Examples of polymerization initiators include BPO (benzoyl peroxide), t-butylperoxy-2-ethylhexanoate, and AMBN (2,2'-azobis(2-methylbutyronitrile)), and for example, BPO (benzoyl peroxide) may be used. The amount of polymerization initiator added may be 0.1 to 10% by weight or 0.1 to 6% by weight in terms of solid content, based on 100% by weight of the carboxyl group-containing resin having a styrene skeleton.

[0112] In the photosensitive resin composition of the present invention, the content of the resin containing (D) an aromatic ring may be 0.1 to 15% by weight, 1 to 10% by weight, or 2 to 6% by weight based on the total weight of the composition. The photosensitive resin composition contains solids and a solvent.

[0113] (D) If the content of the resin containing aromatic rings is within the above range, the decrease in reflectivity and discoloration will be suppressed, the developability and touch-dryness will be excellent, and the effect of improving reflectivity and preventing yellowing will be improved.

[0114] [(E) Photopolymerization initiator]

[0115] A photosensitive resin composition according to one embodiment of the present invention may contain (E) a photopolymerization initiator (hereinafter referred to as "photopolymerization initiator (E)") which is a trimethylbenzoylphosphine oxide group-containing compound having one or more PO bonds.

[0116] Conventional photopolymerization initiators, such as 2,4,6-trimethylbenzoyldiphenylphosphine oxide (TPO), which are widely used, generate a large amount of outgassing during the curing process. This outgassing diffuses into the silicone encapsulant layer and protective film, causing yellowing of the silicone encapsulant, reduced reflectivity, and difficulty in curing the silicone encapsulant. This posed problems with the long-term reliability of the product.

[0117] As a photopolymerization initiator, the trimethylbenzoylphosphine oxide group-containing polymer has a high molecular weight structure, resulting in minimal outgassing due to heat during the final curing stage, reflow process, and firing process.

[0118] On the other hand, even with trimethylbenzoylphosphine oxide group-containing compounds that have a lower molecular weight compared to TPO, it can be inferred that the presence of one or more PO bonds significantly suppresses outgassing of the photopolymerization initiator by improving intermolecular bonding strength (for example, stronger hydrogen bonding with OH groups or COOH groups remaining unreacted in the composition).

[0119] For example, the trimethylbenzoylphosphine oxide group-containing compound may contain three or more hydrogen bonding sites. This improves intermolecular bonding strength and significantly suppresses outgassing of the photopolymerization initiator.

[0120] This improves the problems of yellowing and incomplete curing of the silicone encapsulant, reduces the amount of outgassing from the photopolymerization initiator transferred to the protective film, and can significantly increase the reaction rate of the silicone encapsulant.

[0121] Furthermore, in existing methods, when using photopolymerization initiators such as TPO, an additional curing process (for example, curing at 150°C for 6 hours) was sometimes added after the reflow process to efficiently remove outgassing. However, this curing process significantly reduced reflectivity, leading to increased power consumption when the chip was mounted.

[0122] However, by using the photopolymerization initiator (E) of the present invention as described above, the firing process can be omitted, yield can be increased due to reduced working time, costs can be reduced, reflectivity can be increased, power consumption due to reduced reflectivity can be prevented, the outgassing content of the photopolymerization initiator is very low even without using a protective film for removal of the photopolymerization initiator, the degree of curing of the silicon is greatly increased, long-term reliability is improved, and excellent HAST resistance and reflectivity after HAST testing can be observed. In addition, the decrease in reflectivity under high temperature / high humidity conditions can be suppressed.

[0123] The photopolymerization initiator (E) may be a liquid at room temperature (20°C) and 1 atmosphere.

[0124] The photopolymerization initiator (E) may contain a PO bond.

[0125] The photopolymerization initiator (E) may contain *-C(=O)-P(=O)R1-O-*'moiety (where R1 is an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, or a cyclic group having 5 to 20 carbon atoms).

[0126] When the photopolymerization initiator (E) is a polymer containing a trimethylbenzoylphosphine oxide group, the weight-average molecular weight (M) of the trimethylbenzoylphosphine oxide group-containing polymer is n The weight-average molecular weight (M) may be approximately 1,000 g / mol or more. For example, the trimethylbenzoylphosphine oxide group-containing polymer has a weight-average molecular weight (M n The concentration can be between 1,000 g / mol and 100,000 g / mol.

[0127] The aforementioned trimethylbenzoylphosphine oxide group-containing polymer may be represented by the following chemical formula 1.

[0128] [ka] a = 0 to 100, b = 0 to 100, c = 0 to 100

[0129] When the photopolymerization initiator (E) is a trimethylbenzoylphosphine oxide group-containing compound that includes a PO bond, the trimethylbenzoylphosphine oxide group-containing compound that includes a PO bond may also contain an alkoxy group.

[0130] For example, in the above chemical formula 1, a+b+c>0 may be the case.

[0131] For example, the trimethylbenzoylphosphine oxide group-containing compound having the aforementioned PO bond may also contain an ethoxy group.

[0132] The trimethylbenzoylphosphine oxide group-containing compound having the aforementioned PO bond may be represented by the following chemical formula 2.

[0133] [ka]

[0134] For example, the photopolymerization initiator (E) may further include one or more selected from the group consisting of benzoin and its alkyl ethers, acetophenones, anthraquinones, thioxanthones, ketals, benzophenones, α-aminoacetophenones, acylphosphine oxides, acylphosphineates, and oxime esters.

[0135] In the photosensitive resin composition of the present invention, the content of the photopolymerization initiator (E) may be 0.01 to 10% by weight, 0.01 to 7% by weight, or 0.01 to 5% by weight relative to the total composition. By including the photopolymerization initiator (E) within this range, sufficient photocurability on copper is achieved, the curability of the coating film is improved, coating film properties such as chemical resistance are enhanced, and deep curing properties may also be improved.

[0136] Furthermore, if the content of the photopolymerization initiator (E) is within the aforementioned range, severe undercutting and halation (the phenomenon of the upper part becoming larger) are not significant, resulting in excellent resolution and the formation of numerous solder resist openings. In addition, high reflectivity can be maintained.

[0137] [(F) Silane coupling agent]

[0138] A photosensitive resin composition according to one embodiment of the present invention may further contain a (F) silane coupling agent. By containing a (F) silane coupling agent, the photosensitive resin composition can exhibit improved crack resistance, improved reflectivity compared to existing compositions, and superior gloss.

[0139] The (F) silane coupling agent of the present invention may have an organic group such as a vinyl group, styryl group, acrylic group, methacrylic group, isocyanurate group, acid anhydride group, ureido group, epoxy group, amino group, methacrylicoxy group, mercapto group, or isocyanate group.

[0140] Examples of silane coupling agents having a vinyl group include vinyltrimethoxysilane and vinyltriethoxysilane. Examples of silane coupling agents having a styryl group include p-styrylmethoxysilane. Examples of silane coupling agents having a methacrylic group include 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyldiethoxysilane, and 3-methacryloxypropyltriethoxysilane. Examples of silane coupling agents having an acrylic group include 3-acryloxypropyltrimethoxysilane. Silane coupling agents having an amino group include N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, and N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane. Silane coupling agents having a methacryloxy group include 3-methacryloxypropyltrimethoxysilane and 3-methacryloxypropyltriethoxysilane. Silane coupling agents having a mercapto group include 3-mercaptopropylmethyldimethoxysilane and 3-mercaptopropyltrimethoxysilane. Silane coupling agents having an isocyanate group include 3-isocyanatetopropyltriethoxysilane. Silane coupling agents having an isocyanurate group include tris-(trimethoxysilylpropyl)isocyanurate. Silane coupling agents having a ureido group include 3-ureidopropyltrialkoxysilane. Silane coupling agents having an acid anhydride group include 3-(trimethoxysilyl)propyl succinic anhydride.

[0141] The silane coupling agent may be a silane coupling agent having an epoxy group, for example, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane, for example, 3-glycidoxypropyltriethoxysilane.

[0142] In the photosensitive resin composition of the present invention, the content of (F) silane coupling agent may be 0.1 to 5% by weight, 0.3 to 3% by weight, or 0.4 to 2% by weight based on the total composition. The composition contains solids and a solvent.

[0143] (F) If the content of the silane coupling agent is within the above range, the composition has excellent crack resistance, high reflectivity, excellent adhesion, and low tackiness, making it suitable for film formation.

[0144] (F) The silane coupling agent may be a commercially available product, for example, KBM-1003, KBE-1003, KBM-303, KBM-402, KBM-403, KBE-402, KBE-403, KBM-1403, KBM-502, KBM-503, KBE-502, KBE-503, KBM5103, KBM-602, KBM-603, KBM-903, KBE-903, KBE-9103P, KBM-573, KBM-575, KBM-9659, KBM-585A, KBM-802, KBM-803, KBE-9007N, and X-12-967C, all manufactured by Shin-Etsu Chemical Co., Ltd.

[0145] [(G) Resin having urethane bonding]

[0146] A photosensitive resin composition according to one embodiment of the present invention may further contain (G) a resin having a urethane bond. The (G) resin having a urethane bond may be a resin with excellent flexibility.

[0147] The photosensitive resin composition, by using a resin having (G) urethane bonds, can be used without tearing even on flexible substrates or thin sheets, enabling lamination work of uniform thickness, and may have excellent crack and tear resistance against external impacts and bending.

[0148] The (G) resin having a urethane bond of the present invention may include a modified urethane resin, and the resin having a urethane bond may be an ester-type urethane system, an ether-type urethane system, a modified urethane acrylate system, a modified urethane epoxy, a silicone-modified urethane, a fluorine-based modified urethane, etc., and may be, for example, a modified urethane epoxy acrylate containing an epoxy group.

[0149] As the resin having a urethane bond in the present invention, known compounds having a urethane bond can be used. For example, reaction products of isocyanate compounds (e.g., monoisocyanate, diisocyanate, polyisocyanate) and compounds having an OH group (e.g., monohydric alcohols, polyhydric alcohols such as polyester polyols and polyether polyols, epoxy (meth)acrylates), or modified products thereof can be used.

[0150] In the present invention, the resin having (G) a urethane bond may have a carboxyl group or an epoxy group, or a (meth)acryloyl group, for example, the carboxyl group-containing resin (1), epoxy group-containing resin (2), (meth)acryloyl group-containing resin (3), (4), (5) below.

[0151] (1) A reaction product of diisocyanate and a monocarboxylate compound having an ethylene-based unsaturated double bond, such as a bifunctional epoxy resin (meth)acrylate, bixylenol epoxy resin, phenol-type epoxy resin, etc., a partial anhydride thereof, or a modified product thereof, and a carboxyl group-containing photosensitive polyurethane resin obtained by polyaddition reaction of a carboxyl group-containing dialcohol compound and a diol compound.

[0152] (2) A urethane-modified epoxy resin having a urethane bond and two or more epoxy groups in its molecule, obtained by reacting a urethane bond-containing compound having an isocyanate group, obtained by reacting a polyhydroxy compound and a polyisocyanate compound, with a hydroxyl group-containing epoxy compound.

[0153] (3) Urethane resins obtained by polyaddition reactions of diol compounds such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, aromatic diisocyanates, etc., with polycarbonate-based polyols, polyether-based polyols, polyester-based polyols, polyolefin polyols, acrylic polyols, epoxy resins having hydroxyl groups (when used, urethane resins having epoxy groups are obtained), bisphenol A-based alkylene oxide adduct diols, compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups.

[0154] (4) A photosensitive polyurethane resin obtained by polyaddition reaction of such isocyanate and the diol compound, wherein some or all of the diisocyanate in (3) above is replaced with a reaction product of isophorone diisocyanate and pentaerythritol triacrylate, and / or a compound having one isocyanate group and one or more (meth)acryloyl groups in the molecule.

[0155] (5) A terminally (meth)acrylic photosensitive polyurethane resin obtained by adding a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule, such as a hydroxyalkyl (meth)acrylate, during the synthesis of any one of the resins described in (3) or (4).

[0156] Furthermore, as described above, a single resin may have at least two of the following: carboxyl groups, epoxy groups, or methacryloyl groups.

[0157] The resin having the urethane bond (G) may be (1) from among the carboxyl group-containing resins, (2) from among the epoxy group-containing resins, or (5) from among the (meth)acryloyl group-containing resins.

[0158] The diisocyanate may be, for example, an aromatic polyisocyanate, an aliphatic polyisocyanate, or an alicyclic polyisocyanate. Examples of aromatic polyisocyanates include 4,4'-diphenylmethane diisocyanate, 2,4-diisocyanate-2,6-tolylene diisocyanate, naphthalene-1,5-diisocyanate-o-xylylene diisocyanate, m-xylylene diisocyanate, and 2,4-tolylene dimer. Examples of aliphatic polyisocyanates include tetramethylene diisocyanate, hexamethylene diisocyanate, methylene diisocyanate, trimethylhexamethylene diisocyanate, 4,4-methylenebis(cyclohexyl isocyanate), and isophorone diisocyanate. Examples of alicyclic polyisocyanates include bicycloheptane triisocyanate. For example, diisocyanates may be aliphatic isocyanates.

[0159] (G) When the resin having urethane bonds is a carboxyl group-containing resin having urethane bonds, the acid value of the carboxyl group-containing resin may be 40 to 200 mg KOH / g, or 45 to 120 mg KOH / g. If the acid value of the carboxyl group-containing resin is in the range of 40 to 200 mg KOH / g, adhesion of the cured film is obtained and alkaline development is facilitated, so dissolution of the exposed area by the developer is suppressed, the lines do not become unnecessarily narrowed, and a normal resist pattern can be easily drawn.

[0160] (G) When the resin having urethane bonds is a carboxyl group-containing resin having urethane bonds, the weight-average molecular weight of the carboxyl group-containing resin may vary depending on the resin skeleton, but may be 2,000 to 150,000 g / mol, 5,000 to 50,000 g / mol, or 2,000 to 50,000 g / mol. If the weight-average molecular weight is within the above range, the tackiness is good, the moisture resistance of the cured film is good, and the occurrence of film reduction during development can be reduced. In addition, if the weight-average molecular weight is within the above range, the resolution and developability are good, and the storage stability is improved.

[0161] (G) Examples of commercially available resins having urethane bonds (for example, carboxyl group-containing resins having urethane bonds) include UXE-3000 (Nippon Kayaku Co., Ltd.), EPU-7N (urethane-modified epoxy resin; ADEKA Corporation), and Ebecryl 210 (aromatic urethane acrylate; Daicel Ornex Co., Ltd.).

[0162] In the photosensitive resin composition of the present invention, the content of (G) the resin having urethane bonds may be 0.1 to 15% by weight, 5 to 13% by weight, or 8 to 12% by weight relative to the whole composition. The composition contains solids and a solvent. If the content of (G) the resin having urethane bonds is within the above range, the composition will have excellent flexibility and crack resistance, and will exhibit appropriate tackiness, excellent printability and drying properties.

[0163] In the photosensitive resin composition of the present invention, the weight-average molecular weight of the resin having (G) urethane bonds may be 2,000 to 150,000 g / mol, or 2,000 to 50,000 g / mol. If the weight-average molecular weight of the resin having (G) urethane bonds is within the above range, it may have excellent crack resistance and flexibility.

[0164] [Other optional components]

[0165] The photosensitive resin composition of the present invention may optionally contain various additives as required components. Specifically, thermosetting catalysts, dispersants, antioxidants, colorants, epoxy resins, oxetane compounds, (meth)acrylic resins, and other various additives or mixtures of two or more of these may be added. The optional components may include one or more of the following materials.

[0166] <Epoxy resin>

[0167] The epoxy resin of the present invention can use known and conventional compounds having one or more epoxy groups. For example, the epoxy resin may not overlap with components (A) to (G) described above. For example, it may be a compound having two or more epoxy groups. For example, monoepoxy compounds such as butyl glycidyl ether, phenyl glycidyl ether, and glycidyl (meth)acrylate; bisphenol A type epoxy resin, bisphenol S type epoxy resin, bisphenol F type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, aliphatic ring epoxy resin; trimethylolpropane polyglycidyl ether, phenyl-1,3-diglycidyl ether, biphenyl-4,4'-diglycidyl ether, 1,6-hexanediol diglycidyl ether, ethylene glycol or propylene glycol diglycidyl ether, sorbitol polyglycidyl ether, tris(2,3-epoxypropyl) isocyanurate, and triglycidyl tris(2-hydroxyethyl) isocyanurate may be compounds having two or more epoxy groups in one molecule. These can be used individually or in combination of two or more depending on the required properties.

[0168] Examples of compounds having two or more epoxy groups include jER828, jER834, jER1001, jER1004 from Mitsubishi Chemical Corporation, Epiclon 840, Epiclon 850, Epiclon 1050, Epiclon 2055 from DIC Corporation, Epotote D-011, YD-013, YD127, YD-128 from Nippon Steel Chemical & Materials, and DER317, DER33 from Dow Chemical Japan Ltd. 1. Bisphenol A type epoxy resins such as DER661, DER664, Sumitomo Chemical Co., Ltd.'s SumiEpoxy ESA-011, ESA-014, ELA-115, ELA128, Asahi Kasei Materials Corporation's AER330, AER331, AER661, AER664, etc. (all product names); Mitsubishi Chemical Corporation's jERYL903, DIC Corporation's Epiclon 152, Epiclon 165, Nippon Steel Chemical & Materials Brominated epoxy resins such as ELZ Co., Ltd.'s EPOTOTE YDE-400, YDE-500, Dow Chemical Japan Ltd.'s DER542, Sumitomo Chemical Co., Ltd.'s SumiEpoxy ESB-400, ESB-700, Asahi Kasei Materials Corporation's AER711, AER714, etc. (all product names); Mitsubishi Chemical Corporation's jER152, jER154, Dow Chemical Japan Ltd.'s DEN431, DEN438, DIC Corporation's Epiclon N-730, Epiclon N-770, Epiclon N-865, Epotote YDC-701, YDC-704 from Nippon Steel Chemical & Materials Co., Ltd., EPPN-201, EPPN-1025, EPPN-1020, EPPN-104S, RE-306, NC-3000 from Nippon Chemical Co., Ltd., Sumiepoxy ESCN-195X, ESCN-220 from Sumitomo Chemical Co., Ltd., AER from Asahi Kasei Materials CorporationNovolac-type epoxy resins such as ECN-235, ECN-299, YDCN-700-2, YDCN-700-3, YDCN-700-5, YDCN-700-7, YDCN-700-10, YDCN-704, YDCN-704A from Nippon Steel Chemical & Materials Co., Ltd., and Epiclon N-680, N-690, N-695 from DIC Corporation (all product names); and bisphenol F-type epoxy resins such as Epiclon 830 from DIC Corporation, jER807 from Mitsubishi Chemical Corporation, and Epotote YDF-175, YDF-2004 from Nippon Steel Chemical & Materials Co., Ltd. (all product names). Xylionic resins; hydrogenated bisphenol A type epoxy resins such as Epotote ST-2004, ST-2007, and ST-3000 (product names) from Nippon Steel Chemical & Materials Co., Ltd.; glycidylamine type epoxy resins such as jER604 from Mitsubishi Chemical Corporation, Epotote YH-434 from Nippon Steel Chemical & Materials Co., Ltd., and Sumiepoxy ELM-120 from Sumitomo Chemical Co., Ltd. (all product names); hydantoin type epoxy resins; alicyclic epoxy resins such as Celoxide 2021 from Daicel Corporation (all product names); YL-933 from Mitsubishi Chemical Corporation, and TEN from Dow Chemical Japan Ltd.Trihydroxyphenylmethane type epoxy resins such as EPPN-501, EPPN-502, etc. (all product names); bixylenol type or biphenol type epoxy resins or mixtures thereof such as YL-6056, YX-4000, YL-6121 (all product names) from Mitsubishi Chemical Corporation; bisphenol S type epoxy resins such as EBPS-200 from Nippon Kayaku Co., Ltd., EPX-30 from ADEKA Corporation, and EXA-1514 (product name) from DIC Corporation; bisphenol A novolac type epoxy resins such as jER157S (product name) from Mitsubishi Chemical Corporation; jER Tetraphenyloleethane-type epoxy resins such as YL-931 (product names); heterocyclic epoxy resins such as TEPIC from Nissan Chemical Industries, Ltd. (product names); diglycidyl phthalate resins such as Bremmer DGT from NOF Corporation; tetraglycidyl xylenolethane resins such as ZX-1063 from Nippon Steel Chemical & Materials Co., Ltd.; naphtha such as ESN-190, ESN-360 from Nippon Steel Chemical & Materials Co., Ltd., and HP-4032, EXA-4750, EXA-4700 from DIC Corporation. Examples of epoxy resins that can be used include, but are not limited to, benzene-containing epoxy resins; epoxy resins having a dicyclopentadiene skeleton, such as HP-7200 and HP-7200H from DIC Corporation; glycidyl methacrylate copolymer epoxy resins, such as CP-50S and CP-50M from NOF Corporation; copolymer epoxy resins of cyclohexylmaleimide and glycidyl methacrylate; and CTBN-modified epoxy resins (e.g., YR-102 and YR-450 from Nippon Steel Chemical & Materials Co., Ltd.). Among these, bisphenol A type epoxy resins, heterocyclic epoxy resins, or mixtures thereof may be preferred over those with superior discoloration resistance. These epoxy resins may be used individually or in combination of two or more types.

[0169] In the photosensitive resin composition of the present invention, the epoxy resin may be a bisphenol-based epoxy resin, for example, a bisphenol epoxy resin having two or more epoxy groups. The amount of the bisphenol-based epoxy resin having two or more epoxy groups used in the present invention may be 1 to 15% by weight, 1 to 10% by weight, or 3 to 10% by weight of the whole composition. The composition contains solids and a solvent.

[0170] If the epoxy resin content is within the aforementioned range, the coating film formed by the composition will have excellent adhesion, heat resistance, and pencil hardness, will harden well, and problems such as yellowing and difficulty in achieving high reflectivity after the process can be solved.

[0171] In the photosensitive resin composition of the present invention, the weight-average molecular weight of the epoxy resin may be 150 to 100,000 g / mol.

[0172] <Oxetane compounds>

[0173] Next, we will explain oxetane compounds. The general formula (I) below

[0174] [ka]

[0175] (In the formula, R 1) represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. Specific examples of oxetane compounds containing an oxetane ring represented by ) include 3-ethyl-3-hydroxymethyloxetane (Toagosei Co., Ltd., trade name OXT-101), 3-ethyl-3-(phenoxymethyl)oxetane (Toagosei Co., Ltd., trade name OXT-211), 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane (Toagosei Co., Ltd., trade name OXT-212), 1,4-bis{[(3-ethyl-3-oxetanyl)methoxy]methyl}benzene (Toagosei Co., Ltd., trade name OXT-121), bis(3-ethyl-3-oxetanylmethyl)ether (Toagosei Co., Ltd., trade name OXT-221), etc. Also, phenol novolac type oxetane compounds can be mentioned. Such oxetane compounds may be used in combination with the epoxy compound, or they may be used alone.

[0176] <(meth)acrylic resin>

[0177] The (meth)acrylic resin is a photocurable resin. The photocurable resin is not particularly limited as long as it is a resin that is cured by irradiation with active energy rays and exhibits electrical insulation properties, and may be, for example, a compound having one or more ethylene unsaturated bonds in its molecule. For example, the (meth)acrylic resin may not overlap with the components (A) to (G) described above.

[0178] The compound having an ethylene unsaturated bond may be a known and conventional photopolymerizable oligomer, photopolymerizable monomer, or photopolymerizable vinyl monomer. The photopolymerizable oligomer may be an unsaturated polyester oligomer or a (meth)acrylate oligomer. The (meth)acrylate oligomer may be an epoxy (meth)acrylate such as phenol novolac epoxy (meth)acrylate, cresol novolac epoxy (meth)acrylate, or bisphenol type epoxy (meth)acrylate, or an urethane (meth)acrylate, epoxy urethane (meth)acrylate, polyester (meth)acrylate, polyether (meth)acrylate, or polybutadiene-modified (meth)acrylate.

[0179] Photopolymerizable monomers or photopolymerizable vinyl monomers include well-known and commonly used ones, such as styrene derivatives like styrene, chlorostyrene, and α-methylstyrene; vinyl esters such as vinyl acetate, vinyl butyrate, or vinyl benzoate; ethers such as vinyl isobutyl ether, vinyl-n-butyl ether, vinyl-t-butyl ether, vinyl-n-amyl ether, vinyl isoamyl ether, vinyl-n-octadecyl ether, vinylcyclohexyl ether, ethylene glycol monobutyl ether, and triethylene glycol monomethyl ether; (meth)acrylamides such as acrylamide, methacrylamide, N-hydroxymethylacrylamide, N-hydroxymethylmethacrylamide, N-methoxymethylacrylamide, N-ethoxymethylacrylamide, and N-butoxymethylacrylamide; aryl compounds such as triallyl isocyanurate, diaryl phthalate, and diaryl isophthalate; 2-ethylhexyl (meth)acrylate, lauryl (Meth)acrylic acid esters such as lyl(meth)acrylate, tetrahydrofurfuryl(meth)acrylate, isobornyl(meth)acrylate, phenyl(meth)acrylate, and phenoxyethyl(meth)acrylate; hydroxyalkyl(meth)acrylates such as hydroxyethyl(meth)acrylate, hydroxypropyl(meth)acrylate, and pentaerythritol(meth)acrylate; alkoxyalkylene glycol mono(meth)acrylates such as methoxyethyl(meth)acrylate and ethoxyethyl(meth)acrylate; alkylene polyol poly(meth)acrylates such as ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, trimethylolpropane(meth)acrylate, pentaerythritol tetra(meth)acrylate, and dipentaerythritol hexa(meth)acrylate;Examples include polyoxyalkylene glycol poly(meth)acrylates such as diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, ethoxylated trimethylolpropane triacrylate, and propoxylated trimethylolpropane tri(meth)acrylate; poly(meth)acrylates such as hydroxypivalate neopentyl glycol ester di(meth)acrylate; and isocyanurate-type poly(meth)acrylates such as tris[(meth)acryloxyethyl]isocyanurate. These can be used individually or in combination of two or more.

[0180] In the photosensitive resin composition of the present invention, the (meth)acrylic resin may be an unsaturated polyester oligomer, a (meth)acrylate oligomer, or, for example, a hexafunctional flexible acrylic oligomer. The amount of (meth)acrylic resin blended may be 1 to 15% by weight, 1 to 10% by weight, or 5 to 10% by weight of the whole composition. The composition contains solids and a solvent. If the content of the (meth)acrylic resin is within the above range, the composition exhibits excellent resolution and undercut, and the coating film can be cured to an appropriate level.

[0181] <Thermosetting catalyst>

[0182] In the composition of the present invention, at least one of a curing agent or a curing catalyst can be further added as a thermosetting catalyst. For example, the thermosetting catalyst may not overlap with the components (A) to (G) described above.

[0183] The curing agent may be, for example, a polyfunctional phenol compound, a polycarboxylic acid and its acid anhydride, an aliphatic or aromatic primary or secondary amine, a polyamide resin, an isocyanate compound, or a polymercapto compound. The curing agent may be, for example, a polyfunctional phenol compound, a polycarboxylic acid and its acid anhydride, and excellent workability and insulating properties can be obtained using such a curing agent. The polyfunctional phenol compound is not particularly limited as long as it is a compound having two or more phenolic hydroxyl groups in one molecule, and may be, for example, a known and commonly used compound. For example, the polyfunctional phenol compound may be a phenol novolac resin, a cresol novolac resin, bisphenol A, allylated bisphenol A, bisphenol F, a novolac resin of bisphenol A, or a vinylphenol copolymer resin. The polyfunctional phenol compound may be, for example, bisphenol A, which can increase reactivity and improve heat resistance. The polyfunctional phenol compound can be added to at least one epoxy compound or oxetane compound in the presence of a suitable curing catalyst. Polycarboxylic acids and their acid anhydrides may be, for example, compounds having two or more carboxyl groups in one molecule and their acid anhydrides, such as copolymers of (meth)acrylic acid, copolymers of maleic anhydride, and condensates of dibasic acids. Commercially available products include BASF's Joncryl (product group name), Sartomer's SMA resin (product group name), and Shin Nippon Rika's polyazelaic anhydride.

[0184] Furthermore, the curing catalyst may be a compound that can act as a curing catalyst in the reaction between a thermosetting resin such as an epoxy compound or an oxetane compound and a curing agent, or a compound that acts as a polymerization catalyst when no curing agent is used. Specifically, the curing catalyst may be, for example, a tertiary amine, a tertiary amine salt, a quaternary ammonium salt, a tertiary phosphine, a crown ether compound, and a phosphonium ylide, and any of these may be used individually or in combination of two or more.

[0185] For example, imidazoles such as trade names 2E4MZ, C11Z, C17Z, and 2PZ, imidazole AZINE compounds such as trade names 2MZ-A and 2E4MZ-A, isocyanurates of imidazoles such as trade names 2MZ-OK and 2PZ-OK, imidazole hydroxymethyl derivatives such as trade names 2PHZ and 2P4MHZ (trade name: Shikoku Chemicals Co., Ltd.), dicyandiamide and its derivatives, melamine and its derivatives, diaminomaleonitrile and its derivatives, diethylenetriamine, triethylenetetramine, tetraethylene It may be amines such as antamine, bis(hexamethylene)triamine, triethanolamine, diaminodiphenylmethane, 1,8-diazabicyclo[5,4,0]undecene-7 (trade name DBU, Sunapro Co., Ltd.), 3,9-bis(3-aminopropyl)-2,4,8,10-tetraoxaspiro[5,5]undecane (trade name ATU, Ajinomoto Co., Inc.), or organic phosphine compounds such as triphenylphosphine, tricyclohexylphosphine, tributylphosphine, methyldiphenylphosphine, etc.

[0186] In the photosensitive resin composition of the present invention, the curing catalyst may be an amine-based, phosphine-based, or imidazole-based curing catalyst, for example, a melamine-based amine curing catalyst. The amount of curing catalyst blended may be 0.1 to 10% by weight, 0.1 to 5% by weight, or 0.1 to 3% by weight relative to the total composition.

[0187] If the content of the curing catalyst is within the range described above, the coating film will be sufficiently cured, resulting in excellent adhesion, pencil hardness, and heat resistance, while maintaining an appropriate curing time and preventing a decrease in developability.

[0188] <Antioxidant>

[0189] The photosensitive resin composition of the present invention may also contain an antioxidant. By including an antioxidant, it is possible to prevent oxidative degradation of curable resins and the like, suppress discoloration, and also improve heat resistance and achieve good resolution (reproducibility of line width). In other words, depending on the type of white colorant, resolution may be worsened by reflecting and absorbing light, but by including an antioxidant, good resolution can be obtained regardless of the type of white colorant. The antioxidant may be a radical scavenger that neutralizes generated radicals, or a peroxide decomposition inhibitor that decomposes generated peroxides into harmless substances and prevents the generation of new radicals, and may be a single type or a combination of two or more types.

[0190] Antioxidants that act as radical scavengers include, for example, hydroquinone, 4-t-butylcatechol, 2-t-butylhydroquinone, hydroquinone monomethyl ether, 2,6-di-t-butyl-p-cresol, 2,2-methylene-bis(4-methyl-6-t-butylphenol), 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane, and 1,3,5-trimethyl-2,4,6-tris These may include phenolic compounds such as (3,5-di-t-butyl-4-hydroxybenzyl)benzene and 1,3,5-tris(3',5'-di-t-butyl-4-hydroxybenzyl)-S-triazine-2,4,6-(1H,3H,5H)trione, quinone compounds such as menaquinone and benzoquinone, and amine compounds such as bis(2,2,6,6-tetramethyl-4-piperidyl)-sebacate and phenothiazine. Commercially available products include, for example, IRGANOX1010 (BASF Japan Ltd., trade name).

[0191] Furthermore, antioxidants that have an effect as peroxide decomposition agents include, for example, phosphorus compounds such as triphenyl phosphite, and sulfur compounds such as pentaerythritol tetralaurylthiopropionate, dilaurylthiodipropionate, and distearyl-3,3'-thiodipropionate.

[0192] For example, the antioxidant may be a phenolic compound, and when used, it is possible to suppress discoloration, improve heat resistance, and reproduce better resolution.

[0193] Furthermore, antioxidants, such as phenolic antioxidants, can be used in combination with heat stabilizers. When used in combination, they can exhibit even better results.

[0194] The heat stabilizer may be, for example, a phosphorus-based, hydroxylamine-based, or sulfur-based heat stabilizer. The heat stabilizer may be a single type or a combination of two or more types.

[0195] For example, the antioxidant may be a hydroxylamine-based antioxidant, a sulfur-based antioxidant, or a phenol-based antioxidant. When a phenol-based antioxidant is used, the amount added may be 0.01 to 5% by weight or 0.03 to 3% by weight of the total composition. By adding 0.01 to 1% by weight or more of the antioxidant, the effect of adding the antioxidant can be reliably obtained, and by adding 1% by weight or less, good alkaline development can be obtained without inhibiting the photoreaction, and good touch-drying properties and coating film properties can also be ensured.

[0196] <Organic solvents>

[0197] The photosensitive resin composition of the present invention may contain an organic solvent for purposes such as manufacturing the composition or adjusting its viscosity when applied to a substrate or base material. As the organic solvent, known and commonly used organic solvents can be used, such as esters; aliphatic hydrocarbons such as octane and decane; and petroleum-based solvents such as petroleum ether, petroleum naphtha, and solvent naphtha. These organic solvents can be used individually or in combination of two or more.

[0198] <Other additives>

[0199] Furthermore, the photosensitive resin composition of the present invention may contain other additives known and commonly used in the field of electronic materials. Examples of other additives include thermal polymerization inhibitors, ultraviolet absorbers, plasticizers, flame retardants, antistatic agents, anti-aging agents, antibacterial and antifungal agents, defoaming agents, leveling agents, thickeners, adhesion promoters, thixotropic agents, photoinitiation aids, additive enhancers, curing accelerators, mold release agents, surface treatment agents, dispersants, dispersion aids, surface modifiers, and stabilizers.

[0200] The photosensitive resin composition of the present invention may have a phosphorus content of 500 to 5000 ppm.

[0201] By increasing the phosphorus content of the photosensitive resin composition to 500 ppm or more, surface hardening is improved, and the resistance to gold plating and adhesion are enhanced. By decreasing the phosphorus content to 5000 ppm or less, the reaction rate of the silicone sealant is increased.

[0202] If the phosphorus content is less than 500 ppm, the pencil hardness will be 3H, the adhesion after gold plating will be poor, the gloss will be low, and solder resist openings (SROs) may not form well. On the other hand, if the phosphorus content exceeds 5,000 ppm, the reaction rate of the silicon encapsulant will be very low, resulting in low developability and reflectivity, and SROs may not form easily.

[0203] [Dry film and method for producing the same]

[0204] Another embodiment of the present invention relates to a dry film having a photosensitive resin layer obtained by coating and drying a photosensitive resin composition on a first film.

[0205] To form a dry film, first, the composition of the present invention is diluted with an organic solvent to adjust to an appropriate viscosity, and then applied to a first film to a uniform thickness, for example, in the range of 40 to 60 μm, using a comma coater, blade coater, lip coater, load coater, squeeze coater, reverse coater, transfer roll coater, gravure coater, microgravure coater, spray coater, etc. After that, the applied composition is dried at a temperature usually in the range of 40 to 120°C for 1 to 30 minutes to form a photosensitive resin layer, thereby forming a dry film.

[0206] There are no particular limitations on the thickness of the coating film, but generally, the thickness after drying may be 10 to 150 μm, 10 to 80 μm, or 10 to 60 μm.

[0207] As the first film, a plastic film can be used, such as polyester film like polyethylene terephthalate (PET), polyimide film, polyamide-imide film, polypropylene film, or polystyrene film, and may be polyethylene terephthalate, for example. The thickness of the first film is not particularly limited, but can generally be appropriately selected in the range of 10 to 150 μm. It can also be applied to metal foils such as copper foil or aluminum foil. Furthermore, the used first film can be subjected to a release treatment such as acrylic or silicone.

[0208] Since the dry film of the present invention is white, it can be used to reflect light emitted from light-emitting diodes (LEDs) or electroluminescent (ELs) used as light sources in lighting mechanisms, mobile devices, laptop computers, tablet PCs, monitors, smartphones, personal computers, and backlights of liquid crystal displays in televisions, etc. The dry film of the present invention can be applied to LEDs and light-emitting PCBs, etc.

[0209] To create a cured coating on a printed circuit board using a dry film, a second film, which serves to protect the dry film, is peeled off. The exposed resin layer of the dry film is then placed on the circuit-formed substrate and attached using a laminator or similar device to form a resin layer on the circuit-formed substrate. Subsequently, the formed resin layer is exposed to light, developed, heated, and then cured to form a cured coating. The second film can be peeled off at either the pre-exposure or post-exposure stage.

[0210] [Cured product and method for producing the same]

[0211] The cured product of the present invention may be obtained by curing the solder resist layer of the photosensitive resin composition of the present invention or the dry film of the present invention.

[0212] The cured product of the present invention can be appropriately used in printed circuit boards, electronic components, and the like. The cured product of the present invention exhibits high crack resistance, high resolution, and excellent dielectric properties, including low dielectric constant and low dielectric loss tangent. Furthermore, the cured product of the present invention also exhibits excellent heat resistance and linear expansion coefficient.

[0213] For example, the cured product of the present invention may be a solder resist.

[0214] The solder resist may be manufactured by applying the photosensitive resin composition of the present invention to a substrate to form a photosensitive resin layer, then selectively exposing it with active energy rays using a photomask on which a predetermined pattern has been formed, and developing the unexposed areas with a dilute alkaline aqueous solution (for example, a 0.3-3 wt% sodium carbonate aqueous solution) to form the pattern. Alternatively, in the case of a dry film, after exposure, the first film of the dry film is peeled off and then developed to form a patterned solder resist on the substrate. Furthermore, within a range that does not impair the properties, the first film can be peeled off from the dry film before exposure, and the exposed resin layer can be exposed and developed.

[0215] [Printed wiring board and method for manufacturing the same]

[0216] The printed circuit board of the present invention may include a cured product of the photosensitive resin composition of the present invention or a cured film obtained by curing the photosensitive resin layer of the dry film of the present invention.

[0217] The printed circuit board of the present invention may contain a cured product obtained from the photosensitive resin composition of the present invention or from the photosensitive resin layer of a dry film. The method for manufacturing the printed circuit board of the present invention involves, for example, adjusting the photosensitive resin composition of the present invention to a viscosity suitable for the coating method using the organic solvent, coating it onto a substrate using methods such as dip coating, flow coating, roll coating, bar coating, screen printing, or curtain coating, and then volatilizing (pre-drying) the organic solvent contained in the composition at a temperature of 60 to 100°C to form a tacky-free resin layer. In the case of a dry film, the resin layer can be bonded to the substrate using a laminator or the like so that it is in contact with the substrate, and then the first film can be peeled off to form a resin layer on the substrate.

[0218] The aforementioned substrates include printed circuit boards and flexible printed circuit boards with circuits formed on copper, as well as materials such as paper phenol, paper epoxy, glass fiber epoxy, glass polyimide, glass fiber / epoxy, glass fiber / paper epoxy, synthetic fiber epoxy, fluororesin / polyethylene / polyphenylene ether, and polyphenylene oxide cyanate, and copper foil laminates for high-frequency circuits. Examples include FR-4 substrates, copper foil laminates of all grades (FR-4, etc.), other metal substrates, polyimide films, polyethylene terephthalate films, polyethylene naphthalate (PEN) films, glass substrates, ceramic substrates, and wafer substrates.

[0219] As a method for laminating a dry film onto a substrate, it can be carried out after applying pressure and heating using a vacuum laminator or the like. By using such a vacuum laminator, even if the surface of the circuit board is uneven when a circuit board is used, the dry film adheres closely to the circuit board, preventing the inclusion of air bubbles and improving the easing of recessed areas on the substrate surface. The pressure conditions may be around 0.1 to 2.0 MPa, and the temperature conditions may be 40 to 120°C.

[0220] Furthermore, by performing the following methods on the cured material, a cured film with excellent adhesion, hardness, and other properties can be formed: i) irradiation with active energy rays followed by heat curing (e.g., 100-220°C), ii) irradiation with active energy rays after heat curing, iii) irradiation with active energy rays alone, or iv) heat curing alone.

[0221] The cured product of the present invention can be cured by heating at a temperature of, for example, 100 to 220°C to form a cured film with high reflectivity and excellent properties such as excellent resistance to yellowing and excellent resistance to cracking.

[0222] The exposure apparatus used for the activation energy ray irradiation may be a device equipped with a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a metal halide lamp, a mercury short-arc lamp, etc., that irradiates ultraviolet (UV) light in the range of 350 to 450 nm, or it may be a direct drawing apparatus (for example, a laser direct imaging apparatus that directly draws CAD data on a computer with a laser). The lamp light source or laser light source of the direct drawing apparatus may have a maximum wavelength in the range of 350 to 450 nm. The exposure for image formation varies depending on the thickness, etc., but is generally 10 to 1000 mJ / cm². 2 It may be, or 20-800 mJ / cm² 2 That's fine.

[0223] The aforementioned developing method may be a dipping method, shower method, spray method, brush method, etc., and as the developing solution, an alkaline aqueous solution such as potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, or amines can be used.

[0224] The printed circuit board of the present invention may include a dry film comprising one or more layers formed from the photosensitive resin composition.

[0225] When forming printed circuit boards, a dry film can be placed on a test board and transferred to the test board by vacuum lamination.

[0226] Subsequently, the first film is peeled off, and the substrate onto which the dry film from which the first film was peeled off has been transferred can be UV exposed using an exposure apparatus. When exposed in this manner, the exposed areas (parts irradiated with light) can be cured. After exposure, the substrate is cooled at room temperature, then placed in a developing machine, and the unexposed areas are developed with an alkaline aqueous solution to complete the resist pattern formation. The substrate with the pattern formed by development is then post-cured in a 150°C oven for 1 hour to complete the substrate fabrication. After final curing, a reflow process is performed, followed by the process of mounting the chip. Subsequently, a process of sealing is performed by creating a silicon encapsulant on the cured photosensitive resin layer. The photosensitive resin composition of the present invention can improve the problems of yellowing and incomplete curing of the silicon encapsulant formed on the cured product by reducing outgassing of the photopolymerization initiator, and can improve the reaction rate of the silicon encapsulant.

[0227] The method for manufacturing a printed circuit board containing the cured product of the present invention allows, for example, the first film to be peeled off after an exposure process following a lamination process.

[0228] [Silicone encapsulant layer and method for producing the same]

[0229] The printed circuit board of the present invention may further include a silicon encapsulant layer disposed on the cured product (obtained by curing a photosensitive resin layer). The silicon encapsulant layer may be formed by coating the printed circuit board and the solder resist layer with a silicon-containing composition to encapsulate and protect them.

[0230] To protect the light-emitting chip portion and the photosensitive resin layer (or the cured product obtained by curing it), the aforementioned silicone encapsulant layer can be applied as a coating.

[0231] The following describes an example method for fabricating a silicon encapsulant layer.

[0232] After the printed circuit board has been fully cured or reflowed, a dam measuring 2.0 cm wide, 2.0 cm long, and 250-300 μm thick is created. Then, a 1:1 mixture of silicone encapsulants A and B is added, and a 250-300 μm thick layer of silicone encapsulant is applied. Subsequently, the dam is cured in a 100°C oven for 2 hours to complete the primary curing, and then cured in a 150°C oven for 4 hours to complete the secondary curing of the silicone encapsulant, thereby creating a silicone encapsulant layer.

[0233] To measure the physical properties of the silicone encapsulant layer, the layer can be peeled off after curing is complete, and the reaction rate of the silicone encapsulant and the content of the photopolymerization initiator remaining in the silicone encapsulant layer can be analyzed. Furthermore, the degree of curing (reaction rate) of the silicone encapsulant can be measured to confirm how far the curing has progressed. Additionally, the reflectance of the silicone encapsulant layer can be measured.

[0234] For example, the silicon encapsulant layer may include a lower encapsulant region, which is close to the solder resist layer, and an upper encapsulant region, which is far from the solder resist layer.

[0235] For example, the content of the (E) photopolymerization initiator contained in the upper or lower sealing material region may be 1,000 ppm or less relative to the content of the (E) photopolymerization initiator contained in the solder resist layer, for example, 900 ppm or less, 800 ppm or less, 700 ppm or less, 600 ppm or less, or 500 ppm or less.

[0236] The amount of photopolymerization initiator contained in the upper or lower sealing material region is the amount transferred from the photopolymerization initiator contained in the solder resist layer. In other words, by using a trimethylbenzoylphosphine oxide compound containing one or more PO bonds, which is the (E) photopolymerization initiator of the present invention, the amount of photopolymerization initiator transferred to the nearby upper or lower sealing material region can be reduced.

[0237] For example, if the photopolymerization initiator is transferred to the silicon encapsulant layer by outgassing diffusion, the phosphorus (P) component of the photopolymerization initiator and the catalytic component of the silicon encapsulant layer (e.g., platinum catalyst) inhibit each other, resulting in the silicon encapsulant remaining uncured and a decrease in the silicon encapsulant reaction rate. This decrease in the silicon encapsulant reaction rate may lead to problems with long-term reliability.

[0238] [Protective film]

[0239] The laminate of the present invention may include the cured product and the protective film.

[0240] In this invention, in order to remove the photopolymerization initiator, a protective film can be applied after the photosensitive resin layer has been fully cured to form a cured product. When a protective film is applied, the protective film has a high affinity for the photopolymerization initiator, so the photopolymerization initiator remaining in the solder resist layer can be efficiently removed. By removing this remaining photopolymerization initiator, the amount of photopolymerization initiator remaining after the reflow and firing processes can be reduced. This reduced amount of photopolymerization initiator increases the reaction rate of the silicone sealant when it is coated onto the cured product layer, and this increased reaction rate can greatly improve long-term reliability.

[0241] Examples of protective films that can be used include polyethylene film, polytetrafluoroethylene film, polypropylene film, and surface-treated paper. The thickness of the protective film is not particularly limited, but may be, for example, 10 to 150 μm.

[0242] For example, the amount of (E) photopolymerization initiator contained in the protective film may be 1000 ppm or less relative to the amount of (E) photopolymerization initiator contained in the solder resist layer.

[0243] The amount of photopolymerization initiator contained in the protective film is the amount transferred from the photopolymerization initiator contained in the solder resist layer. In other words, by using a trimethylbenzoylphosphine oxide group-containing compound containing one or more PO bonds, which is the (E) photopolymerization initiator of the present invention, the amount of photopolymerization initiator transferred to nearby protective films can be reduced.

[0244] <Examples>

[0245] The present invention will be described in detail below with reference to examples. The present invention is not limited to the following examples.

[0246] <Synthesis Example 1 (Alkali-soluble resin A, copolymer resin)>

[0247] In a flask equipped with a thermometer, stirrer, dropping funnel, and reflux condenser, 325.0 parts by weight of dipropylene glycol monomethyl ether as a solvent was heated to 110°C. A mixture of 174.0 parts by weight of methacrylic acid, 174.0 parts by weight of ε-caprolactone-modified methacrylic acid (average molecular weight 314), 77.0 parts by weight of methyl methacrylate, 222.0 parts by weight of dipropylene glycol monomethyl ether, and 12.0 parts by weight of t-butylperoxy-2-ethylhexanoate (Perbutyl-O, NOF Corporation) as a polymerization catalyst was added dropwise over 3 hours. After stirring at 110°C for 3 hours, the polymerization catalyst was deactivated to obtain a resin solution. After cooling this resin solution, 289.0 parts by weight of Daicel's Cyclomer M100, 3.0 parts by weight of triphenylphosphine, and 1.3 parts by weight of hydroquinone monomethyl ether were added, and the mixture was heated to 100°C and stirred to carry out the ring-opening addition reaction of the epoxy ring, thereby obtaining resin solution A. The solid content of the obtained resin solution A was 54.5% by weight, and the acid value of the solid content was 79.8 mg KOH / g.

[0248] <Synthesis example 2, D resin solution>

[0249] 200 parts by weight of deionized water and 0.3 parts by weight of sodium sulfate were poured into a pressure vessel equipped with a thermometer, condenser, and stirrer, and their dissolution was confirmed. Subsequently, 5 parts by weight of BPO (benzoyl peroxide) as a polymerization initiator and 5 parts by weight of MSD (α-methylstyrene dimer) as a chain transfer agent were added to a monomer mixture consisting of 10.4 parts by weight of MMA (methyl methacrylate), 5 parts by weight of n-BA (n-butyl acrylate), 24.6 parts by weight of MAA (methacrylic acid), and 60 parts by weight of Stylene (styrene), and then thoroughly dissolved. After that, a dispersant was added to a concentration of 300 ppm, the mixture was thoroughly stirred, the inside of the vessel was purged with nitrogen, and the temperature was raised to carry out suspension polymerization. After polymerization was complete, the obtained suspension solution was filtered through a 30 μm mesh and dried with hot air at 40°C to obtain particulate resin. The granular resin (copolymer resin) obtained in this manner was thoroughly dissolved in the organic solvent DPM (dipropylene glycol methyl ether) to a solid content concentration of 50% by weight, and this was prepared as resin solution D. The solid content acid value was 160 mg KOH / g.

[0250] <Synthesis Example 3, Carboxyl group-containing cresol novolac type epoxy acrylate resin A-2>

[0251] 220 parts by mass of cresol novolac epoxy resin was placed in a four-necked flask equipped with a stirrer and reflux condenser, and 214 parts by mass of carbitol acetate was added and heated until dissolved. Next, 0.1 parts by mass of hydroquinone as a polymerization inhibitor and 2.0 parts by mass of dimethylbenzylamine as a reaction catalyst were added to prepare a mixture. This mixture was heated to 95-105°C, and 72 parts by mass of acrylic acid was gradually added dropwise, followed by a reaction for 16 hours. The reaction product was cooled to 80-90°C, 106 parts by mass of tetrahydrophthalic anhydride was added, and the reaction was carried out for 8 hours. After cooling, the product was removed.

[0252] The resulting photosensitive resin, possessing both ethylenically unsaturated bonds and carboxyl groups, had a non-volatile content of 64%, a solid acid value of 84.4 mg KOH / g, and a weight-average molecular weight (Mw) of approximately 7,500. This resin will be referred to as (A-2) below. The weight-average molecular weight of the obtained resin was measured by GPC.

[0253] Manufacturing of photosensitive resin compositions

[0254] [Table 1] JPEG0007955485000007.jpg247170JPEG0007955485000008.jpg143170

[0255] Production of dry films of photosensitive resin compositions

[0256] In a dust-free room, using a comma coater, (1) the compositions of each example and comparative example were applied to a uniform thickness (50 μm) onto a first film (PET film) (Toray Industries XD-500P, film thickness: 25 μm). (2) The applied compositions were dried in four temperature chambers (chamber 1: 60°C, chamber 2: 80°C, chamber 3: 100°C, chamber 4: 100°C) in the range of 40 to 120°C. (3) The appropriately dried coating film on the first film was laminated with a second film (Polypropylene, PP film) to produce a dry film. At this time, the thickness of the dried coating film was kept in the range of 60 μm.

[0257] Evaluation Example 1: Measurement of outgassing, reaction rate of silicon encapsulant, and photopolymerization initiator content.

[0258] 1. Measurement of outgassing content

[0259] Dry films were prepared by laminating the photosensitive resin compositions according to the examples and comparative examples onto PET films using a vacuum laminator (CVP-300: manufactured by Nikko Materials Co., Ltd.) in the first chamber at 60°C under conditions of a vacuum pressure of 3 hPa and a vacuum time of 10 seconds, and then peeling off the PET films.

[0260] Using a DI exposure system manufactured by Screen, the integrated light meter measured 300 mJ / cm². 2 To achieve this, a Kodak Step Tablet No. 2 (41 steps) was used as a photomask and the entire surface was exposed to 23 steps. Next, development was carried out with a 1.0% Na2CO3 aqueous solution at 30°C under a spray pressure of 0.2 MPa for 60 seconds. After that, the material was cured in a 150°C oven for 60 minutes to obtain a cured photosensitive resin layer.

[0261] Powder samples were taken from the fabricated resist layer and placed in a thermal desorption unit (TDU) manufactured by Güstel. Specifically, the powder samples were heated using helium as a purge gas (50 ml / min), heated at 30°C at a rate of 60°C / min, heated at 150°C for 60 minutes, and desorbed and collected at -50°C. The collected outgassing components were separated and analyzed using an Agilent Technologies gas chromatography-mass spectrometer (8890 / 5977B), quantified in terms of n-dodecane, and then measured by weight % based on the weight of the photopolymerization initiator contained in the cured photosensitive resin layer.

[0262] The measurement conditions for gas chromatography are as follows: Column: Agilent Technologies capillary column DB-1MS (length 30m, inner diameter 0.25mm, thickness 0.25μm), Detector: MS (ITQ900), Carrier gas: Helium, Injector temperature: 300℃, Detector temperature: 230℃, Column temperature conditions: Initial temperature 50℃, held at 50℃ for 2 minutes after sample injection, heating to 300℃ at 12℃ / second, held for 10 minutes after reaching 300℃.

[0263] Separately, as will be described later, a silicone encapsulant was formed on the substrate (a dry film of a photosensitive resin composition laminated onto an FR-4 Cu film, followed by PET peeling), and then cured by heating at 100°C for 2 hours and then at 150°C for 4 hours.

[0264] The outgassing content, silicon reaction rate, and photopolymerization initiator content transferred to the silicon encapsulant and protective film for each example and comparative example were measured and are shown in Table 2 below. See below for details of each measurement method.

[0265] [Method for measuring outgassing content]

[0266] TD-GCMS analysis was performed to identify the peak of the photopolymerization initiator. The unit of this peak was expressed as μg / g, representing the amount of gas generated per gram of sample, converted to n-dodecane. The total outgassing of the photopolymerization initiator peak was measured. The ratio of the peak area of ​​the photopolymerization initiator to the area of ​​n-dodecane (the REF of the GC-MS) was calculated (using the formula below).

[0267] Calculation formula: Area of ​​the analytical peak of the photopolymerization initiator / Area of ​​the measured peak of n-dodecane

[0268] 2. Measurement of reaction rate and photopolymerization initiator content of silicone encapsulant

[0269] [Calculation of reaction rate and photopolymerization initiator content of silicone encapsulant]

[0270] (1) Dry films of each photosensitive resin composition (white solder resist composition) were laminated onto an FR-4Cu film using a vacuum laminator (CVP-300: manufactured by Nikko Materials Co., Ltd.) in the first chamber at 60°C under conditions of a vacuum pressure of 3 hPa and a vacuum time of 10 seconds, and the PET film was peeled off.

[0271] Using a DI exposure system manufactured by Screen, the integrated light meter measured 300 mJ / cm². 2 To achieve this, a Kodak step tablet N0.2 (41 steps) was used as a photomask and exposed to 23 steps. The material was then developed with a 1.0% Na2CO3 aqueous solution at 30°C under a spray pressure of 0.2 MPa for 60 seconds, and cured in a 150°C oven for 60 minutes to obtain a cured photosensitive resin layer (solder resist layer).

[0272] After fabricating a dam with a width of 2.0 cm, a length of 2.0 cm, and a thickness of 250 to 300 μm, the dam was attached to both ends of the cured product of the photosensitive resin layer on the FR-4Cu film. A 1:1 mixture of silicone encapsulants A and B was added to the space formed by the dam, and a silicone encapsulant layer with a thickness of 250 to 300 μm was laminated. Thereafter, the encapsulant was cured in an oven at 100°C for 2 hours to complete primary curing, and then cured in an oven at 150°C for 4 hours to complete secondary curing of the encapsulant. After the secondary curing was completed, the interface between the cured product of the photosensitive resin layer and the silicone encapsulant layer was peeled off using a cutter knife. Then, using FT-IR equipment, the reaction rates of the upper encapsulant region and the lower encapsulant region of the silicone encapsulant layer were measured on a ZnSe crystal plate, and the degree of cure of the silicone encapsulant in the silicone encapsulant layer was measured.

[0273] [Method for calculating silicone reaction rate]

[0274] 1) Samples (upper and lower) of the silicone that had not been subjected to the above primary and secondary curing and the silicone that had been cured up to the secondary curing were prepared.

[0275] 2) The uncured silicone and the cured silicone were placed on a ZnSe crystal plate, and FT-IR measurement was performed.

[0276] 3) The uncured silicone was used as a reference (REF), and the Si-H peak of the cured silicone and the vicinity of 2160 cm -1 ) were compared to calculate the reaction rate (using the calculation formula below).

[0277] Calculation formula: (Height of Si-H peak of cured silicone / Height of Si-H peak of uncured silicone) × 100

[0278] (2) In addition, the content of the photopolymerization initiator was measured using the silicone encapsulant peeled off with a cutter knife by a gel permeation chromatography analysis method.

[0279] Specifically, 0.05 g of a sample peeled off with a cutter knife from the silicon encapsulant layer formed on the cured photosensitive resin layer was prepared as an analysis sample of the secondary final-cured silicon encapsulant. After 0.05 g of the analysis sample was dissolved in 10.0 g of THF, the vial was filled. In order to dissolve the undissolved photosensitive resin composition in the solution, it was dissolved for 5 minutes using an ultrasonic vibrator to prepare a sample. Thereafter, 100 μl of the sample was injected into a gel permeation chromatography (GPC) apparatus to complete the analysis.

[0280] [Calculation of content of photopolymerization initiator transferred to protective film]

[0281] After a PF protective film was attached on the secondary-cured silicon encapsulant, it was left at a temperature of 40° C. and a humidity of 90% for 24 hours. Thereafter, after peeling off the PF protective film, 0.05 g of a sample peeled off with a cutter knife from the silicon encapsulant layer formed on the cured photosensitive resin layer was prepared as a PF protective film analysis sample. After 0.05 g of the analysis sample was dissolved in 5.0 g of tetrahydrofuran (THF), the vial was filled. In order to dissolve the undissolved photosensitive resin composition in the solution, it was dissolved for 5 minutes using an ultrasonic vibrator to prepare a sample. Thereafter, 100 μl of the sample was injected into a gel permeation chromatography (GPC) apparatus to complete the analysis.

[0282] [Measurement method and measurement conditions of gel permeation chromatography (GPC) for photopolymerization initiator content analysis]

[0283] Gel permeation chromatography equipment name: E2695 separation module by water, detector: 2998PDA / 2414 RI, flow rate: 0.5 ml / min, columns: 2 HSP gel HR MB-L columns, 1 HSP gel HR column, measurement temperature: 4°C, mobile phase: THF. The sampled specimen was injected into the GPC equipment. For the calculation method, the analysis was carried out by quantifying the peak at 382 nm, which is the absorption wavelength of TPO as a photopolymerization initiator. TPO was used as the sampled analytical specimen and the REF photopolymerization initiator sample. A calibration curve was obtained by performing the same procedure on specimens containing 1, 10, and 100 ppm TPO. Using the calibration curve results obtained at each concentration, the amount of photopolymerization initiator contained in the sample was quantified.

[0284] (Evaluation of outgas content)

[0285] ◎: Outgas content <500 ppm ○: 500 ppm ≤ outgas content <1,000 ppm △: 1,000 ppm ≤ outgas content <2,000 ppm ×: 2,000 ppm ≤ outgas content

[0286] (Evaluation of reaction rate of the upper silicone encapsulant) ◎: 70% ≤ reaction rate of the upper silicone encapsulant ○: 55% ≤ reaction rate of the upper silicone encapsulant <70% △: 40% ≤ reaction rate of the upper silicone encapsulant <55% ×: reaction rate of the upper silicone encapsulant <40%

[0287] (Evaluation of reaction rate of the lower silicone encapsulant)

[0288] ◎: 50% ≤ reaction rate of the upper silicone encapsulant ○: 40% ≤ reaction rate of the lower silicone encapsulant <50% △: 30% ≤ reaction rate of the upper silicone encapsulant <40% ×: reaction rate of the upper silicone encapsulant <30%

[0289] (Content of photopolymerization initiator transferred to the encapsulant)

[0290] ◎: Photopolymerization initiator content <300 ppm ○: 300 ppm ≤ Photopolymerization initiator content < 500 ppm △: 500 ppm ≤ Photopolymerization initiator content < 700 ppm ×: 700 ppm ≤ Photopolymerization initiator content

[0291] [Table 2]

[0292] Referring to Table 2, it can be seen that the outgassing content of Examples 1 to 10, which contain photopolymerization initiator 1 or 2, is significantly lower than that of Comparative Examples 1 to 4, 6, and 7. This significantly reduced photopolymerization initiator outgassing improves the yellowing of the silicone encapsulant, thereby greatly increasing the reaction rate of the silicone encapsulant. Furthermore, the reduced content of photopolymerization initiator transferred to the silicone encapsulant improves the long-term reliability and stability of the product.

[0293] As shown in Comparative Examples 1-4, 6, and 7, when TPO is used as a photopolymerization initiator, it can be confirmed that the TPO, as a photopolymerization initiator, is transferred to and remains on the silicone encapsulant at a content of 700 ppm or more. This can lead to a decrease in the reflectivity and reaction rate of the silicone encapsulant, as described herein, and may impair the long-term reliability of the product.

[0294] On the other hand, when Omnipol TP alone is used as a photopolymerization initiator, as in Examples 1 and 2, the amount of outgassing of the photopolymerization initiator and the amount of photopolymerization initiator transferred to the silicon encapsulant are significantly reduced. This allows for the maintenance of high reflectivity, an increase in the reaction rate of the encapsulant region, and improved long-term reliability and stability of the product.

[0295] Also, as in Examples 3 to 10, when Omnirad TPO L is used as a photopolymerization initiator, the amount of outgas and the content of the photopolymerization initiator transferred to the silicon encapsulant are significantly reduced, thereby exhibiting effects of maintaining high reflectance, increasing the reaction rate of the encapsulant region, and improving long-term reliability and stability of the product.

[0296] Next, a protective film (PF) is formed on the silicon encapsulant, and after holding at 40°C / 90% humidity for 24 hours, only the protective film is peeled off, and the content of the photopolymerization initiator transferred to the protective film is measured using gel permeation chromatography, and the results are shown in Table 3 below.

[0297] (Evaluation of photopolymerization initiator content)

[0298] ◎: Photopolymerization initiator content <500 ppm ○: 500 ppm ≤ Photopolymerization initiator content <2,000 ppm △: 2,000 ppm ≤ Photopolymerization initiator content <4,000 ppm ×: 4,000 ppm ≤ Photopolymerization initiator content

[0299] [Table 3]

[0300] Referring to Table 3 in conjunction with Table 2, it can be seen that the outgassing content of Examples 1-10 containing photopolymerization initiator 1 or 2 is significantly lower than that of Comparative Examples 1-4, 6, and 7 containing other photopolymerization initiators. This indicates a significant reduction in the amount of photopolymerization initiator transferred to the protective film as well as the silicone encapsulant. Specifically, in Examples 1-10, the transfer of photopolymerization initiator to the protective film (PF) is significantly reduced compared to Comparative Examples 1-4, 6, and 7. This is because using the photopolymerization initiators represented by chemical formulas 1 and 2 reduces outgassing, preventing the transfer of photopolymerization initiator to the silicone encapsulant and protective film. As a result, using the photopolymerization initiators defined in this invention increases reflectivity, improves the reaction rate and curing degree of the silicone encapsulant, and enhances long-term reliability.

[0301] Evaluation Example 2: BHAST Test

[0302] The dry films prepared in Examples 3 and 4 and Comparative Examples 1 to 4 were laminated onto a substrate with comb-shaped electrodes (line / space = 50 μm / 50 μm) using a vacuum laminator (CVP-300: Nikko Materials Co., Ltd.) in the first chamber at 60°C under conditions of vacuum pressure of 3 hPa and vacuum time of 10 seconds. After lamination, the substrates were pressed under conditions of press pressure of 0.2 MPa and press time of 10 seconds to obtain evaluation substrates. After peeling off the PET film, the substrates were exposed using a DI exposure machine (Screen Inc.) to an exposure level that yielded 23 steps on a step tablet (41 steps), followed by development (1 mass% Na2CO3, 30°C, 0.2 MPa) for 60 seconds to complete substrate preparation. After completing substrate preparation, BHAST was performed at a temperature of 110°C, humidity of 85%, and 20 V in the chamber for 250 hours to evaluate insulation reliability, BHAST resistance, reflectivity, etc.

[0303] The BHAST test results are shown in Figures 1A and 1B.

[0304] Next, the reflectance was measured after the BHAST test and is shown in Table 4 below. The reflectance was measured at a wavelength of 450 nm using a spectrophotometer (CM-2600d, Konica Minolta Sensing, Inc.).

[0305] ◎:90%≦Reflectance ○:87%≦Reflectance<90% △:84%≦Reflectance<87% ×:Reflectance<84%

[0306] Furthermore, a HAST resistance test was conducted, and the results are shown in Table 4 below.

[0307] On a substrate on which comb-shaped electrodes (line / space = 50 μm / 50 μm) were formed, the dry films prepared in each example and comparative example were laminated using a vacuum laminator (CVP-300: manufactured by Nikko Materials Co., Ltd.) in the first chamber at 60°C under conditions of a vacuum pressure of 3 hPa and a vacuum time of 10 seconds. The substrates were then pressed under conditions of a press pressure of 0.2 MPa and a press time of 10 seconds to obtain evaluation substrates.

[0308] After peeling off the PET film, the integrated light meter measured 300 mJ / cm². 2 A dry film cured coating was formed by exposing the material to light, developing it with a 1% Na2CO3 aqueous solution at 30°C under a spray pressure of 0.2 MPa for 60 seconds, and curing it in a 150°C oven for 60 minutes, thereby creating a HAST evaluation substrate. This evaluation substrate was placed in a high-temperature, high-humidity chamber at 110°C and 85% humidity, charged with a voltage of 20V, and subjected to a 250-hour in-chamber HAST (Highly Accelerated Stress Test) test. After 250 hours, the discoloration and elution of the dry film cured coating were evaluated according to the following criteria (equipment manufacturer: Espec, Ion Migration System, Equipment name: NY IM1064).

[0309] ○: No peeling, discoloration, or leaching occurs. ×: Peeling, discoloration, or leaching are frequently observed with the naked eye.

[0310] [Table 4]

[0311] Referring to Table 4, it can be confirmed that Examples 3 and 4 have higher reflectivity after the HAST test compared to Comparative Examples 1-4. Furthermore, it can be confirmed that Examples 3 and 4 have higher reflectivity after the HAST test compared to Comparative Examples 1-4, and that the degree of copper oxidation and corrosion is very low, with no peeling, discoloration, or leaching phenomena.

[0312] Evaluation Example 3: Reflectance Test (After Reflow and UV Treatment)

[0313] The dry films prepared in Examples 1-4 and Comparative Examples 1-7 were laminated onto copper substrates using a vacuum laminator (CVP-300: manufactured by Nikko Materials Co., Ltd.) in the first chamber at 60°C under conditions of a vacuum pressure of 3 hPa and a vacuum time of 10 seconds. Then, they were pressed under conditions of a press pressure of 0.2 MPa and a press time of 10 seconds.

[0314] After peeling off the PET film, exposure was performed using a Screen DI exposure system, measuring 300 mJ / cm² with an integrated light meter. 2 To achieve this, a Kodak Step Tablet N0.2 (41 steps) was used as a photomask to expose the substrate to 23 steps. The substrate was then developed with a 1% Na2CO3 aqueous solution at 30°C under a spray pressure of 0.2 MPa for 60 seconds, and cured in a 150°C oven for 60 minutes to obtain the substrate. The reflectance at a wavelength of 450 nm was measured on the surface of the coating film of the obtained substrate using a spectrophotometer (CM-2600d, Konica Minolta Sensing, Inc.). Reflow galvanizing was performed 1 to 3 times at 260°C for 10 seconds each time, and the reflectance was measured. The results are shown in Table 5. In addition, after final curing, UV light was applied at 500 mJ / cm using an integrated light meter. 2 The test was conducted three times under the specified conditions, and the reflectance was measured for each test. The results are shown in Table 6.

[0315] ◎:90%≦Reflectance ○:87%≦Reflectance<90% △:84%≦Reflectance<87% ×:Reflectance<84%

[0316] [Table 5]

[0317] In Examples 1-4, the reflectance at 450 nm was higher than in Comparative Examples 1-7, not only in the initial reflectance without reflow, but also after 1, 2, and 3 reflows, and after firing following 1 reflow. This confirmed that there was little decrease in reflectance after reflow or firing.

[0318] In particular, in Examples 1 to 4, by using Omnipol TP or Omnirad TPO-L as the photopolymerization initiator, the amount of outgassing is reduced, minimizing the impact on the silicone encapsulant, and thus the firing process can be omitted. As a result, high reflectivity can be maintained even after reflow.

[0319] However, in Comparative Examples 1-7, when applied to backlight unit products, the TPO photopolymerization initiator affects the curing properties with the silicone encapsulant, so a firing process to remove the TPO must be performed after the reflow process. Furthermore, it can be confirmed that the reflectivity decreases significantly when the firing process is performed.

[0320] In short, compared to Comparative Examples 1-7, Examples 1-4 exhibit superior reflectivity, being at or above the same level as that applied to actual products. Furthermore, as explained in Table 2 above, they demonstrate superior reaction rate and curing degree of the silicone encapsulant, thereby improving the long-term reliability and stability of the product.

[0321] [Table 6] JPEG0007955485000014.jpg51170

[0322] The reflectance at 450 nm in Examples 1-4 showed a higher initial reflectance compared to Comparative Examples 1-6, and a similar trend was observed even after three UV treatments at 500 mJ. After three UV treatments, the reflectance of Examples 1-4 was 90.2-90.6, while Comparative Examples 1-4 showed a reflectance of 73-89.7 after three UV treatments, which is likely due to more severe yellowing.

[0323] Evaluation Example 4: Test in a chamber at 85°C and 85% humidity, reflectance test in an HS chamber.

[0324] The dry films prepared in Examples 2-4 and Comparative Example 1 were laminated in a first chamber at 60°C under the conditions of a vacuum pressure of 3 hPa and a vacuum time of 10 seconds using a vacuum laminator (CVP-300: manufactured by Nikko Materials Co., Ltd.). After lamination, the films were pressed under the conditions of a press pressure of 0.2 MPa and a press time of 10 seconds to obtain evaluation substrates.

[0325] After peeling off the PET film, the integrated light meter measured 300 mJ / cm². 2 The substrate was exposed to light, developed with a 1% Na2CO3 aqueous solution at 30°C under a spray pressure of 0.2 MPa for 60 seconds, and cured in a 150°C oven for 60 minutes to obtain a substrate. The obtained substrate was placed in a chamber (ETAC's HIFLEX, Temperature and Humidity Chamber) at a temperature of 85°C and 85% humidity and left for 1000 hours. The reflectance at a wavelength of 450 nm was measured on the substrate after 1000 hours in the HS chamber using a spectrophotometer (CM-2600d, Konica Minolta Sensing, Inc.). The results are shown in Table 7.

[0326] ◎:90%≦Reflectance ○:87%≦Reflectance<90% △:84%≦Reflectance<87% ×:Reflectance<84%

[0327] [Table 7]

[0328] Examples 2-4 confirmed that the reflectance at 450 nm decreased minimally even when evaluated over a long period under high temperature and high humidity conditions.

[0329] On the other hand, in Examples 2 to 4, the b-value after evaluation under high temperature and high humidity conditions was smaller than that of Comparative Example 1. This indicates that less yellowing occurred in Examples 2 to 4 under high temperature and high humidity conditions compared to Comparative Example 1. Since less yellowing occurs in Examples 2 to 4 even under harsh high temperature and high humidity conditions compared to Comparative Example 1, they can be used more effectively as materials for backlight units.

[0330] Evaluation Example 5: General Physical Property Evaluation

[0331] <Fabrication of evaluation board>

[0332] The photosensitive resin compositions prepared in each example and comparative example were laminated onto a PET film substrate using a vacuum laminator (CVP-300: manufactured by Nikko Materials Co., Ltd.) in the first chamber at 60°C under conditions of a vacuum pressure of 3 hPa and a vacuum time of 10 seconds. Then, the substrates were pressed under conditions of a press pressure of 0.2 MPa and a press time of 10 seconds to obtain evaluation substrates. After peeling off the PET film, the substrates were exposed to light at 300 mJ / cm² using a DI exposure apparatus manufactured by Screen Inc., with an integrated light meter. 2 To achieve this, a Kodak Step Tablet N0.2 (41 steps) was used as a photomask to expose the sample to 23 steps. The sample was then developed with a 1% Na2CO3 aqueous solution at 30°C under a spray pressure of 0.2 MPa for 60 seconds, and finally cured in a 150°C oven to produce the substrate.

[0333] <Pencil hardness>

[0334] Using the aforementioned substrate, pencils ranging from B to 9H, which had their tips polished to be flattened, were pressed at an angle of approximately 45°, and the hardness of the pencils that did not cause peeling of the coating was recorded.

[0335] <Adhesion>

[0336] A 1mm grid (10x10) was created on the substrate, and transparent adhesive tape was completely attached to the grid. Immediately, one end of the tape was held perpendicular to the substrate and peeled off instantaneously. The number of grid cells that remained without being completely removed was counted. The number of remaining grid cells was used as the numerator, and the total number of grid cells (100) was used as the denominator to record the results.

[0337] PASS: More than 95% of the grid pattern remains. NG: Less than 95% of the grid pattern remains visible.

[0338] <Gloss evaluation>

[0339] The gloss of the coating surface of the substrate was measured at an angle of 60° using a gloss colorimeter (BYK E-4430).

[0340] <Solder heat resistance>

[0341] The aforementioned substrate was immersed in a solder bath at 288°C for 10 seconds. A grid of 1 mm squares (10 x 10) was then created on the substrate. Transparent adhesive tape was completely adhered to the grid, and immediately, one end of the tape was peeled off instantaneously while maintaining a right angle to the substrate. The number of grid squares that remained without being completely removed was counted. The result was recorded by using the number of remaining grid squares as the numerator and the total number of grid squares (100) as the denominator.

[0342] PASS: More than 95% of the grid pattern remains. NG: Less than 95% of the grid pattern remains visible.

[0343] [Table 8]

[0344] However, in Comparative Example 5, the low content of the photopolymerization initiator resulted in poor surface hardening, leading to a low pencil hardness of 3H, a significant decrease in gloss to 72, poor adhesion and solder heat resistance, and poor developability. In Comparative Example 6, the excessive content of the photopolymerization initiator resulted in good surface hardening, leading to excellent adhesion and solder heat resistance, but the increased hardening reduced developability, making it unsuitable for SRO formation. Example 7 showed improved pencil hardness to 6H, and significantly improved adhesion and solder heat resistance, as did Example 8.

[0345] Evaluation Example 6: Analysis of Phosphorus Content in Photosensitive Resin Compositions

[0346] 1) 0.1 g each of the photosensitive resin compositions from Examples 1-8 and Comparative Examples 1-6 was accurately weighed and placed in a beaker. 2 mL of nitric acid was added, and the mixture was heated on a hot plate to allow the reaction to proceed. 2) The sample was temporarily removed from the hot plate and, while cooling to room temperature, 0.03 mL of hydrochloric acid was added at a time to allow the reaction to proceed. 3) A small amount of the nitric acid solution of the sample was left without completely evaporating, and after cooling to room temperature, 1 mL of concentrated nitric acid was added to completely dissolve the sample. After the sample was completely dissolved, it was diluted with ultrapure water. 4) Using ICP-OES analysis equipment (Optima series, Perkin Elmer), the phosphorus (P) concentration for the above examples and comparative examples was analyzed under conditions of wavelengths of 213.617 nm and 214.914 nm.

[0347] [Table 9]

[0348] The compositions of Examples 1-8 and Comparative Examples 1-4 were found to contain approximately 3,000 ppm of phosphorus. Comparative Example 5 did not use a photopolymerization initiator containing phosphorus, so its phosphorus content was found to be low, at approximately 430 ppm. Comparative Example 6 was found to contain 5,500 ppm of phosphorus.

Claims

1. (A) Carboxyl group-containing resin that does not contain aromatic rings, (B) Inorganic fillers, (C) Mercapto-modified (meth)acrylate, and (E) Photopolymerization initiator A photosensitive resin composition comprising, The (E) photopolymerization initiator includes a photopolymerization initiator which is a trimethylbenzoylphosphine oxide group-containing compound containing one or more P-O bonds, and an oxime ester-based photopolymerization initiator. The total content of the photopolymerization initiator, which is a trimethylbenzoylphosphine oxide group-containing compound having one or more P-O bonds, and the oxime ester-based photopolymerization initiator is 0.01 to 3.26% by weight of the total weight of the photosensitive resin composition. The aforementioned photosensitive resin composition.

2. The photopolymerization initiator, which is (E) a trimethylbenzoylphosphine oxide group-containing compound having one or more P-O bonds, is *-C(=O)-P(=O)R 1 -O-*'Moieti (here, R 1 The photosensitive resin composition according to claim 1, comprising: an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, or a cyclic group having 5 to 20 carbon atoms.

3. The photopolymerization initiator, which is (E) a trimethylbenzoylphosphine oxide group-containing compound containing one or more P-O bonds, is a trimethylbenzoylphosphine oxide group-containing polymer, according to claim 1, the photosensitive resin composition.

4. The aforementioned trimethylbenzoylphosphine oxide group-containing polymer has a weight-average molecular weight (M n The photosensitive resin composition according to claim 3, wherein the content of ) is 900 g / mol or more.

5. The photosensitive resin composition according to claim 3, wherein the trimethylbenzoylphosphine oxide group-containing polymer is represented by the following chemical formula 1. 【Chemistry 1】 a=0-100, b=0-100, c=0-100

6. The photopolymerization initiator, which is a trimethylbenzoylphosphine oxide group-containing compound having one or more P-O bonds, comprises an alkoxy group, according to claim 1, the photosensitive resin composition.

7. The photopolymerization initiator, which is a trimethylbenzoylphosphine oxide group-containing compound having one or more P-O bonds, comprises an ethoxy group, as described in claim 1.

8. The photopolymerization initiator described in (E), which is a trimethylbenzoylphosphine oxide group-containing compound having one or more P-O bonds, is represented by the following chemical formula 2, the photosensitive resin composition according to claim 1. 【Chemistry 2】

9. The photosensitive resin composition according to claim 1, wherein the content of (E) a photopolymerization initiator which is a trimethylbenzoylphosphine oxide group-containing compound having one or more P-O bonds is 0.01 to 10% by weight of the total weight of the composition.

10. The photosensitive resin composition according to claim 1, wherein the carboxyl group-containing resin that does not contain an aromatic ring (A) contains an unsaturated double bond.

11. (D) The photosensitive resin composition according to claim 1, further comprising a resin containing an aromatic ring.

12. The photosensitive resin composition according to claim 11, wherein the resin containing the aromatic ring (D) is a melamine resin, a silicone resin, or a resin having a styrene skeleton.

13. (F) The photosensitive resin composition according to claim 1, further comprising a silane coupling agent.

14. (G) The photosensitive resin composition according to claim 1, further comprising a resin having a urethane bond.

15. The photosensitive resin composition according to claim 1, wherein the outgassing content of the photosensitive resin composition, as measured by thermal desorption spectroscopy (TDS) and gas chromatography-mass spectrometry (GC-MS), is 1,000 ppm or less relative to the content of a photopolymerization initiator which is a trimethylbenzoylphosphine oxide group-containing compound having one or more P-O bonds.

16. The photosensitive resin composition according to claim 1, wherein the phosphorus content is 500 to 5000 ppm.

17. A dry film having a photosensitive resin layer obtained by coating and drying a photosensitive resin composition according to any one of claims 1 to 16 on a first film.

18. A cured product obtained by curing the photosensitive resin layer of a photosensitive resin composition according to any one of claims 1 to 16 or a dry film obtained thereby.

19. A printed circuit board comprising the cured product according to claim 18 as a solder resist.

20. The printed wiring substrate according to claim 19, further comprising a silicon encapsulant layer disposed on the solder resist.

21. The aforementioned silicone encapsulant layer includes an upper encapsulant region and a lower encapsulant region. The printed wiring substrate according to claim 20, wherein the content of a photopolymerization initiator which is (E) a trimethylbenzoylphosphine oxide group-containing compound containing one or more P-O bonds, contained in at least one of the upper sealing material region or the lower sealing material region, is 1,000 ppm or less relative to the content of a photopolymerization initiator which is a trimethylbenzoylphosphine oxide group-containing compound containing one or more P-O bonds, contained in the solder resist.

22. The cured product according to claim 18, and A laminate including a protective film.

23. The laminate according to claim 22, wherein the amount of (E) a photopolymerization initiator which is a trimethylbenzoylphosphine oxide group-containing compound containing one or more P-O bonds contained in the protective film is 1,000 ppm or less relative to the amount of (E) a photopolymerization initiator which is a trimethylbenzoylphosphine oxide group-containing compound containing one or more P-O bonds contained in the solder resist.

24. The photosensitive resin composition according to claim 1, wherein the photopolymerization initiator, which is a trimethylbenzoylphosphine oxide group-containing compound having one or more P-O bonds, is liquid at room temperature (20°C) and 1 atm.

Citation Information

Patent Citations

  • Photocurable / thermosetting resin composition and dry film, and printed wiring board using the same

    JP2009169416A

  • Photocurable resin composition, cured product of the same and printed wiring board

    JP2015028588A

  • Polyfunctional Acylphosphine Oxide Photoinitiator

    JP2017522364A

  • Solder resist composition, dry film, printed wiring board, and manufacturing method thereof

    JP2024500726A

  • CURABLE RESIN COMPOSITION, LAMINATE, CURED PRODUCT, AND ELECTRONIC COMPONENT

    JP2024535244A