Dielectric film activator, semiconductor substrate and semiconductor device manufactured using the same

The dielectric film activator addresses the issue of residual carbon impurities by replacing precursor ligands with hydrogen iodide or bromide, enhancing film density and properties.

JP7955492B2Active Publication Date: 2026-11-24SOULBRAIN CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2025518923
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-10-06
Filing Date
2023-10-06
Publication Date
2026-11-24
Estimated Expiration
2043-10-06

AI Technical Summary

Technical Problem

The presence of residual carbon compound impurities from precursors and reaction gases in dielectric films leads to a reduction in dielectric constant and disrupts the crystal arrangement, necessitating a solution to increase thin-film density and capacitance.

Method used

A dielectric film activator replaces the first ligand of a precursor adsorbed on a substrate with a second ligand, promoting reactions with post-injection gases and reducing residual carbon compound impurities, using hydrogen iodide or hydrogen bromide as activators.

Benefits of technology

This process enhances dielectric film density, improves uniformity, and reduces corrosion and degradation, resulting in high-quality dielectric films with improved dielectric properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955492000017
    Figure 0007955492000017
  • Figure 0007955492000018
    Figure 0007955492000018
  • Figure 0007955492000019
    Figure 0007955492000019
Patent Text Reader

Abstract

The present invention relates to a dielectric film activator, and a semiconductor substrate and a semiconductor device manufactured using the same. According to the present invention, by using a dielectric film activator that can reduce the amount of carbon compounds by-produced by a precursor and a reaction gas mixed into a dielectric film and provide an effect of increasing the density of the thin film, the capacitance of the dielectric film can be improved and an effect of increasing the density of the thin film can be provided through a simple process.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a dielectric film activator, a semiconductor substrate and a semiconductor device manufactured using the same, and more particularly to a dielectric film activator that can reduce residual carbon compound impurities of precursors and reaction gases mixed into the dielectric film, thereby improving capacitance and providing an effect of increasing thin film density, and to a semiconductor substrate and a semiconductor device manufactured using the same. [Background technology]

[0002] A dielectric is an insulator that does not conduct electricity but becomes polar in an electric field. Dielectrics play a very important role in semiconductor devices.

[0003] For example, in a capacitor, the material that actually stores electricity is the dielectric.

[0004] On the other hand, when by-product carbon compounds from the precursor and reaction gas are mixed into a high-dielectric material (high-k) with a high dielectric constant, it can result in a very large capacitance difference.

[0005] The content of residual carbon compound impurities, including impurities from the precursor and reaction gas mixed into the dielectric film, is a factor that affects the dielectric properties and chemical properties. This can lead to problems such as a reduction in the dielectric constant, or a decrease in the dielectric constant due to the absorption of by-products such as HCl and hydrocarbons derived from the leaving group of the halogen ligand, which contaminates the dielectric film or disrupts the crystal arrangement of the dielectric film.

[0006] For this reason, there is a current need for dielectric film activators that can increase the dielectric constant by increasing the thin film density while reducing the content of residual carbon compound impurities, including precursors and reaction gases, that are mixed into the dielectric. There is also a need for the manufacturing of dielectric films utilizing these activators, and the development of semiconductor substrates and semiconductor devices manufactured from them.

[0007] [Prior art documents] [Patent Documents]

[0008] [Patent Document 1] U.S. Patent Publication No. 2020 / 0316645 (Publication Date: October 8, 2020) [Overview of the project] [Problems that the invention aims to solve]

[0009] To solve the problems of the conventional technology described above, the present invention aims to provide a high-quality dielectric film with increased capacitance and thin-film density, as well as a semiconductor substrate and semiconductor device containing the dielectric film, by activating a precursor adsorbed on a substrate using a dielectric film activator of a predetermined structure, thereby preventing the contamination of the dielectric film with by-product carbon compounds from the reaction gas between the precursor and the reaction gas.

[0010] The above-mentioned and other objectives of the present invention can all be achieved by the present invention as described below. [Means for solving the problem]

[0011] To achieve the above objective, the present invention provides a dielectric film activator characterized by replacing a first ligand directly attached to the central metal of a precursor adsorbed on a substrate with a second ligand contained in the dielectric film activator, thereby providing an activated substrate-adsorbed precursor.

[0012] The central metal of the precursor may, for example, be a Group 4 element.

[0013] The central metal of the precursor may, in specific examples, be Hf or Zr.

[0014] The precursor molecules adsorbed onto the substrate can be selected from one or more structures represented by the following chemical formula 1 and the following chemical formula 2.

[0015] [Chemical Formula 1]

[0016] [Chemical formula]

[0017] (In the above Chemical Formula 1, M is Zr or Hf, R1 is independently hydrogen or an alkyl group having 1 to 4 carbon atoms, n is an integer of 0 to 5, X'1, X'2, and X'3 are independently selected from -NR'1R'2, -OR'3, Cl, or F, and R'1 to R'3 are independently hydrogen or an alkyl group having 1 to 6 carbon atoms.)

[0018] [Chemical Formula 2]

[0019] [Chemical formula]

[0020] (In the above Chemical Formula 2, M is Zr or Hf, X1 and X2 are independently -NR1R2, -OR3, Cl, or F, R1 to R3 are independently hydrogen or an alkyl group having 1 to 6 carbon atoms, Y is an alkyl group having 1 to 6 carbon atoms, and n is 1 or 2.)

[0021] The precursor molecules adsorbed on the substrate may have a structure in which four types of ligands independently selected from -NR'1R'2, -OR'3, Cl, or F are bonded to a central metal. Here, the central metal may be Zr or Hf, and R'1 to R'3 may independently be hydrogen or an alkyl group having 1 to 6 carbon atoms.

[0022] The first ligand and the second ligand may each independently contain a halogen, a halogen and oxygen, or carbon and hydrogen simultaneously, or may contain nitrogen and carbon simultaneously.

[0023] The first ligand is a ligand of chemical formula 1 or chemical formula 2 described above, and the ligand of the precursor adsorbed on the substrate includes, in addition to this, one or more selected from chlorine, fluorine, and bromine, and the dielectric film activator may include one or more halogens selected from iodine and bromine.

[0024] The dielectric film activator may be hydrogen iodide (HI), hydrogen bromide (HBr), or a mixed gas obtained by mixing these with an inert gas in a mole fraction of 1 to 99.

[0025]

[0026] The activated substrate adsorbed precursor promotes the reaction with the pre-injected or post-injected reaction gas, which is injected before the precursor, and is characterized by a reduction in the content of residual carbon compound impurities.

[0027] The reduction in the content of residual carbon compound impurities may include a decrease in the content of by-product carbon-oxygenated impurities generated by the binding of the precursor desorption ligand to the reactant, and a decrease in the content of carbon compound impurities that have not been desorbed from the precursor.

[0028] The reduction in the content of the undesorbed carbon compound impurities may be due to the replacement of the ligand of the precursor adsorbed on the substrate with the dielectric film activator contained in the dielectric film activator.

[0029] The reaction gas may be one or more selected from H2O, H2O2, N2O, NO2, O2, O3, and O radicals.

[0030]

[0031] The adsorption state of the precursor before ligand exchange can be represented by the following chemical formula 3-1, and the adsorption state of the precursor after ligand exchange can be represented by the following chemical formula 3-2.

[0032] [Chemical formula 3-1]

[0033] [ka]

[0034] (In the above chemical formula 3-1, M is Hf or Zr, n is an integer from 1 to 4, and X is the ligand species of chemical formula 1, chemical formula 2, F, or Cl, which can be different from each other.)

[0035] [Chemical formula 3-2]

[0036] [ka]

[0037] (In the chemical formula 3-2 above, M is either Hf or Zr, M is an integer between 1 and 4, and Y is either Br or I.)

[0038]

[0039] The substrate may be a silicon wafer having -H or -OH terminal groups, an insulating film, or a dielectric film.

[0040] The dielectric film may be a vapor-deposited film.

[0041] Here, the deposition method may be atomic layer deposition (ALD), plasma-enhanced atomic layer deposition (PEALD), vapor deposition (CVD), plasma-enhanced vapor deposition (PECVD), metal-organic vapor deposition (MOCVD), or low-pressure vapor deposition (LPCVD).

[0042]

[0043] Furthermore, the present invention includes a substrate and a dielectric film.

[0044] The present invention provides a semiconductor substrate characterized in that the dielectric film is a film deposited using the aforementioned dielectric film activator.

[0045] The dielectric film may have a multilayer structure of two or more layers.

[0046] The dielectric film may have a deposition rate of 0.5 Å / cycle or higher, as measured on SiO2 or Si (based on a thin film deposited at 300°C).

[0047] ( The dielectric film has a thin film density of 9.8 g / cm³ measured on SiO2 or Si. 3 It could be any of the above.

[0048] The dielectric film may have a carbon impurity content of 1000 counts / second (counts / s) or less, as measured by SIMS (based on a thin film deposited at 300°C) on SiO2 or Si.

[0049] Furthermore, the present invention provides a semiconductor device including the aforementioned semiconductor substrate. [Effects of the Invention]

[0050] According to the present invention, the reaction with the post-injection reaction gas is promoted by the activated substrate adsorption precursor, and a dielectric film activator is provided that can reduce the content of residual carbon compound impurities.

[0051] Specifically, this process improves the density of the dielectric film and further reduces process by-products, preventing corrosion and degradation, and improving the dielectric properties of the dielectric film.

[0052] Furthermore, it is possible to improve the uniformity of the dielectric film thickness, and also to provide a method for manufacturing a dielectric film using this method, a semiconductor substrate manufactured therefrom, and a semiconductor device. [Brief explanation of the drawing]

[0053] [Figure 1] This figure compares the growth rates at different deposition temperatures of the dielectric film in Example 1, which uses a dielectric film activator according to the present invention, with the growth rates at different deposition temperatures of the dielectric film in Comparative Example 1, which does not use a dielectric film activator.

[0054] [Figure 2] This graph shows the C impurity content in the dielectric film of Additional Example 1, which uses a dielectric film activator according to the present invention, as determined by SIMS analysis.

[0055] [Figure 3] This graph shows the C impurity content in the dielectric film of an additional comparative example 1, which did not use a dielectric film activator, as determined by SIMS analysis.

[0056] [Modes for carrying out the invention]

[0057] The dielectric film activator described herein, and the semiconductor substrates and semiconductor devices manufactured using it, will be described in detail below.

[0058]

[0059] The present inventors have found that when forming a dielectric film using a dielectric film activator capable of increasing thin film density while reducing the content of by-product carbon-oxygenated impurities generated by the binding of precursor desorption ligands and reactants mixed into the dielectric film, as well as the content of carbon compound impurities that have not been desorbed from the precursor, the density is improved, corrosion and degradation are prevented, the dielectric properties of the dielectric film are improved, and the uniformity of the dielectric film thickness is improved, resulting in a high-quality dielectric film. Based on this finding, the inventors incorporated this knowledge into their research on dielectric films and completed the present invention.

[0060]

[0061] The following provides a detailed explanation of dielectric film activators, semiconductor substrates containing dielectric films manufactured using them, and semiconductor devices.

[0062]

[0063] In this description, the dielectric film activator is a substance that activates the precursor adsorbed on the substrate in the present invention, thereby promoting the reaction with the post-injection reaction gas by the activated substrate-adsorbed precursor, and also reduces the inclusion of residual carbon compound impurities into the dielectric film.

[0064] The central metal of the precursor adsorbed onto the aforementioned substrate is a Group 4 element, and the ligand may contain two or more halogens that are identical or different from each other and be adsorbed onto the substrate.

[0065] The central metal may preferably be Hf or Zr.

[0066] The precursor compound used to form a dielectric film in the present invention is a group 4 metal consisting of Hf and Zr, and may be Hf(NMe2)4, Zr(NMe2)4, CpZr(CpZr(NMe2)3), CpHf(CpHf(NMe2)3), and derivatives thereof with Hf and Zr as the central metal, and may be a linear or cyclic precursor molecule in which ligands bound to the central metal are linked.

[0067]

[0068] The precursor molecules adsorbed on the substrate can be represented, for example, by the following chemical formulas 1 and 2.

[0069] [Chemical formula 1]

[0070] [ka]

[0071] (In the above chemical formula 1, M is Zr or Hf, R1 is independently hydrogen or an alkyl group having 1 to 4 carbon atoms, n is an integer from 0 to 5, X'1, X'2 and X'3 are independently selected from -NR'1R'2 or -OR'3, Cl, or F, and R'1 to R'3 are independently hydrogen or an alkyl group having 1 to 6 carbon atoms.)

[0072] [Chemical formula 2]

[0073] [ka]

[0074] (In the above chemical formula 2, M is Zr or Hf, X1 and X2 are independently -NR1R2 or -OR3, Cl, or F, R1 to R3 are independently hydrogen or an alkyl group having 1 to 6 carbon atoms, Y is an alkyl group having 1 to 6 carbon atoms, and n is 1 or 2.)

[0075] In the case of a precursor molecule having a transition metal as the central metal atom (M) and one or more ligands consisting of C, N, O, H, and X (halogen), and whose vapor pressure at 25°C is 1 mTorr to 100 Torr, the effect of ligand substitution with the dielectric film activator described later can be maximized.

[0076]

[0077] Furthermore, taking zirconium precursor compounds as an example, tris(dimethylamide)cyclopentadienylzirconium (CpZr(NMe2)3), (methyl-3-cyclopentadienylpropylamino)bis(dimethylamino)zirconium (Cp(CH2)3NM3Zr(NMe2)2), and tetrakis(ethylmethylamide)zirconium ([(Me)(Et)N]4Zr) can be used, and in this case, they can be appropriately filled with dielectric film activators as described later.

[0078] Taking hafnium precursor compounds as an example, tris(dimethylamide)cyclopentadienylhafnium (CpHf(NMe2)3), (methyl-3-cyclopentadienylpropylamino)bis(dimethylamino)hafnium (Cp(CH2)3NM3Hf(NMe2)2), and tetrakis(ethylmethylamide)hafnium ([(Me)(Et)N]4Hf) can be used, and in this case, they can be appropriately filled with the dielectric film activator described above.

[0079] In the present invention, the precursor compound may, for example, be mixed with a nonpolar solvent and introduced into the chamber. In this case, there is the advantage that the viscosity and vapor pressure of the precursor compound can be easily adjusted.

[0080] The nonpolar solvent is preferably one or more selected from the group consisting of alkanes and cycloalkanes. In this case, the solvent contains an organic solvent with low reactivity and solubility, which makes it easy to control moisture content, while still improving the thin film density (step coverage) even when the deposition temperature is increased during dielectric film formation. This has the advantage.

[0081] As a more preferred example, the nonpolar solvent is C1-C 10 Alkanes or C3~C 10 It may contain cycloalkanes, preferably C3-C3. 10 It is a cycloalkane, which has the advantage of being less reactive and less soluble, making it easier to manage moisture levels.

[0082] In this description, C1, C3, etc., refer to the number of carbon atoms.

[0083] The cycloalkane is preferably C3-C 10 It may be a monocycloalkane, and among the said monocycloalkanes, cyclopentane is liquid at room temperature and has the highest vapor pressure, making it suitable for the vapor deposition process, but it is not limited to this.

[0084] The aforementioned nonpolar solvent, for example, has a solubility in water (at 25°C) of 200 mg / L or less, preferably 50 to 400 mg / L, and more preferably 135 to 175 mg / L. Within this range, it has the advantage of low reactivity with the precursor compound and easy moisture control.

[0085] In this description, solubility is not particularly limited to measurement methods or standards commonly used in the art to which the present invention pertains; for example, a saturated solution may be measured by high-performance liquid chromatography (HPLC).

[0086] The nonpolar solvent may preferably be present in an amount of 5 to 95% by weight, more preferably 10 to 90% by weight, even more preferably 40 to 90% by weight, and most preferably 70 to 90% by weight, relative to the total weight of the precursor compound and the nonpolar solvent combined.

[0087] If the nonpolar solvent is added in such a way that its content exceeds the upper limit, it will cause impurities, increasing the resistance and the value of impurities in the dielectric film. Conversely, if the organic solvent is added in such a way that its content falls below the lower limit, there is a drawback in that the effect of improving the thin film density and reducing impurities such as chloride (Cl) ions due to the addition of the solvent is not obtained to a great extent.

[0088]

[0089] The first ligand and the second ligand may independently contain a halogen, a halogen and oxygen, or carbon and hydrogen, or nitrogen and carbon.

[0090] The first ligand is a ligand of chemical formula 1 or chemical formula 2 described above, and the ligand of the precursor adsorbed on the substrate includes, in addition to this, one or more selected from chlorine, fluorine, and bromine, and the dielectric film activator may include one or more halogens selected from iodine and bromine.

[0091] The dielectric film activator may be hydrogen iodide (HI), hydrogen bromide (HBr), or a mixed gas obtained by mixing these with an inert gas in a mole fraction of 1 to 99.

[0092]

[0093] A material having a structure in which the aforementioned ligands are bound to these central metals can be used as a precursor adsorbed onto a substrate. Here, the precursor can be obtained by activating it with the dielectric film activator described above and adsorbing it onto the activated substrate.

[0094] The activated substrate adsorption precursor promotes the reaction with the post-injection reaction gas and reduces the content of residual carbon compound impurities.

[0095] Here, the decrease in the content of residual carbon compound impurities may include a decrease in the content of by-product carbon-oxygenated impurities generated by the binding of the precursor desorption ligand to the reactant, and a decrease in the content of carbon compound impurities that have not been desorbed from the precursor.

[0096] Specifically, the reduction in the content of undesorbed carbon compound impurities may be due to the replacement of the ligand of the precursor adsorbed on the substrate with the dielectric film activator contained in the dielectric film activator.

[0097]

[0098] The adsorption state of the precursor before ligand exchange can be represented by the following chemical formula 3-1, and the adsorption state of the precursor after ligand exchange can be represented by the following chemical formula 3-2.

[0099] [Chemical formula 3-1]

[0100] [ka]

[0101] (In the above chemical formula 3-1, M is Hf or Zr, n is an integer from 1 to 4, and X is the ligand species of chemical formula 1, chemical formula 2, F, or Cl, which can be different from each other.)

[0102] [Chemical formula 3-2]

[0103] [ka]

[0104] (In the chemical formula 3-2 above, M is either Hf or Zr, M is an integer between 1 and 4, and Y is either Br or I.)

[0105] For example, if the precursor adsorbed on the substrate is CpHf(NMe2)3, the precursor structure adsorbed on the substrate activated by the dielectric film activator is the above chemical formula 3-1(substrate-MX n In this equation, M is Hf, and the X molecules, which may be different from each other, can be one Cp ligand and two NMe2 ligands.

[0106]

[0107] The substrate may be a silicon wafer having -H or -OH terminal groups, an insulating film, or a dielectric film.

[0108] The ligand of the precursor adsorbed onto the substrate may, for example, be a ligand species having the structure represented by the above chemical formula 1 or 2, or it may be F or C.

[0109] The ligand of the precursor adsorbed on the substrate may, as other examples, be independently selected from -NR'1R'2 or -OR'3, Cl, or F, where R'1 to R'3 may independently be hydrogen or an alkyl group having 1 to 6 carbon atoms.

[0110]

[0111] When the precursor adsorbed on the substrate contains one or more halogens selected from chlorine, fluorine, nitrogen compounds, and carbon compounds, nitrogen compounds and carbon compounds are preferable to chlorine and fluorine in reacting with iodine-based and bromine-based activators.

[0112] As a specific example, the dielectric film activator may be hydrogen iodide (HI), hydrogen bromide (HBr), or a mixed gas obtained by mixing these with an inert gas in a mole fraction of 1 to 99.

[0113] Furthermore, the dielectric film activator may be an iodine donor, an iodine ion, or an iodine radical, and from the perspective of smooth ligand exchange, it is preferable that it be a substance represented by the above structure.

[0114] In such cases, suppressing side reactions reduces process by-products within the dielectric film, thereby reducing corrosion and degradation. This also controls the growth rate of the thin film, ensures that the metal oxide film reaches a stoichiometric oxidation state during formation, and significantly improves the uniformity of the dielectric film thickness.

[0115] As a specific example, the dielectric film activator is a mixture of pure hydrogen iodide of 3N to 15N purity, a mixture of 1 to 99% by weight of hydrogen iodide of 3N to 15N purity and an inert gas residue so that the total amount is 100% by weight, or an aqueous solution mixture of 0.5 to 70% by weight of hydrogen iodide of 3N to 15N purity and an inert gas residue so that the total amount is 100% by weight. Here, when the inert gas is nitrogen, helium, or argon with a purity of 4N to 9N, the effect of reducing process by-products is significant, the thin film density is excellent, and the effect of improving the thin film density and the electrical properties of the thin film are even more outstanding.

[0116] Preferably, the dielectric film activator is a gas mixture of 5N to 6N pure hydrogen iodide, 1 to 99% by weight of 5N to 6N hydrogen iodide and an inert gas residue so that the total amount is 100% by weight, or an aqueous solution mixture of 0.5 to 70% by weight of 5N to 6N hydrogen iodide and an inert gas residue so that the total amount is 100% by weight, where the inert gas may be nitrogen, helium, or argon having a purity of 4N to 9N. In this case, side reactions are suppressed, the growth rate of the thin film is adjusted, process by-products in the thin film are reduced, corrosion and degradation are reduced, the crystallinity of the thin film is improved, and even when forming a thin film on a substrate with a complex structure, the thin film density (step coverage) and the uniformity of the thin film thickness can be greatly improved.

[0117]

[0118] The dielectric film activator is preferably a compound with a purity of 99.9% or higher, a compound with a purity of 99.95% or higher, or a compound with a purity of 99.99% or higher. For reference, if a compound with a purity of less than 99% is used, there is a risk that impurities may remain in the dielectric film or cause side reactions with precursors or reactants, so it is best to use a substance with a purity of 99% or higher whenever possible.

[0119] The vapor pressure can be 1 atmosphere at 180-240K, and within this range, the transfer of substances into the chamber proceeds smoothly, resulting in outstanding improvements in dielectric film thickness uniformity, dielectric properties, and film quality.

[0120] In the present invention, the dielectric film activator may be injected in a gaseous state, and the precursor compound, described later, may be injected after vaporization and then subjected to plasma post-treatment. In this case, the growth rate of the dielectric film can be improved while reducing process by-products.

[0121]

[0122] The thin film (including the dielectric film) may be a vapor-deposited film.

[0123] The deposition method may be atomic layer deposition (ALD), plasma-enhanced atomic layer deposition (PEALD), vapor deposition (CVD), plasma-enhanced vapor deposition (PECVD), metal-organic vapor deposition (MOCVD), or low-pressure vapor deposition (LPCVD).

[0124]

[0125] The reaction gas may be one or more selected from H2O, H2O2, N2O, NO2, O2, O3, and O radicals.

[0126]

[0127] The dielectric film can be manufactured by a wide variety of methods, and as an example, it can be manufactured by the following method:

[0128] In the first step, a precursor compound having a ligand containing an alkyl, alkylamine, or halogen, a halogen and oxygen, or carbon and hydrogen, or nitrogen and carbon simultaneously, can be injected onto a substrate placed in a chamber.

[0129] The ligand can be selected from one or more alkyls, alkylamines, chlorine, and fluorine, and preferably contains an alkylamine with excellent reactivity.

[0130] The aforementioned structure containing both carbon and hydrogen may, for example, be a cyclopentadienyl (Cp) group.

[0131] In this description, possible methods for distributing the precursor compound throughout the deposition chamber include, as an example, a method utilizing a gas phase mass flow controller (MFC) to transport the volatile gas (Vapor Flow Control; VFC), a mass flow controller method including a liquid phase mass flow controller (LMFC), and a liquid delivery system (LDS).

[0132] In this case, one or more gases selected from the group consisting of argon (Ar), nitrogen (N2), and helium (He) can be used as a carrier gas or diluent gas for moving the precursor compound onto the substrate, but the present invention is not limited thereto.

[0133] In this description, as an example, an inert gas can be used as the purge gas, and preferably, the carrier gas or diluent gas can be used.

[0134] The chamber may be an atomic layer deposition (ALD) chamber, a plasma-enhanced atomic layer deposition (PEALD) chamber, a vapor deposition (CVD) chamber, a plasma-enhanced vapor deposition (PECVD) chamber, an organometallic vapor deposition (MOCVD) chamber, or a low-pressure vapor deposition (LPCVD) chamber.

[0135] The substrates brought into the chamber may include semiconductor substrates such as silicon substrates and silicon oxides.

[0136] The substrate may have a conductive layer or an insulating layer further formed on its upper surface.

[0137] The substrate can be maintained at 50-500°C or 80-500°C.

[0138] The substrate may be heated to, for example, 50-500°C, specifically to 80-500°C, 100-800°C, or 200-500°C. The dielectric film activator or precursor compound may be injected onto the substrate either while unheated or while heated. Depending on the deposition efficiency, the injection may be performed while unheated, and the heating conditions may be adjusted during the deposition process. For example, it may be injected onto the substrate for 1-20 seconds under temperature conditions of 50-500°C.

[0139] The amount (mg / cycle) of the precursor compound to be introduced into the chamber is, for example, 1:1 to 1:100, preferably 1:1 to 1:50, and more preferably 1:1 to 1:25, in which case the ratio of the amount (mg / cycle) of the dielectric film activator used in the second step described later to the amount of the precursor compound introduced into the chamber is 1:1 to 1:100, preferably 1:1 to 1:50, and more preferably 1:1 to 1:25. Within this range, the effect of improving thin film density and reducing process by-products is outstanding.

[0140]

[0141] The first step may include one or more purging steps using an inert gas. The carrier gas or diluent gas described above can be used as the inert gas.

[0142] The amount of purge gas introduced into the chamber in the step of purging the unadsorbed precursor compound is not particularly limited as long as it is sufficient to remove the unadsorbed precursor compound. For example, it may be 10 to 100,000 times the volume of the precursor compound introduced into the chamber, preferably 50 to 50,000 times, and more preferably 100 to 10,000 times. Within this range, the unadsorbed precursor compound can be sufficiently removed to form a uniform dielectric film and prevent deterioration of the film quality. Here, the amounts of purge gas and precursor compound introduced are based on one cycle, and the volume of the precursor compound refers to the volume of vaporized precursor compound vapor.

[0143] In this description, the purging is preferably 1,000 to 50,000 sccm (Standard Cubic Centimeters per Minute), more preferably 2,000 to 30,000 sccm, and even more preferably 2,500 to 15,000 sccm. Within this range, the thin film growth rate per cycle is appropriately controlled, and deposition is performed as a single atomic layer (atomic mono-layer) or approximately thereof, which has the advantage of being advantageous in terms of film quality.

[0144]

[0145] In the second step, a dielectric film activator is injected into the substrate to replace the leaving groups of the precursor adsorbed on the substrate with halogens of the activator. In this case, by effectively replacing the leaving groups of the precursor adsorbed on the substrate with halogens of the activator and forming a thin film without gaps in the crystal lattice, the thin film density is improved, and the dielectric properties and thickness uniformity of the thin film are significantly enhanced.

[0146] The halogen can be selected from, for example, one or more from iodine and bromine, and it is preferable to use iodine.

[0147] The feeding time (seconds) for supplying the dielectric film activator to the surface of the substrate is preferably 0.01 to 10 seconds, more preferably 0.02 to 3 seconds, even more preferably 0.04 to 2 seconds, and most preferably 0.05 to 1 second per cycle. Within this range, there are advantages such as a low thin film growth rate, excellent thin film density, and high economic efficiency.

[0148] In this description, the supply rate of the dielectric film activator is based on a flow rate of 1 to 300 sccm / cycle for a chamber volume of 15 to 20 L, and more specifically, on a flow rate of 10 to 100 sccm / cycle for a chamber volume of 18 L.

[0149] In this description, one possible method for distributing the dielectric film activator throughout the deposition chamber is to use a gas-phase mass flow controller (MFC) method to transport the gas.

[0150] The second step may include one or more purging steps using an inert gas. In this description, the carrier gas or diluent gas may be used as the purging gas, for example.

[0151] In this description, the purging is preferably 1,000 to 50,000 sccm (Standard Cubic Centimeter per Minute), more preferably 2,000 to 30,000 sccm, and even more preferably 2,500 to 15,000 sccm. Within this range, the thin film growth rate per cycle is appropriately controlled, and deposition is performed as a single atomic layer (atomic mono-layer) or approximately thereof, which is advantageous in terms of film quality.

[0152] The amount of purge gas introduced into the chamber in the step of purging the unadsorbed dielectric film activator is not particularly limited as long as it is sufficient to remove the unadsorbed dielectric film activator. For example, it may be 10 to 100,000 times, preferably 50 to 50,000 times, and more preferably 100 to 10,000 times. Within this range, the unadsorbed dielectric film activator can be sufficiently removed to form a uniform thin film and prevent deterioration of the film quality. Here, the amounts of purge gas and dielectric film activator introduced are based on one cycle, and the volume of dielectric film activator refers to the volume of vaporized dielectric film activator vapor.

[0153]

[0154] As a specific example, in the step of injecting the vapor deposition packing material under conditions of a flow rate of 100 sccm and an injection time of 0.5 sec (per cycle), and purging the unadsorbed vapor deposition packing material, if the purge gas is injected under conditions of a flow rate of 3000 sccm and an injection time of 5 sec (per cycle), the amount of purge gas injected is 300 times the amount of vapor deposition packing material injected.

[0155]

[0156] Next, in the third step, a reaction gas can be injected into the substrate to form a thin film in which heteroatoms are bonded to a transition metal.

[0157] The reaction gas may, for example, be one or more selected from H2O, H2O2, N2O, NO2, O2, O3, and O radicals.

[0158] The thin film may include a structure in which a halogen is directly bonded to a Group IV metal.

[0159] The dielectric film formation method can, for example, be carried out at an evaporation temperature in the range of 50 to 800°C, preferably in the range of 100 to 700°C, more preferably in the range of 200 to 650°C, and even more preferably in the range of 220 to 500°C. Within this range, it is possible to grow a thin film with excellent film quality while achieving process characteristics.

[0160] The dielectric film formation method can be carried out, for example, at a deposition pressure in the range of 0.01 to 20 Torr, preferably in the range of 0.1 to 20 Torr, more preferably in the range of 0.1 to 10 Torr, and most preferably in the range of 0.3 to 7 Torr. Within this range, a thin film with a uniform thickness can be obtained.

[0161] In this description, the deposition temperature and deposition pressure may be measured as the temperature and pressure formed within the deposition chamber, or as the temperature and pressure applied to the substrate within the deposition chamber.

[0162] The second step may preferably further include raising the temperature inside the chamber to the deposition temperature before introducing the dielectric film activator into the chamber, and / or purging the chamber by injecting an inert gas into the chamber before introducing the dielectric film activator into the chamber.

[0163] The third step may include a purging step using an inert gas.

[0164] Furthermore, in the purging step performed immediately after the reaction gas supply step, the amount of purge gas introduced into the chamber may, for example, be 10 to 10,000 times the volume of reaction gas introduced into the chamber, preferably 50 to 50,000 times, and more preferably 100 to 10,000 times, and within this range, the desired effect can be sufficiently obtained. Here, the amounts of purge gas and reaction gas introduced are based on one cycle each.

[0165] In this description, the purging is preferably 1,000 to 50,000 sccm (Standard Cubic Centimeter per Minute), more preferably 2,000 to 30,000 sccm, and even more preferably 2,500 to 15,000 sccm. Within this range, the thin film growth rate per cycle is appropriately controlled, and deposition is performed as a single atomic layer (atomic mono-layer) or approximately thereof, which is advantageous from the perspective of film quality.

[0166]

[0167] The dielectric film formation method can be carried out by repeating the unit cycle 1 to 99,999 times as needed, preferably 10 to 10,000 times, more preferably 50 to 5,000 times, and even more preferably 100 to 2,000 times. Within this range, it is possible to reduce the content of by-product carbon compounds and improve the thin film density while obtaining the desired thin film thickness.

[0168]

[0169] As a specific example of the method for manufacturing the dielectric film, in order to deposit the dielectric film onto a substrate located in the deposition chamber, the above-mentioned dielectric film activator and a precursor compound or a mixture thereof with a nonpolar solvent are prepared.

[0170] Subsequently, the precursor compound or a mixture thereof with a nonpolar solvent is injected into the evaporator, converted into a vapor phase, spread throughout the deposition chamber, and adsorbed onto the substrate. The unadsorbed precursor compound is then purged while replacing the ligand of the precursor compound with a dielectric film activator.

[0171] Next, the prepared dielectric film activator is injected into the evaporator, then transformed into a vapor phase and spread throughout the deposition chamber to adsorb onto the substrate. Finally, it is purged to remove any unadsorbed dielectric film activator.

[0172] In this description, one possible method for distributing dielectric film activators and precursor compounds into the deposition chamber is to use a gas-phase mass flow controller (MFC) method to transport the gas.

[0173] In this process, one or more gases selected from the group consisting of argon (Ar), nitrogen (N2), and helium (He) can be used as the carrier gas or diluent gas for moving the dielectric film activator and precursor compound onto the substrate, but there are no limitations to this.

[0174] In this description, as an example, an inert gas can be used as the purge gas, and preferably, the carrier gas or diluent gas can be used.

[0175] Next, a heteroatom-containing gas is supplied. The heteroatom-containing gas is not particularly limited, and is a reaction gas commonly used in the art to which the present invention belongs; preferably, it may contain an oxidizing agent. The oxidizing agent reacts with the precursor compound adsorbed on the substrate to form an oxide film.

[0176] Preferably, the oxidizing agent may be oxygen gas (O2), ozone gas (O3), or a mixture of nitrogen gas and oxygen gas.

[0177] Next, an inert gas is used to purge unreacted residual reactants. This allows not only excess reactants but also generated by-products to be removed together.

[0178] As described above, the method for forming the dielectric film includes, as an example, the steps of: adsorbing a precursor compound onto a substrate; purging the unadsorbed precursor compound; supplying a dielectric film activator onto the substrate; purging the unadsorbed dielectric film activator; supplying a reaction gas; and purging the residual reaction gas. These steps constitute a unit cycle, and the unit cycle may be repeatedly performed to form a dielectric film having a desired thickness.

[0179] As an example, the unit cycle may be repeated 1 to 99,999 times, preferably 10 to 1,000 times, more preferably 50 to 5,000 times, and even more preferably 100 to 2,000 times. Within this range, there is an effect that the desired properties of the dielectric film are favorably exhibited.

[0180]

[0181] When the injection time and purge time of the precursor compound in the first and second steps are denoted as a and b, respectively, the injection time and purge time of the alkyl-free halide in the second step are denoted as c and d, respectively, and the injection time and purge time of the heteroatom-containing gas in the third step are denoted as e and f, respectively, the following conditions may be simultaneously satisfied: 0.1≦a≦10, 2a≦b≦4a, 0.1<c≦10, 2c≦d≦8c, 2<e≦10, and 2e≦b≦8e.

[0182]

[0183] When the injection and purge of the precursor compound and the dielectric film activator, as well as the injection and purge of the heteroatom-containing gas, are defined as one cycle, the following two conditions are met: 1) the deposition rate of the dielectric film on SiO2 is 1 Å / cycle or more, and 2) the density of the dielectric film is 9.8 g / cm 3Both of the above conditions can be met.

[0184] When the injection and purging of the precursor compound and dielectric film activator, and the injection and purging of the heteroatom-containing gas are considered as one cycle, the following two conditions must be met: 1) The deposition rate of the dielectric film onto SiO2 is 1 to 2 Å / cycle, and 2) The density of the dielectric film is 9.8 to 10.5 g / cm³. 3 It is possible to satisfy both conditions.

[0185] The dielectric film manufacturing method can, as an example, be carried out using a dielectric film manufacturing apparatus that includes an ALD chamber, a corrosion-resistant mass flow controller (MFC) including a gold seal for quantitatively introducing a dielectric film activator, a first transport means for transporting the quantitatively introduced dielectric film activator into the ALD chamber, a second evaporator for vaporizing a precursor adsorbed on a substrate, and a second transport means for transporting the vaporized precursor adsorbed on the substrate into the ALD chamber. Here, the evaporator and transport means are not particularly limited as long as they are evaporators and transport means commonly used in the art to which the present invention belongs.

[0186]

[0187] This includes a thin film deposited using the aforementioned dielectric film activator.

[0188] The thin film may be a dielectric film.

[0189] The thin film may have a multilayer structure of two or more layers.

[0190] As an example, the thin film can be obtained by the reaction of an activated substrate adsorption precursor represented by the structure of chemical formula 1 with a reaction gas. In this case, the use of an activated substrate adsorption precursor can reduce the content of by-product carbon compounds, thereby enabling the production of a high-quality thin film.

[0191] The reduction of byproduct carbon compounds between the precursor adsorbed on the activated substrate and the reaction gas may be attributed, for example, to the fact that the activation energy of the precursor adsorbed on the activated substrate is lower than the activation energy of the precursor adsorbed on the substrate.

[0192]

[0193] The dielectric film may have a deposition rate measured by an ellipsometer on SiO2 or Si (based on a thin film deposited at 300°C) of 1.0 Å / cycle or more, or 1.0 to 2.0 Å / cycle, within which thin film uniformity and deposition productivity can be improved.

[0194] The dielectric film may have a thin film density measured on SiO2 or Si of 9.5 g / cm 3 or more, 9.8 g / cm 3 or more, or 9.8 to 10.3 g / cm 3 , within which dielectric properties can be improved.

[0195] The dielectric film may have a carbon impurity content measured by SIMS on SiO2 or Si (based on a thin film deposited at 300°C) of 1000 counts / s or less, 715 counts / s or less, or 700 counts / s or less, within which electron leakage is significantly reduced, thereby improving dielectric properties.

[0196] The dielectric film may have an iodine atom content measured by SIMS of 50 counts / s or more, or 65 counts / s or more, within which the thin film density is increased to provide the effect of increasing the dielectric constant.

[0197] The dielectric film may have a deposition thickness of 410 counts / s or less, or 300 counts / s or less, as measured by SIMS (based on a thin film deposited at 400°C) on SiO2 or Si. Within this range, electron leakage is significantly reduced, thereby improving dielectric properties.

[0198] The dielectric film may contain the aforementioned film composition alone or in a selective area, but the present invention is not limited thereto and encompasses Si, SiH, SiOH, and SiO2 as well.

[0199] The aforementioned dielectric film can be used in semiconductor devices not only for DRAMs, which are typically used, but also as a dielectric film or insulating film for NAND or logic elements.

[0200] The dielectric film may, for example, contain a halogen compound measured using SIMS at a count of 30,000 counts / s or less.

[0201]

[0202] Furthermore, the present invention provides a semiconductor substrate, characterized in that the semiconductor substrate is manufactured by the dielectric film formation method described herein or contains the dielectric film, and in such a case, the thin film density (step coverage) and thickness uniformity of the dielectric film are significantly superior, and moreover, the density characteristics and dielectric properties of the dielectric film are also excellent.

[0203]

[0204] The manufactured dielectric film preferably has a deposition rate of 1 Å / cycle or more on SiO2 and a density of 9.8 g / cm³. 3 Within the above range, it exhibits excellent performance as a diffusion-blocking film, and in particular, it has the effect of improving dielectric properties, but the present invention is not limited in any way thereto.

[0205] Here, the impurity halogens remaining in the dielectric film are, for example, Cl2, Cl, or Cl - This is possible, and the lower the residual amount of halogen in the dielectric film, the better the film quality, making it preferable.

[0206] Furthermore, the lower the carbon content remaining in the dielectric film, the better the dielectric properties, making it preferable.

[0207]

[0208] The dielectric film may, as an example, be a multilayer structure of two or more layers, a multilayer structure of three or more layers, or a multilayer structure of two or three layers, as needed. The two-layer multilayer film may, as a specific example, have a lower layer-middle layer structure, and the three-layer multilayer film may, as a specific example, have a lower layer-middle layer-upper layer structure.

[0209] The aforementioned underlayer film may, for example, consist of one or more elements selected from the group consisting of Si, SiO2, MgO, Al2O3, CaO, ZrSiO4, ZrO2, HfSiO4, Y2O3, HfO2, LaLuO2, Si3N4, SrO, La2O3, Ta2O5, BaO, and TiO2.

[0210] The aforementioned intermediate layer is, as an example, Ti x N y Preferably, it may include TN.

[0211] The aforementioned upper layer may, for example, consist of one or more elements selected from the group consisting of W and Mo.

[0212]

[0213] According to the present invention, a semiconductor device including the aforementioned semiconductor substrate can be provided.

[0214] The semiconductor device may, for example, be a low-resistive metal gate interconnect, a high-aspect-ratio 3D metal-insulator-metal (MIM) capacitor, a DRAM trench capacitor, a 3D gate-all-around (GAA) device, or a 3D NAND flash memory.

[0215]

[0216] The following examples and drawings are provided to further the understanding of the present invention. However, these examples and drawings are merely illustrative of the present invention, and it will be obvious to those skilled in the art that a wide variety of changes and modifications can be made within the scope of the present invention and the technical concept. It goes without saying that such modifications and changes also fall within the scope of the attached claims.

[0217]

[0218] [Examples]

[0219] As precursor compounds, we prepared a compound having the structure represented by the following chemical formula 1-1 and a compound having the structure represented by the following chemical formula 4.

[0220] [Chemical Formula 1-1] (Cyclopentadienyl ligand precursor)

[0221] [ka]

[0222] [Chemical Formula 4] (Alkylamine ligand precursor)

[0223] [ka]

[0224] As the dielectric film activator, 5N HI was prepared.

[0225] Using the aforementioned precursor compound and dielectric film activator, the ALD process was performed with the deposition process sequence according to the present invention as one cycle.

[0226]

[0227] The specific experimental methods for Example 1, Example 2, and Comparative Examples 1 and 2 are as follows.

[0228] Example 1

[0229] The precursor compound represented by chemical formula 1-1 was placed in a canister maintained at 25°C and supplied at room temperature to a separate evaporator heated to 150°C at a flow rate of 0.05 g / min using an LMFC (Liquid Mass Flow Controller). After the precursor compound vaporized into the vapor phase in the evaporator was introduced into the deposition chamber for 1 second using a VFC (Vapor Mass Flow Controller), argon gas was supplied at 3000 sccm for 5 seconds to perform argon purging. At this time, the pressure in the reaction chamber was controlled to 2.5 Torr.

[0230] Next, 5N HI, used as a dielectric film activator, was placed in a canister and supplied to the chamber at room temperature using a Mass Flow Controller (MFC) at a rate of 100 sccm / cycle. After the dielectric film activator was introduced into the deposition chamber where the substrate had been loaded for 2 seconds, argon gas was supplied at 3000 sccm for 8 seconds to perform an argon purge. At this time, the pressure inside the reaction chamber was controlled to 2.5 Torr.

[0231] Next, 1000 sccm of ozone was introduced into the reaction chamber as a reactive gas for 3 seconds, followed by argon purging for 9 seconds. At this time, the substrate on which the dielectric film was to be formed was heated to 300°C, and SiO2 was formed on the upper part of the Si substrate.

[0232] This process was repeated 200 to 400 times to produce dielectric films at the deposition rates for different deposition temperatures shown in Figure 1 below.

[0233] As is clear from Figure 1 below, the dielectric films each had a deposition rate of 1.41 Å / cycle.

[0234]

[0235] Furthermore, the density of the dielectric film was measured using X-ray reflectance (XRR) equipment. The measured density was 9.83 g / cm³. 3 That was the case.

[0236]

[0237] Furthermore, the impurity content of the dielectric film was measured.

[0238] Here, the impurities are H-, C-, NH-, 18 O-, 30 Measurements were performed on elements such as Si- using secondary-ion mass spectrometry (SIMS).

[0239] Specifically, while ion sputtering penetrated the dielectric film axially, the value of the impurity was confirmed from the SIMS graph, taking into account the amount of impurity (counts) present in the substrate surface layer when the sputtering time was 50 seconds, minimizing contamination.

[0240] Among the confirmed SIMS results, the average carbon (C) impurity content in the dielectric film was calculated to be 694 counts / s. Furthermore, it was confirmed that the content of impurities remaining as process by-products, not just carbon, was reduced from 3340 counts / s to 2600 counts / s.

[0241]

[0242] Example 2

[0243] A precursor compound having the structure represented by the above chemical formula 4 was placed in a canister maintained at 25°C and supplied at room temperature at a flow rate of 0.05 g / min to a separate evaporator heated to 150°C using an LMFC (Liquid Mass Flow Controller). The precursor compound vaporized into the vapor phase in the evaporator was introduced into the deposition chamber for 1 second using a VFC (Vapor Flow Controller), and then argon purging was performed by supplying argon gas at 3000 sccm for 5 seconds. At this time, the pressure in the reaction chamber was controlled to 2.5 Torr.

[0244] Next, 5N HI was placed in a canister as a dielectric film activator and supplied to the chamber at room temperature using an MFC (Mass Flow Controller) at a rate of 100 sccm / cycle. After the dielectric film activator was introduced into the deposition chamber where the substrate had been loaded for 2 seconds, argon gas was supplied at 3000 sccm for 8 seconds to perform an argon purge. At this time, the pressure inside the reaction chamber was controlled to 2.5 Torr.

[0245] Next, 1000 sccm of ozone was introduced into the reaction chamber as a reactive gas for 3 seconds, followed by argon purging for 9 seconds. At this time, the substrate on which the dielectric film was to be formed was heated to 300°C, and SiO2 was formed on the upper part of the Si substrate.

[0246]

[0247] This process was repeated 200 to 400 times to produce dielectric films at different deposition rates depending on the deposition temperature. The dielectric film had a deposition rate of 1.46 Å / cycle.

[0248] Furthermore, the density of the dielectric film was measured using X-ray reflectance (XRR) equipment. The measured density was 10.08 g / cm³. 3 That was the case.

[0249]

[0250] Furthermore, the average carbon (C) impurity content within the dielectric film, measured using SIMS (Secondary-ion mass spectrometry), was calculated as 243 counts / s. It was also confirmed that the content of not only carbon but also residual hydrogen (H) impurities, which were residual process by-products, was reduced.

[0251]

[0252] Comparative Example 1

[0253] The same process as in Example 1 was repeated, except that the dielectric film was manufactured without using 5N HI, which was used as a dielectric film activator in Example 1. The measurement results are shown together in Figure 1 below.

[0254] As is clear from Figure 1 below, the rate of increase in the deposition rate of the dielectric film (D / R (dep. rate) increase rate) was 0.84 Å / cycle.

[0255] As a result, it was found that the defect rate was approximately 33% lower compared to Example 1.

[0256] Furthermore, the density of the dielectric film was measured using X-ray reflectance (XRR) equipment. The measured density was 9.71 g / cm³ on average. 3 The calculations show that it is inferior compared to Example 1.

[0257] Furthermore, the impurity content of the dielectric film was measured, and the carbon (C) impurity content in the dielectric film, confirmed using SIMS, was calculated to be 927 counts / s, indicating that it is approximately 33% worse than Example 1.

[0258]

[0259] Comparative Example 2

[0260] The same process as in Example 2 was repeated, except that the dielectric film was manufactured without using 5N HI, which was used as a dielectric film activator in Example 2. The measurement results are shown together in Figure 1 below.

[0261] The increase in the deposition rate of the dielectric film (D / R (dep. rate) increase rate) was 0.91 Å / cycle, which indicates that the defect rate is approximately 60% lower compared to Example 1.

[0262] Furthermore, the density of the dielectric film was measured using X-ray reflectance (XRR) equipment. The measured density was 10.08 g / cm³ on average. 3 The calculations show that it is inferior compared to Example 1.

[0263] Furthermore, the impurity content of the dielectric film was measured, and the carbon (C) impurity content in the dielectric film, confirmed using SIMS, was calculated to be 243 counts / s, indicating that it was approximately 42% worse than Example 1.

[0264]

[0265] From the above results, it was confirmed that, according to the present invention using a dielectric film activator having a predetermined structure, not only are the deposition thickness, deposition rate, and thin film density significantly improved compared to a comparative example in which no dielectric film activator was used, but the dielectric properties are also improved due to the superior impurity reduction characteristics.

[0266] In particular, Example 1 using the dielectric film activator of the present invention exhibited an increase rate of the deposition rate of the dielectric film per cycle and a density of the dielectric film of 10% or more, respectively, and a reduction rate of impurities of 60% or more, as compared with Comparative Example 1 in which the dielectric film was not used although the dielectric film was manufactured under a low temperature condition of 300° C. It was confirmed that excellent values were shown.

[0267]

[0268] Additional Example 1

[0269] A precursor (CpHf) was injected into a Si substrate at 300° C., an activator (HI) was injected, and a process of reacting with a reactant (O3) was repeatedly performed to obtain a thin film of about 13 nm. Using a SIMS (Secondary-ion mass spectrometry) analysis method, while digging into the thin film in the axial direction by ion sputtering, the content of C impurities (counts) when the sputtering time with little contamination in the skin layer of the substrate is 50 seconds was taken into consideration. As a result of checking the value of the C impurity, it was confirmed that it was about 700 counts / s as apparent from the graph of FIG. 2.

[0270]

[0271] Additional Comparative Example 1

[0272] A precursor (CpHf) was injected into a Si substrate at 300° C., and a process of reacting with a reactant (O3) was repeatedly performed to obtain a thin film of about 13 nm.

[0273] Using a SIMS (Secondary-ion mass spectrometry) analysis method, while digging into the thin film in the axial direction by ion sputtering, the content of C impurities (counts) when the sputtering time with little contamination in the skin layer of the substrate is 50 seconds was taken into consideration. As a result of checking the value of the C impurity, it was confirmed that it was about 1100 counts / s as apparent from the graph of FIG. 3.

[0274]

[0275] Therefore, when the predetermined compound is used as the dielectric film activator of the present invention, the rate of increase in dielectric film thickness and deposition rate, density, and dielectric properties are all improved, and the impurity reduction characteristics are also excellent. As a result, it was confirmed that dielectric films can be effectively formed even on substrates with complex patterns.

Claims

1. A dielectric film activator characterized by replacing a first ligand directly attached to the central metal of a precursor adsorbed on a substrate with a second ligand contained in the dielectric film activator, thereby providing an activated substrate-adsorbed precursor. The dielectric film activator is a mixture of hydrogen iodide (HI), hydrogen bromide (HBr), and a mixture of hydrogen iodide (HI) or hydrogen bromide (HBr) and an inert gas, and A dielectric film activator characterized in that the adsorption state of the precursor before ligand exchange is represented by the following chemical formula 3-1, and the adsorption state of the precursor after ligand exchange is represented by the following chemical formula 3-2. [Chemical formula 3-1] 【Chemistry 1】 (In the above chemical formula 3-1, M is Hf or Zr, n is an integer from 1 to 4, and X is a ligand species of chemical formula 1, chemical formula 2, F, or Cl, which may be different from each other.) [Chemical formula 3-2] 【Chemistry 2】 (In the above chemical formula 3-2, M is Hf or Zr, M is an integer from 1 to 4, and Y is Br or I.) [Chemical formula 1] 【Transformation 3】 (In the above chemical formula 1, M is Zr or Hf, R1 is independently hydrogen or an alkyl group having 1 to 4 carbon atoms, n is an integer from 0 to 5, X'1, X'2, and X'3 are independently selected from -NR'1 R'2 or -OR'3, Cl, or F, and R'1 to R'3 are independently hydrogen or an alkyl group having 1 to 6 carbon atoms.) [Chemical formula 2] 【Chemistry 4】 (In the above chemical formula 2, M is Zr or Hf, X1 and X2 are independently -NR1 R2 or -OR3, Cl, or F, R1 to R3 are independently hydrogen or an alkyl group having 1 to 6 carbon atoms, Y is an alkyl group having 1 to 6 carbon atoms, and n is 1 or 2.)

2. The dielectric film activator according to claim 1, characterized in that the precursor adsorbed on the substrate is selected from among the compounds represented by the following chemical formula 1 and the compounds represented by the following chemical formula 2: 【Transformation 5】 【Transformation 6】

3. The dielectric film activator according to claim 1, characterized in that the mixed gas is a mixture of hydrogen iodide (HI) or hydrogen bromide (HBr) and an inert gas in a mole fraction of 1:

99.

4. The dielectric film activator according to claim 1, characterized in that the activated substrate adsorbed precursor promotes the reaction with the pre-injected or post-injected reaction gas, which is injected before the precursor, and the content of residual carbon compound impurities is reduced.

5. The dielectric film activator according to claim 4, characterized in that the reduction in the content of residual carbon compound impurities includes a reduction in the content of by-product carbon-oxygenated impurities generated by the binding of the precursor desorption ligand to the reactant, and a reduction in the content of carbon compound impurities that have not been desorbed from the precursor.

6. The dielectric film activator according to claim 1, characterized in that the substrate is a silicon wafer having -H or -OH terminal groups, an insulating film, or a dielectric film.

7. The dielectric film activator according to claim 1, wherein the dielectric film is a deposited film, and the deposition includes atomic layer deposition (ALD), plasma-enhanced atomic layer deposition (PEALD), vapor deposition (CVD), plasma-enhanced vapor deposition (PECVD), organometallic chemical vapor deposition (MOCVD), or low-pressure vapor deposition (LPCVD).

8. Including a substrate and a dielectric film, The semiconductor substrate is characterized in that the dielectric film is a film deposited using the dielectric film activator described in claim 1.

9. The semiconductor substrate according to claim 8, characterized in that the dielectric film has a multilayer structure of two or more layers.

10. The dielectric film has a thin film density of 9.5 g / cm³ as measured on SiO₂ or Si. 3 The semiconductor substrate according to claim 8, characterized in that the carbon impurities measured by secondary ion mass spectrometry (SIMS) are 1000 counts / s or less, and the iodine atoms measured by secondary ion mass spectrometry (SIMS) are 50 counts / s or more.

11. A semiconductor device comprising the semiconductor substrate described in claim 8.

Citation Information

Patent Citations

  • Growth inhibitor for thin film formation, thin film forming method using the same, and semiconductor substrate manufactured by the same

    JP2021031766A

  • Precursor composition for forming metal film, method for forming metal film using the same, and semiconductor device including the metal film

    JP2022511849A

  • Growth regulator for forming thin film, method for forming thin film and semiconductor substrate prepared therefrom

    KR1020220009906A

  • Atomic layer deposited nanolaminates of HfO2 / ZrO2 films as gate dielectrics

    US20040023461A1

  • Atomic layer etching on microdevices and nanodevices

    US20200316645A1