Chemical mechanical polishing slurry composition and method for manufacturing semiconductor devices

A cerium oxide slurry with small particles and additives enhances oxide film removal rates and selectivity, addressing polishing speed and scratch issues in semiconductor manufacturing.

JP7955501B2Active Publication Date: 2026-11-24SOULBRAIN CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2025524310
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-10-28
Filing Date
2023-10-30
Publication Date
2026-11-24
Estimated Expiration
2043-10-30

AI Technical Summary

Technical Problem

Conventional cerium oxide slurry compositions face challenges in achieving high oxide film removal rates with small particle sizes while minimizing polishing scratches and optimizing the oxide/nitride film polishing selectivity ratio, leading to difficulties in maintaining polishing speed and surface planarization during semiconductor device manufacturing.

Method used

A slurry composition comprising cerium oxide particles with a size of 10 nanometers or smaller, combined with a cationic polymer and a nitride film passivation regulator, is used to enhance the polishing rate of oxide films and reduce nitride film polishing rates, achieving a high oxide film/nitride film polishing selectivity ratio.

Benefits of technology

The composition allows for increased oxide film removal rates and improved selectivity while minimizing surface defects, enabling finer pattern passivation and enhanced planarization in semiconductor manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955501000009
    Figure 0007955501000009
  • Figure 0007955501000010
    Figure 0007955501000010
  • Figure 0007955501000011
    Figure 0007955501000011
Patent Text Reader

Abstract

The present invention provides cerium oxide particles for chemical mechanical polishing (CMP) and a chemical mechanical polishing slurry composition containing the same. The present invention provides a chemical mechanical polishing slurry composition that maximizes the silicon oxide / nitride selectivity during a shallow trench isolation (STI) polishing process while improving the oxide film polishing rate by combining the characteristic cerium oxide particles with a cationic polymer and a nitride film passivation modifier. The present invention also provides a method for manufacturing a semiconductor device using the same.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a chemical mechanical polishing slurry composition containing cerium oxide particles and a method for manufacturing semiconductor devices, and more specifically, to the surface of cerium oxide obtained using a synthesis method different from that of existing cerium oxide particles. 3+ This invention relates to a chemical mechanical polishing slurry composition that increases the ratio of a component to achieve a high oxide film removal rate at low content despite small particle size, and in combination with appropriate additive components to reduce the polishing rate of the nitride film and passivate fine patterns, as well as a method for manufacturing semiconductor devices using the same. [Background technology]

[0002] The recent advancements in the diversification and high integration of semiconductor devices are remarkable, and consequently, even finer pattern formation techniques are being employed. This has led to increased complexity in the surface structure of semiconductor devices, making interlayer flatness in each process extremely important for improving the accuracy of photolithography. Chemical mechanical polishing (CMP) is used as such a planarization technique in the manufacturing of semiconductor devices. For example, it is widely used as a process to remove excess insulating film deposited for interlayer insulation, as well as for planarizing shallow trench isolation (STI) insulating films that provide insulation between the interlayer dielectronic film (ILD) and the chip, and for forming metallic conductive films such as wiring, contact plugs, and via contacts.

[0003] In the CMP (Chemical Polishing) process, polishing speed, surface planarization, and scratch generation are important factors, and these are determined by the CMP process conditions, slurry type, and polishing pad type. High-purity cerium oxide particles are used in cerium oxide slurry. Recently, in the manufacturing process of semiconductor devices, there is a demand for even greater miniaturization of wiring, and polishing scratches generated during polishing have become a concern.

[0004] Conventional cerium oxide slurry uses particles ranging in size from 30 nm to 200 nm. While this was not considered a problem if it resulted in minute polishing scratches, as long as they were smaller than the conventional wiring width, it is now a problem as we continue to achieve consistently high levels of wiring miniaturization. Attempts have been made to reduce the average particle size of cerium oxide particles to address this issue. However, with existing particles, reducing the average particle size leads to a decrease in mechanical action, resulting in a reduction in polishing speed.

[0005] Thus, even when attempting to control the polishing speed and polishing scratches by controlling the average particle size of cerium oxide particles, it is extremely difficult to achieve the target level of polishing scratches while maintaining the polishing speed.

[0006] Furthermore, in conventional chemical mechanical polishing slurry compositions, cerium oxide particles are Ce 3+ Ce 4+ We have not been able to optimize the ratio and present an optimized level of average particle size, and therefore, the Ce on the surface of cerium oxide 3+ Currently, there is a need for research into polishing slurries containing cerium oxide particles that exhibit a high oxide film removal rate despite their small particle size, by increasing the proportion of these particles.

[0007] Furthermore, regarding the CMP slurry containing cerium oxide particles under optimized conditions, research is needed on additive components for improvement from the viewpoint of oxide film polishing efficiency and oxide / nitride film polishing selectivity ratio.

[0008] As described above, the present inventors have developed cerium oxide particles of 10 nanometer or smaller grade, which are obtained by using precipitation in a solution and have a greatly improved polishing rate of an oxide film. By combining the cerium oxide particles under such optimized conditions with an additive substance, the present invention has been completed by developing a slurry composition that can both adjust the passivation of fine patterns on a nitride film and significantly improve the polishing rate of a silicon oxide film. [Summary of the Invention] [Problems to be Solved by the Invention]

[0009] The present invention was created to solve the above-mentioned problems, and one embodiment of the present invention provides a slurry composition for chemical mechanical polishing.

[0010] In addition, another embodiment of the present invention provides a method for manufacturing a semiconductor device.

[0011] The technical problem to be solved by the present invention is not limited to the above-mentioned technical problem, and other technical problems not mentioned should be clearly understood by a person having ordinary knowledge in the technical field to which the present invention belongs from the following description. [Means for Solving the Problems]

[0012] As a technical means for achieving the above technical problem, one aspect of the present invention is A slurry composition for chemical mechanical polishing, comprising cerium oxide particles, a solvent, a cationic polymer, and a nitride film passivation regulator, wherein in an aqueous dispersion in which the content of the cerium oxide particles is adjusted to 1.0% by weight, the average light transmittance for light with a wavelength in the range of 450 to 800 nm is 50% or more.

[0013] The cationic polymer may be characterized in that the polishing rate of the oxide film increases depending on the content.

[0014] The nitride film passivation modifier may be characterized by reducing the polishing rate of the nitride film depending on its content.

[0015] The content of the nitride film passivation modifier may be characterized by being 0.001 to 1% by weight relative to the total weight of the chemical mechanical polishing slurry composition.

[0016] The content of the cationic polymer may be characterized by being 0.001 to 1% by weight relative to the total weight of the chemical mechanical polishing slurry composition.

[0017] The cationic polymer may be characterized by being polydiallyldimethylammonium chloride (Poly(DADMAC)), polydiethylenetriamine 2-(dimethylamino)ethyl methacrylate (Poly(DMAEM)), poly 2-(dimethylamino)ethyl methacrylate (Poly(DMAEM)), polyacrylamide decamethylene diamine (Poly(Aam_DCDA)), poly(dimethylamine)-co-epichlorohydrin, poly(dimethylamine)-co-epichlorohydrin-co-ethylenediamine) or a combination thereof.

[0018] The chemical mechanical polishing slurry composition may be characterized by containing cerium oxide particles in an amount of 0.001 to 5% by weight relative to the total weight of the chemical mechanical polishing slurry composition.

[0019] The nitride film passivation modifier may be characterized by being sugars, amino acids, amine-based substances, or a combination thereof.

[0020] The nitride film passivation modifier may be characterized by being a substance from the group consisting of glucose, mannose, galactose, talose, altrose, allose, and other hexacarbon sugars; one or more monosaccharides selected from the group consisting of ribose, arabinose, and xylose; one or more disaccharides selected from the group consisting of sucrose, lactose, maltose, lactulose, trehalose, and cellobiose; or a polysaccharide sugar that is starch or cellulose; or a substance from the group consisting of lysine, glycine, alanine, arginine, valine, leucine, isoleucine, methionine, cysteine, proline, histidine, phenylalanine, serine, tricine, tyrosine, aspartic acid, tryptophan, and aminobutyric acid, or a combination thereof.

[0021] The chemical mechanical polishing slurry composition may further contain a pH adjusting agent, the pH adjusting agent being characterized by being one or more inorganic acids selected from the group consisting of sulfuric acid, hydrochloric acid, nitric acid, and phosphoric acid; one or more organic acids selected from the group consisting of acetic acid, citric acid, glutaric acid, glycolic acid, formic acid, lactic acid, malic acid, malonic acid, maleic acid, oxalic acid, phthalic acid, succinic acid, and tartaric acid; one or more amino acids selected from the group consisting of lysine, glycine, alanine, arginine, valine, leucine, isoleucine, methionine, cysteine, proline, histidine, phenylalanine, serine, tricine, tyrosine, aspartic acid, tryptophan, and aminobutyric acid; imidazoles; alkylamines; alcoholamines; quaternary amine hydroxides; ammonia; or a combination thereof.

[0022] The pH of the aforementioned composition may be characterized by being between 2 and 10.

[0023] The chemical mechanical polishing slurry composition may be characterized by having a silicon oxide film polishing rate of 1,000 to 5,000 Å / min.

[0024] The chemical mechanical polishing slurry composition may be characterized by having an oxide film / nitride film polishing selectivity ratio of 200 to 2,000.

[0025] The secondary particle size of the cerium oxide particles, as measured by a dynamic light scattering (DLS) particle size distribution analyzer, may be characterized by being 1 to 20 nm.

[0026] The primary particle size of the cerium oxide particles, as measured by electron transmission microscopy (TEM), may be characterized by being 0.5 to 10 nm.

[0027] In the analysis by X-ray photoelectron spectroscopy (XPS), the sum of the XPS peak areas representing the Ce-O bond energy indicating Ce3+ may be 30% or more compared to 100% of the sum of the XPS peak areas representing the Ce-O bond energy on the surface of the cerium oxide particles.

[0028] The cerium oxide particles may be characterized by being produced by a step of precipitating them in a solution containing a raw material precursor at an acidic pH to obtain a dispersion of particles.

[0029] Another aspect of the present invention is, The present invention provides a method for manufacturing a semiconductor device, which includes a step of polishing using the aforementioned chemical mechanical polishing slurry composition. [Effects of the Invention]

[0030] According to an embodiment of the present invention, the manufactured cerium oxide particles have a Ce on the surface of the cerium oxide. 3+By increasing the ratio of cerium oxide particles, these particles have the characteristic of being able to remove oxide films at a high rate even at low concentrations when included in a chemical mechanical polishing slurry, despite their small particle size. Furthermore, it can be confirmed that the addition of the cationic polymer disclosed in this invention further increases the polishing rate of the oxide film, and improves the selectivity ratio of the oxide film / nitride film by the nitride film passivation modifier, making it possible to passivate even finer patterns. Considering that the addition of cationic polymers is usually done to secure other properties at the expense of polishing speed, which is common knowledge in the conventional art, this is recognized as an effect unique to the present invention.

[0031] Furthermore, according to one embodiment of the present invention, surface defects of the wafer can be minimized, and unlike the conventional correlation between surface defects and the removal rate of the oxide film, which has been considered to be a trade-off, it is possible to provide cerium oxide particles and a slurry composition for chemical mechanical polishing that can maximize the removal rate of the oxide film while minimizing surface defects.

[0032] The effects of the present invention are not limited in any way to those described above, and should be understood to include all effects that can be inferred from the configuration of the invention as described in the detailed description or claims. [Brief explanation of the drawing]

[0033] [Figure 1] This illustrates the mechanism for removing oxide films according to one embodiment of the present invention. [Figure 2a] This is a cross-sectional view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. [Figure 2b] This is a cross-sectional view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. [Figure 2c] This is a cross-sectional view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. [Figure 2d] This is a cross-sectional view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. [Figure 2e] This is a cross-sectional view showing a method for manufacturing a semiconductor device according to one aspect of the present invention. [Figure 2f] This shows a stepwise process of chemical mechanical polishing and the structure of a chemical mechanical polishing (CMP) facility according to another aspect of the present invention. [Figure 2g] This shows a stepwise process of chemical mechanical polishing and the structure of a chemical mechanical polishing (CMP) facility according to another aspect of the present invention. [Figure 3] These are images of a visual observation of a dispersion containing conventional cerium oxide particles and cerium oxide particles according to one embodiment of the present invention. [Figure 4] This is an electron transmission microscope (TEM) image of cerium oxide particles according to one embodiment of the present invention. [Figure 5] This shows scanning electron microscope (SEM) and TEM images of conventional cerium oxide particles as a comparative example. [Figure 6] This shows a TEM image of conventional cerium oxide particles as a comparative example. [Figure 7] This shows the results of measuring cerium oxide particles according to one embodiment of the present invention using a dynamic light scattering (DLS) particle size distribution analyzer. The analysis was performed using a Zetasizer Ultra manufactured by Malvern Panalytical Ltd. in the UK. [Figure 8] This is the result of X-ray diffraction (XRD) analysis of cerium oxide particles according to one embodiment of the present invention. [Figure 9] These are the results of X-ray photoelectron spectroscopy (XPS) analysis of cerium oxide particles according to one embodiment of the present invention and conventional 60 nm class cerium oxide particles. [Figure 10] These are the spectroscopic analysis results obtained by Fourier transform infrared (FT-IR) spectroscopy of a powder consisting of cerium oxide particles manufactured according to one embodiment of the present invention and a powder consisting of ordinary cerium hydroxide particles. [Figure 11] This shows the results of FT-IR spectroscopic analysis of a powder consisting of cerium oxide particles manufactured according to one aspect of the present invention and a powder consisting of particles formed under other conditions. [Figure 12]The light transmittance of cerium oxide particles according to one embodiment of the present invention and slurries containing conventional cerium oxide particles from Comparative Examples 1 to 4 was measured using ultraviolet-visible (UV-Vis) spectroscopy. [Figure 13] This example demonstrates the effect of adding a cationic polymer according to one embodiment of the present invention on the polishing rate of the oxide film. [Figure 14] Because the amount of adsorption to the silicon oxide film (TEOS) is higher than that to the polysilicon film, this demonstrates that when the appropriate amount is used, the polishing speed of the TEOS is increased while the polishing speed of the polysilicon film is reduced. [Figure 15] These are images of an oxide wafer scanned before and after CMP (Chemical Modulation) using a CMP slurry composition containing cerium oxide particles according to one embodiment of the present invention and a CMP slurry composition containing cerium oxide particles of 60 nm size. [Figure 16] These are scanned images of oxide wafers after CMP (Chemical Pollaging) using a CMP slurry composition containing cerium oxide particles according to one embodiment of the present invention and a CMP slurry composition containing cerium oxide particles of 60 nm size. [Modes for carrying out the invention]

[0034] The present invention will be described in more detail below. However, the present invention can be embodied in various different forms, and the present invention is not limited in any way by the examples described herein, and the present invention is defined only by the appended claims.

[0035] Furthermore, the terms used herein are used solely to describe specific embodiments and are not intended to limit the invention. Singular expressions include plural expressions unless the context clearly indicates otherwise. Throughout the specification of the invention, when a part "comprises" a certain component, this does not exclude other components, unless otherwise specified, and means that it may further comprise other components.

[0036] In this invention, "monodispersion" means that when cerium oxide particles are dispersed in a slurry, aggregation into secondary particles is suppressed, and the primary particle size is relatively maintained. This may mean that the secondary particle size (D50) obtained using the dynamic light scattering (DLS) method is 3.0 times or less, 2.8 times or less, 2.5 times or less, 2.2 times or less, 2.0 times or less, or, advantageously, 1.9 times or less, the size of the primary particle size obtained using TEM. Furthermore, when considering particle size distribution, this does not exclude the inclusion of unavoidable impurities of relatively coarse size.

[0037] In this invention, the term "transparent" means that when cerium oxide particles are dispersed in the slurry, the slurry composition appears transparent when observed visually. More specifically, it means that the average transmittance to visible light is 50% or more, preferably 70% or more, and even more preferably 80% or more. This also means that the aggregation of the cerium oxide particles into secondary particles is suppressed, and the primary particle size is relatively maintained.

[0038] Polishing compositions can be characterized according to their polishing speed (i.e., removal speed) and planarization efficiency. Polishing speed refers to the rate at which material is removed from the surface of the substrate and is usually expressed in units of length (thickness) per unit time (e.g., angstroms (Å) per minute). Specifically, the polishing surface, for example, the polishing pad, must first contact the "high points" of its surface and remove material to form a flat surface. A process that achieves a flat surface by removing less material is considered more efficient than a process that is forced to remove more material to achieve flatness.

[0039] Often, the removal rate of silicon oxide patterns limits the rate of dielectric polishing in the STI process; therefore, a high removal rate of silicon oxide patterns is preferable for increasing device processing capacity. However, if the blanket removal rate is too high, excessive polishing of the oxide in the exposed trenches can lead to trench corrosion and potentially increase defects in the device.

[0040] The present invention will be described in detail below.

[0041] The following describes in detail embodiments of the present invention so that persons with ordinary skill in the art to which the present invention pertains can easily implement the present invention. However, the present invention can be embodied in various different forms and is not limited in any way to the embodiments described herein.

[0042] Manufacturing Example 1. Production of Cerium Oxide Particles The cerium oxide particles according to one embodiment of the present invention can be synthesized using chemical synthesis via a bottom-up approach. In the embodiment of the present invention, the cerium oxide particles were produced by one of the methods selected from the methods for producing cerium oxide particles presented below.

[0043] According to one embodiment of the present invention, first, approximately 2-4 kg of cerium nitrate was added to a sufficient amount of deionized water and stirred. Nitric acid was added to the precursor solution to adjust the pH to 1.0 or less. Ammonia water was added to the prepared mixture and stirred until a precipitate was formed. The pH of the stirred mixture was strongly acidic (2 or less), and it was confirmed that the product would precipitate quickly if left to stand after stirring was completed. After removing the supernatant liquid from which the precipitate had been removed, a certain amount was added to deionized water to produce a pale yellow cerium oxide particle dispersion. The prepared dispersion was filtered by circulating it through a membrane filter to obtain a clear yellow cerium oxide dispersion.

[0044] According to another embodiment of the present invention, first, 150 g of cerium oxide or cerium hydroxide was dispersed in 3 kg of deionized water and stirred until the particles did not precipitate. Nitric acid was added to the mixture until the pH was 1.0 or lower. The mixture was added to a milling machine packed with 0.05 mm zirconia beads and ground while circulating at 4,000 rpm. As milling progressed, it was observed that the opaque white cerium oxide dispersion gradually changed into a transparent yellow cerium oxide dispersion. After milling was completed, the prepared transparent yellow cerium oxide dispersion was allowed to precipitate, and then filtered by circulation using a membrane filter to obtain a pure transparent yellow cerium oxide dispersion.

[0045] According to yet another embodiment of the present invention, first, approximately 2-4 kg of cerium ammonium nitrate was added to a sufficient amount of ethanol and stirred. A basic imidazole solution was added to the precursor solution and stirred until a precipitate formed. The pH of the stirred mixture was strongly acidic (2 or less), and it was confirmed that the product would precipitate rapidly if left to stand after stirring was complete. After removing the supernatant liquid from which the precipitate had been removed, a certain amount was added to deionized water to produce a cerium oxide particle dispersion. The prepared dispersion was filtered by circulating it through a membrane filter to obtain a clear cerium oxide dispersion.

[0046] According to yet another embodiment of the present invention, first, 1.1 kg of cerium nitrate and 10 kg of deionized water were mixed in a reaction vessel to prepare a strongly acidic solution. The stirring speed of the reaction vessel was maintained at 200 rpm and at room temperature. A 1:1 mixture of 25% ammonia solution and deionized water was prepared and added to the reaction vessel until the pH reached 7.0. After stirring for 1 hour, a 1:1 mixture of 70% nitric acid and deionized water was added until the pH reached 1.0. The temperature of the reaction vessel was raised to 100°C and the reaction was carried out for 4 hours. During the reaction, pale purple large particles were dissociated, and yellow transparent cerium oxide nanoparticles were produced. The obtained particles were circulated using a membrane filter to remove impurities and obtain a pure cerium oxide nanoparticle dispersion.

[0047] Manufacturing Example 2. Preparation of CMP Slurry Containing Cerium Oxide Particles The cerium oxide particles produced in Production Example 1 were added to deionized water, the concentration of the abrasive was adjusted to 0.05% by weight, and triethanolamine was added to adjust the pH to 5.5 to produce a CMP slurry.

[0048] As shown in Figure 3, while conventional slurries containing ceria particles were observed to be highly turbid even by visual inspection, the slurry containing cerium oxide particles of the present invention was observed to be transparent, suggesting that it possesses monodisperse properties.

[0049] Comparative Examples 1-4: Production of conventional slurry compositions containing ceria particles Commercially available wet cerium oxide particles with average particle sizes of 10 nm, 30 nm, and 60 nm, respectively, and cerium oxide particles of the 10-20 nm class produced separately by a sintering method were prepared. These were then added to deionized water to adjust the abrasive concentration to 0.05% by weight, and ammonia was added as a pH adjuster to adjust the final pH to 5.8 to produce a CMP slurry.

[0050] Experimental Example 1. Analysis of cerium oxide particles using scanning electron microscopy (SEM) and transmission electron microscopy (TEM). A dispersion of Production Example 1 according to one embodiment of the present invention was dried at approximately 80-90°C to prepare powdered cerium oxide particles (primary particles) (Sample A). On the other hand, cerium oxide particles used in the production of the dispersions of Comparative Examples 1 to 4 were prepared respectively (Sample B1, Sample B2, Sample B3, and Sample B4). Images were taken of each of the prepared samples using a TEM measuring instrument.

[0051] Figure 4 is a TEM image of cerium oxide particles according to one embodiment of the present invention.

[0052] Referring to Figure 4, it was confirmed that the particle size of cerium oxide particles produced according to one embodiment of the present invention, as measured by TEM, was on average about 4 nm or less (appearing as 3.9 nm, 3.4 nm, and 2.9 nm in repeated measurements). It was found that the average primary particle size of cerium oxide particles according to one embodiment of the present invention is 4 nm or less. Furthermore, it was confirmed that the cerium oxide particles have a spherical particulate shape on average. Spherical cerium oxide particles with a small particle size and a relatively uniform particle size distribution can have a large specific surface area and are characterized by excellent dispersion stability and storage stability.

[0053] Figure 5 shows SEM and TEM images of conventional cerium oxide particles in a comparative example.

[0054] Referring to Figure 5, commercially available cerium oxide particles exhibit particle sizes appropriate to their respective size classes. Even particles manufactured separately by the scorching method show, on average, primary particle sizes exceeding 10 nm. Comparing this to the average particle size of cerium oxide particles measured by TEM in one embodiment of the present invention shown in Figure 4, which is 4 nm or less, it can be confirmed that conventional cerium oxide particles and cerium oxide particles manufactured by the usual scorching method have much coarser particle sizes. In contrast, the cerium oxide particles of the present invention are formed with smaller particle sizes (primary particles), and it can be expected that the smaller the cerium oxide particle size, the more defects such as scratches on the surface of the film to be polished can be reduced.

[0055] Figure 6 shows a TEM image of conventional cerium oxide particles, which are a comparative example. Referring to Figure 6, it can be seen that conventional cerium oxide particles with a particle diameter of 10 nm or less include particles with edges and spherical particles, while conventional cerium oxide particles with a particle diameter of 30 nm or more consist of angular particles with edges. In contrast, as discussed above, the cerium oxide particles according to the examples of the present invention generally exhibit a spherical shape. However, because the cerium oxide particles of the present invention have this spherical particle shape and a minute particle diameter, a large number of particles can be included. Therefore, when polishing a silicon oxide film, the probability of surface defects occurring is lower, and the flatness over a wide area can be increased.

[0056] Experimental Example 2. Analysis of cerium oxide particles using a dynamic light scattering (DLS) particle size distribution analyzer. A slurry composition from Production Example 2 according to one embodiment of the present invention, and slurry compositions from Comparative Examples 1, 2, 3, and 4 were prepared as samples. Each of the prepared samples was analyzed using a dynamic light scattering (DLS) particle size distribution analyzer.

[0057] Figure 7 shows the results of an analysis of cerium oxide particles using a dynamic light scattering (DLS) particle size distribution analyzer (ZetaSizer Ultra, manufactured by Malvern Panalytical, UK) according to one embodiment of the present invention. Table 1 below shows the D50 values ​​obtained by analysis of cerium oxide particles according to one embodiment of the present invention and cerium oxide particles of a comparative example using a dynamic light scattering (DLS) particle size distribution analyzer.

[0058] [Table 1]

[0059] Referring to Figure 7 and Table 1 above, the cerium oxide particles according to the embodiment of the present invention have a secondary particle diameter D50 value of approximately 5.78 nm, which was measured to be 10 nm or less. As measured in Experimental Example 1, this is at a level of approximately 148-199% compared to the primary particle diameter measured by TEM (see Figure 4), and it was confirmed that there was almost no aggregation in the slurry, and the particles were monodisperse with almost no change in particle size.

[0060] In contrast, the D50 particle diameter of conventional cerium oxide particles, measured using a dynamic light scattering (DLS) particle size distribution analyzer, was found to exceed 30 nm. Even in the case of 10 nm class cerium oxide particles, the secondary particle diameter D50 value measured by the dynamic light scattering (DLS) particle size distribution analyzer was approximately 336% of the primary particle diameter measured by TEM. This indicates that conventional cerium oxide particles have a much larger secondary particle diameter, confirming that significant aggregation has occurred.

[0061] In particular, in the case of cerium oxide particles of 10 nanometers or less produced by supercritical hydrothermal synthesis or wet synthesis under basic conditions, it can be confirmed that secondary particles are formed to be larger than the primary particle size, as predicted by the inventors.

[0062] Furthermore, even when the slurry contains a nitride film passivation modifier and a cationic polymer as additives (Example 2), it was confirmed that the monodispersity of the cerium oxide particles in the slurry is maintained. Therefore, it was confirmed that the cationic polymer and nitride film passivation modifier claimed in the present invention are suitable for use in combination with cerium oxide particles according to one embodiment of the present invention.

[0063] Therefore, it can be seen that the cerium oxide particles according to one embodiment of the present invention exhibit even less aggregation in the slurry than the conventional cerium oxide particles according to one comparative example, and can be dispersed in the slurry in an even more monodisperse shape.

[0064] Experimental Example 3. Analysis of cerium oxide particles by X-ray diffraction (XRD). A dispersion of Production Example 1 according to one embodiment of the present invention was dried at approximately 80-90°C to prepare cerium oxide particles (primary particles) in powder form (Sample A). The prepared Sample A was analyzed using an X-ray diffractometer (Ultima IV, manufactured by Rigaku Corporation). At this time, the XRD was set to CuKα (λ=1.5418Å), 40kV, and 40mA.

[0065] Figure 8 shows the results of X-ray diffraction (XRD) analysis of cerium oxide particles according to one embodiment of the present invention.

[0066] X-ray diffraction (XRD) analysis of sample A yielded an XRD spectrum with the shape shown in Figure 8 (X-axis: 2θ(°), Y-axis: intensity). The crystallite size calculated from this spectrum was 3.25 nm. This is at approximately the same level as the TEM analysis result in Experimental Example 1, confirming that the particles of the present invention possess single-crystal properties.

[0067] Experimental Example 4. Analysis of cerium oxide particles by X-ray photoelectron spectroscopy (XPS) FIG. 9 shows analysis results of cerium oxide particles according to an embodiment of the present invention and conventional 60 nm-class cerium oxide particles using X-ray photoelectron spectroscopy (XPS). In X-ray photoelectron spectroscopy (XPS), when soft X-rays are irradiated, Ce 3+ By measuring peaks appearing at 900.2 to 902.2 eV, 896.4 to 898.4 eV, 885.3 to 887.3 eV, and 880.1 to 882.1 eV, which indicate Ce-O binding energies, and analyzing atomic% using XPS fitting, Ce in the cerium oxide particles 3+ and Ce 4+ contents can be measured. Table 2 below shows data of analysis results of cerium oxide particles according to an embodiment of the present invention using X-ray photoelectron spectroscopy (XPS).

[0068] [Table 2]

[0069] From the analysis results using the X-ray photoelectron spectroscopy (XPS), according to the above general formula, Ce 3+ As a result of calculating the content, Ce 3+ It can be seen that the content is 30% or more. In the cerium oxide particles, Ce 3+ Since are reactive sites, it can be inferred that the polishing rate can be increased thereby. Comparative data with conventional cerium oxide particles using the above method are shown in Table 3.

[0070] [Table 3]

[0071] In the case of cerium oxide particles according to an embodiment of the present invention, as is apparent from Table 3 above, Ce 3+ content is about 36.9 atomic%, and in Table 1, this is compared to Ce of conventional 60 nm-class cerium oxide particles 3+The content is less than 14 atomic percent, and compared to the approximately 16.8% cerium oxide content of 10 nm class cerium oxide particles produced by hydrothermal synthesis under supercritical or subcritical conditions, as known from conventional literature, the Ce content is high. 3+ It can be confirmed that it contains the following Ce on the surface. 3+ When the content is at a high level, as in the examples of the present invention, the polishing rate on silicon-containing substrates can be increased by the chemical polishing mechanism that forms Si-O-Ce between silica and cerium.

[0072] Experimental Example 5. Confirmation of cerium oxide particle formation using Fourier transform infrared (FT-IR) spectroscopy. Figure 10 shows the spectroscopic analysis results by Fourier transform infrared (FT-IR) spectroscopy of a powder consisting of cerium oxide particles manufactured according to one embodiment of the present invention and a powder consisting of ordinary cerium hydroxide particles. A dispersion of Production Example 1 according to one embodiment of the present invention was dried at approximately 80-90°C to prepare cerium oxide particles (primary particles) in powder form, and spectra were obtained using a Fourier transform infrared (FT-IR) spectrophotometer. The analysis range was 600-4100 cm⁻¹. -1 The graph was created by repeatedly scanning the area at least once within the region (wavenumber (cm) in the FT-IR spectrum). -1 ) is ±10cm -1 (It may have an error range of .)

[0073] Analysis of the FT-IR spectral spectrum in Figure 10 revealed that the 3000 cm³ of the powder consisting of cerium oxide particles according to one embodiment of the present invention -1 ~3600cm -1 The infrared transmittance within this range is approximately 92-93%, at 720cm. -1 ~770cm -1 It can be confirmed that the infrared transmittance within this range is approximately 93-95%. This can be seen in the FT-IR spectrum of a powder consisting of ordinary cerium hydroxide particles at 3000 cm⁻¹. -1 ~3600cm -1 The infrared transmittance within this range is 75-90%, at 720cm. -1 ~770cm -1Compared to the infrared transmittance of 97-99% within the range of 3000 cm², cerium oxide particles produced according to one embodiment of the present invention exhibit a higher transmittance of 97-99% within 3000 cm². -1 ~3600cm -1 Within this range, the OH group bonding of cerium hydroxide particles is weaker than that of ordinary cerium hydroxide particles, and at 720 cm² -1 ~770cm -1 It can be confirmed that a peak is formed by Ce-O stretching within the specified range. Therefore, the above result can be interpreted as meaning that the cerium compound produced according to one aspect of the present invention is cerium oxide.

[0074] In a comparative example, it has been stated that among cerium oxide particles synthesized by a wet method substantially similar to one aspect of the present invention, when the synthesis is carried out under basic conditions, cerium hydroxide is formed first, and then it is possible to convert it to cerium oxide using a subsequent process. According to the experimental results shown in Figure 11, in the case of particles synthesized under basic pH conditions, when FT-IR was measured immediately after synthesis, 3000 cm³, which represents cerium hydroxide, was found. -1 ~3600cm -1 The range and 720cm -1 ~770cm -1 The appearance of peaks within this range directly reflects the main peak of cerium hydroxide in Figure 10, making it difficult to conclude that the substance contains only cerium oxide.

[0075] Experimental Example 6. Measurement of Transmittance of Slurry Containing Cerium Oxide Particles A slurry composition (Sample A) was prepared in the same manner as in Production Example 2, except that the weight ratio of cerium oxide particles in the CMP slurry was set to 1% by weight. On the other hand, slurry compositions were prepared in the same manner as in Comparative Examples 1, 2, 3, and 4, respectively, except that the weight ratio of cerium oxide particles in the CMP slurry was set to 1% by weight. For each sample, the transmittance to light in the range of 200 to 1100 nm was measured using a UV-Vis spectrophotometer (manufactured by JASCO Corporation).

[0076] Figure 12 shows the results of measuring the light transmittance of cerium oxide particles according to one embodiment of the present invention and slurries containing conventional cerium oxide particles from Comparative Examples 1 to 4 using ultraviolet-visible spectroscopy.

[0077] Cerium oxide particles according to one embodiment and a comparative example of the present invention were added to deionized water to adjust the abrasive concentration to 1.0 wt%, and a CMP slurry was prepared and its transmittance was analyzed. At this time, the optical spectrum was measured in the range of 200 to 1,100 nm using a UV-Vis spectrophotometer (a UV-Vis spectrophotometer manufactured by JASCO Corporation).

[0078] Using the aforementioned UV-Vis analysis graph, the transmittance (%) of samples A, A2, and B1-B4 at wavelengths of 500nm, 600nm, and 700nm are summarized in Table 4 below.

[0079] [Table 4]

[0080] As shown in Figure 11 and Table 2, in the case of the slurry containing cerium oxide particles of the present invention, it can be confirmed that the average light transmittance for light with wavelengths of 450 to 800 nm is 50% or more. Furthermore, it was confirmed that the light transmittance for light with a wavelength of approximately 500 nm is 90% or more, and the light transmittance for light with wavelengths of approximately 600 nm and 700 nm is 95% or more.

[0081] In contrast, the transmittance of slurries containing conventional cerium oxide particles was measured using Comparative Examples 1 to 4 (conventional cerium oxide particles of 10 nm, 30 nm, and 60 nm class, and ceria particles produced by the scorching method). Comparative Example 4 (scorched ceria particles) showed a transmittance of approximately 0%, indicating that the transmittance of the slurry in Comparative Example 1, which contains commercially available conventional cerium oxide particles of 10 nm class, was less than 80% on average, and less than 50% at a wavelength of 500 nm. In the case of Comparative Examples 2 and 3, the primary particle size was 30 nm and 60 nm, respectively, which are coarse, and the secondary particle size was also coarser compared to the examples of the present invention (i.e., the cohesiveness in the slurry was greater), resulting in a transmittance of less than 20% in the visible light region.

[0082] In contrast, cerium oxide particles according to one embodiment of the present invention can be confirmed to exhibit a transmittance of 90% or more in the visible light region. This means that, in the case of cerium oxide particles of the present invention, the primary particle size itself is minute, and aggregation into secondary particles occurs less than with conventional cerium oxide particles. Normally, when secondary particles exceed 20 nm, the opacity of the slurry composition can be observed even with the naked eye, and it is well known that the transmittance in the visible light region is less than 80%.

[0083] According to the slurry composition of the present invention, the high light transmittance is a result of the particles being uniformly distributed due to increased dispersion stability when the primary particle size of the cerium oxide particles is small and the aggregation of secondary particles is low. As a result, the number of particles in contact with the wafer increases, the polishing speed of the oxide film is exceptionally fast. Furthermore, because the particles themselves are minute, it can be easily predicted that the probability of defects such as scratches occurring on the surface when polishing a film to be polished using the slurry composition containing these particles will be low.

[0084] Furthermore, even if the additives, such as cationic polymers and nitride film passivation modifiers, are included, it can be confirmed that the light transmittance characteristics of the present invention are maintained at the same level. However, considering that incorrect selection of additives may impair the monodispersity characteristics of cerium oxide particles in the slurry according to one aspect of the present invention, the cationic polymers and nitride film passivation modifiers selected in the present invention suggest that the required characteristics can be met without impairing the basic particle characteristics in the slurry.

[0085] Experimental Example 7. Comparison of the polishing rate of oxide films by cerium oxide particles. Slurry compositions from Production Examples 2 and 3 according to one embodiment of the present invention, and a slurry composition from a comparative example, were prepared as samples.

[0086] Polishing of the oxide film wafer using the aforementioned sample was performed using a polishing apparatus (Reflexion® LK CMP, manufactured by Applied Materials Japan, Ltd.). Specifically, a PE-TEOS silicon oxide film wafer (300 mm PE-TEOS wafer) was placed on a platen, and the surface of this wafer was brought into contact with the polishing machine's pad (IC1010 (trademark), manufactured by Dow). Next, the sample slurry composition was supplied at a rate of 200 mL / min, and the polishing process was performed while rotating the platen and the polishing machine's pad. At this time, the rotation speed of the platen and the head were set to 67 rpm / 65 rpm, the polishing pressure was set to 2 psi, and the polishing time was set to 60 seconds. Meanwhile, the thickness of the silicon oxide film on the wafer was measured using ST5000 (Spectra Thick 5000ST, manufactured by K-MAC, South Korea). The results are shown in Table 5 below.

[0087] [Table 5]

[0088] As shown in Table 5 above, it was confirmed that when using the slurry composition of the example, the silicon oxide film removal rate was at least about 6 times faster than that of the slurry composition of the comparative example. This is because, in the case of the cerium oxide particles contained in the slurry composition of the example, the particle size is small and the number of particles that work effectively for polishing is large relative to the content, and the Ce on the surface 3+ It is presumed that this is because the high content (molar ratio and / or weight ratio) of the substance increases its chemical reactivity with the surface of the silicon oxide film.

[0089] Furthermore, in the case of the slurry composition further containing the cationic polymer and nitride film passivation modifier of Production Example 3, it was found that the polishing rate of the oxide film was further improved compared to the slurry composition without the additives of Production Example 2. From this, it can be seen that, in the case of the cationic polymer according to one aspect of the present invention, when combined with cerium oxide particles according to one aspect of the present invention, the cationic polymer is positioned between the cerium oxide particles according to one aspect of the present invention, further maximizing its unique monodispersity and maximizing the number and area of ​​particles in contact with the silicon oxide film, so that the polishing rate of the oxide film increases up to a predetermined content range. If the predetermined range is exceeded, the dishing modifier itself may partially block or interfere with the contact between the cerium oxide particles and the oxide film, so that the polishing rate of the oxide film decreases. The characteristic behavior of the oxide film polishing rate depending on the content of the cationic polymer is very much in line with the observation that when the cationic polymer described in the present invention is used in combination with ordinary cerium oxide particles, the polishing rate of the oxide film decreases from the initial content. These characteristics are simplified and shown in Figure 13.

[0090] These characteristics are even more noteworthy when compared to the behavior observed when a cationic polymer according to one aspect of the present invention is included in a slurry composition using ordinary ceria particles of 60 nanometers or less manufactured according to conventional technology (Comparative Examples 9 and 10), which actually reduces the polishing rate of the oxide film.

[0091] Experimental Example 8. Evaluation of defects in cerium oxide particles Figures 15 and 16 show scanned images of an oxide wafer before and after CMP (Chemical Modulation) using a CMP slurry composition containing cerium oxide particles according to one embodiment of the present invention and a CMP slurry composition containing cerium oxide particles with a particle size of 60 nm.

[0092] The surface analysis of the oxide wafer was performed using a full wafer scan method with AIT-XP equipment.

[0093] Referring to Figures 15 and 16, an analysis of the surface of an oxide wafer subjected to CMP using the CMP slurry composition containing cerium oxide particles according to the embodiment of the present invention showed that the number of defects before CMP was counted as 6, and the number of defects after CMP was counted as 1. This confirms that the number of defects on the surface of the oxide wafer decreased after CMP was performed using the CMP slurry composition containing cerium oxide particles according to the embodiment of the present invention, and that no scratches occurred on the surface of the wafer during the CMP process. In contrast, an analysis of the surface of an oxide wafer subjected to CMP using a conventional CMP slurry composition containing cerium oxide particles showed that the number of defects before CMP was 34, while the number of defects after CMP increased to 64. This confirms that the conventional cerium oxide particles caused scratches on the surface of the wafer. This suggests that because the particle size of the cerium oxide particles according to one embodiment of the present invention is smaller than that of the conventional cerium oxide particles, the probability of defects occurring on the surface of the oxide wafer to be polished can be reliably reduced. Furthermore, in the case of cerium oxide particles according to one aspect of the present invention, since they are monodisperse in the slurry and are themselves minute particles, it is quite predictable that defects will be minimized even if additives are included.

[0094] Experimental Example 9. Analysis of the polishing selectivity ratio of oxide / nitride films with the addition of additives. Cerium oxide particles manufactured according to one aspect of the present invention and conventional commercially available 60 nm class cerium oxide particles were added to deionized water, the pH was adjusted to 5.8, and then a cationic polymer was added as shown in Table 6 below. Under polishing conditions as in Experimental Example 7, the polishing rate of the oxide film (Å / min) and the polishing rate of the nitride film (Å / min) were measured.

[0095] [Table 6]

[0096] Referring to Table 6 above, it can be seen that when a cationic polymer and nitride film passivation modifier according to one aspect of the present invention are included, the polishing rate of the nitride film during the STI process is significantly reduced (30-80%) compared to when no additives are included. This is noteworthy because it is an effect that can be obtained without impairing the properties of the particles in the slurry according to one aspect of the present invention. In the case of the cationic polymer according to one aspect of the present invention, as shown in Figure 14, the amount adsorbed to the silicon oxide film (TEOS) is higher than that of the nitride film, so when an appropriate amount is used, the polishing rate of the TEOS is increased, while the polishing rate of the silicon nitride film decreases. Furthermore, it can be seen that the cationic polymer according to one aspect of the present invention basically has the characteristic of lowering the polishing rate of the nitride film when added.

[0097] In contrast, in the case of the slurry compositions of Production Example 2 and Comparative Examples 1 to 8, which do not contain cationic polymers, the cationic polymers are simply added to stabilize the particles by acting as a pH buffer. As mentioned above, it was confirmed that increasing the content of cationic polymers can hinder the polishing process by which the polishing particles perform. However, in the case of the CMP slurry of the present invention, it is clear that the cationic polymers not only contribute to particle stability but also play a role as a polishing accelerator.

[0098] (Modes for carrying out the invention) The first aspect of the present invention is, The present invention provides a chemical mechanical polishing slurry composition comprising cerium oxide particles, a solvent, a cationic polymer, and a nitride film passivation modifier, wherein the content of the cerium oxide particles is adjusted to 1.0% by weight, and the average light transmittance for wavelengths in the 450-800 nm region is 50% or more in an aqueous dispersion.

[0099] The following describes in detail the chemical mechanical polishing slurry composition according to the first aspect of the present invention.

[0100] Figure 1 shows the oxide film removal mechanism according to one embodiment of the present invention. As shown in Figure 1, Ce on the surface of cerium oxide particles 3+ Unless the ions are activated, they cannot react smoothly with SiO2.

[0101] In one embodiment of the present invention, the inclusion of the cationic polymer and the nitride film passivation modifier may significantly reduce the polishing rate of the nitride film. This is a key technical feature of the chemical mechanical polishing slurry composition of the present invention compared to the conventional art, and will be explained in detail below. In particular, this configuration exhibits a unique effect when combined with the cerium oxide particles unique to the present invention, which will be described in detail below.

[0102] In one embodiment of the present invention, the cationic polymer can play several roles in the chemical mechanical polishing slurry composition of the present invention. First, it can reduce the occurrence of dishing and erosion that can occur during the STI process. Second, it can act as a stabilizer for the slurry composition, and can also act as a pH buffer to ensure particle dispersibility and dispersion stability. Furthermore, the cationic polymer of the present invention can also act as a polishing accelerator for oxide films. In conventional polishing slurries, cationic polymers have been added to increase dispersion stability or to protect the field oxide film during step removal, and in order to obtain such properties, the polishing rate of the oxide film had to be partially sacrificed. In contrast, the cationic polymer added to the polishing slurry of the present invention not only increases dispersion stability, but the overall polishing rate of the oxide film can be increased as the amount of cationic polymer added increases.

[0103] As described later, cerium oxide particles according to one aspect of the present invention are obtained by a wet method at an acidic pH, are obtained in the form of a dispersion, and even if a solvent is added to the dispersion itself to immediately produce a slurry, they may also have a form in which ultrafine cerium oxide nanoparticles are monodispersed without a separate redispersion step, and the surface Ce 3+ The content of is also maintained at a high level, and the particles exhibit a very high level of oxide film polishing speed when manufacturing a slurry composition for chemical mechanical polishing. As described above, our research has revealed that even if various additives used in the conventional art are added to cerium oxide particles according to one aspect of the present invention, which have unique properties, it is difficult to achieve the performance intended in the conventional art. Furthermore, from the perspective of an ordinary engineer using nanoparticles, in a composition containing nanoparticles, it is necessary to find and combine substances suitable for specific nanoparticles to achieve the desired properties or performance. In the case of a slurry composition according to one aspect of the present invention, a nitride film passivation modifier may be further added to minimize the nitride film polishing speed without impairing (or even increasing) the excellent oxide film polishing speed performance of the cerium oxide particles.

[0104] In one embodiment of the present invention, the principle by which the cerium oxide particles, cationic polymer, and nitride film passivation modifier substance unique to the present invention exhibit their effects is as follows. In the case of cerium oxide particles according to the embodiment of the present invention, they have the characteristic of being monodispersible in the slurry without any particular dispersion process. In the case of the cationic polymer, as a result of being positioned between the monodisperse cerium oxide particles, the cerium oxide particles can uniformly and smoothly contact the silicon oxide film, thereby maximizing the polishing speed. Furthermore, in the case of the nitride film passivation modifier, it can hinder the cerium oxide particles from contacting the nitride film, thereby minimizing the polishing speed of the nitride film. By using an appropriate content, it is also possible to proceed without hindering the polishing speed of the silicon oxide film.

[0105] In one aspect of the present invention, the content of the cationic polymer may be 0.001% by weight or more, 0.002% by weight or more, 0.003% by weight or more, 0.004% by weight or more, or 0.005% by weight or more, based on the total weight of the chemical mechanical polishing slurry composition, or it may be 1% by weight or less, 0.5% by weight or less, 0.1% by weight or less, 0.05% by weight or less, 0.03% by weight or less, or 0.01% by weight or less. If the content of the cationic polymer is less than 0.001% of the total weight of the chemical mechanical polishing slurry composition, the content is too small to adequately perform its role as an oxide film polishing accelerator, and as a result, it cannot affect the polishing rate of the oxide film. Conversely, if the content of the cationic polymer exceeds 1% of the total weight of the chemical mechanical polishing slurry composition, the added cationic polymer may hinder the polishing process of cerium oxide and actually reduce the polishing rate of the oxide film, or it may become an impurity in the slurry composition.

[0106] In one aspect of the present invention, the content of the nitride film passivation modifier may be 0.001% by weight or more, 0.002% by weight or more, 0.003% by weight or more, 0.004% by weight or more, or 0.005% by weight or more, based on the total weight of the chemical mechanical polishing slurry composition, and may also be 1% by weight or less, 0.5% by weight or less, 0.1% by weight or less, 0.05% by weight or less, 0.03% by weight or less, or 0.01% by weight or less. If the content of the nitride film passivation modifier is less than 0.001% of the total weight of the chemical mechanical polishing slurry composition, the content is too small to adequately perform its role as a nitride film passivation modifier, and as a result, it cannot affect the reduction in the polishing rate of the nitride film. Conversely, if the content of the passivation modifier exceeds 1% of the total weight of the chemical mechanical polishing slurry composition, the added nitride film passivation modifier may hinder the polishing process of cerium oxide, thereby reducing the polishing rate of the oxide film, or it may become an impurity in the slurry composition.

[0107] In one embodiment of the present invention, the cationic polymer may be a polymer or copolymer containing an amine group or an ammonium group. For example, the cationic polymer may be characterized by being polydiallyldimethylammonium chloride (Poly(DADMAC)), polydiethylenetriamine 2-(dimethylamino)ethyl methacrylate (Poly(DMAEM)), poly 2-(dimethylamino)ethyl methacrylate (Poly(DMAEM)), polyacrylamide decamethylene diamine (Poly(Aam_DCDA)), poly(dimethylamine)-co-epichlorohydrin, poly(dimethylamine)-co-epichlorohydrin-co-ethylenediamine) or a combination thereof.

[0108] In one aspect of the present invention, the nitride film passivation modifier may be characterized by being a substance or a combination thereof from the group consisting of hexacarbon sugars such as glucose, mannose, galactose, talose, altrose, and allose, one or more monosaccharides selected from the group consisting of ribose, arabinose, and xylose, one or more disaccharides selected from the group consisting of sucrose, lactose, maltose, lactulose, trehalose, and cellobiose, or sugars that are polysaccharides of starch or cellulose, lysine, glycine, alanine, arginine, valine, leucine, isoleucine, methionine, cysteine, proline, histidine, phenylalanine, serine, tricine, tyrosine, aspartic acid, tryptophan, and aminobutyric acid.

[0109] In one embodiment of the present invention, the passivation modifier may be a nonionic polymer, such as polyethylene glycol, polyvinyl alcohol, or polyvinylpyrrolidone, or a combination thereof.

[0110] The following describes cerium oxide particles according to one aspect of the present invention. In one aspect of the present invention, the chemical mechanical polishing slurry composition is characterized by using cerium oxide particles that have excellent dispersion stability and, in particular, excellent polishing rate against silicon oxide films.

[0111] In one embodiment of the present invention, the cerium oxide particles contained in the slurry as polishing particles may have a positive zeta potential value, preferably 1 to 80 mV, 5 to 60 mV, or 10 to 50 mV in the pH range of 2 to 8. The positive zeta potential value of the cerium oxide particles results in a negative polarity on the surface of the silicon oxide film, which in turn increases the polishing efficiency due to the attractive force between the cerium oxide particles and the surface of the silicon oxide film.

[0112] In one embodiment of the present invention, although the cerium oxide particles have lower hardness than silica particles or alumina particles, the chemical polishing mechanism by which Si-O-Ce bonds are formed between silica and cerium results in a very high polishing rate for silicon-containing surfaces such as glass and semiconductor substrates, making them advantageous for polishing semiconductor substrates.

[0113] In one embodiment of the present invention, the particle size of the cerium oxide particles in the slurry can be measured by dynamic light scattering (DLS) analysis (secondary particles). The dynamic light scattering analysis can be performed using analytical equipment well known to the average technician, preferably using a particle size analyzer from Anton Paar or a Zetasizer Ultra from Malvern Panalytical, UK, but this is merely a non-limiting example and the present invention is not limited thereto. In the case of the secondary particles described above, they are formed by the aggregation of primary particles in the slurry, which will be described later. It can be easily inferred that the larger the surface area of ​​the particles, the wider the range over which attractive forces act, and therefore the more effectively aggregation should occur. Furthermore, as the pH range in the solution passes the isoelectric point where the zeta potential of the particles becomes zero, aggregation into secondary particles occurs. However, in the case of cerium oxide particles, as disclosed in various sections of the conventional technology, the isoelectric pH is about 7. In the case of a wet process, if particle synthesis is completed under basic conditions, the pH inevitably has to be adjusted to produce a slurry while passing the isoelectric point. As a result, it may become difficult for the particles to have monodispersibility in the slurry, as in the particles of one embodiment of the present invention.

[0114] In one embodiment of the present invention, the particle size of the cerium oxide particles measured by a dynamic light scattering (DLS) particle size distribution analyzer may be 1 to 30 nm. In another embodiment of the present invention, the particle size may be 29 nm or less, 27 nm or less, 25 nm or less, 23 nm or less, 22 nm or less, 20.8 nm or less, 20.5 nm or less, 20.2 nm or less, 20 nm or less, 19.8 nm or less, 19.5 nm or less, 19.2 nm or less, 18 nm or less, 17 nm or less, or 15 nm or less, and may be 1.2 nm or more, 1.4 nm or more, 1.5 nm or more, 1.8 nm or more, 2 nm or more, 3 nm or more, or 4 nm or more. If the secondary particle size exceeds the above range, it means that aggregation of primary particles occurs vigorously in the slurry composition, in which case it becomes difficult to recognize it as a monodisperse slurry. If the secondary particle size is less than the above range, there is a risk that the polishing rate on the target film will be excessively inhibited and the polishing efficiency will decrease.

[0115] In one embodiment of the present invention, the particle size of the cerium oxide particles can be measured by electron transmission microscopy (TEM) (primary particles). In one embodiment of the present invention, the particle size of the cerium oxide particles measured by electron transmission microscopy (TEM) may be 11 nm or less. In another embodiment, the particle size of the cerium oxide particles measured by electron transmission microscopy (TEM) may be 10.8 nm or less, 10.5 nm or less, 10.2 nm or less, 10 nm or less, 9.5 nm or less, 9.0 nm or less, 8.5 nm or less, 8.0 nm or less, 7.5 nm or less, 7.0 nm or less, 6.5 nm or less, 6.0 nm or less, 5.5 nm or less, 5.0 nm or less, 4.5 nm or less, or 4.0 nm or less, or 0.3 nm or more, 0.5 nm or more, 0.7 nm or more, 1.0 nm or more, 1.1 nm or more, 1.2 nm or more, 1.3 nm or more, 1.4 nm or more, 1.5 nm or more, 1.6 nm or more, 1.7 nm or more, 1.8 nm or more, 1.9 nm or more, 2.0 nm or more, 2.1 nm or more, 2.2 nm or more, 2.3 nm or more, or 2.4 nm or more. If the particle size of the cerium oxide particles is less than 0.3 nm, the crystallinity may decrease, excessively inhibiting the polishing rate on the target film and potentially reducing polishing efficiency. Conversely, if the particle size of the cerium oxide particles exceeds 11 nm, a large number of surface defects such as scratches may occur. In one embodiment of the present invention, the average particle size of the cerium oxide particles measured by the electron transmission microscope (TEM) may be 0.5 to 10 nm, preferably 1 to 10 nm, and more preferably 2 to 9 nm.

[0116] From the viewpoint of characterizing cerium oxide particles according to one aspect of the present invention, the cerium oxide particles may be characterized in that, when the particle diameter of the cerium oxide particles measured by a dynamic light scattering (DLS) particle size distribution analyzer is a, and the particle diameter of the cerium oxide particles measured by an electron transmission microscope (TEM) is b, the following equation 1 is satisfied.

[0117]

number

[0118] These characteristics should serve as an indicator that the cerium oxide particles of the present invention have low cohesiveness when dispersed in a slurry. If the coefficient of b exceeds 2.2, it means that aggregation occurs actively in the slurry, which should mean that the particle size becomes coarser, making it difficult to suppress surface defects on the wafer during polishing.

[0119] In one embodiment of the present invention, the particle size of the cerium oxide particles can be measured by analysis using X-ray diffraction (XRD) (primary particles). In one embodiment of the present invention, the particle size of the cerium oxide particles measured by analysis using X-ray diffraction (XRD) may be 11 nm or less. In another embodiment, the particle size of the cerium oxide particles, as measured by analysis by X-ray diffraction (XRD), may be 10.8 nm or less, 10.5 nm or less, 10.2 nm or less, 10 nm or less, 9.5 nm or less, 9.0 nm or less, 8.5 nm or less, 8.0 nm or less, 7.5 nm or less, 7.0 nm or less, 6.5 nm or less, 6.0 nm or less, 5.5 nm or less, 5.0 nm or less, 4.5 nm or less, or 4.0 nm or less. Alternatively, it may be 0.3 nm or more, 0.5 nm or more, 0.7 nm or more, 1.0 nm or more, 1.1 nm or more, 1.2 nm or more, 1.3 nm or more, 1.4 nm or more, 1.5 nm or more, 1.6 nm or more, 1.7 nm or more, 1.8 nm or more, 1.9 nm or more, 2.0 nm or more, 2.1 nm or more, 2.2 nm or more, 2.3 nm or more, or 2.4 nm or more. If the particle size of the cerium oxide particles is less than 0.3 nm, the crystallinity may decrease, excessively inhibiting the polishing rate on the target film and potentially reducing polishing efficiency. Conversely, if the particle size of the cerium oxide particles exceeds 11 nm, a large number of surface defects such as scratches may occur. In one embodiment of the present invention, the average particle size of the cerium oxide particles, as measured by the X-ray diffraction (XRD) analysis, may be 0.5 to 10 nm, preferably 1 to 10 nm, and more preferably 2 to 9 nm.

[0120] In one embodiment of the present invention, Ce on the surface of the cerium oxide particles 3+ The content of Ce on the surface of the cerium oxide polished particles can be analyzed using X-ray photoelectron spectroscopy (XPS), for example, using a theta probe base system from Thermo Fisher Scientific. 3+ The content can be calculated using the following general formula 1.

[0121] [ka]

[0122] In one embodiment, when analyzing the surface of the cerium oxide particles by X-ray photoelectron spectroscopy (XPS), Ce 3+ The XPS peaks indicating the Ce-O bond energy appear at 900.2–902.2 eV, 896.4–898.4 eV, 885.3–887.3 eV, and 880.1–882.1 eV, which may be a characteristic feature. Specifically, when analyzing the surface of the cerium oxide particles by X-ray photoelectron spectroscopy (XPS), Ce 3+ The XPS peaks indicating the Ce-O bond energy may be characterized by the appearance of a first peak at 900.2–902.2 eV, a second peak at 896.4–898.4 eV, a third peak at 885.3–887.3 eV, and a fourth peak at 880.1–882.1 eV.

[0123] In one embodiment of the present invention, the area of ​​the first peak may be 3% or more, or 4% or more, of the total XPS peak area; the areas of the second and fourth peaks may be 5% or more, 7% or more, or 10% or more, respectively; and the area of ​​the third peak may be 4% or more, 5% or more, or 6% or more.

[0124] Furthermore, in one embodiment of the present invention, when analyzing by X-ray photoelectron spectroscopy (XPS), the sum of the XPS peak areas representing the Ce-O bond energy on the surface of the cerium oxide particles is used.3+ The ratio of the sum of XPS peak areas indicating the Ce-O bond energy may be 0.29 to 0.70. In another embodiment of the present invention, the ratio of the sum of XPS peak areas indicating the Ce-O bond energy on the surface of the cerium oxide particles to the sum of XPS peak areas indicates the Ce 3+ The ratio of the sum of XPS peak areas indicating the Ce-O bond energy may be 0.18 or higher, 0.19 or higher, 0.192 or higher, 0.195 or higher, 0.198 or higher, 0.20 or higher, 0.202 or higher, 0.205 or higher, 0.208 or higher, 0.21 or higher, 0.22 or higher, 0.24 or higher, 0.25 or higher, 0.27 or higher, 0.28 or higher, 0.30 or higher, 0.32 or higher, or 0.35 or higher. Or, it may be 0.90 or less, 0.88 or less, 0.85 or less, 0.83 or less, 0.80 or less, 0.77 or less, 0.75 or less, 0.72 or less, 0.71 or less, 0.705 or less, 0.70 or less, 0.695 or less, 0.69 or less, 0.68 or less, 0.67 or less, 0.66 or less, 0.65 or less, 0.64 or less, 0.63 or less, 0.62 or less, 0.61 or less, or 0.60 or less. If it is less than the above range, a sufficient amount of Ce on the surface of the cerium oxide particles. 3+ As a result of the inability to exist, it will be difficult to expect a sufficient increase in the polishing rate of the oxide film, and if it exceeds the aforementioned range, when considering the oxidation state, it may become difficult to interpret it as existing as cerium oxide particles.

[0125] In other words, in one embodiment of the present invention, when performing analysis by X-ray photoelectron spectroscopy (XPS), the surface of the cerium oxide particles for chemical mechanical polishing is Ce 3+ It may contain 18 atomic% or more, 19 atomic% or more, 20 atomic% or more, 22 atomic% or more, 24 atomic% or more, 25 atomic% or more, 27 atomic% or more, 28 atomic% or more, 30 atomic% or more, 32 atomic% or more, or 35 atomic% or more, or it may be characterized by containing 90 atomic% or less, 88 atomic% or less, 85 atomic% or less, 83 atomic% or less, 80 atomic% or less, 77 atomic% or less, 75 atomic% or less, 72 atomic% or less, or 70 atomic% or less.

[0126] In the case of cerium oxide particles according to one aspect of the present invention, Ce on the surface of the particles 3+ The particle exhibits a high content of Ce, which is due to the fact that the particle synthesis process is carried out under acidic conditions in a liquid state through a wet process according to one aspect of the present invention. Normally, in the case of cerium precursor materials containing trivalent cerium, the trivalent cerium state is maintained at an acidic pH, and since the manufacturing method according to one aspect of the present invention does not involve conversion to a basic pH during the overall particle synthesis process, the surface of the synthesized particles has a high trivalent cerium content. The trivalent cerium content characteristics on the surface of such cerium oxide particles are determined by the formation and retention of surface defects during the manufacturing process, and are therefore considered to be independent of the technical characteristics such as the primary or secondary particle size mentioned above. As described above, cerium oxide particles according to one aspect of the present invention have a high Ce content on the surface of the particles. 3+ The content of Ce increases, and thus the surface 3+ When the content of is relatively high, the polishing rate of the oxide film can be improved.

[0127] In one embodiment of the present invention, when Fourier-transformation infrared (FT-IR) spectroscopy is performed on the powder consisting of cerium oxide particles, in the spectrum identified by the FT-IR spectroscopy, 3000 cm⁻¹ -1 ~3600cm -1 The infrared transmittance of the powder consisting of cerium oxide particles within the range may be 90% or more, or 100% or less, 97% or less, or 95% or less. In one embodiment of the present invention, 720 cm -1 ~770cm -1 The infrared transmittance of the powder within the range may be characterized as 96% or less, and may be 85% or more, 88% or more, more preferably 90% or more, and more preferably 92% or more. The FT-IR spectrum at 3000 cm⁻¹ -1 ~3600cm -1The fact that the infrared transmittance in the range is within the aforementioned range may mean that the bond by the OH group is relatively weak, which shows a difference from the FT-IR spectrum of a powder consisting of cerium hydroxide particles. Furthermore, the FT-IR spectrum of a powder consisting of cerium oxide particles according to one embodiment of the present invention at 720 cm⁻¹ -1 ~770cm -1 The presence of a peak indicating infrared transmittance within the range may mean that Ce-O stretching occurs within that range, which may mean that particles produced according to one embodiment of the present invention exhibit the characteristics of cerium oxide particles. In particular, in the wet process for producing cerium oxide particles, when synthesized under basic conditions, a process to convert to cerium oxide, such as separate heat treatment or prolonged oxygen exposure, is always required. Therefore, when FT-IR is measured before such a post-process and immediately after the particle synthesis process, there is a risk that peaks related to cerium hydroxide will be detected. In contrast, cerium oxide particles according to one embodiment of the present invention are not produced by a process that first forms cerium hydroxide and then converts it to cerium oxide. Therefore, even if measured immediately after synthesis, only peaks related to cerium oxide can be detected.

[0128] In one embodiment of the present invention, the cerium oxide primary particles may be one or more selected from the group consisting of spherical, cube, tetragonal, orthorhombic, rhombohedral, monoclinic, hexagonal, triclinic, and cuboctahedron shapes, but preferably spherical particles.

[0129] In one embodiment of the present invention, the cerium oxide particles can be produced by a method of growing particles using chemical synthesis, preferably a bottom-up method. Methods for synthesizing the cerium oxide particles include the sol-gel method, supercritical reaction, hydrothermal reaction, or coprecipitation method, and the present invention is not limited thereto. The bottom-up method is a type of chemical synthesis that has recently attracted attention, and involves growing atomic or molecular starting materials into nanometer-sized particles using chemical reactions.

[0130] In one embodiment of the present invention, the abrasive composition comprises wet cerium oxide particles. The wet cerium oxide particles may be any suitable wet cerium oxide particles. For example, the wet cerium oxide particles may be precipitated cerium oxide particles or condensed-polymerized cerium oxide particles, including colloidal cerium oxide particles.

[0131] Furthermore, in one embodiment of the present invention, the wet cerium oxide particles preferably have defects on the surface of the particles. Without attempting to tie to any particular theory, grinding of cerium oxide particles may result in defects on the surface of the cerium oxide particles, and such defects affect the performance of the cerium oxide particles in the chemical mechanical polishing composition. In particular, cerium oxide particles may be crushed when ground, which may expose less favorable surface conditions. This process is referred to as relaxation, in which atoms around the surface of the cerium oxide particles, which have limited reconfiguration ability and limited ability to return to a more favorable state, cause defects to form on the surface of the particles.

[0132] In one embodiment of the present invention, when generating secondary particles of abrasive material, each solvent has its own unique dielectric constant. The dielectric constant of the solvent affects the aggregation and growth of nuclei during powder synthesis by changing the surface energy and surface charge, which in turn affects the size and shape of the powder. The dielectric constant of the solvent and the surface potential (zeta potential) of particles dispersed in the solvent are proportional to each other. If the zeta potential is low, the surface repulsive force between the microparticles or between the nuclei generated by the reaction is small, resulting in an unstable state where aggregation between the microparticles or between the nuclei can occur at a very rapid rate. At this time, the magnitude of the surface repulsive force is approximately the same both between the microparticles and between the nuclei, allowing for aggregation to a uniform size. The secondary particles aggregated in this way will grow into relatively large particles through strong aggregation of primary microparticles or nuclei, or through a particle merging process such as Ostwald ripening, depending on reaction conditions such as temperature and concentration.

[0133] When cerium oxide is used as an abrasive, unlike mechanical polishing which removes only the hydrated layer formed on the surface by the high reactivity of cerium oxide with silicon oxide causing Si-O-Ce chemical bonds, the cerium oxide polishes the silicon oxide film by removing silicon oxide nodules from the surface of the silicon oxide film as if peeling them off. Furthermore, the cerium oxide powder according to the embodiment of the present invention has the advantage of excellent broad-area flatness during polishing due to its low strength caused by its small particle size, and it also solves the problem of micro-scratching caused by large particles.

[0134] The following describes a chemical mechanical polishing slurry composition containing cerium oxide particles and a nitride film passivation modifier according to one aspect of the present invention.

[0135] In one embodiment of the present invention, the aqueous dispersion in which the content of cerium oxide particles is adjusted to 1.0% by weight may be characterized by having an average light transmittance of 50% or more, or 60% or more, with respect to light with a wavelength of 450 to 800 nm, preferably 70% or more, more preferably 80% or more, and even more preferably 90% or more. In another embodiment of the present invention, the dispersion may be characterized by having a light transmittance of 50% or more, 55% or more, 60% or more, 65% or more, 70% or more, 75% or more, or 80% or more, with respect to light with a wavelength of 500 nm. Furthermore, the dispersion may be characterized by having a light transmittance of 75% or more, 80% or more, 85% or more, or 90% or more, with respect to light with a wavelength of 600 nm. In addition, the dispersion may be characterized by having a light transmittance of 87% or more, 90% or more, 93% or more, or 95% or more, with respect to light with a wavelength of 700 nm. The fact that the transmittance value of the slurry composition satisfies the aforementioned range may mean that the primary particle size of the cerium oxide particles according to one aspect of the present invention is small, and that aggregation into secondary particles is even less than that of conventional ceria particles. With such low aggregation, dispersion stability is high and the particles can be uniformly distributed, and the number of particles in contact with the wafer increases, resulting in an exceptionally fast polishing speed of the oxide film. Furthermore, because the particles themselves are minute, it can be easily inferred that the probability of defects such as scratches occurring on the surface when polishing a target film using a slurry composition containing these particles is reduced. In other words, for cerium oxide particles of 10 nm or less relative to the primary particles, it can be predicted that the higher the transmittance in the visible light region, the exceptionally fast the polishing speed of the silicon oxide film should be. Moreover, such transmittance characteristics can be maintained even when further additives such as the cationic polymer and nitride film passivation modifier are included.

[0136] In one aspect of the present invention, the chemical mechanical polishing slurry composition may be characterized by containing cerium oxide particles in an amount of 5% by weight or less relative to the total weight of the chemical mechanical polishing slurry composition. In another aspect of the present invention, the amount of cerium oxide particles relative to the total weight of the chemical mechanical polishing slurry composition may be 4% by weight or less, 3% by weight or less, 2% by weight or less, 1.5% by weight or less, 1% by weight or less, 0.8% by weight or less, 0.5% by weight or less, 0.4% by weight or less, 0.3% by weight or less, 0.2% by weight or less, less than 0.2% by weight, 0.19% by weight or less, 0.15% by weight or less, 0.12% by weight or less, 0.10% by weight or less, 0.09% by weight or less, or 0.07% by weight or less, or 0.0001% by weight or more. The chemical mechanical polishing slurry composition of the present invention may also be characterized in that, even when using a slurry with the same polishing rate, high oxide film polishing efficiency can be achieved even when the cerium oxide particles are added in an even smaller amount relative to the total weight of the chemical mechanical polishing slurry composition.

[0137] In one embodiment of the present invention, the pH of the composition may be characterized by being 2 to 10. In one embodiment of the present invention, the chemical mechanical polishing slurry composition may contain one or more acidic or basic pH adjusting agents and buffers that can adjust the pH considering the final pH of the composition, polishing speed, polishing selectivity ratio, etc. As the pH adjusting agent for adjusting the pH, any agent that can adjust the pH without affecting the properties of the chemical mechanical polishing slurry composition can be used. In one embodiment of the present invention, the pH adjusting agent may be an acidic pH adjusting agent or a basic pH adjusting agent in order to achieve an appropriate pH.

[0138] In one embodiment of the present invention, examples of the pH adjusting agent include one or more inorganic acids selected from the group consisting of sulfuric acid, hydrochloric acid, nitric acid, and phosphoric acid; one or more organic acids selected from the group consisting of acetic acid, citric acid, glutaric acid, glycolic acid, formic acid, lactic acid, malic acid, malonic acid, maleic acid, oxalic acid, phthalic acid, succinic acid, and tartaric acid; imidazoles; alkylamines; alcoholamines; quaternary amine hydroxides; ammonia; or combinations thereof. In particular, the pH adjusting agent may be triethanolamine, tetramethylammonium hydroxide (TMAH or TMAOH), or tetraethylammonium hydroxide (TEAH or TEA-OH). Furthermore, examples of the pH adjusting agent include at least one selected from the group consisting of ammonium methyl propanol (AMP), tetramethylammonium hydroxide (TMAH), potassium hydroxide, sodium hydroxide, magnesium hydroxide, rubidium hydroxide, cesium hydroxide, sodium bicarbonate, sodium carbonate, triethanolamine, tromethamine, and nicotinamide. Preferably, the pH adjusting agent is triethanolamine or aminobutyric acid.

[0139] In one aspect of the present invention, the solvent can be any solvent suitable for use in a chemical mechanical polishing slurry composition, for example, deionized water, but the present invention is not limited thereto. Preferably, ultrapure water can be used. The content of the solvent may be the remaining content of the chemical mechanical polishing slurry composition excluding the content of the cerium oxide particles and other additional additives. In one aspect of the present invention, the solvent may include water (e.g., deionized water) as an aqueous support and may include one or more water-miscible organic solvents. Examples of usable organic solvents include alcohols, such as propenyl alcohol, isopropyl alcohol, ethanol, 1-propanol, methanol, and 1-hexanol; aldehydes, such as acetylaldehyde; ketones, such as acetone, diacetone alcohol, and methyl ethyl ketone; esters, such as ethyl formate, propyl formate, ethyl acetate, methyl acetate, methyl lactate, butyl lactate, and ethyl lactate; sulfoxides, such as dimethyl sulfoxide (DMSO), tetrahydrofuran, dioxane, diglyme, and other ethers; amides, such as N,N-dimethylformamide, dimethylimidazole lydinone, and N-methylpyrrolidone; polyhydric alcohols and their derivatives, such as ethylene glycol, glycerol, diethylene glycol, and diethylene glycol monomethyl ether; and nitrogen-containing organic compounds, such as acetonitrile, amylamine, isopropylamine, and dimethylamine.

[0140] In one embodiment of the present invention, the abrasive composition may further include one or more other additives. The abrasive composition may include rheological modifiers, such as viscosity enhancers and coagulants (e.g., polymer rheological modifiers such as urethane polymers), biocides (e.g., KATHON (trademark) LX), and the like.

[0141] In one embodiment of the present invention, the chemical mechanical polishing slurry composition is characterized by excellent dispersion stability and, in particular, a high polishing rate against silicon oxide films.

[0142] In one aspect of the present invention, the chemical mechanical polishing slurry composition may be characterized by having a silicon oxide film polishing rate of 1,000 Å / min or more, preferably 2,000 Å / min or more, and more preferably 3,000 Å / min or more. Basically, the higher the oxide film polishing rate, the better, and there is no upper limit, but it may be characterized by having a silicon oxide film polishing rate of 10,000 Å / min or less, 9,000 Å / min or less, 8,000 Å / min or less, 7,000 Å / min or less, 6,000 Å / min or less, or 5,000 Å / min or less. In particular, in the case of a chemical mechanical polishing slurry composition using cerium oxide particles according to one aspect of the present invention, even in the range of low cerium oxide particle content, the particle size is small, so the number of particles contained is larger than in conventional slurry compositions containing cerium oxide particles, and the surface Ce 3+ The high content of increases the Si-O-Ce bond, which can significantly increase the polishing speed of the silicon oxide film.

[0143] In one embodiment of the present application, the chemical mechanical polishing slurry composition may have an oxide / nitride polishing selectivity ratio of 50 or more, 100 or more, 150 or more, or 200 or more, and may also be characterized by having an oxide / nitride polishing selectivity ratio of 3,000 or less, 2,000 or less, 1,500 or less, 1,000 or less, 900 or less, or 800 or less. In the case of oxide / nitride selectivity ratio, it should not be ruled out that a selectivity ratio of 3,000 or more can also be achieved by appropriately adjusting the content of cationic polymers.

[0144] A second aspect of the present invention is, The present invention provides a method for manufacturing a semiconductor device, which includes a step of polishing using the aforementioned chemical mechanical polishing slurry composition.

[0145] Although detailed explanations have been omitted for parts that overlap with the first aspect of the present invention, the content described in the first aspect of the present invention is similarly applicable even if the explanation is omitted in the second aspect.

[0146] The method for manufacturing a semiconductor device according to the second aspect of the present invention will be described in detail below.

[0147] First, regarding the shallow trench isolation (STI) routine process, among the processes for planarizing the insulating film, photo-etching, etching, and polishing can be classified as basic processes that are commonly applied.

[0148] The process can begin with the photoprocessing, which is the first step in separating the elements. The photoprocessing is carried out in an exposure apparatus that uses auxiliary equipment called a track and light to transfer the circuit pattern (mask) onto the wafer. First, a photosensitive agent (photoresistor) is applied, but because the photosensitive agent has high viscosity, it is applied thinly on the insulating film while the wafer is rotated. The appropriate depth of exposure is achieved only when the applied photosensitive agent is at a uniform height. If the depth of exposure is insufficient during exposure, photosensitive agent residue will remain during development, resulting in the lower film (insulating layer) not being properly removed in the subsequent etching process. After exposure, the wafer is moved back to the track equipment and the development process proceeds to remove the photosensitive areas.

[0149] The second step, etching of the STI, is the process of removing the insulating layer (oxide layer + nitride layer) and a portion of the substrate, which is the part immediately below the developed area (the area from which the photosensitive film has been removed). For this etching process, either a dry etching process or a wet etching process can be used. Dry etching is typically a method that uses a plasma state to excavate. Compared to wet etching (liquid), dry etching only excavates downwards without etching the side walls (anisotropic etching), which may be advantageous in maintaining the trench shape. In this case, there is a risk of over-etching, so it should be necessary to proceed after accurately calculating the end point of the etching. After etching, residue will remain, which may be treated.

[0150] After etching the trench shape, the photosensitive layer becomes unnecessary and may be removed using ashing. Preferably, the ashing process may be carried out using plasma, which allows for a more precise ashing process. The shape of the semiconductor device after the ashing process is shown in Figure 2a.

[0151] A method for manufacturing a semiconductor device according to one aspect of the present invention may include the step of simultaneously polishing a silicon oxide film, a silicon nitride film, and a polysilicon film using the chemical mechanical polishing slurry composition.

[0152] Figures 2a to 2e are cross-sectional views showing a method for manufacturing a semiconductor device according to one aspect of the present invention.

[0153] Referring to Figure 2a, a trench 13 may be formed within the upper film 11 on the lower film 10. For example, the upper film 11 may be formed on the lower film 10, and a nitride film (polishing stop film) 12 may be formed on the upper film 11. The lower film 10 may comprise any material film. For example, the lower film 10 may be an insulating film, a conductive film, a semiconductor film, or a semiconductor wafer (substrate). The upper film 11 may comprise an insulating film (oxide film), a conductive film, a semiconductor film, or a combination thereof.

[0154] If the upper film 11 includes multiple stacked insulating films, these insulating films may be of the same type or of different types. For example, the upper film 11 may comprise alternating and repeatedly stacked silicon oxide films and silicon nitride films. The upper film 11 may further comprise a semiconductor film and a lower insulating film beneath the silicon oxide and silicon nitride films. For example, the lower insulating film may be located beneath the semiconductor film.

[0155] The nitride film (polishing stop film) 12 may be formed to have a relatively large thickness (e.g., 100 Å to 4,000 Å) by depositing, for example, silicon nitride (e.g., SiN), polysilicon, metal nitride (e.g., TiN), or metal. The trench 13 may be formed by an etching process or a drilling process. The trench 13 may have a depth such that it penetrates the nitride film (polishing stop film) 12 and the upper film 11 to reach the lower film 10. For example, the trench 13 may have a sufficient depth to expose the lower film 10.

[0156] Referring to Figure 2b, in STI, a double oxide film may be formed. First, before filling the trench 13 with insulating material in full, a thin liner oxide film is coated as a first insulating film 14 by diffusion. This is considered to ensure that the second insulating film, which is formed on the silicon substrate by chemical vapor deposition (CVD) in the subsequent step, is successfully formed. According to another aspect of the present invention, it can also serve to prevent damage from high-energy plasma when filling the trench 13 by high-density plasma CVD (HDPCVD). According to one aspect of the present invention, the first insulating film (liner oxide film) can be formed as a thin film, such as a gate oxide film, by introducing oxygen gas into a furnace to be diffused and heating it to a high temperature. Also, according to another aspect of the present invention, a nitride film may be used instead of an oxide film.

[0157] Referring to Figure 2c, a first insulating film 14 and a second insulating film 15 may be formed by depositing multiple insulators to fill the trench 13. The density and deposition rate of the first insulating film 14 and the second insulating film 15 may differ from each other. According to embodiments of the present invention, the first insulating film 14 may be formed by depositing a high-density insulator, and the second insulating film 15 may be formed by depositing a low-density insulator. For example, the first insulating film 14 may be formed by depositing and patterning a high-density plasma (HDP) oxide. The first insulating film 14 may be formed in a shape that extends along the inner surface of the trench 13. For example, the first insulating film 14 may have a U-shape or pipe shape that opens upwards.

[0158] Because the first insulating film 14 has high density, voids are less likely to form within it, thereby eliminating or significantly reducing the occurrence of cracks caused by voids during subsequent heat treatment processes. The second insulating film 15 may be formed, for example, by depositing tetraethyl orthosilicate (TEOS) oxide to a thickness sufficient to cover the polishing stop film 12 while filling the trench 13 with the first insulating film 14. The second insulating film 15 can be formed at an even higher deposition rate than the first insulating film 14. The high deposition rate of the second insulating film 15 allows the trench 13 to be filled relatively quickly by the second insulating film 15.

[0159] In another aspect of the present invention, although not shown, the second insulating film 15 may be partially removed, leaving some of it on the trench 13. For example, the second insulating film 15 may be selectively removed to restrict or open a specific region, such as the cell memory region of a semiconductor device, through a photoprocessing and etching process. This makes it possible to remove some or all of the second insulating film 15 on the polishing stop film 12, while leaving some of the second insulating film 15 on the trench 13. The process of opening the specific region is carried out selectively, not necessarily.

[0160] Referring to Figure 2d, a planarization process may be carried out on the second insulating film 15. For example, the second insulating film 15 may be planarized by a chemical mechanical polishing (CMP) process. The chemical mechanical polishing process may be continued until the nitride film (polishing stop film) 12 is exposed. The chemical mechanical polishing process may be carried out after the formation of the second insulating film 15 in Figure 2b. In this case, the chemical mechanical polishing process can be easily carried out because the surface on the nitride film (polishing stop film) 12 is relatively flat, or even if it is not flat, its non-flatness is not severe.

[0161] Referring to Figure 2e, the nitride film may be removed to form an STI region. The nitride film serves to protect the upper film 11 from being affected by the first insulating film 14. The upper film 11 may become a gate oxide film that is thin and must be highly reliable, so it must be handled carefully. When removing the nitride film by etching (wet etching), the wafer may be immersed in a chemical solution so that only the nitride film is etched and the oxide film is not etched. For this purpose, a solution with a high selectivity ratio (etching ratio) for the nitride film can be used. In another embodiment of the present invention, the nitride film may also be removed by CMP. In this case, it is not necessary to proceed with etching the nitride film, but since it may physically damage the oxide film, it is preferable to chemically treat the nitride film by etching to protect the oxide film.

[0162] In another aspect of the present invention, the chemical mechanical polishing (CMP) step involves removing all of the first insulating film 14 and the second insulating film 15 on top of the nitride film (polishing stop film) 12 after the gap has been filled, thereby isolating the active region from the field region, and the step may be divided into three main steps, as shown in Figure 2f.

[0163] In the first step, the second insulating film 15 is subjected to bulk CMP on the platen while local planarization is performed. In the second step, the second insulating film 15, whose step level has been reduced, is cleaned or polished on the platen, and polishing is stopped when the nitride film (polishing stop film) 12 is exposed. At this time, End Point Detection (EPD) is used to sense the point at which different film materials are exposed. In the third step, any residue of the second insulating film 15 that may remain on the nitride film (polishing stop film) 12 is removed on the platen, and the nitride film and oxide film materials may be polished and targeted.

[0164] Figure 2g shows the structure of a chemical mechanical polishing (CMP) apparatus according to one embodiment of the present invention. This apparatus is characterized by having three platens, and as described above, it may be structured in which the STI CMP is carried out in stages as the platens 1, 2, and 3 are passed in that order. After polishing is complete, the apparatus moves to the cleaning section, and after cleaning is completed, the process is finished.

[0165] In addition, in a method for manufacturing a semiconductor device according to one aspect of the present invention, any conventional polishing method and conditions that are not limited to the present invention can be used as a method for simultaneously polishing a silicon oxide film, a silicon nitride film, and a polysilicon film using the chemical mechanical polishing slurry composition, and the present invention is not particularly limited in this regard.

[0166] A chemical mechanical polishing slurry composition according to one aspect of the present invention has high dispersion stability, and moreover, the Ce on the surface of the cerium oxide particles contained in the slurry composition 3+ Due to its high ceria content, the chemical polishing mechanism that forms Si-O-Ce between silica and cerium can increase the polishing rate on silicon-containing substrates, making it effective for removing silicon oxide films from the surface of semiconductor devices, especially during the CMP process, even under conditions where ceria content is low.

[0167] A third aspect of the present invention is, The present invention provides a semiconductor device comprising a substrate and a trench formed on the substrate and filled with an insulating material, wherein the trench is formed by polishing at least one film selected from the group consisting of a silicon oxide film, a silicon nitride film, and a polysilicon film using a chemical mechanical polishing slurry composition, and the chemical mechanical polishing slurry composition comprises cerium oxide particles, a solvent, a cationic polymer, and a nitride film passivation modifier.

[0168] While detailed explanations have been omitted for parts that overlap with the first and second aspects of the present invention, the content described for the first and second aspects of the present invention is similarly applicable even if its explanation is omitted in the third aspect.

[0169] A fourth aspect of the present invention is, The steps include preparing the raw material precursors, A step of obtaining a dispersion of cerium oxide particles for chemical and mechanical polishing by crushing or precipitating cerium oxide particles in a solution containing a raw material precursor, This invention provides a method for producing cerium oxide particles containing the specified material.

[0170] While detailed explanations have been omitted for parts that overlap with the first to third aspects of the present invention, the content described for the first to third aspects of the present invention is similarly applicable even if its explanation is omitted in the fourth aspect.

[0171] In one embodiment of the present invention, the method for producing cerium oxide particles may include a step of preparing a raw material precursor. The raw material precursor can be used without limitation as long as it is a precursor material capable of producing cerium oxide particles, which are the product.

[0172] In one embodiment of the present invention, the method for producing cerium oxide particles may include the step of grinding or precipitating cerium oxide particles in a solution containing a raw material precursor to obtain a dispersion of cerium oxide particles for chemical and mechanical polishing. The step of grinding the cerium oxide particles in a solution containing a raw material precursor may be, for example, grinding using a milling process, and the grinding method can be determined without limitation within the scope of the common technical knowledge of an ordinary person. In the case of the step of precipitating cerium oxide particles in a solution containing a raw material precursor to obtain a dispersion of cerium oxide particles, the method may further include the step of removing the supernatant or filtering.

[0173] In particular, in one embodiment of the present invention, all processes of particle synthesis can be carried out at room temperature and without going through a basic pH, which has the advantage of achieving an energy-efficient manufacturing process while exhibiting the aforementioned particle characteristics.

[0174] The above description of the present invention is for illustrative purposes only, and a person with ordinary skill in the art to which the present invention pertains will understand that it can be easily modified into other specific forms without altering the technical idea or essential features of the present invention. Therefore, the above-described embodiments should be understood to be illustrative in all respects and not limiting. For example, each component described as being single-type may be implemented in a distributed manner, and similarly, components described as distributed may be implemented in a combined manner.

[0175] The scope of the present invention is expressed by the appended claims, and any modifications or alterations derived from the meaning and scope of the claims, as well as the concept of equivalents thereof, should be construed as being included within the scope of the present invention. [Industrial applicability]

[0176] According to an embodiment of the present invention, the manufactured cerium oxide particles have a Ce on the surface of the cerium oxide. 3+ By increasing the proportion of cerium oxide particles, these particles, despite their small particle size, have the characteristic of being able to remove oxide films at a high rate even at low concentrations when included in chemical mechanical polishing slurries. Furthermore, when combined with the composition of the surface treatment agent disclosed in this invention, the zeta potential of the cerium oxide particles' surface can be converted to a negative value, expanding their applications to various uses such as polishing nitride films. This provides an improved effect compared to when no additives are added, thus offering potential for industrial use.

Claims

1. Cerium oxide particles produced by the step of precipitating a particle in a solution containing a raw material precursor at an acidic pH to obtain a dispersion of particles, Solvent and, Cationic polymers and, Nitride film passivation modifier, Includes, The nitride film passivation modifier is a sugar that is a hexasaccharide selected from the group consisting of glucose, mannose, galactose, talose, altrose, and allose; one or more monosaccharides selected from the group consisting of ribose, arabinose, and xylose; one or more disaccharides selected from the group consisting of sucrose, lactose, maltose, lactulose, trehalose, and cellobiose; or a polysaccharide of starch or cellulose. The chemical mechanical polishing slurry composition has an oxide film / nitride film polishing selectivity ratio of 200 to 2,000. The secondary particle size of the cerium oxide particles, as measured by a dynamic light scattering (DLS) particle size distribution analyzer, was 15 nm or less. A chemical mechanical polishing slurry composition characterized in that, in an aqueous dispersion in which the content of cerium oxide particles is adjusted to 1.0% by weight, the average light transmittance for wavelength light in the 450 to 800 nm region is 50% or more.

2. The chemical mechanical polishing slurry composition according to claim 1, characterized in that the polishing rate of the oxide film increases depending on the content of the cationic polymer.

3. The chemical mechanical polishing slurry composition according to claim 1, characterized in that the nitride film passivation modifier reduces the polishing rate of the nitride film depending on its content.

4. The chemical mechanical polishing slurry composition according to claim 1, characterized in that the content of the nitride film passivation modifier is 0.001 to 1% by weight with respect to the total weight of the chemical mechanical polishing slurry composition.

5. The chemical mechanical polishing slurry composition according to claim 1, characterized in that the content of the cationic polymer is 0.001 to 1% by weight of the total weight of the chemical mechanical polishing slurry composition.

6. The cationic polymers are polydiallyldimethylammonium chloride (Poly(DADMAC)), polydiethylenetriamine 2-(dimethylamino)ethyl methacrylate (Poly(DMAEM)), poly 2-(dimethylamino)ethyl methacrylate (Poly(DMAEM)), and polyacrylamide decamethylenediamine. The chemical mechanical polishing slurry composition according to claim 1, characterized by comprising dimethylamine, Poly(Aam_DCDA), poly(dimethylamine)-co-epichlorohydrin, poly(dimethylamine)-co-epichlorohydrin-co-ethylenediamine, or a combination thereof.

7. The chemical mechanical polishing slurry composition according to claim 1, characterized in that it contains 0.001 to 5% by weight of cerium oxide particles based on the total weight of the chemical mechanical polishing slurry composition.

8. The chemical mechanical polishing slurry composition further comprises a pH adjusting agent, The pH adjusting agent is one or more inorganic acids selected from the group consisting of sulfuric acid, hydrochloric acid, nitric acid, and phosphoric acid, or one or more organic acids selected from the group consisting of acetic acid, citric acid, glutaric acid, glycolic acid, formic acid, lactic acid, malic acid, malonic acid, maleic acid, oxalic acid, phthalic acid, succinic acid, and tartaric acid. The chemical mechanical polishing slurry composition according to claim 1, characterized by comprising imidazole, alkylamines, alcoholamines, quaternary amine hydroxides, ammonia, or a combination thereof.

9. The chemical mechanical polishing slurry composition according to claim 1, characterized in that the pH of the composition is 2 to 10.

10. The chemical mechanical polishing slurry composition according to claim 1, characterized in that it has a silicon oxide film polishing rate of 1,000 to 5,000 Å / min.

11. The chemical mechanical polishing slurry composition according to claim 1, characterized in that the primary particle size of the cerium oxide particles, as measured by electron transmission microscope (TEM), is 0.5 to 10 nm.

12. In the analysis by X-ray photoelectron spectroscopy (XPS), compared to 100% of the total XPS peak area representing the Ce-O bond energy on the surface of the cerium oxide particles, Ce 3+ The chemical mechanical polishing slurry composition according to claim 1, characterized in that the sum of the XPS peak areas indicating the Ce-O bond energy is 30% or more.

13. A method for manufacturing a semiconductor device, comprising the step of polishing using the chemical mechanical polishing slurry composition described in claim 1.

Citation Information

Patent Citations

  • Polishing liquid composition

    JP2019102476A

  • Methods and compositions for processing dielectric substrate

    KR1020180038051A

  • Chemical-mechanical polishing slurry composition for polishing low temperature polysilicon hillock and low temperature polysilicon hillock polishing method using the same

    KR1020200037613A

  • Chemical mechanical planarization slurry composition comprising composite particles, process for removing material using said composition, CMP polishing pad and process for preparing said composition

    WO2014179419A1

  • Cerium oxide particles, chemical mechanical polishing slurry composition comprising same, and method for manufacturing semiconductor device

    WO2022045856A1