Ion-conductive thin film composites for energy storage applications
Low-cost, high-performance TFC membranes with a hydrophilic ionomer polymer coating between microporous support films address the high cost and crossover issues of conventional membranes, enhancing the stability and efficiency of redox flow batteries.
Patent Information
- Application Number
- JP2025537030
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-12-29
- Filing Date
- 2023-12-21
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-12-21
AI Technical Summary
Existing redox flow batteries face challenges due to high costs and electrolyte crossover issues with conventional membranes, limiting their widespread adoption for grid energy storage applications.
Development of low-cost, high-performance ion-conducting thin-film composite (TFC) membranes that combine a size-excluded ion-conductivity separation mechanism with an ion-exchange ion-conductivity separation mechanism, using a hydrophilic ionomer polymer coating sandwiched between microporous support films to enhance stability and reduce electrolyte crossover.
The TFC membranes exhibit improved performance with enhanced membrane stability, lower area resistivity, higher voltage and coulombic efficiency, and energy efficiency, demonstrating stability against damage during battery assembly and operation.
Abstract
Description
[Technical Field]
[0001] (Priority statement) This application claims priority to U.S. Provisional Patent Application No. 63 / 477,591, filed December 29, 2022, which is incorporated herein by reference in its entirety. [Background technology]
[0002] Energy storage systems have played a crucial role in collecting energy from various sources. They can be used to store energy and convert it for use in many different applications, such as buildings, transportation, utilities, and industry. Various energy storage systems are commercially used, and new systems are currently under development. Types of energy storage systems can be classified as electrochemical and battery, thermal, thermochemical, flywheel, compressed air, pumped-storage hydroelectric, magnetic, biological, chemical, and hydrogen energy storage. To address the energy crisis and overcome the mismatch between power generation and end-use, the development of cost-effective and environmentally friendly energy storage systems is necessary.
[0003] Renewable energy sources such as wind and solar power have transient characteristics that require energy storage. Renewable energy storage systems such as redox flow batteries (RFBs) are attracting significant attention for power grids, electric vehicles, and other large-scale stationary applications. RFBs are electrochemical energy storage systems that reversibly convert chemical energy directly into electricity. By converting electricity into hydrogen as an energy carrier via water electrolysis without producing carbon monoxide or carbon dioxide as byproducts, it becomes possible to connect the fields of electricity, chemistry, mobility, and heating. Water electrolysis produces high-quality hydrogen by electrochemically decomposing water into hydrogen and oxygen. When the process is powered by renewable energy sources such as wind, solar, or geothermal energy, the carbon footprint of water electrolysis is zero. Major water electrolysis technologies include alkaline electrolysis, polymer electrolyte membrane (PEM) electrolysis, and solid oxide electrolysis. PEM water electrolysis is one of the preferred methods for converting renewable energy into high-purity hydrogen, offering advantages such as a compact design, high current density, high efficiency, fast response, low footprint, low temperature operation (20-90°C), and high-purity oxygen byproducts.
[0004] An RFB consists of a flow cell with two tanks filled with an active material containing metal ions that can be in different valence states, two circulation pumps, and a separation membrane. The separation membrane is placed between the anode and cathode and is used to separate the anode and cathode liquids, as well as to utilize the current circuit by allowing the movement of equilibrium ions. Of all the redox flow batteries developed to date, the all-vanadium redox flow battery (VRFB) is the most widely studied. VRFBs use the same element vanadium in both half-cells, preventing crossover contamination of the electrolyte from one half-cell to the other. However, VRFBs are inherently expensive due to the use of high-cost vanadium and expensive membranes. All-iron redox flow batteries (IFBs) are particularly attractive for grid-scale storage applications because they use low-cost iron, salt, and water as electrolytes.
[0005] Membranes are one of the key materials that make up batteries or electrolytic cells, serving as a crucial factor for safety and performance. Some important properties of membranes for flow batteries, fuel cells, and membrane electrolysis include high conductivity, high ion permeability (porosity, pore size, and pore size distribution), high ion exchange capacity (for ion exchange membranes), high ion / electrolyte selectivity (low permeability / crossover to electrolytes), and low cost ($150-$200 / m²). 2 Advantages include low area resistance to minimize efficiency losses due to ohmic polarization, high resistance to oxidation and reduction conditions, chemical inertness over a wide pH range, high thermal stability (above 120°C in the case of fuel cells) along with high proton conductivity, high proton conductivity at high T without using H2O, high proton conductivity at high T while maintaining high RH, and high mechanical strength (thickness, low swelling).
[0006] Two main types of membranes for redox flow batteries, fuel cells, and electrolysis applications are polymer ion exchange membranes and microporous separators. Polymer ion exchange membranes include -SO3 - , -COO - , -PO3 2- , -PO3H - , or -C6H4O - cation exchange membranes containing cation exchange functional groups, -NH3 + , -NRH2 + , -NR2H + , or -NR3 + anion exchange membranes containing anion exchange functional groups, or bipolar membranes containing both cation exchange polymers and anion exchange polymers. Polymers for the preparation of ion exchange membranes may be perfluorinated ionomers such as Nafion®, Flemion®, and NEOSEPTA®-F, partially fluorinated polymers, non-fluorinated hydrocarbon polymers, non-fluorinated polymers with aromatic backbones, or acid-base blends. In general, perfluorosulfonic acid (PFSA) based membranes, such as Nafion® and Flemion®, are used in vanadium redox flow battery (VRFB) systems due to their oxidative stability, good ionic conductivity, unique morphology, mechanical strength, and high electrochemical performance. However, these membranes have low equilibrium ion / electrolyte ion selectivity and high crossover of electrolyte metal ions, causing capacity fade in VRFBs, and are expensive.
[0007] Microporous and nanoporous membrane separators may be inert microporous / nanoporous polymer membrane separators, inert nonwoven porous films, or polymer / inorganic material coated / impregnated separators. Inert microporous / nanoporous polymer membrane separators may be microporous polyethylene (PE), polypropylene (PP), PE / PP, or composite inorganic / PE / PP membranes, inert nonwoven porous films, nonwoven PE, PP, polyamide (PA), polytetrafluoroethylene (PTFE), polyvinyl chloride (PVC), polyvinylidene fluoride (PVDF), polyethylene terephthalate (PET), or polyester porous films. For example, microporous Daramic® membrane separators and Celgard® membrane separators made from PE polymer or PP polymer are commercially available. These typically possess high ionic conductivity, but also have high electrolyte crossover for RFB applications.
[0008] Despite extensive research efforts, widespread adoption of redox flow batteries for grid energy storage applications remains a challenge.
[0009] Therefore, there is a need for reliable, high-performance (low electrolyte or gas crossover and excellent conductivity), and low-cost membranes for energy storage applications such as redox flow batteries, fuel cells, and electrolytic applications. [Modes for carrying out the invention]
[0010] Low-cost, high-performance ion-conducting thin-film composite (TFC) membranes have been previously developed for energy storage applications such as redox flow batteries, fuel cells, and electrolytic applications. These TFC membranes provide ion-conducting membranes that combine a size-excluded ion-conductivity separation mechanism derived from the hydrophilicity of the polymer with an ion-exchange ion-conductivity separation mechanism derived from the ionomerity of the polymer. Ion-conducting TFC membranes exhibit improved performance compared to conventional polymer ion-exchange membranes with an ion-exchange ion-conductivity separation mechanism and microporous membrane separators with a size-excluded ion-conductivity separation mechanism. A TFC membrane comprises a microporous support membrane and a hydrophilic ionomer polymer coating layer on the surface of the microporous support membrane. The ionomer polymer can also be present within the micropores of the support membrane. The hydrophilic ionomer polymer coating layer is ion-conductive. This means that the hydrophilic ionomer polymer coating has ion conductivity and can transmit protons or chloride ions (Cl - This means that the electrical circuit can be maintained by transporting charge-carrying ions, such as protons, chloride ions, potassium ions, or sodium ions in an all-iron redox flow battery system, across a membrane containing a hydrophilic ionomer polymer coating layer during the operation of the battery cell.
[0011] The ionic conductivity (σ) of a membrane is a measure of its ability to conduct charge-bearing ions, and the unit of measurement for conductivity is siemens per meter (S / m). The ionic conductivity (σ) of an ion-conductive TFC membrane can be measured by determining the resistance (R) of the membrane between two electrodes separated by a fixed distance. Resistance is determined by electrochemical impedance spectroscopy (EIS), and the unit of measurement for resistance is ohms (Ω). Membrane area specific resistance (RA) is the product of the membrane resistance (R) and the membrane active area (A), and the unit of measurement for membrane area specific resistance is (Ω·cm). 2The film ionic conductivity (σ, S / cm) is proportional to the film thickness (L, cm), and the film area resistivity (RA, Ω·cm) is proportional to the film thickness (L, cm). 2 ) is inversely proportional. The performance of ion-conducting TFC membranes for RFB applications is evaluated by several parameters of the RFB cell, including membrane solubility and stability in the electrolyte, area resistivity, battery charge / discharge cycle count, electrolyte crossover through the membrane, voltage efficiency (VE), coulombic efficiency (CE), and energy efficiency (EE). CE is the ratio of the cell's discharge capacity to its charge capacity. Higher CEs, indicating lower capacity loss, are mainly due to lower crossover rates of electrolyte ions such as ferric and ferrous ions in iron redox flow battery systems. VE is defined as the ratio of the cell's average discharge voltage to its average charge voltage (see M. Skyllas-Kazacos, C. Menictas, and T. Lim, Chapter 12 on Redox Flow Batteries for Medium-to Large-Scale Energy Storage in Electricity Transmission, Distribution and Storage Systems, A volume in Woodhead Publishing Series in Energy, 2013). Higher VE, which indicates higher ionic conductivity, is mainly due to a lower area resistivity of the film. EE is the product of VE and CE, and is an indicator of energy loss during the charge-discharge process. EE is an important parameter for evaluating energy storage systems.
[0012] By incorporating a low-cost, high-performance hydrophilic ionomer polymer into a TFC membrane, an ion-conducting membrane is provided that combines a size-excluded ion-conductivity separation mechanism derived from the polymer's hydrophilicity with an ion-exchange ion-conductivity separation mechanism derived from the polymer's ionomerity. Therefore, the ion-conducting TFC membrane exhibits improved performance for energy storage applications, such as redox flow batteries, compared to conventional polymer ion-exchange membranes with an ion-exchange ion-conductivity separation mechanism and microporous membrane separators with a size-excluded ion-conductivity separation mechanism. For redox flow battery applications, the ion-conducting TFC membrane demonstrated excellent membrane stability in the electrolyte, low area resistivity, high battery charge / discharge cycle count, low electrolyte crossover across the membrane, and high VE, CE, and EE.
[0013] However, it was found that the hydrophilic ionomer polymer coating layer on the surface of the microporous support film near the sealing region of the battery cells can be damaged during stack assembly. The coating layer can also be damaged by fibers on the carbon felt electrodes during battery stack assembly or battery operation. This damage can lead to a decrease in server performance.
[0014] To avoid this potential damage, a new low-cost, high-performance ion-conducting TFC film has been developed. The new TFC film comprises a first microporous support film, a hydrophilic ionomer polymer coating layer on the surface of the first microporous support film, and a second microporous support film on the surface of the hydrophilic ionomer polymer coating layer opposite the first microporous support film. This forms a sandwich structure in which the hydrophilic ionomer polymer coating is positioned between the two microporous support films and protected by them. The second microporous support film may be adhered to a second surface of the hydrophilic ionomer polymer coating layer. Alternatively, the second microporous support film may be positioned adjacent to the hydrophilic ionomer polymer coating layer without being adhered to it.
[0015] Hydrophilic ionomer polymers are hydrophilic ionomer polymers, or electrically neutral repeating units, and -SO3 - Group, -COO - Group, -PO3 2- group, -PO3H - group, -C6H4O - group, -O4B - group, -NH3 + group, -NRH2 + Group, -NR2H + group, -NR3 + Base, or -SR2 - The product contains a crosslinked hydrophilic ionomer polymer that includes repeating units of both a small amount of ionic functional group and a small amount of ionic functional group. The hydrophilic ionomer polymer is -SO3 - Group, -COO - Base, or -NH3 + It contains polar groups or charged functional groups with high water affinity, such as ions. Crosslinked hydrophilic polymers include hydrophilic polymers complexed with complexing agents such as polyphosphate, boric acid, metal ions, or mixtures thereof. Hydrophilic ionomer polymers have high stability in aqueous electrolyte solutions due to their insolubility in aqueous electrolyte solutions, as well as their hydrophilicity and ionomerity due to their compatibility with water and H3O + or Cl - It has a high affinity for charge-carrying ions such as these, and therefore possesses high ionic conductivity and low film specific area resistance.
[0016] The hydrophilic ionomer polymer coating layer on the ion-conducting TFC film typically includes a dense layer having a thickness in the range of 1 to 100 micrometers, or 5 to 50 micrometers. The high-density hydrophilic ionomer polymer coating layer forms very small nanopores with a pore diameter of less than 0.5 nm in the presence of liquid water or water vapor, and in some cases, combined with the presence of a crosslinked polymer structure via a complexing agent to control the degree of polymer swelling, resulting in high selectivity for charge-carrying ions such as protons, hydrated protons, chloride ions, potassium ions, hydrated potassium ions, sodium ions, and hydrated sodium ions to electrolytes such as ferric ions, hydrated ferric ions, ferrous ions, and hydrated ferrous ions.
[0017] Suitable hydrophilic ionomer polymers include, but are not limited to, polyphosphate-complexed polysaccharide polymers, polyphosphate and metal ion-complexed polysaccharide polymers, metal ion-complexed polysaccharide polymers, borate-complexed polysaccharide polymers, alginate polymers such as sodium alginate, potassium alginate, calcium alginate, and ammonium alginate, alginate polymers, hyaluronic acid polymers, borate-complexed polyvinyl alcohol polymers, polyphosphate-complexed polyvinyl alcohol polymers, polyphosphate and metal ion-complexed polyvinyl alcohol polymers, metal ion-complexed poly(acrylic acid) polymers, borate-complexed poly(acrylic acid) polymers, metal ion-complexed poly(methacrylic acid), borate-complexed poly(methacrylic acid), or combinations thereof.
[0018] Various types of polysaccharide polymers can be used, including but not limited to chitosan, sodium alginate, potassium alginate, calcium alginate, ammonium alginate, alginic acid, sodium hyaluronate, potassium hyaluronate, calcium hyaluronate, ammonium hyaluronate, hyaluronic acid, dextran, pullulan, carboxymethyl curdlan, sodium carboxymethyl curdlan, potassium carboxymethyl curdlan, calcium carboxymethyl curdlan, ammonium carboxymethyl curdlan, κ-carrageenan, λ-carrageenan, ι-carrageenan, carboxymethyl cellulose, sodium carboxymethyl cellulose, potassium carboxymethyl cellulose, calcium carboxymethyl cellulose, ammonium carboxymethyl cellulose, pectic acid, chitin, chondroitin, xanthan gum, or a combination thereof.
[0019] In some embodiments, the hydrophilic ionomer polymer is a polyphosphate-complexed chitosan polymer, a polyphosphate and metal ion-complexed chitosan polymer, a metal ion-complexed alginate polymer, or a combination thereof.
[0020] In some embodiments, the hydrophilic ionomer polymer is a boric acid-complexed polyvinyl alcohol polymer, a boric acid-complexed alginic acid, or a blend of boric acid-complexed polyvinyl alcohol and an alginate polymer.
[0021] In some embodiments, the metal ion complexing agent is a ferric ion, a ferrous ion, or a vanadium ion.
[0022] In some embodiments, the hydrophilic ionomer polymer is present within the micropores of the first microporous support membrane.
[0023] The first and second microporous support films should possess good thermal stability (stable up to at least 100°C), high aqueous and organic solution resistance under low pH conditions (e.g., pH less than 6) (insoluble in aqueous and organic solutions), high resistance to oxidation and reduction conditions (no insolubility and performance degradation under oxidation and reduction conditions), high mechanical strength (no dimensional change under system operating conditions), and other factors determined by the operating conditions for energy storage applications. The first and second microporous support films should be compatible with cell chemistry and meet the mechanical requirements of cell lamination or winding assembly operations. The microporous support films should have high ionic conductivity but low selectivity for charge-carrying ions such as protons, hydrated protons, chloride ions, potassium ions, sodium ions, hydrated potassium ions, and hydrated sodium ions, and electrolytes such as ferric ions, hydrated ferric ions, ferrous ions, and hydrated ferrous ions.
[0024] The first microporous support membrane and the second microporous support membrane can be made from the same material or different materials.
[0025] Polymers suitable for the preparation of the first and second microporous support films can be selected from, but are not limited to, polyolefins such as polyethylene and polypropylene, mixtures of polyethylene and silica particles, mixtures of polypropylene and silica particles, polyamides such as nylon 6 and nylon 6,6, polyacrylonitrile, polyethersulfone, sulfonated polyethersulfone, polysulfone, sulfonated polysulfone, poly(etheretherketone), sulfonated poly(etheretherketone), polyester, cellulose acetate, cellulose triacetate, polybenzimidazole, polyimide, polyvinylidene fluoride, polycarbonate, cellulose, or combinations thereof. These polymers offer a range of properties, including low cost, high stability in water and electrolytes over a wide pH range, good mechanical stability, and ease of processability for film formation.
[0026] The first and second microporous support films may have either a symmetrical or asymmetrical porous structure. Asymmetrical microporous support films can be formed by a phase inversion deposition approach followed by direct air drying, or by a phase inversion followed by solvent exchange. The first and second microporous support films may also be produced by dry processing or wet processing of thermoplastic polyolefins. Dry processing of thermoplastic polyolefins utilizes extrusion to raise the polymer above its melting point and shape it into the desired form. Subsequent annealing and stretching processes may be performed to increase the crystallinity, orientation, and size of the micropores. Wet processing of polyolefin separators utilizes a hydrocarbon liquid or low molecular weight oil mixed with a polymer resin or a mixture of polymer resin and inorganic nanoparticles in a molten phase. The molten mixture is extruded through a die similar to that used for dry-processed separators. The thickness of the microporous support film may be in the range of 10 to 1000 micrometers, or 10 to 900 micrometers, or 10 to 800 micrometers, or 10 to 700 micrometers, or 10 to 600 micrometers, or 10 to 500 micrometers, or 20 to 500 micrometers. The pore size of the microporous film may be in the range of 10 nanometers to 50 micrometers, or 50 nanometers to 10 micrometers, or 0.2 micrometers to 1 micrometer.
[0027] Another aspect of the present invention is a method for producing a TFC film. In one embodiment, the method includes applying a layer of aqueous solution containing a hydrophilic ionomer polymer to one surface of a first microporous support film; drying the coated film; optionally, complexing the hydrophilic ionomer polymer using a complexing agent to form a crosslinked hydrophilic ionomer polymer; and applying a second microporous support film to the coated film on the opposite surface of the first microporous support film.
[0028] In some embodiments, the coated film is dried before the hydrophilic ionomer polymer is complexed. In other embodiments, the coated film is dried after the hydrophilic polymer is complexed. In other embodiments, the coated film is dried before the hydrophilic ionomer polymer is complexed, and then dried again after the hydrophilic polymer is complexed. The coated film may be dried for a time ranging from 5 minutes to 5 hours, or 5 minutes to 4 hours, or 5 minutes to 3 hours, or 10 minutes to 2 hours, or 30 minutes to 1 hour, at a temperature ranging from 40°C to 100°C, or 40°C to 80°C, or 55°C to 65°C.
[0029] In some embodiments, the second microporous film is applied to the coated film after the coated film has been dried.
[0030] In some embodiments, the complexing agent is selected from polyphosphate, boric acid, ferric ions, ferrous ions, or vanadium ions, or a combination thereof.
[0031] In some embodiments, complexing a hydrophilic ionomer polymer involves immersing a dried, coated film in a second aqueous solution of polyphosphate, boric acid, a metal salt, hydrochloric acid, or a combination thereof.
[0032] In some embodiments, complexing a hydrophilic ionomer polymer involves in situ complexing a dried, coated film together with a second microporous support film using a complexing agent within a redox flow battery cell.
[0033] In some embodiments, the aqueous solution contains acetic acid or other inorganic or organic acids.
[0034] In some embodiments, the hydrophilic ionomer polymer on the coated film is treated in an aqueous solution of hydrochloric acid before the hydrophilic polymer is complexed.
[0035] In some embodiments, the hydrophilic polymer layer on the coated film is immersed in a second aqueous solution of polyphosphoric acid or boric acid for a period of time ranging from 5 minutes to 24 hours, or 5 minutes to 12 hours, or 5 minutes to 8 hours, or 10 minutes to 5 hours, or 30 minutes to 1 hour, and then immersed in an aqueous solution of a metal salt or hydrochloric acid for a period of time ranging from 5 minutes to 24 hours, or 5 minutes to 12 hours, or 5 minutes to 8 hours, or 10 minutes to 5 hours, or 30 minutes to 1 hour.
[0036] In other embodiments, the hydrophilic polymer is complexed in situ using a complexing agent in the negative electrolyte, positive electrolyte, or both the negative and positive electrolytes within a redox flow battery cell.
[0037] In some embodiments, the hydrophilic ionomer polymer includes a polysaccharide polymer, a poly(acrylic acid) polymer, a poly(methacrylic acid) polymer, or a combination thereof.
[0038] In some embodiments, the polysaccharide polymer includes chitosan, sodium alginate, potassium alginate, calcium alginate, ammonium alginate, alginic acid, sodium hyaluronate, potassium hyaluronate, calcium hyaluronate, ammonium hyaluronate, hyaluronic acid, dextran, pullulan, carboxymethyl curdlan, sodium carboxymethyl curdlan, potassium carboxymethyl curdlan, calcium carboxymethyl curdlan, ammonium carboxymethyl curdlan, κ-carrageenan, λ-carrageenan, ι-carrageenan, carboxymethylcellulose, sodium carboxymethylcellulose, potassium carboxymethylcellulose, calcium carboxymethylcellulose, ammonium carboxymethylcellulose, pectinic acid, chitin, chondroitin, xanthan gum, or a combination thereof.
[0039] Another aspect of the present invention is a redox flow battery system. In one embodiment, the redox flow battery system includes at least one rechargeable cell comprising a positive electrolyte, a negative electrolyte, and an ion-conductive thin film composite (TFC) membrane disposed between the positive and negative electrolytes, wherein the TFC membrane comprises a first microporous support membrane, a hydrophilic ionomer polymer coating layer on a first surface of the microporous support membrane, and a second microporous support membrane on the surface of the hydrophilic ionomer polymer coating layer opposite to the first microporous support membrane, the hydrophilic ionomer polymer coating layer being ion-conductive.
[0040] In some embodiments, the negative electrolyte, the positive electrolyte, or both the negative and positive electrolytes include a boric acid additive that can complex with a hydrophilic polymer on the surface of the first microporous support membrane to form a crosslinked hydrophilic ionomer polymer coating layer.
[0041] In some embodiments, the negative electrolyte, the positive electrolyte, or both the negative and positive electrolytes contain ferrous chloride.
[0042] In some embodiments, the positive electrolyte includes ferrous chloride and hydrochloric acid.
[0043] In some embodiments, the hydrophilic ionomer polymer coating layer is formed in situ by complexing a hydrophilic polymer on the surface of a first microporous support film with a complexing agent, in the case of a negative electrolyte, a positive electrolyte, or both negative and positive electrolytes. This is typically done in the presence of a second microporous support film. [Examples]
[0044] The following embodiments are provided to illustrate one or more preferred embodiments of the present invention, but are not intended to limit them. Numerous modifications can be made to the following embodiments which fall within the scope of the present invention.
[0045] Comparative Example 1. Preparation of an iron flow battery cell (abbreviated as AD-IFB) containing an alginate / Daramic® thin film composite (TFC) film. An iron flow battery cell containing an alginate / Daramic® thin film composite (TFC) membrane, a carbon felt cathode and anode, and a positive and negative electrolyte was prepared as follows.
[0046] A 9.0 wt% sodium alginate aqueous solution was prepared by dissolving sodium alginate polymer in deionized (DI) water. One surface of a Daramic® microporous support film purchased from Daramic, LLC was coated with a thin layer of the 9.0 wt% sodium alginate aqueous solution and dried at 60°C for 2 hours to form a sodium alginate layer on the surface of the Daramic® support film. The dried sodium alginate / Daramic® TFC film was assembled with a carbon felt positive electrode, a carbon felt negative electrode, two plastic flow frames, two graphite bipolar plates, and two copper current collectors to form an iron flow battery cell. A positive electrolyte tank containing the positive electrolyte and a negative electrolyte tank containing the negative electrolyte were connected to the positive and negative sides of the iron flow battery cell, respectively. The positive electrolyte was circulated within the battery cell for 2 hours, and then the battery was activated to form a final iron flow battery cell (AD-IFB) containing an alginate / Daramic® TFC membrane.
[0047] Example 1. Preparation of an iron flow battery cell (abbreviated as DAD-IFB) containing a sandwich-type Daramic® / alginate / Daramic® TFC membrane. An ion flow battery cell comprising a sandwich-like Daramic® / alginate / Daramic® TFC membrane, a carbon felt positive electrode and negative electrode, and a positive electrolyte and a negative electrolyte was prepared as follows. A 9.0 wt% sodium alginate aqueous solution was prepared by dissolving sodium alginate polymer in deionized (DI) water. One surface of a Daramic® microporous support film purchased from Daramic, LLC was coated with a thin layer of the 9.0 wt% sodium alginate aqueous solution and dried at 60°C for 2 hours to form a sodium alginate layer on the surface of the Daramic® support film. A second Daramic® microporous support film was added to the surface of the dried sodium alginate coating layer to form a sandwich-like Daramic® / alginate / Daramic® TFC film. The film was assembled with a carbon felt positive electrode, a carbon felt negative electrode, two plastic flow frames, two graphite bipolar plates, and two copper current collectors to form an iron flow battery cell. A positive electrolyte tank containing the positive electrolyte and a negative electrolyte tank containing the negative electrolyte were connected to the positive and negative sides of the iron flow battery cell, respectively. The positive electrolyte was circulated within the battery cell for two hours, and then the battery was activated to form a final iron flow battery cell (abbreviated as DAD-IFB) containing a sandwich-like Daramic® / alginate / Daramic® TFC membrane.
[0048] Example 2. Performance study of all-iron redox flow batteries related to AD-IFB batteries and DAD-IFB batteries. The battery performance of the all-iron redox flow battery AD-IFB described in Comparative Example 1 and the DAD-IFB described in Example 1 was evaluated at 40°C using an Arbin RBT battery tester (Arbin Instruments, USA). Both batteries used the same electrolyte formulation, including positive and negative electrolyte solutions. Both the positive and negative electrolyte solutions contained FeCl2, NH4Cl, HCl, and glycine in ultrapure water (18.2 MΩ·cm). The results showed that the initial CE of the DAD-IFB was 2% higher than that of the AD-IFB due to the addition of a second microporous support membrane, but the VE of the DAD-IFB was 2.8% lower than that of the AD-IFB. The initial overall performance (EE) of the DAD-IFB and AD-IFB were equivalent. However, more importantly, long-term testing revealed that the EE of the DAD-IFB was far more stable than the EE achieved by the AD-IFB. These results demonstrate that for the novel TFC film, a hydrophilic ionomer polymer coating layer sandwiched between two microporous support films can effectively protect against damage near the sealing area during stack assembly, as well as damage from fibers on the carbon felt during stack assembly or battery operation.
[0049] Specific Embodiments The following will be explained in conjunction with specific embodiments, but it should be understood that this explanation is intended to illustrate the scope of the preceding explanation and the attached claims, and is not intended to limit them.
[0050] A first embodiment of the present invention is a composition comprising a first microporous support film, a hydrophilic ionomer polymer coating layer on the surface of the first microporous support film which is ion-conductive, and a second microporous support film on the surface of the hydrophilic ionomer polymer coating layer opposite to the first microporous support film. One embodiment of the present invention is one, any, or all of the previous embodiments of this paragraph, including the first embodiment of this paragraph, wherein the hydrophilic ionomer polymer includes polyphosphate complexed polysaccharide polymers, polyphosphate and metal ion complexed polysaccharide polymers, metal ion complexed polysaccharide polymers, borate complexed polysaccharide polymers, alginate polymers, alginate polymers, hyaluronic acid polymers, borate complexed polyvinyl alcohol polymers, polyphosphate complexed polyvinyl alcohol polymers, polyphosphate and metal ion complexed polyvinyl alcohol polymers, metal ion complexed polyvinyl alcohol polymers, metal ion complexed poly(acrylic acid) polymers, borate complexed poly(acrylic acid) polymers, metal ion complexed poly(methacrylic acid), borate complexed poly(methacrylic acid), or a combination thereof. One embodiment of the present invention is one, any, or all of the prior embodiments of this paragraph, including the first embodiment of this paragraph, wherein the polysaccharide polymer includes chitosan, sodium alginate, potassium alginate, calcium alginate, ammonium alginate, alginic acid, sodium hyaluronate, potassium hyaluronate, calcium hyaluronate, ammonium hyaluronate, hyaluronic acid, dextran, pullulan, carboxymethyl curdlan, sodium carboxymethyl curdlan, potassium carboxymethyl curdlan, calcium carboxymethyl curdlan, ammonium carboxymethyl curdlan, κ-carrageenan, λ-carrageenan, ι-carrageenan, carboxymethylcellulose, sodium carboxymethylcellulose, potassium carboxymethylcellulose, calcium carboxymethylcellulose, ammonium carboxymethylcellulose, pectinic acid, chitin, chondroitin, xanthan gum, or a combination thereof.One embodiment of the present invention is one or all of the prior embodiments of this paragraph, including up to the first embodiment of this paragraph, and the metal ion is a ferric ion, a ferrous ion, or a vanadium ion. One embodiment of the present invention is one or all of the prior embodiments of this paragraph, including up to the first embodiment of this paragraph, and the hydrophilic ionomer polymer is a polyphosphate-complexed chitosan polymer, a polyphosphate and metal ion-complexed chitosan polymer, a metal ion-complexed alginate polymer, a sodium alginate polymer, an alginate polymer, a hyaluronic acid polymer, or a combination thereof. One embodiment of the present invention is one or all of the prior embodiments of this paragraph, including up to the first embodiment of this paragraph, and the metal ion is a ferric ion, a ferrous ion, or a vanadium ion. One embodiment of the present invention is one or all of the prior embodiments of this paragraph, including up to the first embodiment of this paragraph, wherein the hydrophilic ionomer polymer is a borate-complexed polyvinyl alcohol polymer, a borate-complexed alginic acid, or a blend of a borate-complexed polyvinyl alcohol and an alginic acid polymer. One embodiment of the present invention is one or all of the prior embodiments of this paragraph, including up to the first embodiment of this paragraph, wherein the first microporous support film or the second microporous support film, or both, include polyethylene, polypropylene, a mixture of polyethylene and silica particles, a mixture of polypropylene and silica particles, polyamide, polyacrylonitrile, polyethersulfone, sulfonated polyethersulfone, polysulfone, sulfonated polysulfone, poly(etheretherketone), sulfonated poly(etheretherketone), polyester, cellulose acetate, cellulose triacetate, polybenzimidazole, polyimide, polyvinylidene fluoride, polycarbonate, cellulose, or a combination thereof. One embodiment of the present invention is one, any, or all of the prior embodiments of this paragraph, including the first embodiment of this paragraph, wherein the hydrophilic ionomer polymer is present in the micropores of the first microporous support film.
[0051] A second embodiment of the present invention is a method for preparing an ion-conductive thin-film composite (TFC) film, comprising: applying a layer of aqueous solution containing a hydrophilic ionomer polymer to one surface of a first microporous support film; drying the coated film; optionally, complexing the hydrophilic ionomer polymer using a complexing agent to form a crosslinked hydrophilic ionomer polymer; and applying a second microporous support film to the coated film on the opposite surface of the first microporous support film. One embodiment of the present invention is one or all of the prior embodiments of this paragraph, including up to the second embodiment of this paragraph, wherein the hydrophilic ionomer polymer on the coated film is dried before the hydrophilic ionomer polymer is complexed. Another embodiment of the present invention is one or all of the prior embodiments of this paragraph, including up to the second embodiment of this paragraph, wherein the second microporous support film is applied to the coated film after the coated film has been dried. One embodiment of the present invention is one or all of the prior embodiments of this paragraph, including up to the second embodiment of this paragraph, wherein the complexing agent is selected from polyphosphate, boric acid, ferric ions, ferrous ions, or vanadium ions, or a combination thereof. One embodiment of the present invention is one or all of the prior embodiments of this paragraph, including up to the second embodiment of this paragraph, wherein the complexing of a hydrophilic ionomer polymer includes immersing a dried, coated film in a second aqueous solution of polyphosphate, boric acid, a metal salt, hydrochloric acid, or a combination thereof. One embodiment of the present invention is one or all of the prior embodiments of this paragraph, including up to the second embodiment of this paragraph, wherein the complexing of a hydrophilic ionomer polymer includes in situ complexing a dried, coated film together with a second microporous support film using a complexing agent in a redox flow battery cell. One embodiment of the present invention is one, any, or all of the prior embodiments of this paragraph, including the second embodiment of this paragraph, wherein the hydrophilic ionomer polymer includes a polysaccharide polymer, a poly(acrylic acid) polymer, a poly(methacrylic acid), or a combination thereof.One embodiment of the present invention is one, any, or all of the prior embodiments of this paragraph, including the second embodiment of this paragraph, wherein the polysaccharide polymer includes chitosan, sodium alginate, potassium alginate, calcium alginate, ammonium alginate, alginic acid, sodium hyaluronate, potassium hyaluronate, calcium hyaluronate, ammonium hyaluronate, hyaluronic acid, dextran, pullulan, carboxymethyl curdlan, sodium carboxymethyl curdlan, potassium carboxymethyl curdlan, calcium carboxymethyl curdlan, ammonium carboxymethyl curdlan, κ-carrageenan, λ-carrageenan, ι-carrageenan, carboxymethylcellulose, sodium carboxymethylcellulose, potassium carboxymethylcellulose, calcium carboxymethylcellulose, ammonium carboxymethylcellulose, pectinic acid, chitin, chondroitin, xanthan gum, or a combination thereof.
[0052] A third embodiment of the present invention is a system comprising at least one rechargeable cell comprising a positive electrolyte, a negative electrolyte, and an ion-conductive thin-film composite (TFC) membrane disposed between the positive and negative electrolytes, wherein the TFC membrane comprises a first microporous support membrane, a hydrophilic ionomer polymer coating layer on the surface of the first microporous support membrane, and a second microporous support membrane on the surface of the hydrophilic ionomer polymer coating layer opposite to the first microporous support membrane, the hydrophilic ionomer polymer coating layer being ion-conductive. One embodiment of the present invention is one, any, or all of the prior embodiments of this paragraph, including the third embodiment of this paragraph, wherein the negative electrolyte, the positive electrolyte, or both the negative and positive electrolytes include a boric acid additive that can complex with a hydrophilic ionomer polymer on the surface of the microporous support membrane to form a crosslinked hydrophilic ionomer polymer coating layer. One embodiment of the present invention is one, any, or all of the prior embodiments of this paragraph, including the third embodiment of this paragraph, wherein the hydrophilic ionomer polymer coating layer is formed in situ by complexing a hydrophilic polymer on the surface of a first microporous support film with a complexing agent in a negative electrolyte, a positive electrolyte, or both the negative and positive electrolytes (the positive electr).
[0053] Without further detail, it is expected that those skilled in the art will be able to utilize the invention to the fullest extent without departing from the spirit and scope of the invention, and will readily identify its essential characteristics, and will be able to make various changes and modifications to the invention to suit various uses and conditions. Accordingly, the prior preferred specific embodiments should be interpreted as merely illustrative and not to limit the remainder of this disclosure in any way, but are intended to cover various modifications and equivalent configurations that fall within the scope of the appended claims.
[0054] In the above, all temperatures are given in degrees Celsius, and all parts and percentages are based on weight unless otherwise indicated. The present invention includes the following embodiments. [1] An ion-conducting thin film composite (TFC) film, A first microporous support membrane, A hydrophilic ionomer polymer coating layer on the surface of the first microporous support film, wherein the hydrophilic ionomer polymer coating layer is ion conductive, A TFC film comprising a second microporous support film on the surface of the hydrophilic ionomer polymer coating layer opposite to the first microporous support film. [2] The hydrophilic ionomer polymer comprises a polyphosphate complexed polysaccharide polymer, a polyphosphate and metal ion complexed polysaccharide polymer, a metal ion complexed polysaccharide polymer, a borate complexed polysaccharide polymer, an alginate polymer, an alginate polymer, a hyaluronic acid polymer, a borate complexed polyvinyl alcohol polymer, a polyphosphate complexed polyvinyl alcohol polymer, a polyphosphate and metal ion complexed polyvinyl alcohol polymer, a metal ion complexed polyvinyl alcohol polymer, a metal ion complexed poly(acrylic acid) polymer, a borate complexed poly(acrylic acid) polymer, a metal ion complexed poly(methacrylic acid), a borate complexed poly(methacrylic acid), or a combination thereof, as described in item 1. [3] The hydrophilic ionomer polymer is a polyphosphate-complexed chitosan polymer, a polyphosphate and metal ion-complexed chitosan polymer, a metal ion-complexed alginate polymer, a sodium alginate polymer, an alginate polymer, a hyaluronic acid polymer, or a combination thereof, as described in item 1 or 2. [4] The TFC film according to claim 1 or 2, wherein the hydrophilic ionomer polymer is a borate-complexed polyvinyl alcohol polymer, a borate-complexed alginic acid, or a blend of a borate-complexed polyvinyl alcohol and an alginic acid polymer. [5] The TFC membrane according to claim 1 or 2, wherein the first microporous support membrane or the second microporous support membrane, or both thereof, comprises polyethylene, polypropylene, a mixture of polyethylene and silica particles, a mixture of polypropylene and silica particles, polyamide, polyacrylonitrile, polyethersulfone, sulfonated polyethersulfone, polysulfone, sulfonated polysulfone, poly(etheretherketone), sulfonated poly(etheretherketone), polyester, cellulose acetate, cellulose triacetate, polybenzimidazole, polyimide, polyvinylidene fluoride, polycarbonate, cellulose, or a combination thereof. [6] The hydrophilic ionomer polymer is present in the micropores of the first microporous support film, as described in item 1 or 2. [7] A method for preparing an ion-conductive thin film composite (TFC) film, Applying a layer of aqueous solution containing a hydrophilic ionomer polymer to one surface of the first microporous support film, Drying the coated film, The hydrophilic ionomer polymer may be optionally complexed using a complexing agent to form a crosslinked hydrophilic ionomer polymer. A method comprising applying a second microporous support film to the coated film on the surface opposite to the first microporous support film. [8] The method according to item 7, wherein the complexing agent is selected from polyphosphate, boric acid, a metal ion selected from ferric ions, ferrous ions, or vanadium ions, or a combination thereof. [9] The method according to claim 7 or 8, wherein the complexing of the hydrophilic ionomer polymer comprises immersing the dried, coated film in a second aqueous solution of polyphosphate, boric acid, a metal salt, hydrochloric acid, or a combination thereof.
[10] A redox flow battery system comprising at least one rechargeable cell, the cell comprising a positive electrolyte, a negative electrolyte, and an ion-conductive thin-film composite (TFC) membrane disposed between the positive electrolyte and the negative electrolyte, wherein the TFC membrane comprises a first microporous support membrane, a hydrophilic ionomer polymer coating layer on the surface of the first microporous support membrane, and a second microporous support membrane on the surface of the hydrophilic ionomer polymer coating layer opposite to the first microporous support membrane, the hydrophilic ionomer polymer coating layer being ion-conductive.
Claims
1. An ion-conducting thin film composite (TFC) film, A first microporous support membrane, A hydrophilic ionomer polymer coating layer on the surface of the first microporous support film, wherein the hydrophilic ionomer polymer coating layer is ion conductive, A TFC film comprising a second microporous support film on the surface of the hydrophilic ionomer polymer coating layer opposite to the first microporous support film, wherein the hydrophilic ionomer polymer contains a polysaccharide polymer.
2. The hydrophilic ionomer polymer includes polyphosphate complexed polysaccharide polymers, polyphosphate and metal ion complexed polysaccharide polymers, metal ion complexed polysaccharide polymers, borate complexed polysaccharide polymers, alginate polymers, alginate polymers, hyaluronic acid polymers, or combinations thereof. The TFC film according to claim 1, wherein the first microporous support film or the second microporous support film, or both thereof, comprises polyethylene, polypropylene, a mixture of polyethylene and silica particles, a mixture of polypropylene and silica particles, polyamide, polyacrylonitrile, polyethersulfone, sulfonated polyethersulfone, polysulfone, sulfonated polysulfone, poly(etheretherketone), sulfonated poly(etheretherketone), polyester, cellulose acetate, cellulose triacetate, polybenzimidazole, polyimide, polyvinylidene fluoride, polycarbonate, cellulose, or a combination thereof.
3. A method for preparing an ion-conductive thin film composite (TFC) film, To provide a film coated by applying a layer of aqueous solution containing a hydrophilic ionomer polymer to one surface of a first microporous support film, wherein the hydrophilic ionomer polymer contains a polysaccharide polymer, Drying the hydrophilic ionomer polymer on the coated film, The hydrophilic ionomer polymer is complexed using a complexing agent to form a crosslinked hydrophilic ionomer polymer, The method includes applying a second microporous support film to the coated film on the surface opposite to the first microporous support film, The complexing agent is selected from polyphosphate, boric acid, ferric ions, ferrous ions, or vanadium ions, or a combination thereof. A method for complexing the hydrophilic ionomer polymer comprises immersing the dried, coated film in a second aqueous solution of polyphosphate, boric acid, a metal salt, hydrochloric acid, or a combination thereof.
Citation Information
Patent Citations
Multi-layered polymeric electrolyte membrane for fuel cell
JP2007109657A
Ion exchange membrane, its manufacturing method, and energy storage device including the same
JP2019518588A
Highly reinforced ionomer membranes for high selectivity and strength
JP2020524367A
Composite proton conducting membrane
JP2024508632A
Ionically conductive thin film composite membranes for energy storage applications
US20220134292A1