Lithium replenisher and method for manufacturing the same, positive electrode slurry, and battery
A lithium replenisher with a hexagonal kernel and tetragonal coating layer optimizes lithium replenishment, addressing the capacity loss issue in lithium-ion batteries by improving energy density and stability through enhanced lithium ion release and reduced slurry viscosity.
Patent Information
- Application Number
- JP2025543369
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2024-03-29
- Filing Date
- 2024-06-28
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-06-28
AI Technical Summary
Lithium-ion batteries face capacity loss due to the formation of a solid electrolyte interphase (SEI) film during the initial charging process, and existing lithium replenishment technologies on the positive electrode side face challenges such as high safety and compatibility issues, leading to reduced energy density and stability.
A lithium replenisher with a specific chemical formula Li_x M1_y M2₁-y O6, where 6≤x≤8 and 0
The lithium replenisher effectively compensates for lithium loss, improving energy density and cycle life of lithium batteries by ensuring stable lithium ion release and reducing slurry viscosity, thereby enhancing battery performance.
Smart Images

Figure 0007955523000005 
Figure 0007955523000006 
Figure 0007955523000007
Abstract
Description
TECHNICAL FIELD
[0001] The present disclosure relates to the technical field of batteries, and particularly to a lithium replenisher and a manufacturing method thereof, a positive electrode slurry, and a battery.
BACKGROUND ART
[0002] During the initial charging process of a lithium-ion battery, a solid electrolyte interphase (SEI) film is formed at the negative electrode interface, which causes irreversible loss to the capacity of the battery, thereby reducing the energy density of the lithium-ion battery. The lithium replenishment technology can effectively mitigate the capacity loss during the formation of the SEI film. There are two main lithium replenishment technologies, namely lithium replenishment on the positive electrode side and lithium replenishment on the negative electrode side. Here, the lithium replenishment technology on the negative electrode side requires the use of metallic lithium materials, which has problems such as complex processes and high environmental requirements. The lithium replenishment technology on the positive electrode side has high safety and compatibility, and thus has high feasibility. However, it is believed that the lithium replenishment on the positive electrode side also has many problems to be solved in the actual production and application process.
SUMMARY OF THE INVENTION
MEANS FOR SOLVING PROBLEMS
[0003] In a first aspect of the present application, the present application provides a lithium replenisher, which satisfies the chemical formula Li x M1 y M2 1-y O6, wherein 6≤x≤8, 0<y<1, and M1 is at least one of Zr, Nb, Sb, Bi, Ru, Ta, Sn, Hf, Ir, Pr, Pt, and Np, and M2 is at least one of W, Ge, Ca, Ce, K, and Ta; and a coating layer located on at least a part of the surface of the kernel and containing a lithium-containing metal oxide and a carbon material, wherein the lithium-containing metal oxide satisfies the chemical formula Li a’ M b’ O c’ wherein 1.8≤a ’≤2, 0.7≤b ’ ≤1.1, 2.8≤c ’ ≤3, and M includes Ti and / or Zr. The peak intensity of the diffraction peak for X-rays when the 2θ diffraction angle is in the range of 20.1° to 20.3° is S1, and the peak intensity of the diffraction peak for X-rays when the 2θ diffraction angle is in the range of 17° to 17.3° is S2. The present invention proposes a lithium supplement agent in which S1 / S2 is 0.02 to 0.05. As a result, the lithium supplement agent has a high lithium supplement capacity, a high lithium ion transition rate, and excellent processing performance.
[0004] In some examples, the mass fraction of the lithium-containing metal oxide in the lithium supplement agent is 0.01% to 0.1%, and / or the mass fraction of the carbon material in the lithium supplement agent is 0.01% to 0.5%. As a result, the lithium supplement agent has a high lithium supplement capacity.
[0005] In some examples, the kernel of the crystal lattice lattice constants satisfy a=b, a≠c, and c / a is 2 to 3. As a result, the lithium ion transition rate of the lithium supplement agent can be increased.
[0006] In some examples, a is 0.4 nm to 0.7 nm, and c is 1.4 nm to 1.6 nm. As a result, the lithium ion transition rate of the lithium supplement agent can be further increased.
[0007] In some examples, the Dv50 particle size of the kernel is 1 μm to 10 μm, and / or the thickness of the coating layer is 50 nm to 500 nm. As a result, the coating layer can improve the storage performance of the lithium supplement agent, enhance the conductivity of the lithium supplement agent, and contribute to the full exertion of the lithium supplement function of the lithium supplement agent.
[0008] In some examples, the kernel includes Li8Zr 0.9 W 0.1 O6, Li7Nb 0.8 Ta0.2 O6, Li7Sb 0.9 Ta 0.1 O6, Li7Ru 0.7 W 0.2 Ce 0.1 O6, Li8Sn 0.9 Ca 0.1 O6, Li8Hf 0.7 W 0.2 Ca 0.1 O6, Li8Ir 0.6 W 0.2 Ce 0.2 O6, Li8Pr 0.5 W 0.3 Ca 0.2 O6, Li8Pt 0.7 W 0.2 Ca 0.1 It contains at least one of the O6 species. This effectively improves the lithium supply capacity of the lithium supplement and lowers the decomposition potential of the lithium supplement.
[0009] In some examples, the degree of graphitization of the carbon material is 60% or higher. This further improves the conductivity of the lithium replenisher.
[0010] In a second aspect of the present application, the present application proposes a method for producing the lithium replenisher described above, comprising the steps of: obtaining a kernel by performing a first sintering treatment on a lithium source, an M1 source, and an M2 source in an oxygen-containing atmosphere; and obtaining the lithium replenisher by performing a second sintering treatment on the kernel, an M source, and a carbon source in an inert atmosphere to form a coating layer on at least a portion of the surface of the kernel. This makes it possible to obtain a lithium replenisher having the excellent lithium replenishment performance described above in a simple manner.
[0011] In some embodiments, the lithium source comprises at least one of lithium carbonate, lithium hydroxide, and lithium oxide, and / or the M1 source comprises at least one of the oxide of M1, the chloride of M1, the nitrate of M1, and the hydroxide of M1, and / or the M2 source comprises at least one of the oxide of M2, the chloride of M2, the nitrate of M2, and the hydroxide of M2. This contributes to the formation of a kernel with a high lithium replenishment capacity.
[0012] In some embodiments, the temperature of the first sintering treatment is 700°C to 1200°C, and the duration of the first sintering treatment is 8 hours to 24 hours. This contributes to obtaining pure phase kernel particles with appropriate particle sizes.
[0013] In some embodiments, the M source comprises at least one of zirconium propoxide, zirconium oxide, zirconium nitrate, zirconium oxychloride, lithium zirconate, zirconium chloride, titanium oxide, titanium tetrachloride, titanium nitrate, and titanium alkoxide, and / or the carbon source comprises at least one of glucose, starch, sucrose, and graphite. This contributes to the formation of lithium-containing metal oxides on the surface of the kernel.
[0014] In some embodiments, the temperature of the second sintering treatment is 400°C to 800°C, and the duration of the second sintering treatment is 6H to 10H. This contributes to the formation of lithium-containing metal oxides and carbon materials in the coating layer.
[0015] In some embodiments, the process further includes a step of mixing the kernel, the M source, and the carbon source in a solvent and drying them before the second sintering process. This contributes to improving the uniformity of the coating by the coating layer.
[0016] In some embodiments, the solvent comprises at least one of ethanol and isopropanol, and / or the drying treatment comprises at least one of spray drying, freeze-drying, and flash drying. This contributes to improving the uniformity of the coating by the coating layer.
[0017] In a third aspect of this application, the present application proposes a positive electrode slurry comprising the lithium replenisher described above, or a lithium replenisher manufactured by the method described above. The positive electrode slurry thereby possesses all the constituent elements and advantages of the lithium replenisher and the method for manufacturing the lithium replenisher described above. Further explanation is omitted here.
[0018] In some embodiments, the viscosity of the positive electrode slurry is 1000 mPa·s to 8000 mPa·s. This contributes to improving the processing performance of the positive electrode slurry.
[0019] In a fourth aspect of the present application, the present application proposes a battery comprising a positive electrode tab including a positive electrode current collector and a positive electrode active material layer located on at least one side of the positive electrode current collector, wherein the positive electrode active material layer is manufactured from the positive electrode slurry described above. The battery thus possesses all the constituent requirements and advantages of the positive electrode slurry described above. Further explanation is omitted here. [Brief explanation of the drawing]
[0020] The above-mentioned and / or additional aspects and advantages of this application will become apparent and readily understandable from the description of the embodiments with reference to the following accompanying drawings. [FIG. 1] This is a scanning electron microscope image of the lithium replenisher in Example 1 of the present invention. [FIG. 2] These are X-ray diffraction patterns of the lithium replenisher in Example 1 and Comparative Example 5 of this application. [FIG. 3] This is a charge-discharge graph after a battery has been manufactured using the lithium replenisher in Example 1 of the present invention. [Modes for carrying out the invention]
[0021] The embodiments of this application will be described in detail below. Examples of the embodiments described are shown in the accompanying drawings, but unnecessary descriptive details may be omitted. For example, details of publicly known matters may be omitted, or redundant descriptions of the same structure may be omitted. This is intended to avoid making the following description unnecessarily verbose and to make it easily understandable to those skilled in the art. The accompanying drawings and the following description are provided to enable those skilled in the art to fully understand this application and are not intended to limit the subject matter described in the claims.
[0022] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art, and the technical terms used herein are solely for the purpose of describing specific embodiments and are not intended to limit the application. Furthermore, unless otherwise described, the values of each parameter referred to herein may be measured by various measurement methods commonly used in the art (for example, by the methods provided in the embodiments of this application).
[0023] The technical terms "includes," "equip," and any variations thereof in the specification and claims of this application constitute open expressions, that is, they include the content shown in this application, but do not exclude the content of other embodiments.
[0024] In this description, regardless of whether the words "approximately" or "about" are used, all figures disclosed herein are approximations. The numerical values indicated by each figure may vary by 10% or less, or by a reasonable amount that would be recognized by a person skilled in the art, such as 1%, 2%, 3%, 4%, or 5%.
[0025] (blank)
[0026] Unless otherwise specified, all constituent elements and optional constituent elements in this application can be combined to form new technical solutions.
[0027] Related technologies include lithium replenishers for the positive electrode, such as binary lithium-containing compounds like Li2O, Li2O2, and Li3N, and ternary lithium-containing compounds like Li2NiO2, Li6CoO4, and Li5FeO4. Binary lithium-containing compounds have poor stability in atmospheric environments and are difficult to apply to industrial applications. Ternary lithium-containing compounds are more stable than binary lithium-containing compounds, but they have the drawback of being highly alkaline on the surface and having a high decomposition potential. Specifically, when a lithium replenisher is added to a positive electrode slurry, the strongly alkaline surface of the lithium replenisher causes a lithium deposition reaction, strengthening the alkalinity of the positive electrode slurry. This significantly increases the viscosity of the positive electrode slurry, which can lead to the formation of a jelly-like slurry, making it impossible to meet the application requirements. If the decomposition potential of the lithium replenisher is too high, a high voltage must be applied during the initial charging process of the battery to ensure that the lithium replenishment capacity in the lithium replenisher is sufficiently released. If the voltage applied during the initial charging process is too high, irreversible structural changes occur in the positive electrode active material in the positive electrode active material layer. This reduces the lithium desorption sites in the positive electrode active material, lowering the battery's energy density. If the voltage applied during the initial charging process is too low, the lithium replenishment capacity of the lithium replenisher cannot be sufficiently released, resulting in a reduced lithium replenishment effect by the lithium replenisher.
[0028] In this application, the elemental composition of the lithium replenisher is optimized, and by adding doping elements to a ternary lithium-containing lithium replenisher as a base, the lithium ion transition rate of the lithium replenisher kernel can be further increased. Specifically, the kernel of the lithium replenisher has the chemical formula Li x M1 y M2 1-yO6, where 6≤x≤8 and 0<y<1. Here, since the ternary lithium-containing compound containing the M1 element has a high theoretical capacity, the lithium replenishment capacity of the lithium replenisher can be effectively increased. The M2 element has a relatively smaller lithium replenishment capacity that can be provided than the M1 element, but its ionic radius is larger than that of the M1 element. Therefore, doping with the M2 element contributes to rapid insertion and extraction of lithium ions due to the interlayer distance between the layered structures in the kernel. As a result, the kernel of the lithium replenisher has a high capacity, a high lithium replenishment capacity, and a fast lithium ion transition rate. Furthermore, since the alkaline surface of the kernel of the lithium replenisher described above may cause problems such as gelation of the positive electrode slurry, a coating layer containing a lithium-containing metal oxide and a carbon material is formed on the surface of the kernel of the lithium replenisher described above. The lithium-containing metal oxide in the coating layer can effectively suppress the reaction between the kernel and moisture, carbon dioxide, etc. in the air to generate lithium hydroxide or lithium carbonate impurities. However, since the conductivity of the lithium-containing metal oxide is not good, by further adding an appropriate amount of carbon material to the coating layer, the conductivity of the coating layer can be effectively improved. Then, the electron conductivity on the surface of the lithium replenisher can be further improved, and the transport paths of lithium ions and electrons in the lithium replenisher can be improved.
[0029] The aforementioned lithium replenisher exhibits a characteristic diffraction peak with respect to X-rays when the 2θ diffraction angle is within the range of 20.1° to 20.3°, which indicates that the lithium-containing metal oxide in the coating layer has a tetragonal structure (110 crystal plane). The aforementioned lithium replenisher exhibits a characteristic diffraction peak with respect to X-rays when the 2θ diffraction angle is within the range of 17° to 17.3°, which indicates that the kernel of the lithium replenisher has a hexagonal structure (101 crystal plane). Furthermore, the peak intensity of the diffraction peak with respect to X-rays when the 2θ diffraction angle of the lithium replenisher is within the range of 20.1° to 20.3° is S1, and the peak intensity of the diffraction peak with respect to X-rays when the 2θ diffraction angle of the aforementioned lithium replenisher is within the range of 17° to 17.3° is S2. When S1 / S2 is 0.02 to 0.05, the phase ratio between the kernel of the lithium replenisher with a hexagonal structure and the coating layer with a tetragonal structure is appropriate. In this case, the kernel with a hexagonal structure has a high lithium ion migration rate, which is advantageous for sufficient release of lithium ions in the kernel. Meanwhile, the lithium-containing metal oxide with a tetragonal structure has high structural stability, can effectively suppress the generation of impurities caused by the reaction between the kernel and moisture, carbon dioxide, etc., and simultaneously has good lithium intercalation and deintercalation characteristics. Therefore, the influence of the surface coating layer formed by both the lithium-containing metal oxide and the carbon material on the exertion of the lithium replenishment performance of the kernel is reduced, and the transport paths of lithium ions and electrons in the lithium replenisher can be effectively improved.
[0030] In a first aspect of the present application, the present application provides a lithium replenisher, which satisfies the chemical formula Li x M1 y M2 1-y O6, where 6≤x≤8 and 0<y<1. M1 is at least one selected from the group consisting of Zr, Nb, Sb, Bi, Ru, Ta, Sn, Hf, Ir, Pr, Pt, and Np. M2 is at least one selected from the group consisting of W, Ge, Ca, Ce, K, and Ta. The lithium replenisher further includes a coating layer located on at least a part of the surface of the kernel, the coating layer includes a lithium-containing metal oxide and a carbon material, and the lithium-containing metal oxide satisfies the chemical formula Li a’ Mb’ O c’ The following conditions must be met, where 1.8 ≤ a ’ ≤2, 0.7 ≤b ’ ≤1.1, 2.8 ≤c ’ We propose a lithium replenisher in which M comprises a coating layer containing Ti and / or Zr, the peak intensity of the diffraction peak for X-rays when the 2θ diffraction angle is in the range of 20.1° to 20.3° is S1, the peak intensity of the diffraction peak for X-rays when the 2θ diffraction angle is in the range of 17° to 17.3° is S2, and S1 / S2 is 0.02 to 0.05. Thus, the above lithium replenisher has a high lithium replenishment capacity and a high lithium ion transfer rate. Here, since a stabilized tetragonal coating layer exists on the surface of the hexagonal kernel, when the ratio of S1 to S2 satisfies the above limiting conditions, the coating layer can effectively improve the stability of the kernel and reduce the increase in viscosity of the positive electrode slurry due to the surface alkalinity of the kernel during the use of the lithium replenisher, resulting in excellent processing performance. When the above lithium replenisher is applied to lithium replenishment technology on the positive electrode side, during the battery charging process, the lithium replenisher can sufficiently decompose and release active lithium ions, thereby compensating for the loss of active lithium due to the formation of the SEI film, and thus improving the energy density and cycle life of the lithium battery.
[0031] For example, x could be 6, 6.5, 7, 7.5, or 8.
[0032] For example, y may be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, or 0.9.
[0033] For example, a ’ It may be 1.8, 1.9, or 2.
[0034] For example, b ’ This may be 0.7, 0.8, 0.9, 1, or 1.1.
[0035] For example, c ’is 2.8 or It may be 3.
[0036] For example, S1 / S2 may be 0.02, 0.03, 0.04, or 0.05.
[0037] In this application, the "peak intensity ratio of diffraction peaks" has the meaning known in the art and may be measured by instruments and methods known in the art. For example, it can be obtained by the following method: Using an automated X-ray diffractometer, analyze the physical phase and crystal structure, with an operating voltage of 40kV, an operating current of 250mA, using a means for continuous scanning, a scanning speed of 4° / min, a step length of 0.02°, and a scanning angle range of 10° to 80°.
[0038] In some embodiments, the mass fraction of the lithium-containing metal oxide in the lithium replenisher is 0.01% to 0.1%, and / or the mass fraction of the carbon material in the lithium replenisher is 0.01% to 0.5%.
[0039] For example, the mass fraction of the lithium-containing metal oxide in the lithium replenisher may be 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, or 0.1%.
[0040] When the mass fraction of the lithium-containing metal oxide in the lithium replenisher is within the range described above, the lithium-containing metal oxide in the coating layer can exhibit the advantage of ultra-high ionic conductivity, suppress the reaction between the kernel and water, carbon dioxide, etc., and prevent the formation of a surface impurity layer on the kernel.
[0041] For example, the mass fraction of the carbon material in the lithium additive may be 0.01%, 0.05%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.3%, 0.4%, 0.5%, or 0.5%.
[0042] When the mass fraction of the carbon material in the lithium replenisher is within the range described above, the carbon material in the coating layer effectively improves the conductivity of the coating layer and further improves the electronic conductivity of the surface of the lithium replenisher, thereby improving the transport paths of lithium ions and electrons in the lithium replenisher, while having only a small effect on the lithium replenishment capacity of the lithium replenisher.
[0043] In some embodiments, the kernel of the crystal lattice The lattice constant satisfies a=b and a≠c, and c / a is between 2 and 3. This allows for a faster lithium ion transition rate in lithium replenishers.
[0044] For example, c / a may be 2, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, or 3.
[0045] kernel lattice constant of the crystal lattice If a=b and a≠c are satisfied, the kernel is a hexagonal system, and due to the characteristic symmetry of the hexagonal system, the basis vectors corresponding to the cells of the hexagonal system are characterized in that both sub-axes are perpendicular to the principal axes, the magnitudes of the basis vectors of the two sub-axes are equal, and the included angle between the sub-axes is 120°, that is, lattice constant of the crystal lattice This has the characteristics a=b≠c, α=β=90°, and γ=120°. In this case, the cell has a layered structure, and by combining elements with different valencies and designing a non-equilibrium charge in the transition metal layer, it is possible to contribute to the formation of vacancies in the lithium ion layer, enabling rapid transport and highly efficient utilization of lithium ions.
[0046] In some embodiments, a is 0.4 nm to 0.7 nm and c is 1.4 nm to 1.6 nm. This allows for an even faster lithium ion transition rate of the lithium replenisher.
[0047] For example, a may be 0.4nm, 0.45nm, 0.5nm, 0.55nm, 0.6nm, 0.65nm, or 0.7nm.
[0048] For example, c may be 1.4nm, 1.45nm, 1.5nm, 1.55nm, or 1.6nm.
[0049] In this application lattice constant of the crystal lattice " has the meaning known in the industry and may be measured by instruments and methods known in the industry. For example, lattice constant of the crystal lattice This is obtained by X-ray diffraction testing.
[0050] In some embodiments, the Dv50 particle size of the kernel is 1 μm to 10 μm, and / or the thickness of the coating layer is 50 nm to 500 nm. As a result, the coating layer can improve the storage performance of the lithium replenisher, improve the conductivity of the lithium replenisher, and contribute to the full performance of the lithium replenishment function by the lithium replenisher.
[0051] For example, the Dv50 particle size of the kernel may be 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm, 9.5 μm, or 10 μm.
[0052] For example, the thickness of the coating layer may be 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, or 500 nm.
[0053] In some examples, the kernel is Li8Zr 0.9 W 0.1 O6, Li7Nb 0.8 Ta 0.2 O6, Li7Sb 0.9 Ta 0.1 O6, Li7Ru 0.7 W 0.2 Ce 0.1 O6, Li8Sn 0.9 Ca 0.1 O6, Li8Hf 0.7 W 0.2 Ca 0.1 O6, Li8Ir0.6 W 0.2 Ce 0.2 O6, Li8Pr 0.5 W 0.3 Ca 0.2 O6, Li8Pt 0.7 W 0.2 Ca 0.1 It contains at least one of the O6 species. This effectively improves the lithium supply capacity of the lithium supplement and lowers the decomposition potential of the lithium supplement.
[0054] When the kernel of a lithium replenisher contains the aforementioned substances, the kernel has a high lithium replenishment capacity and a high lithium replenisher capacity.
[0055] For example, Li8Zr 0.9 W 0.1 The theoretical capacity of O6 is 883 mAh / g, and Li7Nb 0.8 Ta 0.2 The theoretical capacity of O6 is 790mAh / g, and Li7Sb 0.9 Ta 0.1 The theoretical capacity of O6 is 704 mAh / g, and Li7Ru 0.7 W 0.2 Ce 0.1 The theoretical capacity of O6 is 764 mAh / g, compared to Li8Sn 0.9 Ca 0.1 The theoretical capacity of O6 is 793 mAh / g, compared to Li8Hf 0.7 W 0.2 Ca 0.1 The theoretical capacity of O6 is 650 mAh / g, and Li8Ir 0.6 W 0.2 Ce 0.2 The theoretical capacity of O6 is 624 mAh / g, and Li8Pr 0.5 W 0.3 Ca 0.2 The theoretical capacity of O6 is 783 mAh / g, compared to Li8Pt. 0.7 W 0.2 Ca 0.1 The theoretical capacity of O6 is 619 mAh / g.
[0056] In some examples, the degree of graphitization of the carbon material is 60% or higher. This further improves the conductivity of the lithium replenisher.
[0057] When the degree of graphitization of a carbon material is within the range described above, the closer the internal structure of the carbon material is to ideal graphite, the better its conductivity.
[0058] In a second aspect of this application, the present application proposes a method for manufacturing the lithium replenisher described above. This makes it possible to manufacture a lithium replenisher with excellent lithium replenishment performance as described above in a simple manner. Specifically, the method for manufacturing the lithium replenisher may include the following steps.
[0059] In Step S100, the lithium source, M1 source, and M2 source are subjected to a first sintering treatment in an oxygen-containing atmosphere.
[0060] In some embodiments, in this step, the M1 source, the M2 source, and the lithium source are uniformly mixed in the ratio of the amounts of the substances in the chemical formula, and a sintering process is carried out in an oxygen-containing atmosphere, thereby creating a Li x M1 y M2 1-y Obtain a kernel for lithium replenisher that is O6, where 6 ≤ x ≤ 8 and 0 <y<1である。
[0061] In some embodiments, the lithium source includes at least one of lithium carbonate, lithium hydroxide, and lithium oxide.
[0062] In some embodiments, the M1 source includes at least one of the oxides of M1, the chlorides of M1, the nitrates of M1, and the hydroxides of M1.
[0063] In some embodiments, the M2 source includes at least one of M2 oxides, M2 chlorides, M2 nitrates, and M2 hydroxides.
[0064] In some embodiments, the temperature of the first sintering treatment is 700°C to 1200°C, and the duration of the first sintering treatment is 8 hours to 24 hours. This contributes to obtaining pure phase kernel particles with appropriate particle sizes.
[0065] For example, the temperature of the first sintering process may be 700°C, 800°C, 900°C, 1000°C, 1100°C, or 1200°C.
[0066] For example, the duration of the first sintering treatment may be 8h, 10h, 12h, 14h, 16h, 18h, 20h, 22h, or 24h.
[0067] When the temperature and time of the first sintering treatment are within the range described above, it is advantageous for the formation of a hexagonal crystal kernel, the stability of the material phase structure is relatively high, there are few impurities, and the particle size of the formed kernel is appropriate.
[0068] In some embodiments, the oxygen-containing atmosphere may be an oxygen-containing atmosphere such as oxygen gas or air.
[0069] In step S200, the kernel, M source, and carbon source are subjected to a second sintering treatment in an inert atmosphere.
[0070] In some embodiments, in this step, the M source and the kernel are uniformly mixed, then further mixed with a carbon source, and then sintered in an inert atmosphere to form a coating layer on at least a portion of the surface of the kernel to obtain the lithium replenisher.
[0071] In some embodiments, the M source includes at least one of zirconium propoxide, zirconium oxide, zirconium nitrate, zirconium oxychloride, lithium zirconate, zirconium chloride, titanium oxide, titanium tetrachloride, titanium nitrate, and titanium alkoxide.
[0072] In some embodiments, the carbon source includes at least one of glucose, starch, sucrose, and graphite, thereby contributing to the formation of lithium-containing metal oxides on the surface of the kernel.
[0073] In some embodiments, the temperature of the second sintering treatment is 400°C to 800°C, and the duration of the second sintering treatment is 6H to 10H. This contributes to the formation of lithium-containing metal oxides and carbon materials in the coating layer.
[0074] For example, the temperature of the second sintering process may be 400°C, 500°C, 600°C, 700°C, or 800°C.
[0075] For example, the duration of the second sintering process may be 6h, 7h, 8h, 9h, or 10h.
[0076] When the temperature and time of the second sintering process are within the range described above, it contributes to the formation of tetragonal lithium-containing metal oxides and carbon materials with a high degree of graphitization, resulting in high stability of the material phase structure and minimal carbon loss.
[0077] In some embodiments, an inert atmosphere is required in the second sintering process for forming the coating layer, thereby effectively reducing the reaction between the carbon source and the active atmosphere and mitigating carbon leaching. For example, in an active atmosphere such as an oxygen-containing atmosphere, the carbon source is oxidized and released as carbon dioxide or carbon monoxide gas, resulting in carbon leaching.
[0078] For example, the inert atmosphere may include non-oxygen-containing and non-hydrogen-containing atmospheres such as nitrogen and argon.
[0079] In some embodiments, the process further includes a step of mixing the kernel, the M source, and the carbon source in a solvent and drying them before the second sintering process. This allows the kernel, carbon source, and M source to be sufficiently dispersed in the solvent, contributing to a more uniform mixing of the kernel, M source, and carbon source, and also contributes to improving the uniformity of the coating by removing the solvent by the drying process.
[0080] In some examples, the solvent includes at least one of ethanol and isopropanol.
[0081] In some embodiments, the drying process includes at least one of spray drying, freeze-drying, and flash drying.
[0082] In a third aspect of this application, the present application proposes a positive electrode slurry comprising the lithium replenisher described above, or a lithium replenisher manufactured by the method described above. The positive electrode slurry thereby possesses all the constituent elements and advantages of the lithium replenisher and the method for manufacturing the lithium replenisher described above. Further explanation is omitted here.
[0083] In some embodiments, the viscosity of the positive electrode slurry is 1000 mPa·s to 8000 mPa·s. This contributes to improving the processing performance of the positive electrode slurry.
[0084] By forming a coating layer on the surface of the lithium replenisher kernel, the influence of the kernel's alkaline surface on the slurry stability is effectively suppressed. After adding the lithium replenisher to the cathode slurry, lithium deposition reactions caused by the strongly alkaline surface of the lithium replenisher are eliminated. This effectively mitigates the significant increase in viscosity of the cathode slurry due to the increased alkalinity of the cathode slurry, contributing to the satisfaction of the cathode slurry coating requirements.
[0085] For example, a positive electrode slurry may be obtained by mixing a positive electrode material, a lithium replenisher, a solvent (e.g., N-methylpyrrolidone), an adhesive (e.g., polyvinylidene fluoride), and a conductive agent (e.g., carbon black, acetylene black) in a mass ratio of 90:2:100:4:4.
[0086] In a fourth aspect of the present application, the present application proposes a battery comprising a positive electrode tab including a positive electrode current collector and a positive electrode active material layer located on at least one side of the positive electrode current collector, wherein the positive electrode active material layer is manufactured from the positive electrode slurry described above. The battery thus possesses all the constituent requirements and advantages of the positive electrode slurry described above. Further explanation is omitted here.
[0087] The following describes the technical proposal of this application with specific examples. These examples are for illustrative purposes only and do not limit the scope of this application. Unless otherwise specified in the examples, specific techniques or conditions shall be followed in accordance with the techniques or conditions described in the literature in this industry or in accordance with the product manual. Unless otherwise specified, the reagents or equipment used shall be general-purpose products available on the market.
[0088] Example 1 (1) Lithium carbonate (lithium source), zirconium dioxide (M1 source), tungsten oxide (M2 source) Li:Zr:W=8:0 . 9:0 . The mixture is uniformly mixed in a high mixer at a molar ratio of 1, and then sintered at 900°C for 10 hours in an air atmosphere, resulting in a chemical formula of Li8Zr 0.9 W 0.1 Obtain the O6 kernel.
[0089] (2) Zirconium propoxide (M source) and the above kernel were weighed and mixed at a molar ratio of Zr:W = 1:10 to obtain a first mixture. The first mixture and glucose (carbon source) were weighed and mixed at a mass ratio of 99:1 to obtain a second mixture. The second mixture was added to pure water at 50% of the intrinsic content to obtain a mixed material. The mixed material was subjected to sand milling in a sand mill at a rotation speed of 2500 rpm for 1 hour, and the obtained mixed slurry was dried in a spray dryer to obtain powder. The powder was sintered at 800°C under a nitrogen atmosphere. Finally, a lithium supplement agent was obtained, wherein the coating layer contained Li2ZrO3 and a carbon material, and the kernel was Li8Zr 0.9 W 0.1 O6.
[0090] Examples 2 to 16 and Comparative Examples 1 to 16 are substantially the same as Example 1, and the differences are shown in Table 1. Here, in Comparative Example 3, no M2 source was added when forming the kernel; in Reference Example 4, no M1 source was added when forming the kernel; in Comparative Example 5, no M source was added when forming the coating layer; and in Comparative Example 6, no carbon source was added when forming the coating layer. Table 1 [Table 1-1] [Table 1-2] The parameters of the lithium supplement agents in the above Examples and Comparative Examples are shown in Table 2. Table 2 [Table 2]
[0091] The lithium supplement agents in the above Examples and Comparative Examples were fabricated into coin-type batteries, and the manufacturing method thereof is as follows.
[0092] The lithium replenishment material, acetylene black (a conductive agent), and polyvinylidene fluoride (an adhesive) are mixed in a mass ratio of 90:5:5. This mixture is applied to aluminum foil, dried, and then press-molded at a pressure of 100 MPa to form an electrode tab with a diameter of 12 mm and a thickness of 120 μm to form the positive electrode tab. A lithium metal tab with a diameter of 17 mm and a thickness of 1 mm is used as the negative electrode tab. A Celgard 2400 porous membrane with a thickness of 25 μm is used as the separator. 1 mol / L LiPF6 is used as the electrolyte, and an equivolute mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) is used as the solvent. The positive electrode tab, separator, negative electrode tab, and electrolyte are assembled into a 2025 type coin cell in an Ar gas glove box with water and oxygen content of less than 5 ppm.
[0093] The coin-type batteries in the above-described examples and comparative examples were subjected to the following tests, and the results of these tests are shown in Table 2.
[0094] Regarding the decomposition potential and charge / discharge capacity, rate tests were performed on assembled coin-type batteries under conditions of 3.0V to 4.9V and 0.1C. The charge ratio capacity, discharge ratio capacity, and discharge ratio energy were read from the test software, where the lithium replenisher decomposition potential = discharge ratio energy / discharge ratio capacity.
[0095] Regarding the lithium-ion transition rate of lithium replenisher, assembled coin-type batteries are subjected to EIS AC impedance testing on an electrochemical workstation, and the lithium-ion transition rate of the lithium replenisher is obtained from the slope of the linear segment in the AC impedance diagram. Table 3 [Table 3]
[0096] As can be seen from the test results, the coating layer on the surface of the lithium replenisher in Examples 1 to 16 effectively reduced the increase in viscosity of the positive electrode slurry caused by the alkalinity of the kernel surface during the use of the lithium replenisher, resulting in excellent processing performance of the positive electrode slurry. The high initial charge capacity of the lithium replenisher indicates sufficient lithium ion release from the lithium replenisher during the charging process, while the low initial discharge capacity of the lithium replenisher indicates that fewer lithium ions are reinserted into the lithium replenisher during the discharge process, thus achieving a good home position pre-lithification effect for lithium batteries.
[0097] Figure 1 is a scanning electron microscope image of the lithium replenisher in Example 1. From this figure, it can be seen that there is a coating layer on the surface of the kernel. Figure 2 shows that the S1 / S2 of the lithium replenisher in Example 1 is 0.03, and the S1 / S2 of the lithium replenisher in Comparative Example 5 is 0. Figure 3 is a charge / discharge graph of the coin cell battery in Example 1.
[0098] In Comparative Example 1, the viscosity of the positive electrode slurry increased significantly because there was too little tetragonal lithium-containing metal oxide in the coating layer of the lithium replenisher. In Comparative Example 2, , positive Because there is a large amount of crystalline lithium-containing metal oxide, the viscosity of the positive electrode slurry decreases, but at the same time, the lithium replenishment capacity of the lithium replenisher also decreases significantly. In Comparative Example 3, since the kernel of the lithium replenisher does not contain the M2 element, the transport rate of lithium ions in the kernel decreases, and in Comparative Example 4 In Comparative Example 1, the kernel of the lithium replenisher does not contain the M1 element, so the lithium replenishment capacity of the lithium replenisher is too small. In Comparative Example 5, since no tetragonal lithium-containing metal oxide was formed on the coating layer of the lithium replenisher, the viscosity of the positive electrode slurry increased significantly. In Comparative Example 6, since no carbon material was formed on the coating layer of the lithium replenisher, the lithium replenishment capacity of the lithium replenisher was poorly exhibited.
[0099] In the description of the present application, the terms "first" and "second" are used for the purpose of description only, and shall not be construed as indicating or implying relative importance or implying the number of indicated constituent features. The definitions of "first constituent feature" and "second constituent feature" are used in the sense that one or more such constituent features may be included.
[0100] In the description of the present application, "A and / or B" may include the case of A alone, the case of B alone, and the case of either A or B, where A and B are examples only, and may be any constituent feature connected by "and / or" in the present application.
[0101] It should be noted that the present application is not limited by the above-described embodiments. The above-described embodiments are merely illustrative. Within the scope of the technical solution of the present application, any embodiment having substantially the same configuration as the technical concept and exhibiting similar functions and effects shall be covered by the technical scope of the present application. In addition, various modifications that can be conceived by those skilled in the art without departing from the spirit of the present application, and other forms constructed by combining some constituent elements in the embodiments, are all included in the scope of the present application. In addition, the present application includes the following aspects. [Claim 1] Chemical formula Li x M1 y M2 1-y O 6 is satisfied, provided that 6≤x≤8 and 0<y<1, wherein M1 is at least one of Zr, Nb, Sb, Bi, Ru, Ta, Sn, Hf, Ir, Pr, Pt and Np, and M2 is at least one of W, Ge, Ca, Ce, K and Ta; and a coating layer disposed on at least a partial surface of the kernel, the coating layer including a lithium-containing metal oxide and a carbon material, wherein the lithium-containing metal oxide has a chemical formula Li a M b O c satisfied, provided that 1.8≤a≤2, 0.7≤b≤1.1 and 2.8≤c≤3, and M includes Ti and / or Zr; and when a 2θ diffraction angle is within a range of 20.1° to 20.3°, a peak intensity of a diffraction peak with respect to X-rays is S1, when the 2θ diffraction angle is within a range of 17° to 17.3°, a peak intensity of a diffraction peak with respect to X-rays is S2, and S1 / S2 is 0.02 to 0.05. The lithium supplementing agent. [Claim 2] The lithium supplementing agent according to claim 1, wherein a mass fraction of the lithium-containing metal oxide in the lithium supplementing agent is 0.01% to 0.1%, and / or a mass fraction of the carbon material in the lithium supplementing agent is 0.01% to 0.5%. [Claim 3] The lithium supplementing agent according to claim 1, wherein lattice constants of the kernel satisfy a=b and a≠c, and c / a is 2 to 3. [Claim 4] The lithium supplementing agent according to claim 3, wherein a is 0.4 nm to 0.7 nm, and c is 1.4 nm to 1.6 nm. [Claim 5] The lithium supplementing agent according to any one of claims 1 to 4, wherein a Dv50 particle size of the kernel is 1 μm to 10 μm, and / or a thickness of the coating layer is 50 nm to 500 nm. [Claim 6] The kernel includes Li 8 Zr 0.9 W 0.1 O 6 , Li 7 Nb 0.8 Ta 0.2 O 6 , Li 7 Sb 0.9 Ta 0.1 O 6 , Li 7 Ru 0.7 W 0.2 Ce 0.1 O 6 , Li 8 Sn 0.9 Ca 0.1 O 6 , Li 8 Hf 0.7 W 0.2 Ca 0.1 O 6 , Li 8 Ir 0.6 W 0.2 Ce 0.2 O 6 , Li 8 Pr 0.5 W 0.3 Ca 0.2 O 6 , Li 8 Pt 0.7 W 0.2 Ca 0.1 O6 The lithium supplementing agent according to any one of claims 1 to 4, comprising at least one of the foregoing. [Claim 7] The lithium supplementing agent according to any one of claims 1 to 4, wherein the carbon material has a graphitization degree of 60% or more. [Claim 8] A method of manufacturing the lithium supplementing agent according to any one of claims 1 to 7, including: The process involves a first sintering treatment of a lithium source, an M1 source, and an M2 source in an oxygen-containing atmosphere to obtain a kernel, A method comprising the steps of: subjecting the kernel, M source, and carbon source to a second sintering treatment in an inert atmosphere to form a coating layer on at least a portion of the surface of the kernel to obtain the lithium replenisher. [Section 9] The lithium source comprises and / or at least one of lithium carbonate, lithium hydroxide, and lithium oxide. The M1 source comprises at least one of the oxides of M1, the chlorides of M1, the nitrates of M1, and the hydroxides of M1, and / or The method according to claim 8, wherein the M2 source comprises at least one of M2 oxides, M2 chlorides, M2 nitrates, and M2 hydroxides. [Section 10] The method according to item 9, wherein the temperature of the first sintering treatment is 700°C to 1200°C, and the duration of the first sintering treatment is 8 hours to 24 hours. [Section 11] The M source comprises at least one of zirconium propoxide, zirconium oxide, zirconium nitrate, zirconium oxychloride, lithium zirconate, zirconium chloride, titanium oxide, titanium tetrachloride, titanium nitrate, and titanium alkoxide, and / or The method according to any one of claims 8 to 10, wherein the carbon source comprises at least one of glucose, starch, sucrose, and graphite. [Section 12] The method according to item 11, wherein the temperature of the second sintering treatment is 400°C to 800°C, and the duration of the second sintering treatment is 6 hours to 10 hours. [Section 13] The method according to claim 8, further comprising the step of mixing the kernel, the M source, and the carbon source in a solvent and performing a drying process before the second sintering process. [Section 14] The solvent comprises at least one of ethanol and isopropanol, and / or The method according to claim 13, wherein the drying treatment includes at least one of spray drying, freeze-drying, and flash drying. [Section 15] A cathode slurry comprising a lithium replenisher described in any one of items 1 to 7, or a lithium replenisher manufactured by the method described in any one of items 8 to 14. [Section 16] The positive electrode slurry according to item 15, wherein the viscosity of the positive electrode slurry is 1000 mPa·s to 8000 mPa·s. [Section 17] A positive electrode tab includes a positive electrode current collector and a positive electrode active material layer located on at least one side of the positive electrode current collector, A battery in which the positive electrode active material layer is manufactured by the positive electrode slurry described in item 15 or 16.
Claims
1. Chemical formula Li x M1 y M2 1-y O 6 A kernel that satisfies the following conditions, where 6 ≤ x ≤ 8 and 0 < y < 1, where M1 is at least one of Zr, Nb, Sb, Bi, Ru, Ta, Sn, Hf, Ir, Pr, Pt, Np, and M2 is at least one of W, Ge, Ca, Ce, K, Ta, and the ionic radius of the M2 element is greater than the ionic radius of the M1 element, At least a coating layer located on a portion of the surface of the kernel, comprising a lithium-containing metal oxide and a carbon material, wherein the lithium-containing metal oxide satisfies the chemical formula Lia'Mb'Oc', where 1.8 ≤ a' ≤ 2, 0.7 ≤ b' ≤ 1.1, and 2.8 ≤ c' ≤ 3, and M comprises a coating layer comprising Ti and / or Zr. When the 2θ diffraction angle is within the range of 20.1° to 20.3°, a diffraction peak is present for X-rays, and the peak intensity of this diffraction peak is S1. When the 2θ diffraction angle is within the range of 17° to 17.3°, a diffraction peak is present for X-rays, the peak intensity of the diffraction peak is S2, and S1 / S2 is 0.02 to 0.
05. The peak intensity of the diffraction peak was obtained by testing using an automatic X-ray diffractometer, with the test conditions being: operating voltage of 40 kV, operating current of 250 mA, continuous scanning using a means, scanning speed of 4° / min, step length of 0.02°, and scanning angle range of 10° to 80°, for a lithium replenisher.
2. The lithium replenisher according to claim 1, wherein the mass fraction of the lithium-containing metal oxide in the lithium replenisher is 0.01% to 0.1%, and / or the mass fraction of the carbon material in the lithium replenisher is 0.01% to 0.5%.
3. The lithium replenisher according to claim 1, wherein the lattice constant of the crystal lattice of the kernel satisfies a = b, a ≠ c, and c / a is 2 to 3.
4. The lithium replenisher according to claim 3, wherein a is 0.4 nm to 0.7 nm and c is 1.4 nm to 1.6 nm.
5. The lithium replenisher according to claim 1, wherein the Dv50 particle size of the kernel is 1 μm to 10 μm, and the thickness of the coating layer is 50 nm to 500 nm.
6. The kernel comprises Li 8 Zr 0.9 W 0.1 O 6 , Li 7 Nb 0.8 Ta 0.2 O 6 , Li 7 Sb 0.9 Ta 0.1 O 6 , Li 7 Ru 0.7 W 0.2 Ce 0.1 O 6 , Li 8 Sn 0.9 Ca 0.1 O 6 , Li 8 Hf 0.7 W 0.2 Ca 0.1 O 6 , Li 8 Ir 0.6 W 0.2 Ce 0.2 O 6 , Li 8 Pr 0.5 W 0.3 Ca 0.2 O 6 , Li 8 Pt 0.7 W 0.2 Ca 0.1 O 6 The lithium replenisher according to claim 1, comprising at least one of the foregoing compounds.
7. The lithium replenisher according to claim 1, wherein the degree of graphitization of the carbon material is 60% or more.
8. A method for producing the lithium replenisher described in claim 1, The process involves a step of obtaining a kernel by performing a first sintering treatment on a lithium source, an M1 source, and an M2 source in an oxygen-containing atmosphere, A method comprising the step of performing a second sintering treatment on the kernel, M source, and carbon source in an inert atmosphere to form a coating layer on at least a portion of the surface of the kernel to obtain the lithium replenisher.
9. The lithium source comprises and / or at least one of lithium carbonate, lithium hydroxide, and lithium oxide. The M1 source comprises at least one of the oxides of M1, the chlorides of M1, the nitrates of M1, and the hydroxides of M1, and / or The method according to claim 8, wherein the M2 source includes at least one of M2 oxide, M2 chloride, M2 nitrate, and M2 hydroxide.
10. The method according to claim 9, wherein the temperature of the first sintering treatment is 700°C to 1200°C, and the duration of the first sintering treatment is 8 hours to 24 hours.
11. The M source comprises at least one of zirconium propoxide, zirconium oxide, zirconium nitrate, zirconium oxychloride, lithium zirconate, zirconium chloride, titanium oxide, titanium tetrachloride, titanium nitrate, and titanium alkoxide, and / or The method according to claim 8, wherein the carbon source comprises at least one of glucose, starch, sucrose, and graphite.
12. The method according to claim 11, wherein the temperature of the second sintering treatment is 400°C to 800°C, and the duration of the second sintering treatment is 6 hours to 10 hours.
13. The method according to claim 8, further comprising the step of mixing the kernel, the M source, and the carbon source in a solvent and performing a drying treatment before the second sintering treatment.
14. The solvent comprises at least one of ethanol and isopropanol. The method according to claim 13, wherein the drying treatment includes at least one of spray drying, freeze-drying, and flash drying.
15. A positive electrode slurry comprising the lithium replenisher according to any one of claims 1 to 7.
16. The positive electrode slurry according to claim 15, wherein the viscosity of the positive electrode slurry is 1000 mPa·s to 8000 mPa·s.
Citation Information
Patent Citations
Composite lithium supplementing material as well as preparation method and application thereof
CN116364905A
Positive electrode material, positive plate and battery
CN116435477A
Positive electrode lithium supplementing agent material and preparation method and application thereof
CN117247051A