High-strength and highly flexible steel parts
The steel component with a refined microstructure and optimized composition addresses the challenge of premature cracking in high-strength steels, achieving high tensile strength and bendability for enhanced automotive safety and weight reduction.
Patent Information
- Application Number
- JP2025553722
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2024-04-15
- Filing Date
- 2025-02-18
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2045-02-18
AI Technical Summary
Existing high-strength steels face challenges in combining high mechanical strength with high impact resistance and bendability, as they tend to crack prematurely under bending loads, compromising crash safety and weight reduction efforts in automotive applications.
A steel component with a specific microstructure and chemical composition, featuring a 10% skin layer and 80% bulk layer, manufactured through hot stamping and controlled heat treatment, achieving a refined prior austenite grain size ratio and optimized element content, including 95% martensite with optional bainite and ferrite phases.
The steel component achieves an ultimate tensile strength of 1350 MPa or higher and a bending angle of 57° or more, ensuring high strength and flexibility for improved crash safety and weight reduction in automotive components.
Smart Images

Figure 0007955527000009 
Figure 0007955527000001 
Figure 0007955527000002
Abstract
Description
Technical Field
[0001] The present invention relates to high-strength steel components and methods for manufacturing the same.
Background Art
[0002] High-strength steel components can be used as structural elements in automotive vehicles for intrusion prevention or energy absorption purposes.
[0003] In such types of applications, it is desirable to produce steel components that combine high mechanical strength with high impact resistance. Furthermore, one of the major challenges in the automotive industry is to reduce vehicle weight in order to improve fuel efficiency without compromising safety requirements.
[0004] This weight reduction can be achieved in particular through the use of steel components that primarily have a martensitic microstructure.
[0005] It is difficult to produce very high-strength steels that also have good resistance to crack formation under bending. Indeed, very high-strength steels tend to crack prematurely when subjected to bending loads. This is detrimental to the crash safety of components made from such high-strength steels, because even though the material can withstand very high loads thanks to its high tensile strength, once cracks begin to appear in the component, these cracks propagate rapidly under continued loading, and the component fails prematurely.
Summary of Invention
Problem to be Solved by the Invention
[0006] The object of the present invention is to address the aforementioned problems and to provide a steel component that has a combination of high strength and high bendability.
Means for Solving the Problem
[0007] An object of the present invention is achieved by providing a steel part as described in claim 1, having optionally the features of claims 2 to 5 individually or in any possible combination. Another object of the present invention is achieved by applying the method for manufacturing such a steel part as described in claim 7.
[0008] Here, the present invention will be described and illustrated in detail by examples, without introducing any limitations, with reference to Figure 1, which is a schematic cross-sectional view of a steel part according to the present invention.
[0009] A steel blank refers to a flat sheet of steel cut into any shape suitable for its use. The blank has a top and bottom surface, also called the upper and bottom sides or upper and bottom surfaces. The distance between these surfaces is specified as the thickness of the blank. The thickness can be measured, for example, using a micrometer, with its spindle and anvil positioned on the top and bottom surfaces. Similarly, the thickness can also be measured for molded parts.
[0010] Steel parts refer to parts formed from steel blanks.
[0011] The average thickness of a part or a portion of a part refers to the overall average thickness of the material that makes up the part after it has been formed from a flat sheet into a three-dimensional part.
[0012] When referring to the thickness of a steel component, it refers to the local thickness measured, for example, using the spindle and angle described above, or, for example, using a cross-sectional micrograph. [Brief explanation of the drawing]
[0013] [Figure 1] Referring to Figure 1, the steel component 1 comprises a bulk portion 3 and top and bottom skin layers 2. The total thickness of the steel component 1 is t0, and the thickness ts of the skin layer 2 is ts = t0 × 10%. In other words, the skin layer 2, or simply the skin, occupies the outermost 10% of the thickness on both sides of the bulk. Conversely, the bulk portion 3, or simply the bulk, occupies the central 80% of the thickness of the steel component. [Modes for carrying out the invention]
[0014] Hot stamping is a forming technique that involves heating a blank to a temperature at which the steel microstructure transforms at least partially into austenite, forming the blank at a high temperature by stamping it, and rapidly cooling the formed part to obtain a microstructure with very high strength. Hot stamping makes it possible to obtain very high-strength parts with complex shapes and presents many technical advantages. It should be understood that the heat treatment undergone by the part includes not only the thermal cycle of the hot stamping process itself described above, but also, in some cases, other subsequent heat treatment cycles performed after the part has been painted to cure the paint, such as a paint curing step. The mechanical properties of the hot-stamped parts below were measured, for example, after a complete thermal cycle including an optional paint curing step.
[0015] Yield strength and ultimate tensile strength are measured according to ISO standard ISO 6892-1, published in October 2009. Tensile test specimens are cut from the flat areas of the hot-stamped parts. Smaller tensile test samples are taken, if necessary, to correspond to the entire available flat area on the part.
[0016] The bending angle is measured according to the VDA-238 bending standard. For the same material, the bending angle depends on the thickness. For simplicity, the bending angle values in this invention refer to those for a thickness of 1.5 mm. If the thickness is different from 1.5 mm, the bending angle values must be normalized to 1.5 mm by the following calculation, where α1.5 is the bending angle normalized to 1.5 mm, t is the thickness, and αt is the bending angle for thickness t.
[0017] α1.5 = (αt × √t) / √1.5
[0018] In this invention, the bending angle was measured transversely, i.e., transverse to the rolling direction in which the steel sheet moved during the hot rolling step. The bending angle was measured using a laser measuring device. The reported value is the value reached when the maximum bending force Fmax, expressed in N, was reached. When performing a bending test on a hot-stamped part, the sample is cut from a flat area of the part. If necessary, small-sized samples are taken to cover the entire available flat area on the part. If the rolling direction of a hot-stamped part is unknown, it can be determined using, for example, the following protocol.
[0019] - Electron backscatter diffraction (EBSD) analysis is performed across a sample fragment using a scanning electron microscope (SEM).
[0020] - The rolling direction is determined according to the intensity of the orientation density function (ODF) representing the main fiber at φ2 = 45°, where φ2 is the Euler angle as defined in "H.-J. Bunge: Texture Analysis in Materials Science - Mathematical Methods. 1st English Edition by Butterworth Co (Publ.) 1982" (see Figures 2.2 and 2.3 of the aforementioned publication for the definition of φ2).
[0021] The bending angle of a part represents its ability to withstand deformation without cracking.
[0022] Here, we describe an example of an experimental protocol for determining the mean prior austenite grain size (PAGS). This protocol is given as an example and is by no means limited.
[0023] - The test specimens are cut from press-hardened steel parts and polished using a solution containing fine oxides in a suspension to produce a perfectly scratch-free and deformation-free surface known as a mirror-polished surface.
[0024] - EBSD maps (Electron Backscatter Diffraction) are then acquired, for example, using a JEOL IT800 Field-Emission-Gun Secondary-Electron-Microscope (FEG-SEM) equipped with a Symmetry2-Oxford CMOS EBSD camera. Each EBSD map represents a zone of 0.25 mm × 0.20 mm. Two EBSD maps are performed for each measurement so that they are both statistically representative of the area considered and of the microstructure.
[0025] - The prior austenite grains can be reconstructed by crystallographic calculations based on both the crystallographic orientation of the measured martensite grains (measured EBSD map) and the orientation relationship linking martensite and austenite.
[0026] - The calculation is performed, for example, using Merengue2(R) software. The calculated austenite map is then post-processed, for example using AZtecCrystal software (Oxford Instruments(R)). Grain boundaries are defined as a minimum misorientation of 8°. The average prior austenite grain size (PAGS) is calculated from the equivalent diameter (d eq ) of each grain of the map considered, as follows:
[0027] [Equation]
[0028] The composition of the steel part according to the invention will now be described.
[0029] The chemical composition is indicated in terms of lower and upper limits of composition ranges, said limits being included within the possible composition ranges according to the invention. When preferred ranges for a given element are disclosed, the invention also discloses all possible combinations of these preferred ranges for the individual elements.
[0030] According to this invention, the carbon content is in the range of 0.18% to 0.27% to ensure satisfactory strength. If the carbon content exceeds 0.27%, the weldability and flexibility of the steel plate may decrease. If the carbon content is less than 0.18%, the tensile strength will not reach the target value.
[0031] The silicon content is in the range of 0.18% to 0.30%. Silicon is an element that is involved in the hardening of solid solutions and limits carbide formation. If it exceeds 0.30%, silicon oxide forms on the surface, impairing the coating properties of the steel. If it is less than 0.18%, the target mechanical properties will not be met.
[0032] The manganese content is in the range of 1.0% to 1.5%. Above 1.5%, the risk of MnS formation increases, impairing flexibility. Below 1.0%, the hardenability of the steel sheet during the hot stamping process decreases, preventing it from achieving the target mechanical properties.
[0033] The chromium content ranges from 0.14% to 0.25%. Chromium is used to provide strength through solid solution hardening and to improve the hardenability of steel sheets during hot stamping. Chromium is limited to 0.25% to limit costs and avoid processing problems. Below 0.14%, the target mechanical properties cannot be met.
[0034] The aluminum content is, manufacturing The titanium content is in the range of 0.02% to 0.06% because it is a very effective element for deoxygenating steel in the liquid phase. If the titanium content is insufficient, aluminum can protect boron. The aluminum content is less than 0.06% to avoid oxidation problems and ferrite formation during press hardening. Below 0.02%, the desired deoxygenation properties of aluminum in the liquid phase are not achieved.
[0035] The titanium content is in the range of 0.02% to 0.06% to protect boron; otherwise, boron would be trapped within the BN precipitate. To avoid excessive TiN formation, the titanium content is limited to 0.06%. Below 0.02%, the desired boron-protecting properties of titanium are not achieved.
[0036] The boron content is in the range of 0.0015% to 0.0040%. Boron improves the hardenability of steel. To avoid the problem of semi-finished products breaking immediately after casting, the boron content is 0.0040% or less. Below 0.0015%, the target mechanical properties cannot be met.
[0037] The presence of sulfur in molten steel can lead to the formation of MnS precipitates, which are detrimental to flexibility; therefore, the sulfur content is controlled to 0.005% or less, preferably 0.003%.
[0038] Phosphorus is controlled to 0.04% or less because it causes brittleness and weldability problems. In certain embodiments, the P content is controlled to 0.02% or less to further avoid brittleness and weldability problems.
[0039] Nitrogen levels should be controlled to 0.020% or less, preferably 0.015% or less. The presence of nitrogen can lead to the formation of precipitates such as TiN or TiNbCN, which can be detrimental to flexibility.
[0040] Molybdenum is added optionally, up to a maximum of 0.3%. Molybdenum improves the hardenability of steel. Molybdenum is limited to 0.3% to limit costs and avoid processing problems.
[0041] Niobium is added selectively, up to a maximum of 0.1%. Niobium improves the ductility of steel. Niobium is limited to 0.1% to limit costs and avoid processing problems.
[0042] Vanadium is added optionally up to a maximum of 0.3%. Vanadium improves the hardenability of steel. Vanadium is limited to 0.3% to limit costs and avoid processing problems.
[0043] If one or more of the above elements are added, the following formula is further validated to limit costs and avoid processing problems: Cr + Mo + Nb + V ≤ 0.5%.
[0044] The remainder of the steel's composition is iron and manufacturing These are impurities that arise from the manufacturing process. manufacturing The level of impurities generated from the process depends on the manufacturing route used and the level of scrap used in the molten steel. For example, when using a basic oxygen furnace route containing low-level steel scrap (recycled steel), the level of impurities remains very low. However, it is also possible to add a large amount of scrap from the converter to the pig iron produced in the basic oxygen furnace, which increases the level of impurities. Furthermore, for example, when using electric furnaces with a very high proportion of recycled scrap steel... manufacturing In this case, the level of impurities increases significantly. When using high-level scrap, the level of Cu can reach 0.25%, Ni can reach 0.25%, Sn can reach 0.05%, As can reach 0.03%, Sb can reach 0.03%, and Pb can reach 0.03%.
[0045] The steel component according to the present invention can be manufactured by any suitable method.
[0046] A preferred method involves first providing a semi-finished product by casting steel having the chemical composition according to the present invention. The casting is carried out continuously or in batches. The semi-finished product has a thickness in the range of, for example, 40 mm to 120 mm, preferably 50 mm to 70 mm. During the casting process, a casting speed of 3.0 m / min or more, preferably 4 m / min or more, is maintained.
[0047] For example, a semi-finished product having the above-mentioned chemical composition is manufactured by continuous casting, and the semi-finished product is optionally subjected to a light reduction process directly during the continuous casting process in order to avoid central segregation.
[0048] The semi-finished products provided by casting can be used directly at high temperatures after the casting step, or they may be first cooled to a low temperature and then reheated for hot rolling.
[0049] Prior to the subsequent hot rolling step, the semi-finished product is maintained or reheated to a reheating temperature of 1075°C to 1200°C, preferably 1100°C to 1200°C. By controlling the temperature of the semi-finished product within this range before hot rolling, the mechanical force required to reduce the thickness of the semi-finished product throughout the hot rolling process can be controlled.
[0050] The manufacturing process further includes the following steps: - A step of pickling the hot-rolled steel sheet, -Optionally, the hot-rolled steel sheet is cold-rolled to obtain a cold-rolled steel sheet. - A step of applying an annealing step to a hot-rolled or cold-rolled steel sheet by heating it in an annealing furnace to an annealing temperature TA expressed in degrees Celsius in the range of 700°C to 850°C, wherein the furnace further includes a soaking section in which the steel sheet is maintained at the temperature TA for a holding time tA of 10 seconds to 20 minutes. -Optionally, the step of cooling the annealed steel sheet to a temperature range of 400°C to 700°C. -Optionally, the step of coating the annealed steel sheet with a metal coating, - In order to obtain a steel blank, the steel plate is cut into a predetermined shape. - The steel blank is heated to a temperature of Ac3 or higher and 950°C or lower for 10 seconds to 15 minutes to obtain a heated steel blank. - A step of transferring the heated steel blank to a forming press, - A step of obtaining a molded part by hot forming the heated blank in a molding press, - A step of die-quenching the molded part to obtain a steel part, -Optionally, the steel part is painted and baked at a temperature of 150°C to 250°C for 10 minutes to 2 hours.
[0051] Optionally, a steel part can be obtained by hot stamping a steel blank having a metal coating on at least one of its outer surfaces. For example, the coating is an aluminum-based coating containing at least 50% aluminum. When the steel blank is hot stamped, the heat from the austenitization step induces interdiffusion between the elements of the steel substrate beneath the coating and the elements of the coating. As a result, the coating on the steel part has an increased iron content, in particular, compared to the amount of iron present in the metal coating on the steel blank.
[0052] Next, the microstructure of the steel component according to the present invention will be described.
[0053] The steel component contains 95% or more martensite by surface fraction, with the remainder being optionally bainite, ferrite, and / or retained austenite. Bainite, ferrite, and retained austenite are optional phases, and in a preferred embodiment, the microstructure of the component consists of 100% martensite.
[0054] Surprisingly, the inventors have found that the steel component according to the present invention exhibits a difference in PAGS between the skin and the bulk. More specifically, the inventors have found that the steel component according to the present invention has finer PAGS in the skin than in the bulk. PAGS_B is the average prior austenite grain size in the bulk, expressed in μm. PAGS_S is the average prior austenite grain size in the skin, expressed in μm. The PAGS skin refinement ratio is defined as PAGS_B / PAGS_S. The steel component according to the present invention has a PAGS skin refinement ratio of 1.2 or higher.
[0055] In certain embodiments, the average prior austenite particle size PAGS_S is 6.0 μm or less.
[0056] The inventors have found that steel parts having the aforementioned properties exhibit excellent strength and flexibility. This provides parts with very good impact resistance and impact absorption capabilities.
[0057] In particular, the inventors have found that the steel part has an ultimate tensile strength of 1350 MPa or more, preferably 1400 MPa or more, measured in the transverse direction, and a bending angle α1.5 of 57° or more, measured in the transverse direction and normalized to a thickness of 1.5 mm. [Examples]
[0058] The present invention will now be explained using examples.
[0059] Samples R1 to R3 are reference samples not according to the present invention. Samples I1 to I4 are inventive samples according to the present invention.
[0060] Tables 1a and 1b summarize the chemical composition (weight %) of the samples and the calculated Ac3 temperature (°C).
[0061] [Table 1]
[0062] [Table 2]
[0063] Table 2 summarizes the process parameters used to produce the samples. Underlined values in the table are not according to the present invention.
[0064] [Table 3]
[0065] Table 3 summarizes the characteristics measured for samples after hot stamping and paint curing.
[0066] [Table 4]
[0067] Table 4 summarizes the microstructural characteristics of the samples after hot stamping. The average prior austenite grain size (PAGS_S and PAGS_B) is expressed in microns. The prior austenite grain surface refinement ratio is calculated by dividing two values having the same units, and is therefore a dimensionless quantity. Underlined values in the table are not according to the present invention.
[0068] [Table 5]
[0069] The steel component according to the present invention has a prior austenite skin grain refinement ratio of 1.2 or higher and the chemical properties according to the present invention, thereby achieving extremely high mechanical properties with an ultimate tensile strength of 1350 MPa or higher in the transverse direction, and at the same time being able to maintain a high bending angle of 57° or higher in the transverse direction, normalized to a thickness of 1.5 mm.
Claims
1. Steel part (1), having the following characteristics: - In mass percent, 0.18 ≤ C ≤ 0.27 0.18 ≤ Si ≤ 0.30 1.0 ≤ Mn ≤ 1.5 0.14 ≤ Cr ≤ 0.25 0.02 ≤ Al ≤ 0.06 0.02 ≤ Ti ≤ 0.06 0.0015 ≤ B ≤ 0.0040 0 ≤ S ≤ 0.008 0 ≤ P ≤ 0.04 0 ≤ N ≤ 0.020 0 ≤ Mo ≤ 0.3 0 ≤ Nb ≤ 0.1 0 ≤ V ≤ 0.3, 0 ≤ Cu ≤ 0.25, 0 ≤ Ni ≤ 0.25, 0 ≤ Sn ≤ 0.05, 0 ≤ As ≤ 0.03, 0 ≤ Sb ≤ 0.03, 0 ≤ Pb ≤ 0.03, Includes, The remaining components of the composition are iron and unavoidable impurities arising from the manufacturing process, - A microstructure containing 95% or more martensite by surface fraction, with the remainder being optionally selected bainite, ferrite, and / or retained austenite. - The steel part (1) comprises a bulk portion (3) that occupies the central 80% of its thickness, and skins (2) that occupy the outermost 10% of its thickness on both sides of the bulk portion (3), - Defined as PAGS_B / PAGS_S, where PAGS_B is the average prior austenite grain size in the bulk (3) expressed in μm, and PAGS_S is the average prior austenite grain size in the skin (2) also expressed in μm, with a prior austenite grain refinement ratio of 1.2 or more. It has, PAGS_B and PAGS_S are determined from electron backscatter diffraction maps, prior austenite grains are reconstructed by crystallographic calculations based on both the crystallographic orientation of the measured martensite grains and the orientation relationship linking martensite and austenite, grain boundaries are defined as a minimum misorientation of 8°, and the average prior austenite grain size (PAGS) is calculated based on the equivalent diameter (d eq) of each particle in the map considered, as follows, for steel parts. [Math 1]
2. The steel part according to claim 1, wherein the average prior austenite grain size PAGS_S in the skin is 6.0 μm or less.
3. It has an ultimate tensile strength of 1350 MPa or more as measured in the lateral direction. The steel part according to claim 1, wherein the lateral direction is lateral to the rolling direction in which the steel plate moved during the hot rolling step.
4. Measured in the lateral direction and normalized to a thickness of 1.5 mm, it has a bending angle α1.5 of 57° or more. α1.5 is normalized by the following formula, where t is the thickness and αt is the bending angle relative to the thickness t. α1.5=(αt×√t) / √1.5 The steel part according to claim 1, wherein the lateral direction is lateral to the rolling direction in which the steel plate moved during the hot rolling step.
5. The steel part according to claim 1, which is covered with a metal coating containing 50% or more aluminum by mass.
6. A method for manufacturing steel parts, comprising the following steps: - A step of providing the steel composition described in claim 1, - A step of casting a semi-finished product having the above composition at a casting speed of 3.0 m / min or more, -Optionally, a step of cooling the semi-finished product after casting, - A step of maintaining or reheating the semi-finished product in a temperature range of 1075°C to 1200°C. The steps of obtaining a hot-rolled steel sheet by hot-rolling the semi-finished product using a finishing temperature of -850°C or higher and a winding temperature of 525°C or higher, - The step of pickling the hot-rolled steel sheet, -Optionally, the hot-rolled steel sheet is cold-rolled to obtain a cold-rolled steel sheet. - A step of applying the step of annealing the hot-rolled or cold-rolled steel sheet by heating it in an annealing furnace to an annealing temperature TA expressed in °C, which is 700 °C to 850 °C, wherein the furnace further includes a soaking section in which the steel sheet is maintained at the temperature TA for a holding time tA of 10 seconds to 20 minutes. -Optionally, a step of cooling the steel plate to which the annealing step has been applied to a temperature range of 400°C to 700°C. -Optionally, a step of coating the steel plate to which the annealing step has been applied with a metal coating. - In order to obtain a steel blank, the steel plate is cut into a predetermined shape. - The steel blank is heated to a temperature of Ac3 or higher and 950°C or lower for 10 seconds to 15 minutes to obtain a heated steel blank. - A step of transferring the heated steel blank to a forming press, - A step of obtaining a molded part by hot forming the heated blank in the molding press, - A step of die-quenching the molded part to obtain a steel part, -Optionally, the steel part is painted and baked at a temperature of 150°C to 250°C for 10 minutes to 2 hours. Includes, The aforementioned steel component has the following characteristics: - A microstructure containing 95% or more martensite by surface fraction, with the remainder being optionally selected bainite, ferrite, and / or retained austenite. - The steel component comprises a bulk portion that occupies the central 80% of its thickness, and skins that occupy the outermost 10% of its thickness on both sides of the bulk, - Defined as PAGS_B / PAGS_S, where PAGS_B is the average prior austenite grain size in the bulk expressed in μm, and PAGS_S is the average prior austenite grain size in the skin expressed in μm, with a prior austenite grain refinement ratio of 1.2 or more. It has, PAGS_B and PAGS_S are determined from electron backscatter diffraction maps, prior austenite grains are reconstructed by crystallographic calculations based on both the crystallographic orientation of the measured martensite grains and the orientation relationship linking martensite and austenite, grain boundaries are defined as a minimum misorientation of 8°, and the average prior austenite grain size (PAGS) is calculated as follows based on the equivalent diameter (d eq) of each particle in the map considered: method. [Math 2]
Citation Information
Patent Citations
High-strength and high-ductility steel plate and its manufacturing method
JP2004244665A
METHOD FOR PRODUCING HIGH IMPACT RESISTANT STEEL PIPE EXCELLENT IN DELAYED FRACTURING CHARACTERISTIC OF 1,700 MPa OR MORE OF TENSILE STRENGTH
JP2007154289A
High-strength thin steel sheet having superior delayed-fracture resistance after having been formed, and manufacturing method therefor
JP2008056991A
Steel sheet for hot stamping, and hot stamp molded body
WO2022059321A1