Polymer film and laminated glass containing the same

A three-layer polymer film with controlled molecular weight and glass transition temperature addresses sound insulation and bubble issues in laminated glass, maintaining performance and appearance across temperature variations.

JP7955541B1Active Publication Date: 2026-11-24CHANG CHUN PETROCHEMICAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2026021285
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2025-11-17
Filing Date
2026-02-12
Publication Date
2026-11-24
Estimated Expiration
2046-02-12

AI Technical Summary

Technical Problem

Existing polymer films used as interlayers in laminated glass exhibit decreased sound insulation properties at low temperatures and form unsightly snowflake-shaped bubbles, compromising aesthetic appeal and practicality.

Method used

A polymer film comprising three layers, with the first layer containing polyvinyl acetal having a specific molecular weight range and glass transition temperature, is used to maintain excellent sound insulation and prevent bubble formation at low temperatures.

Benefits of technology

The polymer film ensures excellent sound insulation and aesthetic appeal at ambient or lower temperatures by controlling molecular weight and glass transition temperature, preventing bubble formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955541000001
    Figure 0007955541000001
  • Figure 0007955541000002
    Figure 0007955541000002
Patent Text Reader

Abstract

By using laminated glass containing the polymer film of the present invention under ambient temperature conditions of room temperature or lower, it is possible to obtain excellent aesthetics and practicality, as well as excellent sound insulation. [Solution] The present invention relates to a polymer film comprising a first layer, a second layer, and a third layer, wherein the first layer is placed between the second layer and the third layer, the first layer comprises a first polyvinyl acetal, the content of a component in the first polyvinyl acetal having a molecular weight in the range of 100,000 to 1,200,000 Da is 70 to 80 wt.%, and the glass transition temperature of the first layer is -16.00°C to 5.00°C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polymer film, and more particularly, but not limited to, a polymer film applied to an interlayer film of laminated glass.

Background Art

[0002] Polyvinyl acetal is a composition produced by condensing polyvinyl alcohol and aldehyde. Its production method generally includes steps such as preparing an aqueous polyvinyl alcohol solution, performing an acetalization reaction, washing to remove impurities, and drying to remove excess water. Polyvinyl acetal has excellent adhesiveness and compatibility with various inorganic and organic substrates, excellent solubility in organic solvents, and further excellent optical properties. It is widely used as various adhesives, ceramic adhesives, inks, paints, etc., or as an interlayer film for laminated glass for vehicles and buildings.

[0003] Laminated glass (or bonded glass, laminated glass, etc.) is a type of safety glass, and generally, an interlayer film is included between two or more layers of glass. As the interlayer film, a polymer film made of polyvinyl butyral (PVB) or ethylene-vinyl acetate (EVA) material is often seen. When the glass bursts, the interlayer film can keep the glass still in an adhesive state, thereby preventing it from breaking into large sharp pieces and forming a specific "spider web" crack pattern.

[0004] In addition to the safety properties described above, laminated glass is also applied to sound insulation. Laminated glass that combines safety and noise reduction capabilities is suitable for automobiles and construction. Compared with single-pane glass windows having the same thickness, laminated glass has a better vibration damping effect on sound waves and has an excellent sound insulation effect. In this application, the interlayer film of laminated glass may adopt a multilayer film structure. The difference in material of the multilayer film structure effectively reduces the energy of sound wave propagation and further improves the sound insulation effect of the interlayer film. [Overview of the project] [Problems that the invention aims to solve]

[0005] Polymer films used as interlayers in laminated glass must have excellent sound insulation properties. Generally, the evaluation temperature for sound insulation is set at 20°C. However, the inventors have discovered that the sound insulation properties of existing polymer films often decrease with decreasing temperature, and that even when using conventionally known laminated glass at low ambient temperatures (e.g., below 10°C), excellent sound insulation cannot be obtained. Furthermore, the inventors have also discovered that using laminated glass with a polymer film that has excellent sound insulation properties at low temperatures as an interlayer always results in the formation of snowflake-shaped bubbles, which reduces the aesthetic appeal and practicality of the laminated glass. [Means for solving the problem]

[0006] To solve the above technical problems, the present invention provides a polymer film comprising a first layer, a second layer, and a third layer, wherein the first layer is placed between the second layer and the third layer, the first layer comprises a first polyvinyl acetal, the content of a component in the first polyvinyl acetal having a molecular weight in the range of 100,000 to 1,200,000 Da is 70 to 80 wt.%, and the glass transition temperature of the first layer is -16.00 to 5.00°C.

[0007] In some embodiments of the present invention, the content of the component in the first polyvinyl acetal having a molecular weight in the range of 100,000 to 1,200,000 Da is 70 to 72 wt.%.

[0008] In some embodiments of the present invention, the glass transition temperature of the first layer is -16.00 to -10.00°C.

[0009] In some embodiments of the present invention, the content of the component with a molecular weight greater than 1,000,000 Da in the first polyvinyl acetal is 2.0 to 9.0 wt.%.

[0010] In some embodiments of the present invention, the weight-average molecular weight of the first polyvinyl acetal is 230,000 to 520,000 Da.

[0011] In some embodiments of the present invention, the weight-average molecular weight of the first polyvinyl acetal is 250,000 to 480,000 Da.

[0012] In some embodiments of the present invention, the degree of polymerization of the first polyvinyl acetal is 2000 to 4500.

[0013] In some embodiments of the present invention, the degree of polymerization of the first polyvinyl acetal is 2200 to 4200.

[0014] In some embodiments of the present invention, the hydroxyl group content of the first polyvinyl acetal is 23.0 to 28.0 mol%.

[0015] In some embodiments of the present invention, the degree of acetylation of the first polyvinyl acetal is 7.0 to 12.0 mol%.

[0016] In some embodiments of the present invention, the degree of acetalization of the first polyvinyl acetal is 60.0 to 68.0 mol%.

[0017] In some embodiments of the present invention, the second layer comprises a second polyvinyl acetal, and the weight-average molecular weight of the second polyvinyl acetal is 200,000 to 280,000 Da.

[0018] In some embodiments of the present invention, the third layer comprises a third polyvinyl acetal, and the weight-average molecular weight of the third polyvinyl acetal is 200,000 to 280,000 Da.

[0019] In some embodiments of the present invention, the first layer further comprises a plasticizer.

[0020] In some embodiments of the present invention, the plasticizer in the first layer is present in an amount of 55 parts by weight to 80 parts by weight, based on 100 parts by weight of the first polyvinyl acetal.

[0021] In another aspect of the present invention, there is provided a laminated glass comprising a first glass sheet, a second glass sheet, and the polymer film disposed between the first glass sheet and the second glass sheet.

Effects of the Invention

[0022] An advantage of the present invention is that, by using a laminated glass including the polymer film of the present invention at an ambient temperature of room temperature or lower, it has excellent aesthetics and practicability, and at the same time, can also have an excellent sound insulation effect.

Description of Embodiments

[0023] To provide a more detailed and complete description of the present invention, the following is a descriptive illustration of embodiments and specific examples of the present invention, which are not the only forms for implementing or using the specific examples of the present invention. In the present specification and the appended claims, unless otherwise specified in the context, "a" and "said" may be interpreted as plural.

[0024] Both the numerical ranges and parameters used to limit the present invention are approximate values, but the relevant numerical values in the specific examples are shown as accurately as possible herein. However, essentially, any numerical value inevitably includes a standard deviation due to its respective measurement method. Therefore, unless otherwise specified, the numerical parameters disclosed in the present specification and the appended claims are approximate values and may be modified as needed. These numerical parameters should be understood to be at least the numerical values obtained by applying the indicated number of significant digits and ordinary rounding.

[0025] In this specification and the appended claims, unless otherwise specified, "disposed between" means directly or indirectly attached to, or otherwise in contact with the surface of, another object. The surface shall be determined based on the context of the preceding and following paragraphs of the specification and common general knowledge in the technical field to which this specification belongs.

[0026] [Polymer Film]

[0027] According to one aspect of the present invention, there is provided a polymer film comprising a first layer, a second layer and a third layer, wherein the first layer is disposed between the second layer and the third layer, and the first layer comprises a first polyvinyl acetal. According to some preferred embodiments of the present invention, the second layer comprises a second polyvinyl acetal. According to other preferred embodiments of the present invention, the third layer comprises a third polyvinyl acetal.

[0028] The first polyvinyl acetal, the second polyvinyl acetal and the third polyvinyl acetal described in the present application are formed by condensing polyvinyl alcohol and an aldehyde. The polyvinyl alcohol is formed by saponifying a vinyl ester polymer obtained by polymerizing a vinyl ester monomer. The saponification degree of the polyvinyl alcohol is usually 70.0 to 99.9 mol%, specifically, a value of 70.0 mol%, 75.0 mol%, 80.0 mol%, 85.0 mol%, 90.0 mol%, 95.0 mol%, 99.0 mol%, 99.9 mol%, or a value between any two of these values.

[0029] Examples of vinyl ester monomers include vinyl formate, vinyl acetate, vinyl propionate, vinyl pentanoate, vinyl octanoate, vinyl laurate, vinyl stearate, vinyl benzoate, vinyl trimethylacetate, 2,2,4,4-tetramethylpentanoate vinyl, and tert-pentanoate vinyl, but the present invention is not limited to these. Preferably, the vinyl ester polymer is a polymer obtained by using one or more vinyl ester monomers individually. More preferably, the polymer is obtained by using one vinyl ester monomer individually. Furthermore, the vinyl ester polymer may be a copolymer of one or more vinyl ester monomers and other copolymerizable monomers.

[0030] The aforementioned covalent elements include, for example, olefins having 3 to 30 carbon atoms such as ethylene, propylene, 1-butene, and isobutene; acrylic acid or its salts; acrylates such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, 2-ethylhexyl acrylate, dodecyl acrylate, and octadecyl acrylate; methacrylic acid or its salts, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, and methacrylic acid. Methacrylates such as isopropyl, n-butyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, 2-ethylhexyl methacrylate, dodecyl methacrylate, octadecyl methacrylate, acrylamide, N-methylacrylamide, N-ethylacrylamide, N,N-dimethylacrylamide, diacetoneacrylamide, acrylamidopropanesulfonic acid or its salts, acrylamidopropyldimethylamine or its salts, N-hydroxymethylacrylamide or its derivatives, and other acrylamide derivatives. These may include methacrylamide, N-methylmethacrylamide, N-ethylmethacrylamide, methacrylamidepropanesulfonic acid or its salts, methacrylamidepropyldimethylamine or its salts, methacrylamide derivatives such as N-hydroxymethylmethacrylamide or its derivatives, N-vinylamides such as N-vinylformamide, N-vinylacetamide, and N-vinylpyrrolidone, vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, n-propyl vinyl ether, isopropyl vinyl ether, n-butyl vinyl ether, isobutyl vinyl ether, tert-butyl vinyl ether, dodecyl vinyl ether, and stearyl vinyl ether, cyanoethylenes such as acrylonitrile and methacrylonitrile, vinyl halogenated groups such as vinyl chloride, vinylidene chloride, vinyl fluoride, and vinylidene fluoride, allyl compounds such as allyl acetate and chloropropene, maleic acid or its salts, esters or acid anhydrides, itaconic acid or its salts, esters or acid anhydrides, vinylsilyl compounds such as vinyltrimethoxysilane, and isopropenyl acetate.Furthermore, the vinyl ester polymer may have one or more structural units derived from these copolymerizable elements.

[0031] Generally, the aldehyde can be an aldehyde having 1 to 10 carbon atoms, for example, formaldehyde, acetaldehyde, propionaldehyde, n-butyraldehyde, isobutyraldehyde, n-pentylaldehyde, 2-ethylbutyraldehyde, n-hexylaldehyde, n-octylaldehyde, n-nonylaldehyde, n-decylaldehyde, benzaldehyde, or a combination thereof. Preferably, it is acetaldehyde, propionaldehyde, n-butyraldehyde, isobutyraldehyde, n-hexylaldehyde, n-pentylaldehyde, or a combination thereof. More preferably, it is acetaldehyde, n-butyraldehyde, isobutyraldehyde, or a combination thereof. According to one preferred embodiment of the present invention, the first polyvinyl acetal is polyvinyl butyral. According to another preferred embodiment of the present invention, the second polyvinyl acetal is polyvinyl butyral. According to another preferred embodiment of the present invention, the third polyvinyl acetal is polyvinyl butyral.

[0032] The polymer film relates to its vibration damping effect against sound waves and its viscoelastic material properties. By controlling the polymer film to have appropriate viscoelasticity, it is possible to reduce the volume by converting sound waves into stored and consumed energy of material molecular motion through interference with the medium as sound waves pass through the polymer film. Although not limited to a specific theory, it is generally believed that the softer the polymer film, the better the sound insulation effect. However, because it is softer, air bubbles are more likely to burst in the laminated glass containing it, forming snowflake-shaped bubbles. The inventors have discovered that the viscoelasticity of the polymer film is related to the distribution of the molecular weight of the first polyvinyl acetal, and that by controlling the distribution of the molecular weight of the polyvinyl acetal, the polymer film can be made to have appropriate viscoelasticity. Specifically, the content of components in the first polyvinyl acetal with a molecular weight in the range of 100,000 to 1,200,000 Da is 70 to 80 wt.%, for example, 70 wt.%, 71 wt.%, 72 wt.%, 73 wt.%, 74 wt.%, 75 wt.%, 76 wt.%, 77 wt.%, 78 wt.%, 79 wt.%, 80 wt.%, or in the range between any two of these values. Preferably, it is 70 to 75 wt.%, and more preferably 70 to 72 wt.%.

[0033] While not limited to any particular theory, a lower glass transition temperature of a material generally indicates greater softness. Consequently, the polymer film formed by it has better sound insulation properties, but it is also more prone to the formation of snowflake-shaped bubbles in the laminated glass. The reverse is also true. In contrast, the inventors have found that by controlling the glass transition temperature of the first layer within a specific range, the polymer film can be made to have appropriate viscoelasticity. Specifically, the glass transition temperature of the first layer is -16.00°C to 5.00°C, for example, -16.00°C, -15.27°C, -15.00°C, -14.00°C, -13.00°C, -12.00°C, -11.00°C, -10.66°C, -10.00°C, -9.00°C, -8.00°C, -7.29°C, -7.00°C, -6.00°C, -5.00°C, -4.00°C, -3.00°C, -2.00°C, -1.00°C, 0.00°C, 0.31°C, 1.00°C, 2.00°C, 3.00°C, 4.00°C, 4.37°C, 5.00°C, or may be in the range between any two of these values. Preferably, the temperature range is -16.00°C to -7.00°C, and more preferably -16.00°C to -10.00°C.

[0034] According to some embodiments of the present invention, the content of components with a molecular weight greater than 1,000,000 Da in the first polyvinyl acetal is 2 to 9 wt.%, and specifically, it may be 2 wt.%, 3 wt.%, 4 wt.%, 5 wt.%, 6 wt.%, 7 wt.%, 8 wt.%, 9 wt.%, or in the range between any two of these values. Preferably, it is 2 to 6 wt.%.

[0035] According to some embodiments of the present invention, the weight-average molecular weight (Mw) of the first polyvinyl acetal is 230,000 to 520,000 Da, and specifically, it may be in the range of 230,000 Da, 250,000 Da, 270,000 Da, 290,000 Da, 310,000 Da, 320,000 Da, 330,000 Da, 350,000 Da, 370,000 Da, 390,000 Da, 400,000 Da, 410,000 Da, 430,000 Da, 450,000 Da, 470,000 Da, 480,000 Da, 490,000 Da, 510,000 Da, 520,000 Da, or any two of these values. Preferably, it is 250,000 to 480,000 Da.

[0036] According to some embodiments of the present invention, the degree of polymerization of the first polyvinyl acetal is 2000 to 4500, and specifically, it may be in the range of 2000, 2200, 2500, 2800, 3000, 3500, 4000, 4200, 4500, or any two of these values. Preferably, it is 2200 to 4200, and more preferably 2200 to 2800.

[0037] According to several embodiments of the present invention, the degree of acetalization of the first polyvinyl acetal is 60.0 to 70.0 mol%, and specifically, it may be 60.0 mol%, 60.5 mol%, 61.0 mol%, 62.0 mol%, 63.0 mol%, 64.0 mol%, 65.0 mol%, 66.0 mol%, 66.6 mol%, 67.0 mol%, 67.1 mol%, 67.5 mol%, 67.8 mol%, 68.0 mol%, 69.0 mol%, 70.0 mol%, or in the range between any two of these values. Preferably, it is 60.0 to 68.0 mol%, more preferably 60.5 to 67.8 mol%. According to other embodiments of the present invention, the degree of acetalization of the second polyvinyl acetal or the third polyvinyl acetal is 60.0 to 75.0 mol%, and specifically, it may be in the range of 60.0 mol%, 65.0 mol%, 70.0 mol%, 70.4 mol%, 70.6 mol%, 70.9 mol%, 71.6 mol%, 75.0 mol%, or any two of these values. Preferably, it is 70.4 to 71.6 mol%.

[0038] According to one embodiment of the present invention, the hydroxyl group content of the first polyvinyl acetal is 20.0 to 32.0 mol%, and specifically, it may be 20.0 mol%, 21.0 mol%, 22.0 mol%, 23.0 mol%, 23.5 mol%, 23.9 mol%, 24.0 mol%, 24.2 mol%, 25.0 mol%, 26.0 mol%, 26.4 mol%, 27.0 mol%, 27.5 mol%, 28.0 mol%, 29.0 mol%, 30.0 mol%, 31.0 mol%, 32.0 mol%, or in the range between any two of these values. Preferably, it is 23.0 to 28.0 mol%, more preferably 23.5 to 27.5 mol%. According to several other embodiments of the present invention, the hydroxyl group content of the second polyvinyl acetal or the third polyvinyl acetal is 20.0 to 35.0 mol%, specifically 20.0 mol%, 25.0 mol%, 27.4 mol%, 28.1 mol%, 28.4 mol%, 28.6 mol%, 30.0 mol%, 35.0 mol%, or a range between any two of these values. Preferably, it is 27.4 to 28.6 mol%.

[0039] According to some embodiments of the present invention, the degree of acetylation of the first polyvinyl acetal is 5.0 to 15.0 mol%, specifically 5.0 mol%, 6.0 mol%, 7.0 mol%, 8.0 mol%, 9.0 mol%, 10.0 mol%, 11.0 mol%, 12.0 mol%, 13.0 mol%, 14.0 mol%, 15.0 mol%, or a range between any two of these values. Preferably, it is 7.0 to 12.0 mol%. According to other embodiments of the present invention, the degree of acetylation of the second or third polyvinyl acetal is 0.1 to 5.0 mol%, specifically 0.1 mol%, 0.5 mol%, 1.0 mol%, 2.0 mol%, 3.0 mol%, 4.0 mol%, 5.0 mol%, or a range between any two of these values. Preferably, it is 0.5 to 1.5 mol%. More preferably, it is 1.0 mol%.

[0040] According to some embodiments of the present invention, the weight-average molecular weight of the second polyvinyl acetal is 200,000 to 280,000 Da, and specifically, it may be in the range of 200,000 Da, 210,000 Da, 220,000 Da, 230,000 Da, 240,000 Da, 250,000 Da, 260,000 Da, 270,000 Da, 280,000 Da, or any two of these values. According to other embodiments of the present invention, the weight-average molecular weight of the third polyvinyl acetal is 200,000 to 280,000 Da, and specifically, it may be in the range of 200,000 Da, 210,000 Da, 220,000 Da, 230,000 Da, 240,000 Da, 250,000 Da, 260,000 Da, 270,000 Da, 280,000 Da, or any two of these values.

[0041] In addition, to the extent that it does not produce adverse effects, the polymer film may further contain plasticizers, stabilizers, antioxidants, heat stabilizers, anti-aging agents, anti-UV agents, ultraviolet absorbers, flame retardants, lubricants, rheological additives, crosslinking agents, colorants, dyes, pigments, fillers, preservatives, antifungal agents, antistatic agents, coupling agents, chelating agents, dispersants, adhesion regulators, moisture-proofing agents, fluorescent whitening agents, infrared absorbers, infrared blocking agents, or combinations thereof.

[0042] The aforementioned plasticizer or plasticizer includes monobasic acid esters, polybasic acid esters, organic phosphoric acid, organic phosphorous acid, or combinations thereof. Specific examples include triethylene glycol bis(2-ethylhexanoate), 3GO, tetraethylene glycol bis(2-ethylhexanoate), triethylene glycol bis(2-ethylbutyrate), tetraethylene glycol bis(2-ethylbutyrate), triethylene glycol diheptanoate, tetraethylene glycol diheptanoate, dihexyl adipate, dioctyl adipate, hexylcyclohexyl adipate, diisononyl adipate, heptylnonyl adipate, dibutyl sebacate, and adipyl This may be bis[2-(2-butoxyethoxy)ethyl] benzoate, polyadipate, propylene glycol dibenzoate, dipropylene glycol dibenzoate, tripropylene glycol dibenzoate, polypropylene glycol dibenzoate, 2,2,4-trimethyl-1,3-pentanediol dibenzoate, isodecyl benzoate, 2-ethylhexyl benzoate, diisononyl phthalate, dibutoxyethyl terephthalate, castor oil, methyl ricinoleate, soybean oil, epoxidized soybean oil, or a combination thereof. Preferably, it is triethylene glycol bis(2-ethylhexanoate).

[0043] According to several embodiments of the present invention, the content of the first layer plasticizer is greater than 55 parts by weight and less than 80 parts by weight per 100 parts by weight of first polyvinyl acetal, specifically greater than 55 parts by weight and less than 80 parts by weight, greater than 60 parts by weight and less than 80 parts by weight, greater than 65 parts by weight and less than 80 parts by weight, greater than 70 parts by weight and less than 80 parts by weight, greater than 75 parts by weight and less than 80 parts by weight, greater than 55 parts by weight and less than 75 parts by weight, greater than 60 parts by weight and less than 75 parts by weight, greater than 65 parts by weight and less than 75 parts by weight, greater than 55 parts by weight and less than 70 parts by weight, greater than 60 parts by weight and less than 70 parts by weight, greater than 55 parts by weight and less than 65 parts by weight, greater than 60 parts by weight and less than 65 parts by weight, or greater than 55 parts by weight and less than 60 parts by weight. Preferably, the amount is 60 to 75 parts by weight, for example, 60 parts by weight, 68 parts by weight, 72 parts by weight, or 75 parts by weight. According to another embodiment of the present invention, the plasticizer content of the second layer is 30 to 50 parts by weight relative to the second polyvinyl acetal, and the plasticizer content of the third layer is 30 to 50 parts by weight relative to the third polyvinyl acetal.

[0044] The antioxidant may be, for example, a phenolic antioxidant, a sulfuric antioxidant, and a phosphorus-based antioxidant. The phenolic antioxidant is an antioxidant having a phenol skeleton, and specific examples include 2,6-di-tert-butyl-p-cresol (BHT), butylhydroxyanisole (BHA), 2,6-di-tert-butyl-4-ethylphenol, β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid stearyl, 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), 4,4'-butylbis(3-methyl-6-tert-butylphenol), and 1,1,3-tris(2-methyl hydroxyphenyl) These include roxy-5-tert-butylphenyl)butane, tetra[methylene-3-(3',5'-butyl-4-hydroxyphenyl)propionate]methane, 1,3,3-tris(2-methyl-4-hydroxy-5-tert-butylphenol)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, bis(3,3'-tert-butylphenol) butyrate ethylene glycol ester, ditriethylene glycol bis(3-tert-butyl-4-hydroxy-5-methylphenylpropionate) ester, or combinations thereof. The aforementioned phosphorus-based antioxidants are antioxidants containing a phosphorus atom, and specific examples include tridecyl phosphite, tri(tridecyl) phosphite, triphenyl phosphite, tri(nonylphenyl) phosphite, diphosphite bis(tridecyl)pentaerythritol ester, diphosphite bis(decyl)pentaerythritol ester, tri(2,4-di-tert-butylphenyl) phosphite, bis(2,4-di-tert-butyl-6-methylphenyl) phosphite ethyl ester, 2,2'-methylenebis(4,6-di-tert-butyl-1-phenyloxy)(2-ethylhexyloxy)phosphorus, and 4,4'-butylidenebis(3-methyl-6-t-butylphenylditridecyl phosphite), etc.

[0045] [Method for producing polyvinyl acetal (1)]

[0046] In another aspect of the present invention, a method for producing the first polyvinyl acetal is provided, comprising: (A1) preparation of an aqueous polyvinyl alcohol solution: a step of preparing an aqueous polyvinyl alcohol solution by adding a nonionic surfactant and an acid catalyst to an aqueous polyvinyl alcohol solution and dissolving them in the aqueous polyvinyl alcohol solution at the dissolution temperature; (A2) an acetalization reaction by adding an aldehyde to the aqueous polyvinyl alcohol solution and carrying out an acetalization reaction at the reaction temperature, with or without the addition of a crosslinking agent as needed; (A3) a washing step of adding an aqueous sodium hydroxide solution (for example, at a concentration of 50 vol.%) to set the pH value to 10 and stop the reaction, performing one hot water wash, and then three cold water washes to remove impurities and residual acid; and (A4) a drying step of drying at a drying temperature to obtain the first polyvinyl acetal.

[0047] In step (A1), the polyvinyl alcohol is formed by saponifying a vinyl ester polymer obtained by polymerizing vinyl ester monomers. The definitions of the degree of saponification of the vinyl ester monomer, vinyl ester polymer, and polyvinyl alcohol are as described above. According to some embodiments of the present invention, the degree of polymerization of the polyvinyl alcohol is 2000 to 4500.

[0048] According to some embodiments of the present invention, in step (A1), the solid content of the polyvinyl alcohol aqueous solution is 12 to 16 wt.% relative to the total weight of the polyvinyl alcohol aqueous solution. Preferably, it is 14 wt.%. The acid catalyst may be, for example, an aqueous solution of sulfuric acid, hydrogen chloride, nitric acid, phosphoric acid, carboxylic acid, or sulfonic acid. Preferably, it is an aqueous solution of hydrogen chloride, nitric acid, or sulfuric acid, and more preferably an aqueous solution of hydrogen chloride (also called hydrochloric acid). Furthermore, the concentration and amount of the acid aqueous solution used as the acid catalyst can be adjusted according to actual needs and are not limited by the present invention.

[0049] According to several embodiments of the present invention, the amount of nonionic surfactant used relative to the total weight of the aqueous polyvinyl alcohol solution is greater than 0.010 wt.% and less than 0.050 wt.%, preferably 0.018 to 0.030 wt.%. Specific examples include 0.018 wt.%, 0.020 wt.%, 0.025 wt.%, or 0.030 wt.%. Without being limited to any particular theory, the nonionic surfactant affects the form of the acetal during the subsequent acetalization reaction, thereby affecting the compatibility of the formed polyvinyl acetal with the plasticizer. The form of the acetal is divided into two types: intramolecular acetal and intermolecular acetal. Generally, without being limited to any particular theory, polyvinyl acetal with a higher proportion of intramolecular acetals has better compatibility with plasticizers than polyvinyl acetal with a higher proportion of intermolecular acetals, and in addition, is considered to have a better sound insulation effect after being manufactured as an intermediate layer in a multilayer polymer film. Increasing the amount of nonionic surfactant facilitates the formation of intramolecular acetals during the acetalization reaction, improving the compatibility between the formed polyvinyl acetal and the plasticizer, thereby enhancing the sound insulation effect after it is manufactured as an intermediate layer in a multilayer polymer film. Decreasing the amount of nonionic surfactant facilitates the formation of intermolecular acetals during the acetalization reaction, reducing the compatibility between the formed polyvinyl acetal and the plasticizer, and decreasing the sound insulation effect of the final product. Furthermore, not limited to any specific theory, intermolecular acetals increase the degree of crosslinking of polyvinyl acetal, thereby increasing its molecular weight. Therefore, the molecular weight distribution of polyvinyl acetal within polyvinyl acetal can be controlled by adjusting the amount of nonionic surfactant used.

[0050] According to some embodiments of the present invention, the type of nonionic surfactant may be, for example, an alkyl ether type surfactant such as polyoxyethylene lauryl ether or polyoxyethylene oil ether, an alkylphenyl ether type surfactant such as polyoxyethylene octylphenyl ether, an alkyl ester type surfactant such as polyoxyethylene lauryl ester, an alkylamine type surfactant such as polyoxyethylene laurylamino ether, an alkylamide type surfactant such as polyoxyethylene laurylamide, a polypropylene glycol ether type surfactant such as polyoxyethylene polyoxypropylene ether, an alkanolamide type surfactant such as lauric acid diethanolamide or oleic acid diethanolamide, or an allylphenyl ether type surfactant such as polyoxyethylene allylphenyl ether. Polyoxyethylene lauryl ether is preferred.

[0051] In process (A1), the melting temperature is 85 to 95°C, specifically within the range of 85°C, 86°C, 87°C, 88°C, 89°C, 90°C, 91°C, 92°C, 93°C, 94°C, 95°C, or any two of these values.

[0052] The aldehyde in step (A2) is defined as described above. According to some embodiments of the present invention, the reaction temperature of the acetalization reaction is 55 to 65°C, specifically 55°C, 56°C, 57°C, 58°C, 59°C, 60°C, 61°C, 62°C, 63°C, 64°C, 65°C, or a range between any two of these values. Preferably, it is 60°C. Furthermore, the type and amount of the crosslinking agent can be adjusted according to actual needs and are not limited by the present invention. Without being limited by any particular logic, by adding a crosslinking agent in the acetalization reaction, more intermolecular acetals are generated, and the molecular weight distribution of the formed polyvinyl acetal and its compatibility with plasticizer can be controlled depending on the amount of crosslinking agent added.

[0053] The drying equipment used in process (A4) is not limited by the present invention. In some embodiments of the present invention, the drying temperature is 60-70°C, specifically, 60°C, 61°C, 62°C, 63°C, 64°C, 65°C, 66°C, 67°C, 68°C, 69°C, 70°C, or any two of these values.

[0054] [Method for producing the second and third polyvinyl acetals]

[0055] In another aspect of the present invention, a method for producing a second polyvinyl acetal and a third polyvinyl acetal is provided. Basically, this method is similar to the method for producing the first polyvinyl acetal, but the difference is that in step (A2), the reaction temperature of the acetalization reaction is 75 to 85°C. Specifically, this range is 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, or any two of these values. Preferably, it is 80°C.

[0056] [Method for manufacturing polymer films]

[0057] In another aspect of the present invention, the present invention provides a method for producing a polymer film comprising: (B1) a resin composition preparation step of dry mixing the aforementioned first polyvinyl acetal, second polyvinyl acetal, and third polyvinyl acetal together with a plasticizer and kneading them using a kneader to form a first polyvinyl acetal resin composition, a second polyvinyl acetal resin composition, and a third polyvinyl acetal resin composition; and (B2) a co-extrusion step of co-extruding the first polyvinyl acetal resin composition, the second polyvinyl acetal resin composition, and the third polyvinyl acetal resin composition into a polymer film having a three-layer structure, wherein the three-layer structure is a second layer (containing the second polyvinyl acetal resin composition) / a first layer (containing the first polyvinyl acetal resin composition) / a third layer (containing the third polyvinyl acetal resin composition).

[0058] According to some embodiments of the present invention, the thickness of the polymer film is 0.500 to 2.000 mm, specifically, 0.500 mm, 0.800 mm, 1.000 mm, 1.300 mm, 1.500 mm, 1.800 mm, 2.000 mm, or a range between any two of these values. Preferably, it is 0.800 mm. According to other embodiments of the present invention, the thickness of the first layer and / or the third layer is 0.110 to 0.150 mm, specifically, 0.110 mm, 0.130 mm, 0.150 mm, or a range between any two of these values. Preferably, it is 0.130 mm. According to other embodiments of the present invention, the thickness of the first layer is 0.320 to 0.350 mm, specifically, 0.320 mm, 0.330 mm, 0.340 mm, 0.335 mm, 0.350 mm, or a range between any two of these values. Preferably, it is 0.335 mm.

[0059] [Laminated glass and its manufacturing method]

[0060] In another aspect of the present invention, a laminated glass is provided comprising a first glass sheet, a second glass sheet, and the aforementioned polymer film placed between the first and second glass sheets. Generally, the first and second glass sheets are transparent plates, such as inorganic glass including float glass, polished glass, molded glass, wired glass, colored plate glass, heat-absorbing glass, or heat-reflective glass. Alternatively, they may be UV-shielding glass with an UV-blocking coating layer formed on the glass surface, or organic plastic sheets such as polyethylene terephthalate, polycarbonate, or polyacrylate. Furthermore, two or more types of transparent plates may be used; for example, the first glass sheet may be float glass and the second glass sheet may be colored plate glass. The shape, dimensions, and thickness of the first and second glass sheets are not limited by the present invention, and their thicknesses may be the same or different.

[0061] The laminated glass of the present invention can be manufactured by methods for manufacturing laminated glass that are conventionally known in the relevant art. For example, the laminated glass can be manufactured by the following method: (C1) A polymer film of the present invention is sandwiched between a first glass sheet and a second glass sheet to obtain a laminate. (C2) The laminate is passed through rollers and pressed using a hot press at a temperature of 140°C to 160°C and a pressure of 2 to 4 kg / cm². 2 Preliminary bonding is performed under the following conditions. Then, (C3) the laminated material after preliminary bonding is placed in an autoclave and thermal bonding, which is the final bonding, is performed for 100 to 150 minutes under high temperature and high pressure conditions to obtain laminated glass. Generally, the high pressure condition is 10 to 15 bar, and the high temperature condition is 100°C to 150°C.

[0062] Examples The present invention will be described in detail below, using specific examples. However, it should be understood that these specific examples are merely for the purpose of making the present invention easier to understand and do not limit its scope.

[0063] 1. Preparation of the first polyvinyl acetal, the second polyvinyl acetal, and the third polyvinyl acetal.

[0064] Herein, the present invention provides a non-limiting method for producing a first polyvinyl acetal, a second polyvinyl acetal, and a third polyvinyl acetal. Examples 1 to 5 and Comparative Examples 1 to 9 below illustrate the common main steps for producing the first polyvinyl acetal, the second polyvinyl acetal, and the third polyvinyl acetal, and Table 1 below details the differences in parameters in one or more production processes between the examples and comparative examples.

[0065] (1) Preparation of the solution: Polyoxyethylene lauryl ether is added as a nonionic surfactant to an aqueous solution of polyvinyl alcohol with a solid content of 14 wt.%, and a 0.2 wt.% aqueous hydrochloric acid solution (concentration 35 vol.%) is added as an acid catalyst. This solution is then dissolved in the aqueous polyvinyl alcohol solution at a dissolution temperature of 85°C to 95°C. Refer to Table 1 for the specific content of the nonionic surfactant.

[0066] (2) Acetalization reaction: n-butyraldehyde is added to the solution and the acetalization reaction is carried out at a temperature of 60°C. Refer to Table 1 for specific details regarding the addition of a crosslinking agent in this step (indicated by ○ if added, and × if not added).

[0067] (3) Washing: Add a 50 vol.% sodium hydroxide solution until the pH value reaches 10 to terminate the reaction, then wash with 60°C water for 1.5 hours, followed by washing each sample with 25°C water for 0.5 hours, repeating this process three times to remove impurities and residual acid.

[0068] (4) Drying: The first polyvinyl acetal is obtained by drying under conditions of a temperature of 65°C.

[0069] Basically, the methods for producing the second polyvinyl acetal and the third polyvinyl acetal are similar to those for producing the first polyvinyl acetal, but the differences are that the reaction temperature for the acetalization reaction is 80°C, the degree of polymerization is 2000, and the content of the nonionic surfactant (polyoxyethylene lauryl ether) is 0.010 wt.%.

[0070] 2. Preparation of polymer film

[0071] Herein, the present invention provides a non-limiting method for producing polymer films. The following shows the main steps common to the production of polymer films in Examples 1 to 5 and Comparative Examples 1 to 9, and Table 1 below shows in detail the differences in parameters in one or more production processes between these examples and comparative examples.

[0072] (1) Preparation of resin compositions: The first polyvinyl acetal, second polyvinyl acetal, and third polyvinyl acetal described above are dry-mixed with a plasticizer and kneaded using a kneader to form the first polyvinyl acetal resin composition, the second polyvinyl acetal resin composition, and the third polyvinyl acetal resin composition. The specific plasticizer content of each resin composition is shown in Table 1.

[0073] (2) Co-extrusion process: Using a T-die co-extruder, the first polyvinyl acetal resin composition, the second polyvinyl acetal resin composition, and the third polyvinyl acetal resin composition are formed into a polymer film having a three-layer structure. The thickness is 0.800 mm. The structure of the polymer film is second layer (containing the second polyvinyl acetal resin composition) / first layer (containing the first polyvinyl acetal resin composition) / third layer (containing the third polyvinyl acetal resin composition). The thickness is 0.335 mm / 0.130 mm / 0.335 mm.

[0074] 3. Manufacturing of laminated glass

[0075] Herein, the present invention provides a non-limiting method for manufacturing laminated glass. The following steps are common to the laminated glass manufactured in Examples 1 to 5 and Comparative Examples 1 to 9.

[0076] (1) A polymer film of the present invention is sandwiched between a first glass sheet and a second glass sheet to obtain a laminate. The first glass sheet and the second glass sheet are clear, transparent float glass with a length of 300 mm, a width of 25 mm, and a thickness of 2 mm.

[0077] (2) The laminate is passed through rollers and a hot press is used at a temperature of 150°C and a pressure of 3 kg / cm². 2 Apply temporary pressure for 3 minutes under these conditions.

[0078] (3) The laminated material after temporary bonding is placed in an autoclave and subjected to final heat bonding at a temperature of 135°C and a pressure of 13 bar for 120 minutes to obtain laminated glass.

[0079] 4.Analysis method

[0080] Herein, the present invention provides analytical and testing methods for polyvinyl acetal and polymer films of Examples 1 to 5 and Comparative Examples 1 to 9 described above.

[0081] [Hydroxyl group content, degree of acetylation, and degree of acetalization]

[0082] The method for measuring the hydroxyl group content, degree of acetylation, and degree of acetalization in this invention conforms to the method specified in the international standard JIS K6728:1977.

[0083] [Degree of polymerization]

[0084] The method for measuring the degree of polymerization of the present invention conforms to the method specified in JIS K6726:1994, an international standard.

[0085] [Molecular weight]

[0086] The molecular weight distribution of components in polyvinyl acetal (including polyvinyl acetal 1, polyvinyl acetal 2, and polyvinyl acetal 3) is measured using gel permeation chromatography (GPC). The polyvinyl acetal is dissolved in tetrahydrofuran (THF), and GPC analysis is performed under the following conditions. The molecular weight is calculated based on the ratio corresponding to the area of ​​the polystyrene standard (Waters PS STD).

[0087] Equipment: Waters 1515 PUMP system

[0088] Detection device: Waters 2414 RI

[0089] Elumination conditions: 1.0 ml / min (mL / min), THF

[0090] The columns are Waters Styragel HR5 THF, Waters Styragel HR4 THF, Waters Styragel HR3 THF, and Waters Styragel HR1 THF.

[0091] Then, the approximate value is rounded to the nearest ten thousand, and the software is used to calculate the weight-average molecular weight (Mw) of polyvinyl acetal, the content of polyvinyl acetal with a molecular weight in the range of 100,000 Da to 1,200,000 Da, and the content of polyvinyl acetal with a molecular weight greater than 1,000,000 Da.

[0092] [Glass transition temperature (Tg)]

[0093] Sample preparation: A polymer film is cut into 8 mm diameter circles and placed in a constant temperature and humidity chamber at 23°C and 55% relative humidity for 24 hours to obtain the sample.

[0094] Measurement method: The sample is analyzed using a rheometer (Discovery Hybrid Rheometer II, DHR) purchased from TA Instruments. The sample is placed on the DHR test bench, the analysis temperature is set to 100 to -10°C, and the viscoelasticity is analyzed by vibration method under the conditions of vibration frequency 1 Hz, strain 1%, clamp pressure 1 N, and cooling rate 3°C / min. The glass transition temperature of the polymer film can be obtained from the analysis results.

[0095] 5. Evaluation Methods and Results

[0096] Herein, the present invention provides the evaluation methods for laminated glass in Examples 1 to 5 and Comparative Examples 1 to 9, and the results of the correspondence between these methods and the analysis content (as shown in Table 1).

[0097] [Loss factor at 10°C]

[0098] The method for measuring the loss coefficient in this application is based on the Mechanical Impedance Measurement (MIM) method described in ISO 16940:2008.

[0099] Sample preparation: The laminated glass described above is placed in a constant temperature and humidity chamber at 10°C and 55% relative humidity for 2 hours to obtain a sample.

[0100] Measurement method: The center of the sample is fixed to a vibration shaker, and vibration is performed under conditions of 10°C. Next, the force and frequency of the vibration are measured using an impedance head, and the experimental data is converted into a loss factor (also called a damping loss factor) at 10°C using an analysis system. Here, the loss factor is the first vibration mode calculated using the half-power method. Generally, the higher the value of the loss factor, the better the sound insulation effect.

[0101] Evaluation Method: A loss coefficient value greater than 0.25 at 10°C indicates excellent sound insulation. A loss coefficient value of 0.25 or less at 10°C indicates poor sound insulation.

[0102] [Loss factor at 20°C]

[0103] The method for measuring the loss factor in this text is based on the MIM mechanical impedance method described in ISO 16940:2008.

[0104] Sample preparation: The laminated glass described above is placed in a constant temperature and humidity chamber at 20°C and 55% relative humidity for 2 hours to obtain a sample.

[0105] Measurement method: The center of the sample is fixed to a vibrating shaker and vibrated under conditions of 20°C. Next, the force and frequency of the vibration are measured using an impedance head, and the experimental data is converted into a loss coefficient at 20°C using an analysis system. Here, the loss coefficient is the first vibration mode calculated based on the half-power method. Generally, the higher the value of the loss coefficient, the greater the sound insulation effect.

[0106] Evaluation Method: If the loss coefficient value at 20°C is greater than 0.25, it is judged as passing, indicating excellent sound insulation. If the loss coefficient value at 20°C is 0.25 or less, it is judged as failing, indicating lower sound insulation.

[0107] [Evaluation of snowflake-shaped bubbles]

[0108] Sample preparation: Using the method for manufacturing laminated glass described above, prepare a laminated glass (i.e., sample) with a length of 150 mm, a width of 150 mm, and a thickness of 2 mm.

[0109] Measurement method: Place the sample in an oven and dry it at a temperature of 120°C for 2 hours. Then, remove it from the oven and observe its appearance with the naked eye.

[0110] Evaluation method: If no "snowflake-like bubbles" appear on the surface of the dried sample, it is judged as passing and marked with a "○". If "snowflake-like bubbles" appear on the appearance of the dried sample, it will be judged as unacceptable and marked with an "X".

[0111] [Table 1]

[0112] [Table 2]

[0113] Based on Table 1, Examples 1 to 5, in which the content of components with a weight-average molecular weight in the first polyvinyl acetal ranging from 100,000 Da to 1,200,000 Da was controlled to 70 to 80 wt.%, and the glass transition temperature of the first layer was controlled to -16.00°C to 5.00°C, showed that the loss coefficients of these polymer films at 10°C and 20°C were both greater than 0.25, exhibiting excellent sound insulation effects. Furthermore, laminated glass containing these films did not exhibit snowflake-like bubbles, resulting in excellent aesthetics and practicality. In contrast, Comparative Examples 1 to 9, in which the content of components with a weight-average molecular weight in the first polyvinyl acetal ranging from 100,000 Da to 1,200,000 Da and the glass transition temperature of the first layer were not controlled within the above range, did not achieve the above technical effects.

[0114] All scopes disclosed herein are intended to include combinations of each specified scope within a given scope and sub-scopes between those defined scopes. Furthermore, unless otherwise specified, all scopes disclosed herein include the endpoints of the described scope. Thus, scopes 1-5 specifically include 1, 2, 3, 4, and 5, and also include sub-scopes such as 2-5, 3-5, 2-3, 2-4, 1-4, etc.

[0115] All publications and patent applications cited herein are incorporated herein by reference, and for all purposes, each publication or patent application is explicitly and individually incorporated herein by reference. In the event of any inconsistency between this specification and any publication or patent application incorporated herein by reference, the content of this specification shall prevail.

Claims

1. It includes a first layer, a second layer and a third layer, the first layer being installed between the second layer and the third layer, The first layer comprises a first polyvinyl acetal. The content of the component in the first polyvinyl acetal having a molecular weight in the range of 100,000 to 1,200,000 Da is 70 to 80 wt.%, and A polymer film wherein the glass transition temperature of the first layer is -16.00°C to 5.00°C.

2. The polymer film according to claim 1, wherein the content of a component having a molecular weight in the range of 100,000 to 1,200,000 Da in the first polyvinyl acetal is 70 to 72 wt.%.

3. The polymer film according to claim 1, wherein the glass transition temperature of the first layer is -16.00°C to -10.00°C.

4. The polymer film according to claim 1, wherein the content of the component with a molecular weight greater than 1,000,000 Da in the first polyvinyl acetal is 2.0 to 9.0 wt.%.

5. The polymer film according to claim 1, wherein the weight-average molecular weight of the first polyvinyl acetal is 230,000 to 520,000 Da.

6. The polymer film according to claim 5, wherein the weight-average molecular weight of the first polyvinyl acetal is 250,000 to 480,000 Da.

7. The polymer film according to claim 1, wherein the degree of polymerization of the first polyvinyl acetal is 2000 to 4500.

8. The polymer film according to claim 7, wherein the degree of polymerization of the first polyvinyl acetal is 2200 to 4200.

9. The polymer film according to claim 1, wherein the hydroxyl group content of the first polyvinyl acetal is 23.0 to 28.0 mol%.

10. The polymer film according to claim 1, wherein the degree of acetylation of the first polyvinyl acetal is 7.0 to 12.0 mol%.

11. The polymer film according to claim 1, wherein the degree of acetalization of the first polyvinyl acetal is 60.0 to 68.0 mol%.

12. The polymer film according to claim 1, wherein the second layer comprises a second polyvinyl acetal, and the weight-average molecular weight of the second polyvinyl acetal is 200,000 to 280,000 Da.

13. The polymer film according to claim 1, wherein the third layer comprises a third polyvinyl acetal, and the weight-average molecular weight of the third polyvinyl acetal is 200,000 to 280,000 Da.

14. The polymer film according to any one of claims 1 to 13, wherein the first layer further comprises a plasticizer.

15. The polymer film according to claim 14, wherein the amount of the plasticizer is greater than 55 parts by weight and less than 80 parts by weight per 100 parts by weight of the first polyvinyl acetal.

16. The first glass sheet and, The second glass sheet and Laminated glass comprising a polymer film according to any one of claims 1 to 13, which is installed between the first glass sheet and the second glass sheet.

Citation Information

Patent Citations

  • Defect-resistant acoustic polymer interlayer

    JP2015515396A

  • Interlayer for glass laminate and glass laminate

    JP2017171574A

  • Interlayer for laminated glass, and laminated glass

    WO2011081191A1

  • Interlayer for laminated glass and laminated glass

    WO2012043818A1

  • Interlayer for laminated glass and laminated glass

    WO2012091116A1