Surface printing varnish composition, laminate, and packaging material

The varnish composition with polyurethane and nitrocellulose resin, along with additives, addresses stretch and blocking resistance issues in surface printing, providing durable printed layers for packaging materials.

JP7955544B1Active Publication Date: 2026-11-24DAINICHISEIKA COLOR & CHEMICALS MFG CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2026057918
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2026-03-31
Publication Date
2026-11-24
Estimated Expiration
2046-03-31

AI Technical Summary

Technical Problem

Existing surface printing varnishes for packaging materials lack sufficient stretch resistance and blocking resistance, particularly when in contact with plastic sheets containing plasticizers, leading to peeling and detachment issues.

Method used

A varnish composition comprising a specific ratio of polyurethane resin and nitrocellulose resin, along with optional additives like hydrocarbon wax dispersion, resin beads, plasticizer, and styrene-maleic acid copolymer, to enhance stretch resistance and blocking resistance.

Benefits of technology

The composition forms a printed layer with improved adhesion to substrates, resistance to stretching, and resistance to blocking, even with plasticizers, ensuring durability and integrity of the printed layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955544000001
    Figure 0007955544000001
  • Figure 0007955544000002
    Figure 0007955544000002
  • Figure 0007955544000003
    Figure 0007955544000003
Patent Text Reader

Abstract

To provide a surface printing varnish composition capable of forming a printed layer with excellent stretch resistance and blocking resistance, a laminate comprising a printed layer formed using the surface printing varnish composition, and a packaging material comprising the laminate. [Solution] A printing varnish composition for surface printing comprising a polyurethane resin (A), a nitrocellulose resin (B), and an organic solvent, wherein the total solid content of the polyurethane resin (A) and the nitrocellulose resin (B) is 48 to 75% by mass of the total mass of solids of the printing varnish composition for surface printing, the mass ratio of solids represented by the polyurethane resin (A) / nitrocellulose resin (B) is 0.95 to 2.5, and the 10% modulus of the mixture of the polyurethane resin (A) and the nitrocellulose resin (B) is 3.0 to 50.0 MPa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a surface printing varnish composition, a laminate, and a packaging material.

Background Art

[0002] For packaging products such as food and daily necessities, packaging materials using a plastic film as a base material are used. For the purpose of decoration, ensuring necessary physical properties, etc., the packaging material is printed on the base material with a printing ink such as a gravure printing ink or a printing varnish such as a gravure printing varnish.

[0003] As a packaging material, a printed matter with a simple configuration called a surface printing method may be used, in which printing is performed on the front side of the base material and no printing is performed on the back side of the base material that comes into contact with the contents. In the back printing method in which printing is performed on the back side of the base material, the printed layer is protected from external contact by the base material, whereas in the surface printing method, the printed layer is exposed to the outside. Therefore, inks and varnishes used in the surface printing method are required to have more excellent coating film physical properties.

[0004] Binder resins have been studied to satisfy various required coating film physical properties. For example, Patent Document 1 discloses a surface printing gravure printing ink composition containing a polyurethane resin and a nitrocellulose resin as binder resins.

Prior Art Documents

Patent Documents

[0005]

Patent Document 1

Summary of the Invention

Problem to be Solved by the Invention

[0006] One of the required coating properties for printing varnishes used for surface printing is the adhesion of the printed layer to the substrate. Conventionally, this adhesion was evaluated by assessing the printed layer immediately after printing. However, when printed materials are processed into bags, or when the resulting packaging material is heated and cooled before use, the substrate may expand or contract. The inventors focused on the deformation of the substrate in these actual usage processes. In particular, if the printed layer does not follow the substrate when the substrate is stretched, the printed layer may peel off. Hereinafter, the property that the printed layer does not easily peel off the substrate when the substrate is stretched will also be called "stretch-resistant adhesion."

[0007] Furthermore, one of the required coating properties for printing varnishes used for surface printing is the blocking resistance of the printed layer. According to the inventors' research, when the printed layer in a printed material comes into contact with a plastic sheet such as a PVC sheet, the printed layer may detach. This is thought to be because hard plastics such as PVC sheets contain plasticizers, and these plasticizers bleed out, causing the printed layer to block against the PVC sheet due to the plasticizers. In other words, in order to prevent blocking even with plastic sheets containing plasticizers, the printed layer needs to have extremely high blocking resistance. Hereafter, blocking resistance to plastic sheets containing plasticizers will also be simply referred to as "blocking resistance."

[0008] The stretch resistance and blocking resistance of the printed layer formed from the gravure printing ink composition for surface printing described in Patent Document 1 are insufficient, and further improvements are needed.

[0009] The present invention aims to provide a surface printing varnish composition capable of forming a printed layer with excellent stretch resistance and blocking resistance, a laminate comprising a printed layer formed using the surface printing varnish composition, and a packaging material comprising the laminate. [Means for solving the problem]

[0010] The present invention has the following aspects. [1] A printing varnish composition for surface printing comprising a polyurethane resin (A), a nitrocellulose resin (B), and an organic solvent, The total solid content of the polyurethane resin (A) and the nitrocellulose resin (B) is 48 to 75% by mass of the total solid content of the surface printing varnish composition. The mass ratio of the solid content represented by the polyurethane resin (A) and the nitrocellulose resin (B) is 0.95 to 2.5. A printing varnish composition for surface printing, wherein the 10% modulus of a mixture of the polyurethane resin (A) and the nitrocellulose resin (B), as measured by the following method, is 3.0 to 50.0 MPa. [Method for measuring 10% modulus] A varnish containing the polyurethane resin (A) and the nitrocellulose resin (B) is applied to release paper using an applicator to form a dry film with a thickness of 30 μm, and then heat-dried. However, the mass ratio of the solid content of the polyurethane resin (A) and the nitrocellulose resin (B) in the varnish is the same as the mass ratio in the printing varnish composition for surface printing. The obtained film is aged for 24 hours under conditions of 25°C to prepare a film for test specimens. After aging, the film is peeled off the release paper and cut into strips measuring 6 cm in length and 1.5 cm in width to prepare test specimens. Under conditions of 25°C, the prepared test specimens are stretched in the longitudinal direction of the test specimen at a tensile speed of 20 cm / min using an autograph. From the obtained stress-strain curve, the stress at the point when the elongation of the test specimen reaches 10% (1.1 times the original length) is read. The measurement was performed three times, and the average value was taken as the 10% modulus of the mixture of the polyurethane resin (A) and the nitrocellulose resin (B). [2] The printing varnish composition for surface printing according to [1], further comprising a hydrocarbon wax dispersion and resin beads, wherein the median diameter of the hydrocarbon wax dispersion is 4.0 to 10.0 μm and the average particle diameter of the resin beads is 0.5 to 2.5 μm. [3] The printing varnish composition for surface printing according to [1] or [2], further comprising a plasticizer, wherein the plasticizer has a freezing point of 3°C or less. [4] The printing varnish composition for surface printing according to any one of [1] to [3], wherein the number average molecular weight of the polyurethane resin (A) is 20,000 or less. [5] A printing varnish composition for surface printing according to any one of [1] to [4], further comprising a styrene-maleic acid copolymer. [6] A surface printing varnish composition for gravure printing, as described in any of [1] to [5]. [7] A laminate comprising a plastic film and a printed layer formed on one surface of the plastic film using a surface printing varnish composition according to any one of [1] to [5]. [8] A laminate comprising a plastic film and a printed layer formed on one surface of the plastic film using the surface printing varnish composition described in [6]. [9] [7] Packaging material comprising the laminate described above.

[10] [8] A packaging material comprising the laminate described above. [Effects of the Invention]

[0011] According to the present invention, it is possible to provide a surface printing varnish composition capable of forming a printed layer with excellent stretch resistance and blocking resistance, a laminate comprising a printed layer formed using the surface printing varnish composition, and a packaging material comprising the laminate. [Modes for carrying out the invention]

[0012] The present invention will now be described in detail. The following embodiments are merely illustrative for illustrating the present invention and are not intended to limit the present invention to these embodiments. The present invention can be implemented in various forms without departing from its spirit. In this specification, the "~" symbol indicating a numerical range means that the numbers before and after it are included as the lower and upper limits, respectively. "Liquid medium" refers to volatile liquids such as organic solvents. The “solid content” of the overprint printing varnish composition refers to the components of the overprint printing varnish composition excluding the liquid medium, which are the components that ultimately form the varnish layer, and can be specifically measured in accordance with JIS K 5601-1-2:2008. The same applies to the solid content of the polyurethane resin and the nitrocellulose resin. The “coating film” is a coating film formed by the overprint printing varnish composition of the present invention. That is, in this specification, “varnish layer,” “print layer,” and “coating film” are synonymous.

[0013] ≪Overprint printing varnish composition≫ The overprint printing varnish composition of the present embodiment (hereinafter also simply referred to as “varnish composition”) contains a polyurethane resin (A), a nitrocellulose resin (B), and an organic solvent. The varnish composition contains no color pigments. The varnish composition can be used as a medium mainly used for adjusting the concentration of ink. The varnish composition may further include a hydrocarbon wax dispersion. The varnish composition may further include resin beads. The varnish composition may further include a plasticizer. The varnish composition may further include a styrene-maleic acid copolymer. The varnish composition may further include components other than the polyurethane resin (A), the nitrocellulose resin (B), the organic solvent, the hydrocarbon wax dispersion, the resin beads, the plasticizer, and the styrene-maleic acid copolymer.

[0014] <Polyurethane resin (A)> Examples of the polyurethane resin (A) include a thermoplastic polyurethane resin that is a reaction product of a polyisocyanate compound and a polyol compound and is soluble in an organic solvent. The polyurethane resin (A) can be produced by a conventionally known method. For example, it is obtained by allowing a urethane prepolymer, which is a reaction product of a polyisocyanate compound and a polyol compound, to react with a chain extender and a reaction terminator as necessary.

[0015] Examples of the polyisocyanate compound include aromatic diisocyanates such as 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, m-xylylene diisocyanate, 4,4′-diphenylmethane diisocyanate, 2,2′-diphenylmethane diisocyanate, 2,4′-diphenylmethane diisocyanate, 4,4-diphenyl ether diisocyanate, 2-nitrodiphenyl-4,4-diisocyanate, 2,2-diphenylpropane-4,4-diisocyanate, 3,3-dimethyldiphenylmethane-4,4-diisocyanate, 4,4-diphenylpropane diisocyanate, m-phenylene diisocyanate, p-phenylene diisocyanate, naphthylene-1,4-diisocyanate, naphthylene-1,5-diisocyanate, and 3,3-dimethoxydiphenyl-4,4-diisocyanate; aliphatic diisocyanates such as tetramethylene diisocyanate, hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, and lysine diisocyanate; and alicyclic diisocyanates such as isophorone diisocyanate, norbornane diisocyanate, hydrogenated tolylene diisocyanate, hydrogenated xylylene diisocyanate, and hydrogenated diphenylmethane diisocyanate, and the like. The polyisocyanate compounds may be used singly or in combination of two or more.

[0016] Examples of the polyol compound include polyester polyols, polycarbonate polyols, and polyether polyols. The polyol compounds may be used singly or in combination of two or more.

[0017] Examples of the polyester polyol include polyester polyols or polyester amide polyols obtained by a dehydration polycondensation reaction between polycarboxylic acids and polyhydric alcohols or secondary or tertiary amines. Examples of polycarboxylic acids include succinic acid, adipic acid, sebacic acid, azelaic acid, terephthalic acid, isophthalic acid, orthophthalic acid, hexahydroterephthalic acid, hexahydroisophthalic acid, hexahydroorthophthalic acid, and polycarboxylic acids such as naphthalenedicarboxylic acid and trimellitic acid, as well as their acid esters and acid anhydrides. Polycarboxylic acids may be used individually or in combination of two or more. Examples of polyhydric alcohols include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, neopentyl glycol, 1,8-octanediol, 1,9-nonanediol, diethylene glycol, dipropylene glycol, 1,4-cyclohexanedimethanol, ethylene oxide or propylene oxide adducts of bisphenol A, trimethylolpropane, glycerin, and low molecular weight alcohol compounds such as pentaerythritol, as well as low molecular weight amino alcohol compounds such as monoethanolamine and diethanolamine. Polyhydric alcohols may be used individually or in combination of two or more. Examples of secondary and tertiary amines include low-molecular-weight amine compounds such as hexamethylenediamine, xylylenediamine, and isophoronediamine. These secondary and tertiary amines may be used individually or in combination of two or more. As polyester polyols, for example, lactone-based polyester polyols obtained by ring-opening polymerization of cyclic ester (lactone) monomers such as ε-caprolactone and γ-valerolactone using low molecular weight alcohol compounds and low molecular weight amino alcohol compounds as initiators can also be used.

[0018] Examples of polycarbonate polyols include those obtained by the dehydrochlorination reaction of a low molecular weight alcohol compound with phosgene, and those obtained by the transesterification reaction of a low molecular weight alcohol compound with a carbonate compound. Examples of low molecular weight alcohol compounds include those similar to those used in the synthesis of polyester polyols. Examples of carbonate compounds include diethylene carbonate, dimethyl carbonate, diethyl carbonate, and diphenyl carbonate.

[0019] Examples of polyether polyols include those obtained by ring-opening polymerization of cyclic ethers using hydroxyl group-containing compounds such as low molecular weight alcohol compounds, low molecular weight amine compounds, low molecular weight amino alcohol compounds, and phenols as initiators. Examples of low molecular weight alcohol compounds, low molecular weight amine compounds, and low molecular weight amino alcohol compounds are the same as those used in the synthesis of polyester polyols. Examples of cyclic ethers include alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide, as well as tetrahydrofuran. Specific examples of polyether polyols include polyoxyethylene polyol, polyoxypropylene polyol, polytetramethylene ether polyol, and polyoxyethylene polyoxypropylene polyol. As the polyether polyol, polyester ether polyols initiated from the aforementioned polyester polyols or polycarbonate polyols can also be used.

[0020] As a chain elongator, a compound having two or more functional groups (such as amino groups and hydroxyl groups) that can react with an isocyanate group in the molecule can be used. Examples of chain elongators include diamine compounds such as ethylenediamine, 1,3-propylenediamine, 1,4-butylenediamine, hexamethylenediamine, isophoronediamine, and 2-ethylaminoethylamine; polyamine compounds such as diethylenetriamine and triethylenetetramine; low molecular weight diol compounds such as ethylene glycol, propylene glycol, butylene glycol, diethylene glycol, and triethylene glycol; aminoethylethanolamine, and aminopropylethanolamine. A single chain elongator may be used alone, or two or more may be used in combination.

[0021] Examples of reaction stoppers include monoalkylamines such as n-propylamine and n-butylamine; dialkylamines such as di-n-butylamine; alkanolamines such as monoethanolamine and diethanolamine; and monoalcohols such as methanol and ethanol. Reaction stoppers may be used individually or in combination of two or more.

[0022] The glass transition temperature of polyurethane resin (A) is preferably -65 to 0°C, more preferably -60 to 5°C, and even more preferably -55 to 10°C. If the glass transition temperature is below the lower limit, the blocking resistance, heat resistance, and abrasion resistance of the resulting printed layer will be slightly reduced. If the glass transition temperature is above the upper limit, the adhesion, crumpling resistance, and cold crumpling resistance of the resulting printed layer to the substrate will be slightly reduced. In low-temperature environments, the printed layer hardens and loses its flexibility, which can frequently cause the printed layer to detach due to cracking when crumpled. Cold crumpling resistance refers to the characteristic of being less prone to the above-mentioned detachment of the printed layer. In this specification, the glass transition temperature is determined in accordance with JIS K 7121:2012, using a differential scanning calorimeter, by heating 10 mg of the sample from -100°C to 160°C at a rate of 20°C / min. The value is obtained from the intersection of the baseline and the tangent to the endothermic curve in the resulting curve (DSC curve).

[0023] The number-average molecular weight of the polyurethane resin (A) is preferably 20,000 or less, more preferably 4,000 to 18,000, more preferably 5,000 to 16,000, and even more preferably 6,000 to 14,000. If the number-average molecular weight is below the lower limit, the blocking resistance, heat resistance, and abrasion resistance of the resulting printed layer will be slightly reduced. If the number-average molecular weight is above the upper limit, the 10% modulus of the mixture of polyurethane resin (A) and nitrocellulose resin (B) tends to be large, resulting in a slight decrease in stretch adhesion resistance. Cold tangling resistance will also be slightly reduced. In this specification, the number-average molecular weight is the value obtained on a standard polystyrene basis by gel permeation chromatography (GPC).

[0024] The hydroxyl value of the polyurethane resin (A) is preferably 50 mgKOH / g or less, more preferably 40 mgKOH / g or less, and even more preferably 30 mgKOH / g or less. If the hydroxyl value exceeds the above upper limit, the blocking resistance of the resulting printed layer will be slightly reduced. In addition, the varnish stability of the varnish composition will be slightly reduced. In this specification, the hydroxyl value is the value measured in accordance with JIS K 1557-1:2007.

[0025] The amine value of the polyurethane resin (A) is preferably 10 mg KOH / g or less, more preferably 5 mg KOH / g or less, and even more preferably 3 mg KOH / g or less. If the amine value exceeds the above upper limit, the printability will be slightly reduced. In this specification, the amine value is a value measured by neutralization titration using hydrochloric acid in accordance with JIS K 7237:1995.

[0026] The acid value of the polyurethane resin (A) is preferably 20 mg KOH / g or less, more preferably 10 mg KOH / g or less, and even more preferably 8 mg KOH / g or less. If the acid value exceeds the above upper limit, the storage stability of the varnish composition will be slightly reduced. In this specification, the acid value is expressed in milligrams as the amount of potassium hydroxide required to neutralize acidic groups such as carboxyl groups per gram of sample solid content, and is a value measured in accordance with JIS K 5601-2-1:1999.

[0027] The storage modulus (E'; dynamic storage modulus) of polyurethane resin (A) at a temperature of 100°C and a frequency of 11Hz is preferably 20 or less, more preferably 10 or less, and even more preferably 5 or less. If the storage modulus exceeds the above upper limit, the adhesion of the resulting printed layer to the substrate will be slightly reduced. In this specification, the storage modulus is a value obtained by measuring the dynamic viscoelasticity of a dried sample (film-like sample) using a dynamic viscoelasticity measuring device under conditions of a temperature of 100°C and a frequency of 11 Hz.

[0028] <Nitrocellulose resin (B)> As for the nitrocellulose resin (B), from the viewpoint of compatibility of the nitrocellulose resin with the varnish, stability of the varnish composition (varnish stability), resistance to stretch adhesion, abrasion resistance, heat resistance, blocking resistance, kneading resistance, and cold kneading resistance, it is preferable that the type and viscosity symbol, as defined by viscosity measurement in accordance with JIS K 6703:1995, be H1 / 16, H1 / 8, H1 / 4, H1 / 2, H1, or H2, more preferably H1 / 2, and even more preferably H1 / 2. If the viscosity symbol of the nitrocellulose resin (B) is H1 / 2, H1, or H2, it is easier to adjust the 10% modulus of the mixture described later to a predetermined range. In order to satisfy the necessary physical properties such as blocking resistance, abrasion resistance, and heat resistance of the resulting printed layer, a certain amount or more of nitrocellulose resin (B) must be included in the varnish composition, but as the content of nitrocellulose resin (B) increases, the 10% modulus of the mixture tends to increase. In adjusting the above necessary physical properties and the 10% modulus of the mixture to a predetermined range, nitrocellulose resin (B) with a viscosity symbol of H1 / 2, H1, or H2 is preferred. In particular, it is preferable to use two or more types of nitrocellulose resin (B) with viscosity symbols of H1 / 2, H1, and H2 in combination, and it is more preferable to use nitrocellulose resin (B) with viscosity symbols of H1 / 2 and H2 in combination.

[0029] The aforementioned types are defined according to the nitrogen content in the nitrocellulose resin. For nitrocellulose resins with a nitrogen content of 10.7% or more and less than 11.5%, the type is L. For nitrocellulose resins with a nitrogen content of 11.5% or more and 12.2% or less, the type is H. The viscosity symbol is defined according to the time it takes for a given steel ball to fall between the markings in a nitrocellulose resin solution at a predetermined solid content concentration (fall time). In the case of a nitrocellulose resin of the aforementioned type and viscosity symbol H1 / 16, the time it takes for a steel ball to fall into a nitrocellulose resin solution with a solid content concentration of 25% by mass is 1.0 to 1.5 seconds. In the case of a nitrocellulose resin of the aforementioned type and viscosity symbol H1 / 8, the time it takes for a steel ball to fall into a nitrocellulose resin solution with a solid content concentration of 25% by mass is 1.6 to 2.9 seconds. In the case of a nitrocellulose resin of the aforementioned type and viscosity symbol H1 / 4, the time it takes for a steel ball to fall into a nitrocellulose resin solution with a solid content concentration of 25% by mass is 3.0 to 8.9 seconds. In the case of a nitrocellulose resin of the aforementioned type and viscosity symbol H1 / 2, the time it takes for a steel ball to fall in a nitrocellulose resin solution with a solid content concentration of 20% by mass is 3.0 to 4.9 seconds. Alternatively, the time it takes for a steel ball to fall in a nitrocellulose resin solution with a solid content concentration of 25% by mass is 9.0 to 22.0 seconds. In the case of a nitrocellulose resin of the aforementioned type and viscosity symbol H1, the time it takes for a steel ball to fall into a nitrocellulose resin solution with a solid content concentration of 20% by mass is 5.1 to 9.0 seconds. In the case of a nitrocellulose resin of the aforementioned type and viscosity symbol H2, the time it takes for a steel ball to fall in a nitrocellulose resin solution with a solid content concentration of 12.2% by mass is 1.5 to 2.5 seconds. Alternatively, the time it takes for a steel ball to fall in a nitrocellulose resin solution with a solid content concentration of 20% by mass is 15.0 to 40.0 seconds. Nitrocellulose resin (B) may be used alone or in combination of two or more types.

[0030] [10% modulus of the mixture] The 10% modulus of the mixture of polyurethane resin (A) and nitrocellulose resin (B) is 3.0 to 50.0 MPa, preferably 5.0 to 40.0 MPa, more preferably 6.0 to 35.0 MPa, and even more preferably 8.0 to 30.0 MPa. If the 10% modulus is below the lower limit, the blocking resistance of the resulting printed layer decreases. If the modulus exceeds the upper limit, the stretch adhesion resistance of the resulting printed layer decreases. Cold tarnish resistance also decreases.

[0031] The 10% modulus of a mixture of polyurethane resin (A) and nitrocellulose resin (B) is measured as follows: A varnish containing polyurethane resin (A) and nitrocellulose resin (B) is applied to release paper using an applicator to create a dry film with a thickness of 30 μm, and then heat-dried. However, the mass ratio of the solid content of polyurethane resin (A) and nitrocellulose resin (B) in the varnish is the same as the mass ratio in the varnish composition. The resulting film is aged for 24 hours under 25°C conditions to prepare a test specimen. After aging, the film is peeled from the release paper and cut into strips measuring 6 cm x 1.5 cm to prepare a test specimen. Under 25°C conditions, the prepared test specimen is stretched in the longitudinal direction of the specimen at a tensile speed of 20 cm / min using an autograph. From the obtained stress-strain curve, the stress at the point when the elongation of the test specimen reaches 10% (1.1 times the original length) is read. Measurements were taken three times, and the average value was taken as the 10% modulus of the mixture of polyurethane resin (A) and nitrocellulose resin (B).

[0032] The 10% modulus of a mixture is an indicator of its hardness (i.e., the binder resin), with a higher value indicating harder material and a lower value indicating softer material. The 10% modulus of a mixture can be controlled by adjusting the type (hardness) of the polyurethane resin (A) and the nitrocellulose resin (B), as well as the mass ratio of the solids.

[0033] The hardness of polyurethane resin (A) can be controlled, for example, by the type, properties, and composition of the polyisocyanate compound and polyol compound. Alternatively, polyurethane resin (A) can be composed of a hard segment and a soft segment, and its hardness can be controlled by adjusting the composition and properties of at least one of the hard or soft segments. An example of controlling the hardness of polyurethane resin (A) is shown below. Long-chain polyol compounds are used as the polyol compounds, and the molecular weight of the long-chain polyol compounds is adjusted. Long-chain polyol compounds are polyol compounds with a number-average molecular weight of 400 or more. When the number-average molecular weight of the long-chain polyol compound is reduced, the polyurethane resin (A) tends to become harder. The ratio of hard segments to soft segments in the polyurethane resin (A) is adjusted. Increasing the proportion of hard segments tends to make the polyurethane resin (A) harder. The proportion of hard segments can be controlled, for example, by adjusting the proportion of at least one of urethane bonds and urea bonds in the polyurethane resin (A). As the proportion of urethane bonds and urea bonds increases, the proportion of hard segments in the polyurethane resin (A) tends to increase. The proportion of urethane bonds and urea bonds can be quantified using the amine value.

[0034] The hardness of nitrocellulose resin (B) can be controlled, for example, by its viscosity. For instance, when the viscosity symbol of nitrocellulose resin (B) is high, the nitrocellulose resin (B) tends to become harder.

[0035] As the mass ratio of the solids represented by polyurethane resin (A) / nitrocellulose resin (B) increases, the 10% modulus of the mixture tends to decrease. In other words, increasing the amount of solids of polyurethane resin (A) relative to nitrocellulose resin (B) tends to make the mixture softer. Thus, the 10% modulus of the mixture is controllable for those skilled in the art.

[0036] <Organic solvents> Examples of organic solvents include aromatic organic solvents such as toluene and xylene; aliphatic hydrocarbon organic solvents such as cyclohexane and methylcyclohexane; ketone organic solvents such as methyl ethyl ketone and methyl isobutyl ketone; ester organic solvents such as ethyl acetate, n-propyl acetate, isopropyl acetate, and isobutyl acetate; alcohol organic solvents such as methanol, ethanol, n-propanol, isopropanol, and n-butanol; and glycol ether organic solvents such as ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, and propylene glycol monomethyl ether.

[0037] From an environmental perspective, the organic solvent is preferably an organic solvent that is substantially free of toluene (a toluene-free organic solvent). In other words, the varnish composition is preferably a toluene-free varnish composition that is substantially free of toluene. More preferably, the organic solvent is an organic solvent that is substantially free of aromatic organic solvents such as toluene and xylene. "Essentially not included" means that it is intentionally not included in the formula.

[0038] From the viewpoint of stably dissolving polyurethane resin (A) and nitrocellulose resin (B), the organic solvent preferably includes ester-based organic solvents and alcohol-based organic solvents. The content of ester-based organic solvents in the organic solvent is preferably 50 to 95% by mass relative to the total mass of the organic solvent. The content of alcohol-based organic solvents in the organic solvent is preferably 5 to 50% by mass relative to the total mass of the organic solvent.

[0039] <Hydroxide wax dispersion> To further improve the abrasion resistance and blocking properties of the resulting printed layer, hydrocarbon wax can be added to the varnish composition. Furthermore, when the varnish composition contains a hydrocarbon wax dispersion, the slip angle of the resulting printed layer tends to be smaller. A smaller slip angle of the printed layer results in a lower coefficient of friction on the surface of the printed layer. As a result, stress on the printed layer is reduced during transportation, display, or use of the packaging material, suppressing abrasion and detachment of the printed layer. Additionally, because the printed layer is more slippery during transportation of the packaging material, work efficiency is improved and transportation problems are reduced. Examples of hydrocarbon waxes include polyethylene wax, Fischer-Tropsch wax, paraffin wax, microstarin wax, and polypropylene wax. Among these, polyethylene wax and Fischer-Tropsch wax are preferred. Examples of polyethylene waxes include high-density polymerized polyethylene, low-density polymerized polyethylene, oxidized polyethylene, acid-modified polyethylene, and special monomer-modified polyethylene. Fischer-Tropsch wax is a wax produced by the Fischer-Tropsch process using carbon monoxide and hydrogen as raw materials, and has a nearly saturated, non-branched linear molecular structure. Hydrocarbon waxes may be used individually or in combination of two or more types.

[0040] The penetration (hardness) of hydrocarbon waxes at 25°C, as specified in JIS K 2207:2006, is preferably 0.1 to 30, more preferably 0.1 to 28, and particularly preferably 0.1 to 25. If the penetration (hardness) of the hydrocarbon wax exceeds the above upper limit, the abrasion resistance of the resulting printed layer will be slightly reduced. Additionally, the printability will be slightly reduced.

[0041] Hydrocarbon waxes are preferably added to the varnish composition as a hydrocarbon wax dispersion. The above-mentioned organic solvents are preferred as the dispersion medium for the dispersion. The median diameter of the hydrocarbon wax dispersion is preferably 3.0 to 15.0 μm, more preferably 4.0 to 10.0 μm, and even more preferably 4.5 to 8.0 μm. If the median diameter exceeds the above upper limit, the adhesion, abrasion resistance, water abrasion resistance, and printability of the resulting printed layer to the substrate will be slightly reduced. Furthermore, the inventors of this application have found that if the median diameter exceeds 10.0 μm, the highlight transferability will be slightly reduced. Highlight transferability means that the varnish transferability is good even in the highlight areas of the printed material. When highlight transferability is excellent, dot defects are less likely to occur in the highlight areas of the printed material. For example, in gravure printing, the holes in the highlight areas of the plate are shallow. If hydrocarbon wax with a large median diameter is present in the highlight areas, it is thought that it inhibits varnish transfer and reduces highlight transferability. Furthermore, we found that if the median diameter is below the lower limit mentioned above, effective surface irregularities cannot be sufficiently formed on the printed layer, resulting in a larger contact area and a tendency for the resulting printed layer to have a larger slip angle. In this specification, the median diameter of a hydrocarbon wax dispersion shall be the value disclosed by the manufacturer, or, if not disclosed by the manufacturer, the particle diameter at 50% of the volume-based integrated value (D50) in the particle size distribution measured by laser diffraction-scattering. During measurement, sufficient dispersion should be ensured using a paint shaker or similar device.

[0042] <Resin beads> To further improve the abrasion resistance and blocking properties of the resulting printed layer, resin beads can be added to the varnish composition. Examples of resins include melamine resins, condensates of melamine resins and formaldehyde, benzoguanamine resins, condensates of benzoguanamine resins and formaldehyde, condensates of benzoguanamine resins, melamine resins, and formaldehyde, (meth)acrylic resins, polystyrene resins, urethane resins, silicone resins, polycarbonate resins, copolymers of (meth)acrylic monomers and styrene monomers, polyolefin resins, polyester resins, polyamide resins, polyimide resins, and polyfluoroethylene resins. Among these, (meth)acrylic resins, condensates of melamine resins and formaldehyde, condensates of benzoguanamine resins and formaldehyde, and condensates of benzoguanamine resins, melamine resins, and formaldehyde are preferred from the viewpoint of excellent matte properties and storage stability. The resin may be crosslinked or non-crosslinked. Resin beads can be used individually or in combination of two or more types.

[0043] The average particle size of the resin beads is preferably 0.1 to 4.0 μm, more preferably 0.5 to 2.5 μm, and even more preferably 0.7 to 2.0 μm. If the average particle size is below the lower limit, the blocking resistance of the resulting printed layer will be slightly reduced. If the average particle size is above the upper limit, the storage stability of the varnish composition and the abrasion resistance of the resulting printed layer will be slightly reduced. In addition, the highlight transfer properties mentioned above will also be slightly reduced. Furthermore, we found that when the average particle size is less than 0.5 μm, effective surface irregularities cannot be sufficiently formed on the printed layer, resulting in a larger contact area and a tendency for the resulting printed layer to have a larger slip angle. In this specification, the average particle size of resin beads shall be the value disclosed by the manufacturer, or, if not disclosed by the manufacturer, the particle size at 50% of the volume-based cumulative value (D50) in the particle size distribution measured by laser diffraction-scattering method.

[0044] <Plasticizer> To further improve the resistance to rubbing and cold rubbing of the resulting printed layer, a plasticizer can be added to the varnish composition. Examples of plasticizers are not particularly limited, but include phthalates, adipicates, trimelliticates, aliphatic dibasicates, phosphates, ricinoleates, sebacates, azelaates, maleates, fumarates, benzoates, polyesters, citrates, acetates, sulfonamides, mixed dibasicates, and vegetable oil derivatives such as epoxidized vegetable oils. Plasticizers may be used individually or in combination of two or more types.

[0045] The freezing point of the plasticizer is preferably 6°C or lower, more preferably 3°C or lower, and even more preferably -10°C or lower. If the freezing point of the plasticizer exceeds the above upper limit, the cold-hardening resistance will be slightly reduced. In low-temperature environments, the varnish coating hardens and loses its flexibility, leading to frequent peeling of the coating due to cracking when kneaded. However, by including a plasticizer with a low freezing point, it becomes possible to maintain flexibility even in low-temperature environments, thus resulting in excellent cold-hardening resistance. The freezing point of the plasticizer is preferably as low as possible, and although there is no particular lower limit, it is, for example, -60°C or higher. In this specification, the freezing point is a value measured in accordance with JIS K 0065:1992.

[0046] <Styrene-maleic acid copolymer> To improve the blocking resistance of the resulting printed layer, a styrene-maleic acid copolymer may be included in the varnish composition. The styrene-maleic acid copolymer is a copolymer reaction product of styrene and maleic acid. In this specification, the styrene-maleic acid copolymer is not included in the binder resin. Furthermore, the styrene-maleic acid copolymer may optionally contain units based on monomers other than styrene-based units and units based on maleic acid (other monomers). The other monomers are not particularly limited as long as they can copolymerize with styrene and maleic acid.

[0047] Other monomers include, for example, vinyl alcohol; halogenated olefins such as vinyl chloride and vinylidene chloride; (meth)acrylates; conjugated diene compounds such as 1,3-butadiene, isoprene, and chloroprene; aromatic vinyl compounds such as α-methylstyrene, halogenated styrene, and divinylbenzene; vinyl cyanide compounds such as acrylonitrile and methacrylonitrile; acrylamides such as N,N-dimethyl(meth)acrylamide and N,N-diethyl(meth)acrylamide; unsaturated carboxylic acid esters such as diethyl maleate, dibutyl maleate, dibutyl fumarate, diethyl itaconate, and dibutyl itaconate; and carboxyl group-containing monomers such as (meth)acrylic acid, fumaric acid, and itaconic acid (itaconic anhydride).

[0048] The total content of styrene-based units and maleic acid-based units relative to the total mass of the styrene-maleic acid copolymer is preferably 60 to 100% by mass, more preferably 70 to 100% by mass, and even more preferably 80 to 100% by mass. If the total content of the above is below the lower limit, the blocking resistance of the resulting printed layer and the storage stability of the varnish composition will be slightly reduced. The styrene-maleic acid copolymer may be used alone or in combination of two or more types.

[0049] <Other ingredients> Other components include, for example, binder resins other than polyurethane resin (A) and nitrocellulose resin (B), fatty acid amides, chelating agents, rosin derivatives, defoaming agents, dispersants, anti-settling agents, UV absorbers, antioxidants, antistatic agents, leveling agents, thickeners, stabilizers, etc. Examples of other binder resins include (meth)acrylic resins, chlorinated polyolefin resins, polyamide resins, terpene resins, etc. Other ingredients may be used individually or in combination of two or more.

[0050] <Content of each ingredient> The total solid content of polyurethane resin (A) and nitrocellulose resin (B) is 48 to 75% by mass, preferably 50 to 72% by mass, more preferably 55 to 70% by mass, and even more preferably 57 to 68% by mass, based on the total mass of solids in the varnish composition. If the total content is below the lower limit, the stretch-resistant adhesion of the resulting printed layer will decrease. Cold-resistant properties will also decrease. If the total content exceeds the upper limit, the blocking resistance of the resulting printed layer will decrease.

[0051] The total solid content of polyurethane resin (A) and nitrocellulose resin (B) is preferably 8 to 25% by mass, more preferably 10 to 20% by mass, and even more preferably 12 to 17% by mass, relative to the total mass of the varnish composition. If the total content is below the lower limit, the stretch-resistant adhesion of the resulting printed layer will decrease. Cold-resistant properties will also decrease. If the total content exceeds the upper limit, the blocking resistance of the resulting printed layer will decrease.

[0052] The solid content of polyurethane resin (A) is preferably 28 to 45% by mass, more preferably 30 to 42% by mass, and even more preferably 34 to 40% by mass, relative to the total mass of solid content of the varnish composition. If the content of polyurethane resin (A) is below the lower limit, the stretch-resistant adhesion and cold-resistant properties of the resulting printed layer will be slightly reduced. If the content of polyurethane resin (A) exceeds the upper limit, the blocking resistance of the resulting printed layer will be slightly reduced.

[0053] The solid content of polyurethane resin (A) is preferably 4.5 to 15% by mass, more preferably 6 to 12% by mass, and even more preferably 7 to 10% by mass, based on the total mass of the varnish composition. If the content of polyurethane resin (A) is below the lower limit, the stretch-resistant adhesion and cold-resistant properties of the resulting printed layer will be slightly reduced. If the content of polyurethane resin (A) exceeds the upper limit, the blocking resistance of the resulting printed layer will be slightly reduced.

[0054] The solid content of nitrocellulose resin (B) is preferably 18 to 32% by mass, more preferably 20 to 29.5% by mass, and even more preferably 22 to 28% by mass, relative to the total mass of solids in the varnish composition. If the content of nitrocellulose resin (B) is below the lower limit, the blocking resistance of the resulting printed layer will be slightly reduced. If the content of nitrocellulose resin (B) exceeds the upper limit, the stretch adhesion resistance and cold tarnish resistance of the resulting printed layer will be slightly reduced.

[0055] The solid content of nitrocellulose resin (B) is preferably 3.2 to 10% by mass, more preferably 4 to 8% by mass, and even more preferably 4.5 to 6.5% by mass, relative to the total mass of the varnish composition. If the content of nitrocellulose resin (B) is below the lower limit, the blocking resistance of the resulting printed layer will be slightly reduced. If the content of nitrocellulose resin (B) exceeds the upper limit, the stretch adhesion resistance and cold tarnish resistance of the resulting printed layer will be slightly reduced.

[0056] The mass ratio of solids represented by polyurethane resin (A) / nitrocellulose resin (B) (hereinafter also referred to as "A / B") is 0.95 to 2.5, preferably 1.0 to 2.3, more preferably 1.1 to 2.0, and even more preferably 1.2 to 1.7. If the A / B ratio is below the lower limit, the stretch-resistant adhesion of the resulting printed layer will decrease. Furthermore, its cold-resistant properties will also decrease. If the A / B ratio exceeds the upper limit, the blocking resistance of the resulting printed layer will decrease.

[0057] The total solid content of polyurethane resin (A) and nitrocellulose resin (B) is preferably 60 to 100% by mass, more preferably 70 to 100% by mass, and even more preferably 80 to 100% by mass, relative to the total mass of solid content of the binder resin. 100% by mass is also acceptable.

[0058] The content of the organic solvent is preferably 40 to 90% by mass, more preferably 50 to 88% by mass, and even more preferably 60 to 85% by mass, based on the total mass of the varnish composition. If the organic solvent content is below the lower limit, the varnish fluidity tends to decrease. If the organic solvent content exceeds the upper limit, the drying properties tend to decrease.

[0059] If the varnish composition contains hydrocarbon wax, the solid content of the hydrocarbon wax is preferably 0.1 to 5% by mass, more preferably 0.2 to 2.5% by mass, and even more preferably 0.3 to 1% by mass, relative to the total mass of the varnish composition. If the hydrocarbon wax content is below the lower limit, the abrasion resistance and blocking resistance of the resulting printed layer will be slightly reduced. Also, the slip angle of the resulting printed layer tends to be larger. If the hydrocarbon wax content exceeds the upper limit, the highlight transfer properties will be slightly reduced.

[0060] When the varnish composition contains hydrocarbon wax, the solid content of the hydrocarbon wax is preferably 0.3 to 13% by mass, more preferably 0.6 to 8% by mass, and even more preferably 1 to 3% by mass, relative to the total mass of solids in the varnish composition. If the hydrocarbon wax content is below the lower limit, the abrasion resistance and blocking resistance of the resulting printed layer will be slightly reduced. Also, the slip angle of the resulting printed layer tends to be larger. If the hydrocarbon wax content exceeds the upper limit, the highlight transfer properties will be slightly reduced.

[0061] If the varnish composition contains resin beads, the solid content of the resin beads is preferably 0.01 to 3% by mass, more preferably 0.05 to 1% by mass, and even more preferably 0.08 to 0.3% by mass, relative to the total mass of the varnish composition. If the resin bead content is below the lower limit, the abrasion resistance and blocking resistance of the resulting printed layer will be slightly reduced. Also, the slip angle of the resulting printed layer tends to be larger. If the resin bead content exceeds the upper limit, the highlight transfer properties will be slightly reduced.

[0062] If the varnish composition contains resin beads, the solid content of the resin beads is preferably 0.05 to 8.5% by mass, more preferably 0.1 to 5% by mass, and even more preferably 0.2 to 1.0% by mass, relative to the total mass of solids in the varnish composition. If the resin bead content is below the lower limit, the abrasion resistance and blocking resistance of the resulting printed layer will be slightly reduced. Also, the slip angle of the resulting printed layer tends to be larger. If the resin bead content exceeds the upper limit, the highlight transfer properties will be slightly reduced.

[0063] If the varnish composition contains a plasticizer, the solid content of the plasticizer is preferably 1 to 20% by mass, more preferably 5 to 18% by mass, and even more preferably 10 to 16% by mass, relative to the total mass of solids in the varnish composition. If the plasticizer content is below the lower limit, the cold resistance of the resulting printed layer will be slightly reduced. If the plasticizer content exceeds the upper limit, the varnish fluidity of the varnish composition may decrease.

[0064] When the varnish composition contains a styrene-maleic acid copolymer, the solid content of the styrene-maleic acid copolymer is preferably 1 to 20% by mass, more preferably 3 to 16% by mass, and even more preferably 5 to 14% by mass, relative to the total mass of the solids of the varnish composition. If the styrene-maleic acid copolymer content is below the lower limit, the blocking resistance of the resulting printed layer will be slightly reduced. If the styrene-maleic acid copolymer content exceeds the upper limit, the abrasion resistance and adhesion to the substrate of the resulting printed layer will be slightly reduced.

[0065] The content of other components is not particularly limited as long as it does not impair the effects of the present invention, but for example, it is preferably 0 to 20% by mass, more preferably 0 to 15% by mass, even more preferably 0 to 10% by mass, particularly preferably 0 to 5% by mass, and particularly preferably 0 to 1% by mass, based on the total mass of the varnish composition. If the varnish composition contains other components, the content of these other components is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and even more preferably 0.5% by mass or more, relative to the total mass of the varnish composition. If the content of these other components is above the above lower limit, the effects of these other components will be fully expressed.

[0066] <Method for manufacturing varnish composition> The varnish composition of this embodiment can be obtained, for example, by dissolving or dispersing a polyurethane resin (A), a nitrocellulose resin (B), and optionally one or more of a hydrocarbon wax dispersion, resin beads, a plasticizer, a styrene-maleic acid copolymer, and other components in an organic solvent. The method for dissolving or dispersing each component in an organic solvent is not particularly limited and can be carried out using known dispersers. Examples of dispersers include paint shakers, ball mills, attritors, sand mills, bead mills, dyno mills, roll mills, ultrasonic mills, and high-pressure impact dispersers. In this case, the dispersion treatment may be performed once or multiple times using one type of disperser, or multiple dispersion treatments may be performed using two or more types of dispersers in combination.

[0067] <Application> The varnish composition of this embodiment is for surface printing and is suitable as a varnish for printing on the front side of a substrate that will become a packaging material (i.e., the side that does not come into contact with the product to be packaged). In particular, it is ideal as a varnish (gravure printing varnish) for printing on the front side of a substrate by gravure printing.

[0068] The varnish composition of this embodiment can form a printing layer with excellent stretch resistance and adhesion to a stretchable film as a substrate, but the substrate to be printed on is not particularly limited. The substrate may or may not be subjected to corona discharge treatment. In addition to corona discharge treatment, surface treatments that generate polar functional groups on the substrate surface, such as plasma treatment, are known, but the substrate may or may not be subjected to such surface treatments. The material of the substrate is also not limited, and examples include various plastics such as polyethylene (PE), polyolefins such as polypropylene (PP), polyesters such as polyethylene terephthalate (PET), polystyrene (PS), and polyamide (NY). Examples of PE include low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), and high-density polyethylene (HDPE). One type of plastic may be used alone, or two or more types may be used in combination.

[0069] A plastic film is preferred as the base material. Examples of plastics that make up the plastic film are the same as those mentioned above. The plastic film may or may not be stretched. Among these, an unstretched film is preferred. Examples of stretched plastic films include biaxially oriented PP film (OPP) and biaxially oriented NY film (ONY). An example of an unstretched plastic film is an unstretched polypropylene film. The plastic film may be used alone or two or more types may be laminated together. The thickness of the plastic film is, for example, 5 to 150 μm.

[0070] By printing on one side (surface) of a plastic film using the varnish composition of this embodiment to form a printed layer, a laminate comprising a plastic film and a printed layer (varnish layer) is obtained. The one side of the plastic film is the side that becomes the front when used as packaging material. The printed layer is typically formed in contact with one side of the plastic film. Furthermore, the printed layer is typically located on the outermost surface of the laminate, and no other layers are formed on top of it. The laminate may or may not have additional layers on the other side (back side) of the plastic film.

[0071] The laminate may further include a pattern layer between the plastic film and the varnish layer. The pattern layer is typically a printed layer formed using ink. The ink may be a known ink. The ink typically contains a pigment. The method for forming the ink layer may be a known printing method, similar to the method for forming the varnish layer.

[0072] The printed layer can be formed by known methods. For example, a varnish composition is applied to one side of a plastic film and dried to form the printed layer. The process of applying the varnish composition and drying may be repeated two or more times. The thickness of the printed layer is, for example, 0.2 to 3 μm. The method of applying the varnish composition is not particularly limited, and known application methods such as gravure printing, flexographic printing, brush application, gravure coater method, die coater method, bar coater method, spray coating method, flow coating method, dip coating method, spin coating method, and curtain coating method can be used. Among these, gravure printing is preferred due to its high quality and productivity. Therefore, the varnish composition of this embodiment is preferably a gravure printing varnish composition. The drying method only needs to remove the organic solvent contained in the varnish composition, and known drying methods such as vacuum drying, pressure drying, heat drying, and air drying can be used. The temperature for heat drying is, for example, 30 to 150°C.

[0073] The resulting laminate is suitable as a packaging material, particularly as a flexible packaging material. "Flexible packaging" refers to packaging materials made of flexible materials, and is used for packaging food, daily necessities, and other items.

[0074] <Mechanism of Action> The surface printing varnish composition of the present invention comprises a polyurethane resin (A), a nitrocellulose resin (B), and an organic solvent. As shown in the examples described below, when the 10% modulus of the mixture of polyurethane resin (A) and the nitrocellulose resin (B) is 3.0 to 50.0 MPa, the stretch resistance and blocking resistance of the resulting printed layer are improved. Furthermore, when the total solid content of polyurethane resin (A) and nitrocellulose resin (B) is 48 to 75% by mass relative to the total mass of solid content of the surface printing varnish composition, the stretch resistance and blocking resistance of the resulting printed layer are improved. Cold tarnish resistance is also improved. Furthermore, when the mass ratio of solid content represented by polyurethane resin (A) / nitrocellulose resin (B) is 0.95 to 2.5, the stretch resistance and blocking resistance of the resulting printed layer are improved. Cold tarnish resistance is also improved. [Examples]

[0075] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples unless it exceeds the gist of the invention. Examples 8-12 and 14 are for reference only. Unless otherwise specified, "%" means "mass%".

[0076] [Raw materials used] <Polyurethane resin (A)> A1: Polyether-based polyurethane resin, solids content: 70%, number average molecular weight: 8,000, acid value: 4.3 mg KOH / g, hydroxyl value: 21.4 mg KOH / g, amine value: 0 mg KOH / g. A2: Polyester / polyether-based polyurethane resin, solids content: 40%, glass transition temperature: -50℃, number average molecular weight: 15,000, amine value: 0.5 mg KOH / g. A3: Polyester-based polyurethane resin. Solids content: 30%, glass transition temperature: -24℃, number average molecular weight: 20,100, hydroxyl value: 4.2 mg KOH / g, amine value: 0.5 mg KOH / g.

[0077] <Nitrocellulose resin (B)> B1: Manufactured by Nobel, product name "DHX30-50", solids content: 21.0%, type and viscosity symbol: H1 / 2. B2: Manufactured by Nobel, product name "DHL5 / 15", solids content: 15.4%, type and viscosity symbol: H2.

[0078] <Organic solvents> A mixed solvent of ethyl acetate, n-propyl acetate, and isopropanol in a mass ratio of 6:2:2.

[0079] <Optional ingredients> (Hydroxide wax dispersion) • Ethyl acetate dispersion of "High Wax 220P," manufactured by Mitsui Chemicals, Inc., median diameter: 5.5 μm, solids content: 15%, penetration: 13. In Tables 1-3, it is referred to as "High Wax 220P." • Ethyl acetate dispersion of "High Wax 110P," manufactured by Mitsui Chemicals, Inc., with a median diameter of 7.0 μm, solids content of 10%, and penetration of 25. In Tables 1-3, it is referred to as "High Wax 110P." Manufactured by Polycon Co., Ltd., product name "Polycon RB-1", isopropanol dispersion, median diameter: 3.5 μm, solids content: 20%. In Tables 1-3, it will be referred to as "Polycon RB-1". • Honeywell product, product name "AC Polyethylene 6A", isopropanol dispersion, median diameter: 12.8 μm, solids content: 25%, penetration degree: 4. In Tables 1-3, it is referred to as "FX AC 6A".

[0080] (Resin beads) • Manufactured by Soken Chemical Co., Ltd., product name "MR-1HG", acrylic resin beads, average particle size: 1 μm. In Tables 1-3, it is referred to as "MR-1HG". • Manufactured by Nippon Shokubai Co., Ltd., product name "Epostor S6", melamine / formaldehyde resin beads, average particle size: 0.4 μm. In Tables 1-3, it will be referred to as "Epostor S6". • Manufactured by Nippon Shokubai Co., Ltd., product name "Epostor M30", benzoquanamine / melamine / formaldehyde resin beads, average particle size: 3.0 μm. In Tables 1-3, it is referred to as "Epostor M30".

[0081] (Plasticizer) • Manufactured by Daihachi Chemical Industry Co., Ltd., product name "BXA-N", solids content: 100%, freezing point: -19℃. In Tables 1-3, it is referred to as "BXA-N". • Manufactured by Daihachi Chemical Industry Co., Ltd., product name "DMP", solids content: 100%, freezing point: 0℃. In Tables 1-3, it will be referred to as "DMP". • Manufactured by ADEKA Corporation, product name "ADEKA Sizer O-130P", solids content: 100%, freezing point: 5℃. In Tables 1-3, it will be referred to as "O-130P".

[0082] (Other optional components) • Chelating agent, manufactured by Matsumoto Fine Chemical Co., Ltd., product name "Orgatics TC-100", solid content: 75%. • Styrene-maleic acid copolymer resin, solids content: 40%. • Fatty acid amide: Manufactured by Nippon Seika Co., Ltd., product name "Neutron S", solid content: 100%. • Defoaming agent: Manufactured by BYK, product name "BYK-1751", solids content: 100%.

[0083] <Method for measuring 10% modulus> A varnish containing polyurethane resin (A) and nitrocellulose resin (B) was applied to release paper using an applicator to create a dry film with a thickness of 30 μm, and then heat-dried. However, the mass ratio of the solid content of polyurethane resin (A) and nitrocellulose resin (B) in the varnish was as shown in Tables 1 to 3. The obtained film was aged for 24 hours under conditions of 25°C to prepare the film for test specimens. After aging, the film was peeled off the release paper and cut into strips measuring 6 cm x 1.5 cm to prepare the test specimens. Under conditions of 25°C, the prepared test specimens were stretched in the longitudinal direction of the specimen at a tensile speed of 20 cm / min using an autograph. From the obtained stress-strain curve, the stress at the point when the elongation of the test specimen reached 10% (1.1 times the original length) was read. Three measurements were taken, and the average value was taken as the 10% modulus of the mixture of polyurethane resin (A) and nitrocellulose resin (B).

[0084] [Examples 1-19, Comparative Examples 1-7] <Preparation of Varnish Composition> According to the compositions shown in Tables 1-3, polyurethane resin (A), nitrocellulose resin (B), organic solvent, and optional components were mixed, and the resulting mixture was kneaded in a paint shaker to obtain a varnish composition. In Tables 1-3, the content of polyurethane resin (A), nitrocellulose resin (B), and other components in the composition [mass %] column refers to the percentage of solids (mass %) relative to the total mass of the varnish composition. However, the "residue" of the organic solvent is the amount that makes the total mass of the varnish composition 100%. Also, a blank space means that the component was not included. In Tables 1-3, the solids base column refers to the content of solids such as polyurethane resin (A) and nitrocellulose resin (B) relative to the total mass of solids in the varnish composition. For example, the content of (A) refers to the content of polyurethane resin (A) relative to the total mass of solids in the varnish composition. Also, the 10% modulus of (A)+(B) in the evaluation column refers to the 10% modulus of the mixture of polyurethane resin (A) and nitrocellulose resin (B). The mass ratio of the solid content of polyurethane resin (A) and nitrocellulose resin (B) in the mixture is as shown in Tables 1-3. The resulting varnish composition was used for the evaluation described below. The results are shown in Tables 1-3.

[0085] <Creating printed materials> The prepared varnish composition was diluted with the same organic solvent used in the formulation so that its viscosity at 25°C, as measured using a Zahn cup #3, was 16 seconds, thereby preparing a varnish for printing. Using a gravure printing press (manufactured by Matsuo Sangyo Co., Ltd., product name "K Printing Proofer") equipped with a Helio 175 lines / inch gravure engraving plate (solid and stepless gradient plates), the prepared varnish for printing was applied to the treated surface of an unoriented polypropylene film (manufactured by RM Tosero Co., Ltd., product name "SC#30", thickness: 30 μm). After drying at 50°C for 10 seconds, solid prints and stepless gradient prints were produced.

[0086] <Evaluation of stretch resistance and adhesion> The obtained solid print material was stretched to 400% using a tensile testing machine (A&D Company, Limited, product name "Tensilon RTG-1225") at a temperature of 20°C and a tensile speed of 300 mm / min. After applying cellophane adhesive tape (Nichiban Co., Ltd.) to the surface of the stretched print coating, the cellophane adhesive tape was quickly peeled off, and the condition of the varnish layer remaining on the substrate was visually inspected. The stretch resistance and adhesion were evaluated according to the following evaluation criteria. A score of 3 to 5 indicates excellent stretch resistance and adhesion. 5: The varnish layer has not peeled off at all. 4. The ratio of the area of ​​the peeled varnish layer to the total area of ​​the varnish layer is greater than 0% and less than or equal to 5%. 3. The ratio of the area of ​​the peeled varnish layer to the total area of ​​the varnish layer is greater than 5% and less than or equal to 20%. 2: The ratio of the area of ​​the peeled varnish layer to the total area of ​​the varnish layer is greater than 20% and less than or equal to 50%. 1: The area of ​​the peeled varnish layer is more than 50% of the total area of ​​the varnish layer.

[0087] <Evaluation of resistance to plasticizer blocking> A thin layer of plasticizer (diisononyl phthalate) was applied to the surface of a commercially available transparent polyvinyl chloride sheet cut to 5cm x 5cm, and left to stand at 20°C for 24 hours. Next, the resulting solid print varnish layer and the plasticizer-coated side of the polyvinyl chloride sheet were placed on top of each other, and 3 kg / cm² of plasticizer was applied. 2 The specimens were subjected to a load and stored in a constant temperature chamber at 40°C and 80% humidity for 24 hours. Afterward, the specimens were peeled off, and their resistance to plasticizer blocking was evaluated according to the evaluation criteria shown below. A score of 3-5 indicates excellent resistance to blocking (plasticizer blocking). 5: No varnish removal. 4. The area of ​​varnish removal is greater than 0% and less than or equal to 5% of the total area of ​​the varnish layer. 3. The area of ​​varnish removal is between 5% and 20% of the total varnish layer area. 2: The area of ​​varnish removal is between 20% and 50% of the total area of ​​the varnish layer. 1: The area affected by varnish removal exceeds 50% of the total surface area of ​​the varnish layer.

[0088] <Evaluation of cold tolerance of rice grains> The obtained solid print materials were stored in a freezer for one day, and then vigorously rubbed in the freezer so that all surfaces of the print material touched each other. The cold resistance to rubbing was then evaluated according to the evaluation criteria shown below. 5: The varnish layer has not peeled off at all. 4. The ratio of the area of ​​the peeled-off varnish layer to the total area of ​​the varnish layer is greater than 0% and less than or equal to 5%. 3. The ratio of the area of ​​the peeled-off varnish layer to the total area of ​​the varnish layer is greater than 5% and less than or equal to 20%. 2: The ratio of the area of ​​the peeled-off varnish layer to the total area of ​​the varnish layer is greater than 20% and less than or equal to 50%. 1: The area of ​​the peeled-off varnish layer is more than 50% of the total area of ​​the varnish layer.

[0089] <Evaluation of highlight transferability> The highlight areas (5% halftone density) of the obtained stepless gradient prints were observed, and the highlight transfer properties were evaluated according to the evaluation criteria shown below. Although the varnish composition and varnish layer are transparent, the presence or absence of dot defects can be confirmed by microscopic observation of the highlight areas. 5: No dead pixels are visible in the highlight areas. 4: Very few dead pixels are visible in the highlight areas. 3: Minor dead pixels are visible in the highlight areas. 2: Dead pixels are visible in the highlight areas. 1: Noticeable dead pixels are visible in the highlight areas.

[0090] <Evaluation of suitability for skid angle> The varnish layers of the obtained solid prints were stacked together, and the slip angle was measured using a friction measuring machine (manufactured by Toyo Seiki Co., Ltd., product name "Friction Measuring Machine AN") in accordance with JIS P 8147:2010 "8 Inclination Method". The suitability of the slip angle was evaluated according to the evaluation criteria shown below. It is 3:30° or less. 2: Greater than 30° and less than or equal to 38°. It is greater than 1:38°.

[0091] [Table 1]

[0092] [Table 2]

[0093] [Table 3]

[0094] The printed layers obtained from the varnish compositions of Examples 1 to 19 exhibited excellent resistance to stretch adhesion and resistance to blocking (resistance to plasticizer blocking). The printed layers obtained from the varnish compositions of Comparative Examples 1 to 7 exhibited inferiority in either resistance to stretch adhesion or resistance to blocking (resistance to plasticizer blocking). [Industrial applicability]

[0095] The printed layer formed from the surface printing varnish composition of this embodiment is useful because it has excellent resistance to stretch adhesion and blocking.

Claims

1. A printing varnish composition for surface printing comprising a polyurethane resin (A), a nitrocellulose resin (B), a hydrocarbon wax dispersion, resin beads, and an organic solvent, The total solid content of the polyurethane resin (A) and the nitrocellulose resin (B) is 48 to 75% by mass of the total solid content of the surface printing varnish composition. The mass ratio of the solid content represented by the polyurethane resin (A) and the nitrocellulose resin (B) is 0.95 to 2.

5. The 10% modulus of the mixture of the polyurethane resin (A) and the nitrocellulose resin (B), as measured by the following method, is 3.0 to 50.0 MPa. A printing varnish composition for surface printing, wherein the median diameter of the hydrocarbon wax dispersion is 4.0 to 10.0 μm, and the average particle size of the resin beads is 0.5 to 2.5 μm. [Method for measuring 10% modulus] A varnish containing the polyurethane resin (A) and the nitrocellulose resin (B) is applied to release paper using an applicator to form a dry film with a thickness of 30 μm, and then heat-dried. However, the mass ratio of the solid content of the polyurethane resin (A) and the nitrocellulose resin (B) in the varnish is the same as the mass ratio in the printing varnish composition for surface printing. The obtained film is aged for 24 hours under conditions of 25°C to prepare a film for test specimens. After aging, the film is peeled off the release paper and cut into strips measuring 6 cm in length and 1.5 cm in width to prepare test specimens. Under conditions of 25°C, the prepared test specimens are stretched in the longitudinal direction of the test specimen at a tensile speed of 20 cm / min using an autograph. From the obtained stress-strain curve, the stress at the point when the elongation rate of the test specimen reaches 10% (1.1 times the original length) is read. The measurement was performed three times, and the average value was taken as the 10% modulus of the mixture of the polyurethane resin (A) and the nitrocellulose resin (B).

2. The printing varnish composition for surface printing according to Claim 1, wherein the mass ratio of the polyurethane resin (A) to the nitrocellulose resin (B) is 0.95 to 2.

3.

3. The printing varnish composition for surface printing according to claim 1, further comprising a plasticizer, wherein the plasticizer has a freezing point of 3°C or lower.

4. The printing varnish composition for surface printing according to claim 1, wherein the number average molecular weight of the polyurethane resin (A) is 20,000 or less.

5. The printing varnish composition for surface printing according to claim 1, further comprising a styrene-maleic acid copolymer.

6. A printing varnish composition for surface printing according to any one of claims 1 to 5, for use in gravure printing.

7. A laminate comprising a plastic film and a printed layer formed on one surface of the plastic film using the surface printing varnish composition described in any one of claims 1 to 5.

8. A laminate comprising a plastic film and a printed layer formed on one surface of the plastic film using the surface printing varnish composition described in claim 6.

9. A packaging material comprising the laminate described in claim 7.

10. A packaging material comprising the laminate described in claim 8.

Citation Information

Patent Citations

  • Method for re-utilizing residual ink

    JP2015101074A

  • Gravure printing ink composition for surface printing

    JP2016196560A

  • Gravure printing ink composition for surface printing and surface-printed gravure printed matter

    JP2017025256A

  • Gravure printing ink composition for surface printing and surface printing gravure printed matter printed therewith

    JP2017039896A

  • Gravure printing ink composition for surface printing

    JP2018188558A