Porous composite elastic materials, silicon carbon, methods for producing the same, and applications

A structured silicon-carbon composite anode material with interpenetrating carbon nanotubes and hard carbon addresses conductivity and volume expansion issues, enhancing the performance and safety of lithium-ion battery electrodes.

JP7955558B1Active Publication Date: 2026-11-24CARBON ONE NEW ENERGY GRP CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2026529793
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2024-03-04
Filing Date
2025-01-17
Publication Date
2026-11-24
Estimated Expiration
2045-01-17

AI Technical Summary

Technical Problem

Silicon-based negative electrode materials for lithium-ion batteries face issues with low electrical conductivity, ion diffusion, severe volume expansion leading to cracking and detachment from the current collector, and poor cycle performance due to simple physical combinations of silicon and carbon not ensuring good ionic conductivity and uniformity.

Method used

A porous composite elastic body is created by interpenetrating flexible carbon nanotubes and rigid hard carbon, with controlled pore sizes and ratios, using a method that includes molding, infiltration, and high-temperature carbonization to form a structured silicon-carbon composite anode material.

Benefits of technology

The composite material enhances ion and electron conductivity, reduces the risk of cracking during volume expansion, and improves the cycle performance and manufacturing safety of electrode plates by ensuring uniform distribution and strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007955558000005
    Figure 0007955558000005
  • Figure 0007955558000006
    Figure 0007955558000006
  • Figure 0007955558000007
    Figure 0007955558000007
Patent Text Reader

Abstract

This application relates to the technical field of negative electrode materials for batteries, and more particularly to porous composite elastic materials, silicon carbon and This application relates to a method for manufacturing a bison and its applications. This application includes a flexible body and a rigid body that penetrate each other. The invention provides a porous composite elastic body having a porous structure, wherein the raw material of the flexible body is carbon nanotubes. The rigid body contains carbon nanotubes and hard carbon. By using hard carbon as a carbon source and compounding it with silicon, silicon-carbon composite materials are manufactured. Compared to conventional silicon-carbon composite materials, carbon nanotubes are made of silicon and hard carbon. By acting as a bridge between vons, it effectively improves conductivity and ionic conduction energy. This improves the rate characteristics of the negative electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present application relates to the technical field of battery negative electrode materials, in particular to porous composite elastomers, silicon carbon and its manufacturing methods and applications. [Background Art]

[0002] Because silicon has an extremely high theoretical lithium storage capacity and a moderate lithium release / storage potential Therefore, silicon-based negative electrode materials are the next generation of ideal lithium-ion battery negative electrode materials after graphite There is no doubt about the fee. However, silicon has very low electrical conductivity and ion diffusion coefficient Moreover, in the process of lithium release / occlusion, silicon undergoes severe volume expansion (>300%) This causes the material to crack, powder, and fall off from the current collector, resulting in a decrease in capacity drops sharply, and the cycle deteriorates. In the prior art, carbon materials and silicon are combined By making it possible to alleviate the volume expansion of silicon to some extent and improve the cycle characteristics Although this is possible, such a simple physical combination of silicon and carbon results in a complex material I cannot guarantee the on-conduction performance.

[0003] Patent (CN114420928A) discloses carbon nanotubes, graphene, and nanosheets By coating soft carbon on the outer layer of recon as a core material, the core shell discloses forming a silicon-carbon composite material with a metal structure. Carbon nanotube and graphene can improve the ionic conductivity of composite materials, but carbon nanomaterials Combining tubes, graphene, and silicon by polishing ensures uniformity of the composite Because it is not possible to guarantee good ionic conductivity in the bulk phase cannot be achieved. In addition, when silicon exists in micrometer form, during the lithium release / insertion process it causes severe volume expansion, which leads to a sharp decline in the cycle performance of the battery. Patent ( CN115663131A) deposits nano-silicon into spherical carbon nanotubes using a CVD vapor-phase growth method. Although the volume expansion is alleviated by reducing the size of silicon, the pores of the formed spherical carbon nanotubes are very large, making it easy for silicon to aggregate during the deposition process. Furthermore, due to the large hardness difference between carbon nanotubes and silicon, the material is damaged during the roll pressing step in electrode plate manufacturing. Additionally, the material becomes pulverized due to volume expansion during lithium release / insertion, further leading to a sharp decline in cycle performance. SUMMARY OF THE INVENTION

[0004] In view of the above-mentioned shortcomings of the prior art, the purpose of this application is to provide a porous composite elastic body, silicon carbon, and a manufacturing method and application thereof.

[0005] To achieve the above and other related objectives, the present invention is manufactured by including the following technical solutions:

[0006] A first aspect of the present application provides a porous composite elastic body with a porous structure, comprising a flexible body and a rigid body that interpenetrate each other. The raw material of the flexible body includes carbon nanotubes, and the rigid body is hard carbon.

[0007] In any embodiment of the present application, the porous composite elastic body includes uniformly distributed micropores and / or mesopores.

[0008] In any embodiment of the present application, the mass ratio of the flexible body to the rigid body is (0.01 to​​​ 2):1. Preferably, the mass ratio of the flexible body to the rigid body is (0.8~1.2): It is 1.

[0009] In any embodiment of this application, the average pore size of the porous composite elastic material is <15 nm The wavelength is preferably 1.8 to 10 nm.

[0010] In any embodiment of this application, the total pore volume of the porous composite elastic body is 0.2 to 1 0.5cm 3 The density is / g, preferably 0.4 to 1.1 cm 3 It is / g.

[0011] In any embodiment of this application, the specific surface area of ​​the porous composite elastic body is >200 m². 2 It is / g, preferably >700m 2 It is / g.

[0012] In any embodiment of this application, D of the porous composite elastic body 50 It is <30 μm. Preferably, it is <20 μm.

[0013] In any embodiment of this application, the tap density of the porous composite elastic body is 0.1 to 1 0.0g / cm 3 The concentration is preferably 0.2 to 0.7 g / cm³. 3 That is the case.

[0014] In any embodiment of this application, the resistivity of the porous composite elastic body is <5Ω·cm. Yes, preferably <0.5Ω·cm, and more preferably <0.05Ω·cm.

[0015] In any embodiment of this application, the pore size concentration of the porous composite elastic material is <7. Preferably, it is between 0.5 and 5.

[0016] A second aspect of this application provides a method for manufacturing the above-mentioned porous composite elastic body, the method comprising: The process involves molding carbon nanotubes to produce carbon nanotube aggregates. Step S1 of manufacturing the Bonn nanotube aggregate, Carbon nanotube aggregates are added to a solution containing a soft template and a polymer. The solution is then permeated into the carbon nanotube aggregates and heat-treated to remove the carbon nanotube aggregates. Step S2 of the manufacturing process for carbon nanotube composite carbon materials involves obtaining a composite carbon material, By carbonizing carbon nanotube composite carbon materials, porous composite elastic materials are obtained. The process includes step S3 of manufacturing a porous composite elastic body.

[0017] In any embodiment of this application, step S1 is performed using a molding machine. Preferably, the main machine frequency of the molding machine is 5-60Hz, and the sub-machine frequency is The frequency is 20-90Hz, the blower is 8-30Hz, and the operating time is 2-100 min. ru.

[0018] In any embodiment of this application, in step S1, the carbon nanotube The length ranges from 0.1 to 50 μm, and the tube diameter ranges from 2 to 20 nm.

[0019] In any embodiment of this application, in step S1, the carbon nanotube aggregate Group D 50 The size is 1 to 100 μm.

[0020] In any embodiment of this application, in step S1, the carbon nanotube aggregate The aggregate has a yarn-ball-like structure. Preferably, the carbon nanotube aggregate after molding is spherical. Alternatively, they are approximately spherical, and the sphericity of carbon nanotube aggregates Sh10% is ≥0.70. Yes, the sphericity of Sh50% is ≥0.80, and the sphericity of Sh90% is ≥0.85.

[0021] In any embodiment of this application, between step S1 and step S2, carbon The tube aggregates are added to an acidic solution, stirred, and then filtered to obtain a solid until neutral. An intermediate modification process was performed to obtain modified carbon nanotube aggregates by washing and drying. It also includes.

[0022] In any embodiment of this application, the mass of carbon nanotube aggregates and acidic solution The ratio is (0.1~100):1.

[0023] In any embodiment of this application, the acidic solution is one of nitric acid, sulfuric acid, and hydrochloric acid. One or more of these will be selected.

[0024] In any embodiment of this application, the reaction temperature during stirring is 30 to 100°C, and the stirring The reaction time is 2 to 12 hours.

[0025] In any embodiment of this application, washing is performed using pure water, and drying is performed in an oven. The drying process is carried out at a temperature of 60-100°C and a drying time of 2-48 hours.

[0026] In any embodiment of this application, in step S2, the monomer of the polymer is of the formula Select from I: [ka] Here, A1 is selected from benzene rings substituted with X, OH, NH2, or X, OH, NH2. is selected, X is selected from halide ions of F, Cl, Br and I, R1, R2, R 3 are each independently at least one selected from H, unsubstituted or substituted phenyl group, unsubstituted or substituted C1-C 20 alkyl group, unsubstituted or substituted C1-C 20 alkoxyl group; the substituent in the substituted phenyl group, the substituent in the substituted C1-C alkyl group, and the substituent in the substituted C1-C 20 alkoxyl group are each independently at least one selected from halogen atom, OH or NH2. The polymer is one or more selected from polyethylene glycol, aqueous polyurethane, polyvinyl alcohol, polyvinylidene fluoride, fluorinated copolymer, polyimide, polyacrylic acid, polyacrylate, polymethyl methacrylate, phenolic resin, epoxy resin, or ionic resin. 20

[0027] In any embodiment of the present application, in step S2, the soft template is selected from nonionic surfactant or ionic surfactant; preferably, the nonionic surfactant is selected from polyoxyethylene-polyoxypropylene copolymer, and the ionic surfactant is selected from hexadecyltrimethylammonium bromide and / or sodium dodecyl sulfonate.

[0028] In any embodiment of the present application, in step S2, the mass ratio of carbon nanotube aggregates to the polymer is (0.1-10):1. Preferably, the mass ratio of the carbon nanotube aggregates to the polymer is 1:3.

[0029] ​​​​​​​ In any embodiment of this application, step S2 contains the solids of the polymer in the solution. The content ranges from 20% to 100%.

[0030] In any embodiment of this application, step S2 involves the carbon nanotubes in solution. Infiltration into aggregates occurs under negative pressure conditions, which range from -0.9 to -0.01. The pressure is in MPa, and the negative pressure time is 0.5 to 10 hours. After the negative pressure treatment, a positive pressure treatment is further included. The positive pressure conditions are 0.15 to 2 MPa, and the holding time is 0.5 to 48 hours.

[0031] In any embodiment of this application, in step S2, after heat treatment, the solvent is further evaporated. It is necessary to do this, thereby obtaining a carbon nanotube composite carbon material, and the heat treatment temperature The temperature is 80-200°C, and the heat treatment time is 0.5-50 hours.

[0032] In any embodiment of this application, in step S3, the carbonization treatment is performed by carbon This involves reacting a notube composite carbon material at high temperatures under a protective gas.

[0033] In any embodiment of this application, the protective gas in the carbonization treatment is nitrogen gas, neon gas Choose one or more of the following gases: argon, krypton, xenon, or radon. The selected protective gas flow rate is 1-20 L / min.

[0034] In any embodiment of this application, the temperature of the high-temperature reaction is 500 to 1000°C. The reaction time is 1 to 30 hours, and the heating rate is 1 to 10°C / min.

[0035] In any embodiment of this application, a post-treatment step is taken, in which the temperature is lowered to room temperature after the high-temperature reaction. Includes further steps.

[0036] A third aspect of this application is a material in which the raw material includes the aforementioned porous composite elastic body and nanosilicon. We provide silicon carbon, including particles.

[0037] In any embodiment of this application, the nanosilicon particles are in the porous composite elastic body The embedded silicon carbon contains uniformly distributed micropores and / or mesopores. ru.

[0038] In any embodiment of this application, the specific surface area of ​​the silicon carbon is <20 m². 2 / g be.

[0039] In any embodiment of this application, the silicon carbon D 50 It is <20 μm. The tap density of silicon carbon is 0.5-2 g / cm³. 3 That is the case.

[0040] In any embodiment of this application, the content of the nanosilicon particles is silicon carbon It is 30-70% of the total mass. The resistivity of the silicon carbon is <20 Ω·cm.

[0041] In any embodiment of this application, the silicon carbon has a specific capacity of >1200mAh The values ​​are / g, the initial Coulomb efficiency is >89%, and the capacity retention rate after 500 cycles is >8 The percentage is 5%, and the 4C / 1C rate characteristic is >90%.

[0042] A fourth aspect of this application provides a method for producing the aforementioned silicon carbon, the method being porous By growing a composite elastic material and a silicon source-containing gas in a vapor phase under high-temperature conditions, silicon carbon This includes the step of obtaining the element.

[0043] In any embodiment of this application, the high-temperature environment is a deposit furnace, and the high temperature is 30 The temperature range is 0 to 600°C, the holding time is 1 to 50 hours, and preferably the internal pressure of the deposition furnace is 5 The pressure is maintained at approximately 10 MPa, and the heating rate is 1-5°C / min.

[0044] In any embodiment of this application, the silicon source gas is monosilane, disilane, dik One or more of lorosilane and trichlorosilane are selected, and the carbon source gas is decomposition temperature It is selected from alkane gases whose temperature is 600°C or lower.

[0045] In any embodiment of this application, the silicon-containing raw material gas also includes a carbon source gas. .

[0046] In any embodiment of this application, the vapor phase growth time is 1 to 50 hours. Preferably The time required for vapor phase growth is 10 to 30 hours.

[0047] In any embodiment of this application, the silicon source containing gas is only the silicon source gas. In this case, the gas flow rate is 1-20 L / min. In any embodiment of this application, the silicon source-containing gas is a silicon source gas and a carbon source gas When including silicon, the volume ratio of the silicon source gas should be 70-99% based on the total volume of the gas. Yes, the volume ratio of the carbon source gas is 1-30%, and the gas flow rate is 5-20 L / min.

[0048] A fifth aspect of this application relates to the aforementioned silicon carbon and carbon coated on the surface of the silicon carbon. A carbon-coated silicon carbon is provided, including a coating layer.

[0049] In any embodiment of this application, the carbon coating amount of carbon-coated silicon carbon is 0.5 to 1 It is 0 wt%. Preferably, the carbon coating amount of carbon-coated silicon carbon is 0.5 to 5 wt%. be.

[0050] In any embodiment of this application, the median particle size D of carbon-coated silicon carbon 50 is <2 It is 0 μm.

[0051] In any embodiment of this application, the silicon content of the carbon-coated silicon carbon is 20 It is approximately 80 wt%.

[0052] In any embodiment of this application, the specific surface area of ​​the carbon-coated silicon carbon is 0.5 to 20 .0m 2 It is / g.

[0053] In any embodiment of this application, the compaction density of the carbon-coated silicon carbon powder is 0.5~ 2 g / cm³ 3 That is the case.

[0054] A sixth aspect of this application involves introducing a mixed gas containing a protective gas and a carbon source gas, and then... The process includes forming carbon-coated silicon carbon by coating it with silicon carbon. The present invention provides a method for producing carbon-coated silicon carbon as described above.

[0055] In any embodiment of this application, the carbon source gas is an alkane with a decomposition temperature of 600°C or lower. Selected from similar gases.

[0056] In any embodiment of this application, the protective gas is nitrogen gas, neon gas, or argon gas. One or more of the following gases are selected: krypton gas, xenon gas, or radon gas.

[0057] In any embodiment of this application, the volume of the carbon source gas is measured based on the total volume of the mixed gas. The volume ratio is 60-80%, and the volume ratio of the protective gas is 20-40%. The flow rate is 0.1 to 50 L / min, preferably 5 to 20 L / min.

[0058] A seventh aspect of this application is a material in which the raw material is the aforementioned porous composite elastic body, the aforementioned silicon carbon, and This provides a silicon-carbon composite anode material containing the aforementioned carbon-coated silicon carbon.

[0059] An eighth aspect of this application is the aforementioned porous composite elastic body, the aforementioned silicon carbon, and the aforementioned carbon coating. Applications of silicon-carbon covering, or the aforementioned silicon-carbon composite anode material, in the manufacture of battery products To provide.

[0060] A ninth aspect of this application is a material in which the raw material is the aforementioned porous composite elastic body, the aforementioned silicon carbon, and Lithium ions containing the carbon-coated silicon carbon described above, or the silicon-carbon composite anode material described above. We provide batteries.

[0061] Compared to the prior art, the beneficial effects of this application are as follows:

[0062] Firstly, in this application, carbon nanotubes and hard carbon are used as carbon sources, and silicon By compounding with , a silicon-carbon composite material is manufactured, and compared with conventional silicon-carbon composite materials... Carbon nanotubes function as bridges between silicon and hard carbon, Effectively improves conductivity and ion conduction energy, thereby enhancing the rate characteristics of the negative electrode material. To improve.

[0063] Secondly, this application describes how to construct a macroporous material using carbon nanotubes in the shape of a ball of yarn. This creates an orderly structure of micro-mesopore carbon with appropriate hardness, and furthermore, micro-meso The pores contain elemental nanosilicon with high hardness. High-strength ordered micro-mesoporous carbon Because it belongs to the hard carbon category, it provides high strength to the composite material, and the negative electrode material during electrode plate manufacturing This significantly reduces the risk of crushing during the roll press process, improving the manufacturing safety of electrode plates. On the other hand, flexible carbon nanotubes can impart a certain degree of elasticity and extensibility to composite materials. Furthermore, it prevents the composite material from detaching from the electrode plate due to volume expansion during the charging and discharging process, and also prevents the electrical... This can avoid the problem of a rapid decline in the pond's cyclical characteristics.

[0064] Thirdly, this application describes how to form pores using a soft template method and a simple heating process Pore ​​formation can be achieved using only this method, and compared to conventional techniques for pore formation by activation, many The process for producing porous carbon has been significantly simplified. [Brief explanation of the drawing]

[0065] [Figure 1] This is a schematic diagram illustrating the manufacturing process of silicon carbon in this application. [Figure 2] This is an SEM image of the CNT aggregates in this application. [Figure 3] This is an SEM image of the CNT composite carbon material in this application. [Figure 4] This is an SEM image of the porous composite elastic material in this application. [Figure 5] This is an SEM image of silicon carbon in this application. [Modes for carrying out the invention]

[0066] To further clarify the purpose, technical proposal, and beneficial effects of this application, please refer to the following examples. The present application will be further described below. The described embodiments are merely illustrative of the present application. It should be understood that this is for the purpose of [specific purpose], and not to limit the scope of the application. The experimental methods used in the examples are all general methods unless otherwise specified. Yes, and those skilled in the art will know of other advantages and effects of this application based on what is disclosed herein. It can be easily understood.

[0067] The “scope” disclosed in this application is limited in the form of a lower and upper limit, and the given scope is one It is limited by selecting two lower limits and one upper limit, and the selected lower and upper limits are The boundaries of a specific range were defined. This defined range may or may not include the endpoints. It may be any combination, and any lower bound is any By combining it with an upper limit, a range can be formed. For example, for a specific parameter In contrast, if the ranges 60-120 and 80-110 are listed, then 60-110 and 8 It can also be understood as a range of 0 to 120. 1 and 2 are listed, and 3, 4, and 5 are listed as the maximum range values. If so, all ranges from 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4, and 2 to 5 are possible. In this application, unless otherwise stated, the numerical range "a to b" is not a. This is a shortened representation of all combinations of real numbers between a and b, where a and b are both real numbers. It is a number. For example, the numerical range "0 to 5" means all real numbers between "0 to 5" in this specification. It means that it is stopped up, and "0-5" is an abbreviated representation of combinations of these numbers. It is not merely that. Also, if we express that a certain parameter is an integer ≥ 2, then this parameter is an example For example, it is revealed that the integers are 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc. This is equivalent to saying that.

[0068] The embodiments of the present invention will be described below through specific examples, and those skilled in the art will be able to follow this specification. Based on the contents disclosed in this document, other advantages and effects of the present invention can be easily understood. The present invention may also be implemented or applied by other different specific embodiments. Each detail in the specifications may deviate from the spirit of the invention based on different perspectives and applications. Various modifications or changes may be made without any prior authorization.

[0069] Before further describing specific embodiments of the present invention, the scope of protection of the present invention is as follows: It should be understood that this invention is not limited to any specific embodiment. The terms used are for the purpose of describing specific embodiments and do not represent the scope of protection of the present invention. This does not restrict the scope. The following examples do not specify concrete conditions for experimental methods. Therefore, it is generally carried out according to conventional conditions or conditions proposed by each manufacturer.

[0070] Unless otherwise defined, all technical and scientific terms used in this invention are the same as those used in this invention. It has the same meaning as generally understood by the person. Specific methods used in the examples, In addition to the apparatus and materials, the present invention is based on the prior art acquired by those skilled in the art and the description of the present invention. Any prior art method, apparatus, or materials similar or equivalent to those described in the examples may be used. The present invention can be realized using the specified materials.

[0071] The inventors of this application, after extensive consideration and research, have found that high cycle and high rate characteristics We have found a silicon-carbon composite anode material having and a method for manufacturing the same. In this application, first we have found a silicon-carbon composite anode material having Bon nanotubes are wound around yarn-ball-like microspheres or microsphere-like structures having ultra-large pores. Carbon nanotubes are interconnected, maximizing their ion conduction and electrical conductivity. This can be guaranteed. Next, using a polymer carbon source material mixed with a soft template The yarn ball-shaped, sparse macropores are filled, and after low-temperature curing, high-temperature carbonization, and pore formation, the CNTs are formed. A sequential micro / mesoporated carbon skeleton is formed, and then silicon is added to this substrate skeleton by CVD. A silicon-carbon composite anode material was fabricated by vapor phase growth. The material is a carbon nanotube. Because it is rich in ions, it has excellent ion and electron transport properties. The material is flexible. By using carbon nanotubes as a base material and filling them with amorphous carbon material, the strength of the composite structure is increased. It can be guaranteed to a certain extent, and by high-temperature carbonization, pores can be formed in amorphous carbon using a template. This process is carried out to obtain a CNT ordered porous carbon composite material, and then a CVD method is applied to this ordered porous material. By growing silicon in the vapor phase, it is possible to ensure the uniform compounding of individual silicon particles. can.

[0072] A first aspect of this application is a porous structure comprising a flexible body and a rigid body that penetrate each other. A porous composite elastic body is provided, wherein the raw material of the flexible body contains carbon nanotubes, and the rigid The body contains hard carbon. Here, the mass ratio of the flexible body to the rigid body is (0.01~2): The answer is 1. Specifically, (0.01~0.5): 1, (0.5~1.0): 1, (1.0~ The ratio may be 1.5):1 or (1.5~2.0):1, etc. Preferably, the flexible body The mass ratio between the rigid body and the rigid body is (0.8~1.2):1. In the specific embodiment of this application, The length of the carbon nanotubes is 0.1 to 50 μm, specifically 0.1 to 1 μm. , 1-10 μm, 10-20 μm, 20-30 μm, 30-40 μm, or 40-50 μm It may also be m, etc. The tube diameter is 2 to 20 nm, specifically 2 to 10 nm, 10 to 1 The carbon nanotube aggregate D 50 The range is 1 to 100 μm, specifically 1 to 10 μm, 10 to 50 μm, or 50 to 10 0 μm is also acceptable.

[0073] The porous composite elastic material provided in this application has uniformly distributed micropores and / or mesopores. It includes. The average pore size of the porous composite elastic material is <15 nm, preferably 1.8 to 1 It is 0 nm. The total pore volume is 0.2–1.5 cm³. 3 The value is / g, preferably 0.4 to 1. 1cm 3 The value is / g. The specific surface area of ​​a porous composite elastic material is >200m². 2 / g, preferably >700m 2 It is / g, more preferably 600~1200m 2 It is / g. Porous composite projectile Sexual body D 50 The thickness is <30 μm, preferably <20 μm, and more preferably 4-8 μm. The value is m. The tap density of the porous composite elastic material is 0.1 to 1.0 g / cm³. 3 And preferably is 0.2~0.7 g / cm³ 3 The resistivity of the porous composite elastic material is <5Ω·cm. Preferably, the impedance is <0.5 Ω·cm, and more preferably, <0.05 Ω·cm. The pore size concentration of the composite elastic material is <7, preferably 0.5 to 5, and the pore size concentration = (V 90 -V 10 ) / V 50 And here, V 10 This means that the percentage of pore volume distribution reaches 10%. This refers to the corresponding pore size when V is used. 50 This refers to the point when the percentage of pore volume distribution reaches 50%. This refers to the pore diameter corresponding to V 90 This corresponds to the point when the percentage of pore volume distribution reaches 90%. This refers to the pore size.

[0074] A second aspect of this application provides a method for manufacturing the above-mentioned porous composite elastic body, the method comprising: The process involves molding carbon nanotubes to produce carbon nanotube aggregates. Step S1 of manufacturing the Bonn nanotube aggregate, Carbon nanotube aggregates are added to a solution containing a soft template and a polymer. The solution is then permeated into the carbon nanotube aggregates and heat-treated to remove the carbon nanotube aggregates. Step S2 of the manufacturing process for carbon nanotube composite carbon materials involves obtaining a composite carbon material, By carbonizing carbon nanotube composite carbon materials, porous composite elastic materials are obtained. The process includes step S3 of manufacturing a porous composite elastic body.

[0075] In any embodiment of this application, step S1 is to shape carbon nanotubes The production of carbon nanotube aggregates refers to the production of carbon nanotube aggregates. vinegar.

[0076] In the manufacturing method provided in this application, step S1 is performed using a molding machine Preferably, the main machine frequency of the molding machine is 5 to 60 Hz, specifically 5 The frequency can be ~10Hz, 10~20Hz, or 20~60Hz, and the sub-unit frequency is The frequency range is 20-90Hz, specifically 20-30Hz, 30-50Hz, or 50-90Hz. It can also be z, and the blower is 8-30Hz, specifically 8-10Hz, 10- The frequency can be 20Hz, or 20-30Hz, and the operating time is 2-100 minutes. Specifically, such as 2-10 min, 10-50 min, or 50-100 min. That's good too.

[0077] In the manufacturing method provided in this application, in step S1, the carbon nanotubes The length ranges from 0.1 to 50 μm, specifically 0.1 to 1 μm, 1 to 10 μm, and 10 to 2 μm. 0 μm, 20-30 μm, 30-40 μm, or 40-50 μm may also be acceptable. The diameter is 2-20 nm, specifically 2-10 nm, 10-15 nm, or 15-20 nm. The median particle size D of the carbon nanotube aggregate may be m or the like. 50 1-10 It is 0 μm, and specifically, 1-10 μm, 10-50 μm, or 50-100 μm, etc. It may be present. The carbon nanotube aggregates after molding have a yarn-ball-like structure. Preferably The carbon nanotube aggregates after molding are spherical or approximately spherical, and the carbon nanotubes The sphericity of the tube aggregates is ≥0.70 for 10% Sh and ≥0.80 for 50% Sh. Yes, the sphericity Sh90% is ≥0.85, where the sphericity Sh10% is the particle size distribution. This refers to the degree of sphericity corresponding to a percentage of 10%, where a sphericity of 50% corresponds to a percentage of 10% of the particle size distribution. This refers to the degree of sphericity corresponding to when the fraction reaches 50%, and a sphericity of 90% is a percentage of the particle size distribution. This refers to the degree of sphericity corresponding to when the rate reaches 90%.

[0078] In the manufacturing method provided in this application, between step S1 and step S2, carbon Nanotube aggregates are added to an acidic solution, stirred under reflux, and then filtered to obtain a solid, which is then neutralized. An intermediate modification process is performed to obtain modified carbon nanotube aggregates by washing and drying them. The principle further includes the following: Here, the mass ratio of the carbon nanotube aggregate to the acidic solution is ( 0.1 to 100: 1, specifically (0.1 to 10): 1, (10 to 50): 1. Alternatively, a ratio such as (50-100):1 may also be used.

[0079] In the manufacturing method provided in this application, the acidic solution is nitric acid, sulfuric acid, and hydrochloric acid. One or more combinations of these are selected. The reaction temperature for stirring is 30-100°C. Specifically, the temperature may be 30-40°C, 40-50°C, or 50-100°C, and stirring may be performed. The reaction time for mixing is 2 to 12 hours, specifically 2 to 4 hours, 4 to 8 hours, or 8 to 12 hours. It may also be done. Washing is done using pure water, and drying is done in an oven. The temperature is 60-100°C, specifically 60-70°C, 70-80°C, or 80-1 The temperature can be 00°C or similar, and the drying time is 2 to 48 hours, specifically 2 to 12 hours, 1 The intermediate modification process can be 2-24 hours or 24-48 hours. This involves modifying the tube aggregates, and the modified carbon nanotube aggregates contain carbon Xyl groups, amino groups, and other groups are formed, and carboxyl groups are formed by modification. The polymer can support -NH2 or -OH groups, and the support is achieved through chemical bonding or physical bonding. This is done by joining.

[0080] In the manufacturing method provided in this application, step S2 is a carbon nanotube aggregate The solution is added to a solution containing a soft template and polymer, and the solution is then filled with carbon nanotubes. The carbon nanotube composite carbon material is obtained by impregnating it into aggregates and then heat-treating it. This refers to the manufacturing of nanotube composite carbon materials.

[0081] The manufacturing method provided in this application uses a polymer having a specific group to produce carbon The tubular aggregates require intermediate modification, which chemically alters the polymer. They fill the pores of the spherical aggregate of carbon nanotubes through bonding or hydrogen bonding. To ensure this is done, if intermediate modification is required, the monomer of the polymer used will be selected from formula I. To be done: [ka] Here, A1 is selected from benzene rings substituted with X, OH, NH2, or X, OH, NH2. X is selected from the halide ions of F, Cl, Br and I, and R1, R2, R 3 independently consists of H, an unsubstituted or substituted phenyl group, and an unsubstituted or substituted C1-C1. 20 Alkyl, unsubstituted or substituted C1-C 20 At least one selected from alkoxyl groups The substituents on the substituted phenyl group, and the substituted C1-C 20 In alkyl groups substituents, and substituted C1-C 20 The substituents on the alkoxyl group are independent of each other. and at least one selected from halogen atoms, OH, or NH2. The polymer It is polyethylene glycol, aqueous polyurethane, polyvinyl alcohol, polyfluoride Nylidene, fluoride copolymer, polyimide, polyacrylic acid, polyacrylic acid ester, Selected from methyl methacrylate, phenolic resin, epoxy resin, or ionic resin. There is one or more. Preferably, the fluorinated copolymer is 1,1-difluoroethylene and Selected from copolymers with xafluoropropylene.

[0082] In the manufacturing method provided in this application, in step S2, phenol is used as the polymer. If you select one or more of the following: resin, epoxy resin, or ion exchange resin, intermediate modification Treated carbon nanotube aggregates, or untreated carbon nanotubes Tube aggregates can be selected, and the polymer here is carbonized by a curing action. It can be used to fill the pores of tube aggregates.

[0083] In the manufacturing method provided in this application, in step S2, the soft template is A nonionic surfactant or an ionic surfactant is selected, preferably the nonionic surfactant. The surfactant is selected from polyoxyethylene-polyoxypropylene copolymers. The ionic surfactant is hexadecyltrimethylammonium bromide and / or dodecyl Selected from sodium sulfonate, and more preferably the nonionic surfactant is From reagents such as F108, F127, F68, or Pluronic Selected.

[0084] In the manufacturing method provided in this application, in step S2, the carbon nanotubes The mass ratio of aggregates to polymer is (0.1~10):1, specifically (0.1~1) :1, (1-5):1, or (5-10):1, etc. One preference of this application In this particular example, the mass ratio of carbon nanotube aggregates to polymer is 1:3.

[0085] In the manufacturing method provided in this application, step S2 is the solidification of the polymer in the solution. The morphological content is 20-100%, specifically 20-30%, 30-50%, or 50%. A percentage like ~100% is also acceptable.

[0086] In the manufacturing method provided in this application, step S2 involves the carbon nanotubes of the solution. Infiltration into the aggregates occurs under negative pressure conditions, which range from -0.9 to -0.0 1 MPa, specifically -0.9 to -0.1 MPa, -0.1 to -0.05 MPa, Alternatively, -0.05 to -0.01 MPa may be used. The negative pressure duration is 0.5 to 10 hours. Specifically, this could be 0.5-1 hour, 1-2 hours, or 2-10 hours. (Negative pressure treatment) Furthermore, a positive pressure treatment is included, with positive pressure conditions of 0.15 to 2 MPa and a holding time of 0.5 The holding time is approximately 48 hours. Preferably, the positive pressure conditions are 0.6 to 1 MPa, and the holding time is 2 to 12 hours. It is h.

[0087] In the manufacturing method provided in this application, in step S2, the heat treatment temperature is 80-2 It is 00℃, specifically 80~100℃, 100~150℃, or 150~200℃. Any is acceptable. The heat treatment time is 0.5 to 50 hours, specifically 0.5 to 1 hour, 1 It could also be ~5 hours, or 5~50 hours, etc.

[0088] In the manufacturing method provided in this application, step S3 is carbon nanotube composite carbon The manufacturing method for porous composite elastic materials involves carbonizing the raw materials to obtain a porous composite elastic material. It refers to construction.

[0089] Here, the carbonization process involves reacting carbon nanotube composite carbon materials at high temperatures under a protective gas. This includes carbonization to form pores. The protective gas used in the carbonization process is nitrogen gas, neon gas. Choose one or more of the following gases: argon, krypton, xenon, or radon. The selected protective gas flow rate is 1-20 L / min, specifically 1-10 L / min. It may also be 10-15 L / min or 15-20 L / min. Carbonization and The temperature for pore formation is 500-1000°C, specifically 500-700°C, 700-800°C. The temperature may be 00°C or 800-1000°C, etc. The time for carbonization and pore formation is 1-3 It can be 0h, or more specifically, 1-10h, 10-15h, or 15-30h, etc. The heating rate is 1-10°C / min, specifically 1-3°C / min and 3-5°C / min. The temperature can be in, or 5-10°C / min. After the high-temperature reaction, the temperature is cooled to room temperature. This further includes the post-processing step.

[0090] The porous composite elastic material has a sponge-like shape, and its pores are uniformly distributed. The reason why pores can be formed in S3 is that after high-temperature carbonization treatment, carbon nanotubes... The polymer in the composite carbon material undergoes thermal decomposition to become hard carbon, and carbon nanotube condensation occurs. By filling the voids in the aggregate, hard carbon and carbon nanotubes penetrate each other. A composite elastic body is formed, and further, in a high-temperature carbonization process, the polymer is thermally decomposed. Gas is generated, which creates pores inside and on the surface of the composite elastic material, resulting in a porous structure. This is because a composite elastic body is obtained. The uniform distribution of pores in this step is due to temperature and It is determined by the heating rate. This technology uses a soft template method to form pores. Pore ​​formation can be achieved with only a simple heating process, unlike conventional pore formation by activation. Compared to other technologies, this significantly simplifies the manufacturing process of porous carbon.

[0091] A third aspect of this application is a material in which the raw material includes the aforementioned porous composite elastic body and nanosilicon. We provide silicon carbon, including particles.

[0092] In the silicon carbon provided in this application, nanosilicon particles are the porous composite elastic body Embedded therein, the silicon carbon contains uniformly distributed micropores and / or mesopores. The specific surface area of ​​silicon carbon is <20m². 2 The total pore volume of the silicon carbon is / g. is <0.05m 2 The D of silicon carbon is / g. 50 The thickness is <20 μm, preferably The tap density is 100 nm to 12 μm. The tap density of the silicon carbon is 0.5 to 2 g / cm³. 3 That is the case.

[0093] In the silicon carbon provided in this application, the content of nanosilicon particles is silicon carbon It is 30-70% of the total mass of the material. Silicon carbon has a specific capacity of >1200mAh / g. Furthermore, the initial Coulomb efficiency is >89%, and the capacity retention rate after 500 cycles is >85%. Furthermore, the 4C / 1C rate characteristic is >90%. C indicates the charge / discharge rate of the battery. It is used for the following purposes. 1C indicates the current strength when the battery is completely discharged in 1 hour, and 4C indicates the current strength when the battery is This indicates the current intensity when the battery is completely discharged in one-quarter of an hour.

[0094] A fourth aspect of this application provides a method for producing the aforementioned silicon carbon, the method being porous By growing a composite elastic material and a silicon source-containing gas in a vapor phase under high-temperature conditions, silicon carbon This includes the step of obtaining the element. Here, the high-temperature environment is a deposit furnace, and the high temperature is 300°C. 600°C, specifically 300-400°C, 400-500°C, or 500-600°C The temperature can be in degrees Celsius or other temperatures, and the incubation time is 1 to 50 hours, specifically 1 to 10 hours, 10 to 2 hours, etc. It may be 0 hours, or 20 to 50 hours, etc. Preferably, the internal pressure of the deposition furnace is 5 to 10 The pressure is maintained at MPa, and the heating rate is 1-5°C / min. The silicon source-containing gas is at high temperature. As it decomposes, atoms such as H and Cl volatilize, and silicon forms nanosilicon particles, creating a porous structure. It is deposited within the pores of the composite elastic material.

[0095] In the method for producing silicon carbon provided in this application, the silicon source gas is monosilane. , selected from one or more of disilane, dichlorosilane, and trichlorosilane, as a carbon source The gas is selected from alkane gases with a decomposition temperature of 600°C or lower, preferably acetylene. Selected from and / or ethylene.

[0096] In the method for producing silicon carbon provided in this application, the silicon source containing gas is silicon If only the source gas is present, the gas flow rate is 1-20 L / min, specifically 1-10 L / It may also be min, 10-15 L / min, or 15-20 L / min, and is preferable. The flow rate is 2-10 L / min. The silicon-containing raw material gas also contains carbon source gases. When the silicon source gas contains both silicon source gas and carbon source gas, the total volume of the gas is used as the basis. The volume ratio of silicon source gas is 70-99%, and the volume ratio of carbon source gas is 1-30%. Yes. The total gas flow rate is 5-20 L / min, specifically 5-10 L / min, 10 It may also be ~15 L / min, or 15~20 L / min, etc. Silicon source containing gas If the gas contains both a silicon source gas and a carbon source gas, the carbon source gas will affect the deposition location of the silicon source gas. This regulates and prevents all the silicon from being deposited within the same pore.

[0097] A fifth aspect of this application relates to the aforementioned silicon carbon and carbon coated on the surface of the silicon carbon. A carbon-coated silicon carbon is provided, including a coating layer.

[0098] In the carbon-coated silicon carbon provided in this application, the carbon-coated silicon carbon composite The carbon coating content in the composite negative electrode material is 0.5 to 10 wt%, preferably 0.5 to 5 wt%. It is t%. The silicon-carbon composite anode material coated with carbon has a median particle size D 50 but <20 It is μm, and specifically, even if it is 4-10 μm, 10-15 μm, 15-20 μm, etc. Often, the silicon content is 20-80 wt%, specifically 20-30 wt%, 30 ~40 wt%, 40~50 wt%, 50~60 wt%, 60~70 wt%, or 70~80 It may also be expressed as wt%, and the specific surface area is 0.5 to 20.0 m². 2 / g, specifically 0 0.5~10.0m 2 / g, 10.0~15.0m 2 / g, or 15.0-20.0m 2 / g It may also be the case that the pore volume is <0.1 cm 3 g -1 The powder compaction density is 0.5-2 g / cm 3 Specifically, 0.5~0.7 g / cm³ 3 , 0.7~0.9 g / cm³ 3 , 0 0.9~1.2g / cm³ 3 , 1.2~1.5 g / cm 3 Or 1.5-2 g / cm³ 3 And so on. That's fine.

[0099] A sixth aspect of this application involves introducing a mixed gas containing a protective gas and a carbon source gas, and then... The process includes forming carbon-coated silicon carbon by coating it with silicon carbon. The present invention provides a method for producing carbon-coated silicon carbon as described above.

[0100] In the manufacturing method provided in this application, the carbon source gas is an alkane with a decomposition temperature of 600°C or lower. A gas is selected, preferably from acetylene and / or ethylene. Protective gas The gases used are nitrogen gas, neon gas, argon gas, krypton gas, xenon gas, and radon gas. One or more of the following are selected. The volume ratio of the carbon source gas is based on the total volume of the mixed gas. The ratio is 60-80%, and the volume ratio of the protective gas is 20-40%. The gas flow rate of the mixed gas is The flow rate is 0.1 to 50 L / min, specifically 0.1 to 10 L / min, 10 to 20 L / It may be min, or 20-50 L / min, and preferably 5-20 L / min n is the value. The role of the mixed gas is to further coat the carbon protective layer.

[0101] A seventh aspect of this application is a material in which the raw material is the aforementioned porous composite elastic body, the aforementioned silicon carbon, and This provides a silicon-carbon composite anode material containing the aforementioned carbon-coated silicon carbon. Using carbon nanotubes and hard carbon as carbon sources, they are compounded with silicon to create silicon We manufacture carbon composite materials and, compared to conventional silicon-carbon composite materials, carbon nanotubes The ribs act as bridges between silicon and hard carbon, thereby improving conductivity and ion transport. This effectively improves the energy conduction, thereby enhancing the rate characteristics of the negative electrode material. The wish is to construct a macroporous material using carbon nanotubes that resemble balls of yarn, and It contains ordered micro-mesopore carbon with a moderate hardness, and the hardness is further enhanced by the micro-mesopores. It contains high-strength elemental nanosilicon. High-strength ordered micro-mesoporous carbon is hard carbon Because it belongs to the group, it gives high strength to the composite material, and the negative electrode material is used in the roll press process during electrode plate manufacturing. This significantly reduces the risk of crushing and improves the manufacturing safety of the electrode plates. On the other hand, flexible carbon nanotubes give composite materials a certain degree of elasticity and extensibility, and charge / discharge over This prevents the composite material from detaching from the electrode plate due to volume expansion during the process, and further enhances the battery's cycle characteristics. This can avoid the problem of a rapid decline in sexual performance.

[0102] An eighth aspect of this application is the aforementioned porous composite elastic body, the aforementioned silicon carbon, and the aforementioned carbon coating. Applications of silicon-carbon covering, or the aforementioned silicon-carbon composite anode material, in the manufacture of battery products To provide.

[0103] A ninth aspect of this application is a material in which the raw material is the aforementioned porous composite elastic body, the aforementioned silicon carbon, and Lithium ions containing the carbon-coated silicon carbon described above, or the silicon-carbon composite anode material described above. We provide batteries.

[0104] The present application will be further described below with reference to examples, but these examples will not cover the scope of this application. It does not restrict anything.

[0105] Example 1 (1) CNT aggregates: Carbon nanotubes with a length of 10 μm and a tube diameter of 5 nm are formed using a molding machine. The molding process is performed with the main machine frequency set to 30Hz, the sub-machine frequency to 60Hz, and the blower frequency to 10Hz. The time was set to 60 min to produce a roughly spherical, yarn-ball-like structural material. Median particle size D 50The diameter is 5.6 μm, and the sphericity Sh 10% is 0.75. 50% is 0.85, sphericity Sh 90% is 0.88, and the average pore size is 38.5n. The value is m, and the pore volume is 1.69 cm³. 3 The specific surface area is 175.8 m² / g. 2 / g Tap density is <0.15 g / cm³ 3 The resistivity is <0.005 Ω·cm.

[0106] (2) Modified CNT aggregates: Carbon nanotubes with a yarn-like structure in a mass ratio of 1:1 Add to a 65% nitric acid solution, react under reflux and stirring at 100°C for 6 hours, and separate by filtration to obtain a solid. After obtaining the result, wash with pure water until neutral, then dry in an oven at 80°C for 10 hours, and modify A refined carbon nanotube aggregate was obtained.

[0107] (3) CNT composite carbon material: CTAB with polyethylene glycol containing 50% solids In addition to the aqueous solution, then polyethylene glycol:modified carbon nanotube aggregates in a mass ratio. Carbon nanotube aggregates modified to a ratio of 1:1 are added to an aqueous solution and stirred. After mixing, the polyethylene glycol aqueous solution was subjected to a -0.50 MPa pressure to form yarn-like aggregates. After evenly penetrating the body and holding pressure for 2 hours to allow the solution to fully permeate, slowly fertilize at 100°C for 5 hours. The solvent is gradually evaporated by heating. The polymer is modified by bonding action. By filling the pores of the notube aggregates, a CNT composite carbon material was obtained.

[0108] (4) CNT porous carbon: CNT composite carbon material is placed in a high-temperature furnace and argon gas is supplied for 10 The material is introduced at a flow rate of L / min and heated to 800°C at a heating rate of 2°C / min for high-temperature carbonization. After pore formation treatment and 10 hours of carbonization, the furnace temperature was allowed to cool naturally to room temperature while maintaining the protective gas. By doing so, a porous carbon nanotube (CNT) with a sponge-like structure and a uniform distribution of pores is produced, that is, A porous elastic composite was obtained. The median particle size D of the porous composite elastic body. 50 It is 6.5 μm, The average pore size is 2.62 nm, and the pore volume is 0.98 cm³. 3 It is / g and the specific surface area is 8 76.7m 2 The values ​​are / g, the pore size concentration is 2.5, and the tap density is 0.33 g / cm³. 3 The resistivity is 0.04 Ω·cm.

[0109] (5) Manufacturing of silicon carbon anode material: The composite material obtained in step (4) is placed in a deposition furnace. After placing it and raising the temperature to 500°C, silicon source gas and carbon source gas (monosilane 70%, A A mixed gas of 30% cetylene is introduced into the deposit reactor at a flow rate of 10 L / min, and the exhaust pipe pressure bar By adjusting the lubricant and continuously introducing gas, silicon carbon was obtained through vapor phase growth for 5 hours. The silicon carbon at this time can be used directly as a silicon carbon composite anode material. Cut.

[0110] As shown in Figure 1, the SEM images of each stage obtained are shown in Figures 2-5. The performance data of the materials at each stage of manufacturing is shown in Table 1.

[0111] [Table 1]

[0112] Example 2 The differences from Example 1 are as follows: A phenolic resin was selected as the polymer. Use.

[0113] (3) Carbon nanotube composite elastic material: CTAB with phenol containing 50% solid content In addition to the resin-ethanol solution, add the following by mass ratio: phenol resin:modified carbon nanotubes Carbon nanotube aggregates modified to have an aggregate ratio of 1:1 are added to the solution. After stirring and mixing, the phenol resin-ethanol solution is formed into a ball-like shape at -0.50 MPa. The solution was uniformly permeated into the aggregates, held under pressure for 2 hours to allow complete penetration, and then allowed to simmer at 120°C for 5 hours. Gently heat and gradually evaporate the solvent. The phenolic resin undergoes curing and bonding processes. By filling the pores of the modified carbon nanotube aggregates, We obtained a nanotube composite elastic material.

[0114] Example 3 The differences from Example 1 are as follows: Polyimide was selected and used as the polymer. ru.

[0115] (3) Carbon nanotube composite elastic material: CTAB with a polyimide containing 50% solids - Add to the NMP solution, then add polyimide:modified carbon nanotube aggregates in a mass ratio of 1: Carbon nanotube aggregates modified to have a ratio of 1 were added to the solution and stirred and mixed. Next, the polyimide-NMP solution was uniformly permeated into the yarn-ball-shaped aggregates under a pressure of -0.50 MPa. After allowing the solution to fully permeate under pressure for 2 hours, gently heat at 120°C for 5 hours to remove the solvent. It is gradually evaporated. The polyimide is modified by hydrogen bonding, resulting in carbon nanotubes. By filling the pores of the spherical aggregates, a CNT composite carbon material was obtained.

[0116] Example 4 The differences from Example 1 are as follows: Epoxy resin was selected as the polymer. In use.

[0117] (3) Carbon nanotube composite elastic body: CTAB was added to an epoxy resin-toluene solution with a solid content of 50% Then, the mass ratio of epoxy resin: carbon nanotube aggregate = 1 :1, the carbon nanotube aggregates were added to the solution, stirred and mixed, and then 12 The epoxy resin-toluene solution was uniformly applied to the yarn ball-shaped aggregate at 0°C and -0.50 MPa After infiltration and holding the pressure for 2 hours to completely infiltrate the solution, it was slowly cooled to room temperature. The epoxy resin is filled into the pores of the modified carbon nanotube aggregate by a curing action. By filling, a CNT composite carbon material was obtained.

[0118] Comparative Example 1 The difference from Example 1 is that step (3) is not performed and the polymer is not complexed. Yes.

[0119] Comparative Example 2 The difference from Example 1 is that step (4) is not performed and no pores are formed. Yes.

[0120] Comparative Example 3 The difference from Example 1 is that steps (1) to (3) are not performed, and the carbon source of the porous carbon is This is to replace the carbon nanotube composite elastic body with a polymer.

[0121] The negative electrode materials produced in each example and each comparative example are assembled into batteries.

[0122] (1) Production of positive electrode plate: Positive electrode active material lithium nickel cobalt manganate (NCM811) ), conductive agent Super P, carbon nanotubes, adhesive polyvinylidene fluoride (PV Mix DF) uniformly with N-methylpyrrolidone (NMP) in a mass ratio of 97:1:0.5:1.5. Combined, a positive electrode slurry (with a solid content of 70 wt%) is manufactured, and the current collector aluminum... The foil is coated on both sides, dried at 100°C, and then cold-pressed at 4 MPa at room temperature. After that, deburring, cutting, slitting, and tab welding are performed to manufacture the positive electrode plate. Ta.

[0123] (2) Manufacturing of the negative electrode plate: Under a protective atmosphere of nitrogen gas, the solvent N-methylpyrrolidone and adhesive Stir the PVDF to mix it uniformly, then add the conductive agent Super P and stir to mix it uniformly. Then, the negative electrode active material is added and thoroughly stirred to mix uniformly, resulting in a negative electrode slurry (containing solids). We manufactured a product with a content of 50 wt%.

[0124] Regarding the negative electrode active material, the silicon carbon composites produced in the above examples and comparative examples were respectively used. The negative electrode material and graphite are used, and the gram capacity of the manufactured negative electrode material is 450 mAh / g. This is obtained by thoroughly and uniformly mixing the ingredients.

[0125] The above negative electrode slurry is applied to both the front and back surfaces of the copper foil current collector, dried at 100°C, and then at room temperature. The material is cold-pressed at 4 MPa, then deburred, cut, slit, and the tabs are welded. Then, the negative electrode plate was manufactured.

[0126] (3) Assembly of lithium-ion batteries A porous polymerized PE film is used as the separator, and the manufactured positive electrode plate, separator, and negative electrode are used. Plates are stacked in order, a separator is placed between the positive and negative electrode plates, and the stack is wound up to obtain a bare cell. The cells are placed in an aluminum plastic shell package, -0.95 × 10 5 Pa phase Dry at 100°C under vacuum pressure until moisture content is 100 ppm or less. Dry bare The electrolyte is injected into the cell, and here the electrolyte is ethylene carbonate (EC) and ethylmethyl Carbonate (EMC), diethyl carbonate (DEC) (EC:EMC:DEC form) Composed of a product ratio of 1:1:1 and LiPF6 (1.0M), packaged, settled, chemical Formation (charging at a constant current of 0.02C for 2 hours, charging at a constant current of 0.1C for 2 hours), molding, capacity testing. (Capacity grading) was performed, and pouch-type liquid lithium-ion batteries were manufactured.

[0127] When assembling the batteries, five batteries are manufactured for each test, for a total of five sets. Test the data and use the average of 5 sets of data as the final performance data.

[0128] We tested the battery's cycle characteristics using Xinwei equipment, specifically, Initial Coulomb efficiency test: Discharge at 0.1C until 0.005V at 25°C, then After that, discharge at 0.08C until the voltage reaches 0.001V, then discharge at 0.05C until the voltage reaches 0.001V. Discharge it at 0.02C until it reaches 0.001V, let it stand for 10 minutes, and then discharge it to 1.5V. Charge at 0.1C until full capacity is reached, leave for 10 minutes, and record the charge / discharge capacity after the first cycle. Calculate the Coulomb efficiency round Cycle capacity retention rate test: Repeat the above method 500 times, 500 cycles The charge / discharge capacity after each cycle was recorded, and the capacity retention rate after 500 cycles was calculated.

[0129] Rate characteristic test: After charging at 1C, discharge with a discharge current of 4C to determine discharge capacity and 1 Test the capacity retention rate at C-rate.

[0130] [Table 2]

[0131] As can be seen from Table 1, in Comparative Example 1, since no polymer is compounded, the data of both the lithium storage specific capacity and the capacity retention rate after 500 cycles of the silicon-carbon negative electrode material are inferior to those of Examples 1 to 4. In Comparative Example 2, since no pores are formed, the lithium storage specific capacity, the initial Coulombic efficiency and the capacity retention rate after 500 cycles are all inferior to those of Examples 1 to 4. In Comparative Example 3, steps (1) to (3) are not performed, and the polymer is directly carbonized to produce porous carbon, and since carbon nanotubes are absent, the conductivity of the negative electrode material decreases, thereby significantly reducing the performance.

[0132] In summary, the present application uses yarn ball-like carbon nanotubes to construct a macroporous material, thereby accommodating ordered micro-mesoporous carbon with moderate hardness, and further accommodates hard elemental nano-silicon through the micro-mesopores. The high-strength ordered micro- mesoporous carbon belongs to hard carbon, which provides high strength to the composite material, greatly reducing the risk of the negative electrode material being crushed in the roll pressing process during electrode plate manufacturing, and improving the manufacturing safety of the electrode plate. On the other hand, the flexible carbon nanotubes provide certain elasticity and extensibility to the composite material, avoiding the composite material from falling off the electrode plate due to volume expansion during the charge and discharge process, and further avoiding the problem of a sharp decrease in the cycle performance of the battery.

[0133] The above examples are only for exemplarily explaining the principles and effects of the present invention, and are not intended to limit the present application. Those skilled in the art can make modifications without departing from the spirit and scope of the present application. ​​​​​The above embodiments can be modified or changed without doing so. Therefore, the technical field A person skilled in the art would be able to complete the invention without departing from the spirit and technical idea disclosed in the present invention. All equivalent modifications or changes made are still included in the claims of this application. Let's assume that.

Claims

1. A porous composite elastic body having a porous structure comprising a flexible body and a rigid body that penetrate each other, wherein the raw material of the flexible body contains carbon nanotubes, the rigid body is hard carbon, the porous composite elastic body contains uniformly distributed micropores and mesopores, the specific surface area of ​​the porous composite elastic body is >700 m² / g, the resistivity of the porous composite elastic body is <5 Ω·cm, the pore diameter concentration of the porous composite elastic body is <7, and the total pore volume of the porous composite elastic body is 0.2 to 1.5 cm³ / g.

2. The porous composite elastic body according to claim 1, characterized in that the mass ratio of the flexible body to the rigid body is (0.01 to 2):

1.

3. a1) The average pore size of the porous composite elastic material is <15 nm. a2) D of the porous composite elastic body 50 The size is <30 μm. a3) The tap density of the porous composite elastic material is 0.1 to 1.0 g / cm³ 3 Being a4) The porous composite elastic body according to claim 2, characterized in that at least one or more of the following are included: the resistivity of the porous composite elastic body is < 5 Ω·cm.

4. a1) The average pore size of the porous composite elastic material is 1.8 to 10 nm. a2) The total pore volume of the porous composite elastic material is 0.4 to 1.1 cm³. 3 / g a3) D of the porous composite elastic body 50 The size is <20 μm. a4) The tap density of the porous composite elastic material is 0.2 to 0.7 g / cm³ 3 Being a5) The resistivity of the porous composite elastic material is < 0.05 Ω·cm. a6) The porous composite elastic body according to claim 3, characterized in that the pore size concentration of the porous composite elastic body is at least one or more of 0.5 to 5.

5. A method for manufacturing a porous composite elastic body according to any one of claims 1 to 4, Step S1 of manufacturing carbon nanotube aggregates involves forming carbon nanotubes to produce carbon nanotube aggregates, Step S2 of the manufacturing of a carbon nanotube composite elastic body involves adding carbon nanotube aggregates to a solution containing a soft template and a polymer, allowing the solution to permeate the carbon nanotube aggregates, and then heating and curing it to obtain a carbon nanotube composite elastic body. A method for producing a porous composite elastic body, comprising step S3 of producing a porous composite elastic body, which involves performing high-temperature carbonization and activation treatment on a carbon nanotube composite elastic body to obtain a porous composite elastic body.

6. In step S1, the molding is performed using a molding machine. And / or, in step S1, the length of the carbon nanotube is 0.1 to 50 μm, and the diameter is 2 to 20 nm. And / or, in step S1, the carbon nanotube aggregate is spherical or approximately spherical, And / or, in step S1, the sphericity Sh10% of the carbon nanotube aggregate is ≥ 0.70, And / or, in step S1, the sphericity Sh50% of the carbon nanotube aggregate is ≥ 0.

80. And / or, in step S1, the sphericity Sh90% of the carbon nanotube aggregate is ≥ 0.

85. And / or, in step S1, the carbon nanotube aggregate D 50 The size is 1 to 100 μm. The manufacturing method according to claim 5, characterized in that, and / or, in step S1, the carbon nanotube aggregate has a yarn-ball-like structure.

7. The manufacturing method according to claim 6, characterized in that the main machine frequency of the molding machine is 5 to 60 Hz, the sub-machine frequency is 20 to 90 Hz, the blower frequency is 8 to 30 Hz, and the operating time is 2 to 100 mins.

8. The manufacturing method according to claim 5, further comprising an intermediate modification treatment between step S1 and step S2, in which carbon nanotube aggregates are added to an acidic solution, stirred, filtered to obtain a solid, washed until neutral, and dried to obtain modified carbon nanotube aggregates.

9. The mass ratio of the carbon nanotube aggregate to the acidic solution is (0.1 to 100):

1. and / or, the acidic solution is selected from one or more of nitric acid, sulfuric acid, and hydrochloric acid. And / or, the reaction temperature during stirring is 30 to 100°C, and the reaction time during stirring is 2 to 12 hours. And / or, washing is carried out using pure water, and drying is carried out in an oven. The manufacturing method according to claim 8, characterized in that the drying temperature is 60 to 100°C and the drying time is 2 to 48 hours.

10. The manufacturing method according to claim 5, characterized in that in step S2, the polymer is one or more selected from polyethylene glycol, aqueous polyurethane, polyvinyl alcohol, polyvinylidene fluoride, fluorinated copolymer, polyimide, polyacrylic acid, polyacrylic acid ester, polymethyl methacrylate, phenolic resin, epoxy resin, or ionic resin.

11. In step S2, the soft template is selected from a nonionic surfactant or an ionic surfactant. And / or, in step S2, the mass ratio of the carbon nanotube aggregate to the polymer is (0.1 to 10):1, And / or, in step S2, the solid content of the polymer in the solution is 20 to 100%, And / or, in step S2, the infiltration of the solution into the carbon nanotube aggregate is carried out under negative pressure conditions. And / or, in step S2, the curing temperature is 80 to 200°C, and the curing time is 0.5 to 50 hours. The manufacturing method according to claim 5, characterized in that, in step S2, the solvent is further evaporated after curing, thereby obtaining a carbon nanotube composite carbon material.

12. In step S2, the nonionic surfactant is selected from a polyoxyethylene-polyoxypropylene copolymer. and / or the ionic surfactant is selected from hexadecyltrimethylammonium bromide and / or sodium dodecylsulfonate. And / or, the negative pressure conditions are -0.9 to -0.01 MPa, and the negative pressure duration is 0.5 to 10 h. And / or, after negative pressure treatment, positive pressure treatment is further included, with positive pressure conditions of 0.15 to 2 MPa and holding time of 0.5 to 48 hours. The manufacturing method according to claim 11, characterized in that and / or the mass ratio of the carbon nanotube aggregate to the polymer is 1:

3.

13. The manufacturing method according to claim 5, characterized in that step S3 includes high-temperature carbonization, in which the carbon nanotube composite carbon material is reacted at a high temperature under a protective gas.

14. The protective gas used in the aforementioned high-temperature carbonization is selected from one or more of the following: nitrogen gas, neon gas, argon gas, krypton gas, xenon gas, and radon gas. and / or, the flow rate of the protective gas is 1 to 20 L / min. And / or, the temperature of the high-temperature reaction is 500 to 1000°C. And / or, the duration of the high-temperature reaction is 1 to 30 hours. And / or, the heating rate of the high-temperature reaction is 1 to 10°C / min. The manufacturing method according to claim 13, further comprising and / or a post-treatment step of lowering the temperature to room temperature after the high-temperature reaction.

15. Silicon carbon, wherein the raw material includes a porous composite elastic body as described in claim 1, and also includes nanosilicon particles embedded in the porous composite elastic body.

16. It includes one or more of the following characteristics: b1) The specific surface area of ​​the silicon carbon is <20 m² 2 / g, b2) The D of the silicon carbon 50 It is <20 μm, b3) The tap density of the silicon carbon is 0.5 to 2 g / cm 3 , and b4) The content of the nanosilicon particles is 30 to 70% of the total mass of silicon carbon. b5) The resistivity of the silicon carbon is <20 Ω·cm, b6) The silicon carbon according to claim 15, characterized in that the silicon carbon has a specific capacity of >1200 mAh / g, an initial Coulomb efficiency of >89%, a capacity retention rate of >85% after 500 cycles, and a 4C / 1C rate characteristic of >90%.

17. A method for producing silicon carbon according to any one of claims 15 to 16, comprising the step of obtaining silicon carbon by vapor-phase growth of a porous composite elastic body and a silicon source-containing gas in a high-temperature environment.

18. The aforementioned high-temperature environment is a deposit furnace, the high temperature is 300 to 600°C, and the holding time is 1 to 50 hours. and / or, the silicon source gas is selected from one or more of monosilane, disilane, dichlorosilane, and trichlorosilane. and / or, the silicon-containing raw material gas also includes a carbon source gas, The manufacturing method according to claim 17, characterized in that and / or the time of vapor phase growth is 1 to 50 hours.

19. The internal pressure of the aforementioned deposition furnace is 5 to 10 MPa, and the heating rate is 1 to 5°C / min. and / or, the carbon source gas is selected from alkane gases having a decomposition temperature of 600°C or less. And / or, if the silicon source gas is only the silicon source gas, the gas flow rate is 1 to 20 L / min. And / or, when the silicon source gas contains both a silicon source gas and a carbon source gas, the volume ratio of the silicon source gas is 70-99% and the volume ratio of the carbon source gas is 1-30% based on the total volume of the gas. And / or, if the silicon source-containing gas includes both a silicon source gas and a carbon source gas, the gas flow rate is 5 to 20 L / min. The manufacturing method according to claim 18, characterized in that and / or the vapor phase growth time is 10 to 30 hours.

20. A carbon-coated silicon carbon comprising the silicon carbon described in claim 15 and a carbon coating layer coated on the surface of the silicon carbon.

21. The carbon coating amount of the carbon-coated silicon carbon is 0.5 to 10 wt%, and / or the median particle size D of the carbon-coated silicon carbon 50 It is <20 μm, and / or, the silicon content of the carbon-coated silicon carbon is 20 to 80 wt%, and / or, the specific surface area of ​​the carbon-coated silicon carbon is 0.5 to 20.0 m². 2 / g, And / or, the compaction density of the carbon-coated silicon carbon powder is 0.5 to 2 g / cm³. 3 The carbon-coated silicon carbon according to claim 20, characterized in that it is such.

22. A method for producing carbon-coated silicon carbon according to any one of claims 20 to 21, comprising introducing a mixed gas containing a protective gas and a carbon source gas and coating silicon carbon with it to form carbon-coated silicon carbon.

23. The carbon source gas is selected from alkane gases with a decomposition temperature of 600°C or lower. and / or, the protective gas is selected from one or more of nitrogen gas, neon gas, argon gas, krypton gas, xenon gas, and radon gas. And / or, the gas flow rate of the mixed gas is 0.1 to 50 L / min. The manufacturing method according to claim 22, characterized in that, and / or, with respect to the total volume of the mixed gas, the volume ratio of the carbon source gas is 60 to 80%, and the volume ratio of the protective gas is 20 to 40%.

24. A silicon-carbon composite anode material comprising a porous composite elastic body according to any one of claims 1 to 4, silicon carbon according to any one of claims 15 to 16, or carbon-coated silicon carbon according to any one of claims 20 to 21.

25. Applications of the porous composite elastic body according to any one of claims 1 to 4, the silicon carbon according to any one of claims 15 to 16, or the carbon-coated silicon carbon according to any one of claims 20 to 21 in the manufacture of battery products.

26. A lithium-ion battery in which the raw material comprises a porous composite elastic body according to any one of claims 1 to 4, silicon carbon according to any one of claims 15 to 16, or carbon-coated silicon carbon according to any one of claims 20 to 21.

Citation Information

Patent Citations

  • Carbon nanotube-containing silicon-carbon composite material as well as preparation method and application thereof

    CN116995206A

  • Hard carbon negative electrode material with multi-layer core-shell structure for sodium ion battery and preparation method of hard carbon negative electrode material

    CN117154029A