Printed circuit board
By aligning copper crystal grains in the (110) direction and controlling grain size, the printed circuit board addresses the adhesion issue between the insulating and copper layers, improving structural integrity through enhanced adhesion.
Patent Information
- Application Number
- JP2026539511
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2026-03-19
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2046-03-19
AI Technical Summary
The adhesion between the insulating layer and the electroplated copper layer in existing printed circuit boards is insufficient, leading to a risk of peeling.
The printed circuit board design includes an electroplated copper layer with crystal grains oriented such that the (110) direction aligns normal to the main surface, and the average grain size is less than 0.2 μm, enhancing the adhesion of the insulating layer by roughening the surface through needle-like crystal grain growth during etching.
This design improves the adhesion between the insulating layer and the electroplated copper layer, effectively preventing peeling and enhancing the structural integrity of the circuit board.
Smart Images

Figure 0007955559000002 
Figure 0007955559000003 
Figure 0007955559000004
Abstract
Description
[Technical Field]
[0001] This disclosure relates to printed circuit boards. [Background technology]
[0002] International Publication No. 2018 / 211733 (Patent Document 1) describes a printed circuit board. The printed circuit board described in Patent Document 1 comprises a base film, wiring, and an insulating layer. The wiring comprises a base conductive layer disposed on the main surface of the base film and an electroplated copper layer disposed on the base conductive layer. The insulating layer is disposed on the main surface of the base film so as to cover the wiring. [Prior art documents] [Patent Documents]
[0003] [Patent Document 1] International Publication No. 2018 / 211733 [Overview of the project]
[0004] The printed circuit board comprises a base film having a main surface, a base conductive layer disposed on the main surface, and an electroplated copper layer disposed on the base conductive layer. The electroplated copper layer contains a plurality of crystal grains. The plurality of crystal grains are oriented such that the (110) direction of the copper crystals aligns with the direction normal to the main surface. In a cross-sectional view perpendicular to the main surface, the average grain size of the plurality of crystal grains in the direction parallel to the main surface is less than 0.2 μm. [Brief explanation of the drawing]
[0005] [Figure 1] This is a first plan view of the printed circuit board 100. [Figure 2] This is a second plan view of the printed circuit board 100. [Figure 3] This is a cross-sectional view taken along line III-III in Figure 1. [Figure 4] This is a schematic diagram illustrating the method for measuring the first average particle size. [Figure 5] This is a manufacturing process diagram for printed circuit board 100. [Figure 6] This is a cross-sectional view illustrating preparation step 50. [Figure 7] This is a cross-sectional view illustrating the process 51 for forming the underlying conductive layer. [Figure 8] This is a cross-sectional view illustrating the resist pattern formation process 52. [Figure 9] This is a cross-sectional view illustrating the electroplating process 53. [Figure 10] This is a cross-sectional view illustrating the resist pattern removal process 54. [Figure 11] This is a cross-sectional view illustrating the etching process 55. [Figure 12] This is a first cross-sectional view of a modified printed circuit board 100. [Figure 13] This is a second cross-sectional view of a modified printed circuit board 100. [Modes for carrying out the invention]
[0006] In the printed circuit board described in Patent Document 1, the adhesion between the insulating layer and the electroplated copper layer is insufficient, and there is a risk that the insulating layer may peel off. This disclosure provides a printed circuit board that can suppress the peeling of the insulating layer.
[0007] First, the embodiments of this disclosure are listed below. (1) The printed circuit board according to the embodiment comprises a base film having a main surface, a base conductive layer disposed on the main surface, and an electroplated copper layer disposed on the base conductive layer. The electroplated copper layer contains a plurality of crystal grains. The plurality of crystal grains are oriented such that the (110) direction of the copper crystals is along the direction normal to the main surface. In a cross-sectional view perpendicular to the main surface, the average grain size of the plurality of crystal grains in the direction parallel to the main surface is less than 0.2 μm. According to the printed circuit board of (1), the adhesion of the insulating layer covering the base conductive layer and the electroplated copper layer is improved.
[0008] (2) In the printed wiring board according to (1), the average grain size of the plurality of crystal grains may be less than 2.4 μm in a cross-sectional view perpendicular to the main surface.
[0009] (3) In the printed wiring board according to (1) or (2), the average aspect ratio of the plurality of crystal grains may be 3.5 or more in a cross-sectional view perpendicular to the main surface.
[0010] (4) In the printed wiring board according to any one of (1) to (3), the standard deviation of the inclination angle of the plurality of crystal grains with respect to the normal direction may be 30° or less in a cross-sectional view perpendicular to the main surface.
[0011] (5) In the printed wiring board according to any one of (1) to (4), the electrolytic copper plating layer may include an upper surface and a side surface. The arithmetic average roughness of the upper surface may be greater than the arithmetic average roughness of the side surface.
[0012] (6) In the printed wiring board according to (5), the arithmetic average roughness of the upper surface may be 0.15 μm or more.
[0013] (7) The printed wiring board according to any one of (1) to (6) may further include an insulating layer. The insulating layer may be disposed on the main surface so as to cover the underlying conductive layer and the electrolytic copper plating layer.
[0014] (8) In the printed wiring board according to (7), the insulating layer may include an adhesive layer and a coverlay disposed on the adhesive layer.
[0015] (9) In the printed wiring board according to (7), the insulating layer may be a solder resist. Next, details of an embodiment of the present disclosure will be described with reference to the drawings. In the following drawings, the same or corresponding parts are denoted by the same reference numerals, and redundant description will not be repeated.
[0016] (Configuration of printed wiring board 100) (Hereinafter, the configuration of the printed wiring board 100 will be described.)
[0017] As shown in Figures 1, 2, and 3, the printed circuit board 100 has a base film 10. The base film 10 has a main surface 11 and a main surface 12. The direction normal to the main surface 11 is defined as the first direction 13. The main surfaces 11 and 12 form the end faces of the base film 10 in the first direction 13. The main surface 12 is the opposite side of the main surface 11 in the first direction 13. The base film 10 is made of a flexible, electrically insulating material. For example, the base film 10 is made of polyimide.
[0018] The printed circuit board 100 has wiring 20 and wiring 21. Wiring 20 is arranged on the main surface 11. Wiring 21 is arranged on the main surface 12. Each of the wirings 20 and 21 extends, for example, in a second direction 14 in a plan view. The wirings 20 are arranged in the second direction 14 with spacing between adjacent wirings 20, and the wirings 21 are arranged in a third direction 15 with spacing between adjacent wirings 21. The third direction 15 is perpendicular to the second direction 14 in a plan view.
[0019] Each of the wirings 20 and 21 has a base conductive layer 30. The base conductive layer 30 is located on the main surface (on the main surface 11 and on the main surface 12) of the base film 10. The base conductive layer 30 has a first layer 31 and a second layer 32. The second layer 32 is located on the first layer 31. Each of the first layer 31 and the second layer 32 is made of, for example, copper or a copper alloy. Each of the wirings 20 and 21 has an electroplated copper layer 33. The electroplated copper layer 33 is located on the base conductive layer 30. The electroplated copper layer 33 is made of copper or a copper alloy.
[0020] The electroplated copper layer 33 has a top surface 34 and a side surface 35. The arithmetic mean roughness on the top surface 34 is defined as the first arithmetic mean roughness, and the arithmetic mean roughness on the side surface 35 is defined as the second arithmetic mean roughness. The first arithmetic mean roughness is greater than the second arithmetic mean roughness. For example, the first arithmetic mean roughness is 0.15 μm or more. The first arithmetic mean roughness is measured using a laser microscope from a direction perpendicular to the main surface 11. The second arithmetic mean roughness is measured using a laser microscope from a third direction 15 after cutting the base film 10 at an arbitrary point parallel to the second direction 14. In each of the above measurements, in accordance with ISO 25178, a VK-X3000 laser microscope manufactured by Keyence Corporation is used to measure the Sdr (interface development area ratio) at 50x magnification at 5 arbitrary points, and the arithmetic mean roughness is calculated by finding the average value of the Sdr at those 5 points. The ratio of the developed area of the interface represents how much the developed area (surface area) of the defined domain increases relative to the area of the defined domain.
[0021] The electroplated copper layer 33 contains multiple crystal grains. Each of the multiple crystal grains extends in a needle-like manner along the first direction 13. More specifically, each of the multiple crystal grains extends such that the (110) direction of the copper crystal aligns with the first direction 13. Even if the (110) direction of the copper crystal is not parallel to the first direction 13, it can still be said that each of the multiple crystal grains extends such that the (110) direction of the copper crystal aligns with the first direction 13. The orientation of the crystal grains in the electroplated copper layer 33 is measured by the following method. Firstly, by performing a wide-angle measurement from a direction perpendicular to the main surface 11 using X-ray diffraction (XRD), the X-ray diffraction intensity in the (111) direction of the copper crystal grain, I, is measured. 111 I is the X-ray diffraction intensity in the (100) direction of the copper crystal grain. 100 and the X-ray diffraction intensity of the copper crystal grain in the (311) direction, I 311 To obtain: Secondly, I 111 , I 100 and I 311The direction of the maximum diffraction intensity is considered to be the orientation direction of the copper crystal grains. The X-ray diffraction method uses EMPYREAN (Malven-Panalytical), with Cu-Kα X-rays used, excitation conditions of 45kV and 40mA, BBHD incident optics, 1 / 4 slit, 10mm mask, 0.27-pixel 3D plane collimator for receiving optics, 2θ-θ scan method, measurement range of 2θ = 30°-130°, and step size of 0.03°.
[0022] In a cross-sectional view perpendicular to the main surface 11, the average grain size (first average grain size) of multiple crystal grains in a direction parallel to the main surface 11 is less than 0.2 μm. The first average grain size may be less than 0.15 μm or less than 0.1 μm. The first average grain size is measured by the following method.
[0023] Firstly, by processing in the third direction 15 using the section polishing method, a cross-section of the electroplated copper layer 33 perpendicular to the second direction 14 is cut out. Secondly, the above cross-section is analyzed by the EBSD (Electron Back Scattered Diffraction) method. Note that areas where the crystal orientation differs by 10° or more are considered to be grain boundaries. For the EBSD analysis, a ZEISS Gemini450 is used as the measuring instrument, and Oxford Symmetry is used as the analysis software. When the EBSD method is performed, the acceleration voltage is set to 15kV, the irradiation current to 10nA, and the EBSD conditions are Binning with speed 2 and sensitivity 2, WD of 15mm, and Tilt of 70°. The observation size is 114μm wide × 17μm high. As shown in Figure 4, thirdly, a measurement line is set on the above cross-sectional image, and the number of grain boundaries intersecting the measurement line is counted. Fourth, the length of the measurement line is divided by the number of grain boundaries that intersect the measurement line, and this value is considered to be the first average grain size.
[0024] In a cross-sectional view perpendicular to the main surface 11, the average grain size (second average grain size) of the multiple crystal grains is, for example, less than 2.4 μm. The second average grain size may be 1.5 μm or less, or 1.0 μm or less. The second average grain size is measured by the following method.
[0025] Firstly, a cross-sectional analysis of the electroplated copper layer 33 perpendicular to the second direction 14 is performed, similar to the measurement of the first average grain size. Secondly, the area of each of the multiple crystal grains is measured on the above cross-sectional image. Thirdly, the equivalent circular diameter of each of the multiple crystal grains is calculated. The equivalent circular diameter of each of the multiple crystal grains is the square root of the value obtained by dividing the area of each of the multiple crystal grains by π / 4. Fourthly, the value obtained by dividing the sum of the equivalent circular diameters of each of the multiple crystal grains by the number of crystal grains is calculated. This value is considered to be the second average grain size.
[0026] In a cross-sectional view perpendicular to the main surface 11, the average aspect ratio of the multiple crystal grains is, for example, 3.5 or greater. The aspect ratio of the multiple crystal grains may be 5 or greater, or 7 or greater. The aspect ratio of the multiple crystal grains is measured by the following method.
[0027] Firstly, a cross-sectional analysis of the electroplated copper layer 33 perpendicular to the second direction 14 is performed, similar to the measurement of the first average grain size. Secondly, the aspect ratio of each of the multiple crystal grains is measured on the above cross-sectional image. The aspect ratio of a crystal grain is the value obtained by dividing the length of the major axis of the elliptically approximated crystal grain by the length of the minor axis. The elliptical approximation of the crystal grain is performed by defining grain boundaries at locations where the crystal orientation difference is 10° or more, and finding the ellipse with the smallest difference between the area of the region enclosed by the grain boundaries and the ellipse. Thirdly, a value is calculated by dividing the sum of the aspect ratios of each of the multiple crystal grains by the number of crystal grains. This value is considered to be the average aspect ratio of the multiple crystal grains.
[0028] In a cross-sectional view perpendicular to the main surface 11, the standard deviation of the inclination angles of multiple crystal grains with respect to the first direction 13 is 30° or less. In a cross-sectional view perpendicular to the main surface 11, the standard deviation of the inclination angles of multiple crystal grains with respect to the first direction 13 may be 25° or less, or 17° or less. The standard deviation of the inclination angles of multiple crystal grains with respect to the first direction 13 in a cross-sectional view perpendicular to the main surface 11 is measured by the following method.
[0029] Firstly, a cross-sectional analysis of the electroplated copper layer 33 perpendicular to the second direction 14 is performed, similar to the measurement of the first average grain size. Secondly, the inclination angle of each of the multiple crystal grains with respect to the first direction 13 is measured on the above cross-sectional image. The inclination angle of the crystal grain with respect to the first direction 13 is the angle between the direction of the major axis of the elliptally approximated crystal grain and the principal surface 11. Thirdly, a frequency distribution of the inclination angles of each of the multiple crystal grains with respect to the first direction 13 is created, and the standard deviation is calculated by performing statistical processing.
[0030] As shown in Figure 3, the printed circuit board 100 has an insulating layer 40 and an insulating layer 41. The insulating layer 40 is placed on the main surface 11 so as to cover the wiring 20. The insulating layer 41 is placed on the main surface 12 so as to cover the wiring 21. Each of the insulating layers 40 and 41 has an adhesive layer 42 and a coverlay 43. The coverlay 43 is placed on the adhesive layer 42. In other words, the coverlay 43 is attached to the base film 10 by the adhesive layer 42.
[0031] (Manufacturing method for printed circuit board 100) The manufacturing method for the printed circuit board 100 is described below.
[0032] As shown in Figure 5, the manufacturing method of the printed circuit board 100 includes a preparation step 50, a base conductive layer formation step 51, a resist pattern formation step 52, an electrolytic plating step 53, a resist pattern removal step 54, an etching step 55, and an insulating layer application step 56.
[0033] As shown in Figure 6, in preparation step 50, the base film 10 is prepared. In the base film 10 prepared in preparation step 50, the first layer 31 is placed on the main surface 11 and the main surface 12. After preparation step 50, the underlay conductive layer formation step 51 is performed.
[0034] As shown in Figure 7, in the underlay conductive layer formation step 51, a second layer 32 is formed on the first layer 31 by, for example, electroless plating. This forms the underlay conductive layer 30. Although not shown, after the preparation step 50 and before the underlay conductive layer formation step 51, through holes are formed that penetrate the base film 10 and the first layer 31. The through holes are formed by, for example, laser processing or drilling. In the underlay conductive layer formation step 51, the second layer 32 is formed not only on the first layer 31 but also on the inner wall surface of the through holes. After the underlay conductive layer formation step 51, a resist pattern formation step 52 is performed.
[0035] As shown in Figure 8, in the resist pattern formation step 52, a resist pattern 60 having openings 61 is formed on the underlying conductive layer 30. The resist pattern 60 is formed by attaching a dry film resist to the underlying conductive layer 30, and then exposing and developing the dry film resist. The openings 61 penetrate the resist pattern 60. In other words, the underlying conductive layer 30 is exposed through the openings 61. After the resist pattern formation step 52, an electroplating step 53 is performed.
[0036] As shown in Figure 9, in the electroplating step 53, an electroplated copper layer 33 is formed on the underlying conductive layer 30 within the opening 61 by electroplating. In the electroplating step 53, the growth of the electroplated copper layer 33 is controlled by adjusting the current value during electroplating. More specifically, by reducing the current value during electroplating, the additives in the plating solution have less effect. As a result, the growth of crystal grains becomes dominant over the formation of crystal nuclei, and each of the multiple crystal grains contained in the electroplated copper layer 33 extends in a needle-like shape along the first direction 13. After the electroplating step 53, a resist pattern removal step 54 is performed.
[0037] As shown in Figure 10, in the resist pattern removal step 54, the resist pattern 60 is removed from the underlying conductive layer 30. Following the resist pattern removal step 54, an etching step 55 is performed. As shown in Figure 11, in the etching step 55, the underlying conductive layer 30 that was beneath the resist pattern 60 is removed. At this time, since each of the multiple crystal grains contained in the electroplated copper layer 33 extends in a needle-like shape along the first direction 13, the surface roughness of the upper surface 34 of the surface of the electroplated copper layer 33 tends to increase. Following the etching step 55, an insulating layer application step 56 is performed.
[0038] In the insulating layer application process 56, an insulating layer 40 is applied to the main surface 11 so as to cover the wiring 20, and an insulating layer 41 is applied to the main surface 12 so as to cover the wiring 21. In the insulating layer application process 56, firstly, the insulating layer 40 and insulating layer 41 are prepared. At this stage, the adhesive layer 42 is not yet cured. Secondly, the insulating layer 40 is positioned on the main surface 11 so as to cover the wiring 20, and the insulating layer 41 is positioned on the main surface 12 so as to cover the wiring 21. Thirdly, the insulating layer 40 and insulating layer 41 are heat-pressed toward the base film 10. This causes the adhesive layer 42 to harden, and the insulating layer 40 and insulating layer 41 are applied to the base film 10. As a result, the structure of the printed circuit board 100 shown in Figures 1 to 3 is formed.
[0039] (Effect of printed circuit board 100) The effects of the printed circuit board 100 are explained below.
[0040] If the surface of the electroplated copper layer 33 is smooth, the anchoring effect between the electroplated copper layer 33 and the insulating layer 40 (insulating layer 41) is not sufficiently effective, and the insulating layer 40 (insulating layer 41) tends to peel off from the wiring 20 (wiring 21). In the printed circuit board 100, the crystal grains contained in the electroplated copper layer 33 are needle-shaped so that the (110) direction of the copper crystals is aligned with the first direction 13. As a result of the etching process 55, the upper surface 34 becomes rougher, improving the adhesion between the insulating layer 40 (insulating layer 41) and the electroplated copper layer 33. Thus, the printed circuit board 100 can suppress the peeling of the insulating layer 40 (insulating layer 41).
[0041] Furthermore, in order to roughen the surface of the electroplated copper layer 33 and improve the adhesion between the insulating layer 40 (insulating layer 41) and the electroplated copper layer 33, it is conceivable to apply a special etching solution in the etching process 55. In the printed circuit board 100, the crystal grains contained in the electroplated copper layer 33 are grown into needle-like shapes, so even if a general etching solution is used in the etching process 55, the upper surface 34 becomes rough.
[0042] (Examples) Samples 1 to 5 were prepared to evaluate the relationship between the crystallinity of the electroplated copper layer 33 and the adhesion to the insulating layer 40. In samples 1 to 5, the orientation of the crystal grains, the first mean grain size, the second mean grain size, the mean aspect ratio, the standard deviation of the tilt angle, the first arithmetic mean roughness, and the second arithmetic mean roughness in the electroplated copper layer 33 were varied, as shown in Table 1.
[0043] [Table 1]
[0044] Condition 1 is defined as the (110) direction of crystal grains contained in the electrolytic copper plating layer 33 being along the main surface 11, and condition 2 is defined as the first average particle size being less than 0.2 μm. As shown in Table 1, both condition 1 and condition 2 were satisfied in samples 1 to 3, while at least one of condition 1 and condition 2 was not satisfied in samples 4 and 5.
[0045] In samples 1 to 5, the adhesion of the insulating layer 40 was evaluated. The insulating layer 40 was formed such that the adhesive layer 42 had a thickness of 30 μm, the adhesive layer 42 was formed of an acrylic adhesive, the cover lay 43 had a thickness of 5 μm, and the cover lay 43 was formed of polyimide. The adhesion of the insulating layer 40 was evaluated by measuring the area of the insulating layer 40 peeled off in a peel test. The area of the peeled insulating layer 40 was 10 mm 2 When the area was less than 10 mm, the evaluation was A, and the area of the peeled insulating layer 40 was 10 mm 2 When the area was 30 mm or more and less than 30 mm, the evaluation was B, and the area of the peeled insulating layer 40 was 30 mm 2 When the area was 30 mm or more and less than 100 mm, the evaluation was C, and the area of the peeled insulating layer 40 was 100 mm 2 When the area was 100 mm or more, the evaluation was D. 2 When the area was less than 100 mm, the evaluation was C, and the area of the peeled insulating layer 40 was 100 mm 2 When the area was 100 mm or more, the evaluation was D.
[0046] In samples 1 to 3, the first arithmetic average roughness was 0.15 μm or more, and the adhesion evaluation of the insulating layer 40 was B or more. On the other hand, in samples 4 and 5, the first arithmetic average roughness was less than 0.15, and the adhesion evaluation of the insulating layer 40 was C or less. From this comparison, it was also experimentally clarified that when condition 1 and condition 2 are satisfied, the upper surface 34 becomes rough, and the adhesion between the insulating layer 40 and the electrolytic copper plating layer 33 is improved.
[0047] (Modification)
[0048] In the example described above, an example was described in which the insulating layer 40 (insulating layer 41) has an adhesive layer 42 and a coverlay 43, but the insulating layer 40 (insulating layer 41) is not limited to this. The insulating layer 40 (insulating layer 41) may be, for example, solder resist.
[0049] As shown in Figure 12, the insulating layer 40 may have a base film 44 instead of a coverlay 43. The base film 44 has a main surface 45 and a main surface 46. The main surface 46 is the opposite side of the main surface 45, and the base film 44 is placed on the adhesive layer 42 such that the main surface 46 faces the adhesive layer 42. The printed circuit board 100 may have wiring 70. The wiring 70, like the wiring 20 and wiring 21, has a base conductive layer 30 placed on the main surface 45 and an electroplated copper layer 33 placed on the base conductive layer 30. The printed circuit board 100 further has an insulating layer 47. The insulating layer 47 has an adhesive layer 48 placed on the main surface 45 so as to cover the wiring 70 and a coverlay 49 placed on the adhesive layer 48. Thus, the printed circuit board 100 may have three or more layers of wiring.
[0050] On the other hand, as shown in Figure 13, the printed circuit board 100 does not have to have wiring 21. That is, the printed circuit board 100 may have only one layer of wiring. In this case, the printed circuit board 100 does not have to have an insulating layer 41.
[0051] It should be understood that at least one configuration or feature described in each embodiment and example can be combined with other embodiments and examples, or modified in various ways. The embodiments disclosed herein should be considered in all respects to be illustrative and not restrictive. The scope of the invention is indicated by the claims rather than the embodiments described above, and all modifications within the meaning and scope of the claims are intended to be included. [Explanation of Symbols]
[0052] 10 Base film, 11 Main surface, 12 Main surface, 13 First direction, 14 Second direction, 15 Third direction, 20 Wiring, 21 Wiring, 30 Underlay conductive layer, 31 First layer, 32 Second layer, 33 Electroplated copper layer, 34 Top surface, 35 Side surface, 40 Insulating layer, 41 Insulating layer, 42 Adhesive layer, 43 Coverlay, 44 Base film, 45 Main surface, 46 Main surface, 47 Insulating layer, 48 Adhesive layer, 49 Coverlay, 50 Preparation process, 51 Underlay conductive layer formation process, 52 Resist pattern formation process, 53 Electroplating process, 54 Resist pattern removal process, 55 Etching process, 56 Insulating layer application process, 60 Resist pattern, 61 Opening, 70 Wiring, 100 Printed circuit board
Claims
1. A base film having a main surface, A base conductive layer disposed on the main surface, The system comprises an electroplated copper layer disposed on the aforementioned conductive underlayer, The electroplated copper layer contains a plurality of crystal grains, The plurality of crystal grains are oriented such that the (110) direction of the copper crystal is aligned with the direction normal to the main surface. A printed circuit board in which, in a cross-sectional view perpendicular to the main surface, the average grain size of the plurality of crystal grains in a direction parallel to the main surface is less than 0.2 μm.
2. The printed circuit board according to claim 1, wherein, in a cross-sectional view perpendicular to the main surface, the average grain size of the plurality of crystal grains is less than 2.4 μm.
3. The printed circuit board according to claim 1, wherein, in a cross-sectional view perpendicular to the main surface, the average aspect ratio of the plurality of crystal grains is 3.5 or more.
4. The printed circuit board according to claim 1, wherein, in a cross-sectional view perpendicular to the main surface, the standard deviation of the inclination angles of the plurality of crystal grains with respect to the normal direction is 30° or less.
5. The electroplated copper layer has an upper surface and side surfaces. The printed circuit board according to claim 1, wherein the arithmetic mean roughness on the upper surface is greater than the arithmetic mean roughness on the side surface.
6. The printed circuit board according to claim 5, wherein the arithmetic mean roughness of the upper surface is 0.15 μm or more.
7. Further equipped with an insulating layer, The printed circuit board according to any one of claims 1 to 6, wherein the insulating layer is disposed on the main surface so as to cover the underlying conductive layer and the electroplated copper layer.
8. The printed circuit board according to claim 7, wherein the insulating layer comprises an adhesive layer and a coverlay disposed on the adhesive layer.
9. The printed circuit board according to claim 7, wherein the insulating layer is solder resist.
Citation Information
Patent Citations
Copper wiring forming method, copper wiring and semiconductor device
JP2010147311A
Laminate for printed wiring board, manufacturing method of printed wiring board and manufacturing method of electronic apparatus
JP2017140838A
JPP7431227B
Integrated circuit and preparation method thereof, three-dimensional integrated circuit, and electronic device
US20250054888A1
Printed circuit board and production method therefor
WO2018211733A1