Resin composition containing acrylic block copolymer

JPWO2022215500A5Inactive Publication Date: 2024-11-19
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023512908
Authority / Receiving Office
JP · JP
Patent Type
Applications
Priority Date
2022-03-18
Filing Date
2022-03-18
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Resin compositions containing acrylic block copolymers face contamination issues when exposed to sebum, particularly due to oleic acid, and struggle to maintain flexibility while avoiding such contamination.

Method used

A resin composition comprising specific acrylic block copolymers with defined polymer blocks and solubility parameters, ensuring a specific mass ratio and molecular weight range, which effectively suppresses contamination by oleic acid and maintains flexibility.

Benefits of technology

The resin composition significantly reduces contamination by sebum components, particularly oleic acid, while maintaining excellent flexibility and adhesive properties.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The purpose of the present invention is to provide a resin composition containing an acrylic block copolymer, the resin composition being sufficiently prevented from the contamination by a substance contained in sebum, particularly oleic acid and being able to retain flexibility. Provided is a resin composition which contains an acrylic block copolymer (I) and an acrylic block copolymer (II) at a specified ratio, in which the acrylic block copolymer (I) has at least one polymer block (A1) containing a methacrylic acid ester unit and at least one polymer block (B1) containing a specific acrylic acid ester unit and satisfies a specific requirement, and the acrylic block copolymer (II) has at least one polymer block (A2) containing a specific methacrylic acid ester unit and at least one polymer block (B2) containing a specific acrylic acid ester unit and satisfies a specific requirement.
Need to check novelty before this filing date? Find Prior Art

Description

Resin composition containing acrylic block copolymer

[0001] The present invention relates to a resin composition containing an acrylic block copolymer.

[0002] Due to their properties, resin compositions containing acrylic block copolymers having a polymer block containing an acrylic ester unit and a polymer block containing a methacrylic ester unit are being investigated for use in various applications such as adhesives, soft materials, etc. Among these acrylic block copolymers, acrylic block copolymers containing an acrylic ester unit having an organic group having 1 to 3 carbon atoms in the polymer block containing the acrylic ester unit have excellent durability against plasticizers, and therefore, are being investigated for use in laminates with, for example, vinyl chloride resins (see, for example, Patent Document 1).

[0003] When resin compositions containing acrylic block copolymers are used as adhesives, soft materials, etc., they may be used in environments where they come into contact with skin, such as hands. When used in such environments where they come into contact with skin, the resin composition may be contaminated by sebum, potentially resulting in a deterioration in the physical properties of the resin composition. Oleic acid, one of the main components of sebum, is a low-molecular-weight organic compound, similar to the plasticizers used in vinyl chloride. Therefore, the use of resin compositions containing the acrylic block copolymers disclosed in Patent Document 1 is expected to solve the problem of sebum-induced contamination of resin compositions.

[0004] International Publication No. 2016 / 175119

[0005] However, the acrylic block copolymer disclosed in Patent Document 1 may have poor flexibility, and a resin composition that can maintain flexibility while avoiding contamination by substances contained in sebum, such as oleic acid, has not yet been found. An object of the present invention is to provide a resin composition containing an acrylic block copolymer that can sufficiently suppress contamination by substances contained in sebum, particularly oleic acid, and maintain flexibility.

[0006] As a result of extensive investigations conducted by the present inventors to achieve the above object, they have found that a resin composition containing, in specific ratios, a specific acrylic block copolymer in which a polymer block containing acrylic ester units contains acrylic ester units having an organic group having 1 to 3 carbon atoms, and a specific acrylic block copolymer in which a polymer block containing acrylic ester units contains acrylic ester units having an organic group having 4 to 12 carbon atoms can sufficiently inhibit contamination by substances contained in sebum, particularly oleic acid, and maintain flexibility.

[0007] According to the present invention, the above object is achieved by: [1] a resin composition comprising 100 parts by mass of an acrylic block copolymer (I) having at least one polymer block (A1) containing a methacrylic acid ester unit and at least one polymer block (B1) containing an acrylic acid ester unit, and 15 to 400 parts by mass of an acrylic block copolymer (II) having at least one polymer block (A2) containing a methyl methacrylate unit and at least one polymer block (B2) containing an acrylic acid ester unit, wherein the content of polymer block (A1) in the acrylic block copolymer (I) is 20% by mass or more, and polymer block (B1) of the acrylic block copolymer (I) is a copolymer represented by the general formula CH═CH-COOR 1 (1) (In formula (1), R 1 represents an organic group having 1 to 3 carbon atoms), and the acrylic block copolymer satisfies the following formulas (i) and (ii): (i) (H) × SP(A1) + (J) × SP(B1) - SP(C) > 1.20 (ii) - 0.80 ≦ SP(A1) - SP(B1) ≦ 0.43 (in the formulas (i) and (ii), SP(A1) represents the solubility parameter (cal / cm) of the polymer block (A1). 3 ) 1 / 2 , SP(B1) is the solubility parameter (cal / cm) of the polymer block (B1) 3 ) 1 / 2 SP(C) is the solubility parameter of oleic acid (cal / cm 3 ) 1 / 2(H) represents the mass proportion of polymer block (A1) in the acrylic block copolymer (I), and (J) represents the mass proportion of polymer block (B1) in the acrylic block copolymer (I). The polymer block (B2) of the acrylic block copolymer (II) is represented by the general formula CH2=CH-COOR 2 (2) (In formula (2), R 2 represents an organic group having 4 to 12 carbon atoms), and the content of the polymer block (A2) in the acrylic block copolymer (II) is less than 35% by mass; [2] The resin composition according to [1], wherein the weight-average molecular weights of the acrylic block copolymers (I) and (II) are both in the range of 30,000 to 300,000; [3] The resin composition according to [1] or [2], wherein a cylindrical test piece having a thickness of 1 mm and a diameter of 25 mm obtained by molding the resin composition is immersed in oleic acid and the mass change rate before and after storage at 25°C for 168 hours is [(mass of the test piece after immersion) - (mass of the test piece before immersion)] / (mass of the test piece before immersion) x 100 is 200% or less; [4] The present invention is achieved by providing the resin composition according to any one of [1] to [3], wherein the acrylic acid ester (b2-2) unit in the acrylic block copolymer (II) is an n-butyl acrylate unit; and [5] the resin composition according to any one of [1] to [4], wherein the acrylic acid ester (b1-1) unit in the acrylic block copolymer (I) is a methyl acrylate unit.

[0008] The resin composition of the present invention can sufficiently inhibit contamination by substances contained in sebum, particularly oleic acid, and can maintain flexibility.

[0009] The present invention will be described in detail below. In this specification, "(meth)acrylic acid ester" is a general term for "methacrylic acid ester" and "acrylic acid ester", and "(meth)acrylic" is a general term for "methacrylic" and "acrylic".

[0010] <Acrylic Block Copolymer (I)> The acrylic block copolymer (I) contained in the resin composition of the present invention has at least one polymer block (A1) containing a methacrylic acid ester unit and at least one polymer block (B1) containing an acrylic acid ester unit, and the acrylic acid ester unit contained in the polymer block (B1) is represented by the general formula CH═CH-COOR 1 (1) (In formula (1), R 1 represents an organic group having 1 to 3 carbon atoms).

[0011] Examples of methacrylate esters that serve as structural units of the polymer block (A1) include alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, n-butyl methacrylate, t-butyl methacrylate, n-hexyl methacrylate, cyclohexyl methacrylate, 2-ethylhexyl methacrylate, n-octyl methacrylate, lauryl methacrylate, tridecyl methacrylate, stearyl methacrylate, and isobornyl methacrylate; methacrylates that do not have a functional group other than alkyl methacrylates such as phenyl methacrylate and benzyl methacrylate; alkoxyalkyl methacrylates such as methoxyethyl methacrylate and ethoxyethyl methacrylate; and methacrylates that have a functional group such as diethylaminoethyl methacrylate, 2-hydroxyethyl methacrylate, 2-aminoethyl methacrylate, glycidyl methacrylate, and tetrahydrofurfuryl methacrylate.

[0012] Among these, alkyl methacrylates are preferred, with methyl methacrylate, ethyl methacrylate, and propyl methacrylate being more preferred, and methyl methacrylate being even more preferred because it is economically readily available and the resulting polymer block (A1) has excellent durability and weather resistance.

[0013] The methacrylic acid ester units of the polymer block (A1) may be obtained from only one type of methacrylic acid ester, or may be obtained from two or more types of methacrylic acid esters. The proportion of the methacrylic acid ester units contained in the polymer block (A1) is preferably 60% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, of the polymer block (A1). Furthermore, the polymer block (A1) may be composed of 100% by mass of methacrylic acid ester units, i.e., composed only of methacrylic acid ester units.

[0014] The polymer block (A1) may contain other monomer units as long as the effects of the present invention are not impaired. Examples of such other monomers include acrylic esters; vinyl monomers having a carboxyl group such as (meth)acrylic acid, crotonic acid, maleic acid, maleic anhydride, and fumaric acid; vinyl monomers having a functional group such as (meth)acrylamide, (meth)acrylonitrile, vinyl acetate, vinyl chloride, and vinylidene chloride; aromatic vinyl monomers such as styrene, α-methylstyrene, p-methylstyrene, and m-methylstyrene; conjugated diene monomers such as butadiene and isoprene; olefin monomers such as ethylene, propylene, isobutene, and octene; and lactone monomers such as ε-caprolactone and valerolactone. The amount of monomer units composed of these other monomers is usually small relative to the total amount of monomer units in the polymer block (A1), and the proportion of other monomer units contained in the polymer block (A1) is preferably 40% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less.

[0015] The glass transition temperature (Tg) of the polymer block (A1) is preferably 50 to 150°C, more preferably 60 to 140°C, and even more preferably 70 to 130°C. When the glass transition temperature of the polymer block (A1) is within the above range, the polymer block (A1) acts as a physical pseudo-crosslinking point at the normal use temperature of the resin composition of the present invention, and cohesive strength is exerted in the resin composition, resulting in excellent adhesive properties, durability, heat resistance, and hot melt moldability. The glass transition temperature is the extrapolated onset temperature of the curve obtained by DSC measurement.

[0016] The acrylic block copolymer (I) may contain two or more polymer blocks (A1), and in that case, the methacrylic acid ester units and other monomers constituting the polymer blocks (A1) may be the same or different.

[0017] The weight-average molecular weight (Mw) of the polymer block (A1) is not particularly limited, but is preferably in the range of 1,000 to 50,000, and more preferably in the range of 4,000 to 20,000. When the Mw of the polymer block (A1) is 1,000 or more, the cohesive strength of the resulting acrylic block copolymer (I) is easily obtained. Furthermore, when the Mw of the polymer block (A1) is 50,000 or less, the melt viscosity of the resulting acrylic block copolymer (I) is not too high, which is unlikely to cause problems in the productivity of the acrylic block copolymer (I) or the moldability of a resin composition containing the resulting acrylic block copolymer (I). In this specification, the weight-average molecular weight (Mw) refers to the weight-average molecular weight measured by gel permeation chromatography (GPC) in terms of standard polystyrene.

[0018] The polymer block (B1) contains an acrylic ester unit, and the acrylic ester unit contained in the polymer block (B1) is represented by the general formula CH2=CH-COOR 1 (1) (In formula (1), R 1 represents an organic group having 1 to 3 carbon atoms) (hereinafter simply referred to as acrylate (b1-1)).

[0019] Examples of the acrylic acid ester (b1-1) include acrylic acid esters having no functional group, such as methyl acrylate, ethyl acrylate, isopropyl acrylate, and n-propyl acrylate; and acrylic acid esters having a functional group, such as 2-methoxyethyl acrylate, 2-hydroxyethyl acrylate, 2-aminoethyl acrylate, and glycidyl acrylate.

[0020] Among these, from the viewpoint of enhancing the stain resistance of the resulting resin composition against substances contained in sebum, such as oleic acid, acrylic acid esters having no functional group are preferred, methyl acrylate and ethyl acrylate are more preferred, and methyl acrylate is even more preferred. These acrylic acid esters (b1-1) may be used alone or in combination of two or more.

[0021] The acrylic acid ester units constituting the polymer block (B1) include, in addition to the acrylic acid ester (b1-1) units, units of the general formula CH2=CH-COOR 2 (2) (wherein, R 2 represents an organic group having 4 to 12 carbon atoms) (hereinafter simply referred to as acrylate (b1-2)).

[0022] Examples of the acrylic acid ester (b1-2) include acrylic acid esters without functional groups, such as n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, amyl acrylate, isoamyl acrylate, n-hexyl acrylate, 2-ethylhexyl acrylate, n-octyl acrylate, isooctyl acrylate, decyl acrylate, isobornyl acrylate, lauryl acrylate, cyclohexyl acrylate, phenyl acrylate, and benzyl acrylate; and acrylic acid esters with functional groups, such as 2-ethoxyethyl acrylate, 2-(diethylamino)ethyl acrylate, tetrahydrofurfuryl acrylate, and 2-phenoxyethyl acrylate.

[0023] Among these, acrylic acid esters having no functional group are preferred, since they result in clearer phase separation between polymer block (A1) and polymer block (B1), alkyl acrylates having an alkyl group of 4 to 12 carbon atoms are more preferred, and n-butyl acrylate and 2-ethylhexyl acrylate are even more preferred. Furthermore, n-butyl acrylate is even more preferred, since it enhances the stain resistance of the resulting resin composition to substances contained in sebum, such as oleic acid, and also because it provides the resulting resin composition with excellent flexibility, adhesive properties (tack, adhesive strength, etc.) at low temperatures (-40 to 10°C), and excellent durability. These acrylic acid esters (b1-2) may be used alone, or two or more types may be used in combination.

[0024] The mass ratio (b1-1) / (b1-2) of the acrylic acid ester (b1-1) units and the acrylic acid ester (b1-2) units in the polymer block (B1) is preferably 90 / 10 to 10 / 90. When the mass ratio is within the above range, both the stain resistance due to substances contained in sebum such as oleic acid, which is attributable to the acrylic acid ester (b1-1) units, and the flexibility due to the acrylic acid ester (b1-2) units are excellent. From the viewpoint of achieving both excellent stain resistance due to substances contained in sebum such as oleic acid and flexibility, the mass ratio (b1-1) / (b1-2) of the acrylic acid esters is preferably 85 / 15 to 10 / 90, more preferably 80 / 20 to 10 / 90, and even more preferably 80 / 20 to 20 / 80. The mass ratio of the acrylic acid ester (b1-1) units and the acrylic acid ester (b1-2) units is 1 It can be determined by H-NMR measurement.

[0025] Furthermore, the proportion of the acrylic acid ester (b1-1) units in the acrylic acid ester units of the polymer block (B1) is preferably 90 mass% or less, more preferably 85 mass% or less, and even more preferably 80 mass% or less, in the polymer block (B1).

[0026] In one preferred embodiment, the acrylic ester units contained in the polymer block (B1) are composed solely of acrylic ester (b1-1) units and acrylic ester (b1-2) units.

[0027] The proportion of the acrylic ester units in the polymer block (B1) is preferably 60% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, in the polymer block (B1). In addition, one preferred embodiment of the polymer block (B1) is one that is composed of 100% by mass of acrylic ester units, i.e., one that is composed only of acrylic ester units.

[0028] The polymer block (B1) may contain other monomer units besides the acrylic acid ester units, provided that the effects of the present invention are not impaired. Examples of other monomers constituting such units include methacrylic acid esters; vinyl monomers having a carboxyl group, such as (meth)acrylic acid, crotonic acid, maleic acid, maleic anhydride, and fumaric acid; vinyl monomers having a functional group, such as (meth)acrylamide, (meth)acrylonitrile, vinyl acetate, vinyl chloride, and vinylidene chloride; aromatic vinyl monomers, such as styrene, α-methylstyrene, p-methylstyrene, and m-methylstyrene; conjugated diene monomers, such as butadiene and isoprene; olefin monomers, such as ethylene, propylene, isobutene, and octene; and lactone monomers, such as ε-caprolactone and valerolactone. The amount of monomer units composed of these other monomers is usually small relative to the total amount of monomer units in the polymer block (B1), and the proportion of other monomer units contained in the polymer block (B1) is preferably 40% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less.

[0029] The acrylic block copolymer (I) may contain two or more polymer blocks (B1), and in this case, the combinations of acrylic acid ester units constituting the polymer blocks (B1) may be the same or different.

[0030] When the acrylic acid ester unit portion contained in the polymer block (B1) contains an acrylic acid ester (b1-1) unit and an acrylic acid ester (b1-2) unit, the portion is composed of a copolymer of the acrylic acid ester (b1-1) and the acrylic acid ester (b1-2). In such a case, the copolymer may be in the form of a random copolymer, block copolymer, or graft copolymer of the acrylic acid ester (b1-1) and the acrylic acid ester (b1-2), or may be a tapered block copolymer (gradient copolymer), but is preferably a random copolymer. When the acrylic block copolymer (I) contains two or more polymer blocks (B1), the structures of the polymer blocks (B1) may be the same or different.

[0031] The glass transition temperature (Tg) of the polymer block (B1) is more preferably −50 to 55° C., more preferably −50 to 50° C., even more preferably −50 to 45° C., and even more preferably −50 to 25° C. When the glass transition temperature is within this range, a resin composition that is excellent in flexibility and durability at use temperatures tends to be easily obtained.

[0032] The difference in glass transition temperature between the polymer block (A1) and the polymer block (B1) in the acrylic block copolymer (I) is preferably 50° C. or more, more preferably 70° C. or more.

[0033] The acrylic block copolymer (I) has the general formula: (A1-B1), where the polymer block (A1) is represented by "A1" and the polymer block (B1) is represented by "B1." n (A1-B1) n -A1 A1- (A1-B1) n (A1-B1) n -Z (B1-A1) n-Z (wherein n is an integer of 1 to 30, and Z represents a coupling moiety (a coupling moiety remaining after a coupling agent reacts with a polymer terminal to form a chemical bond). The value of n is preferably 1 to 15, more preferably 1 to 8, and even more preferably 1 to 4.)

[0034] Among these structures, a structure in which the polymer block (A1) is bonded to both ends of the polymer block (B1) is preferred. Specifically, a structure represented by the following general formula: (A1-B1) n -A1 (A1-B1) m -Z (wherein n is an integer of 1 to 30, m is an integer of 2 to 30, and Z represents a coupling moiety (a coupling moiety remaining after a coupling agent reacts with a polymer terminal to form a chemical bond). The value of m is preferably 2 to 15, more preferably 2 to 8, and even more preferably 2 to 4. The value of n is preferably 1 to 15, more preferably 1 to 8, and even more preferably 1 to 4.)

[0035] Among the above structures, (A1-B1) n , (A1-B1) n -A1, A1- (A1-B1) n A linear block copolymer represented by the formula (I) is more preferred, a diblock copolymer represented by the formula (I) and a triblock copolymer represented by the formula (I) are even more preferred, and a triblock copolymer represented by the formula (I) is particularly preferred. These may be used alone or in combination of two or more.

[0036] The content of polymer block (A1) in the acrylic block copolymer (I) is 20% by mass or more, preferably 20 to 40% by mass. When the content of polymer block (A1) is 20% by mass or more, the cohesive strength of the acrylic block copolymer (I) is likely to be high, and when a resin composition is produced from the acrylic block copolymer (I) and the acrylic block copolymer (II) described below, the shape tends to be easily maintained and good moldability tends to be achieved. When the content of polymer block (A1) is 40% by mass or less, a resin composition with excellent flexibility tends to be obtained. From the viewpoint of obtaining a resin composition with excellent flexibility, the content of polymer block (A1) in the acrylic block copolymer (I) is preferably 20 to 35% by mass, more preferably 25 to 31% by mass.

[0037] The acrylic block copolymer (I) of the present invention must satisfy the following formulas (i) and (ii): (i) (H) × SP(A1) + (J) × SP(B1) − SP(C) > 1.20 (ii) − 0.80 ≦ SP(A1) − SP(B1) ≦ 0.43 In the formulas (i) and (ii), SP(A1) is the solubility parameter (cal / cm) of the polymer block (A1). 3 ) 1 / 2 , SP(B1) is the solubility parameter (cal / cm) of the polymer block (B1) 3 ) 1 / 2 SP(C) is the solubility parameter of oleic acid (cal / cm 3 ) 1 / 2 (H) represents the mass proportion of polymer block (A1) in the acrylic block copolymer (I), and (J) represents the mass proportion of polymer block (B1) in the acrylic block copolymer (I).

[0038] Here, the solubility parameter of each polymer block (A1) and (B1) is a value determined by the Fedors estimation method. The solubility parameter (SP value (δ)) is defined as the square root of the cohesive energy density (ΔE / V) calculated from the cohesive energy (ΔE) and the molar volume (V) of the solvent. The SP values ​​calculated from ΔE and V of polymethyl acrylate (methyl acrylate unit), polyn-butyl acrylate (n-butyl acrylate unit), poly2-ethylhexyl acrylate (2-ethylhexyl acrylate unit), and polymethyl methacrylate (methyl methacrylate unit) are each 11.30 (cal / cm 3 ) 1 / 2 , 10.20 (cal / cm 3 ) 1 / 2 , 9.50 (cal / cm 3 ) 1 / 2 , 10.50 (cal / cm 3 ) 1 / 2 The SP (C) was calculated as 9.14 (cal / cm 3 ) 1 / 2 is.

[0039] (Formula (i)) The value of (H) × SP(A1) + (J) × SP(B1) included on the left side of the above formula (i) is a value that serves as an index of the solubility parameter of the entire acrylic block copolymer (I). It is important that the difference between this value and the solubility parameter SP(C) of oleic acid is within a specific range in order to sufficiently suppress contamination by substances contained in sebum and maintain flexibility. The details of the reason for this are unknown, but it is presumed that when the difference between the solubility parameter of the entire acrylic block copolymer and the solubility parameter of oleic acid exceeds a specific value, contamination by all substances contained in sebum tends to be suppressed.

[0040] From the above viewpoint, it is preferable to satisfy the following formula (i-1), and it is more preferable to satisfy the following formula (i-2): (i-1) (H)×SP(A1)+(J)×SP(B1)−SP(C)>1.25 (i-2) (H)×SP(A1)+(J)×SP(B1)−SP(C)>1.30

[0041] The acrylic block copolymer (I) satisfying the above formula (i) can be obtained, for example, by adjusting the proportion of the acrylic acid ester (b1-1) units in the acrylic acid ester units of the polymer block (B1) and the content of the polymer block (A1).

[0042] (Formula (ii)) The value of SP(A1)-SP(B1) in the above formula (ii) is the difference in solubility parameters between the polymer blocks (A1) and (B1) in the acrylic block copolymer (I), and formula (ii) indicates that it is important that this difference be within a specific range. When this difference in solubility parameters is within a specific range, not only can the copolymer exhibit sufficient flexibility but also sufficient stain resistance against substances contained in sebum, such as oleic acid, even when used in combination with the acrylic block copolymer (II) described below. The details of the reason for this are unknown, but it is presumed that when the difference in solubility parameters of the polymer blocks contained in the acrylic block copolymer (I) is a specific value or less, phase separation of the polymer blocks is suppressed, making it difficult for sebum components to penetrate, and thus tending to suppress staining by all substances contained in sebum.

[0043] From the above viewpoint, it is preferable to satisfy the following formula (ii-1), and it is more preferable to satisfy the following formula (ii-2): (ii-1) -0.70≦SP(A1)-SP(B1)≦0.43 (ii-2) -0.65≦SP(A1)-SP(B1)≦0.43

[0044] The acrylic block copolymer (I) satisfying the above formula (ii) can be obtained, for example, by adjusting the content of the acrylic acid ester (b1-1) unit in the acrylic acid ester units of the polymer block (B1) or the content of the polymer block (A1).

[0045] From the viewpoints of compatibility with the acrylic block copolymer (II) described below and the processability of the resulting resin composition, the Mw of the acrylic block copolymer (I) is preferably 30,000 to 300,000, more preferably 40,000 to 250,000, even more preferably 50,000 to 220,000, and even more preferably 60,000 to 200,000. When the Mw of the acrylic block copolymer (I) is 30,000 or more, the cohesive strength of the acrylic block copolymer (I) is increased, and the durability of the resulting resin composition tends to be more excellent. Furthermore, when a molded article is produced from the resin composition, defects such as bleeding originating from the acrylic block copolymer (I) on the surface of the molded article are less likely to occur. On the other hand, when the Mw of the acrylic block copolymer (I) is 300,000 or less, productivity and processability tend to be excellent. In addition, the compatibility with the acrylic block copolymer (II) described later tends to be good, the transparency of the resulting resin composition tends to be better, and the physical properties of a molded article produced from the resin composition tend to be more stable.

[0046] The acrylic block copolymer (I) preferably has a molecular weight distribution (Mw / Mn) of 1.0 to 1.5. Having a molecular weight distribution of the acrylic block copolymer (I) within this range tends to facilitate an increase in the cohesive strength of the acrylic block copolymer (I) and to facilitate the prevention of mold contamination during molding of the resulting pellets. From the above viewpoints, the molecular weight distribution is more preferably 1.0 to 1.4, and even more preferably 1.0 to 1.3. The above-mentioned Mn refers to the number average molecular weight, and in this specification, the number average molecular weight (Mn) refers to the number average molecular weight in terms of standard polystyrene measured by gel permeation chromatography (GPC).

[0047] <Acrylic Block Copolymer (II)> The acrylic block copolymer (II) contained in the resin composition of the present invention is a polymer different from the acrylic block copolymer (I), and has at least one polymer block (A2) containing a methyl methacrylate unit and at least one polymer block (B2) containing an acrylic ester unit, and the polymer block (B2) has a structure represented by the general formula CH═CH-COOR 2 (2) (In formula (2), R 2 represents an organic group having 4 to 12 carbon atoms), and the content of polymer block (A2) in the acrylic block copolymer (II) is less than 35 mass%. By including the acrylic block copolymer (II) in addition to the acrylic block copolymer (I) in the resin composition of the present invention, it is possible to obtain a resin composition that is not only capable of sufficiently suppressing contamination by substances contained in sebum, particularly oleic acid, but also has excellent flexibility.

[0048] The proportion of methyl methacrylate units contained in the polymer block (A2) is preferably 60% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, in the polymer block (A2). In addition, one preferred embodiment of the polymer block (A2) is one that is composed of 100% by mass of methyl methacrylate units, i.e., one that is composed only of methyl methacrylate units.

[0049] The polymer block (A2) may contain other monomer units besides methyl methacrylate, provided that the effects of the present invention are not impaired. Specific examples of such other monomers include methacrylic acid esters other than methyl methacrylate, acrylic acid esters, vinyl monomers having a carboxyl group such as (meth)acrylic acid, crotonic acid, maleic acid, maleic anhydride, and fumaric acid, vinyl monomers having a functional group such as (meth)acrylamide, (meth)acrylonitrile, vinyl acetate, vinyl chloride, and vinylidene chloride, aromatic vinyl monomers such as styrene, α-methylstyrene, p-methylstyrene, and m-methylstyrene, conjugated diene monomers such as butadiene and isoprene, olefin monomers such as ethylene, propylene, isobutene, and octene, and lactone monomers such as ε-caprolactone and valerolactone. The amount of monomer units composed of these other monomers is usually small relative to the total amount of monomer units in the polymer block (A2), and the proportion of other monomer units contained in the polymer block (A2) is preferably 40% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less.

[0050] The glass transition temperature (Tg) of the polymer block (A2) is preferably 50 to 150° C., more preferably 70 to 140° C., and even more preferably 80 to 130° C. When the glass transition temperature of the polymer block (A2) is within the above range, sticking tends to be reduced (sticking resistance is improved) at high temperatures (for example, 50° C.) when stored as pellets.

[0051] The acrylic block copolymer (II) may contain two or more polymer blocks (A2), and in that case, the methyl methacrylate units and other monomers constituting the polymer blocks (A2) may be the same or different.

[0052] The Mw of the polymer block (A2) is not particularly limited, but is preferably in the range of 1,000 to 50,000, and more preferably in the range of 4,000 to 20,000. If the Mw of the polymer block (A2) is less than 1,000, the cohesive strength of the resulting acrylic block copolymer (II) may be insufficient. If the Mw of the polymer block (A2) is greater than 50,000, the melt viscosity of the resulting acrylic block copolymer (II) may be high, which may result in poor productivity of the acrylic block copolymer (II) and poor moldability of pellets containing the resulting resin composition.

[0053] The polymer block (B2) contains an acrylic ester unit, and the acrylic ester unit contained in the polymer block (B2) is represented by the general formula CH2=CH-COOR 2 (2) (wherein, R 2 represents an organic group having 4 to 12 carbon atoms) (hereinafter simply referred to as acrylate (b2-2)).

[0054] Specific examples of the acrylic acid ester (b2-2) are the same as the acrylic acid ester (b1-2) which can be one of the structural units of the polymer block (B1) of the acrylic block copolymer (I).

[0055] Among these acrylic acid esters (b2-2), acrylic acid esters having no functional group are preferred in that the phase separation between the polymer block (A2) and the polymer block (B2) becomes clearer, alkyl acrylates having an alkyl group having 4 to 12 carbon atoms are more preferred, and n-butyl acrylate and 2-ethylhexyl acrylate are even more preferred. Furthermore, n-butyl acrylate is even more preferred in that the resin composition of the present invention tends to have better flexibility and is more likely to have a resin composition having excellent durability.

[0056] The acrylic acid ester (b2-2) units constituting the acrylic acid ester units contained in the polymer block (B2) may be obtained from only one type of acrylic acid ester (b2-2), or may be obtained from two or more types of acrylic acid ester (b2-2).

[0057] The proportion of the acrylic acid ester units contained in the polymer block (B2) is preferably 60% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, in the polymer block (B2). The polymer block (B2) may also be composed of 100% by mass of acrylic acid ester units, i.e., composed only of acrylic acid ester units.

[0058] The acrylic ester unit contained in the polymer block (B2) is represented by the general formula CH2=CH-COOR 1 (1) (In formula (1), R 1 In one preferred embodiment, the copolymer does not contain an acrylic acid ester (b2-1) unit (hereinafter simply referred to as acrylic acid ester (b2-1)) represented by the formula: (wherein R represents an organic group having 1 to 3 carbon atoms). Specific examples of the acrylic acid ester (b2-1) are the same as the acrylic acid ester (b1-1) that is a structural unit of the polymer block (B1) of the acrylic block copolymer (I). When the polymer block (B2) does not contain an acrylic acid ester (b2-1) unit, a resin composition with improved flexibility can be obtained.

[0059] In one preferred embodiment, the acrylic ester units contained in the polymer block (B2) are composed solely of acrylic ester (b2-2) units, which allows for a resin composition with improved flexibility to be obtained.

[0060] The polymer block (B2) may contain other monomer units besides acrylic acid ester units, provided that the effects of the present invention are not impaired. Specific examples of such other monomers are the same as the other monomers that can serve as structural units of the polymer block (B1) of the acrylic block copolymer (I). The amount of monomer units formed from these other monomers is usually small relative to the total amount of monomer units in the polymer block (B2). The proportion of other monomer units contained in the polymer block (B2) is preferably 40% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less.

[0061] The glass transition temperature of the polymer block (B2) is preferably −100 to 40° C., more preferably −80 to 35° C., and even more preferably −70 to 30° C. When the glass transition temperature of the polymer block (B2) is within the above range, the polymer block (B2) exhibits excellent flexibility even at low temperatures. Among the alkyl acrylates, n-butyl acrylate, 2-ethylhexyl acrylate, and n-octyl acrylate are preferred, as they have a glass transition temperature within the above preferred range and are easily available.

[0062] The acrylic block copolymer (II) may contain two or more polymer blocks (B2). In this case, the combinations of acrylic acid ester units constituting the polymer blocks (B2) may be the same or different.

[0063] The difference in glass transition temperature between the polymer block (A2) and the polymer block (B2) in the acrylic block copolymer (II) is preferably 70° C. or more, more preferably 100° C. or more.

[0064] The acrylic block copolymer (II) can be represented by the general formula: (A2-B2), where the polymer block (A2) is represented by "A2" and the polymer block (B2) is represented by "B2." i (A2-B2) i -A2 A2-(A2-B2) i (A2-B2) i -Z (B2-A2) i -Z (wherein i is an integer of 1 to 30, and Z represents a coupling moiety (a coupling moiety remaining after a coupling agent reacts with a polymer terminal to form a chemical bond). The value of i is preferably 1 to 15, more preferably 1 to 8, and even more preferably 1 to 4.)

[0065] Among these structures, a structure in which polymer block (A2) is bonded to both ends of polymer block (B2) is preferred. Specifically, a structure represented by the following general formula: (A2-B2) i -A2 (A2-B2) k-Z (wherein i is an integer of 1 to 30, k is an integer of 2 to 30, and Z represents a coupling moiety (a coupling moiety remaining after a coupling agent reacts with a polymer terminal to form a chemical bond). The value of k is preferably 2 to 15, more preferably 2 to 8, and even more preferably 2 to 4. The value of i is preferably 1 to 15, more preferably 1 to 8, and even more preferably 1 to 4.)

[0066] Among the above structures, (A2-B2) i , (A2-B2) i -A2, A2- (A2-B2) i A linear block copolymer represented by the formula (I) is more preferred, a diblock copolymer represented by the formula (I) and a triblock copolymer represented by the formula (I) are even more preferred, and a triblock copolymer represented by the formula (I) is particularly preferred. These may be used alone or in combination of two or more.

[0067] The content of polymer block (A2) in the acrylic block copolymer (II) is less than 35% by mass. When the content of polymer block (A2) is less than 35% by mass, the acrylic block copolymer (II) becomes flexible, and the resin composition obtained by mixing the acrylic block copolymer (II) with the acrylic block copolymer (I) has excellent flexibility. The content of polymer block (A2) in the acrylic block copolymer (II) is preferably less than 33% by mass, and more preferably less than 32% by mass, since this makes it easier to obtain a resin composition with excellent flexibility. Furthermore, from the viewpoint of suppressing bleeding originating from the acrylic block copolymer (II), the content of polymer block (A2) is preferably 3% by mass or more.

[0068] From the viewpoints of compatibility with the acrylic block copolymer (I) and the processability of the resulting resin composition, the Mw of the acrylic block copolymer (II) is preferably 30,000 to 300,000, more preferably 30,000 to 200,000, even more preferably 40,000 to 180,000, and even more preferably 50,000 to 160,000. When the Mw of the acrylic block copolymer (II) is 30,000 or more, the cohesive strength of the acrylic block copolymer (II) is increased, and the durability of the resulting resin composition tends to be more excellent. Furthermore, when a molded article is produced from the resin composition, defects such as bleeding originating from the acrylic block copolymer (II) on the surface of the molded article are less likely to occur. On the other hand, when the Mw of the acrylic block copolymer (II) is 300,000 or less, productivity and processability tend to be excellent. Furthermore, the compatibility with the above-mentioned acrylic block copolymer (I) tends to be good, the transparency of the resulting resin composition tends to be better, and the physical properties of a molded article produced from the resin composition tend to be more stable.

[0069] The acrylic block copolymer (II) preferably has a molecular weight distribution (Mw / Mn) of 1.0 to 1.5. Having a molecular weight distribution of the acrylic block copolymer (II) within this range tends to facilitate an increase in the cohesive strength of the acrylic block copolymer (II) and to facilitate the prevention of equipment contamination during processing of the resulting resin composition. From the above viewpoints, the molecular weight distribution is more preferably 1.0 to 1.4, and even more preferably 1.0 to 1.3.

[0070] The MFR of the acrylic block copolymer (II) under conditions of 230°C and a load of 3.8 kg is preferably 20 g / 10 min or more, more preferably 30 g / 10 min or more. When the MFR is above the above lower limit, the miscibility with the acrylic block copolymer (I) is superior, and good compatibility and excellent transparency tend to be obtained. Furthermore, if the MFR is too high, the melt viscosity tends to be low, and the kneading ability during processing tends to be insufficient. Therefore, the MFR is preferably 350 g / 10 min or less, more preferably 300 g / 10 min or less. When the MFR is below the above upper limit, the melt kneading tends to be easy.

[0071] The methods for producing the acrylic block copolymer (I) and the acrylic block copolymer (II) are not particularly limited, and these acrylic block copolymers can be produced by production methods similar to known methods. Generally, a method for obtaining a block copolymer with a narrow molecular weight distribution employs living polymerization of the constituent monomers. Examples of such living polymerization techniques include living polymerization using an organic rare earth metal complex as a polymerization initiator (see, for example, JP-A-11-335432), living anionic polymerization using an organic alkali metal compound as a polymerization initiator in the presence of a mineral acid salt such as an alkali metal or alkaline earth metal salt (see, for example, JP-B-7-25859), living anionic polymerization using an organic alkali metal compound as a polymerization initiator in the presence of an organoaluminum compound (see, for example, JP-A-6-93060), and atom transfer radical polymerization (ATRP) (see, for example, Macromol. Chem. Phys., 2000, 201, pp. 1108-1114).

[0072] Among the above production methods, living anionic polymerization in the presence of an organoaluminum compound results in less deactivation during polymerization, resulting in less homopolymer contamination and high transparency of the resulting block copolymer. Furthermore, the high polymerization conversion of monomers results in less residual monomer in the block copolymer, suppressing the generation of bubbles when producing pellets containing the acrylic block copolymer. Furthermore, the molecular structure of the polymer block composed of methacrylic acid alkyl ester units becomes highly syndiotactic, which enhances the durability of the resulting resin composition containing the acrylic block copolymer. Furthermore, since living anionic polymerization can be performed under relatively mild temperature conditions, industrial production has the advantage of reducing the environmental impact (mainly the power required for the refrigerator to control the polymerization temperature). For these reasons, acrylic block copolymers are preferably produced by living anionic polymerization in the presence of an organoaluminum compound using an organic alkali metal compound as a polymerization initiator.

[0073] As the living anionic polymerization method in the presence of the organoaluminum compound, for example, an organolithium compound and a compound represented by the following general formula (3): AlR 3 R 4 R 5 (3) (In formula (3), R 3 , R 4 and R 5 each independently represents an alkyl group which may have a substituent, a cycloalkyl group which may have a substituent, an aryl group which may have a substituent, an aralkyl group which may have a substituent, an alkoxy group which may have a substituent, an aryloxy group which may have a substituent, or an N,N-disubstituted amino group, or R 3 is any of the groups described above, and R 4 and R 5and a nitrogen-containing compound such as dimethyl ether, dimethoxyethane, diethoxyethane, or 12-crown-4; or a nitrogen-containing compound such as triethylamine, N,N,N',N'-tetramethylethylenediamine, N,N,N',N",N"-pentamethyldiethylenetriamine, 1,1,4,7,10,10-hexamethyltriethylenetetramine, pyridine, or 2,2'-dipyridyl, may be further added to the reaction system, as necessary, to polymerize the (meth)acrylic acid ester.

[0074] Examples of the organolithium compound include alkyllithiums or alkyldilithiums such as n-butyllithium, sec-butyllithium, and tetramethylenedilithium; aryllithiums or aryldilithiums such as phenyllithium and xylyllithium; aralkyllithiums or aralkyldilithiums such as benzyllithium and dilithium produced by the reaction of diisopropenylbenzene with butyllithium; lithium amides such as lithium diisopropylamide; and lithium alkoxides such as methoxylithium.

[0075] As the organoaluminum compound represented by the general formula (3), isobutylbis(2,6-di-tert-butyl-4-methylphenoxy)aluminum, isobutylbis(2,6-di-tert-butylphenoxy)aluminum, isobutyl[2,2'-methylenebis(4-methyl-6-tert-butylphenoxy)]aluminum, etc. are preferred from the viewpoints of high living polymerization properties and ease of handling.

[0076] The resin composition of the present invention contains 15 to 400 parts by mass of the acrylic block copolymer (II) per 100 parts by mass of the acrylic block copolymer (I). If the content of the acrylic block copolymer (II) per 100 parts by mass of the acrylic block copolymer (I) is less than 15 parts by mass, the flexibility of the resulting resin composition is insufficient. On the other hand, if the content of the acrylic block copolymer (II) per 100 parts by mass of the acrylic block copolymer (I) exceeds 400 parts by mass, it becomes difficult to sufficiently suppress contamination of the resulting resin composition by substances contained in sebum. From the viewpoints of further suppressing contamination of the resulting resin composition by substances contained in sebum and improving the flexibility of the resin composition, the content of the acrylic block copolymer (II) per 100 parts by mass of the acrylic block copolymer (I) in the resin composition of the present invention is preferably 15 to 300 parts by mass, more preferably 20 to 200 parts by mass.

[0077] The total content of the acrylic block copolymer (I) and the acrylic block copolymer (II) contained in the resin composition of the present invention is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, and may be 100% by mass.

[0078] The resin composition of the present invention may contain additives such as other polymers, tackifying resins, softeners, plasticizers, heat stabilizers, light stabilizers, antistatic agents, flame retardants, foaming agents, colorants, dyes, refractive index modifiers, fillers, curing agents, lubricants, anti-sticking agents, termite repellents, rodent repellents, etc. These other polymers and additives may be contained alone or in combination with each other, provided that the effects of the present invention are not impaired.

[0079] Examples of the other polymers include acrylic resins such as polymethyl methacrylate and (meth)acrylic acid ester polymers or copolymers; olefin resins such as polyethylene, ethylene-vinyl acetate copolymer, polypropylene, polybutene-1, poly-4-methylpentene-1, and polynorbornene; ethylene ionomers; styrene resins such as polystyrene, styrene-maleic anhydride copolymer, high-impact polystyrene, AS resin, ABS resin, AES resin, AAS resin, ACS resin, and MBS resin; styrene-methyl methacrylate copolymer; styrene-methyl methacrylate-maleic anhydride copolymer; Examples of suitable materials include polyester resins such as polyethylene terephthalate, polybutylene terephthalate, and polylactic acid; polyamides such as nylon 6, nylon 66, and polyamide elastomers; polycarbonate; polyvinyl chloride; polyvinylidene chloride; polyvinyl alcohol; ethylene-vinyl alcohol copolymers; polyacetal; polyvinylidene fluoride; polyurethane; modified polyphenylene ether; polyphenylene sulfide; silicone rubber-modified resins; acrylic rubber; silicone rubber; styrene-based thermoplastic elastomers such as SEPS, SEBS, and SIS; and olefin-based rubbers such as IR, EPR, and EPDM. Among these, from the viewpoint of compatibility with the acrylic block copolymers (I) and (II) contained in the resin composition, polymethyl methacrylate, (meth)acrylic acid ester polymer or copolymer, ethylene-vinyl acetate copolymer, AS resin, styrene-methyl methacrylate-maleic anhydride copolymer, polylactic acid, and polyvinylidene fluoride are preferred, and polymethyl methacrylate, (meth)acrylic acid ester copolymer, and styrene-methyl methacrylate-maleic anhydride copolymer are more preferred.

[0080] Examples of the (meth)acrylic acid ester polymer or copolymer include polymethyl acrylate, polyn-butyl acrylate, poly2-ethylhexyl acrylate, a random copolymer of methyl methacrylate and methyl acrylate, a random copolymer of methyl methacrylate and n-butyl acrylate, and diblock copolymers and triblock copolymers each comprising at least one polymer block consisting of a methacrylic acid ester unit and at least one polymer block consisting of an acrylic acid ester unit (however, the diblock copolymers and triblock copolymers do not include the acrylic block copolymer (I) and acrylic block copolymer (II) of the present invention).

[0081] When the resin composition of the present invention contains a tackifying resin, it is possible to impart pressure-sensitive adhesive properties (adhesiveness) to a layer made of the resin composition. Furthermore, when the resin composition is used as a pressure-sensitive adhesive, it becomes easy to adjust the tack, adhesive strength, and holding power. Examples of the tackifying resin include natural resins such as rosin-based resins and terpene-based resins; and synthetic resins such as petroleum resins, hydrogenated (hereinafter sometimes referred to as "hydrogenated") petroleum resins, styrene-based resins, coumarone-indene-based resins, phenolic resins, and xylene-based resins. Furthermore, when a tackifying resin is contained, from the viewpoint of adhesive strength and durability, the content thereof is preferably 1 to 100 parts by mass, more preferably 3 to 70 parts by mass, even more preferably 5 to 50 parts by mass, particularly preferably 5 to 40 parts by mass, and most preferably 5 to 35 parts by mass, per 100 parts by mass of the combined total of the acrylic block copolymer (I) and the acrylic block copolymer (II).

[0082] Examples of the rosin resin include rosins such as gum rosin, tall oil rosin, and wood rosin; modified rosins such as hydrogenated rosin, disproportionated rosin, and polymerized rosin; and rosin esters such as glycerin esters and pentaerythritol esters of these rosins and modified rosins. Specific examples of the rosins include Pine Crystal KE-100, Pine Crystal KE-311, Pine Crystal KE-359, Pine Crystal KE-604, and Pine Crystal D-6250 (all manufactured by Arakawa Chemical Industries, Ltd.).

[0083] Examples of the terpene resins include terpene resins based on α-pinene, β-pinene, dipentene, etc., aromatic modified terpene resins, hydrogenated terpene resins, terpene phenol resins, etc. Specific examples of the terpene resins include Tamanol 901 (manufactured by Arakawa Chemical Industries, Ltd.). Examples of the (hydrogenated) petroleum resins include (hydrogenated) aliphatic (C5) petroleum resins, (hydrogenated) aromatic (C9) petroleum resins, (hydrogenated) copolymer (C5 / C9) petroleum resins, (hydrogenated) dicyclopentadiene petroleum resins, and alicyclic saturated hydrocarbon resins. Examples of the styrene resins include poly-α-methylstyrene, α-methylstyrene / styrene copolymers, styrene-based monomer / aliphatic monomer copolymers, styrene-based monomer / α-methylstyrene / aliphatic monomer copolymers, styrene-based monomer copolymers, and styrene-based monomer / aromatic monomer copolymers. Specific examples of the styrene-based resin include FTR6000 series and FTR7000 series (manufactured by Mitsui Chemicals, Inc.).

[0084] Among the above tackifier resins, rosin-based resins, terpene-based resins, (hydrogenated) petroleum resins, and styrene-based resins are preferred in terms of exhibiting high adhesive strength, and of these, rosin-based resins are preferred in terms of enhancing adhesiveness, and disproportionated or hydrogenated rosins purified by distillation, recrystallization, extraction, or other procedures are even more preferred in terms of suppressing light resistance degradation, coloration, and the generation of bubbles due to impurities. These may be used alone, or two or more types may be used in combination. Furthermore, the softening point of the tackifier resin is preferably 50 to 150°C in terms of exhibiting high adhesive strength.

[0085] Examples of the plasticizer include fatty acid esters such as dibutyl phthalate, di-n-octyl phthalate, di-2-ethylhexyl phthalate, di-n-decyl phthalate, and diisodecyl phthalate; sebacates such as di-2-ethylhexyl sebacate and di-n-butyl sebacate; azelaates such as di-2-ethylhexyl azelaate; and adipates such as di-2-ethylhexyl adipate and di-n-octyl adipate; paraffins such as chlorinated paraffin; and polypropylene. Examples of suitable oils include glycols such as pyrene glycol; epoxy polymer plasticizers such as epoxidized soybean oil and epoxidized linseed oil; phosphates such as trioctyl phosphate and triphenyl phosphate; phosphites such as triphenyl phosphite; acrylic oligomers such as poly(n-butyl meth)acrylate and poly(2-ethylhexyl meth)acrylate; polybutene; polyisobutylene; polyisoprene; process oil; and naphthenic oil. These may be used alone or in combination of two or more.

[0086] Examples of the filler include inorganic and organic fibers such as glass fiber and carbon fiber; and inorganic fillers such as calcium carbonate, talc, carbon black, titanium oxide, silica, clay, barium sulfate, and magnesium carbonate. The inclusion of inorganic fibers and organic fibers imparts durability to the resulting resin composition. The inclusion of inorganic fillers imparts heat resistance and weather resistance to the resulting resin composition. Furthermore, the inclusion of titanium oxide tends to impart light-shielding properties to the resulting resin composition. The amount of titanium oxide added to the resin composition is preferably 20 to 250 parts by mass, more preferably 30 to 150 parts by mass, per 100 parts by mass of the total of the acrylic block copolymer (I) and the acrylic block copolymer (II).

[0087] When the resin composition of the present invention is used together with a curing agent, it can be suitably used as a layer made of a UV-curable resin composition. It can also be suitably used as a UV-curable pressure-sensitive adhesive. Examples of the curing agent include photocuring agents such as UV curing agents and heat curing agents, such as benzoins, benzoin ethers, benzophenones, anthraquinones, benzils, acetophenones, and diacetyls. Specific examples include benzoin, α-methylolbenzoin, α-t-butylbenzoin, benzoin methyl ether, benzoin ethyl ether, benzoin-n-propyl ether, benzoin isopropyl ether, benzoin isobutyl ether, α-methylolbenzoin methyl ether, α-methoxybenzoin methyl ether, benzoin phenyl ether, benzophenone, 9,10-anthraquinone, 2-ethyl-9,10-anthraquinone, benzil, 2,2-dimethoxy-1,2-diphenylethan-1-one (2,2-dimethoxy-2-phenylacetophenone), and diacetyl. The curing agent may be used alone or in combination of two or more. In order to enhance the effect of these curing agents, monomers such as (meth)acrylic acid, (meth)acrylic acid esters, (meth)acrylamide, (meth)acrylamide derivatives, vinyl esters, vinyl ethers, styrene derivatives, etc., or oligomers containing the above-mentioned monomers as constituent components may be further added. In addition to these monomers, a crosslinking agent consisting of a difunctional or higher functional monomer or oligomer may also be added.

[0088] The resin composition of the present invention has excellent weather resistance because it contains the acrylic block copolymer (I) and the acrylic block copolymer (II). However, by adding an antioxidant, an ultraviolet absorber, and a light stabilizer to the resin composition, even higher weather resistance can be achieved. Examples of antioxidants include phenolic antioxidants and phosphorus-based antioxidants. Examples of ultraviolet absorbers include benzotriazole-based ultraviolet absorbers. Examples of light stabilizers include hindered amine-based light stabilizers. These may be contained alone or in combination. In a preferred embodiment, all of the antioxidant, ultraviolet absorber, and light stabilizer are contained in the molded product. The amount of each of the components added to the resin composition of the present invention is preferably 0.01 to 1.0 part by mass, more preferably 0.03 to 0.60 part by mass, per 100 parts by mass of the combined total of the acrylic block copolymer (I) and the acrylic block copolymer (II).

[0089] The method for producing the resin composition of the present invention is not particularly limited. For example, the resin composition can be produced by mixing the components at a temperature within the range of 100 to 300°C using a known mixing or kneading device such as an extruder (e.g., kneader-ruder or twin-screw extruder), a mixing roll, or a Banbury mixer. Alternatively, the resin composition can be produced by dissolving the components in an organic solvent, mixing them, and then distilling off the organic solvent. The resulting composition can be thermally melted and laminated with a layer of a resin composition containing a plasticizer, as described below. The resulting resin composition can also be thermally melted and used as a hot-melt adhesive, for example.

[0090] When the resin composition of the present invention is produced by dissolving and mixing the components of the resin composition in an organic solvent and then evaporating the organic solvent, the resin composition can be applied to a layer of a resin composition containing a plasticizer before evaporating the organic solvent, and then laminating the layer of the resin composition. When the resin composition is used as a pressure-sensitive adhesive, the components are dissolved and mixed in an organic solvent and then evaporating the organic solvent to produce a pressure-sensitive adhesive. The pressure-sensitive adhesive can be applied to an adherend before evaporating the organic solvent, and then evaporating the organic solvent to achieve heat-sensitive bonding. When the resin composition of the present invention is used by heating and melting it, a low melt viscosity is preferred from the standpoints of processability and handling. For example, when hot-melt coating is used, the melt viscosity at around 200°C is preferably 50,000 mPa·s or less, and more preferably 30,000 mPa·s or less.

[0091] Furthermore, when the raw materials for the resin composition of the present invention include, in addition to the acrylic block copolymer (I) and the acrylic block copolymer (II), other polymers or additives or other components added as needed, a method of melt-mixing these raw materials using the above-mentioned apparatus or the like is recommended in order to improve the dispersibility of each component contained in the raw materials. In particular, the use of a twin-screw extruder is preferred from the viewpoint of improving the kneadability and compatibility of the acrylic block copolymer (I) and the acrylic block copolymer (II) contained in the resin composition of the present invention with the components added as needed. The mixing temperature can be adjusted appropriately depending on the acrylic block copolymer (I) and the acrylic block copolymer (II) and the components added as needed, and mixing is usually performed at a temperature within the range of 110°C to 300°C.

[0092] The resin composition of the present invention thus obtained can be formed at a sufficiently low temperature and can be subjected to heat-sensitive adhesive processing or hot-melt coating processing at a sufficiently low temperature, and these processing can be performed at a temperature of preferably 180°C or less, more preferably 150 to 180°C.

[0093] The resin composition of the present invention is preferably such that, when a cylindrical test piece having a thickness of 1 mm and a diameter of 25 mm obtained by molding the resin composition is immersed in oleic acid and stored at 25°C for 168 hours, the mass change rate [(mass of test piece after immersion) - (mass of test piece before immersion)] / (mass of test piece before immersion) x 100 is 200% or less. A resin composition having such characteristics can more adequately suppress contamination by substances contained in sebum, particularly oleic acid. From this perspective, the mass change rate is more preferably 180% or less, and even more preferably 160% or less.

[0094] The resin composition of the present invention can be molded into a molded article by a commonly used molding method. Examples of the molding method include melt molding methods involving heating and melting, such as extrusion molding, injection molding, compression molding, blow molding, calendar molding, and vacuum molding, and solution casting. Among these molding methods, melt molding is preferred from the viewpoint of ease of handling of the resin composition of the present invention. This molding method can produce molded articles of any shape, such as molded articles, pipes, sheets, films, fibrous articles, and laminates having layers composed of a resin composition containing the acrylic block copolymer (I) and the acrylic block copolymer (II). The hardness of the molded article is preferably 7.5 to 75, more preferably 8 to 65, and even more preferably 10 to 60, from the viewpoint of the physical properties and flexibility of the molded article.

[0095] When the molded article is a monolayer body, a monolayer body containing the resin composition of the present invention can be produced by extrusion molding or injection molding the raw material of the molded article (e.g., pellets made of the resin composition of the present invention). Examples of extrusion molding methods include the T-die method and the inflation method, and among these, the T-die method is preferred. By extrusion molding, the monolayer body can be produced without using a solvent and can be produced using relatively simple production equipment. By producing the monolayer body by extrusion molding, the production process is simplified and the production cost of the monolayer body can be reduced.

[0096] According to the T-die method, for example, the resin composition of the present invention (e.g., pellets made of the resin composition of the present invention), which is the raw material for the molded body, can be heated and melted and extruded through a T-die to produce a single-layer body.

[0097] When a molded article obtained from the resin composition of the present invention is a laminate, a laminate having a polymer layer containing the acrylic block copolymer (I) and the acrylic block copolymer (II) and a substrate layer can be produced by extrusion molding the resin composition of the present invention (e.g., pellets of the resin composition of the present invention), which is the raw material of the molded article, onto a substrate layer. Examples of extrusion molding methods include the T-die method and the inflation method, and among these, the T-die method is preferred. By extrusion molding, a laminate can be produced without using a solvent and can be produced using relatively simple production equipment. By producing a laminate by extrusion molding, the production process is simplified and the production cost of the laminate can be reduced.

[0098] According to an extrusion lamination method, which is an example of the T-die method, for example, the resin composition of the present invention (e.g., pellets of the resin composition of the present invention), which is the raw material of the molded product, is heated and melted and extruded from a T-die onto a substrate layer, and a polymer layer is laminated on the substrate layer, thereby producing a laminate including a layer containing the resin composition of the present invention and a substrate layer. Furthermore, according to a co-extrusion molding method, which is another example of the T-die method, for example, a laminate including a layer containing the resin composition of the present invention and a substrate layer can be produced by heating and melting both the raw materials of the layer containing the resin composition and the raw materials of the substrate layer and extruding them simultaneously.

[0099] In the extrusion lamination method, the resin composition of the present invention is preferably extruded through a die at a temperature of 140 to 260° C. in order to obtain good adhesiveness with the substrate layer.

[0100] Examples of the substrate layer include synthetic polymer film and sheet, metal foil, paper, cellophane, nonwoven fabric, woven fabric, etc. Examples of synthetic polymer compounds include, but are not limited to, polyethylene terephthalate, polyethylene naphthalate, triacetyl cellulose, polyamide, polyvinyl alcohol, polycarbonate, cycloolefin resin, styrene-methyl methacrylate copolymer, polyvinyl chloride, ethylene-vinyl acetate copolymer, polymethyl methacrylate, polyethylene, polypropylene, and mixtures of two or more of these polymers. The synthetic polymer compound may also be a copolymer in which various monomers are copolymerized. These films and sheets may be further vapor-deposited with aluminum, alumina, or silicon dioxide. These synthetic polymer film and sheet may also be printed with urethane ink, etc.

[0101] Examples of metal foils include aluminum foil and copper foil, and examples of papers include kraft paper, fine paper, and glassine paper. Examples of nonwoven fabrics include nonwoven fabrics made of aramid fiber, glass fiber, cellulose fiber, nylon fiber, vinylon fiber, polyester fiber, polyolefin fiber, rayon fiber, etc. Examples of woven fabrics include woven fabrics made of aramid fiber, glass fiber, cellulose fiber, nylon fiber, vinylon fiber, polyester fiber, polyolefin fiber, rayon fiber, etc.

[0102] Examples of the laminate structure include a two-layer structure of a layer containing the resin composition of the present invention and a substrate layer, a three-layer structure of two substrate layers and a layer containing the resin composition of the present invention (substrate layer / resin composition layer / substrate layer), a four-layer structure of a substrate layer and two different resin composition layers (a) and resin composition layer (b) containing the resin composition of the present invention and a substrate layer (substrate layer / resin composition layer (a) / resin composition layer (b) / substrate layer), a four-layer structure of a substrate layer and a layer containing the resin composition of the present invention and a layer containing the resin composition of the present invention (a) and a layer containing the resin composition of the present invention (c) and a substrate layer (substrate layer / resin composition layer (a) / resin composition layer (c) / substrate layer), and a five-layer structure of three substrate layers and two layers containing the resin composition of the present invention (substrate layer / resin composition layer / substrate layer / resin composition layer / substrate layer), but are not limited thereto.

[0103] The thickness ratio of the base material layer of the laminate to the layer containing the resin composition of the present invention is not particularly limited, but in view of the durability and handleability of the resulting laminate, the base material layer / resin composition layer is preferably in the range of 1 / 1000 to 1000 / 1, and more preferably in the range of 1 / 200 to 200 / 1.

[0104] The adhesive surface of the substrate layer in contact with the layer containing the resin composition of the present invention may be oxidized by air or ozone gas. Furthermore, in order to enhance adhesion to the resin composition layer, the adhesive surface of the substrate layer may be subjected to a known surface treatment such as anchor coating agent treatment, corona discharge treatment, flame treatment, or plasma treatment. Furthermore, an anchor layer may be formed on the surface of at least one of the resin composition layer and the substrate layer using an adhesive resin or the like.

[0105] Examples of resins used for such anchor layers include ethylene-vinyl acetate copolymers, ethylene-methyl methacrylate copolymers, ionomers, block copolymers (for example, styrene-based triblock copolymers and diblock copolymers such as SIS and SBS), ethylene-acrylic acid copolymers, ethylene-methacrylic acid copolymers, etc. The anchor layer may consist of one layer or two or more layers.

[0106] The method for forming the anchor layer is not particularly limited, and examples thereof include a method of forming an anchor layer by applying a solution containing the above-mentioned resin to a substrate layer, and a method of heating and melting a composition containing the above-mentioned resin or the like that will become the anchor layer, and forming an anchor layer on the surface of the substrate layer using a T-die or the like.

[0107] Co-extrusion molding methods, which are examples of the T-die method, may be either the feed block method or the multi-manifold method, which can be used to create multilayer structures, such as two-kind, two-layer laminates consisting of a substrate layer and a layer containing the resin composition of the present invention, or three-kind, three-layer laminates having an intermediate layer between the substrate layer and the resin composition layer.

[0108] Materials that can be used as the substrate layer in the co-extrusion molding method include various synthetic polymer compounds, and suitable examples of the synthetic polymer compounds include polyolefins.

[0109] Examples of polyolefin-based materials include low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, ethylene-α-olefin copolymer, ethylene-vinyl acetate copolymer, ethylene-ethyl acrylate copolymer, ethylene-methyl methacrylate copolymer, ethylene-n-butyl acrylate copolymer, and polypropylene (homopolymer, random copolymer, block copolymer). These polyolefin-based materials may be used alone or as a mixture or composition of any combination. In particular, polypropylene block copolymers are preferred as the material for the base layer.

[0110] The substrate layer may contain additives such as pigments, antioxidants, stabilizers, and ultraviolet absorbers as needed. Furthermore, the substrate layer in the laminate is not limited to a single layer, and may have multiple substrate layers. The total thickness of the substrate layer consisting of a single layer or multiple layers is preferably, for example, 20 μm or more and 100 μm or less.

[0111] The laminate may also have an intermediate layer. Examples of resins that can be used as the intermediate layer include ethylene-vinyl acetate copolymers, ethylene-methyl methacrylate copolymers, ionomers, block copolymers (e.g., styrene-based triblock copolymers and diblock copolymers such as SIS and SBS), ethylene-acrylic acid copolymers, and ethylene-methacrylic acid copolymers. The intermediate layer may be a single layer or may be two or more layers, and can be formed by simultaneously co-extrusion molding the base layer and the layer containing the resin composition of the present invention.

[0112] When the molded article obtained from the resin composition of the present invention is a multi-layered article such as a molded article or a sheet, the resin composition of the present invention (e.g., pellets of the resin composition of the present invention) can be injection molded to produce a multi-layered article having a layer (Z) containing the resin composition of the present invention and a polymer layer (Y) made of a material other than the resin composition of the present invention. Examples of injection molding methods include two-color molding and insert molding.

[0113] Examples of polymers constituting the polymer layer (Y) (hereinafter also referred to as layer (Y)) made of a material other than the resin composition of the present invention include acrylic resins such as polymethyl methacrylate and (meth)acrylic acid ester copolymers; olefin resins such as polyethylene, ethylene-vinyl acetate copolymer, polypropylene, polybutene-1, poly-4-methylpentene-1, and polynorbornene; ethylene ionomers; styrene resins such as polystyrene, styrene-maleic anhydride copolymer, high impact polystyrene, AS resin, ABS resin, AES resin, AAS resin, ACS resin, and MBS resin; styrene-methyl methacrylate copolymer; and polyethylene. Examples of suitable resins include polyester resins such as polyethylene terephthalate, amorphous polyethylene terephthalate (PET-G), polybutylene terephthalate, and polylactic acid; polyamides such as nylon 6, nylon 66, and polyamide elastomers; polycarbonate; polyvinyl chloride; polyvinylidene chloride; polyvinyl alcohol; ethylene-vinyl alcohol copolymers; polyacetal; polyvinylidene fluoride; polyurethane; modified polyphenylene ether; polyphenylene sulfide; silicone rubber-modified resins; acrylic rubber; silicone rubber; styrene-based thermoplastic elastomers such as SEPS, SEBS, and SIS; and olefin-based rubbers such as IR, EPR, and EPDM. This multilayer structure may have other layers in addition to the layer (Z) (hereinafter also referred to as layer (Z)) containing the resin composition of the present invention and the layer (Y).

[0114] Examples of the layer (Y) include a layer (YI) containing a polar resin. Examples of the polar resin include acrylic resins such as polymethyl methacrylate and (meth)acrylic acid ester copolymers; styrene resins such as polystyrene, styrene-maleic anhydride copolymer, high-impact polystyrene, AS resin, ABS resin, AES resin, AAS resin, ACS resin, and MBS resin; styrene-methyl methacrylate copolymers; polyester resins such as polyethylene terephthalate, amorphous polyethylene terephthalate (PET-G), polybutylene terephthalate, and polylactic acid; polyamides such as nylon 6, nylon 66, and polyamide elastomers; polycarbonate; polyvinyl chloride; polyvinylidene chloride; polyvinyl alcohol; ethylene-vinyl alcohol copolymer; polyacetal; polyvinylidene fluoride; polyurethane; modified polyphenylene ether; polyphenylene sulfide; silicone rubber-modified resins; acrylic rubber; and silicone rubber.

[0115] In the multilayer structure, the layer (Z) and the layer (YI) are preferably adjacent to each other. The multilayer structure has a layer (Z) that is excellent in low tack, transparency, flexibility, and impact absorption. Even when a highly rigid polar resin is used for the polar resin-containing layer (YI), the multilayer structure can also have excellent properties such as flexibility and impact absorption.

[0116] The thicknesses of the layer (Z) and the layer (Y) constituting the multilayer body are not particularly limited, but from the viewpoint of excellent flexibility and impact absorption of the molded body, the thickness of the layer (Z) is preferably 0.1 to 10 mm, more preferably 0.3 to 5 mm, even more preferably 0.5 to 3 mm, 0.7 to 2 mm, or even 1 to 1.5 mm. The thickness of the layer (Y) is preferably 0.3 to 10 mm, more preferably 0.5 to 5 mm, and even more preferably 1 to 3 mm.

[0117] Specific methods for producing the above-mentioned multilayer body include, for example, a method in which the layer (Z) and the layer (Y) are molded separately in advance and then laminated (Method 1); a method in which the pellets of the present invention in a molten state are disposed on the layer (Y) produced in advance to form the layer (Z) (Method 2); a method in which a polymer in a molten state is disposed on the layer (Z) produced in advance to form the layer (Y) (Method 3), and the like. Among these, methods 2 and 3 are preferred because the adhesive strength between the layer (Z) and the layer (Y) is improved, and method 2 is more preferred because the desired molded body can be easily obtained. In addition, since the resin composition of the present invention (typically pellets of the resin composition of the present invention) has excellent melt fluidity, it is preferable to form the layer (Z) by injection molding, and in particular, it is more preferable to adopt insert molding, in which the pre-molded layer (Y) is placed in a mold and then the resin composition of the present invention in a molten state is injected.

[0118] The applications of the resin composition of the present invention and the molded article obtained from the resin composition are not particularly limited, but because the resin composition of the present invention has excellent heat resistance, transparency, and flexibility, and the appearance of the molded article is excellent, it can be used in a wide range of applications such as the optical field, food field, medical field, consumer field, automotive field, electrical / electronic field, and construction field. The molded article obtained from the resin composition may have various shapes, such as pellets, sheets, plates, pipes, tubes, belts, hoses, rods, and granules.

[0119] In the automotive field, for example, by using this material as automotive interior and exterior components in car audio panels, instrument panels, dashboards, airbag covers, bumper parts, body panels, weather strips, grommets, glass run channels, rack and pinion boots, suspension boots, constant velocity joint boots, side moldings, mudguards, emblems, leather seats, floor mats, armrests, steering wheel coverings, belt line moldings, flush mounts, gears, knobs, etc., it is possible to take advantage of its flexibility and transparency to impart never-before-seen functions, designs, and aesthetic appeal.

[0120] In the electrical and electronics fields, the excellent heat resistance of the material makes it suitable for use as a cover for electronic devices, making it possible to prevent deformation of smartphone covers due to heat generation in smartphone terminals, for example. Furthermore, the excellent transparency and flexibility of the material make it possible to add design and decorative features, and it is easy to attach and remove.

[0121] Other uses include various covers, various terminal boards, printed wiring boards; viewfinders, filters, prisms, Fresnel lenses (used in, for example, speakers, microscopes, binoculars, cameras, clocks, VTRs, projection TVs, etc.); substrate protective films for various optical discs (VD, CD, DVD, MD, LD, etc.), optical switches, optical connectors, liquid crystal displays, light guiding films and sheets for liquid crystal displays, flat panel displays, light guiding films and sheets for flat panel displays, plasma displays, light guiding films and sheets for plasma displays, retardation films and sheets, polarizing films and sheets, polarizer protective films and sheets, wave plates, light diffusion films and sheets, prism films and sheets, reflective films and sheets, anti-reflection films and sheets, viewing angle widening films and sheets, anti-glare films and sheets, brightness enhancement films and sheets, display element substrates for liquid crystal and electroluminescent applications, touch panels, light guiding films and sheets for touch panels, and spacers between various front panels and various modules.

[0122] Furthermore, the present invention can also be used in various liquid crystal display elements such as mobile phones, digital information terminals, pagers, navigation systems, in-vehicle liquid crystal displays, liquid crystal monitors, light control panels, displays for office automation equipment, and displays for audiovisual equipment, as well as electroluminescence display elements and touch panels.

[0123] Furthermore, because of its excellent heat resistance, flexibility, etc., it can be suitably applied to, for example, interior and exterior building materials such as curtain walls, roofing materials, window materials, gutters, exteriors, wall materials, flooring materials, fixtures, coated steel plates, coated plywood, and sealing packings for door and window frames.

[0124] It can also be applied to road construction materials, retroreflective films and sheets, light-shielding films and sheets, heat-shielding films and sheets, agricultural films and sheets, lighting covers, signs, translucent sound-insulating walls, and the like.

[0125] Furthermore, various types of vibration-damping rubber and vibration-damping materials such as vibration-proof rubber, mats, sheets, cushions, dampers, pads, and mount rubber; footwear materials such as sports shoes and fashion sandals; home appliance components such as televisions, stereos, vacuum cleaners, and refrigerators; grips for scissors, screwdrivers, toothbrushes, pens, cameras, ski poles, and the like; office machine parts such as copier feed rollers and take-up rollers; furniture such as sofas and chair seats; parts such as switch covers, casters, stoppers, foot rubber, and earphones; underwater goggles, snorkels, ski boots, snowboard boots, It can be effectively used in a wide range of applications, including sporting goods such as ski and snowboard coverings and golf ball covers; industrial materials such as conveyor belts, electric belts and pelletizer rolls; elastic parts for sanitary materials such as disposable diapers, poultices and bandages; band applications such as hair bands, wristbands, watch bands and eyeglass bands; food packaging materials such as food wrap film; medical devices such as infusion bags, syringes, catheters and rolling tubes; stoppers for containers that store food, beverages, medicines and the like; snow chains, electrical wire covering materials, trays, films, sheets, stationery, toys and daily commodities.

[0126] Furthermore, the laminate, which is one type of molded article of the present invention, can be used for various applications. Examples include pressure-sensitive adhesive tapes and films for surface protection, masking, wrapping / packaging, office use, labeling, decoration / display, bookbinding, dicing tape, medical / hygienic use, laminated glass, shatterproof glass, electrical insulation, holding and fixing electronic devices, semiconductor manufacturing, optical display films, pressure-sensitive adhesive optical films, electromagnetic wave shielding, and sealing materials for electric / electronic components. Specific examples are given below.

[0127] The surface protection applications include various materials such as metals, plastics, rubber, and wood. Specifically, the surface protection applications include painted surfaces, metal plastic working and deep drawing, automotive components, and optical components. Examples of automotive components include painted exterior panels, wheels, mirrors, windows, lights, and light covers. Examples of optical components include various image display devices such as liquid crystal displays, organic electroluminescent displays, plasma displays, and field emission displays; polarizing films, polarizing plates, retardation plates, light guide plates, diffusers, and films constituting optical disks such as DVDs; and precision fine-coated faceplates for electronic and optical applications.

[0128] Masking applications include masking during the manufacture of printed circuit boards and flexible printed circuit boards; masking during plating and soldering processes in electronic devices; and masking during the manufacture of automobiles and other vehicles, painting of vehicles and buildings, textile printing, and civil engineering work cut-offs.

[0129] Packaging applications include heavy-duty packaging, export packaging, sealing cardboard boxes, can seals, etc. Office applications include general office use, sealing, book repair, drafting, memos, etc. Label applications include price and product indication, shipping tags, POP, stickers, stripes, nameplates, decorations, advertising, marking films, etc.

[0130] Label applications include labels having a substrate layer made of paper, processed paper (paper that has been subjected to aluminum vapor deposition, aluminum lamination, varnishing, resin coating, etc.), synthetic paper, etc., cellophane, plastic material, cloth, wood, metal film, etc. Examples of substrate layers include fine paper, art paper, cast paper, thermal paper, wheel paper, polyethylene terephthalate film, polyvinyl chloride film, OPP film, polylactic acid film, synthetic paper, synthetic thermal paper, overlamination film, etc.

[0131] Examples of substrates to which the label can be applied include plastic products such as plastic bottles and foam plastic cases; paper and cardboard products such as cardboard boxes; glass products such as glass bottles; metal products; and other inorganic material products such as ceramics.

[0132] Examples of decorative and display applications include danger sign stickers, line tape, wiring markings, phosphorescent tape, and reflective sheets.

[0133] Examples of applications of pressure-sensitive adhesive optical films include polarizing films, polarizing plates, retardation films, viewing angle widening films, brightness improving films, anti-reflection films, anti-glare films, color filters, light guide plates, diffusion films, prism sheets, electromagnetic wave shielding films, near-infrared absorbing films, functional composite optical films, ITO lamination films, impact resistance imparting films, visibility improving films, and other optical films having a pressure-sensitive adhesive layer formed on at least a portion or all of one or both sides. Such pressure-sensitive adhesive optical films also include protective films used for surface protection of the optical films. Pressure-sensitive adhesive optical films are suitable for use in various image display devices such as liquid crystal displays, PDPs, organic EL displays, electronic paper, game consoles, and mobile terminals.

[0134] Electrical insulation applications include protective coating or insulation for coils, and interlayer insulation for motors, transformers, etc. Electronic device holding and fixing applications include carrier tape, packaging, CRT fixing, splicing, rib reinforcement, etc. Semiconductor manufacturing applications include protection of silicone wafers, etc.

[0135] Medical and hygienic applications include transdermal drug applications such as analgesics and anti-inflammatory agents (plasters, poultices), cold patches, antipruritic patches, and keratin softeners; various tape applications such as first-aid adhesive bandages (containing disinfectants), surgical dressings and surgical tapes, adhesive plasters, hemostatic tapes, tapes for human waste disposal devices (artificial anus fixation tapes), suture tapes, antibacterial tapes, fixation taping, self-adhesive bandages, oral mucosa adhesive tapes, sports tapes, and hair removal tapes; cosmetic applications such as face packs, eye moisturizing sheets, and keratin peeling packs; binding applications for hygienic materials such as diapers and pet sheets; cooling sheets, heated warmers, dustproof and waterproof applications, and pest catching applications.

[0136] Examples of applications for sealing electronic and electrical components include liquid crystal displays, organic EL displays, organic EL lighting, and solar cells.

[0137] As for applications for laminated glass, it is effectively used for automobile windshields, automobile side glass, automobile sunroofs, automobile rear glass, glass for head-up displays, etc.

[0138] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. Various physical properties in the examples and comparative examples were measured or evaluated by the following methods.

[0139] "Weight average molecular weight (Mw), number average molecular weight (Mn), and molecular weight distribution (Mw / Mn)" The weight average molecular weight and number average molecular weight of the acrylic block copolymer were determined in terms of polystyrene by gel permeation chromatography (hereinafter abbreviated as GPC), and the molecular weight distribution was calculated from these values. The detailed conditions for measuring the molecular weight are as follows: Apparatus: GPC apparatus "HLC-8020" manufactured by Tosoh Corporation Separation column: Two "TSK-gel SuperMultipore HZ M" manufactured by Tosoh Corporation connected in series Eluent: Tetrahydrofuran Eluent flow rate: 0.36 ml / min Column temperature: 40°C Detection method: Differential refractive index (RI)

[0140] "Constituent ratio of each polymer block" 1 The content was determined by H-NMR measurement. Apparatus: Nuclear magnetic resonance apparatus "JNM-LA400" manufactured by JEOL Ltd. Deuterated solvent: deuterated chloroform 1In the H-NMR spectrum, the signals at around 3.6 ppm, 3.7 ppm, and 4.0 ppm were assigned to a hydrogen atom (-O-CH3) bonded to the carbon atom adjacent to the oxygen atom contained in the ester group of the methyl methacrylate unit, a hydrogen atom (-O-CH3) bonded to the carbon atom adjacent to the oxygen atom contained in the ester group of the methyl acrylate unit, a hydrogen atom (-O-CH2-CH2-CH2-CH3) bonded to the carbon atom adjacent to the oxygen atom contained in the ester group of the n-butyl acrylate unit, and a hydrogen atom (-O-CH2-CH2-CH2-CH3) bonded to the carbon atom adjacent to the oxygen atom contained in the ester group of the 2-ethylhexyl acrylate unit. The molar ratio of each monomer unit was determined from the ratio of these integral values, and this was converted to a mass ratio based on the molecular weight of the monomer unit to determine the content of each polymer block. The mass proportion of the methyl methacrylate units contained in the acrylic block copolymer was designated as (H), and the mass proportion of the acrylic ester units was designated as (J).

[0141] "Calculation of solubility parameters SP(A1) and SP(B1) of polymer blocks (A1) and (B1)" The solubility parameters SP(A1) and SP(B1) of polymer blocks (A1) and (B1) were determined by the Fedors estimation method. The values ​​described above were used as they were for the methyl acrylate units, n-butyl acrylate units, and 2-ethylhexyl acrylate units contained in each polymer block. Details of the case where each polymer block is a polymer block composed of multiple monomer units will be described below with reference to examples.

[0142] The solubility parameter of the polymer block was calculated using the solubility parameter of the homopolymer corresponding to the monomer unit contained in the polymer block. The solubility parameters of the homopolymers contained in the following synthesis examples were calculated from the ΔE and V of polymethyl acrylate (methyl acrylate unit), polyn-butyl acrylate (n-butyl acrylate unit), poly2-ethylhexyl acrylate (2-ethylhexyl acrylate unit), and polymethyl methacrylate (methyl methacrylate unit), and were 11.30 (cal / cm 3 )1 / 2 , 10.20 (cal / cm 3 ) 1 / 2 , 9.50 (cal / cm 3 ) 1 / 2 , 10.50 (cal / cm 3 ) 1 / 2 The solubility parameter SP(C) of oleic acid was calculated as 9.14 (cal / cm 3 ) 1 / 2 is.

[0143] When the polymer block (A1) (or the polymer block (B1)) is a copolymer composed of a plurality of monomer units, the calculation was carried out using the following formula: SP(X)=[Σ[φi×[SP(X)i]] 2 ]] 1 / 2 (In the formula, SP(X) is the solubility parameter of the polymer block (X), φi is the volume fraction of the monomer unit (i) in the polymer block (X), and SP(X)i is the solubility parameter of a homopolymer consisting of the monomer unit (i) calculated by the Fedors estimation method. The volume fraction was set to be the same as the mass proportion of each monomer unit constituting the polymer block.) The acrylic block copolymer (I-1) used in Example 1 had a polymer block (A1) content of 29 mass%, and the monomer units constituting the polymer block (B1) were n-butyl acrylate:methyl acrylate = 80:20 (mass ratio). From this and the solubility parameter calculated by the Fedors estimation method, the value serving as an index for the solubility parameter of the acrylic block copolymer (I-1) used in Example 1 was determined to be 10.46 (cal / cm 3 ) 1 / 2 he demanded.

[0144] "Oleic Acid Immersion Test" The press sheets prepared in the Examples and Comparative Examples were punched into disks with a diameter of 25 mm to prepare test specimens. First, the mass of the test specimen was measured, and this was designated as the mass before immersion (W1). Next, the test specimen was immersed in oleic acid at 25°C for 168 hours, and then the test specimen was removed and the oleic acid adhering to the surface was wiped off. The mass of this test specimen was measured, and this was designated as the mass after the immersion test (W2). Then, the mass change rate due to the immersion test (W2 - W1) / W1 was calculated as a percentage from W1 and W2.

[0145] "Hardness" The press sheets produced in the examples and comparative examples were cut into a length of 50 mm and a width of 50 mm, and six of the sheets were stacked to a thickness of 6 mm. The hardness was measured using a type A durometer indenter in accordance with JIS 6253-3:2021.

[0146] [Synthesis Example 1] <Acrylic Block Copolymer (I-1)> (1) A three-way stopcock was attached to a 2 L three-neck flask, and the inside of the flask was purged with nitrogen. Then, 1,154 g of toluene and 24.9 g of 1,2-dimethoxyethane were added with stirring at room temperature. Subsequently, 37.8 g of a toluene solution containing 19.0 mmol of isobutylbis(2,6-dibutyl-4-methylphenoxy)aluminum was added, followed by 1.89 g of a cyclohexane solution of sec-butyllithium containing 3.22 mol of sec-butyllithium. (2) Subsequently, 22.9 g of methyl methacrylate was added to the mixture. The reaction solution was initially yellow, but after stirring at room temperature for 60 minutes, it became colorless. (3) Subsequently, the internal temperature of the polymerization solution was cooled to -30°C, and 150 g of a mixture of methyl acrylate / n-butyl acrylate (mass ratio 20 / 80) was added dropwise over 2 hours. After completion of the dropwise addition, the mixture was stirred at -30°C for 5 minutes. (4) 38.2 g of methyl methacrylate was further added to the mixture, and the mixture was stirred overnight at room temperature. (5) 12.2 g of methanol was added to terminate the polymerization reaction, and the resulting reaction liquid was then poured into 15 kg of methanol to precipitate a white precipitate. The white precipitate was then recovered and dried, yielding 200 g of acrylic block copolymer (I-1).

[0147] Synthesis Example 2 Acrylic Block Copolymer (II-1) (1) A three-way stopcock was attached to a 2-L three-neck flask, and the inside of the flask was purged with nitrogen. Then, 936 g of toluene and 51.4 g of 1,2-dimethoxyethane were added with stirring at room temperature. Subsequently, 32.9 g of a toluene solution containing 16.5 mmol of isobutylbis(2,6-dibutyl-4-methylphenoxy)aluminum was added, followed by 3.88 g of a cyclohexane solution of sec-butyllithium containing 6.62 mol of sec-butyllithium. (2) Subsequently, 52.9 g of methyl methacrylate was added to the mixture. The reaction solution was initially yellow, but after stirring at room temperature for 60 minutes, it became colorless. (3) Subsequently, the internal temperature of the polymerization solution was cooled to -30°C, and 226 g of n-butyl acrylate was added dropwise over 2 hours. After the completion of the dropwise addition, the mixture was stirred at -30°C for 5 minutes. (4) Further, 46.2 g of methyl methacrylate was added to the mixture, and the mixture was stirred overnight at room temperature. (5) 13.7 g of methanol was added to terminate the polymerization reaction, and the resulting reaction liquid was then poured into 15 kg of methanol to precipitate a white precipitate. The white precipitate was then recovered and dried, yielding 300 g of acrylic block copolymer (II-1).

[0148] Synthesis Example 3 Acrylic Block Copolymer (II-2) (1) A three-way stopcock was attached to a 2-L three-neck flask, and the inside of the flask was purged with nitrogen. Then, 1,120 g of toluene and 1.96 g of 1,2-dimethoxyethane were added with stirring at room temperature. Subsequently, 16.9 g of a toluene solution containing 9.3 mmol of isobutylbis(2,6-dibutyl-4-methylphenoxy)aluminum was added, followed by 2.37 g of a cyclohexane solution of sec-butyllithium containing 4.6 mol of sec-butyllithium. (2) Subsequently, 24.2 g of methyl methacrylate was added to the reaction mixture. The reaction mixture was initially yellow, but after stirring for 60 minutes at room temperature, it became colorless. (3) Subsequently, the internal temperature of the polymerization mixture was cooled to -30°C, and 152 g of n-butyl acrylate was added dropwise over 2 hours. After the completion of the dropwise addition, the mixture was stirred at -30°C for 5 minutes. (4) Further, 24.2 g of methyl methacrylate was added to the reaction mixture, and the mixture was stirred overnight at room temperature. (5) After 8.3 g of methanol was added to terminate the polymerization reaction, the resulting reaction solution was poured into 15 kg of methanol to precipitate a white precipitate, which was then recovered and dried to obtain 200 g of an acrylic block copolymer (II-2).

[0149] Synthesis Example 4 Acrylic Block Copolymer (II-3) (1) A three-way stopcock was attached to a 2-L three-neck flask, and the inside of the flask was purged with nitrogen. Then, 938 g of toluene and 20.2 g of 1,2-dimethoxyethane were added with stirring at room temperature. Subsequently, 41.4 g of a toluene solution containing 20.8 mmol of isobutylbis(2,6-dibutyl-4-methylphenoxy)aluminum was added, followed by 1.53 g of a cyclohexane solution of sec-butyllithium containing 2.60 mol of sec-butyllithium. (2) Subsequently, 21.8 g of methyl methacrylate was added to the mixture. The reaction solution was initially yellow, but after stirring at room temperature for 60 minutes, it became colorless. (3) Subsequently, the internal temperature of the polymerization solution was cooled to −30° C., and 215 g of a mixture of 2-ethylhexyl acrylate / n-butyl acrylate (50 / 50 by mass) was added dropwise over 2 hours. After the completion of the dropwise addition, the mixture was stirred at −30° C. for 5 minutes. (4) 29.4 g of methyl methacrylate was further added to the mixture, and the mixture was stirred overnight at room temperature. 12.2 g of methanol was added to terminate the polymerization reaction, and the resulting reaction liquid was then poured into 15 kg of methanol to precipitate a white precipitate. The white precipitate was then recovered and dried to obtain 280 g of an acrylic block copolymer (II-3).

[0150] Synthesis Example 5 Acrylic Block Copolymer (II-4) (1) A 2-L three-neck flask was fitted with a three-way stopcock and the inside of the flask was purged with nitrogen. Then, 990 g of toluene and 11.2 g of 1,2-dimethoxyethane were added with stirring at room temperature. Subsequently, 31.1 g of a toluene solution containing 15.6 mmol of isobutylbis(2,6-dibutyl-4-methylphenoxy)aluminum was added, followed by 0.82 g of a cyclohexane solution of sec-butyllithium containing 1.39 mol of sec-butyllithium. (2) Subsequently, 11.0 g of methyl methacrylate was added to the mixture. The reaction solution was initially yellow, but after stirring at room temperature for 60 minutes, it became colorless. (3) Subsequently, the internal temperature of the polymerization solution was cooled to −30°C, and 157 g of 2-ethylhexyl acrylate was added dropwise over 2 hours. After the completion of the dropwise addition, the mixture was stirred at −30°C for 5 minutes. (4) Further, 12.4 g of methyl methacrylate was added to the mixture, and the mixture was stirred overnight at room temperature. (5) 17.3 g of methanol was added to terminate the polymerization reaction, and the resulting reaction liquid was then poured into 15 kg of methanol to precipitate a white precipitate. The white precipitate was then recovered and dried, yielding 180 g of acrylic block copolymer (II-4).

[0151] Synthesis Example 6 Acrylic Block Copolymer (II'-1) (1) A three-way stopcock was attached to a 2-L three-neck flask, and the inside of the flask was purged with nitrogen. Then, 936 g of toluene and 51.4 g of 1,2-dimethoxyethane were added with stirring at room temperature. Subsequently, 32.9 g of a toluene solution containing 16.5 mmol of isobutylbis(2,6-dibutyl-4-methylphenoxy)aluminum was added, followed by 4.10 g of a cyclohexane solution of sec-butyllithium containing 7.00 mmol of sec-butyllithium. (2) Subsequently, 65.0 g of methyl methacrylate was added to the reaction mixture. The reaction mixture was initially yellow, but after stirring for 60 minutes at room temperature, it became colorless. (3) Subsequently, the internal temperature of the polymerization mixture was cooled to -30°C, and 226 g of n-butyl acrylate was added dropwise over 2 hours. After the completion of the dropwise addition, the mixture was stirred for 5 minutes at -30°C. (4) 161 g of methyl methacrylate was added to the reaction mixture, and the mixture was stirred overnight at room temperature. (5) After 13.7 g of methanol was added to terminate the polymerization reaction, the resulting reaction solution was poured into 15 kg of methanol to precipitate a white precipitate, which was then recovered and dried to obtain 430 g of an acrylic block copolymer (II'-1).

[0152] The structures, weight-average molecular weights (Mw), molecular weight distributions (Mw / Mn), SP(A)-SP(B), (H)×SP(A)+(J)×SP(B), and mass change rates in an oleic acid immersion test of the acrylic block copolymers (I-1), (II-1) to (II-4), and (II'-1) obtained in Synthesis Examples 1 to 6 are shown in Table 1. SP(A) represents the solubility parameter of polymer block (A1) or polymer block (A2), and SP(B) represents the solubility parameter of polymer block (B1) or polymer block (B2).

[0153]

[0154] Examples 1 to 7 Acrylic block copolymer (I-1) and acrylic block copolymer (II-1), (II-2), (II-3), or (II-4) were dry-blended in advance in the proportions shown in Table 2 to prepare mixtures. These mixtures were melt-kneaded using a twin-screw extruder ("ZSK-25" manufactured by KRUPP WERNER & PFLEIDERER). The resulting melt-kneaded mixture was extruded from the twin-screw extruder and pelletized by a strand-cutting method. The resulting pellets were hot-press molded at 200°C to prepare pressed sheets (molded articles) measuring 150 mm x 150 mm x 1 mm thick. The resulting pressed sheets were evaluated by the oleic acid immersion test described above and their hardness was measured. The results are shown in Table 2.

[0155] Comparative Examples 1 and 2 Acrylic block copolymer (I-1) and acrylic block copolymer (II-4) or (II'-1) were dry-blended in advance in the proportions shown in Table 2 to prepare a mixture. This mixture was melt-kneaded using a twin-screw extruder ("ZSK-25" manufactured by KRUPP WERNER & PFLEIDERER). The resulting melt-kneaded mixture was extruded from the twin-screw extruder and pelletized by a strand-cutting method. The resulting pellets were hot-press molded at 200°C to prepare pressed sheets (molded articles) measuring 150 mm x 150 mm x 1 mm thick. The resulting pressed sheets were evaluated by the oleic acid immersion test described above and their hardness was measured. The results are shown in Table 2.

[0156]

[0157] As can be seen from the results in Table 2, the mass change rate in the oleic acid immersion test was small in Examples 1 to 7, which satisfied the requirements of the present invention. In addition, the molded bodies obtained in Examples 1 to 7 had low hardness and maintained flexibility.

[0158] On the other hand, in Comparative Example 1, a composition in which 500 parts by mass of acrylic block copolymer (II-4) was added to acrylic block copolymer (I-1) and a molded article of the composition were investigated. However, although the obtained molded article retained flexibility, the mass change rate in the oleic acid immersion test was large and the shape could not be maintained.

[0159] In Comparative Example 2, a composition in which 100 parts by mass of an acrylic block copolymer (II'-1) having a high content of polymer block (A2) was added to the acrylic block copolymer (I-1) and a molded article of the composition were investigated. However, although the obtained molded article showed a good result in terms of the mass change rate in an oleic acid immersion test, it was unable to maintain its flexibility.

Claims

1. A resin composition comprising 100 parts by mass of an acrylic block copolymer (I) having at least one polymer block (A1) containing a methacrylic acid ester unit and at least one polymer block (B1) containing an acrylic acid ester unit, and 15 to 400 parts by mass of an acrylic block copolymer (II) having at least one polymer block (A2) containing a methyl methacrylate unit and at least one polymer block (B2) containing an acrylic acid ester unit, wherein the content of polymer block (A1) in the acrylic block copolymer (I) is 20% by mass or more, and the polymer block (B1) of the acrylic block copolymer (I) is a copolymer represented by the general formula CH2=CH-COOR. 1 (1) (In formula (1), R 1 represents an organic group having 1 to 3 carbon atoms), and the acrylic block copolymer (I) satisfies the following formulas (i) and (ii): (i) (H)×SP(A1)+(J)×SP(B1)-SP(C)>1.20 (ii) -0.80≦SP(A1)-SP(B1)≦0.43 (in the formulas (i) and (ii), SP(A1) represents the solubility parameter (cal / cm) of the polymer block (A1). 3 ) 1 / 2 , SP(B1) is the solubility parameter (cal / cm) of the polymer block (B1) 3 ) 1 / 2 and SP(C) is the solubility parameter of oleic acid (cal / cm 3 ) 1 / 2 (H) represents the mass proportion of polymer block (A1) in the acrylic block copolymer (I), and (J) represents the mass proportion of polymer block (B1) in the acrylic block copolymer (I). The polymer block (B2) of the acrylic block copolymer (II) is represented by the general formula CH2=CH-COOR 2 (2) (In formula (2), R 2 represents an organic group having 4 to 12 carbon atoms), and the content of the polymer block (A2) in the acrylic block copolymer (II) is less than 35 mass%.

2. The resin composition according to claim 1, wherein the weight average molecular weights of both the acrylic block copolymers (I) and (II) are in the range of 30,000 to 300,000.

3. A cylindrical test piece having a thickness of 1 mm and a diameter of 25 mm obtained by molding the resin composition is immersed in oleic acid, and the mass change rate before and after storage at 25°C for 168 hours [(mass of the test piece after immersion) - (mass of the test piece before immersion)] / (mass of the test piece before immersion) × 100 is 200% or less. The resin composition according to claim 1 or 2.

4. The resin composition according to any one of claims 1 to 3, wherein the acrylate (b2-2) unit in the acrylic block copolymer (II) is an n-butyl acrylate unit.

5. The resin composition according to any one of claims 1 to 4, wherein the acrylate (b1-1) unit in the acrylic block copolymer (I) is a methyl acrylate unit.