Polycarbonate-based resin composition and molded object
Patent Information
- Application Number
- JP2023578549
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-11
AI Technical Summary
Conventional polycarbonate resin compositions face challenges in achieving a balance between melt fluidity, impact resistance, and heat resistance, as improving one property often compromises the others.
A polycarbonate resin composition is developed by blending a core-shell type elastomer with a fluidity improver containing a specific monomer composition and weight average molecular weight, along with a modifier, to enhance fluidity, impact resistance, and heat resistance, while potentially incorporating a flame retardant for improved flame retardancy.
The composition achieves a good balance of fluidity during melting, impact resistance, and heat resistance, allowing for reduced flame retardant usage and improved flame retardance, thus optimizing the properties of molded articles.
Abstract
Description
Polycarbonate resin composition and molded article
[0001] The present invention relates to a resin composition containing a polycarbonate resin and a molded article thereof.
[0002] Molded articles made from polycarbonate resins have excellent transparency, impact resistance, heat resistance, dimensional stability, and self-extinguishing properties (flame retardancy), and are used in a wide range of fields, including electrical, electronic, and office equipment, optical components, precision machinery, automobiles, security and medical care, building materials, and miscellaneous goods.
[0003] As a method for improving the impact resistance of molded articles made of polycarbonate-based resins, it is known to blend ABS resins obtained by graft polymerizing a styrene-acrylonitrile copolymer onto a diene-based rubber such as butadiene rubber or a styrene-butadiene copolymer with the polycarbonate-based resins (see, for example, Patent Document 1).
[0004] Furthermore, since polycarbonate resins have relatively low fluidity when melted, it is known to compound a flow improver therewith.
[0005] For example, Patent Document 2 describes blending a polymer having a weight-average molecular weight of less than 15,000 and essentially containing a (meth)acrylate monomer as a flow improver with a polycarbonate resin. The polymer is described as containing 1 to 99% by weight of a (meth)acrylate monomer and 99 to 1% by weight of a vinyl aromatic monomer. It also describes blending an ABS resin with a polycarbonate resin.
[0006] Patent Document 3 describes blending an aromatic polycarbonate with an ABS resin and a non-crosslinked acrylic polymer having a weight-average molecular weight of 25,000 to 50,000. The non-crosslinked acrylic polymer is described as containing 60 to 100% by weight of methyl methacrylate monomer.
[0007] Japanese Patent Application Laid-Open No. 2000-319496 Japanese Patent Application Laid-Open No. 2006-509862 Japanese Patent No. 5781761
[0008] In conventional polycarbonate resin compositions, improving the fluidity during melting tends to result in a decrease in impact resistance or heat resistance, and improving the impact resistance tends to result in a decrease in fluidity during melting or heat resistance, making it difficult to obtain a polycarbonate resin composition that exhibits a good balance of fluidity during melting, impact resistance, and heat resistance.
[0009] In view of the above-mentioned current situation, an object of the present invention is to provide a polycarbonate resin composition having a good balance of flowability in a melt, impact resistance, and heat resistance, and a molded article thereof.
[0010] As a result of intensive research, the present inventors have found that the above-mentioned problems can be solved by blending a flowability improver containing a polymer having a specific monomer composition and weight-average molecular weight, and a core-shell elastomer, with a polycarbonate resin, and have arrived at the present invention. That is, the present invention relates to a polycarbonate resin composition comprising a polycarbonate resin (A), a flowability improver (B) containing a first polymer (b1), and a core-shell elastomer (C), wherein the content of the flowability improver (B) is 1 to 15% by weight of the total of the polycarbonate resin (A) and the flowability improver (B), and the content of the core-shell elastomer (C) is 1 to 30 parts by weight per 100 parts by weight of the total of the polycarbonate resin (A) and the flowability improver (B), and the first polymer (b1) contains, as constituent monomers, 50 to 70% by weight of an aromatic vinyl compound, 5 to 20% by weight of a vinyl cyanide compound, and 10 to 45% by weight of other copolymerizable vinyl compounds, with the total of the first polymer (b1) being 100% by weight, and the weight-average molecular weight of the first polymer (b1) is 15,000 to 120,000. The present invention also relates to a molded article obtained by molding the polycarbonate resin composition.
[0011] According to the present invention, it is possible to provide a polycarbonate resin composition having a good balance of melt flowability, impact resistance, and heat resistance, and a molded article thereof. Furthermore, according to a preferred embodiment of the present invention, by incorporating a flame retardant, it is possible to provide a polycarbonate resin composition having a good balance of melt flowability, impact resistance, and heat resistance, as well as good flame retardancy. Because the flame retardancy can be improved, it is possible to obtain the advantage of being able to reduce the amount of flame retardant incorporated into the polycarbonate resin composition.
[0012]
[0013] The resin composition according to the present disclosure contains a polycarbonate resin (A), a flowability improver (B) containing a first polymer (b1), and a core-shell elastomer (C). The resin composition may further contain a modifier (D) containing a third polymer (d1), and / or a flame retardant (E).
[0013] <Polycarbonate Resin (A)> As the polycarbonate resin (A), a commonly used polycarbonate resin can be used, such as a polycarbonate resin produced by a method of interfacial polycondensation of a dihydric phenol and a carbonyl halide or the like, or a method of melt polymerization of a dihydric phenol and a carbonate diester or the like (transesterification method).
[0014] Examples of the dihydric phenol include 4,4'-dihydroxybiphenyl, bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)cyclohexane, bis(4-hydroxyphenyl)ether, bis(4-hydroxyphenyl)sulfide, bis(4-hydroxyphenyl)sulfone, bis(4-hydroxyphenyl)sulfoxide, bis(4-hydroxyphenyl)ketone, hydroquinone, resorcinol, and catechol. Among these, bis(hydroxyphenyl)alkanes are preferred, and 2,2-bis(4-hydroxyphenyl)propane is particularly preferred.
[0015] Examples of carbonate precursors include carbonyl halides, carbonyl esters, and haloformates. Specific examples include phosgene, diaryl carbonates such as dihaloformates of dihydric phenols, diphenyl carbonate, ditolyl carbonate, bis(chlorophenyl)carbonate, and m-cresyl carbonate, and aliphatic carbonate compounds such as dimethyl carbonate, diethyl carbonate, diisopropyl carbonate, dibutyl carbonate, diamyl carbonate, and dioctyl carbonate.
[0016] The polycarbonate resin may be a resin in which the molecular structure of the polymer chain is a linear structure, or a resin having a branched structure. Examples of branching agents for introducing such a branched structure include 1,1,1-tris(4-hydroxyphenyl)ethane, α,α',α"-tris(4-hydroxyphenyl)-1,3,5-triisopropylbenzene, phloroglucin, trimellitic acid, and isatin bis(o-cresol). Furthermore, examples of molecular weight modifiers that can be used include phenol, p-t-butylphenol, p-t-octylphenol, and p-cumylphenol.
[0017] The polycarbonate resin may be a polymer having only polycarbonate structural units produced using only the dihydric phenol and a carbonate precursor, a copolymer having polycarbonate structural units and polyorganosiloxane structural units, or a resin composition containing the polymer and the copolymer. It may also be a polyester-polycarbonate resin obtained by polymerizing a dihydric phenol or the like in the presence of a difunctional carboxylic acid such as terephthalic acid or an ester-forming precursor thereof.
[0018] <Flow improver (B)> The polycarbonate resin composition according to the present disclosure contains a flow improver (B). The flow improver (B) contains at least a first polymer (b1). In a preferred embodiment, the flow improver (B) has excellent granulation properties during production, and therefore preferably contains a second polymer (b2) in addition to the first polymer (b1).
[0019] [First Polymer (b1)] The first polymer (b1) contains, as constituent monomers, 50 to 70 wt% of an aromatic vinyl compound, 5 to 20 wt% of a vinyl cyanide compound, and 10 to 45 wt% of other copolymerizable vinyl compounds, with the entire first polymer (b1) being 100 wt%. The content of the aromatic vinyl compound is preferably 55 to 70 wt%, the content of the vinyl cyanide compound is preferably 7 to 20 wt%, and the content of the other copolymerizable vinyl compounds is preferably 10 to 38 wt%. By including the aromatic vinyl compound and the vinyl cyanide compound in the above-mentioned proportions in the first polymer (b1), a polycarbonate resin composition can be provided that has a good balance of melt flowability, impact resistance, and heat resistance.
[0020] Examples of aromatic vinyl compounds include styrene, α-methylstyrene, p-methylstyrene, monobromostyrene, dibromostyrene, tribromostyrene, and chlorostyrene, with styrene being preferred. These may be used alone or in combination of two or more.
[0021] Examples of vinyl cyanide compounds include acrylonitrile and methacrylonitrile, with acrylonitrile being preferred. These may be used alone or in combination of two or more.
[0022] Examples of the other copolymerizable vinyl compounds include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, and pentadecyl (meth)acrylate. linear alkyl (meth)acrylates having 1 to 20 carbon atoms, such as acrylate and hexadecyl (meth)acrylate; isopropyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, isopentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, isodecyl (meth)acrylate, isoundecyl (meth)acrylate, isododecyl (meth)acrylate, isotridecyl (meth)acrylate branched alkyl (meth)acrylates having 3 to 20 carbon atoms such as acrylate, isotetradecyl (meth)acrylate, isopentadecyl (meth)acrylate, isohexadecyl (meth)acrylate, isoheptadecyl (meth)acrylate, and isooctadecyl (meth)acrylate; cyclic alkyl (meth)acrylates having 3 to 20 carbon atoms such as cyclopropyl (meth)acrylate, cyclobutyl (meth)acrylate, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, cyclooctyl (meth)acrylate, and cyclodecyl (meth)acrylate; Alkyl (meth)acrylates; aryl (meth)acrylates such as phenyl (meth)acrylate and methylphenyl (meth)acrylate; aralkyl (meth)acrylates such as benzyl (meth)acrylate; unsaturated acid anhydrides such as maleic anhydride, itaconic anhydride, and citraconic anhydride; unsaturated acids such as acrylic acid and methacrylic acid; imide compounds of α,β-unsaturated dicarboxylic acids such as maleimide, N-methylmaleimide, N-butylmaleimide, N-(p-methylphenyl)maleimide, N-phenylmaleimide, and N-cyclohexylmaleimide;Examples of such compounds include epoxy group-containing unsaturated compounds such as glycidyl (meth)acrylate and allyl glycidyl ether; unsaturated carboxylic acid amides such as acrylamide and methacrylamide; amino group-containing unsaturated compounds such as acrylamine, aminomethyl (meth)acrylate, aminoethyl (meth)acrylate, aminopropyl (meth)acrylate, and aminostyrene; hydroxyl group-containing unsaturated compounds such as 3-hydroxy-1-propene, 4-hydroxy-1-butene, cis-4-hydroxy-2-butene, trans-4-hydroxy-2-butene, 3-hydroxy-2-methyl-1-propene, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, and hydroxystyrene; and oxazoline group-containing unsaturated compounds such as vinyloxazoline. These compounds may be used alone or in combination of two or more.
[0023] The weight-average molecular weight of the first polymer (b1) is 15,000 to 120,000. By making the weight-average molecular weight of the first polymer (b1) 120,000 or less, it is possible to provide a polycarbonate resin composition having a good balance of fluidity when melted, impact resistance, and heat resistance. It is more preferably 100,000 or less, even more preferably 80,000 or less, and particularly preferably 60,000 or less. Furthermore, from the viewpoint that if the weight-average molecular weight of the first polymer (b1) is too low, the melting initiation temperature will be low and handling properties will be impaired, the weight-average molecular weight is preferably 20,000 or more, more preferably 25,000 or more, and even more preferably 30,000 or more.
[0024] [Second polymer (b2)] The second polymer (b2) is an optional component and may not be contained. However, when the flow improver (B) contains the second polymer (b2), it is preferable that the second polymer (b2) is present outside the first polymer (b1) and is present so as to cover the first polymer (b1). It is preferable that the first polymer (b1) and the second polymer (b2) are not chemically bonded to each other.
[0025] When the flow improver (B) contains a second polymer (b2), the second polymer (b2) preferably contains, as constituent monomers, 10 to 90% by weight of alkyl methacrylate and 10 to 90% by weight of other copolymerizable vinyl compounds, with the entire second polymer (b2) being 100% by weight. The relatively high proportion of alkyl methacrylate in the second polymer (b2) can increase the Tg (glass transition temperature) of the second polymer (b2), as described below, and can improve the granulation properties of the flow improver (B). The second polymer (b2) preferably contains, as constituent monomers, 50 to 90% by weight of alkyl methacrylate and 10 to 50% by weight of other copolymerizable vinyl compounds, more preferably 60 to 90% by weight of alkyl methacrylate and 10 to 40% by weight of other copolymerizable vinyl compounds, and particularly preferably 70 to 90% by weight of alkyl methacrylate and 10 to 30% by weight of other copolymerizable vinyl compounds, relative to 100% by weight of the entire second polymer (b2). As the other vinyl compounds, the compounds exemplified for the first polymer (b1) above can be used.
[0026] Examples of alkyl methacrylates include linear alkyl methacrylates having 1 to 20 carbon atoms, such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, pentyl methacrylate, hexyl methacrylate, heptyl methacrylate, octyl methacrylate, nonyl methacrylate, decyl methacrylate, undecyl methacrylate, dodecyl methacrylate, tridecyl methacrylate, tetradecyl methacrylate, pentadecyl methacrylate, hexadecyl methacrylate, and ocdecyl methacrylate; isopropyl methacrylate, isobutyl methacrylate, s-butyl methacrylate, t-butyl methacrylate, isopentyl methacrylate, and 2-ethyl methacrylate. branched alkyl methacrylates having 3 to 20 carbon atoms, such as hexyl methacrylate, isooctyl methacrylate, isononyl methacrylate, isodecyl methacrylate, isoundecyl methacrylate, isododecyl methacrylate, isotridecyl methacrylate, isotetradecyl methacrylate, isopentadecyl methacrylate, isohexadecyl methacrylate, isoheptadecyl methacrylate, and isooctadecyl methacrylate; and cyclic alkyl methacrylates having 3 to 20 carbon atoms, such as cyclopropyl methacrylate, cyclobutyl methacrylate, cyclopentyl methacrylate, cyclohexyl methacrylate, cyclooctyl methacrylate, and cyclodecyl methacrylate. These may be used alone, or two or more may be used in combination.
[0027] The number of carbon atoms in the alkyl group of the alkyl methacrylate is preferably 1 to 14, more preferably 1 to 12, even more preferably 1 to 10, still more preferably 1 to 8, and particularly preferably 1 to 6. Of the above, linear alkyl methacrylates are more preferred, and methyl methacrylate and ethyl methacrylate are even more preferred.
[0028] The second polymer (b2) is present outside the first polymer (b1), and the Tg of the second polymer (b2) is 30 to 110°C, thereby improving the granulation properties of the flow improver (B). The Tg of the second polymer (b2) is preferably 60 to 100°C, more preferably 35 to 80°C. The Tg may be calculated by calculating the Tg of each monomer from the Tg of the homopolymer described in "Polymer Handbook Fourth Edition" by J. Brand, published by Wiley in 1998, or may be calculated by differential thermal analysis or differential scanning calorimetry.
[0029] The weight average molecular weight of the second polymer (b2) is not particularly limited, but is preferably from 20,000 to 300,000, and more preferably from 20,000 to 150,000.
[0030] When the flowability improver (B) contains the second polymer (b2), from the viewpoint of the balance of the flowability, impact resistance, and heat resistance when the polycarbonate resin composition is melted, the flowability improver (B) preferably contains 60 to 90 wt% of the first polymer (b1) and 10 to 40 wt% of the second polymer (b2), where the total of the first polymer (b1) and the second polymer (b2) is 100 wt%, more preferably contains 65 to 85 wt% of the first polymer (b1) and 15 to 35 wt% of the second polymer (b2), and even more preferably contains 70 to 80 wt% of the first polymer (b1) and 20 to 30 wt% of the second polymer (b2).
[0031] [Production method of flow improver (B)] Flow improver (B) can be obtained by the polymerization method using water as a medium, such as emulsion polymerization method, suspension polymerization method, etc., from the viewpoints of easy recovery, low odor of polymer, handling, anti-blocking property and economical efficiency.Among these, emulsion polymerization method is more preferred from the viewpoint of dispersibility in polycarbonate resin.Furthermore, emulsion polymerization method, soap-free emulsion polymerization method and dropwise suspension polymerization method, which can obtain particle structure, are particularly preferred polymerization methods for obtaining two or more polymer structures.
[0032] The emulsifier used in the emulsion polymerization method may be any conventionally known emulsifier, including anionic emulsifiers such as fatty acid salts, alkyl sulfate ester salts, alkylbenzene sulfonates, alkyl phosphate ester salts, and sulfosuccinic acid diester salts; cationic emulsifiers such as alkylamine salts; and nonionic emulsifiers such as polyoxyethylene alkyl ethers and polyoxyethylene fatty acid esters. Among these, phosphoric acid emulsifiers or sulfonic acid emulsifiers are preferred, with sulfonic acid emulsifiers being particularly preferred, because they improve impact resistance or heat resistance, inhibit decomposition of polycarbonate resins, and inhibit reduction in impact resistance under humid and hot conditions and color change at high temperatures. These emulsifiers may be used alone or in combination of two or more. Furthermore, polymerization promoters such as ethylenediaminetetraacetic acid disodium salt, sodium formaldehyde sulfoxylate, and ferrous sulfate may be used; latex viscosity modifiers such as sodium sulfate may be used; and pH adjusters such as sodium hydroxide may be used.
[0033] The weight-average molecular weight of the first polymer (b1) or the second polymer (b2) can be adjusted by changing the ratio of the monomers contained therein, and can also be adjusted by changing the amounts of the radical initiator and optionally the chain transfer agent used, the polymerization temperature, the polymerization time, etc.
[0034] Examples of radical initiators that can be used in emulsion polymerization include organic hydroperoxides such as t-butyl hydroperoxide, cumene hydroperoxide, diisopropylbenzene hydroperoxide, paramenthane hydroperoxide, and t-butyl peroxylaurate; redox initiators that combine an oxidizing agent such as the organic hydroperoxides with a reducing agent such as sulfite, hydrogen sulfite, thiosulfate, first metal salt, and sodium formaldehyde sulfoxylate; persulfates such as potassium persulfate and ammonium persulfate; azo compounds such as azobisisobutyronitrile, dimethyl-2,2'-azobisisobutyrate, and 2-carbamoylazaisobutyronitrile; and organic peroxides such as benzoyl peroxide and lauroyl peroxide. Of these, the radical initiator is preferably an organic hydroperoxide, and more preferably t-butyl hydroperoxide.
[0035] The amount of radical initiator used (preferably the amount of radical initiator used during polymerization of the first polymer (b1)) may be, for example, 0.01 to 5.0 parts by weight, preferably 0.1 to 3.5 parts by weight, and more preferably 0.5 to 3.0 parts by weight, relative to 100 parts by weight of the monomers used. If the amount of radical initiator is large, the weight average molecular weight tends to decrease, and if the amount of radical initiator is small, the weight average molecular weight tends to increase.
[0036] Examples of chain transfer agents used in emulsion polymerization include mercaptans such as octyl mercaptan, n-dodecyl mercaptan, t-dodecyl mercaptan, n-hexyl mercaptan, n-hexadecyl mercaptan, n-tetradecyl mercaptan, and t-tetradecyl mercaptan; hydrocarbon salts such as tetraethylthiuram sulfide, carbon tetrachloride, ethylene bromide, and pentanephenylethane; terpenes, acrolein, methacrolein, allyl alcohol, 2-ethylhexyl thioglycol, and α-methylstyrene dimer. Among these, the chain transfer agent is preferably a mercaptan, and more preferably t-dodecyl mercaptan. These may be used alone or in combination of two or more.
[0037] The amount of the chain transfer agent used (preferably the amount of the chain transfer agent used during polymerization of the first polymer (b1)) may usually be 0 to 3 parts by weight relative to 100 parts by weight of the monomer. When a chain transfer agent is used, the amount of the chain transfer agent used may be, for example, 0.01 to 3 parts by weight, preferably 0.1 to 3 parts by weight, and more preferably 0.5 to 2.5 parts by weight.
[0038] The polymerization time may vary depending on the monomer, emulsifier, radical initiator, and chain transfer agent used as needed, and the amounts thereof, but may be, for example, 1 hour to 50 hours, and preferably 5 hours to 24 hours.
[0039] The polymerization temperature can be adjusted depending on the monomers, emulsifier, radical initiator, and chain transfer agent used as needed, and the amounts thereof, and may be, for example, 10°C to 90°C, and preferably 40°C to 80°C.
[0040] The volume average particle diameter of the flowability improver (B) in the latex may be, for example, 0.030 μm or more and 0.500 μm or less. The volume average particle diameter can be calculated using a particle size analyzer (Nanotracwave, manufactured by Nikkiso Co., Ltd.).
[0041] Next, the obtained latex containing the flowability improver (B) may be powdered, for example, by a coagulation method. When powdering the flowability improver (B), a method of treating the latex obtained by the emulsion polymerization method with a coagulation method such as salt coagulation or acid coagulation, or a method of obtaining a powder by spray drying the latex, etc. can be used. In the coagulation method such as salt coagulation or acid coagulation, the latex may be contacted with a coagulant such as an inorganic salt (preferably a divalent inorganic salt, more preferably calcium chloride) or an acid. After coagulation, further heat treatment, dehydration, washing, drying, etc. may be performed to prepare the flowability improver (B).
[0042] The blending amount of the flowability improver (B) in the polycarbonate resin composition according to this embodiment is preferably 1 to 15 wt % of the total of the polycarbonate resin (A) and the flowability improver (B). By blending 1 wt % or more of the flowability improver (B), it is possible to provide a polycarbonate resin composition having a good balance of fluidity in the melt, impact resistance, and heat resistance. Furthermore, by setting the blending amount to 15 wt % or less, it is possible to achieve particularly good impact resistance. The blending amount is more preferably 3 to 14 wt %, even more preferably 5 to 13 wt %, and particularly preferably 7 to 12 wt %.
[0043] <Core-shell type elastomer (C)> The resin composition according to the present disclosure contains a core-shell type elastomer (C), which allows good impact resistance to be achieved.
[0044] The core-shell elastomer (C) may be composed of polymer particles that are graft copolymers. The core-shell elastomer (C) preferably comprises a shell layer and one or more core layers. The shell layer refers to a polymer layer located on the surface side of the polymer particle and is also called a graft layer. The core layer refers to a polymer layer located more inwardly of the polymer particle than the shell layer and is composed of a rubbery polymer. The core layer may consist of only one layer, or may consist of two or more layers with different monomer compositions. The shell layer covers the surface of the core layer, but is not limited to covering the entire surface of the core layer, as long as it covers at least a portion of the surface of the core layer.
[0045] (Core Layer) The core layer is composed of a rubbery polymer. The rubbery polymer preferably contains at least one selected from the group consisting of natural rubber, diene rubber, acrylate rubber, and polyorganosiloxane rubber, and more preferably contains at least one selected from the group consisting of diene rubber, acrylate rubber, and polyorganosiloxane rubber.
[0046] (Diene Rubber) The diene rubber is an elastomer containing a constituent unit derived from a diene monomer as a constituent unit. The core layer more preferably contains a diene rubber, and particularly preferably is a diene rubber, because the glass transition temperature of the resulting elastomer can be lowered, the impact resistance of the resulting molded article of the polycarbonate resin composition is improved, and the raw material cost is low.
[0047] Examples of the diene monomer include 1,3-butadiene, isoprene (2-methyl-1,3-butadiene), 2-chloro-1,3-butadiene, etc. These diene monomers may be used alone or in combination of two or more.
[0048] The diene rubber may further contain, as a structural unit, a structural unit derived from a vinyl monomer other than the diene monomer that is copolymerizable with the diene monomer.
[0049] Examples of vinyl monomers other than diene monomers copolymerizable with diene monomers (hereinafter also referred to as vinyl monomer A) include: (a) aromatic vinyl monomers such as styrene, α-methylstyrene, monochlorostyrene, and dichlorostyrene; (b) vinylcarboxylic acids such as acrylic acid and methacrylic acid; (c) alkyl (meth)acrylates such as ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, and butyl methacrylate; (d) methacrylic acid, alkyl acrylates such as methyl methacrylate, ethyl methacrylate, and butyl methacrylate; (e) hydroxyl group-containing vinyl monomers such as 2-hydroxyethyl acrylate and 4-hydroxybutyl acrylate; (f) glycidyl group-containing vinyl monomers such as glycidyl methacrylate and 4-hydroxybutyl acrylate glycidyl ether; (g) unsaturated nitrile monomers such as acrylonitrile and methacrylonitrile; (h) vinyl acetate; (i) alkenes such as ethylene, propylene, butylene, and isobutylene. The above-mentioned vinyl monomer A may be used alone or in combination of two or more.
[0050] There are no particular limitations on the content of constituent units derived from vinyl monomer A in the diene rubber. The diene rubber preferably contains 50 to 100% by weight of constituent units derived from diene monomers and 0 to 50% by weight of constituent units derived from vinyl monomer A, based on 100% by weight of constituent units.
[0051] The diene rubber may further contain, as a structural unit, a structural unit derived from a polyfunctional monomer such as diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, divinylbenzene, allyl methacrylate, ethylene glycol dimethacrylate, 1,3-butylene dimethacrylate, etc. In other words, these polyfunctional monomers may be used in the polymerization of the diene rubber.
[0052] Suitable examples of diene rubbers include butadiene rubber (polybutadiene rubber), styrene / butadiene copolymer rubber (poly(styrene / butadiene) rubber), poly(acrylonitrile / butadiene) rubber, butadiene / acrylic acid ester copolymer, etc. Butadiene rubber is an elastomer containing 50 to 100% by weight of structural units derived from 1,3-butadiene, out of 100% by weight of structural units.
[0053] The diene rubber is preferably a butadiene rubber containing 50 to 100% by weight of structural units derived from 1,3-butadiene and 0 to 50% by weight of structural units derived from vinyl monomer A, and more preferably a 1,3-butadiene homopolymer containing 100% by weight of structural units derived from 1,3-butadiene.
[0054] The core layer preferably contains butadiene rubber or styrene / butadiene copolymer rubber because it can lower the glass transition temperature of the resulting elastic body, it has a high effect of improving the impact resistance of the resulting molded article of the polycarbonate-based resin composition, and the raw material cost is low.
[0055] (Acrylate-Based Rubber) The acrylate-based rubber is an elastic material containing, as a constituent unit, a constituent unit derived from a (meth)acrylate-based monomer.
[0056] Examples of the (meth)acrylate monomer include: (a) alkyl (meth)acrylate esters having an alkyl group having 1 to 22 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, and behenyl (meth)acrylate; (b) aromatic ring-containing (meth)acrylate esters, such as phenoxyethyl (meth)acrylate and benzyl (meth)acrylate; (c) hydroxyalkyl (meth)acrylate esters, such as 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate; (d) glycidyl group-containing (meth)acrylate esters, such as glycidyl (meth)acrylate and glycidyl alkyl (meth)acrylate; and (e) alkoxyalkyl (meth)acrylate esters. These (meth)acrylate monomers may be used alone or in combination of two or more.
[0057] The acrylate rubber may further contain, as a structural unit, a structural unit derived from a vinyl monomer other than the (meth)acrylate monomer that is copolymerizable with the (meth)acrylate monomer. Examples of the vinyl monomer other than the (meth)acrylate monomer that is copolymerizable with the (meth)acrylate monomer include (a) the diene monomers described above, and (b) monomers of the vinyl monomer A other than the (meth)acrylate monomer.
[0058] The acrylic rubber has a crosslinked structure. To introduce the crosslinked structure, for example, a crosslinking agent and / or a graft crosslinking agent can be used when synthesizing the core layer polymer by polymerizing the monomer components. Examples of crosslinking agents and graft crosslinking agents include: (a) allyl alkyl (meth)acrylates such as allyl (meth)acrylate and allyl alkyl (meth)acrylate; (b) polyfunctional (meth)acrylates such as monoethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, and tetraethylene glycol di(meth)acrylate; and (c) polyfunctional monomers such as diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, and divinylbenzene. These crosslinking agents and graft crosslinking agents may be used alone or in combination of two or more.
[0059] Suitable examples of acrylate rubbers include polybutyl acrylate rubber and butyl acrylate / 2-ethylhexyl acrylate copolymer rubber. Polybutyl acrylate rubber is an elastomer containing 50 to 100% by weight of structural units derived from butyl acrylate, based on 100% by weight of structural units.
[0060] Suitable examples of the polyorganosiloxane rubber include silicone rubber and silicone / acrylate rubber.
[0061] Examples of silicone rubbers include polymethylsilicone rubber and polymethylphenylsilicone rubber, etc. Examples of silicone / acrylate rubbers include polyorganosiloxane / butyl acrylate copolymers, etc.
[0062] In one embodiment, the core layer preferably contains one or more selected from the group consisting of butadiene rubber, styrene / butadiene copolymer rubber, acrylate rubber, and silicone rubber, and more preferably contains butadiene rubber or styrene / butadiene copolymer rubber.
[0063] The weight proportion of the core layer in the entire core-shell type elastomer (C) is preferably 50 to 99% by weight, more preferably 60 to 95% by weight, and even more preferably 70 to 90% by weight, from the viewpoint of compatibility between the core-shell type elastomer (C) and the polycarbonate resin, and from the viewpoint of improving impact resistance.
[0064] (Shell Layer) The shell layer is preferably formed from a polymer containing a structural unit derived from a vinyl monomer, such as an aromatic vinyl compound, a vinyl cyanide compound, an unsaturated carboxylic acid ester, an acrylamide monomer, or a maleimide monomer.
[0065] Suitable examples of the aromatic vinyl compound include styrene, α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, t-butylstyrene, α-methylvinyltoluene, dimethylstyrene, chlorostyrene, dichlorostyrene, bromostyrene, and dibromostyrene.
[0066] Suitable examples of the vinyl cyanide compound include acrylonitrile, methacrylonitrile, and ethacrylonitrile.
[0067] Suitable examples of the unsaturated carboxylic acid ester include: (a) alkyl acrylates having an alkyl group having 1 to 22 carbon atoms, such as methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, octyl acrylate, dodecyl acrylate, stearyl acrylate, and behenyl acrylate; (b) alkyl methacrylates having an alkyl group having 1 to 22 carbon atoms, such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, octyl methacrylate, dodecyl methacrylate, stearyl methacrylate, and behenyl methacrylate; and (c) alkoxyalkyl (meth)acrylates having an alkyl group having 1 to 22 carbon atoms and an alkoxyl group, such as methoxymethyl (meth)acrylate, methoxyethyl (meth)acrylate, ethoxymethyl (meth)acrylate, and ethoxyethyl (meth)acrylate.
[0068] Suitable examples of the acrylamide monomer include acrylamide, methacrylamide, and N-methylacrylamide.
[0069] Suitable examples of the maleimide monomer include N-methylmaleimide, N-ethylmaleimide, N-isopropylmaleimide, N-butylmaleimide, N-hexylmaleimide, N-octylmaleimide, N-dodecylmaleimide, N-cyclohexylmaleimide, and N-phenylmaleimide.
[0070] The polymer constituting the shell layer preferably contains, as a constituent monomer, at least one selected from the group consisting of methyl methacrylate, styrene, and butyl acrylate, which may be used alone or in combination of two or more.
[0071] The polymer constituting the shell layer may further contain, as a constituent monomer, at least one reactive vinyl monomer selected from the group consisting of a carboxyl group-containing vinyl monomer, a hydroxyl group-containing vinyl monomer, and a glycidyl group-containing vinyl monomer. By including the reactive vinyl monomer as a constituent monomer in the shell layer, the core-shell elastomer (C) can be made reactive with the polycarbonate resin. As a result, the dispersibility of the core-shell elastomer (C) in the polycarbonate resin is improved, thereby enhancing the impact resistance. Among the reactive vinyl monomers, carboxyl group-containing vinyl monomers are preferred because of their particularly good reactivity with the polycarbonate resin. The reactive vinyl monomers may be used alone or in combination of two or more.
[0072] Suitable examples of the carboxyl group-containing vinyl monomer include acrylic acid, methacrylic acid, crotonic acid, maleic acid, itaconic acid, fumaric acid, isocrotonic acid, vinyloxyacetic acid, allyloxyacetic acid, 2-(meth)acryloylpropanoic acid, 3-(meth)acryloylbutanoic acid, 4-vinylbenzoic acid, 2-methacryloyloxyethyl succinic acid, 2-methacryloyloxyethyl maleic acid, 2-methacryloyloxyethyl phthalic acid, 2-methacryloyloxyethylhexahydrophthalic acid, etc. Among these, acrylic acid and / or methacrylic acid are preferred, and methacrylic acid is more preferred.
[0073] Suitable examples of the hydroxyl group-containing vinyl monomer include (meth)acrylic acid hydroxyalkyl esters having an alkyl group having 1 to 22 carbon atoms and a hydroxyl group, such as hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate.
[0074] Suitable examples of the glycidyl group-containing vinyl monomer include glycidyl (meth)acrylate.
[0075] The amount of the reactive vinyl monomer used can be appropriately set depending on the desired effect and is not particularly limited. When the reactive vinyl monomer is a carboxyl group-containing vinyl monomer, the proportion of the carboxyl group-containing vinyl monomer in the entire polymer particles that are the core-shell type elastomer (C) may be, for example, 0.01 to 5% by weight.
[0076] The weight proportion of the shell layer in the entire core-shell type elastomer (C) is preferably 1 to 50% by weight, more preferably 5 to 40% by weight, and even more preferably 10 to 30% by weight, from the viewpoint of compatibility between the core-shell type elastomer (C) and the polycarbonate resin, and from the viewpoint of improving impact resistance.
[0077] [Particle Diameter of Core-Shell Elastomer (C)] The particle diameter of the core-shell elastomer (C), which is a polymer particle, can be set as appropriate, but the volume average particle diameter is preferably 100 nm or more. Since impact resistance tends to improve as the particle diameter increases, the volume average particle diameter is preferably 150 nm or more, more preferably 200 nm or more, and even more preferably 250 nm or more. On the other hand, since a larger particle diameter of the polymer particles tends to increase the time required for the polymerization reaction and reduce productivity, the volume average particle diameter is preferably 700 nm or less, more preferably 500 nm or less. The volume average particle diameter of the polymer particles is a value measured using a particle size measuring device in the state of the polymer particles in a latex state, as shown in the Examples section. The volume average particle diameter of the polymer particles can also be calculated from a transmission electron microscope (TEM) image of the polycarbonate resin composition. The particle diameter of the polymer particles can be controlled by the type and amount of polymerization initiator, chain transfer agent, redox agent, emulsifier, etc., polymerization temperature, polymerization time, etc.
[0078] [Method for producing the core-shell type elastomer (C)] The method for producing the core-shell type elastomer (C) can be a conventional method and is not particularly limited. For example, any of bulk polymerization, solution polymerization, suspension polymerization, and emulsion polymerization can be adopted, but emulsion polymerization, i.e., emulsion graft polymerization, is preferred. In emulsion graft polymerization, specifically, first, a latex of particles corresponding to the core layer is produced by emulsion polymerization, and then monomer components for the shell layer, a polymerization initiator, etc. are added to the latex to polymerize the monomer components.
[0079] A known method for efficiently producing a core-shell type elastomer (C) having a relatively large particle size by a conventional emulsion polymerization method is to add a water-soluble electrolyte or an acid group-containing copolymer latex to enlarge the particles before or during graft polymerization. Methods for enlarging the particles using a water-soluble electrolyte are disclosed in JP-A Nos. 4-170458 and 60-192754, among others. Methods for enlarging the particles using an acid group-containing copolymer latex are disclosed in JP-A Nos. 10-245468 and 8-12704, among others.
[0080] [Amount of Core-Shell Elastomer (C)] The amount of core-shell elastomer (C) in the polycarbonate resin composition according to this embodiment is preferably 1 to 30 parts by weight per 100 parts by weight of the total of the polycarbonate resin (A) and the flowability improver (B). When the amount of core-shell elastomer (C) is within this range, a polycarbonate resin composition having a good balance of melt flowability, impact resistance, and heat resistance can be provided. The amount is more preferably 3 to 25 parts by weight, and even more preferably 5 to 20 parts by weight.
[0081] <Modifier (D)> The polycarbonate resin composition according to this embodiment may further contain a modifier (D) containing a third polymer (d1) in addition to the flowability improver (B) containing the first polymer (b1). The third polymer (d1) is a polymer having a higher molecular weight than the first polymer (b1). Even if the modifier (D) is added without the flowability improver (B), the fluidity and heat resistance during melting are insufficient, and it is difficult to obtain a polycarbonate resin composition having a good balance of flowability during melting, impact resistance, and heat resistance. However, by adding the modifier (D) together with the flowability improver (B), a polycarbonate resin composition having a good balance of flowability during melting, impact resistance, and heat resistance can be obtained, and the impact resistance can be further improved compared to the case of using the flowability improver (B) alone.
[0082] The modifier (D) contains at least a third polymer (d1). In a preferred embodiment, the modifier (D) has excellent granulation properties during production, and therefore preferably contains a fourth polymer (d2) in addition to the third polymer (d1).
[0083] The third polymer (d1) may be a polymer of a vinyl compound and / or a (meth)acrylate monomer, and its monomer composition is not particularly limited, but specific examples include the following. According to one embodiment, the third polymer (d1) may contain, as constituent monomers, 50 to 70% by weight of an aromatic vinyl compound, 5 to 20% by weight of a vinyl cyanide compound, and 10 to 45% by weight of other copolymerizable vinyl compounds, relative to 100% by weight of the entire third polymer (d1). The monomer composition is the same as that of the first polymer (b1), and therefore will not be described here.
[0084] In another embodiment, the third polymer (d1) may contain, as constituent monomers, 50 to 99% by weight of an alkyl methacrylate and 1 to 50% by weight of another copolymerizable vinyl compound, with the whole of the third polymer (d1) being 100% by weight. The monomer composition is the same as that of the second polymer (b2), and therefore will not be described here.
[0085] The weight average molecular weight of the third polymer (d1) is larger than that of the first polymer (b1), and is preferably 150,000 to 7,000,000, more preferably 200,000 to 4,000,000, and even more preferably 250,000 to 1,500,000.
[0086] When the modifier (D) contains a fourth polymer (d2), the fourth polymer (d2) is present so as to cover the third polymer (d1), and preferably contains, as constituent monomers, 50 to 90% by weight of an alkyl methacrylate and 10 to 50% by weight of another copolymerizable vinyl compound, where the total weight of the fourth polymer (d2) is 100% by weight. The monomer composition and weight-average molecular weight of the fourth polymer (d2) are the same as those of the second polymer (b2), and therefore are not described here.
[0087] When the modifier (D) contains a fourth polymer (d2), from the viewpoint of the balance of the fluidity, impact resistance, and heat resistance when the polycarbonate resin composition is melted, the modifier (D) preferably contains 60 to 90% by weight of the third polymer (d1) and 10 to 40% by weight of the fourth polymer (d2), where the total of the third polymer (d1) and the fourth polymer (d2) is 100% by weight, more preferably contains 65 to 85% by weight of the third polymer (d1) and 15 to 35% by weight of the fourth polymer (d2), and even more preferably contains 70 to 85% by weight of the third polymer (d1) and 15 to 30% by weight of the fourth polymer (d2).
[0088] The modifier (D) can be produced by the same method as the flow improver (B). Commercially available modifiers (D) include Kane Ace (registered trademark) PA-20 (manufactured by Kaneka Corporation), Kane Ace (registered trademark) PA-40 (manufactured by Kaneka Corporation), Kane Ace (registered trademark) PA-80 (manufactured by Kaneka Corporation), PA-310 (manufactured by Kaneka Corporation), and Blendex 864 (Galata Chemicals).
[0089] The amount of modifier (D) blended in the polycarbonate resin composition according to this embodiment is not particularly limited and can be set as appropriate, but the weight ratio of flow improver (B):modifier (D) is preferably 99:1 to 50:50, more preferably 97:3 to 60:40, and even more preferably 95:5 to 70:30.
[0090] <Flame retardant (E)> The polycarbonate resin composition according to the present disclosure may contain no flame retardant, or may further contain a flame retardant (E). By containing the flame retardant (E), it is possible to provide a polycarbonate resin composition with good flame retardancy.
[0091] As the flame retardant, various flame retardants known to be blended into thermoplastic resins can be used, including, but not limited to, flame retardants described in "Technology and Applications of Polymer Flame Retardation" (pp. 149-221) published by CMC Publishing.
[0092] Particularly, examples of the flame retardants include halogen-based flame retardants such as bromine-based flame retardants such as tetrabromobisphenol A and decabromodiphenyl oxide, and chlorine-based flame retardants such as chlorinated paraffin and chlorinated polyethylene; phosphorus-based flame retardants such as non-halogen phosphate ester-based flame retardants (monophosphate / condensation), halogen-containing phosphate ester-based flame retardants (monophosphate / condensation), inorganic phosphate-based flame retardants, and red phosphorus-based flame retardants; inorganic flame retardants such as antimony trioxide, aluminum hydroxide, and magnesium hydroxide; organic salt-based flame retardants, silicone-based flame retardants, etc. These may be used alone or in combination of two or more.
[0093] Preferred flame retardants include halogenated bisphenol A, halogenated polycarbonate oligomers, and polycarbonate-type flame retardants of halogenated bisphenol A; halogenated flame retardants comprising a combination of a halogen compound such as a brominated epoxy compound and a flame retardant aid such as antimony oxide; organic salt-based flame retardants; phosphorus-based flame retardants such as aromatic phosphate ester-based flame retardants and halogenated aromatic phosphate ester-based flame retardants; and silicone-based flame retardants such as organopolysiloxanes, including branched phenyl silicone compounds and phenyl silicone resins.
[0094] Examples of the halogenated bisphenol A polycarbonate flame retardant include tetrabromobisphenol A polycarbonate flame retardants, and copolymer polycarbonate flame retardants of tetrabromobisphenol A and bisphenol A.
[0095] Examples of the organic salt-based flame retardant include dipotassium diphenylsulfone-3,3'-disulfonate, potassium diphenylsulfone-3-sulfonate, sodium 2,4,5-trichlorobenzenesulfonate, potassium 2,4,5-trichlorobenzenesulfonate, potassium bis(2,6-dibromo-4-cumylphenyl)phosphate, sodium bis(4-cumylphenyl)phosphate, potassium bis(p-toluenesulfone)imide, potassium bis(diphenylphosphate)imide, potassium bis(2,4,6-tribromophenyl)phosphate, potassium bis(2,4-dibromophenyl)phosphate, potassium bis(4-bromophenyl)phosphate, potassium diphenylphosphate, sodium diphenylphosphate, potassium perfluorobutanesulfonate, sodium or potassium lauryl sulfate, and sodium or potassium hexadecyl sulfate.
[0096] Examples of the halogenated aromatic phosphate ester type flame retardants include tris(2,4,6-tribromophenyl)phosphate, tris(2,4-dibromophenyl)phosphate, and tris(4-bromophenyl)phosphate.
[0097] Examples of the aromatic phosphate ester-based flame retardant include triphenyl phosphate, tris(2,6-xylyl)phosphate, tetrakis(2,6-xylyl)resorcinol diphosphate, tetrakis(2,6-xylyl)hydroquinone diphosphate, tetrakis(2,6-xylyl)-4,4'-biphenol diphosphate, tetraphenylresorcinol diphosphate, tetraphenylhydroquinone diphosphate, tetraphenyl-4,4'-biphenol diphosphate, an aromatic polyphosphate in which the aromatic ring source is resorcinol and phenol and does not contain a phenolic hydroxyl group (OH group), an aromatic polyphosphate in which the aromatic ring source is resorcinol and phenol and contains a phenolic OH group, an aromatic polyphosphate in which the aromatic ring source is hydroquinone and phenol and does not contain a phenolic OH group, and an aromatic polyphosphate in which the aromatic ring source is hydroquinone and phenol and does not contain a phenolic OH group. Examples of aromatic polyphosphates include aromatic polyphosphates which are hydroquinone and phenol and contain a phenolic OH group (hereinafter, "aromatic polyphosphate" refers to both aromatic polyphosphates containing and not containing a phenolic OH group), aromatic polyphosphates whose aromatic ring sources are bisphenol A and phenol, aromatic polyphosphates whose aromatic ring sources are tetrabromobisphenol A and phenol, aromatic polyphosphates whose aromatic ring sources are resorcinol and 2,6-xylenol, aromatic polyphosphates whose aromatic ring sources are hydroquinone and 2,6-xylenol, aromatic polyphosphates whose aromatic ring sources are bisphenol A and 2,6-xylenol, and aromatic polyphosphates whose aromatic ring sources are tetrabromobisphenol A and 2,6-xylenol.
[0098] From the viewpoint of achieving both good flame retardancy and impact resistance, the blending amount of the flame retardant (E) is preferably 1 to 80 parts by weight, more preferably 5 to 60 parts by weight, and particularly preferably 10 to 40 parts by weight, per 100 parts by weight of the total of the polycarbonate resin (A) and the flowability improver (B). The polycarbonate resin composition according to this embodiment can have improved flame retardancy compared to conventional compositions, making it possible to reduce the blending amount of the flame retardant. Furthermore, by reducing the blending amount of the flame retardant, further improvements in impact resistance and heat resistance can be expected.
[0099] <Anti-Drip Agent> The polycarbonate-based resin composition according to this embodiment may be blended with an anti-drip agent to prevent melt dripping during combustion. Examples of the anti-drip agent include fluoroolefin-based resins containing a fluoroolefin resin as a main component. Fluoroolefin resins are polymers, copolymers, or composites containing a fluoroethylene structure. Examples of fluoroolefin resins include difluoroethylene polymers, tetrafluoroethylene polymers, tetrafluoroethylene-hexafluoropropylene copolymers, copolymers of tetrafluoroethylene and fluorine-free ethylene-based monomers, and composites of tetrafluoroethylene polymers and vinyl-based resins such as acrylic resins. Of these, polytetrafluoroethylene (PTFE) is preferred. The weight-average molecular weight of polytetrafluoroethylene is preferably 500,000 or more, and particularly preferably 500,000 to 10,000,000.
[0100] Among polytetrafluoroethylenes, compounds having fibril-forming ability are preferred because they can impart even higher melt-dripping prevention properties. Examples of polytetrafluoroethylenes having fibril-forming ability include compounds classified as Type 3 in the ASTM standard. Examples of polytetrafluoroethylenes classified as Type 3 include Teflon (registered trademark) 6-J (manufactured by DuPont-Mitsui Fluorochemicals Co., Ltd.), Polyflon D-1, Polyflon F-103, Polyflon F201 (manufactured by Daikin Industries, Ltd.), CD1, CD076 (manufactured by Asahi ICI Fluoropolymers Co., Ltd.), and the like.
[0101] Examples of polytetrafluoroethylenes other than compounds classified as Type 3 include Algoflon F5 (manufactured by Montefluos Co., Ltd.), Polyflon MPA, and Polyflon FA-100 (manufactured by Daikin Industries, Ltd.) These polytetrafluoroethylenes may be used alone or in combination of two or more types.
[0102] From the viewpoint of achieving both prevention of melt dripping during combustion and impact resistance, the blending amount of the anti-drip agent is preferably 0.05 to 5 parts by weight, more preferably 0.1 to 2 parts by weight, per 100 parts by weight of the total of the polycarbonate resin (A) and the flowability improver (B). The blending amount of the anti-drip agent can be appropriately determined depending on the level of flame retardancy required for the molded article, for example, UL94 V-0, V-1, V-2, etc., and also taking into consideration the blending amounts of other components, etc.
[0103] <Other Resins> The polycarbonate-based resin composition according to this embodiment may contain, or may not contain, a thermoplastic resin other than the polycarbonate-based resin (A). When a thermoplastic resin other than the polycarbonate-based resin is contained, the thermoplastic resin is not particularly limited, and examples thereof include polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyvinyl acetate, polyurethane, polytetrafluoroethylene, ABS resin, AS resin, acrylic resin, polyacetal, polyester, modified polyphenylene ether, polyamide, and cyclic polyolefin. The amount of the other thermoplastic resin is not particularly limited, and is, for example, 0 to 100 parts by weight, preferably 0 to 50 parts by weight, more preferably 0 to 30 parts by weight, even more preferably 0 to 10 parts by weight, and particularly preferably 0 to 5 parts by weight, per 100 parts by weight of the polycarbonate-based resin (A).
[0104] <Other Additives> The polycarbonate resin composition according to this embodiment may contain, as appropriate, additives that can be blended into general thermoplastic resin compositions. Such additives are not particularly limited, but examples thereof include reinforcing materials, fillers, antioxidants, pigments, dyes, conductivity-imparting agents, hydrolysis inhibitors, thickeners, plasticizers, lubricants, UV absorbers, antistatic agents, flow improvers, release agents, compatibilizers, and heat stabilizers.
[0105] <Method for producing resin composition> The method for producing the polycarbonate-based resin composition according to this embodiment is not particularly limited, and known methods can be used. For example, the polycarbonate-based resin composition can be produced by a known method of blending and melt-kneading the components using an apparatus such as a Henschel mixer, a Banbury mixer, a single-screw extruder, a twin-screw extruder, a two-roll mill, a kneader, or a Brabender. In order to suppress yellowing of the resin composition due to thermal degradation of the polycarbonate-based resin, it is preferable that the melt-kneading temperature be as low as possible.
[0106] <Molded Articles and Applications> The polycarbonate-based resin composition according to this embodiment can be molded into a predetermined shape to form a molded article. Specifically, the polycarbonate-based resin composition can be extruded to form, for example, extruded articles having various shapes, extrusion-molded sheets, films, and the like. Examples of extrusion molding methods include cold runner and hot runner molding methods, as well as injection compression molding, injection press molding, gas-assisted injection molding, foam molding (including injection of supercritical fluids), insert molding, in-mold coating molding, adiabatic mold molding, rapid heating and cooling mold molding, two-color molding, sandwich molding, and ultra-high-speed injection molding. Sheet or film molding can also be achieved by inflation, calendaring, casting, or the like. Furthermore, a specific stretching operation can be performed to form a heat-shrinkable tube. Hollow molded articles can also be obtained by rotational molding, blow molding, or the like.
[0107] Molded articles made from the polycarbonate-based resin composition according to this embodiment can be used in a wide range of applications, such as various housings, hard-coated products, glazing materials, light diffusion plates, optical disk substrates, light guide plates, medical materials, and miscellaneous goods. Specifically, the resin can be used as resin products formed into, for example, exterior materials for office automation equipment and home appliances, various containers, miscellaneous goods, such as exterior materials for personal computers, notebook computers, game consoles, display devices (CRT, LCD, plasma, projectors, organic EL, etc.), mice, printers, copiers, scanners, and fax machines (including multifunction devices thereof), keyboard keys, molded switch products, personal digital assistants (so-called PDAs), mobile phones, portable books (dictionaries, etc.), portable televisions, drives for recording media (CDs, MDs, DVDs, Blu-ray discs, hard disks, etc.), readers for recording media (IC cards, smart media, memory sticks, etc.), optical cameras, digital cameras, parabolic antennas, power tools, VTRs, irons, hair dryers, rice cookers, microwave ovens, audio equipment, lighting equipment, refrigerators, air conditioners, air purifiers, negative ion generators, and typewriters. The product may also be a tray, a cup, a plate, a shampoo bottle, an office equipment housing, a cosmetic bottle, a beverage bottle, an oil container, an injection-molded product (golf tee, a cotton swab core, a candy stick, a brush, a toothbrush, a helmet, a syringe, a plate, a cup, a comb, a razor handle, a tape cassette and case, a disposable spoon or fork, stationery such as a ballpoint pen, etc.), etc.
[0108] The molded article may also be used in the form of binding tape (binding band), prepaid cards, balloons, pantyhose, hair caps, sponges, cellophane tape, umbrellas, raincoats, plastic gloves, hair caps, ropes, tubes, foam trays, foam cushioning materials, cushioning materials, packaging materials, cigarette filters, and the like.
[0109] Furthermore, the molded article may be a vehicle part such as a lamp socket, a lamp reflector, a lamp housing, an instrument panel, a center console panel, a deflector part, a car navigation part, a car audiovisual part, or an automobile mobile computer part.
[0110] The following items list preferred aspects of the present disclosure, but the present invention is not limited to the following items. [Item 1] A polycarbonate resin composition comprising: a polycarbonate resin (A); a flowability improver (B) containing a first polymer (b1); and a core-shell elastomer (C), wherein the content of the flowability improver (B) is 1 to 15% by weight of the total of the polycarbonate resin (A) and the flowability improver (B); and the content of the core-shell elastomer (C) is 1 to 30 parts by weight per 100 parts by weight of the total of the polycarbonate resin (A) and the flowability improver (B); and wherein the first polymer (b1) contains, as constituent monomers, 50 to 70% by weight of an aromatic vinyl compound, 5 to 20% by weight of a vinyl cyanide compound, and 10 to 45% by weight of other copolymerizable vinyl compounds, with the total of the first polymer (b1) being 100% by weight, and the weight-average molecular weight of the first polymer (b1) is 15,000 to 120,000. [Item 2] The polycarbonate-based resin composition according to Item 1, wherein the flow improver (B) further comprises a second polymer (b2) covering the first polymer (b1). [Item 3] The polycarbonate-based resin composition according to Item 2, wherein the second polymer (b2) comprises, as constituent monomers, 50 to 90% by weight of an alkyl methacrylate and 10 to 50% by weight of another copolymerizable vinyl compound, with the entire second polymer (b2) being 100% by weight. [Item 4] The polycarbonate-based resin composition according to Item 2 or 3, wherein the content of the first polymer (b1) in the flow improver (B) is 60 to 90% by weight, and the content of the second polymer (b2) is 10 to 40% by weight. [Item 5] The polycarbonate-based resin composition according to any one of Items 1 to 4, wherein the core-shell elastomer (C) has a core layer containing butadiene rubber or styrene / butadiene copolymer rubber, and a shell layer containing a copolymer containing, as a constituent monomer, at least one selected from the group consisting of methyl methacrylate, styrene, and butyl acrylate. [Item 6] The polycarbonate-based resin composition according to any one of Items 1 to 5, wherein the flowability improver (B) contains, as an emulsifier, a phosphoric acid-based emulsifier or a sulfonic acid-based emulsifier.[Item 7] The polycarbonate-based resin composition according to any one of Items 1 to 6, wherein the core-shell elastomer (C) has a volume average particle size of 100 nm or more. [Item 8] The polycarbonate-based resin composition according to any one of Items 1 to 7, further comprising a modifier (D) containing a third polymer (d1), wherein the third polymer (d1) has a weight average molecular weight of 150,000 to 7,000,000. [Item 9] The polycarbonate-based resin composition according to any one of Items 1 to 8, further comprising a flame retardant (E). [Item 10] A molded article obtained by molding the polycarbonate-based resin composition according to any one of Items 1 to 9.
[0111] Examples of the present invention will be described below, but the present invention is not limited to these examples.
[0112] [Abbreviations] AN: Acrylonitrile St: Styrene BA: Butyl acrylate MMA: Methyl methacrylate GMA: Glycidyl methacrylate t-DM: t-dodecyl mercaptan
[0113] [Measurement Methods] In the production examples, physical properties were measured according to the following methods.
[0114] <Weight-Average Molecular Weight of Polymer> The polymer to be measured was dissolved in tetrahydrofuran (THF), and the weight-average molecular weight of the soluble portion was determined by gel permeation chromatography (HLC-8220GPC, manufactured by Tosoh Corporation) using polystyrene as a standard (sample solution: 20 mg sample / 10 mL THF, measurement temperature: 25°C, detector: differential refractometer, injection amount: 1 mL).
[0115] <Volume Average Particle Diameter of Core-Shell Elastomer> The volume average particle diameter of the core-shell elastomer in a latex state was measured using a particle size analyzer (Nanotracwave, manufactured by Nikkiso Co., Ltd.) by light scattering at a wavelength of 546 nm.
[0116] <Production Example 1> 1.0 part (part by weight, the same applies hereinafter) of dioctylsodium sulfosuccinate, 0.0050 parts of disodium ethylenediaminetetraacetic acid, and 0.0025 parts of ferrous sulfate, which had been dissolved in water in advance, were placed in a reactor equipped with a stirrer, and water was further added to make the total amount of water 200 parts.
[0117] The atmosphere inside the reactor was replaced with nitrogen to remove oxygen from the space and water. Subsequently, while stirring, 0.4 parts of sodium formaldehyde sulfoxylate was added to a reactor equipped with a stirrer, and the contents were heated to 75°C. Polymerization was then carried out while continuously adding a mixture of 12.6 parts of acrylonitrile, 43.4 parts of styrene, 6.0 parts of butyl acrylate, 18.0 parts of methyl methacrylate, 0.8 parts of t-dodecyl mercaptan, and 1 part of t-butyl hydroperoxide over 200 minutes. At 50 minutes and 100 minutes into the continuous addition, 0.3 parts of dioctyl sodium sulfosuccinate were added. Furthermore, at 100 minutes into the continuous addition, 0.15 parts of sodium formaldehyde sulfoxylate was added. This resulted in the formation of a first polymer (b1).
[0118] After the polymerization was completed, a mixture of 4 parts of butyl acrylate, 16 parts of methyl methacrylate, and 0.3 parts of t-butyl hydroperoxide was continuously added thereto over 50 minutes to carry out polymerization. After the continuous addition was completed, 0.2 parts of sodium formaldehyde sulfoxylate was added.
[0119] After the addition of the copolymerization components was completed, the contents were kept at 75°C and stirred for at least 1 hour to complete the polymerization. This resulted in the formation of a second polymer (b2). The contents were then cooled to obtain a latex of flowability improver (B-1).
[0120] The resulting flowability improver latex was added to 5 parts of a calcium chloride aqueous solution diluted to a concentration of 1% by weight and coagulated at a temperature of 45° C. The mixture was then heat-treated, dehydrated, washed, and dried to obtain a powder of flowability improver (B-1) containing a first polymer (b1) and a second polymer (b2) having a weight-average molecular weight of 45,000.
[0121] <Production Example 2> A powder of flowability improver (B-2) containing a first polymer (b1) and a second polymer (b2) having a weight average molecular weight of 46,000 was obtained in the same manner as in Production Example 1, except that sodium dodecylbenzenesulfonate was used as the emulsifier.
[0122] <Production Example 3> A powder of flowability improver (B-3) containing a first polymer (b1) and a second polymer (b2) having a weight average molecular weight of 46,500 was obtained in the same manner as in Production Example 1, except that sodium polyoxyethylene lauryl ether phosphate was used as the emulsifier.
[0123] <Production Example 4> A powder of flowability improver (B-4) containing a first polymer (b1) and a second polymer (b2) having a weight average molecular weight of 43,000 was obtained in the same manner as in Production Example 1, except that sodium polyoxyethylene lauryl ether phosphate was used as the emulsifier and the monomers used in forming the first polymer (b1) were changed to 4.0 parts of acrylonitrile, 52.0 parts of styrene, 6.0 parts of butyl acrylate, and 18.0 parts of methyl methacrylate.
[0124] <Production Example 5> A powder of modifier (D-1) containing a third polymer (d1) and a fourth polymer (d2) having a weight average molecular weight of 300,000 was obtained in the same manner as in Production Example 1, except that t-dodecyl mercaptan was not used and the monomers used in the second-stage polymerization were changed to 6.0 parts of butyl acrylate and 14.0 parts of methyl methacrylate.
[0125] <Production Example 6> A powder of a flowability improver (B'-2) for comparison was obtained in the same manner as in Production Example 1, except that the monomers used in the first polymerization step were changed to 16.0 parts of butyl acrylate and 64.0 parts of methyl methacrylate.
[0126] <Production Example 7> A powder of a flowability improver (B'-3) for comparison was obtained in the same manner as in Production Example 1, except that the monomers used in the first-stage polymerization were changed to 46.4 parts of styrene, 31.2 parts of butyl acrylate, and 2.4 parts of glycidyl methacrylate, the amount of t-dodecyl mercaptan used was changed to 0.96 parts, and the monomers used in the second-stage polymerization were changed to 3.0 parts of butyl acrylate and 17.0 parts of methyl methacrylate.
[0127] Table 1 shows the types and amounts of monomers used in Production Examples 1 to 7, as well as the weight average molecular weights of the polymers. The amounts of monomers used in Table 1 are shown in terms of weight % of each polymer.
[0128]
[0129] Production Example 8 Preparation of Polybutadiene Rubber Latex 120 parts of water, 0.002 parts of ethylenediaminetetraacetic acid disodium salt, 0.0012 parts of ferrous sulfate, and 0.008 parts of ethylenediaminetetraacetic acid disodium salt were placed in a 100-liter pressure polymerization vessel and stirred. After sufficient deacidification, 0.10 parts of polyoxyethylene alkyl ether sodium phosphate, 100 parts of butadiene, 0.3 parts of t-dodecyl mercaptan, 0.05 parts of sodium formaldehyde sulfoxylate, and 0.05 parts of paramenthane hydroperoxide were added, and the mixture was heated to 50°C to initiate polymerization. 1.4 parts of polyoxyethylene alkyl ether sodium phosphate was then added dropwise over 6 hours, and the reaction solution was maintained at pH 6.5 to 7.5 and 50°C for 80 hours to obtain a diene rubber latex with a conversion of 98% by weight and a volume average particle size of 110 nm. <Graft copolymerization of polybutadiene> 75 parts (solids equivalent) of the rubber latex obtained above was charged into an 8-liter polymerization vessel, and the temperature was raised to 60°C while stirring and flowing nitrogen. 0.10 parts of sodium formaldehyde sulfoxylate was added, and 0.2 parts of t-butyl hydroperoxide was added to a graft monomer mixture (8 parts styrene, 17 parts methyl methacrylate), and the mixture was continuously added dropwise at a rate of 10 parts / hour using a metering pump. After the addition of the monomer mixture was completed, stirring was continued for another hour to complete the polymerization. The polymerization conversion was 98%, and the average particle size of the latex was 120 nm. To the latex, 1.5 parts each of dilauryl-3,3'-thiodipropionate and triethylene glycol-bis-3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionate were added, and then 5 parts of calcium chloride were added to cause salting out. After heating at 90°C, the mixture was dehydrated and dried to obtain a resin powder of a core-shell type elastomer (C-1).
[0130] <Production Example 9> <Preparation of Polybutadiene Rubber Latex> 200 parts of water, 0.2 parts of potassium persulfate, and 0.2 parts of t-dodecyl mercaptan were placed in a 100-liter pressure polymerization vessel and stirred. After thorough nitrogen substitution to remove oxygen, 1 part of sodium oleate, 2 parts of sodium rosinate, and 100 parts of butadiene were added to the system, and the temperature was raised to 60°C to initiate polymerization. The polymerization was completed in 12 hours. The conversion rate was 96%, and the average particle size of the rubber latex was 70 nm. <Preparation of Acid Group-Containing Latex> 200 parts of water and 0.5 parts of sodium dioctyl sulfosuccinate were placed in an 8-liter polymerization vessel and the temperature was raised to 70°C while stirring and flowing nitrogen. 0.3 parts of sodium formaldehyde sulfoxylate, 0.0025 parts of ferrous sulfate, and 0.01 parts of ethylenediaminetetraacetic acid were added, and after several minutes, a mixture of 2 parts of butyl methacrylate, 23 parts of butyl acrylate, 2 parts of methacrylic acid, 0.125 parts of t-dodecyl mercaptan, and 0.025 parts of cumene hydroperoxide was continuously added dropwise at a rate of 20 parts / hour using a metering pump. After the addition of the mixture, a mixture of 58 parts of butyl methacrylate, 2 parts of butyl acrylate, 13 parts of methacrylic acid, 0.3 parts of t-dodecyl mercaptan, and 0.08 parts of cumene hydroperoxide was added dropwise at a rate of 20 parts / hour. Polymerization was terminated 1.5 hours after the completion of the dropwise addition. The conversion was 99.7%, the average particle size was 120 nm, the concentration was 33%, and the pH was 2.8. <Preparation of Polybutadiene-Enlarged Rubber Latex> 100 parts (solids equivalent) of the polybutadiene rubber latex obtained above and 20 parts of water were placed in an 8-liter polymerization vessel, and the temperature was raised to 60°C while stirring and flowing nitrogen. 0.1 parts of sodium hydroxide and 2.0 parts (solids equivalent) of the acid group-containing latex obtained above were added, and stirring was continued for 1 hour to allow the polybutadiene to expand. 200 parts of water and 0.4 parts of sodium dodecylbenzenesulfonate were added, and stirring was continued for an additional 30 minutes to complete the expansion. A polybutadiene-enlarged rubber latex with an average particle size of 350 nm was obtained. <Graft Copolymerization of Polybutadiene-Enlarged Rubber> 70 parts (solids equivalent) of the polybutadiene-enlarged rubber latex obtained above was placed in an 8-liter polymerization vessel, and the temperature was raised to 60°C while stirring and flowing nitrogen.0.18 parts of sodium formaldehyde sulfoxylate, 0.001 parts of ferrous sulfate, and 0.004 parts of ethylenediaminetetraacetic acid were added, and 0.2 parts of t-butyl hydroperoxide was added to a graft monomer mixture (8 parts of styrene, 22 parts of methyl methacrylate) and continuously dropped at a rate of 10 parts / hour using a metering pump. To maintain the stability of the latex during the addition of the monomer mixture, 0.2 parts of dioctyl sodium sulfosuccinate was added four times at 1-hour intervals. After the completion of the addition of the monomer mixture, stirring was continued for another 1 hour to complete the polymerization. The polymerization conversion was 96%, and the average particle size of the latex was 350 nm. To the latex, 0.5 parts each of dilauryl-3,3'-thiodipropionate and 2,6-di-t-butyl-4-methylphenol were added, and then 5 parts of calcium chloride were added to cause salting out. After heat treatment at 90°C, the mixture was dehydrated and dried to obtain a resin powder of a core-shell type elastomer (C-2).
[0131] <Production Example 10> A glass reactor equipped with a thermometer, a stirrer, a reflux condenser, a nitrogen inlet, and a monomer and emulsifier addition device was charged with 155 parts of deionized water, 0.47 parts of boric acid, 0.047 parts of sodium carbonate, and 0.016 parts of polyoxyethylene lauryl ether phosphate, and the mixture was heated to 50°C while stirring in a nitrogen stream. Next, a mixture of 8.50 parts of butyl acrylate (BA), 0.0425 parts of allyl methacrylate, and 0.0017 parts of t-butyl hydroperoxide was added all at once. Ten minutes after the completion of the addition, 0.0056 parts of disodium ethylenediaminetetraacetate, 0.0014 parts of ferrous sulfate, and 0.2 parts of sodium formaldehyde sulfoxylate were added. After another 50 minutes, 0.02 parts of sodium hydroxide was added, followed by the addition of a mixture of 76.5 parts of BA, 0.38 parts of allyl methacrylate, 0.765 parts of polyoxyethylene lauryl ether phosphate, 0.025 parts of t-butyl hydroperoxide, and 0.06 parts of sodium hydroxide over 173 minutes. After the addition was completed, 0.012 parts of sodium hydroxide was added, and after another 15 minutes, 0.014 parts of t-butyl hydroperoxide was added. After 30 minutes, a mixture of 13.5 parts of MMA, 1.5 parts of BA, 0.141 parts of polyoxyethylene lauryl ether phosphate, and 0.0069 parts of t-butyl hydroperoxide was added over 36 minutes. After the addition was complete, 0.01 parts of sodium hydroxide was added, and after another 15 minutes, 0.015 parts of t-butyl hydroperoxide was added. After another 15 minutes, 0.03 parts of t-butyl hydroperoxide was added, followed by stirring for 30 minutes to obtain a polymer particle latex with a polymerization conversion of 100%. The average particle size of the latex was 300 nm. 500 parts of deionized water and 3.0 parts of a 25 wt% calcium chloride aqueous solution were stirred, and the polymer particle latex was then added to obtain a slurry containing coagulated latex particles. The obtained slurry was then heated to 90°C, dehydrated, and dried to obtain a white resin powder of a core-shell type elastomer (C-3).
[0132] Examples 1 to 10 and Comparative Examples 1 to 12 Pellets and test pieces composed of resin compositions containing polycarbonate resin were prepared using the components shown below according to the formulations shown in Tables 2 and 3, and the Charpy strength (impact strength), tensile properties, flexural properties, HDT, flame retardancy, and MFR were measured. Note that MFR is an index of fluidity when melted. A higher MFR value indicates higher fluidity when melted.
[0133] Component (A): Polycarbonate resin (Panlite L-1225WP, manufactured by Teijin Limited), blending amount (wt%) shown in each table
[0134] Component (B): Flow improver, blending amount (wt%) shown in each table: B-1: Flow improver (B-1) produced in Production Example 1; B-2: Flow improver (B-2) produced in Production Example 2; B-3: Flow improver (B-3) produced in Production Example 3; B-4: Flow improver (B-4) produced in Production Example 4
[0135] Component (B'): Comparative flow improver, blending amount (wt%) shown in each table B'-1: Acrylonitrile-styrene resin (SAN-R, manufactured by Techno Polymer Co., Ltd.), weight average molecular weight: 123,000 B'-2: Comparative flow improver (B'-2) produced in Production Example 6 B'-3: Comparative flow improver (B'-3) produced in Production Example 7
[0136] Component (C): core-shell type elastomer, blending amount shown in each table [parts by weight relative to 100 parts by weight of the total of components (A), (B or (B'), and (D)] C-1: core-shell type elastomer (C-1) produced in Production Example 8, volume average particle diameter 120 nm C-2: core-shell type elastomer (C-2) produced in Production Example 9, volume average particle diameter 350 nm C-3: core-shell type elastomer (C-3) produced in Production Example 10, volume average particle diameter 300 nm
[0137] Component (D): Modifier (D-1) produced in Production Example 5, blending amount (wt %) shown in each table. Component (E): Flame retardant (aromatic condensed phosphate ester, manufactured by Daihachi Chemical Industry Co., Ltd., PX200), 0 part by weight in Table 2, 15 parts by weight per 100 parts by weight of the total of components (A), (B) or (B'), and (D) in Table 3.
[0138] Other additives: Anti-drip agent: PTFE G355, manufactured by Asahi Glass Co., Ltd., 0.1 part by weight per 100 parts by weight of the total of components (A), (B) or (B'), and (D). Stabilizer: Adekastab 2112 and Adekastab AO-60, manufactured by ADEKA Corporation, 0.1 part by weight per 100 parts by weight of the total of components (A), (B) or (B'), and (D).
[0139] (Conditions for preparing pellets and test pieces) A mixture of the components was kneaded and extruded at a screw rotation speed of 100 rpm in a twin-screw extruder (TEX44SS manufactured by The Japan Steel Works, Ltd.) heated to a barrel temperature of 230 to 260°C. The pellets were dried in a dryer at 100°C for 12 hours to sufficiently reduce the moisture content, and then test pieces were prepared in an injection molding machine (FAS100B manufactured by Fanuc Corporation) at a molding temperature of 270 to 290°C and a mold temperature of 50°C.
[0140] (Charpy Strength) The Charpy impact strength of the test piece with a length of 63.5 mm, a width of 12.7 mm, and a thickness of 3.2 mm, and having a V-notch, prepared by the method described above, was measured at −30° C. and 23° C. by a method conforming to the ASTM D6110 standard.
[0141] (Tensile Properties) The ASTM D638-1 type test piece having a thickness of 3.2 mm prepared by the above-mentioned method was measured for yield strength and elongation at break in an absolute dry state at 23°C at a test speed of 50 mm / min by a method in accordance with the ASTM D638 standard.
[0142] (Flexural Properties) In accordance with ASTM D-0790, flexural strength and flexural modulus were measured using a ¼ inch bar at a test speed of 5 mm / min, at 23° C., and with a support distance of 100 mm.
[0143] (HDT) A test piece having a length of 127 mm, a width of 12.7 mm and a thickness of 6.4 mm, prepared by the method described above, was annealed at 60°C for 2 hours, and then subjected to a test of 18.6 kgf / cm by a method conforming to ASTM D648 standard. 2 The HDT (deflection temperature under load) was measured at a load of 1000 kJ / cm.
[0144] (Flame Retardancy) The pellets prepared under the above conditions were dried at 100°C for 8 hours, and then injection molded using an injection molding machine (TOYO (100i), clamping pressure: 100 tons) under conditions of a cylinder setting temperature of 235°C to 260°C and a mold temperature of 50°C to obtain test pieces measuring 127 mm x 12.7 mm x 1.2 mm thick. The resulting bar-shaped test pieces with a thickness of 1.2 mm were used to evaluate flammability in accordance with the UL94 Standard V test.
[0145] (MFR) The MFR value of the pellets prepared under the above conditions was measured in accordance with JIS K7210 Method A at a measurement temperature of 250°C and a load of 5 kg. The results of the above measurements are shown in Tables 2 and 3.
[0146]
[0147] Table 2 shows the results for systems containing no flame retardant (E). The polycarbonate resin compositions of Examples 1 and 2 exhibited good values for fluidity in a melt, impact resistance, and heat resistance, and the balance of the physical properties was good.
[0148] On the other hand, it can be seen that Comparative Examples 1 to 3, which did not contain the core-shell elastomer (C), had extremely low impact resistance and low heat resistance. Comparative Example 4, which contained a general acrylonitrile-styrene resin as the comparative flow improver (B'-1), had good impact resistance but was lower than Examples 1 and 2, had a small MFR value, and had insufficient fluidity when melted, and also had low heat resistance. It can be seen that Comparative Examples 5 and 6, which contained a large amount of flow improver (B), had low impact resistance and low heat resistance. It can be seen that Comparative Example 7, which did not contain the flow improver (B), had low impact resistance and insufficient fluidity when melted.
[0149]
[0150] Table 3 shows the systems containing the flame retardant (E). The polycarbonate resin compositions of Examples 3 to 10 exhibited good values for fluidity when melted, impact resistance, and heat resistance, and had a good balance of the physical properties.
[0151] On the other hand, it can be seen that Comparative Examples 8 and 9, in which the blending amount of flow improver (B) was large, had extremely low impact resistance. It can be seen that Comparative Example 10, in which no flow improver (B) was used but instead a modifier (D-1) with a high polymer weight average molecular weight that does not satisfy the requirements of the flow improver (B) was used, had extremely low heat resistance and relatively low fluidity when melted. It can be seen that Comparative Examples 11 and 12, in which comparative flow improvers (B'-2) or (B'-3) that do not satisfy the monomer composition requirements of the flow improver (B) of the present application were used, had extremely low impact resistance and low heat resistance.
Claims
1. Polycarbonate-based resin (A), A flow improver (B) comprising a first polymer (b1), and Contains a core-shell type elastomer (C), The content of the flow improver (B) is 1 to 15% by weight based on the total weight of the polycarbonate-based resin (A) and the flow improver (B), the content of the core-shell type elastomer (C) is 1 to 30 parts by weight per 100 parts by weight of the total of the polycarbonate-based resin (A) and the flowability improver (B), The first polymer (b1) contains, as constituent monomers, 50 to 70% by weight of an aromatic vinyl compound, 5 to 20% by weight of a vinyl cyanide compound, and 10 to 45% by weight of another copolymerizable vinyl compound, with the entire first polymer (b1) being 100% by weight, The weight average molecular weight of the first polymer (b1) is 15,000 to 120,000, The flow improver (B) further comprises a second polymer (b2) covering the first polymer (b1).
2. The polycarbonate-based resin composition according to claim 1, wherein the second polymer (b2) contains, as constituent monomers, 50 to 90% by weight of an alkyl methacrylate and 10 to 50% by weight of another copolymerizable vinyl compound, with the whole of the second polymer (b2) being 100% by weight.
3. 2. The polycarbonate resin composition according to claim 1, wherein the flow improver (B) contains the first polymer (b1) in an amount of 60 to 90% by weight and the second polymer (b2) in an amount of 10 to 40% by weight.
4. The polycarbonate resin composition according to any one of claims 1 to 3, wherein the core-shell type elastomer (C) has a core layer containing a butadiene rubber or a styrene / butadiene copolymer rubber, and a shell layer containing a copolymer containing at least one monomer selected from the group consisting of methyl methacrylate, styrene, and butyl acrylate as a constituent monomer.
5. 4. The polycarbonate resin composition according to claim 1, wherein the flow improver (B) contains a phosphoric acid-based emulsifier or a sulfonic acid-based emulsifier as an emulsifier.
6. The polycarbonate resin composition according to any one of claims 1 to 3, wherein the core-shell type elastomer (C) has a volume average particle size of 100 nm or more.
7. Further containing a modifier (D) containing a third polymer (d1), The polycarbonate resin composition according to any one of claims 1 to 3, wherein the third polymer (d1) has a weight average molecular weight of 150,000 to 7,000,000.
8. The polycarbonate resin composition according to any one of claims 1 to 3, further comprising a flame retardant (E).
9. A molded article obtained by molding the polycarbonate resin composition according to any one of claims 1 to 3.