Method for producing carbon fiber bundle composite, and carbon fiber bundle composite
Patent Information
- Application Number
- JP2024504659
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-11
AI Technical Summary
Current methods for manufacturing carbon fiber reinforced plastics (CFRP) using chopped carbon fiber bundles are inefficient and costly, and there is a need for a novel prepreg material that can be easily produced from short cut carbon fibers, both virgin and recycled, to improve production efficiency and reduce waste.
A method involving mixing carbon fiber cotton made of short carbon fibers with a molten resin containing an epoxy resin component, solidifying the resin, and incorporating an epoxy curing agent to create a carbon fiber bundle composite, which can be used as an intermediate material for various CFRP production methods, including compression molding.
This approach enhances production efficiency, reduces costs, and allows for the effective use of recycled carbon fibers, resulting in high-quality CFRP products with improved mechanical properties and reduced environmental impact.
Abstract
Description
Manufacturing method of carbon fiber bundle composite and carbon fiber bundle composite
[0001] The present invention mainly relates to a method for producing a carbon-fiber bundle composite and a carbon-fiber bundle composite.
[0002] CFRP (Carbon Fiber Reinforced Plastic), a fiber-reinforced plastic that uses carbon fiber as a reinforcing material, is a lightweight material with excellent mechanical properties that makes it suitable for parts of automobiles, ships, railway vehicles, manned aircraft, unmanned aircraft, and other transportation equipment, and its importance has been increasing in recent years.
[0003] One of the intermediate molding materials used in the production of CFRP products is carbon fiber sheet molding compound (CF-SMC), which is made by cutting continuous carbon fiber bundles to produce chopped carbon fiber bundles, scattering the chopped carbon fiber bundles on a carrier film, and then impregnating the carbon fiber mat with a thermosetting resin matrix (see, for example, Patent Document 1).
[0004] Generally, CFRP molded from CF-SMC using chopped carbon fiber bundles with smaller bundle sizes exhibits higher strength. On the other hand, the larger the bundle size of continuous carbon fiber bundles, the higher the production efficiency. For this reason, a technology has been developed to split large tow continuous carbon fiber bundles with large bundle sizes, such as 48K, into smaller tows (fiber bundles) (Patent Document 2).
[0005] It has been proposed to produce carbon fiber reinforced thermoplastics by adding carbon fiber pellets to a thermoplastic resin. The carbon fiber pellets are produced by mixing wet-cut short carbon fibers with a solution or suspension of a sizing agent to form carbon fiber aggregates, pelletizing the aggregates using a disc pelletizer, and then drying the pellets (Patent Document 3).
[0006] It is known that needle-shaped self-assembled carbon fiber bundles can be obtained by dispersing short carbon fibers in water, adding a small amount of chloroform, and shaking vigorously, and that polyetherimide can be supported on the needle-shaped self-assembled carbon fiber bundles by dissolving polyetherimide in the chloroform in advance (Non-Patent Document 1).
[0007] Japanese Patent Application Laid-Open No. 1-163218 U.S. Patent No. 6,385,828 JP-A-10-503812
[0008] JR Baxter, GR Palmese, NJ Alvarez, Applied Materials Today 20 (2020) 100786
[0009] One object of the present invention is to provide a novel prepreg material that can be easily produced from chopped carbon fibers, which may be virgin carbon fibers or recycled carbon fibers. Another object of the present invention is to provide a novel method for producing a prepreg material using chopped carbon fibers as a reinforcement material. Throughout this specification, problems that can be solved by each embodiment of the present invention may be explicitly or implicitly stated.
[0010] According to one aspect of the present invention, there is provided a method for producing a carbon fiber bundle composite, comprising: mixing carbon fiber batting made of short carbon fibers with a molten resin containing an epoxy resin component to obtain a carbon fiber bundle containing the molten resin; solidifying the molten resin contained in the carbon fiber bundle; and mixing an epoxy curing agent into the molten resin.
[0011] According to another aspect of the present invention, there is provided a carbon fiber bundle composite comprising a plurality of short carbon fibers forming a bundle and an uncured solid epoxy resin composition, wherein the positions of the tips of the plurality of short carbon fibers at each end of the bundle are irregular, and the uncured solid epoxy resin composition contains an epoxy curing agent.
[0012] According to another aspect of the present invention, there are provided a carbon fiber bundle composite sheet obtained by fusing a plurality of the carbon fiber bundle composites together, and a method for producing the same.
[0013] According to a preferred embodiment of the present invention, a prepreg material is provided that can be suitably used as an intermediate material when producing CFRP products by various methods, including compression molding.
[0014] Fig. 1 is a conceptual diagram showing a manufacturing apparatus for a carbon fiber bundle composite sheet. Fig. 2 is a photograph showing a carbon fiber composite having a shape close to a spindle. Fig. 3 is a photograph showing a wire-shaped carbon fiber bundle composite. Fig. 4 is a photograph showing a needle-shaped carbon fiber bundle composite. Fig. 5 is a photograph showing a carbon fiber composite sheet.
[0015] Hereinafter, embodiments of the present invention will be described in detail.
[0016] 1. Method for Manufacturing Carbon Fiber Bundle Composite One embodiment of the present invention relates to a method for manufacturing a carbon fiber bundle composite (hereinafter sometimes abbreviated as "CBC"). This manufacturing method includes mixing carbon fiber batting made of short carbon fibers with a molten resin containing an epoxy resin component to obtain carbon fiber bundles containing the molten resin, solidifying the molten resin contained in the carbon fiber bundles, and mixing an epoxy curing agent into the molten resin.
[0017] Below, the manufacturing method of the CBC according to the embodiment will be explained separately for a method using virgin carbon fiber as the starting material and a method using recycled carbon fiber as the starting material.
[0018] 1.1 Method using virgin carbon fiber as a starting material The method using virgin carbon fiber as a starting material typically includes the following steps (i) to (iv): (i) chopping step, (ii) defibrating step, (iii) bundling step, and (iv) cooling step. Each step is described in detail below.
[0019] (i) Chopping Step In the chopping step, a continuous carbon fiber bundle made of virgin carbon fibers is cut at predetermined intervals in the fiber direction using, for example, a rotary cutter to form chopped carbon fiber bundles.
[0020] The bundle size of the continuous carbon fiber bundle (the number of carbon fiber filaments constituting the bundle) is, for example, 10K or more, and may be 12K or more, 15K or more, 24K or more, 36K or more, 48K or more, or 50K or more. There is no particular upper limit to the bundle size, but it is, for example, 100K or less. Here, "K" is a symbol representing 1000. For example, 1K means 1000, and 10K means 10000.
[0021] The larger the bundle size of the continuous carbon fiber bundle, the greater the number of carbon fiber filaments contained in one piece of chopped carbon fiber bundle, resulting in higher CBC production efficiency. Additionally, the production cost of the continuous carbon fiber bundle also decreases with increasing bundle size. Therefore, the bundle size of the continuous carbon fiber bundle is preferably 24K or more, more preferably 36K or more, and even more preferably 48K or more. The diameter of the carbon fiber filament is generally within the range of 5 μm to 15 μm for PAN-based carbon fibers made from polyacrylonitrile fibers.
[0022] The fiber length of the chopped fiber bundle is set to the length required for the carbon fibers that will make up the CBC to be manufactured, since there is no step of intentionally cutting the carbon fibers after the chopping step.
[0023] The fiber length of the chopped fiber bundle is not limited to, but may be, for example, 3 mm or more, 5 mm or more, or 10 mm or more. The fiber length of the chopped fiber bundle is not limited to, but may be, for example, 60 mm or less, 50 mm or less, 40 mm or less, 30 mm or less, or 20 mm or less.
[0024] The bundle length of a CBC formed from a plurality of short carbon fibers having the same fiber length, in other words, the dimension in the fiber direction, is equal to or greater than the fiber length of the short carbon fibers.
[0025] (ii) Defibration Step In the defibration step, the chopped carbon fiber bundles obtained in the chopping step are loosened and made into a cotton-like form to obtain carbon fiber cotton.
[0026] The defibration is preferably carried out so that all of the carbon fibers contained in the chopped carbon fiber bundle are in the form of monofilaments, but this is not essential. That is, the carbon fiber cotton obtained in the defibration step may include a thin carbon fiber bundle consisting of a small number of filaments, for example, less than 100 filaments.
[0027] In the fiber-opening step, a general fiber-opening machine can be used, and the type of fiber-opening machine to be used is not limited.
[0028] For example, chopped carbon fiber bundles can be defibrated by adding only the chopped carbon fiber bundles to a stirring mixer such as a Henschel mixer and stirring them in a dry state. This method has the advantage that the flocculent carbon fibers can be advanced to the next bundling process without being removed from the stirring mixer.
[0029] For example, chopped carbon fiber bundles can be defibrated by immersing them in an organic solvent, such as acetone, that can dissolve the sizing agent contained in the chopped carbon fiber bundles, and then irradiating them with ultrasonic waves. After the sizing agent is washed away, flocculent carbon fibers remain.
[0030] In a preferred example, the carbon fiber cotton does not contain carbon fibers with a fiber length of less than 3 mm, or if it does contain them, the amount is less than 5 wt% of the total carbon fibers contained in the carbon fiber cotton. In a more preferred example, the carbon fiber cotton does not contain carbon fibers with a fiber length of less than 5 mm, or if it does contain them, the amount is less than 5 wt% of the total carbon fibers contained in the carbon fiber cotton. In an even more preferred example, the carbon fiber cotton does not contain carbon fibers with a fiber length of less than 10 mm, or if it does contain them, the amount is less than 5 wt% of the total carbon fibers contained in the carbon fiber cotton.
[0031] (iii) Bundling Step In the bundling step, the carbon fiber wad obtained in the defibrating step is mixed with a bundling liquid. The carbon fiber filaments or thin carbon fiber bundles that make up the carbon fiber wad are aggregated by capillary force based on the surface tension of the bundling liquid to form carbon fiber bundles containing the bundling liquid.
[0032] The bundling liquid used is a molten resin containing an epoxy resin component. The molten resin corresponds to a melt of a solid resin, but it does not need to be prepared through a process of melting a solid resin. In other words, the molten resin, which is in a molten state at the time of preparation, may be used as the bundling liquid as is.
[0033] In this specification, a solid resin means a resin that is solid at least at a temperature within the range of 15 to 25° C. (so-called normal temperature).
[0034] For convenience, in this specification, a non-crystalline resin or resin composition having a viscosity of 100,000 Pa·s or more is considered to be a "solid." Furthermore, when the temperature of a molten resin is lowered and the viscosity increases without crystallization and reaches 100,000 Pa·s, this is considered to be a "solid."
[0035] This viscosity is a value measured using a rotational viscometer (for example, HAAKE MARS 40 manufactured by Thermo Fisher Scientific) under the following conditions: measurement mode: constant stress, stress value: 300 Pa, frequency: 1.59 Hz, plate diameter: 25 mm, plate type: parallel plate, plate gap: 0.5 mm.
[0036] The molten resin containing an epoxy resin component means, in other words, that the epoxy resin is blended into the molten resin.
[0037] When a compound having one or more epoxy groups per molecule is called an epoxy compound, an epoxy resin is generally a mixture containing multiple epoxy compounds, and has, on average, more than one epoxy group per molecule. One or more epoxy resins can be blended into a molten resin.
[0038] Examples of epoxy resins that can be incorporated into the molten resin include, but are not limited to, glycidyl ether type, glycidyl amine type, glycidyl ester type, and alicyclic type epoxy resins.
[0039] Glycidyl ether epoxy resins are epoxy resins obtained by reacting a compound having a hydroxyl group with epichlorohydrin. Examples of glycidyl ether epoxy resins include, but are not limited to, bisphenol A epoxy resins, bisphenol F epoxy resins, bisphenol S epoxy resins, resorcinol epoxy resins, phenol novolac epoxy resins, trisphenolmethane epoxy resins, aryl glycidyl ether epoxy resins including biphenol (biphenyl) type, benzophenone type, fluorene type, naphthalene type, and anthracene type, and alicyclic polyhydric alcohol polyglycidyl ether epoxy resins.
[0040] Glycidylamine-type epoxy resins are epoxy resins obtained by reacting a compound having an amino group with epichlorohydrin. Examples of glycidylamine-type epoxy resins include, but are not limited to, tetraglycidyldiaminodiphenylmethane-type epoxy resins, triglycidylaminophenol-type epoxy resins, triglycidylaminocresol-type epoxy resins, diglycidylaniline-type epoxy resins, and tetraglycidylmetaxylenediamine-type epoxy resins.
[0041] Examples of glycidyl ester epoxy resins include, but are not limited to, polyglycidyl esters of polycarboxylic acids such as diglycidyl esters of phthalic acid, isophthalic acid, terephthalic acid, tetrahydrophthalic acid, or hexahydrophthalic acid. In one example, an epoxy resin containing an oxazolidone ring may be blended into the molten resin. Alternatively, an isocyanate compound may be blended into the molten resin so that an oxazolidone ring is formed.
[0042] Examples of alicyclic epoxy resins include, but are not limited to, epoxy resins obtained by epoxidizing a compound having multiple cycloalkene skeletons with peracetic acid or the like, and epoxy resins obtained by prepolymerizing a bifunctional cycloalkene oxide having a polymerizable functional group such as a (meth)acrylic group or an allyl group.
[0043] The solidification temperature of the molten resin is, for example, in the range of 30°C to 150°C, and may be in the range of 40°C to 100°C.
[0044] The viscosity of the molten resin when used as the bundling liquid is preferably 10 Pa s or less, more preferably 5 Pa s or less, and may be 3 Pa s or less, 2 Pa s or less, 1 Pa s or less, etc. There is no particular lower limit to this viscosity, but it may be, for example, 0.01 Pa s or more, or 0.1 Pa s or more. The shape of the carbon fiber bundles formed by the action of the bundling liquid can change depending on the viscosity of the bundling liquid. Therefore, the greater the temperature dependency of the viscosity of the molten resin used as the bundling liquid, the stricter temperature control is required in the bundling step.
[0045] This viscosity is a value measured using a rotational viscometer (for example, HAAKE MARS 40 manufactured by Thermo Fisher Scientific) under the following conditions: measurement mode: constant stress, stress value: 300 Pa, frequency: 1.59 Hz, plate diameter: 25 mm, plate type: parallel plate, plate gap: 0.5 mm. However, for viscosity values of less than 1 Pa s, it is practically acceptable to substitute a value measured using a B-type rotational viscometer, which is known for its ease of handling.
[0046] The solidification temperature and viscosity of the molten resin when melted can be controlled by the type and content of the epoxy resin blended into the molten resin. In a preferred embodiment, the molten resin is a melt of an epoxy resin having a melting point. Epoxy resins with a melting point have a low viscosity in the liquid state and little temperature dependence, making them easy to use as bundling liquids. Epoxy resins with a melting point usually have a monomer with a rigid skeleton, a molecular weight of 1,000 or less, and a low oligomer content. Whether an epoxy resin has a melting point can be easily confirmed by conventional DSC measurement.
[0047] The amount of molten resin mixed with the carbon fiber wadding may be, for example, 25 to 150 parts by weight per 100 parts by weight of the carbon fiber wadding. By mixing them sufficiently, a large number of isolated carbon fiber bundles that are not bonded to each other are formed.
[0048] The number of carbon fiber filaments constituting one carbon fiber bundle may be, for example, 1 to 20,000, but is not limited thereto.
[0049] There are no limitations on the method for mixing the carbon fiber cotton and the molten resin, but stirring is preferred in order to mix them efficiently in a short time.
[0050] For the mixing, a powder mixer known as a Henschel mixer can be preferably used. The mixer may be a type equipped with only an agitator blade (stirring impeller), or may be one equipped with a chopper. In a jacketed mixer, the temperature of the mixing vessel can be adjusted by passing a heat transfer medium through the jacket.
[0051] The stirring tank may be preheated before the carbon fiber cotton is charged and maintained at a temperature at which the viscosity of the molten resin falls within the above-mentioned preferred range.
[0052] The carbon fiber floss may be preheated before being introduced into the stirring tank. Preferably, the carbon fiber floss is heated to a temperature at which the viscosity of the molten resin falls within the above-mentioned preferred range before being introduced into the stirring tank.
[0053] The temperature of the molten resin is preferably adjusted before being introduced into the stirred tank so that the viscosity falls within the above-mentioned preferred range. Alternatively, the molten resin may be obtained by heating and melting a solid resin in the stirred tank. In this case, the temperature of the molten resin in the stirred tank can be adjusted so that the viscosity falls within the above-mentioned preferred range.
[0054] An epoxy curing agent is mixed into the molten resin. The timing for mixing the epoxy curing agent into the molten resin is preferably before mixing the molten resin with the carbon fiber wadding or simultaneously with mixing the molten resin with the carbon fiber wadding.
[0055] The epoxy curing agent, which is liquid at the temperature at which the molten resin is mixed with the carbon fiber wadding, is preferably mixed with the molten resin before mixing the molten resin with the carbon fiber wadding.
[0056] An epoxy curing agent that is solid at the temperature at which the molten resin is mixed with the carbon fiber cotton is preferably mixed into the molten resin before or simultaneously with mixing the molten resin with the carbon fiber cotton.
[0057] When the molten resin and the carbon fiber wadding are mixed together and the epoxy resin is mixed into the molten resin at the same time, it is preferable to first mix the carbon fiber wadding and the epoxy curing agent, and then add the molten resin to the resulting mixture and further mix.
[0058] When two or more types of epoxy curing agents are used, all of them may be mixed with the molten resin at the same time, or some of them may be mixed with the molten resin at different times.
[0059] The epoxy hardener to be mixed with the molten resin can be selected from common epoxy hardeners such as dicyandiamides, phenols including novolacs, amines, carboxylic acid anhydrides, thiols, imidazoles, and the like.
[0060] When no epoxy curing agent is mixed in, the viscosity of the molten resin decreases as the temperature rises. When an epoxy curing agent is mixed in, the viscosity shows the same trend until the curing reaction due to the action of the epoxy curing agent begins, but once the curing reaction begins, the viscosity of the molten resin increases rapidly. Therefore, the epoxy curing agent to be mixed in the molten resin must be one that does not immediately initiate the curing reaction when mixed with molten resin that has been heated until the viscosity has decreased to a level that makes it usable as a bundling liquid.
[0061] As can be understood from this, the lower the solidification temperature of the molten resin, the wider the selection of epoxy curing agents that can be used. In this respect, the solidification temperature of the molten resin is preferably 120°C or less, more preferably 100°C or less, and even more preferably 90°C or less, and may be 80°C or less, 70°C or less, or 60°C or less.
[0062] A preferred epoxy curing agent is called a latent curing agent, which is a solid with low solubility in epoxy resins at room temperature, but when heated to a predetermined temperature, it melts or dissolves in the epoxy resin and functions as a curing agent. This predetermined temperature varies depending on the type of latent curing agent. Some latent curing agents have melting points of 100°C or higher, or even 150°C or higher, or even 200°C or higher, and these are epoxy curing agents that can be particularly preferably used in the manufacturing method according to the embodiment.
[0063] Various imidazoles, dicyandiamide and boron trifluoride-amine complexes are typical examples of latent hardeners.
[0064] Imidazoles are compounds having an imidazole ring, and include substituted imidazoles in which the hydrogen atoms of imidazole are substituted with substituents, as well as imidazolium salts and imidazole complexes.
[0065] Suitable examples of the substituted imidazole include substituted imidazoles having an aromatic ring which may be a heteroaromatic ring in the molecule, such as 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2-phenyl-4-methylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2-phenyl-4-benzyl-5-hydroxymethylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-para-toluyl-4-methyl-5-hydroxymethylimidazole, 2-para-toluyl-4,5-dihydroxymethylimidazole, 2-meta-toluyl-4-methyl-5-hydroxymethylimidazole, 2-meta-toluyl-4,5-dihydroxymethylimidazole and 1-cyanoethyl-2-phenylimidazole.
[0066] Imidazolium salts such as 1-cyanoethyl-2-ethyl-4-methylimidazolium trimellitate, 1-cyanoethyl-2-undecylimidazolium trimellitate, and 1-cyanoethyl-2-phenylimidazolium trimellitate are also suitable examples of the imidazole-based latent curing agent.
[0067] Isocyanuric acid adducts of various substituted imidazoles such as 2-phenylimidazole, 2-methylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole, and in particular, isocyanuric acid adducts of substituted imidazoles having a triazine ring such as 2,4-diamino-6-(2'-methylimidazolyl-(1'))-ethyl-s-triazine, 1-(4,6-diamino-s-triazin-2-yl)ethyl-2-undecylimidazole, and 2,4-diamino-6-[2-(2-ethyl-4-methyl-1-imidazolyl)ethyl]-s-triazine are particularly preferred imidazole-based latent curing agents.
[0068] Amine adducts are also suitable examples of latent curing agents. Amine adducts are polymerized by reacting imidazole and / or tertiary amine with epoxy resin and / or isocyanate, and have relatively low solubility in epoxy resins.
[0069] The latent curing agent to be mixed with the molten resin may be one type or two or more types.
[0070] For example, a curing accelerator may be mixed into the molten resin together with the epoxy curing agent. Examples of curing accelerators that can be preferably used in combination with dicyandiamide as the epoxy curing agent include urea derivatives such as 4,4'-methylenebis(phenyldimethylurea) and 2,4-bis(3,3-dimethylureido)toluene.
[0071] In addition to the epoxy curing agent, various additives such as a low shrinkage agent, an antioxidant, an internal mold release agent, a colorant, a modifier (e.g., rubber, elastomer, or thermoplastic resin), a flame retardant, and an antibacterial agent may be mixed into the molten resin as needed.
[0072] As with the epoxy curing agent, additives that are liquid at the temperature at which the molten resin is mixed with the carbon fiber cotton are preferably mixed into the molten resin before mixing the molten resin with the carbon fiber cotton. Also, additives that are solid at the temperature at which the molten resin is mixed with the carbon fiber cotton may be mixed into the molten resin before mixing the molten resin with the carbon fiber cotton, or may be mixed into the molten resin simultaneously with mixing the molten resin with the carbon fiber cotton.
[0073] Flame retardants that can be mixed into the molten resin are as follows: Preferred flame retardants include phosphorus-containing flame retardants.
[0074] Examples of phosphorus-containing flame retardants include non-halogen phosphate esters such as trimethyl phosphate, triethyl phosphate, tributyl phosphate, trioctyl phosphate, tributoxyethyl phosphate, triphenyl phosphate, tricresyl phosphate, cresyl diphenyl phosphate, octyl diphenyl phosphate, and aromatic polyphosphates.
[0075] Other examples of phosphorus-containing flame retardants include halogenated phosphate esters such as tris(chloroethyl)phosphate, tris(dichloropropyl)phosphate, tris(chloropropyl)phosphate, bis(2,3-dibromopropyl)2,3-dichloropropylphosphate, tris(2,3-dibromopropyl)phosphate, bis(chloropropyl)octylphosphate, halogenated alkyl polyphosphates, and halogenated alkyl polyphosphonates.
[0076] Further examples of phosphorus-containing flame retardants include metal phosphinates, which include not only metal salts of phosphinic acids having no organic group, but also metal salts of organic phosphinic acids such as diphenylphosphinic acid, monophenylphosphinic acid, dialkylphosphinic acid, monoalkylphosphinic acid, and alkylphenylphosphinic acid, as well as metal salts of diphosphinic acids such as methane(dimethylphosphinic acid) and benzene-1,4-di(methylphosphinic acid).
[0077] Examples of dialkylphosphinic acids include dimethylphosphinic acid, ethylmethylphosphinic acid, diethylphosphinic acid, and methyl-n-propylphosphinic acid. Examples of monoalkylphosphinic acids include methylphosphinic acid, ethylphosphinic acid, and n-propylphosphinic acid. Examples of alkylphenylphosphinic acids include methylphenylphosphinic acid. The phosphinic acid metal salts may be, but are not limited to, aluminum salts, zinc salts, calcium salts, magnesium salts, and the like.
[0078] Further examples of phosphorus-containing flame retardants include red phosphorus, ammonium polyphosphate, melamine phosphate, guanidine phosphate, and guanylurea phosphate.
[0079] In addition to the phosphorus-containing flame retardant, a phosphorus-free flame retardant may be mixed into the molten resin.
[0080] Examples of phosphorus-free flame retardants include melamine compounds such as melamine cyanurate, triazine compounds, guanidine compounds, nitrogen-based flame retardants such as ammonium phosphate and ammonium carbonate, hydrated metal compounds such as aluminum hydroxide and magnesium hydroxide, and organic metal salt-based flame retardants such as ferrocene and acetylacetone metal complexes.
[0081] In a preferred example, the molten resin and all materials mixed into the molten resin, including the flame retardant, are selected to be halogen-free, thereby making the final product, CBC, flame-retardant and halogen-free.
[0082] The weight ratio of carbon fiber wadding to the total weight of the molten resin, all materials mixed into the molten resin, and carbon fiber wadding can be 20% or more and less than 30%, 30% or more and less than 40%, 40% or more and less than 50%, 50% or more and less than 60%, 60% or more and less than 70%, or 70% or more and less than 80%. This ratio is approximately equal to the fiber weight content in the final CBC product. In reality, carbon fiber wadding made from virgin carbon fiber contains a sizing agent, so the fiber weight content of the CBC is calculated by multiplying the above ratio by the weight ratio of carbon fiber in the carbon fiber wadding.
[0083] (iv) Cooling Step In the cooling step, the carbon fiber bundles formed in the bundling step are cooled to solidify the bundling liquid, i.e., the molten resin, contained in the carbon fiber bundles, thereby completing the CBC. The cooling may be forced cooling or natural cooling.
[0084] In one example, the carbon fiber bundles formed in the stirring tank of the stirring mixer can be cooled while being stirred in the stirring tank without being removed from the stirring tank. In another example, the carbon fiber bundles formed in the stirring tank of the stirring mixer can be removed from the stirring tank and cooled in another location. The other location may be, for example, in a disc pelletizer, or in a transport pipe or on a conveyor belt. Ultimately, the temperature of the CBC is usually lowered to below room temperature.
[0085] Carbon fiber bundles are unstable before the molten resin they contain solidifies. If a large number of carbon fiber bundles at this stage are placed in a large container, the carbon fibers near the bottom of the container may stick together due to their own weight.
[0086] The higher the solidification temperature of the molten resin, the faster the solidification of the molten resin in the cooling step occurs. Therefore, the higher the solidification temperature of the molten resin, the faster the carbon fiber bundle becomes stable. From this viewpoint, the solidification temperature of the molten resin is preferably 40°C or higher, more preferably 50°C or higher, and may be 60°C or higher, 70°C or higher, or 80°C or higher.
[0087] 1.2. Method using recycled carbon fiber as starting material In the CBC manufacturing method described in 1.1 above, all or part of the virgin carbon fiber as starting material can be replaced with recycled carbon fiber.
[0088] Suitable examples of recycled carbon fibers are carbon fibers recovered from scraps of SMC (sheet molding compound) or waste CFRP made by curing SMC. Substantially all of the carbon fibers contained in SMC have the same fiber length, which is usually within the range of 3 mm to 60 mm.
[0089] For example, when the above-mentioned scrap or waste material is dry distilled at a temperature of preferably 600°C or higher and then further heated in an oxidizing atmosphere to, for example, 550°C or higher, preferably 600°C or higher, to completely pyrolyze the matrix resin, a flocculent carbon fiber remains, consisting of recycled carbon fibers almost all of which have the same fiber length. This recycled carbon fiber has been thermally deteriorated and is weaker than virgin carbon fiber, but it still has sufficient strength to be used as a reinforcing material for FRP.
[0090] Another method for recovering carbon fibers from CFRP waste is to decompose the matrix resin using a subcritical or supercritical fluid. The matrix resin is completely removed to obtain cotton-like recycled carbon fibers. Residual resin that remains can be removed by heat treatment in an oxidizing atmosphere. The recycled carbon fibers obtained by this method are also thermally deteriorated and therefore have lower strength than virgin carbon fibers.
[0091] As yet another method for recovering carbon fibers from CFRP waste, a method of decomposing the matrix resin by microwave heating can also be used. A small amount of carbon, which is a pyrolysis product of the matrix resin, may remain in recycled carbon fiber bundles extracted from SMC or CFRP waste by pyrolyzing the matrix resin. Carbon fiber bundles in which the carbon fiber filaments are bound together by a small amount of residual carbon can be defibrated, for example, by stirring in a dry state using a stirring mixer.
[0092] Another method for recovering carbon fibers from SMC scraps is to wash out the uncured matrix resin using a solvent, which may be a subcritical or supercritical fluid. This method allows for the production of recycled carbon fibers that have the same strength as virgin carbon fibers and are not thermally degraded.
[0093] The recycled carbon fibers recovered by the above method from CFRP or SMC scraps obtained by curing SMC are usually short fibers having a fiber length in the range of 3 mm to 60 mm, and do not require further cutting for use in the production of CBC, and the sizing agent has also been removed. When using only such recycled carbon fibers as the starting material, the (ii) defibrating step can be carried out as necessary, followed by the (iii) bundling step and (iv) cooling step described above in the same manner as when virgin carbon fibers are used as the starting material.
[0094] Recycled carbon fibers recovered by cutting off scraps of UD prepreg (uni-directional prepreg) or woven prepreg, or waste CFRP obtained by curing UD prepreg or woven prepreg to contain carbon fibers in a length within a range of 3 mm to 60 mm, and then subjecting the cut carbon fibers to the treatments exemplified above can also be preferably used in the manufacturing method of the CBC according to the embodiment.
[0095] The recycled carbon fiber batting may contain fibers other than carbon fiber. For example, the carbon fiber batting recovered from CFRP that uses carbon fiber cloth containing glass fiber stitches as a reinforcing material may contain glass fiber.
[0096] When recycled carbon fibers are used as a starting material, they may be used after removing fibers other than carbon fibers that have been mixed in. However, this is not essential. In other words, in the manufacturing method according to the embodiment, carbon fiber batting mixed with fibers other than carbon fibers may be used as a starting material.
[0097] For example, it is desirable to use carbon fiber wadding containing glass fibers as long as it contains the glass fibers as long as it does not cause any practical problems, from the viewpoint of reducing the burden on the environment. On the other hand, from the viewpoint of stabilizing the quality of CBC, the content of fibers other than carbon fibers in the carbon fiber wadding, which is the starting material, is preferably less than 10 wt%, more preferably less than 5 wt%, and even more preferably less than 1 wt%.
[0098] 2. Carbon Fiber Bundle Composite Another embodiment of the present invention is a CBC produced by the production method described in Section 1. This CBC comprises a plurality of short carbon fibers in bundles and an uncured solid epoxy resin composition.
[0099] The uncured solid epoxy resin composition contains an epoxy curing agent.
[0100] The number of short carbon fibers (filament count) forming the bundle may be, for example, 1000 to 20000. All of the short carbon fibers forming the bundle may have a fiber length of 60 mm or less, 50 mm or less, 40 mm or less, 30 mm or less, or 20 mm or less.
[0101] Since carbon fibers with too short a fiber length have a low reinforcing effect when used in FRP, the majority of the short carbon fibers constituting the bundle preferably have a fiber length of 3 mm or more, more preferably 5 mm or more, and even more preferably 10 mm or more. To increase the strength of CFRP molded using a CBC, it is effective to limit the content of carbon fibers shorter than a certain length. In a preferred example, the CBC does not contain carbon fibers with a fiber length of less than 3 mm, or if it does contain such fibers, the amount is less than 5 wt% of the total carbon fibers contained in the CBC. In a more preferred example, the CBC does not contain carbon fibers with a fiber length of less than 5 mm, or if it does contain such fibers, the amount is less than 5 wt% of the total carbon fibers contained in the CBC. In an even more preferred example, the CBC does not contain carbon fibers with a fiber length of less than 10 mm, or if it does contain such fibers, the amount is less than 5 wt% of the total carbon fibers contained in the CBC.
[0102] In a CBC in which all of the short carbon fibers in the bundle have the same fiber length L (mm), the bundle length will usually exceed L (mm). Depending on the bundle length and the length and number of short carbon fibers contained, the CBC may have a spindle, needle, or wire shape.
[0103] In the CBC according to the embodiment, by using only short carbon fibers having the same fiber length, it is possible to reduce the variation in quality between production lots. In this case, the difference between the maximum and minimum fiber lengths of the short carbon fibers constituting the bundle is preferably within 5 mm, more preferably within 4 mm, and even more preferably within 3 mm.
[0104] There is no particular limitation on the filament diameter of the short carbon fibers forming the bundle, and it may be, for example, within the range of filament diameters normally possessed by PAN-based carbon fibers, for example, within the range of 5 μm to 15 μm.
[0105] The uncured solid epoxy resin composition contained in the CBC according to the embodiment contains one or more epoxy resins. Examples of epoxy resins that can be blended include, but are not limited to, glycidyl ether, glycidyl amine, glycidyl ester, and alicyclic epoxy resins. The uncured solid epoxy resin composition may also contain an epoxy resin containing an oxazolidone ring.
[0106] Since the uncured solid epoxy resin composition contained in the CBC according to the embodiment is a solidified version of the molten resin used as a bundling liquid during the production of the CBC, the epoxy resin that may be contained in the solid epoxy resin composition is the same as the epoxy resin that may be blended into the molten resin. For the same reason, the components other than the epoxy resin that may be contained in the solid epoxy resin composition are the same as the various components other than the epoxy resin that may be blended into the molten resin.
[0107] The uncured solid epoxy resin composition contained in the CBC according to the embodiment is solid at least at a temperature within a range of 15 to 25°C (so-called room temperature), and is preferably solid at a temperature of 40°C, and more preferably solid at a temperature of 50°C.
[0108] The fiber weight content in the CBC according to embodiments can be 40 wt% or more but less than 50 wt%, 50 wt% or more but less than 60 wt%, 60 wt% or more but less than 70 wt%, or 70 wt% or more but less than 80 wt%.
[0109] The carbon fibers contained in the CBC according to the embodiment may be entirely non-thermally degraded carbon fibers, partially non-thermally degraded carbon fibers and the remainder thermally degraded carbon fibers, or entirely thermally degraded carbon fibers. A typical example of non-thermally degraded carbon fibers is virgin carbon fibers. A typical example of thermally degraded carbon fibers is recycled carbon fibers recovered from CFRP waste, which are thermally degraded in the process of pyrolysis and removal of the matrix resin.
[0110] In the CBC according to the embodiment, the bundles formed by the plurality of short carbon fibers may contain fibers other than carbon fibers. Such a CBC can be obtained, for example, when recycled carbon fibers are used as the starting material. When recycled carbon fibers containing glass fibers are used as the starting material, a CBC is obtained that is composed of a plurality of short carbon fibers that form bundles together with the glass fibers and an uncured solid epoxy resin composition. When the fiber bundles contained in the CBC contain fibers other than carbon fibers, the content of such fibers is preferably less than 10 wt %, more preferably less than 5 wt %, and even more preferably less than 1 wt %.
[0111] The CBC according to the embodiment is a prepreg material used in molding CFRP. A preferred molding method for producing CFRP products using the CBC according to the embodiment is press molding, but this is not limited to this. Molding methods other than press molding, such as autoclave molding, can also be used.
[0112] 3. Carbon Fiber Bundle Composite Sheet Using the CBC according to the embodiment, a CBC sheet, which is a sheet-shaped thermosetting molding material, can be manufactured, for example, by sequentially performing the following first to third steps. First step: Prepare a first protective film and a second protective film. Second step: Sprinkle the CBC on the first protective film to deposit a CBC layer. Third step: Place the second protective film on top of the CBC layer, and then heat and pressurize the CBC layer using a double belt press or a roll press to fuse the CBC together and form a sheet.
[0113] As the first protective film and the second protective film, release paper that is generally used in the production of carbon fiber prepregs can be preferably used.
[0114] When the CBC layer is heated and pressurized in the third step, the temperature is adjusted so that the solid epoxy resin composition contained in the CBC does not harden and lose its fluidity.
[0115] A conceptual diagram of a manufacturing apparatus that can be used to manufacture a CBC sheet using the above procedure is shown in Figure 1. This manufacturing apparatus has a section for depositing a CBC layer by spraying CBC onto a first protective film unwound from a roll, a section for covering the CBC layer with a second protective film unwound from a roll, a section for heating and pressurizing the CBC layer, and a section for winding up the CBC sheet.
[0116] The orientation of the CBC in the CBC layer may be random or biased in one direction. For example, the slower the running speed of the first protective film, the more random the orientation of the CBC. When the running speed of the first protective film is increased, the CBC tends to be oriented along the running direction.
[0117] In one example, the fiber weight content of a CBC sheet can be adjusted by adding uncured epoxy resin during its manufacture. This can be achieved by coating the surface of a first protective film with the supplemental uncured epoxy resin before depositing the CBC layer. Alternatively, or in addition, the surface of a second protective film can be coated with the supplemental uncured epoxy resin before applying the CBC layer.
[0118] The basis weight of the CBC sheet can be appropriately designed depending on the application. The basis weight is, for example, 300 g / m 2 More than 500g / m 2 Less than 500 g / m 2 More than 1000g / m 2 Less than 1000 g / m 2 More than 2000g / m 2 Less than 2000 g / m 2 More than 4000g / m 2 Less than 4000 g / m 2 More than 6000g / m2 Less than 6000 g / m 2 More than 8000g / m 2 Less than or equal to 8000 g / m 2 More than 10000g / m 2 It may be less than.
[0119] The thickness of the CBC sheet can be designed to be, for example, 0.5 mm or more and less than 1.5 mm, 1.5 mm or more and less than 3 mm, or 3 mm or more and 5 mm or less, but is not limited thereto.
[0120] The CBC sheet according to the embodiment is a prepreg material used in molding CFRP. A preferred example of a molding method for producing a CFRP product using the CBC sheet according to the embodiment is press molding, but this is not limited thereto, and molding methods other than press molding, such as autoclave molding, can also be used.
[0121] 4. Summary of Embodiments Embodiments of the present invention include, but are not limited to, the following.
[0122] [Embodiment 1] A method for producing a carbon fiber bundle composite, comprising mixing carbon fiber wadding made of short carbon fibers with a molten resin containing an epoxy resin component to obtain a carbon fiber bundle containing the molten resin, solidifying the molten resin contained in the carbon fiber bundle, and mixing at least one epoxy curing agent into the molten resin. [Embodiment 2] The production method according to embodiment 1, in which a stirring mixer is used for the mixing. [Embodiment 3] The production method according to embodiment 1 or 2, in which the molten resin is solidified by cooling the carbon fiber bundle containing the molten resin in a disc pelletizer. [Embodiment 4] The production method according to embodiment 1 or 2, in which the molten resin is solidified by cooling the carbon fiber bundle containing the molten resin in a transport pipe or on a conveyor belt. [Embodiment 5] The production method according to any one of embodiments 1 to 4, in which at least a portion of the at least one epoxy curing agent is mixed into the molten resin before mixing the molten resin with the carbon fiber wadding or simultaneously with mixing the molten resin with the carbon fiber wadding. [Embodiment 6] A manufacturing method according to any one of embodiments 1 to 5, wherein the molten resin is a melt of a resin that is solid at least at a temperature within the range of 15 to 25°C. [Embodiment 7] A manufacturing method according to any one of embodiments 1 to 6, wherein the molten resin is a melt of a resin that is solid at 40°C. [Embodiment 8] A manufacturing method according to any one of embodiments 1 to 7, wherein a flame retardant is mixed into the molten resin. [Embodiment 9] A manufacturing method according to any one of embodiments 1 to 8, wherein all of the carbon fibers contained in the carbon fiber batting have a fiber length of 60 mm or less, 50 mm or less, 40 mm or less, 30 mm or less, or 20 mm or less. [Embodiment 10] A manufacturing method according to any one of embodiments 1 to 9, wherein the carbon fiber batting does not contain carbon fibers with a fiber length of less than 3 mm, or if it does contain such fibers, the amount of such fibers is less than 5 wt% of the total carbon fibers contained in the carbon fiber batting. [Embodiment 11] A manufacturing method according to any one of embodiments 1 to 9, wherein the carbon fiber cotton does not contain carbon fibers with a fiber length of less than 5 mm, or if it does contain such fibers, the amount is less than 5 wt% of the total carbon fibers contained in the carbon fiber cotton.[Embodiment 12] The manufacturing method according to any one of embodiments 1 to 9, wherein the carbon fiber wadding does not contain carbon fibers with a fiber length of less than 10 mm, or if it does contain such fibers, the amount is less than 5 wt % of the total carbon fibers contained in the carbon fiber wadding. [Embodiment 13] The manufacturing method according to any one of embodiments 1 to 12, wherein some of the carbon fibers contained in the carbon fiber wadding are provided by defibrating chopped carbon fiber bundles. [Embodiment 14] The manufacturing method according to any one of embodiments 1 to 8, wherein all of the carbon fibers contained in the carbon fiber wadding are provided by defibrating chopped carbon fiber bundles. [Embodiment 15] The manufacturing method according to embodiment 14, wherein the fiber length of the chopped carbon fiber bundles is 3 mm or more, 5 mm or more, or 10 mm or more. [Embodiment 16] The manufacturing method according to embodiment 14 or 15, wherein the fiber length of the chopped carbon fiber bundles is 60 mm or less, 50 mm or less, 40 mm or less, 30 mm or less, or 20 mm or less. [Embodiment 17] A manufacturing method according to any one of embodiments 1 to 16, wherein all of the short carbon fibers are carbon fibers that have not been thermally deteriorated. [Embodiment 18] A manufacturing method according to any one of embodiments 1 to 13, wherein the short carbon fibers include thermally deteriorated carbon fibers. [Embodiment 19] A manufacturing method according to any one of embodiments 1 to 13 and 18, wherein the carbon fiber batting is mixed with fibers other than carbon fibers, and the fibers other than carbon fibers may be glass fibers. [Embodiment 20] A manufacturing method according to any one of embodiments 1 to 19, wherein the carbon fiber bundles containing the molten resin are isolated fiber bundles. [Embodiment 21] A carbon fiber bundle composite manufactured by the manufacturing method according to any one of embodiments 1 to 20.
[0123] [Embodiment 22] A carbon fiber bundle composite comprising a plurality of short carbon fibers forming bundles and an uncured solid epoxy resin composition, wherein the positions of the tips of the plurality of short carbon fibers at each end of the bundle are irregular, and the uncured solid epoxy resin composition contains at least one epoxy curing agent. [Embodiment 23] The carbon fiber bundle composite according to embodiment 22, wherein the uncured solid epoxy resin composition is solid at least at a temperature in the range of 15 to 25°C. [Embodiment 24] The carbon fiber bundle composite according to embodiment 22, wherein the uncured solid epoxy resin composition is solid at 40°C. [Embodiment 25] The carbon fiber bundle composite according to any one of embodiments 22 to 24, wherein the bundles are isolated. [Embodiment 26] The carbon fiber bundle composite according to embodiment 25, wherein the shape is needle-like or wire-like. [Embodiment 27] A carbon fiber bundle composite according to any one of embodiments 22 to 26, wherein all of the plurality of short carbon fibers have a fiber length of 60 mm or less, 50 mm or less, 40 mm or less, 30 mm or less, or 20 mm or less. [Embodiment 28] A carbon fiber bundle composite according to any one of embodiments 22 to 27, having a bundle length of 3 mm or more, 5 mm or more, or 10 mm or more. [Embodiment 29] A carbon fiber bundle composite according to any one of embodiments 22 to 28, which does not contain any carbon fibers with a fiber length of less than 3 mm, or if it contains any, the amount thereof is less than 5 wt % of the total carbon fibers in the carbon fiber bundle composite. [Embodiment 30] A carbon fiber bundle composite according to any one of embodiments 22 to 27, which has a bundle length of 5 mm or more or 10 mm or more, and which does not contain any carbon fibers with a fiber length of less than 5 mm, or if it contains any, the amount thereof is less than 5 wt % of the total carbon fibers in the carbon fiber bundle composite. [Embodiment 31] A carbon fiber bundle composite according to any one of embodiments 22 to 27, having a bundle length of 10 mm or more, and not containing any carbon fibers with fiber lengths less than 10 mm, or if any carbon fibers are contained, the amount of such fibers is less than 5 wt % of the total carbon fibers in the carbon fiber bundle composite. [Embodiment 32] A carbon fiber bundle composite according to any one of embodiments 22 to 31, wherein the difference between the maximum and minimum fiber lengths of the plurality of short carbon fibers is 5 mm or less. [Embodiment 33] A carbon fiber bundle composite according to embodiment 25, having a spindle shape.[Embodiment 34] The carbon fiber bundle composite according to any one of embodiments 22 to 33, wherein the at least one epoxy curing agent comprises a latent curing agent. [Embodiment 35] The carbon fiber bundle composite according to any one of embodiments 22 to 34, wherein the fiber weight content is 40 wt% or more and less than 50 wt%, 50 wt% or more and less than 60 wt%, 60 wt% or more and less than 70 wt%, or 70 wt% or more and 80 wt% or less. [Embodiment 36] The carbon fiber bundle composite according to any one of embodiments 22 to 35, wherein all of the plurality of short carbon fibers are carbon fibers that have not been thermally deteriorated. [Embodiment 37] The carbon fiber bundle composite according to any one of embodiments 22 to 35, wherein the plurality of short carbon fibers include thermally deteriorated carbon fibers. [Embodiment 38] The carbon fiber bundle composite according to any one of embodiments 22 to 35 and 37, wherein the plurality of short carbon fibers form the bundle together with fibers other than carbon fibers, and the fibers other than carbon fibers may be glass fibers.
[0124] [Embodiment 39] A carbon fiber bundle composite sheet formed by fusing together a plurality of the carbon fiber bundle composites according to any one of embodiments 21 to 38. [Embodiment 40] A carbon fiber bundle composite sheet comprising a plurality of the carbon fiber bundle composites according to any one of embodiments 21 to 38, each of the carbon fiber bundle composites being fused to at least one other of the carbon fiber bundle composites. [Embodiment 41] A method for producing a carbon fiber bundle composite sheet, comprising fusing together a plurality of the carbon fiber bundle composites according to any one of embodiments 21 to 38. [Embodiment 42] A production method according to embodiment 41, wherein uncured epoxy resin is added to the carbon fiber bundle composites during the fusing.
[0125] [Embodiment 43] The production method according to any one of embodiments 1 to 20, wherein the molten resin is a melt of an epoxy resin having a melting point. [Embodiment 44] A carbon fiber bundle composite produced by the production method according to embodiment 43. [Embodiment 45] A carbon fiber bundle composite according to any one of embodiments 22 to 38, wherein the uncured solid epoxy resin composition has a melting point. [Embodiment 46] A carbon fiber bundle composite sheet obtained by fusing together a plurality of carbon fiber bundle composites according to embodiment 45. [Embodiment 47] A carbon fiber bundle composite sheet comprising a plurality of carbon fiber composites according to embodiment 45, each of the carbon fiber bundle composites being fused to at least one other of the carbon fiber bundle composites. [Embodiment 48] A method for producing a carbon fiber bundle composite sheet, comprising fusing together a plurality of carbon fiber bundle composites according to embodiment 45. [Embodiment 49] The production method according to embodiment 48, wherein uncured epoxy resin is supplemented to the carbon fiber bundle composites during the fusing.
[0126] 5. Experimental Results The results of the experiments conducted by the inventors are described below. The materials used in each experiment are as follows. Carbon fiber: Water-sized chopped carbon fiber with a fiber length of 6 mm was dried at 120°C for 1 hour and then hand-unraveled to obtain cotton-like carbon fiber. Epoxy resin: YX4000 manufactured by Mitsubishi Chemical Corporation, a biphenyl-type epoxy resin with a nominal melting point of 105°C, was used. The viscosity of this epoxy resin at 120°C was measured using a Brookfield LVDV-1 rotational viscometer (spindle S61, 50 rpm), and was found to be 0.048 Pa·s. Epoxy curing agent: DICY7 powder epoxy curing agent manufactured by Mitsubishi Chemical Corporation was used. The melting point of dicyandiamide, a component of this epoxy curing agent, is approximately 210°C.
[0127] [Experiment 1] 10 g of epoxy resin powder and 0.3 g of epoxy curing agent were mixed in a container (a polypropylene bottle with a lid) and then placed in a thermostatic chamber at 120 °C for 10 minutes to obtain a molten epoxy resin containing dispersed epoxy curing agent. Immediately after removing the container from the thermostatic chamber, 23 g of carbon fiber was added. The container was then shaken by hand to mix the molten epoxy resin and carbon fiber. After the temperature dropped and the epoxy resin solidified during shaking, the container was returned to the thermostatic chamber at 120 °C for 10 minutes to melt the epoxy resin. The container was then shaken outside the thermostatic chamber until the epoxy resin solidified again. This process was repeated four times until all the flocculent carbon fiber was mixed with the epoxy resin, resulting in a carbon fiber bundle composite with a nearly spindle-shaped shape, as shown in Figure 2. The carbon fiber bundle composites were generally within the range of 1 to 3 cm in length.
[0128] [Experiment 2] The carbon fibers were mixed with the molten epoxy resin in which the epoxy curing agent had been dispersed in the same manner as in Experiment 1, except that the amount of carbon fibers was changed from 23 g to 10 g. After repeating the procedure twice, which was repeated four times in Experiment 1, all of the cotton-like carbon fibers were mixed with the epoxy resin, and a wire-like carbon fiber bundle composite was obtained, as shown in Figure 3. The length of the carbon fiber bundle composite was generally within the range of 4 to 10 cm.
[0129] [Experiment 3] Carbon fibers were mixed with molten epoxy resin in which an epoxy curing agent had been dispersed in the same manner as in Experiment 1, except that the amount of carbon fibers was changed from 23 g to 30 g. After repeating the procedure 10 times, which was repeated four times in Experiment 1, all of the cotton-like carbon fibers were mixed with the epoxy resin, and needle-like carbon fiber bundle composites were obtained, as shown in Figure 4. The length of the carbon fiber bundle composites was generally within the range of 1 to 2 cm.
[0130] [Experiment 4] A carbon fiber bundle composite sheet measuring 100 mm x 60 mm and 1.8 mm thick was molded from 15 g of the spindle-shaped carbon fiber bundle composite obtained in Experiment 1 by pressing for 10 minutes using a press mold consisting of a cavity and a core at a temperature of 120°C and a pressure of 8 MPa. The appearance of the obtained carbon fiber bundle composite sheet is shown in Figure 5. This carbon fiber bundle composite sheet was flexible immediately after being removed from the press mold at a temperature of 120°C, but lost its flexibility when the temperature was reduced to room temperature.
[0131] [Experiment 5] The carbon fiber bundle composite sheet obtained in Experiment 4 was sandwiched between two metal plates and pressed for 120 minutes at a temperature of 180°C and a pressure of 8 MPa to form a CFRP plate. The resulting CFRP plate had dimensions of 105 mm x 70 mm and a thickness of 1.5 mm. This indicates that the carbon fiber composite sheet flowed slightly during molding. The CFRP plate did not soften even when heated to 120°C, indicating that the epoxy resin contained in the CFRP plate was hardened.
[0132] Although the present invention has been described above with reference to specific embodiments, each embodiment is presented as an example and does not limit the scope of the present invention. Each embodiment described in this specification can be modified in various ways within the scope of the effects of the invention and can be combined with features described in other embodiments to the extent possible. This application is based on Japanese Patent Application No. 2022-33126 filed on March 4, 2022 and Japanese Patent Application No. 2022-180699 filed on November 11, 2022, and is incorporated by reference in its entirety.
[0133] The CBC and CBC sheet according to the embodiments can be preferably used to manufacture various CFRP parts used in automobiles, motorcycles, bicycles, ships, railroad vehicles, manned aircraft, unmanned aircraft, and other transportation equipment, as well as sporting goods, leisure goods, home appliances, agricultural machinery, building materials, and the like.
Claims
1. A method for producing a carbon fiber bundle composite, comprising: mixing carbon fiber wadding made of short carbon fibers with a molten resin containing an epoxy resin component to obtain a carbon fiber bundle containing the molten resin; solidifying the molten resin contained in the carbon fiber bundle; and mixing at least one epoxy curing agent into the molten resin, A method for producing a carbon fiber bundle composite, wherein the carbon fiber cotton does not contain carbon fibers with a fiber length of less than 5 mm, or even if it does contain such fibers, the amount of such fibers is less than 5 wt % of the total carbon fibers contained in the carbon fiber cotton.
2. The method according to claim 1 , wherein a stirring mixer is used for the mixing.
3. The method according to claim 1 , wherein the molten resin is solidified by cooling the carbon fiber bundles containing the molten resin in a disc pelletizer.
4. The method according to claim 1 , wherein the carbon fiber bundle containing the molten resin is cooled in a transport pipe or on a conveyor belt to solidify the molten resin.
5. The manufacturing method according to claim 1 , wherein at least a portion of the at least one epoxy curing agent is mixed into the molten resin before mixing the molten resin with the carbon fiber cotton or simultaneously with mixing the molten resin with the carbon fiber cotton.
6. The method according to claim 1, wherein the molten resin is a melt of a resin that is solid at a temperature in the range of at least 15 to 25°C.
7. The manufacturing method according to claim 1 , wherein the molten resin is a melt of a resin that is solid at 40° C.
8. The method according to claim 1 , wherein a flame retardant is mixed into the molten resin.
9. The manufacturing method according to claim 1 , wherein all of the carbon fibers contained in the carbon fiber cotton have a fiber length of 60 mm or less, 50 mm or less, 40 mm or less, 30 mm or less, or 20 mm or less.
10. The manufacturing method according to claim 1 , wherein the carbon fiber cotton does not contain carbon fibers having a fiber length of less than 3 mm, or even if it does contain such carbon fibers, the amount of such carbon fibers is less than 5 wt % of the total carbon fibers contained in the carbon fiber cotton.
11. The manufacturing method according to claim 1 , wherein the carbon fiber cotton does not contain carbon fibers having a fiber length of less than 10 mm, or even if it does contain such carbon fibers, the amount of such carbon fibers is less than 5 wt % of the total carbon fibers contained in the carbon fiber cotton.
12. The manufacturing method according to claim 1 , wherein at least a portion of the carbon fibers contained in the carbon fiber cotton is provided by defibrating chopped carbon fiber bundles.
13. The manufacturing method according to claim 1 , wherein all of the carbon fibers contained in the carbon fiber cotton are provided by defibrating chopped carbon fiber bundles.
14. The manufacturing method according to claim 13, wherein the chopped carbon fiber bundles have a fiber length of 3 mm or more, 5 mm or more, or 10 mm or more.
15. The manufacturing method according to claim 13, wherein the chopped carbon fiber bundles have a fiber length of 60 mm or less, 50 mm or less, 40 mm or less, 30 mm or less, or 20 mm or less.
16. The method according to claim 1 , wherein all of the short carbon fibers are non-thermally deteriorated carbon fibers.
17. The method of claim 1 , wherein the short carbon fibers comprise thermally degraded carbon fibers.
18. The manufacturing method according to claim 1 , wherein the carbon fiber cotton is mixed with fibers other than carbon fibers, and the fibers other than carbon fibers may be glass fibers.
19. The method according to claim 1 , wherein the carbon fiber bundles containing the molten resin are isolated fiber bundles.
20. A carbon fiber bundle composite produced by the method according to claim 1.
21. A carbon fiber bundle composite comprising a plurality of short carbon fibers forming a bundle and an uncured solid epoxy resin composition, the ends of the plurality of short carbon fibers at each end of the bundle being irregularly positioned, and the uncured solid epoxy resin composition containing at least one epoxy curing agent, A carbon fiber bundle composite having a fiber weight content of 40 wt % or more and less than 50 wt %, 50 wt % or more and less than 60 wt %, 60 wt % or more and less than 70 wt %, or 70 wt % or more and less than 80 wt %.
22. The carbon fiber bundle composite of claim 21, wherein the uncured solid epoxy resin composition is solid at least at a temperature in the range of 15 to 25°C.
23. 22. The carbon fiber bundle composite of claim 21, wherein the uncured solid epoxy resin composition is solid at 40°C.
24. 22. The carbon fiber bundle composite of claim 21 , wherein the bundles are isolated.
25. The carbon fiber bundle composite of claim 24, having a needle-like or wire-like shape.
26. 22. The carbon fiber bundle composite of claim 21, wherein all of the plurality of short carbon fibers have a fiber length of 60 mm or less, 50 mm or less, 40 mm or less, 30 mm or less, or 20 mm or less.
27. 22. The carbon fiber bundle composite of claim 21 having a bundle length of 3 mm or more, 5 mm or more, or 10 mm or more.
28. A carbon fiber bundle composite according to claim 21, which does not contain any carbon fibers with a fiber length of less than 3 mm, or if it does contain any, the amount of such carbon fibers is less than 5 wt % of the total carbon fibers in the carbon fiber bundle composite.
29. A carbon fiber bundle composite according to claim 21, having a bundle length of 5 mm or more or 10 mm or more, and not containing any carbon fibers with a fiber length of less than 5 mm, or if any, the amount of such fibers is less than 5 wt% of the total carbon fibers in the carbon fiber bundle composite.
30. A carbon fiber bundle composite according to claim 21, having a bundle length of 10 mm or more, and not containing any carbon fibers with fiber lengths less than 10 mm, or if any, the amount of such carbon fibers is less than 5 wt% of the total carbon fibers in the carbon fiber bundle composite.
31. The carbon fiber bundle composite according to claim 21 , wherein the difference between the maximum and minimum fiber lengths of the short carbon fibers is within 5 mm.
32. 25. The carbon fiber bundle composite of claim 24, having a spindle shape.
33. 22. The carbon fiber bundle composite of claim 21, wherein the at least one epoxy curing agent comprises a latent curing agent.
34. 22. The carbon fiber bundle composite of claim 21, wherein all of the plurality of short carbon fibers are non-thermally degraded carbon fibers.
35. 22. The carbon fiber bundle composite of claim 21, wherein the plurality of short carbon fibers comprises thermally degraded carbon fibers.
36. The carbon fiber bundle composite according to claim 21 , wherein the plurality of short carbon fibers form the bundle together with fibers other than carbon fibers, and the fibers other than carbon fibers may be glass fibers.
37. A carbon fiber bundle composite sheet obtained by fusing a plurality of the carbon fiber bundle composites according to any one of claims 20 to 36 to each other.
38. A carbon fiber bundle composite sheet comprising a plurality of carbon fiber bundle composites according to any one of claims 20 to 36, each of which is fused to at least one other of the carbon fiber bundle composites.
39. A method for producing a carbon fiber bundle composite sheet, comprising fusing a plurality of the carbon fiber bundle composites according to any one of claims 20 to 36 to each other.
40. 40. The method of claim 39, wherein the carbon fiber bundle composite is supplemented with uncured solid epoxy resin composition during said fusing.
41. The manufacturing method according to any one of claims 1 to 19, wherein the molten resin is a melt of an epoxy resin having a melting point.
42. A carbon fiber bundle composite produced by the method of claim 41.
43. The carbon fiber bundle composite according to any one of claims 21 to 36, wherein the uncured solid epoxy resin composition has a melting point.
44. A carbon fiber bundle composite sheet obtained by fusing a plurality of the carbon fiber bundle composites according to claim 43 to each other.
45. A carbon fiber bundle composite sheet comprising a plurality of carbon fiber bundle composites according to claim 43, each of said carbon fiber bundle composites being fused to at least one other of said carbon fiber bundle composites.
46. A method for producing a carbon fiber bundle composite sheet, comprising fusing together a plurality of the carbon fiber bundle composites according to claim 43.
47. 47. The method of claim 46, wherein the carbon fiber bundle composite is supplemented with uncured epoxy resin during the fusing.