Polypropylene foam particles, polypropylene foam molded body, method for producing polypropylene foam particles, and method for producing polypropylene foam molded body
Patent Information
- Application Number
- JP2024509936
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-03-06
AI Technical Summary
Conventional polypropylene foam molded products for electrical components lack sufficient flame retardancy, which is a concern for safety and compliance with stringent standards, especially in the context of electric vehicles where peripheral members require enhanced fire resistance.
The development of expanded polypropylene particles made from a specific blend of polypropylene resins with intumescent flame retardants, which are processed using a method involving dispersion and foaming to create a foam structure with improved flame retardancy, including a base resin with a specific composition and a controlled foaming process to achieve enhanced properties.
The resulting polypropylene foam molded articles exhibit excellent flame retardancy, meeting or exceeding UL94V standards, including self-extinguishing properties and reduced risk of combustion spread, thus ensuring safety and compliance with stringent fire resistance requirements.
Abstract
Description
Polypropylene-based expanded beads, polypropylene-based expanded molded article, and methods for producing the same
[0001] The present invention relates to expanded polypropylene beads, expanded polypropylene molded articles, and methods for producing the same.
[0002] Molded articles (foamed molded articles) obtained by molding polypropylene-based expanded beads have conventionally been widely used as interior materials and cushioning materials for automobiles. Recently, with the shift to electric vehicles, there has been an increasing demand for applying polypropylene-based foamed molded articles to peripheral members for electrical components.
[0003] Polypropylene foam molded articles used as peripheral members of electrical components are required to have high flame retardancy, and techniques for imparting flame retardancy to polypropylene foam molded articles have been proposed (for example, Patent Document 1).
[0004] International Publication No. 2016 / 052739
[0005] The above-mentioned conventional techniques have room for further improvement in terms of the flame retardancy of the resulting foamed molded articles.
[0006] In view of the above circumstances, an object of one embodiment of the present invention is to provide polypropylene-based expanded beads that can provide polypropylene-based expanded molded articles having excellent flame retardancy.
[0007] The present inventors have conducted extensive research to solve the above problems and have completed the present invention.
[0008] That is, the expanded polypropylene beads according to one embodiment of the present invention are obtained by expanding polypropylene resin particles containing a base resin including: a polypropylene resin (a) having an MI of 4.00 g / 10 min to 15.00 g / 10 min and a melting point of 135°C to 155°C; and a polypropylene resin (b) having an MI of 0.05 g / 10 min to 3.00 g / 10 min and a melting point of 135°C to 155°C; and an intumescent flame retardant.
[0009] Further, a method for producing polypropylene-based expanded beads according to one embodiment of the present invention includes a dispersing step of dispersing polypropylene-based resin particles, an aqueous dispersion medium, and a blowing agent in a container, and a discharging step of discharging the dispersion obtained in the dispersing step into a region having a pressure lower than the pressure inside the container, wherein the polypropylene-based resin particles include a base resin including a polypropylene-based resin (a) having an MI of 4.00 g / 10.00 min to 15.00 g / 10 min and a melting point of 135°C to 155°C, and a polypropylene-based resin (b) having an MI of 0.05 g / 10 min to 3.00 g / 10 min and a melting point of 135°C to 155°C, and an intumescent flame retardant.
[0010] According to one embodiment of the present invention, it is possible to provide a polypropylene-based foamed molded article having excellent flame retardancy, and it is also possible to provide polypropylene-based foamed beads.
[0011] An embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to the respective configurations described below, and various modifications are possible within the scope of the claims. Furthermore, embodiments or examples obtained by combining the technical means disclosed in different embodiments or examples are also included in the technical scope of the present invention. Furthermore, new technical features can be formed by combining the technical means disclosed in each embodiment. All academic literature and patent documents described in this specification are incorporated herein by reference. Furthermore, unless otherwise specified in this specification, the term "A to B" representing a numerical range means "greater than or equal to A (including and greater than A) and less than or equal to B (including and less than B)."
[0012] In this specification, a constitutional unit derived from an X monomer contained in a polymer or copolymer may be referred to as an "X unit".
[0013] Unless otherwise specified in this specification, the structural unit is X 1 Units and X 2 Units, ... and X n A copolymer containing units (n is an integer of 2 or more) is referred to as "X 1 / X2 / ・・・ / X n Also referred to as "copolymer". X 1 / X 2 / ・・・ / X n Unless otherwise specified, the polymerization mode of the copolymer is not particularly limited, and the copolymer may be a random copolymer, an alternating copolymer, a block copolymer, or a graft copolymer.
[0014] [1. Expanded Polypropylene-Based Beads] Expanded polypropylene-based beads according to one embodiment of the present invention are obtained by expanding polypropylene-based resin particles containing a base resin including: a polypropylene-based resin (a) having an MI of 4.00 g / 10.00 min to 15.00 g / 10 min and a melting point of 135° C. to 155° C.; and a polypropylene-based resin (b) having an MI of 0.05 g / 10 min to 3.00 g / 10 min and a melting point of 135° C. to 155° C.; and an intumescent flame retardant.
[0015] The expanded beads according to one embodiment of the present invention have the above-described structure, and therefore have the advantage of being able to provide a polypropylene-based expanded molded article having excellent flame retardancy. The expanded beads according to one embodiment of the present invention can also be said to be expanded beads made from the polypropylene-based resin beads according to one embodiment of the present invention.
[0016] A polypropylene-based expanded molded article can be provided by in-mold foaming of the polypropylene-based expanded beads according to one embodiment of the present invention using a known method.
[0017] In this specification, "polypropylene-based resin particles" may be referred to as "resin particles," "polypropylene-based resin particles according to one embodiment of the present invention" may be referred to as "the present resin particles," "polypropylene-based expanded particles" may be referred to as "expanded particles," "polypropylene-based expanded particles according to one embodiment of the present invention" may be referred to as "the present expanded particles," and "polypropylene-based expanded molded body" may be referred to as "expanded molded body."
[0018] Hereinafter, each component that may be contained in the present resin particles, which are the raw materials for the present expanded beads, will be described.
[0019] <Base Resin> The present resin particles contain a base resin including: (a) a polypropylene-based resin having an MI of 4.00 g / 10 min to 15.00 g / 10 min and a melting point of 135° C. to 155° C.; and (b) a polypropylene-based resin having an MI of 0.05 g / 10 min to 3.00 g / 10 min and a melting point of 135° C. to 155° C. In this specification, the term "base resin" refers to the resin component that substantially constitutes the present resin particles.
[0020] The base resin preferably contains 20 to 95% by weight, more preferably 30 to 90% by weight, and even more preferably 35 to 75% by weight of the polypropylene-based resin (a) relative to 100% by weight of the base resin. Expanded beads obtained by expanding resin beads containing a base resin satisfying this composition have the advantage of being able to provide an expanded molded article with excellent surface properties.
[0021] The base resin preferably contains 5 to 80% by weight, more preferably 10 to 70% by weight, and even more preferably 25 to 65% by weight of the polypropylene-based resin (b) based on 100% by weight of the base resin. Expanded beads obtained by expanding resin beads containing a base resin satisfying this composition have the advantage of being able to provide foamed molded articles with excellent flame retardancy that can meet the standards of the UL94V vertical flame test, which is an indicator of high flame retardancy.
[0022] The present resin particles preferably contain 70.0 wt% or more of the base resin relative to 100 wt% of the total amount of the resin particles, more preferably 75.0 wt% or more, and even more preferably 77.0 wt% or more. When the resin particles contain (i) 70.0 wt% or more of the base resin, a foamed molded article without sink marks and excellent strength (e.g., compressive strength) can be obtained. The upper limit of the content of the base resin in the present foamed resin is not particularly limited, but can be, for example, 89.0 wt% or less, preferably 85.0 wt% or less, and more preferably 80.0 wt% or less relative to 100 wt% of the total amount of the resin particles.
[0023] (Polypropylene-based resin) The base resin contained in the resin particles includes two types of polypropylene-based resins (polypropylene-based resin (a) and polypropylene-based resin (b)). In the following description, unless otherwise specified, the description of "polypropylene-based resin" can apply to either "polypropylene-based resin (a)" or "polypropylene-based resin (b)."
[0024] In this specification, the term "polypropylene resin" refers to a resin containing 50 mol % or more of propylene units out of 100 mol % of all structural units constituting the polypropylene resin.
[0025] In this specification, a "structural unit derived from a propylene monomer" may also be referred to as a "propylene unit."
[0026] The polypropylene-based resin may be (i) a homopolymer of propylene, (ii) a block copolymer, alternating copolymer, random copolymer, or graft copolymer of propylene and a monomer other than propylene, or (iii) a mixture of two or more of these.
[0027] Among these, it is preferable that the polypropylene-based resin is a random copolymer of propylene and a monomer other than propylene, since this has the advantage that the resin particles and expanded particles can be processed at a low heating temperature in the foaming process and in-mold foam molding process described below.
[0028] In one embodiment of the present invention, from the viewpoint of achieving excellent heat resistance, impact absorption, and chemical resistance of the resulting foamed molded article, it is preferable that the polypropylene-based resin (a) and / or the polypropylene-based resin (b) are each a random copolymer, and it is more preferable that the polypropylene-based resin (a) and the polypropylene-based resin (b) are each a random copolymer.
[0029] A polypropylene-based resin may have, in addition to a propylene unit, one or more structural units derived from a monomer other than a propylene monomer, and may have one or more types of structural units. A "monomer other than a propylene monomer" used in the production of a polypropylene-based resin may also be referred to as a "comonomer." A "structural unit derived from a monomer other than a propylene monomer" contained in a polypropylene-based resin may also be referred to as a "comonomer unit."
[0030] Comonomers include α-olefins having 2 or 4 to 12 carbon atoms, such as ethylene, 1-butene, isobutene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3,4-dimethyl-1-butene, 1-heptene, 3-methyl-1-hexene, 1-octene, and 1-decene.
[0031] Specific examples of polypropylene-based resins include polypropylene homopolymers, ethylene / propylene random copolymers, 1-butene / propylene random copolymers, 1-butene / ethylene / propylene random copolymers, ethylene / propylene block copolymers, 1-butene / propylene block copolymers, propylene / chlorinated vinyl copolymers, propylene / maleic anhydride copolymers, and styrene-modified polypropylene-based resins.
[0032] As the polypropylene-based resin, one of the above-mentioned specific examples may be used alone, or two or more may be used in combination. Among the above-mentioned specific examples, ethylene / propylene random copolymers and 1-butene / ethylene / propylene random copolymers are preferred because the resulting resin particles have good expandability and the resulting expanded particles have good moldability.
[0033] Consider a case where an ethylene / propylene random copolymer is used as the polypropylene-based resin (Case A). In Case A, the ethylene content of the ethylene / propylene random copolymer is preferably 0.2 wt% to 15.0 wt%, more preferably 0.5 wt% to 10.0 wt%, and even more preferably 0.5 wt% to 4.0 wt%, based on 100 wt% of each copolymer. The ethylene content can also be referred to as the content of structural units derived from ethylene (ethylene units). When the ethylene unit content in the ethylene / propylene random copolymer is (i) 0.2 wt% or more, the expandability of the resin particles in the production of the expanded beads and / or the moldability of the resulting expanded beads tend to be good, and (ii) when it is 15.0 wt% or less, there is no risk of a decrease in the mechanical properties of the expanded molded article obtained from the expanded beads.
[0034] The melting point of the polypropylene resin (a) is preferably 135° C. to 155° C., more preferably 136° C. to 154° C., more preferably 137° C. to 153° C., more preferably 138° C. to 152° C., even more preferably 139° C. to 151° C., and particularly preferably 140° C. to 150° C. When the melting point of the polypropylene resin is (i) 135° C. or higher, a foamed molded article having excellent dimensional stability at high temperatures tends to be obtained, and (ii) when it is 155° C. or lower, a foamed molded article can be foam-molded in a mold at low steam pressure.
[0035] The melting point of the polypropylene resin (b) is preferably 135° C. to 155° C., more preferably 136° C. to 154° C., more preferably 137° C. to 153° C., more preferably 138° C. to 152° C., even more preferably 139° C. to 151° C., and particularly preferably 140° C. to 150° C. When the melting point of the polypropylene resin (b) is (i) 135° C. or higher, a foamed molded article having excellent dimensional stability at high temperatures tends to be obtained, and (ii) when the melting point is 155° C. or lower, a foamed molded article having excellent surface properties can be obtained by in-mold foam molding at low steam pressure.
[0036] The resin particles of the present invention contain, as base resins, polypropylene-based resin (a) and polypropylene-based resin (b) each having a melting point of 135°C to 155°C, and therefore tend to easily produce foamed molded articles with excellent dimensional stability at high temperatures, and also enable in-mold foaming of foamed molded articles at lower water vapor pressures.
[0037] In this specification, the melting point of a polypropylene-based resin is a value determined by measurement using a differential scanning calorimeter (hereinafter referred to as the "DSC method"). The specific operating procedure is as follows: (1) 5 mg to 6 mg of polypropylene-based resin are melted by raising the temperature from 40.0°C to 220.0°C at a heating rate of 10.0°C / min; (2) The temperature of the molten polypropylene-based resin is then lowered from 220.0°C to 40.0°C at a heating rate of 10°C / min to crystallize the polypropylene-based resin; (3) The temperature of the crystallized polypropylene-based resin is then further raised from 40.0°C to 220.0°C at a heating rate of 10°C / min. The temperature of the peak (melting peak) of the DSC curve of the polypropylene-based resin obtained during the second heating (i.e., during (3)) can be determined as the melting point of the polypropylene-based resin. In addition, when there are multiple peaks (melting peaks) in the DSC curve of the polypropylene-based resin obtained during the second temperature increase by the above-mentioned method, the temperature of the peak (melting peak) with the largest heat of fusion is taken as the melting point of the polypropylene-based resin. As the differential scanning calorimeter, for example, DSC6200 manufactured by Seiko Instruments Inc. can be used.
[0038] The melt index (MI) of the polypropylene resin (a) at 230°C is 4.00 g / 10 min to 15.00 g / 10 min, preferably 5.00 g / 10 min to 15.00 g / 10 min, more preferably 5.50 g / 10 min to 12.00 g / 10 min, even more preferably 6.00 g / 10 min to 10.00 g / 10 min, and even more preferably 6.50 g / 10 min to 8.00 g / 10 min. Incidentally, MI is sometimes referred to as "melt flow rate (MFR)".
[0039] When the MI of the polypropylene-based resin (a) is 4.00 g / 10 min or more, the polypropylene-based resin has good fluidity during foaming and is easy to foam. Furthermore, when the MI of the polypropylene-based resin (a) is 15.00 g / 10 min or less, the polypropylene-based resin has appropriate fluidity, allowing for the production of expanded beads with a high expansion ratio. In particular, when the MI of the polypropylene-based resin (a) is 4.00 g / 10 min to 8.00 g / 10 min, expanded beads that can suitably provide foamed molded articles with a relatively high density can be efficiently produced, which is preferred.
[0040] The melt index (MI) of the polypropylene resin (b) at 230°C is 0.05 g / 10 min to 3.00 g / 10 min, preferably 0.10 g / 10 min to 2.00 g / 10 min, more preferably 0.30 g / 10 min to 1.00 g / 10 min, and even more preferably 0.40 g / 10 min to 0.60 g / 10 min.
[0041] When the polypropylene resin (b) has an MI of 0.05 g / 10 min or more, it has the advantage of being less likely to become non-dispersed when kneaded with the polypropylene resin (a) in the granulation step described below, allowing for more uniform mixing. Furthermore, when the polypropylene resin (b) has an MI of 3.00 g / 10 min or less, expanded particles can be obtained that can provide foamed molded articles with excellent flame retardancy. The method for measuring the MI of the polypropylene resin is as described in the Examples.
[0042] The weight average molecular weight (Mw) of the polypropylene resin (a) is not particularly limited, but is preferably 1×10 4 That's it, 80 x 10 4 Preferably, it is less than 5×10 4 ~75 x 10 4 is more preferable, and 10×10 4 ~50 x 10 4 is more preferable.
[0043] The weight average molecular weight (Mw) of the polypropylene resin (b) is not particularly limited, but is preferably 80×10 4 It is preferable that the ratio is 100×10 or more. 4More preferably, it is 110×10 4 It is more preferable that the polypropylene resin (b) is 100×10 4 By using a resin having a relatively large Mw as described above, it is possible to provide a foamed molded article having excellent flame retardancy that satisfies the high flame retardancy standard (UL94V) even when the resin is relatively light (low density) or has a relatively thin thickness (sample thickness). The upper limit of the Mw of the polypropylene-based resin (b) is not particularly limited, but it can be, for example, 200 × 10 4 It can be the following:
[0044] In this specification, the Mw of a polypropylene-based resin is a value measured as a polystyrene equivalent value by gel permeation chromatography (GPC). An example of GPC measurement conditions for measuring the Mw of a polypropylene-based resin is shown below.
[0045] (Measurement conditions) Sample pretreatment: 30 mg of sample (polypropylene resin) was completely dissolved in 20 mL of o-dichlorobenzene at 145°C, and the solution was then filtered through a sintered filter with a pore size of 1.0 μm to obtain the filtrate used as the analytical sample. Measurement device: Gel permeation chromatograph Alliance GPC 2000 (manufactured by Waters) Analysis device: Data processing software Empower Professional (manufactured by Waters) Columns: Two TSKgel GMH6-HT columns, two TSKgel GMH6-HTL columns (each column size 7.5 mm inner diameter x 300 mm length, manufactured by Tosoh Corporation) Mobile phase: o-dichlorobenzene (containing 0.025% BHT) Column temperature: 140°C Detector: Differential refractometer Flow rate: 1.0 mL / min.
[0046] The molecular structures of the polypropylene resin (a) and the polypropylene resin (b) are not particularly limited, and may be linear or branched. Among them, it is preferable that the polypropylene resin (b) has a linear structure, and it is more preferable that both the polypropylene resin (a) and the polypropylene resin (b) have a linear structure, since this allows for the production of a molded product with few intergranular gaps and excellent surface properties.
[0047] The polypropylene resin can be obtained by a known method. The polymerization catalyst used for synthesizing the polypropylene resin is not particularly limited, and Ziegler catalysts, metallocene catalysts, etc. can be used.
[0048] <Intumescent Flame Retardant> The resin particles contain an intumescent flame retardant. In this specification, the term "intumescent flame retardant" refers to a substance that contains phosphorus and nitrogen as constituents and that can impart flame retardancy to an object (e.g., a foam molded article) containing the intumescent flame retardant. When a foam molded article containing an intumescent flame retardant is burned, the foam molded article is heated by combustion, and a foamed expansion layer consisting of a foam-like coating is formed on the surface of the foam molded article. This (i) prevents heat from the burning area on the surface of the foam molded article from being transferred to the interior of the foam molded article (insulation), suppressing thermal decomposition of the resin, and (ii) blocks the supply of oxygen to the interior of the foam expansion layer, thereby suppressing oxidation reactions, thereby demonstrating excellent flame retardancy. The intumescent flame retardant can also be said to be a substance that has the effect of forming a foamed expansion layer consisting of such a foam-like coating when a foam molded article containing the intumescent flame retardant is burned.
[0049] The resin particles preferably contain more than 4.0 wt% and 30.0 wt% or less of an intumescent flame retardant, more preferably 6.0 wt% to 25.0 wt%, even more preferably 11.0 wt% to 23.0 wt%, and even more preferably 15.0 wt% to 21.0 wt%, based on 100 wt% of the resin particles. When the resin particles contain (i) more than 4.0 wt% of the intumescent flame retardant, a foamed molded article with excellent flame retardancy can be provided. When the resin particles contain (ii) 30.0 wt% or less of the intumescent flame retardant, a foamed molded article without sink marks and excellent strength (e.g., compressive strength) can be provided. Note that when multiple compounds are used in combination as the intumescent flame retardant, the content of the intumescent flame retardant in the resin particles refers to the total amount of the multiple compounds.
[0050] The intumescent flame retardant according to one embodiment of the present invention (hereinafter, may be referred to as "the intumescent flame retardant") may be (i) a compound containing both a phosphorus atom and a nitrogen atom in the molecule, (ii) a combination of a compound containing a phosphorus atom in the molecule and a compound containing a nitrogen atom in the molecule, or (iii) a combination of two or more of these. Among these, the intumescent flame retardant is preferably a combination of a compound containing a phosphorus atom in the molecule and a compound containing a nitrogen atom in the molecule, because this has the advantages of being less susceptible to thermal denaturation during expansion of the resin particles and molding of the expanded beads, having good dispersibility in the base resin, and easily exhibiting the flame retardant effect of the foamed layer that is formed.
[0051] Examples of compounds containing both phosphorus atoms and nitrogen atoms in the molecule that the resin particles may contain as an intumescent flame retardant include phosphates such as ammonium polyphosphate, melamine polyphosphate, melamine phosphate, and phosphoric acid ester amide; pyrophosphates such as piperazine pyrophosphate and melamine pyrophosphate; etc. These may be used alone or in combination of two or more.
[0052] When the intumescent flame retardant is a combination of a compound containing a phosphorus atom in its molecule and a compound containing a nitrogen atom in its molecule, examples of the phosphorus atom-containing compound include organic phosphorus compounds and red phosphorus. Examples of compounds containing a nitrogen atom in its molecule include hindered amines, melamine, ammonium borate, and ammonium carbonate. Among these, organic phosphorus compounds are preferred as the phosphorus atom-containing compound, because they have the advantage of being able to provide foamed particles that can provide foamed molded articles that are not only flame retardant but also have excellent surface aesthetics and productivity. As examples of compounds containing a nitrogen atom in its molecule, hindered amines are preferred. That is, the resin particles preferably contain an organic phosphorus compound and a hindered amine as the intumescent flame retardant, and more preferably contain only an organic phosphorus compound and a hindered amine. Note that compounds containing both a phosphorus atom and a nitrogen atom are not considered "compounds containing a phosphorus atom" in this specification, and compounds containing a nitrogen atom and a phosphorus atom are not considered "compounds containing a nitrogen atom" in this specification.
[0053] (Organophosphorus Compound) Examples of the organophosphorus compound include phosphonates, organic phosphites, organic phosphinites, metal salts of phosphinic acids, metal salts of diphosphinic acids, phosphinates, and polyol phosphate alcohols.
[0054] Among the above-mentioned organic phosphorus compounds, phosphonates are preferred because they can provide foamed molded articles that are more excellent in ignition and non-ignition properties and self-extinguishing properties.
[0055] (Phosphonate) Phosphonate is M-PO(OH) 2 group and / or M-PO(OM 1 ) 2 group, where M is a monovalent hydrocarbon group (e.g., methyl, benzyl, aryl, alkynyl, allenyl, vinyl, or substituted vinyl group), and M 1 is a hydrocarbyl group (such as an alkyl group or an aryl group), and salts thereof.
[0056] Phosphonates include alkyl and aryl phosphonic acids and their esters; mono-phosphonates; acyclic bisphosphonates; cyclic phosphonates; and the like.
[0057] Among the phosphonates, cyclic phosphonates are preferred, and cyclic bisphosphonates are particularly preferred.
[0058] Examples of cyclic phosphonates include compounds represented by the following structural formula (i):
[0059] In the above structural formula (i), R 1 and R 2 are independently 1-4 is an alkyl group, and R 3 is H or C 1-4 is an alkyl group, and R 4 is C 9-22 Alkyl group, C 9-22 Cycloalkyl group, C 9-22 Aryl group or C 9-22 It is an aralkyl group, and n is 0 or 1.
[0060] The cyclic phosphonates represented by the above structural formula (i) are disclosed in more detail in French Patent Application Publication No. 1,503,429.
[0061] As the cyclic phosphonate, a cyclic bisphosphonate, such as pentaerythrityl diphosphonate, which is a compound represented by the following structural formula (ii), can also be suitably used:
[0062] In the above structural formula (ii), A 1 and A 2 are independently 1-10 Alkyl group, C 2-10 It is an alkenyl group, a benzyl group, a phenylethyl group, a phenyl group, or a naphthyl group.
[0063] Cyclic bisphosphonates are disclosed in more detail in US Pat. No. 4,174,343 and GB 1,515,223.
[0064] Among cyclic bisphosphonates, pentaerythrityl diphosphonate represented by the following structural formula (iii) (e.g., AFLAMMIT (registered trademark) PCO 900 (phosphorus content 24%) manufactured by Thor GmbH) is particularly preferred because it allows the production of foamed molded articles with excellent heat resistance and dimensional stability. Specifically, 3,9-dimethyl-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5,5]undecane-3,9-dioxide is particularly preferred as the pentaerythrityl diphosphonate.
[0065] As other cyclic phosphate esters, the compounds disclosed in French Patent Application Publication No. 1,503,429 may be used.
[0066] As the organic phosphorus compound, an organic phosphorus compound whose surface has been coated (for example, a surface-coated phosphonate) can also be used.
[0067] (Hindered Amine) In this specification, the term "hindered amine" refers to a hindered amine having an OR group (wherein R is a saturated or unsaturated monovalent hydrocarbon group) directly substituted on the N atom (hereinafter, this may be referred to as an N-substituted hindered amine). The hindered amine is not particularly limited as long as it is a hindered amine having an OR group directly substituted on the N atom, and known hindered amines can be used. As the hindered amine, one type of hindered amine may be used alone, or two or more types of hindered amines may be used in combination.
[0068] In this specification, hindered amines that do not have an OR group substituted directly on the N atom are not considered to be hindered amines.
[0069] As the hindered amine, an N-substituted hindered amine containing a triazine component (hereinafter, sometimes referred to as a "triazine skeleton-containing hindered amine") is preferred because it can exhibit flame retardant effects over a wide temperature range. The triazine skeleton-containing hindered amine is not particularly limited, but examples thereof include (i) a compound having CAS number 191680-81-6 ((i-1) a reaction product of N,N'-bis(3-aminopropyl)ethylenediamine with a product obtained by reacting cyclohexane with a reaction product of peroxidized N-butyl-2,2,6,6-tetramethyl-4-piperidinamine and 2,4,6-trichloro-1,3,5-triazine, and (i-2) 2,4-bis((1-cyclohexyloxy-2,2,6,6-tetramethylpiperidin-4-yl)butyl (i-3) N,N',N'''-tris{2,4-bis[(1-hydrocarbyloxy-2,2,6,6-tetramethylpiperidin-4-yl)alkylamino]-s-triazin-6-yl}-3,3'-ethylenediiminodipropylamine), and / or (ii) bis(1-undecanoxy-2,2,6,6-tetramethylpiperidin-4-yl)carbonate, which may be a reaction product of N,N'-bis(3-aminopropyl)ethylenediamine with N,N'-bis(3-aminopropyl)ethylenediamine, are preferred. Furthermore, isomers of the above-mentioned triazine skeleton-containing hindered amines and crosslinked derivatives of the above-mentioned triazine skeleton-containing hindered amines may also be used. More detailed information about triazine skeleton-containing hindered amines is disclosed in European Patent No. 0889085, page 2, line 32 to page 4, line 6.
[0070] Commercially available products of the triazine skeleton-containing hindered amine can also be suitably used. Examples of commercially available products of the triazine skeleton-containing hindered amine include FLAMSTAB (registered trademark) NOR116 (a compound having CAS number 191680-81-6) manufactured by BASF, HOSTAVIN (registered trademark) NOW XP manufactured by CLARIANT, and Adeka STAB LA-81 (bis(1-undecaneoxy-2,2,6,6-tetramethylpiperidin-4-yl)carbonate) manufactured by Adeka Corporation.
[0071] (Organophosphorus Compound and Hindered Amine Content) When the resin particles contain an organophosphorus compound and a hindered amine as an intumescent flame retardant, the resin particles contain 3.0 wt% to 20.0 wt%, preferably 5.0 wt% to 19.0 wt%, more preferably 7.0 wt% to 18.0 wt%, even more preferably 10.0 wt% to 17.0 wt%, and even more preferably 13.0 wt% to 16.0 wt%, of the organophosphorus compound, based on a total weight of 100 wt% of the resin particles. When the resin particles contain (i) 3.0 wt% or more of the organophosphorus compound, a foamed molded article having excellent flame retardancy can be stably provided. When the resin particles contain (ii) 20.0 wt% or less of the organophosphorus compound, a foamed molded article having no sink marks and excellent strength (e.g., compressive strength) can be provided.
[0072] Furthermore, the present resin particles preferably contain 1.0 wt % to 10.0 wt % of hindered amine, more preferably 2.0 wt % to 8.0 wt %, even more preferably 2.5 wt % to 7.0 wt %, and even more preferably 3.0 wt % to 6.0 wt %, based on the total weight of the resin particles (100 wt %). When the present resin particles contain (i) more than 1.0 wt % of hindered amine, a foamed molded article with excellent non-ignition and self-extinguishing properties can be obtained, and (ii) when the resin particles contain 10.0 wt % or less, adhesion (blocking) of resin particles to each other can be suppressed in the foaming step described below.
[0073] Because of the above advantages, the resin particles preferably contain 3.0 to 20.0% by weight of an organic phosphorus compound and 1.0 to 10.0% by weight of a hindered amine, based on a total weight of 100% by weight of the resin particles.
[0074] <Other Additives> In addition to the base resin and the intumescent flame retardant, the resin particles may optionally contain other additives as long as the effects of the present invention are not impaired. Examples of other additives include other flame retardants (other than intumescent flame retardants), ultraviolet protection agents (e.g., Tinuvin 622 manufactured by BASF), peroxide scavengers, nucleating agents, antistatic agents, antioxidants (e.g., Irgafos 168 and Irganox 1010 manufactured by BASF), light stabilizers, conductive agents, lubricants, fillers, carbon black, powdered activated carbon, etc.
[0075] Examples of other flame retardants include brominated flame retardants such as brominated bisphenol A flame retardants, brominated bisphenol S flame retardants, brominated butadiene-styrene block copolymer flame retardants, and brominated polyphenylene ether flame retardants, and examples of melamine flame retardants include melamine sulfate, melamine polyphosphate, melamine cyanurate, melamine pyrophosphate, melamine hydrogen bromide, etc. These other flame retardants may be used alone or in combination of two or more.
[0076] The content of the other flame retardant in the present resin particles is, for example, preferably greater than 0 wt% to 1.00 wt%, more preferably 0.05 wt% to 0.75 wt%, and even more preferably 0.10 wt% to 0.50 wt%, based on the total amount (100 wt%) of the polypropylene-based resin particles. Since the present resin particles contain an intumescent flame retardant as an essential component, expanded particles can be provided that can provide foamed molded articles with excellent flame retardancy even without the inclusion of these other flame retardants. In other words, the content of the other flame retardant in the present resin particles may be 0 wt%.
[0077] (Melting Point of Resin Particles) The melting point of the resin particles is not particularly limited, but is preferably, for example, 122.0°C to 159.0°C.
[0078] <Physical Properties of Polypropylene-Based Expanded Beads> (Average Cell Diameter) The average cell diameter of the expanded beads is not particularly limited, but is preferably 100 μm to 600 μm, more preferably 150 μm to 450 μm, and even more preferably 200 μm to 400 μm. When the average cell diameter of the expanded beads is (i) 100 μm or more, expanded molded articles with excellent surface beauty can be obtained. Furthermore, when the average cell diameter of the expanded beads is (ii) 600 μm or less, the secondary expansion properties during in-mold expansion molding of the expanded beads are good, and expanded molded articles with excellent surface beauty can be obtained. The average cell diameter of the expanded beads can also be said to be the cell diameter of the expanded beads. In this specification, the method for measuring the average cell diameter of the expanded beads is as described in the Examples.
[0079] (High-Temperature Side Heat of Fusion of Expanded Beads) The high-temperature side heat of fusion of the expanded beads is preferably 5.0 J / g to 25.0 J / g, more preferably 8.0 J / g to 20.0 J / g, and even more preferably 10.0 J / g to 15.0 J / g. When the high-temperature side heat of fusion of the expanded beads is (i) 5.0 J / g or more, the occurrence of sink marks on the surface of the resulting expanded molded article and dimensional shrinkage during in-mold foam molding can be suppressed. When the high-temperature side heat of fusion is 25.0 J / g or less, expanded molded articles with excellent internal fusion properties and smooth surfaces can be obtained. The high-temperature side heat of fusion can also be referred to as the high-temperature side heat of fusion peak. Note that, in this specification, the method for measuring the high-temperature side heat of fusion of expanded beads is as described in the Examples.
[0080] Furthermore, since the present expanded beads have the advantage of being free from shrinkage-induced sink marks and surface irregularities and capable of providing a foamed molded article with excellent surface properties, it is preferred that the present expanded beads have at least two melting peaks in a DSC curve obtained by measurement with a differential scanning calorimeter. That is, it is preferred that the present expanded beads have at least two melting peaks in a DSC curve obtained by measurement with a differential scanning calorimeter and have a high-temperature heat of fusion of 5.0 J / g to 25.0 J / g.
[0081] (Expanded Bead Density) The bulk density of the expanded beads (expanded bead bulk density) is not particularly limited, but is preferably 15 g / L to 400 g / L, more preferably 60 g / L to 300 g / L, even more preferably 70 g / L to 250 g / L, even more preferably 80 g / L to 250 g / L, and particularly preferably 90 g / L to 250 g / L. When the expanded beads have a bulk density of (i) 15 g / L or more, there is an advantage that the internal pressure required for molding the expanded beads is low, and when the bulk density is (ii) 400 g / L or less, there is an advantage that a foamed molded article with excellent lightness can be obtained. In this specification, the method for measuring the bulk density of the expanded beads is as described in the Examples.
[0082] In addition, when air is impregnated (internal pressure is applied) during molding of the present expanded beads, the density of the expanded beads refers to the bulk density of the expanded beads before air is impregnated (before internal pressure is applied).
[0083] [2. Method for producing expanded beads] A method for producing expanded beads according to one embodiment of the present invention preferably includes a dispersing step of dispersing polypropylene-based resin particles, an aqueous dispersion medium, and a blowing agent in a container, and a discharging step of discharging the dispersion obtained in the dispersing step into a region having a lower pressure than the pressure inside the container, wherein the polypropylene-based resin particles are a base resin including a polypropylene-based resin (a) having an MI of 4.00 g / 10.00 min to 15.00 g / 10 min and a melting point of 135°C to 155°C, and a polypropylene-based resin (b) having an MI of 0.05 g / 10 min to 3.00 g / 10 min and a melting point of 135°C to 155°C, and an intumescent flame retardant.
[0084] In this specification, the "method for producing expanded beads according to one embodiment of the present invention" may be referred to as the "present production method."
[0085] For the resin particles used in this production method, the explanation in the above section [1. Expanded polypropylene particles] can be appropriately applied.
[0086] (Granulation Step) The present production method preferably includes a granulation step of preparing resin particles prior to the expansion step.
[0087] The granulation step in this production method is not particularly limited as long as it can produce resin particles, and any known method can be used. An example of the granulation step is a method in which the following steps (S1) to (S3) are carried out in order: (S1) predetermined amounts of polypropylene resin (a), polypropylene resin (b), and an intumescent flame retardant, and, if necessary, other additives, are melt-kneaded using an extruder to prepare a melt-kneaded product; (S2) the melt-kneaded product is extruded through a die provided in the extruder; and (S3) the extruded melt-kneaded product is chopped into desired shapes (e.g., cylindrical, spherical, etc.) to obtain resin particles.
[0088] In the step (S1), a blend may be prepared in advance by blending predetermined amounts of the polypropylene resin (a), the polypropylene resin (b), the intumescent flame retardant, and, if necessary, other additives. The blend may be fed to an extruder and melt-kneaded to prepare a melt-kneaded product.
[0089] In the step (S3), before the molten kneaded material is chopped, the extruded molten kneaded material may be cooled and solidified using a cooling medium such as water.
[0090] (Dispersion Step) The dispersion step can also be said to be a step of preparing a dispersion in which the present resin particles, a foaming agent, and, if necessary, a dispersant and / or a dispersion aid are dispersed in an aqueous dispersion medium.
[0091] The container used in the dispersion step is not particularly limited, but is preferably a container that can withstand the foaming temperature and foaming pressure described below. The container is preferably, for example, a pressure-resistant container, more preferably an autoclave-type pressure-resistant container. The container may be equipped with a stirrer inside.
[0092] The aqueous dispersion medium is not particularly limited as long as it can uniformly disperse the resin particles, the foaming agent, etc.
[0093] Examples of aqueous dispersion media include (a) dispersion media obtained by adding methanol, ethanol, ethylene glycol, glycerin, or the like to water, (b) water such as tap water and industrial water, and (c) solutions containing salts such as sodium chloride or sodium sulfate (aqueous solutions).
[0094] Examples of the blowing agent include (a) (a-1) inorganic blowing agents such as nitrogen, carbon dioxide, air (a mixture of oxygen, nitrogen, and carbon dioxide), and (a-2) water; and (b) organic blowing agents such as (b-1) saturated hydrocarbons having 3 to 5 carbon atoms such as propane, normal butane, isobutane, normal pentane, isopentane, and neopentane, (b-2) ethers such as dimethyl ether, diethyl ether, and methyl ethyl ether, and (b-3) halogenated hydrocarbons such as monochloromethane, chloroethane, and hydrofluoroolefins.
[0095] Among these, the blowing agent is preferably water and / or carbon dioxide gas, because it has a low environmental impact and is economical and safe.
[0096] In the present method for producing expanded beads, it is preferable to use a dispersant (e.g., an inorganic substance such as tricalcium phosphate or kaolin) and a dispersing aid (e.g., an anionic surfactant such as sodium dodecylbenzenesulfonate). This configuration can reduce adhesion of resin particles (sometimes called blocking) and improve the stability of the dispersion in the container. As a result, it has the advantage of enabling stable production of expanded beads.
[0097] The aqueous dispersion medium and the blowing agent may each be used alone or in combination of two or more.
[0098] (Temperature-Pressure Increase Step and Holding Step) The present production method preferably further includes, after the dispersion step and before the release step, (i) a temperature-pressure increase step in which the temperature inside the container is increased to a constant temperature and the pressure inside the container is increased to a constant pressure, and (ii) a holding step in which the temperature and pressure inside the container are held at a constant temperature and a constant pressure. The holding step is preferably carried out after the temperature-pressure increase step. In this specification, the (a) constant temperature in the temperature-pressure increase step and the holding step may be referred to as the foaming temperature, and the (b) constant pressure in the foaming pressure may be referred to as the foaming pressure.
[0099] The foaming temperature cannot be generally defined because it differs depending on the types of base resin and intumescent flame retardant contained in the resin particles, the type of blowing agent, etc. The foaming temperature is preferably (i) from the melting point of (a) the mixture of base resin and intumescent flame retardant, (b) the polypropylene resin composition, or (c) the resin particles −20.0°C to the melting point +20.0°C, more preferably (ii) from the melting point of (a) the mixture of base resin and intumescent flame retardant, (b) the polypropylene resin composition, or (c) the resin particles −10.0°C to the melting point +15.0°C, and even more preferably (iii) from the melting point of (a) the mixture of base resin and intumescent flame retardant, (b) the polypropylene resin composition, or (c) the resin particles −5.0°C to the melting point +13.0°C.
[0100] The expansion pressure is preferably 0.5 MPa (gauge pressure) to 10.0 MPa (gauge pressure), more preferably 0.6 MPa (gauge pressure) to 5.0 MPa (gauge pressure), and even more preferably 0.6 MPa (gauge pressure) to 2.5 MPa (gauge pressure). When the expansion pressure is 0.5 MPa (gauge pressure) or more, expanded beads with a suitable density can be obtained.
[0101] In the holding step, the time (holding time) for which the dispersion in the container is held at temperatures near the foaming temperature and foaming pressure is not particularly limited. The holding time is preferably 10 to 60 minutes, more preferably 12 to 50 minutes, and even more preferably 15 to 40 minutes.
[0102] (Discharging Step) The resin particles can be expanded by the discharging step, resulting in expanded particles. The discharging step can also be described as a step of opening one end of the container and discharging the dispersion liquid in the container into a region (space) with a pressure lower than the expansion pressure (i.e., the pressure inside the container).
[0103] In the releasing step, the "region under a pressure lower than the foaming pressure" refers to a "region under a pressure lower than the foaming pressure" or a "space under a pressure lower than the foaming pressure", and can also be referred to as "an atmosphere under a pressure lower than the foaming pressure". The region under a pressure lower than the foaming pressure is not particularly limited as long as it is lower than the foaming pressure, and may be, for example, a region under atmospheric pressure.
[0104] (Expansion Process) The process from the dispersion process to the release process may be referred to as the expansion process. The process of producing expanded beads from resin beads in this manner is referred to as the "first-stage expansion process," and the obtained expanded beads are referred to as "first-stage expanded beads."
[0105] (Second-stage expansion process) In order to obtain expanded beads with a high expansion ratio, the first-stage expanded beads obtained in the first-stage expansion process may be expanded again. The process of increasing the expansion ratio of the first-stage expanded beads is called the "second-stage expansion process", and the polypropylene-based expanded beads obtained by the second-stage expansion process are called "second-stage expanded beads". The specific method for the second-stage expansion process is not particularly limited, and known methods can be used.
[0106] [3. Polypropylene-Based Foam Molded Article] A polypropylene-based foam molded article according to one embodiment of the present invention is a foam molded article obtained by molding (e.g., in-mold foam molding) the foamed beads. In this specification, the "polypropylene-based foam molded article according to one embodiment of the present invention" may be referred to as the "foam molded article of the present invention." The foam molded article of the present invention can also be said to be a foam molded article obtained by molding polypropylene-based foamed beads obtained by foaming polypropylene-based resin particles containing a base resin including: a polypropylene-based resin (a) having an MI of 4.00 g / 10 min to 15.00 g / 10 min and a melting point of 135°C to 155°C; and a polypropylene-based resin (b) having an MI of 0.05 g / 10 min to 3.00 g / 10 min and a melting point of 135°C to 155°C; and an intumescent flame retardant.
[0107] The foamed molded article has the above-mentioned structure and is therefore excellent in flame retardancy.
[0108] (Flame retardancy of foam molded article) In this specification, the flame retardancy of a foam molded article can be evaluated by UL94V "Vertical Combustion Foam Material Test" (UL94V test). The test method and evaluation criteria of UL94V "Vertical Combustion Foam Material Test" are as described in the examples.
[0109] In the UL94V test, the foam molded article preferably satisfies at least criterion V-2, more preferably criterion V-1, and particularly preferably criterion V-0. A foam molded article that satisfies criterion V-2 can be said to have superior flame retardancy compared to foam molded articles that are NG, a foam molded article that satisfies criterion V-1 can be said to have superior flame retardancy compared to foam molded articles that only satisfy criterion V-2, and a foam molded article that satisfies criterion V-0 can be said to have particularly superior flame retardancy compared to foam molded articles that only satisfy V-2 and / or V-1 or that are NG.
[0110] In foam molded articles that meet the standard V-0 in the UL94V test, no sample continues to burn for 10 seconds or more when exposed to flame, and particles from the dropped test sample do not ignite the absorbent cotton placed below the test sample. In other words, not only is combustion of the foam molded article more suppressed, but even if flammable particles are generated (melted and dripping) during combustion, the fire is extinguished before reaching the absorbent cotton (a combustible material), making it a foam molded article with excellent self-extinguishing properties.
[0111] In the UL94V test, the thickness of the test sample is one of the factors that affect the evaluation results. Even for test samples obtained from the same foam molded article, the thinner the test sample, the greater the ratio of the surface area to the volume of the test sample, i.e., the greater the ratio of the burning area during combustion, and for other reasons, the worse the flame retardancy evaluation tends to be. In other words, a foam molded article that meets the excellent flame retardancy standard even when the test sample is thinner (e.g., 8 mm or 5 mm) can be said to have better flame retardancy. Therefore, from the viewpoint of providing a foamed molded article with superior flame retardancy, in the UL94V test, it is preferable that the foamed molded article satisfies criterion V-0 when the test sample thickness is 13 mm and 8 mm, and satisfies criterion V-2 when the test sample thickness is 5 mm, it is more preferable that the foamed molded article satisfies criterion V-0 when the test sample thickness is 13 mm and 8 mm, and satisfies criterion V-1 when the test sample thickness is 5 mm, and it is particularly preferable that the foamed molded article satisfies criterion V-0 in all cases where the test sample thickness is 13 mm, 8 mm, and 5 mm.
[0112] (Residual Weight Ratio of Foam Molded Article) In this specification, the flame retardancy of a foam molded article can also be evaluated by the remaining weight ratio of the foam molded article after the UL94V test. In this specification, the remaining weight ratio of the foam molded article is a value that can be calculated by measuring the weight (weight after combustion) of a test sample after the UL94V test (after the second combustion) and calculating the remaining weight ratio of the foam molded article based on the following formula: remaining weight ratio of foam molded article (%) = (weight of test sample after combustion (after UL94V test) / weight of test sample before combustion (before UL94V test)) × 100.
[0113] The higher the residual weight ratio of a foam molded product, the more excellent the flame retardancy of the foam molded product. As with the evaluation in the UL94V test, the residual weight ratio of a foam molded product is affected by the thickness of the test sample. Even when test samples are obtained from the same foam molded product, the thinner the test sample, the lower the residual weight ratio tends to be.
[0114] Therefore, from the viewpoint of providing a foamed molded article having better flame retardancy, the residual weight ratio of the present foam molding is, (i) when the thickness of the test sample is 13 mm, preferably 70% or more, more preferably 80% or more, even more preferably 85% or more, even more preferably 90% or more, and particularly preferably 95% or more; (ii) when the thickness of the test sample is 8 mm, preferably 50% or more, more preferably 60% or more, even more preferably 70% or more, even more preferably 75% or more, and particularly preferably 80% or more; and (iii) when the thickness of the test sample is 5 mm, preferably 40% or more, more preferably 50% or more, even more preferably 60% or more, even more preferably 70% or more, even more preferably 75% or more, and particularly preferably 75% or more.
[0115] Regarding the flame retardancy of foamed molded articles, the density of the foamed molded article is also one of the factors that affect the test results of the UL94V test and the measurement results of the residual weight ratio. The lower the density of the foamed molded article, the smaller the amount of components (base resin and flame retardant) derived from the foamed particles contained in the foamed molded article, making it difficult to enjoy the flame retardancy improvement effects of the base resin composition and the use of the flame retardant. For these reasons, the flame retardancy evaluation tends to be worse. Therefore, it is not possible to simply compare the test results of the UL94V test and the measurement results of the residual weight ratio between foamed molded articles with significantly different densities. Therefore, with regard to the present foamed molded article, "excellent flame retardancy" means that the foamed molded article has better flame retardancy than a foamed molded article with the same density (a foamed molded article that does not meet one embodiment of the present invention).
[0116] (Density of Foam Molded Article) The density of the foam molded article is preferably 15 g / L to 400 g / L, preferably 50 g / L to 300 g / L, and preferably 98 g / L to 200 g / L. A foam molded article having a density of 15 g / L or higher has the advantage of being free of sink marks, smooth, and having excellent surface aesthetics. A foam molded article having a density of 400 g / L or lower can be obtained with a sufficiently light weight. Furthermore, a foam molded article having a density of 98 g / L or higher is particularly preferable because it can provide a foam molded article with superior flame retardancy, which satisfies the V-0 standard in the UL94V test even when the test sample is 5 mm thick. In this specification, the method for measuring the density of a foam molded article is as described in the Examples.
[0117] <Method for producing foamed molded article> The method for producing the foamed molded article is not particularly limited as long as it is possible to produce a foamed molded article by molding the foamed beads (preferably in-mold foam molding), and any known method can be used. As a method for producing the foamed molded article, for example, the method described in the section <Method for producing foamed molded article> of International Publication WO2022 / 149538 can be suitably used.
[0118] An embodiment of the present invention may include the following features.
[0119] [1] Polypropylene-based expanded particles obtained by expanding polypropylene-based resin particles containing a base resin including: a polypropylene-based resin (a) having an MI of 4.00 g / 10 min to 15.00 g / 10 min and a melting point of 135°C to 155°C; and a polypropylene-based resin (b) having an MI of 0.05 g / 10 min to 3.00 g / 10 min and a melting point of 135°C to 155°C; and an intumescent flame retardant.
[0120] [2] The expanded polypropylene beads according to [1], wherein the polypropylene resin (a) and the polypropylene resin (b) are random polypropylene resins.
[0121] [3] The expanded polypropylene beads according to [1] or [2], wherein the polypropylene resin (b) is contained in an amount of 5 to 80% by weight based on 100% by weight of the base resin.
[0122] [4] The expanded polypropylene beads according to any one of [1] to [3], wherein the intumescent flame retardant comprises an organic phosphorus compound and a hindered amine.
[0123] [5] The polypropylene-based resin particles contain 3.0 wt% to 20.0 wt% of an organic phosphorus compound and 1.0 wt% to 10.0 wt% of a hindered amine, based on 100 wt% of the polypropylene-based resin particles. [4] Expanded polypropylene-based beads.
[0124] [6] The expanded polypropylene beads according to [4] or [5], wherein the organic phosphorus compound is at least one selected from the group consisting of phosphonates, organic phosphites, organic phosphinites, metal salts of phosphinic acids, metal salts of diphosphinic acids, phosphinates, and polyol phosphate alcohols.
[0125] [7] The expanded polypropylene beads according to any one of [4] to [6], wherein the organic phosphorus compound is a cyclic phosphonate.
[0126] [8] The weight average molecular weight of the polypropylene resin (b) is 80 × 10 4 The expanded polypropylene beads according to any one of [1] to [7] above.
[0127] [9] The expanded polypropylene beads according to any one of [1] to [8], wherein the polypropylene resin (b) is a linear polypropylene resin.
[0128]
[10] The expanded polypropylene beads according to any one of [1] to [9], having a bulk density of 15.0 g / L to 400.0 g / L.
[0129]
[11] Expanded polypropylene beads according to any one of [1] to
[10] , which have at least two melting peaks in a DSC curve obtained by measurement using a differential scanning calorimeter, and have a high-temperature heat of fusion of 5.0 J / g to 25.0 J / g.
[0130]
[12] The polypropylene-based expanded beads according to any one of [1] to
[11] , wherein the polypropylene-based resin (a) and / or the polypropylene-based resin (b) is an ethylene / propylene random copolymer.
[0131]
[13] The expanded polypropylene beads according to any one of [1] to
[12] , having an average cell diameter of 100 μm to 600 μm.
[0132]
[14] The expanded polypropylene beads according to any one of [1] to
[13] , wherein the polypropylene resin (a) is contained in an amount of 20% by weight to 95% by weight based on 100% by weight of the base resin.
[0133]
[15] A polypropylene-based foamed molded article obtained by in-mold foaming of the polypropylene-based foamed beads according to any one of [1] to
[14] .
[0134]
[16] The polypropylene-based foam molded article according to
[15] , having a bulk density of 15.0 g / L to 400.0 g / L.
[0135]
[17] The polypropylene foam molded article according to
[15] or
[16] , which satisfies standard V-2 in the UL94V test.
[0136]
[18] The polypropylene-based foam molded article according to any one of
[15] to
[17] , which satisfies standard V-1 in the UL94V test.
[0137]
[19] The polypropylene-based foam molded article according to any one of
[15] to
[18] , which satisfies the standard V-0 in the UL94V test.
[0138]
[20] A method for producing expanded polypropylene-based particles, the method comprising: a dispersing step of dispersing polypropylene-based resin particles, an aqueous dispersion medium, and a blowing agent in a container; and a discharging step of discharging the dispersion obtained in the dispersing step into a region having a pressure lower than the pressure inside the container, wherein the polypropylene-based resin particles comprise a base resin containing: a polypropylene-based resin (a) having an MI of 4.00 g / 10.00 min to 15.00 g / 10 min and a melting point of 135°C to 155°C; and a polypropylene-based resin (b) having an MI of 0.05 g / 10 min to 3.00 g / 10 min and a melting point of 135°C to 155°C; and an intumescent flame retardant.
[0139]
[21] The method for producing expanded polypropylene beads according to
[20] , wherein the polypropylene resin (a) and the polypropylene resin (b) are random polypropylene resins.
[0140]
[22] The method for producing expanded polypropylene beads according to
[20] or
[21] , wherein the polypropylene resin (b) is contained in an amount of 5 to 80% by weight based on 100% by weight of the base resin.
[0141]
[23] The method for producing expanded polypropylene beads according to any one of
[20] to
[22] , wherein the intumescent flame retardant contains an organic phosphorus compound and a hindered amine.
[0142]
[24] The method for producing expanded polypropylene beads according to
[23] , wherein the polypropylene resin particles contain 3.0 wt% to 20.0 wt% of an organic phosphorus compound and 1.0 wt% to 10.0 wt% of a hindered amine, based on 100 wt% of the polypropylene resin particles.
[0143]
[25] The method for producing expanded polypropylene-based beads according to
[23] or
[24] , wherein the organic phosphorus compound is at least one selected from the group consisting of phosphonates, organic phosphites, organic phosphinites, metal salts of phosphinic acids, metal salts of diphosphinic acids, phosphinates, and polyol phosphate alcohols.
[0144]
[26] The method for producing expanded polypropylene beads according to any one of
[23] to
[25] , wherein the organic phosphorus compound is a cyclic phosphonate.
[0145]
[27] The weight average molecular weight of the polypropylene resin (b) is 80 × 10 4 The method for producing expanded polypropylene beads according to any one of
[20] to
[26] above.
[0146]
[28] The method for producing expanded polypropylene beads according to any one of
[20] to
[27] , wherein the polypropylene resin (b) is a linear polypropylene resin.
[0147]
[29] The method for producing expanded polypropylene beads according to any one of
[20] to
[28] , wherein the polypropylene resin (a) and / or the polypropylene resin (b) is an ethylene / propylene random copolymer.
[0148]
[30] The method for producing expanded polypropylene beads according to any one of
[20] to
[29] , wherein the polypropylene resin (a) is contained in an amount of 20 to 95% by weight based on 100% by weight of the base resin.
[0149]
[31] The method for producing expanded polypropylene beads according to any one of
[20] to
[30] , wherein the blowing agent is water and / or carbon dioxide gas.
[0150] The present invention will be specifically explained below with reference to examples, but the technical scope of the present invention is not limited to these examples.
[0151] [Materials] The materials used in the examples and comparative examples are shown below.
[0152] <Base Resin> (Polypropylene Resin (a)) Polypropylene (a1): Linear ethylene / propylene random copolymer, MI=7.00 g / 10 min, melting point 144° C., ethylene content 3.2%, Mw=44×10 4(Polypropylene Resin (b)) Polypropylene (b1): Linear ethylene / propylene random copolymer, MI = 0.48 g / 10 min, melting point 142°C, ethylene content 3.5%, Mw = 121 × 10 4 Polypropylene (b2): Linear ethylene / propylene random copolymer, MI = 0.51 g / 10 min, melting point 149°C, ethylene content 2.5%, Mw = 116 × 10 4 <Intumescent flame retardant> (Organophosphorus compound) AFLAMMIT (registered trademark) PCO900 (cyclic phosphonate) manufactured by Thor GmbH (Hindered amine) FLAMESTAB (registered trademark) NOR116 (compound with CAS number 191680-81-6) manufactured by BASF <Other additives> (Nucleating agent) Talcan Powder PK-S manufactured by Hayashi Kasei Co., Ltd. (Antioxidant) Irgafos168 manufactured by BASF Irganox1010 (UV inhibitor) Tinuvin622 manufactured by BASF <Blowing agent> Carbon dioxide: manufactured by Air Water Inc. <Dispersant> Kaolin ASP-170 manufactured by BASF Calcium phosphate tertiary manufactured by Taihei Chemical Co., Ltd. <Dispersing aid> DBS manufactured by Kao Corporation G-15: Since the dispersant and dispersion aid are added to the dispersion liquid or a pressure-resistant sealed container in the dispersion step described below, they do not remain in the resin particles or expanded beads, or only in trace amounts. Furthermore, the carbon dioxide used as a blowing agent is released from the resulting expanded beads because the expanded beads have high gas permeability.
[0153] [Measurement Methods] The evaluation methods used in the examples and comparative examples are described below.
[0154] (MI of Polypropylene-Based Resins (Polypropylene-Based Resin (a) and Polypropylene-Based Resin (b))) The MI of the polypropylene-based resins was measured using an MI measuring device described in JIS K7210:1999 under the conditions of an orifice diameter of 2.0959±0.005 mmφ, an orifice length of 8.000±0.025 mm, a load of 2160 g, and a temperature of 230±0.2°C.
[0155] (Measurement of Average Cell Diameter of Expanded Beads) The average cell diameter of expanded beads was measured by the following methods (1) to (5): (1) Using a razor (high-stainless double-edged blade manufactured by Feather Corporation), the expanded beads were cut so that the cut surface passed through the center of the expanded beads; (2) Using an optical microscope (VHX-5000 manufactured by Keyence Corporation) at a magnification of 50 times, the cut surface of the expanded beads was observed; (3) In the image obtained by observation, a straight line passing through the center or approximately the center of the cut surface of the expanded beads was drawn; (4) (4-1) the number n of cells present on the straight line was measured; (4-2) The length of the line segment cut from the straight line at the intersection of the straight line with the surface of the expanded beads was measured and defined as the expanded bead diameter L; (5) The average cell diameter of expanded beads was calculated by the following formula: average cell diameter (μm) = L / n.
[0156] (High-temperature side heat of fusion of expanded beads) The high-temperature side heat of fusion of expanded beads was as follows (1) to (5): (1) Approximately 5 mg of expanded beads was weighed out; (2) The temperature of the weighed expanded beads was increased from 10°C to 190°C at a heating rate of 10°C / min in measurement by differential scanning calorimetry to melt the expanded beads; (3) In the DSC curve of the expanded beads obtained in the process (2), a baseline was created by connecting a point representing the temperature before the start of melting with a point representing the temperature after the end of melting with a straight line; (4) A line passing through the high-temperature side melting peak or the maximum point between the highest temperature melting peak and the adjacent melting peak was drawn perpendicular to the X-axis; (5) The heat (J / g) calculated from the high-temperature side region surrounded by the baseline, the line passing through the maximum point, and the DSC curve was taken as the high-temperature side heat of fusion of the expanded beads.
[0157] (Bulk Density of Expanded Beads) The bulk density of expanded beads was measured by the following methods (1) to (3): (1) Expanded beads were divided into a volume V (cm 3 (2) The powder surface (top end) of the container was scraped off, and the weight W (g) of the expanded beads in the container was measured. (3) The bulk density of the expanded beads was calculated using the following formula: Bulk density of expanded beads (g / L) = Weight W (g) of expanded beads / {Volume V (cm) of container 3 ) / 1000}.
[0158] (Density of foam molded article) The density of the foam molded article was measured by the following methods (1) to (3): (1) the length (mm), width (mm), and thickness (mm) of the foam molded article were measured, and the volume V (L) of the foam molded article was calculated; (2) the weight W (g) of the foam molded article was measured; and (3) the density of the foam molded article was calculated based on the following formula: Density (g / L) of foam molded article = W / V.
[0159] (Surface properties of foamed molded article) The obtained foamed molded article was visually observed, and the surface properties of the foamed molded article were evaluated according to the following criteria: Good (◯): Almost no gaps between particles (between foam particles) throughout the foamed molded article, no noticeable unevenness on the surface, and no wrinkles or shrinkage; Fairly poor (Δ): Some gaps between particles, surface unevenness, wrinkles and / or shrinkage are observed throughout the foamed molded article; Poor (×): Clearly many gaps between particles, surface unevenness, wrinkles and / or shrinkage are observed throughout the foamed molded article.
[0160] (Flame Retardancy and Residual Weight Ratio of Foam Molded Article) The flame retardancy of the foam molded article was measured and evaluated by the UL94V "vertical burning test" and the residual weight ratio.
[0161] (UL94V "Vertical Flame Test") The test method for the UL94V "Vertical Flame Test" was as follows (1) to (5): (1) A test specimen having specific dimensions (length 125±5 mm x width 13±0.5 mm) and specific thickness (thickness (t) of the test specimen = 13 mm, 8 mm, or 5 mm) was cut out from the foam molded article; (2) The upper part of the cut test specimen was fixed with a fixing clamp to hold the test specimen vertically, and absorbent cotton was placed directly underneath; (2) Below the held test specimen, The flame of a gas burner was applied to the end for 10 seconds and allowed to burn (first combustion); (3) The burning time and red-hot time of the test sample were measured, and if the burning stopped within 30 seconds, the flame of a gas burner was applied to the lower end of the test sample for 10 seconds again and allowed to burn (second combustion); (4) The burning time and red-hot time of the test sample were measured again; (5) The test sample was changed and the steps (1) to (4) were repeated a total of five times, and the flame retardancy was evaluated according to the following evaluation criteria.
[0162] Evaluation criteria [NG (Fail)]: During the first or second combustion, the sample continues to burn for 30 seconds or more, or there is a sample that burns down to the fixing clamp; [V-2]: No sample continues to burn for 30 seconds or more after the first flame application, the total burning time after a total of 10 flame applications for five samples is 250 seconds or less, no sample burns down to the fixing clamp, no sample has a sum of burning time and glow time of 250 seconds or more after the second flame application, and there is a sample in which absorbent cotton placed below the test sample ignites due to particles of the test sample that fell during combustion; [V-1]: No sample continues to burn for 30 seconds or more after both the first and second flame applications, the total burning time after a total of 10 flame applications for five samples is 250 seconds or less, no sample burns down to the fixing clamp, no sample has a sum of burning time and glow time of 250 seconds or more after the second flame application, and During any combustion, no sample caused the absorbent cotton placed below it to ignite due to particles from the dropped test sample; [V-0]: No sample continued to burn for more than 10 seconds after either the first or second exposure to flame, the total burning time after a total of 10 exposures to flame for five samples was 50 seconds or less, no sample burned down to the position of the fixing clamp, no sample had a sum of burning time and glow time of 30 seconds or more after the second exposure to flame, and no sample caused the absorbent cotton placed below it to ignite due to particles from the dropped test sample during any combustion.
[0163] (Residual Weight Ratio) After the UL94V test (after the second combustion), the weight of the test sample (weight after combustion) was measured, and the residual weight ratio of the foamed molded article was calculated based on the following formula: Residual weight ratio of foamed molded article (%) = (weight of test sample after combustion (after UL94V test) / weight of test sample before combustion (before UL94V test)) × 100.
[0164] [Example 1] (Preparation of polypropylene-based resin particles) In 100% by weight of the blend, the base resins were 29.6% by weight of polypropylene-based resin (a1) and 50.0% by weight of polypropylene-based resin (b1); as intumescent flame retardants, 15.0% by weight of an organic phosphorus compound and 5.0% by weight of a hindered amine; and as other additives, 0.1% by weight of talcan powder PK-S as a nucleating agent, 0.133% by weight of Irgafos168 as an antioxidant, 0.067% by weight of Irganox1010, and 0.1% by weight of Tinuvin622 as an ultraviolet inhibitor (total of other additives was 0.4% by weight). The components were dry-blended.
[0165] The resulting blend was placed in a twin-screw extruder (Shibaura Machinery, TEM26SX) and melt-kneaded at a resin temperature of 200°C. The melt-kneaded polypropylene resin composition was extruded into strands through a die with circular holes attached to the tip of the extruder. The extruded polypropylene resin composition was cooled with water and then cut with a cutter to obtain resin particles (granulation step).
[0166] (Preparation of Polypropylene-Based Expanded Beads) 100 parts by weight of the obtained resin particles, 442 parts by weight of pure water, 1.1 parts by weight of tribasic calcium phosphate as a dispersant, 0.22 parts by weight of kaolin ASP-170, and 0.027 parts by weight of DBS as a dispersing aid were placed in a pressure-resistant sealed container. Thereafter, while stirring the raw materials in the pressure-resistant sealed container, 2.1 parts by weight of carbon dioxide as a foaming agent was introduced into the pressure-resistant sealed container to prepare a dispersion (dispersion step). Next, the temperature inside the pressure-resistant sealed container was heated to a foaming temperature of 150.2°C. Thereafter, carbon dioxide was additionally injected into the pressure-resistant sealed container, and the pressure inside the pressure-resistant sealed container was increased to a foaming pressure of 1.1 MPa (gauge pressure) (heating-pressure increase step). Next, the pressure-resistant sealed container was maintained at the foaming temperature and foaming pressure for 20 minutes (maintenance step), and then the valve at the bottom of the sealed container was opened to release the dispersion through a 3.6 mm orifice into a foaming tube under atmospheric pressure to obtain expanded beads (release step). During this release, carbon dioxide was additionally injected into the pressure-resistant sealed container to maintain the pressure inside the pressure-resistant sealed container at 1.1 MPa (gauge pressure) to prevent the pressure inside the pressure-resistant sealed container from dropping below the foaming pressure. The resulting expanded beads were dried at 60°C for 6 hours, and then the average cell diameter, high-temperature heat of fusion, and bulk density (expanded particle bulk density) were measured. The results are shown in Table 1. The resulting expanded beads contained 15.0 wt% of an organophosphorus compound and 5.0 wt% of a hindered amine, based on 100 wt% of the total weight of the expanded beads.
[0167] (Preparation of Polypropylene-Based Foam Molded Articles) The resulting foamed beads were placed in a pressure-resistant sealed container, and air was introduced into the pressure-resistant sealed container to impregnate the foamed beads in the container with pressurized air, applying an internal pressure (absolute pressure) of 0.25 MPa (absolute pressure) to the foamed beads. The air-impregnated foamed beads were heated and molded with steam at 0.32 MPa (gauge pressure) using a molding machine (a polypropylene in-mold foam molding machine manufactured by Daisen Co., Ltd.) to obtain a foamed molded article. The resulting foamed molded article was left at room temperature for 1 hour, then cured and dried in a thermostatic chamber at 75°C for 12 hours, and then left at room temperature for another 4 hours. The density, surface properties, flame retardancy, and residual weight ratio of the resulting foamed molded article were then measured and evaluated using the methods described above. The results are shown in Table 1.
[0168] Examples 2 to 12, Comparative Examples 1 to 8 Resin particles, expanded particles, and foamed molded articles were obtained, and their physical properties were measured and evaluated in the same manner as in Example 1, except that the blending amounts of each component and / or the foaming conditions were changed as shown in Tables 1 to 4. The results are shown in Tables 1 to 4.
[0169] In Examples 9 and 10, the resulting expanded beads were subjected to second-stage expansion according to the following procedure, and the resulting second-stage expanded beads were molded to obtain foamed molded articles.
[0170] (Preparation of Polypropylene-Based Expanded Beads (Second-Stage Expanded Beads)) The resulting expanded beads (first-stage expanded beads) were dried at 60°C for 6 hours and then placed in a pressure-resistant sealed container. Air was introduced into the pressure-resistant sealed container, and the first-stage expanded beads in the pressure-resistant sealed container were impregnated with pressurized air, imparting an internal pressure (absolute pressure) of 0.30 MPa (absolute pressure) to the first-stage expanded beads. Approximately 20 L of the air-impregnated first-stage expanded beads (to which internal pressure was imparted) were placed in an expansion machine. Next, the first-stage expanded beads in the expansion machine were heated with steam at 0.10 MPa (gauge pressure) for 30 seconds, thereby further expanding the first-stage expanded beads (second-stage expansion), and thereby obtaining expanded beads (second-stage expanded beads). The density of the resulting second-stage expanded beads is shown in Table 3.
[0171] In all of the Examples (Examples 1 to 12) and Comparative Examples (Comparative Examples 1 to 9), the resulting expanded beads had two melting peaks in the DSC curves obtained by differential scanning calorimetry (DSC).
[0172] [Summary] Tables 1 to 4 show that foamed molded articles obtained by in-mold foam molding of the present foamed beads have excellent flame retardancy by comparing foamed molded articles of comparable density in each Example and Comparative Example. Specifically, the following (1) to (4) are true: (1) Comparing the foamed molded articles of Examples 1 and 2 with the foamed molded article of Comparative Example 1, the foamed molded article of Comparative Example 1 was rated NG when the test sample thickness (t) was 5 mm, whereas the foamed molded article of Example 1 obtained by in-mold foam molding of the present foamed beads satisfied the V-0 standard even when t was 5 mm. Furthermore, the foamed molded article of Example 2, despite the addition of a relatively small amount of organophosphorus compound (13 wt%), satisfied the V-2 standard even when t was 5 mm.Furthermore, it is clear that both the foamed molded articles of Example 1 and Example 2 have high residual weight ratios and excellent flame retardancy; (2) A comparison between the foamed molded article of Example 3 and the foamed molded article of Comparative Example 2 shows that the foamed molded article of Comparative Example 2 is rated as NG when the thickness (t) of the test sample is 5 mm, whereas the foamed molded article of Example 3 obtained by in-mold foam molding of the present foamed beads, despite its relatively light density of 167 g / L, satisfies the standard V-0 even when t is 5 mm, and also has a high residual weight ratio, demonstrating excellent flame retardancy; (3) A comparison between the foamed molded articles of Examples 4 and 5 and the foamed molded article of Comparative Example 3 shows that the foamed molded article of Comparative Example 3 is rated as NG when t is 5 mm, whereas the foamed molded articles of Examples 4 and 5 obtained by in-mold foam molding of the present foamed beads, even when t is 5 mm, satisfy the standard V-2 or higher, also have a high residual weight ratio, and demonstrate excellent flame retardancy; (4) A comparison of the foamed molded articles of Examples 6 and 7 with the foamed molded articles of Comparative Examples 4 and 5 shows that the foamed molded articles of Comparative Examples 4 and 5 were rated V-2 when t was 13 mm and 8 mm, and rated NG when t was 5 mm, whereas the foamed molded articles of Examples 6 and 7 obtained by in-mold foam molding of the present foamed beads met the standard V-0 or higher when t was 13 mm and 8 mm, and also had a high residual weight ratio, indicating excellent flame retardancy; (5) A comparison of the foamed molded articles of Examples 8 to 10 with the foamed molded articles of Comparative Examples 6 and 7 shows that the foamed molded articles of Comparative Examples 6 and 7 were rated NG even when t was 13 mm due to their low density, whereas the foamed molded articles of Examples 8 to 10, despite their relatively low density of 80 g / L or less, were able to meet the standard V-2 when t was 13 mm. This shows that the foamed molded article obtained by in-mold foaming of the present foamed beads can exhibit flame retardancy even when the density is relatively low, which is usually difficult to impart flame retardancy to.
[0173] (6) A comparison of the foamed molded articles of Examples 11 and 12 with the foamed molded articles of Comparative Examples 8 and 9 shows that the foamed molded articles of Comparative Examples 8 and 9 were rated V-2 when t was 13 mm, whereas the foamed molded articles of Examples 11 and 12 met the standard V-0 when t was 13 mm. This shows that foamed molded articles obtained by in-mold foam molding of the present foamed beads can exhibit excellent flame retardancy even when a relatively small amount of flame retardant is used.
[0174] By in-mold foam molding of the polypropylene-based expanded beads according to one embodiment of the present invention, a polypropylene-based expanded molded article having excellent flame retardancy can be provided. The polypropylene-based expanded molded article having excellent flame retardancy can be used for various purposes such as cushioning packaging materials, logistics materials, heat insulating materials, civil engineering and construction materials, and automotive parts, and can be particularly suitably used in various fields that require compliance with strict flame retardancy standards, such as transportation, buildings, structures, furniture, electrical equipment, and electronic equipment.
Claims
1. A polypropylene-based resin (a) having an MI of 4.00 g / 10 min to 15.00 g / 10 min and a melting point of 135° C. to 155° C.; A base resin including a polypropylene-based resin (b) having an MI of 0.05 g / 10 min to 3.00 g / 10 min and a melting point of 135° C. to 155° C.; and an intumescent flame retardant.
2. 2. The polypropylene-based expanded beads according to claim 1, wherein the polypropylene-based resin (a) and the polypropylene-based resin (b) are each a random copolymer.
3. 2. The polypropylene-based expanded beads according to claim 1, wherein the polypropylene-based resin (b) is contained in an amount of 5 to 80% by weight based on 100% by weight of the base resin.
4. The polypropylene-based expanded particles according to claim 1 , wherein the intumescent flame retardant comprises an organic phosphorus compound and a hindered amine.
5. The polypropylene-based resin particles include, based on 100% by weight of the polypropylene-based resin particles, 3.0% by weight to 20.0% by weight of an organic phosphorus compound; 5. The polypropylene-based expanded beads according to claim 4, further comprising 1.0% by weight to 10.0% by weight of a hindered amine.
6. The polypropylene-based expanded beads according to claim 4, wherein the organic phosphorus compound is a cyclic phosphonate.
7. The weight average molecular weight of the polypropylene resin (b) is 80×10 4 The polypropylene-based expanded particles according to claim 1 .
8. The polypropylene-based expanded beads according to claim 1 , wherein the polypropylene-based resin (b) is a linear polypropylene-based resin.
9. 2. The polypropylene-based expanded beads according to claim 1, having a bulk density of 15 g / L to 400 g / L.
10. 2. The expanded polypropylene beads according to claim 1, which has at least two melting peaks in a DSC curve obtained by measurement using a differential scanning calorimeter, and has a high-temperature side heat of fusion of 5.0 J / g to 25.0 J / g.
11. 2. The polypropylene-based expanded beads according to claim 1, wherein the polypropylene-based resin (a) and / or the polypropylene-based resin (b) is an ethylene / propylene random copolymer.
12. 2. The polypropylene-based expanded beads according to claim 1, having an average cell diameter of 100 μm to 600 μm.
13. A polypropylene-based foamed molded article obtained by in-mold foaming of the polypropylene-based foamed beads according to any one of claims 1 to 12.
14. The polypropylene-based foamed molded article according to claim 13, having a bulk density of 15 g / L to 400 g / L.
15. A dispersing step of dispersing polypropylene-based resin particles, an aqueous dispersion medium, and a blowing agent in a container; A discharging step of discharging the dispersion obtained in the dispersing step into a region with a lower pressure than the pressure inside the container, The polypropylene resin particles are A polypropylene-based resin (a) having an MI of 4.00 g / 10.00 min to 15.00 g / 10 min and a melting point of 135° C. to 155° C.; A base resin including a polypropylene-based resin (b) having an MI of 0.05 g / 10 min to 3.00 g / 10 min and a melting point of 135° C. to 155° C.; and an intumescent flame retardant.