Method for producing chloroprene-based polymer composition

JPWO2023188801A5Active Publication Date: 2024-12-03DENKA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024511336
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-12-03
Estimated Expiration
2043-02-02

AI Technical Summary

Technical Problem

Chloroprene polymer compositions used in dip-molded products often suffer from low recovery rates from polymerization containers and inadequate mechanical properties, such as high modulus at 100% elongation and insufficient tensile strength at break, which affect their performance in applications like medical gloves and rubber boots.

Method used

A method involving the polymerization of chloroprene polymer B in the presence of diene polymer A, where the diene polymer A and chloroprene polymer B have distinct weight average molecular weights, to produce a chloroprene-based polymer composition with improved recovery rates and mechanical properties, specifically a low modulus at 100% elongation and high tensile strength at break.

Benefits of technology

The method results in chloroprene-based polymer compositions that exhibit a high recovery rate from the polymerization container, low modulus at 100% elongation, and excellent tensile strength at break, enhancing the performance and efficiency of dip-molded products.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Provided is a method for producing a chloroprene-based polymer composition that supports a high recovery ratio from the polymerization vessel and that makes it possible to obtain dip-molded articles having a low 100% elongation modulus and an excellent tensile strength at break. The present invention provides a method for producing a chloroprene-based polymer composition, wherein the chloroprene-based polymer composition comprises a diene-based polymer A and a chloroprene-based polymer B and the diene-based polymer A and the chloroprene-based polymer B have different weight-average molecular weights. The method for producing this chloroprene-based polymer composition comprises a polymerization step for polymerizing the chloroprene-based polymer B in the presence of the diene-based polymer A.
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing chloroprene polymer composition

[0001] The present invention relates to a method for producing a chloroprene polymer composition.

[0002] Chloroprene polymers are known as materials for dip-molded products such as medical surgical gloves, medical examination gloves, industrial gloves, balloons, catheters, and rubber boots.

[0003] Various techniques have been proposed for improving the flexibility of chloroprene polymers, including chloroprene polymer latexes for dip-molded products and dip-molded products of chloroprene polymers. Patent Document 1 describes a polychloroprene latex with a pH of 7 to 14 for use in dip-molded products, which contains 100 parts by mass of modified polychloroprene obtained by copolymerizing chloroprene and methacrylic acid, 90 to 150 parts by mass of water, 1 to 5 parts by mass of an emulsifier, and 0.5 to 2.5 parts by mass of potassium ions. Patent Document 2 describes a mercaptan-modified polychloroprene latex for use in dip-molded products, which is obtained by copolymerizing chloroprene and 2,3-dichloro-1,3-butadiene, and in which the peak areas (A) at 126.2 to 127.6 ppm, (B) at 122.0 to 126.2 ppm, and (C) at 129.9 to 130.3 ppm in the C-solid-state NMR spectrum of the polychloroprene are within the ranges represented by the following general formula (I): Patent Document 3 describes a chloroprene polymer latex for use in dip-molded products, which contains high-molecular-weight and low-molecular-weight components, thereby achieving both excellent flexibility and mechanical properties in the vulcanized rubber produced by dip molding. Patent Document 4 describes a chloroprene polymer latex that exhibits excellent flexibility and mechanical properties even under mild vulcanization conditions, which is obtained by copolymerizing a chloroprene monomer with an isoprene monomer, which is a raw material for isoprene rubber. Patent Document 5 describes a dip-molded product of an isoprene / chloroprene polymer that exhibits excellent flexibility without containing a diphenylguanidine vulcanization accelerator by mixing an isoprene polymer latex with a chloroprene polymer latex. Patent Document 6 describes a dip-molded product that exhibits excellent mechanical properties by mixing a nitrile-butadiene polymer (NBR) latex or an isoprene polymer latex with a chloroprene polymer latex.

[0004]

[0005] Japanese Patent Application Laid-Open No. 2014-114342 International Publication No. 2019 / 009038 Japanese Patent Application Laid-Open No. 2019-143002 International Publication No. 2021-132460 Special Publication No. 2017-508840 Japanese Patent Application Laid-Open No. 2020-189963

[0006] Chloroprene polymer compositions containing chloroprene polymers have been widely used in applications such as gloves, balloons, boots, catheters, etc. Furthermore, particularly in applications such as medical rubber gloves, there is a growing demand for chloroprene polymer compositions that can give dip-molded products having excellent flexibility and tensile strength at break, similar to dip-molded products obtained using natural rubber or polyisoprene. Furthermore, for example, when the production conditions for a chloroprene polymer are adjusted to obtain a dip-molded product having a low modulus at 100% elongation, the chloroprene polymer composition obtained after polymerization can be sticky and adhere to the polymerization vessel, resulting in a reduced recovery rate.

[0007] The present invention has been made in view of the above circumstances, and provides a method for producing a chloroprene polymer composition which allows for a high recovery rate from a polymerization vessel and for obtaining a dip-molded product having a low modulus at 100% elongation and excellent tensile strength at break.

[0008] The present invention provides a method for producing a chloroprene polymer composition, the chloroprene polymer composition comprising a diene polymer A and a chloroprene polymer B, wherein the diene polymer A and the chloroprene polymer B have different weight-average molecular weights, and the method for producing the chloroprene polymer composition includes a polymerization step of polymerizing the chloroprene polymer B in the presence of the diene polymer A.

[0009] As a result of extensive investigations, the present inventors have found that, when a chloroprene polymer composition containing a diene polymer A and a chloroprene polymer B having different weight-average molecular weights is produced by a production method including a polymerization step of polymerizing the chloroprene polymer B in the presence of the diene polymer A, the chloroprene polymer composition can be recovered at a high rate from a polymerization vessel and can give a dip-molded product having a low modulus at 100% elongation and excellent tensile strength at break, thereby completing the present invention.

[0010] Various embodiments of the present invention are exemplified below. The embodiments shown below can be combined with each other. Preferably, this is the above-described method for producing a chloroprene polymer composition, wherein the difference between the weight-average molecular weight of the diene polymer A and the weight-average molecular weight of the chloroprene polymer B is 100,000 or more. Preferably, this is the above-described method for producing a chloroprene polymer composition, wherein the weight-average molecular weight of the diene polymer A is 5,000 to 80,000. Preferably, this is the above-described method for producing a chloroprene polymer composition, wherein, in the polymerization step of polymerizing the chloroprene polymer B, the amount of the diene polymer A charged is 5.0 to 60.0 parts by mass per 100 parts by mass of the chloroprene monomer or raw material monomer charged. Preferably, in the method for producing a chloroprene polymer composition described above, the diene polymer A is at least one selected from natural rubber, an isoprene polymer, a butadiene polymer, a styrene-butadiene polymer, a chloroprene polymer, and an acrylonitrile-butadiene polymer.

[0011] The chloroprene polymer of the present invention can provide a chloroprene polymer composition that can be used to obtain a dip-molded product having a high recovery rate from a polymerization vessel, a low modulus at 100% elongation, and excellent tensile strength at break.

[0012] The present invention will be described in detail below by illustrating embodiments of the present invention. The present invention is not limited by these descriptions. The features of the embodiments of the present invention described below can be combined with each other. Furthermore, each feature can be an invention independently.

[0013] 1. Method for Producing Chloroprene Polymer Composition The method for producing a chloroprene polymer composition according to the present invention includes a polymerization step of polymerizing a chloroprene polymer B in the presence of a diene polymer A. The chloroprene polymer composition according to the present invention contains the diene polymer A and the chloroprene polymer B, and the diene polymer A and the chloroprene polymer B have different weight-average molecular weights. First, the diene polymer A and the chloroprene polymer B according to the present invention will be described below.

[0014] 1.1 Diene Polymer A In the present invention, the diene polymer A means a polymer containing diene monomer units derived from a diene monomer. The diene polymer A may contain monomer units derived from a monomer other than the diene monomer, as long as the object of the present invention is not impaired.

[0015] The diene polymer A according to one embodiment of the present invention may contain 50 to 100 mass%, and preferably 70 to 100 mass%, of monomer units derived from a diene monomer, based on 100 mass% of the diene polymer A. The content of the monomer units derived from the diene monomer may be, for example, 50, 55, 60, 65, 70, 75, 80, 85, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, or 100 mass%, or may be within a range between any two of the values ​​exemplified here.

[0016] The diene monomer may be a conjugated diene monomer having 4 to 6 carbon atoms, and specific examples thereof include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, chloroprene, 2,3-dichloro-1,3-butadiene, and 1-chloro-1,3-butadiene. The diene polymer A preferably contains a chloroprene monomer unit.

[0017] The diene polymer A according to one embodiment of the present invention preferably contains at least one selected from natural rubber, an isoprene polymer, a butadiene polymer, a styrene-butadiene polymer, a chloroprene polymer, and an acrylonitrile-butadiene polymer.

[0018] The diene polymer A according to one embodiment of the present invention preferably contains a monomer unit derived from chloroprene, and further preferably contains a monomer unit derived from 2,3-dichloro-1,3-butadiene. The diene polymer A according to one embodiment of the present invention may be one that does not contain sulfur, and the diene polymer A according to one embodiment of the present invention may be one that does not have an -S-S- structure due to sulfur in the main chain.

[0019] The diene polymer A according to one embodiment of the present invention may contain 50 to 100 mass%, and preferably 70 to 100 mass%, of monomer units derived from chloroprene, based on 100 mass% of the diene polymer A. The content of the monomer units derived from chloroprene is, for example, 50, 55, 60, 65, 70, 75, 80, 85, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, or 100 mass%, and may be within a range between any two of the values ​​exemplified here.

[0020] The diene polymer A according to one embodiment of the present invention may contain 0 to 30% by mass of monomer units derived from 2,3-dichloro-1,3-butadiene, relative to 100% by mass of the diene polymer A. The content of the monomer units derived from 2,3-dichloro-1,3-butadiene is, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30% by mass, and may be within a range between any two of the numerical values ​​exemplified here.

[0021] The diene polymer A according to the present invention has a weight-average molecular weight different from that of the chloroprene polymer B. The difference between the weight-average molecular weight of the diene polymer A according to one embodiment of the present invention and the weight-average molecular weight of the chloroprene polymer B described below is preferably 100,000 or more, more preferably 400,000 or more. The difference between the weight-average molecular weight of the diene polymer A and the weight-average molecular weight of the chloroprene polymer B described below is, for example, 100,000, 200,000, 300,000, 400,000, 500,000, 600,000, 700,000, 800,000, 900,000, 1,000,000, 1,200,000, 1,300,000, 1,400,000, or 1,500,000, and may be within a range between any two of the numerical values ​​exemplified here.

[0022] For example, the weight average molecular weight of the diene polymer A may be smaller than the molecular weight of the chloroprene polymer B. The weight average molecular weight of the diene polymer A may be 5,000 to 80,000. The weight average molecular weight of the diene polymer A may be, for example, 5,000, 6,000, 7,000, 8,000, 9,000, 10,000, 11,000, 12,000, 13,000, 14,000, 15,000, 16,000, 17,000, 18,000, 19,000, 20,000, 21,000, 22,000, 23,000, 24,000, 25,000, 26,000, 27,000, 28,000, 29,000, 30,000, 35,000, 40,000, 50,000, 60,000, 70,000, 80,000, and may be within a range between any two of the numerical values ​​exemplified here.

[0023] As another example, the weight-average molecular weight of the diene polymer A can be larger than the molecular weight of the chloroprene polymer B. The weight-average molecular weight of the diene polymer A can be 200,000 to 1,500,000. The weight-average molecular weight of the diene polymer A is, for example, 200,000, 300,000, 400,000, 500,000, 600,000, 700,000, 800,000, 900,000, 1,000,000, 1,100,000, 1,200,000, 1,300,000, 1,400,000, or 1,500,000, and may be within a range between any two of the numerical values ​​exemplified here.

[0024] The weight-average molecular weight of the diene polymer A can be determined by analyzing a sample obtained by dissolving a diene polymer A in tetrahydrofuran after mixing a polymerization solution containing the diene polymer A, for example, a latex, with a large amount of methanol, precipitating, filtering, and drying the resulting diene polymer A, using gel permeation chromatography (GPC). The GPC measurement conditions can be as described in the Examples. The weight-average molecular weight of the diene polymer A can be controlled by adjusting the polymerization recipe, the type and amount of chain transfer agent, polymerization temperature, polymerization time, polymerization conversion rate, etc., during the polymerization of the diene polymer A, and particularly by adjusting the type and amount of the chain transfer agent.

[0025] 1.2 Method for Producing Diene Polymer A There is no particular limitation on the method for producing the diene polymer A according to the present invention. As an example, the diene polymer A according to one embodiment of the present invention may include a diene polymer A polymerization step of polymerizing raw material monomers including a diene monomer to obtain a diene polymer.

[0026] In the polymerization step, the raw material monomers include one or more diene monomers and may also include other monomers copolymerizable with the diene monomers. Examples of the diene monomers include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, chloroprene, 2,3-dichloro-1,3-butadiene, and 1-chloro-1,3-butadiene. Examples of the other monomers copolymerizable with the diene monomers include styrene, methacrylic acid, acrylonitrile, and sulfur.

[0027] The type and amount of each monomer charged are preferably adjusted so that the content of each monomer unit falls within the above-mentioned numerical range in the resulting diene polymer A. For example, when the diene polymer A contains chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units and contains 0 to 30% by mass of 2,3-dichloro-1,3-butadiene monomer units relative to 100% by mass of the total of the chloroprene monomer and 2,3-dichloro-1,3-butadiene, the amount of 2,3-dichloro-1,3-butadiene charged is preferably in the range of 0 to 30 parts by mass relative to 100 parts by mass of the total of the chloroprene monomer and the 2,3-dichloro-1,3-butadiene monomer.

[0028] When producing the diene polymer A, raw material monomers are polymerized by a polymerization method such as emulsion polymerization, solution polymerization, suspension polymerization, bulk polymerization, etc. Among these polymerization methods, emulsion polymerization is preferred because it has various advantages such as ease of control, ease of extracting the polymer from the polymerization-terminated liquid, and a relatively fast polymerization rate.

[0029] In the polymerization step of the diene polymer A, the raw material monomers can be polymerized by charging them into a polymerization vessel together with a polymerization initiator and necessary agents such as a chain transfer agent and a solvent. As an example, when the diene polymer A is polymerized by emulsion polymerization, the raw material monomers can be polymerized by charging them into a reaction vessel together with a chain transfer agent, water, an alkali (e.g., a metal hydroxide such as potassium hydroxide or sodium hydroxide), an emulsifier (dispersant), a reducing agent (e.g., sodium hydrogen sulfite), a polymerization initiator, etc.

[0030] The polymerization initiator is not particularly limited, and any known polymerization initiator generally used for the polymerization of diene polymers can be used, including potassium persulfate, ammonium persulfate, sodium persulfate, hydrogen peroxide, t-butyl hydroperoxide, and other organic peroxides.

[0031] The type of chain transfer agent used in emulsion polymerization is not particularly limited, and may be any known chain transfer agent generally used in the polymerization of diene polymers, such as long-chain alkyl mercaptans such as n-dodecyl mercaptan and tert-dodecyl mercaptan, dialkyl xanthogen disulfides such as diisopropyl xanthogen disulfide and diethyl xanthogen disulfide, iodoform, etc. As the chain transfer agent, long-chain alkyl mercaptans are preferred, and n-dodecyl mercaptan is more preferred.

[0032] By adjusting the type and amount of the chain transfer agent, the weight average molecular weight of the resulting diene polymer A can be adjusted.

[0033] For example, to obtain a diene polymer A having a weight-average molecular weight of 5,000 to 80,000, the amount of the chain transfer agent charged before the start of emulsion polymerization is preferably 0.5 to 10.0 parts by mass per 100 parts by mass of the monomers. In this case, the amount may be, for example, 0.5, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, or 10.0 parts by mass, or may be within a range between any two of the numerical values ​​exemplified here.

[0034] For example, to obtain a diene polymer A having a weight-average molecular weight of 200,000 or more, preferably 500,000 to 1,500,000, the amount of chain transfer agent charged is preferably 0 to less than 0.40 parts by mass per 100 parts by mass of monomer. The amount of chain transfer agent charged is more preferably 0.02 to 0.05 parts by mass, and may be, for example, 0, 0.005, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.20, or 0.30 parts by mass, or less than 0.40 parts by mass, or may be within a range between any two of the values ​​exemplified here. In particular, when attempting to obtain a diene polymer A having a weight-average molecular weight of 200,000 or more, a chain transfer agent may not be used.

[0035] In the case of emulsion polymerization, the pH of the aqueous emulsion is preferably 10.5 to 13.5. The aqueous emulsion refers to a mixed solution of a chain transfer agent and a monomer immediately before the start of emulsion polymerization, but also includes cases where the composition changes due to the subsequent addition or divided addition of each component. When the pH of the aqueous emulsion at the start of emulsion polymerization is 10.5 or higher, the polymerization reaction can be controlled more stably. When the pH is 13.5 or lower, excessive viscosity increase during polymerization is suppressed, and the polymerization reaction can be controlled more stably.

[0036] In the polymerization step, the monomers may include chloroprene and 2,3-dichloro-1,3-butadiene, and may also include other monomers copolymerizable with chloroprene and 2,3-dichloro-1,3-butadiene. The other monomers are as described above as the monomer units that the chloroprene polymer may contain. The type and amount of each monomer charged are preferably adjusted so that the content of each monomer unit in the resulting chloroprene polymer falls within the above-described numerical range.

[0037] The emulsifier preferably contains rosin acid and / or a rosin acid salt. Examples of rosin acid salts include alkali metal salts such as sodium salts and potassium salts. The amount of rosin acid and rosin acid salt added may be 3.0 to 7.0 parts by mass per 100 parts by mass of the raw material monomer used. The amount of rosin acid and rosin acid salt added may be, for example, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, or 7.0 parts by mass, and may be within a range between any two of the values ​​exemplified here.

[0038] The emulsifier may also include emulsifiers and dispersants other than rosin acid and rosin acid salts. Examples of emulsifiers and dispersants other than rosin acid and rosin acid salts include cationic, anionic, and nonionic emulsifiers and dispersants. In one embodiment of the present invention, the emulsifier used in the emulsion polymerization process may include rosin acid and / or rosin acid salts, and an anionic emulsifier or dispersant. As anionic emulsifiers and dispersants, sulfate- or sulfonate-based anionic emulsifiers and dispersants are preferably used in combination to stabilize the chloroprene polymer latex when a pH adjuster is added. Specific examples include alkyl sulfonates having 8 to 20 carbon atoms, alkyl aryl sulfates, condensates of sodium β-naphthalene sulfonate and formaldehyde, and sodium alkyl diphenyl ether disulfonates. The amount of anionic emulsifier or dispersant added may be 0.05 to 5 parts by mass per 100 parts by mass of the raw material monomers. The amount of anionic emulsifier or dispersant added is, for example, 0.05, 0.1, 0.2, 0.3, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, or 5.0 parts by mass relative to 100 parts by mass of the raw material monomer, and may be within a range between any two of the numerical values ​​exemplified here.

[0039] The polymerization temperature is preferably within the range of 5 to 55° C. If it is 5° C. or higher, the emulsion will not freeze, and if it is 55° C. or lower, the diene monomer will not evaporate or boil.

[0040] The polymerization conversion is preferably in the range of 50 to 95%. The polymerization reaction is terminated by adding a polymerization terminator. When the desired polymerization conversion is reached, the polymerization can be controlled by adding a polymerization terminator to terminate the polymerization or by stopping the addition of the polymerization initiator.

[0041] Examples of the polymerization terminator include diethylhydroxylamine, thiodiphenylamine, 4-tert-butylcatechol, and 2,2'-methylenebis-4-methyl-6-tert-butylphenol. In the polymerization step of the diene polymer A according to one embodiment of the present invention, a polymerization terminator may not be used. After completion of the polymerization, unreacted monomers can be removed by a conventional method such as vacuum distillation.

[0042] Furthermore, to a composition (e.g., latex) containing the diene polymer A obtained by the production method of one embodiment of the present invention, a freezing stabilizer, an emulsion stabilizer, a viscosity modifier, an antioxidant, a preservative, and the like can be optionally added after polymerization, within a range that does not impair the effects of the present invention.

[0043] In the polymerization step of the diene polymer A, all of the raw material monomers and chemicals to be used in the polymerization step can be charged into a polymerization vessel before the start of polymerization, and then the polymerization can be started. Alternatively, at least a portion of the raw material monomers and / or chemicals to be used in the polymerization step can be charged into a polymerization vessel before the start of polymerization, and the remainder can be added in portions after the start of polymerization.

[0044] When at least a portion of the raw material monomers and chemicals are charged into a polymerization vessel before the initiation of polymerization, and the remaining raw material monomers and / or chemicals are added after the initiation of polymerization, the remaining raw material monomers and / or chemicals can be added in one or more divided portions, or can be added continuously at a constant flow rate. In one embodiment of the present invention, at least a portion of the raw material monomers can be added in divided portions after the initiation of polymerization. For example, when chloroprene and 2,3-dichloro-1,3-butadiene are used as raw material monomers, a portion of the chloroprene can be added in divided portions after the initiation of polymerization.

[0045] For example, the portionwise addition of the remaining raw material monomers and / or agents can be started when the polymerization rate of the raw material monomers charged before the start of polymerization reaches 50 to 95%. The polymerization rate at which portionwise addition starts can be, for example, 50, 55, 60, 65, 70, 75, 80, 85, 90, or 95%, and may be within a range between any two of the values ​​exemplified here.

[0046] When at least a portion of the raw material monomer is added after the initiation of polymerization, 50 parts by mass or less of 100 parts by mass of all raw material monomers used in the polymerization step can be added after the initiation of polymerization. In this case, the amount of raw material monomer added after the initiation of polymerization can be, for example, 0, 5, 10, 15, 20, 25, 30, 35, 40, 45, or 50 parts by mass, or may be within a range between any two of the values ​​exemplified here. As an example, the raw material monomer, for example, chloroprene, can be added portionwise continuously over a period of 30 to 300 minutes.

[0047] 1.3 Chloroprene Polymer B In the present invention, a chloroprene polymer refers to a polymer containing monomer units derived from 2-chloro-1,3-butadiene (hereinafter also referred to as chloroprene). Furthermore, a chloroprene polymer according to one embodiment of the present invention may be a copolymer of chloroprene and another monomer copolymerizable with chloroprene. Examples of such other monomers include 1-chloro-1,3-butadiene, 2,3-dichloro-1,3-butadiene, isoprene, styrene, methacrylic acid, acrylonitrile, and sulfur. Two or more of these may be used in combination as the other monomer. The chloroprene polymer B according to one embodiment of the present invention preferably contains monomer units derived from 2,3-dichloro-1,3-butadiene. The chloroprene polymer B according to one embodiment of the present invention may be sulfur-free, or the chloroprene polymer B according to one embodiment of the present invention may be free of an —S—S— structure resulting from sulfur in the main chain.

[0048] The chloroprene polymer B according to one embodiment of the present invention may contain 50 to 100 mass% of chloroprene-derived monomer units, and preferably 70 to 100 mass%, of chloroprene-derived monomer units, relative to 100 mass% of the chloroprene polymer B. The content of the chloroprene-derived monomer units is, for example, 50, 55, 60, 65, 70, 75, 80, 85, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, or 100 mass%, and may be within a range between any two of the values ​​exemplified here.

[0049] Chloroprene polymer B according to one embodiment of the present invention may contain 0 to 30% by mass of monomer units derived from 2,3-dichloro-1,3-butadiene, relative to 100% by mass of chloroprene polymer B. The content of the monomer units derived from 2,3-dichloro-1,3-butadiene is, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30% by mass, and may be within a range between any two of the numerical values ​​exemplified here.

[0050] The chloroprene polymer B according to the present invention has a weight-average molecular weight different from that of the diene polymer A. As described above, the difference between the weight-average molecular weight of the diene polymer A according to one embodiment of the present invention and the weight-average molecular weight of the chloroprene polymer B described below is preferably 100,000 or more, more preferably 400,000 or more.

[0051] For example, the weight-average molecular weight of the chloroprene polymer B may be larger than that of the diene polymer A. The weight-average molecular weight of the chloroprene polymer B may be 200,000 to 1,500,000. The weight-average molecular weight of the chloroprene polymer B may be, for example, 200,000, 300,000, 400,000, 500,000, 600,000, 700,000, 800,000, 900,000, 1,000,000, 1,100,000, 1,200,000, 1,300,000, 1,400,000, or 1,500,000, or may be within a range between any two of the numerical values ​​exemplified here.

[0052] As another example, the weight-average molecular weight of chloroprene polymer B can be smaller than the molecular weight of chloroprene polymer B. The weight-average molecular weight of chloroprene polymer B can be 5,000 to 80,000. The weight-average molecular weight of chloroprene polymer B can be, for example, 5,000, 6,000, 7,000, 8,000, 9,000, 10,000, 11,000, 12,000, 13,000, 14,000, 15,000, 16,000, 17,000, 18,000, 19,000, 20,000, or 21,000. , 22,000, 23,000, 24,000, 25,000, 26,000, 27,000, 28,000, 29,000, 30,000, 35,000, 40,000, 50,000, 60,000, 70,000, 80,000, and may be within a range between any two of the numerical values ​​exemplified here.

[0053] The weight-average molecular weight of the chloroprene polymer B can be determined by analyzing a sample obtained by dissolving the chloroprene polymer B in tetrahydrofuran using gel permeation chromatography (GPC), after mixing a polymerization solution containing the chloroprene polymer B, for example, a chloroprene polymer composition (latex), with a large amount of methanol, precipitating, filtering, and drying the resulting solution. The GPC measurement conditions can be as described in the Examples. The weight-average molecular weight of the chloroprene polymer B can be controlled by adjusting the polymerization recipe, the type and amount of chain transfer agent, polymerization temperature, polymerization time, polymerization conversion, and the like during the polymerization of the chloroprene polymer B, and particularly by adjusting the type and amount of the chain transfer agent.

[0054] 1.4 Method for Polymerizing Chloroprene Polymer B The method for producing a chloroprene polymer composition according to the present invention includes a polymerization step of polymerizing a chloroprene polymer B in the presence of a diene polymer A. According to the present invention, by polymerizing a chloroprene polymer B in the presence of a diene polymer A, a chloroprene polymer composition can be obtained that is highly recovered from a polymerization vessel and that can give a dip-molded product having a low modulus at 100% elongation and excellent tensile strength at break.

[0055] The mechanism by which a chloroprene polymer composition can be obtained by polymerizing a chloroprene polymer B in the presence of a diene polymer A, which allows a high recovery rate from a polymerization vessel and enables the production of dip-molded articles having a low modulus at 100% elongation and excellent tensile strength at break is not entirely clear. However, it is presumed that the chloroprene polymer composition obtained by polymerizing a chloroprene polymer B in the presence of a diene polymer A has a highly uniform mixture of the diene polymer A and the chloroprene polymer B in the chloroprene polymer composition, compared to a chloroprene polymer composition obtained by polymerizing the diene polymer A and the chloroprene polymer B separately and mixing them after polymerization, and therefore the resulting chloroprene polymer composition and the resulting dip-molded articles have excellent physical properties.

[0056] The diene polymer A may be added to the polymerization solution in any form. For example, the polymerization solution obtained by polymerizing the diene polymer A may be used as is. As an example, when the diene polymer A is polymerized by emulsion polymerization, a latex containing the diene polymer A may be added to the polymerization solution of the chloroprene polymer B. Alternatively, for example, the diene polymer A may be precipitated from the polymerization solution obtained by polymerizing the diene polymer A, and the precipitated diene polymer A may be added to the polymerization solution of the chloroprene polymer B. As an example, when the diene polymer A is polymerized by emulsion polymerization, the diene polymer A may be precipitated with methanol from the latex containing the diene polymer A and added to the polymerization solution of the chloroprene polymer B, or the diene polymer A obtained by freeze-drying the latex containing the diene polymer A may be added to the polymerization solution of the chloroprene polymer B.

[0057] In the polymerization step of polymerizing the chloroprene polymer B, the amount of the diene polymer A charged can be 5.0 to 60.0 parts by mass, or 40.0 to 95.0 parts by mass, relative to 100 parts by mass of the chloroprene monomer (or raw material monomer). In one embodiment of the present invention, when the weight-average molecular weight of the diene polymer A is smaller than the weight-average molecular weight of the chloroprene polymer B, for example, when the weight-average molecular weight of the diene polymer A is 5,000 to 80,000, the amount of the diene polymer A charged can be 5.0 to 60.0 parts by mass per 100 parts by mass of the chloroprene monomer (or raw material monomer). When the molecular weight of the diene polymer A is larger than the molecular weight of the chloroprene polymer B, for example, when the weight-average molecular weight of the diene polymer A is 200,000 to 1,500,000, the amount of the diene polymer A charged can be 40.0 to 95.0 parts by mass per 100 parts by mass of the chloroprene monomer (or raw material monomer).

[0058] When the weight-average molecular weight of the diene polymer A is smaller than the weight-average molecular weight of the chloroprene polymer B, the amount of the diene polymer A charged per 100 parts by mass of the chloroprene monomer (or raw material monomer) may be, for example, 5.0, 10.0, 15.0, 20.0, 25.0, 30.0, 35.0, 40.0, 50.0, or 60.0 parts by mass, or may be within a range between any two of the numerical values ​​exemplified here. When the molecular weight of the diene polymer A is larger than the molecular weight of the chloroprene polymer B, the amount of the diene polymer A charged relative to 100 parts by mass of the chloroprene monomer (or raw material monomer) is, for example, 40.0, 50.0, 60.0, 65.0, 70.0, 75.0, 80.0, 85.0, 90.0, or 95.0 parts by mass, and may be within a range between any two of the numerical values ​​exemplified here.

[0059] In the polymerization step, the raw material monomers include chloroprene and may also include other monomers copolymerizable with chloroprene, such as 1-chloro-1,3-butadiene, 2,3-dichloro-1,3-butadiene, 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, styrene, methacrylic acid, acrylonitrile, and sulfur.

[0060] The type and amount of each monomer to be charged are preferably adjusted so that the content of each monomer unit in the resulting chloroprene polymer B falls within the above-mentioned range.

[0061] When producing the chloroprene polymer B, raw material monomers are polymerized by a polymerization method such as emulsion polymerization, solution polymerization, suspension polymerization, bulk polymerization, etc. Among these polymerization methods, emulsion polymerization is preferred because it has various advantages such as ease of control, ease of extracting the polymer from the polymerization-terminated liquid, and a relatively high polymerization rate.

[0062] In the polymerization step of the chloroprene polymer B, raw material monomers can be polymerized by charging them into a polymerization vessel together with a polymerization initiator and necessary agents such as a chain transfer agent and a solvent. For example, when the chloroprene polymer B is polymerized by emulsion polymerization, the raw material monomers can be polymerized by charging them into a reaction vessel together with a chain transfer agent, water, an alkali (e.g., a metal hydroxide such as potassium hydroxide or sodium hydroxide), an emulsifier (dispersant), a reducing agent (e.g., sodium hydrogen sulfite), a polymerization initiator, etc.

[0063] The polymerization initiator is not particularly limited, and any known polymerization initiator generally used for polymerization of chloroprene polymers can be used, including potassium persulfate, ammonium persulfate, sodium persulfate, hydrogen peroxide, t-butyl hydroperoxide, and other organic peroxides.

[0064] The type of chain transfer agent used in emulsion polymerization is not particularly limited, and known chain transfer agents generally used in chloroprene polymerization can be used, such as long-chain alkyl mercaptans such as n-dodecyl mercaptan and tert-dodecyl mercaptan, dialkyl xanthogen disulfides such as diisopropyl xanthogen disulfide and diethyl xanthogen disulfide, iodoform, etc. As the chain transfer agent, long-chain alkyl mercaptans are preferred, and n-dodecyl mercaptan is more preferred.

[0065] By adjusting the type and amount of the chain transfer agent, the weight average molecular weight of the resulting chloroprene polymer B can be adjusted.

[0066] For example, to obtain a chloroprene polymer B having a weight-average molecular weight of 200,000 or more, preferably 500,000 to 1,500,000, the amount of chain transfer agent charged is preferably 0 to less than 0.40 parts by mass per 100 parts by mass of monomer. The amount of chain transfer agent charged is more preferably 0 to 0.05 parts by mass, and may be, for example, 0, 0.005, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.20, or 0.30 parts by mass, or less than 0.40 parts by mass, or may be within a range between any two of the values ​​exemplified here. In particular, when attempting to obtain a chloroprene polymer B having a weight-average molecular weight of 200,000 or more, it is not necessary to use a chain transfer agent.

[0067] For example, to obtain a chloroprene polymer B having a weight-average molecular weight of 5,000 to 80,000, the amount of the chain transfer agent charged before the start of emulsion polymerization is preferably 0.5 to 10.0 parts by mass per 100 parts by mass of the monomers. In this case, the amount may be, for example, 0.5, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, or 10.0 parts by mass, or may be within a range between any two of the numerical values ​​exemplified here.

[0068] By adjusting the weight-average molecular weights of the diene polymer A and the chloroprene polymer B to fall within the above-mentioned ranges and controlling the amount of the diene polymer A charged relative to 100 parts by mass of the chloroprene monomer charged to fall within the above-mentioned ranges, a chloroprene polymer composition can be obtained that gives a dip-molded product having a low modulus at 100% elongation and excellent tensile strength at break.

[0069] In the case of emulsion polymerization, the pH of the aqueous emulsion is preferably 10.5 to 13.5. The aqueous emulsion refers to a mixed solution of a chain transfer agent and a monomer immediately before the start of emulsion polymerization, but also includes cases where the composition changes due to the subsequent addition or divided addition of each component. When the pH of the aqueous emulsion at the start of emulsion polymerization is 10.5 or higher, the polymerization reaction can be controlled more stably. When the pH is 13.5 or lower, excessive viscosity increase during polymerization is suppressed, and the polymerization reaction can be controlled more stably.

[0070] In the polymerization step, the monomers may include chloroprene and 2,3-dichloro-1,3-butadiene, and may also include other monomers copolymerizable with chloroprene and 2,3-dichloro-1,3-butadiene. The other monomers are as described above as the monomer units that the chloroprene polymer may contain. The type and amount of each monomer charged are preferably adjusted so that the content of each monomer unit in the resulting chloroprene polymer falls within the above-described numerical range.

[0071] The emulsifier preferably contains rosin acid and / or a rosin acid salt. Examples of rosin acid salts include alkali metal salts such as sodium salts and potassium salts. The amount of rosin acid and rosin acid salt added may be 3.0 to 7.0 parts by mass per 100 parts by mass of the raw material monomer used. The amount of rosin acid and rosin acid salt added may be, for example, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, or 7.0 parts by mass, and may be within a range between any two of the values ​​exemplified here.

[0072] The emulsifier may also include emulsifiers and dispersants other than rosin acid and rosin acid salts. Examples of emulsifiers and dispersants other than rosin acid and rosin acid salts include cationic, anionic, and nonionic emulsifiers and dispersants. In one embodiment of the present invention, the emulsifier used in the emulsion polymerization process may include rosin acid and / or rosin acid salts, and an anionic emulsifier or dispersant. As anionic emulsifiers and dispersants, sulfate- or sulfonate-based anionic emulsifiers and dispersants are preferably used in combination to stabilize the chloroprene polymer latex when a pH adjuster is added. Specific examples include alkyl sulfonates having 8 to 20 carbon atoms, alkyl aryl sulfates, condensates of sodium β-naphthalene sulfonate and formaldehyde, and sodium alkyl diphenyl ether disulfonates. The amount of anionic emulsifier or dispersant added may be 0.05 to 5 parts by mass per 100 parts by mass of the raw material monomers. The amount of anionic emulsifier or dispersant added is, for example, 0.05, 0.1, 0.2, 0.3, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, or 5.0 parts by mass relative to 100 parts by mass of the raw material monomer, and may be within a range between any two of the numerical values ​​exemplified here.

[0073] The polymerization temperature is preferably within the range of 5 to 55° C. A temperature of 5° C. or higher is preferred because the emulsion does not freeze, and a temperature of 55° C. or lower is preferred because the chloroprene monomer does not evaporate or boil.

[0074] The polymerization conversion rate is preferably in the range of 50 to 95%. The polymerization reaction is terminated by adding a polymerization terminator. When the desired polymerization conversion rate is reached, the polymerization can be terminated by adding a polymerization terminator that terminates the polymerization reaction.

[0075] Examples of the polymerization terminator include diethylhydroxylamine, thiodiphenylamine, 4-tert-butylcatechol, 2,2'-methylenebis-4-methyl-6-tert-butylphenol, etc. After the polymerization is completed, unreacted monomers can be removed by a conventional method such as vacuum distillation.

[0076] Furthermore, to the chloroprene polymer composition (e.g., latex) containing the diene polymer A and the chloroprene polymer B obtained by the production method of one embodiment of the present invention, after polymerization, any additives such as a freeze stabilizer, an emulsion stabilizer, a viscosity modifier, an antioxidant, and a preservative may be added, as long as the effects of the present invention are not impaired.

[0077] In the polymerization step for the chloroprene polymer B, all of the raw material monomers and chemicals to be used in the polymerization step may be charged into a polymerization vessel before the start of polymerization, and then the polymerization may be initiated. Alternatively, at least a portion of the raw material monomers and / or chemicals to be used in the polymerization step may be charged into a polymerization vessel before the start of polymerization, and the remainder may be added in portions after the start of polymerization.

[0078] When at least a portion of the raw material monomers and chemicals are charged into a polymerization vessel before the initiation of polymerization, and the remaining raw material monomers and / or chemicals are added after the initiation of polymerization, the remaining raw material monomers and / or chemicals can be added in one or more divided portions, or can be added continuously at a constant flow rate. In one embodiment of the present invention, at least a portion of the raw material monomers and / or chemicals can be added in divided portions after the initiation of polymerization. For example, a portion of the polymerization initiator can be added in divided portions after the initiation of polymerization.

[0079] 1.5 Chloroprene Polymer Composition A chloroprene polymer composition according to one embodiment of the present invention comprises a diene polymer A and a chloroprene polymer B, and the diene polymer A and the chloroprene polymer B have different weight-average molecular weights.

[0080] In the chloroprene polymer composition according to one embodiment of the present invention, the chloroprene polymer composition is mixed with a large amount of methanol, precipitated, filtered, and dried. The resulting polymer is dissolved in tetrahydrofuran to obtain a sample, and the sample is subjected to gel permeation chromatography. In the molecular weight distribution obtained, preferably, a peak corresponding to a weight average molecular weight of 5,000 to 80,000 and a peak corresponding to a weight average molecular weight of 200,000 to 1,500,000 are detected, more preferably, a peak corresponding to a weight average molecular weight of 5,000 to 50,000 and a peak corresponding to a weight average molecular weight of 300,000 to 1,500,000 are detected, and even more preferably, a peak corresponding to a weight average molecular weight of 8,000 to 30,000 and a peak corresponding to a weight average molecular weight of 500,000 to 1,500,000 are detected. The chloroprene polymer composition according to one embodiment of the present invention preferably contains a diene polymer A having a weight-average molecular weight of 5,000 to 80,000 and a chloroprene polymer B having a weight-average molecular weight of 200,000 to 1,500,000, or a chloroprene polymer B having a weight-average molecular weight of 5,000 to 80,000 and a diene polymer A having a weight-average molecular weight of 200,000 to 1,500,000. It is more preferable that the polymer composition contains a chloroprene polymer B having a weight-average molecular weight of 5,000 to 50,000 and a diene polymer A having a weight-average molecular weight of 300,000 to 1,500,000, and it is even more preferable that the polymer composition contains a diene polymer A having a weight-average molecular weight of 8,000 to 30,000 and a chloroprene polymer B having a weight-average molecular weight of 500,000 to 1,500,000, or a chloroprene polymer B having a weight-average molecular weight of 8,000 to 30,000 and a diene polymer A having a weight-average molecular weight of 500,000 to 1,500,000.

[0081] The chloroprene polymer composition according to one embodiment of the present invention preferably contains 5 to 40% by mass of a polymer having a weight-average molecular weight of 5,000 to 80,000, relative to 100% by mass of the polymer contained in the chloroprene polymer composition. The content of the polymer having a weight-average molecular weight of 5,000 to 80,000 may be, for example, 5, 10, 15, 20, 25, 30, 35, or 40% by mass, and may be within a range between any two of the values ​​exemplified here.

[0082] The chloroprene polymer composition according to one embodiment of the present invention preferably contains 60 to 95 mass% of a polymer having a weight-average molecular weight of 200,000 to 1,500,000, relative to 100 mass% of the polymer contained in the chloroprene polymer composition. The content of the polymer having a weight-average molecular weight of 200,000 to 1,500,000 is, for example, 60, 65, 70, 75, 80, 85, 90, or 95 mass%, and may be within a range between any two of the values ​​exemplified here.

[0083] In the chloroprene polymer composition according to one embodiment of the present invention, the recovery rate of the chloroprene polymer composition in the polymerization step of the chloroprene polymer B is preferably 95.0% by mass or more. The recovery rate may be, for example, 95.0, 95.5, 96.0, 96.5, 97.0, 97.5, 98.0, 98.5, 99.0, 99.5, or 100.0% by mass, and may be within a range between any two of the values ​​exemplified here. In the chloroprene polymer composition according to one embodiment of the present invention, the chloroprene polymer B is polymerized in the presence of the diene polymer A, thereby reducing adhesion of the chloroprene polymer composition to a polymerization vessel and increasing the recovery rate. The recovery rate of the chloroprene polymer composition in the polymerization step of the chloroprene polymer B can be determined by the method described in the Examples.

[0084] In the chloroprene polymer composition according to one embodiment of the present invention, a dip-molded product obtained using the chloroprene polymer composition preferably has a tensile strength at break of 18.0 MPa or more, more preferably 19.0 MPa or more, as measured in accordance with JIS K 6251. The tensile strength at break is, for example, 18.0, 19.0, 20.0, 21.0, 22.0, 23.0, 24.0, 25.0, 26.0, 27.0, 28.0, 29.0, 30.0, 31.0, 32.0, 33.0, 34.0, 35.0, 36.0, 37.0, 38.0, 39.0, or 40.0 MPa, and may be within a range between any two of the values ​​exemplified here.

[0085] In the chloroprene polymer composition according to one embodiment of the present invention, a dip-molded product obtained using the chloroprene polymer composition preferably has a modulus at 100% elongation of 0.65 MPa or less, more preferably 0.60 MPa or less, as measured in accordance with JIS K 6251. The modulus at 100% elongation may be, for example, 0.30, 0.35, 0.40, 0.45, 0.50, 0.55, 0.60, or 0.65 MPa, or may be within a range between any two of the values ​​exemplified here.

[0086] The dip-molded product obtained using the chloroprene polymer composition can be obtained through a dip-molding step in which a composition for forming a dip-molded product containing the chloroprene polymer composition is dip-molded to obtain a dip-molded product, and a drying step in which the dip-molded product is heated and dried at 140°C for 1 hour to obtain a dip-molded product. The composition for forming a dip-molded product contains the chloroprene polymer composition and can also contain necessary chemicals such as metal oxides and antioxidants, and can have the formulations shown in the Examples. The dip-molded product can contain diene polymer A and chloroprene polymer B as base polymers, and can contain 70% by mass or more, preferably 80% by mass or more, and more preferably 90% by mass or more of the diene polymer A and chloroprene polymer B when the dip-molded product is taken as 100% by mass. When the dip-molded product is taken as 100% by mass, the content of the diene polymer A and the chloroprene polymer B in the dip-molded product is, for example, 70, 75, 80, 85, 90, 95, 96, 97, 98, 99, or 100% by mass, and may be within a range between any two of the values ​​exemplified here.

[0087] The tensile strength at break and modulus at 100% elongation of the dip-molded product containing the chloroprene polymer composition can be controlled by adjusting the weight-average molecular weights of the diene polymer A and chloroprene polymer B contained in the dip-molded product, the types and contents of the monomer units contained therein, the polymerization conditions for each polymer, the blending ratio, etc. The tensile strength at break and modulus at 100% elongation can be measured as described in the Examples.

[0088] 2. Method for Producing Dip-Molded Product A method for producing a dip-molded product according to one embodiment of the present invention may include a dip-molding step of dip-molding a composition for forming a dip-molded product, which contains the above-described chloroprene polymer composition, to obtain a dip-molded product, and a drying step of heating and drying the dip-molded product to obtain a dip-molded product.

[0089] 2.1 Composition for Forming Dip-Molded Body The composition for forming a dip-molded body according to one embodiment of the present invention contains the chloroprene polymer composition described above. The composition for forming a dip-molded body according to one embodiment of the present invention may contain, in addition to the chloroprene polymer composition, a metal oxide, an antioxidant, and other necessary chemicals. The composition for forming a dip-molded body according to one embodiment of the present invention may be one that does not contain a vulcanizing agent or a vulcanization accelerator, and may not contain sulfur or a vulcanization accelerator such as a thiuram, dithiocarbamate, thiourea, guanidine, xanthogenate, or thiazole.

[0090] 2.1.1 Metal Oxide The composition for forming an immersion molded body according to one embodiment of the present invention may contain a metal oxide. There are no particular limitations on the metal oxide, and examples include zinc oxide, lead oxide, trilead tetroxide, magnesium oxide, aluminum oxide, iron oxide, beryllium oxide, and titanium oxide. The metal oxide preferably contains zinc oxide. Zinc oxide is generally believed to function as a scavenger for dechlorinated atoms in chloroprene-based polymers. These metal oxides may be used alone or in combination of two or more.

[0091] The amount of metal oxide added is preferably 0.5 to 15.0 parts by mass per 100 parts by mass of the solids content of the chloroprene polymer composition contained in the composition for forming dip-molded bodies. When the amount of metal oxide added is 0.5 parts by mass or more, the cross-linking effect between polymers is expected to improve the tensile strength at break. When the amount of metal oxide added is 15.0 parts by mass or less, a dip-molded body with excellent flexibility can be obtained. Furthermore, from the viewpoint of the balance of physical properties between the flexibility and tensile strength at break of the obtained dip-molded body, the amount of metal oxide added is more preferably 0.5 to 5.0 parts by mass.

[0092] 2.1.2 Antioxidant The composition for forming a dip-molded body according to one embodiment of the present invention may also contain an antioxidant. The antioxidant is not particularly limited, and phenolic antioxidants, amine-based antioxidants, heat-resistant oxidation (aging) inhibitors, ozone-resistant antioxidants, etc. can be used. When the obtained dip-molded body is used as a medical glove, a phenolic antioxidant can be used from the viewpoint of the color tone, texture, and hygiene of the dip-molded body. In particular, hindered phenolic antioxidants have a strong effect as described above. Examples of hindered phenol-based antioxidants include 2,2'-methylenebis(4-ethyl-6-t-butylphenol), 2,2'-methylenebis(4-methyl-6-t-butylphenol), 4,4'-butylidene(3-methyl-6-t-butylphenol), 4,4'-thiobis(3-methyl-6-t-butylphenol), butylated reaction products of p-cresol and dicyclopentadiene, 2,5'-di-t-butylhydroquinone, and 2,5'-di-t-amylhydroquinone. Among these, butylated reaction products of p-cresol and dicyclopentadiene are desirable from the viewpoint of general dispersibility in aqueous materials. Furthermore, these compounds may be used alone or in combination of two or more.

[0093] The amount of antioxidant added is preferably 0.5 to 10.0 parts by mass per 100 parts by mass of the solids content of the chloroprene polymer composition contained in the composition for forming a dip-molded body. The amount of antioxidant added may be, for example, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, or 10.0 parts by mass, or may be within a range between any two of the values ​​exemplified here. When the amount of antioxidant added is 0.5 parts by mass or more, the effect of suppressing color change in the dip-molded body can be obtained. When the amount of antioxidant added is 10.0 parts by mass or less, the stability of the composition for forming a dip-molded body can be ensured. Furthermore, from the viewpoint of the balance of physical properties between the flexibility and tensile strength at break of the obtained dip-molded body, the amount of antioxidant added is more preferably 0.5 to 5.0 parts by mass.

[0094] 2.1.3 Vulcanizing Agent and Vulcanization Accelerator The composition for forming a dip-molded body according to one embodiment of the present invention may also contain a vulcanizing agent and / or a vulcanization accelerator. Furthermore, the composition for forming a dip-molded body according to one embodiment of the present invention may not contain sulfur or the aforementioned thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthogenate-based, thiazole-based, or other vulcanization accelerators. That is, the composition for forming a dip-molded body includes those containing a vulcanizing agent but not a vulcanization accelerator, those containing a vulcanization accelerator but not a vulcanizing agent, those containing a vulcanization accelerator and a vulcanization accelerator, and those containing neither a vulcanizing agent nor a vulcanization accelerator. Whether or not a vulcanizing agent and a vulcanization accelerator are added can be determined depending on the desired dip-molded body.

[0095] Examples of vulcanizing agents include, but are not limited to, sulfur. The amount of vulcanizing agent added can be 0 to 10.0 parts by mass per 100 parts by mass of the solid content of the chloroprene polymer composition contained in the composition for forming dip-molded bodies. The amount of vulcanizing agent added can be, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 parts by mass, and may be within a range between any two of the values ​​exemplified here.

[0096] A vulcanization accelerator is a chemical added during the vulcanization of raw rubber to act with the vulcanizing agent to increase the vulcanization speed, thereby shortening the vulcanization time, lowering the vulcanization temperature, reducing the amount of vulcanizing agent, and improving the physical properties of the vulcanized rubber. It usually refers to a chemical that accelerates the sulfur vulcanization reaction.

[0097] Examples of vulcanization accelerators include, but are not limited to, thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthogenate-based, thiazole-based, etc. These may be used alone or in combination of two or more types as required.

[0098] Examples of thiuram vulcanization accelerators include tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, tetrakis(2-ethylhexyl)thiuram disulfide, tetramethylthiuram monosulfide, and dipentamethylenethiuram tetrasulfide.

[0099] Examples of the dithiocarbamate vulcanization accelerator include sodium dibutyldithiocarbamate, zinc dimethyldithiocarbamate, zinc diethyldithiocarbamate, zinc N-ethyl-N-phenyldithiocarbamate, zinc N-pentamethylenedithiocarbamate, copper dimethyldithiocarbamate, ferric dimethyldithiocarbamate, and tellurium diethyldithiocarbamate, and zinc dibutyldithiocarbamate is particularly preferred.

[0100] Examples of the thiourea-based vulcanization accelerator include ethylene thiourea, N,N'-diethyl thiourea, trimethyl thiourea, and N,N'-diphenyl thiourea.

[0101] Examples of the guanidine vulcanization accelerator include 1,3-diphenylguanidine, 1,3-di-o-tolylguanidine, 1-o-tolylbiguanide, and di-o-tolylguanidine salts of dicatechol borate.

[0102] Examples of xanthogenate-based vulcanization accelerators include zinc butylxanthogenate and zinc isopropylxanthogenate.

[0103] Examples of the thiazole vulcanization accelerator include 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, 2-mercaptobenzothiazole zinc salt, 2-mercaptobenzothiazole cyclohexylamine salt, and 2-(4'-morpholinodithio)benzothiazole.

[0104] The amount of the vulcanization accelerator added may be 0 to 5.0 parts by mass relative to 100 parts by mass of the solid content of the chloroprene polymer composition contained in the composition for forming a dip-molded body, and may be, for example, 0, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, or 5.0, or may be within a range between any two of the values ​​exemplified here.

[0105] 2.1.4 Other Agents (Heteroaromatic Ring Compounds) The composition for forming a dip-molded body according to one embodiment of the present invention may contain a heteroaromatic ring compound in the chloroprene polymer. The heteroaromatic ring compound contained in the composition for forming a dip-molded body used to obtain a dip-molded body according to one embodiment of the present invention can be represented by chemical formula (1) and has a benzimidazole structure. Note that compounds having this structure may be used as secondary antioxidants, mainly in the formulation of rubber compositions.

[0106]

[0107] In chemical formula (1), X of the mercapto group represents a hydrogen atom or a metal atom. X may be a hydrogen atom and have a thiol group. X may also be a metal atom, and examples of the metal atom include zinc, sodium, copper, nickel, and tellurium, with zinc being preferred. R in chemical formula (1) 1 ~R 4 R represents a hydrogen atom, an alkyl group which may have a substituent, an ether group which may have a substituent, a nitro group, an amino group, or a carboxyl group. 1 ~R 4 may be the same or different. The heteroaromatic ring compounds may be used singly or in combination of two or more.

[0108] Examples of heteroaromatic ring compounds include 2-mercaptobenzimidazole, 5-methyl-2-mercaptobenzimidazole, 4-methyl-2-mercaptobenzimidazole, 5-methoxy-2-mercaptobenzimidazole, 4-methoxy-2-mercaptobenzimidazole, 5-nitro-2-mercaptobenzimidazole, 5-amino-2-mercaptobenzimidazole, 5-carboxy-2-mercaptobenzimidazole, and zinc salts of 2-mercaptobenzimidazole. Among these, 2-mercaptobenzimidazole, 5-methyl-2-mercaptobenzimidazole, 4-methyl-2-mercaptobenzimidazole, 5-methoxy-2-mercaptobenzimidazole, 4-methoxy-2-mercaptobenzimidazole, and zinc salts of 2-mercaptobenzimidazole are preferred.

[0109] The amount of the heteroaromatic ring compound added is preferably 0.2 to 10.0 parts by mass per 100 parts by mass of the solids content of the chloroprene polymer composition contained in the composition for forming dip-molded articles. The amount of the heteroaromatic ring compound added is, for example, 0.2, 0.3, 0.4, 0.5, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, or 10.0 parts by mass, and may be within a range between any two of the values ​​exemplified here. When the amount added is 0.2 parts by mass or more, the dip-molded article obtained using this composition exhibits very high breaking strength. When the amount added is 10.0 parts by mass or less, the stability of the composition for forming dip-molded articles is ensured. Furthermore, from the viewpoint of the balance of physical properties between flexibility and breaking strength of the resulting dip-molded article, the amount added is more preferably 0.3 to 5.0 parts by mass.

[0110] A method for producing a composition for forming an immersion molded body according to one embodiment of the present invention may include a raw material mixing step of mixing raw materials containing a chloroprene polymer composition, a metal oxide, an antioxidant, and other required chemicals. In the mixing step, an aqueous dispersion containing the metal oxide, the antioxidant, and other required chemicals may be prepared in advance, and the chloroprene polymer composition and the aqueous dispersion may be mixed. The mixing step may be performed using a known mixing device such as a ball mill.

[0111] 2.2 Dip-molding step A method for producing a dip-molded product according to one embodiment of the present invention may include a dip-molding step of dip-molding a composition for forming a dip-molded product, which contains the chloroprene polymer composition obtained by the above-described method for producing a chloroprene polymer composition, to obtain a dip-molded product.

[0112] Examples of dip molding methods in one embodiment of the present invention include immersion solidification, simple immersion, thermal immersion, and electrodeposition. The immersion solidification method can be used from the viewpoints of ease of production and the ease of obtaining dip-molded bodies of a uniform thickness. Specifically, a ceramic mold coated with a calcium-based coagulation liquid is immersed in a dip-molded body composition, and the dip-molded body composition is solidified. After leaching to remove water-soluble impurities, the composition is dried, and then heated and vulcanized to form a dip-molded film (rubber film), which is then demolded. This allows for the production of a film-like dip-molded body.

[0113] 2.3 Drying Step The method for producing a dip-molded product according to one embodiment of the present invention may include a drying step of heating and drying the dip-molded product to obtain a dip-molded product.

[0114] The heat drying temperature may be set appropriately depending on the composition of the chloroprene polymer composition and may be 120 to 180°C. The heating temperature is preferably 120 to 150°C. The heating temperature may be, for example, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, or 220°C, or may be within a range between any two of the values ​​exemplified here. The heating time may be set appropriately depending on the composition of the chloroprene polymer composition, the shape of the unvulcanized molded body, and the like and may be 10 to 300 minutes. The heating time may be, for example, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, or 300 minutes, or may be within a range between any two of the values ​​exemplified here. As an example, a dip-molded product according to one embodiment of the present invention may be one that has been subjected to a heat drying treatment at 140°C for 1 hour.

[0115] 3. Dip-molded Products (Dip-molded Product Coatings / Films) A dip-molded product according to one embodiment of the present invention can be obtained using the chloroprene polymer composition described above. A dip-molded product can be obtained by dip-molding the above-described composition for forming a dip-molded product, either alone or in a blend with other compositions for forming a dip-molded product. The dip-molded product according to the present invention can be obtained by dip-molding the composition for forming a dip-molded product by a dip coagulation method, followed by heating and drying at 140°C for 1 hour. The dip-molded product according to the present invention has high tensile strength at break and low modulus at 100% elongation. Furthermore, the dip-molded product can be efficiently produced due to its high recovery rate from the polymerization vessel. The dip-molded product according to one embodiment of the present invention can be suitably used as industrial and general household gloves, medical gloves, balloons, catheters, and boots.

[0116] The dip-molded product according to the present invention may contain the components contained in the composition for forming a dip-molded product. The dip-molded product may contain a diene polymer A and a chloroprene polymer B as base polymers, and may contain 70% by mass or more, preferably 80% by mass or more, and more preferably 90% by mass or more of the diene polymer A and the chloroprene polymer B relative to 100% by mass of the dip-molded product. The contents of the diene polymer A and the chloroprene polymer B in the dip-molded product relative to 100% by mass of the dip-molded product may be, for example, 70, 75, 80, 85, 90, 95, 96, 97, 98, 99, or 100% by mass, or may be within a range between any two of the values ​​exemplified here.

[0117] The dip-molded article containing the chloroprene polymer according to the present invention has high tensile strength at break and low modulus at 100% elongation, regardless of whether a vulcanizing agent and a vulcanization accelerator are added. The dip-molded article according to one embodiment of the present invention may be free of a vulcanizing agent and a vulcanization accelerator, and may be free of sulfur and vulcanization accelerators such as thiuram, dithiocarbamate, thiourea, guanidine, xanthogenate, and thiazole.

[0118] 3.1 Characteristics of Dip-Molded Product In the dip-molded product according to one embodiment of the present invention, when the soluble fraction obtained by dissolving the dip-molded product in tetrahydrofuran is subjected to gel permeation chromatography, the molecular weight distribution preferably exhibits a peak corresponding to a weight-average molecular weight of 5,000 to 80,000 and a peak corresponding to a weight-average molecular weight of 200,000 to 1,500,000, more preferably a peak corresponding to a weight-average molecular weight of 5,000 to 50,000 and a peak corresponding to a weight-average molecular weight of 300,000 to 1,500,000, and even more preferably a peak corresponding to a weight-average molecular weight of 8,000 to 30,000 and a peak corresponding to a weight-average molecular weight of 500,000 to 1,500,00. The weight-average molecular weights and blending ratios of the low molecular weight component and the high molecular weight component may be as described above.

[0119] In the chloroprene polymer composition according to one embodiment of the present invention, a dip-molded product containing the chloroprene polymer composition preferably has a tensile strength at break of 18.0 MPa or more, more preferably 19.0 MPa or more, as measured in accordance with JIS K 6251. The tensile strength at break may be, for example, 18.0, 19.0, 20.0, 21.0, 22.0, 23.0, 24.0, 25.0, 26.0, 27.0, 28.0, 29.0, 30.0, 31.0, 32.0, 33.0, 34.0, 35.0, 36.0, 37.0, 38.0, 39.0, or 40.0 MPa, or may be within a range between any two of the values ​​exemplified here.

[0120] In the chloroprene polymer composition according to one embodiment of the present invention, a dip-molded product containing a chloroprene polymer preferably has a modulus at 100% elongation of 0.65 MPa or less, more preferably 0.60 MPa or less, as measured in accordance with JIS K 6251. The modulus at 100% elongation may be, for example, 0.30, 0.35, 0.40, 0.45, 0.50, 0.55, 0.60, or 0.65 MPa, or may be within a range between any two of the values ​​exemplified here.

[0121] The dip-molded product contains a chloroprene polymer and may further contain an antioxidant or a metal oxide. The dip-molded product may also contain a vulcanizing agent, a vulcanization accelerator, and an antioxidant. The manufacturing method of the dip-molded product and the methods for measuring the tensile strength at break and the modulus at 100% elongation may be as described in the Examples.

[0122] The tensile strength at break and the modulus at 100% elongation of the dip-molded product can be controlled by adjusting the types and amounts of raw materials used in polymerizing the diene polymer A and the chloroprene polymer B, the types and amounts of agents used, and the polymerization conditions.

[0123] 3.2 Shape of the Dip-Molded Product The thickness (e.g., minimum thickness) of the dip-molded product may be 0.01 to 0.50 mm. The thickness of the dip-molded product may be, for example, 0.01, 0.05, 0.10, 0.20, 0.30, 0.40, or 0.50 mm, and may be within a range between any two of the values ​​exemplified here. The thickness of the dip-molded product can be adjusted by the time for immersing the mold in the composition for forming a dip-molded product, the solids concentration of the composition for forming a dip-molded product, and the like. To reduce the thickness of the dip-molded product, the immersion time may be shortened or the solids concentration of the composition for forming a dip-molded product may be reduced.

[0124] The dip-molded product may contain sulfur or a vulcanization accelerator. However, even if the dip-molded product does not contain sulfur or a vulcanization accelerator, it has mechanical properties equivalent to or superior to those of vulcanized dip-molded products obtained from conventional dip-molded product compositions containing chloroprene polymers. Therefore, the chloroprene polymer composition according to the present invention is suitable as a raw material for the dip-molded product (dip-molded product) of the chloroprene polymer of this embodiment.

[0125] The method for producing a dip-molded product according to one embodiment of the present invention may also include a step of subjecting the obtained dip-molded product to a heat drying treatment to vulcanize the unvulcanized dip-molded product.

[0126] The present invention will be described in more detail below based on examples, but the present invention should not be construed as being limited to these examples.

[0127] <Preparation of Chloroprene Polymer A> (Synthesis Example A-1) A 30 L polymerization vessel was charged with 64 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 77 parts by mass of pure water, 17.6 parts by mass of a gum rosin-based disproportionated rosin aqueous solution (trade name "LONDIS K-25", solids content 25% by mass, manufactured by Arakawa Chemical Industries, Ltd.), 3.4 parts by mass of n-dodecyl mercaptan, 0.8 parts by mass of potassium hydroxide, 0.5 parts by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), and 0.5 parts by mass of sodium hydrogen sulfite. Polymerization was carried out at a polymerization temperature of 35°C under a nitrogen stream by continuously adding a 0.35 wt % aqueous potassium persulfate solution as a polymerization initiator. When the polymerization rate of the charged monomers reached 80%, 27 parts by mass of chloroprene (monomer) was continuously added over 100 minutes. When the polymerization rate of the initially charged monomers and the continuously added monomers reached 91%, the addition of the aqueous potassium persulfate solution was stopped to terminate the polymerization, thereby obtaining a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a latex of chloroprene polymer A-1 with a solids concentration of 60% by weight. The obtained latex was used in the preparation of chloroprene polymer B in Example 7. A portion of the obtained latex was used to precipitate chloroprene polymer A-1 by the method described below, which was then analyzed and used in the preparation of chloroprene polymer B in Examples 1 to 3.

[0128] (Precipitation of Chloroprene Polymer A with Methanol) The obtained latex of chloroprene polymer A-1 was mixed with a large amount of methanol to precipitate a rubber component (chloroprene polymer A-1), which was then filtered and dried to obtain a sample of chloroprene polymer A-1. The weight-average molecular weight of the chloroprene polymer was measured from the obtained sample. This sample was also used to produce chloroprene polymer B in Examples 1 to 3 described below. The analytical results are shown in Table 1. The measurement method will be described later.

[0129] Synthesis Example A-2 Polymerization was carried out in the same manner as in Synthesis Example A-1, except that the amount of n-dodecyl mercaptan used in Synthesis Example A-1 was changed to 5.3 parts by mass. The resulting polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a latex of chloroprene polymer A-2 with a solid content of 60% by weight. From the resulting latex, chloroprene polymer A-2 was precipitated in the same manner as in Synthesis Example A-1, and used in the production of chloroprene polymer B. The weight-average molecular weight of chloroprene polymer A-2 was measured in the same manner as in Synthesis Example A-1. The analytical results are shown in Table 1.

[0130] Synthesis Example A-3 Polymerization was carried out in the same manner as in Synthesis Example A-1, except that the amount of n-dodecyl mercaptan used in Synthesis Example A-1 was changed to 2.4 parts by mass. The resulting polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a latex of chloroprene polymer A-3 with a solid content of 60% by weight. From the resulting latex, chloroprene polymer A-3 was precipitated in the same manner as in Synthesis Example A-1, and used in the production of chloroprene polymer B. The weight-average molecular weight of chloroprene polymer A-3 was measured in the same manner as in Synthesis Example A-1. The analytical results are shown in Table 1.

[0131] Synthesis Example A-4 Polymerization was carried out in the same manner as in Synthesis Example A-1, except that the amount of n-dodecyl mercaptan used in Synthesis Example A-1 was changed to 1.5 parts by mass. The resulting polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a latex of chloroprene polymer A-4 with a solid content of 60% by weight. From the resulting latex, chloroprene polymer A-4 was precipitated in the same manner as in Synthesis Example A-1, and used in the production of chloroprene polymer B. The weight-average molecular weight of chloroprene polymer A-4 was measured in the same manner as in Synthesis Example A-1. The analytical results are shown in Table 1.

[0132] Synthesis Example A-5 To a 30 L polymerization vessel were added 64 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 351 parts by mass of pure water, 92 parts by mass of a gum rosin-based disproportionated rosin aqueous solution (trade name "LONDIS K-25", solids content 25% by mass, manufactured by Arakawa Chemical Industries, Ltd.), 3.4 parts by mass of n-dodecyl mercaptan, 4 parts by mass of potassium hydroxide, 2 parts by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), and 0.5 parts by mass of sodium hydrogen sulfite so that the total volume of the charged solution was 18 L. Polymerization was carried out at a polymerization temperature of 35°C under a nitrogen stream by continuously adding a 0.35 wt % aqueous potassium persulfate solution as a polymerization initiator. When the polymerization rate of the charged monomers reached 80%, 27 parts by mass of chloroprene (monomer) was continuously added over 100 minutes. When the polymerization rate of the initially charged monomers and the continuously added monomers reached 91%, the addition of the aqueous potassium persulfate solution was stopped to terminate the polymerization, thereby obtaining a polymerization liquid. The resulting latex of chloroprene polymer A-5 (solids concentration: 21.8% by mass) was used in Example 8. Furthermore, chloroprene polymer A-5 was precipitated in the same manner as in Synthesis Example A-1, and the weight-average molecular weight of chloroprene polymer A-5 was measured. The analytical results are shown in Table 1.

[0133] Synthesis Example A-6: To a 30 L polymerization vessel were added 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 100 parts by mass of pure water, 17.6 parts by mass of a gum rosin-based disproportionated rosin aqueous solution (trade name "LONDIS K-25", solids content 25% by mass, manufactured by Arakawa Chemical Industries, Ltd.), 0.03 parts by mass of n-dodecyl mercaptan, 0.8 parts by mass of potassium hydroxide, 0.5 parts by mass of a sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogensulfite, and 0.04 parts by mass of thiourea dioxide, so that the total volume of the charged solution was 25 L. Polymerization was carried out at a polymerization temperature of 13°C under a nitrogen stream by continuously adding a 0.35 wt % aqueous potassium persulfate solution as a polymerization initiator. When the polymerization rate reached 85%, the addition of the aqueous potassium persulfate solution was stopped to terminate the polymerization, thereby obtaining a polymerization solution. The resulting latex of chloroprene polymer A-6 (solid content concentration: 41.7% by mass) was used in Example 9. Chloroprene polymer A-6 was precipitated in the same manner as in Synthesis Example A-1, and the weight-average molecular weight of chloroprene polymer A-6 was measured. The analytical results are shown in Table 1.

[0134]

[0135] Preparation of Chloroprene Polymer B Example 1 A 30 L polymerization vessel was charged with 21.3 parts by mass of the chloroprene polymer A-1 prepared and precipitated in Synthesis Example A-1, 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 87 parts by mass of pure water, 17.6 parts by mass of a gum rosin-based disproportionated rosin aqueous solution (trade name "LONDIS K-25", solids content 25% by mass, manufactured by Arakawa Chemical Industries, Ltd.), 0.8 parts by mass of potassium hydroxide, 0.5 parts by mass of a sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogensulfite, and 0.03 parts by mass of thiourea dioxide. Polymerization was carried out at a polymerization temperature of 13°C under a nitrogen stream by continuously adding a 0.35 wt % aqueous potassium persulfate solution as a polymerization initiator. When the polymerization rate reached 85%, 0.1 parts by mass of diethylhydroxylamine, a polymerization terminator, was added to terminate the polymerization, yielding a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to yield a latex of chloroprene polymer B-1 with a solids concentration of 60% by weight, i.e., a chloroprene polymer composition. The entire amount of the resulting chloroprene polymer composition was withdrawn from the polymerization vessel, and the actual weight of the chloroprene polymer composition after polymerization was measured. The recovery rate of the chloroprene polymer composition during polymerization of chloroprene polymer B was calculated from the measured actual weight of the chloroprene polymer composition after polymerization. The calculation results are shown in Table 2. The calculation method will be described later.

[0136] After measuring the actual weight of the chloroprene polymer composition after polymerization, 50 ml of the chloroprene polymer composition was sampled, and the remaining chloroprene polymer composition was used to prepare a dip-molded product for evaluation.

[0137] The sampled chloroprene polymer composition was mixed with a large amount of methanol to precipitate a rubber component, which was then filtered and dried to obtain a sample of chloroprene polymer B-1. The weight average molecular weight of the chloroprene polymer B-1 was measured using the obtained sample. The analytical results are shown in Table 2. The measurement method will be described later.

[0138] (Examples 2 and 3) Polymerization was carried out in the same manner as in Example 1, using the raw material charging amounts and polymerization conditions shown in Table 2. The obtained polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a latex of chloroprene polymer B having a solids concentration of 60% by weight, i.e., a chloroprene polymer composition. The entire amount of the obtained chloroprene polymer composition was extracted from the polymerization vessel, and the recovery rate of the chloroprene polymer composition during polymerization of chloroprene polymer B was calculated in the same manner as in Example 1. The calculation results are shown in Table 2.

[0139] After measuring the actual weight of the chloroprene polymer composition after polymerization, 50 ml of the chloroprene polymer composition was sampled, and the remaining chloroprene polymer composition was used to prepare a dip-molded product for evaluation.

[0140] The sampled chloroprene polymer composition was mixed with a large amount of methanol to precipitate a rubber component, which was then filtered and dried to obtain a sample of chloroprene polymer B. The weight average molecular weight of the obtained sample was measured. The analytical results are shown in Table 2.

[0141] Example 4 A 30 L polymerization vessel was charged with 21.3 parts by mass of the rubber component of chloroprene polymer A-2 prepared in Synthesis Example A-2, 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 87 parts by mass of pure water, 17.6 parts by mass of a gum rosin-based disproportionated rosin aqueous solution (trade name "LONDIS K-25", solids content 25% by mass, manufactured by Arakawa Chemical Industries, Ltd.), 0.8 parts by mass of potassium hydroxide, 0.5 parts by mass of a sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogensulfite, and 0.03 parts by mass of thiourea dioxide. Polymerization was carried out at a polymerization temperature of 13°C under a nitrogen stream by continuously adding a 0.35 wt % aqueous potassium persulfate solution as a polymerization initiator. When the polymerization rate reached 85%, 0.1 parts by mass of diethylhydroxylamine, a polymerization terminator, was added to terminate the polymerization, yielding a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to yield a latex of chloroprene polymer B-4 with a solids concentration of 60% by weight, i.e., a chloroprene polymer composition. The entire amount of the resulting chloroprene polymer composition was extracted from the polymerization vessel, and the recovery rate of the chloroprene polymer composition during polymerization of chloroprene polymer B was calculated using the same procedure as in Example 1. The calculation results are shown in Table 2.

[0142] After measuring the actual weight of the chloroprene polymer composition after polymerization, 50 ml of the chloroprene polymer composition was sampled, and the remaining chloroprene polymer composition was used to prepare a dip-molded product for evaluation.

[0143] The sampled chloroprene polymer composition was mixed with a large amount of methanol to precipitate a rubber component, which was then filtered and dried to obtain a sample of chloroprene polymer B-4. The weight average molecular weight of the obtained sample was measured. The analytical results are shown in Table 2.

[0144] Example 5 A 30 L polymerization vessel was charged with 21.3 parts by mass of the rubber component of chloroprene polymer A-3 prepared in Synthesis Example A-3, 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 87 parts by mass of pure water, 17.6 parts by mass of a gum rosin-based disproportionated rosin aqueous solution (trade name "LONDIS K-25", solids content 25% by mass, manufactured by Arakawa Chemical Industries, Ltd.), 0.8 parts by mass of potassium hydroxide, 0.5 parts by mass of a sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogensulfite, and 0.03 parts by mass of thiourea dioxide. Polymerization was carried out at a polymerization temperature of 13°C under a nitrogen stream by continuously adding a 0.35 wt % aqueous potassium persulfate solution as a polymerization initiator. When the polymerization rate reached 85%, 0.1 parts by mass of diethylhydroxylamine, a polymerization terminator, was added to terminate the polymerization, yielding a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to yield a latex of chloroprene polymer B-5 with a solids concentration of 60% by weight, i.e., a chloroprene polymer composition. The entire amount of the resulting chloroprene polymer composition was extracted from the polymerization vessel, and the recovery rate of the chloroprene polymer composition during polymerization of chloroprene polymer B was calculated using the same procedure as in Example 1. The calculation results are shown in Table 2.

[0145] After measuring the actual weight of the chloroprene polymer composition after polymerization, 50 ml of the chloroprene polymer composition was sampled, and the remaining chloroprene polymer composition was used to prepare a dip-molded product for evaluation.

[0146] The sampled chloroprene polymer composition was mixed with a large amount of methanol to precipitate a rubber component, which was then filtered and dried to obtain a sample of chloroprene polymer B-5. The weight average molecular weight of the obtained sample was measured. The analytical results are shown in Table 2.

[0147] Example 6 A 30 L polymerization vessel was charged with 21.3 parts by mass of the rubber component of chloroprene polymer A-4 prepared in Synthesis Example A-4, 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 87 parts by mass of pure water, 17.6 parts by mass of a gum rosin-based disproportionated rosin aqueous solution (trade name "LONDIS K-25", solids content 25% by mass, manufactured by Arakawa Chemical Industries, Ltd.), 0.8 parts by mass of potassium hydroxide, 0.5 parts by mass of a sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogensulfite, and 0.03 parts by mass of thiourea dioxide. Polymerization was carried out at a polymerization temperature of 13°C under a nitrogen stream by continuously adding a 0.35 wt % aqueous potassium persulfate solution as a polymerization initiator. When the polymerization rate reached 85%, 0.1 parts by mass of diethylhydroxylamine, a polymerization terminator, was added to terminate the polymerization, yielding a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to yield a latex of chloroprene polymer B-6 with a solids concentration of 60% by weight, i.e., a chloroprene polymer composition. The entire amount of the resulting chloroprene polymer composition was extracted from the polymerization vessel, and the recovery rate of the chloroprene polymer composition containing chloroprene polymer B was calculated using the same procedure as in Example 1. The calculation results are shown in Table 2.

[0148] After measuring the actual weight of the chloroprene polymer composition after polymerization, 50 ml of the chloroprene polymer composition was sampled, and the remaining chloroprene polymer composition was used to prepare a dip-molded product for evaluation.

[0149] The sampled chloroprene polymer composition was mixed with a large amount of methanol to precipitate a rubber component, which was then filtered and dried to obtain a sample of chloroprene polymer B-6. The weight average molecular weight of the obtained sample was measured. The analytical results are shown in Table 2.

[0150] Example 7 A 30 L polymerization vessel was charged with 39 parts by mass of the chloroprene polymer A-1 latex prepared in Synthesis Example A-1, 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 74 parts by mass of pure water, 13.6 parts by mass of a gum rosin-based disproportionated rosin aqueous solution (trade name "LONDIS K-25", solids content 25% by mass, manufactured by Arakawa Chemical Industries, Ltd.), 0.6 parts by mass of potassium hydroxide, 0.4 parts by mass of a sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), 0.4 parts by mass of sodium hydrogensulfite, and 0.03 parts by mass of thiourea dioxide. Polymerization was carried out at a polymerization temperature of 13°C under a nitrogen stream by continuously adding a 0.35 wt % potassium persulfate aqueous solution as a polymerization initiator. When the polymerization rate reached 85%, 0.1 parts by mass of diethylhydroxylamine, a polymerization terminator, was added to terminate the polymerization, yielding a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to yield a latex of chloroprene polymer B-7 with a solids concentration of 60% by weight, i.e., a chloroprene polymer composition. The entire amount of the resulting chloroprene polymer composition was extracted from the polymerization vessel, and the recovery rate of the chloroprene polymer composition containing chloroprene polymer B was calculated using the same procedure as in Example 1. The calculation results are shown in Table 2.

[0151] After measuring the actual weight of the latex after polymerization, 50 ml of the chloroprene polymer composition was sampled, and the remaining chloroprene polymer composition was used to prepare a dip-molded product for evaluation.

[0152] The sampled chloroprene polymer composition was mixed with a large amount of methanol to precipitate a rubber component, which was then filtered and dried to obtain a sample of chloroprene polymer B-7. The weight average molecular weight of the obtained sample was measured. The analytical results are shown in Table 2.

[0153] Example 8 To a 30 L polymerization vessel were added 130.8 parts by mass of the latex of chloroprene polymer A-5 prepared in Synthesis Example A-5, 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 0.5 parts by mass of sodium hydrogen sulfite, and 0.03 parts by mass of thiourea dioxide. Polymerization was carried out at a polymerization temperature of 13°C under a nitrogen stream by continuously adding a 0.35 wt% aqueous solution of potassium persulfate as a polymerization initiator. When the conversion rate reached 85%, 0.1 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization, yielding a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomer, and then concentrated to obtain a latex of chloroprene polymer B-8 with a solids concentration of 60 wt%, i.e., a chloroprene polymer composition. The entire amount of the obtained chloroprene polymer composition was discharged from the polymerization vessel, and the recovery rate of the chloroprene polymer composition during polymerization of chloroprene polymer B was calculated in the same manner as in Example 1. The calculation results are shown in Table 2.

[0154] After measuring the actual weight of the chloroprene polymer composition after polymerization, 50 ml of the chloroprene polymer composition was sampled, and the remaining chloroprene polymer composition was used to prepare a dip-molded product for evaluation.

[0155] The sampled chloroprene polymer composition was mixed with a large amount of methanol to precipitate a rubber component, which was then filtered and dried to obtain a sample of chloroprene polymer B-8. The weight average molecular weight of the obtained sample was measured. The analytical results are shown in Table 2.

[0156] Example 9 To a 30 L polymerization vessel were added 1,000 parts by mass of the latex of chloroprene polymer A-6 prepared in Synthesis Example A-6, 74 parts by mass of chloroprene (monomer), 7 parts by mass of 2,3-dichloro-1,3-butadiene, 2.7 parts by mass of n-dodecyl mercaptan, 0.4 parts by mass of sodium hydrogen sulfite, and 0.03 parts by mass of thiourea dioxide. Polymerization was carried out at a polymerization temperature of 13°C under a nitrogen stream by continuously adding a 0.35 wt% aqueous solution of potassium persulfate as a polymerization initiator. When the conversion rate reached 85%, 0.1 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization, yielding a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomer, and then concentrated to obtain a latex of chloroprene polymer B-9 with a solids concentration of 60 wt%, i.e., a chloroprene polymer composition. The entire amount of the obtained chloroprene polymer composition was discharged from the polymerization vessel, and the recovery rate of the chloroprene polymer composition containing chloroprene polymer B was calculated in the same manner as in Example 1. The calculation results are shown in Table 2.

[0157] After measuring the actual weight of the chloroprene polymer composition after polymerization, 50 ml of the chloroprene polymer composition was sampled, and the remaining chloroprene polymer composition was used to prepare a dip-molded product for evaluation.

[0158] The sampled chloroprene polymer composition was mixed with a large amount of methanol to precipitate a rubber component, which was then filtered and dried to obtain a sample of chloroprene polymer B-9. The weight average molecular weight of the obtained sample was measured. The analytical results are shown in Table 2.

[0159] Comparative Example 1 A 30 L polymerization vessel was charged with 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 77 parts by mass of pure water, 17.6 parts by mass of a gum rosin-based disproportionated rosin aqueous solution (trade name "LONDIS K-25", solids content 25% by mass, manufactured by Arakawa Chemical Industries, Ltd.), 0.02 parts by mass of n-dodecyl mercaptan, 0.8 parts by mass of potassium hydroxide, 0.5 parts by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogensulfite, and 0.04 parts by mass of thiourea dioxide. Polymerization was carried out at a polymerization temperature of 13°C under a nitrogen stream by continuously adding a 0.35 wt % aqueous potassium persulfate solution as a polymerization initiator. When the polymerization rate reached 85%, 0.1 parts by mass of diethylhydroxylamine, a polymerization terminator, was added to terminate the polymerization, yielding a polymerization solution. The polymerization solution was distilled under reduced pressure to remove unreacted monomers, and then concentrated to yield a latex of chloroprene polymer C with a solids concentration of 60% by weight, i.e., a chloroprene polymer composition. The entire amount of the resulting chloroprene polymer composition was extracted from the polymerization vessel, and the recovery rate of the chloroprene polymer composition from chloroprene polymer C was calculated using the same procedure as in Example 1. The calculation results are shown in Table 3. Furthermore, a dip-molded product for evaluation was prepared using the resulting chloroprene polymer composition. A portion of the resulting chloroprene polymer composition was used in Comparative Example 2.

[0160] Comparative Example 2 Polymerization was carried out in the same manner as in Synthesis Example A-1. The obtained polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a latex of chloroprene polymer D having a solids concentration of 60% by weight, i.e., a chloroprene polymer composition. The entire amount of the obtained chloroprene polymer composition was extracted from the polymerization vessel, and the recovery rate of the chloroprene polymer was calculated in the same manner as in Example 1. The calculation results are shown in Table 3.

[0161] The chloroprene polymer composition of chloroprene polymer C obtained in Comparative Example 1 and the chloroprene polymer composition of chloroprene polymer D were mixed in a weight ratio of C / D=80 / 20 to obtain a chloroprene polymer composition of chloroprene polymer E. A dip-molded product for evaluation was produced using the obtained chloroprene polymer composition.

[0162] Chloroprene polymers A and B were analyzed by the following method. <Measurement of weight-average molecular weight of chloroprene polymers A and B> As described above, the weight-average molecular weight was measured by gel permeation chromatography (GPC) under the following measurement conditions using samples obtained by subjecting the latex of chloroprene polymer A and the latex containing a chloroprene polymer, i.e., the chloroprene polymer composition, to methanol precipitation, filtering, and drying, and dissolving the resulting polymer in 20 ml of tetrahydrofuran. Apparatus: HLC-8320 (manufactured by Tosoh Corporation) Column: Three TSKgel GMHHR-H columns in series Temperature: 40°C Detection: differential refractive index Solvent: tetrahydrofuran Calibration curve: prepared using standard polystyrene (PS).

[0163] The recovery rate of the chloroprene polymer composition was evaluated by the following method. <Recovery rate of chloroprene polymer composition> In each Example and Comparative Example, the recovery rate of the chloroprene polymer composition was calculated based on the actual weight of the chloroprene polymer composition after polymerization when the obtained chloroprene polymer composition was withdrawn from the piping at the bottom of the polymerization vessel and the amount of the chloroprene polymer composition charged during polymerization, using the following formula. When the chloroprene polymer composition was withdrawn from the piping at the bottom of the polymerization vessel, the stickier the chloroprene polymer composition, the more the chloroprene polymer composition adheres to the wall of the polymerization vessel, and the smaller the recovery amount. The theoretical weight indicates the amount of chloroprene polymer composition present in the polymerization vessel just before the recovery operation, calculated by subtracting the amount removed from the system by vacuum distillation removal of unreacted monomer and concentration from the charged amount. (Recovery rate of chloroprene polymer composition) = (actual weight of chloroprene polymer composition) / (theoretical weight of chloroprene polymer composition) × 100

[0164] A composition for forming a dip-molded body containing the above-mentioned latex, i.e., a chloroprene polymer composition, was prepared by the following method, and the composition was dip-molded to obtain a dip-molded body. The dip-molded body was further subjected to a heat-drying treatment to produce a dip-molded product, which was then evaluated.

[0165] Preparation of Dip-Molded Products: 100 parts by mass of the solids content of the chloroprene polymer composition containing each chloroprene polymer was mixed with 7.1 parts by mass of the aqueous dispersion, and water was added to adjust the overall solids concentration of the mixture to 30% by mass. The aqueous dispersion was prepared by mixing 2 parts by mass of two zinc oxide species, 2 parts by mass of a butylated reaction product of p-cresol and dicyclopentadiene (trade name "Nocrac PBK" manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 0.7 parts by mass of the heteroaromatic compound 2-mercaptobenzimidazole (trade name "Nocrac MB" manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 0.1 parts by mass of a sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N" manufactured by Kao Corporation), and 10.7 parts by mass of water in a ceramic ball mill at 20°C for 16 hours. The obtained composition for forming a dip-molded body contained, relative to 100 parts by mass of the solid content of the chloroprene polymer composition, 2 parts by mass of two types of zinc oxide, 2 parts by mass of a butylated reaction product of p-cresol and dicyclopentadiene (trade name "Nocrac PBK", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 0.7 parts by mass of 2-mercaptobenzimidazole (trade name "Nocrac MB", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), which is a heteroaromatic ring compound, 0.1 part by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "Demol N", manufactured by Kao Corporation), and 10.7 parts by mass of water.

[0166] A ceramic cylindrical mold (manufactured by Shinko Co., Ltd.) with an outer diameter of 50 mm was immersed for 1 second in a coagulation solution containing 62 parts by weight of water, 35 parts by weight of potassium nitrate tetrahydrate, and 3 parts by weight of calcium carbonate, and then removed. After drying for 3 minutes, the molded product was immersed for 2 minutes in the dip-molded body composition prepared by the procedure described above. The molded product was then washed with running water at 45°C for 1 minute and dried at 140°C for 1 hour to produce a dip-molded film for evaluation.

[0167] (Film Thickness) The thickness (film thickness) of the dip-molded film for evaluating tensile properties was measured at three points in the center using a test piece thickness gauge (manufactured by Kobunshi Keiki Co., Ltd., product name: ASKER SDA-12), and the smallest thickness was taken as the thickness of the dip-molded film for evaluation. The results are shown in Tables 2 and 3.

[0168] (Measurement of Tensile Properties) Using the dip-molded film for evaluating tensile properties, the modulus at 100% elongation and the tensile strength at break were measured in accordance with JIS K 6251. The results are shown in Tables 2 and 3.

[0169]

[0170]

Claims

1. A method for producing a chloroprene polymer composition, comprising the steps of: The chloroprene polymer composition contains a diene polymer A and a chloroprene polymer B, The diene polymer A and the chloroprene polymer B have different weight average molecular weights, The method for producing a chloroprene polymer composition includes a polymerization step of polymerizing the chloroprene polymer B in the presence of the diene polymer A.

2. 2. The method for producing a chloroprene polymer composition according to claim 1, wherein a difference between a weight average molecular weight of the diene polymer A and a weight average molecular weight of the chloroprene polymer B is 100,000 or more.

3. The method for producing a chloroprene polymer composition according to claim 1 or 2, wherein the diene polymer A has a weight average molecular weight of 5,000 to 80,000.

4. 3. The method for producing a chloroprene polymer composition according to claim 1, wherein in the polymerization step of polymerizing the chloroprene polymer B, a charged amount of the diene polymer A is 5.0 to 60.0 parts by mass relative to 100 parts by mass of a charged amount of a chloroprene monomer or a raw material monomer.

5. 3. The method for producing a chloroprene polymer composition according to claim 1 or 2, wherein the diene polymer A is at least one selected from the group consisting of natural rubber, an isoprene polymer, a butadiene polymer, a styrene-butadiene polymer, a chloroprene polymer, and an acrylonitrile-butadiene polymer.