Chloroprene-based polymer composition, chloroprene-based polymer latex, and dip-molded article
Patent Information
- Application Number
- JP2024511337
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Chloroprene-based polymer compositions used in dip-molded products often experience a deterioration in flexibility over long-term storage, compromising their tensile strength and performance.
A chloroprene-based polymer composition with a weight average molecular weight of 5,000 to 80,000 and a toluene swelling degree of 12.0% or less, combined with specific additives like zinc oxide, a butylation reaction product of p-cresol and dicyclopentadiene, 2-mercaptobenzimidazole, and a sodium salt of β-naphthalenesulfonic acid formalin condensate, is used to create a dip-molded product that maintains excellent tensile strength and flexibility after long-term storage.
The resulting dip-molded products exhibit enhanced tensile strength and flexibility, suitable for applications such as medical gloves, balloons, catheters, and boots, with improved durability and performance over time.
Abstract
Description
Chloroprene polymer composition, chloroprene polymer latex, and dip-molded product
[0001] The present invention relates to a chloroprene polymer composition, a chloroprene polymer latex, and a dip-molded product.
[0002] Chloroprene polymers are known as materials for dip-molded products such as medical surgical gloves, medical examination gloves, industrial gloves, balloons, catheters, and rubber boots.
[0003] Various techniques have been proposed for chloroprene polymer latexes for dip-molded products and dip-molded articles of chloroprene polymers. Patent Document 1 describes a polychloroprene latex with a pH of 7 to 14 that contains 100 parts by mass of modified polychloroprene obtained by copolymerizing chloroprene and methacrylic acid, 90 to 150 parts by mass of water, 1 to 5 parts by mass of an emulsifier, and 0.5 to 2.5 parts by mass of potassium ions, for use in dip-molded products. Patent Document 2, relating to applications for dip-molded products, describes a mercaptan-modified polychloroprene latex obtained by copolymerizing chloroprene and 2,3-dichloro-1,3-butadiene, in which the peak areas (A) at 126.2 to 127.6 ppm, (B) at 122.0 to 126.2 ppm, and (C) at 129.9 to 130.3 ppm in the C-solid-state NMR spectrum of the polychloroprene are within the ranges represented by the following general formula (I): Patent Document 3, relating to applications for dip-molded products, describes a chloroprene polymer latex that contains high-molecular-weight and low-molecular-weight components, thereby achieving both excellent flexibility and mechanical properties in the vulcanized rubber produced by dip molding. Patent Document 4, relating to applications for dip-molded products, describes a chloroprene polymer latex that exhibits excellent flexibility and mechanical properties even under mild vulcanization conditions, obtained by copolymerizing a chloroprene monomer with an isoprene monomer, which is a raw material for isoprene rubber. Patent Document 5 describes a dip-molded product of an isoprene / chloroprene polymer that exhibits excellent flexibility without containing a diphenylguanidine vulcanization accelerator by mixing an isoprene polymer latex with a chloroprene polymer latex. Patent Document 6 describes a dip-molded product that exhibits excellent mechanical properties by mixing a nitrile-butadiene polymer (NBR) latex or an isoprene polymer latex with a chloroprene polymer latex.
[0004]
[0005] Japanese Patent Application Laid-Open No. 2014-114342 International Publication No. 2019 / 009038 Japanese Patent Application Laid-Open No. 2019-143002 International Publication No. 2021-132460 Special Publication No. 2017-508840 Japanese Patent Application Laid-Open No. 2020-189963
[0006] Chloroprene polymer compositions containing chloroprene polymers have been widely used in applications such as gloves, balloons, boots, catheters, etc. Furthermore, particularly in applications such as medical rubber gloves, there has been a growing demand for chloroprene polymer compositions that can give dip-molded products having excellent flexibility and excellent tensile strength at break, similar to dip-molded products obtained using natural rubber or polyisoprene. However, dip-molded products using chloroprene polymer compositions containing conventional chloroprene polymers sometimes show a deterioration in flexibility after long-term storage, making it difficult to achieve both high tensile strength at break and high flexibility after long-term storage.
[0007] The present invention has been made in view of the above circumstances, and provides a chloroprene polymer composition which has excellent tensile strength at break and flexibility and which can give a dip-molded product which is excellent in flexibility even after long-term storage.
[0008] According to the present invention, there is provided a chloroprene polymer composition containing a chloroprene polymer, wherein a peak of a weight average molecular weight of 5,000 to 80,000 is detected when a tetrahydrofuran-soluble portion of the chloroprene polymer composition is measured by gel permeation chromatography, a test dip-molded product of the chloroprene polymer composition has a toluene swelling degree of 12.0 or less, and the test dip-molded product is obtained by molding a test dip-molded product composition by a dip coagulation method, followed by heat drying at 140°C for 60 minutes, The composition for forming a test immersion molded body contains, relative to 100 parts by mass of the solid content of the chloroprene polymer composition, 2 parts by mass of zinc oxide, 2 parts by mass of a butylated reaction product of p-cresol and dicyclopentadiene, 1.0 part by mass of 2-mercaptobenzimidazole, 0.1 part by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate, and water, the amount of the water being adjusted so that the solid content concentration of the composition for forming a test immersion molded body is 30% by mass, and the toluene swelling degree is represented by Formula (1). Formula (1): Toluene swelling degree=1+(W2 / W1-1)(P1 / P2)(1 / r) (In formula (1), W1 represents the mass of the test dip-molded product before it is immersed in toluene, W2 represents the mass of the test dip-molded product after it has been immersed in toluene, P1 represents the specific gravity of the rubber component of the chloroprene polymer composition, P2 represents the specific gravity of toluene, and r represents the mass fraction of the rubber component of the chloroprene polymer composition in the test dip-molded product.) Formula (1): Toluene swelling degree (mass %)=(TB-TA) / TA×100 (In formula (1), TA represents the mass of the test dip-molded product before it is immersed in toluene, TB represents the mass of the test immersion molding after immersing the test immersion molding in toluene.
[0009] The present inventors have conducted extensive studies and have found that, in a chloroprene polymer composition containing a chloroprene polymer, a peak having a weight-average molecular weight of 5,000 to 80,000 is detected, and by adjusting the toluene swelling degree of a test dip-molded product produced under specific conditions to a specific range, a chloroprene polymer composition can be obtained from which a dip-molded product having excellent tensile strength at break and flexibility and excellent flexibility after long-term storage can be obtained, thereby completing the present invention.
[0010] Various embodiments of the present invention will be exemplified below. The embodiments shown below can be combined with each other. [1] A chloroprene polymer composition containing a chloroprene polymer, wherein a peak of a weight average molecular weight of 5,000 to 80,000 is detected when a tetrahydrofuran-soluble portion of the chloroprene polymer composition is measured by gel permeation chromatography, and a test dip-molded product of the chloroprene polymer composition has a toluene swelling degree of 12.0 mass % or less, and the test dip-molded product is obtained by molding a test dip-molded product composition by a dip coagulation method and then subjecting the product to heat drying at 140°C for 60 minutes, The composition for forming an immersion molded body contains, relative to 100 parts by mass of the solid content of the chloroprene polymer composition, 2 parts by mass of zinc oxide, 2 parts by mass of a butylation reaction product of p-cresol and dicyclopentadiene, 1.0 part by mass of 2-mercaptobenzimidazole, 0.1 part by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate, and water, the amount of the water being adjusted so that the solid content concentration of the composition for forming a test immersion molded body is 30% by mass, and the toluene swelling degree is represented by Formula (1): Formula (1): Toluene swelling degree=1+(W2 / W1-1)(P1 / P2)(1 / r) (In formula (1), W1 represents the mass of the test dip-molded article before it is immersed in toluene, W2 represents the mass of the test dip-molded article after it is immersed in toluene, P1 represents the specific gravity of the rubber content of the chloroprene polymer composition, P2 represents the specific gravity of toluene, and r represents the mass fraction of the rubber content of the chloroprene polymer composition in the test dip-molded article.) [2] The chloroprene polymer composition according to [1], wherein a toluene-insoluble content is 50 to 90 mass%.[3] The chloroprene polymer composition according to [1] or [2], comprising chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units, wherein the chloroprene polymer composition contains 8 to 20% by mass of the 2,3-dichloro-1,3-butadiene monomer units relative to 100% by mass in total of the chloroprene monomer units and the 2,3-dichloro-1,3-butadiene monomer units. [4] The chloroprene polymer composition according to any one of [1] to [3], wherein the test dip-molded product has a low-temperature hardness change ΔH1 of 30 or less, and the low-temperature hardness change ΔH1 is expressed as HB1-HA1, where HA1 represents the Shore hardness obtained by stacking the test dip-molded products to a thickness of 6.00±0.20 mm under heat treatment at 70°C for 30 minutes, and measuring the Shore hardness using a durometer type A at 23°C. HB1 represents the Shore hardness obtained by stacking the test dip-molded products to a thickness of 6.00±0.20 mm under heat treatment at 70°C for 30 minutes, storing the test dip-molded products at −10°C for 168 hours, and measuring the Shore hardness using a durometer type A at −10°C. [5] The chloroprene polymer composition according to any one of [1] to [4], wherein the ratio RB / RA of the total amount RB of peak areas of abietic acid, neoabietic acid, palustric acid, levopimaric acid and their salts to the total amount RA of peak areas of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid and their salts is 0.10 or more and 0.70 or less, as obtained by gas chromatography analysis of an extract obtained from the test dip-molded product with an ethanol / toluene azeotropic mixture specified in JIS K 6229. [6] A chloroprene polymer latex comprising the chloroprene polymer composition according to any one of [1] to [5] and water. [7] A dip-molded product of a composition for forming a dip-molded product, comprising the chloroprene polymer latex according to [6]. [8] The dip-molded product according to [7], which is an industrial or general household glove, a medical glove, a balloon, a catheter, or a boot.[9] A dip-molded product according to [7], having a low-temperature hardness change ΔH2 of 30 or less, the low-temperature hardness change ΔH2 being expressed as HB2-HA2, where HA2 represents the Shore hardness measured in an environment of 23°C using a durometer type A after the dip-molded product has been heat-treated under conditions of 70°C and 30 minutes, and the dip-molded product has been stacked to a thickness of 6.00±0.20 mm, and HB2 represents the Shore hardness measured in an environment of -10°C using a durometer type A after the dip-molded product has been heat-treated under conditions of 70°C and 30 minutes and then stored at -10°C for 168 hours, and the dip-molded product has been stacked to a thickness of 6.00±0.20 mm.
[10] A dip-molded product of a composition for forming a dip-molded product containing a chloroprene polymer latex, wherein the dip-molded product has a low-temperature hardness change of 30 or less, and the low-temperature hardness change ΔH2 is expressed as HB2-HA2, where HA2 represents the Shore hardness of the dip-molded product obtained by heat-treating the dip-molded product at 70°C for 30 minutes, stacking the dip-molded product to a thickness of 6.00±0.20 mm, and measuring the Shore hardness using a durometer type A in an environment of 23°C, and HB2 represents the Shore hardness of the dip-molded product obtained by heat-treating the dip-molded product at 70°C for 30 minutes, storing the dip-molded product at -10°C for 168 hours, stacking the dip-molded product to a thickness of 6.00±0.20 mm, and measuring the Shore hardness using a durometer type A in an environment of -10°C, and the dip-molded product meets JIS K The dip-molded product has a tensile strength at break of 18.0 MPa or more and a modulus at 100% elongation of 0.65 MPa or less, as measured in accordance with JIS No. 6251.
[0011] The chloroprene polymer composition containing the chloroprene polymer of the present invention can provide a dip-molded product having excellent tensile strength at break and flexibility, and also having excellent flexibility after long-term storage. Furthermore, the obtained dip-molded product can be used to make various products and components that require excellent tensile strength at break and flexibility after long-term storage, taking advantage of its properties. Specifically, the product can be used as industrial or general household gloves, medical gloves, balloons, catheters, or boots.
[0012] The present invention will be described in detail below by illustrating embodiments of the present invention. The present invention is not limited by these descriptions. The features of the embodiments of the present invention described below can be combined with each other. Furthermore, each feature can be an invention independently.
[0013] 1. Chloroprene Polymer Composition The chloroprene polymer composition according to the present invention contains a chloroprene polymer. Furthermore, when the tetrahydrofuran-soluble portion of the chloroprene polymer composition according to the present invention is subjected to gel permeation chromatography, a peak corresponding to a weight-average molecular weight of 5,000 to 80,000 is detected. Furthermore, a test dip-molded product of the chloroprene polymer composition has a toluene swelling index of 12.0 or less.
[0014] The chloroprene polymer composition according to the present invention contains at least one chloroprene polymer. The chloroprene polymer according to the present invention refers to a polymer containing monomer units derived from 2-chloro-1,3-butadiene (hereinafter also referred to as chloroprene).
[0015] The chloroprene polymer composition according to one embodiment of the present invention may contain a diene polymer A and a chloroprene polymer B. In the present invention, the diene polymer A refers to a polymer containing diene monomer units derived from a diene monomer. As described below, the diene polymer A according to one embodiment of the present invention preferably contains monomer units derived from chloroprene. That is, the chloroprene polymer composition according to one embodiment of the present invention may contain the chloroprene polymer A and the chloroprene polymer B. The diene polymer A and the chloroprene polymer B will be described later.
[0016] When the chloroprene polymer composition according to the present invention is subjected to gel permeation chromatography measurement of a tetrahydrofuran-soluble portion of the chloroprene polymer composition, a peak corresponding to a weight-average molecular weight of 5,000 to 80,000 is detected. More specifically, when the chloroprene polymer composition according to the present invention is mixed with a large amount of methanol, precipitated, filtered, dried, and the resulting polymer is dissolved in tetrahydrofuran, the resulting sample is subjected to gel permeation chromatography measurement, and a peak corresponding to a weight-average molecular weight of 5,000 to 80,000 is detected in the molecular weight distribution.
[0017] In addition, in the chloroprene polymer composition according to one embodiment of the present invention, the chloroprene polymer composition is mixed with a large amount of methanol, precipitated, filtered, and dried. The resulting polymer is dissolved in tetrahydrofuran to obtain a sample, and the sample is subjected to gel permeation chromatography. In the molecular weight distribution obtained, preferably, a peak corresponding to a weight average molecular weight of 5,000 to 80,000 and a peak corresponding to a weight average molecular weight of 200,000 to 1,500,000 are detected, more preferably, a peak corresponding to a weight average molecular weight of 5,000 to 50,000 and a peak corresponding to a weight average molecular weight of 300,000 to 1,500,000 are detected, and even more preferably, a peak corresponding to a weight average molecular weight of 8,000 to 30,000 and a peak corresponding to a weight average molecular weight of 500,000 to 1,500,000 are detected. The chloroprene polymer composition according to one embodiment of the present invention preferably contains a diene polymer A having a weight-average molecular weight of 5,000 to 80,000 and a chloroprene polymer B having a weight-average molecular weight of 200,000 to 1,500,000, or a chloroprene polymer B having a weight-average molecular weight of 5,000 to 80,000 and a diene polymer A having a weight-average molecular weight of 200,000 to 1,500,000. It is more preferable that the polymer B contains a chloroprene polymer B having a weight-average molecular weight of 5,000 to 50,000 and a diene polymer A having a weight-average molecular weight of 300,000 to 1,500,000, and it is even more preferable that the polymer A contains a diene polymer A having a weight-average molecular weight of 8,000 to 30,000 and a chloroprene polymer B having a weight-average molecular weight of 500,000 to 1,500,000, or it is still more preferable that the polymer B contains a chloroprene polymer B having a weight-average molecular weight of 8,000 to 30,000 and a diene polymer A having a weight-average molecular weight of 500,000 to 1,500,000.
[0018] The chloroprene polymer composition according to one embodiment of the present invention preferably contains 5 to 40% by mass of a polymer having a weight-average molecular weight of 5,000 to 80,000, relative to 100% by mass of the polymer contained in the chloroprene polymer composition. The content of the polymer having a weight-average molecular weight of 5,000 to 80,000 may be, for example, 5, 10, 15, 20, 25, 30, 35, or 40% by mass, and may be within a range between any two of the values exemplified here.
[0019] The chloroprene polymer composition according to one embodiment of the present invention preferably contains 60 to 95 mass% of a polymer having a weight-average molecular weight of 200,000 to 1,500,000, relative to 100 mass% of the polymer contained in the chloroprene polymer composition. The content of the polymer having a weight-average molecular weight of 200,000 to 1,500,000 is, for example, 60, 65, 70, 75, 80, 85, 90, or 95 mass%, and may be within a range between any two of the values exemplified here.
[0020] The weight-average molecular weight can be determined, for example, by mixing a chloroprene polymer composition with a large amount of methanol, precipitating, filtering, and drying the resulting chloroprene polymer composition, dissolving the resulting chloroprene polymer composition in tetrahydrofuran, and analyzing the resulting sample using gel permeation chromatography (GPC). The GPC measurement conditions can be as described in the Examples. The weight-average molecular weight can be controlled by adjusting the production conditions, specifically, the polymerization formulation of the diene polymer A and chloroprene polymer B contained in the chloroprene polymer composition, the type and amount of chain transfer agent, the polymerization temperature, the polymerization time, the polymerization conversion rate, etc.
[0021] The chloroprene polymer composition according to one embodiment of the present invention preferably has a toluene-insoluble content of 50 to 90% by mass, more preferably 60 to 85% by mass, and may be, for example, 50, 55, 60, 65, 70, 75, 80, 85, or 90%, or may be within a range between any two of the values exemplified here.
[0022] The toluene-insoluble content can be calculated by the following formula, specifically by the method described in the Examples: Toluene-insoluble content (gel content) = B / A × 100 (%), where Ag is the chloroprene-based polymer composition obtained by freeze-drying a latex containing the chloroprene-based polymer composition, the chloroprene-based polymer composition is immersed in toluene for 16 hours, and the chloroprene-based polymer composition after freeze-drying is taken as Ag and B g is the gel content (insoluble content) separated from the toluene-dissolved mixture.
[0023] The toluene-insoluble content can be controlled by adjusting the production conditions of the chloroprene polymer composition, for example, the polymerization formulation of the polymers (e.g., diene polymer A and chloroprene polymer B) contained in the chloroprene polymer composition, the formulation of the type and amount of the chain transfer agent, the polymerization temperature, the polymerization time, the polymerization conversion rate, etc., and by adjusting the type and amount of the polymers (e.g., diene polymer A and chloroprene polymer B) blended.
[0024] A chloroprene polymer composition according to one embodiment of the present invention preferably contains chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units, and the chloroprene polymer composition preferably contains 8 to 20 mass% of 2,3-dichloro-1,3-butadiene monomer units, and more preferably 10 to 17 mass%, based on 100 mass% of the total of the chloroprene monomer units and the 2,3-dichloro-1,3-butadiene monomer units. The content of the 2,3-dichloro-1,3-butadiene monomer units is, for example, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20 mass%, and may be within a range between any two of the values exemplified here.
[0025] The chloroprene polymer composition according to one embodiment of the present invention may contain 70 to 100% by mass of chloroprene monomer units, based on 100% by mass of the chloroprene polymer composition. The content of the chloroprene monomer units may be, for example, 70, 75, 80, 85, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, or 100% by mass, or may be within a range between any two of the values exemplified here.
[0026] A chloroprene polymer composition according to one embodiment of the present invention may contain 0 to 30% by mass of other monomer units other than chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units, based on 100% by mass of the chloroprene polymer composition. The content of the other monomer units may be, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30, or may be within a range between any two of the values exemplified here. A chloroprene polymer according to one embodiment of the present invention may be composed of chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units.
[0027] When the chloroprene polymer composition is a mixture of two or more different chloroprene polymers, the content of each monomer unit means the total amount of each monomer unit in all chloroprene polymers contained in the chloroprene polymer composition.
[0028] The content of 2,3-dichloro-1,3-butadiene monomer units in the chloroprene polymer composition can be calculated by measuring a test piece of the chloroprene polymer composition obtained by freeze-drying a latex containing the chloroprene polymer composition by pyrolysis gas chromatography, determining the area ratio of the peak derived from chloroprene to the peak derived from 2,3-dichloro-1,3-butadiene, and using a calibration curve of the 2,3-dichloro-1,3-butadiene content. Specifically, the content can be calculated by the method described in the Examples.
[0029] The content of 2,3-dichloro-1,3-butadiene monomer units in the chloroprene polymer composition can be controlled by adjusting the production conditions of the polymer contained in the chloroprene polymer composition, such as the type and amount of raw materials blended and the blend amount of the polymer (e.g., diene polymer A or chloroprene polymer B).
[0030] The chloroprene polymer composition according to the present invention has a toluene swelling degree of 12.0 or less, preferably 10.0 or less, of a test dip-molded article. The toluene swelling degree is expressed by formula (1). Formula (1): Toluene swelling degree=1+(W2 / W1-1)(P1 / P2)(1 / r) In formula (1), W1 represents the mass of the test dip-molded article before immersion in toluene, W2 represents the mass of the test dip-molded article after immersion in toluene, P1 represents the specific gravity of the rubber component of the chloroprene polymer composition, P2 represents the specific gravity of toluene, and r represents the mass fraction of the rubber component of the chloroprene polymer composition in the test dip-molded article. Here, the rubber content of the chloroprene polymer composition refers to the chloroprene polymer content in the latex containing the chloroprene polymer composition, which can be obtained by mixing a latex containing the chloroprene polymer composition with methanol to precipitate, followed by filtration and drying. The specific gravity of the rubber content of the chloroprene polymer composition and the specific gravity of toluene can be measured at 20°C, and P2 can be 0.867. P1 can be the specific gravity of the rubber content of the chloroprene polymer composition measured at 20°C, and P1 can be 1.23.
[0031] The toluene swelling degree of a test dip-molded product of a chloroprene polymer composition is, for example, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, 10.0, 11.0, or 12.0, and may be within a range between any two of the numerical values exemplified herein. The toluene swelling degree of a test dip-molded product of a chloroprene polymer composition is thought to be related to the degree of crosslinking of the chloroprene polymer composition, and it is presumed that the higher the degree of crosslinking, the lower the swelling degree tends to be. The chloroprene polymer composition according to the present invention has a peak detected at a weight-average molecular weight of 5,000 to 80,000, and by controlling the toluene swelling degree of a test dip-molded product produced under specific conditions to 12.0 or less, the chloroprene polymer composition has excellent tensile strength at break and flexibility, and is capable of giving a dip-molded product that exhibits excellent flexibility even after long-term storage.
[0032] The toluene swelling degree can be measured by the method described in Examples. The toluene swelling degree can be adjusted by appropriately selecting a production method for the chloroprene polymer composition. For example, a chloroprene polymer composition having a toluene swelling degree of 12.0 or less can be obtained by a production method including a polymerization step of polymerizing the chloroprene polymer B in the presence of a diene polymer A, as described below.
[0033] In the chloroprene polymer composition according to one embodiment of the present invention, the low-temperature hardness change ΔH1 of a test dip-molded product prepared from the composition for forming a test dip-molded product is preferably 30 or less, and more preferably 20 or less. The low-temperature hardness change ΔH1 is expressed as HB1-HA1. The low-temperature hardness change ΔH1 can be determined by storing the test dip-molded product at -10°C for 168 hours and subtracting the hardness before low-temperature storage from the hardness after low-temperature storage. Specifically, HA1 represents the Shore hardness measured using a durometer type A at 23°C after heat-treating the test dip-molded products (before storing them at -10°C for 168 hours) and then stacking the test dip-molded products to a thickness of 6.00±0.20 mm. HB1 represents the Shore hardness measured in an environment of −10°C using a durometer type A after the test dip-molded specimens were heated at 70°C for 30 minutes (before storing them at −10°C for 168 hours) and then stored at −10°C for 168 hours and then stacked to a thickness of 6.00±0.20 mm.
[0034] The low-temperature hardness change ΔH1 is, for example, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30, and may be within a range between any two of the values exemplified here.
[0035] The low-temperature hardness change ΔH1 can be measured by the method described in the Examples. The heat treatment at 70°C for 30 minutes is intended to melt the crystalline structure contained in the test dip-molded product before storing it at -10°C for 168 hours, and it is believed that the crystalline structure is melted by performing the heat treatment at 70°C for 30 minutes. The low-temperature hardness change ΔH1 can be controlled by adjusting the production conditions of the chloroprene polymer composition.
[0036] In the chloroprene polymer composition according to one embodiment of the present invention, the ratio RB / RA of the total peak area RB of abietic acid, neoabietic acid, palustric acid, levopimaric acid, and their salts to the total peak area RA of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid, and their salts, obtained by gas chromatography analysis of an extract obtained from a test dip-molded product prepared from the composition for forming a test dip-molded product with an ethanol / toluene azeotrope as specified in JIS K 6229, is preferably 0.10 or more and 0.70 or less, more preferably 0.15 or more and 0.50 or less. RB / RA may be, for example, 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, or 0.70, or may be within a range between any two of the values exemplified here.
[0037] RB / RA can be determined by extracting a test immersion molding with an ethanol / toluene azeotropic mixture (ETA solution) specified in JIS K 6229, treating the extract with hydrochloric acid, analyzing the resulting extract by gas chromatography, and calculating the ratio RB / RA ((conjugated resin acid component b) / (non-conjugated resin acid component a)) of the total amount RB of the peak areas of abietic acid, neoabietic acid, palustric acid, levopimaric acid, and their salts to the total amount RA of the peak areas of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid, and their salts. Specifically, it can be determined by the method described in the Examples. RB / RA can be controlled by adjusting the type and amount of emulsifier (particularly rosin acid and its salts) used during emulsion polymerization of the polymer contained in the chloroprene polymer composition.
[0038] In the chloroprene polymer composition according to one embodiment of the present invention, a test dip-molded product prepared from the composition for forming a test dip-molded product has a tensile strength at break of preferably 18.0 MPa or more, more preferably 19.0 MPa or more, and even more preferably 20.0 MPa or more, as measured in accordance with JIS K 6251. The tensile strength at break is, for example, 18.0, 19.0, 20.0, 21.0, 22.0, 23.0, 24.0, 25.0, 26.0, 27.0, 28.0, 29.0, 30.0, 31.0, 32.0, 33.0, 34.0, 35.0, 36.0, 37.0, 38.0, 39.0, or 40.0 MPa, and may be within a range between any two of the values exemplified here.
[0039] In the chloroprene polymer composition according to one embodiment of the present invention, a test dip-molded product prepared from the composition for forming a test dip-molded product preferably has a modulus at 100% elongation of 0.65 MPa or less, more preferably 0.60 MPa or less, as measured in accordance with JIS K 6251. The modulus at 100% elongation may be, for example, 0.30, 0.35, 0.40, 0.45, 0.50, 0.55, 0.60, or 0.65 MPa, or may be within a range between any two of the values exemplified here.
[0040] In the chloroprene polymer composition according to one embodiment of the present invention, a dip-molded article made from a composition for forming dip-molded articles containing the chloroprene polymer composition, particularly a test dip-molded article made from the composition for forming a test dip-molded article, is preferably stored at 23° C. for 6 months and has a modulus at 100% elongation measured according to JIS K 6251 of 0.80 MPa or less, more preferably 0.7 MPa or less. The modulus at 100% elongation is, for example, 0.30, 0.35, 0.40, 0.45, 0.50, 0.55, 0.60, 0.65, 0.70, 0.75, or 0.80 MPa, and may be within a range between any two of the values exemplified here.
[0041] The tensile strength at break, modulus at 100% elongation, and modulus at 100% elongation after 6 months of storage at 23° C. of a dip-molded product containing a chloroprene polymer composition can be controlled by adjusting the weight-average molecular weights of the diene polymer A and chloroprene polymer B contained in the dip-molded product, the types and contents of the monomer units contained therein, the polymerization conditions for each polymer, the blending ratio, etc. The tensile strength at break, modulus at 100% elongation, and modulus at 100% elongation after 6 months of storage at 23° C. can be measured as described in the Examples.
[0042] The test dip-molded product can be obtained by molding the test dip-molded product composition by the dip coagulation method, followed by heating and drying at 140°C for 60 minutes. The test dip-molded product composition contains, relative to 100 parts by mass of the solids content of the chloroprene polymer composition, 2 parts by mass of zinc oxide, 2 parts by mass of a butylated reaction product of p-cresol and dicyclopentadiene, 1.0 part by mass of 2-mercaptobenzimidazole, 0.1 parts by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate, and water, with the amount of water adjusted so that the solids concentration of the test dip-molded product composition is 30% by mass. Specifically, the test dip-molded product can be prepared by the method described in the examples.
[0043] 2. Method for Producing Chloroprene Polymer Composition The method for producing the chloroprene polymer composition according to the present invention is not particularly limited, and the composition can be obtained, for example, by the following method. The method for producing a chloroprene polymer composition according to one embodiment of the present invention may include a polymerization step of polymerizing a chloroprene polymer B in the presence of a diene polymer A. As described above, the chloroprene polymer composition according to the present invention contains a diene polymer A and a chloroprene polymer B, and the diene polymer A and the chloroprene polymer B may have different weight-average molecular weights. First, the diene polymer A and the chloroprene polymer B according to one embodiment of the present invention will be described below.
[0044] 2.1 Diene Polymer A In the present invention, the diene polymer A means a polymer containing diene monomer units derived from a diene monomer. The diene polymer A may contain monomer units derived from a monomer other than the diene monomer, as long as the object of the present invention is not impaired.
[0045] The diene polymer A according to one embodiment of the present invention may contain 50 to 100 mass%, and preferably 70 to 100 mass%, of monomer units derived from a diene monomer, based on 100 mass% of the diene polymer A. The content of the monomer units derived from the diene monomer may be, for example, 50, 55, 60, 65, 70, 75, 80, 85, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, or 100 mass%, or may be within a range between any two of the values exemplified here.
[0046] The diene monomer may be a conjugated diene monomer having 4 to 6 carbon atoms, and specific examples thereof include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, chloroprene, 2,3-dichloro-1,3-butadiene, and 1-chloro-1,3-butadiene. The diene polymer A preferably contains a chloroprene monomer unit.
[0047] The diene polymer A according to one embodiment of the present invention preferably contains at least one selected from natural rubber, an isoprene polymer, a butadiene polymer, a styrene-butadiene polymer, a chloroprene polymer, and an acrylonitrile-butadiene polymer.
[0048] The diene polymer A according to one embodiment of the present invention preferably contains a monomer unit derived from chloroprene, and further preferably contains a monomer unit derived from 2,3-dichloro-1,3-butadiene. The diene polymer A according to one embodiment of the present invention may be one that does not contain sulfur, and the diene polymer A according to one embodiment of the present invention may be one that does not have an -S-S- structure due to sulfur in the main chain.
[0049] The diene polymer A according to one embodiment of the present invention may contain 50 to 100 mass%, and preferably 70 to 100 mass%, of monomer units derived from chloroprene, based on 100 mass% of the diene polymer A. The content of the monomer units derived from chloroprene is, for example, 50, 55, 60, 65, 70, 75, 80, 85, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, or 100 mass%, and may be within a range between any two of the values exemplified here.
[0050] The diene polymer A according to one embodiment of the present invention may contain 0 to 30% by mass of monomer units derived from 2,3-dichloro-1,3-butadiene, relative to 100% by mass of the diene polymer A. The content of the monomer units derived from 2,3-dichloro-1,3-butadiene is, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30% by mass, and may be within a range between any two of the numerical values exemplified here.
[0051] The diene polymer A according to the present invention may have a weight-average molecular weight different from that of the chloroprene polymer B. The difference between the weight-average molecular weight of the diene polymer A according to one embodiment of the present invention and the weight-average molecular weight of the chloroprene polymer B described below is preferably 100,000 or more, more preferably 400,000 or more. The difference between the weight-average molecular weight of the diene polymer A and the weight-average molecular weight of the chloroprene polymer B described below is, for example, 100,000, 200,000, 300,000, 400,000, 500,000, 600,000, 700,000, 800,000, 900,000, 1,000,000, 1,200,000, 1,300,000, 1,400,000, or 1,500,000, and may be within a range between any two of the numerical values exemplified here.
[0052] For example, the weight average molecular weight of the diene polymer A may be smaller than the molecular weight of the chloroprene polymer B. The weight average molecular weight of the diene polymer A may be 5,000 to 80,000. The weight average molecular weight of the diene polymer A may be, for example, 5,000, 6,000, 7,000, 8,000, 9,000, 10,000, 11,000, 12,000, 13,000, 14,000, 15,000, 16,000, 17,000, 18,000, 19,000, 20,000, 21,000, 22,000, 23,000, 24,000, 25,000, 26,000, 27,000, 28,000, 29,000, 30,000, 35,000, 40,000, 50,000, 60,000, 70,000, 80,000, and may be within a range between any two of the numerical values exemplified here.
[0053] As another example, the weight-average molecular weight of the diene polymer A can be larger than the molecular weight of the chloroprene polymer B. The weight-average molecular weight of the diene polymer A can be 200,000 to 1,500,000. The weight-average molecular weight of the diene polymer A is, for example, 200,000, 300,000, 400,000, 500,000, 600,000, 700,000, 800,000, 900,000, 1,000,000, 1,100,000, 1,200,000, 1,300,000, 1,400,000, or 1,500,000, and may be within a range between any two of the numerical values exemplified here.
[0054] The weight-average molecular weight of the diene polymer A can be determined by analyzing a sample obtained by dissolving a diene polymer A in tetrahydrofuran after mixing a polymerization solution containing the diene polymer A, for example, a latex, with a large amount of methanol, precipitating, filtering, and drying the resulting diene polymer A, using gel permeation chromatography (GPC). The GPC measurement conditions can be as described in the Examples. The weight-average molecular weight of the diene polymer A can be controlled by adjusting the polymerization recipe, the type and amount of chain transfer agent, polymerization temperature, polymerization time, polymerization conversion rate, etc., during the polymerization of the diene polymer A, and particularly by adjusting the type and amount of the chain transfer agent.
[0055] 2.2 Method for Producing Diene Polymer A There is no particular limitation on the method for producing the diene polymer A according to the present invention. As an example, the diene polymer A according to one embodiment of the present invention may include a diene polymer A polymerization step of polymerizing raw material monomers including a diene monomer to obtain a diene polymer.
[0056] In the polymerization step, the raw material monomers include one or more diene monomers and may also include other monomers copolymerizable with the diene monomers. Examples of the diene monomers include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, chloroprene, 2,3-dichloro-1,3-butadiene, and 1-chloro-1,3-butadiene. Examples of the other monomers copolymerizable with the diene monomers include styrene, methacrylic acid, acrylonitrile, and sulfur.
[0057] The type and amount of each monomer charged are preferably adjusted so that the content of each monomer unit falls within the above-mentioned numerical range in the resulting diene polymer A. For example, when the diene polymer A contains chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units and contains 0 to 30% by mass of 2,3-dichloro-1,3-butadiene monomer units relative to 100% by mass of the total of the chloroprene monomer and 2,3-dichloro-1,3-butadiene, the amount of 2,3-dichloro-1,3-butadiene charged is preferably in the range of 0 to 30 parts by mass relative to 100 parts by mass of the total of the chloroprene monomer and the 2,3-dichloro-1,3-butadiene monomer.
[0058] When producing the diene polymer A, raw material monomers are polymerized by a polymerization method such as emulsion polymerization, solution polymerization, suspension polymerization, bulk polymerization, etc. Among these polymerization methods, emulsion polymerization is preferred because it has various advantages such as ease of control, ease of extracting the polymer from the polymerization-terminated liquid, and a relatively fast polymerization rate.
[0059] In the polymerization step of the diene polymer A, the raw material monomers can be polymerized by charging them into a polymerization vessel together with a polymerization initiator and necessary agents such as a chain transfer agent and a solvent. As an example, when the diene polymer A is polymerized by emulsion polymerization, the raw material monomers can be polymerized by charging them into a reaction vessel together with a chain transfer agent, water, an alkali (e.g., a metal hydroxide such as potassium hydroxide or sodium hydroxide), an emulsifier (dispersant), a reducing agent (e.g., sodium hydrogen sulfite), a polymerization initiator, etc.
[0060] The polymerization initiator is not particularly limited, and any known polymerization initiator generally used for the polymerization of diene polymers can be used, including potassium persulfate, ammonium persulfate, sodium persulfate, hydrogen peroxide, t-butyl hydroperoxide, and other organic peroxides.
[0061] The type of chain transfer agent used in emulsion polymerization is not particularly limited, and may be any known chain transfer agent generally used in the polymerization of diene polymers, such as long-chain alkyl mercaptans such as n-dodecyl mercaptan and tert-dodecyl mercaptan, dialkyl xanthogen disulfides such as diisopropyl xanthogen disulfide and diethyl xanthogen disulfide, iodoform, etc. As the chain transfer agent, long-chain alkyl mercaptans are preferred, and n-dodecyl mercaptan is more preferred.
[0062] By adjusting the type and amount of the chain transfer agent, the weight average molecular weight of the resulting diene polymer A can be adjusted.
[0063] For example, to obtain a diene polymer A having a weight-average molecular weight of 5,000 to 80,000, the amount of the chain transfer agent charged before the start of emulsion polymerization is preferably 0.5 to 10.0 parts by mass per 100 parts by mass of the monomers. In this case, the amount may be, for example, 0.5, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, or 10.0 parts by mass, or may be within a range between any two of the numerical values exemplified here.
[0064] For example, to obtain a diene polymer A having a weight-average molecular weight of 200,000 or more, preferably 500,000 to 1,500,000, the amount of chain transfer agent charged is preferably 0 parts by mass or more and less than 0.40 parts by mass per 100 parts by mass of monomer. The amount of chain transfer agent charged is more preferably 0.02 to 0.05 parts by mass, and may be, for example, 0, 0.005, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.20, or 0.30 parts by mass, or less than 0.40 parts by mass, or may be within a range between any two of the values exemplified here. In particular, when attempting to obtain a diene polymer A having a weight-average molecular weight of 200,000 or more, the chain transfer agent may not be used.
[0065] In the case of emulsion polymerization, the pH of the aqueous emulsion is preferably 10.5 to 13.5. The aqueous emulsion refers to a mixed solution of a chain transfer agent and a monomer immediately before the start of emulsion polymerization, but also includes cases where the composition changes due to the subsequent addition or divided addition of each component. When the pH of the aqueous emulsion at the start of emulsion polymerization is 10.5 or higher, the polymerization reaction can be controlled more stably. When the pH is 13.5 or lower, excessive viscosity increase during polymerization is suppressed, and the polymerization reaction can be controlled more stably.
[0066] In the polymerization step, the monomers include chloroprene and 2,3-dichloro-1,3-butadiene, and may also include other monomers copolymerizable with chloroprene and 2,3-dichloro-1,3-butadiene. The other monomers are as described above as the monomer units that the chloroprene polymer may contain. The type and amount of each monomer charged are preferably adjusted so that the content of each monomer unit in the resulting chloroprene polymer falls within the above-described numerical range.
[0067] The emulsifier preferably contains rosin acid and / or a rosin acid salt. Examples of rosin acid salts include alkali metal salts such as sodium salts and potassium salts. The amount of rosin acid and rosin acid salt added may be 3.0 to 7.0 parts by mass per 100 parts by mass of the raw material monomer used. The amount of rosin acid and rosin acid salt added may be, for example, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, or 7.0 parts by mass, and may be within a range between any two of the values exemplified here.
[0068] The rosin acid and / or rosin acid salt may contain a conjugated resin acid component and a non-conjugated resin acid component. Examples of the conjugated resin acid component include abietic acid, neoabietic acid, palustric acid, levopimaric acid, and salts thereof. Examples of the non-conjugated resin acid component include dehydroabietic acid, pimaric acid, isopimaric acid, dihydropimaric acid, dihydroabietic acid, and salts thereof.
[0069] The rosin acid and rosin acid salts used in the emulsion polymerization step may have a ratio RB / RA of 0.10 or more and 0.70 or less, where RB is the total peak area of abietic acid, neoabietic acid, palustric acid, levopimaric acid, and their salts relative to RA, the total peak area of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid, and their salts, as determined by gas chromatography analysis of an extract extracted with an ethanol / toluene azeotrope as specified in JIS K 6229. The RB / RA of the rosin acid and rosin acid salt may be, for example, 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, or 0.70, or may be within a range between any two of the values exemplified here. The RB / RA of the dip-molded test specimens of the resulting chloroprene polymer composition can be adjusted by adjusting the type and amount of the rosin acid and / or rosin acid salt.
[0070] The emulsifier may also include emulsifiers and dispersants other than rosin acid and rosin acid salts. Examples of emulsifiers and dispersants other than rosin acid and rosin acid salts include cationic, anionic, and nonionic emulsifiers and dispersants. In one embodiment of the present invention, the emulsifier used in the emulsion polymerization process may include rosin acid and / or rosin acid salts, and an anionic emulsifier or dispersant. As anionic emulsifiers and dispersants, sulfate- or sulfonate-based anionic emulsifiers and dispersants are preferably used in combination to stabilize the chloroprene polymer latex when a pH adjuster is added. Specific examples include alkyl sulfonates having 8 to 20 carbon atoms, alkyl aryl sulfates, condensates of sodium β-naphthalene sulfonate and formaldehyde, and sodium alkyl diphenyl ether disulfonates. The amount of anionic emulsifier or dispersant added may be 0.05 to 5 parts by mass per 100 parts by mass of the raw material monomers. The amount of anionic emulsifier or dispersant added is, for example, 0.05, 0.1, 0.2, 0.3, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, or 5.0 parts by mass relative to 100 parts by mass of the raw material monomer, and may be within a range between any two of the numerical values exemplified here.
[0071] The polymerization temperature is preferably within the range of 5 to 55° C. If it is 5° C. or higher, the emulsion will not freeze, and if it is 55° C. or lower, the diene monomer will not evaporate or boil.
[0072] The polymerization conversion is preferably in the range of 50 to 95%. The polymerization reaction is terminated by adding a polymerization terminator. When the desired polymerization conversion is reached, the polymerization can be controlled by adding a polymerization terminator to terminate the polymerization or by stopping the addition of the polymerization initiator.
[0073] Examples of the polymerization terminator include diethylhydroxylamine, thiodiphenylamine, 4-tert-butylcatechol, and 2,2'-methylenebis-4-methyl-6-tert-butylphenol. In the polymerization step of the diene polymer A according to one embodiment of the present invention, a polymerization terminator may not be used. After completion of the polymerization, unreacted monomers can be removed by a conventional method such as vacuum distillation.
[0074] Furthermore, to a composition (e.g., latex) containing the diene polymer A obtained by the production method of one embodiment of the present invention, a freezing stabilizer, an emulsion stabilizer, a viscosity modifier, an antioxidant, a preservative, and the like can be optionally added after polymerization, within a range that does not impair the effects of the present invention.
[0075] In the polymerization step of the diene polymer A, all of the raw material monomers and chemicals to be used in the polymerization step can be charged into a polymerization vessel before the start of polymerization, and then the polymerization can be started. Alternatively, at least a portion of the raw material monomers and / or chemicals to be used in the polymerization step can be charged into a polymerization vessel before the start of polymerization, and the remainder can be added in portions after the start of polymerization.
[0076] When at least a portion of the raw material monomers and chemicals are charged into a polymerization vessel before the initiation of polymerization, and the remaining raw material monomers and / or chemicals are added after the initiation of polymerization, the remaining raw material monomers and / or chemicals can be added in one or more divided portions, or can be added continuously at a constant flow rate. In one embodiment of the present invention, at least a portion of the raw material monomers can be added in divided portions after the initiation of polymerization. For example, when chloroprene and 2,3-dichloro-1,3-butadiene are used as raw material monomers, a portion of the chloroprene can be added in divided portions after the initiation of polymerization.
[0077] For example, the portionwise addition of the remaining raw material monomers and / or agents can be started when the polymerization rate of the raw material monomers charged before the start of polymerization reaches 50 to 95%. The polymerization rate at which portionwise addition starts can be, for example, 50, 55, 60, 65, 70, 75, 80, 85, 90, or 95%, and may be within a range between any two of the values exemplified here.
[0078] When at least a portion of the raw material monomer is added after the initiation of polymerization, 50 parts by mass or less of 100 parts by mass of all raw material monomers used in the polymerization step can be added after the initiation of polymerization. In this case, the amount of raw material monomer added after the initiation of polymerization can be, for example, 0, 5, 10, 15, 20, 25, 30, 35, 40, 45, or 50 parts by mass, or may be within a range between any two of the values exemplified here. As an example, the raw material monomer, for example, chloroprene, can be added portionwise continuously over a period of 30 to 300 minutes.
[0079] 2.3 Chloroprene Polymer B The chloroprene polymer B according to one embodiment of the present invention contains at least a chloroprene monomer unit and may be a copolymer of chloroprene and another monomer copolymerizable with chloroprene. Examples of the other monomer include 1-chloro-1,3-butadiene, 2,3-dichloro-1,3-butadiene, isoprene, styrene, methacrylic acid, acrylonitrile, and sulfur. Two or more of these may be used in combination as the other monomer. The chloroprene polymer B according to one embodiment of the present invention preferably contains a monomer unit derived from 2,3-dichloro-1,3-butadiene. The chloroprene polymer B according to one embodiment of the present invention may not contain sulfur, and the chloroprene polymer B according to one embodiment of the present invention may not have an —S—S— structure due to sulfur in the main chain.
[0080] The chloroprene polymer B according to one embodiment of the present invention may contain 50 to 100 mass% of chloroprene-derived monomer units, and preferably 70 to 100 mass%, of chloroprene-derived monomer units, relative to 100 mass% of the chloroprene polymer B. The content of the chloroprene-derived monomer units is, for example, 50, 55, 60, 65, 70, 75, 80, 85, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, or 100 mass%, and may be within a range between any two of the values exemplified here.
[0081] Chloroprene polymer B according to one embodiment of the present invention may contain 0 to 30% by mass of monomer units derived from 2,3-dichloro-1,3-butadiene, relative to 100% by mass of chloroprene polymer B. The content of the monomer units derived from 2,3-dichloro-1,3-butadiene is, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30% by mass, and may be within a range between any two of the numerical values exemplified here.
[0082] The chloroprene polymer B according to the present invention may have a weight-average molecular weight different from that of the diene polymer A. As described above, the difference between the weight-average molecular weight of the diene polymer A according to one embodiment of the present invention and the weight-average molecular weight of the chloroprene polymer B described below is preferably 100,000 or more, more preferably 400,000 or more.
[0083] For example, the weight-average molecular weight of the chloroprene polymer B may be larger than that of the diene polymer A. The weight-average molecular weight of the chloroprene polymer B may be 200,000 to 1,500,000. The weight-average molecular weight of the chloroprene polymer B may be, for example, 200,000, 300,000, 400,000, 500,000, 600,000, 700,000, 800,000, 900,000, 1,000,000, 1,100,000, 1,200,000, 1,300,000, 1,400,000, or 1,500,000, or may be within a range between any two of the numerical values exemplified here.
[0084] As another example, the weight-average molecular weight of chloroprene polymer B can be smaller than the molecular weight of chloroprene polymer B. The weight-average molecular weight of chloroprene polymer B can be 5,000 to 80,000. The weight-average molecular weight of chloroprene polymer B can be, for example, 5,000, 6,000, 7,000, 8,000, 9,000, 10,000, 11,000, 12,000, 13,000, 14,000, 15,000, 16,000, 17,000, 18,000, 19,000, 20,000, or 21,000. , 22,000, 23,000, 24,000, 25,000, 26,000, 27,000, 28,000, 29,000, 30,000, 35,000, 40,000, 50,000, 60,000, 70,000, 80,000, and may be within a range between any two of the numerical values exemplified here.
[0085] The weight-average molecular weight of the chloroprene polymer B can be determined by analyzing a sample obtained by dissolving the chloroprene polymer B in tetrahydrofuran using gel permeation chromatography (GPC), after mixing a polymerization solution containing the chloroprene polymer B, for example, a chloroprene polymer composition (latex), with a large amount of methanol, precipitating, filtering, and drying the resulting solution. The GPC measurement conditions can be as described in the Examples. The weight-average molecular weight of the chloroprene polymer B can be controlled by adjusting the polymerization recipe, the type and amount of chain transfer agent, polymerization temperature, polymerization time, polymerization conversion, and the like during the polymerization of the chloroprene polymer B, and particularly by adjusting the type and amount of the chain transfer agent.
[0086] 2.4 Method for Producing Chloroprene Polymer B A method for producing a chloroprene polymer composition according to one embodiment of the present invention may include a polymerization step of polymerizing a chloroprene polymer B in the presence of a diene polymer A. According to one embodiment of the present invention, by polymerizing a chloroprene polymer B in the presence of a diene polymer A, a chloroprene polymer composition can be obtained that has a low modulus at 100% elongation, excellent tensile strength at break, and is capable of producing a dip-molded product that has a low modulus at 100% elongation after storage at 23°C for 6 months.
[0087] The mechanism by which a chloroprene polymer composition can be obtained by polymerizing a chloroprene polymer B in the presence of a diene polymer A, which has a lower modulus at 100% elongation, a better tensile strength at break, and from which a dip-molded article having a low modulus at 100% elongation after storage at 23°C for 6 months can be obtained is not entirely clear. However, it is presumed that the chloroprene polymer composition obtained by polymerizing a chloroprene polymer B in the presence of a diene polymer A has a highly uniform mixture of the diene polymer A and the chloroprene polymer B in the chloroprene polymer composition, compared to a chloroprene polymer composition obtained by polymerizing the diene polymer A and the chloroprene polymer B separately and mixing them after polymerization, and therefore the resulting chloroprene polymer composition and the resulting dip-molded article have superior physical properties.
[0088] The diene polymer A may be added to the polymerization solution in any form. For example, the polymerization solution obtained by polymerizing the diene polymer A may be used as is. As an example, when the diene polymer A is polymerized by emulsion polymerization, a latex containing the diene polymer A may be added to the polymerization solution of the chloroprene polymer B. Alternatively, for example, the diene polymer A may be precipitated from the polymerization solution obtained by polymerizing the diene polymer A, and the precipitated diene polymer A may be added to the polymerization solution of the chloroprene polymer B. As an example, when the diene polymer A is polymerized by emulsion polymerization, the diene polymer A may be precipitated with methanol from the latex containing the diene polymer A and added to the polymerization solution of the chloroprene polymer B, or the diene polymer A obtained by freeze-drying the latex containing the diene polymer A may be added to the polymerization solution of the chloroprene polymer B.
[0089] In the polymerization step of polymerizing the chloroprene polymer B, the amount of the diene polymer A charged can be 5.0 to 60.0 parts by mass, or 40.0 to 95.0 parts by mass, relative to 100 parts by mass of the chloroprene monomer (or raw material monomer). In one embodiment of the present invention, when the weight-average molecular weight of the diene polymer A is smaller than the weight-average molecular weight of the chloroprene polymer B, for example, when the weight-average molecular weight of the diene polymer A is 5,000 to 80,000, the amount of the diene polymer A charged can be 5.0 to 60.0 parts by mass per 100 parts by mass of the chloroprene monomer (or raw material monomer). When the molecular weight of the diene polymer A is larger than the molecular weight of the chloroprene polymer B, for example, when the weight-average molecular weight of the diene polymer A is 200,000 to 1,500,000, the amount of the diene polymer A charged can be 40.0 to 95.0 parts by mass per 100 parts by mass of the chloroprene monomer (or raw material monomer).
[0090] When the weight-average molecular weight of the diene polymer A is smaller than the weight-average molecular weight of the chloroprene polymer B, the amount of the diene polymer A charged per 100 parts by mass of the chloroprene monomer (or raw material monomer) may be, for example, 5.0, 10.0, 15.0, 20.0, 25.0, 30.0, 35.0, 40.0, 50.0, or 60.0 parts by mass, or may be within a range between any two of the numerical values exemplified here. When the molecular weight of the diene polymer A is larger than the molecular weight of the chloroprene polymer B, the amount of the diene polymer A charged relative to 100 parts by mass of the chloroprene monomer (or raw material monomer) is, for example, 40.0, 50.0, 60.0, 65.0, 70.0, 75.0, 80.0, 85.0, 90.0, or 95.0 parts by mass, and may be within a range between any two of the numerical values exemplified here.
[0091] In the polymerization step, the raw material monomers include chloroprene and may also include other monomers copolymerizable with chloroprene, such as 1-chloro-1,3-butadiene, 2,3-dichloro-1,3-butadiene, 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, styrene, methacrylic acid, acrylonitrile, and sulfur.
[0092] The type and amount of each monomer to be charged are preferably adjusted so that the content of each monomer unit in the resulting chloroprene polymer B falls within the above-mentioned range.
[0093] When producing the chloroprene polymer B, raw material monomers are polymerized by a polymerization method such as emulsion polymerization, solution polymerization, suspension polymerization, bulk polymerization, etc. Among these polymerization methods, emulsion polymerization is preferred because it has various advantages such as ease of control, ease of extracting the polymer from the polymerization-terminated liquid, and a relatively high polymerization rate.
[0094] In the polymerization step of the chloroprene polymer B, raw material monomers can be polymerized by charging them into a polymerization vessel together with a polymerization initiator and necessary agents such as a chain transfer agent and a solvent. For example, when the chloroprene polymer B is polymerized by emulsion polymerization, the raw material monomers can be polymerized by charging them into a reaction vessel together with a chain transfer agent, water, an alkali (e.g., a metal hydroxide such as potassium hydroxide or sodium hydroxide), an emulsifier (dispersant), a reducing agent (e.g., sodium hydrogen sulfite), a polymerization initiator, etc.
[0095] The polymerization initiator is not particularly limited, and any known polymerization initiator generally used for polymerization of chloroprene polymers can be used, including potassium persulfate, ammonium persulfate, sodium persulfate, hydrogen peroxide, t-butyl hydroperoxide, and other organic peroxides.
[0096] The type of chain transfer agent used in emulsion polymerization is not particularly limited, and known chain transfer agents generally used in chloroprene polymerization can be used, such as long-chain alkyl mercaptans such as n-dodecyl mercaptan and tert-dodecyl mercaptan, dialkyl xanthogen disulfides such as diisopropyl xanthogen disulfide and diethyl xanthogen disulfide, iodoform, etc. As the chain transfer agent, long-chain alkyl mercaptans are preferred, and n-dodecyl mercaptan is more preferred.
[0097] By adjusting the type and amount of the chain transfer agent, the weight average molecular weight of the resulting chloroprene polymer B can be adjusted.
[0098] For example, to obtain a chloroprene polymer B having a weight-average molecular weight of 200,000 or more, preferably 500,000 to 1,500,000, the amount of chain transfer agent charged is preferably 0 to less than 0.40 parts by mass per 100 parts by mass of monomer. The amount of chain transfer agent charged is more preferably 0 to 0.05 parts by mass, and may be, for example, 0, 0.005, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.20, or 0.30 parts by mass, or less than 0.40 parts by mass, or may be within a range between any two of the values exemplified here. In particular, when attempting to obtain a chloroprene polymer B having a weight-average molecular weight of 200,000 or more, it is not necessary to use a chain transfer agent.
[0099] For example, to obtain a chloroprene polymer B having a weight-average molecular weight of 5,000 to 80,000, the amount of the chain transfer agent charged before the start of emulsion polymerization is preferably 0.5 to 10.0 parts by mass per 100 parts by mass of the monomers. In this case, the amount may be, for example, 0.5, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, or 10.0 parts by mass, or may be within a range between any two of the numerical values exemplified here.
[0100] By adjusting the weight-average molecular weights of the diene polymer A and the chloroprene polymer B to fall within the above-mentioned ranges and controlling the amount of the diene polymer A charged relative to 100 parts by mass of the chloroprene monomer charged to fall within the above-mentioned ranges, a chloroprene polymer composition can be obtained that gives a dip-molded product having a lower modulus at 100% elongation and superior tensile strength at break.
[0101] In the case of emulsion polymerization, the pH of the aqueous emulsion is preferably 10.5 to 13.5. The aqueous emulsion refers to a mixed solution of a chain transfer agent and a monomer immediately before the start of emulsion polymerization, but also includes cases where the composition changes due to the subsequent addition or divided addition of each component. When the pH of the aqueous emulsion at the start of emulsion polymerization is 10.5 or higher, the polymerization reaction can be controlled more stably. When the pH is 13.5 or lower, excessive viscosity increase during polymerization is suppressed, and the polymerization reaction can be controlled more stably.
[0102] In the polymerization step, the monomers include chloroprene and 2,3-dichloro-1,3-butadiene, and may also include other monomers copolymerizable with chloroprene and 2,3-dichloro-1,3-butadiene. The other monomers are as described above as the monomer units that the chloroprene polymer may contain. The type and amount of each monomer charged are preferably adjusted so that the content of each monomer unit in the resulting chloroprene polymer falls within the above-described numerical range.
[0103] The emulsifier preferably contains rosin acid and / or a rosin acid salt. Examples of rosin acid salts include alkali metal salts such as sodium salts and potassium salts. The amount of rosin acid and rosin acid salt added may be 3.0 to 7.0 parts by mass per 100 parts by mass of the raw material monomer used. The amount of rosin acid and rosin acid salt added may be, for example, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, or 7.0 parts by mass, and may be within a range between any two of the values exemplified here.
[0104] The rosin acid and / or rosin acid salt may contain a conjugated resin acid component and a non-conjugated resin acid component. Examples of the conjugated resin acid component include abietic acid, neoabietic acid, palustric acid, levopimaric acid, and salts thereof. Examples of the non-conjugated resin acid component include dehydroabietic acid, pimaric acid, isopimaric acid, dihydropimaric acid, dihydroabietic acid, and salts thereof.
[0105] The rosin acid and rosin acid salts used in the emulsion polymerization step may have a ratio RB / RA of 0.10 or more and 0.70 or less, where RB is the total peak area of abietic acid, neoabietic acid, palustric acid, levopimaric acid, and their salts relative to RA, the total peak area of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid, and their salts, as determined by gas chromatography analysis of an extract extracted with an ethanol / toluene azeotrope as specified in JIS K 6229. The RB / RA of the rosin acid and rosin acid salt may be, for example, 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, or 0.70, or may be within a range between any two of the values exemplified here. The RB / RA of the dip-molded test specimens of the resulting chloroprene polymer composition can be adjusted by adjusting the type and amount of the rosin acid and / or rosin acid salt.
[0106] The emulsifier may also include emulsifiers and dispersants other than rosin acid and rosin acid salts. Examples of emulsifiers and dispersants other than rosin acid and rosin acid salts include cationic, anionic, and nonionic emulsifiers and dispersants. In one embodiment of the present invention, the emulsifier used in the emulsion polymerization process may include rosin acid and / or rosin acid salts, and an anionic emulsifier or dispersant. As anionic emulsifiers and dispersants, sulfate- or sulfonate-based anionic emulsifiers and dispersants are preferably used in combination to stabilize the chloroprene polymer latex when a pH adjuster is added. Specific examples include alkyl sulfonates having 8 to 20 carbon atoms, alkyl aryl sulfates, condensates of sodium β-naphthalene sulfonate and formaldehyde, and sodium alkyl diphenyl ether disulfonates. The amount of anionic emulsifier or dispersant added may be 0.05 to 5 parts by mass per 100 parts by mass of the raw material monomers. The amount of anionic emulsifier or dispersant added is, for example, 0.05, 0.1, 0.2, 0.3, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, or 5.0 parts by mass relative to 100 parts by mass of the raw material monomer, and may be within a range between any two of the numerical values exemplified here.
[0107] The polymerization temperature is preferably within the range of 5 to 55° C. A temperature of 5° C. or higher is preferred because the emulsion does not freeze, and a temperature of 55° C. or lower is preferred because the chloroprene monomer does not evaporate or boil.
[0108] The polymerization conversion rate is preferably in the range of 50 to 95%. The polymerization reaction is terminated by adding a polymerization terminator. When the desired polymerization conversion rate is reached, the polymerization can be terminated by adding a polymerization terminator that terminates the polymerization reaction.
[0109] Examples of the polymerization terminator include diethylhydroxylamine, thiodiphenylamine, 4-tert-butylcatechol, 2,2'-methylenebis-4-methyl-6-tert-butylphenol, etc. After the polymerization is completed, unreacted monomers can be removed by a conventional method such as vacuum distillation.
[0110] Furthermore, to the chloroprene polymer composition (e.g., latex) containing the diene polymer A and the chloroprene polymer B obtained by the production method of one embodiment of the present invention, a freezing stabilizer, an emulsion stabilizer, a viscosity modifier, an antioxidant, a preservative, and the like can be optionally added after polymerization, within a range that does not impair the effects of the present invention.
[0111] In the polymerization step for the chloroprene polymer B, all of the raw material monomers and chemicals to be used in the polymerization step may be charged into a polymerization vessel before the start of polymerization, and then the polymerization may be initiated. Alternatively, at least a portion of the raw material monomers and / or chemicals to be used in the polymerization step may be charged into a polymerization vessel before the start of polymerization, and the remainder may be added in portions after the start of polymerization.
[0112] When at least a portion of the raw material monomers and chemicals are charged into a polymerization vessel before the initiation of polymerization, and the remaining raw material monomers and / or chemicals are added after the initiation of polymerization, the remaining raw material monomers and / or chemicals can be added in one or more divided portions, or can be added continuously at a constant flow rate. In one embodiment of the present invention, at least a portion of the raw material monomers and / or chemicals can be added in divided portions after the initiation of polymerization. For example, a portion of the polymerization initiator can be added in divided portions after the initiation of polymerization.
[0113] 3. Chloroprene Polymer Latex The chloroprene polymer latex according to one embodiment of the present invention may contain a chloroprene polymer composition and water. A latex containing a chloroprene polymer composition containing a diene polymer A and a chloroprene polymer B, obtained after polymerization of the chloroprene polymer B, may be referred to as a chloroprene polymer latex. When the polymer (e.g., the diene polymer A and / or the chloroprene polymer B) contained in the chloroprene polymer composition according to the present invention is obtained by emulsion polymerization, the chloroprene polymer latex may further contain raw materials used in the emulsion polymerization step, such as an emulsifier.
[0114] 4. Dip-molded product (dip-molded coating / film) A dip-molded product according to one embodiment of the present invention can be a dip-molded product made from a composition for forming a dip-molded product, which contains a chloroprene polymer latex.
[0115] A dip-molded product according to one embodiment of the present invention is obtained using the above-described chloroprene polymer composition. The dip-molded product can be obtained by dip-molding the composition for forming a dip-molded product described below, either alone or in a blend with other compositions for forming a dip-molded product. The dip-molded product according to the present invention can be obtained by dip-molding the composition for forming a dip-molded product by a dip coagulation method, followed by heating and drying at 140°C for 1 hour. The dip-molded product according to the present invention has high tensile strength at break, low modulus at 100% elongation, and low modulus at 100% elongation after long-term storage. The dip-molded product according to one embodiment of the present invention can be suitably used as industrial and general household gloves, medical gloves, balloons, catheters, and boots.
[0116] The dip-molded product according to the present invention may contain the components contained in the composition for forming a dip-molded product. The dip-molded product may contain a diene polymer A and a chloroprene polymer B as base polymers, and may contain 70% by mass or more, preferably 80% by mass or more, and more preferably 90% by mass or more of the diene polymer A and the chloroprene polymer B relative to 100% by mass of the dip-molded product. The contents of the diene polymer A and the chloroprene polymer B in the dip-molded product relative to 100% by mass of the dip-molded product may be, for example, 70, 75, 80, 85, 90, 95, 96, 97, 98, 99, or 100% by mass, or may be within a range between any two of the values exemplified here.
[0117] The dip-molded article containing the chloroprene polymer according to the present invention has high tensile strength at break, low modulus at 100% elongation, and low modulus at 100% elongation after long-term storage, regardless of whether a vulcanizing agent and a vulcanization accelerator are added. The dip-molded article according to one embodiment of the present invention may be free of vulcanizing agents and vulcanization accelerators, and may be free of sulfur and vulcanization accelerators such as thiuram, dithiocarbamate, thiourea, guanidine, xanthogenate, and thiazole vulcanization accelerators.
[0118] 4.1 Characteristics of Dip-Molded Product In the dip-molded product according to one embodiment of the present invention, when the soluble fraction obtained by dissolving the dip-molded product in tetrahydrofuran is subjected to gel permeation chromatography, the molecular weight distribution preferably exhibits a peak corresponding to a weight-average molecular weight of 5,000 to 80,000, more preferably a peak corresponding to a weight-average molecular weight of 5,000 to 80,000 and a peak corresponding to a weight-average molecular weight of 200,000 to 1,500,000, more preferably a peak corresponding to a weight-average molecular weight of 5,000 to 50,000 and a peak corresponding to a weight-average molecular weight of 300,000 to 1,500,000, and even more preferably a peak corresponding to a weight-average molecular weight of 8,000 to 30,000 and a peak corresponding to a weight-average molecular weight of 500,000 to 1,500,00. The weight-average molecular weights and blending ratios of the low molecular weight component and the high molecular weight component may be as described above.
[0119] The dip-molded product according to one embodiment of the present invention preferably has a toluene swelling degree of 12.0 or less, more preferably 10.0 or less, and may have a toluene swelling degree of, for example, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, 10.0, 11.0, or 12.0, or may have a value within a range between any two of the values exemplified here.
[0120] The dip-molded product according to one embodiment of the present invention preferably has a low-temperature hardness change ΔH2 of 30 or less, and more preferably 20 or less. The low-temperature hardness change ΔH2 may be, for example, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30, or may be within a range between any two of the values exemplified here. The hardness change ΔH2 is expressed as HB2 - HA2. HA2 represents the Shore hardness measured using a durometer type A in an environment at 23°C after a dip-molded product has been heat-treated at 70°C for 30 minutes, and then stacked to a thickness of 6.00±0.20 mm. HB2 represents the Shore hardness measured using a durometer type A in an environment at -10°C after a dip-molded product has been heat-treated at 70°C for 30 minutes and further stored at -10°C for 168 hours.
[0121] In the dip-molded product according to one embodiment of the present invention, the ratio RB / RA of the total amount RB of peak areas of abietic acid, neoabietic acid, palustric acid, levopimaric acid, and their salts to the total amount RA of peak areas of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid, and their salts, obtained by gas chromatography analysis of an extract extracted with an ethanol / toluene azeotropic mixture as specified in JIS K 6229, is preferably 0.10 or more and 0.70 or less, more preferably 0.15 or more and 0.50 or less. RB / RA is, for example, 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, or 0.70, and may be within a range between any two of the values exemplified here.
[0122] The dip-molded product according to one embodiment of the present invention preferably has a tensile strength at break of 18.0 MPa or more, more preferably 19.0 MPa or more, and even more preferably 20.0 MPa or more, as measured in accordance with JIS K 6251. The tensile strength at break may be, for example, 18.0, 19.0, 20.0, 21.0, 22.0, 23.0, 24.0, 25.0, 26.0, 27.0, 28.0, 29.0, 30.0, 31.0, 32.0, 33.0, 34.0, 35.0, 36.0, 37.0, 38.0, 39.0, or 40.0 MPa, or may be within a range between any two of the values exemplified here.
[0123] The dip-molded product according to one embodiment of the present invention preferably has a modulus at 100% elongation of 0.65 MPa or less, more preferably 0.60 MPa or less, as measured in accordance with JIS K6251 for dip-molded products containing chloroprene polymers. The modulus at 100% elongation may be, for example, 0.30, 0.35, 0.40, 0.45, 0.50, 0.55, 0.60, or 0.65 MPa, or may be within a range between any two of the values exemplified here.
[0124] The dip-molded product according to one embodiment of the present invention preferably has a modulus at 100% elongation of 0.80 MPa or less, more preferably 0.70 MPa or less, measured according to JIS K6251 after storage at 23° C. for 6 months. The modulus at 100% elongation may be, for example, 0.30, 0.35, 0.40, 0.45, 0.50, 0.55, 0.60, 0.65, 0.70, 0.75, 0.80, 0.85, 0.90, 0.95, or 1.00 MPa, or may be within a range between any two of the values exemplified here.
[0125] The weight-average molecular weight, toluene swelling degree, low-temperature hardness change ΔH2, RB / RA, tensile strength at break, modulus at 100% elongation, and modulus at 100% elongation after storage at 23°C for 6 months of the dip-molded product are measured by the methods described above in the section on the chloroprene polymer composition.
[0126] A dip-molded product according to one embodiment of the present invention may have a low-temperature hardness change of 30 or less and a tensile strength at break of 18.0 MPa or more as measured in accordance with JIS K 6251. A dip-molded product according to one embodiment of the present invention may have a low-temperature hardness change of 30 or less, a tensile strength at break of 18.0 MPa or more as measured in accordance with JIS K 6251, and a modulus at 100% elongation of 0.65 MPa or less. Furthermore, a dip-molded product according to one embodiment of the present invention may satisfy the above-mentioned requirements for any two or more, three or more, four or more, five or more, six or more, or all of the weight-average molecular weight, toluene swelling index, low-temperature hardness change ΔH2, RB / RA, tensile strength at break, modulus at 100% elongation, and modulus at 100% elongation after storage at 23°C for six months.
[0127] The dip-molded product according to one embodiment of the present invention contains a chloroprene polymer composition and may further contain an antioxidant and a metal oxide. The dip-molded product may also contain a vulcanizing agent, a vulcanization accelerator, and an antioxidant. The dip-molded product may be produced as described in the Examples.
[0128] The weight-average molecular weight, toluene swelling degree, low-temperature hardness change ΔH2, RB / RA tensile strength at break, modulus at 100% elongation, and modulus at 100% elongation after storage at 23°C for 6 months of the dip-molded product can be controlled by adjusting the production method of the chloroprene polymer composition, for example, the types and amounts of raw materials used in polymerizing the diene polymer A and the chloroprene polymer B, the types and amounts of agents used, and the polymerization conditions.
[0129] 4.2 Shape of the Dip-Molded Product The thickness (e.g., minimum thickness) of the dip-molded product may be 0.01 to 0.50 mm. The thickness of the dip-molded product may be, for example, 0.01, 0.05, 0.10, 0.20, 0.30, 0.40, or 0.50 mm, and may be within a range between any two of the values exemplified here. The thickness of the dip-molded product can be adjusted by the time for immersing the mold in the composition for forming a dip-molded product, the solids concentration of the composition for forming a dip-molded product, and the like. To reduce the thickness of the dip-molded product, the immersion time may be shortened or the solids concentration of the composition for forming a dip-molded product may be reduced.
[0130] The dip-molded product may contain sulfur or a vulcanization accelerator. However, even if the dip-molded product does not contain sulfur or a vulcanization accelerator, it can have mechanical properties equivalent to or superior to those of vulcanized dip-molded products obtained from conventional dip-molded product compositions containing chloroprene polymers. Therefore, the chloroprene polymer composition according to the present invention is suitable as a raw material for the dip-molded product (dip-molded product) of the chloroprene polymer of this embodiment.
[0131] 5. Method for Producing Dip-Molded Product A method for producing a dip-molded product according to one embodiment of the present invention may include: a dip-molding step of dip-molding a composition for forming a dip-molded product, which contains the above-described chloroprene polymer composition, to obtain a dip-molded product; and a drying step of heating and drying the dip-molded product to obtain a dip-molded product.
[0132] 5.1 Composition for Forming Dip-Molded Body The composition for forming a dip-molded body according to one embodiment of the present invention contains the chloroprene polymer composition described above. The composition for forming a dip-molded body according to one embodiment of the present invention may contain, in addition to the chloroprene polymer composition, a metal oxide, an antioxidant, and other necessary chemicals. The composition for forming a dip-molded body according to one embodiment of the present invention may be one that does not contain a vulcanizing agent or a vulcanization accelerator, and may not contain sulfur or a vulcanization accelerator such as a thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthogenate-based, or thiazole-based vulcanization accelerator.
[0133] 5.1.1 Metal Oxide The composition for forming an immersion molded body according to one embodiment of the present invention may contain a metal oxide. There are no particular limitations on the metal oxide, and examples include zinc oxide, lead oxide, trilead tetroxide, magnesium oxide, aluminum oxide, iron oxide, beryllium oxide, and titanium oxide. The metal oxide preferably contains zinc oxide. Zinc oxide is generally believed to function as a scavenger for dechlorinated atoms in chloroprene-based polymers. These metal oxides may be used alone or in combination of two or more.
[0134] The amount of metal oxide added is preferably 0.5 to 15.0 parts by mass per 100 parts by mass of the solids content of the chloroprene polymer composition contained in the composition for forming dip-molded bodies. When the amount of metal oxide added is 0.5 parts by mass or more, the cross-linking effect between polymers is expected to improve the tensile strength at break. When the amount of metal oxide added is 15.0 parts by mass or less, a dip-molded body with excellent flexibility can be obtained. Furthermore, from the viewpoint of the balance of physical properties between the flexibility and tensile strength at break of the obtained dip-molded body, the amount of metal oxide added is more preferably 0.5 to 5.0 parts by mass.
[0135] 5.1.2 Antioxidant The composition for forming a dip-molded body according to one embodiment of the present invention may also contain an antioxidant. The antioxidant is not particularly limited, and phenolic antioxidants, amine-based antioxidants, heat-resistant oxidation (aging) inhibitors, ozone-resistant antioxidants, etc. can be used. When the obtained dip-molded body is used as a medical glove, a phenolic antioxidant can be used from the viewpoint of the color tone, texture, and hygiene of the dip-molded body. In particular, hindered phenolic antioxidants have a strong effect as described above. Examples of hindered phenol-based antioxidants include 2,2'-methylenebis(4-ethyl-6-t-butylphenol), 2,2'-methylenebis(4-methyl-6-t-butylphenol), 4,4'-butylidene(3-methyl-6-t-butylphenol), 4,4'-thiobis(3-methyl-6-t-butylphenol), butylated reaction products of p-cresol and dicyclopentadiene, 2,5'-di-t-butylhydroquinone, and 2,5'-di-t-amylhydroquinone. Among these, butylated reaction products of p-cresol and dicyclopentadiene are desirable from the viewpoint of general dispersibility in aqueous materials. Furthermore, these compounds may be used alone or in combination of two or more.
[0136] The amount of antioxidant added is preferably 0.5 to 10.0 parts by mass per 100 parts by mass of the solids content of the chloroprene polymer composition contained in the composition for forming a dip-molded body. The amount of antioxidant added may be, for example, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, or 10.0 parts by mass, or may be within a range between any two of the values exemplified here. When the amount of antioxidant added is 0.5 parts by mass or more, the effect of suppressing color change in the dip-molded body can be obtained. When the amount of antioxidant added is 10.0 parts by mass or less, the stability of the composition for forming a dip-molded body can be ensured. Furthermore, from the viewpoint of the balance of physical properties between the flexibility and tensile strength at break of the obtained dip-molded body, the amount of antioxidant added is more preferably 0.5 to 5.0 parts by mass.
[0137] 5.1.3 Vulcanizing Agent and Vulcanization Accelerator The composition for forming a dip-molded body according to one embodiment of the present invention may also contain a vulcanizing agent and / or a vulcanization accelerator. Furthermore, the composition for forming a dip-molded body according to one embodiment of the present invention may not contain sulfur or the aforementioned thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthogenate-based, thiazole-based, or other vulcanization accelerators. That is, the composition for forming a dip-molded body includes those containing a vulcanizing agent but not a vulcanization accelerator, those containing a vulcanization accelerator but not a vulcanizing agent, those containing a vulcanization accelerator and a vulcanization accelerator, and those containing neither a vulcanizing agent nor a vulcanization accelerator. Whether or not a vulcanizing agent and a vulcanization accelerator are added may be determined depending on the desired dip-molded body.
[0138] Examples of vulcanizing agents include, but are not limited to, sulfur. The amount of vulcanizing agent added can be 0 to 10.0 parts by mass per 100 parts by mass of the solid content of the chloroprene polymer composition contained in the composition for forming dip-molded bodies. The amount of vulcanizing agent added can be, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 parts by mass, and may be within a range between any two of the values exemplified here.
[0139] A vulcanization accelerator is a chemical added during the vulcanization of raw rubber to act with the vulcanizing agent to increase the vulcanization speed, thereby shortening the vulcanization time, lowering the vulcanization temperature, reducing the amount of vulcanizing agent, and improving the physical properties of the vulcanized rubber. It usually refers to a chemical that accelerates the sulfur vulcanization reaction.
[0140] Examples of vulcanization accelerators include, but are not limited to, thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthogenate-based, thiazole-based, etc. These may be used alone or in combination of two or more types as required.
[0141] Examples of thiuram vulcanization accelerators include tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, tetrakis(2-ethylhexyl)thiuram disulfide, tetramethylthiuram monosulfide, and dipentamethylenethiuram tetrasulfide.
[0142] Examples of the dithiocarbamate vulcanization accelerator include sodium dibutyldithiocarbamate, zinc dimethyldithiocarbamate, zinc diethyldithiocarbamate, zinc N-ethyl-N-phenyldithiocarbamate, zinc N-pentamethylenedithiocarbamate, copper dimethyldithiocarbamate, ferric dimethyldithiocarbamate, and tellurium diethyldithiocarbamate, and zinc dibutyldithiocarbamate is particularly preferred.
[0143] Examples of the thiourea-based vulcanization accelerator include ethylene thiourea, N,N'-diethyl thiourea, trimethyl thiourea, and N,N'-diphenyl thiourea.
[0144] Examples of the guanidine vulcanization accelerator include 1,3-diphenylguanidine, 1,3-di-o-tolylguanidine, 1-o-tolylbiguanide, and di-o-tolylguanidine salts of dicatechol borate.
[0145] Examples of xanthogenate-based vulcanization accelerators include zinc butylxanthogenate and zinc isopropylxanthogenate.
[0146] Examples of the thiazole vulcanization accelerator include 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, 2-mercaptobenzothiazole zinc salt, 2-mercaptobenzothiazole cyclohexylamine salt, and 2-(4'-morpholinodithio)benzothiazole.
[0147] The amount of the vulcanization accelerator added may be 0 to 5.0 parts by mass relative to 100 parts by mass of the solid content of the chloroprene polymer composition contained in the composition for forming a dip-molded body, and may be, for example, 0, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, or 5.0, or may be within a range between any two of the values exemplified here.
[0148] 5.1.4 Other Agents (Heteroaromatic Ring Compounds) The composition for forming a dip-molded body according to one embodiment of the present invention may contain a heteroaromatic ring compound in the chloroprene polymer. The heteroaromatic ring compound contained in the composition for forming a dip-molded body used to obtain a dip-molded body according to one embodiment of the present invention can be represented by chemical formula (1) and has a benzimidazole structure. Note that compounds having this structure may be used as secondary antioxidants, mainly in the formulation of rubber compositions.
[0149]
[0150] In chemical formula (1), X of the mercapto group represents a hydrogen atom or a metal atom. X may be a hydrogen atom and have a thiol group. X may also be a metal atom, and examples of the metal atom include zinc, sodium, copper, nickel, and tellurium, with zinc being preferred. R in chemical formula (1) 1 ~R 4 R represents a hydrogen atom, an alkyl group which may have a substituent, an ether group which may have a substituent, a nitro group, an amino group, or a carboxyl group. 1 ~R 4 may be the same or different. The heteroaromatic ring compounds may be used singly or in combination of two or more.
[0151] Examples of heteroaromatic ring compounds include 2-mercaptobenzimidazole, 5-methyl-2-mercaptobenzimidazole, 4-methyl-2-mercaptobenzimidazole, 5-methoxy-2-mercaptobenzimidazole, 4-methoxy-2-mercaptobenzimidazole, 5-nitro-2-mercaptobenzimidazole, 5-amino-2-mercaptobenzimidazole, 5-carboxy-2-mercaptobenzimidazole, and zinc salts of 2-mercaptobenzimidazole. Among these, 2-mercaptobenzimidazole, 5-methyl-2-mercaptobenzimidazole, 4-methyl-2-mercaptobenzimidazole, 5-methoxy-2-mercaptobenzimidazole, 4-methoxy-2-mercaptobenzimidazole, and zinc salts of 2-mercaptobenzimidazole are preferred.
[0152] The amount of the heteroaromatic ring compound added is preferably 0.2 to 10.0 parts by mass per 100 parts by mass of the solids content of the chloroprene polymer composition contained in the composition for forming dip-molded bodies. The amount of the heteroaromatic ring compound added is, for example, 0.2, 0.3, 0.4, 0.5, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, or 10.0 parts by mass, and may be within a range between any two of the values exemplified here. When the amount added is 0.2 parts by mass or more, the dip-molded product obtained using this composition exhibits very high breaking strength. When the amount added is 10.0 parts by mass or less, the stability of the composition for forming dip-molded bodies is ensured. Furthermore, from the viewpoint of the balance of physical properties between flexibility and breaking strength of the obtained dip-molded product, the amount added is more preferably 0.3 to 5.0 parts by mass.
[0153] A method for producing a composition for forming an immersion molded body according to one embodiment of the present invention may include a raw material mixing step of mixing raw materials containing a chloroprene polymer composition, a metal oxide, an antioxidant, and other required chemicals. In the mixing step, an aqueous dispersion containing the metal oxide, the antioxidant, and other required chemicals may be prepared in advance, and the chloroprene polymer composition and the aqueous dispersion may be mixed. The mixing step may be performed using a known mixing device such as a ball mill.
[0154] 5.2 Dip-molding step A method for producing a dip-molded product according to one embodiment of the present invention may include a dip-molding step of dip-molding a composition for forming a dip-molded product, which contains the chloroprene polymer composition obtained by the above-described method for producing a chloroprene polymer composition, to obtain a dip-molded product.
[0155] Examples of dip molding methods in one embodiment of the present invention include immersion solidification, simple immersion, thermal immersion, and electrodeposition. The immersion solidification method can be used from the viewpoints of ease of production and the ease of obtaining dip-molded bodies of a uniform thickness. Specifically, a ceramic mold coated with a calcium-based coagulation liquid is immersed in a dip-molded body composition, and the dip-molded body composition is solidified. After leaching to remove water-soluble impurities, the composition is dried, and then heated and vulcanized to form a dip-molded film (rubber film), which is then demolded. This allows for the production of a film-like dip-molded body.
[0156] 5.3 Drying Step The method for producing a dip-molded product according to one embodiment of the present invention may include a drying step of heating and drying the dip-molded product to obtain a dip-molded product.
[0157] The heating and drying temperature may be set appropriately depending on the composition of the chloroprene polymer composition, and may be 120 to 180°C. The heating temperature is preferably 120 to 150°C. The heating temperature may be, for example, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, or 220°C, or may be within a range between any two of the values exemplified here. The heating time may be set appropriately depending on the composition of the chloroprene polymer composition, the shape of the unvulcanized molded body, and the like, and may be 10 to 300 minutes. The heating time may be, for example, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, or 300 minutes, or may be within a range between any two of the values exemplified here. As an example, a dip-molded product according to one embodiment of the present invention may be one that has been subjected to a heat drying treatment at 140°C for 1 hour.
[0158] The present invention will be described in more detail below based on examples, but the present invention should not be construed as being limited to these examples.
[0159] <Preparation of Chloroprene-Based Polymer A> (Synthesis Example A-1) To a 30 L polymerization vessel were added 64 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 90 parts by mass of pure water, 4.5 parts by mass of conjugated resin acid-based rosin acid (trade name "Harthall R-WW", manufactured by Harima Chemicals Co., Ltd.), 3.4 parts by mass of n-dodecyl mercaptan, 1.6 parts by mass of potassium hydroxide, 0.5 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N", manufactured by Kao Corporation), and 0.5 parts by mass of sodium hydrogen sulfite. Polymerization was carried out at a polymerization temperature of 35°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous solution of potassium persulfate as a polymerization initiator. When the polymerization rate of the charged monomers reached 80%, 27 parts by mass of chloroprene (monomer) was continuously added over 100 minutes. When the conversion of the initially charged monomer and the continuously added monomer reached 91%, the addition of the aqueous potassium persulfate solution was stopped to terminate the polymerization, yielding a polymerization solution. The polymerization solution was distilled under reduced pressure to remove unreacted monomer, and the resulting solution was concentrated to yield a latex of chloroprene polymer A-1 with a solids concentration of 60% by mass. A portion of the obtained latex was used to precipitate chloroprene polymer A-1 by the method described below, which was then analyzed and used to prepare chloroprene polymer B in Examples 1, 2, and 8.
[0160] (Precipitation of Chloroprene Polymer A with Methanol) The obtained latex of chloroprene polymer A-1 was mixed with a large amount of methanol to precipitate a rubber component (chloroprene polymer A-1), which was then filtered and dried to obtain a sample of chloroprene polymer A-1, which was also used to prepare chloroprene polymer B in Examples 1, 2, and 8 described below.
[0161] Synthesis Example A-2 Polymerization was carried out in the same manner as in Synthesis Example A-1, except that the amount of n-dodecyl mercaptan used in Synthesis Example A-1 was changed to 5.3 parts by mass. The resulting polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a latex of chloroprene polymer A-2 with a solids concentration of 60% by mass. From the resulting latex, chloroprene polymer A-2 was precipitated in the same manner as in Synthesis Example A-1, and this was used in the production of chloroprene polymer B in Example 3.
[0162] Synthesis Example A-3 Polymerization was carried out in the same manner as in Synthesis Example A-1, except that the amount of n-dodecyl mercaptan used in Synthesis Example A-1 was changed to 2.4 parts by mass. The resulting polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a latex of chloroprene polymer A-3 with a solids concentration of 60% by mass. From the resulting latex, chloroprene polymer A-3 was precipitated in the same manner as in Synthesis Example A-1, and this was used in the production of chloroprene polymer B in Example 4.
[0163] Synthesis Example A-4 Polymerization was carried out in the same manner as in Synthesis Example A-1, except that the amount of n-dodecyl mercaptan used in Synthesis Example A-1 was changed to 1.5 parts by mass. The resulting polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a latex of chloroprene polymer A-4 with a solids concentration of 60% by mass. From the resulting latex, chloroprene polymer A-4 was precipitated in the same manner as in Synthesis Example A-1, and this was used in the production of chloroprene polymer B in Example 5.
[0164] Synthesis Example A-5 Polymerization was carried out in the same manner as in Synthesis Example A-1, except that the amounts of chloroprene (monomer) and 2,3-dichloro-1,3-butadiene charged at the beginning of the polymerization were 70 parts by mass, 0 parts by mass, and 30 parts by mass of chloroprene (monomer) continuously added during the polymerization. The resulting polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a latex of chloroprene polymer A-5 with a solids concentration of 60% by mass. Chloroprene polymer A-5 was precipitated from the resulting latex in the same manner as in Synthesis Example A-1, and used to produce chloroprene polymer B in Example 6.
[0165] Synthesis Example A-6 To a 30 L polymerization vessel were added 64 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 77 parts by mass of pure water, 17.6 parts by mass of a gum rosin-based disproportionated rosin aqueous solution (trade name "LONDIS K-25", solids content 25% by mass, manufactured by Arakawa Chemical Industries, Ltd.), 3.4 parts by mass of n-dodecyl mercaptan, 0.8 parts by mass of potassium hydroxide, 0.5 parts by mass of a sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), and 0.5 parts by mass of sodium hydrogen sulfite. Polymerization was carried out at a polymerization temperature of 35°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous potassium persulfate solution as a polymerization initiator. When the polymerization rate of the charged monomers reached 80%, 27 parts by mass of chloroprene (monomer) was continuously added over 100 minutes. When the conversion of the initially charged monomer and the continuously added monomer reached 91%, the addition of the aqueous potassium persulfate solution was stopped to terminate the polymerization, yielding a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomer, and the resulting mixture was concentrated to yield a latex of chloroprene polymer A-6 with a solids concentration of 60% by mass. The resulting latex was subjected to precipitation of chloroprene polymer A-6 in the same manner as in Synthesis Example A-1, and this was used to produce chloroprene polymer B in Example 7.
[0166] Preparation of Chloroprene Polymer B and Chloroprene Polymer Composition Example 1 A 30 L polymerization vessel was charged with 21.3 parts by mass of the chloroprene polymer A-1 prepared and precipitated in Synthesis Example A-1, 85 parts by mass of chloroprene (monomer), 15 parts by mass of 2,3-dichloro-1,3-butadiene, 100 parts by mass of pure water, 5.5 parts by mass of conjugated resin acid-based rosin acid (trade name "Harthall R-WW" manufactured by Harima Chemicals Co., Ltd.), 2 parts by mass of potassium hydroxide, 0.5 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N" manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogensulfite, and 0.03 parts by mass of thiourea dioxide. Polymerization was carried out at a polymerization temperature of 13°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous solution of potassium persulfate as a polymerization initiator. When the polymerization rate reached 85%, 0.1 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization, yielding a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and the resulting mixture was concentrated to yield a chloroprene polymer composition having a solids concentration of 60% by mass and containing chloroprene polymer B-1.
[0167] 50 ml of the chloroprene polymer latex was sampled, and the remaining chloroprene polymer latex was used to prepare a dip-molded test specimen.
[0168] The sampled chloroprene polymer latex was mixed with a large amount of methanol to precipitate the rubber component, which was then filtered and dried to obtain a sample of a chloroprene polymer composition. The weight-average molecular weight of the chloroprene polymer composition was measured from the obtained sample. Furthermore, the 2,3-dichloro-1,3-butadiene content and toluene-insoluble content of the chloroprene polymer composition obtained by freeze-drying the chloroprene polymer latex were measured. The analysis results are shown in Table 1. The measurement method will be described later. When the weight-average molecular weight of the chloroprene polymer composition of Example 1 was measured, a peak derived from chloroprene polymer A having a weight-average molecular weight of 5,000 to 80,000 and a peak derived from chloroprene polymer B having a weight-average molecular weight of 200,000 to 1,500,000 were confirmed.
[0169] Example 2 Polymerization was carried out in the same manner as in Example 1, except that the amounts of chloroprene (monomer) and 2,3-dichloro-1,3-butadiene were changed to 91 parts by mass and 9 parts by mass, respectively. The obtained polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a chloroprene polymer composition containing chloroprene polymer B-2 and having a solids concentration of 60% by mass. Using the obtained latex, a dip-molded test specimen was prepared in the same manner as in Example 1. Furthermore, the weight-average molecular weight, 2,3-dichloro-1,3-butadiene content, and toluene-insoluble matter of the chloroprene polymer composition were measured in the same manner as in Example 1. The analytical results are shown in Table 1.
[0170] Example 3 To a 30 L polymerization vessel were added 21.3 parts by mass of the chloroprene polymer A-2 prepared and precipitated in Synthesis Example A-2, 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 100 parts by mass of pure water, 5.5 parts by mass of a conjugated resin acid-based rosin acid (trade name "Harthall R-WW" manufactured by Harima Chemicals Co., Ltd.), 2 parts by mass of potassium hydroxide, 0.5 parts by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "Demol N" manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogen sulfite, and 0.03 parts by mass of thiourea dioxide. Polymerization was carried out at a polymerization temperature of 13°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous solution of potassium persulfate as a polymerization initiator. When the conversion rate reached 85%, 0.1 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization, thereby obtaining a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and the resulting mixture was concentrated to obtain a chloroprene polymer composition containing chloroprene polymer B-2 and having a solids concentration of 60% by mass. Using the obtained latex, a dip-molded test article was prepared in the same manner as in Example 1. Furthermore, the weight-average molecular weight, 2,3-dichloro-1,3-butadiene content, and toluene-insoluble matter of the chloroprene polymer composition were measured in the same manner as in Example 1. The analytical results are shown in Table 1.
[0171] Example 4 Polymerization was carried out in the same manner as in Example 3, except that chloroprene polymer A-3 was used instead of chloroprene polymer A-2 in Example 3. The obtained polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a chloroprene polymer composition containing chloroprene polymer B-4 and having a solids concentration of 60% by mass. Using the obtained latex, a dip-molded test article was prepared in the same manner as in Example 1. Furthermore, the weight-average molecular weight, 2,3-dichloro-1,3-butadiene content, and toluene-insoluble matter of the chloroprene polymer composition were measured in the same manner as in Example 1. The analytical results are shown in Table 1.
[0172] Example 5 Polymerization was carried out in the same manner as in Example 3, except that chloroprene polymer A-4 was used instead of chloroprene polymer A-2 in Example 3. The obtained polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a chloroprene polymer composition containing chloroprene polymer B-5 and having a solids concentration of 60% by mass. Using the obtained latex, a dip-molded test article was prepared in the same manner as in Example 1. Furthermore, the weight-average molecular weight, 2,3-dichloro-1,3-butadiene content, and toluene-insoluble matter of the chloroprene polymer composition were measured in the same manner as in Example 1. The analytical results are shown in Table 1.
[0173] Example 6 Polymerization was carried out in the same manner as in Example 3, except that chloroprene polymer A-5 was used instead of chloroprene polymer A-2 in Example 3. The obtained polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a chloroprene polymer composition containing chloroprene polymer B-6 and having a solids concentration of 60% by mass. Using the obtained latex, a dip-molded test article was prepared in the same manner as in Example 1. Furthermore, the weight-average molecular weight, 2,3-dichloro-1,3-butadiene content, and toluene-insoluble matter of the chloroprene polymer composition were measured in the same manner as in Example 1. The analytical results are shown in Table 1.
[0174] Example 7 A 30 L polymerization vessel was charged with 21.3 parts by mass of the chloroprene polymer A-6 prepared and precipitated in Synthesis Example A-6, 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 87 parts by mass of pure water, 17.6 parts by mass of a gum rosin-based disproportionated rosin aqueous solution (trade name "LONDIS K-25", solids content 25% by mass, manufactured by Arakawa Chemical Industries, Ltd.), 0.8 parts by mass of potassium hydroxide, 0.5 parts by mass of a sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogensulfite, and 0.03 parts by mass of thiourea dioxide. Polymerization was carried out at a polymerization temperature of 13°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous potassium persulfate solution as a polymerization initiator. When the polymerization rate reached 85%, 0.1 parts by mass of diethylhydroxylamine, a polymerization terminator, was added to terminate the polymerization, yielding a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a chloroprene polymer composition containing chloroprene polymer B-7 and having a solids concentration of 60% by mass. Using the obtained latex, a dip-molded test specimen was prepared in the same manner as in Example 1. Furthermore, the weight-average molecular weight, 2,3-dichloro-1,3-butadiene content, and toluene-insoluble matter of the chloroprene polymer composition were measured in the same manner as in Example 1. The analytical results are shown in Table 1.
[0175] Example 8 A 30 L polymerization vessel was charged with 45.8 parts by mass of the chloroprene polymer A-1 prepared and precipitated in Synthesis Example A-1, 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 120 parts by mass of pure water, 6.5 parts by mass of conjugated resin acid-based rosin acid (trade name "Harthall R-WW" manufactured by Harima Chemicals Co., Ltd.), 2.4 parts by mass of potassium hydroxide, 0.6 parts by mass of a sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N" manufactured by Kao Corporation), 0.6 parts by mass of sodium hydrogensulfite, and 0.03 parts by mass of thiourea dioxide. Polymerization was carried out at a polymerization temperature of 13°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous solution of potassium persulfate as a polymerization initiator. When the polymerization rate reached 85%, 0.1 parts by mass of diethylhydroxylamine, a polymerization terminator, was added to terminate the polymerization, yielding a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a chloroprene polymer composition containing chloroprene polymer B-8 and having a solids concentration of 60% by mass. Using the obtained latex, a dip-molded test specimen was prepared in the same manner as in Example 1. Furthermore, the weight-average molecular weight, 2,3-dichloro-1,3-butadiene content, and toluene-insoluble content of the chloroprene polymer composition were measured in the same manner as in Example 1. The analytical results are shown in Table 1.
[0176] Comparative Example 1 To a 30 L polymerization vessel were added 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 100 parts by mass of pure water, 4.5 parts by mass of conjugated resin acid-based rosin acid (trade name "Harthall R-WW" manufactured by Harima Chemicals Co., Ltd.), 0.02 parts by mass of n-dodecyl mercaptan, 1.6 parts by mass of potassium hydroxide, 0.5 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N" manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogen sulfite, and 0.03 parts by mass of thiourea dioxide. Polymerization was carried out at a polymerization temperature of 13°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous solution of potassium persulfate as a polymerization initiator. When the polymerization rate reached 85%, 0.1 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization, yielding a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and the resulting mixture was concentrated to obtain a chloroprene polymer composition containing chloroprene polymer C and having a solids concentration of 60% by mass. The resulting chloroprene polymer composition was used to prepare a dip-molded test article. The weight-average molecular weight, 2,3-dichloro-1,3-butadiene content, and toluene-insoluble matter of the chloroprene polymer composition were measured in the same manner as in Example 1. The analytical results are shown in Table 1. A portion of the resulting chloroprene polymer composition was used in Comparative Example 2.
[0177] Comparative Example 2 Polymerization was carried out in the same manner as in Synthesis Example A-1. The obtained polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a chloroprene polymer composition containing chloroprene polymer D and having a solid content of 60% by mass.
[0178] The chloroprene polymer composition of chloroprene polymer C obtained in Comparative Example 1 and the chloroprene polymer composition of chloroprene polymer D were mixed in a mass ratio of C / D = 80 / 20 to obtain a chloroprene polymer composition of chloroprene polymer E. Using the obtained chloroprene polymer composition, a dip-molded product for testing was produced.
[0179] Comparative Example 3 To a 30 L polymerization vessel were added 85 parts by mass of the chloroprene polymer A-1 prepared and precipitated in Synthesis Example A-1, 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 150 parts by mass of pure water, 8.5 parts by mass of conjugated resin acid-based rosin acid (trade name "Harthall R-WW" manufactured by Harima Chemicals Co., Ltd.), 3 parts by mass of potassium hydroxide, 0.7 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N" manufactured by Kao Corporation), 0.7 parts by mass of sodium hydrogen sulfite, and 0.03 parts by mass of thiourea dioxide. Polymerization was carried out at a polymerization temperature of 13°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous solution of potassium persulfate as a polymerization initiator. When the conversion reached 85%, 0.1 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization, yielding a polymerization solution. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and the resulting mixture was concentrated to obtain a chloroprene polymer composition containing chloroprene polymer B-9 and having a solids concentration of 60% by mass. Using the obtained latex, a dip-molded test article was prepared in the same manner as in Example 1. Furthermore, the weight-average molecular weight, 2,3-dichloro-1,3-butadiene content, and toluene-insoluble matter of the chloroprene polymer composition were measured in the same manner as in Example 1. The analytical results are shown in Table 1.
[0180] The chloroprene polymer compositions were analyzed by the following method. <Measurement of Weight-Average Molecular Weight of Chloroprene Polymer Composition> The weight-average molecular weight was measured by gel permeation chromatography (GPC) under the following measurement conditions using a sample obtained by precipitating each chloroprene polymer composition with methanol, filtering, drying the polymer, and dissolving it in 20 ml of tetrahydrofuran, as described above. Apparatus: HLC-8320 (manufactured by Tosoh Corporation) Column: Three TSKgel GMHHR-H columns in series Temperature: 40°C Detection: Differential refractive index Solvent: Tetrahydrofuran Calibration curve: Prepared using standard polystyrene (PS).
[0181] <Measurement of 2,3-dichloro-1,3-butadiene Content in Chloroprene Polymer Composition> The chloroprene polymer composition obtained by freeze-drying a latex containing the chloroprene polymer composition was cut into a 0.05 mg test piece and measured by pyrolysis gas chromatography to determine the area ratio of the peak derived from chloroprene to the peak derived from 2,3-dichloro-1,3-butadiene. Using a calibration curve of the area ratio of the peak derived from chloroprene to the peak derived from 2,3-dichloro-1,3-butadiene and the 2,3-dichloro-1,3-butadiene content, the content (mass%) of 2,3-dichloro-1,3-butadiene monomer units relative to 100 mass% of the total of chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units was determined.
[0182] [Conditions for pyrolysis gas chromatography measurement] Device name: HP5890-II Column: DB-5 0.25 mmφ×30 m (film thickness 1.0 μm) Column temperature: 50°C (5 min) → 10°C / min → 150°C → 25°C / min → 300°C Injection port temperature: 250°C Detector temperature: 280°C Detector: FID
[0183] <Toluene-insoluble content> A chloroprene polymer composition obtained by freeze-drying a latex containing the chloroprene polymer composition was cut into 2 mm squares to obtain a test piece. The test piece was placed in a conical beaker and dissolved in 80 g of toluene for 16 hours. Subsequently, after centrifugation, the gel content (insoluble content) was separated using a 200-mesh wire netting. The gel content was then dried and the mass of the dried product was measured. The toluene-insoluble content in the chloroprene polymer composition was calculated using the following formula, where Ag is the chloroprene polymer composition after freeze-drying and B g is the gel content (insoluble content) separated from the mixture dissolved in toluene. Toluene-insoluble content (gel content) = B / A × 100 (%)
[0184] A composition for forming a test dip-molded body was prepared using the above-mentioned latex, i.e., a latex containing a chloroprene-based polymer composition, by the following method, and the composition was dip-molded to obtain a dip-molded body. The dip-molded body was further subjected to a heat drying treatment to prepare a test dip-molded body, which was then evaluated.
[0185] Preparation of Dip-Molded Articles: 100 parts by mass of the solids content of each chloroprene polymer composition was mixed with an aqueous dispersion, and water was added to adjust the overall solids concentration of the mixture to 30% by mass to prepare a test composition for forming a dip-molded article. The aqueous dispersion was prepared by mixing 2 parts by mass of two zinc oxides, 2 parts by mass of a butylated reaction product of p-cresol and dicyclopentadiene (trade name "Nocrac PBK" manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 1.0 part by mass of the heteroaromatic compound 2-mercaptobenzimidazole (trade name "Nocrac MB" manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 0.1 part by mass of a sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N" manufactured by Kao Corporation), and 10.7 parts by mass of water in a ceramic ball mill at 20°C for 16 hours. The obtained composition for forming a test dip-molded body contained, relative to 100 parts by mass of the solids content of the chloroprene polymer composition, 2 parts by mass of two types of zinc oxide, 2 parts by mass of a butylated reaction product of p-cresol and dicyclopentadiene (trade name "Nocrac PBK", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 1.0 part by mass of 2-mercaptobenzimidazole (trade name "Nocrac MB", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), which is a heteroaromatic ring compound, 0.1 part by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "Demol N", manufactured by Kao Corporation), and water.
[0186] A ceramic cylindrical mold (manufactured by Shinko Co., Ltd.) with an outer diameter of 50 mm was immersed for 1 second in a coagulation solution containing 62 parts by weight of water, 35 parts by weight of potassium nitrate tetrahydrate, and 3 parts by weight of calcium carbonate, and then removed. After drying for 3 minutes, the molded product was immersed for 2 minutes in the dip-molded body composition prepared by the procedure described above. The molded product was then washed with running water at 45°C for 1 minute and dried at 140°C for 1 hour to produce a dip-molded body film for testing.
[0187] (Film Thickness) Using a test piece thickness gauge (manufactured by Kobunshi Keiki Co., Ltd., product name: ASKER SDA-12), the thickness (film thickness) of the dip-molded film for evaluation of tensile properties was measured at three points in the center, and the minimum thickness was taken as the thickness of the dip-molded film for test. The results are shown in Table 2.
[0188] (Measurement of Tensile Properties) Using dip-molded test films for evaluating tensile properties, the modulus at 100% elongation and the tensile strength at break were measured in accordance with JIS K 6251. The dip-molded test compositions of each Example and Comparative Example were stored at 23°C for 6 months, and the modulus at 100% elongation was measured in accordance with JIS K 6251. The results are shown in Table 1.
[0189] (Toluene Swelling Degree) The dip-molded test article was cut into a 10 mm x 15 mm piece to obtain a test piece. The mass W1 of the obtained test piece before immersion was measured, and the test piece was then immersed in toluene in an environment of 23°C for 20 hours. After immersion, the test piece was removed from the toluene, the toluene on the film surface was wiped off, and the mass W2 after immersion was measured. The toluene swelling degree was calculated from the measured mass W1 before immersion and mass W2 after immersion using the following formula. The results are shown in Table 1. Toluene swelling degree = 1 + (W2 / W1 - 1) (P1 / P2) (1 / r), where P1 is the specific gravity of the rubber component of the chloroprene polymer composition, P2 is the specific gravity of toluene, and r is the mass fraction of the rubber component of the chloroprene polymer composition in the dip-molded article. The calculation was performed assuming P1 to be 1.23 and P2 to be 0.867. The rubber content of the chloroprene polymer composition refers to the chloroprene polymer in the latex containing the chloroprene polymer composition, which can be obtained by mixing the latex containing the chloroprene polymer composition according to the Examples and Comparative Examples with methanol to cause precipitation, followed by filtration and drying. The specific gravity of the rubber content of the chloroprene polymer composition was calculated by measuring the density of the rubber content of the chloroprene polymer composition obtained by the above method at room temperature (20°C).
[0190] (Low-Temperature Hardness Change) The test dip-molded specimens were stored at −10° C. for 168 hours, and the low-temperature hardness change was calculated from the hardness of the test dip-molded specimens before and after storage using formula (2). The results are shown in Table 1. Equation (2): ΔH = HB - HA In equation (2), HA represents the Shore hardness measured using a durometer type A in an environment of 23°C after the test dip-molded specimens before storage at -10°C for 168 hours were heated at 70°C for 30 minutes, and then stacked to a thickness of 6.00 ± 0.20 mm, and HB represents the Shore hardness measured using a durometer type A in an environment of -10°C after the test dip-molded specimens before storage at -10°C for 168 hours were heated at 70°C for 30 minutes and further stored at -10°C for 168 hours, and then stacked to a thickness of 6.00 ± 0.20 mm. For example, when the thickness of the test dip-molded specimen was 0.20 mm, 30 specimens were stacked and the hardness was measured.
[0191] (The ratio RB / RA of the total peak area RB of abietic acid, neoabietic acid, palustric acid, levopimaric acid, and their salts to the total peak area RA of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid, and their salts.) 3 g of the above-mentioned immersion-molded test specimen was cut into 2 mm square pieces to obtain test specimens. The test specimens were placed in an eggplant-shaped flask equipped with a condenser, extracted with an ethanol / toluene azeotropic mixture (ETA solution) specified in JIS K 6229, and then treated with hydrochloric acid. Gas chromatography was performed under the following conditions using the extract. From the gas chromatography measurement results, the total peak area RA of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid, and their salts was determined. In addition, the total amount RB of the peak areas of abietic acid, neoabietic acid, palustric acid, levopimaric acid, and their salts was determined, and the ratio RB / RA ((conjugated resin acid component b) / (non-conjugated resin acid component a)) of the total amount RB of the peak areas of abietic acid, neoabietic acid, palustric acid, levopimaric acid, and their salts to the total amount RA of the peak areas of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid, and their salts in the test dip-molded product was calculated.
[0192] [Gas chromatography measurement conditions] Column used: FFAP 0.32 mmφ×25 m (film thickness 0.3 μm) Detector: FID Column temperature: 200° C. (hold for 90 min) → 250° C. Heating rate: 10° C. / min Injection port temperature: 270° C. Detector temperature: 270° C. Injection volume: 2 μL
[0193]
Claims
1. A chloroprene-based polymer composition comprising a chloroprene-based polymer, When the tetrahydrofuran-soluble portion of the chloroprene polymer composition was subjected to gel permeation chromatography, a peak having a weight average molecular weight of 5,000 to 80,000 was detected. The chloroprene polymer composition has a toluene swelling degree of 12.0 or less for a test dip-molded product, The test dip-molded product was obtained by molding a test dip-molded product-forming composition by a dip-solidification method, followed by heat-drying at 140° C. for 60 minutes, the composition for forming a test immersion molding contains, relative to 100 parts by mass of a solid content of the chloroprene polymer composition, 2 parts by mass of zinc oxide, 2 parts by mass of a butylated reaction product of p-cresol and dicyclopentadiene, 1.0 part by mass of 2-mercaptobenzimidazole, 0.1 part by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate, and water, the amount of the water being adjusted so that the solid content concentration of the composition for forming a test immersion molding is 30% by mass, The toluene swelling degree is represented by the formula (1). Formula (1): Toluene swelling degree = 1 + (W2 / W1-1) (P1 / P2) (1 / r) (In formula (1), W1 represents the mass of the test immersion molding before the test immersion molding is immersed in toluene, W2 represents the mass of the test immersion molding after the test immersion molding is immersed in toluene, P1 represents the specific gravity of the rubber component of the chloroprene polymer composition, P2 represents the specific gravity of toluene, r represents the mass fraction of the rubber content of the chloroprene polymer composition in the test dip-molded product.
2. 2. The chloroprene polymer composition according to claim 1, wherein the toluene-insoluble matter is 50 to 90% by mass.
3. The chloroprene polymer composition according to claim 1 or 2, The chloroprene polymer composition contains chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units, The chloroprene polymer composition contains 8 to 20% by mass of 2,3-dichloro-1,3-butadiene monomer units relative to 100% by mass in total of chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units.
4. The chloroprene polymer composition according to claim 1 or 2, The low-temperature hardness change ΔH1 of the test dip molded product is 30 or less, The low-temperature hardness change ΔH1 is expressed as HB1-HA1, HA1 represents the Shore hardness measured by heating the test dip-molded products at 70°C for 30 minutes, stacking the test dip-molded products to a thickness of 6.00±0.20 mm, and measuring the Shore hardness using a durometer type A at 23°C. HB1 represents the Shore hardness measured in an environment of -10°C using a durometer type A after the test dip-molded products are heated at 70°C for 30 minutes and then stored at -10°C for 168 hours and the test dip-molded products are stacked to a thickness of 6.00±0.20 mm.
5. The chloroprene polymer composition according to claim 1 or 2, A chloroprene polymer composition, wherein a ratio RB / RA of the total amount RB of peak areas of abietic acid, neoabietic acid, palustric acid, levopimaric acid and salts thereof to the total amount RA of peak areas of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid and salts thereof, obtained by gas chromatography analysis of an extract extracted from the test immersion molded product with an ethanol / toluene azeotropic mixture specified in JIS K 6229, is 0.10 or more and 0.70 or less.
6. A chloroprene polymer latex comprising the chloroprene polymer composition according to claim 1 or 2 and water.
7. A dip-molded product made from a composition for forming a dip-molded product, comprising the chloroprene polymer latex according to claim 6 .
8. 8. The dip-molded product according to claim 7, which is an industrial or general household glove, a medical glove, a balloon, a catheter or a boot.
9. The dip-molded product according to claim 7, wherein a low-temperature hardness change ΔH2 is 30 or less, The low-temperature hardness change ΔH2 is expressed as HB2-HA2, HA2 represents the Shore hardness measured by heating the dip-molded product at 70° C. for 30 minutes, stacking the dip-molded product to a thickness of 6.00±0.20 mm, and measuring the Shore hardness using a durometer type A at 23° C.; HB2 represents the Shore hardness of the dip-molded product measured in an environment of -10°C using a durometer type A after the dip-molded product is subjected to a heat treatment at 70°C for 30 minutes, the dip-molded product is stored at -10°C for 168 hours, and the dip-molded product is stacked to a thickness of 6.00±0.20 mm.
10. A dip-molded product of a composition for forming a dip-molded product, comprising a chloroprene polymer latex, The dip-molded product has a low-temperature hardness change ΔH2 of 30 or less, The low-temperature hardness change ΔH2 is expressed as HB2-HA2, HA2 represents the Shore hardness measured by heating the dip-molded product at 70° C. for 30 minutes, stacking the dip-molded product to a thickness of 6.00±0.20 mm, and measuring the Shore hardness using a durometer type A at 23° C.; HB2 represents the Shore hardness measured in an environment of -10°C using a durometer type A after the dip-molded product is heated at 70°C for 30 minutes and then stored at -10°C for 168 hours and the dip-molded product is stacked to a thickness of 6.00±0.20 mm. The dip-molded product has a tensile strength at break of 18.0 MPa or more, and a modulus at 100% elongation of 0.65 MPa or less, as measured in accordance with JIS K 6251.