Composition, crosslinked product, and sealing material

JPWO2023189547A5Inactive Publication Date: 2024-11-19
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024511725
Authority / Receiving Office
JP · JP
Patent Type
Applications
Filing Date
2024-09-12
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent
Patent Text Reader

Abstract

Provided is a composition which contains a perfluoro elastomer and a filler. The filler contains silicon carbide and graphite. The ratio (area (C) / area (SiC)) of the area (C) of a peak derived from the graphite in the filler relative to the area (SiC) of a peak derived from the silicon carbide in the filler, as measured by means of X-Ray photoelectron spectroscopy (XPS), is 0.7 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Composition, crosslinked product, and sealing material

[0001] The present disclosure relates to a composition, a crosslinked product, and a sealant.

[0002] Perfluoroelastomers are used as sealing materials due to their excellent sealing properties and heat resistance. Since sealing materials used in semiconductor manufacturing equipment are required to be plasma resistant, a technique for imparting plasma resistance to sealing materials by blending fillers into perfluoroelastomers is known.

[0003] For example, Patent Document 1 describes a crosslinkable elastomer composition comprising a crosslinkable elastomer and a non-oxide ceramic such as a carbide or nitride.

[0004] Patent Document 2 describes a crosslinkable fluorine-containing elastomer and a polymer having a bulk density of 0.15 g / cm 3 The document describes a crosslinkable fluorine-containing elastomer composition containing the following silicon carbide particles:

[0005] International Publication No. 03 / 051999 Special Publication No. 2012-509975

[0006] An object of the present disclosure is to provide a composition that can give a crosslinked product having excellent plasma resistance and excellent compression set resistance.

[0007] According to the present disclosure, there is provided a composition containing a perfluoroelastomer and a filler, wherein the filler contains silicon carbide and graphite, and the ratio of the area of ​​the peak (C) derived from the graphite in the filler to the area of ​​the peak (SiC) derived from the silicon carbide in the filler (area (C) / area (SiC)) measured by X-ray photoelectron spectroscopy (XPS) is 0.7 or more.

[0008] In the composition of the present disclosure, the BET specific surface area of ​​the filler determined by a nitrogen adsorption method is 15 to 200 m 2In the composition of the present disclosure, it is preferable that the ratio (water vapor / nitrogen) of the BET specific surface area of ​​the filler determined by a water vapor adsorption method to the BET specific surface area of ​​the filler determined by a nitrogen adsorption method is 1 to 60%. In the composition of the present disclosure, it is preferable that the bulk density of the filler is 0.10 g / cm 3 Preferably, the content of the filler in the composition of the present disclosure is 0.1 to 100 parts by mass relative to 100 parts by mass of the perfluoroelastomer. Preferably, the composition of the present disclosure further contains at least one selected from the group consisting of inorganic nitrides, organotin compounds, compounds that generate ammonia, and crosslinking agents.

[0009] The present disclosure also provides a crosslinked product obtained by crosslinking the above composition.

[0010] The crosslinked product of the present disclosure can be suitably used as a sealing material. The crosslinked product of the present disclosure preferably has a compression set of 50% or less, as measured by leaving it at 300°C for 70 hours at a compression ratio of 25%.

[0011] According to the present disclosure, it is possible to provide a composition that can give a crosslinked product having excellent plasma resistance and excellent compression set resistance.

[0012] Specific embodiments of the present disclosure will be described in detail below, but the present disclosure is not limited to the following embodiments.

[0013] The compositions of the present disclosure contain a perfluoroelastomer and a filler.

[0014] In Patent Document 1, by using non-oxide ceramics such as carbides and nitrides as fillers to be blended in a crosslinkable elastomer composition, it is possible to reduce the NF exposed in the semiconductor manufacturing process. 3 Plasma treatment and O 3 Furthermore, Patent Document 2 describes that a filler having a bulk density of 0.15 g / cm3 can be used as a filler to be blended in a crosslinkable fluorine-containing elastomer composition, and that a molded article having a small change in weight can be obtained by both treatments. 3By using the following silicon carbide particles, O 2 Plasma treatment and O 2 / CF 4 It is described that a molded article with small weight change can be obtained by both plasma treatments.

[0015] In contrast, the composition of the present disclosure uses a filler that contains silicon carbide and graphite, and has a ratio (area (C) / area (SiC)) of the area of ​​the peak attributable to graphite in the filler to the area of ​​the peak attributable to silicon carbide in the filler (SiC) as measured by X-ray photoelectron spectroscopy (XPS) of 0.7 or more. It has been found that the use of such a filler makes it possible to obtain a crosslinked product that exhibits excellent plasma resistance and excellent compression set resistance at high temperatures.

[0016] <Filler> The filler contained in the composition of the present disclosure contains silicon carbide and graphite, and the ratio (area (C) / area (SiC)) is 0.7 or more.

[0017] The area of ​​the peak (SiC) derived from silicon carbide in the filler and the area of ​​the peak (C) derived from graphite in the filler can be determined by analyzing the filler using X-ray photoelectron spectroscopy. The area of ​​the peak (SiC) and the area of ​​the peak (C) are the areas of the carbon 1s peaks derived from silicon carbide and graphite in the filler.

[0018] The filler ratio (area (C) / area (SiC)) is preferably 1.0 or more, more preferably 1.6 or more, and is preferably 3.0 or less, more preferably 2.0 or less, because the plasma resistance and compression set resistance of the crosslinked product are further improved.

[0019] The filler of the present disclosure contains silicon carbide and graphite. The presence of silicon carbide and graphite in the filler can be confirmed, for example, by obtaining a transmission electron microscope (TEM) equipped with an energy dispersive X-ray analyzer (EDS) and a transmission electron microscope photograph of the filler and an elemental mapping image of carbon element.

[0020] The graphite content is preferably 0 to 10% by mass, more preferably 0.1% by mass or more, even more preferably 0.5% by mass or more, particularly preferably 1.0% by mass or more, more preferably 8.0% by mass or less, even more preferably 6.0% by mass or less, and particularly preferably 5.0% by mass or less, relative to the mass of the filler. The filler contained in the composition of the present disclosure also includes fillers containing such a small amount of graphite that weight loss cannot be measured by simultaneous differential thermal and thermogravimetry.

[0021] The graphite content can be measured by the following method. That is, using a thermogravimetric and differential thermal analyzer, approximately 10 mg of filler is heated in an air atmosphere, the filler temperature is raised from room temperature to 1000°C at a rate of 10°C / min, and the weight at the point of greatest weight loss is measured. Next, the weight loss at the point of greatest weight loss is calculated by subtracting the weight at the point of greatest weight loss from the initial weight (weight at room temperature before heating). Then, the weight loss percentage is calculated as the ratio (%) of the weight loss at the point of greatest weight loss to the initial weight. In the present disclosure, room temperature may be a temperature in the range of 10 to 40°C. The temperature range of 10 to 40°C does not significantly affect the calculated weight loss percentage.

[0022] When a filler contains silicon carbide and graphite, weight loss due to heating of the filler is presumably caused by graphite combining with oxygen in the air and sublimating. Therefore, when a filler contains silicon carbide and graphite, the graphite content in the filler can be determined by determining the weight loss rate of the filler.

[0023] The BET specific surface area of ​​the filler determined by the nitrogen adsorption method is preferably 15 to 150 m, since this further improves the plasma resistance and compression set resistance of the resulting crosslinked product. 2 / g, more preferably 20m 2 / g or more, and more preferably 40m 2 / g or more, and even more preferably 50m 2 / g or more, more preferably 100m 2 / g or less, and more preferably 80m 2 / g or less.

[0024] The BET specific surface area of ​​the filler determined by the nitrogen adsorption method can be measured by the BET flow method (single-point method) using nitrogen gas and a mixed gas (30% nitrogen + 70% helium).

[0025] The BET specific surface area of ​​the filler determined by the water vapor adsorption method is preferably 1 to 15 m, since this further improves the plasma resistance and compression set resistance of the resulting crosslinked product. 2 / g, more preferably 3m 2 / g or more, and more preferably 4m 2 / g or more, more preferably 12m 2 / g or less, and more preferably 10m 2 / g or less.

[0026] The BET specific surface area of ​​the filler determined by the water vapor adsorption method can be calculated from the water vapor adsorption / desorption isotherm by measuring the water vapor adsorption of the filler and then using the water vapor adsorption / desorption isotherm according to the BET method.

[0027] The ratio (water vapor / nitrogen) of the BET specific surface area of ​​the filler determined by the water vapor adsorption method to the BET specific surface area of ​​the filler determined by the nitrogen adsorption method is preferably 1 to 60%, more preferably 3 to 40%, even more preferably 4% or more, still more preferably 5% or more, more preferably 30% or less, and even more preferably 20% or less, because the plasma resistance and compression set resistance of the resulting crosslinked product are further improved.

[0028] The ratio (water vapor / nitrogen) of the BET specific surface area of ​​a filler determined by the water vapor adsorption method to the BET specific surface area of ​​a filler determined by the nitrogen adsorption method is an index of the hydrophilicity of the filler, and a higher ratio (water vapor / nitrogen) means a higher hydrophilicity of the filler.

[0029] The bulk density of the filler is preferably 0.10 g / cm 3 More preferably, 0.12 g / cm3 More preferably, it is 0.14 g / cm 3 More preferably, 0.30 g / cm 3 More preferably, it is 0.20 g / cm or less. 3 The following is the result.

[0030] The bulk density of the filler can be calculated from the volume by putting 5 g of powder into a 100 ml measuring cylinder (inner diameter 28 mm), tapping it 20 times from a height of 2 cm, and reading the scale.

[0031] The average particle size of the filler is preferably 10 to 100 nm, more preferably 15 nm or more, even more preferably 20 nm or more, more preferably 90 nm or less, and even more preferably 80 nm or less, because the plasma resistance and compression set resistance of the obtained crosslinked product are further improved.

[0032] The average particle size (DBET) of the filler was determined by measuring the BET specific surface area of ​​the filler using a nitrogen adsorption method, and the formula was: average particle size (nm) = 6000 / (specific surface area (m 2 / g) x true density (g / cm 3 The true density can be calculated from the true density of silicon carbide, which is 3.22 g / cm 3 It can be said that:

[0033] The filler used in the present disclosure is preferably produced by a thermal plasma method. The filler used in the present disclosure can be produced, for example, by using an inert gas as a carrier gas to introduce silicon powder or silicon carbide powder into a thermal plasma flame, evaporating the powder to form a gaseous mixture, and then contacting the gaseous mixture with a hydrocarbon gas. In this case, the ratio (area (C) / area (SiC)) of the resulting filler can be adjusted by using the methods described in JP 2007-138287 A, JP 2011-213524 A, and non-patent document (Ya-Li LI and Takamasa ISHIGAKI, "Synthesis and Structural Characterization of Core-Shell Si-SiC Composite Particles by Thermal Plasma In-Flight Carburization of Silicon Powder," Journal of the Ceramic Society of Japan, 2007, 115(11), pp. 717-723).

[0034] The content of the filler in the composition of the present disclosure is preferably 0.1 to 100 parts by mass, more preferably 0.5 part by mass or more, even more preferably 1.0 part by mass or more, particularly preferably 5 parts by mass or more, more preferably 50 parts by mass or less, even more preferably 30 parts by mass or less, and particularly preferably 25 parts by mass or less, relative to 100 parts by mass of the perfluoroelastomer, because the plasma resistance and compression set resistance of the obtained crosslinked product are further improved.

[0035] The composition of the present disclosure preferably has a sea-island structure formed by islands composed of a filler and a sea composed of a perfluoroelastomer, since this further improves the plasma resistance and compression set resistance of the crosslinked product. Such a sea-island structure can be formed by blending a filler containing silicon carbide and exhibiting the above ratio (area (C) / area (SiC)) with a perfluoroelastomer. Blending conventional silicon carbide with a perfluoroelastomer, particularly when the BET specific surface area (nitrogen adsorption method) or average particle size of the silicon carbide is small, results in a composition having a network structure formed by high dispersion of silicon carbide in the perfluoroelastomer. On the other hand, when a filler exhibiting the above ratio (area (C) / area (SiC)) is used, a composition having a sea-island structure can be obtained even when the BET specific surface area (nitrogen adsorption method) or average particle size of the filler is small. The dispersion state of the filler in the composition can be confirmed, for example, by observing the surface or cross-section of the composition using a transmission electron microscope (TEM).

[0036] <Perfluoroelastomer> The composition of the present disclosure contains a perfluoroelastomer.

[0037] In the present disclosure, a perfluoroelastomer is a fluoropolymer in which the content of perfluoromonomer units relative to all polymerized units is 90 mol% or more, preferably 91 mol% or more, and which has a glass transition temperature of 20°C or less and a melting peak (ΔH) magnitude of 4.5 J / g or less, and further, a polymer in which the concentration of fluorine atoms contained in the fluoropolymer is 71 mass% or more, preferably 71.5 mass% or more. In the present disclosure, the concentration of fluorine atoms contained in the fluoropolymer is determined by calculation of the concentration (mass%) of fluorine atoms contained in the fluoropolymer from the type and content of each monomer constituting the fluoropolymer.

[0038] In the present disclosure, a perfluoromonomer is a monomer that does not contain a carbon atom-hydrogen atom bond in the molecule. The perfluoromonomer may be a monomer containing carbon atoms and fluorine atoms, or a monomer in which some of the fluorine atoms bonded to carbon atoms have been substituted with chlorine atoms, or may contain nitrogen atoms, oxygen atoms, sulfur atoms, phosphorus atoms, boron atoms, or silicon atoms in addition to carbon atoms. The perfluoromonomer is preferably a monomer in which all hydrogen atoms have been substituted with fluorine atoms. The perfluoromonomer does not include monomers that provide crosslinking sites.

[0039] The monomer that provides a crosslinking site is a monomer (cure site monomer) having a crosslinkable group that provides a crosslinking site to the fluoropolymer for forming a crosslink with a curing agent.

[0040] In the present disclosure, the content of each monomer constituting the perfluoroelastomer can be calculated by appropriately combining NMR, FT-IR, elemental analysis, X-ray fluorescence analysis, and other known methods depending on the type of monomer.

[0041] Examples of perfluoromonomers that provide perfluoromonomer units constituting perfluoroelastomers include tetrafluoroethylene [TFE], hexafluoropropylene [HFP], and compounds represented by the general formula (13): CF 2 =CF-ORf 13 (wherein, Rf 13 represents a perfluoroalkyl group having 1 to 8 carbon atoms, a fluoromonomer represented by general formula (14): CF 2 = CFOCF 2 ORf 14 (wherein, Rf 14 is a linear or branched perfluoroalkyl group having 1 to 6 carbon atoms, a cyclic perfluoroalkyl group having 5 to 6 carbon atoms, or a linear or branched perfluorooxyalkyl group having 2 to 6 carbon atoms and containing 1 to 3 oxygen atoms), and a fluoromonomer represented by the general formula (15): CF 2 = CFO (CF 2 CF (Y 15 ) O) m (CF 2 )n F (wherein, Y 15 represents a fluorine atom or a trifluoromethyl group, m is an integer of 1 to 4, and n is an integer of 1 to 4.

[0042] The perfluoroelastomer is preferably at least one selected from the group consisting of perfluoroelastomers containing TFE units, such as TFE / fluoromonomer copolymers represented by general formula (13), (14) or (15), and TFE / fluoromonomer copolymers represented by general formula (13), (14) or (15) / monomer copolymers that provide crosslinking sites.

[0043] In the case of a TFE / perfluoro(methyl vinyl ether) (PMVE) copolymer, the composition is preferably 45 to 90 / 10 to 55 (mol %), more preferably 55 to 80 / 20 to 45, even more preferably 55 to 70 / 30 to 45, and most preferably 56 to 69.5 / 30.5 to 44.

[0044] In the case of a copolymer of TFE / PMVE / a monomer that provides a crosslinking site, the ratio is preferably 45 to 89.9 / 10 to 54.9 / 0.01 to 4 (mol %), more preferably 55 to 77.9 / 20 to 49.9 / 0.1 to 3.5, even more preferably 55 to 69.8 / 30 to 44.8 / 0.2 to 3, and most preferably 55.3 to 69.5 / 30.3 to 44.5 / 0.2 to 2.8.

[0045] In the case of TFE / fluoromonomer copolymers having 4 to 12 carbon atoms and represented by general formula (13), (14) or (15), the ratio is preferably 50 to 90 / 10 to 50 (mol%), more preferably 60 to 88 / 12 to 40, even more preferably 65 to 85 / 15 to 35, and most preferably 66 to 84 / 16 to 34.

[0046] In the case of TFE / fluoromonomer having 4 to 12 carbon atoms represented by general formula (13), (14) or (15) / monomer copolymer that provides crosslinking sites, it is preferably 50 to 89.9 / 10 to 49.9 / 0.01 to 4 (mol%), more preferably 60 to 87.9 / 12 to 39.9 / 0.1 to 3.5, even more preferably 65 to 84.8 / 15 to 34.8 / 0.2 to 3, and most preferably 66 to 84.3 / 15.5 to 33.8 / 0.2 to 2.8. Outside these composition ranges, the properties of rubber elastic body are lost and tend to become similar to the properties of resin.

[0047] The perfluoroelastomer is preferably at least one selected from the group consisting of TFE / fluoromonomer represented by general formula (15) / monomer copolymer providing a crosslinking moiety, TFE / fluoromonomer copolymer represented by general formula (15), TFE / fluoromonomer copolymer represented by general formula (13), and TFE / fluoromonomer represented by general formula (13) / monomer copolymer providing a crosslinking moiety.

[0048] Examples of the perfluoroelastomer include those described in International Publication No. 97 / 24381, Japanese Patent Publication No. 61-57324, Japanese Patent Publication No. 4-81608, and Japanese Patent Publication No. 5-13961.

[0049] The monomer that provides a crosslinking site is a monomer (cure site monomer) having a crosslinkable group that provides a perfluoroelastomer with a crosslinking site for forming a crosslink with a crosslinking agent.

[0050] The monomer that provides the crosslinking site is represented by the general formula (16): CX 4 2 =CX 5 R f 2 X 6 (In the formula, X 4 , X 5 are each independently H, F or an alkyl group having 1 to 5 carbon atoms, and R f 2is a linear or branched alkylene or oxyalkylene group which may have one or more ether-bonded oxygen atoms and which may have an aromatic ring, and in which some or all of the hydrogen atoms may be substituted with fluorine atoms; X 6 is an iodine atom, a bromine atom, a nitrile group, a carboxyl group, an alkoxycarbonyl group, a hydroxyl group, a vinyl group, an azide group, a sulfonyl azide group, a carbonyl azide group, or an alkyne group. The alkyne group may be an ethynyl group.

[0051] Among them, the monomer that provides the crosslinking site is a monomer represented by the general formula (17): CX 16 2 =CX 16 -Rf 16 CHR 16 X 17 (In the formula, X 16 are each independently a hydrogen atom, a fluorine atom, or CH 3 , Rf 16 represents a fluoroalkylene group, a perfluoroalkylene group, a fluoro(poly)oxyalkylene group or a perfluoro(poly)oxyalkylene group, R 16 is a hydrogen atom or CH 3 , X 17 is an iodine atom or a bromine atom), a fluoromonomer represented by the general formula (18): CX 16 2 =CX 16 -Rf 17 X 17 (In the formula, X 16 are each independently a hydrogen atom, a fluorine atom, or CH 3 , Rf 17 represents a fluoroalkylene group, a perfluoroalkylene group, a fluoro(poly)oxyalkylene group or a perfluoro(poly)oxyalkylene group, X 17 is an iodine atom or a bromine atom), a fluoromonomer represented by the general formula (19): CF 2 = CFO (CF 2 CF (CF 3 ) O) m (CF 2 ) n -X 18(wherein m is an integer of 0 to 5, n is an integer of 1 to 3, X 18 represents a cyano group, an azide group, a sulfonyl azide group, a carbonyl azide group, a carboxyl group, an alkoxycarbonyl group, an alkyne group, an iodine atom, a bromine atom, or —CH 2 I), a fluoromonomer represented by general formula (20): CH 2 =CFCF 2 O(CF(CF 3 )CF 2 O) m (CF (CF 3 )) n -X 19 (wherein m is an integer of 0 to 5, n is an integer of 1 to 3, X 19 represents a cyano group, a carboxyl group, an alkoxycarbonyl group, an iodine atom, a bromine atom, or —CH 2 OH), and a fluoromonomer represented by the general formula (21): CR 20 2 =CR 20 -Z-CR 20 =CR 20 2 (In the formula, R 20 are each independently a hydrogen atom or an alkyl group having 1 to 5 carbon atoms. Z is a linear or branched alkylene group having 1 to 18 carbon atoms, a cycloalkylene group having 3 to 18 carbon atoms, or an at least partially fluorinated alkylene or oxyalkylene group having 1 to 10 carbon atoms, which may have an oxygen atom, or -(Q) p -CF 2 O-(CF 2 CF 2 O) m (CF 2 O) n -CF 2 -(Q) p - (wherein Q is an alkylene group or an oxyalkylene group, p is 0 or 1, and m / n is 0.2 to 5), and is a (per)fluoropolyoxyalkylene group having a molecular weight of 500 to 10,000.

[0052] X 16is preferably a fluorine atom. 16 and Rf 17 is preferably a perfluoroalkylene group having 1 to 5 carbon atoms. 16 is preferably a hydrogen atom. 18 represents a cyano group, an alkoxycarbonyl group, an iodine atom, a bromine atom, or —CH 2 Preferably, X is I. 19 represents a cyano group, an alkoxycarbonyl group, an iodine atom, a bromine atom, or —CH 2 It is preferably OH.

[0053] The monomer that provides the crosslinking site is CF 2 = CFOCF 2 CF (CF 3 ) OCF 2 CF 2 C.N., C.F. 2 = CFOCF 2 CF (CF 3 ) OCF 2 CF 2 COOH, CF 2 = CFOCF 2 CF (CF 3 ) OCF 2 CF 2 CH 2 I, CF 2 = CFOCF 2 CF 2 CH 2 I, CH 2 =CFCF 2 OCF (CF 3 )CF 2 OCF (CF 3 ) CN, CH 2 =CFCF 2 OCF (CF 3 )CF 2 OCF (CF 3 ) COOH, CH 2 =CFCF 2 OCF (CF 3 )CF 2 OCF (CF 3 ) CH 2 OH, CH 2 = CHCF 2 CF 2 I, CH2 =CH(CF 2 ) 2 CH=CH 2 , C.H. 2 =CH(CF 2 ) 6 CH=CH 2 , C.F. 2 = CFO (CF 2 ) 3 CN and CF 2 = CFO (CF 2 ) 5 CN, and CF 2 = CFOCF 2 CF (CF 3 ) OCF 2 CF 2 C.N., C.F. 2 = CFO (CF 2 ) 5 CN and CF 2 = CFOCF 2 CF 2 CH 2 It is more preferable that the compound is at least one selected from the group consisting of I.

[0054] The perfluoroelastomer preferably has a glass transition temperature of −30° C. or higher, more preferably −20° C. or higher, and even more preferably −10° C. or higher, in view of excellent compression set properties at high temperatures. Furthermore, in view of good cold resistance, the glass transition temperature is preferably 10° C. or lower, more preferably 5° C. or lower, and even more preferably 0° C. or lower.

[0055] The glass transition temperature can be determined by obtaining a DSC curve using a differential scanning calorimeter (DSC822e, manufactured by Mettler Toledo) by heating 10 mg of a sample at a rate of 10°C / min, and by determining the temperature as the midpoint between two intersections of an extension of the baseline of the DSC curve before and after the second-order transition and a tangent to the inflection point of the DSC curve.

[0056] In terms of good heat resistance, the perfluoroelastomer preferably has a Mooney viscosity ML(1+20) at 170°C of 30 or more, more preferably 40 or more, and even more preferably 50 or more. In terms of good processability, the Mooney viscosity ML(1+20) is preferably 100 or less, more preferably 90 or less, and even more preferably 80 or less.

[0057] In terms of good heat resistance, the perfluoroelastomer preferably has a Mooney viscosity ML(1+20) at 140°C of 30 or more, more preferably 40 or more, and even more preferably 50 or more. In terms of good processability, the Mooney viscosity ML(1+20) is preferably 180 or less, more preferably 150 or less, and even more preferably 110 or less.

[0058] In terms of good heat resistance, the perfluoroelastomer preferably has a Mooney viscosity ML(1+10) at 100°C of 10 or more, more preferably 20 or more, and even more preferably 30 or more. In terms of good processability, the Mooney viscosity ML(1+10) is preferably 120 or less, more preferably 100 or less, and even more preferably 80 or less.

[0059] The Mooney viscosity can be measured using a Mooney viscometer MV2000E manufactured by ALPHA TECHNOLOGIES at 170°C, 140°C, or 100°C in accordance with JIS K6300.

[0060] Perfluoroelastomers can be produced by conventional methods, but iodine compounds or bromine compounds can also be used as chain transfer agents because the molecular weight distribution of the resulting polymer is narrow, molecular weight control is easy, and iodine atoms or bromine atoms can be introduced into the terminals.The polymerization method using iodine compounds or bromine compounds can be, for example, a method of emulsion polymerization in an aqueous medium under pressure in the presence of iodine compounds or bromine compounds in a substantially oxygen-free state (iodine transfer polymerization method).Typical examples of the iodine compounds or bromine compounds used include, for example, compounds represented by the general formula: R 21 I x Bry (wherein x and y are each an integer of 0 to 2 and satisfy 1≦x+y≦2; R 21 is a saturated or unsaturated fluorohydrocarbon group or chlorofluorohydrocarbon group having 1 to 16 carbon atoms, or a hydrocarbon group having 1 to 3 carbon atoms, which may contain an oxygen atom). By using an iodine compound or a bromine compound, iodine atoms or bromine atoms are introduced into the polymer and function as crosslinking points.

[0061] Examples of iodine compounds and bromine compounds include 1,3-diiodoperfluoropropane, 2-iodoperfluoropropane, 1,3-diiodo-2-chloroperfluoropropane, 1,4-diiodoperfluorobutane, 1,5-diiodo-2,4-dichloroperfluoropentane, 1,6-diiodoperfluorohexane, 1,8-diiodoperfluorooctane, 1,12-diiodoperfluorododecane, 1,16-diiodoperfluorohexadecane, diiodomethane, 1,2-diiodoethane, 1,3-diiodo-n-propane, CF 2 Br 2 , BrCF 2 CF 2 Br, CF 3 CFBrCF 2 Br, CFClBr 2 , BrCF 2 CFClBr, CFBrClCFClBr, BrCF 2 CF 2 CF 2 Br, BrCF 2 CFBrOCF 3 , 1-bromo-2-iodoperfluoroethane, 1-bromo-3-iodoperfluoropropane, 1-bromo-4-iodoperfluorobutane, 2-bromo-3-iodoperfluorobutane, 3-bromo-4-iodoperfluorobutene-1, 2-bromo-4-iodoperfluorobutene-1, monoiodomonobromo-substituted benzene, diiodomonobromo-substituted benzene, and (2-iodoethyl)- and (2-bromoethyl)-substituted benzenes. These compounds may be used alone or in combination with one another.

[0062] Among these, it is preferable to use 1,4-diiodoperfluorobutane, 1,6-diiodoperfluorohexane, and 2-iodoperfluoropropane in terms of polymerization reactivity, crosslinking reactivity, availability, and the like.

[0063] The perfluoroelastomer preferably has a cyano group (-CN group). Perfluoroelastomers having a cyano group (-CN group) are, for example, those which can be crosslinked by forming a triazine ring through cyclotrimerization of the cyano group, or those which can be crosslinked by forming an imidazole ring using a tetramine compound as a crosslinking agent, and can impart excellent compression set properties and heat resistance to the crosslinked product.

[0064] The perfluoroelastomer having a cyano group preferably has a cyano group (-CN group) at the end of the main chain and / or on a side chain.

[0065] Examples of perfluoroelastomers having a cyano group (-CN group) at the main chain end and / or side chain include the above-mentioned copolymers of TFE / fluoromonomer represented by general formula (13), (14) or (15) / monomer that provides crosslinking moieties, in which the monomer that provides crosslinking moieties is a monomer having a cyano group (-CN group).In this case, from the viewpoint of good crosslinking properties and heat resistance, the content of the monomer unit having a cyano group (-CN group) may be 0.1 to 5 mol%, or may be 0.3 to 3 mol%, based on the total amount of TFE units and fluoromonomer units represented by general formula (13), (14) and (15).More preferable compositions are as described above.

[0066] Furthermore, examples of the monomer having a cyano group (-CN group) include a monomer represented by the formula: CY 1 2 =CY 1 (CF 2 ) n —CN (wherein Y 1 are each independently a hydrogen atom or a fluorine atom, and n is an integer of 1 to 8. 2 =CFCF 2 Rf 8 -CN (wherein, Rf8 Ha-(OCF 2 ) n - or - (OCF (CF 3 )) n -, and n is an integer from 0 to 5) Formula: CF 2 =CFCF 2 (OCF (CF 3 )CF 2 ) m (OCH 2 CF 2 CF 2 ) n OCH 2 CF 2 -CN (wherein m is an integer of 0 to 5, and n is an integer of 0 to 5) Formula: CF 2 =CFCF 2 (OCH 2 CF 2 CF 2 ) m (OCF (CF 3 )CF 2 ) n OCF (CF 3 )-CN (wherein m is an integer of 0 to 5, and n is an integer of 0 to 5) Formula: CF 2 =CF(OCF 2 CF (CF 3 )) m O (CF 2 ) n -CN (wherein m is an integer of 0 to 5, and n is an integer of 1 to 8) Formula: CF 2 =CF(OCF 2 CF (CF 3 )) m -CN (wherein m is an integer of 1 to 5) Formula: CF 2 = CFOCF 2 (CF (CF 3 ) OCF 2 ) n CF(-CN)CF 3 (wherein n is an integer of 1 to 4) Formula: CF 2 = CFO (CF 2 ) n OCF (CF 3 )-CN (wherein n is an integer of 2 to 5) Formula: CF 2 = CFO (CF 2 ) n -(C6 H 4 )-CN (wherein n is an integer of 1 to 6) Formula: CF 2 =CF(OCF 2 CF (CF 3 )) n OCF 2 CF (CF 3 )-CN (wherein n is an integer of 1 to 2) Formula: CH 2 =CFCF 2 O(CF(CF 3 )CF 2 O) n CF (CF 3 )-CN (wherein n is an integer of 0 to 5), Formula: CF 2 = CFO (CF 2 CF (CF 3 ) O) m (CF 2 ) n —CN (wherein m is an integer of 0 to 5, and n is an integer of 1 to 3) Formula: CH 2 =CFCF 2 OCF (CF 3 ) OCF (CF 3 )-CN Formula: CH 2 =CFCF 2 OCH 2 CF 2 -CN Formula: CF 2 = CFO (CF 2 CF (CF 3 ) O) m CF 2 CF (CF 3 )-CN (wherein m is an integer of 0 or more) Formula: CF 2 = CFOCF(CF 3 )CF 2 O (CF 2 ) n -CN (wherein n is an integer of 1 or more) Formula: CF 2 = CFOCF 2 OCF 2 CF (CF 3 ) OCF 2 -CN Formula: CF 2 = CFO (CF 2 ) 3 CN formula: CF 2 = CFO (CF 2 )5 These may be used alone or in any combination.

[0067] Among the above, the formula: CF 2 =CF(OCF 2 CF (CF 3 )) m O (CF 2 ) n -CN (wherein m is an integer of 0 to 5, and n is an integer of 1 to 8) is preferred, and CF 2 = CFOCF 2 CF (CF 3 ) OCF 2 CF 2 CN is more preferred.

[0068] These perfluoroelastomers can be produced by conventional methods.

[0069] Specific examples of such perfluoroelastomers include fluororubbers described in International Publication No. 97 / 24381, Japanese Patent Publication No. 61-57324, Japanese Patent Publication No. 4-81608, and Japanese Patent Publication No. 5-13961.

[0070] <Other Components> The composition of the present disclosure may further contain a filler other than the above-described silicon carbide-containing filler.

[0071] Examples of the filler include imide-based fillers having an imide structure such as polyimide, polyamideimide, and polyetherimide; organic fillers made of engineering plastics such as polyarylate, polysulfone, polyethersulfone, polyphenylene sulfide, polyetheretherketone, polyetherketone, and polyoxybenzoate; metal oxide fillers such as silicon oxide, aluminum oxide, and yttrium oxide; metal carbides such as aluminum carbide; metal nitride fillers such as silicon nitride and aluminum nitride; and inorganic fillers such as carbon black, aluminum fluoride, and carbon fluoride.

[0072] Among these, carbon black, aluminum oxide, silicon oxide, yttrium oxide, silicon nitride, polyimide, and carbon fluoride are preferred in terms of their shielding effect against various plasmas.

[0073] The inorganic fillers and organic fillers may be used alone or in combination of two or more.

[0074] In particular, in fields where high purity and non-staining properties are not required, ordinary additives that are blended into compositions, such as processing aids, plasticizers, colorants, etc., may be blended as needed, and one or more commonly used crosslinking agents or crosslinking aids different from those described above may also be blended.

[0075] The composition may contain an organic basic compound. Examples of the organic basic compound include a compound represented by the formula: CH 3 (CH 2 ) 17 -NH 2 Octadecylamine of formula: H 2 NC(O)-(CH 2 ) 11 -CH=CH-(CH 2 ) 7 CH 3 Erucamide of formula: H 2 NC(O)-(CH 2 ) 7 -CH=CH-(CH 2 ) 7 CH 3 Oleamide of formula: H 2 N-(CH 2 ) 6 -NH 2 Hexamethylenediamine of the formula: Examples of suitable cyclopentadiene compounds include 1,8-diazabicycloundec-7-ene (DBU) of the formula:

[0076] <Crosslinking Agents, etc.> The composition of the present disclosure may further contain at least one selected from the group consisting of an inorganic nitride, an organotin compound, a compound that generates ammonia, and a crosslinking agent. By containing these components, such as a crosslinking agent, in the composition of the present disclosure, a crosslinked product can be easily obtained from the composition of the present disclosure.

[0077] The inorganic nitride is not particularly limited, but silicon nitride (Si 3 N 4 ), lithium nitride, titanium nitride, aluminum nitride, boron nitride, vanadium nitride, zirconium nitride, etc. Among these, silicon nitride is preferred because it can be supplied as nano-sized fine particles.

[0078] Examples of the organotin compounds include tetraphenyltin and triphenyltin.

[0079] The compound that generates ammonia is preferably a compound that generates ammonia at 40 to 330°C.

[0080] The ammonia-generating compound is preferably urea or its derivatives, or an ammonium salt, more preferably urea or an ammonium salt, and even more preferably urea. The ammonium salt may be an organic ammonium salt or an inorganic ammonium salt. The ammonia-generating compound may also be one that reacts with a trace amount of water to generate ammonia.

[0081] Examples of urea derivatives include biurea, thiourea, urea hydrochloride, and biuret.

[0082] Examples of organic ammonium salts include ammonium salts of non-fluorine-containing carboxylic acids or sulfonic acids such as ammonium benzoate, ammonium adipate, and ammonium phthalate.

[0083] Examples of inorganic ammonium salts include compounds described in JP-A-9-111081, such as ammonium sulfate, ammonium carbonate, ammonium nitrate, and ammonium phosphate.

[0084] Further, examples of the ammonia-generating compound include acetaldehyde ammonia, hexamethylenetetramine, formamidine, formamidine hydrochloride, formamidine acetate, t-butyl carbamate, benzyl carbamate, and phthalamide.

[0085] Examples of the crosslinking agent include crosslinking agents used in peroxide crosslinking, polyol crosslinking, polyamine crosslinking, triazine crosslinking, oxazole crosslinking, imidazole crosslinking, and thiazole crosslinking. When the perfluoroelastomer has a cyano group (-CN group), the crosslinking agent is preferably at least one selected from the group consisting of an oxazole crosslinking agent, an imidazole crosslinking agent, and a thiazole crosslinking agent.

[0086] The crosslinking agent used in peroxide crosslinking may be any organic peroxide that can easily generate peroxy radicals in the presence of heat or a redox system, and specific examples thereof include 1,1-bis(t-butylperoxy)-3,5,5-trimethylcyclohexane, 2,5-dimethylhexane-2,5-dihydroperoxide, di-t-butyl peroxide (Perbutyl D), t-butylcumyl peroxide (Perbutyl C), dicumyl peroxide (Percumyl D, Percumyl D-40, Percumyl D-40MB(T)), α,α- Bis(t-butylperoxy)-p-diisopropylbenzene, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane (Perhexa 25B, Perhexa 25B-40), 2,5-dimethyl-2,5-di(t-butylperoxy)-hexyne-3 (Perhexyne 25B, Perhexyne 25B-40), benzoyl peroxide, t-butylperoxybenzene, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane (Perhexa 25Z), t-butylperoxymaleic acid (t-butyl MA), t-butyl Chilperoxy isopropyl carbonate (Perbutyl I-75), methyl ethyl ketone peroxide (Permec D (DR), Permec H (HR, HY), Permec N (NR, NY), Permec S (SR), Permec F (FR), Permec G (GR, GY)), cyclohexanone peroxide (Perhexa H), acetylacetone peroxide (Percure AH, AL), 1,1-di(t-hexylperoxy)-3,3,5-trimethylcyclohexane (Perhexa TMH), 1,1-di(t-hexyl peroxy)cyclohexane (Perhexa HC), 1,1-di(t-butylperoxy)-2-methylcyclohexane (Perhexa MC), 1,1-di(t-butylperoxy)cyclohexane (Perhexa C-80(S), Perhexa C-75(EB), Perhexa C(C), Perhexa C-40, Perhexa C-40MB(S)), 2,2-di(t-butylperoxy)butane (Perhexa 22), 4,4-di-(t-butylperoxy)butylpentanoate (Perhexa V, Perhexa V-40(F)), 2,2-di(4,4-Di-(t-butylperoxy)cyclohexyl)propane (Pertetra A), p-menthane hydroperoxide (Permenta H), diisopropylbenzene hydroperoxide (Percumyl P), 1,1,3,3-tetramethylbutyl hydroperoxide (Perocta H), cumene hydroperoxide (Percumyl H-80), t-butyl hydroperoxide (Perbutyl H-69), di(2-t-butylperoxyisopropyl)benzene (Perbutyl P, Perbutyl P-40, Peroximon F-40, Perbutyl P-40MB(K)), di-t-hexyl peroxide (Perhexyl D), diisobutyryl peroxide (Perloyl IB), di(3,5,5-trimethylhexanoyl) peroxide (Perloyl 355(S)), dilauroyl peroxide (Perloyl L), disuccinic acid peroxide (Perloyl SA), di-(3-methylbenzoyl) Dibenzoyl peroxide, benzoyl (3-methylbenzoyl) peroxide, and dibenzoyl peroxide mixture (Niper BMT-K40, Niper BMT-M), dibenzoyl peroxide (Niper BW, Niper BO, Niper FF, Niper BS, Niper E, Niper NS), di(4-methylbenzoyl) peroxide (Niper PMB), di-n-propyl peroxydicarbonate (Perroyl NPP-50M) ), diisopropyl peroxydicarbonate (Perloyl IPP-50, Perloyl IPP-27), di(4-t-butylcyclohexyl) peroxydicarbonate (Perloyl TCP), di(2-ethylhexyl) peroxydicarbonate (Perloyl OPP), di-sec-butyl peroxydicarbonate (Perloyl SBP), cumyl peroxyneodecanoate (Percumyl ND, Percumyl ND-50E), 1,1,3,3-Tetramethylbutyl peroxyneodecanoate (Perocta ND, Perocta ND-50E), t-hexyl peroxyneodecanoate (Perhexyl ND, Perhexyl ND-50E), t-butyl peroxyneodecanoate (Perbutyl ND, Perbutyl ND-50E), t-butyl peroxyneoheptanoate (Perbutyl NHP), t-hexyl peroxypivalate (Perhexyl PV, Perhexyl PV-50E), t -butyl peroxypivalate (Perbutyl PV, Perbutyl PV-40E), 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate (Perocta O), 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane (Perhexa 25 O), t-hexylperoxy-2-ethylhexanoate (Perhexyl O, Percure HO(N)), t-butylperoxy-2-ethylhexanoate (Perb Percure O), t-hexylperoxyisopropyl monocarbonate (Perhexyl I), t-butylperoxy-3,5,5-trimethylhexanoate (Perbutyl 355), t-butylperoxylaurate (Perbutyl L), t-butylperoxy-2-ethylhexyl monocarbonate (Perbutyl E), t-hexylperoxybenzoate (Perhexyl Z), t-butylperoxyacetate (Perbutyl A), a mixture of t-butylperoxy-3-methylbenzoate and t-butylperoxybenzoate (Perbutyl ZT), t-butylperoxybenzoate (Perbutyl Z), t-butylperoxyallyl monocarbonate (Peromer AC), 3,3',4,4'-tetra(t-butylperoxycarbonyl)benzophenone (BTTB-25), 2,3-dimethyl-2,3-diphenylbutane (Nofumer BC-90), and the like can be mentioned. Among these, dialkyl-type organic peroxides are preferred. 2,5-dimethyl-2,5-di(t-butylperoxy)hexane is particularly preferred. Generally, the type and amount of organic peroxide used are selected taking into consideration the amount of active -O-O-, decomposition temperature, etc.

[0087] In this case, the crosslinking aid that can be used may be any compound that has reactivity with peroxy radicals and polymer radicals, such as -CH=CH 2 , -CH 2 CH=CH 2 , -CF=CF 2 , -C(CF 3 ) = CF 2 , -C(CH 3 ) = CF 2 , -CF=CF(CF 3 ), -CF=CF(CH 3 ), -C(C 6 H 5 ) = CF 2 , -CF=CF(C 6 H 5 ), —CH═CF 2 , -CF=CHF, -C(CF 3 )=CHF, -CF=CH(CF 3 ), -CH=CF(CF 3 ) and other polyfunctional compounds having functional groups such as ("C" in each formula) 6 H 5 " represents a phenyl group). Specific examples include triallyl cyanurate, triallyl isocyanurate (TAIC), triacryl formal, triallyl trimellitate, N,N'-n-phenylene bismaleimide, dipropargyl terephthalate, diallyl phthalate, tetraallyl terephthalate amide, triallyl phosphate, bismaleimide, fluorinated triallyl isocyanurate (1,3,5-tris(2,3,3-trifluoro-2-propenyl)-1,3,5-triazine 2,4,6-trione), tris(diallylamine)-S-triazine, triallyl phosphite, N,N-diallylacrylamide, and 1,6-divinyldodecafluorohexane.

[0088] Furthermore, examples of the crosslinking aid used together with the peroxide crosslinking agent include a crosslinking aid represented by the general formula (31): (Wherein, six R 31 are each independently H, a halogen atom, or an optionally halogenated group having 1 to 5 carbon atoms which may contain an ether bond; Z 31may also include compounds represented by a linear or branched alkylene group, cycloalkylene group, or (per)fluoropolyoxyalkylene group having 1 to 18 carbon atoms, which optionally contains a heteroatom and is optionally halogenated.

[0089] The compound represented by general formula (31) includes compounds represented by general formula (32): (wherein j is an integer of 2 to 10, preferably an integer of 4 to 8, and four R 32 are each independently H, F, or an alkyl group or (per)fluoroalkyl group having 1 to 5 carbon atoms, a compound represented by general formula (33): (In the formula, Y 31 are each independently F, Cl or H, and Y 32 are each independently F, Cl, H or OR 33 (where R 33 is a branched or straight chain alkyl group which may be partially, substantially or completely fluorinated or chlorinated; Z 33 is a divalent group having 2 to 10 carbon atoms, optionally fluorinated, optionally interrupted by ether linkages, preferably Z 33 m is an integer of 3 to 5, -(CF 2 ) m - group, and the compound represented by general formula (33) is preferably F 2 C=CF-O-(CF 2 ) 5 -O-CF=CF 2 a compound represented by general formula (34): (In the formula, Y 31 , Y 32 and Z 33 is as described above, and R 34 are each independently H, F, or an alkyl group or (per)fluoroalkyl group having 1 to 5 carbon atoms.

[0090] The crosslinking agent or the crosslinking aid used together with the peroxide crosslinking agent may be a crosslinking aid represented by the general formula (35):

[0091] (In the formula, R 35 ~R 37 are each independently a hydrogen atom, a fluorine atom, an alkyl group, a fluorinated alkyl group, or a substituted or unsubstituted aryl group, and R 35 ~R 37 At least one of R is a fluorine atom or a group containing a fluorine atom. m is an integer of 1 to 5. When m is 2 or more, m R 35 ~R 37 may be the same or different. A hydrogen atom on the benzene ring may be substituted. When m is 1, it is preferable that the compound has two or more of the structure.

[0092] The compound having the structure represented by general formula (36) includes compounds represented by general formula (36):

[0093] (In the formula, R 35 ~R 37 is as defined above, p is an integer of 0 to 2, and n is an integer of 2 to 6.), a compound represented by general formula (37):

[0094] (In the formula, R 35 ~R 37 is as above. 38 is a single bond, -SO 2 -, -O-, -S-, -CO-, a heteroatom-containing group, a substituted or unsubstituted alkylene group, a substituted or unsubstituted cycloalkylene group, or a substituted or unsubstituted arylene group. m is an integer of 1 to 5. These groups may be partially or completely fluorinated.

[0095] The heteroatom-containing group is not particularly limited as long as it is a divalent group containing a heteroatom, and examples of the heteroatom include an oxygen atom, a nitrogen atom, a sulfur atom, a boron atom, and a phosphorus atom.

[0096] Examples of crosslinking agents used for polyol crosslinking include polyhydric alcohol compounds such as bisphenol A and bisphenol AF.

[0097] Examples of crosslinking agents used for polyamine crosslinking include polyamine compounds such as hexamethylenediamine carbamate, N,N'-dicinnamylidene-1,6-hexanediamine, and 4,4'-bis(aminocyclohexyl)methane carbamate.

[0098] Examples of crosslinking agents used for oxazole crosslinking, imidazole crosslinking, and thiazole crosslinking include those represented by the general formula (41):

[0099]

[0100] (In the formula, R 41 Ha-SO 2 -, -O-, -CO-, an alkylene group having 1 to 6 carbon atoms, a perfluoroalkylene group having 1 to 10 carbon atoms or a single bond, or

[0101]

[0102] and R 42 and R 43 One side is -NH 2 and the other is -NHR 44 , -NH 2 , —OH or —SH, and R 44 is a hydrogen atom, a fluorine atom or a monovalent organic group, and preferably R 42 Ga-NH 2 And R 43 Ga-NHR 44 Preferred specific examples of the alkylene group having 1 to 6 carbon atoms include a methylene group, an ethylene group, a propylene group, a butylene group, a pentylene group, and a hexylene group, and preferred specific examples of the perfluoroalkylene group having 1 to 10 carbon atoms include:

[0103]

[0104] These compounds are known as examples of bisdiaminophenyl compounds in JP-B 2-59177, JP-A 8-120146, etc.), bisaminophenol-based crosslinking agents, bisaminothiophenol-based crosslinking agents represented by general formula (42):

[0105] (R41 As mentioned above, R 45 are each independently any of the following groups:

[0106] Bisamidrazone crosslinking agents represented by general formula (43):

[0107]

[0108] (wherein, Rf 41 is a perfluoroalkylene group having 1 to 10 carbon atoms), or an amidrazone crosslinking agent represented by the general formula (44):

[0109]

[0110] (wherein n is an integer of 1 to 10), a bisamidoxime crosslinking agent represented by the general formula (45): HN=CR 45 R 46 (In the formula, R 45 , H, NH 2 , and N.H.R. 47 and R 46 is Ph, SO 2 H, N.R. 48 R 49 , 2-pyridine, and CH 2 CONH 2 and R 47 Ph, NH 2 and CN, R 48 is H, NHPh, CH 2 CONH 2 , a linear alkyl group having 1 to 8 carbon atoms, and a branched alkyl group having 1 to 8 carbon atoms; and R 49 is Ph, COOC (CH 3 ) 3 , N.H. 2 , C.H. 2 COOH, CSNH 2 , CNHNH 3 + Cl - , p-phenylCN, and COPh). These bisaminophenol-based crosslinking agents, bisaminothiophenol-based crosslinking agents, and bisdiaminophenyl-based crosslinking agents have conventionally been used in crosslinking systems using cyano groups as crosslinking points, but they also react with carboxyl groups and alkoxycarbonyl groups to form oxazole rings, thiazole rings, and imidazole rings, thereby giving crosslinked products.

[0111] The crosslinking agent may be a compound represented by the general formula (46): X 41 - (CH 2 ) n -R 50 - (CH 2 ) m -X 41 (In the formula, X 41 each independently represents an alkyne group, a nitrile group, or Y 41 P N 3 (Y 41 SO, SO 2 , C 6 H 4 or CO, and p is 0 or 1, n and m are independently integers of 1 to 4, and R 50 The crosslinking agent may be selected from the group consisting of: i) a fluoroalkylene group having 3 to 10 carbon atoms, ii) a fluoroalkoxylene group having 3 to 10 carbon atoms, iii) a substituted arylene group, iv) an oligomer containing copolymerized units of vinylidene fluoride and perfluoro(methyl vinyl ether), v) an oligomer containing copolymerized units of vinylidene fluoride and hexafluoropropylene, vi) an oligomer containing copolymerized units of tetrafluoroethylene and perfluoro(methyl vinyl ether), and vii) an oligomer containing copolymerized units of tetrafluoroethylene and a hydrocarbon olefin. This crosslinking agent is preferably used together with a perfluoroelastomer having a nitrile group, an azide group, a sulfonyl azide group, a carbonyl azide group, or an alkyne group. For example, the nitrile group of the perfluoroelastomer reacts with the azide group of the crosslinking agent to form a tetrazole ring, resulting in a crosslinked product.

[0112] Particularly preferred crosslinking agents include compounds having a plurality of 3-amino-4-hydroxyphenyl groups or 3-amino-4-mercaptophenyl groups, or compounds represented by the general formula (47):

[0113]

[0114] (In the formula, R 41 , R 42 and R 43 are as described above), and specific examples thereof include 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (general name: bis(aminophenol) AF), 2,2-bis(3-amino-4-mercaptophenyl)hexafluoropropane, tetraaminobenzene, bis-3,4-diaminophenylmethane, bis-3,4-diaminophenyl ether, 2,2-bis(3,4-diaminophenyl)hexafluoropropane, 2,2-bis[3-amino-4-(N-phenylamino)phenyl] [3-amino-4-(N-methylamino)phenyl]hexafluoropropane, 2,2-bis[3-amino-4-(N-ethylamino)phenyl]hexafluoropropane, 2,2-bis[3-amino-4-(N-propylamino)phenyl]hexafluoropropane, 2,2-bis[3-amino-4-(N-perfluorophenylamino)phenyl]hexafluoropropane, 2,2-bis[3-amino-4-(N-benzylamino)phenyl]hexafluoropropane, and the like.

[0115] Among these, 2,2-bis[3-amino-4-(N-phenylamino)phenyl]hexafluoropropane is preferred as the crosslinking agent from the viewpoints of heat resistance, steam resistance, amine resistance and good crosslinking properties.

[0116] The content of at least one selected from the group consisting of inorganic nitrides, organotin compounds, compounds that generate ammonia, and crosslinking agents is preferably 0.05 to 10 parts by mass, more preferably 0.1 to 5.0 parts by mass, even more preferably 0.2 to 2.0 parts by mass, and particularly preferably 0.3 to 1.0 part by mass, relative to 100 parts by mass of the perfluoroelastomer.

[0117] The composition can be prepared by mixing the above components using a conventional polymer processing machine, such as an open roll, a Banbury mixer, or a kneader. Alternatively, it can be prepared by a method using an internal mixer. The composition can be suitably used as a molding material for crosslinking and molding to obtain a crosslinked product.

[0118] <Crosslinked Product> A crosslinked product can be obtained by crosslinking the composition of the present disclosure. 2 Plasma durability and CF 4 It has excellent durability against plasma and exhibits small compression set even when used at high temperatures exceeding 300°C.

[0119] The crosslinked product of the present disclosure preferably has a compression set of 50% or less, more preferably 46% or less, measured by leaving it at 300°C for 70 hours at a compression rate of 25%. The compression set can be calculated by leaving the crosslinked product compressed at a compression rate of 25% at 300°C for 70 hours, further leaving it at 70°C for 24 hours, releasing the compression, leaving it at 20°C for 30 minutes, and then measuring the thickness of the crosslinked product before and after compression.

[0120] A method for obtaining a crosslinked product from the composition includes a method in which the composition is molded as a molding material to obtain a preform, and then the preform is crosslinked. A preform can be obtained from the composition by a conventional method, and can be performed by known methods such as a method of heating and compressing in a mold, a method of forcing into a heated mold, or a method of extruding with an extruder. In the case of extruded products such as hoses and electric wires, a crosslinked product can be obtained by performing heat crosslinking with steam or the like after extrusion.

[0121] The crosslinking can be carried out in the order of primary crosslinking and secondary crosslinking. The primary crosslinking is preferably carried out at 150 to 250°C for 5 to 120 minutes, and more preferably at 170 to 200°C for 5 to 60 minutes. Any known crosslinking means may be used for the crosslinking, and examples thereof include press crosslinking.

[0122] The secondary crosslinking is preferably carried out at 200 to 320°C for 2 to 48 hours, more preferably at 250 to 310°C for 5 to 24 hours. The temperature may be varied within this temperature range. Any known crosslinking method may be used, such as oven crosslinking. The crosslinking atmosphere may be air or an inert atmosphere such as nitrogen.

[0123] The crosslinked product of the present disclosure can be suitably used as a sealing material for semiconductor manufacturing equipment that requires high heat resistance, particularly semiconductor manufacturing equipment that is exposed to high-density plasma. Examples of such sealing materials include O-rings, square rings, gaskets, packing, oil seals, bearing seals, and lip seals. It can also be used for various polymer products used in semiconductor manufacturing equipment, such as diaphragms, tubes, hoses, various rubber rolls, and belts. It can also be used as a coating material or a lining material.

[0124] It should be noted that the semiconductor manufacturing equipment referred to in this disclosure is not limited to equipment specifically for manufacturing semiconductors, but broadly includes all manufacturing equipment used in the semiconductor field that requires a high degree of cleanliness, such as equipment for manufacturing liquid crystal panels and plasma panels, and examples thereof include the following:

[0125] (1) Etching equipment Dry etching equipment Plasma etching equipment Reactive ion etching equipment Reactive ion beam etching equipment Sputter etching equipment Ion beam etching equipment Wet etching equipment Ashing equipment (2) Cleaning equipment Dry etching cleaning equipment UV / O 3 Cleaning equipment Ion beam cleaning equipment Laser beam cleaning equipment Plasma cleaning equipment Gas etching cleaning equipment Extraction cleaning equipment Soxhlet extraction cleaning equipment High temperature and high pressure extraction cleaning equipment Microwave extraction cleaning equipment Supercritical extraction cleaning equipment (3) Exposure equipment Stepper Coater / Developer (4) Polishing equipment CMP equipment (5) Film formation equipment CVD equipment Sputtering equipment (6) Diffusion / ion implantation equipment Oxidation diffusion equipment Ion implantation equipment

[0126] The crosslinked product of the present disclosure exhibits excellent performance as a sealing material for, for example, a CVD apparatus, a plasma etching apparatus, a reactive ion etching apparatus, an ashing apparatus, or an excimer laser exposure apparatus.

[0127] Although the embodiments have been described above, it will be understood that various changes in form and details can be made without departing from the spirit and scope of the claims.

[0128] Next, embodiments of the present disclosure will be described with reference to examples, but the present disclosure is not limited to these examples.

[0129] The values ​​in the examples were measured by the following methods.

[0130] (Perfluoroelastomer composition) 19 It was determined by F-NMR analysis.

[0131] (Mooney Viscosity of Perfluoroelastomer) Measurement was carried out at 170° C. in accordance with JIS K6300 using a Mooney viscometer MV2000E manufactured by ALPHA TECHNOLOGIES.

[0132] (BET Specific Surface Area of ​​Filler (Nitrogen Adsorption Method, Water Vapor Adsorption Method)) The BET specific surface area of ​​the filler determined by the nitrogen adsorption method was determined by the BET flow method (single-point method) using nitrogen gas and a mixed gas (30% nitrogen + 70% helium) using a fully automatic BET specific surface area measuring device Macsorb HM-1208 manufactured by Mountech Co., Ltd. The BET specific surface area of ​​the filler determined by the water vapor adsorption method was determined by vacuum degassing the filler at 100°C for 3 hours, and then determining the water vapor adsorption isotherm at 25°C using a high-precision gas / vapor adsorption measuring device BELLSORP-max II manufactured by Microtrac-Bell, and analyzing this isotherm by the BET method.

[0133] (Ratio (Water Vapor / Nitrogen)) The ratio (Water Vapor / Nitrogen) was calculated from the BET specific surface area of ​​the filler measured above according to the following formula. A filler showing a high ratio (Water Vapor / Nitrogen) has a high degree of hydrophilicity. Ratio (Water Vapor / Nitrogen) (%) = (BET specific surface area determined by water vapor adsorption method) / (BET specific surface area determined by nitrogen adsorption method) × 100

[0134] (Graphite Content (Weight Reduction Rate of Filler)) The graphite content was determined by heating the filler in air at 10°C / min to 1,000°C using a simultaneous differential thermogravimetry analyzer STA7200 manufactured by Hitachi High-Tech Science Corporation, and was the value at which the weight was reduced to its maximum.

[0135] (Bulk Density of Filler) 5 g of powder was placed in a 100 ml measuring cylinder (inner diameter 28 mm), and the cylinder was tapped 20 times from a height of 2 cm, after which the scale was read and the bulk density was calculated from the volume.

[0136] (Average particle diameter of filler) From the specific surface area (BET value) obtained using a fully automatic BET specific surface area measuring device Macsorb HM-1208 manufactured by Mountech Co., Ltd., average particle diameter (nm) = 6000 / (specific surface area (m 2 / g) x true density (g / cm 3 The true density was calculated from the true density of silicon carbide, 3.22 g / cm 3 was used.

[0137] (X-ray Photoelectron Spectroscopy Measurement) Surface elemental analysis of the filler (SiC particles) was performed using an X-ray photoelectron spectrometer ESCA-3400 (manufactured by Shimadzu Corporation). The measurement was performed with the filler attached to carbon tape. The measurement conditions were X-ray: Mg-Kα radiation, 10 mA, 8 kV, measurement area: 3 mmφ. Peak separation processing was performed using data analysis software (Vision2 (Vision Processing)). Background processing was performed using the linear method, and curve fitting using the nonlinear least squares method was used for peak separation. The spectral structure was divided into a total of four peaks and fitted. For the C1s peak, the peak positions were 283.5 ± 0.5 eV, 284.8 ± 0.6 eV, 286.0 ± 0.5 eV, and 289.1 ± 0.5 eV, in order of decreasing binding energy. The peak at 283.5±0.5 eV was determined to be a peak derived from SiC, and the peak at 284.8±0.6 eV was determined to be a peak derived from graphite. Based on the results of the peak separation treatment, the ratio of the area of ​​the peak derived from graphite to the area of ​​the peak derived from SiC (graphite peak area / SiC peak area) was calculated.

[0138] (Compression set) Compression set was measured in accordance with the method described in ASTM D395 or JIS K6262. The O-rings produced in the examples and comparative examples were compressed to a compression rate of 25% at room temperature using a compression device (an O-ring with a thickness (wire diameter) of 3.5 mm was compressed to a thickness of 2.625 mm). Next, the compression device with the compressed O-ring fixed thereto was placed in an electric furnace and left at 300°C for 70 hours or 168 hours, and then the compression device was removed from the electric furnace. Thereafter, the compression device with the compressed O-ring fixed thereto was placed in another electric furnace and left at 70°C for 24 hours. The O-ring was removed from the compression device, and the removed O-ring was placed in a constant temperature room and left at 23°C for 30 minutes, and the thickness (t 2 The compression set was calculated using the following formula: Compression set (%) = (t 0 -t 2 ) / (t 0 -t 1 ) x 100 t 0 t: Original thickness of O-ring (mm) 1 t: Spacer thickness (mm) 2 : Thickness of the O-ring after compression test (mm) In the above test, t 0 = 3.5 mm, t 1 = 2.625 mm.

[0139] (Plasma resistance (weight loss rate of cross-linked product before and after plasma treatment)) The O-rings (P24 size) produced in the examples and comparative examples were placed in a process chamber. Plasma generated using a radical generator was sent into the process chamber, and the O-rings were irradiated with plasma under the following plasma irradiation conditions. The O-ring mass was calculated from the mass of the O-ring before and after plasma irradiation. 2 and C.F. 4 The ICP plasma weight loss rate was calculated.

[0140] (Plasma irradiation conditions) Radical generator: ICP high density plasma device (RIE-101iPH manufactured by SAMCO) Gas flow rate: 16 sccm Power: 400 W Pressure: 2.66 Pa Irradiation time: 1 hour

[0141] (Plasma resistance (amount of particles generated)) An O-ring (P24 size) was irradiated with plasma in the same manner as above. The mass of the O-ring after plasma irradiation was measured, and then the O-ring after plasma irradiation was wiped with a nonwoven fabric impregnated with ethanol to remove particles present on the surface, and then dried in an oven at 150°C for 1 hour, and the mass of the O-ring was measured again. The difference in mass before and after wiping corresponds to the mass of surface particles. The ratio of the mass of surface particles to the mass before wiping (amount of particles generated) was calculated.

[0142] The following materials were used in the examples and comparative examples: Perfluoroelastomer: TFE / PMVE / CF 2 = CFOCF 2 CF (CF 3 ) OCF 2 CF 2 CN = 59.3 / 39.9 / 0.8 ​​(mol %), Mooney viscosity ML(1+20)(170°C) = 66

[0143] Crosslinker: 2,2-bis[3-amino-4-(N-phenylamino)phenyl]hexafluoropropane

[0144] Fillers Fillers 1 to 4: graphite-coated silicon carbide Filler 5: silicon carbide Filler 6: silicon carbide (DU A-1 manufactured by Showa Denko K.K.)

[0145] The physical properties of each filler are shown in Table 1.

[0146]

[0147] Examples 1 to 4 and Comparative Examples 1 and 2 100 parts by mass of perfluoroelastomer, 15 parts by mass of filler, and 0.8 parts by mass of crosslinking agent were kneaded with an open roll to prepare a composition.

[0148] The resulting composition was pressed at 180°C for 30 minutes to crosslink, and then further oven-crosslinked in an air oven at 290°C for 18 hours to produce P24 size O-rings. The resulting O-rings were used to measure the compression set, ICP plasma weight loss rate, and particle generation amount using the methods described above. The results are shown in Table 2.

[0149]

Claims

1. A composition containing a perfluoroelastomer and a filler, wherein the filler contains silicon carbide and graphite, and the ratio of the area (C) of a peak derived from the graphite in the filler to the area (SiC) of a peak derived from the silicon carbide in the filler (area (C) / area (SiC)) measured by X-ray photoelectron spectroscopy (XPS) is 0.7 or more.

2. The BET specific surface area of ​​the filler determined by the nitrogen adsorption method is 15 to 200 m 2 The composition of claim 1, wherein the molecular weight is 1 / g.

3. 3. The composition according to claim 1, wherein a ratio (water vapor / nitrogen) of a BET specific surface area of ​​the filler determined by a water vapor adsorption method to a BET specific surface area of ​​the filler determined by a nitrogen adsorption method is 1 to 60%.

4. The bulk density of the filler is 0.10 g / cm 3 The composition according to claim 1 or 2, wherein

5. 3. The composition according to claim 1, wherein the content of the filler is 0.1 to 100 parts by mass based on 100 parts by mass of the perfluoroelastomer.

6. 3. The composition according to claim 1, further comprising at least one member selected from the group consisting of inorganic nitrides, organotin compounds, compounds that generate ammonia, and crosslinking agents.

7. A crosslinked product obtained by crosslinking the composition according to claim 1 or 2.

8. The crosslinked product according to claim 7, which is a sealing material.

9. 8. The crosslinked product according to claim 7, which has a compression set of 50% or less when measured by leaving it at 300° C. for 70 hours at a compression ratio of 25%.