Labeled container and method for manufacturing the same

JPWO2023189983A5Active Publication Date: 2024-11-11株式会社ユポ
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024512242
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-23
Filing Date
2023-03-23
Publication Date
2024-11-11
Estimated Expiration
2043-03-23

AI Technical Summary

Technical Problem

Stretch blow molding of large containers can cause stress on in-mold labels, leading to distortion and reduced aesthetic appeal due to differences in dimensions between the preform and the molded container.

Method used

Adjust the orientation of in-mold labels with a tensile strength of 10 kN/m or more to align with the direction of stress, use a heated preform at 105°C or higher, and control gas pressure to 3.5 MPa or less during the blow molding process, with optional vertical stretching by a rod to minimize label distortion.

Benefits of technology

The method reduces label distortion and maintains the appearance of the label even when the container dimensions are relatively large, ensuring minimal changes in the label's appearance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a labeled container and a method for manufacturing the same.

Background Art

[0002] As a method for molding a hollow resin container, blow molding is known, in which air is blown into molten resin in a mold and expanded to form the shape of the mold. Blow molding includes a direct blow method and a stretch blow method. In the direct blow method, a parison of raw material resin is used, and after heating and melting the parison above its melting point, air pressure is applied to expand it.

[0003] On the other hand, in the stretch blow method using a preform of raw material resin, the preform is heated to near its softening point and then expanded by applying air pressure. Generally, the stretch blow method is used for raw material resins such as polyethylene terephthalate.

[0004] As a label for a resin container to be blow molded, an in-mold label is known. The in-mold label is adhered to the surface of the resin container by the heat of the heated and melted raw material resin. For example, an in-mold label in which a heat-sensitive adhesive layer containing an ethylene-vinyl acetate copolymer is laminated on a polypropylene film is used for a polyethylene container (see, for example, Patent Document 1).

[0005] In addition, an in-mold label has been proposed which includes a heat-sealable resin layer containing a polyethylene-based resin on a base material layer, and the adhesiveness to polyethylene terephthalate is enhanced by surface oxidation treatment of the heat-sealable resin layer (see, for example, Patent Document 2).

Prior Art Documents

Patent Documents

[0006]

Patent Document 1

Patent Document 2

[0007] When attempting to mold a container relatively large relative to the dimensions of the preform using the stretch blow method, stress can be generated within the mold as the preform expands, attempting to stretch the in-mold label. This stretching and deformation of the in-mold label's printed layer can result in issues affecting the appearance, such as unclear printing or reduced aesthetic appeal.

[0008] The present invention aims to provide a method for manufacturing labeled containers in which the appearance of the label is less altered even when the dimensions are relatively large. [Means for solving the problem]

[0009] As a result of diligent research conducted by the inventors to solve the above problems, the present invention has been completed as follows.

[0010] [1] An arrangement step of placing an in-mold label on the inner wall surface of the mold, A preparation step for preparing a heated preform that has a cavity inside, An insertion step of inserting the preform into the mold, The process includes a blow step of forming a labeled container to which the in-mold label is attached by blowing gas into the cavity of the preform and inflating the preform, The in-mold label has a tensile strength of 10 kN / m or more in one direction. A method for manufacturing a labeled container, wherein the arrangement step includes the following step (a) or step (b) for adjusting the orientation of the in-mold label. (a) If the dimensions of the labeled container in the horizontal direction are at least twice the dimensions of the preform, and the dimensions of the labeled container in the depth direction are at least once and less than twice the dimensions of the preform, then the step of aligning one direction of the in-mold label substantially with the horizontal direction. (b) If the dimensions of the labeled container in the horizontal direction are 1 to 2 times the dimensions of the preform, and the dimensions of the labeled container in the depth direction are 1 to 2 times the dimensions of the preform, then the step of substantially aligning one direction of the in-mold label with the vertical direction.

[0011] [2] The in-mold label has a tensile strength of 12 kN / m or more in the one direction. A method for manufacturing the labeled container described in [1] above.

[0012] [3] The temperature of the heated preform is 105°C or higher. A method for manufacturing a labeled container as described in [1] or [2] above.

[0013] [4] The pressure of the gas blown in during the blowing process is 3.5 MPa or less. A method for manufacturing a labeled container as described in any of the above [1] to [3].

[0014] [5] If the orientation of the in-mold label is adjusted by step (b), and a rod is inserted into the cavity of the preform during the blowing process, and the preform is stretched vertically by the rod, the blowing of the gas is started after the length of the inserted portion of the rod exceeds half the vertical dimension of the labeled container. A method for manufacturing a labeled container as described in any of the above [1] to [4].

[0015] [6] The in-mold label includes a stretched layer. A method for manufacturing a labeled container as described in any of the above [1] to [5].

[0016] [7] The in-mold label has a thickness of 50 to 300 μm. The method for manufacturing a labeled container according to any one of [1] to [6] above.

[0017] [8] A container having a neck portion and a body portion, and an in-mold label adhered to the outer surface of the body portion. The in-mold label has a tensile strength of 10 kN / m or more in one direction, A labeled container that satisfies the following condition (I) or the following condition (II). (I) In the horizontal direction, the ratio of the dimension of the body portion to the dimension of the neck portion is 2 or more, in the depth direction, the ratio of the dimension of the body portion to the dimension of the neck portion is 1 or more and less than 2, and the one direction of the in-mold label substantially coincides with the horizontal direction (II) In the horizontal direction, the ratio of the dimension of the body portion to the dimension of the neck portion is 1 or more and less than 2, in the depth direction, the ratio of the dimension of the body portion to the dimension of the neck portion is 1 or more and less than 2, and the one direction of the in-mold label substantially coincides with the vertical direction [Advantages of the Invention]

[0018] According to the present invention, it is possible to provide a method for manufacturing a labeled container with little change in the appearance of the label even when the dimensions are relatively large. [Brief Description of the Drawings]

[0019] [Figure 1a] It is a cross-sectional view of a preform expanding in a substantially square mold as viewed from the vertical direction. [Figure 1b] It is a cross-sectional view of a preform expanding in a substantially rectangular mold as viewed from the vertical direction. [Figure 2] It is a perspective view showing an α-type labeled container and a preform used for its manufacture. [Figure 3] It is a perspective view showing a β-type labeled container and a preform used for its manufacture. [Figure 4]This is a perspective view showing a γ-type labeled container and the preform used in its manufacture. [Figure 5a] This diagram shows the expansion process of the preform when the timing of gas injection is simultaneous with the start of rod insertion. [Figure 5b] This figure shows the expansion process of the preform when the timing of gas injection is adjusted. [Modes for carrying out the invention]

[0020] The following describes in detail the labeled container and its manufacturing method according to the present invention. The following description is an example (representative example) of the present invention and is not limited thereto. In the following explanation, the term "(meth)acrylic" refers to both acrylic and methacrylic.

[0021] (Method of manufacturing labeled containers) The method for manufacturing a labeled container according to the present invention includes the following steps. (S1) Placement process for placing the in-mold label on the inner wall surface of the mold. (S2) Preparation step of preparing a heated preform having an internal cavity. (S3) Insertion process in which the heated preform is inserted into the mold. (S4) A blow process in which gas is blown into the cavity of the preform to inflate the preform and form a labeled container with an in-mold label attached. The following describes each step.

[0022] <Placement process> In the placement step (S1), an in-mold label is inserted into the mold used for forming the container and placed on its inner wall surface. The position of the in-mold label may be fixed by making it adhere to the inner wall surface by suction or static electricity.

[0023] During the blow molding process (S4), the expanding preform can generate stress that stretches the in-mold label. If a large stress acts in one direction, it can disrupt the aspect ratio of the label, causing distortion of the printed content and significantly altering the appearance of the label on the labeled container. This stress, which alters the label's appearance, can arise from the dimensional difference between the preform and the molded container.

[0024] Figures 1a and 1b are cross-sectional views of the preform 10 expanding in molds 51 and 52, viewed from the vertical z direction. The preform 10 before expansion is represented by the dotted line. The horizontal x, depth y, and vertical z directions are orthogonal to each other.

[0025] As shown in Figure 1a, the expanded preform 10 is pressed against the inner wall surface of the mold 51 and molded into the same shape as the internal shape of the mold 51. An in-mold label (hereinafter sometimes simply referred to as the label) 20 is placed on the inner wall surface of the mold 51. When the label 20 comes into contact with the preform 10 pressed against the inner wall surface, it adheres to its outer surface due to the heat of the preform 10. Subsequently, the further expanding preform 10 generates stress that attempts to stretch the label 20. The arrows in the figure indicate the direction in which the stress acts.

[0026] According to mold 51 in Figure 1a, the dimensions in the horizontal direction x and the depth direction y are approximately the same, and a container with a square cross-section is formed. In contrast, when using mold 52 shown in Figure 1b to form a flat container with a rectangular cross-section that is long in the horizontal direction x, the preform 10 has more room to expand in the horizontal direction x compared to the case of a square shape. Therefore, the stress that tries to stretch the label 20 in the horizontal direction x is greater than when using mold 51, and distortion is more likely to occur in the appearance of the label.

[0027] In the direct blow method, the parison resin is fully melted at high temperatures, resulting in a flexible parison that easily conforms to the mold's shape, and thus the stress applied to the label is relatively small. In contrast, the stretch blow method does not use raw resin that has been molten at high temperatures like a parison, but rather uses the raw resin as a preform. The preform remains in a softened state, maintained at a relatively low temperature. Because the preform has a higher viscosity than the parison, a stronger blowing pressure is required than in the direct blow method. As a result, the stress applied to the label is stronger in the stretch blow method compared to the direct blow method, and the label's appearance tends to change more easily.

[0028] As shown in Figures 2 to 4, the labeled containers 30, which may exhibit changes in the appearance of the labels, are broadly classified into three types, α, β, and γ, based on the dimensional difference from the preform 10. The preform 10 and the labeled containers 30 are arranged so that the long side of the bottom surface coincides with the horizontal direction x, and the in-mold label 20 is placed on the surface formed by the horizontal direction x and the vertical direction z of the labeled container 30.

[0029] As shown in Figures 2 to 4, the preform 10 has a cavity inside and is usually a bottomed cylindrical molded body. The preform 10 comprises a neck portion 11, a body portion 12, and a fringe 13. The labeled container 30 comprises a neck portion 31, a body portion 32, and an in-mold label 20 attached to the outer surface of the body portion 32.

[0030] The preform 10 is fixed to the mold by the engagement of the fringe 13 with the opening periphery of the mold after the body 12 is inserted into the mold. In the blow blowing process (S4), the body 12 inside the mold below the fringe 13 expands and stretches, forming the body 32 of the labeled container 30. Since the neck 11 of the preform 10 is not stretched in the blow blowing process (S4), the dimensions of the neck 31 of the labeled container 30 are the same as those of the neck 11 of the preform 10. A spiral groove can be provided along the circumferential direction on the outer circumference of the necks 11 and 31, allowing them to be fitted with a cap having a similar structure.

[0031] <<α type>> As shown in Figure 2, the α-type labeled container 30 has a flattened cross-section, with the horizontal dimension Dx being larger than the depth dimension Dy. In the α-type, a flattened shape means, for example, that the ratio of the horizontal dimension Dx to the depth dimension Dy of the body 32 (flattening ratio Dx / Dy) is 1.6 or greater. The flattening ratio Dx / Dy can be, for example, 5.0 or less. In the α type, a preform 10 is used to manufacture the labeled container 30 in which the horizontal dimension dx of the body 12 in the x direction and the depth dimension dy in the y direction are approximately the same. As a result, the stretch ratio in the horizontal direction x (Dx / dx) of the labeled container 30 produced by stretch blow molding is high, and the stretch ratio in the depth direction y (Dy / dy) is low.

[0032] Specifically, in the α-type labeled container 30, the horizontal dimension Dx in the x direction and the depth dimension Dy in the y direction of the body 32 satisfy the following relationship with respect to the horizontal dimension dx in the x direction and the depth dimension dy in the y direction of the body 12 of the preform 10. In this case, the label 20 attached to a surface parallel to the horizontal direction x tends to be stretched in the horizontal direction x. 2 ≤ Dx / dx 1 ≤ Dy / dy < 2

[0033] The above tendency is particularly likely to occur when the stretching ratios in the horizontal x direction and the depth y direction are far apart. Specifically, this occurs when (Dx×dy) / (Dy×dx), which is expressed by the horizontal x dimension Dx and depth y dimension Dy of the body 32, and the horizontal x dimension dx and depth y dimension dy of the body 12 of the preform 10, is 2.0 or greater, 2.5 or greater, or 3.0 or greater. (Dx×dy) / (Dy×dx) can be, for example, 5.0 or less. Similarly, the above tendency is more likely to occur when the stretching ratio (Dz / dz) in the vertical direction z is low. Specifically, a low stretching ratio means that the dimension dz of the body 12 of the preform 10 and the dimension Dz of the body 32 of the labeled container 30 satisfy the following relationship in the vertical direction z. 1 ≤ Dz / dz < 1.5

[0034] As described above, the neck portion 11 of the preform 10 shows almost no change due to blow molding, and the dimensions of the neck portion 11 and 31 are approximately the same (ndx ≈ NDx, ndy ≈ NDy). Therefore, in the α type, the horizontal dimension Dx and depth dimension Dy of the body portion 32 satisfy the following relationship with respect to the horizontal dimension NDx and depth dimension NDy of the neck portion 31. 2 ≤ Dx / NDx 1 ≤ Dy / NDy < 2

[0035] <<β type>> As shown in Figure 3, the β-type labeled container 30 has a roughly square cross-section, and the difference between the dimension Dy in the depth direction y and the dimension Dx in the horizontal direction x is small. Roughly square means, for example, that the ratio of the dimension Dx in the horizontal direction x to the dimension Dy in the depth direction y of the body 32 (flatness ratio Dx / Dy) is less than 1.6. The flatness ratio Dx / Dy can be, for example, 1.0 or more. In the manufacture of the β-type labeled container 30, a preform 10 is used in which the horizontal dimension dx and the depth dimension dy of the body 12 are approximately the same, similar to the α-type. Therefore, the stretch ratio by blow molding is relatively low in both the horizontal x and depth y directions of the labeled container 30.

[0036] Specifically, in the β-type labeled container 30, the horizontal dimension Dx in the x direction and the depth dimension Dy in the y direction of the body 32 satisfy the following relationship with respect to the horizontal dimension dx in the x direction and the depth dimension dy in the y direction of the body 12 of the preform 10. In this case, the label 20 attached to a surface parallel to the horizontal direction x tends to be stretched in the vertical direction z. 1 ≤ Dx / dx < 2 1 ≤ Dy / dy < 2

[0037] The above tendency is particularly likely to occur when the stretching ratios in the horizontal x direction and the depth y direction are close. Specifically, this occurs when (Dx×dy) / (Dy×dx), which is expressed by the horizontal x dimension Dx and depth y dimension Dy of the body 32, and the horizontal x dimension dx and depth y dimension dy of the body 12 of the preform 10, is less than 2.0, less than 1.7, or less than 1.4. (Dx×dy) / (Dy×dx) can be, for example, 1.0 or more. Similarly, the above tendency is more likely to occur when the stretching ratio in the vertical direction z is high. Specifically, a high stretching ratio means that the dimension dz of the body 12 of the preform 10 and the dimension Dz of the body 32 of the labeled container 30 satisfy the following relationship in the vertical direction z. 1.5 ≤ Dz / dz

[0038] In the β type as well, the dimensions of the neck sections 11 and 31 are approximately the same (ndx ≈ NDx, ndy ≈ NDy). Therefore, in the β type, the horizontal dimension Dx and depth dimension Dy of the body section 32 satisfy the following relationship with respect to the horizontal dimension NDx and depth dimension NDy of the neck section 31. 1 ≤ Dx / NDx < 2 1 ≤ Dy / NDy < 2

[0039] <<γ type>> As shown in Figure 4, the γ-type labeled container 30 has a flattened shape similar to the α-type, but the preform 10 also has a flattened shape, and the horizontal dimension dx of the body 12 is longer than the depth dimension dy. Similarly, the neck 11 has a dimension ndy that is longer than the dimension ndx. Therefore, the γ-type is similar to the α-type in the shape of the labeled container 30, but is similar to the β-type in that the stretching ratio in the horizontal x and depth y directions by blow molding is low. A flattened shape is defined as, for example, a case where the ratio of the horizontal dimension Dx to the depth dimension Dy of the body 32 (flattening ratio Dx / Dy) is 1.6 or more. The flattening ratio Dx / Dy can be, for example, 5.0 or less.

[0040] In the γ type, the dimensions Dx in the horizontal x direction and Dy in the depth direction of the body 32 of the labeled container 30 satisfy the following relationship with respect to the dimensions dx in the horizontal x direction and dy in the depth direction of the body 12 of the preform 10. In this case, the label 20 attached to a surface parallel to the horizontal x direction tends to be stretched in the vertical z direction, similar to the β type. 1 ≤ Dx / dx < 2 1 ≤ Dy / dy < 2

[0041] The above tendency is particularly likely to occur when the stretching ratios in the horizontal x direction and the depth y direction are close. Specifically, this occurs when (Dx×dy) / (Dy×dx), which is expressed by the horizontal x dimension Dx and depth y dimension Dy of the body 32, and the horizontal x dimension dx and depth y dimension dy of the body 12 of the preform 10, is less than 2.0, less than 1.8, or less than 1.6. (Dx×dy) / (Dy×dx) can be, for example, 1.0 or more. Similarly, the above tendency is more likely to occur when the stretching ratio in the vertical direction z is high. A high stretching ratio is defined as the case where the dimension dz of the body 12 of the preform 10 and the dimension Dz of the body 32 of the labeled container 30 satisfy the following relationship in the vertical direction z. 1.5 ≤ Dz / dz

[0042] In the γ type as well, the dimensions of the neck sections 11 and 31 are approximately the same (ndx ≈ NDx, ndy ≈ NDy). Therefore, in the γ type, the horizontal dimension Dx and depth dimension Dy of the body section 32 satisfy the following relationship with respect to the horizontal dimension NDx and depth dimension NDy of the neck section 31. 1 ≤ Dx / NDx < 2 1 ≤ Dy / NDy < 2

[0043] In this invention, an in-mold label having a tensile strength of 10 kN / m or more in one direction is used, and the direction in which the tensile strength of this in-mold label is high is made to substantially coincide with the direction in which stress acts for each α to γ ​​type. As a result, the label is less likely to be stretched in the direction in which stress acts, and the deformation of the label can be reduced.

[0044] Specifically, in the manufacturing method of the present invention, the in-mold label placement step (S1) includes the following step (a) or step (b) for adjusting the orientation of the in-mold label. (a) When the dimensions (Dx) of the labeled container in the horizontal direction (x) are at least twice the dimensions (dx) of the preform, and the dimensions (Dy) of the labeled container in the depth direction (y) are between one and two times the dimensions (dy) of the preform, the process of approximately aligning one direction of the in-mold label's tensile strength of 10 kN / m or more with the horizontal direction (x). (b) When the dimensions (Dx) of the labeled container in the horizontal direction (x) are between 1 and 2 times the dimensions (dx) of the preform, and the dimensions (Dy) of the labeled container in the depth direction (y) are between 1 and 2 times the dimensions (dy) of the preform, the process of aligning one direction in which the tensile strength of the in-mold label is 10 kN / m or more with the vertical direction (z).

[0045] In this specification, "approximately identical" means, for example, that the angle between one direction of the in-mold label and the horizontal direction x or vertical direction z is in the range of 0 to 5°, 0 to 10°, 0 to 15°, or 0 to 30°.

[0046] As described above, the α type satisfies the conditions of process (a), and therefore the orientation of the in-mold label is adjusted by process (a). In the α type, stress acts in the horizontal direction x, but according to process (a), the in-mold label is less likely to be stretched in the horizontal direction x in response to this stress, thus reducing changes in the appearance of the label.

[0047] On the other hand, since types β and γ satisfy the conditions of process (b), the orientation of the in-mold label is adjusted by process (b). In types β and γ, stress acts in the vertical direction z, but according to process (b), the in-mold label is less likely to be stretched in the vertical direction z against this stress, thus reducing changes in the appearance of the label.

[0048] <Preparation process> In the preparation step (S2), a heated preform is prepared by molding a preform from a heated and molten raw resin. Alternatively, a preform that has been molded in advance and stored at room temperature is heated using a heating device such as a heater. The heated preform softens and expands in the blow blowing step (S4) due to the gas pressure applied to the cavity inside the preform. Generally, the preform is heated to a temperature near its softening point, but not exceeding the melting point of the raw resin. From the viewpoint of sufficient softening, for example, it is preferable that the temperature of the heated preform be 90°C or higher.

[0049] In particular, the temperature of the heated preform is preferably 95°C or higher, more preferably 100°C or higher, and even more preferably 105°C or higher. If the temperature of the preform is 105°C or higher, the preform becomes softer and more pliable. This can reduce the stress applied to the label when the preform expands, and further reduce changes in the appearance of the label. From the viewpoint of stable container moldability, the temperature of the heated preform is preferably 120°C or lower, and more preferably 110°C or lower.

[0050] <Insertion Process> In the insertion process (S3), the heated preform is inserted into the mold. The body of the preform is positioned inside the mold, and the neck is positioned outside the mold.

[0051] <Blow-drying process> In the blowing process (S4), gas is blown into the cavity of the preform, and the preform expands due to the pressure (hereinafter sometimes referred to as blowing pressure). In the blowing process (S4), a rod may be used for vertical stretching. When a rod is used, the rod is inserted vertically into the cavity of the preform. The bottom of the preform is pushed by the rod, and the body of the preform is stretched vertically downward.

[0052] The greater the blow pressure, the greater the stress applied to the label due to the expansion of the preform. Therefore, from the viewpoint of reducing the stress applied to the label, the blow pressure in the blowing process is preferably 3.5 MPa or less, more preferably 3.0 MPa or less, even more preferably 2.7 MPa or less, and particularly preferably 2.3 MPa or less. From the viewpoint of moldability, the above blow pressure is usually 0.5 MPa or more, and preferably 1.0 MPa or more.

[0053] The blowing time for injecting gas can be set according to molding conditions such as the temperature of the preform and the blowing pressure. When the blowing pressure is 4.0 MPa or less as described above, the blowing time is preferably 3 seconds or more, more preferably 5 seconds or more, from the viewpoint of sufficient expansion, and preferably 10 seconds or less, more preferably 8 seconds or less, from the viewpoint of reducing the stress applied to the label.

[0054] In the positioning step (S1), the orientation of the in-mold label is adjusted by step (b) above, and in the blowing step (S4), the preform is stretched by a rod. In this case, it is preferable to adjust the timing of starting gas injection in the blowing step (S4) to coincide with the insertion position of the rod. Specifically, gas injection is started after the length of the rod insertion portion exceeds preferably 1 / 2, more preferably 3 / 4, of the vertical dimension of the labeled container. This also reduces the stress applied to the label in the vertical direction due to the expansion of the preform.

[0055] As shown in Figure 5a, when gas is injected into the preform 10 placed in the mold 50 at the same time as the stretching by the rod 55 begins, the preform 10 expands in the vertical direction z upward and comes into contact with the label 20 placed on the inner wall surface of the mold 50. Even after the preform 10 comes into contact with the label 20, stress is generated that stretches the preform 10 in the vertical direction z downward, from the rod 55 and the injection of gas to the label 20.

[0056] On the other hand, as shown in Figure 5b, by delaying the timing of starting gas injection compared to the start of stretching by the rod 55, the stretching of the preform 10 by the rod 55 can proceed before contact between the preform 10 and the label 20 on the upper side in the vertical z direction. This makes it less likely for the label 20 to be stretched due to the expansion of the preform 10. By starting gas injection after the length of the insertion portion of the rod 55 exceeds 1 / 2Dz of the vertical z dimension of the labeled container 30 to be molded, the preform 10 expands and makes contact with the label 20 across its entire surface at once, thereby reducing the stress applied from the preform to the label 20.

[0057] (Labeled container) The labeled container of the present invention is manufactured by the manufacturing method described above. The labeled container of the present invention comprises a neck portion, a body portion, and an in-mold label attached to the outer surface of the body portion, as illustrated in Figures 2 to 4. This in-mold label has a tensile strength of 10 kN / m or more in one direction, and its orientation is adjusted in step (a) or step (b) described above.

[0058] As described above, the neck of the labeled container is not stretched by the blow-blowing process and has the same dimensions as the neck of the preform. Therefore, the labeled container of the present invention satisfies either condition (I) or condition (II) below. (I) In the horizontal direction (x), the ratio of the body dimension (Dx) to the neck dimension (NDx) (Dx / NDx) is 2 or more, and in the depth direction (y), the ratio of the body dimension (Dy) to the neck dimension (NDy) (Dy / NDy) is 1 or more and less than 2, and one direction in which the tensile strength of the in-mold label is 10 kN / m or more approximately coincides with the horizontal direction (x). (II) In the horizontal direction (x), the ratio of the body dimension (Dx) to the neck dimension (NDx) (Dx / NDx) is 1 or more and less than 2, and in the depth direction (y), the ratio of the body dimension (Dy) to the neck dimension (NDy) (Dy / NDy) is 1 or more and less than 2, and one direction in which the tensile strength of the in-mold label is 10 kN / m or more approximately coincides with the vertical direction (z).

[0059] <In-mold labels> The in-mold label used in the present invention only needs to have a tensile strength of 10 kN / m or more in at least one direction, and may have a tensile strength of 10 kN / m or more in multiple directions. In this case, it is sufficient that one of the multiple directions coincides with the horizontal direction x in step (a) or with the vertical direction z in step (b). From the viewpoint of reducing deformation of the label's appearance, it is preferable that the direction with the maximum tensile strength among the multiple directions coincides with the horizontal direction x in step (a) or with the vertical direction z in step (b).

[0060] From the viewpoint of further reducing deformation of the label's appearance, the tensile strength of the in-mold label is preferably 12 kN / m or more, more preferably 15 kN / m or more, and even more preferably 18 kN / m or more. From the viewpoint of obtaining an excellent appearance by following the shrinkage after molding of the container, the tensile strength of the in-mold label is preferably 40 kN / m or less, more preferably 35 kN / m or less, and even more preferably 30 kN / m or less. Furthermore, from the viewpoint of manufacturing and quality stability, the tensile strength of the stretched layer in the direction perpendicular to the above-mentioned one direction (especially the mechanical direction (MD)) may be less than 10 kN / m. From a similar viewpoint, the tensile strength in the direction perpendicular to the above-mentioned one direction may be 8 kN / m or less, or 6 kN / m or less.

[0061] In-mold labels are typically laminates comprising a heat-seal layer on a substrate layer. A printed layer consisting of an ink composition may be formed on the surface of the substrate layer opposite the heat-seal layer by printing. In-mold labels may also have a coating layer on the substrate layer to improve adhesion with the ink.

[0062] <<Base material layer>> The base layer is not particularly limited as long as it can impart tensile strength to the label. For example, a thermoplastic resin film or pulp paper can be used as the base layer, and a thermoplastic resin film is preferred from the viewpoint of water resistance, etc. From the viewpoint of producing a white label, the base layer may be a porous film containing a thermoplastic resin and a filler.

[0063] From the viewpoint of controlling the tensile strength within a specific range, the thickness of the base layer is preferably 30 μm or more, more preferably 50 μm or more, and even more preferably 70 μm or more. Similarly, from the viewpoint of controlling the thickness of the base layer is preferably 250 μm or less, more preferably 150 μm or less, and even more preferably 120 μm or less.

[0064] Examples of thermoplastic resins that can be used for the base layer include polyolefin resins, polyester resins, polyvinyl chloride resins, polyamide resins, polystyrene resins, and polycarbonate resins, and one or more of these can be used. From the viewpoint of mechanical strength, polyolefin resins or polyester resins are preferred, and polyolefin resins are more preferred.

[0065] Examples of polyolefin resins that can be used for the base layer include polypropylene resin and polyethylene resin. Among these, polypropylene resin is preferred from the viewpoint of easily obtaining the desired tensile strength at the stretch blow molding temperature, as well as from the viewpoint of moldability and mechanical strength.

[0066] Examples of fillers that can be used in the base layer include inorganic particles such as heavy calcium carbonate, light calcium carbonate, calcined clay, silica, talc, or titanium dioxide, and organic particles such as polyethylene terephthalate, polyamide, polystyrene, or melamine resin.

[0067] Methods for forming the base layer film include extrusion molding (cast molding) using a T-die, inflation molding using an O-die, or calendering using rolling mills. The film may be stretched as needed. Stretching creates numerous fine pores within the film, originating from the filler, resulting in a porous film. Stretching methods include, for example, longitudinal stretching using the difference in peripheral speed of a group of rolls, transverse stretching using a tenter oven, sequential biaxial stretching combining these methods, rolling, simultaneous biaxial stretching using a tenter oven and pantograph, and simultaneous biaxial stretching using a tenter oven and linear motor.

[0068] <<Heat seal layer>> The heat-seal layer melts due to the heat of the preform and adheres to the resin container. Within the mold, the in-mold label is positioned so that the surface with the heat-seal layer faces the preform. A thermoplastic resin film can be used as the heat seal layer. The heat seal layer can use a thermoplastic resin with a lower melting point than the thermoplastic resin in the base layer. Preferably, the melting point of the thermoplastic resin is 10°C or more lower than that of the thermoplastic resin in the base layer, more preferably 20°C or more lower, and even more preferably 30°C or more lower.

[0069] Suitable thermoplastic resins for the heat seal layer include high-density polyethylene, medium-density polyethylene, low-density polyethylene, linear low-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-(meth)acrylic acid copolymer, ethylene-(meth)acrylic acid alkyl ester copolymer (alkyl group has 1 to 8 carbon atoms), and metal salts of ethylene-(meth)acrylic acid copolymer (e.g., salts with metals selected from Zn, Al, Li, K, and Na).

[0070] While known methods can be used to form the heat seal layer, it is preferable to form it by applying a coating liquid. From the viewpoint of ease of process control, suitable solvents for the coating liquid include water; water-soluble solvents such as methyl alcohol, ethyl alcohol, isopropyl alcohol, acetone, and methyl ethyl ketone; and water-insoluble solvents such as ethyl acetate, toluene, and xylene.

[0071] The coating solution is preferably in the form of a solution or dispersion in which the thermoplastic resin is homogeneously dissolved or dispersed in the above-mentioned solvent. From the viewpoint of process control, it is preferable to prepare the coating solution by mixing aqueous solutions or aqueous dispersions of each component. From the viewpoint of reducing the drying load, the solid content concentration in the coating liquid is preferably 0.1% by mass or more, and more preferably 0.2% by mass or more. From the viewpoint of obtaining a uniform coated surface, the above solid content concentration is preferably 20% by mass or less, and more preferably 10% by mass or less.

[0072] From the viewpoint of facilitating adjustment to the desired tensile strength, the in-mold label preferably includes a stretched layer stretched in at least one axial direction, and more preferably includes a biaxially stretched layer. Preferably, the base layer with a large thickness ratio is the stretched layer, and the heat seal layer may also be the stretched layer. The stretching ratio of the stretched layer is preferably 3 times or more in one direction, more preferably 4 times or more, even more preferably 5 times or more, and particularly preferably 6 times or more. From the viewpoint of moldability, the stretching ratio of the stretched layer may be, for example, 20 times or less. Furthermore, the stretching ratio of the stretched layer in the direction perpendicular to the above-mentioned one direction is preferably 3 times or more. Moreover, from the viewpoint of manufacturing and quality stability, the stretching ratio of the stretched layer in the direction perpendicular to the above-mentioned one direction (especially the mechanical direction (MD)) is preferably 10 times or less, may be 6 times or less, and may be 4 times or less.

[0073] <<Thickness>> From the viewpoint of increasing tensile strength, the thickness of the in-mold label is preferably 50 μm or more, more preferably 60 μm or more, even more preferably 70 μm or more, even more preferably 80 μm or more, and particularly preferably 90 μm or more. From the viewpoint of conforming to the container to reduce wrinkles, etc., and reducing partial thinning of the container due to label embedding, the thickness of the above in-mold label is preferably 300 μm or less, more preferably 250 μm or less, and even more preferably 150 μm or less.

[0074] <Container body> The resin material that can be used for the neck and body of the labeled container of the present invention is not particularly limited, and examples include thermoplastic resins such as polyester resins, polyolefin resins, or polystyrene resins. The present invention is particularly applicable when the resin material is a polyester resin.

[0075] Examples of polyester resins include polyethylene terephthalate (PET), polybutylene terephthalate, polybutylene succinate, and polylactic acid. Examples of polyolefin resins include polypropylene resins and polyethylene resins. [Examples]

[0076] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples. Unless otherwise specified, "parts," "%," etc., in the examples refer to mass-based measurements.

[0077] (Manufacturing of in-mold labels) Table 1 lists the materials used for the in-mold labels. [Table 1]

[0078] (In-mold label (L1)) A resin composition for forming a base layer was prepared by mixing 60% by mass of propylene homopolymer (manufactured by Nippon Polypropylene Co., Ltd., product name: Novatec PP MA4, MFR (230℃, 2.16 kg load): 5 g / 10 min, melting point: 167℃), 10% by mass of high-density polyethylene (Novatec HD HJ490, manufactured by Nippon Polyethylene Co., Ltd., MFR (190℃, 2.16 kg load): 20 g / 10 min, melting point: 133℃), and 30% by mass of heavy calcium carbonate (manufactured by Bihoku Powdering Industry Co., Ltd., product name: Softon 1800, average particle size: 1.8 μm).

[0079] The above resin composition was melt-kneaded in an extruder heated to 230°C, extruded into a sheet, and cooled to obtain an unstretched sheet. This unstretched sheet was heated to 150°C and stretched five times in the longitudinal direction (MD: Machine Direction). It was then cooled to 60°C, heated again to 150°C, and stretched eight times in the transverse direction (TD: Transverse Direction) using a tenter. Annealing was performed at 160°C, and the sheet was cooled to 60°C to obtain a white, opaque, biaxially oriented film base layer.

[0080] An in-mold label (L1) was obtained in which a heat-seal layer was laminated on the base layer by gravure coating an ethylene-vinyl acetate copolymer (manufactured by Toyo Morton Co., Ltd., product name: Adcoat AD1790-15, main component: ethylene-vinyl acetate copolymer (EVA), solid content 15% by mass) onto one side of the above base layer sheet. In the in-mold label, the thickness of the base layer was 105 μm, and the thickness of the heat-seal layer was 3 μm.

[0081] (In-mold labels (L2) to (L5) and (L7)) Each in-mold label (L2) to (L5) and (L7) was manufactured in the same manner as in-mold label (L1), except that the composition, thickness, or molding method of the base layer was changed as shown in Table 2.

[0082] (In-mold label (L6)) An in-mold label (L6) was obtained by forming a heat-seal layer on one side of natural pulp paper in the same manner as the in-mold label (L1).

[0083] <Measurement of tensile strength> The tensile strength of each in-mold label (L1) to (L7) in the longitudinal and transverse directions was measured in accordance with JIS K7113.

[0084] Table 2 shows a list of in-mold labels (L1) to (L7). [Table 2]

[0085] (Example 1) The in-mold label (L1) was charged using an electrostatic charging device, and then fixed to the inner wall surface of the molding die of a stretch blow molding machine (manufactured by Nissei ASB Co., Ltd., machine name: ASB-70DPH) and clamped. An α-type container forming die was used as the die. The orientation of the in-mold label (L1) was adjusted so that its vertical direction (MD) coincided with the horizontal direction, assuming the long side of the bottom surface of the die was the horizontal direction. The base material layer of the in-mold label (L1) was then fixed by suction so that it was in contact with the cavity of the die. Subsequently, the temperature of the die was controlled by circulating water so that the surface temperature on the cavity side of the die was 45°C.

[0086] Meanwhile, a bottomed cylindrical preform made of polyethylene terephthalate (PET) resin (Novapex BK-2180, manufactured by Mitsubishi Chemical Corporation; glass transition temperature: 74.9°C, melting point: 247°C, intrinsic viscosity: 0.7 dl / g) was molded using the stretch blow molding machine described above, and this preform was heated and held at 107°C. The heated preform was guided into a mold and inserted into the interior, and a rod was then inserted into the cavity of the preform and stretched vertically while a blow pressure of 2 MPa was applied for 6 seconds to perform blow molding. The delay time from the start of stretching with the rod to the start of blowing was 0.2 seconds, and blowing was started when the length of the inserted portion of the rod reached half the vertical dimension (Dz) of the cavity of the mold. After cooling to 50°C in 15 seconds, the mold was opened to obtain a labeled container.

[0087] (Examples 2 and 3) Labeled containers for Examples 2 and 3 were obtained in the same manner as in Example 1, except that the in-mold label (L1) was changed to an in-mold label (L2) and the blow pressure was changed as shown in Table 3.

[0088] (Examples 4-9) Labeled containers for Examples 4 to 9 were obtained in the same manner as in Example 1, except that the in-mold label, blow pressure, or preform temperature was changed as shown in Table 3.

[0089] (Example 10) A labeled container of Example 10 was obtained in the same manner as in Example 5, except that a mold for forming a β type was used, the lateral direction (TD) of the in-mold label was aligned with the horizontal direction, and blowing was started after the length of the rod insertion portion exceeded half of the vertical dimension (Dz) of the container.

[0090] (Examples 11-13) Labeled containers for Examples 11 to 13 were obtained in the same manner as in Example 10, except that the length of the in-mold label or the rod insertion portion at the start of blowing was changed as shown in Table 4.

[0091] (Example 14) Using a mold and preform for γ-type formation, the labeled container of Example 14 was obtained in the same manner as in Example 1, except that the transverse direction (TD) of the in-mold label was aligned with the horizontal direction, and the delay time from the start of stretching with a rod to the start of blowing was changed as shown in Table 4.

[0092] (Examples 15 and 16) Labeled containers for Examples 15 and 16 were obtained in the same manner as in Example 14, except that the temperature of the in-mold label or preform was changed as shown in Table 4.

[0093] (Comparative Example 1) A labeled container for Comparative Example 1 was obtained in the same manner as in Example 5, except that the lateral direction (TD) of the in-mold label was aligned with the horizontal direction and the length of the rod insertion portion at the start of blowing was changed as shown in Table 4.

[0094] (Comparative Example 2) A labeled container for Comparative Example 2 was obtained in the same manner as for Comparative Example 1, except that the in-mold label (L1) was changed to an in-mold label (L7) and the orientation of the in-mold label (L7) was adjusted so that the lateral direction (TD) matched the horizontal direction.

[0095] (Comparative Example 3) A labeled container for Comparative Example 3 was obtained in the same manner as in Example 11, except that the vertical direction (MD) of the in-mold label was aligned with the horizontal direction.

[0096] (Measurement and evaluation) The following measurements and evaluations were performed on each labeled container.

[0097] <Stretch ratio of labeled containers> Two lines were marked at equal intervals in the horizontal, depth, and vertical directions of the preform's body. The dimensions between each line in each direction were measured using a scale on both the preform and the labeled container molded from the preform. The ratios of the dimensions measured on the labeled container to the dimensions measured on the preform were determined as the stretch ratios (Dx / dx), (Dy / dy), and (Dz / dz) of the body in the horizontal, depth, and vertical directions, respectively.

[0098] <Stretching ratio of labeled containers (horizontal direction)> The ratio of the body dimensions to the neck dimensions in the horizontal direction of the labeled container (Dx / ndx) was determined as the ratio of the dimensions of the labeled container to the dimensions of the preform in the horizontal direction (Dx / dx). This dimensional ratio (Dx / dx) also represents the horizontal stretching ratio of the body.

[0099] <Stretch ratio of labeled container (depth direction)> The ratio of the body dimensions to the neck dimensions in the depth direction of the labeled container (Dy / ndy) was determined as the ratio of the dimensions of the labeled container to the dimensions of the preform in the depth direction (Dy / dy). This dimensional ratio (Dy / dy) also represents the stretch ratio of the body in the depth direction.

[0100] <Flatness ratio of labeled containers> The ratio of the horizontal dimension to the depth dimension (Dx / Dy) of a labeled container was determined as the flattening ratio. When the bottom of the labeled container is square, the flattening ratio is 1. When the labeled container is flat, the flattening ratio is greater than 1. Furthermore, (Dx × dy) / (Dy × dx) was calculated using the horizontal dimension Dx and depth dimension Dy of the body of the labeled container, and the horizontal dimension dx and depth dimension dy of the body of the preform.

[0101] <Label growth rate> In both the horizontal and depth directions, the ratio of the dimensions of the label on the blow-molded container to the dimensions of the in-mold label before blow molding was determined as the elongation rate (%).

[0102] <Wrinkles> The condition of wrinkles on the label surface of labeled containers was visually assessed according to the following evaluation criteria. Wrinkle-free: No wrinkles are visible, just like the label before molding. Slightly present: There are small wrinkles, but they are not noticeable and are within an acceptable range. Wrinkled: Large or numerous wrinkles are present, making it unsuitable for practical use.

[0103] <Break> We visually inspected the labels on the labeled containers to determine if they were broken or damaged.

[0104] <Distortion of printed content> The degree of distortion of the printed characters on the label surface of the labeled container was visually assessed according to the following evaluation criteria. No distortion: No distortion is observed, just like the printed text before molding. Minor distortion: A slight distortion of the characters is noticeable, but it does not pose any practical problems. Distortion: Some distortion is observed in the characters, but it is within acceptable limits. Severe distortion: The text is distorted, making the content unclear and unsuitable for practical use.

[0105] Tables 3 and 4 show the measurement and evaluation results. [Table 3]

[0106] [Table 4]

[0107] As shown in Tables 3 and 4, in Examples 1 to 16, the orientation of the in-mold label was adjusted by process (a) for α-type labeled containers and by process (b) for β and γ-type labeled containers, and the direction in which the tensile strength of 10 kN / m or more was aligned to the horizontal or vertical direction. In all of these examples, the distortion of the printed characters was not significant, and the deformation of the label's appearance was reduced.

[0108] On the other hand, in Comparative Examples 1-3, the orientation of the in-mold labels was not adjusted so that one direction with a tensile strength of 10 kN / m or more coincided with the horizontal or vertical direction. As a result, the elongation rate of the labels in the horizontal or vertical direction was more than twice as large as in the examples, and the distortion of the printed characters was also greater. Furthermore, the labels could not withstand the stress applied from the preform during molding, resulting in wrinkles and breakage.

[0109] While all of Examples 1-16 are well within acceptable limits as products, for reference, Example 3 uses the same molding conditions as Example 2 but with the in-mold label (L1) changed to in-mold label (L2), resulting in slightly lower tensile strength and slightly higher label elongation compared to Example 2. In Example 4, the preform temperature is lower than in Example 3, and the preform is stretch-blown while still rigid, resulting in approximately 4% higher label elongation. Consequently, the evaluation results for wrinkles or printed character distortion after container molding are improved in Example 2 compared to Example 3, and in Example 3 compared to Example 4.

[0110] Example 8 uses the molding conditions of Example 4, but changes the in-mold label (L2) to in-mold label (L5). In-mold label (L5) has a higher resin content, resulting in higher tensile strength, lower label elongation, and no wrinkles. Example 10 is a container with a β-type label, where the in-mold label (L1) is prone to stretching in the vertical direction, and the molding conditions are optimal for the β type. Because the stretching rod is inserted all the way in before blowing, the label elongation is suppressed. In all of these examples, the distortion of the printed characters is not significant, and the deformation of the label's appearance is reduced, so the products are well within acceptable limits.

[0111] This application claims priority based on Japanese Patent Application No. 2022-057046, filed on March 30, 2022, and incorporates all the contents of said Japanese Patent Application. [Explanation of symbols]

[0112] 10 preforms 11 Neck 12 Torso 20 In-Mold Labels 30 labeled containers 31 Neck 32 Torso 50-52 molds 55 Rod

Claims

1. a placement step of placing the in-mold label on an inner wall surface of a mold; preparing a preform having a cavity therein and being heated; an inserting step of inserting the preform into the mold; a blowing step of blowing gas into a cavity of the preform to inflate the preform, thereby forming a labeled container to which the in-mold label is attached; The in-mold label has a tensile strength of 10 kN / m or more in one direction, A method for manufacturing a labeled container, wherein the positioning step includes the following step (a) or the following step (b) of adjusting the orientation of the in-mold label. (a) when the dimension of the labeled container in the horizontal direction is at least twice the dimension of the preform and the dimension of the labeled container in the depth direction is at least one time but less than two times the dimension of the preform, a step of substantially aligning the one direction of the in-mold label with the horizontal direction; (b) when the dimension of the labeled container in the horizontal direction is 1 to 2 times the dimension of the preform and the dimension of the labeled container in the depth direction is 1 to 2 times the dimension of the preform, a step of approximately aligning the one direction of the in-mold label with the vertical direction.

2. The in-mold label has a tensile strength of 12 kN / m or more in the one direction. A method for producing a labeled container according to claim 1.

3. The temperature of the heated preform is 105° C. or higher. A method for producing a labeled container according to claim 1 or 2.

4. The pressure of the gas blown in the blowing step is 3.5 MPa or less. A method for producing a labeled container according to claim 1 or 2.

5. When the orientation of the in-mold label is adjusted by the step (b) and a rod is inserted into the cavity of the preform in the blowing step and the preform is stretched in the vertical direction by the rod, the blowing of the gas is started after the length of the inserted part of the rod exceeds 1 / 2 of the vertical dimension of the labeled container. A method for producing a labeled container according to claim 1 or 2.

6. The in-mold label includes an extension layer. A method for producing a labeled container according to claim 1 or 2.

7. The in-mold label has a thickness of 50 to 300 μm. A method for producing a labeled container according to claim 1 or 2.

8. a container having a neck and a body; and an in-mold label attached to the outer surface of the body portion, The in-mold label has a tensile strength of 10 kN / m or more in one direction, A labeled container that satisfies the following condition (I) or the following condition (II). (I) A ratio of the dimension of the body portion to the dimension of the neck portion in the horizontal direction is 2 or more, a ratio of the dimension of the body portion to the dimension of the neck portion in the depth direction is 1 or more and less than 2, and the one direction of the in-mold label substantially coincides with the horizontal direction. (II) A ratio of the dimension of the body portion to the dimension of the neck portion in the horizontal direction is 1 or more and less than 2, a ratio of the dimension of the body portion to the dimension of the neck portion in the depth direction is 1 or more and less than 2, and the one direction of the in-mold label substantially coincides with the vertical direction.

9. A method for manufacturing a labeled container as described in claim 1 or 2, wherein the preform is a cylindrical molded body with a bottom.