Chloroprene polymer and dip-molded product

JPWO2023190144A5Active Publication Date: 2024-12-03DENKA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024512343
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-12-03
Estimated Expiration
2043-03-24

AI Technical Summary

Technical Problem

Chloroprene polymers used in dip-molded products, such as medical gloves and rubber boots, often lack high tensile strength and flexibility, making it difficult to achieve products with optimal texture and mechanical properties.

Method used

A chloroprene-based polymer with specific molecular weight and monomer composition, including 2,3-dichloro-1,3-butadiene, is developed to achieve high tensile strength at break and low modulus at 100% elongation, using a non-resonant forced vibration method to control loss tangent tan δ within a specific range, allowing for the production of dip-molded products with improved texture and mechanical properties.

Benefits of technology

The resulting dip-molded products exhibit high tensile strength at break, low modulus at 100% elongation, and excellent texture, suitable for applications like medical gloves and industrial gloves, without the need for vulcanization accelerators.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Provided is a chloroprene polymer which has high tensile strength at break and a low modulus at 100% elongation, and which makes it possible to obtain a dip-molded product having excellent texture. The present invention provides a chloroprene polymer, wherein the loss tangent tanδ in the 10 Hz frequency region of a film containing the chloroprene polymer, as obtained when the tensile-type dynamic viscoelasticity is measured in accordance with the non-resonant forced vibration technique at a temperature of 25°C and under a strain of 0.75%, is 0.08 to 0.14, and the film is obtained by drying chloroprene polymer latex containing the chloroprene polymer for three days at 23°C or lower.
Need to check novelty before this filing date? Find Prior Art

Description

Chloroprene polymers and dip-molded products

[0001] The present invention relates to a chloroprene polymer and a dip-molded product.

[0002] Chloroprene polymers are known as materials for dip-molded products such as medical surgical gloves, medical examination gloves, industrial gloves, balloons, catheters, and rubber boots.

[0003] Various techniques have been proposed for improving the flexibility of chloroprene polymers and for dip-molded products of chloroprene polymers. Patent Document 1 describes a polychloroprene latex with a pH of 7 to 14 for use in dip-molded products, which contains 100 parts by mass of modified polychloroprene obtained by copolymerizing chloroprene and methacrylic acid, 90 to 150 parts by mass of water, 1 to 5 parts by mass of an emulsifier, and 0.5 to 2.5 parts by mass of potassium ions. Patent Document 2 describes a mercaptan-modified polychloroprene latex for use in dip-molded products, which is obtained by copolymerizing chloroprene and 2,3-dichloro-1,3-butadiene, and in which the peak areas (A) at 126.2 to 127.6 ppm, (B) at 122.0 to 126.2 ppm, and (C) at 129.9 to 130.3 ppm in the C-solid-state NMR spectrum of the polychloroprene are within the ranges represented by the following general formula (I): Patent Document 3 describes a chloroprene polymer latex for use in dip-molded products, which contains high-molecular-weight and low-molecular-weight components, thereby achieving both excellent flexibility and mechanical properties in the vulcanized rubber produced by dip molding. Patent Document 4 describes a chloroprene polymer latex that exhibits excellent flexibility and mechanical properties even under mild vulcanization conditions, which is obtained by copolymerizing a chloroprene monomer with an isoprene monomer, which is a raw material for isoprene rubber. Patent Document 5 describes a dip-molded product of a chloroprene polymer that exhibits excellent flexibility without containing a vulcanization accelerator by mixing a chloroprene polymer latex with an isoprene polymer latex. Patent Document 6 describes a dip-molded product that exhibits excellent mechanical properties by mixing a chloroprene polymer latex with a nitrile-butadiene polymer (NBR) latex or an isoprene polymer latex.

[0004]

[0005] Japanese Patent Application Laid-Open No. 2014-114342 International Publication No. 2019 / 009038 Japanese Patent Application Laid-Open No. 2019-143002 International Publication No. 2021-132460 Special Publication No. 2017-508840 Japanese Patent Application Laid-Open No. 2020-189963

[0006] Chloroprene polymers are used as materials for dip-molded products such as medical surgical gloves, medical examination gloves, industrial gloves, balloons, catheters, and rubber boots. In particular, for use in medical rubber gloves, there is a demand for chloroprene polymers that can give dip-molded products having high tensile strength at break, low modulus at 100% elongation, and excellent texture.

[0007] The present invention has been made in view of the above circumstances, and provides a chloroprene polymer from which a dip-molded product having high tensile strength at break, low modulus at 100% elongation, and excellent texture can be obtained.

[0008] The present invention provides a chloroprene polymer, wherein a film containing the chloroprene polymer has a loss tangent tanδ of 0.080 to 0.140 in a frequency range of 10 Hz, as determined by tensile dynamic viscoelasticity measurement in accordance with a non-resonant forced vibration method at a temperature of 25°C and a strain of 0.75%, and the film is obtainable by drying a chloroprene polymer latex containing the chloroprene polymer at 23°C for 3 days.

[0009] As a result of extensive investigations, the present inventors have found that by controlling the loss tangent tanδ in the 10 Hz frequency region of a chloroprene polymer film, which is determined by measuring the tensile dynamic viscoelasticity according to a non-resonant forced vibration method at a temperature of 25°C and a strain of 0.75%, to a specific value, a chloroprene polymer can be obtained that has low tensile strength at break and modulus at 100% elongation and that can give a dip-molded product having excellent texture. This finding led to the completion of the present invention.

[0010] Various embodiments of the present invention are exemplified below. The embodiments shown below can be combined with each other. Preferably, the chloroprene polymer described above exhibits a peak corresponding to a weight average molecular weight of 5,000 to 80,000 when the tetrahydrofuran-soluble portion of the chloroprene polymer is subjected to gel permeation chromatography. Preferably, the chloroprene polymer described above contains a monomer unit derived from 2,3-dichloro-1,3-butadiene.

[0011] According to another aspect of the present invention, there is provided a dip-molded article comprising the above-described chloroprene-based polymer. The above-described dip-molded article is preferably an industrial or general household glove, a medical glove, a balloon, a catheter, or a boot.

[0012] The chloroprene polymer of the present invention can provide a dip-molded product having high tensile strength at break, low modulus at 100% elongation, and excellent texture.

[0013] The present invention will be described in detail below by illustrating embodiments of the present invention. The present invention is not limited by these descriptions. The features of the embodiments of the present invention described below can be combined with each other. Furthermore, each feature can be an invention independently.

[0014] 1. Chloroprene-Based Polymer The chloroprene-based polymer according to the present invention is a polymer containing monomer units derived from 2-chloro-1,3-butadiene (hereinafter also referred to as chloroprene). Furthermore, the chloroprene-based polymer according to one embodiment of the present invention may also be a copolymer of chloroprene and another monomer copolymerizable with chloroprene. Examples of the other monomer include 1-chloro-1,3-butadiene, 2,3-dichloro-1,3-butadiene, isoprene, styrene, methacrylic acid, acrylonitrile, and sulfur. Two or more of these may be used in combination as the other monomer. The chloroprene-based polymer according to one embodiment of the present invention preferably contains monomer units derived from 2,3-dichloro-1,3-butadiene. The chloroprene-based polymer according to one embodiment of the present invention may also be sulfur-free, and the chloroprene-based polymer according to one embodiment of the present invention may also be free of an —S—S— structure resulting from sulfur in the main chain.

[0015] The chloroprene polymer according to one embodiment of the present invention may be obtained by mixing two or more different chloroprene polymers. The chloroprene polymer preferably contains at least one selected from the group consisting of a homopolymer of chloroprene (2-chloro-1,3-butadiene), a copolymer of chloroprene and 1-chloro-1,3-butadiene, a copolymer of chloroprene and 2,3-dichloro-1,3-butadiene, and a copolymer of chloroprene, 1-chloro-1,3-butadiene, and 2,3-dichloro-1,3-butadiene, and more preferably contains at least one selected from the group consisting of a homopolymer of chloroprene and a copolymer of chloroprene and 2,3-dichloro-1,3-butadiene.

[0016] The chloroprene polymer according to one embodiment of the present invention may contain 50 to 100 mass% of chloroprene-derived monomer units, preferably 70 to 100 mass%, of the chloroprene polymer in the chloroprene polymer latex composition, based on 100 mass% of the chloroprene polymer. The content of the chloroprene-derived monomer units may be, for example, 50, 55, 60, 65, 70, 75, 80, 85, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, or 100 mass%, or may be within a range between any two of the values ​​exemplified here.

[0017] A chloroprene polymer according to one embodiment of the present invention may contain 0 to 30% by mass of monomer units derived from 2,3-dichloro-1,3-butadiene, relative to 100% by mass of the chloroprene polymer contained in the chloroprene polymer latex composition. The content of the monomer units derived from 2,3-dichloro-1,3-butadiene is, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30% by mass, and may be within a range between any two of the values ​​exemplified here.

[0018] A chloroprene polymer according to one embodiment of the present invention may contain monomer units derived from chloroprene and monomer units derived from 2,3-dichloro-1,3-butadiene. In this case, the chloroprene polymer preferably contains 0 to 30% by mass, and more preferably 5 to 25% by mass, of the monomer units derived from 2,3-dichloro-1,3-butadiene, when the total of the monomer units derived from chloroprene and the monomer units derived from 2,3-dichloro-1,3-butadiene contained in the chloroprene polymer is taken as 100% by mass.

[0019] When the chloroprene polymer is a mixture of two or more different chloroprene polymers, the content of each monomer unit means the total amount of each monomer unit in all chloroprene polymers contained in the chloroprene polymer latex composition.

[0020] In the chloroprene polymer according to one embodiment of the present invention, when the chloroprene polymer contained in the chloroprene polymer latex composition is taken as 100% by mass, the content of the sulfur-modified chloroprene polymer contained in the chloroprene polymer latex composition is preferably 20% by mass or less. The content of the sulfur-modified chloroprene polymer is, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20% by mass, and may be within a range between any two of the values ​​exemplified here. The chloroprene polymer according to one embodiment of the present invention may not contain a sulfur-modified chloroprene polymer.

[0021] The chloroprene polymer according to the present invention has a loss tangent tanδ in a 10 Hz frequency range of 0.080 to 0.140, preferably 0.090 to 0.140, and more preferably 0.100 to 0.140, when measured by a non-resonant forced vibration method at a temperature of 25°C and a strain of 0.75%. The loss tangent tanδ in a 10 Hz frequency range is, for example, 0.080, 0.085, 0.090, 0.095, 0.100, 0.105, 0.110, 0.115, 0.120, 0.125, 0.130, 0.135, or 0.140, and may be within a range between any two of the values ​​exemplified here.

[0022] Here, the film containing a chloroprene polymer is obtained by drying a chloroprene polymer latex containing a chloroprene polymer at 23°C for 3 days. As an example, a chloroprene polymer latex containing a chloroprene polymer is poured into an iron frame to a thickness of about 1.5 mm, and left to stand at 23°C for 3 days to evaporate volatiles, resulting in a dried sheet, which can be used as the film containing a chloroprene polymer. That is, the film containing a chloroprene polymer is obtained by removing water from a chloroprene polymer latex containing a chloroprene polymer at room temperature, and the film containing a chloroprene polymer can be one that has not been subjected to a heat treatment at a temperature that would cause a crosslinking / vulcanization reaction in the chloroprene polymer. After polymerization, the chloroprene polymer contained in the film may have no thermal history of, for example, 100°C or higher, preferably no thermal history of 80°C or higher, and more preferably no thermal history of 60°C or higher.

[0023] A film containing a chloroprene polymer may have components that can be contained in a chloroprene polymer latex. Chloroprene polymer latex will be described later. A film containing a chloroprene polymer may contain a chloroprene polymer as a main component, and may contain 70% by mass or more of the chloroprene polymer, preferably 80% by mass or more, and more preferably 90% by mass or more, of the film taken as 100% by mass. The content of the chloroprene polymer in the film, taken as 100% by mass, may be, for example, 70, 75, 80, 85, 90, 95, 96, 97, or 98% by mass, or may be within a range between any two of the values ​​exemplified here.

[0024] The thickness of the film containing a chloroprene polymer may be 0.5 to 1.5 mm. The thickness of the film containing a chloroprene polymer may be, for example, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, or 1.5 mm, or may be within a range between any two of the values ​​exemplified here. The thickness of the film containing a chloroprene polymer can be adjusted by the solids concentration of the chloroprene polymer latex.

[0025] The tensile dynamic viscoelasticity measurement based on the non-resonant forced vibration method can be performed by cutting out a film containing the chloroprene polymer to prepare a strip-shaped test piece (width: 4.5 mm, length: 30 mm, thickness: 0.80 to 0.90 mm) and using the resulting strip-shaped test piece. The measurement conditions can be a static tension of 5 gf, a temperature of 25°C, a strain of 0.75%, and a chuck distance of 20 mm. Specifically, the measurement can be performed by the method described in the examples.

[0026] By adjusting the loss tangent tanδ in the 10 Hz frequency range to a specific value, the chloroprene polymer according to the present invention can be made into a chloroprene polymer capable of producing a dip-molded product having high tensile strength at break, low modulus at 100% elongation, and excellent texture. The loss tangent tanδ in the 10 Hz frequency range can be controlled by adjusting the types and amounts of raw materials used in polymerization of the chloroprene polymer, the types and amounts of chemicals used, and polymerization conditions (e.g., polymerization temperature, whether or not raw material monomers are added separately in the polymerization step, etc.), and by adjusting the types and amounts of monomer units contained in the resulting chloroprene polymer, as well as the weight-average molecular weight and the mixing ratio of the chloroprene polymer.

[0027] In the chloroprene polymer according to one embodiment of the present invention, a peak having a weight-average molecular weight of 5,000 to 80,000 is preferably detected in the molecular weight distribution obtained by measuring a tetrahydrofuran-soluble sol fraction of the chloroprene polymer by gel permeation chromatography. The peak position of the peak detected in the weight-average molecular weight range of 5,000 to 80,000 may be, for example, 5,000, 6,000, 7,000, 8,000, 9,000, 10,000, 11,000, 12,000, 13,000, 14,000, 15,000, 16,000, 17,000, 18,000, 19,000, 20,000, 21,000, 22,000, 23,000, 24,000, 25,000, 26,000, 27,000, 28,000, 29,000, 30,000, 31,000, 32,000, 33,000, 34,000, 35,000, 36,000, 37,000, 38,000, 39,000, 40,000, 41,000, 42,000, 43,000, 44,000, 45,000, 46,000, 47,000, 48,000, 49,000, 50,000, 51,000, 52,000, 53,000, 54,000, 5 The weight-average molecular weight of the chloroprene polymer according to one embodiment of the present invention may be a mixture of two or more different chloroprene polymers, and preferably includes a chloroprene polymer having a weight-average molecular weight of 5,000 to 80,000.

[0028] The chloroprene polymer according to one embodiment of the present invention may further include a chloroprene polymer having a weight-average molecular weight of 200,000 to 1,500,000. That is, the chloroprene polymer according to one embodiment of the present invention may have a peak corresponding to a weight-average molecular weight of 200,000 to 1,500,000 detected in the molecular weight distribution obtained by measuring a tetrahydrofuran-soluble sol fraction of the chloroprene polymer by gel permeation chromatography. The peak positions of peaks detected in the weight average molecular weight range of 200,000 to 1,500,000 are, for example, 200,000, 300,000, 400,000, 500,000, 600,000, 700,000, 800,000, 900,000, 1,000,000, 1,100,000, 1,200,000, 1,300,000, 1,400,000, and 1,500,000, and may be within a range between any two of the numerical values ​​exemplified here.

[0029] The molecular weight distribution of the tetrahydrofuran-soluble sol fraction of a chloroprene polymer can be obtained by measuring the weight-average molecular weight by gel permeation chromatography (GPC). The GPC measurement conditions can be as described in the Examples. The weight-average molecular weight of a chloroprene polymer can be controlled by adjusting the type and amount of chain transfer agent, polymerization temperature, polymerization time, polymerization conversion rate, and the like during polymerization of each chloroprene polymer. Furthermore, as described below, the loss tangent tanδ can be adjusted by adjusting the weight-average molecular weight of the chloroprene polymer or the blending ratio of chloroprene polymers having different weight-average molecular weights.

[0030] In a chloroprene polymer according to one embodiment of the present invention, a peak corresponding to a weight-average molecular weight of 5,000 to 80,000 and a peak corresponding to a weight-average molecular weight of 200,000 to 1,500,000 are preferably detected in the molecular weight distribution obtained by measuring a tetrahydrofuran-soluble sol fraction of the chloroprene polymer by gel permeation chromatography. That is, the chloroprene polymer according to one embodiment of the present invention preferably includes a chloroprene polymer having a weight-average molecular weight of 5,000 to 80,000 and a chloroprene polymer having a weight-average molecular weight of 200,000 to 1,500,000.

[0031] The chloroprene polymer according to one embodiment of the present invention preferably contains 10 to 40 mass%, and more preferably 15 to 30 mass%, of a chloroprene polymer having a weight-average molecular weight of 5,000 to 80,000, based on 100 mass% of the chloroprene polymer. The chloroprene polymer according to one embodiment of the present invention may contain, for example, 10, 15, 20, 25, 30, 35, or 40 mass% of the chloroprene polymer having a weight-average molecular weight of 5,000 to 80,000, based on 100 mass% of the chloroprene polymer, and may be within a range between any two of the numerical values ​​exemplified here.

[0032] The chloroprene polymer according to one embodiment of the present invention preferably contains 60 to 90 mass%, and more preferably 70 to 85 mass%, of a chloroprene polymer having a weight-average molecular weight of 200,000 to 1,500,000, based on 100 mass% of the chloroprene polymer. The chloroprene polymer according to one embodiment of the present invention may contain, for example, 60, 65, 70, 75, 80, 85, or 90 mass% of a chloroprene polymer having a weight-average molecular weight of 200,000 to 1,500,000, based on 100 mass% of the chloroprene polymer, and may be within a range between any two of the numerical values ​​exemplified here.

[0033] By adjusting the contents of the chloroprene polymers having different weight-average molecular weights to fall within the above range, the loss tangent tan δ can be adjusted more appropriately.

[0034] In the chloroprene polymer according to one embodiment of the present invention, the tensile strength at break of a dip-molded product containing the chloroprene polymer, as measured in accordance with JIS K 6251, is preferably 17.0 MPa or more, and more preferably 20.0 MPa or more, and may be, for example, 17.0, 18.0, 19.0, 20.0, 21.0, 22.0, 23.0, 24.0, 25.0, 26.0, 27.0, 28.0, 29.0, 30.0, 31.0, 32.0, 33.0, 34.0, 35.0, 36.0, 37.0, 38.0, 39.0, or 40.0 MPa, or may be within a range between any two of the values ​​exemplified here.

[0035] In the chloroprene polymer according to one embodiment of the present invention, the modulus at 100% elongation of a dip-molded product containing the chloroprene polymer, measured in accordance with JIS K 6251, is preferably 0.70 MPa or less, more preferably 0.5 MPa or less, and may be, for example, 0.30, 0.35, 0.40, 0.45, 0.50, 0.55, 0.60, 0.65, or 0.70 MPa, or may be within a range between any two of the values ​​exemplified here.

[0036] The dip-molded product containing a chloroprene polymer can be obtained by dip-molding a chloroprene polymer latex composition containing a chloroprene polymer by a dip coagulation method, followed by heating and drying the resulting product at 150°C for 60 minutes. The dip-molded product can contain a chloroprene polymer as a base polymer, and can contain 70% by mass or more of the chloroprene polymer, preferably 80% by mass or more, and more preferably 90% by mass or more, of the chloroprene polymer, based on 100% by mass of the dip-molded product. The chloroprene polymer content in the dip-molded product, based on 100% by mass of the dip-molded product, can be, for example, 70, 75, 80, 85, 90, 95, 96, 97, 98, 99, or 100% by mass, or can be within a range between any two of the values ​​exemplified here. Specifically, the dip-molded product can be obtained by the method described in the examples. The modulus at 100% elongation and the tensile strength at break can be measured as described in the Examples.

[0037] The modulus at 100% elongation and tensile strength at break of the dip-molded product containing a chloroprene polymer can be controlled by adjusting the type (weight average molecular weight, type and content of monomer units contained, etc.) and amount of the chloroprene polymer contained in the dip-molded product.

[0038] 2. Chloroprene Polymer Latex A chloroprene polymer latex according to one embodiment of the present invention includes the chloroprene polymer according to the present invention. The chloroprene polymer latex may be one in which a chloroprene polymer is dispersed in water, and at least one selected from the group consisting of a chloroprene homopolymer, a copolymer of chloroprene and 1-chloro-1,3-butadiene, a copolymer of chloroprene and 2,3-dichloro-1,3-butadiene, and a copolymer of chloroprene, 1-chloro-1,3-butadiene, and 2,3-dichloro-1,3-butadiene may be dispersed in water, or the chloroprene homopolymer or the copolymer of chloroprene and 2,3-dichloro-1,3-butadiene may be dispersed in water.

[0039] 3. Method for Producing Chloroprene Polymer Latex The method for producing a chloroprene polymer latex according to one embodiment of the present invention may include a polymerization step of polymerizing a chloroprene-containing monomer to obtain a chloroprene polymer latex. The method for producing a chloroprene polymer latex may further include a mixing step of mixing two or more chloroprene polymer latexes having different weight-average molecular weights.

[0040] In the polymerization process, the monomer includes chloroprene and may also include other monomers copolymerizable with chloroprene. Examples of other monomers copolymerizable with chloroprene include 1-chloro-1,3-butadiene, 2,3-dichloro-1,3-butadiene, isoprene, styrene, methacrylic acid, acrylonitrile, sulfur, etc. The monomer may also include chloroprene and 2,3-dichloro-1,3-butadiene.

[0041] The type and amount of each monomer are preferably adjusted so that the amount of each monomer in the resulting chloroprene polymer falls within the above-mentioned numerical range. For example, the copolymerization amount of 2,3-dichloro-1,3-butadiene in the chloroprene polymer contained in the chloroprene polymer latex can be set to a range of 0 to 30 mass% relative to 100 mass% of the total of the chloroprene monomer and 2,3-dichloro-1,3-butadiene contained in the chloroprene polymer. In this case, the amount of 2,3-dichloro-1,3-butadiene charged before the start of emulsion polymerization is preferably set to a range of 0 to 30 parts by mass relative to 100 parts by mass of the total of the chloroprene monomer and 2,3-dichloro-1,3-butadiene monomer. From the viewpoint of controlling the polymerization, it is more preferable to set the amount of 2,3-dichloro-1,3-butadiene charged to 5 to 25 parts by mass per 100 parts by mass of the total of the chloroprene monomer and the 2,3-dichloro-1,3-butadiene monomer.

[0042] In the polymerization step, all of the raw material monomers to be used in the polymerization step can be charged into a polymerization vessel before the initiation of polymerization, and then the polymerization can be initiated. Alternatively, at least a portion of the raw material monomers to be used in the polymerization step can be charged into a polymerization vessel before the initiation of polymerization, and the remaining raw material monomers (e.g., a portion of chloroprene) can be added portionwise after the initiation of polymerization. When at least a portion of the raw material monomers are added before the initiation of polymerization and the remaining raw material monomers are added after the initiation of polymerization, the remaining raw material monomer, for example, chloroprene, can be added in one or more divided portions, or can be added continuously at a constant flow rate. For example, in the polymerization step to obtain a latex containing a chloroprene-based polymer having a weight-average molecular weight of 5,000 to 80,000, at least a portion of the raw material monomers can be added portionwise.

[0043] When producing a chloroprene polymer, raw material monomers are polymerized by a polymerization method such as emulsion polymerization, solution polymerization, suspension polymerization, bulk polymerization, etc. Among these polymerization methods, emulsion polymerization is preferred because it has various advantages such as ease of control, ease of extracting the polymer from the polymerization-finished liquid, and a relatively fast polymerization rate.

[0044] Emulsion polymerization is a type of radical polymerization, in which raw material monomers are charged into a reaction vessel together with a chain transfer agent, water, an alkali (e.g., a metal hydroxide such as potassium hydroxide or sodium hydroxide), an emulsifier (dispersant), a reducing agent (e.g., sodium hydrogen sulfite), a polymerization initiator, and the like, to polymerize them.

[0045] The type of chain transfer agent used in the emulsion polymerization is not particularly limited, and known chain transfer agents generally used in the emulsion polymerization of chloroprene can be used, such as long-chain alkyl mercaptans such as n-dodecyl mercaptan and tert-dodecyl mercaptan, dialkyl xanthogen disulfides such as diisopropyl xanthogen disulfide and diethyl xanthogen disulfide, iodoform, etc. As the chain transfer agent, long-chain alkyl mercaptans are preferred, and n-dodecyl mercaptan is more preferred.

[0046] By adjusting the type and amount of the chain transfer agent, the weight average molecular weight of the resulting chloroprene polymer latex can be adjusted.

[0047] For example, to obtain a latex containing a chloroprene polymer having a weight-average molecular weight of 5,000 to 80,000, i.e., to obtain a chloroprene polymer latex having a peak showing a weight-average molecular weight of 5,000 to 80,000 in its molecular weight distribution, the amount of the chain transfer agent added before the start of emulsion polymerization is preferably 0.5 to 10.0 parts by mass per 100 parts by mass of the monomer. In this case, the amount may be, for example, 0.5, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, or 10.0 parts by mass, or may be within a range between any two of the values ​​exemplified here.

[0048] For example, in order to obtain a latex containing a chloroprene polymer having a weight average molecular weight of 200,000 or more, preferably 200,000 to 1,500,000, that is, in order to obtain a chloroprene polymer latex having a peak showing a weight average molecular weight of 200,000 or more, preferably 200,000 to 1,500,000 in its molecular weight distribution, it is preferable to set the amount of the chain transfer agent before the start of emulsion polymerization to 0.01 to less than 0.10 part by mass per 100 parts by mass of the monomer (for example, 100 parts by mass in total of chloroprene and 2,3-dichloro-1,3-butadiene). From the viewpoint of obtaining a chloroprene polymer latex in which a peak showing a weight-average molecular weight of 500,000 or more is detected, the amount of the chain transfer agent is more preferably 0.02 to 0.05 parts by mass, for example, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09 parts by mass, or less than 0.10 parts by mass, and may be within a range between any two of the values ​​exemplified here. When the amount of the chain transfer agent, particularly a long-chain alkyl mercaptan, is 0.01 part by mass or more, the flexibility of a dip-molded product obtained by dip-molding the resulting chloroprene polymer latex is improved, and when the amount is less than 0.10 parts by mass, particularly less than 0.05 parts by mass, the tensile strength at break of a dip-molded product obtained by dip-molding the resulting chloroprene polymer latex is further increased.

[0049] Examples of emulsifiers include anionic emulsifiers and nonionic emulsifiers. Examples of anionic emulsifiers include fatty acid salts such as potassium tallow fatty acid, partially hydrogenated potassium tallow fatty acid, potassium oleate, and sodium oleate; resin acid salts such as potassium rosinate, sodium rosinate, hydrogenated potassium rosinate, and hydrogenated sodium rosinate; alkylbenzene sulfonates such as sodium dodecylbenzene sulfonate; and sodium salts of β-naphthalenesulfonic acid formalin condensates. Examples of nonionic emulsifiers include polyethylene glycol ester-type emulsifiers and polyvinyl alcohol. Among these, anionic emulsifiers are preferred, resin acid salts are preferred, rosin acids including rosin acid and rosin acid salts are preferred, and at least one selected from the group consisting of potassium rosinate and sodium rosinate is more preferred. These emulsifiers can be used alone or in combination. The amount of emulsifier used is preferably 1.0 to 6.5 parts by mass per 100 parts by mass of monomer.

[0050] In particular, the emulsifier used in emulsion polymerization preferably contains an anionic emulsifier, and more preferably contains a resin acid salt, particularly a rosin acid. The use of a rosin acid can more effectively prevent aggregation of rubber solids and pH fluctuations when blended with a base chloroprene polymer latex. Rosin acids include disproportionated rosin acid, conjugated resin acid, alkali metal salts of disproportionated rosin acid, and alkali metal salts of conjugated resin acid. Examples of disproportionated rosin acids include sesquiterpenes, 8,5-isopimaric acid, dihydropimaric acid, secodehydroabietic acid, dehydroabietic acid, dihydroabietic acid, deisopropyldehydroabietic acid, and demethyldehydroabietic acid. Examples of conjugated resin acids include abietic acid, palustric acid, neoabietic acid, and levopimaric acid. As the rosin acid, from the viewpoint of increasing the tensile strength at break of a dip-molded product obtained by dipping the resulting chloroprene polymer latex, it is preferable to use a conjugated resin acid, and it is preferable to use at least one kind selected from the group consisting of abietic acid, palustric acid, neoabietic acid and levopimaric acid.

[0051] In the method for producing a chloroprene polymer latex according to one embodiment of the present invention, in addition to the rosin acids, other commonly used emulsifiers or fatty acids can also be used in combination. Examples of the other emulsifiers include, for example, an anionic emulsifier, such as the above-mentioned anionic emulsifiers, as well as metal salts of aromatic sulfinic acid-formalin condensates, sodium dodecylbenzenesulfonate, potassium dodecylbenzenesulfonate, sodium alkyldiphenylethersulfonate, potassium alkyldiphenylethersulfonate, sodium polyoxyethylene alkylethersulfonate, sodium polyoxypropylene alkylethersulfonate, potassium polyoxyethylene alkylethersulfonate, and potassium polyoxypropylene alkyletherethersulfonate.

[0052] The content of the anionic emulsifier excluding rosin acids is preferably 0.2 to 1.0% by mass relative to 100% by mass of the chloroprene polymer contained in the chloroprene polymer latex. Therefore, the amount of the anionic emulsifier excluding rosin acids charged before the start of emulsion polymerization is preferably set within the range of 0.2 to 0.9 parts by mass relative to 100 parts by mass of the monomer (for example, the total of chloroprene and 2,3-dichloro-1,3-butadiene).

[0053] The pH of the aqueous emulsion at the start of emulsion polymerization is preferably 10.5 to 13.5. The aqueous emulsion refers to a mixed solution of a chain transfer agent and a monomer (chloroprene, 2,3-dichloro-1,3-butadiene, etc.) immediately before the start of emulsion polymerization, but also includes cases where the composition changes due to the subsequent addition or divided addition of each component. When the pH of the aqueous emulsion at the start of emulsion polymerization is 10.5 or higher, the polymerization reaction can be controlled more stably. When the pH is 13.5 or lower, excessive viscosity increase during polymerization is suppressed, and the polymerization reaction can be controlled more stably.

[0054] The polymerization temperature for emulsion polymerization is preferably within the range of 5 to 55° C. A temperature of 5° C. or higher is preferred because the emulsion does not freeze, and a temperature of 55° C. or lower is preferred because the chloroprene monomer does not evaporate or boil.

[0055] As the polymerization initiator, potassium persulfate, benzoyl peroxide, ammonium persulfate, hydrogen peroxide, etc., which are used in ordinary radical polymerization, can be used.

[0056] The polymerization conversion rate is preferably in the range of 50 to 95%. The polymerization reaction is terminated by adding a polymerization terminator. If the polymerization conversion rate is 50% or more, the tensile strength at break of the resulting dip-molded coating tends to be high. This is also advantageous from the viewpoint of production costs. If the polymerization conversion rate is less than 95%, it is possible to avoid a decrease in polymerization reactivity due to a decrease in unreacted monomer, and thus a decrease in productivity.

[0057] Examples of the polymerization terminator include diethylhydroxylamine, thiodiphenylamine, 4-tert-butylcatechol, 2,2'-methylenebis-4-methyl-6-tert-butylphenol, etc. After the emulsion polymerization is completed, unreacted monomers can be removed by a conventional method such as vacuum distillation.

[0058] Furthermore, to the chloroprene polymer latex obtained by the production method according to one embodiment of the present invention, after polymerization, any additive such as a freeze stabilizer, an emulsion stabilizer, a viscosity modifier, an antioxidant, or a preservative may be added, as long as the effects of the present invention are not impaired.

[0059] The method for producing a chloroprene polymer latex according to one embodiment of the present invention may further include a mixing step of mixing two or more chloroprene polymer latexes having different weight-average molecular weights after the polymerization step. In the mixing step, the two or more chloroprene polymer latexes may be mixed by a known method. In the mixing step, the chloroprene polymer latex may be obtained by stirring and mixing using a paddle blade at 30 to 300 rpm for 20 seconds to 3 minutes, e.g., at 100 rpm for 2 minutes.

[0060] 4. Chloroprene Polymer Latex Composition The chloroprene polymer latex composition according to one embodiment of the present invention comprises a chloroprene polymer latex containing the chloroprene polymer according to the present invention. The chloroprene polymer latex composition according to one embodiment of the present invention may contain a metal oxide, an antioxidant, and other necessary chemicals in addition to the chloroprene polymer latex. The types and amounts of the metal oxide, antioxidant, and other necessary chemicals that may be contained in the chloroprene polymer latex composition will be described below as components that may be contained in the dip-molded product.

[0061] 5. Method for Producing Chloroprene Polymer Latex Composition The method for producing a chloroprene polymer latex composition may include a raw material mixing step of mixing raw materials containing a chloroprene polymer latex, a metal oxide, an antioxidant, and other required chemicals. In the mixing step, an aqueous dispersion containing the metal oxide, the antioxidant, and other required chemicals may be prepared in advance, and the chloroprene polymer latex and the aqueous dispersion may be mixed. The mixing step may be performed using a known mixing device such as a ball mill.

[0062] 6. Dip-molded Product (Dip-molded Product Coating / Film) A dip-molded product according to one embodiment of the present invention is obtained using a chloroprene polymer latex composition containing the above-described chloroprene polymer latex. The dip-molded product of this embodiment can be obtained by dip-molding the above-described chloroprene polymer latex composition, either alone or in a blend with other chloroprene polymer latex compositions, and then dip-molding the dip-molded product according to the present invention. The dip-molded product can be obtained by dip-molding a chloroprene polymer latex composition containing a chloroprene polymer by a dip coagulation method, followed by heating and drying at 150°C for 60 minutes. The dip-molded product according to the present invention has high tensile strength at break, low modulus at 100% elongation, and excellent texture. The dip-molded product can be suitably used for industrial and general household gloves, medical gloves, balloons, catheters, and boots.

[0063] The dip-molded product according to the present invention may contain components contained in the chloroprene polymer latex. The dip-molded product may contain a chloroprene polymer as a base polymer, and may contain 70% by mass or more, preferably 80% by mass or more, and more preferably 90% by mass or more of the chloroprene polymer, based on 100% by mass of the dip-molded product. The content of the chloroprene polymer in the dip-molded product based on 100% by mass of the dip-molded product may be, for example, 70, 75, 80, 85, 90, 95, 96, 97, 98, 99, or 100% by mass, or may be within a range between any two of the values ​​exemplified here.

[0064] The dip-molded article containing the chloroprene polymer according to the present invention has low tensile strength at break and low modulus at 100% elongation, and has excellent texture, regardless of whether a vulcanizing agent and a vulcanization accelerator are added. The chloroprene polymer latex composition according to one embodiment of the present invention may be free of a vulcanizing agent and a vulcanization accelerator, and may be free of sulfur and vulcanization accelerators such as thiuram, dithiocarbamate, thiourea, guanidine, xanthogenate, and thiazole. Components that may be contained in the dip-molded article according to the present invention are described in detail below.

[0065] 6.1 Metal Oxide The chloroprene polymer dip-molded product according to the present invention may contain a metal oxide. The metal oxide contained in the chloroprene polymer latex composition used to obtain the dip-molded product is not particularly limited, and examples thereof include zinc oxide, lead oxide, trilead tetroxide, magnesium oxide, aluminum oxide, iron oxide, beryllium oxide, and titanium oxide. The metal oxide preferably contains zinc oxide. Zinc oxide is generally believed to function as a scavenger for dechlorinated atoms in the chloroprene polymer. These metal oxides may be used alone or in combination of two or more.

[0066] The amount of metal oxide added is preferably 0.5 to 15.0 parts by mass per 100 parts by mass of the solids content of the chloroprene polymer latex contained in the chloroprene polymer latex composition used to obtain the dip-molded product. When the amount of metal oxide added is 0.5 parts by mass or more, an improvement in tensile strength at break is expected due to the crosslinking effect between polymers. When the amount of metal oxide added is 15.0 parts by mass or less, a dip-molded product with excellent flexibility can be obtained. Furthermore, from the viewpoint of the balance of physical properties between flexibility and tensile strength at break of the obtained dip-molded product, the amount of metal oxide added is more preferably 0.5 to 5.0 parts by mass.

[0067] 6.2 Antioxidant The dip-molded product of the chloroprene polymer according to the present invention may contain an antioxidant. The antioxidant is not particularly limited, and phenolic antioxidants, amine-based antioxidants, heat-resistant oxidation (aging) inhibitors, ozone-resistant antioxidants, etc. can be used. When the obtained dip-molded product is used as a medical glove, a phenolic antioxidant can be used from the viewpoint of the color tone, texture, and hygiene of the dip-molded product. In particular, hindered phenolic antioxidants have a strong effect. Examples of hindered phenol-based antioxidants include 2,2'-methylenebis(4-ethyl-6-t-butylphenol), 2,2'-methylenebis(4-methyl-6-t-butylphenol), 4,4'-butylidene(3-methyl-6-t-butylphenol), 4,4'-thiobis(3-methyl-6-t-butylphenol), butylated reaction products of p-cresol and dicyclopentadiene, 2,5'-di-t-butylhydroquinone, and 2,5'-di-t-amylhydroquinone. Among these, butylated reaction products of p-cresol and dicyclopentadiene are desirable from the viewpoint of general dispersibility in aqueous materials. Furthermore, these compounds may be used alone or in combination of two or more.

[0068] The amount of antioxidant added is preferably 0.5 to 10.0 parts by mass per 100 parts by mass of the solids content of the chloroprene polymer latex contained in the chloroprene polymer latex composition used to obtain the dip-molded product. The amount of antioxidant added is, for example, 0.5, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, or 10.0 parts by mass, and may be within a range between any two of the values ​​exemplified here. When the amount of antioxidant added is 0.5 parts by mass or more, the effect of suppressing color change in the dip-molded product can be obtained. When the amount of antioxidant added is 10.0 parts by mass or less, the stability of the chloroprene polymer latex composition can be ensured. Furthermore, from the viewpoint of the balance of physical properties between the flexibility and tensile strength at break of the obtained dip-molded product, the amount of antioxidant added is more preferably 0.5 to 5.0 parts by mass.

[0069] 6.3 Vulcanizing Agent and Vulcanization Accelerator The dip-molded product of a chloroprene polymer according to one embodiment of the present invention may contain a vulcanizing agent and / or a vulcanization accelerator. The chloroprene polymer latex composition used to obtain the dip-molded product may not contain sulfur or the aforementioned thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthogenate-based, thiazole-based, or other vulcanization accelerators. That is, the chloroprene polymer latex composition molded product includes those containing a vulcanizing agent but not a vulcanization accelerator, those containing a vulcanization accelerator but not a vulcanizing agent, those containing a vulcanization accelerator and a vulcanization accelerator, and those containing neither a vulcanizing agent nor a vulcanization accelerator. Whether or not a vulcanizing agent and a vulcanization accelerator are added may be determined depending on the desired dip-molded product.

[0070] Examples of vulcanizing agents include, but are not limited to, sulfur. The amount of the vulcanizing agent added can be 0 to 10.0 parts by mass per 100 parts by mass of the solid content of the chloroprene polymer latex contained in the chloroprene polymer latex composition. The amount of the vulcanizing agent added is, for example, 0, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, or 10.0 parts by mass, and may be within a range between any two of the values ​​exemplified here.

[0071] A vulcanization accelerator is a chemical added during the vulcanization of raw rubber to act with the vulcanizing agent to increase the vulcanization speed, thereby shortening the vulcanization time, lowering the vulcanization temperature, reducing the amount of vulcanizing agent, and improving the physical properties of the vulcanized rubber. It usually refers to a chemical that accelerates the sulfur vulcanization reaction.

[0072] Examples of vulcanization accelerators generally used in the vulcanization of chloroprene polymer latex include, but are not limited to, thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthogenate-based, thiazole-based, etc. These accelerators may be used singly or in combination of two or more types as required.

[0073] Examples of thiuram vulcanization accelerators include tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, tetrakis(2-ethylhexyl)thiuram disulfide, tetramethylthiuram monosulfide, and dipentamethylenethiuram tetrasulfide.

[0074] Examples of the dithiocarbamate vulcanization accelerator include sodium dibutyldithiocarbamate, zinc dimethyldithiocarbamate, zinc diethyldithiocarbamate, zinc N-ethyl-N-phenyldithiocarbamate, zinc N-pentamethylenedithiocarbamate, copper dimethyldithiocarbamate, ferric dimethyldithiocarbamate, and tellurium diethyldithiocarbamate, and zinc dibutyldithiocarbamate is particularly preferred.

[0075] Examples of the thiourea-based vulcanization accelerator include ethylene thiourea, N,N'-diethyl thiourea, trimethyl thiourea, and N,N'-diphenyl thiourea.

[0076] Examples of the guanidine vulcanization accelerator include 1,3-diphenylguanidine, 1,3-di-o-tolylguanidine, 1-o-tolylbiguanide, and di-o-tolylguanidine salts of dicatechol borate.

[0077] Examples of xanthogenate-based vulcanization accelerators include zinc butylxanthogenate and zinc isopropylxanthogenate.

[0078] Examples of the thiazole vulcanization accelerator include 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, 2-mercaptobenzothiazole zinc salt, 2-mercaptobenzothiazole cyclohexylamine salt, and 2-(4'-morpholinodithio)benzothiazole.

[0079] The amount of the vulcanization accelerator added may be 0 to 5.0 parts by mass relative to 100 parts by mass of the solid content of the chloroprene polymer latex contained in the chloroprene polymer latex composition, and may be, for example, 0, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, or 5.0, or may be within a range between any two of the numerical values ​​exemplified here.

[0080] 6.4 Other Agents (Heteroaromatic Ring Compounds) The dip-molded chloroprene polymer product according to the present invention may contain a heteroaromatic ring compound in the chloroprene polymer. The heteroaromatic ring compound contained in the chloroprene polymer latex composition used to obtain the dip-molded product can be represented by chemical formula (1) and has a benzimidazole structure. Compounds having this structure are sometimes used as secondary antioxidants, mainly in the formulation of rubber compositions.

[0081]

[0082] In chemical formula (1), X of the mercapto group represents a hydrogen atom or a metal atom. X may be a hydrogen atom and have a thiol group. X may also be a metal atom, and examples of the metal atom include zinc, sodium, copper, nickel, and tellurium, with zinc being preferred. R in chemical formula (1) 1 ~R 4 R represents a hydrogen atom, an alkyl group which may have a substituent, an ether group which may have a substituent, a nitro group, an amino group, or a carboxyl group. 1 ~R 4 may be the same or different. The heteroaromatic ring compounds may be used singly or in combination of two or more.

[0083] Examples of heteroaromatic ring compounds include 2-mercaptobenzimidazole, 5-methyl-2-mercaptobenzimidazole, 4-methyl-2-mercaptobenzimidazole, 5-methoxy-2-mercaptobenzimidazole, 4-methoxy-2-mercaptobenzimidazole, 5-nitro-2-mercaptobenzimidazole, 5-amino-2-mercaptobenzimidazole, 5-carboxy-2-mercaptobenzimidazole, and zinc salts of 2-mercaptobenzimidazole. Among these, 2-mercaptobenzimidazole, 5-methyl-2-mercaptobenzimidazole, 4-methyl-2-mercaptobenzimidazole, 5-methoxy-2-mercaptobenzimidazole, 4-methoxy-2-mercaptobenzimidazole, and zinc salts of 2-mercaptobenzimidazole are preferred.

[0084] The amount of the heteroaromatic ring compound added is preferably 0.2 to 10.0 parts by mass per 100 parts by mass of the solids content of the chloroprene polymer latex contained in the chloroprene polymer latex composition. The amount of the heteroaromatic ring compound added is, for example, 0.2, 0.3, 0.4, 0.5, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, or 10.0 parts by mass, and may be within a range between any two of the values ​​exemplified here. When the amount added is 0.2 parts by mass or more, the dip-molded article obtained using this composition exhibits extremely high tensile strength at break. When the amount added is 10.0 parts by mass or less, the stability of the chloroprene polymer latex composition is ensured. Furthermore, from the viewpoint of the balance of physical properties between the flexibility and tensile strength at break of the dip-molded article obtained, the amount added is more preferably 0.3 to 5.0 parts by mass.

[0085] 6.5 Properties of Dip-Molded Product The tensile strength at break of the dip-molded product according to the present invention, measured in accordance with JIS K6251, is preferably 17.0 MPa or more, and more preferably 20.0 MPa or more. The tensile strength at break is, for example, 17.0, 18.0, 19.0, 20.0, 21.0, 22.0, 23.0, 24.0, 25.0, 26.0, 27.0, 28.0, 29.0, 30.0, 31.0, 32.0, 33.0, 34.0, 35.0, 36.0, 37.0, 38.0, 39.0, or 40.0 MPa, and may be within a range between any two of the values ​​exemplified here. In particular, the ASTM standard "D3577" for surgical glove applications specifies that the tensile strength at break (breaking strength) must be 17 MPa or more, and it can be said that a tensile strength of 20 MPa indicates even more sufficient mechanical properties.

[0086] The dip-molded product according to one embodiment of the present invention preferably has a modulus at 100% elongation of 0.70 MPa or less, more preferably 0.5 MPa or less, as measured in accordance with JIS K 6251. The modulus at 100% elongation may be, for example, 0.30, 0.35, 0.40, 0.45, 0.50, 0.55, 0.60, 0.65, or 0.70 MPa, or may be within a range between any two of the values ​​exemplified here.

[0087] The dip-molded product contains a chloroprene polymer and may further contain an antioxidant or a metal oxide. The dip-molded product may also contain a vulcanizing agent, a vulcanization accelerator, and other chemicals. The manufacturing method of the dip-molded product and the methods for measuring the tensile strength at break and the modulus at 100% elongation may be as described in the Examples.

[0088] As described above, the tensile strength at break and the modulus at 100% elongation of the dip-molded product containing the chloroprene polymer latex composition can be controlled by adjusting the types and amounts of raw materials used in polymerizing the chloroprene polymer, the types and amounts of agents used, and polymerization conditions, and by adjusting the types and amounts of monomer units contained in the resulting chloroprene polymer, as well as the weight-average molecular weight and the mixing ratio of the chloroprene polymer.

[0089] 6.5 Shape of Dip-Molded Product The thickness (e.g., minimum thickness) of the dip-molded product may be 0.01 to 0.50 mm. The thickness of the dip-molded product may be, for example, 0.01, 0.05, 0.10, 0.20, 0.30, 0.40, or 0.50 mm, or may be within a range between any two of the values ​​exemplified here. The thickness of the dip-molded product can be adjusted by the time for immersing the mold in the polymer latex composition, the solids concentration of the chloroprene polymer latex composition, and the like. To reduce the thickness of the dip-molded product, the immersion time may be shortened or the solids concentration of the chloroprene polymer latex composition may be reduced.

[0090] The dip-molded product obtained from the chloroprene polymer latex composition may contain sulfur or a vulcanization accelerator. However, even if the dip-molded product does not contain sulfur or a vulcanization accelerator, the dip-molded product has mechanical properties equivalent to or superior to those of vulcanized dip-molded products obtained from conventional chloroprene polymer latexes. Therefore, the chloroprene polymer latex composition is suitably used as a raw material for the dip-molded product (dip-molded article) of the chloroprene polymer of this embodiment.

[0091] 7. Method for Producing Dip-Molded Article The method for producing a dip-molded article containing a chloroprene polymer according to the present invention can include: a molding step of molding a chloroprene polymer latex composition containing the chloroprene polymer using a calcium-based coagulation liquid by a dip coagulation method to obtain a dip-molded article; and a drying step of subjecting the obtained dip-molded article to a heat-drying treatment to obtain a dip-molded article.

[0092] The molding method for producing the immersion molded article of one embodiment of the present invention is not particularly limited, and may be performed according to a conventional method. Examples of molding methods include immersion coagulation, simple immersion, thermal immersion, and electrodeposition. The immersion coagulation method can be used from the viewpoints of ease of production and the ease of obtaining immersion molded articles of a uniform thickness. Specifically, a ceramic mold coated with a calcium-based coagulation liquid is immersed in a chloroprene polymer latex composition to coagulate the chloroprene polymer latex composition. After removing water-soluble impurities by leaching, the composition is dried, and then heated and vulcanized to form a immersion molded film (rubber film), which is then demolded. This allows for the production of a film-like immersion molded article.

[0093] Furthermore, a method for producing a dip-molded product according to one embodiment of the present invention may include a step of subjecting the obtained dip-molded product to a heat-drying treatment to vulcanize the unvulcanized dip-molded product. The heat-drying temperature may be appropriately set depending on the composition of the chloroprene polymer latex composition, and may be 100 to 220°C or 120 to 180°C. The vulcanization temperature may be, for example, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, or 220°C, or may be within a range between any two of the values ​​exemplified here. The heat-drying time may be appropriately set depending on the composition of the chloroprene polymer latex composition, the shape of the unvulcanized molded product, and the like, and may be 10 to 300 minutes. The heat drying time may be, for example, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, or 300 minutes, or may be within a range between any two of the values ​​exemplified here. As an example, a dip-molded product according to one embodiment of the present invention may be subjected to a heat drying treatment at 150°C for 1 hour.

[0094] The present invention will be described in more detail below based on examples, but the present invention should not be construed as being limited to these examples.

[0095] Example 1 Preparation of Chloroprene Polymer Example 1 Synthesis Example 1 A 30 L polymerization vessel was charged with 86 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 77 parts by mass of pure water, 17.6 parts by mass of gum rosin-based disproportionated potassium rosinate (aqueous solution) (trade name "LONDIS K-25" manufactured by Arakawa Chemical Industries, Ltd.), 0.02 parts by mass of n-dodecyl mercaptan, 0.8 parts by mass of potassium hydroxide, 0.5 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N" manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogensulfite, and 0.04 parts by mass of thiourea dioxide. Polymerization was carried out at a polymerization temperature of 13°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous solution of potassium persulfate as a polymerization initiator. When the polymerization rate reached 50%, 5 parts by mass of chloroprene (monomer) was added. When the polymerization rate reached 83%, 0.1 parts by mass of diethylhydroxylamine, a polymerization terminator, was added to terminate the polymerization, yielding a polymerization solution. The polymerization solution was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain latex a with a solids concentration of 55% by mass. The weight average molecular weight of latex a was measured using the method described below and found to be 735,432.

[0096] Synthesis Example 2 A 30 L polymerization vessel was charged with 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 77 parts by mass of pure water, 17.6 parts by mass of gum rosin-based disproportionated potassium rosinate (aqueous solution) (trade name "LONDIS K-25" manufactured by Arakawa Chemical Industries, Ltd.), 3.6 parts by mass of n-dodecyl mercaptan, 0.8 parts by mass of potassium hydroxide, 0.5 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N" manufactured by Kao Corporation), and 0.5 parts by mass of sodium hydrogen sulfite. Polymerization was carried out at a polymerization temperature of 35°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous solution of potassium persulfate as a polymerization initiator. When the polymerization rate reached 80%, 0.1 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization, yielding a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a latex b having a solid content of 55% by mass.

[0097] (Preparation of Chloroprene Polymer I) Next, these latexes a and b were mixed in a mass ratio of a / b = 80 / 20 to obtain a latex containing chloroprene polymer I. For measuring physical properties, 200 ml of the obtained latex was sampled, and a dipped film for evaluation was prepared using the remaining latex.

[0098] (Preparation of sample for dynamic viscoelasticity measurement) The sampled latex was poured into an iron frame (150 mm x 210 mm) to a height of about 1.5 mm, and left to stand at 23°C for 3 days to evaporate volatile matter, thereby obtaining a dried sheet. Dynamic viscoelasticity measurement was carried out using the obtained dried sheet. The results are shown in Table 1. The measurement conditions will be described later.

[0099] (Preparation of Samples for Measuring Weight-Average Molecular Weight and 2,3-Dichloro-1,3-Butadiene Content in Chloroprene Polymer) The sampled latex was mixed with a large amount of methanol to precipitate a rubber component (polymer), which was then filtered and dried to obtain a sample of chloroprene polymer I. The weight-average molecular weight of the chloroprene copolymer was measured from the obtained sample. In addition, the 2,3-dichloro-1,3-butadiene content (mass%) in the chloroprene polymer was determined by analysis. The analytical results are shown in Table 1. The measurement method will be described later.

[0100] (Example 2) (Synthesis Example 3) Polymerization was carried out in the same manner as in Synthesis Example 2, except that the amount of n-dodecyl mercaptan was changed to 5.3 parts by mass. The obtained polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and the resulting mixture was concentrated to obtain a latex c having a solid content of 55 mass%.

[0101] (Preparation of Chloroprene Polymer II) Chloroprene polymer latex II was obtained by mixing latex a and latex c obtained in the same procedure as in Synthesis Example 1 in a mass ratio of a / c = 80 / 20. 200 ml of the obtained latex was sampled for measuring physical properties, and a dipped film for evaluation was prepared using the remaining latex.

[0102] Using the sampled latex, a dry sheet was obtained in the same manner as in Example 1, and the dynamic viscoelasticity was measured in the same manner as in Example 1. The results are shown in Table 1.

[0103] Using the sampled latex, the weight average molecular weight of the chloroprene copolymer and the 2,3-dichloro-1,3-butadiene content (mass%) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0104] (Example 3) (Synthesis Example 4) Polymerization was carried out in the same manner as in Synthesis Example 2, except that the amount of n-dodecyl mercaptan was changed to 2.4 parts by mass. The obtained polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and the resulting mixture was concentrated to obtain a latex d having a solid content of 55 mass%.

[0105] (Preparation of Chloroprene Polymer III) Chloroprene polymer latex III was obtained by mixing latex a and latex d obtained in the same procedure as in Synthesis Example 1 in a mass ratio of a / d = 80 / 20. 200 ml of the obtained latex was sampled for measuring physical properties, and a dipped film for evaluation was prepared using the remaining latex.

[0106] Using the sampled latex, a dry sheet was obtained in the same manner as in Example 1, and the dynamic viscoelasticity was measured in the same manner as in Example 1. The results are shown in Table 1.

[0107] Using the sampled latex, the weight average molecular weight of the chloroprene copolymer and the 2,3-dichloro-1,3-butadiene content (mass%) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0108] (Example 4) (Synthesis Example 5) Polymerization was carried out in the same manner as in Synthesis Example 2, except that the amount of n-dodecyl mercaptan was changed to 1.5 parts by mass. The obtained polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and the resulting mixture was concentrated to obtain a latex e having a solid content of 55% by mass.

[0109] (Preparation of Chloroprene Polymer IV) Chloroprene polymer latex IV was obtained by mixing latex a and latex e obtained in the same procedure as in Synthesis Example 1 in a mass ratio of a / e = 80 / 20. 200 ml of the obtained latex was sampled for measuring physical properties, and a dipped film for evaluation was prepared using the remaining latex.

[0110] Using the sampled latex, a dry sheet was obtained in the same manner as in Example 1, and the dynamic viscoelasticity was measured in the same manner as in Example 1. The results are shown in Table 1.

[0111] Using the sampled latex, the weight average molecular weight of the chloroprene copolymer and the 2,3-dichloro-1,3-butadiene content (mass%) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0112] (Example 5) (Synthesis Example 6) Polymerization was carried out in the same manner as in Synthesis Example 1, except that 95 parts by mass of chloroprene (monomer) and 0 parts by mass of 2,3-dichloro-1,3-butadiene were used. When the polymerization rate reached 50%, 5 parts by mass of chloroprene (monomer) was added. When the polymerization rate reached 83%, 0.1 parts by mass of diethylhydroxylamine, a polymerization terminator, was added to terminate the polymerization, thereby obtaining a polymerization liquid. The obtained polymerization liquid was distilled under reduced pressure to remove unreacted monomer, and then concentrated to obtain latex f having a solids concentration of 55% by mass. The weight average molecular weight of latex f was measured by the method described below and was found to be 689,512.

[0113] Synthesis Example 7 Polymerization was performed in the same manner as in Synthesis Example 2, except that 100 parts by mass of chloroprene (monomer) and 0 part by mass of 2,3-dichloro-1,3-butadiene were used. The obtained polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a latex g having a solid content of 55 mass%.

[0114] (Preparation of Chloroprene Polymer V) Next, these latexes f and g were mixed in a mass ratio of f / g = 80 / 20 to obtain a chloroprene polymer latex V. For measuring physical properties, 200 ml of the obtained latex was sampled, and a dipped film for evaluation was prepared using the remaining latex.

[0115] Using the sampled latex, a dry sheet was obtained in the same manner as in Example 1, and the dynamic viscoelasticity was measured in the same manner as in Example 1. The results are shown in Table 1.

[0116] Using the sampled latex, the weight average molecular weight of the chloroprene copolymer and the 2,3-dichloro-1,3-butadiene content (mass%) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0117] Example 6 Polymerization was carried out in the same manner as in Synthesis Example 1, and the resulting polymer solution was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a latex a having a solid content of 55% by mass.

[0118] Polymerization was carried out in the same manner as in Synthesis Example 2, and the resulting polymer solution was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a latex b having a solid content of 55% by mass.

[0119] (Preparation of Chloroprene Polymer VI) Next, these latexes a and b were mixed in a mass ratio of a / b = 60 / 40 to obtain chloroprene polymer latex VI. For measuring physical properties, 200 ml of the obtained latex was sampled, and a dipped film for evaluation was prepared using the remaining latex.

[0120] Using the sampled latex, a dry sheet was obtained in the same manner as in Example 1, and the dynamic viscoelasticity was measured in the same manner as in Example 1. The results are shown in Table 1.

[0121] Using the sampled latex, the weight average molecular weight of the chloroprene copolymer and the 2,3-dichloro-1,3-butadiene content (mass%) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0122] Example 7 Polymerization was carried out in the same manner as in Synthesis Example 1, and the resulting polymer solution was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a latex a having a solid content of 55% by mass.

[0123] Polymerization was carried out in the same manner as in Synthesis Example 2, and the resulting polymer solution was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a latex b having a solid content of 55% by mass.

[0124] (Preparation of Chloroprene Polymer VII) Next, these latexes a and b were mixed in a mass ratio of a / b=90 / 10 to obtain chloroprene polymer latex VII. 200 ml of the obtained latex was sampled for measuring physical properties, and the remaining latex was used to prepare a dipped film for evaluation.

[0125] Using the sampled latex, a dry sheet was obtained in the same manner as in Example 1, and the dynamic viscoelasticity was measured in the same manner as in Example 1. The results are shown in Table 1.

[0126] Using the sampled latex, the weight average molecular weight of the chloroprene copolymer and the 2,3-dichloro-1,3-butadiene content (mass%) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0127] Example 8 Synthesis Example 8 A 30 L polymerization vessel was charged with 86 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 90 parts by mass of pure water, 4.4 parts by mass of potassium salt of conjugated resin acid-based rosin acid (trade name "Harthall R-WW" manufactured by Harima Chemicals Co., Ltd.), 0.02 parts by mass of n-dodecyl mercaptan, 0.8 parts by mass of potassium hydroxide, 0.5 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N" manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogen sulfite, and 0.04 parts by mass of thiourea dioxide. Polymerization was carried out at a polymerization temperature of 13°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous solution of potassium persulfate as a polymerization initiator. When the conversion rate reached 50%, 5 parts by mass of chloroprene (monomer) was added. When the polymerization rate reached 83%, 0.1 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization, and the polymerization solution was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a latex h with a solid content of 55% by mass.

[0128] Synthesis Example 9 To a 30 L polymerization vessel were added 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 90 parts by mass of pure water, 4.4 parts by mass of potassium salt of conjugated resin acid-based rosin acid (trade name "Harthall R-WW" manufactured by Harima Chemicals Co., Ltd.), 3.6 parts by mass of n-dodecyl mercaptan, 0.8 parts by mass of potassium hydroxide, 0.5 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N" manufactured by Kao Corporation), and 0.5 parts by mass of sodium hydrogen sulfite. Polymerization was carried out at a polymerization temperature of 35°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous solution of potassium persulfate as a polymerization initiator. When the polymerization rate reached 80%, 0.1 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization, yielding a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a latex i having a solid content of 55% by mass.

[0129] (Preparation of Chloroprene Polymer VIII) Next, these latexes h and i were mixed in a mass ratio of h / i = 80 / 20 to obtain chloroprene polymer latex VIII. 200 ml of the obtained latex was sampled for measuring physical properties, and the remaining latex was used to prepare a dipped film for evaluation.

[0130] Using the sampled latex, a dry sheet was obtained in the same manner as in Example 1, and the dynamic viscoelasticity was measured in the same manner as in Example 1. The results are shown in Table 1.

[0131] Using the sampled latex, the weight average molecular weight of the chloroprene copolymer and the 2,3-dichloro-1,3-butadiene content (mass%) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0132] Comparative Example 1 Polymerization was carried out in the same manner as in Synthesis Example 1, and the resulting polymer solution was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a latex a having a solid content of 55% by mass.

[0133] 200 ml of latex a was sampled, and the remaining latex was used to prepare a dipped film for evaluation.

[0134] Using the sampled latex, a dry sheet was obtained in the same manner as in Example 1, and the dynamic viscoelasticity was measured in the same manner as in Example 1. The results are shown in Table 1.

[0135] Using the sampled latex, the weight average molecular weight of the chloroprene copolymer and the 2,3-dichloro-1,3-butadiene content (mass%) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0136] Comparative Example 2 Polymerization was carried out in the same manner as in Synthesis Example 1, and the resulting polymer solution was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a latex a having a solid content of 55% by mass.

[0137] Polymerization was carried out in the same manner as in Synthesis Example 2, and the resulting polymer solution was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a latex b having a solid content of 55% by mass.

[0138] (Preparation of Chloroprene Polymer IX) Next, these latexes a and b were mixed in a mass ratio of a / b = 50 / 50 to obtain chloroprene polymer latex IX. For measuring physical properties, 200 ml of the obtained latex was sampled, and a dipped film for evaluation was prepared using the remaining latex.

[0139] Using the sampled latex, a dry sheet was obtained in the same manner as in Example 1, and the dynamic viscoelasticity was measured in the same manner as in Example 1. The results are shown in Table 1.

[0140] Using the sampled latex, the weight average molecular weight of the chloroprene copolymer and the 2,3-dichloro-1,3-butadiene content (mass%) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0141] Comparative Example 3 Synthesis Example 10 A 30 L polymerization vessel was charged with 100 parts by mass of chloroprene (monomer), 80 parts by mass of pure water, 4 parts by mass of gum rosin-based disproportionated potassium rosinate (aqueous solution) (trade name "LONDIS K-25" manufactured by Arakawa Chemical Industries, Ltd.), 0.05 parts by mass of n-dodecyl mercaptan, 0.4 parts by mass of sodium hydroxide, and 0.7 parts by mass of a sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N" manufactured by Kao Corporation). Polymerization was carried out at a polymerization temperature of 40°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous solution of potassium persulfate as a polymerization initiator. When the polymerization rate reached 90%, 0.05% by mass of 2,6-tert-butyl-4-methylphenol as a polymerization terminator was added to terminate the polymerization, thereby obtaining a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a latex j having a solid content of 55% by mass.

[0142] Synthesis Example 11 Polymerization was performed in the same manner as in Synthesis Example 10, except that the amount of n-dodecyl mercaptan was changed to 0.25 parts by mass. The obtained polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a latex k having a solid content of 55% by mass.

[0143] (Preparation of Chloroprene Polymer X) Next, these latexes j and k were mixed in a mass ratio of j / k = 50 / 50 to obtain a chloroprene polymer latex X. For measuring physical properties, 200 ml of the obtained latex was sampled, and a dipped film for evaluation was prepared using the remaining latex.

[0144] Using the sampled latex, a dry sheet was obtained in the same manner as in Example 1, and the dynamic viscoelasticity was measured in the same manner as in Example 1. The results are shown in Table 1.

[0145] Using the sampled latex, the weight average molecular weight of the chloroprene copolymer and the 2,3-dichloro-1,3-butadiene content (mass%) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0146] (Comparative Example 4) (Synthesis Example 12) Polymerization was performed in the same procedure as in Synthesis Example 10, except that the amounts of chloroprene (monomer), 2,3-dichloro-1,3-butadiene, and n-dodecyl mercaptan were changed to 90 parts by mass, 10 parts by mass, and 0.07 parts by mass of n-dodecyl mercaptan in Synthesis Example 10. The obtained polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain latex 1 having a solid content of 55 mass%.

[0147] Synthesis Example 13 Polymerization was performed in the same procedure as in Synthesis Example 10, except that the amounts of chloroprene (monomer) 90 parts by mass, 2,3-dichloro-1,3-butadiene 10 parts by mass, and n-dodecyl mercaptan 0.31 parts by mass were changed. The obtained polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a latex m having a solid content of 55 mass%.

[0148] (Preparation of Chloroprene Polymer XI) Next, these latexes 1 and m were mixed in a mass ratio of 1 / m = 30 / 70 to obtain chloroprene polymer latex XI. For measuring physical properties, 200 ml of the obtained latex was sampled, and a dipped film for evaluation was prepared using the remaining latex.

[0149] Using the sampled latex, a dry sheet was obtained in the same manner as in Example 1, and the dynamic viscoelasticity was measured in the same manner as in Example 1. The results are shown in Table 1.

[0150] Using the sampled latex, the weight average molecular weight of the chloroprene copolymer and the 2,3-dichloro-1,3-butadiene content (mass%) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.

[0151] The chloroprene polymer was analyzed by the following method. <Measurement of dynamic viscoelasticity of chloroprene polymer> The dried sheet of each Example and Comparative Example was used as a film containing a chloroprene polymer. A strip-shaped test piece (width: 4.5 mm, length: 30 mm, thickness: 0.80 to 0.90 mm) was cut out of the chloroprene polymer-containing film of each Example and Comparative Example. Using the obtained strip-shaped test piece, tensile dynamic viscoelasticity measurement (chuck distance: 20 mm) was performed in accordance with the non-resonant forced vibration method. The measurement conditions were a static tension of 5 gf, a temperature of 25°C, and a strain of 0.75%, and the loss tangent tanδ was measured in the frequency range of 10 Hz. The measurement device used was a DDV-25FP manufactured by Orientec Co., Ltd. The results are shown in Table 1.

[0152] <Measurement of Weight-Average Molecular Weight of Chloroprene-Based Polymer> The weight-average molecular weight was measured by gel permeation chromatography (GPC) under the following measurement conditions using a sample obtained by dissolving a polymer precipitated from a latex containing a chloroprene-based polymer in 20 ml of tetrahydrofuran. Apparatus name: HLC-8320 (manufactured by Tosoh Corporation) Column: Three TSKgel GMHHR-H columns in series Temperature: 40°C Detection: Differential refractive index Solvent: Tetrahydrofuran Calibration curve: Prepared using standard polystyrene (PS).

[0153] <Measurement of 2,3-dichloro-1,3-butadiene Content in Chloroprene Polymer> A polymer precipitated from a latex containing a chloroprene polymer was cut into a 0.05 mg test piece and measured by pyrolysis gas chromatography to determine the area ratio of the peak derived from chloroprene to the peak derived from 2,3-dichloro-1,3-butadiene. The content of 2,3-dichloro-1,3-butadiene (mass%) in the chloroprene polymer was determined using a calibration curve of the area ratio of the peak derived from chloroprene to the peak derived from 2,3-dichloro-1,3-butadiene and the 2,3-dichloro-1,3-butadiene content.

[0154] [Gas chromatogram measurement conditions] Pyrolysis gas chromatogram measurement conditions Device name: HP5890-II Column: DB-5 0.25 mmφ×30 m (film thickness 1.0 μm) Column temperature: 50°C (5 min) → 10°C / min → 150°C → 25°C / min → 300°C Injection port temperature: 250°C Detector temperature: 280°C Detector: FID

[0155] Dip-molded articles containing chloroprene polymers were evaluated by the following method. <Preparation of Dip-molded Articles for Evaluation of Tensile Properties> A chloroprene polymer latex composition was prepared by mixing 100 parts by mass of the solids content of each chloroprene polymer-containing latex with an aqueous dispersion, and adding water to adjust the overall solids concentration of the blend to 30% by mass. The aqueous dispersion was prepared by mixing 2 parts by mass of two types of zinc oxide, 2 parts by mass of a butylated reaction product of p-cresol and dicyclopentadiene (trade name "Nocrac PBK", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 2 parts by mass of dibutyldithiocarbamic acid (trade name "Nocrac BZ", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 1 part by mass of sulfur, 0.1 part by mass of a sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N", manufactured by Kao Corporation), and 10.7 parts by mass of water in a ceramic ball mill at 20°C for 16 hours. The obtained chloroprene polymer latex composition contains, relative to 100 parts by mass of the solid content of the chloroprene polymer latex, 2 parts by mass of two types of zinc oxide, 2 parts by mass of a butylated reaction product of p-cresol and dicyclopentadiene (trade name "Nocrac PBK", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 2 parts by mass of dibutyldithiocarbamic acid (trade name "Nocrac BZ", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 1 part by mass of sulfur, 0.1 part by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "Demol N", manufactured by Kao Corporation), and water.

[0156] A ceramic hand-shaped 7.5 size surgical glove mold (manufactured by Shinko Co., Ltd.) was immersed for 1 second in a coagulation solution containing 62 parts by weight of water, 35 parts by weight of calcium nitrate tetrahydrate, and 3 parts by weight of calcium carbonate, and then removed. After drying for 3 minutes, the mold was immersed for 2 minutes in the chloroprene polymer latex composition prepared by the procedure described above. The mold was then washed with running water at 45°C for 1 minute and dried at 150°C for 60 minutes to prepare a glove-shaped dip-molded film for texture evaluation. Using the same procedure, a ceramic cylindrical mold with an outer diameter of 50 mm was used to prepare a dip-molded film for tensile property evaluation.

[0157] <Tensile Properties> (Film Thickness) The thickness (film thickness) of the dip-molded film for evaluating tensile properties was measured at three points in the center using a test piece thickness gauge (manufactured by Kobunshi Keiki Co., Ltd., product name: ASKER SDA-12), and the smallest thickness was taken as the thickness of the film for evaluation. The results are shown in Table 1.

[0158] (Measurement of Tensile Properties) Using the dip-molded film for evaluating tensile properties, the modulus at 100% elongation and the tensile strength at break were measured in accordance with JIS K 6251. The results are shown in Table 1.

[0159] <Evaluation of texture of glove-shaped dip-molded products> Five subjects were asked to touch the obtained dip-molded products (glove-shaped films) and evaluate the texture of the dip-molded products by touching the surface condition, stretching, and bending. The evaluation was carried out according to the following criteria, and the average of the evaluations of each subject was rounded off to the nearest whole number.

[0160] (Texture evaluation criteria) 3: Extremely soft and pleasant to the touch, excellent texture 2: Soft, no practical problems with the touch, good texture 1: Not very soft, felt a little hard to the touch, poor texture

[0161]

Claims

1. A chloroprene-based polymer, a loss tangent tanδ of a film containing the chloroprene polymer in a frequency range of 10 Hz, as measured by a non-resonant forced vibration method under conditions of a temperature of 25° C. and a strain of 0.75%, is 0.08 to 0.14; The film is obtained by drying a chloroprene polymer latex containing the chloroprene polymer at 23° C. for 3 days. Chloroprene polymer.

2. 2. The chloroprene polymer according to claim 1, wherein a peak having a weight average molecular weight of 5,000 to 80,000 is detected when a tetrahydrofuran-soluble portion of the chloroprene polymer is measured by gel permeation chromatography.

3. 2. The chloroprene polymer according to claim 1, which contains a monomer unit derived from 2,3-dichloro-1,3-butadiene.

4. A dip-molded product comprising the chloroprene polymer according to any one of claims 1 to 3.

5. The dip-molded article according to claim 4, which is an industrial or general household glove, a medical glove, a balloon, a catheter or a boot.