Oxide-containing plate-like copper particles, paste composition, semiconductor device, electrical component and electronic component

JPWO2023191024A5Active Publication Date: 2024-11-19KYOCERA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024512885
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2023-03-31
Publication Date
2024-11-19
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

Conductive pastes with oxide-containing copper particles suffer from low bonding strength and reliability due to the generation of pores in the bonding layer when spherical particles are sintered and bonded, leading to reduced thermal conductivity and stability in semiconductor and electronic devices.

Method used

The use of oxide-containing plate-shaped copper particles with a specific oxygen content range (2.1-25.0% by mass) and sintering conditions, which facilitate denser bonding layers with higher strength and reliability by promoting copper atom movement and phase stability, resulting in improved thermal conductivity and bonding reliability.

Benefits of technology

The oxide-containing plate-shaped copper particles form high-density bonding layers with enhanced bonding strength and reliability, improving thermal conductivity and stability in semiconductor and electronic devices, even under repeated thermal cycles.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides: oxide-containing plate-like copper particles which enable the achievement of a paste composition that is capable of forming a bonding layer having high denseness, high bonding strength and high bonding reliability; a paste composition which uses the oxide-containing plate-like copper particles; and a semiconductor device, an electrical component and an electronic component. Copper oxide-containing plate-like copper particles according to the present disclosure contain Cu, Cu2O and Cu64O; and the content of Cu64O is 2.1% by mass to 25.0% by mass relative to a total of 100% by mass of Cu, Cu2O and Cu64O.
Need to check novelty before this filing date? Find Prior Art

Description

Oxide-containing plate-shaped copper particles, paste composition, semiconductor device, electrical component and electronic component

[0001] The present disclosure relates to oxide-containing plate-like copper particles, a paste composition using the same, and semiconductor devices, electrical components, and electronic components.

[0002] In semiconductor devices and various electric and electronic components, highly thermally conductive pastes are used as adhesives for joining components. Semiconductor devices generate more heat due to their higher integration and faster operation. To ensure stable operation, measures have been taken to dissipate heat, such as bonding heat-generating components such as semiconductor elements to heat-dissipating components with highly thermally conductive adhesives (pastes). Highly thermally conductive conductive pastes are also used for die-bonding bare chips, bonding LED chips, bonding electrodes to lead wires, and the like.

[0003] A paste composition containing copper particles has been proposed as one type of conductive paste with high thermal conductivity. Applications of such paste compositions to printed electronics are also being considered. For example, Patent Documents 1 and 2 disclose that oxide-containing copper particles obtained by sintering a copper raw material at a low temperature are used as a constituent material of a conductive paste.

[0004] JP 2020-29392 A International Publication No. 2022 / 045252

[0005] The present disclosure relates to the following: [1] Cu, Cu 2 O and Cu 64 Contains O, Cu 64 The content of O is Cu, Cu 2 O and Cu 64 Copper oxide-containing plate-like copper particles, wherein the content of the copper oxide is 2.1 to 25.0 mass% relative to 100 mass% of the total of O.

[0006] 1 is an image of the oxide-containing plate-like copper particles of Example 4 observed by a scanning electron microscope. 2 is an image of the oxide-containing copper particles of Comparative Example 2 observed by a scanning electron microscope.

[0007] The conductive pastes using oxide-containing copper particles as described in Patent Documents 1 and 2 have substantially spherical particles, which may result in voids in the bonding layer when sintered and bonded, resulting in low density and difficulty in obtaining sufficient bonding strength, which may result in low bonding reliability.

[0008] The present disclosure relates to oxide-containing copper particles that can provide a paste composition capable of forming a bonding layer that has high density, high bonding strength, and high bonding reliability, as well as a paste composition using the same, and a semiconductor device, an electrical component, and an electronic component.

[0009] The present disclosure will be described in detail below with reference to one embodiment. The oxide-containing plate-like copper particles in the present disclosure refer to particles that contain metallic copper and at least one copper oxide and have a plate-like particle shape. Hereinafter, they will also be referred to simply as copper particles.

[0010] In this specification, the expression "XX to YY" means "XX or more and YY or less." In addition, in this specification, for a numerical range (for example, a range of content, etc.), lower limit values ​​and upper limit values ​​described in stages can be independently combined. In addition, in a numerical range described in this specification, the upper limit value or lower limit value of the numerical range may be replaced with a value shown in an example.

[0011] [Oxide-containing plate-like copper particles] The oxide-containing plate-like copper particles of the present disclosure are Cu, Cu 2 O and Cu 64 Contains O, Cu 64 The content of O is Cu, Cu 2 O and Cu 64 The copper content is 2.1 to 25.0 mass% relative to 100 mass% of the total of O. The copper particles of the present disclosure are composed of Cu and copper oxide, Cu 2 O and Cu 64 O, and has good sinterability and reducibility. 64 When the O content is within the above range, it is possible to obtain a paste composition that can form a bonding layer that is highly dense, has high bonding strength, and has high bonding reliability.

[0012] Cu 64 O is CuO and Cu2 The proportion of oxygen atoms is low compared to O, and the phase stability is low. 64 If the O content is high, self-oxidation decomposition is likely to occur during sintering, making it difficult to reduce, while Cu is easily decomposed by heating. 64 It is believed that the copper atoms constituting O become more easily mobile or diffuse, facilitating sintering. 64 If the O content is 2.1 mass% or more, Cu 64 The movement or diffusion of copper atoms constituting O facilitates sintering. 64 If the O content is 25.0 mass% or less, Cu 64 O is sufficiently reduced, and copper particles with good sinterability are obtained. 64 The O content may be 2.5 to 25.0 mass %, or 3.0 to 20.0 mass %.

[0013] The copper particles are Cu 2 The content of Cu, CuO is determined from the viewpoint of good sinterability of the copper particles. 2 O and Cu 64 With respect to 100% by mass of the total of O, the content may be 5.0% by mass or less, may be 0.1 to 4.5% by mass, or may be 1.0 to 4.0% by mass.

[0014] Cu in copper particles, Cu 64 O and Cu 2 Cu relative to 100% by mass of the total of O 64 O and Cu 2 The content of each of the O components is determined from the X-ray diffraction (XRD) pattern by the reference intensity ratio (RIR) method. The XRD pattern is obtained by performing XRD measurement by irradiating the sample with characteristic X-rays of CuKα rays (wavelength 0.15418 nm). Specifically, the measurement is performed by the method described in the Examples. In the XRD pattern, the strongest rays of each component (Cu(111), Cu 64 O(044) and Cu 2 For Cu(111), the integrated intensity after subtracting the background intensity and each RIR value (Cu: 8.86, Cu 64 O: 4.89, Cu 2The diffraction angle 2θ of each peak is 43.298° for Cu (111), 44.298° for Cu (111), and 44.298° for Cu (111). 64 O(044) is 40.710°, Cu 2 O(111) is 36.419°.

[0015] The copper particles may have a ratio (C2 / C1) of 2.0 or more of the Cu(111) crystallite size (C2) after heating to the Cu(111) crystallite size (C1) before heating when heated at 200°C under a nitrogen atmosphere. That is, the ratio C2 / C1 of the Cu(111) crystallite size before and after heating at 200°C under a nitrogen atmosphere may be 2.0 or more, 3.0 to 10.0, or 4.0 to 8.0, from the viewpoints of sinterability, compactness, and bonding strength.

[0016] From a practical standpoint, heating at 200°C under a nitrogen atmosphere is a heating condition that takes into account the atmosphere and temperature when using a paste composition containing copper particles as a joining material and joining is performed by sintering the copper particles.

[0017] The crystallite diameter (C2) may be 55.0 nm or more, 57.0 to 80.0 nm, or 58.0 to 75.0 nm, from the viewpoints of sinterability, density, and bonding strength.

[0018] The crystallite size (C1) may be 5.0 to 30.0 nm, 7.0 to 25.0 nm, or 8.0 to 20.0 nm, from the viewpoints of sinterability, density, and bonding strength.

[0019] The crystallite size of Cu(111) of the copper particles can be determined from the XRD pattern, specifically by the method described in the Examples.

[0020] The copper particles are plate-shaped particles. The thickness of the copper particles may be 5 to 50 nm, 8 to 40 nm, or 10 to 30 nm. The major axis of the copper particles may be 30 to 300 nm, 50 to 200 nm, or 75 to 150 nm, and the major axis may be greater than the thickness.

[0021] The aspect ratio (major axis / thickness) of the copper particles may be 1.5 to 10.0, 2.0 to 9.0, or 3.0 to 8.0.

[0022] Since the copper particles are plate-shaped particles, the contact area between the particles is larger than that of spherical particles. It is presumed that the bonding layer formed from the paste composition using the plate-shaped particles has a high density, high bonding strength, and is likely to have high bonding reliability.

[0023] The thickness and major axis of the copper particles are each the median of the measured length values ​​of at least 200 particles extracted from images taken by scanning electron microscope (SEM) observation. Specifically, the thickness and major axis of the copper particles can be measured by the method described in the Examples. The plate-like particles have a shape having a pair of approximately parallel flat surfaces, and the distance between the pair of flat surfaces is defined as the "thickness" and the longest diameter on the flat surfaces is defined as the "major axis."

[0024] The copper particles are typically sintered by heating to 100 to 250°C in an inert gas atmosphere. Examples of inert gases include nitrogen, argon, and helium. Nitrogen is preferred from the viewpoints of availability and cost. The heating temperature may be 120 to 230°C or 150 to 200°C from the viewpoint of good sinterability. Sintering may be performed under normal pressure or under pressure. The heating time is appropriately set depending on the heating temperature, the shape of the sintered body, and the like. From the viewpoint of sufficient sintering progress, the heating time may be, for example, 5 to 180 minutes, 10 to 120 minutes, or 30 to 90 minutes.

[0025] [Method for producing oxide-containing plate-like copper particles] The method for producing oxide-containing plate-like copper particles of the present disclosure is not particularly limited.For example, a method of reducing a copper compound using a reducing compound in the presence of a shape stabilizer can be mentioned.The copper compound, the shape stabilizer and the reducing compound can be mixed in an organic solvent.

[0026] (Copper Compound) Examples of copper compounds include copper oxide, copper hydroxide, copper nitride, copper carboxylate, etc. The copper compound may be copper oxide from the viewpoint of obtaining the copper particles of the present disclosure in high yield. The copper compound may be used alone or in combination of two or more.

[0027] Copper oxide includes copper oxide (I) (cuprous oxide: Cu 2 Examples of copper carboxylates include copper (I) formate, copper (I) acetate, copper (I) propionate, copper (I) butyrate, copper (I) valerate, copper (I) hexanoate, copper (I) octanoate, and copper (I) decanoate, as well as copper carboxylate anhydrides or hydrates such as copper (II) formate, copper (II) acetate, copper (II) propionate, copper (II) butyrate, copper (II) valerate, copper (II) hexanoate, copper (II) octanoate, and copper (II) decanoate. Commercially available copper carboxylates may be used. Copper carboxylates synthesized by known methods may also be used. From the viewpoints of availability and the production efficiency of the copper particles of the present disclosure, the copper carboxylate may be copper (II) acetate monohydrate.

[0028] (Shape Stabilizer) The shape stabilizer may be, for example, at least one selected from the group consisting of an amine compound, a carboxylic acid, and a phosphate ester, or a combination of an amine compound and a carboxylic acid. The shape stabilizer coats at least a portion of the oxide-containing copper particles of the present disclosure, making it easier to obtain the desired light absorption characteristics of the present disclosure. Furthermore, the fluidity of a paste composition using the copper particles is improved.

[0029] Examples of the amine compound include monoamines such as dipropylamine, butylamine, dibutylamine, hexylamine, cyclohexylamine, heptylamine, octylamine, nonylamine, decylamine, 3-aminopropyltriethoxysilane, dodecylamine, oleylamine, monoethanolamine, 2-aminoethoxy-2-ethanol, 3-amino-1-propanol, 3-amino-2-propanol, 4-amino-1-butanol, 3-amino-1-hexanol, and 2-(2-aminoethoxy)ethanol; ethylenediamine, N,N-dimethylethylenediamine, and the like. Examples of the amine compound include diamines such as hexane, N,N'-dimethylethylenediamine, N,N-diethylethylenediamine, N,N'-diethylethylenediamine, 1,3-propanediamine, 2,2-dimethyl-1,3-propanediamine, N,N-dimethyl-1,3-diaminopropane, N,N'-dimethyl-1,3-diaminopropane, N,N-diethyl-1,3-diaminopropane, 1,4-diaminobutane, 1,5-diamino-2-methylpentane, 1,6-diaminohexane, N,N'-dimethyl-1,6-diaminohexane, 1,7-diaminoheptane, and 1,8-diaminooctane. The amine compound may be used alone or in combination of two or more. The amine compound may be an amino alcohol, and the molecular weight of the amino alcohol may be 80 or more and 150 or less.

[0030] Examples of carboxylic acids include monocarboxylic acids such as formic acid, acetic acid, propionic acid, butyric acid, valeric acid, hexanoic acid, heptanoic acid, octanoic acid, octylic acid, nonanoic acid, decanoic acid, oleic acid, stearic acid, and isostearic acid; and dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, and diglycolic acid. The carboxylic acid may be an aromatic carboxylic acid such as benzoic acid, phthalic acid, isophthalic acid, terephthalic acid, salicylic acid, or gallic acid, or a hydroxy acid such as glycolic acid, lactic acid, tartronic acid, malic acid, glyceric acid, hydroxybutyric acid, tartaric acid, citric acid, or isocitric acid. One type of carboxylic acid may be used alone, or two or more types may be used in combination. The carboxylic acid may be a monocarboxylic acid. The molecular weight of the monocarboxylic acid may be 80 or more and 150 or less.

[0031] The phosphate ester can remove the oxide film formed on the surface of copper particles by heating in the atmosphere, thereby improving the sinterability of the copper particles. The phosphate ester can also improve the lubricity of the copper particles in the paste composition. The phosphate ester may be added after the reduction reaction. Examples of the phosphate ester include alkyl phosphates, polyoxyethylene alkyl ether phosphates, and polyoxyethylene alkyl phenyl ether phosphates. The acid value and amine value of the phosphate ester may both be 130 mg KOH / g or less, 120 mg KOH / g or less, or 110 mg KOH / g or less. The ratio of the acid value to the amine value (acid value / amine value) may be 0 to 1.5 or 0 to 1.2. The acid value is determined by a method in accordance with JIS K 0070:1992, and the amine value is determined by a method in accordance with JIS K 7237:1995.

[0032] The total amount of the shape stabilizer used may be 0.1 to 10 mol, 0.5 to 8 mol, or 1 to 5 mol, per mol of the copper compound. When, for example, an amine compound and a carboxylic acid are used as the shape stabilizer, the blending molar ratio of the amine compound to the carboxylic acid may be 1 / 5 to 5 / 1, 1 / 3 to 3 / 1, or 1 / 2 to 2 / 1.

[0033] (Reducing Compound) The reducing compound is not particularly limited as long as it has the reducing power to reduce the copper compound and liberate metallic copper. Examples of the reducing compound include hydrazine derivatives. The reducing compound may be used alone or in combination of two or more. Examples of hydrazine derivatives include hydrazine monohydrate, methylhydrazine, ethylhydrazine, n-propylhydrazine, isopropylhydrazine, n-butylhydrazine, isobutylhydrazine, sec-butylhydrazine, tert-butylhydrazine, n-pentylhydrazine, isopentylhydrazine, neopentylhydrazine, tert-pentylhydrazine, n-hexylhydrazine, isohexylhydrazine, n-heptylhydrazine, n-octylhydrazine, n-nonylhydrazine, n-decylhydrazine, n-undecylhydrazine, n-dodecylhydrazine, cyclohexylhydrazine, phenylhydrazine, 4-methylphenylhydrazine, benzylhydrazine, 2-phenylethylhydrazine, 2-hydrazinoethanol, and acetohydrazine.

[0034] The amount of the reducing compound used may be 0.1 to 10 mol, 0.5 to 5 mol, or 0.8 to 3 mol per mol of the copper compound.

[0035] (Organic Solvent) The organic solvent is not particularly limited as long as it is capable of carrying out a uniform reaction without inhibiting the properties of the complex formed by mixing the copper compound, shape stabilizer, and reducing compound. The organic solvent may be compatible with the reducing compound. Examples of the organic solvent include alcohols such as 1-propanol, 2-propanol, butanol, pentanol, hexanol, heptanol, octanol, ethylene glycol, 1,3-propanediol, 1,2-propanediol, butyl cellosolve, ethyl carbitol, and butyl carbitol; butyl carbitol acetate, ethyl carbitol acetate, and diethylene glycol diethyl ether. One type of organic solvent may be used alone, or two or more types may be used in combination.

[0036] When an organic solvent is used, the amount used may be such that the copper compound, the shape stabilizer, and the reducing compound can be uniformly mixed. The amount of the organic solvent used may be, for example, 0.1 to 500 times by volume the volume of the shape stabilizer.

[0037] The reduction reaction of the copper compound may be heated from the viewpoint of sufficient reaction progress. The reaction temperature may be −20 to 140° C., 25 to 120° C., or 40 to 100° C. The reaction time may be 20 to 360 minutes, 30 to 300 minutes, or 40 to 240 minutes from the viewpoint of sufficient reaction progress.

[0038] When the content of the vessel in which the reduction reaction was carried out is a liquid (liquid mixture), the solid matter may be separated, for example, by centrifugation or the like. The obtained solid matter may be washed with an organic solvent, and further, by centrifugation or the like, the solid matter may be obtained as a cake of copper particles. The washing method is not particularly limited as long as the shape stabilizer, reducing compound, etc. are sufficiently removed. The organic solvent for washing may be alcohol. Examples of alcohol include ethanol, 1-propanol, 2-propanol, butanol, pentanol, hexanol, heptanol, octanol, ethylene glycol, 1,3-propanediol, 1,2-propanediol, diethylene glycol, butyl cellosolve, ethyl carbitol, butyl carbitol, etc. The organic solvent for washing may be used alone, or two or more types may be used in combination.

[0039] [Paste Composition] The paste composition of the present disclosure contains the oxide-containing plate-like copper particles of the present disclosure. The content of the copper particles in the paste composition may be 10 to 95% by mass, 20 to 90% by mass, or 30 to 85% by mass. Note that in the present disclosure, the nonvolatile content, which is the components excluding the organic solvent in the paste composition, is considered to be the content of the copper particles.

[0040] The paste composition may be diluted with an organic solvent from the viewpoints of handleability during use, viscosity, etc. Examples of organic solvents include 1-propanol, 2-propanol, ethylene glycol, 1,3-propanediol, 1,2-propanediol, diethylene glycol, propylene glycol, dipropylene glycol, 1,4-butanediol, 3-methyl-1,5-pentanediol, glycerin, polyethylene glycol, etc., from the viewpoints of dispersibility of copper particles and volatility during sintering of the paste composition. The organic solvent may be used alone, or two or more types may be used in combination. The organic solvent for dilution may be the same as the organic solvent for washing the copper particles.

[0041] The paste composition of the present disclosure may contain, in addition to copper particles, an organic solvent, and components derived from the production of the copper particles, known additives that are commonly used in conductive pastes, as needed. Examples of additives include thermosetting resins, curing accelerators, stress-reducing agents such as rubber and silicone, coupling agents, antifoaming agents, surfactants, colorants such as pigments and dyes, polymerization inhibitors, and antioxidants. The additives may be used alone or in combination of two or more.

[0042] The paste composition of the present disclosure can be prepared by kneading a mixture of copper particles, an organic solvent, and additives used as needed using a kneading machine such as a disperse, kneader, three-roll mill, or planetary mixer, followed by degassing.

[0043] A cured product of the paste composition of the present disclosure contains a sintered body of the copper particles of the present disclosure and has high thermal conductivity and excellent heat dissipation. Therefore, when the paste composition of the present disclosure is used as a bonding material for substrates of elements or heat dissipation components, the thermal conductivity of the device is improved and the ability to dissipate heat from inside the device to the outside is improved. Therefore, the use of the paste composition of the present disclosure can stabilize the operation of various products such as semiconductor devices, electrical components, and electronic components.

[0044] [Semiconductor Device] At least a portion of the semiconductor device of the present disclosure is bonded using the paste composition of the present disclosure. For example, the semiconductor device may be one in which a semiconductor element and a substrate serving as an element support member are bonded using the paste composition. The paste composition may be used as a die bond.

[0045] By using the paste composition of the present disclosure for bonding, a bonding layer with high density and high bonding strength is formed. The bonding layer has a low rate of change in thermal resistance even when subjected to repeated temperature changes, and high bonding reliability, resulting in a semiconductor device with stable operation.

[0046] The semiconductor element may be a known semiconductor element, for example, a transistor, a diode, etc., or a wide band gap semiconductor element using SiC, GaN, etc., or a light emitting element such as an LED. Examples of the element support member include a copper plate, a silver-plated copper plate, a lead frame (PPF; Pre Plated Leadframe) plated with Ni / Pd, Ti / Pd / Au, Ni / Pd / Au, etc., a glass epoxy plate, a ceramic member, etc.

[0047] The bonding strength of the bonding layer formed using the paste composition for bonding varies depending on the purpose and object of bonding, but from the viewpoint of sufficient bonding strength, it may be 20 MPa or more, 30 MPa or more, or 40 MPa or more. The bonding strength is a die shear strength, and specifically, it can be measured by the method described in the examples.

[0048] From the viewpoint of good bonding strength and high bonding reliability, the density of the bonding layer may be 78% or more, 80% or more, or 82% or more. The density is the proportion of the sintered body portion in the bonding layer, and specifically, can be measured by the method described in the examples.

[0049] [Electrical and Electronic Components] At least a portion of the electrical or electronic components of the present disclosure is bonded using the paste composition of the present disclosure. Examples of the electrical or electronic components include those in which a heat-generating component and a heat-dissipating component are bonded using the paste composition. The paste composition may be used as an adhesive for heat-dissipating components.

[0050] By using the paste composition of the present disclosure for bonding, a bonding layer with high density and high bonding strength is formed. The bonding layer has a low rate of change in thermal resistance and high bonding reliability even when subjected to repeated thermal cycles (heat cycles), resulting in high heat dissipation and reduced temperature rise in heat-generating components, resulting in an electric or electronic component with stable operation.

[0051] Examples of heat-generating components include optical pickups and power transistors. The heat-generating component may be the semiconductor element or a component having the semiconductor element. Examples of heat-dissipating components include heat sinks and heat spreaders. The heat-generating component and the heat-dissipating component may be directly bonded via the paste composition, or may be indirectly bonded via another component with high thermal conductivity sandwiched therebetween.

[0052] Next, the present disclosure will be specifically described using examples, but the present disclosure is not limited to these examples in any way.

[0053] [Production of Oxide-Containing Copper Particles] The compounds used in the production of oxide-containing copper particles in each of the Examples and Comparative Examples are as follows: <Copper Compound> FRC-D70: Cuprous oxide; manufactured by Furukawa Chemicals Corporation; specific surface area 0.2 m 2 / g FRC-D30: Cuprous oxide; manufactured by Furukawa Chemicals Co., Ltd.; specific surface area 0.5 m 2 / g FRC-05B: Cuprous oxide; manufactured by Furukawa Chemicals Co., Ltd.; specific surface area 2.3 m 2 / g <Amine compounds> 4-amino-1-butanol; manufactured by Tokyo Chemical Industry Co., Ltd. 2-(2-aminoethoxy)ethanol; manufactured by Tokyo Chemical Industry Co., Ltd. 6-amino-1-hexanol; manufactured by Tokyo Chemical Industry Co., Ltd. 3-amino-1-propanol; manufactured by Tokyo Chemical Industry Co., Ltd. n-Octylamine; manufactured by Tokyo Chemical Industry Co., Ltd. <Carboxylic acids> Hexanoic acid; manufactured by Tokyo Chemical Industry Co., Ltd. Octanoic acid; manufactured by Tokyo Chemical Industry Co., Ltd. Acetic acid; manufactured by Tokyo Chemical Industry Co., Ltd. Decanoic acid; manufactured by Tokyo Chemical Industry Co., Ltd. <Reducing compounds> Hydrazine monohydrate; manufactured by Fujifilm Wako Pure Chemical Industries Co., Ltd. <Organic solvents> 1-propanol; manufactured by Tokyo Chemical Industry Co., Ltd. Ethanol; manufactured by Tokyo Chemical Industry Co., Ltd. Diethylene glycol; manufactured by Tokyo Chemical Industry Co., Ltd.

[0054] Example 1: A 2000 mL round-bottom flask was charged with 10 mmol of cuprous oxide (FRC-D70), 20 mmol of 4-amino-1-butanol, 20 mmol of hexanoic acid, 10 mmol of hydrazine monohydrate, and 400 mL of 1-propanol. The mixture was heated in an 80°C oil bath while stirring at 250 rpm and mixed for 180 minutes. The resulting mixture was centrifuged (25°C, 10,000 rpm, 15 minutes; the same conditions apply hereinafter), and the supernatant was removed. Ethanol was added to the residue, and the mixture was washed by stirring for 10 minutes in a vacuum planetary centrifugal mixer (25°C, 1,000 rpm). The mixture was then centrifuged and the supernatant was removed. This procedure was repeated four times. Furthermore, the ethanol was replaced with diethylene glycol, and the same procedure of washing, centrifugation, and removal of the supernatant was repeated twice to obtain a cake of oxide-containing copper particles.

[0055] Examples 2 to 4, Comparative Examples 1 and 2 Using the raw material components shown in Table 1, the same operation as in Example 1 was carried out to obtain cakes of oxide-containing copper particles.

[0056] [Measurement and Evaluation of Oxide-Containing Copper Particles] The oxide-containing copper particles (cakes) produced in the Examples and Comparative Examples were subjected to the following measurement and evaluation. The evaluation results are shown in Table 1.

[0057] (X-ray Diffraction (XRD) Measurement) A cake of oxide-containing copper particles was applied to a glass plate to a thickness of 200 μm, and XRD measurement was performed using an X-ray diffractometer ("SmartLab SE", manufactured by Rigaku Corporation; CuKα radiation, focusing method). The obtained XRD pattern was fitted using a split pseudo-Voigt function.

[0058] <Cu 64 O and Cu 2 By XRD pattern analysis, it was found that Cu, Cu 64 O and Cu 2 Cu relative to 100% by mass of the total of O 64 O and Cu 2 The content of each of the O components was determined by the reference intensity ratio (RIR) method. Specifically, the strongest lines of each component (Cu(111), Cu 64 O(044) and Cu 2For Cu(111), the integrated intensity after subtracting the background intensity and each RIR value (Cu: 8.86, Cu 64 O: 4.89, Cu 2 The content of each component was calculated using the JIS K 02000:8.28.

[0059] <Cu (111) Crystallite Diameter> The half width (full width at half maximum: FWHM) of the Cu (111) peak in the XRD pattern was calculated from β and the Bragg angle θ (1 / 2 of the diffraction angle 2θ) by the Scherrer formula below to calculate the crystallite diameter C of Cu (111). C = K · λ / (β · cos θ) where the Scherrer constant: K = 0.94, and the characteristic X-ray wavelength of CuKα rays: λ = 0.15418 [nm]. XRD measurement was also performed in the same manner on a sample obtained by heating a cake of oxide-containing copper particles coated on a glass plate at 200 ° C. for 1 hour under a nitrogen atmosphere, to determine the crystallite diameter of Cu (111). Table 1 shows the crystallite diameter (C1) before heating (room temperature), the crystallite diameter (C2) after heating (200 ° C.), and the ratio C2 / C1 of the two.

[0060] (Scanning Electron Microscope (SEM) Observation) A cake of oxide-containing copper particles was applied to a brass sample stage with carbon tape attached, and dried at 90°C for 3 hours in a nitrogen atmosphere to prepare a sample. This sample was observed with an SEM (Schottky field emission scanning electron microscope "JSM-F100", manufactured by JEOL Ltd.; acceleration voltage 15 kV, magnification 100,000 times; the same applies hereinafter). The lengths of 200 particles in the SEM image were measured to determine the particle thickness and major axis. Table 1 shows the median values ​​for thickness and major axis. SEM images of the samples of Example 4 and Comparative Example 2 are shown in Figures 1 and 2, respectively, as representative examples.

[0061] [Evaluation of Characteristics of Sintered Body] The sintered bodies of the oxide-containing copper particles produced in the Examples and Comparative Examples were subjected to the following measurements and evaluations. The evaluation results are also shown in Table 1.

[0062] (Bonding Strength) The oxide-containing copper particles (cake) produced in the Examples and Comparative Examples were diluted with diethylene glycol to prepare a paste composition with a non-volatile content of 80% by mass. Using the prepared paste composition, a Ti / Pd / Au-plated aluminum nitride piece (3 mm x 3 mm, thickness 200 μm) was bonded to a Ni / Pd-plated copper substrate, and heated at 200 ° C. for 60 minutes in a nitrogen atmosphere (containing 3% by volume of hydrogen) to sinter the copper particles to prepare a bonded test piece (a test piece without a sealing resin). The die shear strength (bonding strength) of the bonded test piece was measured using a bond strength tester ("4000Plus Bond Tester", manufactured by Nordon DAGE; room temperature (25 ° C.), a distance from the substrate to the load jig of 0.15 mm, and a load speed of 30 mm / min).

[0063] (Density) After embedding the test piece without sealing resin in epoxy resin, the sample was cut in the thickness direction and observed under SEM. The area ratio of the sintered body portion in the binary image of the cross section of the bonding layer was determined, and this was taken as the density.

[0064] (Cold-Heat Cycle Test) Using the paste composition, a Ti / Au-plated silicon chip (3 mm x 3 mm, 200 μm thick) was bonded to a Ni / Pd / Au-plated die pad (4 mm x 4 mm) of a QFP (Quad Flat Package) frame. The resulting mixture was heated at 200°C for 60 minutes in a nitrogen atmosphere (containing 3% by volume of hydrogen) to sinter the copper particles. This was then mold-sealed with an encapsulating epoxy resin ("KE-G3000D" manufactured by Kyocera Corporation) to prepare a bonded test specimen (a test specimen with encapsulating resin). A cold-heat cycle test (1 cycle: -40°C to 120°C / 30 minutes, 2000 cycles) was performed on the test specimens without encapsulating resin and with encapsulating resin. The rate of change in thermal resistance of the junction before and after the test was measured using a transient thermal resistance measurement device ("Simcenter T3Ster" manufactured by Siemens). The rate of change in this thermal resistance is shown in Table 1. The lower the rate of change, the higher the bonding reliability, and when it exceeded 10%, the bonding reliability was low and was evaluated as poor.

[0065]

[0066] Cu 64The content of O is Cu, Cu 2 O and Cu 64 The oxide-containing copper particles (Examples 1 to 4) in which the content of Cu in the oxide-containing copper particles is in the range of 2.1 to 25.0 mass% relative to the total of 100 mass% of O have a plate-like particle shape (see Figure 1). 64 Copper particles (Comparative Examples 1 and 2) with an O content outside the above range had a substantially spherical particle shape (see FIG. 2). Furthermore, the copper particles of Comparative Examples 1 and 2 had a Cu(111) crystallite diameter of over 30.0 nm in an unheated state (room temperature), which was larger than those of Examples 1 to 4, and showed little change before and after heating at 200°C. Therefore, it is presumed that the bonding layers formed using the paste compositions of Comparative Examples 1 and 2 had low density, did not achieve sufficient bonding strength, and had low bonding reliability. It was confirmed that the paste compositions of Examples 1 to 4 were capable of forming bonding layers with high density, high bonding strength, and high bonding reliability.

Claims

1. Cu, Cu 2 O and Cu 64 Contains O, Cu 64 The content of O is Cu, Cu 2 O and Cu 64 The copper oxide-containing plate-like copper particles are 2.1 to 25.0 mass% relative to 100 mass% of the total of O.

2. Cu 2 The content of O is Cu, Cu 2 O and Cu 64 The oxide-containing plate-like copper particles according to claim 1, wherein the oxide content is 5.0 mass% or less relative to 100 mass% of the total of O.

3. 2. The oxide-containing plate-like copper particles according to claim 1, wherein the ratio (C2 / C1) of the crystallite diameter (C2) of Cu (111) measured by X-ray diffraction after heating to the crystallite diameter (C1) of Cu (111) measured by X-ray diffraction before heating when heated at 200 ° C. in a nitrogen atmosphere is 2.0 or more.

4. The oxide-containing plate-like copper particles according to claim 3, wherein the crystallite size (C2) is 55.0 nm or more.

5. The oxide-containing plate-like copper particles according to claim 1, having a thickness of 5 to 50 nm and a major axis of 30 to 300 nm, the major axis being greater than the thickness.

6. A paste composition comprising the oxide-containing plate-like copper particles according to any one of claims 1 to 5.

7. A semiconductor device, at least a portion of which is bonded using the paste composition according to claim 6.

8. An electrical component, at least a portion of which is joined using the paste composition according to claim 6.

9. An electronic component, at least a portion of which is bonded using the paste composition according to claim 6.