Rubber composition, vulcanized molded body, and vulcanizate

JPWO2023210519A5Inactive Publication Date: 2024-11-19
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024517274
Authority / Receiving Office
JP · JP
Patent Type
Applications
Filing Date
2024-10-09
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Rubber compositions containing chloroprene rubber face challenges in achieving high levels of properties such as oil resistance, cold resistance, and bending fatigue resistance in vulcanized molded products, with existing combinations often deteriorating ozone resistance.

Method used

A rubber composition comprising chloroprene rubber, epichlorohydrin rubber, and a compound with a p-phenylenediamine structure, where specific mass ratios and types of unsaturated nitrile monomers are used to enhance processing safety and mechanical properties, including ozone resistance.

Benefits of technology

The composition yields vulcanizates and vulcanized molded products with excellent oil resistance, cold resistance, bending fatigue resistance, and ozone resistance, suitable for various industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2023210519000001
    Figure 2023210519000001
Patent Text Reader

Abstract

Provided are: a rubber composition from which it is possible to obtain a vulcanized molded body that has excellent processing safety, and excellent oil resistance, cold resistance, and flex fatigue resistance; and a vulcanizate and a vulcanized molded body which have excellent oil resistance, cold resistance, and flex fatigue resistance. The present invention provides a rubber composition that contains a chloroprene-based rubber and an epichlorohydrin-based rubber. When the amount of rubber contained in the rubber composition is defined as 100 parts by mass, the rubber composition contains 5-95 parts by mass of the chloroprene-based rubber, 5-95 parts by mass of the epichlorohydrin-based rubber, and 0.1-10 parts by mass of a compound having a p-phenylene diamine structure. The chloroprene-based rubber contains a chloroprene-based rubber having an unsaturated nitrile monomer unit content of less than 25 mass%.
Need to check novelty before this filing date? Find Prior Art

Description

Rubber composition, vulcanized molded product, and vulcanizate

[0001] The present invention relates to a rubber composition, a vulcanizate, and a vulcanized molded article.

[0002] Chloroprene rubber has various excellent properties, and by utilizing these properties, it is used in a wide range of fields such as automobile parts, adhesives, various industrial rubber parts, etc. As technologies using chloroprene rubber, the rubber compositions described in Patent Documents 1 to 3 listed below are known.

[0003] Furthermore, rubber compositions containing chloroprene-based rubber and rubbers other than chloroprene-based rubber have also been studied. For example, Patent Document 4 discloses a rubber composition containing (a1) epichlorohydrin rubber and (a2) chloroprene rubber. Furthermore, various chemicals are known that can be added to rubber compositions to improve the physical properties of vulcanizates and vulcanized molded articles obtained from the rubber compositions. For example, Non-Patent Document 1 discloses that a combination of epichlorohydrin-based rubber and a compound having a p-phenylenediamine structure ("Nocrac 6C" manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) deteriorates ozone resistance.

[0004] JP 2016-23191 A JP 2012-111899 A JP 9-268239 A JP 2015-44965 A

[0005] "NOC Technical Note No. 349: Effect of Antioxidants on Epichlorohydrin Rubber (2)," Journal of the Society of Rubber Science and Technology of Japan, Vol. 63, No. 1, pp. 61-62, 1990

[0006] For rubber compositions containing chloroprene-based rubber, it is sometimes required that a vulcanized molded article of the rubber composition achieves a high degree of compatibility between various properties. However, it has been difficult to obtain a rubber composition that can give a vulcanized molded article that is excellent in processing safety and has excellent oil resistance, cold resistance, and flex fatigue resistance.

[0007] The present invention has been made in view of the above circumstances, and provides a rubber composition that is excellent in processing safety and that can give a vulcanized molded article that is excellent in oil resistance, cold resistance, and flex fatigue resistance, as well as a vulcanizate and a vulcanized molded article that are excellent in oil resistance, cold resistance, and flex fatigue resistance.

[0008] According to the present invention, there is provided a rubber composition containing a chloroprene-based rubber and an epichlorohydrin-based rubber, wherein the rubber composition contains 5 to 95 parts by mass of the chloroprene-based rubber, 5 to 95 parts by mass of the epichlorohydrin-based rubber, and 0.1 to 10 parts by mass of a compound having a p-phenylenediamine structure, relative to 100 parts by mass of the rubber contained in the rubber composition, and the chloroprene-based rubber contains a chloroprene-based rubber having an unsaturated nitrile monomer unit content of less than 25% by mass.

[0009] The present inventors have conducted extensive research and have found that, although it has been known that a combination of an epichlorohydrin rubber and a compound having a p-phenylenediamine structure deteriorates ozone resistance and the like, by adjusting the contents of the chloroprene rubber, epichlorohydrin rubber, and compound having a p-phenylenediamine structure in a rubber composition containing a chloroprene rubber and an epichlorohydrin rubber to fall within specific numerical ranges, a rubber composition can be obtained that is excellent in processing safety and that can give vulcanizates and vulcanized molded articles that are excellent in oil resistance, cold resistance, and flex fatigue resistance, leading to the completion of the present invention.

[0010] Various embodiments of the present invention are exemplified below. The embodiments shown below can be combined with each other. [1] A rubber composition containing a chloroprene-based rubber and an epichlorohydrin-based rubber, wherein the rubber composition contains 5 to 95 parts by mass of the chloroprene-based rubber, 5 to 95 parts by mass of the epichlorohydrin-based rubber, and 0.1 to 10 parts by mass of a compound having a p-phenylenediamine structure, based on 100 parts by mass of the rubber contained in the rubber composition, and the chloroprene-based rubber contains a chloroprene-based rubber having an unsaturated nitrile monomer unit content of less than 25% by mass. [2] The rubber composition according to [1], wherein the compound having a p-phenylenediamine structure is represented by the following formula (1):

[0011]

[0012] (In formula (1), R 1 and R 2represents an organic group, and R 1 and R 2At least one of the compounds having a p-phenylenediamine structure contains at least one compound selected from the group consisting of N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine, N-phenyl-N'-isopropyl-p-phenylenediamine, N-1-methylheptyl-N'-phenyl-p-phenylenediamine, N-phenyl-N'-(3-methacryloyloxy-2-hydroxypropyl)-p-phenylenediamine, N,N'-di-2-naphthyl-p-phenylenediamine, N,N'-diphenyl-p-phenylenediamine, p-(p-toluenesulfonylamido)diphenylamine, and N-cyclohexyl-N'-phenyl-p-phenylenediamine. [4] The rubber composition according to any one of [1] to [3], wherein the unsaturated nitrile monomer unit is an acrylonitrile monomer unit. [5] The rubber composition according to any one of [1] to [4], wherein the chloroprene-based rubber includes: Rubber A, which is a chloroprene-based rubber having 1 to 20 mass% unsaturated nitrile monomer units, 60 to 99 mass% chloroprene monomer units, and 0 to 20 mass% of monomer units other than chloroprene monomers and unsaturated nitrile monomers; and Rubber B, which is a chloroprene-based rubber having 80 to 100 mass% chloroprene monomer units and 0 to 20 mass% of monomer units other than chloroprene monomers and unsaturated nitrile monomers. [6] The rubber composition according to any one of [1] to [5], wherein, when the chloroprene-based rubber contained in the rubber composition is taken as 100 mass%, the rubber composition contains 20 to 99 mass% of Rubber A and 1 to 80 mass% of Rubber B. [7] The rubber composition according to any one of [1] to [6], wherein the epichlorohydrin-based rubber contains 5 to 90 mol% ethylene oxide monomer units. [8] The rubber composition according to any one of [1] to [7], wherein the rubber composition contains 0.1 to 20 parts by mass of an acid acceptor when the rubber contained in the rubber composition is taken as 100 parts by mass, and the acid acceptor includes at least one selected from the group consisting of hydrotalcite compounds, zinc oxide, magnesium-aluminum solid solutions, magnesium oxide, lead oxide, trimlead tetroxide, iron trioxide, titanium dioxide, and calcium oxide.[9] The rubber composition according to any one of [1] to [8], which contains at least one compound selected from the group consisting of sulfur, trimethylthiourea, ethylenethiourea, diphenylthiourea, diethylthiourea, dibutylthiourea, 1,3-trimethylene-2-thiourea, and 3-methylthiazolidine-2-thione.

[10] The rubber composition according to any one of [1] to [9], which contains at least one compound selected from the group consisting of 2-mercaptobenzimidazole, 2-mercaptomethylbenzimidazole, and a zinc salt of 2-mercaptobenzimidazole.

[11] A vulcanizate of the rubber composition according to any one of [1] to

[10] .

[12] A vulcanized molded article using the vulcanizate according to

[11] .

[0013] The rubber composition according to the present invention has excellent processing safety, and can provide vulcanizates and vulcanized molded articles that are excellent in oil resistance, cold resistance, and flex fatigue resistance. Furthermore, the obtained vulcanizates and vulcanized molded articles can be used to their full potential as various components that require oil resistance, cold resistance, flex fatigue resistance, and the like. Specifically, the vulcanizates and vulcanized molded articles according to one embodiment of the present invention can be suitably used as industrial parts such as accumulators, boots, hoses, belts, vibration-isolating rubber, vibration-damping materials, electric wires, gaskets, oil seals, packings, diaphragms, and sponges, and can be particularly used as components for accumulators, diaphragms, and hoses. The vulcanizates and vulcanized molded articles according to one embodiment of the present invention can be particularly used as components used in environments that require oil resistance, cold resistance, and / or flex fatigue resistance.

[0014] The present invention will be described in detail below by illustrating embodiments of the present invention. The present invention is not limited by these descriptions. The features of the embodiments of the present invention described below can be combined with each other. Furthermore, each feature can be an invention independently.

[0015] 1. Rubber Composition The rubber composition according to the present invention contains, per 100 parts by mass of rubber contained in the rubber composition, 5 to 95 parts by mass of a chloroprene-based rubber, 5 to 95 parts by mass of an epichlorohydrin-based rubber, and 0.1 to 10 parts by mass of a compound having a p-phenylenediamine structure. According to the present invention, by setting the amounts of the chloroprene-based rubber, the epichlorohydrin-based rubber, and the compound having a p-phenylenediamine structure contained in the rubber composition within specific numerical ranges and specifying that the chloroprene-based rubber contains a specific type of chloroprene-based rubber, it is possible to obtain a vulcanizate and a vulcanized molded article that have excellent processing safety and excellent oil resistance, cold resistance, and flex fatigue resistance. Furthermore, the rubber composition according to one embodiment of the present invention can also produce a vulcanizate and a vulcanized molded article that have excellent processability and processing safety, and excellent oil resistance, cold resistance, ozone resistance, flex fatigue resistance, and compression set resistance.

[0016] 1.1 Chloroprene-Based Rubber The chloroprene-based rubber according to the present invention refers to a rubber containing a chloroprene-based polymer having chloroprene (2-chloro-1,3-butadiene) as a monomer unit (monomer unit = structural unit). Examples of the chloroprene-based polymer include a chloroprene homopolymer and a chloroprene copolymer (a copolymer of chloroprene and a monomer copolymerizable with chloroprene). The polymer structure of the chloroprene-based polymer is not particularly limited.

[0017] Commercially available 2-chloro-1,3-butadiene may contain a small amount of 1-chloro-1,3-butadiene as an impurity. 2-chloro-1,3-butadiene containing such a small amount of 1-chloro-1,3-butadiene can also be used as the chloroprene monomer according to one embodiment of the present invention.

[0018] The rubber composition according to the present invention may contain one or more types of chloroprene-based rubber. The chloroprene-based rubber according to one embodiment of the present invention includes a chloroprene-based rubber having an unsaturated nitrile monomer unit content of less than 25% by mass. The unsaturated nitrile monomer unit content may be, for example, 0, 0.1, 0.2, 0.5, 1, 2, 5, 10, 15, 20, 24% by mass, or less than 25% by mass, and may be within a range between any two of the values ​​exemplified herein. By including the unsaturated nitrile monomer unit in the chloroprene-based rubber according to one embodiment of the present invention, the resulting vulcanizate and vulcanized molded article have more sufficient oil resistance. Furthermore, by setting the content of the unsaturated nitrile monomer unit to the above-mentioned lower limit or less, the resulting vulcanizate and vulcanized molded article have more sufficient cold resistance.

[0019] When the rubber composition according to one embodiment of the present invention contains two or more types of chloroprene-based rubbers, the total content of unsaturated nitrile monomer units contained in the two or more chloroprene-based rubbers is preferably less than 25% by mass relative to the total of 100% by mass of the two or more chloroprene-based rubbers contained in the rubber composition. The content of unsaturated nitrile monomer units in the chloroprene-based rubber according to one embodiment of the present invention may be, for example, 0, 0.1, 0.2, 0.5, 1, 2, 5, 10, 15, 20, 24% by mass, or less than 25% by mass, and may be within a range between any two of the numerical values ​​exemplified here.

[0020] Examples of the unsaturated nitrile monomer unit according to one embodiment of the present invention include an acrylonitrile monomer unit, a methacrylonitrile monomer unit, an ethacrylonitrile monomer unit, and a phenylacrylonitrile monomer unit. The chloroprene rubber according to one embodiment of the present invention may contain one or more types of unsaturated nitrile monomer units. From the viewpoint of obtaining excellent moldability and obtaining excellent mechanical properties and oil resistance in a vulcanized molded product, the unsaturated nitrile monomer unit preferably contains an acrylonitrile monomer unit, and more preferably is an acrylonitrile monomer unit.

[0021] The content of unsaturated nitrile monomer units contained in chloroprene-based rubber can be calculated from the content of nitrogen atoms in the chloroprene-based rubber. Specifically, the content of nitrogen atoms in 100 mg of chloroprene-based rubber can be measured using an elemental analyzer (Sumigraph 220F, manufactured by Sumika Chemical Analysis Center Co., Ltd.), and the content of structures derived from unsaturated nitrile monomers can be calculated. Elemental analysis can be performed under the following conditions. For example, the electric furnace temperatures are set to 900°C for the reactor, 600°C for the reduction furnace, 70°C for the column, and 100°C for the detector, and oxygen is flowed at 0.2 mL / min as the combustion gas and 80 mL / min as the carrier gas. A calibration curve can be created using aspartic acid (10.52%), which has a known nitrogen content, as a standard substance.

[0022] The chloroprene-based rubber according to one embodiment of the present invention preferably contains 60 to 100% by mass of chloroprene monomer units, relative to 100% by mass of the chloroprene-based rubber contained in the rubber composition. The chloroprene monomer unit content in the chloroprene-based rubber may be, for example, 60, 65, 70, 75, 80, 85, 90, 95, 99, or 100% by mass, or may be within a range between any two of the values ​​exemplified here. By ensuring that the chloroprene monomer unit content falls within the above-mentioned range, a rubber composition can be obtained that can produce vulcanizates and vulcanized molded articles with an excellent balance between mechanical properties and cold resistance. As described above, the rubber composition according to one embodiment of the present invention may contain two or more types of chloroprene-based rubber. When the rubber composition contains two or more types of chloroprene-based rubber, the total content of the chloroprene monomer units contained in the two or more types of chloroprene-based rubbers, relative to 100% by mass of the total of the two or more types of chloroprene-based rubbers contained in the rubber composition, is preferably within the above-mentioned range.

[0023] The chloroprene-based rubber according to one embodiment of the present invention may also have a monomer unit other than the chloroprene monomer and the unsaturated nitrile monomer. The monomer unit other than the chloroprene monomer and the unsaturated nitrile monomer is not particularly limited as long as it is copolymerizable with the chloroprene monomer or the chloroprene monomer and the unsaturated nitrile monomer, and examples thereof include (meth)acrylic acid esters (methyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, etc.), hydroxyalkyl (meth)acrylates (2-hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, etc.), 2,3-dichloro-1,3-butadiene, 1-chloro-1,3-butadiene, butadiene, isoprene, ethylene, styrene, sulfur, etc.

[0024] A chloroprene-based rubber according to one embodiment of the present invention may contain 0 to 20 mass% of monomer units other than chloroprene monomer and unsaturated nitrile monomer, based on 100 mass% of the chloroprene-based rubber. The content of monomer units other than chloroprene monomer and unsaturated nitrile monomer in the chloroprene-based rubber may be, for example, 0, 2, 4, 6, 8, 10, 12, 14, 16, 18, or 20 mass%, and may be within a range between any two of the values ​​exemplified here. By adjusting the copolymerization amount of monomers other than chloroprene monomer and unsaturated nitrile monomer within this range, the effects of copolymerizing these monomers can be achieved without impairing the properties of the resulting rubber composition. Furthermore, a chloroprene-based rubber according to one embodiment of the present invention may be composed solely of chloroprene monomer units and unsaturated nitrile monomer units. As described above, the rubber composition according to one embodiment of the present invention may contain two or more types of chloroprene-based rubber. When the rubber composition contains two or more types of chloroprene-based rubber, it is preferable that the total content of monomer units other than the chloroprene monomer and the unsaturated nitrile monomer contained in the two or more types of chloroprene-based rubbers be within the above-mentioned numerical range relative to 100% by mass of the total of the two or more types of chloroprene-based rubbers contained in the rubber composition.

[0025] The chloroprene polymer contained in the chloroprene rubber according to the present invention may be a sulfur-modified chloroprene polymer, a mercaptan-modified chloroprene polymer, a xanthogen-modified chloroprene polymer, a dithiocarbonate-based chloroprene polymer, a trithiocarbonate-based chloroprene polymer, a carbamate-based chloroprene polymer, or the like.

[0026] The chloroprene-based rubber according to one embodiment of the present invention preferably includes a rubber A containing 1 to 20% by mass of unsaturated nitrile monomer units. The rubber A may contain, for example, 1, 2, 4, 6, 8, 10, 12, 14, 16, 18, or 20% by mass of unsaturated nitrile monomer units, and may be within a range between any two of the values ​​exemplified here.

[0027] Rubber A according to one embodiment of the present invention preferably contains 60 to 99% by mass of chloroprene monomer units when Rubber A is taken as 100% by mass. The content of chloroprene monomer units in Rubber A is, for example, 60, 65, 70, 75, 80, 85, 90, 95, or 99% by mass, and may be within a range between any two of the numerical values ​​exemplified here.

[0028] Rubber A according to one embodiment of the present invention may contain 0 to 20% by mass of monomer units other than chloroprene monomers and unsaturated nitrile monomers when Rubber A is taken as 100% by mass. The content of monomer units other than chloroprene monomers and unsaturated nitrile monomers in Rubber A is, for example, 0, 2, 4, 6, 8, 10, 12, 14, 16, 18, or 20% by mass, and may be within a range between any two of the values ​​exemplified here.

[0029] Rubber A according to one embodiment of the present invention may contain 1 to 20% by mass of unsaturated nitrile monomer units, 60 to 99% by mass of chloroprene monomer units, and 0 to 20% by mass of other copolymerizable monomer units other than chloroprene monomers and unsaturated nitrile monomers. Alternatively, Rubber A according to one embodiment of the present invention may consist only of chloroprene monomer units and unsaturated nitrile monomer units.

[0030] The chloroprene-based rubber according to one embodiment of the present invention may also contain a chloroprene-based rubber other than the above-described rubber A. That is, the chloroprene-based rubber according to one embodiment of the present invention may contain only rubber A, or may contain rubber A and one or more types of rubber different from rubber A.

[0031] A chloroprene-based rubber according to one embodiment of the present invention may include Rubber B, which is a chloroprene-based rubber different from Rubber A. Rubber B may be a chloroprene-based rubber having a higher content of chloroprene monomer units than Rubber A. Rubber B preferably contains 80 to 100% by mass of chloroprene monomer units when Rubber B is taken as 100% by mass. The content of chloroprene monomer units in Rubber B may be, for example, 80, 85, 90, 95, or 100% by mass, and may be within a range between any two of the values ​​exemplified here.

[0032] Rubber B according to one embodiment of the present invention may contain 0 to 20% by mass of monomer units other than chloroprene monomers and unsaturated nitrile monomers when Rubber B is taken as 100% by mass. The content of monomer units other than chloroprene monomers and unsaturated nitrile monomers in Rubber B is, for example, 0, 2, 4, 6, 8, 10, 12, 14, 16, 18, or 20% by mass, and may be within a range between any two of the numerical values ​​exemplified here.

[0033] The content of unsaturated nitrile monomer units in Rubber B according to one embodiment of the present invention may be lower than the content of unsaturated nitrile monomer units in Rubber A. The content of unsaturated nitrile monomer units in Rubber B according to one embodiment of the present invention may be less than 1% by mass. Furthermore, Rubber B according to one embodiment of the present invention may not contain any unsaturated nitrile monomer units. Rubber B according to one embodiment of the present invention may have 80 to 100% by mass of chloroprene monomer units and 0 to 20% by mass of monomer units other than chloroprene monomers and unsaturated nitrile monomers. Rubber B according to one embodiment of the present invention may also be composed only of chloroprene monomer units and monomer units other than chloroprene monomers and unsaturated nitrile monomers. Furthermore, Rubber B according to one embodiment of the present invention may also be composed only of chloroprene monomer units. Rubber B according to one embodiment of the present invention may also be a mercaptan-modified chloroprene-based rubber. The chloroprene-based rubber according to one embodiment of the present invention may contain only Rubber B, or may contain Rubber B and one or more rubbers different from Rubber B.

[0034] The chloroprene-based rubber according to one embodiment of the present invention may include: Rubber A, which is a chloroprene-based rubber having 1 to 20% by mass of unsaturated nitrile monomer units, 60 to 99% by mass of chloroprene monomer units, and 0 to 20% by mass of monomer units other than chloroprene monomers and unsaturated nitrile monomers; and Rubber B, which is a chloroprene-based rubber having 80 to 100% by mass of chloroprene monomer units and 0 to 20% by mass of monomer units other than chloroprene monomers and unsaturated nitrile monomers.

[0035] A rubber composition according to one embodiment of the present invention preferably contains 20 to 99% by mass of rubber A when the chloroprene rubber contained in the rubber composition is taken as 100% by mass. The content of rubber A in the chloroprene rubber can be, for example, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, or 99% by mass when the chloroprene rubber is taken as 100% by mass, and may be within a range between any two of the numerical values ​​exemplified here. A chloroprene rubber according to one embodiment of the present invention preferably contains 1 to 80% by mass of rubber B when the chloroprene rubber contained in the rubber composition is taken as 100% by mass. The chloroprene rubber may have a content of Rubber B of, for example, 1, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, or 80% by mass, relative to 100% by mass of the chloroprene rubber, and may be within a range between any two of the values ​​exemplified here. A chloroprene rubber according to one embodiment of the present invention may contain 20 to 99% by mass of Rubber A and 1 to 80% by mass of Rubber B, relative to 100% by mass of the chloroprene rubber. By including Rubber B in addition to Rubber A, flexural fatigue resistance can be further improved.

[0036] 1.2 Method for Producing Chloroprene-Based Rubber The method for producing the chloroprene-based rubber according to the present invention is not particularly limited, but the rubber can be obtained by a production method including an emulsion polymerization step in which raw material monomers including a chloroprene monomer are emulsion-polymerized. In the emulsion polymerization step according to one embodiment of the present invention, raw material monomers including a chloroprene monomer or a chloroprene monomer and an unsaturated nitrile monomer are emulsion-polymerized using an emulsifier, a dispersant, a catalyst, a chain transfer agent, etc., as appropriate. When the target final conversion rate is reached, a polymerization terminator is added to obtain a latex containing a chloroprene-based polymer containing chloroprene monomer units. Next, unreacted monomers can be removed from the polymerization solution obtained by the emulsion polymerization step. The method for this removal is not particularly limited, and examples include steam stripping. Thereafter, the pH is adjusted, and the resulting mixture is subjected to conventional processes such as freeze coagulation, water washing, and hot air drying, thereby obtaining a chloroprene-based rubber containing a chloroprene-based polymer.

[0037] The polymerization initiator used in emulsion polymerization is not particularly limited, and any known polymerization initiator generally used in emulsion polymerization of chloroprene can be used. Examples of the polymerization initiator include potassium persulfate, ammonium persulfate, sodium persulfate, hydrogen peroxide, and organic peroxides such as t-butyl hydroperoxide.

[0038] The emulsifier used in emulsion polymerization is not particularly limited, and any known emulsifier generally used in emulsion polymerization of chloroprene can be used. Examples of the emulsifier include alkali metal salts of saturated or unsaturated fatty acids having 6 to 22 carbon atoms, alkali metal salts of rosin acid or disproportionated rosin acid (e.g., potassium rosinate), and alkali metal salts of formalin condensates of β-naphthalenesulfonic acid (e.g., sodium salt).

[0039] The molecular weight modifier used in emulsion polymerization is not particularly limited, and any known molecular weight modifier commonly used in emulsion polymerization of chloroprene can be used, such as mercaptan compounds, xanthogen compounds, dithiocarbonate compounds, trithiocarbonate compounds, and carbamate compounds. Xanthogen compounds, dithiocarbonate compounds, trithiocarbonate compounds, and carbamate compounds are preferably used as molecular weight modifiers for the chloroprene rubber according to one embodiment of the present invention.

[0040] The polymerization temperature and the final conversion rate of the monomer are not particularly limited, but the polymerization temperature may be, for example, 0 to 50°C or 10 to 50°C. The polymerization may be carried out so that the final conversion rate of the monomer falls within the range of 40 to 95% by mass. In order to adjust the final conversion rate, a polymerization terminator that terminates the polymerization reaction may be added to terminate the polymerization when the desired conversion rate is reached.

[0041] The polymerization terminator is not particularly limited, and any known polymerization terminator generally used in emulsion polymerization of chloroprene can be used, such as phenothiazine (thiodiphenylamine), 4-t-butylcatechol, and 2,2-methylenebis-4-methyl-6-t-butylphenol.

[0042] The chloroprene rubber according to one embodiment of the present invention can be obtained, for example, by removing unreacted monomers by a steam stripping method, adjusting the pH of the latex, and then performing conventional steps such as freeze coagulation, water washing, and hot air drying.

[0043] Chloroprene rubbers are classified into mercaptan-modified, xanthogen-modified, sulfur-modified, dithiocarbonate-based, trithiocarbonate-based and carbamate-based types depending on the type of molecular weight modifier.

[0044] 1.3 Epichlorohydrin-Based Rubber The rubber composition according to the present invention contains 5 to 95 parts by mass of an epichlorohydrin-based rubber. The epichlorohydrin-based rubber according to the present invention refers to a rubber containing a polymer having epichlorohydrin as a monomer unit. The epichlorohydrin-based rubber may contain a homopolymer of epichlorohydrin, or may contain a copolymer of epichlorohydrin monomer with one or more other monomers. Examples of the copolymer include an epichlorohydrin-ethylene oxide copolymer, an epichlorohydrin-propylene oxide copolymer, an epichlorohydrin-ethylene oxide-allyl glycidyl ether terpolymer, and an epichlorohydrin-ethylene oxide-propylene oxide-allyl glycidyl ether tetrapolymer. The epichlorohydrin-based rubber according to one embodiment of the present invention preferably contains an epichlorohydrin-ethylene oxide-allyl glycidyl ether terpolymer and / or an epichlorohydrin-ethylene oxide copolymer. The epichlorohydrin-based rubber may contain one or more rubbers having different types and / or contents of monomer units.

[0045] The epichlorohydrin-based rubber according to one embodiment of the present invention preferably contains ethylene oxide monomer units. The epichlorohydrin-based rubber according to one embodiment of the present invention preferably contains 5 to 90 mol% of ethylene oxide monomer units. The ethylene oxide monomer unit content in the epichlorohydrin-based rubber is, for example, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, or 90 mol%, and may be within a range between any two of the values ​​exemplified here. By setting the type and amount of the monomer units contained in the epichlorohydrin-based rubber within the above-mentioned ranges, a rubber composition can be obtained that can produce vulcanized molded products with better cold resistance and flex fatigue resistance.

[0046] The rubber composition according to the present invention may have, when the rubber contained in the rubber composition is taken as 100 parts by mass, the content of the chloroprene-based rubber is, for example, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, or 95 parts by mass, or may be within a range between any two of the numerical values ​​exemplified herein. Furthermore, the rubber composition according to the present invention may have, when the rubber contained in the rubber composition is taken as 100 parts by mass, the content of the epichlorohydrin-based rubber is, for example, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, or 95 parts by mass, or may be within a range between any two of the numerical values ​​exemplified herein.

[0047] The rubber composition according to one embodiment of the present invention may also contain rubbers other than chloroprene-based rubbers and epichlorohydrin-based rubbers. The rubber composition according to one embodiment of the present invention preferably contains 70 parts by mass or more, more preferably 80 parts by mass or more, and even more preferably 90 parts by mass or more of the chloroprene-based rubber and epichlorohydrin-based rubber in total, based on 100 parts by mass of the rubber contained in the rubber composition. The rubber composition according to one embodiment of the present invention may not contain any rubber other than the chloroprene-based rubber and epichlorohydrin-based rubber. By containing specific types of chloroprene-based rubber and specific amounts of epichlorohydrin-based rubber, the rubber composition according to the present invention becomes a rubber composition that is excellent in processability and processing safety, and that can give vulcanizates and vulcanized molded articles that are excellent in oil resistance, cold resistance, ozone resistance, flex fatigue resistance, and compression set resistance.

[0048] 1.4 Compound Having a p-Phenylenediamine Structure The rubber composition according to the present invention contains a compound having a p-phenylenediamine structure. The compound having a p-phenylenediamine structure is preferably represented by the following formula (1):

[0049]

[0050] In formula (1), R 1 and R 2 represents an organic group. 1 and R 2 At least one of R contains an aromatic ring structure. 1 and R 2 may contain an aromatic ring structure, and R 1 or R 2 It is preferable that either one of the above contains an aromatic ring structure.

[0051] The aromatic ring structure may be an aryl group which may have a substituent. Examples of the aryl group include a phenyl group, a 1-naphthyl group, a 2-naphthyl group, a 2-biphenyl group, a 3-biphenyl group, and a 4-biphenyl group. The aryl group is preferably a phenyl group or a naphthyl group, and more preferably a phenyl group.

[0052] In formula (1), R 1 or R 2 When either of R contains an aromatic ring structure, the other structure is not particularly limited, but can be an organic group having 1 to 10 carbon atoms, and the number of carbon atoms may be, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10, or may be within a range between any two of the numerical values ​​exemplified here. 1 or R 2 When either one of them contains an aromatic ring structure, the other is preferably an alkyl group having 1 to 10 carbon atoms, more preferably an alkyl group having 3 to 10 carbon atoms. The alkyl group may be a branched or linear alkyl group, and is more preferably a branched alkyl group.

[0053] Compounds having a p-phenylenediamine structure include N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine, N-phenyl-N'-isopropyl-p-phenylenediamine, N-1-methylheptyl-N'-phenyl-p-phenylenediamine, N-phenyl-N'-(3-methacryloyloxy-2-hydroxypropyl)-p-phenylenediamine, N,N'-di-2-naphthyl-p-phenylenediamine, N,N'-diphenyl-p-phenylenediamine, p-(p-toluenesulfonylamido)diphenylamine, N-cyclohexyl-N' ... It is preferable that the curable composition contains at least one compound selected from the group consisting of N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine, N-phenyl-N'-isopropyl-p-phenylenediamine, N-1-methylheptyl-N'-phenyl-p-phenylenediamine, N-phenyl-N'-(3-methacryloyloxy-2-hydroxypropyl)-p-phenylenediamine, and more preferable that the curable composition contains at least one compound selected from the group consisting of N-cyclohexyl-N'-phenyl-p-phenylenediamine.

[0054] The rubber composition according to the present invention contains, relative to 100 parts by mass of the rubber contained in the rubber composition, 5 to 95 parts by mass of a chloroprene-based rubber, 5 to 95 parts by mass of an epichlorohydrin-based rubber, and 0.1 to 10 parts by mass of a compound having a p-phenylenediamine structure. The content of the compound having a p-phenylenediamine structure is, for example, 0.1, 0.2, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 parts by mass, and may be within a range between any two of the values ​​exemplified here.

[0055] The rubber composition according to the present invention contains specific amounts of a chloroprene rubber, an epichlorohydrin rubber, and a compound having a p-phenylenediamine structure, and is therefore a rubber composition that can provide vulcanizates and vulcanized molded articles that are excellent in processability and processing safety and that are excellent in oil resistance, cold resistance, ozone resistance, flex fatigue resistance, and compression set resistance. Although it has been known that the combination of an epichlorohydrin rubber and a compound having a p-phenylenediamine structure deteriorates ozone resistance, etc., the reason why a rubber composition that provides vulcanizates and vulcanized molded articles that are excellent in processability and processing safety and that are excellent in oil resistance, cold resistance, ozone resistance, flex fatigue resistance, and compression set resistance by setting the contents of the chloroprene rubber, the epichlorohydrin rubber, and the compound having a p-phenylenediamine structure within specific numerical ranges is not necessarily clear, but is presumed to be as follows. That is, when a vulcanizate made of a rubber composition containing a chloroprene-based rubber and an epichlorohydrin-based rubber is exposed to ozone, it is thought that the chloroprene-based rubber in the vulcanizate is particularly susceptible to degradation and is highly likely to become the starting point of breakdown such as cracks. When a compound having a p-phenylenediamine structure is added to a rubber composition containing a chloroprene-based rubber and an epichlorohydrin-based rubber, the ozone resistance of the epichlorohydrin-based rubber may deteriorate, but the ozone resistance of the chloroprene-based rubber, which may become the starting point of breakdown, is improved, and since the latter has a significantly greater effect on the ozone resistance of the entire vulcanizate, it is presumed that the ozone resistance of the entire vulcanizate containing the two types of rubber is dramatically improved.

[0056] 1.5 Antiaging Agent The rubber composition according to one embodiment of the present invention may further contain an antioxidant in addition to the chloroprene rubber, epichlorohydrin rubber, and compound having a p-phenylenediamine structure. Examples of the antioxidant include aromatic secondary amine compounds (excluding compounds having a p-phenylenediamine structure), dithiocarbamate compounds, phenolic compounds, waxes, phosphorus-based antioxidants, and sulfur-based antioxidants. The rubber composition according to one embodiment of the present invention may contain one or more antioxidants.

[0057] The rubber composition according to one embodiment of the present invention may further contain an aromatic secondary amine compound other than the compound having a p-phenylenediamine structure. Examples of the aromatic secondary amine compound include 4,4'-bis(α,α-dimethylbenzyl)diphenylamine, N-phenyl-1-naphthylamine, and alkylated diphenylamine.

[0058] A rubber composition according to one embodiment of the present invention may contain 0 to 4.0 parts by mass, preferably 0.1 to 3 parts by mass, of an aromatic secondary amine compound other than a compound having a p-phenylenediamine structure, based on 100 parts by mass of rubber contained in the rubber composition. The content of the aromatic secondary amine compound other than a compound having a p-phenylenediamine structure may be, for example, 0, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, or 4.0 parts by mass, and may be within a range between any two of the values ​​exemplified herein. By containing the aromatic secondary amine compound within the above numerical range, the flex fatigue resistance, heat resistance, and compression set resistance of the resulting vulcanizate and vulcanized molded article can be further improved. A rubber composition according to one embodiment of the present invention may be free of aromatic secondary amine compounds other than a compound having a p-phenylenediamine structure.

[0059] The rubber composition according to an embodiment of the present invention may contain a dithiocarbamate compound, such as nickel dibutyldithiocarbamate.

[0060] A rubber composition according to one embodiment of the present invention may contain 0 to 3.0 parts by mass, preferably 0.1 to 2.0 parts by mass, of a dithiocarbamate compound, based on 100 parts by mass of rubber contained in the rubber composition. The content of the dithiocarbamate compound may be, for example, 0, 0.5, 1.0, 1.5, 2.0, 2.5, or 3.0 parts by mass, or may be within a range between any two of the values ​​exemplified herein. By containing the dithiocarbamate compound within the above numerical range, the ozone resistance and heat resistance of the resulting vulcanizate and vulcanized molded article can be further improved. Furthermore, by setting the content of the dithiocarbamate compound to the above upper limit or less, the occurrence of blooming can be suppressed. A rubber composition according to one embodiment of the present invention may not contain a dithiocarbamate compound.

[0061] The rubber composition according to one embodiment of the present invention may contain, for example, 0.1 to 10 parts by mass in total of the antioxidants listed above, based on 100 parts by mass of the rubber contained in the rubber composition.

[0062] 1.6 Acid Acceptor The rubber composition according to one embodiment of the present invention may contain an acid acceptor. The acid acceptor may include at least one selected from the group consisting of hydrotalcite compounds, magnesium-aluminum solid solutions, zinc oxide, magnesium oxide, lead oxide, trimlead tetroxide, iron trioxide, titanium dioxide, and calcium oxide, and may include at least one selected from the group consisting of hydrotalcite compounds, magnesium-aluminum solid solutions, zinc oxide, and magnesium oxide. The acid acceptor preferably includes zinc oxide. The acid acceptor preferably further includes at least one of hydrotalcite compounds and magnesium-aluminum solid solutions, and more preferably includes a hydrotalcite compound. The rubber composition according to one embodiment of the present invention may include one or more types of acid acceptors.

[0063] The hydrotalcite compound preferably has a chemical composition represented by the following formula: M x Al y (OH) z CO 3 ・mH2 O

[0064] In the above formula, M represents a divalent metal ion consisting of at least one of Mg and Zn, x represents a coefficient value ranging from 3 to 7, y represents a coefficient value ranging from 1 to 3, z represents a coefficient value ranging from 7 to 20, and m represents a coefficient value ranging from 2 to 7.

[0065] The hydrotalcite compound contains Mg 4.3 Al 2 (OH) 12.6 CO 3 ・3.5H 2 O, Mg 3 ZnAl 2 (OH) 12 CO 3 ・3H 2 O, Mg 4.5 Al 2 (OH) 13 CO 3 ・3.5H 2 O, Mg 4.5 Al 2 (OH) 13 CO 3 , Mg 4 Al 2 (OH) 12 CO 3 ・3.5H 2 O, Mg 6 Al 2 (OH) 16 CO 3 ・4H 2 O, Mg 5 Al 2 (OH) 14 CO 3 ・4H 2 O, Mg 3 Al 2 (OH) 10 CO 3 ・1.7H 2 It is preferable that the material contains at least one of Mg 4.3 Al 2 (OH) 12.6 CO 3 ・3.5H 2 O, Mg 3 ZnAl 2 (OH) 12 CO 3 ・3H 2 It is more preferable that at least one of O is contained.

[0066] The magnesium-aluminum solid solution preferably has a chemical composition represented by the following formula: (1-a) Al a O 3.83a

[0067] In the above formula, M represents a divalent metal ion consisting of at least one of Mg and Zn, and a represents a coefficient value ranging from 0.2 to 0.5. Magnesium-aluminum solid solutions are characterized by the presence of Mg 0.7 Al 0.3 O 1.15 It is preferred that the compound contains:

[0068] The acid acceptor preferably has a layered structure, and the thickness of each layer is preferably 5 Å or more, more preferably 10 Å or more. 4.3 Al 2 (OH) 12.6 CO 3 ・3.5H 2 O ("DHT-4A" manufactured by Kyowa Chemical Industry Co., Ltd.) has a layered structure, and each layer is 10 Å or more in thickness. It is presumed that a layer thickness of at least a certain level can inhibit the acid acceptor from crosslinking the epichlorohydrin rubber through complex formation, thereby inhibiting a decrease in the vulcanization rate and an increase in compression set in the resulting vulcanizate and vulcanized molded article.

[0069] The rubber composition according to the present invention may contain 0.1 to 20 parts by mass of an acid acceptor relative to 100 parts by mass of the rubber contained in the rubber composition. The content of the acid acceptor is, for example, 0.1, 0.2, 0.3, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20 parts by mass, and may be within a range between any two of the numerical values ​​exemplified here.

[0070] 1.7 Sulfur / Vulcanization Accelerator The rubber composition according to the present invention may contain a vulcanizing agent and a vulcanization accelerator, and may contain sulfur and a vulcanization accelerator. The type of vulcanization accelerator is not particularly limited as long as it does not impair the effects of the present invention. The vulcanization accelerator is preferably a vulcanization accelerator that can be used for vulcanizing chloroprene-based rubber and / or epichlorohydrin-based rubber. The rubber composition according to one embodiment of the present invention may contain one or more types of vulcanization accelerators.

[0071] The rubber composition according to one embodiment of the present invention may contain at least one compound selected from the group consisting of sulfur, thiourea-based compounds, thiuram-based compounds, thiazole-based compounds, sulfenamide-based compounds, dithiocarbamate-based compounds, guanidine-based compounds, xanthogenate-based compounds, imidazole-based compounds, and 3-methylthiazolidine-2-thione.

[0072] Examples of thiourea compounds include ethylene thiourea, diethyl thiourea (N,N'-diethyl thiourea), trimethyl thiourea, diphenyl thiourea (N,N'-diphenyl thiourea), 1,3-trimethylene-2-thiourea, etc. Examples of thiuram compounds include tetramethyl thiuram disulfide (TMTD), tetraethyl thiuram disulfide, tetrabutyl thiuram disulfide, tetrakis(2-ethylhexyl)thiuram disulfide, tetramethyl thiuram monosulfide, dipentamethylene thiuram tetrasulfide, etc. Examples of thiazole compounds include 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, 2-mercaptobenzothiazole zinc salt, 2-mercaptobenzothiazole cyclohexylamine salt, 2-(4'-morpholinodithio)benzothiazole, and N-cyclohexylbenzothiazole-2-sulfenamide. Examples of sulfenamide compounds include N-cyclohexylbenzothiazole-2-sulfenamide. Examples of dithiocarbamate compounds include sodium dibutyldithiocarbamate, zinc dimethyldithiocarbamate, zinc diethyldithiocarbamate, zinc N-ethyl-N-phenyldithiocarbamate, zinc N-pentamethylenedithiocarbamate, copper dimethyldithiocarbamate, ferric dimethyldithiocarbamate, and tellurium diethyldithiocarbamate. Examples of guanidine compounds include 1,3-diphenylguanidine, 1,3-di-o-tolylguanidine, 1-o-tolylbiguanide, and di-o-tolylguanidine salts of dicatechol borate. Examples of xanthate compounds include zinc butylxanthate and zinc isopropylxanthate. Examples of imidazole compounds include 2-mercaptobenzimidazole, 2-mercaptomethylbenzimidazole, and zinc salts of 2-mercaptobenzimidazole.

[0073] The rubber composition according to one embodiment of the present invention may contain at least one of sulfur, a thiourea-based compound, and 3-methylthiazolidine-2-thione, and preferably contains at least one compound selected from the group consisting of sulfur, trimethylthiourea, ethylenethiourea, diphenylthiourea, diethylthiourea, dibutylthiourea, 1,3-trimethylene-2-thiourea, and 3-methylthiazolidine-2-thione. The rubber composition according to one embodiment of the present invention may contain 10.0 parts by mass or less in total of sulfur, a thiourea-based compound, and 3-methylthiazolidine-2-thione, based on 100 parts by mass of rubber contained in the rubber composition. The total content of sulfur, thiourea compound, and 3-methylthiazolidine-2-thione is, for example, 0, 0.1, 0.3, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, 7.0, 8.0, 9.0, or 10.0 parts by mass, and may be within a range between any two of the numerical values ​​exemplified here.

[0074] The rubber composition according to one embodiment of the present invention may contain an imidazole-based compound, and preferably contains at least one compound selected from the group consisting of 2-mercaptobenzimidazole, 2-mercaptomethylbenzimidazole, and a zinc salt of 2-mercaptobenzimidazole. By containing the imidazole-based compound, the rubber composition according to one embodiment of the present invention can further improve the flex fatigue resistance of the resulting vulcanizate and vulcanized molded article. The rubber composition according to one embodiment of the present invention may contain 0 to 2.0 parts by mass, and preferably 0.1 to 1.5 parts by mass, of the imidazole-based compound in total, based on 100 parts by mass of rubber contained in the rubber composition. The content of the imidazole compound is, for example, 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, or 2.0, or may be within a range between any two of the values ​​exemplified here. By setting the content of the imidazole compound to be equal to or greater than the above-mentioned lower limit, the flex fatigue resistance of the vulcanizate and vulcanized molded article can be further improved. Furthermore, by setting the content of the imidazole compound to be equal to or less than the above-mentioned upper limit, it is possible to prevent a decrease in the processing safety of the rubber composition due to ionic crosslinking and a decrease in the compression set resistance of the vulcanizate and vulcanized molded article.

[0075] The rubber composition according to one embodiment of the present invention may contain 10.0 parts by mass or less of sulfur and a vulcanization accelerator in total, relative to 100 parts by mass of rubber contained in the rubber composition. The content of sulfur and a vulcanization accelerator may be, for example, 0, 0.1, 0.3, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, 7.0, 8.0, 9.0, or 10.0 parts by mass, or may be within a range between any two of the values ​​exemplified here.

[0076] 1.8 Fillers and Reinforcing Materials The rubber composition according to one embodiment of the present invention may contain a filler and / or a reinforcing material. Examples of fillers and reinforcing materials include furnace carbon black such as SAF, ISAF, HAF, EPC, XCF, FEF, GPF, HMF, and SRF; modified carbon black such as hydrophilic carbon black; thermal carbon such as channel black, lamp black, FT, and MT; acetylene black, ketjen black, silica, clay, talc, and calcium carbonate. The rubber composition according to one embodiment of the present invention may contain one or more fillers and / or reinforcing materials.

[0077] A rubber composition according to one embodiment of the present invention may contain a total of 20 to 90 parts by mass, and preferably 35 to 80 parts by mass, of filler and reinforcing material, based on 100 parts by mass of rubber contained in the rubber composition. The content of the filler and reinforcing material may be, for example, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, or 90 parts by mass, or may be within a range between any two of the values ​​exemplified here. By containing the filler and reinforcing material contents within the above numerical ranges, the rubber composition according to one embodiment of the present invention can improve the hardness of the vulcanizate and vulcanized molded article.

[0078] 1.9 Plasticizer and Softener The rubber composition according to one embodiment of the present invention may contain a plasticizer and / or a softener. The plasticizer and softener are added to adjust the processability of the unvulcanized rubber composition and the flexibility of the vulcanized product and vulcanized molded article after vulcanization. There are no particular restrictions on the plasticizer and softener, as long as they are compatible with rubber. Examples of plasticizers and softeners include vegetable oils such as rapeseed oil, linseed oil, castor oil, and palm oil, phthalate-based plasticizers, ester-based plasticizers such as DUP (diundecyl phthalate), DOP (dioctyl phthalate), DINP (diisononyl phthalate), DOTP (dioctyl terephthalate), DOS (dioctyl sebacate), DBS (dibutyl sebacate), DOA (dioctyl adipate), DINCH (diisononyl 1,2-cyclohexanedicarboxylate), TOP (trioctyl phosphate), and TBP (tributyl phosphate), ether ester-based compounds, thioether-based plasticizers, aromatic oils, naphthenic oils, lubricating oils, process oils, paraffin, liquid paraffin, Vaseline, and petroleum-based plasticizers such as petroleum asphalt. The rubber composition according to one embodiment of the present invention may contain one or more types of plasticizers and / or softeners.

[0079] A rubber composition according to one embodiment of the present invention may contain a total of 50 parts by mass or less of a plasticizer and a softener, based on 100 parts by mass of rubber contained in the rubber composition. The total content of the plasticizer and the softener may be, for example, 0, 1, 2, 3, 4, 5, 10, 15, 20, 25, 30, 35, 40, 45, or 50 parts by mass, or may be within a range between any two of the values ​​exemplified here. A rubber composition according to one embodiment of the present invention may also be free of a plasticizer and / or a softener.

[0080] 1.10 Lubricants and Processing Aids The rubber composition according to the present invention may further contain a lubricant and / or a processing aid. Lubricants and processing aids are added primarily to improve processability, such as by making it easier for the rubber composition to be released from rolls, molding dies, extruder screws, etc. Examples of lubricants and processing aids include fatty acids such as stearic acid, paraffin-based processing aids such as polyethylene, fatty acid amides, petrolatum, and factice. The rubber composition according to one embodiment of the present invention may contain one or more types of lubricants and / or processing aids.

[0081] The rubber composition according to the present invention may contain a total of 15 parts by mass or less of lubricant and processing aid, and may also contain 10 parts by mass or less, based on 100 parts by mass of rubber contained in the rubber composition. The total content of lubricant and processing aid may be, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or 15 parts by mass, or may be within a range between any two of the values ​​exemplified here. The rubber composition according to the present invention may also be free of lubricant and / or processing aid.

[0082] 1.11 Others In addition to the above-mentioned components, the rubber composition according to the present invention may further contain components such as a silane coupling agent, a co-crosslinking agent, a stabilizer, a flame retardant, and a vulcanization retarder, as long as the effects of the present invention are not impaired. An example of a vulcanization retarder is tetrabenzyl thiuram disulfide. The rubber composition according to one embodiment of the present invention may contain 0 to 5.0 parts by mass of a vulcanization retarder, based on 100 parts by mass of rubber contained in the rubber composition.

[0083] 2. Method for Producing Rubber Composition The rubber composition according to one embodiment of the present invention can be obtained by kneading a chloroprene rubber, an epichlorohydrin rubber, a compound having a p-phenylenediamine structure, and other necessary components at a temperature equal to or lower than the vulcanization temperature. Examples of devices for kneading the raw material components include conventionally known kneading devices such as a mixer, a Banbury mixer, a kneader mixer, and an open roll.

[0084] 3. Properties of Rubber Composition A rubber composition according to one embodiment of the present invention preferably has the following properties. (Processing Safety) When a Mooney scorch test is performed on a rubber composition according to JIS K 6300-1 using an L-type rotor at a test temperature of 125°C, and the scorch time is defined as the time required for the measured Mooney viscosity to increase by 5M, the rubber composition preferably has a scorch time of 4 minutes or more, more preferably 7 minutes or more, and even more preferably 10 minutes or more. The scorch time may be, for example, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20 minutes, and may be within a range between any two of the values ​​exemplified here.

[0085] (Processability) The rubber composition according to one embodiment of the present invention has a vulcanization time (T90) at 170°C measured in accordance with JIS K 6300-2 of preferably less than 20 minutes, more preferably less than 15 minutes, and even more preferably less than 10 minutes. The vulcanization time (T90) is, for example, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 minutes, or less than 20 minutes, and may be within a range between any two of the values ​​exemplified here.

[0086] In a rubber composition according to one embodiment of the present invention, a vulcanizate of the rubber composition preferably has the following properties. (Oil Resistance) In a rubber composition according to one embodiment of the present invention, a vulcanizate of the rubber composition is immersed in a test oil (high-grade automotive lubricating oil, ASTM No. 3, IRM 903 oil) at 130°C for 72 hours, and the volume change ΔV calculated in accordance with JIS K 6258 is preferably less than 40%, more preferably less than 30%, and even more preferably less than 20%. The volume change ΔV may be, for example, 0, 5, 10, 15, 20, 25, 30, 35%, or less than 40%, and may be within a range between any two of the values ​​exemplified here.

[0087] (Cold Resistance) The rubber composition according to one embodiment of the present invention has a vulcanizate of the rubber composition, whose T10, determined by a Gehman torsion test based on JIS K 6261, is preferably less than −26° C., more preferably less than −30° C., and even more preferably less than −34° C. The T10 is, for example, −50, −45, −40, −35, −30, −27° C., or less than −26° C., and may be within a range between any two of the values ​​exemplified here.

[0088] (Flexural fatigue resistance) In the rubber composition according to one embodiment of the present invention, a vulcanizate of the rubber composition is subjected to a de Mattia flexural fatigue test based on JIS K6260, and the number of flexural tests at the time of crack occurrence measured under conditions of a stroke of 58 mm and a speed of 300±10 rpm is preferably 300,000 or more, more preferably 650,000 or more, and even more preferably 1,000,000 or more. For example, 300,000, 350,000, 400,000, 450,000, 500,000, 550,000, 600,000, 650,000, 700,000, 750,000, 800,000, 850,000, 900,000, 950,000, 1,000,000, 2,000,000, 3,000,000, 4,000,000, 5,000,000, 6,000,000, 7,000,000, 8,000,000, and may be within a range between any two of the values ​​exemplified here.

[0089] (Ozone Resistance) When a vulcanizate of the rubber composition according to one embodiment of the present invention is subjected to a dynamic ozone degradation test based on JIS K 6259-1 under conditions of a test temperature of 40°C, an ozone concentration of 50 pphm, and an elongation rate of 30%, the time until cracks appear on the surface or side is preferably 100 hours or more, more preferably 300 hours or more, and even more preferably 500 hours or more. The time until cracks appear is, for example, 100, 200, 300, 400, 500, 600, 700, or 800 hours, and may be within a range between any two of the values ​​exemplified here.

[0090] (Compression Set Resistance) The rubber composition according to one embodiment of the present invention is press-vulcanized at 170°C for 30 minutes to obtain a cylindrical vulcanized molded article having a diameter of 29 mm and a height of 12.5 mm. The compression set measured under test conditions of 130°C and 72 hours in accordance with JIS K 6262:2013 is preferably less than 55, more preferably less than 50, and even more preferably less than 45.

[0091] The vulcanized rubber composition used to evaluate oil resistance, cold resistance, and ozone resistance can be, for example, a vulcanized product or vulcanized molded product obtained by press-vulcanization at 170 ° C. × 20 minutes according to JIS K6299. The vulcanized product used to evaluate compression set resistance can be a cylindrical vulcanized molded product with a diameter of 29 mm and a height of 12.5 mm obtained by press-vulcanization at 170 ° C. × 30 minutes. The vulcanized product used to evaluate flexural fatigue resistance can be a vulcanized molded product for the De Mattia flexural fatigue test obtained by press-vulcanization at 170 ° C. × 20 minutes. Each physical property can be specifically evaluated by the method described in the examples. The processing safety and processability of the rubber composition, and the oil resistance, cold resistance, ozone resistance, flex fatigue resistance, and compression set resistance of the vulcanizate can be controlled by adjusting the content of each monomer unit in each rubber contained in the rubber composition, the blending amount of each rubber, and the types and blending amounts of components other than rubber contained in the rubber composition, etc. The rubber composition according to the present invention is excellent in processing safety and processability, and can give vulcanizates and vulcanized molded articles that are excellent in oil resistance, cold resistance, ozone resistance, flex fatigue resistance, and compression set resistance.

[0092] 4. Unvulcanized molded body, vulcanized product, and vulcanized molded body The unvulcanized molded body according to this embodiment uses the rubber composition according to this embodiment, and is a molded body (molded article) of the rubber composition (unvulcanized state) according to this embodiment. The manufacturing method of the unvulcanized molded body according to this embodiment includes a step of molding the rubber composition (unvulcanized state) according to this embodiment. The unvulcanized molded body according to this embodiment is made of the rubber composition (unvulcanized state) according to this embodiment.

[0093] The vulcanizate according to the present embodiment is a vulcanizate of the rubber composition according to the present embodiment. The method for producing the vulcanizate according to the present embodiment includes a step of vulcanizing the rubber composition according to the present embodiment.

[0094] The vulcanization molded article according to this embodiment is a vulcanization molded article of the rubber composition according to this embodiment. The vulcanization molded article according to this embodiment uses the vulcanizate according to this embodiment and is a molded article (molded product) of the vulcanizate according to this embodiment. The vulcanization molded article according to this embodiment is made of the vulcanizate according to this embodiment.

[0095] The vulcanized molded article according to this embodiment can be obtained by molding a vulcanized product obtained by vulcanizing the rubber composition according to this embodiment (in an unvulcanized state), and can also be obtained by vulcanizing a molded article obtained by molding the rubber composition according to this embodiment (in an unvulcanized state). The vulcanized molded article according to this embodiment can be obtained by vulcanizing the rubber composition according to this embodiment after molding or during molding. The method for producing the vulcanized molded article according to this embodiment includes a step of molding the vulcanized product according to this embodiment, or a step of vulcanizing the unvulcanized molded article according to this embodiment.

[0096] The vulcanizate and vulcanized molded article according to one embodiment of the present invention preferably have the above-mentioned oil resistance, cold resistance, ozone resistance, flex fatigue resistance, and compression set resistance. The unvulcanized molded article, vulcanized article, and vulcanized molded article according to this embodiment can be used as rubber parts in various industrial fields such as buildings, structures, ships, railways, coal mines, and automobiles. The vulcanizate made from the rubber composition according to one embodiment of the present invention has excellent oil resistance, cold resistance, ozone resistance, flex fatigue resistance, and compression set resistance, and can be used as various components requiring these properties. The rubber composition according to one embodiment of the present invention can be used as rubber parts in various industrial fields such as buildings, structures, ships, railways, coal mines, and automobiles, and can be used as rubber parts for automobiles (e.g., automotive seals), hose materials, rubber molds, gaskets, rubber rolls, industrial cables, industrial conveyor belts, sponges, and in particular as components for accumulators, diaphragms, and hoses.

[0097] (Automotive Rubber Components) Automotive rubber components include gaskets, oil seals, and packings, which are components used in machines and equipment to prevent the leakage of liquids and gases and the intrusion of debris and foreign objects such as rainwater and dust. Specifically, there are gaskets used for fixed applications and oil seals and packings used for moving parts. Gaskets in which the sealing part is fixed with bolts or the like are made of various materials depending on the purpose, as opposed to soft gaskets such as O-rings and rubber sheets. Packings are also used for rotating parts such as pump and motor shafts, moving parts of valves, reciprocating parts such as pistons, coupler connections, and water stop parts of water faucets. A vulcanizate made from a rubber composition according to one embodiment of the present invention has excellent oil resistance, cold resistance, ozone resistance, flex fatigue resistance, and compression set resistance, making it possible to manufacture seals that utilize these properties, for example.

[0098] (Hose Material) A hose material is a bendable pipe, and specific examples include high- and low-pressure hoses for water supply, oil supply, air supply, steam supply, hydraulic pressure, etc. A vulcanizate made from the rubber composition according to one embodiment of the present invention is excellent in oil resistance, cold resistance, ozone resistance, flex fatigue resistance, and compression set resistance, and therefore, for example, it can be used to manufacture a hose material that takes advantage of these properties.

[0099] (Rubber molded products) Examples of rubber molded products include anti-vibration rubber, vibration-damping materials, and boots. Anti-vibration rubber and vibration-damping materials are rubbers that prevent the transmission of vibrations. Specific examples include torsional dampers, engine mounts, and muffler hangers for automobiles and various other vehicles that absorb vibrations during engine operation to prevent noise. The rubber composition of the present invention can improve the durability of anti-vibration rubber and vibration-damping materials. This makes it possible to produce anti-vibration rubber and vibration-damping materials that can be used in high-load applications that were difficult to achieve with conventional rubber compositions. Boots are bellows-shaped components whose outer diameter gradually increases from one end to the other. Specific examples include constant velocity joint cover boots, ball joint cover boots (dust cover boots), and rack and pinion gear boots that protect drive parts such as automobile drive systems. A vulcanizate made from the rubber composition according to one embodiment of the present invention has excellent oil resistance, cold resistance, ozone resistance, flex fatigue resistance, and compression set resistance, making it possible to produce boots that take advantage of these properties.

[0100] (Gaskets, etc.) Gaskets, oil seals, and packings are components in machines and devices that prevent the leakage of liquids and gases and the intrusion of debris and foreign objects such as rainwater and dust into the interior. Specifically, there are gaskets used for fixed applications and oil seals and packings used for moving parts. Gaskets in which the sealing part is fixed with bolts or the like are made of various materials depending on the purpose, as opposed to soft gaskets such as O-rings and rubber sheets. Packings are also used for rotating parts such as pump and motor shafts, moving parts of valves, reciprocating parts such as pistons, coupler connections, and water stop parts of water faucets. A vulcanizate made from a rubber composition according to one embodiment of the present invention has excellent oil resistance, cold resistance, ozone resistance, flex fatigue resistance, and compression set resistance, making it possible to manufacture seals that utilize these properties, for example.

[0101] (Rubber Roll) A rubber roll is manufactured by adhesively coating a metal core, such as an iron core, with rubber, and is generally manufactured by spirally winding a rubber sheet around a metal iron core. Rubber materials such as NBR, EPDM, and CR are used for rubber rolls depending on the required characteristics for various applications, such as papermaking, various metal manufacturing, film manufacturing, printing, general industrial use, agricultural machinery such as rice hullers, and food processing. CR has good mechanical strength that can withstand friction from the objects being conveyed, and is therefore used in a wide range of rubber roll applications. However, rubber rolls used in environments where oil is present, such as during the manufacture of industrial materials and products for steelmaking and papermaking, lack sufficient oil resistance, and improvements are needed. Furthermore, when plating products with gold, silver, nickel, chromium, and zinc, they may be exposed to acidic environments with a pH of 4 or less or alkaline environments with a pH of 11 or more, and resistance to these environments is also needed. Furthermore, rubber rolls used to convey heavy loads have the problem of deformation under load, and improvements are needed. The vulcanizate of the rubber composition according to one embodiment of the present invention is excellent in oil resistance, cold resistance, ozone resistance, flex fatigue resistance, and compression set resistance, and therefore, for example, it is possible to manufacture a rubber roll that takes advantage of these properties.

[0102] (Industrial Cable) Industrial cables are linear components for transmitting electrical or optical signals. They are made by covering a good conductor such as copper or a copper alloy, or an optical fiber, with an insulating covering layer, and a wide variety of industrial cables are manufactured depending on their structure and installation location. A vulcanizate made from the rubber composition according to one embodiment of the present invention is excellent in oil resistance, cold resistance, ozone resistance, flex fatigue resistance, and compression set resistance, and therefore can be used to manufacture industrial cables that utilize these properties, for example.

[0103] (Industrial Conveyor Belts) Industrial conveyor belts are available in rubber, resin, and metal, and are selected to suit a wide variety of uses. Among these, rubber conveyor belts are inexpensive and widely used, but when used in environments where there is a lot of friction and collision with the transported goods, they have been prone to damage due to deterioration. A vulcanizate made from a rubber composition according to one embodiment of the present invention has excellent oil resistance, cold resistance, ozone resistance, flex fatigue resistance, and compression set resistance, and can therefore be used to produce, for example, industrial conveyor belts that take advantage of these properties.

[0104] (Sponge) Sponges are porous materials with countless fine pores inside, and are specifically used in vibration-damping materials, sponge sealing parts, wetsuits, shoes, etc. The rubber composition of the present invention can increase the tensile strength of the sponge. Furthermore, the use of chloroprene-based rubber can also increase the flame retardancy of the sponge. A vulcanizate made from the rubber composition according to one embodiment of the present invention has excellent oil resistance, cold resistance, ozone resistance, flex fatigue resistance, and compression set resistance, and can therefore be used to produce, for example, sponges that take advantage of these properties or sponges with excellent flame retardancy. Furthermore, the hardness of the resulting sponge can be appropriately adjusted by adjusting the content of the foaming agent, etc.

[0105] (Accumulator) An accumulator is a pressure-storing vessel that utilizes the compressibility of nitrogen gas and is used for volume compensation and pulsation absorption in fluid circuits. The accumulator's mechanism utilizes the compressibility of nitrogen gas to store the pressure of a fluid such as oil or water, allowing it to instantaneously supply large amounts of pressurized fluid and absorb pulsation and impact pressure. Accumulators are available in bladder, diaphragm, and piston types depending on the gas-fluid isolation structure, and rubber materials such as NBR and CR are used for the bladders and diaphragms depending on the type of fluid used. The rubber composition of the present invention produces vulcanized rubber with excellent oil resistance, cold resistance, and flex fatigue resistance, making it possible to manufacture accumulators with superior durability compared to conventional rubber compositions.

[0106] (Diaphragm) A diaphragm is a separating membrane that separates fluids, and those with a particularly deep constriction and a folded cylindrical section are called Bellofram. Bellofram diaphragms are not used alone, but are assembled into devices to perform their functions. They are available in both rubber only and rubber-coated polyester fabrics. Diaphragms are specifically used in pressure reducing valves, pumps, and cylinders. The rubber composition of the present invention can enhance the oil resistance and flexural fatigue resistance of these diaphragms. This makes it possible to manufacture diaphragms for use with non-polar fluids such as engine oil and gear oil, which was difficult to achieve with conventional rubber compositions.

[0107] Methods for molding the rubber composition (unvulcanized state) and vulcanized product according to this embodiment include press molding, extrusion molding, calendar molding, etc. The temperature for vulcanizing the rubber composition may be set appropriately depending on the composition of the rubber composition, and may be 140 to 220°C, or 160 to 190°C. The vulcanization time for vulcanizing the rubber composition may be set appropriately depending on the composition of the rubber composition, the shape of the unvulcanized molded product, etc., and may be 2 to 60 minutes.

[0108] The present invention will be described in more detail below based on examples, but the present invention should not be construed as being limited to these examples.

[0109] <Method for Producing Chloroprene Rubber A-2> 24 parts by mass of chloroprene (monomer), 24 parts by mass of acrylonitrile (monomer), 0.5 parts by mass of diethylxanthogen disulfide, 200 parts by mass of pure water, 5.00 parts by mass of potassium rosinate (manufactured by Harima Chemicals Co., Ltd.), 0.40 parts by mass of sodium hydroxide, and 2.0 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (manufactured by Kao Corporation) were added to a 3 L polymerization vessel equipped with a heating / cooling jacket and a stirrer. Next, 0.1 parts by mass of potassium persulfate was added as a polymerization initiator, and emulsion polymerization was carried out in a nitrogen stream at a polymerization temperature of 40°C. The chloroprene was added in portions starting 20 seconds after the start of polymerization. The portion-by-portion addition flow rate was adjusted with a solenoid valve based on the change in the heat quantity of the refrigerant over the first 10 seconds of polymerization, and the flow rate was readjusted every 10 seconds thereafter, for continuous polymerization. When the polymerization rate relative to the total amount of chloroprene and acrylonitrile reached 50%, 0.02 parts by mass of phenothiazine as a polymerization terminator was added to terminate the polymerization. Thereafter, unreacted monomers in the reaction solution were removed under reduced pressure to obtain a latex of chloroprene rubber A-2 containing a chloroprene-acrylonitrile copolymer.

[0110] The above-mentioned polymerization rate [%] of the chloroprene latex was calculated from the dry mass of the air-dried chloroprene latex. Specifically, it was calculated using the following formula (A). In the formula, "solid content concentration" refers to the concentration [% by mass] of the solid content obtained by heating 2 g of a sample of chloroprene latex at 130°C and removing volatile components such as the solvent (water), volatile chemicals, and raw materials. "Total charge amount" refers to the total amount [g] of raw materials, reagents, and solvent (water) charged into the polymerization vessel from the start of polymerization to a certain time. "Evaporation residue" refers to the mass [g] of chemicals and raw materials charged from the start of polymerization to a certain time that do not volatilize under conditions of 130°C and remain as solids together with the polymer. "Monomer charge amount" refers to the sum [g] of the amount of monomer initially charged into the polymerization vessel and the amount of monomer added in portions from the start of polymerization to a certain time. Note that "monomer" here refers to the total amount of chloroprene and acrylonitrile. Conversion rate = {[(total charge amount × solid content concentration / 100) - evaporation residue] / charge amount of monomer} × 100 (A)

[0111] The content of acrylonitrile monomer units contained in the chloroprene rubber A-2 was calculated from the content of nitrogen atoms in the chloroprene-acrylonitrile copolymer rubber. Specifically, the content of nitrogen atoms in 100 mg of the chloroprene rubber A-2 was measured using an elemental analyzer (Sumigraph 220F, manufactured by Sumika Chemical Analysis Center, Ltd.), and the content of acrylonitrile monomer units was calculated.

[0112] The above elemental analysis was carried out as follows. The electric furnace temperatures were set to 900°C for the reactor, 600°C for the reduction furnace, 70°C for the column, and 100°C for the detector, and oxygen gas was flowed at 0.2 mL / min as the combustion gas and helium gas was flowed at 80 mL / min as the carrier gas. A calibration curve was prepared using aspartic acid (10.52%) with a known nitrogen content as the standard substance. The chloroprene rubber A-2 obtained by the above production method had an acrylonitrile monomer unit content of 10.0% by mass.

[0113] <Method for producing chloroprene rubbers A-1, and A-3 to A-5> The amount of acrylonitrile monomer added in the polymerization step was changed to obtain chloroprene rubber A-1 having an acrylonitrile monomer unit content of 5.0 mass% in the chloroprene rubber, chloroprene rubber A-3 having an acrylonitrile monomer unit content of 15.0 mass%, chloroprene rubber A-4 having an acrylonitrile monomer unit content of 20.0 mass%, and chloroprene rubber A-5 having an acrylonitrile monomer unit content of 25.0 mass%.

[0114] <Preparation of Rubber Composition> The components shown in Tables 1 to 3 were mixed and kneaded with an 8-inch open roll to obtain rubber compositions of the examples and comparative examples.

[0115] The components used to obtain the rubber compositions are as follows. <Chloroprene-based rubbers> Rubber A: Chloroprene-based rubbers A-1 to A-5 described above Rubber B: Mercaptan-modified chloroprene-based rubber, "S-40V" manufactured by Denka Co., Ltd. <Epichlorohydrin-based rubbers> Epichlorohydrin-ethylene oxide-allyl glycidyl ether terpolymer (ethylene oxide 56 mol%), "Epichromer CG102" manufactured by Osaka Soda Co., Ltd. Epichlorohydrin-ethylene oxide-allyl glycidyl ether terpolymer (ethylene oxide 35 mol%), "Hydrin T3102" manufactured by Nippon Zeon Co., Ltd. Epichlorohydrin-ethylene oxide copolymer (ethylene oxide 61 mol%), "Epichromer D" manufactured by Osaka Soda Co., Ltd.

[0116] <Anti-aging agents> Compounds having a p-phenylenediamine structure: N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine, "Nocrac 6C" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Compounds having a p-phenylenediamine structure: N-phenyl-N'-isopropyl-p-phenylenediamine, "Nocrac 810-NA" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Compounds having a p-phenylenediamine structure: N-phenyl-N'-(3-methacryloyloxy-2-hydroxypropyl)-p-phenylenediamine, "Nocrac G-1" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Aromatic secondary amine compounds (excluding compounds having a p-phenylenediamine structure): 4,4'-bis(α,α-dimethylbenzyl)diphenylamine, "Nocrac CD" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Dithiocarbamate compounds: nickel dibutyldithiocarbamate, "Nocrac NBC" manufactured by Ouchi Shinko Chemical Industry Co., Ltd.

[0117] <Acid acceptor> Hydrotalcite compound: Chemical composition Mg 4.3 Al 2 (OH) 12.6 CO 3 ・3.5H 2 O. "DHT-4A" manufactured by Kyowa Chemical Industry Co., Ltd. Magnesium-aluminum solid solution: Chemical composition Mg 0.7 Al 0.3 O 1.15, "KW-2100" manufactured by Kyowa Chemical Industry Co., Ltd. Magnesium oxide: "Kyowamag 150" manufactured by Kyowa Chemical Industry Co., Ltd. Zinc oxide, "Zinc oxide type 2" manufactured by Sakai Chemical Industry Co., Ltd.

[0118] <Vulcanization accelerator> Ethylene thiourea, "Accel 22S" manufactured by Kawaguchi Chemical Industry Co., Ltd. 3-methyl-thiazolidine-2-thione, "Rhenogran MTT-80" manufactured by Lanxess AG 2-mercaptobenzimidazole, "Nocrac MB" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Tetrabenzyl thiuram disulfide, "Noccela TBZTD" manufactured by Ouchi Shinko Chemical Industry Co., Ltd.

[0119] <Filler> Carbon black (FEF), Asahi Carbon Co., Ltd. "Asahi #60UG" <Plasticizer> Polyether ester, ADEKA Corporation "RS-700" <Lubricant / processing aid> - Stearic acid, New Japan Chemical Co., Ltd. "Stearic acid 50S" - Lubricant / processing aid: Sorbitan monostearate, Span 60, Fujifilm Wako Pure Chemical Corporation "Sorbitan monostearate"

[0120] <Evaluation of Rubber Composition> (Processing Safety) The obtained rubber composition was subjected to a Mooney scorch test using an L-type rotor at a test temperature of 125°C in accordance with JIS K 6300-1. The time required for the measured Mooney viscosity to increase by 5M was taken as the scorch time. The obtained scorch time was evaluated according to the following evaluation criteria: A: 10 minutes or more B: 7 minutes or more but less than 10 minutes C: 4 minutes or more but less than 7 minutes D: Less than 4 minutes

[0121] (Processability) The vulcanization time (T90) of the obtained rubber composition at 170°C was measured in accordance with JIS K 6300-2 and evaluated according to the following criteria: A: Less than 10 minutes B: 10 minutes or more but less than 15 minutes C: 15 minutes or more but less than 20 minutes D: 20 minutes or more

[0122] <Preparation of vulcanized molded body> The obtained rubber composition was press-vulcanized at 170 ° C × 20 minutes according to JIS K6250 to prepare a sheet-shaped vulcanized molded body with a thickness of 2 mm. The obtained rubber composition was also press-vulcanized at 170 ° C × 30 minutes to prepare a cylindrical vulcanized molded body with a diameter of 29 mm and a height of 12.5 mm for compression set measurement. The obtained rubber composition was also press-vulcanized at 170 ° C × 20 minutes to prepare a vulcanized molded body for the De Mattia flexural fatigue test.

[0123] <Evaluation of vulcanized molded articles> The vulcanized molded articles obtained were evaluated by the following methods. The results are shown in Tables 1 to 3.

[0124] (Oil Resistance) Test specimens measuring 25 mm in length and 20 mm in width were punched out from the above-mentioned sheet-like vulcanized molded article to obtain test specimens. The obtained test specimens were immersed in a test oil (high-grade lubricating oil for automobiles, ASTM No. 3, IRM 903 oil) at 130°C for 72 hours. The volume change rate ΔV was calculated in accordance with JIS K 6258. The obtained volume change rate ΔV was evaluated according to the following criteria: A: less than 20% B: 20% or more but less than 30% C: 30% or more but less than 40% D: 40% or more

[0125] (Cold Resistance) A Gehman torsion test was performed based on JIS K 6261 to determine T10. For the above-mentioned sheet-like vulcanized molded article, the temperature (T10) at which the 180° torsion modulus became 10 times the 180° torsion modulus at room temperature was determined. The obtained T10 was evaluated according to the following criteria: A: Less than -34°C B: -34°C or higher but less than -30°C C: -30°C or higher but less than -26°C D: -26°C or higher

[0126] (Flexural Fatigue Resistance) A De Mattia flexural fatigue test was conducted based on JIS K6260. Under conditions of a stroke of 58 mm and a speed of 300±10 rpm, the number of flexural tests (unit: 10,000 times) at which cracks occurred was measured to evaluate fatigue durability. Measurements were carried out up to 10 million times. The number of flexural tests at which cracks occurred was evaluated according to the following evaluation criteria: S: 5 million or more times; A: 1 million or more times, but less than 5 million times; B: 650,000 or more times, but less than 1 million times; C: 300,000 or more times, but less than 650,000 times; D: Less than 300,000 times.

[0127] (Compression set resistance) A cylindrical vulcanized molded article having a diameter of 29 mm and a height of 12.5 mm was obtained by press vulcanization at 170°C for 30 minutes, and the compression set was measured at 130°C for 72 hours in accordance with JIS K 6262:2013. The compression set was evaluated according to the following criteria: A: Less than 45 B: 45 or more but less than 50 C: 50 or more but less than 55 D: 55 or more

[0128] (Ozone Resistance) Test pieces measuring 25 mm in length and 20 mm in width were punched out from the above-mentioned sheet-like vulcanized molded product to obtain test pieces, which were subjected to a dynamic ozone degradation test in accordance with JIS K 6259-1. The test pieces were continuously exposed to ozone under the conditions of a test temperature of 40°C, an ozone concentration of 50 pphm, and an elongation rate of 30%, and the time until cracks appeared on the surface or side was measured and evaluated according to the following criteria: A: 500 hours or more B: 300 hours or more but less than 500 hours C: 100 hours or more but less than 300 hours D: Less than 100 hours

[0129]

[0130]

[0131]

Claims

1. A rubber composition comprising a chloroprene-based rubber and an epichlorohydrin-based rubber, The rubber composition contains, when the rubber contained in the rubber composition is taken as 100 parts by mass, 5 to 95 parts by mass of a chloroprene-based rubber, 5 to 95 parts by mass of an epichlorohydrin-based rubber, and 0.1 to 10 parts by mass of a compound having a p-phenylenediamine structure, and the chloroprene-based rubber contains a chloroprene-based rubber having an unsaturated nitrile monomer unit content of less than 25% by mass. Rubber composition.

2. The rubber composition according to claim 1, wherein the compound having a p-phenylenediamine structure is represented by the following formula (1): [Case 1] (In formula (1), R 1 and R 2 represents an organic group; R 1 and R 2 At least one of the above contains an aromatic ring structure.

3. The rubber composition according to claim 1 or 2, wherein the compound having a p-phenylenediamine structure is selected from the group consisting of N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine, N-phenyl-N'-isopropyl-p-phenylenediamine, N-1-methylheptyl-N'-phenyl-p-phenylenediamine, N-phenyl-N'-(3-methacryloyloxy-2-hydroxypropyl)-p-phenylenediamine, N,N'-di-2-naphthyl-p-phenylenediamine, N,N'-diphenyl-p-phenylenediamine, p-(p-toluenesulfonylamide)diphenylamine, and N-cyclohexyl-N'-phenyl-p-phenylenediamine.

4. 3. The rubber composition according to claim 1, wherein the unsaturated nitrile monomer unit is an acrylonitrile monomer unit.

5. The chloroprene-based rubber includes rubber A which is a chloroprene-based rubber having 1 to 20 mass% of unsaturated nitrile monomer units, 60 to 99 mass% of chloroprene monomer units, and 0 to 20 mass% of monomer units other than chloroprene monomers and unsaturated nitrile monomers, and rubber B which is a chloroprene-based rubber having 80 to 100 mass% of chloroprene monomer units and 0 to 20 mass% of monomer units other than chloroprene monomers and unsaturated nitrile monomers. The rubber composition according to claim 1 or 2.

6. The rubber composition according to claim 5, wherein the rubber A is 20 to 99 mass% and the rubber B is 1 to 80 mass% when the chloroprene-based rubber contained in the rubber composition is 100 mass%.

7. 3. The rubber composition according to claim 1, wherein the epichlorohydrin rubber contains 5 to 90 mol % of ethylene oxide monomer units.

8. 3. The rubber composition according to claim 1 or claim 2, wherein the rubber composition contains 0.1 to 20 parts by mass of an acid acceptor when the rubber contained in the rubber composition is taken as 100 parts by mass, and the acid acceptor includes at least one selected from the group consisting of hydrotalcite compounds, magnesium-aluminum solid solutions, zinc oxide, magnesium oxide, lead oxide, trimead tetroxide, iron trioxide, titanium dioxide, and calcium oxide.

9. The rubber composition according to claim 1 or claim 2, which contains at least one compound selected from the group consisting of sulfur, trimethylthiourea, ethylenethiourea, diphenylthiourea, diethylthiourea, dibutylthiourea, 1,3-trimethylene-2-thiourea, and 3-methylthiazolidine-2-thione.

10. 3. The rubber composition according to claim 1, further comprising at least one compound selected from the group consisting of 2-mercaptobenzimidazole, 2-mercaptomethylbenzimidazole and a zinc salt of 2-mercaptobenzimidazole.

11. A vulcanizate of the rubber composition according to claim 1 or 2.

12. A vulcanized molded article using the vulcanizate according to claim 11.