Sintered member, and method for producing sintered member

JPWO2023210568A5Active Publication Date: 2024-12-04SUMITOMO ELECTRIC INDUSTRIES LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024517304
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-12-04
Estimated Expiration
2043-04-24

AI Technical Summary

Technical Problem

Current methods for manufacturing sintered members struggle to produce hole or groove features with depths significantly larger than their respective diameters or widths, leading to limitations in achieving desired geometric ratios.

Method used

A method involving the preparation of raw material powder with a lubricant having a melting point of 150°C or less, pressurization to form a compact with a relative density of 95% or more, and subsequent machining to create holes or grooves that satisfy specific diameter-to-depth and width-to-depth ratios, ensuring minimal shrinkage during sintering and maintaining precise feature sizes.

Benefits of technology

The method effectively produces sintered members with hole or groove features that have depths greater than their diameters or widths, achieving high relative density and maintaining dimensional accuracy, thus overcoming the limitations of traditional manufacturing techniques.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A sintered member composed of a metal, wherein the sintered member has a relative density of 95% or greater and has at least one of a hole for which the diameter x1 (mm) and depth y1 (mm) satisfy specific requirements and a groove for which the width x2 (mm) and depth y2 (mm) satisfy specific requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Sintered member and method for manufacturing the same

[0001] The present disclosure relates to a sintered member and a method for manufacturing a sintered member. This application claims priority to Japanese Patent Application No. 2022-071901 filed on April 25, 2022, and incorporates by reference all of the contents of said Japanese application.

[0002] The method for manufacturing a sintered part in Patent Document 1 includes the steps of press-molding raw material powder to produce a green compact, forming holes in the green compact, and sintering the green compact with the holes formed in. The raw material powder includes iron powder, copper powder, carbon powder, and ethylene bisstearamide.

[0003] Japanese Patent Application Laid-Open No. 2019-14971

[0004] The sintered member of the present disclosure is a sintered member made of metal, has a relative density of 95% or more, and has at least one of a hole portion whose diameter x1 (mm) and depth y1 (mm) satisfy the following requirements (a1) to (a7), and a groove portion whose width x2 (mm) and depth y2 (mm) satisfy the following requirements (b1) to (b3). (a1) y1 > 2.67x1 + 0.217 for 0.05≦x1 < 0.08. (a2) y1 > 28.5x1 - 1.85 for 0.08≦x1 < 0.1. (a3) ​​y1 > 10x1 for 0.1≦x1 < 0.3. (a4) y1 > 8x1 + 0.6 for 0.3≦x1 < 0.8. (a5) y1 > 32.9x1 - 19.3 for 0.8≦x1 < 1.5. (a6) y1 > 20x1 for 1.5≦x1 < 2.0. (a7) y1 > 10x1 + 20 for 2.0≦x1. (b1) y2 > 5x2 + 0.4 for 0.05≦x2 < 0.2. (b2) In the range of 0.2≦x2<0.5, y2>28.7x2−4.3 (b3) In the range of 0.5≦x2, y2>6x2+7

[0005] The method for manufacturing a sintered member of the present disclosure includes the steps of: preparing a raw material powder containing a metal powder and a lubricant; compressing the raw material powder to produce a powder compact having a relative density of 95% or more; performing at least one of hole processing and groove processing on the powder compact to produce a processed body having at least one of a hole portion whose diameter x1 (mm) and a depth y1 (mm) satisfy the following requirements (a1) to (a7) and a groove portion whose width x2 (mm) and a depth y2 (mm) satisfy the following requirements (b1) to (b3); and sintering the processed body, wherein the raw material powder contains 0.025 mass % or more and 0.2 mass % or less of the lubricant, and the melting point of the lubricant is 150°C or less. (a1) y1 > 2.67x1 + 0.217 for 0.05≦x1 < 0.08. (a2) y1 > 28.5x1 - 1.85 for 0.08≦x1 < 0.1. (a3) ​​y1 > 10x1 for 0.1≦x1 < 0.3. (a4) y1 > 8x1 + 0.6 for 0.3≦x1 < 0.8. (a5) y1 > 32.9x1 - 19.3 for 0.8≦x1 < 1.5. (a6) y1 > 20x1 for 1.5≦x1 < 2.0. (a7) y1 > 10x1 + 20 for 2.0≦x1. (b1) y2 > 5x2 + 0.4 for 0.05≦x2 < 0.2. (b2) In the range of 0.2≦x2<0.5, y2>28.7x2−4.3 (b3) In the range of 0.5≦x2, y2>6x2+7

[0006] FIG. 1 is a schematic perspective view showing a sintered member of an embodiment. FIG. 2 is a cross-sectional view taken along line II-II of FIG. 1. FIG. 3 is a partial cross-sectional view showing another example of a sintered member of an embodiment. FIG. 4 is a cross-sectional view taken along line IV-IV of FIG. 3. FIG. 5 is a graph showing the relationship between the diameter and depth of the hole of the sintered member produced in Test Example 1. FIG. 6 is an enlarged graph of region A of FIG. 5. FIG. 7 is an enlarged graph of region B of FIG. 6. FIG. 8 is a graph showing the relationship between the width and depth of the groove of the sintered member produced in Test Example 2. FIG. 9 is an enlarged graph of region C of FIG. 8.

[0007] [Problem to be Solved by the Present Disclosure] It is desired to manufacture a sintered member having a hole portion whose depth is large relative to its diameter, or a groove portion whose depth is large relative to its width.

[0008] An object of the present disclosure is to provide a sintered member having a hole portion whose depth is large relative to its diameter or a groove portion whose depth is large relative to its width.Another object of the present disclosure is to provide a method for manufacturing the sintered member.

[0009] [Advantages of the Present Disclosure] The sintered member of the present disclosure has a hole portion whose depth is large relative to its diameter or a groove portion whose depth is large relative to its width. The method for manufacturing a sintered member of the present disclosure can manufacture the sintered member of the present disclosure.

[0010] <Description of Embodiments of the Present Disclosure> First, embodiments of the present disclosure will be listed and described.

[0011] (1) A sintered member according to one embodiment of the present disclosure is a sintered member made of metal, having a relative density of 95% or more, and having at least one of a hole portion having a diameter x1 (mm) and a depth y1 (mm) that satisfy the following requirements (a1) to (a7), and a groove portion having a width x2 (mm) and a depth y2 (mm) that satisfy the following requirements (b1) to (b3). (a1) y1 > 2.67x1 + 0.217 for 0.05≦x1 < 0.08. (a2) y1 > 28.5x1 - 1.85 for 0.08≦x1 < 0.1. (a3) ​​y1 > 10x1 for 0.1≦x1 < 0.3. (a4) y1 > 8x1 + 0.6 for 0.3≦x1 < 0.8. (a5) y1 > 32.9x1 - 19.3 for 0.8≦x1 < 1.5. (a6) y1 > 20x1 for 1.5≦x1 < 2.0. (a7) y1 > 10x1 + 20 for 2.0≦x1. (b1) y2 > 5x2 + 0.4 for 0.05≦x2 < 0.2. (b2) In the range of 0.2≦x2<0.5, y2>28.7x2−4.3 (b3) In the range of 0.5≦x2, y2>6x2+7

[0012] The sintered member has a hole portion whose depth is greater than its diameter, or a groove portion whose depth is greater than its width.

[0013] (2) In the sintered member of (1) above, the metal may be pure iron or an iron alloy.

[0014] The sintered member made of pure iron or an iron alloy has holes whose depth is greater than their diameter, or grooves whose depth is greater than their width.

[0015] (3) In the sintered member of (1) above, the metal may be stainless steel.

[0016] The sintered member made of stainless steel has holes whose depth is greater than their diameter, or grooves whose depth is greater than their width.

[0017] (4) A method for manufacturing a sintered member according to one embodiment of the present disclosure includes the steps of: preparing a raw material powder containing a metal powder and a lubricant; compressing the raw material powder to produce a powder compact having a relative density of 95% or more; performing at least one of hole processing and groove processing on the powder compact to produce a processed body having at least one of a hole portion having a diameter x1 (mm) and a depth y1 (mm) that satisfy the following requirements (a1) to (a7) and a groove portion having a width x2 (mm) and a depth y2 (mm) that satisfy the following requirements (b1) to (b3); and sintering the processed body, wherein the raw material powder contains 0.025 mass % or more and 0.2 mass % or less of the lubricant, and the melting point of the lubricant is 150°C or less. (a1) y1 > 2.67x1 + 0.217 for 0.05≦x1 < 0.08. (a2) y1 > 28.5x1 - 1.85 for 0.08≦x1 < 0.1. (a3) ​​y1 > 10x1 for 0.1≦x1 < 0.3. (a4) y1 > 8x1 + 0.6 for 0.3≦x1 < 0.8. (a5) y1 > 32.9x1 - 19.3 for 0.8≦x1 < 1.5. (a6) y1 > 20x1 for 1.5≦x1 < 2.0. (a7) y1 > 10x1 + 20 for 2.0≦x1. (b1) y2 > 5x2 + 0.4 for 0.05≦x2 < 0.2. (b2) In the range of 0.2≦x2<0.5, y2>28.7x2−4.3 (b3) In the range of 0.5≦x2, y2>6x2+7

[0018] The method for manufacturing a sintered member described above compresses raw material powder containing a lubricant with a melting point of 150°C or lower, thereby easily spreading the lubricant between the particles of the resulting powder compact. Because the lubricant spreads between the particles of the powder compact, the holes can be formed by drilling holes in the powder compact, and the grooves can be formed by drilling grooves in the powder compact. The relative density of the powder compact and the relative density of the processed body are the same. Since the relative density of the produced powder compact is 95% or higher, the amount of shrinkage upon sintering the processed body is very small. Therefore, the sizes of the holes and grooves in the sintered member are substantially the same as those of the processed body. Therefore, the method for manufacturing a sintered member described above can produce sintered members having holes whose depth is large relative to their diameter or grooves whose depth is large relative to their width.

[0019] (5) In the method for producing a sintered member according to (4), the lubricant may be stearic acid, erucic acid amide, or stearic acid amide.

[0020] The lubricant easily spreads over a wide range between the particles of the powder compact when the raw material powder is compressed.

[0021] <Details of the Embodiments of the Present Disclosure> The embodiments of the present disclosure will be described below with reference to the drawings. The same reference numerals in the drawings indicate the same objects. The sizes of the components shown in each drawing are expressed for the purpose of clarity of explanation and do not necessarily represent the actual dimensional relationships.

[0022] 1 to 4, a sintered member 1 according to an embodiment will be described. The sintered member 1 is made of metal. One of the features of the sintered member 1 according to this embodiment is that it has a high relative density and at least one of a hole 2 of a specific size and a groove 3 of a specific size.

[0023] [Material] The material of the sintered member 1 is a metal, such as pure iron, an iron alloy, or a non-ferrous metal.

[0024] Pure iron is iron with a purity of 99% or more, that is, pure iron has an iron (Fe) content of 99% by mass or more.

[0025] An iron alloy is an alloy containing additive elements, with the remainder being iron (Fe) and unavoidable impurities. Iron alloys contain the largest amount of Fe. The additive elements contained in iron alloys are, for example, one or more elements selected from the group consisting of nickel (Ni), copper (Cu), chromium (Cr), molybdenum (Mo), manganese (Mn), carbon (C), silicon (Si), aluminum (Al), phosphorus (P), boron (B), nitrogen (N), and cobalt (Co). Specific examples of iron alloys include stainless steel, Fe—C alloys, Fe—Cu—Ni—Mo alloys, Fe—Ni—Mo—Mn alloys, Fe—P alloys, Fe—Cu alloys, Fe—Cu—C alloys, Fe—Cu—Mo alloys, Fe—Ni—Mo—Cu—C alloys, Fe—Ni—Cu alloys, Fe—Ni—Mo—Cu alloys, Fe—Ni—Cu alloys, Fe—Ni—Mo—C alloys, Fe—Ni—Cr alloys, Fe—Ni—Mo—Cr alloys, Fe—Cr alloys, Fe—Mo—Cr alloys, Fe—Cr—C alloys, Fe—Ni—C alloys, and Fe—Mo—Mn—Cr—C alloys. An example of stainless steel is austenitic stainless steel. An example of austenitic stainless steel is SUS304 or SUS304L.

[0026] The non-ferrous metal is, for example, copper, a copper alloy, aluminum, or an aluminum alloy.

[0027] The composition of the sintered portion 1 can be confirmed by component analysis using ICP optical emission spectrometry (ICP-OES).

[0028] [Relative Density] The relative density of the sintered member 1 is 95% or more. A sintered member 1 with a relative density of 95% or more has excellent mechanical properties such as strength. The relative density of the sintered member 1 may be 96% or more, particularly 97% or more. The upper limit of the relative density of the sintered member 1 is not particularly limited and can be appropriately selected within the range that can be produced. The relative density of the sintered member 1 may be, for example, 99.9% or less. That is, the relative density of the sintered member 1 may be 95% or more and 99.9% or less, further 96% or more and 99.9% or less, particularly 97% or more and 99.9% or less.

[0029] The relative density of the sintered part 1 refers to the ratio (%) of the actual density of the sintered part 1 to the true density of the sintered part 1. That is, the relative density of the sintered part 1 is calculated by [(actual density of the sintered part 1 / true density of the sintered part 1) × 100]. The actual density of the sintered part 1 can be calculated by immersing the sintered part 1 in oil to impregnate the sintered part 1 with oil and calculating [oil-impregnated density × (mass of the sintered part 1 before oil impregnation / mass of the sintered part 1 after oil impregnation)]. The oil-impregnated density is (mass of the sintered part 1 after oil impregnation / volume of the sintered part 1 after oil impregnation). That is, the actual density of the sintered part 1 can be calculated by (mass of the sintered part 1 before oil impregnation / volume of the sintered part 1 after oil impregnation). The volume of the sintered part 1 after oil impregnation can typically be measured by the liquid displacement method. The true density of the sintered part 1 is the theoretical density calculated from the composition of the sintered part 1 when it is assumed that no voids are present inside.

[0030] [Hole] The hole 2 is a through hole or a blind hole. A blind hole has a bottom. The number of the hole 2 is not particularly limited and can be selected appropriately. When there are a plurality of the hole 2, both a through hole and a blind hole may be provided. The hole 2 has a substantially uniform diameter in a direction along the depth of the hole 2.

[0031] The diameter x1 (mm) and depth y1 (mm) of the hole 2 satisfy the following requirements (a1) to (a7). Details will be explained in Test Example 1 with reference to Figures 5 to 7. (a1) y1 > 2.67x1 + 0.217 in the case of 0.05 ≦ x1 < 0.08 (a2) y1 > 28.5x1 - 1.85 in the case of 0.08 ≦ x1 < 0.1 (a3) ​​y1 > 10x1 in the case of 0.1 ≦ x1 < 0.3 (a4) y1 > 8x1 + 0.6 in the case of 0.3 ≦ x1 < 0.8 (a5) y1 > 32.9x1 - 19.3 in the case of 0.8 ≦ x1 < 1.5 (a6) y1 > 20x1 in the case of 1.5 ≦ x1 < 2.0 (a7) y1 > 10x1 + 20 in the case of 2.0 ≦ x1

[0032] The upper limit of the depth y1 (mm) relative to the diameter x1 (mm) of the hole 2 depends, for example, on the maximum diameter and length of the tool or the maximum size of the powder compact during the manufacturing process. For example, commercially available drills used to form the hole 2 typically have an L / D ratio (the ratio of the drill flute length L (mm) to the drill diameter D (mm)) of 20 or less or 30 or less. Although this also depends on the diameter D and the material of the tool, even drills dedicated to drilling particularly deep holes are said to have an L / D limit of 40 or 50 or less. For example, the upper limit of the depth y1 relative to the diameter x1 of the hole 2 is at least 50 times the diameter x1 in any of (a1) to (a7) above. It is considered possible to make the depth of the hole 2 formed by the manufacturing method of the sintered member of this embodiment described below deeper than a hole drilled with a drill having an L / D of 50, to the extent that such a drill is available.

[0033] [Groove Portion] The number of groove portions 3 is not particularly limited and can be selected appropriately. The groove portions 3 have a substantially uniform width in the direction along the depth of the groove portions 3.

[0034] The width x2 (mm) and depth y2 (mm) of the groove 3 satisfy the following requirements (b1) to (b3). Details will be explained in Test Example 2 with reference to Figures 8 and 9. (b1) When 0.05 ≤ x2 < 0.2, y2 > 5x2 + 0.4 (b2) When 0.2 ≤ x2 < 0.5, y2 > 28.7x2 - 4.3 (b3) When 0.5 ≤ x2, y2 > 6x2 + 7

[0035] The upper limit of the depth y2 (mm) of the groove 3 relative to the width x2 (mm) depends on, for example, the width limit of the tool or the size limit of the powder compact in the manufacturing process.

[0036] Although not shown, the sintered member 1 may have both the hole 2 and the groove 3 .

[0037] [Method for manufacturing a sintered member] The method for manufacturing a sintered member according to the embodiment includes step A of preparing a raw material powder, step B of producing a powder compact, step C of producing a processed body, and step D of sintering the processed body. One of the features of the method for manufacturing a sintered member is that a specific raw material powder is prepared in step A, and at least one of a specific hole and a groove is formed in step C. The method for manufacturing a sintered member according to the embodiment manufactures the sintered member 1 described above.

[0038] [Step A: Preparation of Raw Powder] In step A, a raw powder containing a metal powder and a lubricant is prepared. The raw powder does not contain an organic binder. The metal powder is, for example, an iron-based powder or a non-iron-based powder.

[0039] (Iron-based powder) The iron-based powder is one type of powder selected from the group consisting of pure iron powder, ferrous alloy powder, first mixed powder, second mixed powder, third mixed powder, and fourth mixed powder. As described above, the pure iron constituting the pure iron powder has a purity of 99% or more. The type of ferrous alloy constituting the ferrous alloy powder is the iron alloy described above. The first mixed powder is composed of pure iron powder and powder of alloying elements. The powder of alloying elements is powder of elements that produce the iron alloy described above when step D is performed. The alloying elements are additive elements of the iron alloy described above. When the sintered component 1 to be manufactured is composed of an iron alloy containing multiple additive elements, the powder of alloying elements includes powder of multiple additive elements. The second mixed powder is composed of ferric alloy powder and carbon powder. Examples of ferric alloys constituting the ferric alloy powder include Fe-Cu alloys, Fe-Ni-Mo-Cu alloys, Fe-Ni-Mo alloys, Fe-Cr alloys, Fe-Ni alloys, and Fe-Mo-Mn-Cr alloys. The third mixed powder is composed of pure iron powder, powders of the alloying elements, and ferrous alloy powder. The fourth mixed powder is composed of pure iron powder, powders of the alloying elements, ferric alloy powder, and carbon powder.

[0040] (Non-ferrous Powder) The non-ferrous powder is copper powder, copper alloy powder, aluminum powder, or aluminum alloy powder.

[0041] (Lubricant) The lubricant is a lubricant that spreads between multiple particles due to the processing heat generated when the raw material powder is compressed in step B. Such a lubricant has a melting point of 150°C or lower. The melting point of the lubricant may further be 110°C or lower, particularly 85°C or lower. The melting point of the lubricant is, for example, 50°C or higher. That is, the melting point of the lubricant may be 50°C or higher and 150°C or lower, further 55°C or higher and 110°C or lower, particularly 60°C or higher and 85°C or lower. Specific examples of lubricants are stearic acid, erucic acid amide, and stearic acid amide. These lubricants are likely to spread over a wide area between multiple particles due to the processing heat generated in step B.

[0042] The proportion of lubricant contained in the raw material powder is, for example, 0.025% by mass or more and 0.2% by mass or less. If the proportion is 0.025% by mass or more, the lubricant is likely to spread over a wide area between multiple particles due to processing heat generated in step B. Therefore, it is easy to form at least one of holes and grooves in step C. In particular, it is easy to form at least one of multiple holes and multiple grooves using the same tool. If the proportion is 0.2% by mass or less, a dense powder compact is likely to be produced in step B. Furthermore, volumetric shrinkage due to loss of lubricant when the processed body is sintered in step D can be suppressed, making it easy to produce sintered parts with high dimensional accuracy and high density. The proportion may further be 0.04% by mass or more and 0.18% by mass or less. The proportions are values ​​when the entire raw material powder is 100% by mass.

[0043] [Step B: Preparation of Green Compact] In step B, the raw material powder is compressed to prepare a green compact having a relative density of 95% or more. The relative density may be 97% or more, particularly 98% or more. The relative density of the green compact is calculated by [(density of actual green compact / true density of green compact) x 100]. The density of the actual green compact has the same meaning as the density of the actual sintered member described above. The true density of the green compact has the same meaning as the true density of the sintered member described above. The shape of the green compact can be selected appropriately and is not particularly limited. The shape of the green compact is, for example, columnar or cylindrical. The green compact is prepared using an appropriate mold that can be molded into the above shape.

[0044] The compacting pressure is set so that the relative density of the powder compact to be compacted is 95% or more, and so that heat is generated to the extent that the lubricant spreads between the particles. That is, in this process, the lubricant spreads due to the processing heat generated during compacting. The mold is not heated by a heater to spread the lubricant. The compacting pressure is, for example, 1560 MPa or more. The higher the compacting pressure, the higher the relative density of the powder compact produced. The compacting pressure may further be 1660 MPa or more, 1760 MPa or more, particularly 1860 MPa or 1960 MPa or more. There is no particular upper limit to the compacting pressure.

[0045] [Step C: Fabrication of Workpiece] In step C, the powder compact is subjected to at least one of cutting processes, i.e., drilling and grooving, to fabricate a workpiece having at least one of a hole and a groove. The relationship between the diameter x1 and depth y1 of the formed hole is within the range described above. The relationship between the width x2 and depth y2 of the formed groove is within the range described above. Because the lubricant spreads between the particles of the powder compact, at least one of a hole and a groove that satisfies the range described above can be formed. An example of a tool for forming a hole is a drill. Hole drilling may be performed under wet conditions, either with internal or external oil supply, depending on the diameter of the drill. An example of a tool for forming a groove is a dicing blade, a metal saw, or a grooving tool.

[0046] [Step D: Sintering of the Workpiece] In step D, the workpiece is sintered. The sintered body 1 is produced by sintering the workpiece. The workpiece shrinks due to sintering. The relative density of the workpiece is the same as that of the powder compact. That is, the relative density of the workpiece is high. Therefore, the amount of shrinkage of the workpiece due to sintering is very small. Therefore, the relative density of the sintered body 1 is equal to or higher than that of the workpiece. That is, the relative density of the sintered body 1 is 95% or higher. The sizes of the holes 2 and grooves 3 of the sintered body 1 are substantially the same as those of the workpiece. The sintering conditions can be appropriately selected depending on the composition of the raw material powder. The sintering temperature is, for example, 1100°C to 1400°C, and may be 1200°C to 1300°C. The sintering time is, for example, 15 minutes to 150 minutes, and may be 20 minutes to 60 minutes. Known sintering conditions can be applied.

[0047] [Other Steps] The method for producing a sintered member may include at least one of a step α of heat treating the sintered member 1 and a step β of finish-processing the sintered member 1 .

[0048] (Step α: Heat Treatment of Sintered Member) In step α, the sintered member 1 is carburized, quenched, and tempered. By step α, the mechanical properties of the sintered member 1, particularly hardness and toughness, tend to be improved.

[0049] (Step β: Finishing of Sintered Member) In step β, the surface roughness of the sintered member 1 is reduced and the dimensions of the sintered member 1 are adjusted to the design dimensions. An example of the finishing process is polishing the surface of the sintered member 1.

[0050] Test Example 1 In Test Example 1, a sintered member having a hole was manufactured, and the relationship between the diameter x1 and depth y1 of the hole was evaluated.

[0051] [Samples No. 1 to No. 7] The sintered members of Samples No. 1 to No. 7 were manufactured by carrying out the above steps A to D in the same manner as in the manufacturing method of the sintered member of the above embodiment.

[0052] [Step A] In step A, a raw material powder containing stainless steel powder and a lubricant was prepared. The stainless steel powder had a composition of 16 mass% Cr and 12 mass% Ni, with the remainder being Fe and unavoidable impurities. The lubricant was stearic acid. The melting point of stearic acid is 69.3°C. The proportion of the lubricant contained in the raw material powder was 0.1 mass%.

[0053] [Step B] In step B, the raw material powder was pressed to produce a powder compact. The compacting pressure was 1960 MPa.

[0054] The relative density of the produced powder compact was 99.5%, which was calculated by [(density of actual powder compact / true density of powder compact)×100] as described above.

[0055] [Step C] In step C, a processed body having a hole was fabricated by drilling the powder compact. The diameter x1 of the hole formed in Sample No. 1 to Sample No. 7 was 0.05 mm, 0.08 mm, 0.1 mm, 0.3 mm, 0.8 mm, 1.5 mm, and 2.0 mm, respectively.

[0056] The hole diameter x1 was varied by changing the diameter of the drill. Hole processing was performed using minimum quantity lubrication (MQL) processing, which involves supplying a very small amount of cutting fluid together with a large amount of compressed gas. When forming holes with diameters of 0.05 mm, 0.08 mm, 0.1 mm, 0.3 mm, or 0.8 mm, the cutting fluid was supplied using an external lubrication method. When forming holes with diameters of 1.5 mm or 2.0 mm, the cutting fluid was supplied using an internal lubrication method.

[0057] The machining conditions for each sample are as shown in Table 1. The holes in each sample were formed by step machining. Step machining is a process in which holes are formed by alternately advancing and retreating the drill. The step width in Table 1 refers to the depth of the hole drilled by one advance of the drill. For example, a step width of 2 mm in Table 1 refers to the following procedure: The drill is advanced to machine the powder compact until the tip of the drill reaches a point 2 mm deep from the surface of the powder compact. The drill is retracted until the tip of the drill reaches the surface of the powder compact from the bottom of the hole, or reaches a point behind the surface of the powder compact from the bottom of the hole. Next, the drill is advanced to machine the powder compact until the tip of the drill reaches a point 2 mm deep from the bottom of the hole. Next, the drill is retracted until the tip of the drill reaches the surface of the powder compact from the bottom of the hole, or reaches a point behind the surface of the powder compact from the bottom of the hole. In this manner, the advancement and retreat of the drill are alternately repeated. The number of steps is the number of times the drill is advanced and retracted until it reaches depth y1. That is, if the step width is 2 mm and the depth y1 is 70 mm, the number of steps is 70 divided by 2, or 35. The values ​​shown in the column for the relationship between diameter x1 and step width were obtained by dividing diameter x1 by the step width. The values ​​shown in the column for the relationship between diameter x1 and feed rate were obtained by dividing the feed rate by diameter x1.

[0058]

[0059] Graphs showing the relationship between hole diameter x1 and depth y1 for Samples No. 1 to No. 7 are shown in Figures 5 to 7. Figure 6 is an enlarged graph of region A in Figure 5. Figure 7 is an enlarged graph of region B in Figure 6. The horizontal axis of the graphs in Figures 5 to 7 represents hole diameter x1 (mm). The vertical axis of the graphs in Figures 5 to 7 represents hole depth y1 (mm). In the graphs in Figures 5 to 7, the results for Samples No. 1 to No. 7 are indicated by circles.

[0060] In sample No. 1, a hole having a diameter x1 of 0.05 mm and a depth y1 of 0.4 mm was formed. In sample No. 2, a hole having a diameter x1 of 0.08 mm and a depth y1 of 0.8 mm was formed. In sample No. 3, a hole having a diameter x1 of 0.1 mm and a depth y1 of 3.3 mm was formed. In sample No. 4, a hole having a diameter x1 of 0.3 mm and a depth y1 of 6.0 mm was formed. In sample No. 5, a hole having a diameter x1 of 0.8 mm and a depth y1 of 15.0 mm was formed. In sample No. 6, a hole having a diameter x1 of 1.5 mm and a depth y1 of 50.0 mm was formed. In sample No. 7, a hole having a diameter x1 of 2.0 mm and a depth y1 of 70.0 mm was formed. In each sample, 20 of the above holes could be formed in succession.

[0061] [Step D] In step D, a workpiece having a hole was heated to remove the lubricant, and the workpiece from which the lubricant had been removed was sintered to produce a sintered component. The lubricant was removed from the workpiece by increasing the temperature from 100°C to 250°C. The workpiece from which the lubricant had been removed was held at 1100°C for 60 minutes. The sintering atmosphere was a vacuum atmosphere.

[0062] The relative density of the sintered components was 96.2%. The relative density of the green compact was calculated as described above by [(actual density of sintered component / true density of sintered component) × 100]. For each sample, the diameter x1 and depth y1 of the hole in the sintered component were substantially the same as the diameter x1 and depth y1 of the hole in the processed body.

[0063] [Samples No. 101 to 108] Sintered members No. 101 to 107 were produced in the same manner as samples No. 1 to 7, respectively, except that no lubricant was used in step A. Sintered member No. 108 was produced in the same manner as sample No. 107, except that the diameter x1 of the hole formed in step C was 3.0 mm.

[0064] The graphs in Figures 5 to 7 also show the relationship between the hole diameter x1 and the depth y1 for Samples No. 101 to 108. In the graphs in Figures 5 to 7, the results for Samples No. 101 to 108 are indicated by triangles.

[0065] The hole diameter x1 of Sample No. 101 was 0.05 mm, and the limit of the hole depth y1 was 0.35 mm. The hole diameter x1 of Sample No. 102 was 0.08 mm, and the limit of the hole depth y1 was 0.43 mm. The hole diameter x1 of Sample No. 103 was 0.1 mm, and the limit of the hole depth y1 was 1.0 mm. The hole diameter x1 of Sample No. 104 was 0.3 mm, and the limit of the hole depth y1 was 3.0 mm. The hole diameter x1 of Sample No. 105 was 0.8 mm, and the limit of the hole depth y1 was 7.0 mm. The hole diameter x1 of Sample No. 106 was 1.5 mm, and the limit of the hole depth y1 was 30.0 mm. The diameter x1 of the hole of Sample No. 107 was 2.0 mm, and the limit of the depth y1 of the hole was 40.0 mm. The diameter x1 of the hole of Sample No. 108 was 3.0 mm, and the limit of the depth y1 of the hole was 50.0 mm. The limit of the depth y1 here refers to the limit of the depth that can be drilled at the diameter x1 without the drill breaking.

[0066] [Evaluation] Samples No. 1 to No. 7 and Samples No. 101 to No. 107 having the same hole diameter x1 were compared. As shown in Figures 5 to 7 , it can be seen that regardless of the diameter x1, the depth y1 of each of Samples No. 1 to No. 7 was greater than the depth y1 of each of Samples No. 101 to No. 107.

[0067] The line L1 connecting the points for sample No. 101 and the points for sample No. 102 shown in FIG. 7 is y1 = 2.67x1 + 0.217. The slope and intercept values ​​are rounded. The line L2 connecting the points for sample No. 102 and the points for sample No. 103 shown in FIG. 6 is y1 = 28.5x1 - 1.85. The line L3 connecting the points for sample No. 103 shown in FIG. 6 and the points for sample No. 104 shown in FIG. 5 is y1 = 10x1. The line L4 connecting the points for sample No. 104 and the points for sample No. 105 shown in FIG. 5 is y1 = 8x1 + 0.6. The line L5 connecting the points for sample No. 105 and the points for sample No. 106 shown in FIG. 5 is y1 = 32.9x1 - 19.3. The values ​​of the slope and intercept are rounded. The line L6 connecting the points of sample No. 106 and sample No. 107 shown in Figure 5 has a value of y1 = 20x1. The line L7 connecting the points of sample No. 107 and sample No. 108 shown in Figure 5 has a value of y1 = 10x1 + 20.

[0068] It can be seen that a sintered component having a hole manufactured using a raw material powder containing a lubricant with a melting point of 150°C or less satisfies the following requirements (a1) to (a7): (a1) y1 > 2.67x1 + 0.217 in the range of 0.05≦x1<0.08 (a2) y1 > 28.5x1 - 1.85 in the range of 0.08≦x1<0.1 (a3) ​​y1 > 10x1 in the range of 0.1≦x1<0.3 (a4) y1 > 8x1 + 0.6 in the range of 0.3≦x1<0.8 (a5) y1 > 32.9x1 - 19.3 in the range of 0.8≦x1<1.5 (a6) y1 > 20x1 in the range of 1.5≦x1<2.0 (a7) y1 > 10x1 + 20 in the range of 2.0≦x1

[0069] The line L8 connecting the points for sample No. 1 and the points for sample No. 2 shown in FIG. 7 is y1 = 13.3x1 + 0.267. The slope and intercept values ​​are rounded. The line L9 connecting the points for sample No. 2 and the points for sample No. 3 shown in FIG. 6 is y1 = 125x1 - 9.2. The slope and intercept values ​​are rounded. The line L10 connecting the points for sample No. 3 shown in FIG. 6 and the points for sample No. 4 shown in FIG. 5 is y1 = 13.5x1 + 1.95. The line L11 connecting the points for sample No. 4 and the points for sample No. 5 shown in FIG. 5 is y1 = 18x1 + 0.6. The line L12 connecting the points for sample No. 5 and the points for sample No. 6 shown in FIG. 5 is y1 = 50x1 - 25. The line L13 connecting the points for sample No. 3 shown in FIG. 6 and the points for sample No. 4 shown in FIG. 5 is y1 = 13.5x1 + 1.95. The line L11 connecting the points for sample No. 4 and the points for sample No. 5 shown in FIG. 5 is y1 = 18x1 + 0.6. The line L12 connecting the points for sample No. 5 and the points for sample No. 6 shown in FIG. 5 is y1 = 50x1 - 25. The line L13 connecting the point of sample No. 6 and the point of sample No. 7 has an equation of y1 = 40x1 - 10. The line L14 passing through sample No. 7 shown in Figure 5 and parallel to the line L7 has an equation of y1 = 10x1 + 50.

[0070] It can be seen that a sintered member having a hole manufactured using a raw material powder containing a lubricant having a melting point of 150° C. or less also satisfies the following requirements (a51) to (a56). (a51) For 0.05≦x1<0.08, y1 = 13.3x1 + 0.267. (a52) For 0.08≦x1<0.1, y1 = 125x1 - 9.2. (a53) For 0.1≦x1<0.3, y1 = 13.5x1 + 1.95. (a54) For 0.3≦x1<0.8, y1 = 18x1 + 0.6. (a55) For 0.8≦x1<1.5, y1 = 50x1 - 25. (a56) For 1.5≦x1<2.0, y1 = 40x1 - 10. (a57) For 2.0≦x1, y1 = 10x1 + 50.

[0071] Test Example 2 In Test Example 2, a sintered member having a groove was produced, and the relationship between the width x2 and depth y2 of the groove was evaluated.

[0072] [Samples No. 21 to 25] Sintered members No. 21 to 25 were produced in the same manner as Sample No. 1, except that in step C, grooves were formed in the powder compact to produce processed bodies having grooves.

[0073] [Step C] The width x2 of the grooves formed in Samples No. 21 to 25 was 0.05 mm, 0.1 mm, 0.2 mm, 0.3 mm, and 0.5 mm, respectively. Grooves with a width x2 of 0.05 mm or 0.1 mm were formed using a dicing blade. Grooves with a width x2 of 0.2 mm, 0.3 mm, and 0.5 mm were formed using a metal saw.

[0074] Graphs showing the relationship between groove width x2 and depth y2 for Samples No. 21 to 25 are shown in Figures 8 and 9. Figure 9 is an enlarged graph of region C in Figure 8. The horizontal axis of the graphs in Figures 8 and 9 represents groove width x2 (mm). The vertical axis of the graphs in Figures 8 and 9 represents groove depth y2 (mm). In the graphs in Figures 8 and 9, the results for Samples No. 21 to 25 are indicated by circles.

[0075] In sample No. 21, grooves having a width x2 of 0.05 mm and a depth y2 of 0.7 mm were formed. In sample No. 22, grooves having a width x2 of 0.1 mm and a depth y2 of 1.0 mm were formed. In sample No. 23, grooves having a width x2 of 0.2 mm and a depth y2 of 1.6 mm were formed. In sample No. 24, grooves having a width x2 of 0.3 mm and a depth y2 of 9.0 mm were formed. In sample No. 25, grooves having a width x2 of 0.5 mm and a depth y2 of 19.0 mm were formed.

[0076] [Samples No. 201 to 207] Sintered members No. 201 to No. 205 were produced in the same manner as samples No. 21 to 25, respectively, except that no lubricant was used in step A. Sintered members No. 206 and No. 207 were produced in the same manner as sample No. 205, respectively, except that the width x2 of the groove formed in step C was set to 1.5 mm and 3.0 mm, respectively. The grooves with width x2 of 1.5 mm and 3.0 mm were formed using a grooving tool.

[0077] The graphs in Figures 8 and 9 also show the relationship between the width x2 and depth y2 of the grooves for Samples No. 201 to 207. In the graphs in Figures 8 and 9, the results for Samples No. 201 to 207 are indicated by triangles.

[0078] The groove width x2 of Sample No. 201 was 0.05 mm, and the limit of the groove depth y2 was 0.65 mm. The groove width x2 of Sample No. 202 was 0.1 mm, and the limit of the groove depth y2 was 0.9 mm. The groove width x2 of Sample No. 203 was 0.2 mm, and the limit of the groove depth y2 was 1.4 mm. The groove width x2 of Sample No. 204 was 0.3 mm, and the limit of the groove depth y2 was 3.0 mm. The groove width x2 of Sample No. 205 was 0.5 mm, and the limit of the groove depth y2 was 10.0 mm. The groove width x2 of Sample No. 206 was 1.5 mm, and the limit of the groove depth y2 was 15.0 mm. The width x2 of the groove 207 was 3.0 mm, and the limit of the depth y2 of the groove was 25.0 mm. The limit of the depth y2 here refers to the limit of the depth that can be machined at the width x2 without the tool breaking.

[0079] [Evaluation] Samples No. 21 to No. 25 and Samples No. 201 to No. 205, which have the same groove width x2, were compared. As shown in Figures 8 and 9, it can be seen that regardless of the width x2, the depth y2 of each of Samples No. 21 to No. 25 was greater than the depth y2 of each of Samples No. 201 to No. 205.

[0080] The line L21 connecting the points for sample No. 201 and sample No. 203 shown in Figure 9 has a value of y2 = 5x2 + 0.4. The line L222 connecting the points for sample No. 203 shown in Figure 9 and sample No. 205 shown in Figure 8 has a value of y2 = 28.7x2 - 4.3. The values ​​of the slope and intercept are rounded. The line L23 connecting the points for sample No. 205 and sample No. 207 shown in Figure 8 has a value of y2 = 6x2 + 7.

[0081] It can be seen that a sintered member having grooves manufactured using raw material powder containing a lubricant with a melting point of 150°C or less satisfies the following requirements (b1) to (b3): ​​(b1) y2>5x2+0.4 in the case of 0.05≦x2<0.2 (b2) y2>28.7x2-4.3 in the case of 0.2≦x2<0.5 (b3) y2>6x2+7 in the case of 0.5≦x2

[0082] The line L24 connecting the points of sample No. 21, sample No. 22, and sample No. 23 shown in Figure 9 has an equation of y2 = 6x2 + 0.4. The line L25 connecting the points of sample No. 23 shown in Figure 9 and the points of sample No. 24 shown in Figure 8 has an equation of y2 = 74x2 - 13.2. The line L26 connecting the points of sample No. 24 and sample No. 25 shown in Figure 8 has an equation of y2 = 50x2 - 6. The line L27 passing through sample No. 25 shown in Figure 8 and parallel to line L23 has an equation of y2 = 6x2 + 16.

[0083] It can be seen that a sintered member having grooves manufactured using raw material powder containing a lubricant with a melting point of 150°C or less satisfies the following requirements (b51) to (b54): (b51) y2 = 6x2 + 0.4 in the range of 0.05≦x2<0.2 (b52) y2 = 74x2 - 13.2 in the range of 0.2≦x2<0.3 (b53) y2 = 50x2 - 6 in the range of 0.3≦x2<0.5 (b54) y2 = 6x2 + 16 in the range of 0.5≦x2

[0084] Test Example 3 In Test Example 3, the number of holes that can be formed with the same drill was evaluated.

[0085] [Samples No. 31 to 34, Samples No. 301 to 304] Sintered members No. 31 to No. 34 were produced in the same manner as Sample No. 1, except that the diameter of the hole formed in the powder compact in Step C was different. Sintered members No. 301 to No. 304 were produced in the same manner as Sample No. 31 to No. 34, except that no lubricant was used in Step A.

[0086] [Process C] The diameters of the holes formed in Samples No. 31 to No. 34 were 0.4 mm, 0.6 mm, 0.8 mm, and 1.0 mm, respectively. The diameters of the holes formed in Samples No. 301 to No. 304 were 0.4 mm, 0.6 mm, 0.8 mm, and 1.0 mm, respectively. When forming holes with a diameter of 0.4 mm or 0.6 mm, the cutting fluid was supplied by an external coolant supply method. When forming holes with a diameter of 0.8 mm or 1.0 mm, the cutting fluid was supplied by an internal coolant supply method. The depths of the holes formed in each sample were the same.

[0087] [Evaluation] For each sample, the number of holes formed with the same drill was counted. Drilling was stopped when the number of holes formed reached 20. A value less than 20 indicates the number of holes formed without the drill breaking.

[0088] In sample No. 31, 20 holes with a diameter of 0.4 mm were formed. In sample No. 32, 20 holes with a diameter of 0.6 mm were formed. In sample No. 33, 20 holes with a diameter of 0.8 mm were formed. In sample No. 34, 20 holes with a diameter of 1.0 mm were formed.

[0089] In sample No. 301, the number of holes that were able to be formed was 0 with a diameter of 0.4 mm. In sample No. 302, the number of holes that were able to be formed was 1 with a diameter of 0.6 mm. In sample No. 303, the number of holes that were able to be formed was 8 with a diameter of 0.8 mm. In sample No. 304, the number of holes that were able to be formed was 18 with a diameter of 1.0 mm.

[0090] A comparison was made between samples No. 31 to No. 34 and samples No. 301 to No. 304, which have the same hole diameter. It was found that the smaller the diameter of the formed holes, the greater the number of holes that can be formed when the raw material powder contains a lubricant with a melting point of 150°C or less, compared to when the raw material powder does not contain a lubricant with a melting point of more than 150°C.

[0091] Test Example 4 In Test Example 4, a drill with a particularly long flute length was prepared, and the upper limit of the hole depth was evaluated.

[0092] [Samples No. 41 to No. 44] The sintered members of each sample were produced in the same manner as Sample No. 1, except that the processing conditions in Step C were as shown in Table 2.

[0093] [Step C] For sample No. 41, a drill having a flute length L of 30 mm, a diameter D of 0.6 mm, and an L / D ratio of 50 was used to form the hole. For sample No. 42, a drill having a flute length L of 40 mm, a diameter D of 0.8 mm, and an L / D ratio of 50 was used to form the hole. For sample No. 43, a drill having a flute length L of 40 mm, a diameter D of 1.0 mm, and an L / D ratio of 40 was used to form the hole. For sample No. 44, a drill having a flute length L of 50 mm, a diameter D of 1.0 mm, and an L / D ratio of 50 was used to form the hole. In the graph of Figure 5, the results for samples No. 41 to No. 44 are indicated by circles.

[0094]

[0095] [Evaluation] For each sample, 320 holes were continuously formed using the same drill. No drill breakage or other processing problems occurred during the hole formation process. From these results, it can be inferred that the upper limit of hole depth y1 is determined by the constraint of whether or not a drill tool is available. At least, it was confirmed that holes with y1 / x1 ≥ 50 can be obtained within the demonstrated range. From these results, it is believed that if a drill can be obtained, holes with y1 / x1 = 60, even y1 / x1 = 80, and especially y1 / x1 = 100 can be formed.

[0096] The line L40 connecting the points of sample No. 41, sample No. 42, and sample No. 44 shown in Figure 5 is y1 = 50x1. Combining the results of Test Example 1 and Test Example 4, when the upper limit is set to y1 / x1 = 50, the following results are obtained: (a3) ​​50x1 ≧ y1 > 10x1 for 0.1 ≦ x1 < 0.3 (a4) 50x1 ≧ y1 > 8x1 + 0.6 for 0.3 ≦ x1 < 0.8 (a5) 50x1 ≧ y1 > 32.9x1 - 19.3 for 0.8 ≦ x1 < 1.5 (a6) 50x1 ≧ y1 > 20x1 for 1.5 ≦ x1 < 2.0

[0097] Combining the results of Test Example 1 and Test Example 4, when the upper limit is set to y1 / x1 = 80, the results are as follows: (a3) ​​80x1 ≧ y1 > 10x1 in the case of 0.1 ≦ x1 < 0.3 (a4) 80x1 ≧ y1 > 8x1 + 0.6 in the case of 0.3 ≦ x1 < 0.8 (a5) 80x1 ≧ y1 > 32.9x1 - 19.3 in the case of 0.8 ≦ x1 < 1.5 (a6) 80x1 ≧ y1 > 20x1 in the case of 1.5 ≦ x1 < 2.0

[0098] The results of Test Examples 1 and 4 revealed the following: A hole having a depth y1 greater than the diameter x1 is easily formed by step machining. The upper limit of the number of steps is not particularly limited, and it may be set to a number that does not make the machining time too long. The smaller the diameter x1, the smaller the step width should be. For example, the step width should be equal to or less than the diameter x1. The step width may be equal to or less than 1 / 2 the diameter x1, or even equal to or less than 1 / 5 the diameter x1. The feed rate should be equal to or less than 250 times the diameter x1.

[0099] The present invention is not limited to these examples, but is defined by the scope of the claims, and is intended to include all modifications within the meaning and scope equivalent to the claims.

[0100] In relation to the above-described embodiments of the present invention, the following supplementary notes are further disclosed.

[0101] [Appendix 1] A sintered component made of metal, having a relative density of 95% or more, and having a hole portion whose diameter x1 (mm) and depth y1 (mm) satisfy the following requirements (α1) to (α4): (α1) 50x1≧y1≧10x1+2 for 0.1≦x1<0.3 (α2) 50x1≧y1≧20x1-1 for 0.3≦x1<0.8 (α3) 50x1≧y1≧50x1-25 for 0.8≦x1<1.5 (α4) 50x1≧y1≧40x1-10 for 1.5≦x1<2.0

[0102] The sintered member of Supplementary Note 1 has a hole whose depth is large relative to its diameter.

[0103] 1 Sintered member 2 Hole portion 3 Groove portion x1 Diameter y1 Depth x2 Width y2 Depth A, B, C Regions L1, L2, L3, L4, L5, L6, L7 Straight line L8, L9, L10, L11, L12, L13, L14 Straight line L21, L22, L23 Straight line L24, L25, L26, L27 Straight line

Claims

1. A sintered member made of a metal, The relative density is 95% or more, The diameter x1 (mm) and the depth y1 (mm) of the hole portion satisfy the following requirements (a1) to (a7). Sintered parts. (a1) In the range of 0.05≦x1<0.08, y1>2.67x1+0.217 (a2) In the range of 0.08≦x1<0.1, y1>28.5x1−1.85 (a3) 0.1≦x1<0.3, y1>10x1 (a4) In the range of 0.3≦x1<0.8, y1>8x1+0.6 (a5) In the range of 0.8≦x1<1.5, y1>32.9x1−19.3 (a6) 1.5≦x1<2.0, y1>20x1 (a7) y1>10x1+20 in the range of 2.0≦x1

2. A sintered member made of a metal, The relative density is 95% or more, The groove portion has a width x2 (mm) and a depth y2 (mm) that satisfy the following requirements (b1) to (b3). Sintered parts. (b1) 0.05≦x2<0.2, y2>5x2+0.4 (b2) In the range of 0.2≦x2<0.5, y2>28.7x2−4.3 (b3) In the range of 0.5≦x2, y2>6x2+7

3. 3. The sintered component according to claim 1 or 2, wherein the metal is pure iron or an iron alloy.

4. The sintered member according to claim 1 or 2, wherein the metal is stainless steel.

5. 3. The sintered member according to claim 1, having a relative density of 97% or more.

6. preparing a raw material powder including a metal powder and a lubricant; a step of compressing the raw material powder to produce a green compact having a relative density of 95% or more; a step of producing a processed body having a hole portion whose diameter x1 (mm) and depth y1 (mm) satisfy the following requirements (a1) to (a7) by subjecting the powder compact to hole processing; and sintering the processed body. The ratio of the lubricant contained in the raw material powder is 0.025% by mass or more and 0.2% by mass or less, The melting point of the lubricant is 150° C. or less. A method for manufacturing a sintered part. (a1) In the range of 0.05≦x1<0.08, y1>2.67x1+0.217 (a2) In the range of 0.08≦x1<0.1, y1>28.5x1−1.85 (a3) 0.1≦x1<0.3, y1>10x1 (a4) In the range of 0.3≦x1<0.8, y1>8x1+0.6 (a5) In the range of 0.8≦x1<1.5, y1>32.9x1−19.3 (a6) 1.5≦x1<2.0, y1>20x1 (a7) y1>10x1+20 in the range of 2.0≦x1

7. preparing a raw material powder including a metal powder and a lubricant; a step of compressing the raw material powder to produce a green compact having a relative density of 95% or more; a step of producing a processed body having a groove portion whose width x2 (mm) and depth y2 (mm) satisfy the following requirements (b1) to (b3) by performing groove processing on the powder molded body; and sintering the processed body. The ratio of the lubricant contained in the raw material powder is 0.025% by mass or more and 0.2% by mass or less, The melting point of the lubricant is 150° C. or less. A method for manufacturing a sintered part. (b1) 0.05≦x2<0.2, y2>5x2+0.4 (b2) In the range of 0.2≦x2<0.5, y2>28.7x2−4.3 (b3) In the range of 0.5≦x2, y2>6x2+7

8. The method for producing a sintered member according to claim 6, wherein the hole machining is a step machining.

9. The method for producing a sintered member according to claim 6 , wherein the lubricant is stearic acid, erucic acid amide, or stearic acid amide.