Adsorption member and method for producing same

JPWO2023286741A5Active Publication Date: 2024-11-19KYOCERA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023534796
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-07-11
Filing Date
2022-07-11
Publication Date
2024-11-19
Estimated Expiration
2042-07-11

AI Technical Summary

Technical Problem

Conventional adsorption members, such as vacuum chucks and electrostatic chucks, face issues with particles adhering to the object being processed due to friction and external disturbances, which can lead to re-adhesion from scratches and pores, causing surface contamination and deformation.

Method used

An adsorption member with a ceramic substrate containing silicon carbide as the main component, featuring independent protrusions with a tantalum film coating, designed to minimize contact between the object and the substrate, reducing particle adherence and static electricity, and incorporating a mounting surface with a low open pore area and specific thermal expansion properties to prevent film peeling or cracking.

Benefits of technology

The solution effectively reduces particle adherence and static electricity, maintains the flatness of the mounting surface, and enhances heat dissipation, ensuring minimal deformation and contamination of the object being processed.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

An adsorption member according to the present disclosure is provided with a substrate which is formed of a ceramic that is mainly composed of silicon carbide and a plurality of projected parts which are formed on the surface of the substrate; each of the projected parts comprises a stage part that has a stage surface on which an object to be processed is to be placed, and a support part that supports the stage part; the stage part is formed of a film which is mainly composed of at least one substance that is selected from among silicon carbide, diamond-like carbon, amorphous silicon, molybdenum, chromium and tantalum; and respective films of the projected parts are independent from each other.
Need to check novelty before this filing date? Find Prior Art

Description

Adsorption member and manufacturing method thereof

[0001] The present disclosure relates to an attraction member, such as a vacuum chuck or electrostatic chuck, for holding an object to be processed, such as a semiconductor wafer, and a method for manufacturing the same.

[0002] Conventionally, a workpiece such as a semiconductor wafer is held on an attraction member such as a vacuum chuck or an electrostatic chuck in a manufacturing device or an inspection device. When the workpiece is placed on the mounting surface of the attraction member, particles generated by friction between the back surface of the workpiece and the mounting surface of the attraction member may adhere to the workpiece, or particles that have entered scratches, pores, etc. on the mounting surface of the attraction member may sporadically re-adhere to the workpiece due to disturbances such as vibrations.

[0003] In order to solve this problem, in Patent Document 1, yttria (Y 2 O 3 A stage on which a yttria (Y) film is formed has been proposed. 2 O 3 ) membrane is Y 2 O 3 It is described that the sintered body has a large number of protrusions consisting of

[0004] JP 2015-23168 A

[0005] The adsorption member of the present disclosure comprises a substrate made of ceramic containing silicon carbide as a main component, and a plurality of protrusions formed on the surface of the substrate, the protrusions having a mounting portion with a mounting surface for placing an object to be treated on it and a support portion for supporting the mounting portion, the mounting portion being made of a film containing at least one material selected from silicon carbide, diamond-like carbon (hereinafter referred to as DLC), amorphous silicon, molybdenum, chromium, and tantalum as a main component, and the film is independent of each other for each protrusion.

[0006] The method for manufacturing the adsorption member of the present disclosure includes the following steps, performed in the following order: (1) forming recesses and protrusions, which are the remainders of the recesses, on the surface of a substrate made of ceramics containing silicon carbide as a main component, (2) coating the recesses and protrusions with a film containing at least one material selected from silicon carbide, DLC, amorphous silicon, molybdenum, chromium, and tantalum as a main component, (3) subjecting the film to at least one of grinding and polishing until the top surfaces of the protrusions are exposed, thereby dividing the film, and (4) removing the protrusions to obtain an adsorption member comprising a substrate and protrusions.

[0007] The present disclosure provides a processing device and an inspection device that use the above-described suction member.

[0008] Fig. 1 is a partially broken perspective view schematically illustrating one embodiment of an adsorption member of the present disclosure. Fig. 2 is an enlarged cross-sectional view of part A of Fig. 1. Fig. 3 is a cross-sectional view showing another example of a protrusion according to the present disclosure. Fig. 4 is a cross-sectional view showing another example of a protrusion according to the present disclosure. Fig. 5 is a cross-sectional view showing yet another example of a protrusion according to the present disclosure. Fig. 6 is a cross-sectional view showing yet another example of a protrusion according to the present disclosure. Fig. 7 is a process explanatory diagram showing a method for manufacturing an adsorption member of the present disclosure.

[0009] An adsorption member according to an embodiment of the present disclosure will now be described. Fig. 1 schematically shows an adsorption member 10 according to this embodiment.

[0010] The adsorption member 10 has a plurality of protrusions 2 formed on the upper surface (surface) of a disk-shaped substrate 1. Figure 2 is an enlarged cross-sectional view of portion A in Figure 1. The protrusions 2 are frustum-shaped, such as a truncated cone or a truncated triangular pyramid, and include a mounting portion 21 having a mounting surface 3 for mounting a workpiece (not shown) thereon, and a support portion 22 for supporting the mounting portion 21. The protrusions 2 are not limited to a truncated cone shape, and may be cylindrical, conical, triangular pyramidal, or the like. In particular, the protrusions 2 are preferably frustum-shaped, because this shape facilitates rapid heat dissipation toward the substrate 1 even if the temperature of the workpiece rises.

[0011] The substrate 1 is the main body of the adsorption member 10 and is required to have the property of preventing deformation of the object to be treated placed thereon. Therefore, the substrate 1 preferably has high rigidity, hardness, and strength. Examples of materials for the substrate 1 include ceramics primarily composed of silicon carbide. That is, the substrate 1 is a silicon carbide sintered body primarily composed of silicon carbide (more than 50% by mass). Such silicon carbide sintered bodies have high thermal conductivity and excellent heat dissipation properties, resulting in little temperature change of the object to be treated. Furthermore, since silicon carbide sintered bodies are electrically conductive (semiconductive), they have advantages such as less static electricity generation and less electrostatic adhesion of particles. In particular, the silicon carbide content is preferably 80% by mass or more out of a total of 100% by mass of the components constituting the ceramic. Other components constituting the ceramic include, for example, boron carbide. The components constituting the ceramic can be identified using an X-ray diffraction (XRD) device using CuKα radiation. The content of each component can be determined by identifying the component, then determining the content of the elements that make up the component using an X-ray fluorescence analyzer (XRF) or an ICP optical emission spectrometer, and converting the content into the identified component.

[0012] The protrusions 2 are formed on the surface of the substrate 1 and adsorb and support the object to be processed. The object to be processed is supported by the plurality of protrusions 2 to prevent contact between the object to be processed and the substrate 1. By adsorbing and supporting the object to be processed by the protrusions 2, fewer particles are trapped between the object to be processed and the mounting surface 3 than when the object to be processed is adsorbed and supported directly by the substrate 1, and the flatness of the object to be processed is less likely to deteriorate.

[0013] The support portion 22 constituting the protrusion portion 2 is made of ceramics having the same main component as the substrate 1, is formed integrally with the substrate 1, and is a frustum-shaped protrusion provided on the upper surface of the substrate 1. The mounting portion 21 is formed on the upper surface of the support portion 22.

[0014] The mounting portion 21 is provided to prevent particles trapped in scratches or minute irregularities on the surface of the substrate 1, or particles attached to the surface of the support portion 2, from floating due to external forces such as vibration and adhering to the workpiece. Therefore, the mounting portion 21 is required to have a dense surface with minimal irregularities. The mounting portion 21 is required to have, for example, a film 4 that can form a smooth surface and to be able to form a film without peeling or cracking of the film 4. In particular, if the difference in thermal expansion coefficient between the support portion 22 and the mounting portion 21 is large, peeling or cracking will occur in the mounting portion 21 during film formation, preventing good film formation. Therefore, it is important to minimize the difference in thermal expansion coefficient between the support portion 22 and the mounting portion 21. It is preferable that the mounting surface 3 have few open pores; for example, the area occupancy rate of open pores on the mounting surface 3 should be 0.5% or less, particularly 0.2% or less.

[0015] To determine the area occupancy rate of open pores, first select a portion where the size and distribution of open pores are observed on average. For example, select a portion with an area of ​​3.84 × 10 -2 mm 2 An observation image of the area (horizontal length 0.226 mm, vertical length 0.170 mm) is taken with a scanning electron microscope at a magnification of 500x. This observation image is then analyzed by a particle analysis technique using image analysis software "A-zo-kun (ver. 2.52)" (registered trademark, manufactured by Asahi Kasei Engineering Co., Ltd.; in the following description, the image analysis software "A-zo-kun" refers to the image analysis software manufactured by Asahi Kasei Engineering Co., Ltd.), to determine the average circle-equivalent diameter of the open pores. The particle analysis setting conditions are, for example, a threshold value indicating the brightness of the image of 83, brightness of dark, and a small figure removal area of ​​0.2 μm. 2 In the above measurement, the threshold value was set to 83, but the threshold value can be adjusted according to the brightness of the observed image. The brightness was set to dark, the binarization method was set to manual, and the small figure removal area was set to 0.2 μm 2 With the noise reduction filter enabled, the threshold value can be manually adjusted so that the markers in the observed image, whose size changes depending on the threshold value, match the shape of the open pores.

[0016] The mounting portion 21 is made of a film 4 containing at least one material selected from silicon carbide, diamond-like carbon, amorphous silicon, molybdenum, chromium, and tantalum as its main component. The mounting portion 21, which includes the film 4, has a small difference in thermal expansion coefficient from the support portion 22. The high thermal conductivity of these main components facilitates heat dissipation when adsorbing a workpiece. Furthermore, a film with almost no open pores is obtained, making it difficult for particles to adhere to the mounting surface 3. Furthermore, static electricity accumulated on the mounting surface 3 can be released, reducing particle adhesion. When the film 4 is primarily composed of silicon carbide, diamond-like carbon, or amorphous silicon, these main components have high rigidity, reducing deformation of the film 4. On the other hand, when the film 4 is primarily composed of molybdenum, chromium, or tantalum, these main components have low rigidity, making the film 4 more likely to follow the microscopic behavior of the adsorbed object in the planar direction. Film 4 containing these metals as its main component includes a film made of a molybdenum alloy, a chromium alloy, or a tantalum alloy. The main component of film 4 refers to a component that accounts for 90 mass% or more of a total of 100 mass% of the components that make up film 4. The components that make up film 4 can be identified using a thin film X-ray diffraction device, and the content of each component can be determined using the Rietveld method.

[0017] When the film 4 is mainly composed of silicon, the crystal structure can be examined using a thin film X-ray diffraction device. If the half-width of the silicon peak appearing around a diffraction angle (2θ) of 28° is 1.0° or more, the silicon crystal structure is amorphous. When the film 4 is mainly composed of diamond-like carbon, it can also be identified using a Raman spectrometer. In this case, the peak intensity I of the G band in the Raman spectrum obtained by the Raman spectrometer is G D-Band I D Ratio of peak intensities I D / I G , for example, 0.7 or more and 1.3 or less.

[0018] The films 4 are independent from each other for each protrusion 2. Being independent from each other means that the films 4 are divided into sections for each protrusion 2. This reduces residual strain in the film 4 compared to when the film 4 covers the entire surface of the substrate 1 and the outer circumferential surface of the protrusion 2, making it less likely that the flatness of the mounting surface 3 will be impaired by thermal deformation or the like. The film 4 may extend toward the outer circumferential surface of the support 22 and cover at least a portion of the outer circumferential surface of the support 22. In this case, particle shedding from the outer circumferential surface of the support 22 is reduced, and particles floating and adhering to the adsorbate can be reduced.

[0019] The thickness of the film 4 is preferably 30 μm or more and 400 μm or less. Since the specific heat capacity of the film 4 is small, the flatness of the mounting surface 3, which is the top of the multiple protrusions 2, is not impaired. In particular, the thickness of the film 4 is preferably 50 μm or more and 200 μm or less.

[0020] The surface of the substrate 1 preferably has a larger average value of the cut level difference (Rδc), which represents the difference between the cut level at a load length ratio of 25% on the roughness curve and the cut level at a load length ratio of 75% on the roughness curve, than the mounting surface 3. This reduces the risk of the reaction products adhering to the surface of the substrate 1 and re-floating even when the workpiece is adsorbed to an adsorption member installed in the plasma processing apparatus and the reaction products generated by the plasma processing float. The mounting surface 3 has fewer irregularities, making it less likely to scratch the backside of the workpiece. Specifically, the difference in the average value of the cut level difference (Rδc) between the surface of the substrate 1 and the mounting surface 3 is preferably 0.38 μm or more. Here, the average value of the cut level difference (Rδc) on the surface of the substrate 1 is preferably 1.4 μm or less. This reduces the likelihood of large particles detaching from the surface of the substrate 1 and reducing the risk of these particles adhering to the workpiece.

[0021] The cut level difference (Rδc) is the difference in height between cut levels C (Rrm1) and C (Rrm2) that correspond to the load length ratios Rmr1 and Rmr2, respectively, in the roughness curve specified in JIS B0601: 2001. When the cut level difference (Rδc) is large, the unevenness of the measurement surface becomes large, and when it is small, the unevenness of the surface becomes small.

[0022] The cut level difference (Rδc) can be measured in accordance with JIS B 0601:2001 using a laser microscope (Keyence Corporation, Ultra-Deep Color 3D Shape Measuring Microscope (VK-X1000 or its successor model)). Measurement conditions include a coaxial illumination method, a magnification of 480x, no cutoff value λs, a cutoff value λc of 0.08 mm, no cutoff value λf, end effect correction, and a measurement range of 710 μm x 533 μm per location from the measurement surface. When the surface of the substrate 1 is the measurement surface, a circumference to be measured is drawn around the support portion 22, and the length of one circumference is set to, for example, 1360 μm. When the mounting surface 3 is the measurement surface, a circumference to be measured is drawn near the outer edge of the mounting surface 3, and the length of one circumference is set to, for example, 240 μm. The average value may be calculated from the measured values, with the number of measurements for each being eight or more.

[0023] Furthermore, the surface of the substrate 1 preferably has a larger average value of the root-mean-square slope (RΔq) in the roughness curve than the mounting surface 3. This reduces the risk of the reaction products adhering to the surface of the substrate 1 and re-adhering, even if the workpiece is adsorbed to an adsorption member installed in the plasma processing apparatus and reaction products generated by the plasma processing float. The mounting surface 3 has fewer irregularities, making it less likely that the backside of the workpiece will be scratched. Specifically, the difference in the average values ​​of the root-mean-square slope (RΔq) between the surface of the substrate 1 and the mounting surface 3 is preferably 0.34 or more. Here, the average value of the root-mean-square slope (RΔq) of the surface of the substrate 1 is preferably 1.1 or less. This reduces the likelihood of large particles detaching from the surface, reducing the risk of these particles adhering to the workpiece.

[0024] The root mean square slope (RΔq) of a roughness curve is the root mean square of the local slope dZ / dx of the roughness curve at a reference length l measured in accordance with JIS B 0601:2001, and is calculated by the following formula: It is defined by:

[0025] When the root mean square slope (RΔq) value is large, the surface unevenness is steep, and when the root mean square slope (RΔq) value is small, the surface unevenness is gentle. The root mean square slope (RΔq) can be measured in accordance with JIS B 0601:2001 using a laser microscope (Keyence Corporation, VK-X1100 or its successor model). The measurement conditions and calculation of the average value are as described above.

[0026] As shown in Figures 3A and 3B, the protrusions 120, 120' may have step portions 5, 5' around the support portions 122, 122'. This increases the rigidity of the protrusions 120, 120'. The protrusion 120 shown in Figure 3A has a step portion 5 formed around the support portion 122, and a mounting portion 121 formed above the step surface. The protrusion 120' shown in Figure 3B has a mounting portion 121' that covers the step surface of the step portion 5'. This can prevent the film 4 on the mounting portion 121' from shedding, which may occur from the step surface of the support portion 122'. The step surface shown in Figures 3A and 3B is annular, but may also be a square or rectangular frame.

[0027] The upper surface of the film 4 covering the step surface of the step portion 5 or the step surface of the step portion 5' preferably has a larger average cut level difference (Rδc), which represents the difference between the cut level at a load length ratio of 25% on the roughness curve and the cut level at a load length ratio of 75% on the roughness curve, than the mounting surface 3. This reduces the risk that even if reaction products generated by plasma processing of the workpiece float, these reaction products will adhere to the step surface of the step portion 5 or the upper surface of the film 4 covering the step surface of the step portion 5' and float again. Furthermore, since the mounting surface 3 has fewer irregularities, it is less likely to scratch the back surface of the workpiece. Specifically, the difference in the average cut level difference (Rδc) between the step surface and the mounting surface 3 is preferably 0.38 μm or more. The average cut level difference (Rδc) of the step surface is preferably 1.4 μm or less. This makes it difficult for large particles to detach from the stepped surface, reducing the risk of these particles adhering to the workpiece.The cutting level difference (Rδc) is measured in the same manner as described above.

[0028] Furthermore, the step surfaces of the step portions 5, 5' preferably have a larger average value of the root-mean-square slope (RΔq) in the roughness curve than the mounting surface 3. This reduces the risk of floating reaction products resulting from plasma processing of the workpiece and adhering to the step surface and re-floating. Furthermore, the mounting surface 3 has fewer irregularities, making it less likely to scratch the back surface of the workpiece. Specifically, the difference in the average value of the root-mean-square slope (RΔq) between the step surface and the mounting surface 3 is preferably 0.34 or more. The average value of the root-mean-square slope (RΔq) of the step surface is preferably 1.1 or less. This reduces the likelihood of large particles detaching from the step surface and adhering to the workpiece. The method for measuring the root-mean-square slope (RΔq) is the same as described above.

[0029] The average value of the skewness (RSK1) in the roughness curve of the mounting surface 3 may be smaller than the average value of the skewness (RSK2) in the roughness curve of the stepped surface or the upper surface of the film 4, 4' covering the stepped surface (hereinafter collectively referred to as the stepped surface). The skewness (RSK) in the roughness curve is defined in JIS B 0601:2001 and is an index indicating the ratio of peaks to valleys when the average height in the roughness curve is taken as the center line. If the average value of the skewness (RSK1) is smaller than the average value of the skewness (RSK2), the flatness of the peaks on the mounting surface 3 will be higher than the flatness of the peaks on the stepped surface, thereby suppressing the aggressiveness of the mounting surface to the workpiece. On the other hand, the steepness of the peaks on the step surface is greater than that of the peaks on the mounting surface. Therefore, when particles adhere to the step surface, a high trapping effect is achieved, reducing the risk of the particles re-floating even when subjected to external disturbances such as vibration. Specifically, the difference between the average value of skewness (RSK1) and the average value of skewness (RSK2) is preferably 0.2 or more, particularly 0.3 or more. The average value of skewness (RSK2) is preferably 1.5 or less. When the average value of skewness (RSK2) is within this range, particles are less likely to detach from the peaks on the mounting surface 3, reducing the likelihood of the detached particles floating and adhering to the adsorbate. Skewness (RSK1 and RSK2) can be measured in accordance with JIS B 0601:2001 using a laser microscope (Keyence Corporation, VK-X1100 or its successor model). The measurement conditions and calculation of the average value were as described above.

[0030] In the present disclosure, as in the protrusion 220 shown in Fig. 4A , an annular recess 6 extending from the surface of the substrate 1 in the depth direction is provided around the support portion 222, and the radial width w of the recess 6 is preferably narrower than the circle-equivalent diameter d of the mounting surface 3 of the mounting portion 221. Alternatively, as in the protrusion 320 shown in Fig. 4B , an annular recess 6' extending from the step surface in the depth direction is provided, and similarly to the above, the radial width w of the recess 6' is preferably narrower than the circle-equivalent diameter d of the mounting surface 3 of the mounting portion 321. When the recess 6 is provided around the support portion 222 or on the step surface in this way, the reaction products can be easily captured by the recesses 6, 6' and the captured reaction products can be prevented from floating again. 4B shows an annular recess 6' extending in the depth direction from the inner periphery of the step surface, but recess 6' may also extend in the depth direction from the outer periphery of the step surface, or may extend in the depth direction from a portion that includes both the inner and outer peripheries of the step surface. The inner periphery of the step surface refers to the range that starts from the inner periphery of the step surface and is half the width of the step surface, and the outer periphery of the step surface refers to the range excluding the inner periphery of the step surface.

[0031] The recess 6 is annular and surrounds the protrusion 220, and the recess 6' is annular and surrounds the area above the step surface, including the mounting portion 321. The outer periphery of the recess 6, 6' is preferably circular in top view, but may be polygonal, including triangular. The radial width w of the recess 6, 6' is preferably 5% to 35% of the circle-equivalent diameter d of the mounting surface 3.

[0032] Next, a manufacturing method of the adsorbent member of the present disclosure will be described with reference to Figures 5A to 5E. To manufacture the adsorbent member of the present disclosure, first, a ceramic 7 containing silicon carbide as a primary component is prepared (Figure 5A). Specifically, pure water, a dispersant, boron carbide powder, and a sintering aid such as phenolic resin are added to silicon carbide powder, and then wet-mixed in a ball mill to produce a slurry. Here, the content of boron carbide powder relative to 100% by mass of silicon carbide powder is, for example, 1% by mass or more and 3% by mass or less.

[0033] Next, an organic binder is added to the slurry, and the mixture is spray-dried to form granules. The granules are then formed into a compact using various forming methods (e.g., cold isostatic pressing (CIP)), and the compact is then machined to produce a compact of the desired shape. If necessary, the compact is then heated in a nitrogen atmosphere for 10 to 40 hours, held at 450 to 650°C for 2 to 10 hours, and then naturally cooled and degreased. The degreased compact is then fired at 1800°C to 2000°C in a reduced pressure atmosphere of an inert gas, such as argon gas, to produce ceramics 7.

[0034] Next, as shown in Fig. 5B, the surface that will become the substrate's front surface is subjected to laser processing using, for example, a carbon dioxide laser, a YAG laser, an ArF excimer laser, a KrF excimer laser, or a XeCl excimer laser, to form recesses 8 and protrusions 9 that are the remainder of the recesses 8. Next, as shown in Fig. 5C, the recesses 8 and protrusions 9 are coated with a film 4 containing, as a main component, at least one selected from silicon carbide, DLC, amorphous silicon, molybdenum, chromium, and tantalum. The film 4 can be formed by, for example, chemical vapor deposition (CVD), physical vapor deposition (PVD), plating, vapor deposition, plasma ion implantation, ion plating, or thermal spraying. Of these, chemical vapor deposition is preferred, as the resulting mounting portions 21, 121, 221, and 321 are extremely dense and have almost no fine irregularities on their surfaces, thereby significantly reducing the amount of particles generated by the adsorption member 10.

[0035] On the other hand, warping is likely to occur due to internal stress caused by the difference in thermal expansion between the ceramic 7 and the film 4 during film formation by chemical vapor deposition or the like. Therefore, as shown in Fig. 5D, the film 4 is divided by grinding and / or polishing until the upper surfaces of the protrusions 9 are exposed. This reduces the internal stress accumulated in the mounting portion, and the flatness of the mounting surface 3 is reduced.

[0036] Next, as shown in FIG. 5E, the convex portions 9 are removed by laser processing, blasting, milling, or the like, thereby obtaining the substrate 1 and the suction member 10 having the frustum-shaped protrusions 2, 120, and 121.

[0037] To provide step portions 5, 5' around support portion 122 as shown in Figure 3A or 3B, or to provide annular recessed portions 6, 6' around support portions 222, 322 as shown in Figure 4A or 4B, the step portions 5, 5' and / or recessed portions 6, 6' may be formed at the same time as removing protrusions 9 by laser processing, blasting, milling, or the like.

[0038] The suction member of the present disclosure is suitable for use in holding a workpiece in a processing device such as an exposure device that processes the workpiece, such as a silicon wafer used in the manufacture of semiconductor integrated circuits or a glass substrate used in the manufacture of liquid crystal display devices, or in an inspection device that inspects silicon wafers, glass substrates, etc.

[0039] Although the embodiments of the present disclosure have been described above, the present disclosure is not limited to the above embodiments, and various modifications and improvements are possible within the scope of the present disclosure. For example, the present disclosure is not limited to a configuration using a vacuum chuck as the attraction member 10, and an electrostatic chuck that electrostatically attracts the workpiece may also be used.

[0040] REFERENCE SIGNS LIST 1 substrate 2, 120, 120', 220, 320 protrusion 3 mounting surface 4, 4' film 5, 5' step 6, 6' recess 7 ceramics 8 recess 9 protrusion 10 suction member 21, 121, 121', 221, 321 mounting portion 22, 122, 122', 222, 322 support portion

Claims

1. The present invention comprises a substrate made of a ceramic material containing silicon carbide as a main component, and a plurality of protrusions formed on a surface of the substrate, the protrusion portion includes a mounting portion having a mounting surface for mounting an object to be processed and a support portion for supporting the mounting portion; the mounting portion includes a film containing at least one selected from silicon carbide, diamond-like carbon, amorphous silicon, molybdenum, chromium, and tantalum as a main component; The membranes are independent of each other for each of the protrusions.

2. The adsorption member according to claim 1 , wherein the film extends toward an outer circumferential surface of the support and covers at least a portion of the outer circumferential surface of the support.

3. The adsorption member according to claim 1 or 2, wherein the surface of the substrate has a larger average value of a cut level difference (Rδc) representing the difference between a cut level at a load length ratio of 25% on a roughness curve and a cut level at a load length ratio of 75% on the roughness curve than the placement surface.

4. 4. The adsorption member according to claim 3, wherein an average value of the cut level difference (R.delta.c) on the surface of the substrate is 1.4 [mu]m or less.

5. 4. The attraction member according to claim 3, wherein a difference in average value of the cutting level difference (Rδc) between the surface of the substrate and the placement surface is 0.38 μm or more.

6. 3. The attraction member according to claim 1, wherein the surface of the substrate has a larger average value of the root mean square slope (RΔq) in a roughness curve than the placement surface.

7. The attraction member according to claim 6 , wherein the average value of the root mean square slope (RΔq) of the surface of the substrate is 1.1 or less.

8. The adsorption member according to claim 6 , wherein the difference in the average value of the root mean square slope (RΔq) is 0.34 or more.

9. The attraction member according to claim 1 or 2, wherein the protrusion has a step portion having a step surface around the support portion.

10. The adsorption member according to claim 9 , wherein the film covers a step surface of the step portion.

11. The adsorption member according to claim 9, wherein the step surface or the upper surface of the film covering the step surface has a larger average value of a cut level difference (Rδc) representing a difference between a cut level at a load length ratio of 25% on a roughness curve and a cut level at a load length ratio of 75% on the roughness curve than the placement surface.

12. The adsorption member according to claim 11, wherein an average value of the cut level difference (Rδc) of the step surface or the upper surface of the film covering the step surface is 1.4 μm or less.

13. The adsorption member according to claim 11, wherein the difference in average value of the cut level difference (Rδc) is 0.38 μm or more.

14. The adsorption member according to claim 10 , wherein the step surface or an upper surface of the film covering the step surface has a larger average value of the root-mean-square slope (RΔq) in a roughness curve than the placement surface.

15. The adsorption member according to claim 14 , wherein the average value of the root-mean-square slope (RΔq) of the step surface or the upper surface of the film covering the step surface is 1.1 or less.

16. The adsorption member according to claim 14 , wherein the difference in the average value of the root mean square slope (RΔq) is 0.34 or more.

17. 3. The suction member according to claim 1, further comprising an annular recess around the support portion, the recess extending in a depth direction from a surface of the substrate, the radial width of the recess being narrower than a circular equivalent diameter of the placement surface.

18. The attraction member according to claim 9 , further comprising an annular recess extending in a depth direction from the step surface, the radial width of the recess being narrower than a circular equivalent diameter of the placement surface.

19. A method for producing the adsorption member according to claim 1 or 2, comprising the steps of: A method for manufacturing an adsorption member, comprising the steps of: (1) forming a recess and a protrusion, which is the remainder of the recess, on one surface of a substrate made of a ceramic containing silicon carbide as a main component; (2) A step of coating the recesses and protrusions with a film containing, as a main component, at least one selected from silicon carbide, diamond-like carbon, amorphous silicon, molybdenum, chromium, and tantalum. (3) A step of cutting the film by at least one of grinding and polishing the film until the upper surfaces of the protrusions are exposed. (4) A step of removing the protrusions to obtain an adsorption member including the substrate and the frustum-shaped protrusions.

20. A processing device comprising the adsorption member according to claim 1 or 2.

21. An inspection device comprising the adsorption member according to claim 1 or 2.