Porous membrane and desalination method
Patent Information
- Application Number
- JP2023568518
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2043-09-25
AI Technical Summary
Porous membranes used in water treatment and other fields face challenges with filtration solutions that are easily contaminated, leading to clogging due to adsorption of organic matter, which reduces filtration flux and requires excessive chemical cleaning that can damage the membrane over time.
A porous membrane with a high proportion of β-type structure crystals and a small surface pore diameter is developed, featuring a specific ratio of α-type to β-type structure crystals, optimized phase separation, and a denser surface structure to prevent organic matter adsorption and maintain high filtration flux.
The membrane achieves high water permeability and excellent stain resistance, ensuring sustained filtration performance even with contaminated solutions without the need for excessive chemical cleaning, thereby extending the membrane's lifespan and reducing operational costs.
Abstract
Description
Porous membrane and water production method
[0001] The present invention relates to a porous membrane for use in the fields of water treatment, pharmaceutical manufacturing, food industry, fermentation, etc.
[0002] In recent years, porous membranes such as microfiltration membranes and ultrafiltration membranes have been used in a variety of fields, including water treatment (e.g., water purification or wastewater treatment), medical treatment (e.g., blood purification), and the food industry. Recently, there has been a demand for highly fouling-resistant porous membranes that can efficiently filter easily fouling raw filtrates, which have previously been considered difficult to filter. Easily fouling raw filtrates are characterized by containing a higher than normal amount of fouling substances, which often contain organic matter. Typical examples of organic matter include proteins, polysaccharides, and humic acids.
[0003] However, when filtering the above-mentioned easily contaminated raw filtrate, the porous membrane is clogged by the contaminants contained in the raw filtrate, resulting in a decrease in the filtration flux of the porous membrane. In particular, when the raw filtrate contains a large amount of organic matter, the interaction between the porous membrane and the organic matter causes the organic matter to be adsorbed onto the porous membrane, which easily clogs the pores of the porous membrane. Furthermore, when the porous membrane is clogged and the number of pores decreases, high pressure is required for filtration, and the contaminants are pressed against the porous membrane surface under high pressure, making adsorption more likely. In order to prevent a decrease in filtration flux, it is important to reduce the adsorption of organic matter onto the porous membrane.
[0004] Here, one effective method for eliminating the adsorption of organic matter and restoring the filtration flux is to decompose and remove the organic matter accumulated in the porous membrane using chemicals, for example, oxidizing agents such as sodium hypochlorite or alkalis such as sodium hydroxide. However, such chemicals not only decompose the accumulated organic matter but can also decompose the polymers that make up the membrane, so continuous chemical cleaning can cause the membrane pores to become coarse, making it difficult to maintain the separation performance and mechanical strength of the membrane for a long period of time.
[0005] In response to this, Patent Documents 1 and 2 disclose methods for increasing the proportion of stable α-structure crystals in polyvinylidene fluoride resin (hereinafter also referred to as "PVDF resin"). It is disclosed that a high proportion of stable crystals improves chemical resistance and increases cleaning strength.
[0006] JP 2015-73916 A JP 2021-176629 A JP 2017-29934 A
[0007] However, the α-structure crystals in the polyvinylidene fluoride resin porous membranes of Patent Documents 1 and 2 have a TGTG' (T: Trans, G: Gauche) structure. Because α-structure crystals have a twisted structure, the dipole moments are arranged in alternating directions and lack polarity. Therefore, they have weak interactions with polar water molecules, and conversely, they have strong interactions with organic substances due to hydrophobic interactions. In other words, porous membranes made of polyvinylidene fluoride resin with α-structure crystals are prone to adsorption of organic substances and are therefore prone to clogging. Therefore, they require cleaning with large amounts of chemicals. While Patent Documents 1 and 2 improve the chemical resistance of the porous membranes, the chemicals are expensive and may adversely affect module components equipped with the porous membrane and processes other than the porous membrane. For example, the adhesive used to bond the porous membrane may deteriorate, resulting in a shortened lifespan of the porous membrane module. Furthermore, if a separate separation membrane with relatively poor chemical resistance is used downstream of the porous membrane, this may lead to deterioration of the downstream separation membrane.
[0008] Patent Documents 2 and 3 disclose porous films that contain not only α-type structure crystals but also a large amount of β-type structure crystals, which are a relatively metastable phase. β-type structure crystals have a TTTT planar zigzag structure, and the dipole moments are arranged in the same direction, and there are many electron donating components on the film surface, which is considered to have polarity. For example, Patent Document 2 discloses a film in which the proportion of infrared absorbance derived from α-type structure crystals among the infrared absorbance derived from α-type structure crystals and β-type structure crystals is 32.5%. In other words, α-type structure crystals (H α ) and β-type structure crystals (H β ) ratio (H α / H β) is 0.38. Patent Document 3 also discloses a membrane in which the abundance ratio of α crystal structure to β crystal structure is 0.11. Therefore, these membranes also have a strong interaction with water molecules, which have polarity, and conversely, they are less likely to adsorb organic matter.
[0009] However, according to the inventors' findings, the porous membrane manufacturing method of Patent Document 2 tends to produce porous membranes with large pore sizes due to a relatively fast phase separation rate during membrane formation. Because the pore size is large, the number of pores is insufficient. In such porous membranes, contaminants easily penetrate the porous membrane, causing clogging, and the desired filtration rate is not achieved. This is because, although the membrane-forming solution is described as containing polyvinylidene fluoride resin as the polymer and a mixture of multiple good solvents as the solvent, the method does not focus on the self-diffusion coefficient of the polymer, and the good solvent does not include the hydrogen-bonding solvent described below. Similarly, the manufacturing method described in Patent Document 3 does not focus on the self-diffusion coefficient of the polymer. Furthermore, the polymer content in the membrane-forming solution is high at 30 wt %, resulting in a small number of pores in the formed porous membrane and a low pure water permeability. Such porous membranes require high pressure during filtration, and the high pressure forces contaminants against the membrane surface, promoting adsorption and clogging of the porous membrane, making it difficult to obtain sufficient permeate when filtering a filtrate containing a large amount of contaminants.
[0010] The problem to be solved by the present invention is to obtain a porous membrane that can maintain high filtrate permeability even when using a filtrate stock solution that is prone to contamination, as described above, and which has been considered difficult to filter due to the significant fouling of the porous membrane. In the prior art, as in Patent Document 1, porous membranes containing a large amount of α-structure crystals, which emphasize chemical resistance, were common. As described above, in Patent Document 3, the high polymer concentration in the membrane-forming stock solution made it easy to form a porous membrane containing a large amount of β-structure crystals, which is a metastable phase. However, the number of pores in the porous membrane was small, making it easy to form a porous membrane containing a large amount of β-structure crystals and resulting in low pure water permeability. Furthermore, as in Patent Document 2, even when the polymer concentration in the membrane-forming stock solution was low, it was easy to form a porous membrane containing a large amount of β-structure crystals by using a mixed solvent. However, the phase separation rate was not sufficiently slow, making it easy to form a porous membrane with a large pore size. In other words, it was difficult to form a porous membrane that combined the three elements of being difficult to adsorb by containing a large amount of β-structure crystals, increasing the number of surface pores, ensuring flow paths, and showing high pure water permeability, and having a relatively small surface pore size.
[0011] The present invention aims to provide a porous membrane that has a high content of β-structure crystals and excellent fouling resistance, and that further has high pure water permeability, thereby reducing adsorption even to easily fouling filtrate raw solutions, and that has a relatively small surface pore size to prevent fouling components from penetrating into the porous membrane, thereby ensuring a high filtration flux over a long period of time.
[0012] In order to solve the above problems, the present invention provides a porous membrane having the following configuration: (1) A porous membrane containing polyvinylidene fluoride resin, one surface of which is designated as surface A and the other surface of which is designated as surface B, and the α-type structure crystal (H) in the crystalline part of the polyvinylidene fluoride resin measured on surface A by an ATR method (attenuated total reflection method) is α ) and β-type structure crystals (H β ) ratio (H α / H β The ratio of the porous membrane to the pure water permeability is 0.25 m 3 / m 2 / h / 50kPa or more 1.2m 3 / m 2 / h / 50 kPa or less, and the average surface pore size of the surface pores on the surface A of the porous membrane is 5.0 nm or more and 12.0 nm or less. (2) The porous membrane according to (1), wherein the crystallinity of the vinylidene fluoride resin on the surface A of the porous membrane is 30% or more. (3) The porous membrane according to (1) or (2), wherein the removal rate of 40,000 Da dextran of the porous membrane is 45% or more and 80% or less. (4) The number of the surface pores [number / μm 2 ] divided by the average surface pore diameter [nm]: X is 30 / μm 2 / nm or more 100 pieces / μm 2 / nm or less. (5) The porous membrane according to any one of (1) to (4), wherein the standard deviation of the surface pore diameter at surface A of the porous membrane is 1.0 nm or more and 5.0 nm or less. (6) The porous membrane according to any one of (1) to (5), wherein the surface portion from surface A to a thickness of 10 μm of the porous membrane is denser than the interior. (7) A method for filtering a liquid using the porous membrane according to any one of (1) to (6). (8) A membrane filtration device comprising the porous membrane according to any one of (1) to (6). (9) A freshwater production method including a pretreatment step of pretreating water to obtain reverse osmosis membrane feed water and a reverse osmosis membrane treatment step of filtering the reverse osmosis membrane feed water through a reverse osmosis membrane to obtain permeate water, the water to be treated having a biopolymer concentration of 100 μg C / L or more, and the reverse osmosis membrane feed water having a biopolymer concentration of 75 μg C / L or less through pretreatment is supplied to the reverse osmosis membrane, the pretreatment step having an ultrafiltration membrane treatment section equipped with an ultrafiltration membrane, and the ultrafiltration membrane being the porous membrane described in any one of (1) to (6). (10) A freshwater production method including a pretreatment step of pretreating water to obtain permeate water, the pretreatment step having an ultrafiltration membrane treatment section equipped with an ultrafiltration membrane, and the ultrafiltration membrane being the porous membrane described in any one of (1) to (6). 2 More than 2000 pieces / μm 2 (11) The fresh water production method according to (9) or (10), characterized in that the water to be treated does not contain a coagulant in the ultrafiltration membrane treatment in the pretreatment step.
[0013] According to the present invention, a porous membrane can be obtained that has a high proportion of β-structure crystals to which organic matter does not easily adhere, a small surface pore size, and a sufficiently large number of pores, thereby providing a porous membrane that has high water permeability and excellent fouling resistance and can maintain high filtrate permeability for a long period of time even for a fouling raw solution.
[0014] Fig. 1 is a schematic diagram showing the filtration state of the porous membrane of the present invention. Fig. 2 is a schematic diagram showing the filtration state of a conventional porous membrane. Fig. 3 is a schematic diagram showing the filtration state of a conventional porous membrane. Fig. 4 is a schematic diagram of the formation process of the porous membrane of the present invention. Fig. 5 is an electron microscope photograph showing the surface (part) of the porous membrane of one embodiment of the present invention. It is a schematic diagram showing an example of the fresh water production method of the present invention.
[0015] The following describes in detail an embodiment of the present invention with reference to the drawings, but the present invention is not limited thereto. In this specification, "mass" and "weight" are synonymous. Furthermore, a filtrate that is easily soiled is characterized by a higher than normal amount of contaminants, and these contaminants often contain useful substances that are the target of removal. Examples of organic matter typically include proteins, polysaccharides, humic acid, etc.
[0016] The fouling in the "fouling resistance" of the present invention refers to clogging of the porous membrane with organic matter contained in the raw filtrate during the filtration process. As the clogging of the porous membrane with organic matter progresses, the filtration resistance increases and the amount of liquid that can pass through the porous membrane decreases.
[0017] Generally, porous membranes with α-structure crystals are prone to adsorb organic matter, and to resolve this issue, methods such as decomposing and removing accumulated organic matter using large amounts of chemicals are used as an effective means. However, such chemicals not only decompose the accumulated organic matter, but also decompose the polymers that make up the membrane, and may even have adverse effects on module components equipped with the porous membrane and processes other than the porous membrane. Therefore, porous membranes with β-structure crystals that have excellent fouling resistance are promising, but there have been no porous membranes with β-structure crystals and high water permeability. The present invention provides a membrane with β-structure crystals that further has high pure water permeability, thereby reducing adsorption even for easily fouled filtrate stock solutions and ensuring high filtration flux. The porous membrane of the present invention with improved fouling resistance will be described below.
[0018] <Regarding the porous membrane> The porous membrane according to an embodiment of the present invention is a porous membrane containing polyvinylidene fluoride resin, and has a surface A and a surface B. In the IR spectrum of surface A measured by an ATR method (attenuated total reflection method), α-type structure crystals (H α ) and β-type structure crystals (H β ) ratio (H α / H β ratio) is 0 or more and 0.5 or less, and the pure water permeability is 0.25 m 3 / m 2 / h / 50kPa or more 1.2m 3 / m 2 / h / 50kPa or less. α / H β The ratio of 0 is β-type structure crystal (H β ) indicates that the percentage is 100%.
[0019] The α-type structure crystals (H α ) and β-type structure crystals (H β ) ratio (H α / H β) must be between 0 and 0.50. Three types of crystal structures are known for polyvinylidene fluoride resin: α-type, β-type, and γ-type, which exists in extremely small amounts. Of these, we focused on α-type and β-type, which are generally known to form more frequently than γ-type. β-type structure crystals have a TTTT planar zigzag structure, with dipole moments arranged in the same direction, and are considered to have a large number of electron-donating components on the film surface, making them polar. Therefore, they have a strong interaction with water molecules, which also have polarity, and conversely, organic substances are less likely to be adsorbed. H α / H β When the ratio is 0 or more and 0.50 or less, excellent stain resistance against organic matter is exhibited. α ) and β-type structure crystals (H β ) and the ratio (H α / H β The ratio of H to H can be calculated by the following formula (1), and is more preferably 0.25 or more and 0.40 or less, and even more preferably 0.30 or more and 0.40 or less. α / H β The smaller the ratio, the more β-type structure crystals there are, which is preferable. α / H β ...Formula (1).
[0020] The porous membrane of the present invention is a polyvinylidene fluoride resin having a β-type structure crystal (H β In the prior art, the β-type structure crystal (H βIn order to obtain this, it was necessary to increase the concentration of the PVDF polymer in the film-forming process. When the polymer concentration of the PVDF polymer is high, the resulting porous membrane has a high polymer density, resulting in low porosity and a small number of pores. Attempts have been made to obtain β-structure crystals by lowering the PVDF polymer concentration in the film-forming process, but the low concentration tends to result in large pores and a sparse porous membrane with a small number of pores. In contrast, the porous membrane of the present invention can produce a large number of fine pores even at a low PVDF polymer concentration by controlling the phase separation rate between the polymer and the solvent. By achieving a relatively slow phase separation rate during the phase separation process between the polymer and the solvent, it is possible to produce a large number of pores with a small pore size. The self-diffusion coefficient of the polymer can be used as an indicator of the phase separation rate. By optimizing the polymer concentration, the solvent and temperature of the coagulation bath, a porous membrane with a large number of pores, a small surface pore size, and a large number of pores, while having a high concentration of β-structure crystals and excellent stain resistance, can be obtained.
[0021] The porous membrane of the present invention is mainly composed of a crystalline polymer resin containing polyvinylidene fluoride, and the crystallinity of the polymer resin constituting the porous membrane is not limited as long as it has crystals within 50 μm from the surface A of the porous membrane, but it is more preferable that the crystallinity of PVDF is 30% or more. A crystallinity of 30% or more is preferable because it makes it easier to suppress the deformation of the pores when turbidity hits the porous membrane and makes it easier for the turbidity to bounce off the membrane surface. In order to suppress the deformation of the pores and improve the rebound of the turbidity, the crystallinity is more preferably 35% or more, and even more preferably 40% or more. However, if it is 80% or more, the flexibility of the porous membrane is lost and it becomes easier to break during operation, for example, cross-flow operation, so it is preferable that it is 80% or less. H α / H βA small ratio and a crystallinity of 30% or more leads to a strong interaction with polar water molecules, making it difficult for organic substances to be adsorbed. The crystallinity of a porous membrane can be calculated from the results of a differential scanning calorimeter (DSC). Sections within 50 μm from the outer surface of the porous membrane used for measuring crystallinity are taken using a commercially available freezing microtome. The microtome moves the porous membrane a fixed distance, then brings the blade into contact with the porous membrane to cut it. The blade is placed parallel to the surface of the porous membrane. First, the porous membrane is cut once by approaching the blade at 5 μm intervals. Then, by increasing the movement distance to 40 μm and cutting once more, a thickness of 40 μm to 45 μm can be obtained from surface A.
[0022] Pure water permeability is 0.25m 3 / m 2 / h / 50kPa or more 1.2m 3 / m 2 By setting the permeability to 50 kPa or less, it is possible to perform filtration at a relatively low pressure even for a feed solution that is easily contaminated, and since the contaminants are not pressed against the membrane surface at high pressure, adsorption and clogging of the porous membrane are suppressed, and sufficient permeate can be obtained even when filtering a feed solution that contains a large amount of contaminants. 3 / m 2 / h / 50kPa or more 1.2m 3 / m 2 / h / 50 kPa or less, and more preferably 0.40 m 3 / m 2 / h / 50kPa or more 1.2m 3 / m 2 / h / 50 kPa or less.
[0023] FIG. 1 shows a schematic diagram of the filtration of a difficult-to-filter raw solution using the porous membrane of the present invention. FIG. 1 is a conceptual schematic diagram showing a portion of the cross section of a porous membrane. In FIG. 1, the solid line drawn on the surface portion 102 schematically represents the mesh structure. The filtration direction FL is the direction from the surface portion 102 toward the interior portion 103. The organic matter in the raw solution often contains coarse contaminant components 201 and fine contaminant components 202. The porous membrane has a β-type crystal structure, which makes it highly polar and suppresses adsorption of the coarse contaminant components 201 and the fine contaminant components 202. Furthermore, due to its high pure water permeability, the fine contaminant components 202 can pass through the porous membrane at relatively low pressure. Since the fine contaminant components 202 are not pressed strongly against the pores in the porous membrane, adsorption and clogging of the fine contaminant components 202 to the porous membrane are easily suppressed, and high filtrate permeability can be maintained. The porous membrane 101 also includes a surface portion 102 and an interior portion 103. The surface portion 102 has a denser structure than the interior portion 103, which makes it difficult for dirt components to penetrate into the interior of the porous membrane, and is therefore preferred because it tends to exhibit excellent dirt resistance. If the micropores in the surface portion 102 are dense, coarse dirt components 201 cannot penetrate into the porous membrane and do not clog the surface layer 102 of the porous membrane, making the porous membrane less susceptible to dirt, which is preferred.
[0024] Figure 2 shows a schematic diagram of a previously known porous membrane with large pores containing many α-structure crystals filtering a highly difficult-to-filter raw solution. Because the porous membrane contains many α-structure crystals, it has low polarity and is prone to adsorb coarse organic contaminant components 201 and fine organic contaminant components 202 through hydrophobic-hydrophobic interactions. Furthermore, because the pore size is large, the coarse contaminant components 201 penetrate deep into the porous membrane, easily causing clogging. Furthermore, because the number of pores is small, the filtrate permeability is low.
[0025] Furthermore, Figure 3 shows a schematic diagram of a filtrate stock solution that is difficult to filter, filtered through a porous membrane known to date that has a relatively high content of β-structure crystals but low pure water permeability. Such porous membranes often have a small number of pores and low pure water permeability. Because the porous membrane contains a high content of β-structure crystals, it adsorbs relatively little coarse contaminant components 201 and fine contaminant components 202. However, because the pure water permeability is low, high pressure is required for the filtrate stock solution containing fine contaminant components 202 to pass through the porous membrane. As a result, the fine contaminant components 202 are pressed strongly against the pores in the porous membrane, and adsorption into the porous membrane gradually occurs. This tends to result in low filtrate permeability.
[0026] The porous membrane of the present invention further has a dextran rejection rate of 45% to 80% with a weight-average molecular weight of 40,000 Da, which prevents coarse contaminants and substances to be removed in the filtrate from penetrating into the membrane, and therefore exhibits excellent anti-fouling properties. The dextran rejection rate is more preferably 50% to 80%. The dextran rejection rate can be calculated by filtering a commercially available dextran solution prepared at 25°C with a weight-average molecular weight of 40,000 Da at a cross-flow linear velocity of 1.0 m / sec through the porous membrane at a transmembrane pressure difference of 10 kPa using the following formula (2): T = {(refractive index of the filtrate) - (refractive index of the permeate)} / (refractive index of the filtrate) × 100 ... formula (2). Here, the cross-flow linear velocity is the value obtained by dividing the flow rate of the filtrate in a direction perpendicular to the filtration direction by the cross-sectional area of the flow path. The transmembrane pressure difference is the difference between the pressure on the raw liquid side and the pressure on the permeate side across the porous membrane.
[0027] The average surface pore diameter [nm] of the surface portion of the porous membrane is preferably 5.0 nm or more and 12 nm or less, which prevents coarse contaminants in the filtrate and the substances to be removed from penetrating into the porous membrane and tends to exhibit high anti-fouling properties. It is more preferable that the average surface pore diameter [nm] of the surface portion is 5.0 nm or more and 8.0 nm or less. The surface pore diameter is the diameter of the pores present in the surface when observing the surface of the porous membrane. To determine the surface pore diameter of the porous membrane, an image obtained by SEM observing the surface of the porous membrane is binarized using the free software "ImageJ". When binarizing, Subtract Background is set to 1 pixel, and then Create Background is selected as the Threshold (binarization threshold), and the condition: RenyiEntropy is selected. In the obtained binarized image, the area of each pore is calculated by selecting Area in Analyze Particles, and the diameter calculated assuming each pore is a circle is used as the surface pore size. The average surface pore size is calculated by averaging the sizes of more than 1,000 pores.
[0028] The standard deviation of the surface pore diameter [nm] of the porous membrane is 1.0 nm or more and 5.0 nm or less, so that the load of the fouling substance on the porous membrane can be uniform, and it is easy to show excellent fouling resistance, and it is preferred.The standard deviation of the surface pore diameter is 1.0 nm or more and 5.0 nm or less, so that the load of the fouling substance on the porous membrane can be uniform, and it is easy to show excellent fouling resistance, and it is preferred.The standard deviation of the surface pore diameter is more preferably 1.0 nm or more and 4.0 nm or less, and more preferably 1.0 nm or more and 3.0 nm or less.The standard deviation of the surface pore diameter can be obtained by binarizing and analyzing the SEM image of the surface of the porous membrane as described above.
[0029] The number of surface pores observed on the surface of the porous film is 200 / μm 2 ~2000 pieces / μm 2 This is preferable because it allows the contaminants in the raw filtrate to be dispersed within the porous membrane, making it easier to stably filter highly turbid water for a long period of time. Even if the contaminants in the raw filtrate block some of the surface pores as the filtration progresses, a large number of surface pores makes it easier to ensure a sufficient number of flow paths through which the raw filtrate passes through the porous membrane, which is preferable.2 If the number of surface pores of the porous membrane is 290 / μm or more, it is easy to ensure a sufficient flow path until cleaning such as back pressure washing is performed, even if the filtrate raw solution is easily soiled. 2 ~1500 pieces / μm 2 More preferably, 350 particles / μm 2 ~1000 pieces / μm 2 It is particularly preferable that the number of surface pores of a porous film is the number of pores present in the plane when the surface of the porous film is observed. When determining the number of surface pores of a porous film, an image obtained by observing the surface of the porous film with an SEM is binarized using the free software "ImageJ". When binarizing, after setting 1 pixel in Subtract Background and performing Create Background, the condition: RenyiEntropy is selected in Threshold (binarization threshold). In the obtained binarized image, the number of pores in the range observed with Analyze Particles is determined. The number of surface pores per unit area [number / μm 2 When determining the surface pore diameter, 1,000 or more pores are observed and the number of pores is divided by the total area of the observed region. 2 / nm or more 100 pieces / μm 2 When X is 50 / μm or less, the contamination components in the raw filtrate are prevented from penetrating into the pores, and the number of flow paths through which the permeated liquid permeates the porous membrane can be sufficiently secured, which is preferable because the permeation property is easily exhibited. 2 / nm or more 100 pieces / μm 2 / nm or less, and more preferably 60 / μm 2 / nm or more 100 pieces / μm 2 / nm or less is more preferable. The number of surface pores of the porous membrane can be obtained by binarizing an image obtained by observing the surface of the porous membrane with an SEM in the same way as when determining the surface pore diameter, and analyzing it with Analyze Particles. The number of surface pores is calculated by dividing the number of surface pores by the area of the analyzed image. As with the pore diameter, it is calculated by analyzing an image containing 1000 or more pores.
[0030] The porous membrane of the present invention preferably has a nanomesh structure on its surface. The nanomesh structure is a structure in which, in the surface of the porous membrane, the outermost surface portion from the surface to a thickness of 2 μm has an average cross-sectional pore diameter [nm] of 1 nm to 99 nm in the cross section of the outermost surface portion, and the number of cross-sectional pores is 100 / μm. 2 ~1000 pieces / μm 2 The nanomesh structure makes the porous membrane more likely to exhibit excellent anti-fouling properties, which is preferable. The cross-sectional pores refer to pores observed in the cross section of the outermost surface. Since the average cross-sectional pore diameter [nm] in the cross section of the outermost surface is as fine as 1 nm to 99 nm, coarse contaminant components and substances to be removed in the filtrate are easily captured at the outermost surface of the porous membrane and prevented from penetrating into the porous membrane. Furthermore, the number of cross-sectional pores is 100 / μm 2 ~1000 pieces / μm 2 Since the number of pores is large, the pores are formed in all directions, making it easy for the flow paths to be connected linearly, and the porous membrane is less likely to become clogged when fine dirt components pass through it. Furthermore, even if some of the pores become clogged, a flow path for the raw filtrate to pass through the porous membrane can be secured, making the porous membrane preferable as it tends to exhibit excellent fouling resistance.
[0031] <Regarding the method for producing a porous membrane> The porous membrane of the present invention comprises step (A) of dissolving a polymer in a solvent to obtain a polymer solution, and then step (B) of solidifying the polymer solution in a non-solvent to form a porous membrane, and the self-diffusion coefficient [m 2 / sec] is 0.8 × 10 -11 m 2 / sec ~ 1.6 × 10 -11 m 2 / sec, the non-solvent used in step (B) contains 90 to 100% by weight of water, and the temperature of the non-solvent is 6°C to 45°C.
[0032] The type of polymer used in step (A) is not particularly limited, and specific examples include polysulfone resins, polyethersulfone resins, polyvinylidene fluoride resins, nylon, cellulose esters such as cellulose acetate and cellulose acetate propionate, fatty acid vinyl esters, polyvinyl alcohol, polyvinyl acetate, polyvinylpyrrolidone, polymers of acrylic acid esters or methacrylic acid esters such as ethylene oxide, propylene oxide and polymethyl methacrylate, and copolymers thereof.
[0033] In particular, in order to use a porous membrane for long-term filtration, it is preferable to periodically chemically clean accumulated contaminants, and it is particularly preferable to include a polyvinylidene fluoride resin, which has excellent chemical resistance. Polyvinylidene fluoride resin refers to a vinylidene fluoride homopolymer or a vinylidene fluoride copolymer. Here, vinylidene fluoride copolymer refers to a polymer having a vinylidene fluoride residue structure. Polymers having a vinylidene fluoride residue structure are typically copolymers of vinylidene fluoride monomers and other fluorine-based monomers. Examples of such fluorine-based monomers include vinyl fluoride, tetrafluoroethylene, hexafluoropropylene, and trifluorochloroethylene. In the vinylidene fluoride copolymer, ethylene or other fluorine-based monomers other than the above may be copolymerized to the extent that the effects of the present invention are not impaired.
[0034] The polyvinylidene fluoride resin preferably accounts for 50% by weight or more, and particularly preferably 60% by weight or more, when the weight of the porous membrane is taken as 100%. The weight-average molecular weight of the polymer is preferably 50,000 to 1,000,000 Da, since this makes it easier to control the self-diffusion coefficient (described below) to a relatively slow, appropriate range. Furthermore, a mixture of multiple types of polymers may be used.
[0035] The solvent preferably contains a good solvent. Here, a "good solvent" refers to a solvent that can dissolve 5% by weight or more of a polymer even in a low temperature range of 60°C or less. Examples of good solvents include N-methyl-2-pyrrolidone (hereinafter "NMP"), 2-pyrrolidone (hereinafter "2P"), ε-caprolactam (hereinafter "ε-CL"), dimethyl sulfoxide (hereinafter "DMSO"), dimethylacetamide (hereinafter "DMAc"), dimethylformamide (hereinafter "DMF"), methyl ethyl ketone, acetone, tetrahydrofuran, tetramethylurea, trimethyl phosphate, or a mixture thereof. It is more preferable that the good solvent accounts for 40% by weight or more of the solvent, and particularly preferably 60% by weight or more. A large amount of good solvent is preferable because it allows polymer chains to expand in the polymer solution, making it easier to control the self-diffusion coefficient (described below) to a relatively slow, appropriate range. Here, the "non-solvent" in step (B) refers to a solvent that does not dissolve or swell a polymer even when heated to its boiling point. Examples of non-solvents include aliphatic hydrocarbons, aromatic hydrocarbons, aliphatic polyhydric alcohols, aromatic polyhydric alcohols, chlorinated hydrocarbons, other chlorinated organic liquids, and mixed solvents thereof, such as water, hexane, pentane, benzene, toluene, methanol, ethanol, carbon tetrachloride, o-dichlorobenzene, trichloroethylene, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butylene glycol, pentanediol, hexanediol, and low-molecular-weight polyethylene glycol. The polymer concentration (wt%) in the polymer solution is preferably equal to or higher than the entanglement concentration in order to control the self-diffusion coefficient within an appropriate range, and more specifically, is preferably 10 to 40 wt%, more preferably 12 to 30 wt%, and particularly preferably 15 to 25 wt%.
[0036] The porous membrane formation step (B), in which a polymer solution is solidified in a non-solvent to form a porous membrane, is a so-called non-solvent-induced phase separation process. When the polymer solution comes into contact with the non-solvent, the polymer cannot be completely dissolved in the solvent, and phase separation occurs into a polymer-rich phase and a solvent-rich phase. Each phase coarsens while coalescing with the surrounding identical phase.
[0037] Figure 4 is a schematic diagram showing the porous membrane formation process in step (B). Phase separation progresses in the polymer solution in the order of Figures 4(a) to (f), and the areas with high polymer concentration (polymer-rich phase 301) become coarse. During this phase separation and / or coarse-graining process, the exchange of solvent and non-solvent progresses, and when the non-solvent concentration reaches a certain level, the polymer solidifies and the structure of the porous membrane is fixed. At this time, the solvent-rich phase 302 becomes the pores of the porous membrane.
[0038] As a result of intensive research, the inventors have found that in the production of the porous membrane of the present invention, the self-diffusion coefficient of the polymer is set to a relatively low range of 0.8 × 10 -11 m 2 / sec ~ 1.6 × 10 -11 m 2 / sec, it was found that the progress of phase separation and coarsening could be suppressed, and the polymer-rich phase 301 and the solvent-rich phase 302 could be solidified in a state where they existed in fine and large amounts. -11 m 2 / sec or more, the polymer and the solvent have a diffusion coefficient sufficient for phase separation, and pores are easily formed. If the diffusion of the polymer is so slow that phase separation is difficult, pores are difficult to form. -11 m 2 / sec or less, excessive phase separation and coarsening are suppressed, and pore coalescence is suppressed, making it easy to form many micropores. In other words, by appropriately controlling the self-diffusion coefficient of the polymer within a relatively low range, a porous film having many micropores can be formed. The self-diffusion coefficient is 0.8 × 10 -11 m 2 / sec ~ 1.4 × 10 -11 m 2 / sec, and more preferably 0.8 × 10 -11 m 2 / sec ~ 1.1 × 10 -11 m 2 It is more preferable that the time is / sec.
[0039] The self-diffusion coefficient can be determined by all-atom molecular dynamics calculations. All-atom molecular dynamics calculations are a method for determining the trajectory of each atom by solving the equation of motion of a molecular ensemble system for all of the constituent atoms one by one. First, a polymer solution system is created to achieve the polymer concentration (wt%) that will actually be used. At this time, a single model polymer chain is modeled so that its molecular weight is 800 to 6000 and 1 / 200 to 1 / 5 of the weight-average molecular weight of the polymer that will actually be used. Potential parameters used in molecular dynamics calculations include those of DREIDING [S. L. Mayo, B. D. Olafson, W. A. Goddard III, J. Phys. Chem. 94, 8897 (1990)], GAFF [J. Wang, R. M. Wolf, J. W. Caldwell, P. A. Kollman, D. A. Case, J. Compute. Chem. 25, 1157 (2004)], OPLS-AA [W. L. Jorgensen, D. S. Maxwell, Julian Tirado-Rives, J. Am. Chem. Soc. 118, 11225 (1996)], CHARMM [B. R. Brooks, R. E. Bruccoleri, B. D. Olafson, D. J. States, S. Swaminathan, M. Karplus, J. Compute. Chem. 4, 187 (1983)] can be used, but parameters that reproduce the density and cohesive energy, which are physical quantities that represent the cohesive state of a solution system, are preferred.
[0040] As a result of the inventors' investigation into the reproducibility of the aggregation state, it was found that the use of GAFF or OPLS-AA is particularly preferable. Furthermore, a constant pressure and temperature ensemble is constructed by controlling the temperature at 25°C using the Nose-Hoover method [Hoover, W. G. Phys. Rev. A, 31, 1695 (1985)] and the pressure at 1 bar using the Andersen method [H. C. Andersen, J. Chem. Phys. 72, 2384 (1980)]. At this time, short-range Lennard-Johns interactions are handled by applying a switch function from 1.0 nm and cutting off at 1.2 nm, and long-range electrostatic interactions are calculated using the Particle Mesh Ewald method. Molecular dynamics calculations are performed in a constant pressure and temperature ensemble until the density becomes constant. The unit cell length is then adjusted to achieve the average density, and an additional 11 ns of calculations are performed in a constant temperature ensemble. Using a 10 ns trajectory, the mean square displacement (MSD) of each atom in the polymer is determined, and the self-diffusion coefficient of the polymer is calculated using the following equation (3). The range of MSD and t used to calculate D is confirmed to be between 0.9 and 1.1, where log(MSD) divided by log(t). When multiple polymers are mixed to form a polymer solution, the weighted average of the self-diffusion coefficients of each polymer, based on the weight percentage of the polymer, is used as the self-diffusion coefficient of the polymer in the polymer solution.
[0041] D = MSD / 6t (3) D: self-diffusion coefficient t: time In the production of the porous membrane of the present invention, when the non-solvent used for coagulation contains 90 to 100 wt. % water, coagulation is rapid, and the self-diffusion coefficient in the polymer solution is likely to affect the rate of phase separation and coarsening. Furthermore, when the temperature of the non-solvent is 6 to 45°C, coagulation is rapid, and the self-diffusion coefficient in the polymer solution is likely to affect the rate of phase separation and coarsening. The temperature of the non-solvent is preferably 35 to 40°C. By setting the temperature of the non-solvent to 35 to 40°C, coagulation is particularly rapid, and a large amount of β-structure crystals can be produced. In other words, as described above, by keeping the self-diffusion coefficient of the polymer in the polymer solution within a low range and efficiently exchanging the solvent in the polymer solution with the non-solvent in the coagulation bath to further accelerate coagulation, a porous membrane can be obtained that simultaneously increases the proportion of β-structure crystals and has a large number of surface pores.
[0042] In the above-described step (A) of the production of the porous membrane of the present invention, the solvent preferably comprises a hydrogen-bonding solvent having hydrogen bond donor and hydrogen bond acceptor properties and a molecular weight of 500 Da or less, which facilitates controlling the self-diffusion coefficient of the polymer within an appropriate range. Having hydrogen bond donor properties means having a positively polarized hydrogen atom, specifically, a hydroxyl group (OH group), a carboxyl group (COOH group), an amino group (NH group), or the like. Having hydrogen bond acceptor properties means having a lone electron pair, specifically, a carbonyl group, an alkoxy group, a cyano group, or the like. When the solvent has hydrogen bond donor and hydrogen bond acceptor properties, strong hydrogen-bond interactions between the solvents suppress the movement of the solvated polymer, making it easier to control the self-diffusion coefficient of the polymer within a relatively slow, appropriate range. The hydrogen bond donor and hydrogen bond acceptor solvents are not particularly limited, but specific examples include 2P, ε-CL, 1,3-dimethylurea, N-methylacetamide, hydantoin, 2-imidazolidinone, and DL-pyroglutamic acid.
[0043] In the above-mentioned step (A), the dissolved polymer preferably contains a polymer having hydrogen bond donor and / or hydrogen bond acceptor properties, which facilitates controlling the self-diffusion coefficient of the polymer within an appropriate range. When the polymer has hydrogen bond donor and / or hydrogen bond acceptor properties, it interacts with the solvent having hydrogen bond donor and hydrogen bond acceptor properties through hydrogen bonds, which facilitates controlling the self-diffusion coefficient of the polymer within a relatively slow, appropriate range. It is more preferable that the polymer having hydrogen bond donor and / or hydrogen bond acceptor properties account for 10 wt % to 50 wt % of the porous membrane, from the viewpoint of controlling the self-diffusion coefficient of the polymer within an appropriate range.
[0044] Furthermore, when the value obtained by dividing the number of moles of hydrogen bond acceptor functional groups contained in the solvent in the above-mentioned step (A) by the number of moles of hydrogen bond donor functional groups contained in the polymer having hydrogen bond donor and / or hydrogen bond acceptor properties is 1.0 to 12, the hydrogen bonding between the polymer and the solvent is in an appropriate range, and the self-diffusion coefficient of the polymer is easily controlled to a relatively slow, appropriate range. This value is more preferably 2.0 to 9.0, and particularly preferably 5.4 to 8.0.
[0045] When the value obtained by dividing the number of moles of hydrogen bond donor functional groups contained in the solvent in step (A) by the number of moles of hydrogen bond acceptor functional groups contained in the polymer having hydrogen bond donor and / or hydrogen bond acceptor properties is 0.5 to 5.0, the hydrogen bonding between the polymer and the solvent is in an appropriate range, and it is easy to control the self-diffusion coefficient of the polymer to a relatively slow, appropriate range. This value is more preferably 1.5 to 2.3, and particularly preferably 1.8 to 2.3.
[0046] The porous membrane of the present invention may further comprise other layers. In this case, it is preferable that the porous membrane of the present invention is disposed on the surface. By disposing the porous membrane of the present invention on the surface, components contained in the filtrate are less likely to penetrate into the porous membrane, and high permeability can be maintained for a long period of time. The other layer is not particularly limited as long as it is a component that can be overlapped with the porous membrane to form a layer, but it is preferable that the other layer is a support. Here, the term "support" refers to a structure that physically reinforces the porous membrane and has a higher breaking strength than the porous membrane. In order to increase the breaking strength of the support, the breaking strength (breaking strength per unit area) of the support is preferably 3 MPa or more, more preferably 10 MPa or more. In addition, when the composite membrane in which the other layer and the porous membrane of the present invention are arranged in layers is in the form of a hollow fiber, the breaking strength of the support is preferably 300 gf or more, more preferably 800 gf or more.
[0047] A membrane filtration device using the porous membrane of the present invention obtained as described above can be used to filter liquids. Examples of membrane filtration devices include, but are not limited to, those equipped with a raw water tank, a booster pump, a module consisting of several thousand to several tens of thousands of the porous hollow fiber membranes of the present invention, a filtrate tank, and a backwash pump. Examples of methods for filtering liquids include, but are not limited to, using the membrane filtration device to filter raw liquid such as industrial wastewater at an operating pressure of 10 kPa to 1 MPa, and removing organic matter and the like contained in the raw water.
[0048] Water production systems using reverse osmosis membranes are applied to many industries and water treatment fields, including seawater desalination, and have been proven to be superior to other separation methods in terms of separation performance, energy efficiency, etc. However, these water production systems have the problem that the transmembrane pressure increases rapidly due to the growth of microorganisms on the membrane surface or the adhesion of biological films (biofilms) to the membrane surface, i.e., biofouling, which reduces the membrane's permeability and separation ability.
[0049] When biofouling causes an increase in transmembrane pressure or a decrease in membrane permeability and separation ability, the membrane is typically cleaned. Cleaning methods include flushing, in which filtration is stopped and raw water or filtered water is supplied to the membrane surface to clean it, and chemical cleaning, in which a cleaning agent is used. However, once fouling progresses, even cleaning does not completely restore transmembrane pressure, permeability, or separation ability, and cleaning becomes more frequent until the system becomes inoperable and the membrane must be replaced.
[0050] Japanese Patent Nos. 6,561,082 and 6,630,689 focus on biopolymers contained as part of the organic matter in the water to be treated, and disclose methods for performing membrane separation by adjusting the biopolymer concentration in the water to a predetermined threshold value or less, the predetermined threshold value being a value in the range of 9 μg / L to 12 μg / L or 9 μg / L to 17 μg / L. Biopolymers are hydrophilic high molecular weight organic substances (polysaccharides, proteins, etc.) that have a molecular weight of approximately 10 to 20 kDa or more among organic substances.
[0051] However, when the inventors measured the biopolymer concentration in seawater during the course of their research into the present invention, it was found to be 122 to 218 μg C / L, which is a very low value compared to the predetermined threshold values disclosed in Japanese Patent Nos. 6,561,082 and 6,630,689. As described above, the biopolymer concentration in water to be treated, such as ordinary seawater or sewage treatment water, is high, making it difficult to achieve the predetermined threshold values disclosed in Japanese Patent Nos. 6,561,082 and 6,630,689. Furthermore, the proposed method is intended to be supplied to microfiltration or ultrafiltration membranes rather than reverse osmosis membranes, which differs from the fouling mechanism of reverse osmosis membranes, making it difficult to apply the proposed method directly.
[0052] Therefore, the present invention provides a method for producing freshwater with a high biofouling potential, which suppresses the progression of fouling in a pretreatment process and a reverse osmosis membrane when using a membrane to desalinate seawater, brine, or the like, or when purifying sewage treatment water or industrial wastewater to produce reuse water. To solve the above problems, the present invention provides a freshwater production method having any of the following configurations: A pretreatment process for pretreating the water to be treated to obtain reverse osmosis membrane feed water, and a reverse osmosis membrane treatment process for filtering the reverse osmosis membrane feed water to obtain permeate water, wherein the water to be treated, having a biopolymer concentration of 100 μg C / L or more, has been pretreated to have a biopolymer concentration of 75 μg C / L or less, and the pretreatment process includes ultrafiltration membrane treatment, and the ultrafiltration membrane is the porous membrane described above.
[0053] The freshwater production method of the present invention is implemented in a freshwater production system in which water to be treated 401 is pretreated using an ultrafiltration membrane, then treated using a reverse osmosis membrane 402 and separated into permeate 403 and concentrate 404. Examples of water to be treated include seawater, brine, river water, lake water, groundwater, sewage, and secondary sewage treatment water. Because the water to be treated contains solid components such as suspended solids, if it is directly filtered using a reverse osmosis membrane, many solid components will adhere to the membrane surface, causing a sudden increase in differential pressure and making the system inoperable. For this reason, the water to be treated 401 is first treated in a pretreatment step 405 to produce reverse osmosis membrane feed water 406, which is then supplied to the reverse osmosis membrane.
[0054] In the present invention, in order to suppress the progression of reverse osmosis membrane fouling, the reverse osmosis membrane feed water 406 is supplied to the reverse osmosis membrane after pretreating the water to be treated 1 having a biopolymer concentration of 100 μg C / L or more to a biopolymer concentration of 75 μg C / L or less. It is more preferable to pretreat the water to be treated 401 having a biopolymer concentration of 100 μg C / L or more to a biopolymer concentration of 50 μg C / L or less and supply the reverse osmosis membrane feed water 406 to the reverse osmosis membrane. On the other hand, since pretreating the water to be treated 401 having a biopolymer concentration of 100 μg C / L or more to a biopolymer concentration of less than 20 μg C / L requires a great deal of energy and cost, it is preferable to supply the reverse osmosis membrane feed water 406 to the reverse osmosis membrane after pretreating the water to be treated 401 having a biopolymer concentration of 100 μg C / L or more to a biopolymer concentration of less than 20 μg C / L.
[0055] Biopolymers are hydrophilic organic polymers (polysaccharides, proteins, etc.) with a molecular weight of approximately 10 to 20 kDa or more. The definition and measurement method of biopolymers are described, for example, in Huber, S.A., Balz, A., Abert, M., Pronk, W., 2011. Characterization of aquatic humic and non-humic matter with size-exclusion chromatography, organic carbon detection, organic carbon detection, and organic nitrogen detection (LC-OCD-OND). As described in Water Research 45(2), 879-885, TOC can be measured by organic carbon exclusion chromatography (LC-OCD). Here, the LC-OCD method is an analytical method in which TOC components in a sample are fractionated by molecular weight and displayed as a chromatogram. On the chromatogram, organic substances with higher molecular weights and hydrophilicity tend to have shorter retention times. Measurement conditions for the LC-OCD method include a 250 mm x 20 mm TSK HW50S column, a flow rate of 1.1 mL / min, a sample injection volume of 1 mL, a UV wavelength of 254 nm, an acid injection volume into the OCD meter of 0.2 mL / min, a pH 6.85 phosphate buffer as the eluent, and an acidifying solution prepared by adding 4 mL of 85% O-phosphoric acid and 0.5 g of potassium peroxodisulfate to 1 L of ultrapure water. As a measuring device used in the LC-OCD method, for example, an LC-OCD device (manufactured by DOC-Labar) in which a wet total organic carbon meter (OCD meter) is connected to a high performance liquid chromatograph (HPLC) can be used.
[0056] The porous membrane of the present invention can be used as an ultrafiltration membrane. That is, in the water production method of the present invention, the ultrafiltration membrane is a porous membrane containing polyvinylidene fluoride resin, which has a surface A and a surface B, and in the ATR method (attenuated total reflection method) of surface A, α-type structure crystals (H α ) and β-type structure crystals (H β) ratio (H α / H β ) is 0 or more and 0.50 or less, and the pure water permeability is 0.25 m 3 / m 2 / h / 50kPa or more 1.2m 3 / m 2 / h / 50 kPa or less, and the average surface pore size on surface A of the porous membrane is 5.0 nm or more and 12.0 nm or less.
[0057] As an ultrafiltration membrane, a porous membrane with a 40,000 Da dextran rejection rate of 45% to 80% is preferred. A dextran rejection rate of 45% to 80% prevents coarse contaminants and substances to be removed in the raw filtrate from penetrating the membrane, demonstrating excellent fouling resistance. Furthermore, the membrane's biopolymer rejection rate is likely to be high, allowing for reduced or no flocculant addition, thereby achieving a biopolymer concentration of 75 μg C / L or less in the reverse osmosis membrane feed water. "Flocculant-free water treatment" means that no flocculant is added to the water treatment, i.e., the water treatment does not use a flocculant. The type of flocculant is not limited as long as it aggregates biopolymers, and the flocculant concentration corresponds to 0% to 0.05%. In particular, an ultrafiltration membrane with a dextran rejection rate of 45% to 80%, or even 50% to 80%, is particularly preferred.
[0058] The reverse osmosis membrane 2 may be made of any material that can reduce the salt concentration so that the treated water can be used as drinking water, industrial water, municipal water, etc., but examples include membranes made of cellulose acetate-based or polyamide-based materials. Among these, membranes made of polyamide-based materials are particularly effective in the method of the present invention. Polyamide-based membranes have low resistance to chlorine, which is the most commonly used disinfectant to prevent biofilm growth, and even small concentrations of chlorine cause significant membrane deterioration, making it difficult to prevent biofouling. Therefore, the effects of implementing the present invention are particularly pronounced.
[0059] The lower the rate of decrease in permeability of the reverse osmosis membrane, the longer the interval between chemical cleanings of the reverse osmosis membrane and the less frequently it is replaced. Furthermore, when the reverse osmosis membrane is operated at a low flow rate, the increase in operating differential pressure can be suppressed. This is preferable because it reduces the number of reverse osmosis membranes required for freshwater production. The rate of decrease in permeability of the reverse osmosis membrane is preferably 0.20 (% / hr) or less, and more preferably 0.18 (% / hr) or less.
[0060] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. First, measurement methods and evaluation methods are described below.
[0061] (i) Measurement of the ratio of α-type structure crystals to β-type structure crystals in the crystalline portion of PVDF resin Using Shimadzu Corporation's IRTracer-100, the ATR method (total reflection measurement method) was performed at a resolution of 8 cm -1 The IR spectrum of the film surface was measured at 763 cm in the measured area and the obtained spectrum. -1 The peak height (H α ) and 840 cm -1 The peak height (H β ) and the ratio of α-type structure crystals to β-type structure crystals was calculated using the following formula:
[0062] Ratio of α-type / β-type structure crystals = H α / H β ...Formula (1).
[0063] (ii) Pure water permeability A small module of about 10 cm in length consisting of about 1 to 10 hollow fiber membranes was prepared, and distilled water was fed from surface A under the conditions of a temperature of 25°C and a filtration differential pressure of 18.6 kPa, and the total amount was filtered. 3 ) and the obtained value is expressed as a unit time (hr) and a unit effective membrane area (m 2 ), and calculated in terms of per 50 kPa.
[0064] (iii) Method for Evaluating the Removal Rate of Dextran with a Weight-Average Molecular Weight of 40,000 Da: Dextran (manufactured by Aldrich; weight-average molecular weight of 40,000 Da) was mixed with 1,000 ppm distilled water to prepare an aqueous dextran solution. The prepared aqueous dextran solution was supplied to a porous membrane at 25°C so that the transmembrane pressure difference was 10 kPa, and cross-flow filtration was performed at a cross-flow linear velocity of 1.0 m / sec, and the permeate was sampled. At the same time as the permeate was sampled, the aqueous dextran solution (stock solution) supplied to the porous membrane was also sampled. The refractive indices of the permeate and stock solutions were measured, and the removal rate: T was calculated based on equation (2): T = {(refractive index of stock solution) - (refractive index of permeate solution)} / (refractive index of stock solution) × 100 (equation (2)).
[0065] (iv) Measurement of the crystallinity of the polymer resin constituting the porous membrane This section describes the measurement of the crystallinity of the polymer resin of a porous membrane in the form of a hollow fiber membrane. For the measurement, a section within 50 μm from the outer surface of the hollow fiber membrane was used. The outer surface of the hollow fiber membrane was cut using a commercially available freezing microtome (Leica; Jung CM3000) to obtain a sample. The hollow fiber membrane immersed in distilled water was frozen at -20 ° C using a freezing microtome (Leica; Jung CM3000), and a blade was placed parallel to the surface of the hollow fiber membrane. First, the hollow fiber membrane was cut once by moving the blade close to it at 5 μm intervals. Then, the movement distance was set to 40 μm, and cutting was performed once more to obtain a hollow fiber membrane section 40 to 45 μm thick from the surface. When a slice was set in a DSC (SEIKO DSC6200) and the temperature was raised from room temperature to 300°C at a rate of 5°C / min, the endothermic peak of each polymer resin was regarded as the heat of fusion, and this heat was divided by the heat of fusion of the complete crystal of the polymer resin to calculate the percentage. For example, for polyvinylidene fluoride resin, the endothermic peak observed in the range of 100 to 190°C was regarded as the heat of fusion of the polyvinylidene fluoride resin, and this heat was divided by 104.6 J / g, which is the heat of fusion of the complete crystal of the polyvinylidene fluoride resin, to calculate the percentage.
[0066] (v) Regarding the surface structure of the surface portion (pore size, number, standard deviation) After vacuum drying the porous membrane overnight at 25 ° C., it was observed at a magnification of 30,000 to 100,000 times using an SEM (Hitachi High-Technologies Corporation; S-5500). The image obtained by observing the surface of the porous membrane with an SEM was binarized using the free software "ImageJ". When binarizing, after setting Subtract Background to 1 pixel and selecting Create Background, the condition: RenyiEntropy was selected as the Threshold (binarization threshold). In the obtained binarized image, the area of each hole was determined by selecting Area in Analyze Particles, and the diameter calculated assuming each hole to be a circle was used as the surface pore size. When determining the average surface pore size, the pore sizes of 1,000 or more holes were averaged. Similarly, the standard deviation of each surface pore size was determined, and the number of pores was divided by the area of the observed region to obtain the number of pores per unit area.
[0067] (vi) Self-Diffusion Coefficient of Polymer The self-diffusion coefficient was determined by all-atom molecular dynamics calculations. A polymer solution system was prepared to achieve the actual polymer concentration (wt%). A single model polymer chain was modeled to have a molecular weight of 800 to 6,000, and 1 / 200 to 1 / 5 of the weight-average molecular weight of the polymer actually used. GAFF2 was used as the potential parameter for the molecular dynamics calculations. A constant pressure-temperature ensemble was constructed by controlling the temperature to 25°C and the pressure to 1 bar. Short-range Lennard-Johns interactions were handled by applying a switch function starting from 1.0 nm and cutting off at 1.2 nm. Long-range electrostatic interactions were calculated using the Particle Mesh Ewald method. After performing molecular dynamics calculations in the constant pressure-temperature ensemble until the density was constant, the unit cell length was adjusted to achieve the average density, and an additional 11 ns of calculations were performed in the constant temperature ensemble. Using a 10 ns trajectory, the mean square displacement (MSD) of each atom in the polymer was determined, and the self-diffusion coefficient was calculated from the following formula (3). At this time, it was confirmed that the range of MSD and t used to calculate D was between 0.9 and 1.1, where log(MSD) divided by log(t). When multiple types of polymers were mixed to make a polymer solution, the self-diffusion coefficient of each polymer was weighted and averaged based on the weight percentage of the polymer, and this was used as the self-diffusion coefficient of the polymer in the polymer solution. D = MSD / 6t Formula (3) D: self-diffusion coefficient t: time
[0068] (vii) Method for evaluating filtration of chemical factory wastewater Chemical factory wastewater (TOC: 30 mg / L, turbidity: 11 NTU) was supplied to the porous membrane at 25°C so that the transmembrane pressure difference was 100 kPa, and the total amount was filtered, and the permeate volume was measured. 2 When this occurs, the reverse filtration permeation rate is set to 3 L / m so that the transmembrane pressure difference is 150 kPa. 2 Filtration and backfiltration were repeated until the filtration flux (F1) immediately after the start of filtration and the amount of permeated liquid per unit area reached 400 L / m 2The ratio of the filtration flux immediately after the start of filtration (F2) after the filtration reached or exceeded the above value (F2 / F1) to the initial ratio of the filtration flux was calculated. The closer the initial ratio of the filtration flux is to 1, the more the initial characteristics are maintained, and the porous membrane is less likely to clog even after long-term use, and a guideline for good filtration is 50% or more.
[0069] (viii) Cross-sectional structure of the outermost surface (presence or absence of nanomesh structure, pore size, number, standard deviation) A porous membrane embedded in a commercially available embedding medium for preparing frozen tissue sections (Tissue-Tec; O.C.T. Compound) was used to prepare 100 nm thick sections of the porous membrane perpendicular to the surface at -40°C using a cryo-ultramicrotome (Leica; FC7), and the sections were then vacuum dried at room temperature for 12 hours. The cross section of the outermost surface of the porous membrane was observed using a TEM (JEOL; JEM-1400Plus), and images were binarized using the free software "ImageJ." For binarization, the threshold (binarization threshold) condition: Minimum was selected. In the obtained binarized image, the area of each pore was determined by selecting Area in Analyze Particles, and the diameter calculated assuming each pore to be a circle was used as the cross-sectional pore diameter.
[0070] When determining the average cross-sectional pore size, the pore sizes of 1,000 or more pores are averaged. The number of cross-sectional pores is divided by the area of the analyzed region to determine the number of pores per unit area. As with the pore size, an image containing 1,000 or more pores is analyzed and calculated. Similarly, the standard deviation of each cross-sectional pore size is determined. The total perimeter of the cross-sectional pore size is determined by binarizing the TEM image of the cross-section of the porous membrane as described above, selecting Perim in Analyze Particles, and determining the perimeter of each pore, and dividing the sum by the area of the observed region. Within the surface portion of the porous membrane, the outermost surface portion from the surface to a thickness of 2 μm has an average cross-sectional pore size [nm] in the cross-section of the outermost surface portion of 1 nm to 99 nm, and the number of cross-sectional pores is 100 / μm. 2 ~1000 pieces / μm 2 When the mesh structure was larger than 100%, it was judged to have a nanomesh structure.
[0071] (ix) Biopolymer concentration, biopolymer removal rate The biopolymer concentrations of the treated water and the reverse osmosis membrane feed water were determined using the method described in Huber, S.A., Balz, A., Abert, M., Pronk, W., 2011. Characterization of aquatic humic and non-humic matter with size-exclusion chromatography, organic carbon detection, organic carbon detection, and organic nitrogen detection (LC-OCD-OND). The organic carbon detection exclusion chromatography (LC-OCD) method was used as described in Water Research 45(2), 879-885. A 250 mm x 20 mm TSK HW50S column was used, with a flow rate of 1.1 mL / min, a sample injection volume of 1 mL, a UV wavelength of 254 nm, and an acid injection volume of 0.2 mL / min into the OCD analyzer. The eluent was a pH 6.85 phosphate buffer, and the acidification solution consisted of 4 mL of 85% O-phosphoric acid and 0.5 g of potassium peroxodisulfate per 1 L of ultrapure water.
[0072] (x) Permeability Decrease Rate of Reverse Osmosis Membrane The reverse osmosis membrane was operated at a pressure of 5.5 MPa and a recovery rate of 37%. The recovery rate was calculated by the formula: (flow rate of reverse osmosis membrane permeate) / (flow rate of reverse osmosis membrane permeate + flow rate of reverse osmosis membrane concentrate) x 100. The permeability decrease rate of the reverse osmosis membrane was calculated based on the formula (4) using the permeate flow rate 1 hour after the start of reverse osmosis membrane operation and the flow rate 50 hours after the start of operation. Here, the amount of permeate (g) permeated over 5 minutes was used for each flow rate. Permeability decrease rate of reverse osmosis membrane [% / hr] = (amount of permeate [g] 51 hours after the start of operation) / (amount of permeate [g] 1 hour after the start of operation) / 50 x 100... formula (4).
[0073] (xi) Ultrafiltration membrane initial water permeability ratio The water to be treated was supplied to the ultrafiltration membrane so that the transmembrane pressure difference was 100 kPa, and the total amount was filtered, and the permeate volume was measured. When the permeate volume reached 28 L / m 2 , backfiltration was performed until the backfiltration permeate volume reached 3 L / m 2 so that the transmembrane pressure difference was 150 kPa. Filtration and backfiltration were repeated, and the permeate flow rate F1 (g) immediately after the start of filtration with the ultrafiltration membrane and the permeate flow rate F2 (g) immediately after the start of filtration after the permeate volume per unit area reached 400 L / m 2 or more were measured. Here, the permeate volume (g) for 5 minutes was used for each flow rate, and the ratio of the permeate flow rates (F2 / F1) was calculated and used as the initial water permeability ratio.
[0074] Example 1 The porous membrane used was a hollow fiber porous membrane containing a support obtained by the following manufacturing method. 38% by mass of PVDF (KF1300 manufactured by Kureha Corporation, weight-average molecular weight 350,000 Da) and 62% by mass of γ-butyrolactone were mixed and dissolved at 160°C to prepare a support membrane stock solution. This support membrane stock solution was discharged from a double-tube nozzle while accompanying an 85% by mass aqueous γ-butyrolactone solution as a hollow-portion-forming liquid. The discharged support membrane stock solution was solidified in a cooling bath containing an 85% by mass aqueous γ-butyrolactone solution at 20°C and placed 30 mm below the nozzle, to produce a hollow fiber support having a spherical structure.
[0075] A polymer solution having the composition shown in Table 1 was prepared by mixing 12% by mass of PVDF1 (Kynar (registered trademark) 710 manufactured by Arkema, weight average molecular weight 180,000 Da), 4.8% by mass of cellulose diacetate (manufactured by Eastman Co.; CA-398-3), 2.4% by mass of cellulose triacetate (manufactured by Eastman Co.; CA-436-80S), 68.7% by mass of NMP, and 12.1% by mass of 2P and stirring at 120°C for 4 hours.
[0076] Next, the polymer solution was uniformly applied to the outer surface of the hollow fiber support at 10 m / min (thickness: 50 μm). One second after application, the support to which the polymer solution was applied was immersed in a coagulation bath of distilled water at 35°C for 10 seconds to coagulate, forming a porous membrane with a three-dimensional network structure. The evaluation results of the obtained porous membrane are shown in Table 1. The surface portion of the porous membrane from the surface to a thickness of 10 μm was denser than the interior. Figure 5 shows an image of the cross section of the outermost surface portion of the porous membrane observed with a TEM. It was determined to have a nanomesh structure from the cross-sectional pore diameter and the number of cross-sectional pores. The H of the obtained porous membrane α / H β is 0.37, and pure water permeability is 0.43 m 3 / m 2 / h / 50 kPa, and the dextran removal rate was good at 55%. The crystallinity of the outer surface resin was also high at 49%. Furthermore, the value X obtained by dividing the number of surface pores by the average surface pore size was 66, the average surface pore size was 7.2 nm, and the standard deviation was 2.5. (vii) When the long-term stability was evaluated using the industrial wastewater filtration evaluation method, the permeate flow rate was 400 L / m 2 The initial ratio (F2 / F1) of the filtration flux after (F2) to that immediately after the start of filtration (F1) was 0.63, and the filtration flux was maintained even after long-term use.
[0077] (Example 2) A porous membrane was obtained in the same manner as in Example 1, except that NMP in the polymer solution was changed to DMSO and the distilled water in the coagulation bath was set to 40°C. The evaluation results of the porous membrane are shown in Table 1. The surface portion of the porous membrane up to a thickness of 10 μm from the surface was denser than the inside. α / H β is 0.27, and pure water permeability is 0.29 m 3 / m 2 / h / 50 kPa, the dextran removal rate was good at 63%.
[0078] Furthermore, X was 78, the average surface pore size was 7.3 nm, and the standard deviation was 1.8. (vii) When the long-term stability was evaluated by the industrial wastewater filtration evaluation method, the permeate flow rate was 400 L / m 2 The initial ratio (F2 / F1) of the filtration flux after (F2) to that immediately after the start of filtration (F1) was 0.55, and the filtration flux was maintained even after long-term use.
[0079] (Example 3) A porous membrane was obtained in the same manner as in Example 1, except that NMP in the polymer solution was changed to DMF and the distilled water in the coagulation bath was set to 25°C. The evaluation results of the porous membrane are shown in Table 1. The surface portion of the porous membrane up to a thickness of 10 μm from the surface was denser than the inside. α / H β is 0.24, and pure water permeability is 0.45m 3 / m 2 / h / 50 kPa, the dextran removal rate was good at 47%.
[0080] Furthermore, X was 48, the average surface pore size was 8.5 nm, and the standard deviation was 3.1. (vii) When the long-term stability was evaluated by the industrial wastewater filtration evaluation method, the permeate flow rate was 400 L / m 2 The initial ratio (F2 / F1) of the filtration flux after (F2) to that immediately after the start of filtration (F1) was 0.50, and the filtration flux was maintained even after long-term use.
[0081] (Comparative Example 1) A porous membrane was obtained by the same membrane production as in Example 1, except that the solvent in the polymer solution was changed to NMP and the composition ratio was changed. The evaluation results of the porous membrane are shown in Table 2. The porous membrane did not have a nanomesh structure. The surface portion of the porous membrane from the surface to a thickness of 10 μm was denser than the inside. The H of the obtained porous membrane α / H β is 1.0, and pure water permeability is 0.41 m 3 / m 2 / h / 50 kPa, and the dextran removal rate was 55%. Furthermore, X was 13, the average surface pore size was 15 nm, and the standard deviation was 6.0. The crystallinity of the outer surface resin was low at 11%. (vii) When the long-term stability was evaluated using the industrial wastewater filtration evaluation method, the permeate flow rate was 400 L / m 2 The initial ratio (F2 / F1) of the filtration flux after (F2) to that immediately after the start of filtration (F1) was 0.38, and the filtration flux could not be maintained after long-term use.
[0082] (Comparative Example 2) A porous membrane was obtained in the same manner as in Comparative Example 1, except that the coagulation bath temperature was set to 6°C. The evaluation results of the porous membrane are shown in Table 2. The surface portion of the porous membrane from the surface to a thickness of 10 µm was denser than the inside. α / H β is 0.10, pure water permeability is 0.10m 3 / m 2 / h / 50 kPa, and the dextran removal rate was 70%, which did not satisfy the conditions. Furthermore, X was 10, the average surface pore size was 8.0 nm, and the standard deviation was 1.9. (vii) When the long-term stability was evaluated using the industrial wastewater filtration evaluation method, the permeate flow rate was 400 L / m 2 The initial ratio (F2 / F1) of the filtration flux after (F2) to that immediately after the start of filtration (F1) was 0.37, and the filtration flux could not be maintained after long-term use.
[0083] (Comparative Example 3) A porous membrane was obtained by the same membrane production as in Comparative Example 1, except that in the membrane production of Example 1, PVDF1 in the polymer solution was changed to PVDF2 (Solef9009 manufactured by Solvay) and the composition ratio was changed. The evaluation results of the porous membrane are shown in Table 2. The porous membrane did not have a nanomesh structure. The surface portion of the porous membrane from the surface to a thickness of 10 μm was denser than the inside. H of the obtained porous membrane α / H β is 0.22, and pure water permeability is 0.21 m 3 / m 2 / h / 50 kPa, and the dextran removal rate was 57%. Furthermore, X was 7.6, the average surface pore size was 10 nm, and the standard deviation was 4.1, which did not satisfy the conditions. (vii) When the long-term stability was evaluated using the industrial wastewater filtration evaluation method, the permeate volume was 400 L / m 2 The initial ratio (F2 / F1) of the filtration flux after (F2) to that immediately after the start of filtration (F1) was 0.40, and the filtration flux could not be maintained after long-term use.
[0084] (Comparative Example 4) A polymer solution was prepared by mixing 20% by mass of PVDF3 (Kureha Corporation; KF polymer #110, weight average molecular weight 280,000 Da) and 80% by mass of a mixed solvent (DMAc:GBL = 89:11) and stirring at 120°C for 4 hours. A porous membrane was obtained by film formation in the same manner as in Example 1, except that the distilled water in the coagulation bath was set to 21°C. The evaluation results of the porous membrane are shown in Table 2. The H of the obtained porous membrane α / H β is 0.63, and pure water permeability is 0.022 m 3 / m 2 / h / 50 kPa, and the dextran removal rate was 66%, which did not satisfy the conditions. Furthermore, X was 0.90, the average surface pore size was 15 nm, and the standard deviation was 8.5. (vii) When the long-term stability was evaluated using the industrial wastewater filtration evaluation method, the amount of permeate was extremely small, making it difficult to measure the filtration flux.
[0085] (Example 4) Using the flow chart shown in Figure 6, permeated water through a reverse osmosis membrane was produced from water to be treated. Specifically, seawater 1 (biopolymer concentration 122 μg C / L) was used as the water to be treated, and the porous membrane of Example 1 was used for pretreatment. As a result, the biopolymer concentration of the reverse osmosis membrane feed water was 35 μg C / L. This reverse osmosis membrane feed water was pressurized with a high-pressure pump and filtered through the reverse osmosis membrane to obtain permeated water. The reverse osmosis membrane was made of polyamide, had a salt rejection rate of 99.8%, and had a membrane area of 37 m. 2 It was a spiral-type reverse osmosis membrane.
[0086] Here, the initial permeability ratio of the ultrafiltration membrane was 0.71, and the permeability reduction rate of the reverse osmosis membrane was 0.15% / hr. Despite the high concentration of biopolymer in the treated water, filtration through the ultrafiltration membrane and reverse osmosis membrane was stable without the use of a coagulant. The results are shown in Table 3.
[0087] (Example 5) Using the flow chart shown in Figure 6, permeated water from the water to be treated was produced through a reverse osmosis membrane. Specifically, seawater 2 (biopolymer concentration 218 μg C / L) was used as the water to be treated, and the porous membrane of Example 1 was used for pretreatment. As a result, the biopolymer concentration of the reverse osmosis membrane feed water was 47 μg C / L. This reverse osmosis membrane feed water was pressurized with a high-pressure pump and filtered through the reverse osmosis membrane to obtain permeated water. The reverse osmosis membrane was made of polyamide, had a salt rejection rate of 99.8%, and had a membrane area of 37 m. 2 It was a spiral-type reverse osmosis membrane.
[0088] Here, the initial permeability ratio of the ultrafiltration membrane was 0.63, and the permeability reduction rate of the reverse osmosis membrane was 0.18% / hr. Despite the very high biopolymer concentration in the treated water, filtration through the ultrafiltration membrane and reverse osmosis membrane was stable without the use of a coagulant. The results are shown in Table 3.
[0089] (Comparative Example 5) Using the flow chart shown in Figure 6, permeated water from the water to be treated was produced through a reverse osmosis membrane. Specifically, seawater 1 (biopolymer concentration 122 µg C / L) was used as the water to be treated, and the porous membrane of Comparative Example 1 was used for pretreatment. As a result, the biopolymer concentration of the water fed to the reverse osmosis membrane was 85 µg C / L. This water fed to the reverse osmosis membrane was pressurized with a high-pressure pump and filtered through the reverse osmosis membrane to obtain permeated water. The reverse osmosis membrane was made of polyamide, had a salt rejection rate of 99.8%, and had a membrane area of 37 m. 2 It was a spiral-type reverse osmosis membrane.
[0090] The initial water permeability ratio of the ultrafiltration membrane was 0.53, and the water permeability decrease rate of the reverse osmosis membrane was 0.25% / hr, indicating that the rate of decrease in permeability of the reverse osmosis membrane was large. The results are shown in Table 3.
[0091] (Comparative Example 6) Using the flow chart shown in Figure 6, permeated water from the water to be treated was produced through a reverse osmosis membrane. Specifically, seawater 2 (biopolymer concentration 218 µg C / L) was used as the water to be treated, and the porous membrane of Comparative Example 1 was used for pretreatment. As a result, the biopolymer concentration of the reverse osmosis membrane feed water was 139 µg C / L. This reverse osmosis membrane feed water was pressurized with a high-pressure pump and filtered through the reverse osmosis membrane to obtain permeated water. The reverse osmosis membrane was made of polyamide, had a salt rejection rate of 99.8%, and had a membrane area of 37 m. 2It was a spiral-type reverse osmosis membrane.
[0092] The initial permeability ratio of the ultrafiltration membrane was 0.45, and the rate of decrease in permeability of the reverse osmosis membrane was 0.45% / hr. This was probably due to the very high concentration of biopolymer in the treated water, and the decrease in permeability of the ultrafiltration membrane was large, and the rate of decrease in permeability of the reverse osmosis membrane was also significantly large. The results are shown in Table 3.
[0093]
[0094]
[0095]
[0096] 101 Porous membrane 102 Surface portion 103 Inside 201 Coarse dirt components 202 Fine dirt components 300 Polymer solution 301 Polymer-rich phase 302 Solvent-rich phase FL Filtration direction 401 Water to be treated 402 Reverse osmosis membrane 403 Permeated water 404 Concentrated water 405 Pretreatment step 406 Water supplied to reverse osmosis membrane 407 High-pressure pump 408 Liquid supply pump 409 Supply pump 410 Detergent 411 Bactericide
Claims
1. A porous membrane containing polyvinylidene fluoride resin, one surface of which is surface A and the other surface of which is surface B, and the α-type structure crystal (H) in the crystalline portion of the polyvinylidene fluoride resin measured on surface A by an ATR method (attenuated total reflection measurement method) α ) and β-type crystals (H β ) ratio (H α / H β The ratio of (a) is 0 or more and 0.50 or less, The pure water permeability of the porous membrane is 0.25 m 3 / m 2 / h / 50kPa or more 1.2m 3 / m 2 / h / 50 kPa or less, an average surface pore diameter of the surface pores on the surface A of the porous membrane is 5.0 to 12.0 nm, and a value X obtained by dividing the number of surface pores [holes / μm 2 ] on the surface A of the porous membrane by the average surface pore diameter [nm] of the surface pores is 30 holes / μm 2 / nm or more and 100 holes / μm 2 / nm or less.
2. 2. The porous membrane according to claim 1, wherein the crystallinity of the polyvinylidene fluoride resin on the surface A of the porous membrane is 30% or more.
3. 3. The porous membrane according to claim 1, wherein the removal rate of 40,000 Da dextran by the porous membrane is 45% or more and 80% or less.
4. 3. The porous membrane according to claim 1, wherein the standard deviation of the surface pore diameters on surface A of the porous membrane is 1.0 nm or more and 5.0 nm or less.
5. 3. The porous membrane according to claim 1, wherein a surface portion of the porous membrane ranging from surface A to a thickness of 10 μm is denser than an interior portion.
6. A method for filtering a liquid using the porous membrane according to claim 1 or 2.
7. A membrane filtration device comprising the porous membrane according to claim 1 or 2.
8. A fresh water production method including a pretreatment step of pretreating water to obtain reverse osmosis membrane feed water, and a reverse osmosis membrane treatment step of filtering the reverse osmosis membrane feed water through a reverse osmosis membrane to obtain permeated water, the water to be treated has a biopolymer concentration of 100 μg C / L or more, the reverse osmosis membrane feed water has a biopolymer concentration of 75 μg C / L or less obtained by the pretreatment step, and the reverse osmosis membrane feed water is supplied to the reverse osmosis membrane treatment step, The pretreatment step has an ultrafiltration membrane treatment section equipped with an ultrafiltration membrane, The method for producing fresh water, wherein the ultrafiltration membrane is the porous membrane according to claim 1 or 2.
9. The number of surface pores on the surface A of the porous membrane is 200 / μm 2 More than 2000 pieces / μm 2 The fresh water production method according to claim 8, wherein the following is true: