Laminate and packaging bag

JPWO2024135533A5Active Publication Date: 2024-11-19TOPPAN HOLDINGS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024529796
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-05-20
Publication Date
2024-11-19
Estimated Expiration
2043-12-14

AI Technical Summary

Technical Problem

Conventional multi-material packaging laminates face challenges in heat sealing due to similar melting points of innermost and outermost polypropylene layers, leading to narrow heat sealing temperature margins, which can result in distortion, reduced seal strength, and decreased productivity.

Method used

A laminate structure with a base layer, intermediate layer, and sealant layer all made of polypropylene, where the base layer has a softening temperature above 200°C and the sealant layer below 150°C, and the difference between their softening temperatures is greater than 53°C, ensuring a wider heat sealing temperature margin and improved sealing performance.

Benefits of technology

The laminate provides a wider heat sealing temperature margin, maintaining sufficient sealing strength and minimizing thermal shrinkage, thus enhancing the stability and productivity of packaging bags.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A laminate comprising at least a substrate layer, an intermediate layer, and a sealant layer, wherein: the substrate layer is disposed on one outermost surface of the laminate, and the sealant layer is disposed on the other outermost surface of the laminate; the substrate layer, the intermediate layer, and the sealant layer all contain polypropylene; an inorganic oxide layer and a gas barrier coating layer are provided to the intermediate-layer-side surface of the substrate layer or to at least one surface of the intermediate layer; and T1 and T2 meet the conditions indicated below, where T1 is the softening temperature at the substrate-layer surface measured through local thermal analysis (LTA) of the substrate layer, and T2 is the softening temperature at the sealant-layer surface measured in the same manner. T1 > 200ºC; T2 < 150ºC
Need to check novelty before this filing date? Find Prior Art

Description

Laminate and packaging bag

[0001] The present disclosure relates to a laminate and a packaging bag.

[0002] BACKGROUND ART Laminates are known that include a biaxially oriented PET (polyethylene terephthalate) film, which has excellent heat resistance and toughness, as a base film and a polyolefin film, such as polyethylene or polypropylene, as a sealant layer (see, for example, Patent Document 1).

[0003] Japanese Patent Application Laid-Open No. 2017-178357

[0004] As the issue of plastic waste gains global attention, the demand for environmentally friendly packaging materials is increasing as efforts to realize a circular economy are underway. Many global companies have set goals for better plastic resource circulation and are implementing various measures regarding packaging materials. Furthermore, the United States has begun to establish recycling routes for PE (polyethylene), from collection to reuse. Globally, efforts toward mono-material recycling are accelerating. This means that there is a growing demand for mono-material packaging laminates, which have traditionally been made by combining various different materials to achieve high performance.

[0005] When converting conventional multi-material packaging materials for retort pouches into mono-material packaging materials, it is possible to consider switching to packaging materials made solely of PP (polypropylene) from the perspective of sealant properties. However, when converting packaging materials into mono-materials, the melting points of the innermost layer (the layer closest to the contents) and the outermost layer become very close.

[0006] Since the outermost layer is the part that is most exposed to heat in the heat-sealing step during bag production, a film that is difficult to heat-seal is used for the outermost layer, but when high temperatures are applied to fuse the sealant, which is the innermost layer, in the heat-sealing step, the outermost layer is deformed by heat shrinkage, causing problems such as bag distortion, reduced transportability, and reduced workability when filling the contents. Therefore, with a laminate using polypropylene for the innermost and outermost layers, the range (tolerance) of heat-sealing temperatures that can suppress heat shrinkage of the laminate while ensuring sufficient seal strength is narrow, and even a slight deviation in the heat-sealing temperature from the specified value is likely to cause a decrease in seal strength or heat shrinkage, resulting in a problem that the mass productivity of packaging bags is likely to decrease.

[0007] The present disclosure has been made in consideration of the above circumstances, and aims to provide a laminate using polypropylene for the innermost and outermost layers, which can widen the tolerance for heat sealing temperature, and a packaging bag using the same.

[0008] In order to solve the above problems, the present disclosure provides the following laminate and packaging bag: [1] A laminate including at least a base material layer, an intermediate layer, and a sealant layer, wherein the base material layer is disposed on one outermost surface of the laminate and the sealant layer is disposed on the other outermost surface, the base material layer, the intermediate layer, and the sealant layer all contain polypropylene, and an inorganic oxide layer and a gas barrier coating layer are provided on the surface of the base material layer facing the intermediate layer or on at least one surface of the intermediate layer, and the softening temperature of the surface of the base material layer measured by local thermal analysis (LTA) is T 1 , the softening temperature of the sealant layer surface is T 2 When this is done, T 1 and T 2 A laminate that satisfies the following conditions: 1 >200℃ T 2 <150 ° C [2] T 1 and T 2 The laminate according to the above [1], which satisfies the following conditions: (T 1 -T 2) > 53°C [3] The laminate according to the above [1] or [2], wherein when the sealant layers of the laminate are placed opposite each other and heat-sealed using a heat sealer made of metal on the upper side and silicone rubber on the lower side under conditions of an upper seal actual temperature of 145°C, a lower seal actual temperature of 90°C, a sealing pressure of 0.3 MPa, and a heating time of 1 second, the resulting seal strength of the sealed portion is 20 N / 15 mm or more. [4] The laminate according to any of the above [1] to [3], wherein when the sealant layers of the laminate are placed opposite each other and heat-sealed using a heat sealer made of metal on the upper side and silicone rubber on the lower side under conditions of an upper seal actual temperature of 160°C, a lower seal actual temperature of 90°C, a sealing pressure of 0.3 MPa, and a heating time of 1 second, the resulting seal shrinkage of the sealed portion is less than 3%. [5] With the sealant layers of the laminate facing each other, a heat sealer with an upper metal sealer and a lower silicone rubber sealer is used to heat seal the laminate under the conditions of a lower seal temperature of 90°C, a sealing pressure of 0.3 MPa, and a heating time of 1 second, while varying the upper seal temperature. The lowest upper seal temperature at which the seal strength of the resulting seal reaches 20 N / 15 mm is defined as T L The maximum actual temperature of the upper seal at which the heat shrinkage rate of the resulting seal portion can be maintained at less than 3% is T H In this case, T H -T L The laminate according to any one of the above [1] to [4], wherein T 2 The laminate according to any one of the above [1] to [5], which satisfies the following condition: T 2 ≧135°C [7] The laminate according to any one of [1] to [6] above, wherein the base material layer and the intermediate layer, and the intermediate layer and the sealant layer are both bonded via an adhesive layer using a two-component curing urethane adhesive. [8] The laminate according to [7] above, wherein at least one of the base material layer and the intermediate layer, and the intermediate layer and the sealant layer are bonded via an adhesive layer using a solventless two-component curing urethane adhesive. [9] A packaging bag produced by forming the laminate according to any one of [1] to [8] above.

[0009] According to the present disclosure, it is possible to provide a laminate using polypropylene for the innermost and outermost layers, which can widen the tolerance for heat sealing temperature, and a packaging bag using the same.

[0010] FIG. 1 is a schematic cross-sectional view showing a laminate according to one embodiment.

[0011] Preferred embodiments of the present disclosure will be described in detail below, with reference to the drawings where appropriate. In the drawings, identical or corresponding parts are designated by the same reference numerals, and duplicate explanations will be omitted. Furthermore, the dimensional ratios of the drawings are not limited to those shown.

[0012] <Laminate> FIG. 1 is a schematic cross-sectional view showing a laminate according to one embodiment. The laminate 100 shown in FIG. 1 includes, in this order, a base layer 11, an intermediate layer 12, and a sealant layer 13. The base layer 11 and the intermediate layer 12, and the intermediate layer 12 and the sealant layer 13, may each be bonded with an adhesive layer S. The base layer, the intermediate layer, and the sealant layer all contain polypropylene. The base layer, the intermediate layer, and the sealant layer may each contain a polypropylene film. From the viewpoint of improving gas barrier properties against water vapor and oxygen, the laminate includes an inorganic oxide layer and a gas barrier coating layer on the surface of the base layer 11 facing the intermediate layer 12 or on at least one surface of the intermediate layer 12. The base layer 11 is disposed on one outermost surface of the laminate 100, and the sealant layer 13 is disposed on the other outermost surface of the laminate 100. The base layer 11 is also referred to as the outermost layer of the laminate 100 (the layer opposite the content side when used as a packaging bag). The sealant layer 13 is also referred to as the innermost layer of the laminate 100 (the layer on the content side when used as a packaging bag).

[0013] [Base layer 11] The base layer is a layer that serves as one of the supports and contains polypropylene. The base layer may contain a polypropylene film or may be made of a polypropylene film.

[0014] The polypropylene film may be an acid-modified polypropylene film obtained by graft-modifying polypropylene with an unsaturated carboxylic acid, an acid anhydride of an unsaturated carboxylic acid, an ester of an unsaturated carboxylic acid, or the like. Furthermore, polypropylene-based resins such as homopolypropylene resin (PP), propylene-ethylene random copolymer, propylene-ethylene block copolymer, and propylene-α-olefin copolymer can be used. Here, random copolymers and block copolymers tend to have a lower softening temperature due to the disruption of the regularity of their molecular structure caused by the inclusion of heterogeneous components. Therefore, the polypropylene constituting the base layer is preferably homopolypropylene.

[0015] The polypropylene film constituting the base layer may contain various additives such as a flame retardant, a slip agent, an antiblocking agent, an antioxidant, a light stabilizer, a tackifier, and an antistatic agent.

[0016] The polypropylene film constituting the base layer is preferably a stretched film from the viewpoints of impact resistance, heat resistance, water resistance, dimensional stability, etc. This can prevent the base layer from thermally fusing during the heat sealing process during bag production. Furthermore, the laminate can be more suitably used for applications requiring retort treatment or boiling treatment. The stretching method is not particularly limited, and any method can be used, such as inflation stretching, uniaxial stretching, or biaxial stretching, as long as it can provide a dimensionally stable film.

[0017] The thickness of the substrate layer is not particularly limited and can be set to 6 to 200 μm depending on the application, but may be 9 to 50 μm, 12 to 38 μm, or 18 to 30 μm from the viewpoint of reducing materials to reduce environmental impact and from the viewpoint of obtaining excellent heat resistance, impact resistance, and excellent gas barrier properties.

[0018] The surface of the substrate layer may be subjected to various pretreatments such as corona treatment, plasma treatment, and flame treatment within the range that does not impair the barrier performance, or a coating layer such as an easy-adhesion layer may be provided.

[0019] The substrate layer has a surface softening temperature T 1 (°C) must satisfy the following conditions: 1 >200℃ T 1 Since the temperature is higher than 200°C, the occurrence of thermal shrinkage and distortion of the laminate can be suppressed even when the heat sealing temperature is increased (for example, about 160°C). Therefore, the heat sealing temperature tolerance of the laminate can be widened. 1 T may be 201°C or higher, 203°C or higher, or 205°C or higher. 1 The upper limit is not particularly limited, but may be, for example, 220°C or less. The softening temperature of the substrate surface may be 200°C or more and 220°C or less, 201°C or more and 220°C or less, 203°C or more and 220°C or less, or 205°C or more and 220°C or less. The softening temperature of the substrate layer surface can be adjusted, for example, by the crystallinity, molecular weight, and copolymer blending ratio. The softening temperature can also be measured by differential scanning calorimetry (DSC), but the softening temperature measured by DSC is the softening temperature that includes information not only on the surface of the substrate layer or sealant layer, but also on other layers such as the intermediate layer. By measuring the softening temperature by LTA, the softening temperature of the surface of the substrate layer or sealant layer can be selectively measured.

[0020] The melting point (melting peak temperature) of the substrate layer measured by differential scanning calorimetry (DSC) may be greater than 161 ° C, greater than 163 ° C, or greater than 165 ° C. A melting point greater than 161 ° C tends to result in a desired surface softening temperature (greater than 200 ° C). The upper limit of the melting point is not particularly limited, but may be, for example, 180 ° C or less. The melting point of the substrate layer may be greater than 161 ° C and less than 180 ° C, greater than 163 ° C and less than 180 ° C, or greater than 165 ° C and less than 180 ° C. The melting point of the substrate layer can be adjusted, for example, by the crystallinity, molecular weight, and copolymer blending ratio. The melting point of the substrate layer can be measured using a differential scanning calorimeter (for example, Hitachi High-Tech Science Corporation, product name: DSC7000X) at a heating rate of 10 ° C / min.

[0021] [Softening Temperature Measurement Method] The softening temperature is the temperature at which a material such as a resin exhibits softening behavior. To evaluate the softening temperature in this embodiment, local thermal analysis (LTA) using an atomic force microscope is used. The sample is heated by applying a voltage to a cantilever equipped with a heater. In local thermal analysis (LTA), after measuring the shape of the sample, a constant force (contact pressure) is applied to the sample surface with the cantilever at a predetermined location. The sample is heated while maintaining the constant contact pressure. The softening temperature is calculated as the temperature at which the cantilever height (Z displacement) reaches its maximum due to the change in hardness of the sample surface before and after heating. The cantilever height changes due to the vertical rise of the cantilever caused by thermal expansion of the sample surface and the vertical fall of the cantilever caused by softening of the sample surface. In other words, the sample reaches its softening temperature just before the cantilever position begins to fall. Therefore, by converting the voltage applied to the heater of the cantilever when the height position of the cantilever is at its maximum into a temperature, it is possible to determine the softening temperature locally in the nanoscale region and near the surface.

[0022] The equipment used is an atomic force microscope (AFM) MFP-3D-SA (trade name) manufactured by Oxford Instruments, with a local thermal analysis option, Ztherm. The shape measurement uses AC mode (tapping mode), and the softening temperature measurement uses contact mode.

[0023] The cantilever used is an AN2-200 (trade name) manufactured by Anasys Instruments, with a spring constant of 0.5 to 3.5 N / m.

[0024] In measuring the softening temperature, the voltage application rate (temperature increase rate) of the cantilever is set to 0.5 V / sec.

[0025] In Ztherm, measurements are performed by controlling the contact pressure of the cantilever (change in cantilever deflection) at a constant value. However, because cantilever deflection changes with applied voltage even without contact with the sample, it is necessary to control the contact pressure after subtracting the cantilever deflection due to the applied voltage. Ztherm has a detrend correction function that acquires changes in cantilever deflection with applied voltage. The maximum applied voltage used for measurement is applied to the cantilever without the cantilever contacting the sample surface, and detrend correction is performed. In this embodiment, after shape measurement, detrend correction is performed at the maximum applied voltage used for measurement and a voltage application rate (heating rate) of 0.5 V / sec before softening temperature measurement, and then measurement is performed. The contact pressure is set to 0.5 V.

[0026] The set value for the downward displacement of the cantilever to stop the measurement is 50 nm.

[0027] The softening point is determined as the point where the vertical height (Z displacement) of the cantilever is maximum, and the applied voltage at this point is read.

[0028] To convert the applied voltage of the cantilever heater into a softening temperature, a calibration curve of applied voltage and melting point (peak melting temperature) is created. As calibration samples, samples whose melting points (peak melting temperatures) have already been measured using a differential scanning calorimeter (DSC) are used. The softening temperatures are measured at different measurement positions for each calibration sample, and a calibration curve is created by approximating the average applied voltage at the softening point and the melting point (peak melting temperature) with a cubic function using the least squares method. The calibration samples are polycaprolactone pellets (melting point: 60°C), low-density polyethylene pellets (melting point: 112°C), polypropylene pellets (melting point: 166°C), and biaxially stretched polyethylene terephthalate film (melting point: 255°C). Cross-sectional samples prepared in an environment below the glass transition temperature are used. An ultramicrotome and cryosystem are used to prepare cross-sectional samples, and cross-sections are cut in an environment of -80°C for polycaprolactone, -140°C for low-density polyethylene, -40°C for polypropylene, and room temperature 25°C for polyethylene terephthalate.

[0029] Using this calibration curve of applied voltage and melting point (melting peak temperature), the applied voltage at the softening point is converted into a temperature, which is taken as the softening temperature.

[0030] [Adhesion Layer] When the laminate has an inorganic oxide layer on a substrate layer, an adhesion layer (anchor coat layer) may be provided on the surface of the substrate layer on which the inorganic oxide layer is to be laminated. The adhesion layer is provided on the substrate layer, and can achieve two effects: improving the adhesion performance between the substrate layer and the inorganic oxide layer, and improving the smoothness of the substrate layer surface. The improved smoothness makes it easier to form the inorganic oxide layer uniformly without defects, and makes it easier to exhibit high barrier properties. The adhesion layer can be formed using an anchor coat agent.

[0031] Examples of anchor coating agents include polyester-based polyurethane resins, polyether-based polyurethane resins, etc. As the anchor coating agent, polyester-based polyurethane resins are preferred from the viewpoints of heat resistance and interlayer adhesive strength.

[0032] The thickness of the adhesive layer is not particularly limited, but is preferably in the range of 0.01 to 5 μm, more preferably in the range of 0.03 to 3 μm, and particularly preferably in the range of 0.05 to 2 μm. When the thickness of the adhesive layer is equal to or greater than the lower limit, more sufficient interlayer adhesive strength tends to be obtained, while when the thickness is equal to or less than the upper limit, desired gas barrier properties tend to be easily exhibited.

[0033] The method for applying the adhesive layer onto the substrate layer can be any known application method without any particular limitation, and examples thereof include an immersion method (dipping method), and methods using a spray, a coater, a printer, a brush, etc. In addition, examples of the types of coaters and printers used in these methods and the application methods thereof include gravure coaters such as direct gravure, reverse gravure, kiss reverse gravure, and offset gravure, reverse roll coaters, microgravure coaters, coaters combined with a chamber doctor, air knife coaters, dip coaters, bar coaters, comma coaters, and die coaters.

[0034] The amount of adhesive layer applied is 1 m after applying and drying the anchor coating agent. 2 Mass per unit is 0.01 to 5 g / m 2 It is preferable that the density is 0.03 to 3 g / m 2 It is more preferable that the thickness of the anchor coating agent is 1 m after it is applied and dried. 2 When the mass per unit area is equal to or greater than the lower limit, film formation tends to be sufficient, whereas when the mass per unit area is equal to or less than the upper limit, the film tends to be sufficiently dried and the solvent tends not to remain.

[0035] The method for drying the adhesive layer is not particularly limited, but examples thereof include a method of natural drying, a method of drying in an oven set at a predetermined temperature, and a method using a dryer attached to the coater, such as an arch dryer, a floating dryer, a drum dryer, an infrared dryer, etc. Furthermore, the drying conditions can be appropriately selected depending on the drying method, and for example, in a method of drying in an oven, it is preferable to dry at a temperature of 60 to 100°C for about 1 second to 2 minutes.

[0036] Instead of the polyurethane resin, a polyvinyl alcohol resin can be used for the adhesive layer. The polyvinyl alcohol resin may be any resin having a vinyl alcohol unit formed by saponifying a vinyl ester unit, such as polyvinyl alcohol (PVA) or ethylene-vinyl alcohol copolymer (EVOH).

[0037] When a polyvinyl alcohol resin is used as the adhesive layer, the adhesive layer may be formed by coating a polyvinyl alcohol resin solution or by multi-layer extrusion.

[0038] [Inorganic Oxide Layer] The inorganic oxide layer contributes to improving gas barrier properties. Examples of inorganic oxides contained in the inorganic oxide layer include aluminum oxide, silicon oxide, magnesium oxide, and tin oxide. From the viewpoint of transparency and barrier properties, the inorganic oxide may be selected from the group consisting of aluminum oxide, silicon oxide, and magnesium oxide. Furthermore, from the viewpoint of excellent tensile stretchability during processing, it is preferable that the inorganic oxide layer be a layer using silicon oxide. By using an inorganic oxide layer containing silicon oxide, higher barrier properties can be obtained with a very thin layer that does not affect the recyclability of the laminate.

[0039] When the inorganic oxide layer contains silicon oxide, the O / Si ratio of the inorganic oxide layer is desirably 1.7 or more. An O / Si ratio of 1.7 or more suppresses the content of metallic Si, making it easier to achieve good transparency. Furthermore, the O / Si ratio is preferably 2.0 or less. An O / Si ratio of 2.0 or less increases the crystallinity of SiO, preventing the inorganic oxide layer from becoming too hard and providing good tensile strength. This makes it possible to prevent cracks from occurring in the inorganic oxide layer when laminating a gas barrier coating layer. Even after forming into a packaging bag, the substrate layer or intermediate layer may shrink due to heat during boiling or retort treatment. However, an O / Si ratio of 2.0 or less makes it easier for the inorganic oxide layer to adapt to this shrinkage, thereby preventing a decrease in barrier properties. To more fully achieve these effects, the O / Si ratio of the inorganic oxide layer is preferably 1.75 to 1.9, more preferably 1.8 to 1.85.

[0040] The O / Si ratio of the inorganic oxide layer can be determined by X-ray photoelectron spectroscopy (XPS). For example, the measurement can be performed using an X-ray photoelectron spectrometer (manufactured by JEOL Ltd., product name: JPS-90MXV) with a non-monochromated MgKα (1253.6 eV) X-ray source and an X-ray output of 100 W (10 kV-10 mA). For quantitative analysis to determine the O / Si ratio, relative sensitivity factors of 2.28 for O1s and 0.9 for Si2p can be used.

[0041] The thickness of the inorganic oxide layer is preferably 10 nm or more and 50 nm or less. A thickness of 10 nm or more can provide sufficient water vapor barrier properties. Furthermore, a thickness of 50 nm or less can prevent cracks from occurring due to deformation caused by internal stress in the thin film, thereby preventing a decrease in water vapor barrier properties. Note that a thickness exceeding 50 nm is undesirable from an economic standpoint, as it increases costs due to an increase in the amount of material used and a longer film formation time. From the same viewpoint as above, the thickness of the inorganic oxide layer is more preferably 20 nm or more and 40 nm or less.

[0042] The inorganic oxide layer can be formed by, for example, vacuum film formation. In vacuum film formation, physical vapor deposition or chemical vapor deposition can be used. Examples of physical vapor deposition include, but are not limited to, vacuum deposition, sputtering, and ion plating. Examples of chemical vapor deposition include, but are not limited to, thermal CVD, plasma CVD, and photo CVD.

[0043] In the vacuum film formation, resistance heating vacuum deposition, EB (Electron Beam) heating vacuum deposition, induction heating vacuum deposition, sputtering, reactive sputtering, dual magnetron sputtering, plasma enhanced chemical vapor deposition (PECVD), and the like are particularly preferably used. However, in terms of productivity, vacuum deposition is currently the most superior. As a heating means for vacuum deposition, it is preferable to use any of the electron beam heating method, resistance heating method, and induction heating method.

[0044] [Gas barrier coating layer] The gas barrier coating layer protects the inorganic oxide layer, contributes to improving gas barrier properties, and exhibits high gas barrier properties through a synergistic effect with the inorganic oxide layer. The gas barrier coating layer may be a layer formed using a gas barrier coating layer-forming composition containing at least one selected from the group consisting of a hydroxyl group-containing polymer compound, a metal alkoxide, a silane coupling agent, and a hydrolyzate thereof.

[0045] The gas barrier coating layer can be formed using a composition for forming a gas barrier coating layer (hereinafter also referred to as a coating agent) containing, as a main component, an aqueous solution or a water / alcohol mixed solution containing at least one selected from the group consisting of a hydroxyl-containing polymer compound, a metal alkoxide, a silane coupling agent, and their hydrolysates. From the viewpoint of more adequately maintaining gas barrier properties after hot water treatment such as retort treatment, the coating agent preferably contains at least a silane coupling agent or its hydrolysate, more preferably at least one selected from the group consisting of a hydroxyl-containing polymer compound, a metal alkoxide, and their hydrolysates, and a silane coupling agent or its hydrolysate, and even more preferably a hydroxyl-containing polymer compound or its hydrolysate, a metal alkoxide or its hydrolysate, and a silane coupling agent or its hydrolysate. The coating agent can be prepared, for example, by mixing a metal alkoxide and a silane coupling agent directly, or after prior hydrolysis, with a solution of a hydroxyl-containing polymer compound, which is a water-soluble polymer, dissolved in an aqueous solvent (water or a water / alcohol mixture).

[0046] Examples of hydroxyl group-containing polymer compounds used in coating agents include polyvinyl alcohol, polyvinylpyrrolidone, starch, methyl cellulose, carboxymethyl cellulose, sodium alginate, etc. Among these, polyvinyl alcohol (PVA) is preferred when used in the coating agent for the gas barrier coating layer, as it provides particularly excellent gas barrier properties.

[0047] The metal alkoxides include tetraethoxysilane [Si(OC 2 H 5 ) 4 ], triisopropoxyaluminum [Al(O-2'-C 3 H 7 ) 3 Tetraethoxysilane and triisopropoxyaluminum are preferred because they are relatively stable in aqueous solvents after hydrolysis.

[0048] Examples of the silane coupling agent include vinyltrimethoxysilane, γ-chloropropylmethyldimethoxysilane, γ-chloropropyltrimethoxysilane, glycidoxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropylmethyldimethoxysilane, etc. The silane coupling agent may be a polymer thereof.

[0049] The coating agent may contain known additives such as an isocyanate compound, a dispersant, a stabilizer, a viscosity modifier, a colorant, etc., as needed, within the range that does not impair the gas barrier properties. The coating agent may also contain an acid catalyst, an alkali catalyst, a photopolymerization initiator, etc., as needed.

[0050] The thickness of the gas barrier coating layer is preferably 50 to 1,000 nm, more preferably 100 to 500 nm, from the viewpoint of obtaining excellent gas barrier properties while maintaining a polypropylene content of 90% by mass or more in the laminate. When the thickness of the gas barrier coating layer is 50 nm or more, more sufficient gas barrier properties tend to be obtained, and when it is 1,000 nm or less, sufficient flexibility tends to be maintained.

[0051] The coating agent for forming the gas barrier coating layer can be applied by, for example, dipping, roll coating, gravure coating, reverse gravure coating, air knife coating, comma coating, die coating, screen printing, spray coating, gravure offset, etc. The coating film obtained by applying this coating agent can be dried by, for example, hot air drying, heat roll drying, high frequency irradiation, infrared irradiation, UV irradiation, or a combination thereof.

[0052] The temperature at which the coating film is dried can be, for example, 50 to 150° C., and preferably 70 to 100° C. By keeping the drying temperature within the above range, the occurrence of cracks in the inorganic oxide layer and the gas barrier coating layer can be further suppressed, and excellent barrier properties can be achieved.

[0053] [Intermediate layer 12] The configuration of the intermediate layer can be appropriately referenced to the above description of the configuration of the substrate layer. The above-mentioned adhesion layer, inorganic oxide layer, and gas barrier coating layer may be provided on at least one surface of the intermediate layer. By providing an intermediate layer in a laminate, deformation of the laminate during bag production can be further reduced compared to when an intermediate layer is not provided.

[0054] The thickness of the intermediate layer is not particularly limited, but may be the same as the thickness of the substrate layer, and the ratio of the thicknesses of these layers (thickness of substrate layer / thickness of intermediate layer) may be 1.00 or more, may be greater than 1.00, may be 1.25 or more, or may be 1.50 or more. The substrate layer is the part that directly contacts or is in close proximity to the heat seal bar during heat sealing, and is the part that is particularly exposed to heat among the layers of the laminate, so it is prone to heat shrinkage during heat sealing. Therefore, by making the substrate layer thicker than the intermediate layer, heat shrinkage of the substrate layer can be suppressed.

[0055] [Printed Layer] The laminate may include a printed layer. The printed layer can be provided on at least one surface of the base layer or on at least one surface of the intermediate layer. The printed layer is provided in a position visible from the outside of the laminate for the purpose of displaying information about the contents, identifying the contents, improving concealment, or improving the design of the packaging bag. The printing method and printing ink are not particularly limited, and are appropriately selected from known printing methods and printing inks taking into consideration printability on the film, design such as color tone, adhesion, safety as a food container, etc. Examples of printing methods that can be used include gravure printing, offset printing, gravure offset printing, flexographic printing, and inkjet printing. Among these, gravure printing is preferably used from the viewpoints of productivity and high resolution of the image.

[0056] In order to improve the adhesion of the printed layer, the surface of the layer on which the printed layer is to be formed may be subjected to various pretreatments such as corona treatment, plasma treatment, and flame treatment, or a coating layer such as an easy-adhesion layer may be formed on the surface of the layer on which the printed layer is to be formed. Examples of the surface of the layer on which the printed layer is to be formed include the surface of the base layer or intermediate layer, and the surface of the gas barrier coating layer.

[0057] [Adhesive Layer S] The substrate layer and intermediate layer can be laminated via an adhesive layer. Examples of adhesive materials that can be used include polyester-isocyanate resins, urethane resins, and polyether resins. For use of packaging bags in retort applications, a two-component curing urethane adhesive with retort resistance can be preferably used. When a two-component curing urethane adhesive is used, the crosslinking density is higher than when a one-component curing urethane adhesive is used, making it easier to achieve high adhesion even after retort processing. Alternatively, a solventless two-component curing urethane adhesive may be used as the two-component curing urethane adhesive. From an environmental perspective, the adhesive does not need to contain 3-glycidyloxypropyltrimethoxysilane (GPTMS).

[0058] The thickness of the adhesive layer is not particularly limited, but may be, for example, 0.5 to 5 μm, or 0.3 to 7 μm. When the thickness of the adhesive layer is 0.5 μm or more, the adhesion between the base layer and the intermediate layer is easily improved, and when it is 5 μm or less, the barrier properties and recyclability of the laminate are easily improved.

[0059] [Sealant Layer 13] The sealant layer is a layer that provides heat-sealing properties to the laminate, and contains polypropylene. The sealant layer may contain a polypropylene film or may be made of a polypropylene film.

[0060] The polypropylene film may be an acid-modified polypropylene film obtained by graft-modifying polypropylene with an unsaturated carboxylic acid, an acid anhydride of an unsaturated carboxylic acid, an ester of an unsaturated carboxylic acid, etc. Furthermore, as the polypropylene, a polypropylene-based resin such as a homopolypropylene resin (PP), a propylene-ethylene random copolymer, a propylene-ethylene block copolymer, or a propylene-α-olefin copolymer can be used.

[0061] The polypropylene film constituting the sealant layer is preferably a non-oriented film from the viewpoint of improving the sealing property by heat sealing.

[0062] The polypropylene film constituting the sealant layer may contain various additives such as a flame retardant, a slip agent, an antiblocking agent, an antioxidant, a light stabilizer, a tackifier, and an antistatic agent.

[0063] The thickness of the sealant layer is determined depending on the mass of the contents, the shape of the packaging bag, etc., but may be approximately 30 to 150 μm, 40 to 100 μm, or 50 to 80 μm.

[0064] The sealant layer can be formed by any of the known lamination methods, such as a dry lamination method in which a film-like sealant layer made of the above-mentioned polypropylene is laminated with an adhesive such as a one-component curing or two-component curing urethane adhesive, a non-solvent lamination method in which a film-like sealant layer is laminated with a solventless adhesive, or an extrusion lamination method in which the above-mentioned polypropylene is heated and melted, extruded into a curtain shape, and laminated. In the non-solvent lamination method, a solventless two-component curing urethane adhesive may be used as the solventless adhesive. These lamination methods can also be used when laminating a substrate layer and an intermediate layer.

[0065] When using the non-solvent lamination method, the adhesive component does not contain an organic solvent, so the amount of residual solvent in the laminate can be reduced. Furthermore, when a laminate comprising a base layer made of oriented polypropylene and an intermediate layer made of oriented polypropylene is produced using the dry lamination method, the drying temperature must be lower to prevent thermal shrinkage of the laminate compared to laminates using polyester-based materials. In this case, the solvent in the adhesive may not be sufficiently volatilized and remain in the laminate, resulting in an odor due to the residual solvent. By using a solvent-free adhesive, the amount of residual solvent can be further reduced.

[0066] In addition, the non-solvent lamination method allows for a thinner adhesive layer than the dry lamination method. This further increases the polypropylene content in the entire laminate. Furthermore, the thinner adhesive layer improves heat conduction from the heat seal bar during heat sealing, allowing for reduced sealing time and temperature, and suppressing the occurrence of wrinkles and other problems associated with heat sealing. Such laminates are suitable for producing mono-material packaging bags.

[0067] The sealant layer and intermediate layer can be laminated via the adhesive layer S described above. The sealant layer and intermediate layer are bonded together by applying an adhesive to the intermediate layer and then laminating the sealant layer. If the adhesive is a solventless, two-component curing urethane adhesive, the intermediate layer is not subjected to a thermal load when the solvent dries. Therefore, the inorganic oxide layer and the gas barrier coating layer are less likely to be damaged by dimensional changes in the intermediate layer, and the barrier properties are less likely to deteriorate.

[0068] The sealant layer has a surface softening temperature T 2 (°C) must satisfy the following conditions: 2 <150℃ T 2 By setting the temperature to less than 150°C, sufficient seal strength can be obtained even when the heat sealing temperature is low (for example, about 145°C). Therefore, the heat sealing tolerance of the laminate can be widened. 2 On the other hand, from the viewpoint of suppressing adhesion of the sealant layers to each other and bleeding out of the additives during the retort treatment and boiling treatment, T 2 The softening temperature T of the sealant layer surface may be 80° C. or higher, or 100° C. or higher. 2may be 80°C or higher and lower than 150°C, 80°C or higher and lower than 148°C, 80°C or higher and lower than 147°C, 100°C or higher and lower than 150°C, 100°C or higher and lower than 148°C, or 100°C or higher and lower than 147°C. The softening temperature of the sealant layer surface can be adjusted, for example, by the crystallinity, molecular weight, and blending ratio of the copolymer. The method for measuring the softening temperature is as described above.

[0069] In addition, in order to prevent the occurrence of inner surface fusion during retort processing (the adhesion of unsealed heat-sealed surfaces due to the heat during retort processing), T 2 may satisfy the following conditions: 2 ≧135℃

[0070] In the laminate, the softening temperature T 1 and the softening temperature T of the sealant layer surface 2 The difference between (T 1 -T 2 ) preferably satisfies the following conditions: 1 -T 2 ) >53℃ T 1 -T 2 When T is greater than 53°C, the tolerance of the heat sealing temperature at which the thermal shrinkage of the laminate can be suppressed while ensuring sufficient seal strength can be widened. 1 -T 2 may be 55°C or higher, may be 58°C or higher, or may be 60°C or higher.

[0071] The laminate may contain polypropylene in an amount of 90% by mass or more of the total amount of the laminate. This allows the laminate to be referred to as a mono-material packaging material made of a single material, and has excellent recyclability. From the viewpoint of further improving recyclability, the polypropylene content in the laminate may be 95% by mass or more of the total amount of the laminate.

[0072] When the laminate is heat-sealed with the sealant layers facing each other using a heat sealer with an upper metal seal and a lower silicone rubber seal under conditions of an upper seal actual temperature of 145°C, a lower seal actual temperature of 90°C, a sealing pressure of 0.3 MPa, and a heating time of 1 second, the resulting seal strength is preferably 20 N / 15 mm or more, more preferably 25 N / 15 mm or more. By satisfying these conditions, the heat seal tolerance of the laminate can be widened.

[0073] When the laminate is heat-sealed with the sealant layers facing each other using a heat sealer with an upper metal seal and a lower silicone rubber seal under conditions of an upper seal actual temperature of 160°C, a lower seal actual temperature of 90°C, a sealing pressure of 0.3 MPa, and a heating time of 1 second, the heat shrinkage of the resulting sealed portion is preferably less than 3%, and more preferably 2.8% or less. By satisfying these conditions, the heat seal tolerance of the laminate can be widened.

[0074] The laminate was heat-sealed with the sealant layers facing each other using a heat sealer with an upper metal sealer and a lower silicone rubber sealer under the conditions of a lower seal temperature of 90°C, a sealing pressure of 0.3 MPa, and a heating time of 1 second, while varying the upper seal temperature. The lowest upper seal temperature at which the seal strength of the resulting seal reached 20 N / 15 mm was determined as T L The maximum actual temperature of the upper seal at which the heat shrinkage rate of the resulting seal portion can be maintained at less than 3% is T H In this case, T H -T L is preferably 15° C. or higher, and more preferably 20° C. or higher. By satisfying the above conditions, the heat seal tolerance of the laminate can be widened.

[0075] The laminate according to this embodiment has a wide heat-sealing temperature tolerance that can suppress thermal shrinkage of the laminate while ensuring sufficient seal strength. This makes it possible to suppress deterioration of packaging quality, such as bag distortion and reduced barrier properties, during heat sealing, as well as a decrease in the mass productivity of packaging bags. In other words, the present disclosure provides a laminate (packaging laminate) with a wide heat-sealing tolerance that is excellent in the mass production stability of packaging bags, even when using a PP monomaterial packaging material.

[0076] <Packaging Bag> The packaging bag is made by making the above-mentioned laminate into a bag, and is not particularly limited in shape, but may be, for example, a bag formed by folding one laminate in half so that the sealant layers face each other and then heat-sealing three sides, or a bag formed by stacking two laminates so that the sealant layers face each other and then heat-sealing four sides, or a self-standing standing pouch formed by stacking two laminates so that the sealant layers face each other and sealing the bottom material between them. The packaging bag can contain contents such as food, medicine, etc., and can be subjected to heat sterilization treatment such as retort treatment or boiling treatment.

[0077] Retort processing is a method of pressure sterilization of microorganisms such as mold, yeast, and bacteria, typically for the preservation of food, pharmaceuticals, etc. Typically, packaging bags containing food, etc., are pressure sterilized at 105-140°C and 0.15-0.30 MPa for 10-120 minutes. Retort devices are available in two types: steam type, which uses heated steam, and hot water type, which uses pressurized heated water. The appropriate method is used depending on the sterilization conditions of the food, etc. contained within. Boiling is a moist heat sterilization method for preserving food, pharmaceuticals, etc. Typically, packaging bags containing food, etc., are moist heat sterilized at 60-100°C and atmospheric pressure for 10-120 minutes, depending on the contents. Boiling is typically performed in a hot water bath at temperatures below 100°C. Methods include a batch method, in which the food is immersed in a hot water bath at a constant temperature for a set period of time and then removed, and a continuous method, in which the food is passed through a tunnel-type hot water bath for processing.

[0078] The packaging bag is less likely to deform during manufacturing, and is therefore easy to transport and to work with when the contents are enclosed.

[0079] The present disclosure will be explained in more detail by the following examples, but the present disclosure is not limited to these examples.

[0080] <Preparation of Adhesion Layer-Forming Composition> Acrylic polyol and tolylene diisocyanate were mixed such that the number of NCO groups in tolylene diisocyanate was equal to the number of OH groups in the acrylic polyol, and the mixture was diluted with ethyl acetate to a total solids content (total amount of acrylic polyol and tolylene diisocyanate) of 5 mass %. β-(3,4-epoxycyclohexyl)trimethoxysilane was further added to the diluted mixture in an amount of 5 parts by mass per 100 parts by mass of the total amount of acrylic polyol and tolylene diisocyanate, and these were mixed to prepare an adhesion layer-forming composition (anchor coating agent).

[0081] <Preparation of Composition for Forming Gas Barrier Coating Layer> A composition for forming a gas barrier coating layer was prepared by mixing the following liquids A, B, and C in a mass ratio of 65 / 25 / 10, respectively. Liquid A: tetraethoxysilane (Si(OC 2 H 5 ) 4 72.1 g of 0.1N hydrochloric acid was added to 17.9 g of SiO 2 and 10 g of methanol, and the mixture was stirred for 30 minutes to obtain a hydrolyzed solids content of 5% by mass (SiO 2 Solution B: A 5% by mass water / methanol solution of polyvinyl alcohol (mass ratio of water:methanol is 95:5). Solution C: A hydrolysis solution obtained by diluting 1,3,5-tris(3-trialkoxysilylpropyl)isocyanurate with a water / isopropyl alcohol mixed solution (mass ratio of water:isopropyl alcohol is 1:1) to a solids content of 5% by mass.

[0082] Example 1 The above-described adhesive layer-forming composition was applied by gravure roll coating to the corona-treated surface of a stretched polypropylene film (thickness: 20 μm) having one side subjected to corona treatment as an intermediate layer, and dried and cured at 60° C. to give a coating amount of 0.1 g / m 2An adhesive layer made of a polyester-based polyurethane resin was then formed. Next, a 30 nm-thick transparent inorganic oxide layer (silica vapor deposition layer) made of silicon oxide was formed using a vacuum deposition apparatus employing an electron beam heating system. The vapor deposition material type was adjusted to form a vapor deposition layer with an O / Si ratio of 1.8. The O / Si ratio was measured using an X-ray photoelectron spectrometer (manufactured by JEOL Ltd., product name: JPS-90MXV) with a non-monochromated MgKα (1253.6 eV) X-ray source and an X-ray output of 100 W (10 kV-10 mA). Quantitative analysis to determine the O / Si ratio was performed using relative sensitivity factors of 2.28 for O1s and 0.9 for Si2p, respectively.

[0083] Next, the composition for forming a gas barrier coating layer was applied onto the inorganic oxide layer by gravure roll coating, and the applied composition was dried by heating in an oven under conditions of a tension of 20 N / m and a drying temperature of 120° C. to form a gas barrier coating layer with a thickness of 0.3 μm. This resulted in a gas barrier film having a laminated structure of intermediate layer / adhesion layer / inorganic oxide layer / gas barrier coating layer.

[0084] Next, a stretched polypropylene film (20 μm thick) serving as a base layer was dry laminated onto the gas barrier coating layer of the gas barrier film using a two-component curing adhesive (manufactured by Mitsui Chemicals, Inc., product name: Base Agent A525 / Curing Agent A52) . Next, the non-corona-treated side of the intermediate layer was subjected to a corona treatment, and a non-stretched polypropylene film (60 μm thick) serving as a sealant layer was dry laminated onto the intermediate layer using a two-component curing adhesive (manufactured by Mitsui Chemicals, Inc., product name: Base Agent A525 / Curing Agent A52) . This produced a laminate having a laminated structure of base layer / adhesive layer / gas barrier coating layer / inorganic oxide layer / adhesion layer / intermediate layer / adhesive layer / sealant layer. Each adhesive layer had a thickness of 3 μm. A stretched polypropylene film having the melting point and surface softening temperature shown in Table 1 below was used as the base layer. A non-stretched polypropylene film having the surface softening temperature shown in Table 1 below was used as the sealant layer.

[0085] (Examples 2 to 9 and 11, and Comparative Examples 1 and 2) Laminates were produced in the same manner as in Example 1, except that a stretched polypropylene film having a melting point and a surface softening temperature shown in Table 1 below was used as the base layer, and a non-stretched polypropylene film having a surface softening temperature shown in Table 1 below was used as the sealant layer.

[0086] Example 10 A gas barrier film having a laminated structure of intermediate layer / adhesion layer / inorganic oxide layer / gas barrier coating layer was obtained in the same manner as in Example 1. Next, a stretched polypropylene film (thickness 20 μm) as a base layer was laminated onto the gas barrier coating layer of the gas barrier film using a non-solvent lamination method with a solventless two-component curing urethane adhesive (manufactured by Toyo-Morton Co., Ltd., product name: TSN-4864A / TSN-4864B3). The solventless adhesive was applied using a roll coater. Next, the non-corona-treated side of the intermediate layer was subjected to a corona treatment, and a non-stretched polypropylene film (thickness 60 μm) as a sealant layer was laminated onto the intermediate layer using a non-solvent lamination method with a solventless two-component curing urethane adhesive (manufactured by Toyo-Morton Co., Ltd., product name: TSN-4864A / TSN-4864B3). The solventless adhesive was applied using a roll coater. This produced a laminate having a laminate structure of substrate layer / adhesive layer / gas barrier coating layer / inorganic oxide layer / adhesive layer / intermediate layer / adhesive layer / sealant layer. The thickness of each adhesive layer was 2 μm. The substrate layer and sealant layer were the same as those used in Example 1.

[0087] <Measurement of Melting Point> The melting point of the substrate layer was measured by the following method. The substrate layer was cut from the laminates produced in the Examples and Comparative Examples to prepare measurement samples. The melting points (melting peak temperatures) of these measurement samples were measured by differential scanning calorimetry (DSC) at a heating rate of 10°C / min. A DSC7000X (trade name) manufactured by Hitachi High-Tech Science Corporation was used as the differential scanning calorimeter.

[0088] <Measurement of Surface Softening Temperature> The softening temperatures of the substrate layer surface and the sealant layer surface were measured by the following method using local thermal analysis (LTA) with an atomic force microscope. When measuring the softening temperature of the substrate layer surface using the laminates produced in the Examples and Comparative Examples, the sealant layer side was corona-treated and then fixed to a metal disk with an epoxy adhesive, and when measuring the softening temperature of the sealant layer surface, the substrate layer side was corona-treated and then fixed to a metal disk with an epoxy adhesive to prepare a measurement sample. The corona treatment was carried out using a corona treater (product name: CT-0212) manufactured by Kasuga Electric Co., Ltd., at 0.20 kW.

[0089] The atomic force microscope (AFM) was an MFP-3D-SA (trade name) manufactured by Oxford Instruments Ltd., with a local thermal analysis option being a Ztherm system, and the cantilever was an AN2-200 (trade name) manufactured by Anasys Instruments Ltd. with a spring constant of 0.5 to 3.5 N / m, and the softening temperature was measured on the surface of each measurement sample.

[0090] When the sample surface was heated after Detrend correction with the cantilever contact pressure (change in cantilever deflection) set to 0.2 V, the voltage application rate (heating rate) set to 0.5 V / sec, and the maximum applied voltage set to 6.0 V, the sample surface expanded and the cantilever position rose. Further heating of the sample surface softened the sample surface, and the measurement was terminated when the cantilever position dropped 30 nm. If the Z displacement did not drop 30 nm from the change point and reached the maximum applied voltage, the maximum applied voltage during Detrend correction and measurement was increased by 0.5 V, and the measurement was performed again.

[0091] The voltage applied at the point where the vertical height (Z displacement) of the cantilever was maximum was taken as the voltage applied at the softening point, and the voltage value was read.

[0092] A calibration curve was created to calculate the softening temperature of the sample. Four types of calibration samples were used: polycaprolactone (melting point: 60°C), low-density polyethylene (LDPE, melting point: 112°C), polypropylene (PP, melting point: 166°C), and polyethylene terephthalate (PET, melting point: 255°C). The maximum applied voltage during detrend correction was 3.5 V for polycaprolactone, 5.5 V for low-density polyethylene, 6.7 V for polypropylene, and 7.9 V for polyethylene terephthalate. The cantilever contact pressure (change in cantilever deflection) was 0.2 V, and the voltage application rate (heating rate) was 0.5 V / sec. The calibration sample was measured 20 times at different measurement positions, and a calibration curve was created by approximating the average applied voltage at the softening point and the melting point with a cubic function using the least squares method.

[0093] Using a calibration curve of applied voltage and melting point (melting point peak temperature), the applied voltage at the softening point of the substrate layer surface and the sealant layer surface was converted into a temperature, which was taken as the softening temperature. The softening temperatures of 12 or more points within a 10 μm field of view were measured, and the average value was calculated to be the surface softening temperature of each measurement sample.

[0094]

[0095] <Preparation of Heat-Sealed Samples> The laminates obtained in the Examples and Comparative Examples were cut into 60 mm x 120 mm pieces with the machine direction aligned longitudinally. The cut laminates were folded in half at the center longitudinally so that the sealant layers faced each other, and one side opposite the folded portion (at a position at least 3 mm away from the edge) was heat-sealed over a width of 10 mm using a heat sealer (model number: TP-701-B) manufactured by Tester Sangyo Co., Ltd. The heat-sealing conditions were as follows. The folded portion was then cut with scissors so that the upper and lower laminates were approximately equal in length, and the upper and lower laminates were separated. This resulted in heat-sealed samples. (Heat-sealing conditions) Upper seal bar: A 10 mm-wide metal seal bar (aluminum alloy 2000 series (Al-Cu)) was used, and the actual sealing temperature was varied from 130°C to 165°C in 5°C increments. Lower seal bar: A 50 mm wide silicone rubber seal bar was used, and the seal temperature was fixed at 90° C. Sealing pressure: 0.3 MPa Heating time: 1.0 second

[0096] <Measurement of seal strength> The heat-sealed sample was cut with a cutter to a width of 15 mm x length of 60 mm to obtain a rectangular sample for measuring seal strength. The width direction of the sample for measuring seal strength was perpendicular to the width direction of the sealed portion. The obtained sample for measuring seal strength was subjected to a peel test of the sealed portion under normal conditions (23°C, 50% RH) using a Tensilon universal testing machine (manufactured by Shimadzu Corporation, product name: AGS-100NX) with a chuck distance of 10 mm and a peel speed of 100 m / min. The seal strength at each actual seal temperature is shown in Table 2. A seal strength of 20 N / 15 mm or more was determined to be at a level that is acceptable for practical use, and the lowest upper actual seal temperature at which a seal strength of 20 N / 15 mm or more was obtained was determined to be T L The temperature was recorded as (°C). L The values ​​are shown in Table 3.

[0097] <Measurement of Heat Shrinkage Ratio> The length A (mm) of the sealed portion of the heat-sealed sample in the TD direction (direction perpendicular to the width direction of the sealed portion) and the lengths B and C (mm) of the unsealed portion in the TD direction 3 mm from each end of the width direction of the sealed portion were measured, and the heat shrinkage ratio of the sealed portion was calculated using the following formula. Note that lengths B and C are the lengths of portions that are sufficiently far from the sealed portion and are not affected by heat. Heat shrinkage ratio (%) = [1 - A / {(B + C) / 2}] x 100 The heat shrinkage ratios at each actual sealing temperature (155 to 165°C) are shown in Table 2. A heat shrinkage ratio of less than 3% was determined to be at a level that is acceptable for practical use, and the highest actual upper sealing temperature at which a heat shrinkage ratio of less than 3% could be maintained was defined as T H The temperature was recorded as (°C). H The values ​​are shown in Table 3.

[0098] <Evaluation of distortion> The presence or absence of distortion (heat wrinkles) in the sealed portion of heat-sealed samples at an actual upper seal temperature of 160°C was visually observed and rated according to the following criteria. A rating of B or higher indicates a level that is acceptable for practical use. The results are shown in Table 3. A: No distortion (heat wrinkles) was observed in either the sealed portion or the non-sealed portion near the sealed portion. B: Some distortion (heat wrinkles) was observed in the sealed portion, but no distortion (heat wrinkles) was observed in the non-sealed portion near the sealed portion. C: Distortion (heat wrinkles) was observed in both the sealed portion and the non-sealed portion near the sealed portion.

[0099] <Heat seal tolerance> The maximum actual upper seal temperature T at which the heat shrinkage rate of the sealed area can be maintained at less than 3%. H and the lowest temperature T of the upper seal actual temperature at which the seal strength of the seal portion reaches 20 N / 15 mm or more. L The difference between (T H -T L The heat seal tolerance of the laminate was evaluated according to the following criteria. If the evaluation was B or higher, it was at a level that would not pose a problem in practical use. The results are shown in Table 3. A: T H -T L is 20℃ or more B:T H -T L is 15℃ or more and less than 20℃ C:T H -T L is 10℃ or more and less than 15℃ D:T H -TL is less than 10°C

[0100]

[0101]

[0102] 11...substrate layer, 12...intermediate layer, 13...sealant layer, S...adhesive layer, 100...laminated body.

Claims

1. A laminate comprising at least a base layer, an intermediate layer, and a sealant layer, the base material layer is disposed on one outermost surface of the laminate, and the sealant layer is disposed on the other outermost surface of the laminate; the base layer, the intermediate layer and the sealant layer all comprise polypropylene; an inorganic oxide layer and a gas barrier coating layer are provided on a surface of the base layer facing the intermediate layer or on at least one surface of the intermediate layer; The softening temperature of the surface of the substrate layer measured by local thermal analysis (LTA) of the substrate layer is defined as T 1 The softening temperature of the sealant layer surface is T 2 Then, T 1 and T 2 A laminate satisfying the following conditions. T 1 >200℃ T 2 <150℃ (T 1 - T 2 )>53℃

2. A laminate comprising at least a base layer, an intermediate layer, and a sealant layer, the base material layer is disposed on one outermost surface of the laminate, and the sealant layer is disposed on the other outermost surface of the laminate; the base layer, the intermediate layer and the sealant layer all comprise polypropylene; an inorganic oxide layer and a gas barrier coating layer are provided on a surface of the base layer facing the intermediate layer or on at least one surface of the intermediate layer; The softening temperature of the surface of the substrate layer measured by local thermal analysis (LTA) of the substrate layer is defined as T 1 The softening temperature of the sealant layer surface is T 2 Then, T 1 and T 2 satisfies the following conditions, A laminate in which, when the sealant layers of the laminate are placed facing each other and heat sealed using a heat sealer made of metal on the upper side and silicone rubber on the lower side under conditions of an upper seal actual temperature of 145°C, a lower seal actual temperature of 90°C, a sealing pressure of 0.3 MPa, and a heating time of 1 second, the seal strength of the resulting seal is 20 N / 15 mm or more. T 1 >200℃ T 2 <150℃

3. A laminate comprising at least a base layer, an intermediate layer, and a sealant layer, the base material layer is disposed on one outermost surface of the laminate, and the sealant layer is disposed on the other outermost surface of the laminate; the base layer, the intermediate layer and the sealant layer all comprise polypropylene; an inorganic oxide layer and a gas barrier coating layer are provided on a surface of the base layer facing the intermediate layer or on at least one surface of the intermediate layer; The softening temperature of the surface of the substrate layer measured by local thermal analysis (LTA) of the substrate layer is defined as T 1 The softening temperature of the sealant layer surface is T 2 Then, T 1 and T 2 satisfies the following conditions, A laminate in which, when the sealant layers of the laminate are placed facing each other and heat sealed using a heat sealer made of metal on the upper side and silicone rubber on the lower side under conditions of an upper seal actual temperature of 160°C, a lower seal actual temperature of 90°C, a sealing pressure of 0.3 MPa, and a heating time of 1 second, the heat shrinkage rate of the resulting sealed portion is less than 3%. T 1 >200℃ T 2 <150℃

4. A laminate comprising at least a base layer, an intermediate layer, and a sealant layer, the base material layer is disposed on one outermost surface of the laminate, and the sealant layer is disposed on the other outermost surface of the laminate; the base layer, the intermediate layer and the sealant layer all comprise polypropylene; an inorganic oxide layer and a gas barrier coating layer are provided on a surface of the base layer facing the intermediate layer or on at least one surface of the intermediate layer; The softening temperature of the surface of the substrate layer measured by local thermal analysis (LTA) of the substrate layer is defined as T 1 The softening temperature of the sealant layer surface is T 2 Then, T 1 and T 2 satisfies the following conditions, With the sealant layers of the laminate facing each other, a heat sealer having an upper metal member and a lower silicone rubber member is used to perform heat sealing under conditions of a lower seal actual temperature of 90°C, a sealing pressure of 0.3 MPa, a heating time of 1 second, and varying the upper seal actual temperature; where T L is the minimum upper seal actual temperature at which the seal strength of the resulting seal reaches 20 N / 15 mm, and T H is the maximum upper seal actual temperature at which the heat shrinkage rate of the resulting seal can be maintained at less than 3%, T H -T L is 15°C or more. T 1 >200℃ T 2 <150℃

5. 2. The laminate according to claim 1, wherein when the sealant layers of the laminate are placed facing each other and heat sealed using a heat sealer having an upper metal layer and a lower silicone rubber layer under conditions of an upper seal actual temperature of 145°C, a lower seal actual temperature of 90°C, a sealing pressure of 0.3 MPa, and a heating time of 1 second, the seal strength of the resulting seal is 20 N / 15 mm or more.

6. 3. The laminate according to claim 1 or 2, wherein when the sealant layers of the laminate are placed facing each other and heat sealed using a heat sealer having an upper metal surface and a lower silicone rubber surface under conditions of an upper seal actual temperature of 160°C, a lower seal actual temperature of 90°C, a sealing pressure of 0.3 MPa, and a heating time of 1 second, the heat shrinkage rate of the resulting sealed portion is less than 3%.

7. With the sealant layers of the laminate facing each other, a heat sealer made of metal on the top and silicone rubber on the bottom was used to perform heat sealing under conditions of a lower seal actual temperature of 90° C., a sealing pressure of 0.3 MPa, and a heating time of 1 second, while varying the upper seal actual temperature. The minimum upper seal actual temperature at which the seal strength of the resulting seal reaches 20 N / 15 mm was determined as T L The maximum upper seal actual temperature at which the thermal shrinkage rate of the resulting seal portion can be maintained at less than 3% is T H In this case, T H -T L The laminate according to any one of claims 1 to 3, wherein the temperature is 15°C or higher.

8. T 2 The laminate according to any one of claims 1 to 4, wherein the laminate satisfies the following conditions: T 2 ≧135℃

9. The laminate according to any one of claims 1 to 4, wherein the base material layer and the intermediate layer, and the intermediate layer and the sealant layer are both bonded via an adhesive layer using a two-component curing urethane adhesive.

10. 10. The laminate according to claim 9, wherein at least one of the base material layer and the intermediate layer, and the intermediate layer and the sealant layer are bonded via an adhesive layer using a solvent-free two-component curing urethane adhesive.

11. A packaging bag produced by producing the laminate according to any one of claims 1 to 4.