Solid oxide fuel cell comprising alloy-plated interconnect and method for manufacturing the same
The Co-Ni alloy-plated interconnects in solid oxide fuel cells address chromium volatilization and poisoning by forming a stable, high-quality thin film that suppresses chromium diffusion and oxidation, improving performance and lifespan.
Patent Information
- Application Number
- KR1020250059438
- Authority / Receiving Office
- KR · KR
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-08
- Publication Date
- 2026-11-17
AI Technical Summary
Solid oxide fuel cells experience high-temperature degradation and thermal breakdown due to chromium volatilization and poisoning, which contaminates the air electrode, degrading performance.
A solid oxide fuel cell with an interconnect alloy-plated by an electroplating method, using a Co-Ni alloy thin film with a mixed phase of FCC and HCP, forming a nanometer-scale equiaxed crystal grain structure to suppress chromium volatilization and enhance mechanical properties.
The Co-Ni alloy plating effectively blocks chromium diffusion and oxidation pathways, improving oxidation resistance and lifespan of interconnects, reducing chromium volatilization, and enhancing mechanical properties and electrical conductivity.
Smart Images

Figure PAT00001_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a solid oxide fuel cell (SOFC) with alloy-plated interconnects to suppress chromium volatilization and a method for manufacturing the same.
[0002] This research was funded by the Ministry of Trade, Industry and Energy and the Korea Institute of Industrial Technology Planning and Evaluation (KEIT) in 2024 (Development of Material and Component Technology for 48V-Class Transparent Heated Safety Glass Based on Metal Thin Film Coating, RS-2024-00507673). Background Technology
[0004] Generally, solid oxide fuel cells have high power generation efficiency and are applicable to a wide range of applications, from vehicles and ships to homes, buildings, and power generation; they have a structure in which multiple single cells are electrically connected through an interconnect made of metal.
[0005] Here, the solid oxide fuel cell has an operating temperature of 600 to 900°C, and this operating temperature is used to separate hydrogen molecules entering the fuel electrode into hydrogen atoms and electrons. The separated electrons from the fuel electrode flow into an external circuit and are used for power generation in the solid oxide fuel cell, and the process of them entering the air electrode is repeated.
[0006] This is the operating mechanism of a solid oxide fuel cell, in which interconnects connect cells to send electrons to an external circuit and transfer them to the air electrode of the next cell. Additionally, they serve to separate gases to prevent the fuel and air from mixing.
[0007] However, solid oxide fuel cells used in high-temperature environments can experience problems such as high-temperature degradation and thermal breakdown. These issues are closely related to the oxide protective film formed on the surface of the interconnects.
[0008] Fe-Cr stainless steel, used as a metal interconnect material for solid oxide fuel cells, possesses corrosion resistance due to the formation of a protective oxide film, such as Cr2O3, on its surface. This protective oxide film, which has a thickness of approximately 3 nm at room temperature, thickens upon exposure to high temperatures. Chromium oxide detaches from the thickened protective oxide film and migrates to the air electrode, where it reacts with oxygen to contaminate the air electrode. The detachment of the protective oxide film formed on the surface of the interconnect can be referred to as chromium volatilization, while the contamination of the air electrode by the reaction of the detached chromium oxide with oxygen can be referred to as chromium poisoning.
[0009] In other words, the metal interconnects of solid oxide fuel cells are generally composed of Fe-Cr alloys, and chromium poisoning occurs—a phenomenon in which chromium oxide formed at high temperatures volatilizes and redeposits onto the surface of the air electrode, degrading its performance. This chromium poisoning is the cause of problems such as high-temperature degradation and thermal breakdown in solid oxide fuel cells.
[0010] Therefore, there is an urgent need for technological development of solid oxide fuel cells equipped with interconnects capable of suppressing chromium volatilization. Prior art literature
[0011] Korean Registered Patent Publication No. 10-2491289, published on January 25, 2023. Korean Published Patent Publication No. 10-2022-0106080, published on July 28, 2022. The problem to be solved
[0012] The present invention was developed to resolve the aforementioned problems, and aims to provide a solid oxide fuel cell with an interconnect alloy-plated by an electroplating method and a method for manufacturing the same.
[0013] The objectives of the present invention are not limited to those mentioned above, and other unmentioned objectives may be clearly understood from the descriptions below and may be sufficiently included in the objectives of the present invention. means of solving the problem
[0014] A solid oxide fuel cell having an alloy-plated interconnect according to one aspect of the present invention for achieving the above objective comprises a plurality of single cells in which a solid oxide electrolyte is disposed between a fuel electrode and an air electrode, and an interconnect that electrically connects the plurality of single cells, wherein a Co-Ni alloy thin film containing 50% or more and 84% or less of Co is formed on the surface of the interconnect, and the Co-Ni alloy thin film has a mixed phase of FCC and HCP, and the Co-Ni alloy thin film may have a nanometer-scale equiaxed crystal grain shape.
[0015] A method for manufacturing a solid oxide fuel cell with an alloy-plated interconnect according to another aspect of the present invention for achieving the above objective is to prepare an interconnect for manufacturing a solid oxide fuel cell comprising a plurality of single cells in which a solid oxide electrolyte is disposed between a fuel electrode and an air electrode, and an interconnect that electrically connects the plurality of single cells, and may include an interconnect preparation step, a Co strike plating step, and a Co-Ni alloy thin film electroplating step. Effects of the invention
[0016] The solid oxide fuel cell and manufacturing method applying the alloy-plated interconnect of the present invention can expect the following effects.
[0017] First, by forming an electroplated alloy thin film on the interconnect surface, chromium volatilization can be suppressed, and mechanical properties can be enhanced through solid solution strengthening caused by nanometer-scale crystal grains and a mixture of FCC and HCP.
[0018] In addition, by plating an alloy onto the interconnect surface through electroplating, it is possible to realize high-quality thin films with a simple and economical process.
[0019] In addition, Co-Ni alloy plating forms a plating layer with high oxidation stability, which can block the diffusion and oxidation pathways of chromium and suppress chromium volatilization. This can contribute to improving the oxidation resistance and lifespan of interconnects in high-temperature operating environments.
[0020] The effects of the present invention are not limited to those mentioned above, and other unmentioned effects may be sufficiently included from the descriptions below. Brief explanation of the drawing
[0021] Figure 1 is an XRD pattern of a Co-Ni alloy according to an embodiment of the present invention. Figure 2 is a crystal structure of a Co-Ni alloy thin film according to an embodiment of the present invention. Figure 3 shows the microhardness of a Co-Ni alloy thin film according to the Co content in an embodiment of the present invention. FIG. 4 is a flowchart of the interconnect manufacturing step in the method for manufacturing a solid oxide fuel cell with an alloy-plated interconnect according to an embodiment of the present invention. Figure 5 shows the XRD measurement results of Example 1, Comparative Example 1, and Comparative Example 2 according to an embodiment of the present invention. Figures 6a and 6b are the SEM imaging and EDS line scan results of Example 1, Comparative Example 1, and Comparative Example 2 according to an embodiment of the present invention. FIG. 7 shows the tensile test results of Example 1-1, Comparative Example 1-1, and Comparative Example 2-1 according to an embodiment of the present invention. Figure 8 shows the micro-Vickers hardness test results of Example 1 and Comparative Example 2 according to an embodiment of the present invention. FIG. 9 is the ASR evaluation result of Example 1, Comparative Example 1, and Comparative Example 2 according to an embodiment of the present invention. FIG. 10 is the ICP-OES analysis result of Example 1 and Comparative Example 2 according to an embodiment of the present invention. FIG. 11 is the result of capturing FIB channeling images of Example 1, Comparative Example 1, and Comparative Example 2 according to an embodiment of the present invention. Specific details for implementing the invention
[0022] The advantages and features of the present invention, and the methods for achieving them, will become clear by referring to the embodiments described below in detail together with the accompanying drawings. However, the present invention is not limited to the embodiments disclosed below but may be implemented in various different forms; these embodiments are provided merely to ensure that the disclosure of the present invention is complete and to fully inform those skilled in the art of the scope of the invention. Meanwhile, the terms used in this specification are for describing the embodiments and are not intended to limit the present invention. In this specification, the singular form includes the plural form unless specifically stated otherwise in the text.
[0023] The present invention relates to a solid oxide fuel cell having an alloy-plated interconnect capable of effectively suppressing air electrode chromium volatilization at high temperatures by plating a Co-Ni alloy on the surface of the interconnect and applying it to the solid oxide fuel cell, and a method for manufacturing the same.
[0025] Hereinafter, a solid oxide fuel cell with an alloy-plated interconnect according to a preferred embodiment of the present invention and a method for manufacturing the same will be described in detail with reference to the drawings.
[0027] A solid oxide fuel cell having an alloy-plated interconnect according to one embodiment of the present invention may be configured to include a plurality of single cells in which a solid oxide electrolyte is disposed between a fuel electrode and an air electrode, an interconnect that electrically connects the plurality of single cells, and a Co-Ni alloy thin film formed on the surface of the interconnect.
[0028] Here, since a plurality of single cells comprising a fuel electrode, an air electrode, and a solid oxide electrolyte, excluding the interconnect which is a characteristic component of the present invention, can be configured identically to the corresponding configuration of a conventional solid oxide electrolyte, a detailed description is omitted.
[0030] The above interconnect may be made of a heat-resistant material including Fe-Cr-based stainless steel, nickel, etc., so that it can be used at the operating temperature of a solid oxide fuel cell.
[0031] The above Co-Ni alloy thin film is plated on the surface of the interconnect. Through Co-Ni alloy plating, a plating layer with high oxidation stability is formed, which can block the diffusion and oxidation pathways of chromium and suppress chromium volatilization. This can contribute to improving the oxidation resistance and lifespan of the interconnect in high-temperature operating environments.
[0032] More specifically, chromium can diffuse and evaporate along metal surfaces at high temperatures, and a Co-Ni alloy plating layer can act as a diffusion barrier by blocking the diffusion pathway of chromium—that is, physically inhibiting it. Furthermore, in high-temperature oxidizing environments, chromium readily forms Cr2O3, and this protective oxide film volatilizes easily. In this case, the Co-Ni alloy plating layer not only prevents direct contact between oxygen and chromium but also forms more stable spinel-structured metal oxide films such as Co2O3 and NiCo2O4, thereby suppressing and delaying the formation of chromium oxide.
[0033] Both Co and Ni exhibit high oxidation stability at high temperatures. Furthermore, upon oxide formation, they create a dense protective layer of spinel structure that oxidizes before chromium, thereby blocking chromium from reacting with the external environment. Additionally, Co and Ni are a completely solid-solution alloy system; their mixed-phase structure makes it difficult for Cr to diffuse at grain boundaries or escape from the lattice, which can suppress the phenomenon of chromium atoms migrating to the surface and volatilizing.
[0034] A Co-Ni alloy thin film containing 50% or more and 84% or less of Co can be formed on the surface of an interconnect. The Co-Ni alloy has the characteristic that the phase structure varies depending on the Co content and can form both FCC and HCP.
[0035] Through the XRD pattern of the Co-Ni alloy in Fig. 1, it can be confirmed that it has a mixed phase of FCC and HCP at a Co content of 66% or more and 84% or less. Since it exhibits a single FCC phase at a Co content of 49% or less, the Co-Ni alloy may have a mixed phase at a Co content of 50% or more and 84% or more.
[0036] Figure 2 shows the crystal structure of a Co-Ni alloy thin film. Through Figure 2a, the crystal structure of FCC phase Ni contained in Co having an HCP phase can be confirmed, and through Figure 2b, the crystal structure of HCP phase Co contained in Ni having an FCC phase can be confirmed. These crystal structures exist in the form of substitutional solid solutions and can contribute to the improvement of mechanical strength through a solid solution strengthening mechanism.
[0037] The Co-Ni alloy thin film of the present invention contains 50% or more and 84% or less of Co, thereby having a mixed phase of FCC and HCP and exhibiting a nanometer-scale equiaxed grain shape.
[0038] Figure 3 shows the microhardness of Co-Ni alloy thin films according to Co content. According to Figure 3, it can be confirmed that the highest microhardness is exhibited at the peak present at a Co content of 40 to 60%. In addition, it can be confirmed that the microhardness is higher than that of pure Ni at Co content of 5% or more and 81% or less.
[0039] In the present invention, with reference to the results of FIGS. 1 and FIGS. 3, the mechanical properties of the interconnect surface were improved through the solid solution strengthening effect of the mixed phase by plating a Co-Ni alloy with a Co content of 50% or more and 84% or less on the surface of the interconnect.
[0040] A solid oxide fuel cell with an alloy-plated interconnect according to one embodiment of the present invention may further include a Co strike plating layer.
[0041] The above Co strike plating layer is formed between the interconnect and the Co-Ni alloy thin film, and may be formed on the surface of the interconnect to obtain the effects of improved adhesion and surface activation before performing electroplating of the Co-Ni alloy.
[0043] A method for manufacturing a solid oxide fuel cell with an alloy-plated interconnect according to another embodiment of the present invention may comprise a step of preparing a plurality of single cells in which a solid oxide electrolyte is disposed between a fuel electrode and an air electrode, and a step of manufacturing an interconnect that electrically connects the plurality of single cells.
[0044] Here, the step of preparing a plurality of single cells consisting of a fuel electrode, an air electrode, and a solid oxide electrolyte, excluding the interconnect manufacturing step which is a characteristic step of the present invention, can be applied in the same way as the corresponding step of a conventional solid oxide fuel cell manufacturing method, so a detailed description is omitted.
[0045] The interconnect manufacturing step (S100) of the present invention may include an interconnect preparation step (S110), a Co strike plating step (S120), and a Co-Ni alloy thin film electroplating step (S130), as shown in FIG. 4.
[0046] In the interconnect preparation step (S110), a heat-resistant material including Fe-Cr-based stainless steel, nickel, etc., can be prepared so that it can be used at the operating temperature of the solid oxide fuel cell.
[0047] The Co strike plating step (S120) may include a Co strike plating solution preparation step (S121) and a step of forming a Co strike plating layer on the interconnect (S122).
[0048] In the step of preparing a Co strike plating solution (S121), a Co strike plating solution containing 100 g / L of CoCl2·6H2O and 100 ml / L of HCl can be prepared.
[0049] The step (S122) of forming a Co strike plating layer on the interconnect may involve performing strike plating on the interconnect, which is the cathode, using a Pt mesh as the anode. In this case, the strike plating is performed at a flow rate of 200 rpm and 300 mA / cm². 2 It can be performed for 50 seconds at a current density. All strike plating of the present invention is performed under the above conditions.
[0050] The Co-Ni alloy electroplating step (S130) may include a Co-Ni alloy plating solution preparation step (S131) and a Co-Ni alloy thin film formation step (S132).
[0051] In the step of preparing the Co-Ni alloy plating solution (S131), a Co-Ni alloy plating solution containing 40 to 70 g / L of CoCl2·6H2O can be prepared.
[0052] In the Co-Ni alloy thin film formation step (S132), the strike-plated interconnect can be immersed in the Co-Ni alloy plating solution prepared in the Co-Ni alloy plating solution preparation step (S131) to form a Co-Ni alloy thin film on the surface of the interconnect.
[0053] The Co-Ni alloy thin film may contain 50% or more and 84% or less of Co, and may have a mixed phase of FCC and HCP.
[0054] In addition, Co-Ni alloy thin films can have an equiaxed grain structure on the nanometer scale.
[0055] Here, performing electroplating to form a Co-Ni alloy thin film on the surface of the interconnect is intended to obtain the advantage of realizing high-quality thin films while being simple and economical, unlike sputtering, sol-gel, and electrophoretic deposition.
[0057] The following provides a more detailed explanation through specific examples, comparative examples, and experimental examples. The following examples, comparative examples, and experimental examples are merely illustrative to aid in understanding the present invention and do not limit the scope of the present invention.
[0059] <Example 1>
[0060] Manufacture of 60Co-40Ni alloy plated interconnects
[0061] Interconnects plated with a 60Co-40Ni alloy were manufactured using SUS430, an Fe-Cr stainless steel. Electroplating was performed on the strike-plated interconnects using an alloy plating solution containing 100–300 g / L NiSO4·6H2O, 10–100 g / L NiCl2·6H2O, 1–100 g / L CoSO4·7H2O, 40–70 g / L CoCl2·6H2O, 1–50 g / L H3BO3, 1–50 g / L C6H8O6, and 1–50 g / L C7H5NO3SNa·2H2O. Ni was used as the anode, and the other conditions were a temperature of 50 ℃, a flow rate of 200 rpm, and a current density of 30 mA / cm². 2 It was performed in. It is a 60Co-40Ni alloy plated interconnect manufactured by the method described above.
[0063] <Example 1-1>
[0064] Fabrication of 60Co-40Ni alloy thin films
[0065] To perform a tensile test on the alloy thin film, the alloy thin film was peeled off after alloy plating. Unlike Example 1, electroplating was performed on a Ti plate, and the pump voltage was set to 160 V. This is a 60Co-40Ni alloy thin film prepared by the above method.
[0067] <Comparative Example 1>
[0068] Manufacture of 40Co-60Ni alloy plated interconnects
[0069] Interconnects plated with a 40Co-60Ni alloy were manufactured using SUS430, an Fe-Cr stainless steel. Electroplating was performed on the strike-plated interconnects using an alloy plating solution containing 100–300 g / L NiSO4·6H2O, 10–100 g / L NiCl2·6H2O, 1–100 g / L CoSO4·7H2O, 5–10 g / L CoCl2·6H2O, 1–50 g / L H3BO3, 1–50 g / L C6H8O6, and 1–50 g / L C7H5NO3SNa·2H2O. Ni was used as the anode, and the other conditions were a temperature of 50 ℃, a flow rate of 200 rpm, and a current density of 30 mA / cm². 2 It was performed in. It is a 40Co-60Ni alloy plated interconnect manufactured by the method described above.
[0071] <Comparative Example 1-1>
[0072] Fabrication of 40Co-60Ni Alloy Thin Film
[0073] To perform a tensile test on the alloy thin film, the alloy thin film was peeled off after electroplating. Unlike Comparative Example 1, electroplating was performed on a Ti plate, and the pump voltage was set to 160 V. This is a 40Co-60Ni alloy thin film prepared by the above method.
[0075] <Comparative Example 2>
[0076] Manufacture of pure Co-plated interconnects
[0077] Pure Co-plated interconnects were manufactured using SUS430, an Fe-Cr stainless steel. Electroplating was performed on the strike-plated interconnects using a plating solution containing 100 g of CoCl2·6H2O and 35 g / L of H3BO3. A Pt mesh was used as the anode, and the other conditions were a temperature of 25 ℃, a flow rate of 200 rpm, and a current density of 30 mA / cm². 2 It was performed in. It is a pure Co-plated interconnect manufactured by the method described above.
[0079] <Comparative Example 2-1>
[0080] Fabrication of 100Co alloy thin films
[0081] To perform a tensile test on a pure Co thin film, the film was peeled off after electroplating. Unlike Comparative Example 2, electroplating was performed on a Ti plate, and the pump voltage was set to 160 V. This is a pure Co thin film prepared by the above method.
[0083] XRD measurement results and chromium volatility evaluation (SEM, EDS line scan) of Co-Ni alloy plated interconnects
[0084] Figure 5 shows the XRD measurement results of Example 1, Comparative Example 1, and Comparative Example 2, which are interconnects in which a Co-Ni alloy thin film with a different Co content or a pure Co thin film is plated on the surface of the interconnect. In this case, the plating thickness of the thin film may be 5 to 8 μm.
[0085] Referring to Fig. 5, in Comparative Example 2, where a pure Co thin film was plated, the (110)HCP peak appeared as the dominant crystalline phase. On the other hand, in Example 1 and Comparative Example 1, which are Co-Ni alloy thin films, it can be confirmed that (002)HCP, (111)FCC, and (020)FCC peaks mainly appeared. This supports the FCC and HCP mixed phases of the Co-Ni alloy. Additionally, the intensity of the (020)FCC peak in Example 1 showed a tendency to decrease compared to Comparative Example 1. That is, it can be determined that the FCC phase decreases as the Co content increases.
[0087] The composition of alloy elements was analyzed by performing an EDS line scan on the cross-sections of Example 1, Comparative Example 1, and Comparative Example 2, in which Co-Ni alloy thin films with different Co contents or pure Co thin films were plated on the surface of the interconnect. At this time, the plating thickness of the thin film may be 5 to 8 μm. The results are shown in Fig. 6a.
[0088] Referring to Fig. 6a, the EDS line scan analysis results confirm that Example 1 contains 60.83 wt% Co and 39.17 wt% Ni, Comparative Example 1 contains 41.08 wt% Co and 58.92 wt% Ni, and Comparative Example 2 contains 100 wt% Co. This confirms that thin films composed of components corresponding to 60Co-40Ni, 40Co-60Ni, and 100Co, respectively, were plated.
[0090] To evaluate the chromium volatility after heat treatment, SEM imaging and EDS line scanning were performed on the cross-sections of each sample to measure the thickness of the chromium oxide, i.e., the chromium enrichment layer, formed after heat treatment at 800 °C for 100 hours in Example 1, Comparative Example 1, and Comparative Example 2. The results are shown in Fig. 6b, and it can be confirmed whether diffusion of chromium oxide to the outside occurred through EDS line scan analysis. At this time, the plating thickness of the thin film may be 5 to 8 μm.
[0091] Referring to Fig. 6b, it can be seen that a chromium element peak was formed at the interface between the interconnect and the thin film in all of Example 1, Comparative Example 1, and Comparative Example 2. This means that no chromium diffusion to the outside occurred. These results can be seen as evidence that chromium volatilization at high temperatures was suppressed by plating a thin film on the interconnect.
[0092] In addition, through the thickness of the chromium oxide layer shown in each image, it can be confirmed that the thickness of the chromium oxide decreased as the Co content of the alloy thin film increased, moving from Comparative Example 1 to Example 1, compared to Comparative Example 2 where a pure Co thin film was plated. The thickness of the chromium oxide is 1.36 μm for Example 1, 2.04 μm for Comparative Example 1, and 2.28 μm for Comparative Example 2, respectively.
[0093] In particular, in the case of Example 1, where a 60Co-40Ni alloy thin film was plated on the interconnect, a 55% reduction in chromium oxide thickness was observed compared to Comparative Example 2. This can be seen as a result of the concentrated formation of a chromium enrichment layer at the interconnect-alloy thin film interface, as chromium within the interconnect is relatively easy to diffuse, whereas chromium diffusion is difficult within a spinel-type oxide layer such as Cr2O3.
[0095] Through the above results, it is possible to provide a manufacturing method for electroplating a Co-Ni alloy thin film having a mixed phase of FCC and HCP on the surface of an interconnect with a desired composition, and at the same time, it is possible to understand the effect of reducing chromium volatilization and chromium oxide thickness that can be obtained by plating the Co-Ni alloy thin film.
[0097] Evaluation of mechanical properties (tensile test, micro-Vickers hardness test) of Co-Ni alloy plated interconnects
[0098] To evaluate the mechanical properties of electroplated thin films, Examples 1-1, Comparative Example 1-1, and Comparative Example 2-1 were prepared. At this time, the thin film thickness was 10 μm and the tensile specimen size was 100 × 12.5 mm, and a tensile test was performed, and the results are shown in Fig. 7.
[0099] Figure 7 shows graphs representing the stress-strain curve, maximum tensile strength, and elongation, respectively. Through the stress-strain curve, it can be seen that Example 1-1, a 60Co-40Ni alloy thin film, exhibits the highest stress and strain in the tensile test results. Additionally, compared to Comparative Example 2-1, a pure Co thin film, it can be confirmed that the alloy thin films Example 1-1 and Comparative Example 1-1 exhibit higher stress and strain.
[0100] In addition, the results regarding the maximum tensile strength and elongation according to the Co content can be confirmed more specifically through the graphs of maximum tensile strength and elongation. In the case of the alloy thin films of Example 1-1 and Comparative Example 1-1, the maximum tensile strength and elongation graphs showed values of 1500 MPa or higher and 3% or higher, respectively. On the other hand, it can be confirmed that Comparative Example 2-1, a pure Co thin film, showed values of around 500 MPa and 1.75%.
[0102] Additionally, to evaluate the mechanical properties of the electroplated thin films, micro-Vickers hardness tests were performed on Example 1 and Comparative Example 2. The plating thickness was set to 150 μm, taking into account the criterion that the minimum thickness of the sample must be at least approximately 80 μm (based on an indentation diameter of 50 μm) for micro-hardness testing, as determined by theoretical calculations based on standard test specifications ASTM E384 and ISO 6507. To ensure stable and reliable measurements, the plating thickness was set to 150 μm with sufficient margin.
[0103] To minimize measurement errors caused by surface roughness after plating, surface grinding was performed in the order of 400, 600, 800, and 1200 grit to complete flattening. During the micro-Vickers hardness test, the indentation load was set to 0.3 kgf, and the measured indentation diameter ranged from 35 to 45 μm. Hardness measurements were repeated five times per sample to calculate the average value, and measurement reliability was ensured by moving a distance of at least three times the indentation diameter between measurements to conduct additional measurements. The results are shown in Fig. 8.
[0104] Referring to Fig. 8, it can be seen that the micro-Vickers hardness test results show that Example 1 has a hardness value of 500 MPa or higher and 600 MPa or lower, while Comparative Example 2 has a hardness value of around 300 MPa. In other words, it can be confirmed that the Co-Ni alloy plated interconnect has a higher hardness value.
[0106] Therefore, through the above results, it can be seen that the Co-Ni alloy thin film has superior mechanical properties compared to a pure Co thin film, and that as the Co content of the Co-Ni alloy thin film increases, the tensile strength, elongation, and hardness also increase.
[0108] ASR evaluation of Co-Ni alloy plated interconnects
[0109] To verify the chromium volatilization suppression effect of the alloy thin film, an Area Specific Resistance (ASR) evaluation was performed after oxidation, i.e., heat treatment at 800 °C for 500 hours. ASR is an indicator representing electrical resistance per unit area in an electrochemical system; a lower ASR of a component signifies lower energy loss and higher system efficiency in a solid oxide fuel cell. The electrical resistance of Example 1, Comparative Example 1, and Comparative Example 2, which were plated with 1 μm on each side, was measured using a 4-probe method while maintaining the temperature after heat treatment at 800 °C for 500 hours. Using the 4-probe method separates the current path and the voltage measurement path, allowing only the resistance of the sample itself to be measured. The results are shown in Fig. 9.
[0110] Referring to FIG. 9, Comparative Example 2, in which a pure Co thin film is plated on the interconnect, has an ASR value of 65.45 mΩ·cm 2 Thus, a value more than twice that of the interconnect plated with a Co-Ni alloy thin film can be confirmed. In addition, Comparative Example 1 is 31.36 mΩ·cm 2 , Example 1 is 21.87 mΩ·cm 2 It can be seen that it has an ASR value. Through this, the decrease in ASR with increasing Co content of the alloy thin film can be confirmed.
[0111] The low ASR of the interconnect can have the effects of improving the output, extending the lifespan, optimizing the operating temperature, and miniaturizing and reducing the weight of solid oxide fuel cells.
[0112] More specifically, since interconnects are components that electrically connect cells within a solid oxide fuel cell stack, lowering the interconnect's Anti-Resistance Ratio (ASR) allows current to flow more easily throughout the entire stack. Consequently, voltage loss is reduced, and cell output can be increased. While high resistance generates heat, a lower ASR reduces heat generation, thereby improving the reliability and lifespan of the entire stack. The smooth current flow resulting from the interconnect's low resistance enables stable operation of solid oxide fuel cells even at relatively low temperatures. This allows for the use of less expensive materials instead of high-cost heat-resistant metals or ceramics, thereby reducing manufacturing costs. Simultaneously, the reduced power loss caused by the use of low-ASR interconnects enables the same output while reducing the number of cells. Consequently, benefits such as stack size reduction, overall system weight reduction, and lower installation and transportation costs can be expected.
[0113] In other words, applying Co-Ni alloy-plated interconnects lowers the interconnect's ASR, which reduces current loss and heat generation, thereby improving the performance of solid oxide fuel cells and enabling stack miniaturization and cost reduction.
[0115] Results of chromium volatility measurement and microstructural analysis of Co-Ni alloy-plated interconnects
[0116] To measure the chromium volatilization of Co-Ni alloy plated interconnects, samples of Example 1 and Comparative Example 2 were prepared, heat-treated, and then ICP-OES analysis was performed.
[0117] The amount of volatilized chromium was analyzed after heat treatment for 100, 300, 600, and 1000 hours, respectively, in an atmosphere of 800 ℃ and air + 2H2O injected at a flow rate of 5000 ml / min. The results are shown in Fig. 10.
[0118] Referring to Fig. 10, it can be seen that compared to Comparative Example 2, the amount of accumulated volatilized chromium per unit area of Example 1 decreased to a level of 28.79% or more and 54.13% or less. Additionally, when averaging the values over 300, 600, and 1000 hours, it can be seen that the amount of chromium volatilized in Example 1 decreased by 41.87% compared to Comparative Example 2.
[0119] This is the result of effectively suppressing the chromium volatilization problem that occurs during the operation of solid oxide fuel cells, and it can be concluded that stable operation for a long time is possible.
[0121] Figure 11 shows the results of taking FIB channeling images to analyze the microstructures of Example 1, Comparative Example 1, and Comparative Example 2.
[0122] Referring to Fig. 11, the microstructure of Comparative Example 1 and Comparative Example 1, in which Co-Ni alloy was plated on the interconnect, showed a nanometer-scale equiaxed grain shape.
[0123] On the other hand, in Comparative Example 2, where a pure Co thin film was plated on the interconnect, elongated dendrites on a micrometer scale were exhibited. Through this, it can be confirmed that not only is there a solid solution strengthening effect due to the formation of a substitution solid solution of Co and Ni, but there is also a strength increase effect due to the reduction in grain size.
[0125] Ultimately, if Co-Ni alloy plating is applied to the interconnects of solid oxide fuel cells, it is expected that interconnects with excellent mechanical properties and electrical conductivity, as well as effectively suppressing chromium volatilization, can be fabricated.
[0127] The above-described embodiments are merely exemplary, and various other modified embodiments are possible therefrom for those skilled in the art.
[0128] Therefore, the true technical scope of protection of the present invention should include not only the above embodiments but also other embodiments that are variously modified according to the technical concept of the invention described in the following claims. Explanation of the symbols
[0129] S100: Interconnect manufacturing stage S110: Interconnect preparation stage S120: Co strike plating step S121 : Co Strike Plating Solution Preparation Step S122: Step of forming a Co-strike plating layer on the interconnect S130: Co-Ni alloy electroplating step S131 : Co-Ni alloy plating solution preparation step S132: Step of forming a Co-Ni alloy thin film on a Co strike-plated interconnect
Claims
Claim 1 A solid oxide fuel cell having an alloy-plated interconnect comprising: a plurality of single cells in which a solid oxide electrolyte is disposed between a fuel electrode and an air electrode; an interconnect that electrically connects the plurality of single cells; and a Co-Ni alloy thin film formed on the surface of the interconnect, having a mixed phase of FCC and HCP and having a nanometer-scale equiaxed grain shape, containing 50% or more and 84% or less of Co. Claim 2 A solid oxide fuel cell having an alloy-plated interconnect, further comprising, in claim 1, a Co strike plating layer formed between the surface of the interconnect and the Co-Ni alloy thin film. Claim 3 A method for manufacturing a solid oxide fuel cell comprising a plurality of single cells in which a solid oxide electrolyte is disposed between a fuel electrode and an air electrode, and an interconnect that electrically connects the single cells, comprising the steps of: preparing an Fe-Cr interconnect; striking-plating Co onto the Fe-Cr interconnect; and electroplating a Co-Ni alloy thin film onto the strike-plated Fe-Cr interconnect. Claim 4 In claim 3, the step of electroplating the Co-Ni alloy thin film is performed by immersing the strike-plated Fe-Cr-based interconnect in a Co-Ni alloy plating solution containing 40 to 70 g / L of CoCl2·6H2O, and the Co-Ni alloy thin film is a method for manufacturing a solid oxide fuel cell using an alloy-plated interconnect containing 50% or more and 84% or less of Co. Claim 5 In paragraph 3, the method for manufacturing a solid oxide fuel cell using an alloy-plated interconnect having a mixed phase of FCC and HCP is described. Claim 6 In paragraph 3, the Co-Ni alloy thin film is a method for manufacturing a solid oxide fuel cell using an alloy-plated interconnect having a nanometer-scale equiaxed grain shape.