Prussian Blue Analogue-Based Core-Shell Composite Cathode Active Material, Preparation Method Thereof, and Secondary Battery Comprising the Same
A core-shell structured PBA-based cathode active material with an organic shell addresses structural instability and metal ion leaching, enhancing electrochemical performance and enabling efficient, low-temperature manufacturing for sodium secondary batteries.
Patent Information
- Application Number
- KR1020250059938
- Authority / Receiving Office
- KR · KR
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-08
- Publication Date
- 2026-11-17
AI Technical Summary
Conventional Prussian Blue Analogue (PBA)-based cathode active materials suffer from structural instability, metal ion leaching, and interfacial side reactions, which degrade electrochemical performance and are exacerbated by high-temperature processing methods that conflict with low-cost and mass production advantages.
A core-shell structured PBA-based cathode active material is developed, featuring a PBA core coated with an organic shell containing ionic functional groups, formed through low-temperature wet processes, to enhance structural stability and suppress metal ion leaching and interfacial reactions.
The core-shell structure improves electrochemical performance by stabilizing the lattice, reducing interfacial resistance, and maintaining long-term cycle life, while allowing for simpler and more efficient manufacturing processes.
Smart Images

Figure PAT00001_ABST
Abstract
Description
Technology Field
[0001] The present disclosure relates to a Prussian Blue Analogue (PBA)-based cathode active material, a method for manufacturing the same, and a secondary battery comprising the same. More specifically, the present disclosure relates to a PBA-based core-shell structured organic composite cathode active material capable of simultaneously improving structural stability and interfacial stability by including PBA as a core and forming a shell layer made of an organic composition on the surface, a method for manufacturing the same, and a sodium secondary battery comprising the cathode active material. Background Technology
[0002] Due to their high energy density and long cycle life, lithium-ion batteries are widely used in applications ranging from small electronic devices to electric vehicles and energy storage systems (ESS). However, lithium resources are geographically uneven and supply is limited, and rising prices driven by increasing demand make it difficult to ensure economic viability when applied to large-scale energy storage systems.
[0003] Accordingly, sodium secondary batteries utilizing sodium, which is relatively abundant and inexpensive compared to lithium, have recently garnered attention as a next-generation energy storage medium, and active research based on various materials is underway (Chem. Eur. J. 2023, 29, e202202380). Sodium secondary batteries have the advantage of significantly reducing raw material costs while maintaining an operating principle similar to that of lithium secondary batteries, and are suitable for large-capacity storage systems due to the abundance of sodium resources and low cost.
[0004] One of the key factors determining the performance of sodium secondary batteries is the cathode active material, and various material groups are being proposed for this purpose. For example, transition metal oxides with a layered structure (Na₂S) 1-xMO2, M= Mn, Ni, Co, etc.), NASICON (Na Super Ionic Conductor)-based polyanionic compounds (Na3V2(PO4)3, etc.), and cyanide-based Prussian Blue and its analogues (Prussian Blue Analogue, PBA, Na x There are TM[TM(CN)6], TM= Mn, Ni, Fe, Co, etc.
[0005] Among these, PBA is based on a unique three-dimensional open lattice and sodium ions (Na + Insertion and removal of ) is easy, and Fe 2 + / Fe 3 + It exhibits high-speed charge and discharge characteristics through reversible oxidation-reduction reactions. In addition, it has the advantage of being capable of low-temperature synthesis based on an aqueous solution and being economically viable as it uses low-cost transition metals such as iron (Fe), manganese (Mn), and nickel (Ni) as main components.
[0006] However, zeolitic water and vacancies formed within the PBA structure can cause structural instability, and low electronic conductivity and metal ion leaching during repeated charge-discharge cycles can lead to the collapse of the electrode structure and degradation of electrochemical performance. Additionally, side reactions caused by interfacial reactions with the electrolyte are also pointed out as a problem (Nature Communications volume 16, Article number: 2520 (2025)).
[0007] To overcome these limitations, various surface modification technologies have been proposed. For example, techniques such as carbon coating, metal ion doping, acid treatment, and water of crystallization removal demonstrate a certain level of effectiveness; however, most require high-temperature heat treatment conditions, which entail problems such as crystal structure distortion, complex process conditions, and low yields. In particular, high-temperature processes conflict with the advantages of PBA, such as low-cost and mass production.
[0008] Therefore, a new surface modification method is required to overcome the technical limitations of conventional PBA-based cathode active materials. The problem to be solved
[0009] In one embodiment of the present disclosure, an organic composite PBA-based cathode active material having a core-shell structure is provided to improve the structural instability and electrochemical performance degradation caused by interfacial reactions of conventionally known Prussian blue analog (PBA)-based cathode active materials.
[0010] In another embodiment of the present disclosure, an organic composite PBA-based cathode active material having a core-shell structure is provided, which can suppress the leaching of metal ions, lattice breakdown, and interfacial side reactions, and improve initial efficiency and long-term cycle life by forming an organic shell having ionic functional groups on the surface of PBA particles.
[0011] According to another embodiment of the present disclosure, a method for manufacturing a positive electrode active material is provided through an organic composite shell forming process that can be performed under low-temperature wet conditions and does not require complex processes or high-temperature heat treatment, thereby simultaneously ensuring structural stability of the electrode active material and simplicity of the manufacturing process.
[0012] In another embodiment of the present disclosure, a sodium secondary battery is provided using a PBA-based positive electrode active material of the aforementioned organic composite core-shell structure. means of solving the problem
[0013] According to the first aspect of the present disclosure,
[0014] An organic composite cathode active material having a core-shell structure based on a Prussian blue analog (PBA) may be provided, comprising: a core containing PBA; and a shell formed of a low-molecular-weight or high-molecular-weight organic composition that is bonded to the surface of the core through coordination bonding or hydrogen bonding and comprises an ionic functional group containing sodium ions or having sodium ion conductivity.
[0015] According to an exemplary embodiment, the Prussian blue analog can be represented by the following chemical formula 1.
[0016] [Chemical Formula 1]
[0017] A x M[M'(CN)6] 1- y (Vac) y ·nH2O
[0018] In the above chemical formula 1, A may be a group 1 element, M and M' may be at least one selected from the group consisting of Mg, Ca, Al, Ga, In, Sn, Pb, Sc, Ti, V, Cr, Fe, Co, Ni, Mn, Cu, Zn, Pd, Ag, Cd or combinations thereof, Vac may be a vacancy of M'(CN)6, 0 < x ≤ 2, 0 ≤ y ≤ 1, and 0 ≤ n ≤ 6.
[0019] According to an exemplary embodiment, the organic composition may include at least one selected from p-type, n-type, or bipolar organic materials.
[0020] According to an exemplary embodiment, the p-type organic material may be an aromatic polycarboxylic acid derivative and may include at least one selected from the group consisting of terephthalic acid, 2,5-dihydroxyterephthalic acid, trimesic acid, pyromellitic acid, melitic acid, 4,4'-biphenyldicarboxylic acid, 2,6-naphthalenedicarboxylic acid, and 4,4'-dithiobisbenzoic acid.
[0021] According to an exemplary embodiment, the n-type organic material may be a quinone-based or rhodizonate-based compound and may include at least one selected from the group consisting of 1,4,5,8-tetraaminoanthraquinone, anthraquinone, 1,4-naphthoquinone, disodium rhodizonate, dipotassium rhodizonate, and dilithium rhodizonate.
[0022] According to an exemplary embodiment, the organic composition may comprise at least one selected from the group consisting of tetrasodium 2,5-dihydroxyterephthalate (Na4DHTP), disodium 1,4,5,8-tetraaminoanthraquinone (Na2TAAQ), or a mixture thereof.
[0023] According to an exemplary embodiment, the shell may further include an organic compound containing an ionic functional group.
[0024] According to an exemplary embodiment, the core has an average particle size (D) controlled in the range of 0.1 to 10 μm. 50 Can have ).
[0025] According to an exemplary embodiment, the charge transfer resistance (Rct) of the electrode composed of the positive active material may be 10 to 300 Ω.
[0026] According to an exemplary embodiment, the thickness of the shell may be 0.01 to 5 μm.
[0027] According to an exemplary embodiment, the thickness ratio of the core to the shell can be adjusted in the range of 1:0.02 to 0.8.
[0028] According to an exemplary embodiment, the positive electrode active material has an average particle size (D) controlled in the range of 0.1 to 10 μm. 50 Can have ).
[0029] According to the second aspect of the present disclosure,
[0030] A method for manufacturing an organic composite cathode active material having a core-shell structure based on the above-mentioned Prussian blue analog (PBA), wherein
[0031] A method for manufacturing an anode active material may be provided, comprising the steps of: forming a core comprising a Prussian blue analog (PBA) represented by the following chemical formula 1; preparing a dispersion by dispersing a low molecular weight or high molecular weight organic composition in a solvent; neutralizing the dispersion to a pH of 6 to 10 by adding a basic compound; and adding the core to the dispersion to form an organic composite shell layer on the surface of the core.
[0032] [Chemical Formula 1]
[0033] A x M[M'(CN)6] 1- y (Vac) y ·nH2O
[0034] In the above chemical formula 1, A may be a group 1 element, M and M' may be at least one selected from Mg, Ca, Al, Ga, In, Sn, Pb, Sc, Ti, V, Cr, Fe, Co, Ni, Mn, Cu, Zn, Pd, Ag, Cd, or a combination thereof, Vac may be a vacancy of M'(CN)6, 0 < x ≤ 2, 0 ≤ y ≤ 1, and 0 ≤ n ≤ 6.
[0035] According to an exemplary embodiment, the core may be formed by adding sodium ferrocyanide to a saturated NaCl solution, adding HCl dropwise, stirring at 40 to 100°C for 1 to 12 hours, and aging at 10 to 80°C for 4 to 24 hours.
[0036] According to an exemplary embodiment, the solvent may be selected from an aqueous solvent, a non-aqueous (anhydrous) solvent, or a mixture thereof, and the aqueous solvent may be selected from the group consisting of deionized water (DIW), distilled water, ultrapure water, or a combination thereof, and the non-aqueous solvent may be selected from the group consisting of anhydrous ethanol, anhydrous acetonitrile, anhydrous methanol, anhydrous tetrahydrofuran, anhydrous acetone, anhydrous propylene carbonate, dimethyl sulfoxide (DMSO), dimethylformamide (DMF), or a combination thereof.
[0037] According to an exemplary embodiment, the basic compound may be at least one selected from the group consisting of sodium hydroxide (NaOH), sodium carbonate (Na2CO3), sodium methoxide (NaOCH3), sodium tert-butoxide (NaOC(CH3)3) or derivatives thereof.
[0038] According to an exemplary embodiment, the reaction forming the organic composite shell layer can be carried out at 20 to 80°C.
[0039] According to an exemplary embodiment, the method may further include a step of drying at a temperature of 50 to 200°C and a pressure of 0.2 Torr or less after forming the shell layer.
[0040] According to the third aspect of the present disclosure,
[0041] A sodium secondary battery may be provided comprising: a positive electrode including the positive active material; a negative electrode disposed opposite to the positive electrode; a separator disposed between the positive electrode and the negative electrode; and an electrolyte in contact with the positive electrode and the negative electrode. Effects of the invention
[0042] According to one embodiment, a composite cathode active material based on a Prussian blue analog (PBA) can effectively suppress the breakdown of the lattice structure and the leaching of metal ions during charge and discharge cycles by forming a low-molecular-weight or high-molecular-weight organic shell layer on the surface of the PBA core through coordination bonding or hydrogen bonding, thereby preventing degradation of electrochemical performance.
[0043] In addition, according to one embodiment, the organic material-based shell layer is a sodium ion (Na + It contains ) so that a stable initial capacity can be secured by replenishing sodium ions that are detached from the PBA core during initial charging.
[0044] In addition, according to one embodiment, the organic shell layer acts as a physical and chemical barrier at the interface with the electrolyte, thereby reducing side reactions and interfacial resistance, and thus has the advantage of simultaneously improving long-term cycle life and high-speed charge / discharge characteristics.
[0045] In addition, the manufacturing method according to one embodiment can uniformly form an organic shell layer using only a wet process under low-temperature conditions without high-temperature heat treatment, so that an active material can be manufactured reproducibly while maintaining the stability of the PBA crystal structure, and can also provide advantageous effects in terms of process simplification and mass production.
[0046] Therefore, the core-shell structured organic composite PBA-based cathode active material according to the present embodiment can exhibit excellent performance in terms of long lifespan, initial efficiency, structural stability, and ease of manufacturing, and is expected to be effectively applied in high-reliability applications such as large-scale energy storage systems (ESS) and batteries for electric vehicles. Brief explanation of the drawing
[0047] FIG. 1 is a diagram schematically illustrating the form and layer structure of a core-shell structured organic composite cathode active material based on a Prussian Blue Analogue (PBA) according to one embodiment; FIG. 2 is a flowchart schematically illustrating a process for manufacturing a core-shell structured organic composite cathode active material based on a Prussian Blue Analogue (PBA) according to an exemplary embodiment; FIGS. 3a to 3c are each graphs showing the results of X-ray diffraction (XRD) analysis for the cathode active material samples prepared in Example 1 and Comparative Examples 1 to 2, respectively; and Figures 4a to 4c are FE-SEM images of the positive electrode active materials prepared in Example 1 and Comparative Examples 1 to 2, respectively. Specific details for implementing the invention
[0048] The present disclosure can be fully achieved by the following description. The following description should be understood as describing preferred embodiments of the present disclosure, but is not necessarily limited thereto. Additionally, the accompanying drawings are for illustrative purposes only and are not limiting to the present disclosure; details regarding individual configurations may be appropriately understood in accordance with the specific intent of the relevant descriptions set forth below.
[0049] “Positive” and “negative” respectively refer to the electrodes of a battery; in the charging cycle of a sodium-ion secondary battery, Na ions (Na + ) separates from the anode and moves to the cathode, while electrons move from the anode to the cathode through the external circuit. On the other hand, in a discharge cycle, Na ions move from the cathode to the anode, while electrons detach from the cathode and move to the anode through the external circuit.
[0050] "Prussian blue analogues (PBAs)" are a type of metal-organic framework (MOF), and their lattice structure consists of two or more transition metal cations each having six cyanide ligands (CN - It is formed by coordination bonding with ) and octahedrons, and exhibits a face-centered cubic or face-centered structure in which cyanide ligands act as bridges to connect two transition metal cations. Therefore, PBA has an open framework, and as a result, the interstitial sites and ion diffusion channels within the crystal are wider compared to other crystalline inorganic materials.
[0051] “Crystal” or “crystallism” typically refers to any solid material in which atoms are arranged to have a lattice structure (e.g., three-dimensional order), which can generally be identified by XRD analysis.
[0052] "Electrode density" refers to the mass per unit volume of a battery electrode (positive or negative electrode) and can be calculated by dividing the total mass, including all constituent components such as active material, binder, and conductive material contained in the electrode sheet, by the volume of the electrode. A higher electrode density allows for a greater amount of active material to be packed within the same volume, indicating that a battery of the same size can store a greater amount of energy.
[0053] “Loading” or “coating” can be understood as a concept that includes not only cases where it is formed in the form of an externally distinguishable layer or film on the surface of a specific structure, but also cases where it is formed in a form that penetrates into pores or voids formed in the surface area of the structure.
[0054] "Electrolyte" can refer to a substance that acts as an ion-conducting medium, enabling the movement of electrons and cations within electrochemical devices, such as secondary batteries.
[0055] "Capacity" may refer to a measurement of the total charge that can be delivered by the battery, which determines the run time that the battery can provide under given load conditions, and can be calculated by multiplying the delivered current by the delivery time. Additionally, specific capacity may be defined as the total capacity per unit weight or volume of the battery, and can typically be expressed in Ah / g or mAh / g.
[0056] "Capacity retention rate" may refer to the fraction of the total capacity available from a battery under specific discharge conditions after being cycled or stored for a certain period.
[0057] In a narrow sense, "contact" means direct contact between two objects, but in a broad sense, it can be understood as allowing any additional component to be involved.
[0058] Where a numerical range is specified as a lower limit and / or an upper limit in this specification, it may be understood that any sub-combination within said numerical range is also disclosed. For example, if written as “1 to 5,” it may include 1, 2, 3, 4 and 5, as well as any sub-combination between them.
[0059] The expressions "on" and "above" can be understood as being used to refer to concepts of relative position. Therefore, this includes not only cases where other components or layers exist directly on the mentioned layer, but also cases where other layers (intermediate layers) or components are interposed or exist between them, or forms formed by partially overlapping in the space between the relevant members. Similarly, expressions such as "below," "in the lower part," and "below," as well as the expression "between," can also be understood as concepts of relative position. Furthermore, the expression "sequentially" can also be understood as a concept of relative position.
[0060] In this specification, when a component is described as "comprising," it means that, unless otherwise noted, it may further include other components and / or steps.
[0062] Prussian Blue Analogue ( PBA )-based core-shell structured organic composite cathode active material
[0064] According to one embodiment of the present disclosure, an organic composite cathode active material having a core-shell structure based on a Prussian blue analog (PBA) is provided, comprising: a core containing PBA; and a shell formed from a low-molecular-weight or high-molecular-weight organic composition that is bonded to the surface of the core via coordination bonding or hydrogen bonding and comprises an ionic functional group containing sodium ions or having sodium ion conductivity. Through this structure, electron and ion transport pathways can be shortened while interfacial stability can be improved, and the problem of reduced initial storage of sodium ions can also be mitigated.
[0065] The PBA-based organic composite cathode active material according to one embodiment can minimize lattice instability issues caused by vacancies or crystal water that may exist within the PBA crystal structure, and can maintain structural stability even during long-term charging and discharging by suppressing interfacial reactions with the electrolyte. In particular, as the organic shell acts as a physical and chemical buffer layer between the inner core and the outer electrolyte, it can effectively prevent the leaching of metal ions (such as Mn) and cracking caused by changes in electrode volume that may occur during repeated charging and discharging processes. As a result, it exhibits excellent performance in terms of electrochemical cycle life, initial efficiency, and charge transfer resistance (Rct), and can overcome the technical limitations of existing inorganic-based single-core or single-core-shell structures.
[0066] The shape and layer structure of a PBA-based organic composite cathode active material according to an exemplary embodiment are as shown in FIG. 1.
[0067] Referring to the drawing above, the organic composite cathode active material (100) having a PBA-based core-shell structure comprises a core (110) and a shell (120), and the core (110) and the shell (120) are formed (stacked) in a core-shell structure.
[0068] According to the illustrated embodiment, the core (110) is a crystal containing PBA and may include one or more transition metals such as, for example, Mn, Fe, Ni, Cu, Zn, Co. The core (110) according to the exemplary embodiment may be, for example, Mn-PBA, Fe-PBA, Ni-PBA, Cu-PBA, Zn-PBA, or Co-PBA.
[0069] At this time, the size (or average particle size (D) of the core (110) 50 )) can be determined by considering the synthesis conditions and application purpose, for example, it may be controlled within the range of about 0.1 to 10 μm, specifically about 0.3 to 8 μm, and more specifically about 0.5 to 6 μm.
[0070] According to an exemplary embodiment, the PBA forming the core (110) can be represented by Chemical Formula 1.
[0071] [Chemical Formula 1]
[0072] A x M[M'(CN)6] 1- y (Vac) y ·nH2O
[0073] In the above chemical formula 1, A may be a Group 1 element and may include, for example, sodium (Na), lithium (Li), potassium (K), rubidium (Rb), cesium (Cs), etc. M and M' may be at least one selected from the group consisting of Mg, Ca, Al, Ga, In, Sn, Pb, Sc, Ti, V, Cr, Fe, Co, Ni, Mn, Cu, Zn, Pd, Ag, Cd, or combinations thereof. Vac refers to a defect or vacancy in M'(CN)6. x may be in the range 0 < x ≤ 2 (specifically 0.2 ≤ x ≤ 1.9, more specifically 0.5 ≤ x ≤ 1.8), y may be in the range 0 ≤ y ≤ 1 (specifically 0 ≤ y ≤ 0.8, more specifically 0 ≤ y ≤ 0.5), and n may be in the range 0 ≤ n ≤ 6 (specifically 0 ≤ n ≤ 4, more specifically 0 ≤ n ≤ 2).
[0075] Referring again to FIG. 1, a shell layer (120) may be formed along the surface or outer surface of the core (110). Specifically, the shell (120) may be an organic layer that surrounds the surface of the core (110) and is chemically or physically bonded through coordination bonds or hydrogen bonds. The shell (120) may be made of a low-molecular or high-molecular organic composition containing sodium ions or ionic functional groups having sodium ion conductivity. Such an organic shell (120) can stabilize the crystal structure of the core, suppress side reactions that may occur at the electrode-electrolyte interface by blocking direct interfacial contact with the electrolyte, and improve electrochemical durability by preventing the leaching of metal ions and structural collapse.
[0076] The organic composition according to the exemplary embodiment is a low-molecular-weight or high-molecular-weight organic material, and the range of their molecular weights can be controlled considering the stable bonding of ionic functional groups, effective coating properties on the core surface, and improved interfacial stability with the electrolyte. For example, the low-molecular-weight organic material may have a molecular weight in the range of about 50 to 1,300 g / mol, specifically about 70 to 1,000 g / mol, more specifically about 100 to 700 g / mol, but is not limited thereto. Meanwhile, in the case of the high-molecular-weight organic material, the molecular weight may be selected in the range of, for example, about 10,000 to 300,000 g / mol, specifically about 50,000 to 200,000 g / mol, more specifically about 70,000 to 150,000 g / mol, but is not limited thereto. The molecular weight of the organic material can contribute to securing the coating thickness and physical stability of the organic material.
[0077] The above organic composition may include ionic functional groups such as carboxylic acid groups (-COOH), hydroxyl groups (-OH), sulfonic acid groups (-SO3H), and amino groups (-NH2). These functional groups can simultaneously improve interfacial stability and electrochemical activity by forming coordination bonds with the metal center of the core or by providing transport pathways for sodium ions. Specifically, the above ionic functional groups [contain] sodium ions (Na + It may include ) or be a functional group that forms a binding structure favorable for the transport of sodium ions. For example, a negatively charged carboxylate (-COO - ), phosphate (-PO4 2- ), sulfonate (-SO3 - Functional groups such as ) can contribute to lowering ion transport resistance at the interface with the electrolyte by providing a transport channel for sodium ions.
[0078] In addition, sodium ions present in the organic shell (120) can minimize initial irreversible capacity loss and improve initial efficiency by replenishing sodium ions that are depleted from the core during initial charging.
[0079] The organic composition included in the shell (120) may include at least one selected from p-type organic material, n-type organic material, or bipolar organic material.
[0080] The above p-type organic material is an organic compound acting as an electron donor and may be an aromatic polycarboxylic acid derivative, for example, carbozol, thiophene, triphenylamine, phthalic acid (benzene-1,2-dicarboxylic acid), isophthalic acid (benzene-1,3-dicarboxylic acid), terephthalic acid (benzene-1,4-dicarboxylic acid), 2,5-dihydroxyterephthalic acid, fumaric acid (trans-1,2-ethane dicarboxylic acid), trimesic acid (benzene-1,3,5-tricarboxylic acid), pyromellitic acid (benzene-1,2,4,5-tetraarboxylic acid), melitic acid (benzene hexacarboxylic acid), 4,4'-biphenyldicarboxylic acid, 2,6-naphthalenedicarboxylic acid, Diphenic acid, 4,4'-oxydibenzoic acid (4,4'-Dicarboxydiphenyl ether), 4,4'-dithiobisbenzoic acid (4,4'-Dithiobisbenzoic acid), etc. may be included.
[0081] The above n-type organic material may be a quinone-based or rhodizonate-based compound, for example, as a quinone-based compound, 1,4-benzoquinone, 1,2-benzoquinone (ortho-benzoquinone), anthraquinone, 1,4-naphthoquinone, 2,6-dihydroxy-1,4-benzoquinone, 5,8-dihydroxy-1,4-naphthoquinone, 2,5-dihydroxy-1,4-benzoquinone, 2,3-dihydroxy-1,4-naphthoquinone, 1,4,5,8-Tetraaminoanthraquinone, 9,10-anthraquinone, 5,12-naphthacenquinone, etc. may be included, and as rhodizonate compounds, disodium rhodizonate, dipotassium rhodizonate, diammonium rhodizonate, dicalcium rhodizonate, dibarium rhodizonate, dilithium rhodizonate, dimagnesium rhodizonate, distrontium rhodizonate, etc. may be included.
[0082] The above-mentioned bipolar organic material may include, for example, tetrathiafulvalene (TTF), tetracyanoquinodimethane (TCNQ), hydroquinone (1,4-benzenediol), pyromellitic diimide, perylene tetracarboxylic anhydride (PTCDA), etc.
[0083] The electron / ion conductivity characteristics can be adjusted according to the composition of the shell as described above, and accordingly, electrochemical performance and cycle life can also be improved.
[0084] According to an exemplary embodiment, the thickness of the shell (120) can be adjusted in the range of, for example, about 0.01 to 5 μm, specifically about 0.02 to 3 μm, more specifically about 0.05 to 2 μm.
[0085] According to one embodiment, the ratio between the core and the shell may be appropriately adjusted to achieve interfacial stability and improved electrochemical performance. In this regard, the thickness ratio of the core (110) to the shell (120) may be adjusted in the range of 1: about 0.02 to 0.8, specifically 1: about 0.05 to 0.5, more specifically 1: about 0.08 to 0.3. Since performance degradation due to inhibition of ion transfer or reduced protective effect of the shell may occur if the ratio between the core and the shell is not adjusted to an appropriate range, it may be advantageous to adjust it appropriately within the aforementioned range, but this should be understood as illustrative.
[0087] The organic composite core-shell according to the present embodiment offers the advantage of controlling reactivity with the outside while maintaining the structure of the core, and as a result, electrochemical cycle life, initial efficiency, and characteristics can be significantly improved. In addition, by controlling the composition and thickness of the organic shell layer, interparticle cohesion and dispersibility can be improved, and it can also contribute to improving coating uniformity and slurry stability during electrode manufacturing.
[0089] According to exemplary embodiments, water in the PBA, particularly water of crystallization, may refer to water molecules occupying the interstitial space or gaps of the PBA product, specifically water molecules contained in a certain proportion within the crystal structure. Since these water molecules exist without being directly coordinated to metal ions or other ions and can act as a limiting factor in actual capacity by reducing active sites, it may be advantageous to have a water of crystallization content as low as possible. In this regard, the total water of crystallization content in the cathode active material according to exemplary embodiments may be, for example, about 8 wt% or less, specifically about 5 wt% or less, more specifically about 3 wt% or less, particularly specifically about 1 wt% or less. In certain embodiments, the cathode active material may not substantially contain water of crystallization.
[0091] In addition, the cathode active material according to the exemplary embodiment may exhibit a capacity retention rate of, for example, at least about 75%, specifically at least about 84%, more specifically at least 89% after 200 cycles, which may be a significant improvement compared to the capacity retention rates of 88% and 75%, respectively, of a cathode active material made of a single PBA and a single organic material under the same conditions.
[0093] Prussian Blue Analogue ( PBA Method for manufacturing an organic composite cathode active material having a )-based core-shell structure
[0095] According to another embodiment of the present disclosure, a method for manufacturing an organic composite cathode active material having a core-shell structure based on the aforementioned Prussian blue analog (PBA) is provided.
[0096] According to another embodiment of the present disclosure, a method for manufacturing an organic composite cathode active material having a core-shell structure based on a Prussian blue analog (PBA) may be provided, comprising the steps of: forming a core comprising a Prussian blue analog (PBA); preparing a dispersion by dispersing a low molecular weight or high molecular weight organic composition in a solvent; neutralizing the dispersion to a pH of 6 to 10 by adding a basic compound; and adding the core to the dispersion and stirring so that an organic composite shell layer is formed on the surface of the core.
[0097] According to an exemplary embodiment, the solvent may be selected from an aqueous solvent, a non-aqueous (anhydrous) solvent, or a mixture thereof, and the aqueous solvent may be selected from the group consisting of deionized water (DIW), distilled water, ultrapure water, or a combination thereof, and the non-aqueous solvent may be selected from the group consisting of anhydrous ethanol, anhydrous acetonitrile, anhydrous methanol, anhydrous tetrahydrofuran, anhydrous acetone, anhydrous propylene carbonate, dimethyl sulfoxide (DMSO), dimethylformamide (DMF), or a combination thereof.
[0098] For example, a dropwise method with a controlled addition rate can be adopted during the bonding reaction between the core surface and the shell, and it may involve maintaining a pH within an appropriate range during the synthesis of the core and the shell, respectively. The above manufacturing method can stably form an interface between the core and the shell based on a wet reaction process without high temperature and high pressure conditions or complex gas phase reactions, thereby providing excellent process reproducibility, and can effectively improve the electrochemical performance of the cathode active material by precisely controlling the composition and thickness of the organic shell.
[0099] FIG. 2 is a flowchart illustrating the manufacturing process of a Prussian blue analog (PBA)-based organic composite cathode active material according to one embodiment of the present disclosure.
[0100] Referring to FIG. 2, a PBA-based core-shell structure organic composite cathode active material according to one embodiment of the present disclosure can be manufactured by a manufacturing method comprising: a step of forming a Prussian blue analog core; a step of preparing an organic dispersion; a step of adding and neutralizing a basic compound; a step of forming a core-shell structure; and a step of filtration, washing, and drying.
[0101] First, the PBA core formation step is explained in detail below.
[0103] - Core formation
[0104] According to one embodiment of the present disclosure, a core comprising a Prussian blue analog (PBA) represented by the following chemical formula 1 is formed.
[0105] [Chemical Formula 1]
[0106] A x M[M'(CN)6] 1- y (Vac) y ·nH2O
[0107] In the above chemical formula 1, A may be a group 1 element, M and M' may be at least one selected from Mg, Ca, Al, Ga, In, Sn, Pb, Sc, Ti, V, Cr, Fe, Co, Ni, Mn, Cu, Zn, Pd, Ag, Cd, or a combination thereof, Vac represents a defect or vacancy of M'(CN)6, x may be 0 < x ≤ 2, y may be 0 ≤ y ≤ 1, and n may be 0 ≤ n ≤ 6.
[0108] According to an exemplary embodiment, the process of forming a core having a Prussian blue analog structure using an aqueous solution containing a metal cyanide compound and an acid is as follows.
[0109] First, an aqueous solution of a metal cyanide compound (e.g., hexacyanoferrate (II), hexacyanomanganate (II), hexacyanocobaltate (III), hexacyanochromate (III), etc.) is prepared, and the pH of the reaction solution is adjusted by adding an acid (e.g., hydrochloric acid, sulfuric acid, nitric acid, etc.). Then, a PBA core having a crystal structure can be formed by aging the reaction mixture.
[0110] For example, the core may be formed by adding sodium ferrocyanide (Na4Fe(CN)6) to a saturated NaCl solution, adjusting the pH by adding hydrochloric acid (HCl) dropwise, stirring at 40 to 100°C for 1 to 12 hours, and aging at 10 to 80°C for 4 to 24 hours.
[0111] As an example, aging can be controlled in a range of, for example, about 10 to 80°C, specifically about 15 to 60°C, more specifically about 20 to 40°C, and the aging time can be controlled in a range of, for example, about 4 to 24 hours, specifically about 5 to 20 hours, more specifically about 6 to 18 hours. The aforementioned aging conditions should be understood as exemplary.
[0112] Meanwhile, the concentration of PBA in a saturated NaCl solution can be adjusted by considering the stability of sodium ion supply within the PBA structure, the formation of the crystal structure, and the maintenance of compositional balance, for example, in the range of about 0.01 to 1 M, specifically about 0.02 to 0.5 M, and more specifically about 0.04 to 0.1 M, but is not limited thereto.
[0113] In the present embodiment, the PBA formation reaction may be carried out in air or an inert atmosphere; however, it may be advantageous to carry out the reaction in an inert atmosphere to suppress the formation of oxides within the crystal structure. In this case, the inert atmosphere may be formed by at least one gas selected from nitrogen (N2), argon (Ar), helium (He), krypton (Kr), xenon (Xe), etc.
[0114] According to an exemplary embodiment, the reaction temperature for forming the PBA core can be performed in a range of, for example, about 40 to 150 ℃, specifically about 50 to 100 ℃, more specifically about 60 to 80 ℃.
[0115] According to an exemplary embodiment, maintaining the pH of the saturated solution within a predetermined range after adding sodium ferrocyanide to a saturated NaCl solution may be advantageous in terms of ensuring the stability of the PBA crystal structure and suppressing the formation of impurities. In this regard, the pH of the saturated solution (reaction medium) after the addition of sodium ferrocyanide (specifically after the dropping point is completed) may be controlled in a range of, for example, about 5 to 10, specifically about 6 to 9, and more specifically about 6.5 to 8.5. Subsequently, an acid is added (specifically, dropwise) after the addition of sodium ferrocyanide to form PBA, and this acid may be at least one selected from hydrochloric acid (HCl), sulfuric acid (H2SO4), nitric acid (HNO3), etc., and specifically may be hydrochloric acid. In addition, the concentration of the added acid may be controlled in a range of, for example, about 0.01 to 8 M, specifically about 0.05 to 5 M.
[0117] - Synthesis of organic composite shells
[0118] Referring to FIG. 2, a powder or suspension containing the above-described PBA-based core is prepared, and then a low-molecular-weight or high-molecular-weight organic composition is added to a dispersion prepared by dispersing it in a solvent, and then a basic compound is added to neutralize the pH of the dispersion to a range of about 6 to 10, and the mixture is stirred to perform a reaction so that an organic composite shell layer is formed on the surface of the core.
[0119] According to an exemplary embodiment, the solvent may be selected from an aqueous solvent, a non-aqueous (anhydrous) solvent, or a mixture thereof, and the aqueous solvent may be selected from the group consisting of deionized water (DIW), distilled water, ultrapure water, or a combination thereof, and the non-aqueous solvent may be selected from the group consisting of anhydrous ethanol, anhydrous acetonitrile, anhydrous methanol, anhydrous tetrahydrofuran, anhydrous acetone, anhydrous propylene carbonate, dimethyl sulfoxide (DMSO), dimethylformamide (DMF), or a combination thereof.
[0120] In addition, the above organic composition may have a structure containing sodium ions or ionic functional groups having sodium ion conductivity, and may include at least one of low-molecular-weight or high-molecular-weight materials, specifically examples include tetrasodium 2,5-dihydroxyterephthalate (Na4DHTP), disodium 1,4,5,8-tetraaminoanthraquinone (Na2TAAQ), etc.
[0121] The above basic compound may be at least one selected from the group consisting of sodium hydroxide (NaOH), sodium carbonate (Na2CO3), sodium methoxide (NaOCH₃), sodium tert-butoxide (NaOC(CH₃)₃), or derivatives thereof, and enables stable attachment of the organic composite shell layer through a neutralization reaction with organic ions generated during the reaction.
[0122] In addition, the synthesis reaction for forming the organic composite shell layer can be carried out in the atmosphere mentioned in the aforementioned core synthesis.
[0123] In an exemplary embodiment, the reaction for synthesizing the organic composite shell layer may be carried out at a lower temperature than the preceding core synthesis reaction. For example, the reaction for forming the organic composite shell layer may be in the range of, for instance, about 10 to 80°C, specifically about 15 to 60°C, more specifically about 20 to 40°C, and this may be understood as being for illustrative purposes.
[0124] According to exemplary embodiments, maintaining the pH of the reaction medium, i.e., the dispersion, within a predetermined range during the process of adding a basic compound may be advantageous in terms of stably dissociating ionic functional groups, ensuring uniform adhesion to the core surface of the organic composition, and controlling the progress and reactivity of the shell formation reaction. In this regard, the pH of the reaction medium after the addition of the basic compound (specifically after the dropping point is finished) can be controlled within the aforementioned range (e.g., about 6 to 10), and in some cases, may involve the addition of an acid component to control the pH. As this has been described in detail above, further details are omitted.
[0126] - Post-processing stage
[0127] As described above, after the synthesis process of the core-shell structured organic composite PBA product is completed, a step of obtaining a high-purity composite PBA compound may be performed through a post-processing process known in the art, such as separation (or separation-purification). As an example, to obtain a product in solid form, solid-liquid separation known in the art, such as filtration or centrifugation, may be performed. Then, to remove by-products, residual reactants, and various impurities contained in the solid, a washing or cleaning process may be performed at least once if necessary. Such washing or cleaning may be, for example, water washing, and may be performed two or more times if necessary; since post-processing processes such as washing or cleaning are known in the art, a detailed description will be omitted.
[0128] Meanwhile, after washing or cleaning is completed, a normal drying step may be performed, and such drying is not limited to a specific method. For example, drying may be performed under elevated temperature conditions, and the drying temperature may be controlled, for example, in the range of about 50 to 200 ℃ or about 70 to 170 ℃, specifically about 80 to 150 ℃, more specifically about 90 to 130 ℃.
[0129] However, considering that if the composite PBA product contains an excess amount of moisture, it may exist in a state where it is not directly coordinated to metal ions or other ions, thereby reducing active sites and acting as a limiting factor for actual capacity, drying may be performed under reduced pressure or vacuum conditions. At this time, the applied pressure may be controlled, for example, to about 0.2 Torr or less, specifically about 0.1 Torr or less, and more specifically about 0.05 Torr or less, but this should be understood as illustrative. The aforementioned drying conditions should be understood as illustrative.
[0131] Manufacturing of electrodes (anodes)
[0133] According to an exemplary embodiment, a series of processes for manufacturing a core-shell structured organic composite cathode based on a Prussian blue analog (PBA) is as follows. The material of the electrode substrate (or current collector) used in the manufacture of the cathode is not particularly limited, as long as it is of a type generally applicable in the manufacture of sodium-ion secondary batteries. According to an exemplary embodiment, the electrode substrate may be, for example, aluminum, stainless steel, nickel, titanium, copper, or aluminum or stainless steel with carbon, nickel, titanium, or silver treated on its surface, but this should be understood as being for illustrative purposes. According to a specific embodiment, the material of the electrode substrate may be aluminum.
[0134] In addition, the thickness of the electrode substrate can be determined by considering conductivity and resistance characteristics, mechanical strength, etc., and may be, for example, in the range of about 2 to 50 μm, specifically about 5 to 30 μm, more specifically about 10 to 20 μm, but is not limited thereto.
[0135] Subsequently, a layer containing the aforementioned PBA-based organic composite cathode active material can be formed on an electrode substrate. To this end, an electrode forming slurry containing the PBA cathode active material is prepared. According to an exemplary embodiment, the content of the PBA cathode active material in the electrode forming slurry can be controlled in the range of, for example, about 10 to 98 weight%, specifically about 30 to 96 weight%, more specifically about 50 to 94 weight%, and particularly specifically about 70 to 92 weight%. According to an exemplary embodiment, the electrode forming slurry may contain PBA, a conductive material, a binder, etc., in a solvent.
[0136] According to an exemplary embodiment, the binder usable in the preparation of the slurry may be of a type known in the art, for example, a polymeric binder. Exemplarily, a fluorine-containing resin may be used, examples of which may include polytetrafluoroethylene (PTFE), polyvinylene difluoride (PVdF), poly(vinylene difluoride-hexafluoropropylene) copolymer (PVdF-HFP), etc. According to an exemplary embodiment, a thermoplastic resin may be used as a binder, for example, styrene-butadiene rubber (SBR), polyacrylonitrile (PAN), nitrile-butylene rubber (NBR), polybutadiene, polyisoprene, etc. According to exemplary embodiments, acrylic resins may be used, such as polymethyl (meth)acrylate, polyethyl (meth)acrylate, polyisopropyl (meth)acrylate, polyisobutyl (meth)acrylate, polybutyl (meth)acrylate, etc. In addition, cellulose-based polymers may be used, such as carboxymethyl cellulose (CMC), carboxyethyl cellulose, starch, regenerated cellulose, ethyl cellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, etc. Furthermore, polycondensation polymers may be used, such as polyurea, polyamide, polyimide, polyester, etc., and one or more of the binders listed above may be used in combination.
[0137] According to an exemplary embodiment, the content of the binder in the slurry can be controlled in the range of, for example, about 1 to 25 weight%, specifically about 3 to 20 weight%, more specifically about 5 to 15 weight%, based on the solid content (the remaining solids excluding the solvent used in the preparation of the slurry, including, for example, the positive active material, the binder, and the conductive material), but is not limited thereto.
[0138] According to exemplary embodiments, the solvent (dispersion medium) for preparing the slurry is not limited to a specific type as long as it can effectively dissolve (or disperse) the aforementioned electrode active material, conductive material, binder, etc. In this regard, the exemplary solvent (dispersion medium) may be an alcohol-based solvent, an ether-based solvent, an amide-based solvent, a ketone-based solvent, an aromatic-based solvent, an ester-based solvent, etc. As an example, in the case of an alcohol-based solvent, methanol, ethanol, 1-propanol, 2-propanol, 2-butanol, t-butanol, ethylene glycol, propylene glycol, 1,6-hexanediol, cyclohexanediol, sorbitol, xylitol, 2-methyl-2,4-pentanediol, 1,3-butanediol, 1,4-butanediol, etc. may be used. Examples of ether-based solvents include alkylene glycol alkyl ethers (e.g., ethylene glycol monomethyl ether, ethylene glycol monobutyl ether, diethylene glycol, dipropylene glycol, propylene glycol monomethyl ether, propylene glycol dimethyl ether, etc.), dimethyl ether, diethyl ether, diisopropyl ether, dibutyl ether, cyclohexylmethyl ether, t-butylmethyl ether, tetrahydrofuran, dioxane, etc. In the case of amide-based solvents, examples include N,N-dimethylformamide, 1-methyl-2-pyrrolidone, 2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, ε-caprolactam, formamide, N-methylformamide, acetamide, N-methylacetamide, N,N-dimethylacetamide, N-methylpropanamide, etc. In addition, as ketone-based solvents, examples such as acetone, methyl ethyl ketone, methyl isobutyl ketone, diisobutyl ketone, etc. may be used. Examples of aromatic-based solvents may include benzene, toluene, xylene, etc. Furthermore, as ester-based solvents, ethyl acetate, propyl acetate, butyl acetate, ethyl formate, etc. may be used. One or more combinations of the solvents (dispersion media) listed above may be used, but the present disclosure is not limited thereto.
[0139] According to exemplary embodiments, the conductive material may be any type known in the art without special limitations, such as graphite types including natural graphite and artificial graphite; carbon black types including acetylene black; amorphous carbon such as needle coke; carbon fiber types such as vapor-grown carbon fiber or carbon nanotubes (CNT); and carbonaceous materials such as graphene and fullerene. Alternatively, metal powders or metal fibers such as copper, nickel, tin, tin oxide, titanium oxide, LaSrCoO3, and LaSrMnO3; and conductive polymers such as polyaniline, polypyrrole, polythiophene, polyacetylene, and polyphenylene derivatives may also be used. One of the types listed above may be used, or two or more may be used in combination.
[0140] According to exemplary embodiments, the content of the conductive material in the slurry can be controlled, based on the solid content, in a range of, for example, about 1 to 30 weight%, specifically about 5 to 25 weight%, more specifically about 8 to 20 weight%, but is not limited thereto.
[0141] According to exemplary embodiments, the step of loading or coating an electrode-forming slurry onto a substrate or a current collector is not limited to a specific method, and any means capable of coating the slurry onto the substrate may be applied. As an example, a doctor blade, slot die coating, etc. may be applied.
[0142] According to an exemplary embodiment, after applying an electrode-forming slurry onto a substrate or a current collector, a drying process may be performed to remove a solvent or the like contained in the slurry layer. At this time, the drying method may be heat drying, vacuum drying, or a combination thereof, and specifically, vacuum drying. As an example, the drying temperature may be controlled in the range of, for example, about 70 to 170 °C, specifically about 80 to 150 °C, and more specifically about 90 to 130 °C. In addition, when adopting a vacuum drying method, the pressure may be controlled in the range of, for example, about 0.2 Torr or less, specifically about 0.1 Torr or less, and more specifically about 0.05 Torr or less, but this may be understood as exemplary. Furthermore, the drying time may be controlled in the range of, for example, about 1 to 24 hours, specifically about 2 to 18 hours, and more specifically about 3 to 12 hours. However, these drying conditions may be understood as exemplary. A layer containing a PBA-based organic composite positive active material is formed on a substrate or current collector through the drying process described above.
[0143] According to exemplary embodiments, the loading amount of the positive active material applied to the electrode substrate or current collector can be controlled in the range of, for example, about 0.5 to 10 mg / cm², specifically about 1 to 8 mg / cm², more specifically about 2 to 6 mg / cm², and particularly specifically about 3 to 5 mg / cm², but is not limited thereto. In addition, the slurry may be coated on one side of the electrode substrate or current collector, and in some cases, may be coated on both sides.
[0144] According to an exemplary embodiment, after the drying process, the electrode (anode) can be cut into a desired shape using methods known in the art, for example, by pressing (e.g., roll pressing), and further by performing a punching step.
[0145] According to exemplary embodiments, the thickness of the positive active material layer within the electrode can be controlled considering rapid ion conductivity and excellent electrolyte penetration, for example, in a range of about 10 to 500 μm, specifically about 30 to 300 μm, and more specifically about 50 to 100 μm. If the thickness of the positive active material layer is less than 10 μm, the mechanical strength is low, and the lifespan characteristics may be reduced due to electrode detachment and structural collapse during repeated charge / discharge processes. On the other hand, if the thickness of the positive active material layer exceeds 500 μm, it is difficult for the electrolyte to completely penetrate into the positive active material layer, which may result in reduced electrochemical performance and reduced capacitance performance by hindering the diffusion of carrier ions. Therefore, it may be advantageous to control the thickness within the aforementioned range, but it is not necessarily limited thereto.
[0147] Production of sodium secondary batteries
[0149] According to another embodiment of the present disclosure, a sodium secondary battery can be manufactured using an electrode structure loaded with a PBA-based organic composite cathode active material as the cathode.
[0150] The basic structure of a sodium secondary battery is known in the art and may include, for example, a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and an electrolyte or an electrolyte layer.
[0151] In the case of the anode, it can typically be applied in the form of a sheet, and such anode sheet may include a cathode current collector and a layer of cathode active material formed on one or both sides thereof. At this time, the cathode current collector may be selected from types that are conductive without causing chemical changes in the sodium-ion secondary battery, such as gold, stainless steel, nickel, aluminum, titanium, copper, or alloys thereof. According to a specific embodiment, the material of the cathode current collector may be aluminum or an aluminum alloy. According to another embodiment, a material such as copper or stainless steel with a surface treated with carbon, nickel, titanium, silver, etc. may be used. Additionally, fine irregularities may be formed on the surface to increase the bonding strength of the cathode active material, and it may be used in various forms such as a film, sheet, foil, foam, or nonwoven fabric.
[0152] According to an exemplary embodiment, the thickness of the negative current collector is not particularly limited, but may be in the range of, for example, about 2 to 50 μm, specifically about 5 to 30 μm, more specifically about 8 to 20 μm.
[0153] According to exemplary embodiments, types known in the art may be applied as negative electrode active materials, such as carbonaceous materials (specifically artificial graphite, natural graphite, soft carbon, hard carbon, etc.), silicon-based materials (specifically silicon oxide, silicon-carbon composite, silicon-nitrogen composite, etc.), tin-based materials (specifically tin oxide, tin alloy, etc.), sodium alloy, etc., and at least one of the listed types may be used. According to specific embodiments, hard carbon may be used as the negative electrode active material, and since hard carbon has a wide interlayer spacing, the insertion and extraction rates of sodium ions are fast, so it can exhibit good charge and discharge characteristics.
[0154] In addition, a cathode structure can be fabricated in a manner similar to the anode structure using the aforementioned PBA-based core-shell organic composite anode active material layer. For example, a cathode active material-containing slurry prepared by introducing a cathode active material, a conductive material, and a binder into a solvent can be loaded or coated onto a substrate or current collector for the cathode, and then a cathode can be formed through subsequent processes such as drying and pressing.
[0155] According to an exemplary embodiment, a separator may be disposed between mutually opposing anodes (anode sheets) and cathodes (cathode sheets), wherein the anodes, cathodes, and separator are in contact with an electrolyte (a medium that transfers sodium ions between the anodes and cathodes), so that sodium ions can pass through the separator and move toward the anode or cathode.
[0156] According to an exemplary embodiment, the material of the separator is not particularly limited, but can be selected from porous materials with good chemical and mechanical stability. It may be a polyolefin-based polymer of a type known in the art, such as ethylene homopolymer, propylene homopolymer, ethylene / butylene copolymer, ethylene / hexene copolymer, ethylene / methacrylate copolymer, etc., and may be in the form of a porous polymer film prepared therefrom. Additionally, the separator may include a nonwoven fabric formed of high-melting-point glass fibers, polyethylene terephthalate fibers, etc. According to another embodiment, the separator may be in the form of a ceramic-coated porous polymer film with high mechanical strength.
[0157] According to an exemplary embodiment, the thickness of the separator can be determined by considering the movement path of sodium ions, for example, in a range of about 3 to 20 μm, specifically about 4 to 18 μm, and more specifically about 5 to 15 μm. In addition, the pore diameter of the separator can be controlled in a range of about 10 to 3000 nm, specifically about 40 to 1000 nm, and more specifically about 60 to 500 nm.
[0158] According to an exemplary embodiment, the anode sheet, cathode sheet, and separator may be manufactured into an electrode assembly through a winding process or a lamination process.
[0159] Meanwhile, the electrolyte serves as a medium for transferring ions between the anode (anode sheet) and the cathode (cathode sheet). In this regard, the electrolyte may be in a liquid, gel, or solid state.
[0160] According to a specific embodiment, an electrolyte solution may be used as the electrolyte, and such an electrolyte solution may contain an electrolyte salt (specifically a sodium salt) and a solvent. For example, the electrolyte salt may be sodium chloride, sodium fluoride, sodium sulfate, sodium carbonate, sodium phosphate, sodium nitrate, sodium difluorooxalate borate, sodium pyrophosphate, sodium dodecylbenzenesulfonate, dodecyl sulfate, sodium citrate, sodium metaborate, sodium borate, sodium molybdate, sodium tungstate, sodium bromide, sodium nitrite, sodium iodide, sodium silicate, sodium lignin sulfonate, sodium hexafluorophosphate, sodium oxalate, sodium aluminate, sodium methylsulfonic acid, sodium acetate, etc., and at least one of these may be selected and used.
[0161] According to an exemplary embodiment, the solvent for preparing the electrolyte is, for example, a carbonate-based solvent (e.g., ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate and fluoroethylene carbonate), an ester-based solvent (e.g., methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, and ethyl butyrate), an ether-based solvent (e.g., dimethyl ether, diethyl ether, dibutyl ether, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, triethylene glycol dimethyl ether, triethylene glycol diethyl ether, 1,3-dioxolane, 4-methyldioxolane, 1,4-dioxane, It may be 3,5-dimethyl isoxazole, 2,5-dimethylfuran, furan, 2-methylfuran, tetrahydrofuran, and 2-methyltetrahydrofuran), and at least one thereof may be used. According to an exemplary embodiment, the concentration of the sodium salt in the electrolyte may be controlled in the range of, for example, about 0.1 to 8 mol / L, specifically about 0.5 to 5 mol / L, more specifically about 0.8 to 3 mol / L.
[0162] As the basic structure of sodium secondary batteries and the like are known in the industry, detailed explanations other than those described above will be omitted.
[0163] According to another embodiment of the present disclosure, a sodium secondary battery manufactured using an electrode based on the aforementioned PBA-based core-shell structured organic composite cathode active material as the cathode, and a battery module or battery pack in which a plurality of such secondary batteries are assembled are provided. The sodium secondary battery, battery module, or battery pack according to the present embodiment can be applied to various mobile devices (e.g., smartphones, tablets, laptops, etc.), electric vehicles (pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), energy storage systems (ESS), etc.
[0164] The present disclosure may be more clearly understood by the following examples, which are merely for illustrative purposes and are not intended to limit the scope of the invention.
[0166] Examples
[0167] The analysis device and analysis conditions are as follows.
[0168] - Morphology and composition of the positive electrode active material: Field Emission Scanning Electron Microscope (FE-SEM)
[0169] - Analysis of the crystal structure of the cathode active material: X-ray diffraction analysis (XRD (Cu Kα, 2θ = 10⁻⁹⁴°), Rietveld refinement)
[0170] - Electrochemical Characterization: Electrochemical Impedance Spectroscopy (EIS)
[0171] - Evaluation of electrochemical cycle characteristics: Charge / discharge tests using constant current / constant voltage charging and constant current discharge methods (CC / CV mode, Galvanostatic charge / discharge test), (Current conditions: range of 0.05 C to 5 C)
[0173] Examples 1: Tetrasodium 2,5- Dihydroxyterephthalate ( Na 4 DHTP ) Organic complex PBA's manufacturing
[0174] (1) Core synthesis
[0175] A saturated solution was prepared by saturating deionized water (DIW) bubbling with N2 gas for at least 30 minutes with NaCl (Sigma-Aldrich), and 0.05 M sodium ferrocyanide (Sigma-Aldrich) was dissolved in it. HCl (SAMCHUN) was added dropwise at a rate of 1.0 mL / min while maintaining the pH at approximately 4.0 or lower, and the reaction was carried out by stirring at 60°C for at least 3 hours. The resulting precipitate was aged for 12 hours, filtered, washed with anhydrous ethanol and DIW, and dried under vacuum at 100°C for 12 hours to obtain Na₂S with an average particle size of 5 µm or less. x Fe y [Fe(CN)6](PBA,0 < x ≤2, 0 < y ≤1) cores were obtained.
[0176] (2) Formation of an organic composite shell layer
[0177] A dispersion was prepared by adding 2,5-dihydroxyterephthalic acid (DHTP; TCI) to anhydrous ethanol, and NaOH (SAMCHUN) was added to adjust the pH to 8.5. The PBA core was added to the dispersion and stirred at room temperature for more than 2 hours to form an organic composite shell layer. After the reaction, the product was filtered, washed with anhydrous ethanol, and dried at 100°C under vacuum for 12 hours to obtain PBA@Na4DHTP powder with a Na4DHTP coating layer formed thereon.
[0179] Comparative example 1: Solo PBA's manufacturing
[0180] A PBA core was manufactured in the same manner as in Example 1 above, but the step of forming an organic composite shell layer was omitted, and uncoated PBA powder (Na x Fe y [Fe(CN)6], 0 < x ≤ 2, 0 < y ≤ 1) was obtained.
[0182] Comparative example 2: Exclusive Tetrasodium 2,5- Dihydroxyterephthalate (Na₂O₃) 4 of DHTP manufacturing
[0183] The same organic precursor (DHTP) as in Example 1 was used, but without preparing a PBA core, and the reaction was carried out with the organic material alone to obtain tetrasodium 2,5-dihydroxyterephthalate (Na4DHTP) powder.
[0185] Battery Manufacturing and Performance Evaluation
[0186] - Battery manufacturing
[0187] A sodium-ion secondary battery was manufactured using the PBA-based organic composite electrode active material prepared in Example 1 above and the organic electrode active materials prepared in Comparative Examples 1 and 2, respectively.
[0188] First, a slurry was prepared by mixing a conductive material (Super P; Imerys Graphite & Carbon) and a binder (PVDF; MTI Korea) with each active material in a weight ratio of 80:10:10. The slurry was uniformly applied onto a 16 μm thick aluminum film and then dried under vacuum conditions at 100°C or higher for at least 4 hours. Subsequently, the dried electrode sheet was compressed to high density through a roll pressing process and then cut to a specified size to manufacture an anode electrode.
[0189] Sodium (Na) metal foil was used as the negative electrode, and a porous polypropylene film (Celgard) was applied as the separator. The battery was assembled in an argon (Ar) charging glove box in which moisture and oxygen concentrations were each maintained at 1 ppm or less. The assembly method involved interposing the separator between the positive and negative electrodes and injecting the electrolyte.
[0190] The electrolyte contained sodium hexafluorophosphate or sodium perchlorate as the electrolyte salt, and the solvent system contained carbonate-based solvents such as ethylene carbonate (EC) and dimethyl carbonate (DMC). The assembled cell was fabricated with a CR2032 coin-type structure.
[0192] - X-ray diffraction analysis ( XRD ) result
[0193] XRD was performed to analyze the crystal structure of the cathode active material prepared in Example 1 and Comparative Examples 1 and 2, respectively, and the results are shown in FIGS. 3a to 3c.
[0194] As shown in Figures 3a and 3b, the main diffraction peaks representing the crystal structure of PBA were clearly observed in the XRD patterns of the samples prepared in Example 1 and Comparative Example 1. This suggests that the intrinsic lattice structure of PBA is maintained regardless of whether an organic composite shell layer is formed.
[0195] Meanwhile, referring to FIGS. 3a and 3b, a faint additional peak was observed in Example 1 at approximately 2θ 20˚ compared to Comparative Example 1. This is attributed to the organic composite shell layer, such as tetrasodium 2,5-dihydroxyterephthalate (Na4DHTP).
[0196] While the positions of the main PBA diffraction peaks were maintained, some peaks showed positional shifts or peak width expansions, which is interpreted as reflecting fine lattice distortion and surface changes within the crystal system caused by the organic composite shell layer.
[0197] In addition, the organic composite shell layer does not form an independent crystalline phase but exists thinly on the surface of the PBA crystal, so rather than forming a new diffraction peak, it appears as a decrease in intensity or a change in the existing peak. This suggests that the composite process of the present disclosure forms an organic layer while maintaining the crystallinity and structural stability of the PBA.
[0198] On the other hand, as shown in Fig. 3c, in the case of the organic sample prepared in Comparative Example 2, no diffraction peaks characteristic of PBA were observed on the XRD pattern, which clearly shows that the sample does not contain a PBA structure.
[0199] From the above results, it was confirmed that the PBA-based organic composite cathode active material of the present disclosure successfully introduced an organic shell layer without damaging the PBA crystal structure, and that this can contribute to improving the structural regularity and interfacial stability of the electrode active material.
[0201] - FE- SEM Analysis results
[0202] To observe the surface morphology and particle structure of the electrode active materials prepared in Example 1 and Comparative Examples 1 and 2, analysis was performed using a scanning electron microscope (FE-SEM; TESCAN S8000), and the observation results are shown in Figures 4a to 4c, respectively.
[0203] As shown in Fig. 4b, the uncoated PBA of Comparative Example 1 had smooth and distinct grain boundaries and exhibited a cubic crystal structure. This suggests that the inherent crystallinity of the PBA is maintained.
[0204] On the other hand, as shown in Fig. 4a, the surface of the PBA-based organic composite cathode active material of Example 1 is coated with tetrasodium 2,5-dihydroxyterephthalate, and as a result, the particle surface exhibits a relatively coarse and non-uniform composite layer shape. This indicates that the organic shell layer is uniformly formed on the surface of the core particle.
[0205] Meanwhile, as shown in Fig. 4c, Comparative Example 2 was composed solely of organic material, so it had low crystallinity and an irregular shape, and appeared in an amorphous form in which no distinct crystal shape was observed.
[0206] Through the above FE-SEM analysis results, it is proven that the PBA-based organic composite cathode active material of the present disclosure maintains the crystal structure of PBA while having an organic shell layer formed on the core surface, functioning as a physical / chemical protective layer, and confirms morphological characteristics that are clearly distinguishable from organic particles alone.
[0208] - Cycle life and capacity retention rate evaluation
[0209] After forming a positive electrode using the electrode active materials prepared in Example 1 and Comparative Examples 1 and 2, respectively, a coin-type sodium-ion secondary battery with sodium metal as the negative electrode was assembled. For each battery, a cycle test was performed 200 times under conditions of 25°C, repeating charging at 0.1 C (constant current / constant voltage CC / CV method, upper voltage limit: 4.0 V) and discharging at 0.1 C (constant current CC method, lower voltage limit: 2.0 V). The initial discharge capacity and the discharge capacity after 200 cycles were measured, and the capacity retention rate (%) was calculated from this. The results are shown in Table 1 below.
[0211] division Examples 1 Comparative example 1 Comparative example 2 Initial discharge capacity (mAh / g) 120 110 126 200 cycle capacity (mAh / g) 111.6 96.8 94.5 Dose retention rate (%) 93 88 75
[0213] According to Table 1 above, Example 1 showed a relatively high initial discharge capacity of 120 mAh / g, while maintaining a capacity of 111.6 mAh / g after 200 cycles, demonstrating a capacity retention rate of 93%. This indicates superior cycle life characteristics compared to Comparative Examples 1 and 2.
[0214] In particular, Comparative Example 2 showed the highest initial discharge capacity, but the capacity retention rate dropped sharply to 75% after 200 cycles. This suggests that the structural and electrochemical stability as an electrode active material is insufficient when using the organic material (Na4DHTP) alone.
[0215] On the other hand, when the same organic material series is coated on the surface of the PBA (Example 1), the organic material acts as a functional interface stabilization layer rather than an electrode active material, thereby improving the interface stability between the electrolyte and the PBA, and Na + It is determined that it provides electron transfer pathways and structural stress buffering functions. Therefore, it has been confirmed that the organic composite PBA cathode active material of the present disclosure has a significant effect in terms of electrode-electrolyte interface stability and long-term cycle life compared to a single organic material or an uncoated PBA.
[0217] - Electrochemical Impedance Spectroscopic (EIS) Analysis
[0218] To confirm the effect of the organic composite shell layer of the present disclosure on the characteristics at the electrode-electrolyte interface, electrochemical impedance spectroscopy (EIS) analysis was performed. EIS measurements were performed by assembling symmetrical coin cells using the electrodes prepared in Example 1 and Comparative Examples 1 and 2, respectively, as the anode and cathode, and the frequency range was set to 7 mHz to 100 kHz. EIS measurements were conducted on the symmetrical coin cells with the electrodes prepared in Example 1 and Comparative Examples 1 and 2, divided into immediately after assembly and after 200 cycles. Subsequently, the charge transfer resistance (Rct) was compared through Nyquist plot analysis, and long-term stability was evaluated. The results are shown in Table 2 below.
[0220] division Examples 1 Comparative example 1 Comparative example 2 Initial interface resistance (Ω) 35 42 55 Interface resistance (Ω) after 200 cycles 48 67 95
[0222] According to Table 2 above, the electrode of Example 1 showed an initial interfacial resistance of 35 Ω, which increased to 48 Ω after 200 cycles, an increase of only 13 Ω. On the other hand, Comparative Example 1 increased from 42 Ω to 67 Ω, a rise of 25 Ω, and Comparative Example 2 showed a large increase of 40 Ω, from 55 Ω to 95 Ω.
[0223] These results indicate that the organic composite shell layer of the present disclosure substantially improves electrochemical stability at the interface during battery operation. By acting as a functional shell layer within an interface composite structure with PBA rather than as a single electrode active material, it induces stabilization of the electrode / electrolyte interface and facilitates the transfer of sodium ions and electrons, thereby suppressing the increase in interfacial resistance even during long-term operation.
[0224] Accordingly, it was confirmed that the organic composite shell layer of the present disclosure functions as a more effective interface stabilization layer when combined with a Prussian blue analogue than when used alone, and that this can contribute to improving battery performance during long-term cycle operation.
[0226] According to the foregoing, the organic composite shell according to the present disclosure can simultaneously improve the stability and performance of the electrode by exhibiting various electrochemical synergistic effects, going beyond the function of merely coating the surface. For example, by blocking direct contact between the electrolyte and the PBA interface, the organic composite shell can suppress oxidation of the PBA surface and metal ion leaching by the electrolyte, and induce interface stabilization even during long-term cycling. Furthermore, an organic composite shell containing ionic functional groups having sodium ion conductivity [regarding] Na at the electrode / electrolyte interface + It can contribute to reducing initial interfacial resistance and enhancing electrochemical reaction rates by assisting electron transfer pathways. Furthermore, the organic composite shell provides structural stability by absorbing and buffering electrode structural changes (e.g., volume expansion, particle detachment) that occur during repeated charge and discharge cycles, thereby contributing to the extension of the electrode's physical lifespan. Finally, the organic composite shell can improve the electrode's corrosion resistance and long-term stability by passivating micro-defects or active sites on the PBA surface (e.g., reaction sites exposed by the elution of transition metal ions, localized oxidation regions, etc.), thereby suppressing unnecessary interfacial reactions with the electrolyte and reducing electrochemical degradation.
[0227] As confirmed in the above experimental example, the synergistic effect is realized in the electrode of Example 1 with the coating layer introduced, with an excellent capacity retention rate and a low increase rate in interfacial resistance, demonstrating a significant improvement in performance compared to a single PBA electrode or an organic single electrode.
[0228] All simple variations or modifications to the foregoing content of the present disclosure fall within the scope of the present disclosure, and the specific scope of protection of the present disclosure will be clarified by the appended claims. Explanation of the symbols
[0229] 100: Organic composite cathode active material having a PBA-based core-shell structure 110: Core 120: Shell
Claims
Claim 1 An organic composite cathode active material having a core-shell structure based on a Prussian blue analog (PBA), comprising: a core containing PBA; and a shell formed from a low-molecular-weight or high-molecular-weight organic composition bonded to the surface of the core via coordination bonding or hydrogen bonding, and comprising an ionic functional group containing sodium ions or having sodium ion conductivity. Claim 2 In claim 1, the Prussian blue analog is a positive active material represented by the following chemical formula 1: [Chemical Formula 1]A x M[M'(CN)6] 1- y (Vac) y ·nH2O In the above chemical formula 1, A is a group 1 element, M and M' are at least one selected from the group consisting of Mg, Ca, Al, Ga, In, Sn, Pb, Sc, Ti, V, Cr, Fe, Co, Ni, Mn, Cu, Zn, Pd, Ag, Cd or combinations thereof, Vac is a vacancy of M'(CN)6, 0 < x ≤ 2, 0 ≤ y ≤ 1, and 0 ≤ n ≤ 6. Claim 3 In claim 1, the organic composition comprises a positive active material including at least one selected from p-type, n-type, or positive organic material. Claim 4 In claim 3, the p-type organic material is an aromatic polycarboxylic acid derivative comprising at least one selected from the group consisting of terephthalic acid, 2,5-dihydroxyterephthalic acid, trimesic acid, pyromellitic acid, melitic acid, 4,4'-biphenyldicarboxylic acid, 2,6-naphthalenedicarboxylic acid, and 4,4'-dithiobisbenzoic acid. Claim 5 In claim 3, the n-type organic material is a quinone-based or rhodizonate-based compound, comprising at least one selected from the group consisting of 1,4,5,8-tetraaminoanthraquinone, anthraquinone, 1,4-naphthoquinone, disodium rhodizonate, dipotassium rhodizonate, and dilithium rhodizonate, forming an anode active material. Claim 6 The positive electrode active material according to claim 1, wherein the organic composition comprises at least one selected from the group consisting of tetrasodium 2,5-dihydroxylephthalate (Na4DHTP), disodium 1,4,5,8-tetraaminoanthraquinone (Na2TAAQ), or a mixture thereof. Claim 7 In claim 1, the shell is a positive active material further comprising an organic compound containing an ionic functional group. Claim 8 In claim 1, the core has an average particle size (D) controlled in the range of 0.1 to 10 μm. 50 A positive electrode active material having ). Claim 9 A positive active material according to claim 1, wherein the charge transfer resistance (Rct) of the electrode composed of the positive active material is 10 to 300 Ω. Claim 10 A positive active material according to claim 1, wherein the thickness of the shell is 0.01 to 5 μm. Claim 11 A positive active material according to claim 1, wherein the thickness ratio of the core to the shell is controlled within the range of 1:0.02 to 0.
8. Claim 12 In claim 1, the positive electrode active material has an average particle size (D) controlled in the range of 0.1 to 10 μm. 50 A positive electrode active material having ). Claim 13 A method for manufacturing an organic composite cathode active material having a core-shell structure based on a Prussian blue analog (PBA) according to any one of claims 1 to 12, comprising: a step of forming a core comprising a Prussian blue analog (PBA) represented by the following chemical formula 1; a step of preparing a dispersion by dispersing a low molecular weight or high molecular weight organic composition in a solvent; a step of neutralizing the pH to 6 to 10 by adding a basic compound to the dispersion; and a step of adding the core to the dispersion to form an organic composite shell layer on the surface of the core; a method for manufacturing a cathode active material comprising: [Chemical Formula 1]A x M[M'(CN)6] 1- y (Vac) y ·nH2O In the above chemical formula 1, A is a group 1 element, M and M' are at least one selected from Mg, Ca, Al, Ga, In, Sn, Pb, Sc, Ti, V, Cr, Fe, Co, Ni, Mn, Cu, Zn, Pd, Ag, Cd or a combination thereof, Vac is a vacancy of M'(CN)6, 0 < x ≤ 2, 0 ≤ y ≤ 1, and 0 ≤ n ≤ 6. Claim 14 A method for manufacturing an anode active material according to claim 13, wherein the solvent is selected from an aqueous solvent, a non-aqueous (anhydrous) solvent, or a mixture thereof, the aqueous solvent is selected from the group consisting of deionized water (DIW), distilled water, ultrapure water, or a combination thereof, and the non-aqueous solvent is selected from the group consisting of anhydrous ethanol, anhydrous acetonitrile, anhydrous methanol, anhydrous tetrahydrofuran, anhydrous acetone, anhydrous propylene carbonate, dimethyl sulfoxide (DMSO), dimethylformamide (DMF), or a combination thereof. Claim 15 A method for manufacturing a positive active material according to claim 13, wherein the basic compound is at least one selected from the group consisting of sodium hydroxide (NaOH), sodium carbonate (Na2CO3), sodium methoxide (NaOCH3), sodium tert-butoxide (NaOC(CH3)3) or derivatives thereof. Claim 16 A method for manufacturing an anode active material according to claim 13, wherein the reaction forming the organic composite shell layer is performed at 20 to 80 ℃. Claim 17 A method for manufacturing an anode active material according to claim 13, further comprising the step of drying at a temperature of 50 to 200 ℃ and a pressure of 0.2 Torr or less after forming the shell layer. Claim 18 A sodium secondary battery comprising: a positive electrode comprising a positive active material according to any one of claims 1 to 12; a negative electrode disposed opposite to the positive electrode; a separator disposed between the positive electrode and the negative electrode; and an electrolyte in contact with the positive electrode and the negative electrode.