Plant and method for manufacturing half cells for solid fuel cells

The continuous manufacturing process for SOC half-cells using calendering and slot die deposition addresses inefficiencies in tape casting, reducing waste and costs while enhancing production speed and defect resistance.

KR1020260163979APending Publication Date: 2026-11-17하이드로스파크 에스알엘
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
KR1020267028608
Authority / Receiving Office
KR · KR
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-03-19
Filing Date
2025-03-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The manufacturing of solid oxide fuel cells (SOC) is hindered by high costs, material waste, and susceptibility to defects due to tape casting processes, which are sensitive to external variables and require controlled environments, leading to inefficiencies and increased production time.

Method used

A method and plant for manufacturing half-cells using a continuous process that involves calendering and slot die deposition, eliminating tape casting, allowing for the use of different binders and additives, and enabling interruption without slip loss, with a scalable and cost-effective production of half-cells.

Benefits of technology

The method achieves reduced waste, lower costs, increased manufacturing speed, and improved defect resistance, enabling the production of half-cells with enhanced efficiency and flexibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCT00001_ABST
    Figure PCT00001_ABST
Patent Text Reader

Abstract

A method (100) for manufacturing a half cell (1) for a solid fuel cell, particularly a half cell (1) formed by a double ceramic layer consisting of electrodes (4) and an electrolyte (5) joined together, comprises: a process (200) for manufacturing a green electrode body (2); a process (300) for manufacturing a green electrolyte body (3); a joining step (400) in which the green electrode body (2) and the green electrolyte body (3) are joined together; and a sintering step (500) after the joining step (400), wherein the green electrode body (2) and the green electrolyte body (3) joined together are sintered to manufacture the half cell (1) formed by the joined electrodes (4) and the electrolyte (5).
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a plant and a method for continuously manufacturing a half-cell for a solid-state fuel cell, also known as a solid oxide cell (SOC), in particular an electrode and an electrolyte forming a double ceramic layer. Background Technology

[0002] Among the many challenges facing humanity in the 21st century, the issue of sustainable energy supply is emerging as an undeniable top priority. The growth of the global population and the consequent increase in energy consumption are further intensifying this challenge. The energy revolution has already begun. We are witnessing a gradual transition from the unconditional use of fossil fuels to an era where renewable resources are steadily increasing their market share, thereby fundamentally changing existing paradigms. Therefore, it is necessary to find pollution-free technological solutions that can be integrated into new energy systems based on the use of effective energy carriers generated and utilized within a closed cycle of carbon dioxide emission and reuse.

[0003] A solid fuel cell is an electrochemical device capable of converting chemical energy into electricity and heat, or reversibly storing excess electrical energy and heat to produce chemical fuel.

[0004] SOC generates high-efficiency energy by utilizing electricity from renewable sources and produces clean chemicals such as eco-friendly hydrogen, ammonia, or synthesis gas. Hydrogen can be used as fuel for hydrogen vehicles or steel manufacturing, ammonia for fertilizer production, and synthesis gas for energy generation.

[0005] Furthermore, since the chemical reaction to generate synthesis gas utilizes CO2, it contributes to the absorption of carbon dioxide. Alternatively, electricity is obtained as a result by supplying methane or hydrogen to the battery. When hydrogen is used as fuel, the only byproduct is water, and when methane is used, carbon dioxide is produced, but NO X and SO X The formation of is prevented.

[0006] This technology possesses several positive features, including reversibility, high efficiency, low cost, and fuel flexibility. Additionally, the SOC is manufactured from widely available ceramic oxide materials such as zirconium oxide and nickel oxide.

[0007] Nevertheless, SOC still has several serious problems that hinder its widespread adoption. In particular, manufacturing costs are one of the major obstacles that must be overcome.

[0008] The half-cell of the SOC is formed by electrodes and an electrolyte, and the electrodes represent one of the largest factors in cell cost. In fact, in terms of thickness, this accounts for more than 90% of the total thickness. The electrodes have a thickness of 100 to 500 μm before sintering. The electrolyte has a thickness of 3 to 20 μm before sintering.

[0009] In the prior art, both layers can be manufactured individually by tape casting and then rolled, or by co-casting of the electrolyte after electrode tape casting, or by screen printing of the electrolyte after electrode tape casting.

[0010] The use of tape casting technology requires the preparation of a suspension having a viscosity of 100 to 900 cps, which requires a preparation time of 5 to 48 hours depending on whether a continuous or static flow mill is used. The powder is mixed with a binder and additives. Subsequently, they are ground for several hours to achieve homogenization of the suspension. Some preparations also involve the subsequent addition of binders and additives after the grinding process. The suspension must also be filtered and degassed.

[0011] The tape casting technique includes the step of drawing a suspension from a pressure vessel and pouring it into a tank, also referred to as a Dr. Blade, which is configured to allow an appropriate amount of suspension to pass under the blade and ultimately deposit the suspension onto a sliding support. Subsequently, the layer thus cast is applied to a drying step. For solid oxide batteries, the typical speed of this process is 0.2 to 2 meters per minute, depending on the length of the tape casting and the thickness of the layer to be cast. For the same length of tape casting, the thickness significantly affects the process speed. The thicker the layer being cast, the slower the casting speed.

[0012] The tape casting process is a casting process that cannot be interrupted as required. In fact, if the process were to be interrupted, a portion of the suspension already present inside the calm Dr. Blade tank, the suspension already present inside the tube connecting the suspension container, and a portion of the already cast suspension would be lost.

[0013] Furthermore, tape casting technology remains highly sensitive to external variables such as changes in input materials (e.g., viscosity and dispersion quality), ambient temperature, humidity, the quality of the plastic support used for casting, and its non-stick coating.

[0014] The addition of the second layer, the electrolyte, may occur by another deposition using tape casting on a layer that has already been previously cast and dried, or by joining two individually cast layers by rolling after depositing a new layer at once. In the prior art relating to the first case, a thin layer is cast first, and a thicker layer is cast on top of it. Simultaneous casting may occur continuously or in batches.

[0015] In the case of simultaneous casting, special attention is required in the selection of binders and additives used to create the suspension to be cast. In practice, for both the first and second layers, adhesives of the same family must be used to ensure that defects such as delamination, cracking, bubbles, surface roughness, and various deformations do not occur during the step of drying the second layer over the first layer. Given the significant thickness difference between the two layers forming the ceramic half-cell, it may be appropriate to use different types of binders and additives to shorten the drying time of the layers while maintaining their porosity, and to obtain a thin green layer that already has a high density, i.e., a pre-sintering layer.

[0016] Tape casting is very susceptible to defect formation due to contamination of the suspension before and during casting. Therefore, it is required to operate in a controlled environment where it is essential to maintain strict standards of air cleanliness and purity, having at least an ISO Grade 5 cleanliness level.

[0017] The manufacturing waste of half-cells by traditional methods is 10 to 30%, a figure that accounts for material loss occurring during all manufacturing stages, from suspension generation to green cell generation by tape casting, as well as cutting waste required to obtain cells of the desired dimensions. Tape casting machines also incur very high costs.

[0018] Therefore, there is a need for an improved plant and method for manufacturing half-cells for solid fuel cells compared to the prior art. The problem to be solved

[0019] The object of the present invention is to provide a plant and a method for manufacturing half cells for solid fuel cells, which enables the continuous manufacturing of half cells for solid fuel cells.

[0020] A further specific object of the present invention is to provide a plant and a method for manufacturing half cells for solid fuel cells that are scalable, cost-effective, and continuous.

[0021] A further specific object of the present invention is to provide a plant and a method for manufacturing half cells for solid fuel cells, which allow for the reduction or elimination of waste or scrap of slip used in the manufacture of half cells, and in particular allow for the interruption of the manufacturing process that does not generate slip loss or waste.

[0022] A further specific object of the present invention is to provide a plant and a method for manufacturing half cells for solid fuel cells, which allow for the use of any series of binders and additives that do not necessarily have to be part of the same series, regardless of whether they are used in the manufacture of thin-layer slips and / or suspensions, and have a low probability of defects occurring due to contamination.

[0023] A further specific objective of the present invention is to provide a plant and a method for manufacturing a half cell for a solid fuel cell that allows for an increase in the manufacturing speed of the half cell.

[0024] A further specific objective of the present invention is to provide a plant and a method for manufacturing a half cell for a solid fuel cell, which reduces the total time and cost of manufacturing the half cell. means of solving the problem

[0025] These and other objectives are achieved by a plant and method for manufacturing a half cell for a solid fuel cell according to an independent claim.

[0026] Dependent claims relate to preferred and advantageous embodiments of the present invention. Brief explanation of the drawing

[0027] To better understand the invention and to recognize the advantages of the invention, some non-limiting exemplary embodiments of the invention will be described below with reference to the accompanying drawings, in which: - FIG. 1 is a schematic diagram of a plant for manufacturing a half-cell for a solid fuel cell according to one embodiment of the present invention; - FIG. 2 is a schematic diagram of a plant for manufacturing a half-cell for a solid fuel cell according to an additional embodiment of the present invention; - FIG. 3 shows a microscopic image representing a porous layer of a green electrode body manufactured by a plant and method for manufacturing a half-cell for a solid fuel cell according to one embodiment of the present invention; - FIG. 4 is a micrograph showing a layer of a thin green electrolyte body manufactured by a plant and method for manufacturing a half-cell for a solid fuel cell according to one embodiment of the present invention. Specific details for implementing the invention

[0028] Description of some preferred embodiments

[0029] Method (100)

[0030] A method (100) for manufacturing a half cell (1) for a solid fuel cell, in particular a half cell (1) formed by a double ceramic layer comprising a coupled electrode (4) and an electrolyte (5), comprises the following steps:

[0031] - A process (200) for manufacturing a green electrode body (2), and

[0032] - Process (300) for manufacturing the green electrolyte body (3).

[0033] The process (200) for manufacturing the green electrode body (2) is performed before, after, or simultaneously with the process (300) for manufacturing the green electrolyte body (3).

[0034] The above method (100) further includes the following steps:

[0035] - A bonding step (400) in which the green electrode body (2) and the green electrolyte body (3) are combined together,

[0036] - A step of sintering (500) after a bonding step (400) by sintering the green electrode body (2) and the green electrolyte body (3) bonded together to produce the half cell (1) formed by the bonded electrode (4) and electrolyte (5).

[0037] Specifically, in the sintering step (500), the green electrode body (2) is sintered to form an electrode (4), and the green electrolyte body (3) is sintered to form an electrolyte (5).

[0038] The process (200) for manufacturing the green electrode body (2) includes the following manufacturing steps:

[0039] - Step (210) of preparing a viscous ceramic composition also referred to as slip (20);

[0040] - A step (220) of mixing the above slip (20) to form a slurry (21);

[0041] - Step (230) of extruding the above slurry (21) to form an extruded slurry (22);

[0042] - A step (240) of calendering the extruded slurry (22) to form a green electrode body (2).

[0043] The process (300) for manufacturing the green electrolyte body (3) includes the following manufacturing steps:

[0044] - Step (310) of preparing an electrolyte suspension (30);

[0045] - Step (320) of depositing the electrolyte suspension (30) by means of a slot die, preferably a curtain slot die, to form a film of the green electrolyte body (3);

[0046] - Optionally, a drying step (330) for heating, in particular drying, the film of the green electrolyte body (3).

[0047] The method (100) configured in this way to manufacture a half cell for a solid fuel cell allows for the continuous manufacturing of half cells, is scalable, and has a lower cost compared to the prior art.

[0048] As an additional advantage, the method (100) configured in this way includes or does not require a tape casting step, thereby allowing for the reduction or elimination of slip loss and waste, and also allows for the interruption of the manufacturing process that does not cause slip loss or waste.

[0049] As an additional advantage, the method (100) configured in this way allows for an increased manufacturing speed of the half-cell, which allows for a layer having a width of 100 mm to 3000 mm and to be manufactured at a speed of 5 to 10 m / min.

[0050] As an additional advantage, the method (100) configured in this way allows calendering a layer of 100 μm to 500 μm, i.e., an electrode, by a single calendering or a series of calendering rollers.

[0051] According to one embodiment, the slip (20) is manufactured in step (210) by the following components, preferably only by the following components:

[0052] - Nickel oxide (NiO);

[0053] - Zirconium oxide (YSZ);

[0054] - Pore-forming agent;

[0055] - binder; and

[0056] - Plasticizer.

[0057] The above elements are combined to form a slip (20).

[0058] According to one embodiment, the components of the slip (20) have the following weight percentages:

[0059] - Nickel oxide (NiO): 20 to 40%;

[0060] - Zirconium oxide (YSZ): 20 to 40%;

[0061] - Pore-forming agent: 1 to 15%;

[0062] - Binder: 30 to 50%; and

[0063] - Plasticizer: 1 to 15%.

[0064] According to one embodiment, nickel oxide and zirconium oxide are in powder form.

[0065] According to one embodiment, both the nickel oxide powder and the zirconium oxide powder have a particle size distribution (PSD) of less than 0.5 μm.

[0066] According to one embodiment, both the binder and the plasticizer are composed of polyacrylate, but may also include ethylene copolymer, maleic acid copolymer, styrene copolymer, acrylate or methacrylate copolymer, vinyl acetate copolymer, polyvinyl butyral resin, vinyl acetal resin, vinyl resin, vinyl alcohol resin, wax, and cellulose such as ethyl cellulose. These binders may be used alone or in combination with each other.

[0067] According to one embodiment, the binder is a binder based on a partially water-soluble acrylic polymer, and the binder has a solid content loading amount of 30% to 40%.

[0068] According to one embodiment, the binder is an acrylic binder, and / or vinyl, and / or water-based or solvent-based cellulose. According to one embodiment, the water-based binder may be formed of a polymer that is partially or completely water-soluble or a polymer emulsion.

[0069] According to one embodiment, the plasticizer is a plasticizer composed of 100% amine-containing polymer.

[0070] According to one embodiment, the pore-forming agent is one of starch, cellulose, acrylic polymer, carbon black, or a combination thereof.

[0071] According to one embodiment, the step (220) of mixing the slip (20) includes the step of mixing the components by a wet mixer (62) to form a slurry (21).

[0072] According to one embodiment, the components forming the slip (20) are mixed in a wet mixer (62) for a period of 10 to 30 minutes, preferably 15 to 25 minutes, preferably about 20 minutes.

[0073] According to one embodiment, when mixing, the step (220) of mixing the slip (20) may include the step of degassing the slurry (21) to form a degassing slurry (21).

[0074] Advantageously, the production of the slip (20) and slurry (21) configured in this way does not require ball milling. Therefore, the method allows for the prevention of material loss and has a shortened time compared to the prior art.

[0075] According to one embodiment, after degassing, a step (230) of extruding the slurry (21) to produce the extruded slurry (22) is performed.

[0076] According to one embodiment, the extruded slurry (22) has a thickness of less than 2 mm.

[0077] The calendering step (240) is performed after the extrusion step (230) of the extruded slurry (22).

[0078] According to one embodiment, a calendering step (240) is performed to manufacture a green electrode body (2) with a thickness of 50 μm to 10,000 μm, preferably about 350 μm ± 10 μm or less.

[0079] According to one embodiment, a calendering step (240) is performed to manufacture a green electrode body (2) with a thickness of about 100 μm ± 10 μm.

[0080] According to one embodiment, a calendering step (240) is performed by at least one pair of rollers (80) facing each other with respect to the extruded slurry (22) to be extruded, thereby forming a green electrode body (2).

[0081] According to one embodiment, the calendaring step (240) is performed by a pair of rollers (80).

[0082] Advantageously, this configuration allows not only to shorten the manufacturing time of the half cell (1) but also to reduce the overall dimensions of the manufacturing plant (1000) of the half cell (1).

[0083] According to one embodiment, during the calendering step (240), at least one roller (80) of at least one pair of rollers (80), preferably each roller of at least one pair of rollers (80), is heated.

[0084] According to one embodiment, one or more rollers (80) are heated to a temperature of 40°C to 50°C.

[0085] According to one embodiment, during the calendering step (240), the roller (80) rotates at a tangential speed of 5 m / min to 10 m / min or at a speed of about 5 m / min. Accordingly, the extruded slurry (22) applied to the calendering to form the green electrode body (2) advances between at least one pair of opposing rollers (80) at a speed of 5 m / min to 10 m / min, preferably about 5 m / min.

[0086] As an additional advantage, the green electrode body (2) formed in this way does not require a drying step, unlike that required in the prior art.

[0087] First embodiment of the combination step (400)

[0088] One implementation example ( Fig. 1 According to ), the drying step (330) is performed after the bonding step (400) between the film of the green electrolyte body (3) and the green electrode body (2).

[0089] According to the present embodiment, the step (320) of depositing the electrolyte suspension (30) by the slot die includes the step of directly depositing the electrolyte suspension (30) onto the electrode body (2) drawn.

[0090] Accordingly, a film of the green electrolyte body (3) is continuously deposited on the green electrode body (2) manufactured after the calendering step (240) by the slot die. By this, the bonding step (400) occurs.

[0091] According to the present embodiment, after the bonding step (400) between the green electrolyte body (3) deposited on the green electrode body (2) by a slot die and the green electrode body (2), a drying step (330) of the green electrolyte body (3) is performed. By doing so, the green electrolyte body (3) is dried.

[0092] Second embodiment of the combination step (400)

[0093] One implementation example ( Fig. 2 According to ), the drying step (330) is performed before the bonding step (400) between the green electrolyte body (3) and the green electrode body (2).

[0094] According to the present embodiment, the step (320) of depositing an electrolyte suspension (30) by a slot die, preferably a curtain slot die, includes the step of depositing the electrolyte suspension (30) on a sliding support (32), preferably a flat polymer support.

[0095] Accordingly, by means of a slot die, a film of the green electrolyte body (3) is continuously deposited on the sliding support (32).

[0096] According to the present embodiment, after depositing a film of the electrolyte body (3) on a sliding support (32) by means of a slot die, a drying step (330) of the electrolyte body (3) is performed.

[0097] This drying step (330) is performed before the bonding step (400) between the green electrolyte body (3) and the green electrode body (2).

[0098] According to the present embodiment, the coupling step (400) between the green electrolyte body (3) and the green electrode body (2) provides that both the green electrolyte body (3) and the green electrode body (2) are transported in the direction of a rolling station (5000).

[0099] The rolling station (5000) includes at least one pair of opposing rolling rollers.

[0100] The green electrolyte body (3) and the green electrode body (2) being transported toward the rolling station (5000) are stacked, that is, positioned facing each other.

[0101] The connection between the green electrode body (2) and the green electrolyte body (3) is performed by the rolling roll of the rolling station (5000).

[0102] Plant (1000)

[0103] According to a further aspect of the present invention, a plant (1000) for manufacturing a half cell (1) for a solid fuel cell, in particular a half cell (1) formed by a double ceramic layer comprising an electrode (4) and an electrolyte (5) combined together, comprises the following:

[0104] - Electrode station (2000) where the manufacture of the green electrode body (2) is performed,

[0105] - Electrolyte station (3000) where the manufacture of the green electrolyte body (3) is performed.

[0106] - A coupling station (4000) where the coupling between the green electrode body (2) and the green electrolyte body (3) is performed,

[0107] - A sintering station (5000) that sinters the green electrode body (2) and the green electrolyte body (3) combined together to produce the half cell (1) formed by the combined electrode (4) and electrolyte (5).

[0108] The electrode station (2000) includes a slip station (7000) for manufacturing, mixing, and extruding the slip (20) to produce an extruded slurry (22).

[0109] The electrode station (2000) further includes a calendering station (8000). The calendering station (8000) is configured to calender the slip (20), and in particular, to calender the extruded slurry (22) to form a green electrode body (2).

[0110] The electrolyte station (3000) includes a casting station (6000) for manufacturing an electrolyte suspension (30) and depositing the electrolyte suspension (30) by a slot die, preferably a curtain slot die, to produce a film of a green electrolyte body (3).

[0111] Optionally, the electrolyte station (3000) further includes a drying station (9000) for drying the film of the green electrolyte body (3).

[0112] Advantageously, the plant (1000) configured in this way allows for continuous manufacturing, is scalable, and has a lower cost compared to the prior art.

[0113] As an additional advantage, the method (100) configured in this way does not include or require a tape casting step, thereby allowing for the reduction or elimination of slip loss and waste.

[0114] As an additional advantage, the method (100) configured in this way allows for an increased manufacturing speed of the half cell, because it allows for manufacturing the half cell at a speed of 5 to 10 m / min with a layer having a width of 100 mm to 3000 mm.

[0115] As an additional advantage, the method (100) configured in this way allows calendering a layer, i.e., an electrode, of 100 μm to 10,000 μm, preferably about 350 μm ± 10 μm or less, by a single calendering or a series of calendering rollers.

[0116] According to one embodiment, the slip station (7000) includes a wet mixer (62).

[0117] The components forming the slip (20) can be mixed by a wet mixer (62).

[0118] According to one embodiment, the slip station (7000) includes a hopper (61) fluidly connected to a wet mixer (62).

[0119] The components forming the slip (20) can be loaded into the hopper (61) and mixed by a wet mixer (62).

[0120] According to one embodiment, the slip station (7000) includes an extruder (63) configured to extrude the extruded slurry (22).

[0121] The extruder (63) is fluidically connected to the wet mixer (62) to extrude the extruded slurry (22) produced from the mixing of the slip (20) in the wet mixer (62).

[0122] According to one embodiment, the slip station (7000) includes a degasser configured to degas the slip (20) to form a slurry (21).

[0123] According to one embodiment, the calendaring station (8000) includes at least one pair of opposing rollers.

[0124] According to one embodiment, at least one of the two rollers of a pair of opposing rollers is heated.

[0125] The calendaring station (8000) is located downstream of the electrode station (2000).

[0126] The calendaring station (8000) is located upstream of the combining station (4000).

[0127] According to one embodiment, the drying station (9000) is located downstream of the combining station (4000). Fig. 1 ).

[0128] According to the present embodiment, the electrode station (3000) is configured to directly deposit an electrolyte suspension (30) onto the electrode body (2) on which the electrode is drawn.

[0129] According to one embodiment, the drying station (9000) is located upstream of the combining station (4000). Fig. 2 ).

[0130] According to the present embodiment, the electrode station (3000) is configured to deposit an electrolyte suspension (30) onto a sliding support (32), preferably a flat polymer support. Thus, a film of the green electrolyte body (3) is continuously deposited onto the sliding support (32) by means of a slot die.

[0131] According to the present embodiment, after depositing a film of the electrolyte body (3) on a sliding support (32) by means of a slot die, a drying step (330) of the electrolyte body (3) is performed.

[0132] Accordingly, the film of the green electrolyte body (3) deposited on the sliding support (32) is heated.

[0133] This drying step (330) is performed before the bonding step (400) between the green electrolyte body (3) and the green electrode body (2).

[0134] According to one embodiment, the plant (1000) includes a rolling station (5000).

[0135] The rolling station (5000) includes at least one pair of opposing rolling rollers.

[0136] The rolling station (5000) is configured to roll and combine the green electrolyte body (3) and the green electrode body (2) that are stacked and transported to the rolling station (5000).

[0137] "Upstream" and "downstream" refer to the forward directions of the electrode (2), electrolyte (3), and components generally forming the half-cell (1).

[0138] Clearly, a person skilled in the art will be able to make changes or modifications to the present invention without departing from the scope of the following claims. Explanation of the symbols

[0139] 1. Half-cell 2. Green electrode body 3. Green Electrolyte Body 4. electrode 5. electrolytes 20. slip 21. slurry 22. Extruded slurry 30. electrolyte suspension 32. sliding support 61. Hopper 62. Wet mixer 63. extruder 80. roller 100. method 200. Electrode manufacturing process 210. Slip manufacturing stage 220. Slip mixing stage 230. Extrusion step 240. Calendaring stage 300. Electrolyte manufacturing process 310. Suspension preparation steps 320. Suspension deposition stage 330. drying stage 400. Combination step 500. Sintering stage 1000. plant 2000. electrode station 3000. Electrolyte station 4000. Combined station 5000. Rolling station 5500. Sintering station 6000. Casting Station 7000. Sleep Station 8000. Calendaring Station 9000. Drying station

Claims

Claim 1 A method (100) for manufacturing a half-cell (1) for a solid fuel cell, wherein the half-cell is formed by a double ceramic layer consisting of a coupled electrode (4) and an electrolyte (5), wherein the method (100) comprises: - a process (200) for manufacturing a green electrode body (2); - a process (300) for manufacturing a green electrolyte body (3); - a coupling step (400) in which the green electrode body (2) and the green electrolyte body (3) are coupled together; - a sintering step (500) after the coupling step (400), wherein the coupled green electrode body (2) and the green electrolyte body (3) are sintered to manufacture the half-cell (1) formed by the coupled electrode (4) and the electrolyte (5); and wherein the process (200) for manufacturing the green electrode body (2) comprises the following manufacturing steps: - Step (210) of manufacturing a slip (20); - A step (220) of mixing the above slip (20) to form a slurry (21); - Step (230) of extruding the above slurry (21) to form an extruded slurry (22); and - A step (240) of forming the green electrode body (2) by calendering the extruded slurry (22); and the process (300) for manufacturing the green electrolyte body (3) comprises the following manufacturing steps: - Step (310) of preparing an electrolyte suspension (30); - Step (320) of manufacturing a film of a green electrolyte body (3) by depositing the electrolyte suspension (30) by a slot die, preferably a curtain slot die; and - Optionally, a drying step (330) for drying the film of the green electrolyte body (3); comprising a method (100). Claim 2 A method (100) in which the slip (20) is prepared in step (210) by the following components, preferably only the following components: - nickel oxide (NiO); - zirconium oxide (YSZ); - pore-forming agent; - binder; and - plasticizer. Claim 3 A method (100) according to claim 1, wherein the following components combined together to form the slip (20) have the following percentages: - nickel oxide (NiO): 20 to 40%; - zirconium oxide (YSZ): 20 to 40%; - pore-forming agent: 1 to 15%; - binder: 30 to 50%; and - plasticizer: 1 to 15%. Claim 4 In claim 2 or 3, the nickel oxide and the zirconium oxide are in powder form, optionally, both the nickel oxide powder and the zirconium oxide powder have a particle size distribution (PSD) of less than 0.5 μm, and / or both the binder and the plasticizer are composed of polyacrylate, and / or comprise ethylene copolymer, or maleic acid copolymer, or styrene copolymer, or acrylate or methacrylate copolymer, or vinyl acetate copolymer, or polyvinyl butyral resin, or vinyl acetal resin, or vinyl resin, or vinyl alcohol resin, or wax or cellulose, or a combination thereof, and / or the binder is a binder based on a partially water-soluble acrylic polymer, and the binder has a solid content loading of 30% to 40%, and / or the binder is an acrylic binder, and / or vinyl, and / or water-based or solvent-based cellulose, and / or the water-based binder is partially or may be formed of a completely water-soluble polymer or may be a polymer emulsion, and / or the plasticizer is a plasticizer consisting of a 100% amine-containing polymer, and / or the pore-forming agent is one of starch, cellulose, acrylic polymer, carbon black or a combination thereof, method (100). Claim 5 In any one of claims 1 to 4, the step (220) of mixing the slip (20) comprises the step of mixing the components forming the slip (20) by a wet mixer (62) to form the slurry (21), wherein the components forming the slip (20) are mixed in the wet mixer (62) for a period of 10 to 30 minutes, or 15 to 25 minutes, or about 20 minutes, and optionally, when mixing, the step (220) of mixing the slip (20) comprises the step of degassing the slurry (21) to form a degassing slurry (21). Claim 6 A method (100) wherein, in any one of claims 1 to 5, the extruded slurry (22) has a thickness of less than 2 mm, and optionally, the step (230) of extruding the slurry (21) to produce the extruded slurry (22) is performed after the degassing step. Claim 7 In any one of claims 1 to 6, the calendering step (240) is performed to produce a green electrode body (2) with a thickness of 50 μm to 10,000 μm, preferably about 350 μm ± 10 μm or less, or the calendering step (240) is performed to produce an electrode body (2) with a thickness of 50 μm to 10,000 μm, preferably about 350 μm ± 10 μm or less, or the calendering step (240) is performed to produce an electrode body (2) with a thickness of about 100 μm ± 10 μm, and / or the calendering step (240) is performed by at least one pair of rollers (80) facing each other with respect to the extruded slurry (22) to be extruded to form the electrode body (2), and optionally, the calendering step (240) is performed by a pair of rollers (80). A method (100) wherein, optionally, during the calendering step (240), at least one roller (80) of the at least one pair of rollers (80), preferably each roller of the at least one pair of rollers (80), is optionally heated to a temperature of 40°C to 50°C, and optionally, during the calendering step (240), the roller (80) is rotated at a tangential speed of 5 m / min to 10 m / min, or about 5 m / min. Claim 8 A method (100) wherein, in any one of claims 1 to 7, the drying step (330) is performed after the bonding step (400) between the film of the green electrolyte body (3) and the green electrode body (2), and the step (320) of depositing the electrolyte suspension (30) by the slot die includes the step of directly depositing the electrolyte suspension (30) onto the green electrode body (2). Claim 9 A method (100), wherein in any one of claims 1 to 7, the drying step (330) is performed before the bonding step (400) between the green electrolyte body (3) and the green electrode body (2), the step (320) of depositing the electrolyte suspension (30) by the slot die, preferably a curtain slot die, comprises the step of depositing the electrolyte suspension (30) on a sliding support (32), preferably a flat polymer support, and the bonding step (400) between the green electrolyte body (3) and the green electrode body (2) provides that both the green electrolyte body (3) and the green electrode body (2) are transported in a stacked state toward a rolling station (5000) comprising at least one pair of opposing rolling rollers, and the bonding between the green electrode body (2) and the green electrolyte body (3) is performed by the rolling rollers of the rolling station (5000). Claim 10 A plant (1000) for manufacturing a half cell (1) for a solid fuel cell, wherein the half cell (1) is particularly formed by a double ceramic layer consisting of an electrode (4) and an electrolyte (5) combined together, and the plant (1000) comprises: - an electrode station (2000) where the manufacture of a green electrode body (2) is performed; - an electrolyte station (3000) where the manufacture of a green electrolyte body (3) is performed; - a coupling station (4000) where coupling between the green electrode body (2) and the green electrolyte body (3) is performed; and - a sintering station (5000) that sinters the green electrode body (2) and the green electrolyte body (3) combined together to manufacture the half cell (1) formed by the combined electrode (4) and electrolyte (5); wherein the electrode station (2000) manufactures, mixes, and extrudes a slip (20) and extrudes A plant (1000) comprising a slip station (7000) for manufacturing a slurry (22), the electrode station (2000) further comprises a calendering station (8000) configured to calender the slip (20), particularly the extruded slurry (22), to form the green electrode body (2), the electrolyte station (3000) comprises a casting station (6000) for manufacturing an electrolyte suspension (30) and depositing the electrolyte suspension (30) by a slot die, preferably a curtain slot die, to manufacture a film of the green electrolyte body (3), and optionally, the electrolyte station (3000) further comprises a drying station (9000) for drying the film of the green electrolyte body (3). Claim 11 In claim 10, the slip station (7000) comprises a wet mixer (62), optionally the slip station (7000) comprises a hopper (61) fluidly connected to the wet mixer (62), optionally the slip station (7000) comprises an extruder (63) configured to extrude the extruded slurry (22), the extruder (63) fluidly connected to the wet mixer (62) to extrude the extruded slurry (22) generated from the mixing of the slip (20) in the wet mixer (62), and optionally the slip station (7000) comprises a degasser configured to degas the slip (20) to form the slurry (21), a plant (1000). Claim 12 In claim 10 or 11, the calendering station (8000) comprises at least one pair of opposing rollers, at least one of the two rollers of the pair of bulk rollers is heated, and the calendering station (8000) is located downstream of the electrode station (2000) and upstream of the coupling station (4000), in a plant (1000). Claim 13 A plant (1000) according to any one of claims 10 to 12, wherein the drying station (9000) is located downstream of the combining station (4000), and the electrode station (3000) is configured to directly deposit the electrolyte suspension (30) onto the green electrode body (2). Claim 14 A plant (1000), wherein in any one of claims 10 to 12, the drying station (9000) is located upstream of the coupling station (4000), and the electrode station (3000) is configured to deposit the electrolyte suspension (30) onto a sliding support (32), preferably a flat polymer support. Claim 15 In claim 14, the plant (1000) comprises a rolling station (5000) including at least one pair of opposing rolling rollers, and the rolling station (5000) is configured to roll and combine the green electrolyte body (3) and the green electrode body (2) that are stacked and transferred to the rolling station (5000).