Iron soft magnetic powder for pressed magnetic cores, insulating coated soft magnetic powder for pressed magnetic cores, and mixed powder for pressed magnetic cores

By employing an iron-based soft magnetic powder with controlled impurities and a dual-coating insulating layer, the hysteresis loss in compacted magnetic cores is minimized, enhancing magnetic performance and cost-efficiency for three-dimensional magnetic circuits.

KR1020260164084APending Publication Date: 2026-11-17JFE STEEL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
KR1020267034778
Authority / Receiving Office
KR · KR
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-03-27
Filing Date
2024-10-29
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Conventional soft magnetic powders for compacted magnetic cores suffer from high hysteresis loss, limiting their practical application in motors and transformers, despite efforts to reduce this loss through methods like crystal grain coarsening and reducing inclusion density.

Method used

The use of an iron-based soft magnetic powder with controlled impurity levels (S: 20 ppm or less, Sn and Sb: total 200 ppm or less, with S: 10 ppm or less and Sn and Sb: total 5 ppm or more) and an insulating coating comprising condensed aluminum phosphate and silicone resin, along with a lubricant, to enhance grain growth and reduce hysteresis loss.

Benefits of technology

The solution results in a powder core with significantly reduced hysteresis loss, enabling improved magnetic properties and cost-effectiveness for three-dimensional magnetic circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCT00001
    Figure PCT00001
Patent Text Reader

Abstract

The present invention provides an iron-based soft magnetic powder for dust cores capable of producing a dust core with reduced hysteresis loss. The iron-based soft magnetic powder for dust cores has a component composition satisfying at least one of the following: in terms of mass concentration, S: 20 ppm or less, Sn and Sb: total 200 ppm or less, and also S: 10 ppm or less, and Sn and Sb: total 5 ppm or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to an iron-based soft magnetic powder for a dust core, an insulating coated soft magnetic powder for a dust core, and a mixed powder for a dust core. Background Technology

[0002] Magnetic cores used in motors, transformers, etc., require characteristics such as high magnetic flux density and low iron loss. Conventionally, laminated electrical steel sheets have been used for motor cores, but recently, powdered magnetic cores are attracting attention.

[0003] The greatest feature of a pressed powder core is that it allows for the formation of three-dimensional magnetic circuits. When electrical steel sheets are used as the material, the core is formed by lamination, so there are limitations to the degree of freedom in the shape. Furthermore, since the steel sheets with insulated surfaces are laminated, the magnetic properties differ in the direction of the steel sheet's surface and the direction perpendicular to the surface, and there is a drawback that the magnetic properties in the direction perpendicular to the surface are poor. On the other hand, a pressed powder core is formed by press-forming soft magnetic particles equipped with an insulating film, and since the shape can be changed by changing the mold, a degree of freedom in the shape exceeding that of electrical steel sheets can be obtained. In addition, because each particle is covered with an insulating film, the magnetic properties become uniform in all directions, which is advantageous for the formation of three-dimensional magnetic circuits.

[0004] Furthermore, since press forming requires fewer steps and is less expensive than the process of laminating electrical steel sheets, combined with the low cost of the base powder, the powder core demonstrates excellent cost performance.

[0005] As such, the compacted powder core enables the design of three-dimensional magnetic circuits while offering excellent cost performance. For these reasons, active research and development is being conducted on motors with three-dimensional magnetic circuits using compacted powder cores to realize the miniaturization, rare-earth-free, and low-cost requirements of motors that have recently been demanded.

[0006] On the other hand, there are several challenges. Among them, the greatest obstacle to the practical application of powder cores is iron loss. Iron loss consists mainly of two types: eddy current loss and hysteresis loss. However, powder cores have higher hysteresis loss compared to conventional iron core materials such as electrical steel sheets, so a reduction of this is required.

[0007] Against this backdrop, research has been conducted on reducing hysteresis loss in powdered magnetic cores.

[0008] Patent documents 1 and 2 disclose a technique for obtaining a compacted magnetic core with low hysteresis loss by reducing deformation in soft magnetic powder measured by X-ray diffraction.

[0009] Patent Document 3 discloses a technique for obtaining a compacted magnetic core with low hysteresis loss by coarsening the crystal grains in a soft magnetic powder.

[0010] Patent Document 4 discloses an iron-based soft magnetic powder for a compacted magnetic core in which the number density of inclusions of 0.1 μm or more is reduced. Prior art literature

[0011] Japanese Published Patent Application No. 2022-123416, Japanese Published Patent Application No. 2014-49643, Japanese Published Patent Application No. 2008-63652, Japanese Published Patent Application No. 2012-140679 The problem to be solved

[0012] However, even when using the soft magnetic powder proposed in Patent Documents 1 to 4, the hysteresis loss of the compacted magnetic core was not sufficiently reduced, and further performance improvement was required.

[0013] The present invention, made in consideration of the above circumstances, aims to provide an iron-based soft magnetic powder for a powder core capable of manufacturing a powder core with reduced hysteresis loss. means of solving the problem

[0014] The present invention was made to solve the above problem, and the gist thereof is as follows.

[0015] 1. By mass concentration,

[0016] S: 20ppm or less,

[0017] Sn and Sb: Total is 200 ppm or less, and also,

[0018] Iron-based soft magnetic powder for compacted magnetic cores having a component composition satisfying at least one of S: 10 ppm or less, and Sn and Sb: 5 ​​ppm or more in total.

[0019] 2. Insulated coated soft magnetic powder for a powder core, having an insulating coating on the surface of the particles constituting the iron-based soft magnetic powder for a powder core described in 1 above.

[0020] 3. The insulating coating soft magnetic powder for a compressed particle core described in 2, wherein the insulating coating comprises, in this order, a first coating comprising condensed aluminum phosphate and a second coating comprising silicone resin, extending outward from the surface of the particle.

[0021] 4. The insulating coating soft magnetic powder for a powder core described in 2 or 3, wherein the content of the insulating coating is 0.2 to 1.0 parts by mass per 100 parts by mass of the iron-based soft magnetic powder for a powder core.

[0022] 5. A mixed powder for a powder core comprising the insulating coated soft magnetic powder for a powder core described in any one of 2 to 4 above, and 0.2 to 0.8 parts by mass of a lubricant per 100 parts by mass of the insulating coated soft magnetic powder for a powder core. Effects of the invention

[0023] According to the present invention, an iron-based soft magnetic powder for a powder core can be provided, which enables the production of a powder core with reduced hysteresis loss. Specific details for implementing the invention

[0024] (Form for carrying out the invention)

[0025] Hereinafter, a method for carrying out the present invention will be described in detail. Furthermore, the following description is intended to represent examples of suitable embodiments of the present invention, and the present invention is not limited thereto. Additionally, the iron-based soft magnetic powder for powder cores, the insulating-coated soft magnetic powder for powder cores, and the mixed powder for powder cores may be referred to simply as "iron-based soft magnetic powder," "insulating-coated soft magnetic powder," and "mixed powder," respectively.

[0026] [Prepared Iron Soft Magnetic Powder for Magnetic Cores]

[0027] The iron-based soft magnetic powder for a compacted magnetic core according to the present invention has a composition satisfying at least one of the following: in terms of mass concentration, S: 20 ppm or less, Sn and Sb: total of 200 ppm or less, and also S: 10 ppm or less, and Sn and Sb: total of 5 ppm or more. In the present invention, "iron-based soft magnetic powder" refers to a soft magnetic powder containing 50 mass% or more of Fe.

[0028] As the above iron-based soft magnetic powder, for example, iron powder or iron-based alloy powder may be used; however, iron powder is preferred due to its good compressibility during pressure molding and ease of high-density formation. Here, "iron powder" refers to a powder composed of Fe and unavoidable impurities, and in the field of the art, it is generally referred to as "pure iron powder." Furthermore, "iron-based alloy powder" refers to an alloy powder containing 50 mass% or more of Fe. The alloying elements of the above iron-based alloy powder are not particularly limited, and in addition to S, Sn, and Sb, at least one selected from the group consisting of, for example, Al, Si, Co, Cr, Mn, Mo, and Ni may be used. The above iron-based alloy powder may be, for example, powders such as Fe-Al alloy, Fe-Si alloy, Sendust, or Permalloy. The above Fe-Si alloy may be, for example, an Fe-3 mass% Si alloy or an Fe-6.5 mass% Si alloy. In addition, the crystal state of the above-mentioned iron-based soft magnetic powder is not particularly limited, and the above-mentioned iron-based soft magnetic powder may be, for example, an amorphous powder.

[0029] The above iron soft magnetic powder may be atomized powder, or at least one selected from the group consisting of gas atomized powder, water atomized powder, and centrifugal atomized powder. Here, gas atomized powder, water atomized powder, and centrifugal atomized powder refer to powders obtained by the gas atomization method, water atomization method, and centrifugal atomization method described below, respectively. For the reasons described below, water atomized powder is preferred, and water atomized iron powder is more preferred.

[0030] (Composition)

[0031] The inventors of the present invention have carefully examined the cause of the failure to reduce hysteresis loss of the powder core when using conventional soft magnetic powder, and have obtained the following findings.

[0032] In reducing hysteresis loss in a powdered core, it is effective to coarsen the crystal grains within the microstructure of the powdered core. Here, during the heat treatment for strain relief after pressure forming, recrystallization behavior can be observed in which nuclei of recrystallized grains are generated within the microstructure and subsequently, recrystallized grains grow from said nuclei. It is presumed that conventional methods (for example, the methods proposed in Patent Documents 1 to 3) aimed to coarsen the crystal grains within the powdered core by suppressing the generation of recrystallization nuclei. However, even if the generation of recrystallization nuclei in the microstructure is suppressed, if the growth of recrystallized grains is inhibited, the crystal grains remain fine, and a sufficient effect of reducing hysteresis loss is not obtained.

[0033] Furthermore, if S is present in excess, the growth of recrystallized grains is inhibited. In addition, during strain relief heat treatment, nitride-based precipitates and inclusions formed depending on the content of S, Sn, and Sb—elements prone to grain boundary segregation—also inhibit the growth of recrystallized grains.

[0034] Based on the above understanding, the above iron soft magnetic powder, in terms of mass concentration,

[0035] S: 20ppm or less,

[0036] Sn and Sb: Total is 200 ppm or less, and also,

[0037] It has a component composition satisfying at least one of the following: S: 10 ppm or less, and Sn and Sb: total of 5 ppm or more. In other words, in terms of mass concentration,

[0038] S: 10 ppm or less, and additionally, Sn and Sb: a total of 200 ppm or less, component composition, or

[0039] It has a component composition in which S: greater than 10 ppm and less than or equal to 20 ppm, and Sn and Sb: total of 5 ppm or more and less than or equal to 200 ppm.

[0040] The composition of the above-mentioned iron-based soft magnetic powder is described in detail below. Furthermore, in the following description, "ppm" as a unit of content is expressed as a mass concentration unless otherwise specified.

[0041] (S content)

[0042] S inhibits grain growth through grain boundary segregation and the formation of MnS. If the S content exceeds 20 ppm, the hysteresis loss of the manufactured powdered core increases. Therefore, the S content is kept below 20 ppm. From the perspective of ease of manufacturing, the S content may exceed 10 ppm, but from the perspective of further promoting grain growth, the S content is preferably 10 ppm or less, and more preferably 5 ppm or less. Meanwhile, the lower limit of the S content is not limited, but it may be 0 ppm, and S may not be included. The S content is measured by the combustion-infrared absorption method.

[0043] (Total content of Sn and Sb)

[0044] Including one or both of Sn and Sb has the effect of coarsening the crystal grains by suppressing the formation of nitride-based precipitates and inclusions from grain boundaries due to grain boundary segregation. For this reason, the total content of Sn and Sb is preferably 5 ppm or more, and more preferably 10 ppm or more. On the other hand, if the total content of Sn and Sb exceeds 200 ppm, grain growth is inhibited by grain boundary segregation, and the hysteresis loss of the manufactured powdered core increases. Therefore, the total content of Sn and Sb is set to 200 ppm or less. The total content of Sn and Sb is preferably 150 ppm or less, and more preferably 100 ppm or less.

[0045] Here, if the S content exceeds 10 ppm and the total content of Sn and Sb is less than 5 ppm, the hysteresis loss of the manufactured powdered core increases. Therefore, the above compositional composition satisfies at least one of the following: S: 10 ppm or less, and Sn and Sb: total of 5 ppm or more. In other words, if the S content exceeds 10 ppm, the total content of Sn and Sb is 5 ppm or more. In this way, even if the S content exceeds 10 ppm, grain growth can be promoted by including Sn and Sb in total of 5 ppm or more. It is preferable that the above compositional composition satisfies at least one of the following: S: 10 ppm or less, and Sn and Sb: total of 10 ppm or more. Furthermore, if the S content is 10 ppm or less, the lower limit of the total content of Sn and Sb is not limited and may be 0, or may not include either Sn or Sb.

[0046] The content of Sn and the content of Sb shall both be 200 ppm or less to satisfy the aforementioned condition regarding the total content of Sn and Sb. Meanwhile, the lower limit of the content of Sn and Sb is not limited. The Sn content may be 0, and Sn may not be included, but 5 ppm or more is preferred. The Sb content may be 0, and Sb may not be included, but 5 ppm or more is preferred.

[0047] In the above composition, components other than S, Sn, and Sb are not particularly limited, and the composition may additionally include Fe: 50 mass% or more and alloying elements, with the remainder consisting of unavoidable impurities. Furthermore, the composition may additionally include Fe: 50 mass% or more and at least one selected from the group consisting of Al, Si, Co, Cr, Mn, Mo, and Ni, with the remainder consisting of unavoidable impurities. However, for good compressibility during pressure molding and ease of high-density formation, it is preferable that the composition further include Fe: 50 mass% or more and the remainder consist of unavoidable impurities. The iron-based soft magnetic powder may include, for example, Al, Si, Mn, and Cr as unavoidable impurities. When each element is included as an impurity, it is desirable to reduce the content as much as possible.

[0048] Next, a suitable composition of elements that may be included in the above-mentioned iron-based soft magnetic powder is described.

[0049] (Al content)

[0050] Al is a readily oxidizable metallic element, and if included, a large amount of oxide-based inclusions may be generated during atomization, potentially hindering grain growth. Therefore, from the perspective of suppressing the formation of oxide-based inclusions, it is desirable to limit the Al content to 0.010 mass% or less when Al is included as an impurity. The lower limit of the Al content is not limited; it may be 0%, or Al may not be included at all. However, from the perspective of manufacturing costs, 0.001 mass% or more is desirable. Additionally, Al may be used as an alloying element. For example, the Al content may be greater than 0.010 mass% and less than or equal to 50 mass%.

[0051] (Si content)

[0052] Si is a metallic element that can cause oxidation, and if included, it may generate a large amount of oxide-based inclusions during atomization, potentially hindering grain growth. Therefore, from the perspective of suppressing the formation of oxide-based inclusions, it is desirable to limit the Si content to 0.010 mass% or less when Si is included as an impurity. The lower limit of the Si content is not limited; it may be 0%, or Si may not be included at all. However, from the perspective of manufacturing costs, 0.001 mass% or more is desirable. Additionally, Si may be used as an alloy component. For example, the Si content can be greater than 0.010 mass% and less than or equal to 50 mass%. When Si is used as an alloy component, the Si content is preferably 10 mass% or less from the perspective of facilitating the securing of magnetic flux density, and 7 mass% or less from the perspective of further reducing iron loss. Similarly, when Si is used as an alloy component, the Si content is preferably 1 mass% or more from the perspective of further reducing iron loss.

[0053] (Mn content)

[0054] Mn is a metallic element that is oxidizable, and if included, a large amount of oxide-based inclusions may be generated during atomization, potentially hindering grain growth. Therefore, from the perspective of suppressing the formation of oxide-based inclusions, when Mn is included as an impurity, it is desirable to keep the Mn content at 0.100 mass% or less, and more desirable to keep it at 0.070 mass% or less. Since a lower Mn content is preferable, the lower limit of the Mn content is not limited; it may be 0%, or Mn may not be included at all. However, from the perspective of manufacturing costs, 0.010 mass% or more is desirable. Additionally, Mn may be used as an alloying element. For example, the Mn content may be greater than 0.100 mass% and less than or equal to 50 mass%.

[0055] (Cr content)

[0056] Cr is a metallic element that can cause oxidation, and if included, it may generate a large amount of oxide-based inclusions during atomization, potentially hindering grain growth. Therefore, from the perspective of suppressing the formation of oxide-based inclusions, when Cr is included as an impurity, it is desirable to keep the Cr content at 0.050 mass% or less, and more desirable to keep it at 0.040 mass% or less. Since a lower Cr content is preferable, there is no lower limit to the Cr content; it may be 0%, or Cr may not be included at all. However, from the perspective of manufacturing costs, 0.001 mass% or more is desirable. Additionally, Cr may be used as an alloying element. For example, the Cr content may be greater than 0.050 mass% and less than or equal to 50 mass%.

[0057] (Apparent density)

[0058] The apparent density of the above iron-based soft magnetic powder is not limited, but from the perspective that a high-density pressed powder core can be easily produced, it is preferable to have a density of 2.8 Mg / m³ or higher. The upper limit of the apparent density is also not particularly limited, but typically it can be 5.0 Mg / m³ or lower. The above apparent density can be measured according to JIS Z 2504.

[0059] (Average particle diameter)

[0060] The average particle diameter of the above-mentioned iron-based soft magnetic powder is not particularly limited, but it is desirable that it be within a predetermined range from the perspective of increasing fluidity and facilitating filling into a mold during the manufacture of a powder core. Specifically, the volume-based median diameter D measured by laser diffraction is 50 It is preferable that the average particle diameter based on mass measured by the sieving method be 10㎛ or more. In addition, it is preferable that the average particle diameter based on mass measured by the sieving method be 60㎛ or more, and it is also preferable that the average particle diameter based on mass measured by the sieving method be 200㎛ or less.

[0061] (Maximum particle size)

[0062] The maximum particle size of the above iron-based soft magnetic powder is not particularly limited, but it is preferably 600 μm or less to suppress the increase in eddy current loss. The above maximum particle size can be measured by the sieving method.

[0063] [Insulating Coated Soft Magnetic Powder for Compacted Magnetic Cores]

[0064] The insulating coated soft magnetic powder for a compressed powder core according to the present invention has an insulating coating on the surface of the particles constituting the iron-based soft magnetic powder. By having the insulating coating, insulation between particles is secured, thereby suppressing short circuits between particles.

[0065] (Insulation)

[0066] Any covering may be used as the insulating covering. The insulating covering may consist of one covering or two or more coverings. If the insulating covering consists of two or more coverings, it may consist of coverings of the same type or coverings of different types. The insulating covering may have a layered form. That is, the insulating covering may be a single-layer film or a multilayer film consisting of two or more layers. The multilayer film may be a multilayer film consisting of a film of the same type or a multilayer film consisting of a film of different types.

[0067] As the above insulating covering, for example, one or both of an inorganic insulating covering and an organic insulating covering may be used.

[0068] The above-mentioned inorganic insulating sheath may utilize either or both amorphous materials and crystalline materials as inorganic insulating materials. Examples of the amorphous materials include metal phosphate salts and metal borate salts. Among the metal phosphate salts, condensed aluminum phosphate is preferred. Examples of the crystalline materials include metal oxides and SiO2. Examples of the metal oxides include MgO, forsterite, talc, and Al2O3. The above-mentioned inorganic insulating sheath is a sheath comprising the above-mentioned inorganic insulating material, and it is preferable that it be composed of the above-mentioned inorganic insulating material.

[0069] Examples of condensed aluminum phosphate include aluminum dihydrogen tripolyphosphate, aluminum metaphosphate, and mixtures thereof, all of which can be obtained by heating aluminum monophosphate to undergo a dehydration reaction. Among these, aluminum dihydrogen tripolyphosphate is preferred. Hereinafter, aluminum dihydrogen tripolyphosphate may be referred to as aluminum tripolyphosphate.

[0070] The above organic insulating coating is a coating containing an organic resin, and it is preferable that it be made of an organic resin. It is preferable to use silicone resin as the organic resin. Since silicone resin forms Si-O bonds with excellent heat resistance through heat treatment, excellent insulation properties can be preserved even when a deformation removal heat treatment is performed on the molded body at a high temperature (e.g., 600°C) during the production of the powder core.

[0071] As for the silicone resin, resin-based silicone resins may be used, for example, silicone resins having 60 mol% or more of T units (trifunctional siloxane units). Among these, silicone resins having 50 mol% or more of the functional groups on the Si phase as methyl groups are preferred, for example, methylphenyl silicone resins (KR-255, KR-311, KR-300, etc. manufactured by Shin-Etsu Kagaku Co., Ltd.) and methyl silicone resins (KR-251, KR-400, KR-220L, KR-220LP, KR-242A, KR-240, KR-500, KC-89, etc. manufactured by Shin-Etsu Kagaku Co., Ltd.). In addition, SR2400 and Torefil R-910 manufactured by Tore Dow Corning may also be used.

[0072] In a preferred embodiment of the present invention, the insulating coating has, in this order, a first coating comprising condensed aluminum phosphate and a second coating comprising silicone resin, extending outward from the surface of the particle. That is, the insulating coating soft magnetic powder preferably has, in this order from the inside, the iron-based soft magnetic powder, the first coating, and the second coating. It is more preferable that the insulating coating consists of the first coating and the second coating.

[0073] The content of condensed aluminum phosphate in the first coating is not limited and may be, for example, 50 mass% or more. However, the content is preferably 99 mass% or more, and it is more preferable that the first coating be made of condensed aluminum phosphate. It is preferable that the first coating be a coating using condensed aluminum phosphate.

[0074] The content of the silicone resin in the second coating is not limited and may be, for example, 50 mass% or more. However, the content is preferably 99 mass% or more, and it is more preferable that the second coating be made of silicone resin. It is preferable that the second coating be a coating using silicone resin.

[0075] The above insulating coating soft magnetic powder comprises the insulating coating and the iron-based soft magnetic powder, and preferably consists of the insulating coating and the iron-based soft magnetic powder. In order to further enhance insulation properties, it is preferable that the content of the insulating coating be 0.2 parts by mass or more per 100 parts by mass of the iron-based soft magnetic powder. On the other hand, if the amount of coating is excessively large, the magnetic flux density decreases, which may impair the function as an iron core, and the density of the iron core also decreases. Therefore, it is preferable that the content of the insulating coating be 1.0 part by mass or less per 100 parts by mass of the iron-based soft magnetic powder.

[0076] [Mixed Powder for Compaction Cores]

[0077] The mixed powder for a compressed magnetic core according to the present invention comprises the insulating coated soft magnetic powder and a lubricant in a predetermined ratio. The mixed powder for a compressed magnetic core may also be composed of the insulating coated soft magnetic powder and a lubricant.

[0078] (slush)

[0079] A powdered magnetic core is manufactured by pressure-molding a soft magnetic powder using a mold. To improve release properties from the mold, the mixed powder of the present invention comprises a lubricant in addition to the insulating-coated soft magnetic powder. Hereinafter, the lubricant content is expressed as 100 parts by mass of the insulating-coated soft magnetic powder. To ensure sufficient lubricity, the mixed powder comprises 0.2 parts by mass or more of the lubricant. Furthermore, since including more than 0.8 parts by mass of the lubricant results in a decrease in the density of the powdered magnetic core, the mixed powder comprises 0.8 parts by mass or less of the lubricant. As for the material of the lubricant, organic lubricants such as fatty acid amides and inorganic lubricants such as MoS2, WS2, BN, and talc are used. Examples of fatty acid amides include stearic acid amide, EBS (ethylenebis-stearic acid amide), erucic acid amide, and oleic acid amide. These may be used individually or in a mixture of two or more types.

[0080] [Method for manufacturing iron soft magnetic powder]

[0081] Next, a method for manufacturing the iron-based soft magnetic powder according to one embodiment of the present invention will be described. Furthermore, the following description represents an example of a manufacturing method, and the present invention is not limited to the description below.

[0082] Powders obtained by oxide reduction and electrolytic precipitation methods have low apparent density, and even if further processing such as crushing is performed to increase apparent density, sufficient apparent density is not obtained. Therefore, from the perspective of improving the density of the obtained powdered magnetic core, it is preferable to manufacture the above-mentioned iron-based soft magnetic powder using the atomization method. The atomization method is a method of powdering molten metal and cooling and solidifying it, and water atomization, gas atomization, and centrifugal atomization methods can all be used. Water atomization is a method of powdering molten metal by spraying water onto it, and gas atomization is a method of powdering molten metal by spraying gas. It is also acceptable to powder by spraying both water and gas. Centrifugal atomization is a method of powdering molten metal using centrifugal force generated by rotation. Powders obtained using two or more of these methods may also be combined. When using the water atomization method, the particles have numerous irregularities on their surface, making them prone to entanglement. When formed into a powder core, the strength of the powder core can be improved. Additionally, the water atomization method is inexpensive. Therefore, from the perspective of the strength and cost of the resulting powder core, the water atomization method is preferable. In contrast, since the gas atomization method allows for production in relatively large quantities, the gas atomization method is preferable from the perspective of mass production. Below, a manufacturing method using the water atomization method is described as an example.

[0083] Molten steel is used as the above-mentioned molten metal. The above-mentioned molten steel is not limited to those with iron as the main component. However, if a large amount of S is included, desulfurization in subsequent processes may be difficult. Therefore, in order to easily obtain iron-based soft magnetic powder having the aforementioned composition, it is preferable that the S content of the above-mentioned molten steel be less than 50 ppm.

[0084] The Sn content, Sb content, remainder, and suitable content of other elements that may be included in the molten steel may be determined in the same manner as the composition of the iron-based soft magnetic powder described above. Furthermore, the content of the oxidizing metal element is not limited and may be included as an alloying element in the molten steel. However, in that case, to prevent the formation of a large amount of oxide-based inclusions, it is desirable to reduce the infusion of oxygen from the atmosphere, for example, during atomization.

[0085] (Annealing)

[0086] Next, by performing annealing on the powder obtained by the above atomization method, the amount of S in the powder can be reduced, thereby obtaining the above iron-based soft magnetic powder. The above annealing may be performed by decarburization and reduction annealing as described later.

[0087] The above-mentioned reduction annealing is preferably performed by a single or multiple heat treatment. By reducing annealing, the amount of sulfur in the powder can be reduced, and the crystal grain size in the resulting iron-based soft magnetic powder can be coarsened. Particle size adjustment, such as grinding, may be performed before and after each stage of heat treatment.

[0088] The temperature of the heat treatment is preferably 700°C or higher, more preferably 800°C or higher, and even more preferably 900°C or higher. Additionally, the temperature of the heat treatment is preferably less than 1200°C, and more preferably less than 1100°C. The retention time of the heat treatment is preferably 1 hour or more. Additionally, the retention time of the heat treatment is preferably 7 hours or less, and more preferably 5 hours or less. The atmosphere of the heat treatment is typically a reducing atmosphere, and an atmosphere containing hydrogen is preferred. The upper limit of the dew point of the atmosphere is not particularly limited, but is preferably 30°C or lower. Additionally, the lower limit of the dew point of the atmosphere is not particularly limited, but may be, for example, -40°C or higher.

[0089] The above decarburization is preferably performed as a heat treatment in a damp hydrogen atmosphere. Through the above decarburization, not only the C content but also the S content in the powder can be reduced. Since desulfurization occurs through oxidation, the S content is more easily reduced by the above decarburization than by the above reductive annealing. Here, a damp hydrogen atmosphere refers to an atmosphere containing water vapor and hydrogen, and specifically, refers to an atmosphere containing hydrogen with a dew point greater than 30°C. The dew point of the heat treatment in the above damp hydrogen atmosphere is preferably 60°C or lower. The temperature and holding time of the heat treatment in the above damp hydrogen atmosphere can be the same as those of the heat treatment for the above reductive annealing.

[0090] After performing the heat treatment in the above-mentioned damp hydrogen atmosphere, it is preferable to perform the heat treatment for the above-mentioned reduction annealing at least once in an atmosphere containing hydrogen with a dew point of 30°C or lower, under conditions of a temperature of 800°C or higher and a holding time of 1 hour or more. When heat treatment is performed in a damp hydrogen atmosphere, fine inclusions are formed by water vapor. Therefore, by subsequently performing a heat treatment for a predetermined time in a low dew point and high temperature atmosphere to decompose the inclusions, the number density of inclusions in the iron-based soft magnetic powder produced can be reduced, and the hysteresis loss of the powder core produced accordingly can be further reduced. For example, the above-mentioned annealing can be performed as a two-stage heat treatment, the first stage being a heat treatment in a damp hydrogen atmosphere, and the second stage being a heat treatment in an atmosphere containing hydrogen with a dew point of 30°C or lower, under conditions of a temperature of 800°C or higher and a holding time of 1 hour or more.

[0091] After the above annealing, appropriate grinding and sieving can be performed to adjust the apparent density and particle size distribution of the iron-based soft magnetic powder.

[0092] In addition, typically, in the final iron-based soft magnetic powder, the content of metal elements such as Sn, Sb, Al, Si, Cr, and Mn is equivalent to the composition of the molten steel.

[0093] [Method for manufacturing insulating coated soft magnetic powder]

[0094] Next, a method for manufacturing the insulating coated soft magnetic powder according to one embodiment of the present invention will be described. Furthermore, the following description represents an example of a manufacturing method, and the present invention is not limited to the description below.

[0095] The above insulating coated soft magnetic powder can be manufactured by forming the insulating coating on the above iron-based soft magnetic powder. The above insulating coating can be formed by a method such as a wet method or a dry method without being particularly limited. The wet method is a method of mixing the material used for the insulating coating and the above iron-based soft magnetic powder using a solvent such as water or an organic solvent. On the other hand, the dry method is a method of mixing the material used for the insulating coating and the above iron-based soft magnetic powder without using a solvent. The above mixing may be performed using a mixer, and the mixer may be, for example, a rotary blade type. Examples of rotary blade type mixers include the FM mixer series (manufactured by Nippon Coke) and the high-speed mixer series (manufactured by Earth Technica).

[0096] Below, details are described regarding the case where the insulating coating has a first coating made of condensed aluminum phosphate and a second coating made of silicone resin in this order, extending outward from the surface of the particle.

[0097] (First covering)

[0098] First, a first coating consisting of condensed aluminum phosphate is formed on the above-mentioned iron-based soft magnetic powder. The formation of the first coating can be carried out, for example, by a dry method; specifically, it can be formed by mixing the iron-based soft magnetic powder and the condensed aluminum phosphate powder, preferably by heating and mixing. By using a dry method, the problem of oxidation of the iron-based soft magnetic powder can be avoided, and since a process of dissolving in a solvent is unnecessary, it is advantageous in terms of equipment and workability. Furthermore, by forming the first coating by heating and mixing, the first coating can be formed in a layer shape or as a continuous film. Here, the continuous film may be a complete coating or a partial coating, but the powders are fused together so that the coated area is continuous, and it is distinguished from a state where the powder is attached sporadically. It is preferable that most of the surface of the iron-based soft magnetic powder is covered by the continuous film, and it is more preferable that substantially the entire surface is covered. In addition, excellent adhesion to the surface of the iron-based soft magnetic powder of the first coating can be achieved through the above-mentioned heating and mixing. This is presumed to be because a reaction occurs at the interface between the continuous film of condensed aluminum phosphate and the iron-based soft magnetic powder.

[0099] The average particle diameter of the above-mentioned condensed aluminum phosphate powder may be 1 μm or more, and preferably 1.5 μm or more. Meanwhile, the above-mentioned average particle diameter may be 10 μm or less, and preferably 7.5 μm or less. If the above-mentioned average particle diameter is set to 1 μm or more and 10 μm or less, sufficient fluidity can be secured to improve workability, and furthermore, it can be made easier to uniformly form the above-mentioned first coating as a continuous film. In addition, the above-mentioned average particle diameter is the volume-based median diameter D measured by laser diffraction. 50 am.

[0100] For the above mixing, the aforementioned mixer may be used. The rotational speed of the mixer is not particularly limited, but in order to efficiently form the first coating and to make the first coating a continuous film, a speed of 100 rpm or more is preferred, and 200 rpm or more is more preferred. On the other hand, excessive high-speed stirring may cause plastic deformation of the iron-based soft magnetic powder, which may result in a decrease in compressibility and an increase in hysteresis loss during pressure molding. Therefore, the rotational speed is preferably 1000 rpm or less, and more preferably 800 rpm or less.

[0101] In the above mixing, the maximum temperature reached during mixing is not particularly limited. However, in order to facilitate the formation of the first coating as a continuous film, the maximum temperature reached is preferably 100°C or higher, more preferably 130°C or higher, and even more preferably 150°C or higher. On the other hand, since condensed aluminum phosphate may deteriorate due to high temperatures, the maximum temperature reached is preferably 200°C or lower. Furthermore, the temperature referred to herein refers to the temperature of the powder during mixing, and when using a rotary blade type mixer, it is the temperature indicated by a thermocouple protruding from the tank wall of the stirring tank to the extent that it does not come into contact with the rotary blade. Furthermore, the maximum temperature reached during mixing refers to the highest temperature among the temperatures of the powder during mixing, and can be the highest temperature among the temperatures of the powder containing the iron-based soft magnetic powder and the condensed aluminum phosphate powder measured by the thermocouple. The above mixing is preferably carried out in an inert gas atmosphere to suppress the oxidation of the iron-based soft magnetic powder, and for example, it is preferably carried out in a nitrogen atmosphere.

[0102] After the above mixing, the powder having the first coating is discharged from the mixer. For the purpose of inhibiting oxidation, the temperature of the powder at discharge is preferably 80°C or lower, more preferably 60°C or lower. The lower limit of the temperature of the powder at discharge is not particularly limited and, for example, can be room temperature or higher, 0°C or higher, or 30°C or higher.

[0103] (Second covering)

[0104] Next, a second coating made of silicone resin is formed on the powder obtained by the aforementioned method. The formation of the second coating can be carried out, for example, by a wet method using an organic solvent or a dry method without using a solvent, and both can be used to form a coating made of silicone resin in a layer shape. The dry method is preferred because it eliminates the need for safety measures associated with the use of organic solvents and is advantageous in terms of cost, equipment, and workability.

[0105] In the case of the wet method, the silicone resin can be attached by mixing a solution in which the silicone resin is dissolved in an organic solvent with the insulating coated soft magnetic powder obtained by the above method and drying. Examples of the organic solvent include petroleum-based organic solvents such as alcohols, xylene, and toluene. The solid content concentration of the silicone resin in the solution can be 1 to 10 mass%. Drying can be performed in the atmosphere. The drying temperature can be the temperature at which the organic solvent used volatilizes, and can also be lower than the curing temperature of the silicone resin. In the case of the wet method, as the silicone resin, it is preferable to use at least one selected from the group consisting of, for example, SR2400 manufactured by Toledo Dow Corning, KR-311 manufactured by Shin-Etsu Kagaku, and LR-220L.

[0106] In the case of the dry method, the silicone resin can be attached by mixing the solid silicone resin with the powder having the first coating obtained by the aforementioned method. The aforementioned mixer may be used for the above mixing. The rotational speed of the mixer is not particularly limited, but to efficiently form the second coating, 100 rpm or more is preferred, and 200 rpm or more is more preferred. On the other hand, excessive high-speed stirring may cause plastic deformation of the iron-based soft magnetic powder, leading to a decrease in compressibility and an increase in hysteresis loss during pressure molding. Therefore, the rotational speed is preferably 2000 rpm or less, and more preferably 1500 rpm or less. Mixing can be performed, for example, by starting the mixing at room temperature and discharging the powder from the mixer when the powder temperature reaches a temperature of 40°C or higher and 70°C or lower. The solid silicone resin is not particularly limited, and one or both of the following may be used: a silicone resin in powder form or a flake form. It is preferable to use a solid silicone resin that softens upon heating. In the case of the dry method, as a silicone resin, it is preferable to use at least one selected from the group consisting of, for example, Torefil R-910 manufactured by Tore Dow Corning and KR-220LP manufactured by Shin-Etsu Kagaku.

[0107] After attaching the silicone resin by a wet method or a dry method, heat treatment may be performed to increase the hardness of the attached silicone resin. The temperature of the heat treatment may be, for example, 150°C or higher and 250°C or lower. The heat treatment may be performed in the atmosphere or in an inert gas atmosphere (for example, a nitrogen atmosphere).

[0108] [Method for manufacturing mixed powder]

[0109] The above mixed powder can be prepared by adding, for example, the above lubricant to the above insulating coated soft magnetic powder. The type and amount of the added lubricant are as described above.

[0110] [Abun Jasim]

[0111] Next, a method for manufacturing a powder core using the iron-based soft magnetic powder for powder cores, the insulating coated soft magnetic powder for powder cores, or the mixed powder for powder cores of the present invention will be described. Furthermore, the following description represents an example of a manufacturing method, and the present invention is not limited to the description below.

[0112] (Pressure molding)

[0113] The above iron-based soft magnetic powder forms the insulating coating, and if necessary, a lubricant is mixed in, then loaded into a mold and pressure-molded to obtain the desired dimensions and shape. The method of pressure-molding is not particularly limited, and any conventional molding method, such as room-temperature molding or mold lubrication molding, can be applied. Mold lubrication molding is a method that can increase ejectability by applying a lubricant to the mold wall and performing pressure-molding, and it can be suitably used even when no lubricant is added to the above insulating-coated soft magnetic powder. Suitable lubricants for applying to the wall include metal soaps such as lithium stearate, zinc stearate, and calcium stearate, and waxes such as fatty acid amides. Additionally, the molding pressure is appropriately determined according to the application, but since increasing the molding pressure can increase the density of the resulting compressed magnetic core, it is preferably 10 t / cm² or more, and more preferably 15 t / cm² or more.

[0114] (Deformation removal heat treatment)

[0115] After pressure molding, the above powder undergoes heat treatment (deformation removal heat treatment) for the purpose of reducing hysteresis loss by removing deformation or improving the strength of the molded body. The heat treatment temperature is not particularly limited. In addition, the holding time for the heat treatment is not particularly limited, but it is preferable to set it to 5 to 120 minutes. Furthermore, a step of maintaining a constant temperature during the temperature rise or fall during the heat treatment may be formed. The atmosphere for the heat treatment is not limited and may be, for example, in an atmosphere, an inert atmosphere, a reducing atmosphere, or a vacuum. The dew point of the above atmosphere is not particularly limited and may be determined appropriately according to the application.

[0116] Examples

[0117] The present invention will be described in detail below based on examples.

[0118] First, iron powder with an S content of less than 50 ppm was prepared from molten steel by the water atomization method. Next, a two-stage heat treatment was performed on the obtained iron powder. First, heat treatment was carried out in a damp hydrogen atmosphere (dew point 40°C). The holding temperature was set to 950°C and the holding time to 1 hour. The obtained lump-shaped material was crushed. Subsequently, to reduce fine inclusions, additional heat treatment was carried out in a hydrogen atmosphere (dew point 20°C). The holding temperature was set to 950°C and the holding time to 1 hour. The obtained iron soft magnetic powder was adjusted to have a maximum particle size of less than 250 μm as measured by the aforementioned method, and also a volume-based median diameter D as measured by laser diffraction 50The average particle diameter based on mass, measured by the sieving method, was set to 100–180 μm. The above iron-based soft magnetic powder had a composition consisting of the components listed in Table 1, plus Al: 0.010 mass% or less, Si: 0.010 mass% or less, Mn: 0.100 mass% or less, and Cr: 0.050 mass% or less, with the remainder being Fe and other unavoidable impurities. Here, the S content was measured using the aforementioned method with a CS844 manufactured by LECO. Furthermore, it was confirmed that the content of Sn, Sb, Al, Si, Mn, and Cr was the same as the content of each component in the iron-based powder prior to the heat treatment. Additionally, Sn+Sb in the table represents the total content of Sn and Sb.

[0119] Next, an insulating coating was formed on these iron-based soft magnetic powders. First, a coating made of aluminum tripolyphosphate was formed by heating and mixing aluminum tripolyphosphate powder with an average particle diameter of 5 μm. A high-speed mixer (LFS-GS-2J type manufactured by Earth Technica (formerly manufactured by Fukae Powtech Co.)) was used for mixing. The atmosphere inside the stirring tank was set to nitrogen, the heater temperature of the stirring tank was set to 190°C, and heating and mixing were performed while stirring for 20 minutes at a rotation speed of 500 rpm of the rotating blades. Afterward, the powder was removed by cooling it to 60°C inside the stirring tank.

[0120] Next, a coating made of silicone resin was formed on the outer surface of the coating made of aluminum tripolyphosphate. The silicone resin was dissolved in toluene to prepare a resin dilution solution in which the solid content concentration of the silicone resin in the solution was 2.0 mass%. The powder after the above heating and mixing was kneaded with the resin dilution solution, dried, and then subjected to heat treatment at 200°C for 120 minutes in the atmosphere. The content of the insulating coating was adjusted so that, relative to 100 mass parts of the iron-based soft magnetic powder, the coating made of aluminum tripolyphosphate was 0.3 mass parts and the coating made of silicone resin was 0.3 mass parts. A ring-shaped test specimen was produced by pressure molding using these powders and by performing heat treatment. The pressure molding was performed using a mold lubrication molding method at a molding pressure of 980 MPa, and the shape was formed with an outer diameter of 38 mm, an inner diameter of 25 mm, and a height of 6 mm. The above heat treatment was performed in nitrogen at a temperature of 600°C and a retention time of 45 minutes.

[0121] Winding was performed on the fabricated ring-shaped test specimen (100 turns for the first winding and 20 turns for the second winding), and hysteresis loss was measured using a DC magnetization meter (SK-110 manufactured by Metron Kikensha). Using a DC power source, the magnetization curve at a frequency of 1 Hz and an excitation flux density of 1.0 T was evaluated, and the hysteresis loss at 400 Hz was calculated by multiplying the loop area at 1 Hz by 400. A hysteresis loss of 25 W / kg or less was accepted, and a loss exceeding 25 W / kg was rejected. It is known that the iron loss at 400 Hz is high due to the higher hysteresis loss of the powder core compared to conventional iron cores made of electrical steel sheets. By reducing the hysteresis loss at 400 Hz to 25 W / kg or less, it is possible to achieve an iron loss level equivalent to that of a 0.30 mm thick electrical steel sheet, which is a relatively high-grade product among general-purpose electrical steel sheets. Therefore, it can be particularly suitable for use, for example, as a motor.

[0122] The evaluation results are shown together in Table 1. All powdered magnetic cores made of powder satisfying the requirements of the present invention had a hysteresis loss of 25 W / kg or less and passed the test.

[0123]

Claims

Claim 1 Iron-based soft magnetic powder for compacted magnetic cores having a component composition satisfying at least one of the following: mass concentration, S: 20 ppm or less, Sn and Sb: total 200 ppm or less, and also, S: 10 ppm or less, and Sn and Sb: total 5 ppm or more. Claim 2 Insulated soft magnetic powder for a compacted magnetic core, having an insulating coating on the surface of the particles constituting the iron-based soft magnetic powder for a compacted magnetic core described in claim 1. Claim 3 In paragraph 2, the insulating coating comprises, in this order, a first coating comprising condensed aluminum phosphate and a second coating comprising silicone resin, extending outward from the surface of the particle, an insulating coating soft magnetic powder for a compacted magnetic core. Claim 4 In paragraph 2 or 3, the insulating coating soft magnetic powder for a pressed powder core, wherein the content of the insulating coating is 0.2 to 1.0 parts by mass per 100 parts by mass of the iron-based soft magnetic powder for a pressed powder core. Claim 5 A mixed powder for a powder core comprising an insulating coated soft magnetic powder for a powder core as described in any one of claims 2 to 4, and 0.2 to 0.8 parts by mass of a lubricant per 100 parts by mass of the insulating coated soft magnetic powder for a powder core.