Spherical composite oxide particle material and method for manufacturing the same, slurry composition and transparent resin composition
A spherical composite oxide particle material with controlled alkali metal and crystallinity is manufactured to address transparency and refractive index issues in resin compositions, enhancing their suitability for optoelectronic and optical applications.
Patent Information
- Application Number
- KR1020267037130
- Authority / Receiving Office
- KR · KR
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-04-05
- Publication Date
- 2026-11-17
AI Technical Summary
Existing resin compositions using silica or alumina fillers face challenges in achieving high transparency due to significant refractive index deviations and high alkali metal content, especially when forming composite oxides like mullite, which are not transparent enough for optical applications.
A spherical composite oxide particle material composed of Si and Al with controlled alkali metal content below 20 ppm and crystallinity below 0.5% is manufactured through a deflagration and spheroidization process, ensuring a refractive index of 1.50 ± 0.03 and high circularity.
The solution enhances transparency and refractive index control, making the composite oxide suitable for transparent resin compositions, particularly in optoelectronic devices and optical materials.
Smart Images

Figure PCT00002_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a spherical composite oxide particle material and a method for manufacturing the same, a slurry composition, and a transparent resin composition. Background Technology
[0002] To achieve heat resistance or low thermal expansion of the resin, a resin composition in which a filler made of metal oxide particle material is dispersed is used. When optical properties (transparency) are required along with heat resistance and low thermal expansion as a resin composition, it is necessary to make the refractive index of the dispersed filler close to that of the resin material.
[0003] Silica and alumina are commonly used as metal oxides constituting fillers. The refractive index of silica is 1.46 and the refractive index of alumina is 1.77. When using resin materials with refractive indices that deviate significantly from these, it is difficult to obtain a resin composition with high transparency even if silica or alumina is employed. Therefore, in the prior art, a composite oxide of silica and alumina is formed to control the refractive index to between 1.46 and 1.77 and is used as a filler (Patent Documents 1 and 2).
[0004] Patent Document 1 describes a "manufacturing method comprising the steps of: a step of obtaining an emulsion by mixing raw materials including an aqueous alkali silicate solution, an aluminum compound or an aqueous solution thereof, a surfactant, and an organic solvent in a predetermined ratio; and a step of mixing the emulsion obtained in the mixing step with at least one salt selected from inorganic salts and organic salts" (Claim 9, Paragraph 0007, etc.).
[0005] In Patent Document 2, a mullite composition (Al6O), which is a crystalline complex oxide, is described. 13 A method for producing a composite oxide powder containing mullite by reacting metallic silicon and metallic aluminum mixed in a molar ratio of Si2 with oxygen in a flame is disclosed. Prior art literature
[0006] Japanese Published Patent Application No. 2020-033240, Japanese Public Patent Application No. Hei 07-108766 The problem to be solved
[0007] In the invention of Patent Document 1, since particulate silica is manufactured using an aqueous alkali silicate solution containing an alkali metal as a raw material (see paragraph 0029), the obtained particulate silica contains a large amount of alkali metal.
[0008] In addition, Patent Document 2 aims to manufacture mullite, and since a mixture of mullite, which is a crystalline composite oxide, and an amorphous composite oxide is obtained, it is difficult to say that it has sufficient transparency when adopted as a filler used in a transparent resin composition.
[0009] The present invention has been completed in consideration of the above circumstances, and the problem to be solved is to provide a spherical composite oxide particle material composed of a composite oxide containing Si and Al that has high transparency, a method for manufacturing the same, a slurry composition, and a transparent resin composition. means of solving the problem
[0010] (1) The spherical composite oxide particle material of the present invention that solves the above problem is composed of a composite oxide including Si and Al, and
[0011] Alkali metal content of 20 ppm or less,
[0012] The degree of crystallinity is 0.5% or less.
[0013] By keeping the content of alkali metals such as Na, which are prone to leaching out, at 20 ppm or less, adverse effects caused by alkali metals can be suppressed. In addition, by keeping the degree of crystallinity at 0.5% or less, transparency can be improved when dispersed in a resin material.
[0014] In particular, it is desirable to have the mass of Al be less than 50% based on the mass of Si and Al, the moles of Al be 10% or more based on the moles of Si, the refractive index be 1.50 ± 0.03, the circularity be 0.9 or more, and the volume average particle size be 0.1 μm or more and 20 μm or less.
[0015] (2) And, another spherical composite oxide particle material of the present invention that solves the above problem comprises a preparation process for preparing a raw particle material comprising metallic silicon and metallic aluminum, wherein the alkali metal content is 20 ppm or less, and
[0016] A deflagration and spheroidization process in which the above raw particle material is introduced under a high-temperature oxidizing atmosphere, deflagrated to form an oxide, and then rapidly cooled to spheroidize it into a spherical composite oxide particle material having a crystallinity of 0.5% or less.
[0017] It is a spherical composite oxide particle material that can be manufactured by a method for manufacturing a spherical composite oxide particle material having a spherical composite oxide particle material.
[0018] (3) The method for manufacturing a spherical composite oxide particle material of the present invention that solves the above problem is a method for manufacturing a spherical composite oxide particle material of the present invention, and
[0019] A preparation process for preparing raw particle materials containing metallic silicon and metallic aluminum, with an alkali metal content of 20 ppm or less, and
[0020] A deflagration and spheroidization process in which the above raw particle material is introduced under a high-temperature oxidizing atmosphere, deflagrated to form an oxide, and then rapidly cooled to spheroidize it into a spherical composite oxide particle material having a crystallinity of 0.5% or less.
[0021] have.
[0022] (4) The slurry composition of the present invention that solves the above problem has a spherical composite oxide particle material of the present invention and a dispersion medium that disperses the spherical composite oxide particle material.
[0023] (5) The transparent resin composition of the present invention that solves the above problem has a spherical composite oxide particle material of the present invention and a transparent resin material that disperses the spherical composite oxide particle material. Effects of the invention
[0024] The spherical composite oxide particle material of the present invention can improve transparency when dispersed in a resin material or a dispersion medium by having the above composition. Brief explanation of the drawing
[0025] Figure 1 is the XRD spectrum of each test sample in the example. Specific details for implementing the invention
[0026] The spherical composite oxide particle material of the present invention will be described in detail below based on the embodiments. The spherical composite oxide particle material of the present embodiment can be used as a composition dispersed in a resin material or a dispersion medium. In particular, by making it a transparent resin composition dispersed in a transparent resin material, it can be used for electronic materials such as optoelectronic fusion devices that combine and process optical and electrical signals in logic ICs, analog ICs, etc., optical materials such as lenses, LED encapsulating materials, dental materials, etc.
[0027] (Spherical composite oxide particle material)
[0028] The spherical composite oxide particle material of the present embodiment is composed of an oxide (including a composite oxide) containing Si and Al, and has a crystallinity of 0.5% or less. Regarding the composition ratio of Si and Al, it is preferable that the mass of Al is less than 50% based on the mass of Si and Al, and it is more preferable to adopt 35%, 30%, 27.5%, 25%, and 20% as upper limits.
[0029] In addition, based on the moles of Si, it is preferable that the moles of Al be 10% or more, more preferable that they be 15% or more, and even more preferable that they be 20% or more. These upper and lower limits can be combined arbitrarily. It is preferable that the spherical composite oxide particle material has a uniform composition.
[0030] The spherical composite oxide particle material may include oxides of other metals in addition to oxides of Si and Al. The content of Si and Al is preferably such that, based on the total mass, the lower limit of the mass of the oxides of Si and Al converted to SiO2 and Al2O3 is 85%, 90%, 95%, or 100%.
[0031] The spherical composite oxide particle material preferably has an alkali metal content of 5 ppm or less, 3 ppm or less, and more preferably 1 ppm or less. The alkali metal content is measured by methods such as ICP emission spectroscopic analysis.
[0032] The degree of crystallinity of the spherical composite oxide particle material is preferably 0.5% or less, and more preferably 0.3% or less. The degree of crystallinity is measured by using a spectrum of 5° to 90° measured by XRD (CuKα line), measuring the area of the amorphous region (a) and the area of the crystalline region (40.8°) (b), and calculating it as b / (a + b) × 100 (%).
[0033] The spherical composite oxide particle material preferably has a sphericity of 0.9 or higher, more preferably 0.95 or higher, even more preferably 0.98 or higher, and particularly preferably 0.99 or higher. A higher sphericity tends to improve packing properties and lower the viscosity of the composition when dispersed in a composition. Sphericity is determined by taking an SEM image and using the observed particle area and periphery length as follows: (Sphericity) = {4π × (Area) ÷ (Periphery Length)} 2 It is calculated as a value obtained from}. The closer it is to 1, the closer it is to a perfect ball. Specifically, the average value measured for 100 particles using image analysis software (Asahi Kasei Engineering Co., Ltd.: A. Jokun) is adopted.
[0034] It is preferable that the spherical composite oxide particle material has a refractive index of 1.50 ± 0.03. The refractive index can be controlled by controlling the ratio of Si to Al, and the refractive index can be increased by increasing the amount of Al. It is preferable that all constituent particles of the spherical composite oxide particle material fall within this range, and it is preferable that the range be ±0.02, more preferable that it be ±0.01, and particularly preferable that it be ±0.005.
[0035] The refractive index of the spherical composite oxide particle material is measured by the following method. Multiple levels of mixed solvents with different mixing ratios using two types of solvents with known refractive indices are prepared, and when the particle material is dispersed in these solvents at a concentration of 10 g / L, the refractive index of the mixture at which the mixture is most transparent is taken as the refractive index of the particle material. The refractive indices of the multiple mixed solvents are prepared at intervals of 0.01, based on 1.50.
[0036] It is preferable that the spherical composite oxide particle material has a volume average particle size of 0.1 μm or more and 20 μm or less. Examples of upper limits for the volume average particle size include 20 μm, 10 μm, and 5 μm, and examples of lower limits include 0.1 μm, 0.5 μm, and 1.0 μm. These upper and lower limits can be arbitrarily combined. It is preferable that the spherical composite oxide particle material is dispersed down to the primary particles.
[0037] The spherical composite oxide particle material may be surface-treated. Examples of surface treatment agents include organosilicon compounds. Additionally, organoaluminum compounds and organotitanium compounds may be used. Examples of organosilicon compounds include silane compounds such as silane coupling agents and silane residues. Examples of silane compounds include compounds having an alkoxy group, a phenyl group, a vinyl group, an epoxy group, a methacrylic group, an amino group, a ureido group, a mercapto group, an isocyanate group, or an acrylic group.
[0038] The amount of surface treatment agent bonded to the surface is not specifically limited, and an amount such as 100%, 75%, 50%, 25%, etc. can be selected based on the amount of OH groups present on the surface of the spherical composite oxide particle material. An excess amount exceeding 100% (120%, 150%, etc.) can also be selected.
[0039] (Method for manufacturing spherical composite oxide particle material)
[0040] The method for manufacturing a spherical composite oxide particle material of the present embodiment is a method for manufacturing a spherical composite oxide particle material of the present embodiment, and comprises a preparation process, a deflagration spheroidization process, and other processes that can be selected as necessary.
[0041] · Preparation process
[0042] This process is a process for preparing raw particle materials. The raw particle material is a particle material containing metallic silicon and metallic aluminum, and is a mixture of separate particle materials of metallic silicon and metallic aluminum, or a particle material composed of an alloy of metallic silicon and metallic aluminum. Since the purity of the raw particle material affects the purity of the spherical composite oxide particle material manufactured as is, the purity of the raw particle material is adjusted to the required purity.
[0043] Metallic silicon or metallic aluminum can be melted and converted into a particle material by an atomizer or by a grinding operation. The abundance ratio of metallic silicon and metallic aluminum contained in the raw particle material can be approximately the same as the abundance ratio of Si and Al contained in the spherical composite oxide particle material being manufactured. The particle size of the raw particle material is not particularly limited, but can be approximately 0.1 μm to 40 μm.
[0044] In addition, the raw particle material may undergo surface treatment. By performing surface treatment, the aggregation of the raw particle material can be suppressed when introduced under the high-temperature oxidizing atmosphere described later. Examples of surface treatments include organosilicon compounds such as silane compounds, organoaluminum compounds such as aluminate coupling agents, and organotitanium compounds such as titanate coupling agents.
[0045] · Explosive spheroidization process
[0046] This process involves introducing raw particle materials under a high-temperature oxidizing atmosphere and is a method also known as the so-called VMC method. As a result, the raw particle materials become oxides through a deflagration reaction. The obtained oxides fall due to gravity or the like and are rapidly cooled away from the high-temperature oxidizing atmosphere to obtain spherical composite oxide particle materials. The obtained spherical composite oxide particle materials can be recovered by a bag filter or a cyclone.
[0047] A high-temperature oxidizing atmosphere can be exemplified by a flame formed by burning a combustible gas in an oxidizing atmosphere. A high-temperature oxidizing atmosphere can be formed within a suitable furnace. Examples of combustible gases include hydrocarbon gases such as methane, propane, and butane, as well as hydrogen and ammonia. An oxidizing atmosphere (combustion-supporting gas) can be realized using oxygen gas or air. The amount of oxygen in the oxidizing atmosphere can be 1.0 times or more, 1.1 times or more, 1.2 times or more, 1.3 times or more, 1.4 times or more, 1.5 times or more, 1.75 times or more, or 2.0 times or more, based on the stoichiometric amount of oxygen required to oxidize raw particle materials and combustible gases.
[0048] It is preferable to introduce the raw particle material by dispersing it in a carrier gas. Examples of carrier gases include air or nitrogen gas. The concentration at which the raw particle material is dispersed in the carrier gas is 0.3 kg / Nm³. 3 ~ 8 kg / Nm 3 You can do it to that extent.
[0049] · Other processes
[0050] After the deflagration spheroidization process, other processes selected as necessary, such as a surface treatment process or a classification process, may be included. If these processes are not particularly necessary, their timing is irrelevant.
[0051] · Surface treatment process
[0052] The surface treatment process is a process of surface treating spherical composite oxide particle materials with a surface treatment agent such as an organosilicon compound, an organoaluminum compound, or an organotitanium compound. Surface treatment is performed by directly contacting the surface treatment agent (either in liquid or gaseous form) with the surface treatment agent, or by contacting the surface treatment agent while it is dissolved in a solvent. After performing surface treatment, heating may be used to promote the reaction between the surface treatment agent and the surface of the spherical composite oxide particle material.
[0053] The surface treatment agent is not particularly limited. Examples of surface treatment agents include those having a phenyl group, an alkyl group, a vinyl group, a methacrylic group, an epoxy group, a phenylamino group, an amino group, a styryl group, etc.
[0054] The amount of surface treatment agent used for surface treatment is not particularly limited, and an amount such as 100%, 75%, 50%, or 25% can be selected based on the amount of OH groups present on the surface of the spherical composite oxide particle material. An excess amount exceeding 100% (120%, 150%, etc.) can also be selected.
[0055] · Classification process
[0056] The classification process is a process of performing classification operations on manufactured spherical composite oxide particle materials to achieve a desired particle size distribution or to remove coarse particles. Classification operations include sieving using a sieve with an appropriate mesh size, centrifugation in an appropriate dispersion medium, or sedimentation classification. Suitable dispersion media include gases such as air, and liquids such as organic solvents or water as exemplified in the slurry composition described later. By using a liquid as the dispersion medium, it becomes possible to remove impurities contained in the spherical composite oxide particle materials after they have been transferred into the dispersion medium, thereby reducing the amount of impurities. The classification operation can be repeated until the desired particle size distribution is achieved. Additionally, in the classification process, the particle size distribution can be adjusted by mixing the spherical composite oxide particle materials that have been adjusted to different particle size distributions through the classification operation.
[0057] (Slurry composition)
[0058] The slurry composition of the present embodiment is a composition in which the spherical composite oxide particle material of the present embodiment is dispersed in a dispersion medium such as an organic solvent. The organic solvent is not particularly limited, but examples of organic solvents include methanol, ethanol, isopropanol, propylene glycol, propylene glycol monomethyl ether, propylene glycol monomethyl acetate, ethyl acetate, toluene, hexane, THF, ethyl methyl ketone, methyl isobutyl ketone, cyclohexanone, dimethylacetamide, dimethylformamide, acetic acid, and oleic acid.
[0059] The mixing ratio of the spherical composite oxide particle material and the organic solvent is not particularly limited as long as fluidity is maintained, but for example, the mass ratio of (particle material) : (organic solvent) can be set to approximately 5 : 95 to 85 : 15. The slurry composition of the present embodiment may be used to supply particle material when mixing with resin material, other particle material, etc., or it may be used to apply particle material by drying the organic solvent after applying it to a target area.
[0060] (Transparent resin composition)
[0061] The transparent resin composition of the present embodiment is a composition in which the spherical composite oxide particle material of the present embodiment is dispersed in a transparent resin material. As the transparent resin material, polymer compounds capable of melting by heating, polymer compounds after curing, polymer precursors capable of curing by reaction, etc. may be employed, and although not particularly limited, examples include acrylic resin, silicone resin, epoxy resin, urea resin, polyester resin, polyimide resin, LCP resin (liquid crystal resin), COC resin (cyclic olefin copolymer), and fluoropolymer.
[0062] The mixing ratio of the spherical composite oxide particle material and the resin material is not particularly limited as long as fluidity is maintained, but for example, the mass ratio of (particle material) : (resin material) can be set to approximately 5 : 95 (lower limit) to 90 : 10 (upper limit), and as a lower limit, it can be set to 10 : 90, 20 : 80, 30 : 70, 40 : 60, 50 : 50, 60 : 40, 70 : 30, or 80 : 20. In addition to being usable for some or all of the semiconductor encapsulation material, the resin composition of the present embodiment can be used for some or all of the substrate material.
[0063] Examples
[0064] The spherical composite oxide particle material of the present invention and the method for manufacturing the same will be described in detail below based on examples.
[0065] <Example 1>
[0066] A raw particle material was prepared by mixing metallic silicon powder with an average particle size of 20 μm and a purity of 99% or higher, and metallic aluminum powder with an average particle size of 20 μm and a purity of 99% or higher, in a mass ratio of Si : Al = 60 : 40 (preparation process).
[0067] This raw particle material was introduced into a flame acting as a high-temperature oxidizing atmosphere formed in a furnace (volume 0.4 to 5 kL) using propane gas as a combustible gas and air as a combustion-supporting gas. The raw particle material was 1500 g / Nm³ in air as a carrier gas. 3 0.4 Nm at a concentration 3 It was supplied at a rate of / h (10 g / min). The obtained spherical composite oxide particle material was recovered using a bag filter and used as the test sample for this example. In addition, the ratio of the amount of O2 introduced into the furnace to the theoretical amount of O2 required for combustion and oxidation was set to 1.0 to 2.0 times.
[0068] <Example 2>
[0069] A spherical composite oxide particle material was prepared in the same manner as in Example 1, except that the raw particle material was changed to Si : Al = 70 : 30, and this was used as a test sample for this example.
[0070] <Example 3>
[0071] A spherical composite oxide particle material was prepared in the same manner as in Example 1, except that the raw particle material was changed to Si : Al = 74 : 26, and this was used as a test sample for this example.
[0072] <Example 4>
[0073] A spherical composite oxide particle material was prepared in the same manner as in Example 1, except that the raw particle material was changed to Si : Al = 76 : 24, and this was used as a test sample for this example.
[0074] <Example 5>
[0075] A spherical composite oxide particle material was prepared in the same manner as in Example 1, except that the raw particle material was changed to Si : Al = 80 : 20, and this was used as a test sample for this example.
[0076] <Comparative Example 1>
[0077] A spherical composite oxide particle material was prepared in the same manner as in Example 1, except that the raw particle material was changed to Si : Al = 40 : 60, and this was used as a test sample for the comparative example.
[0078] <Comparative Example 2>
[0079] A spherical composite oxide particle material was prepared in the same manner as in Example 1, except that the raw particle material was changed to Si : Al = 25 : 75, and this was used as a test sample for the comparative example.
[0080] <Comparative Example 3>
[0081] A spherical composite oxide particle material was prepared in the same manner as in Example 1, except that the raw particle material was changed to Si : Al = 15 : 85, and this was used as a test sample for the comparative example.
[0082] <Comparative Example 4>
[0083] Particulate silica was prepared by the method of Example 1 of Patent Document 1 and used as a test sample for the present comparative example.
[0084] <Comparative Example 5>
[0085] A dispersion was prepared by dispersing the test sample of Comparative Example 4 in ion-exchanged water at a concentration of 20 mass%, and then particulate silica with water-soluble impurities removed was obtained by removing the dispersion medium using a centrifuge. Afterward, it was dried to be used as the test sample of the present Comparative Example.
[0086] <Evaluation Method>
[0087] · Refractive index
[0088] When particles were dispersed in a mixture of two types of solvents with known refractive indices, the refractive index of the mixture at the point where the transparency of the mixture was highest was taken as the refractive index of the particles.
[0089] · Degree of crystallization
[0090] XRD measurements were performed using the SmartLab X-ray diffraction apparatus manufactured by Rigaku, and the ratio of amorphous to crystalline phases was calculated. For reference, the XRD spectra for Examples 1-5 and Comparative Examples 1-5 are shown in Fig. 1. As is evident from Fig. 1, in Comparative Example 1-3, a peak corresponding to the crystal exists at 40.8°, indicating a higher degree of crystallinity than in the Examples. Additionally, in Fig. 1, the horizontal axis is 2θ (°) and the vertical axis is intensity (arbitrary unit).
[0091] · Al (mol%) and Si (mol%)
[0092] 6.0 to 6.1 g of test samples from each example and comparative example were placed in a cell and calculated using a fluorescence X-ray analyzer (Supermini200, manufactured by Rigaku). From the measurement results, the percentage of the moles of Al based on the moles of Si was calculated as Al (mol%) / Si (mol%) × 100 (%).
[0093] · Circular equivalent diameter (grain diameter), circularity
[0094] Photos were taken with an SEM, and the average value measured for more than 100 particles was adopted using image analysis software (Asahi Kasei Engineering Co., Ltd.: A-Jokun).
[0095] · Average particle size
[0096] The volume average particle size was measured using a laser diffraction particle size measuring device (Malvern Panalytica, Mastersizer 3000), and D50 was set as the average particle size.
[0097] · Alkali metal content
[0098] The alkali metal content was measured by ICP emission spectroscopy. As a result, since the values were below the detection limit for all metals except Na, the value for the Na content was measured.
[0099] The above results are shown in Table 1.
[0100]
[0101] As is evident from Table 1, in the test samples of the examples, transparency was sufficient and the refractive index could be measured by making the mass of Al 45% or less (less than 50%) based on the sum of the masses of metallic aluminum (Al) and metallic silicon (Si), whereas in the test samples of Comparative Examples 1 to 3, transparency was insufficient and the refractive index could not be measured because the degree of crystallization was high.
[0102] In addition, the refractive index could be increased by increasing the proportion of Al. Also, the particulate silica of Example 1 of Patent Document 1 (Comparative Example 4) had a lower degree of crystallinity than Comparative Examples 1-3, so the refractive index could be measured, but the circularity was low and the Na content was high. Also, the test sample of Comparative Example 5 was the test sample of Comparative Example 4 washed with water, but the Na content was still high, making it difficult to remove Na.
Claims
Claim 1 A spherical composite oxide particle material composed of a composite oxide containing Si and Al, having an alkali metal content of 20 ppm or less and a degree of crystallinity of 0.5% or less. Claim 2 A spherical composite oxide particle material according to claim 1, wherein the mass of Al is less than 50% based on the mass of Si and Al, the moles of Al are 10% or more based on the moles of Si, the refractive index is 1.50 ± 0.03, the circularity is 0.9 or more, and the volume average particle size is 0.1 μm or more and 20 μm or less. Claim 3 A spherical composite oxide particle material that can be manufactured by a method for manufacturing a spherical composite oxide particle material comprising: a preparation process for preparing a raw particle material containing metallic silicon and metallic aluminum and having an alkali metal content of 20 ppm or less; and a deflagration and spheroidization process for introducing the raw particle material under a high-temperature oxidizing atmosphere, deflagrating it to form an oxide, and then rapidly cooling it to spheroidize it into a spherical composite oxide particle material having a crystallinity of 0.5% or less. Claim 4 A spherical composite oxide particle material according to claim 1 or 3, wherein the mass of Al is less than 50% based on the masses of Si and Al. Claim 5 A spherical composite oxide particle material having a refractive index of 1.50 ± 0.03 in any one of claims 1, 3, and 4. Claim 6 A spherical composite oxide particle material according to any one of claims 1, 3 to 5, wherein the molar content of Al is 10% or more based on the molar content of Si. Claim 7 A spherical composite oxide particle material having a circularity of 0.9 or higher, in any one of claims 1, 3 to 6. Claim 8 A spherical composite oxide particle material according to any one of claims 1, 3 to 7, having a volume average particle size of 0.1 μm or more and 20 μm or less. Claim 9 A spherical composite oxide particle material surface-treated with an organosilicon compound, in any one of claims 1 to 8. Claim 10 A slurry composition having a spherical composite oxide particle material described in any one of claims 1 to 9, and a dispersion medium for dispersing the spherical composite oxide particle material. Claim 11 A transparent resin composition having a spherical composite oxide particle material described in any one of claims 1 to 9, and a transparent resin material for dispersing said spherical composite oxide particle material. Claim 12 A method for manufacturing a spherical composite oxide particle material according to any one of claims 1 to 9, comprising: a preparation process for preparing a raw particle material containing metallic silicon and metallic aluminum and having an alkali metal content of 20 ppm or less; and a deflagration and spheroidization process for introducing the raw particle material under a high-temperature oxidizing atmosphere, deflagrating it to form an oxide, and then rapidly cooling it to spheroidize it into a spherical composite oxide particle material having a crystallinity of 0.5% or less.