Quartz Crystal Microbalance Sensor

The quartz crystal oscillator sensor with aluminum electrodes and chromium layers addresses low deposition power and rate variation for lithium, enhancing deposition stability and productivity in thin film processes.

KR1020260164321APending Publication Date: 2026-11-17OTWOCOM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
KR1020250060528
Authority / Receiving Office
KR · KR
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing quartz crystal oscillator sensors face challenges with low deposition power and high deposition rate variation for light metals like lithium, leading to prolonged initial stabilization times and reduced productivity in thin film deposition processes.

Method used

A quartz crystal oscillator sensor with aluminum electrodes and chromium surface modification layers is developed, enhancing deposition power and reducing deposition rate variation by stabilizing the sensor's frequency changes during lithium deposition.

Benefits of technology

The sensor improves lithium deposition power, shortens initial stabilization time, and reduces deposition rate dispersion, enabling precise monitoring and increased productivity in thin film deposition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PAT00002_ABST
    Figure PAT00002_ABST
Patent Text Reader

Abstract

The present invention provides a quartz oscillator sensor comprising: a quartz plate; a first electrode formed on one side of the quartz plate; a second electrode formed on the other side of the quartz plate; and a first surface modification layer formed on the first electrode, wherein the first electrode and the second electrode comprise aluminum (Al) and the first surface modification layer comprises chromium (Cr). The quartz oscillator sensor according to the present invention can improve the deposition power of light metals such as lithium and shorten the initial stabilization time of deposition, as well as reduce deposition rate variation.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a quartz crystal oscillator sensor, and more specifically, to a quartz crystal oscillator sensor capable of improving the deposition power of light metals such as lithium, shortening the initial stabilization time of deposition, and reducing deposition rate variation. Background Technology

[0002] A crystal oscillator vibrates when voltage is applied and generates frequency through this vibration; since it can obtain a stable frequency, it is used in various technical fields such as computers, communication devices, and measuring instruments.

[0003] For example, a sensor using a quartz crystal oscillator can be used in vacuum deposition, which is mainly used in semiconductor processes, that is, in the process of depositing sources such as metal materials like aluminum, dielectrics such as oxides, sulfides, and nitrides, precious metals such as gold, silver, platinum, and palladium, or rare earth elements onto a semiconductor substrate, and can also be used in the manufacture of display devices such as organic light emitting display devices (OLEDs).

[0004] Such a crystal oscillator sensor is placed within the internal space of a chamber constituting a thin film deposition equipment, and when a thin film deposition process is performed on a substrate within the internal space of the chamber, the thickness or deposition rate of the thin film deposited on the substrate can be measured by utilizing the phenomenon in which the vibration (frequency) of the crystal oscillator changes according to the change in mass of the crystal oscillator when a deposition material is deposited on the surface of the sensor.

[0005] Figure 1 is a cross-sectional view of a conventional crystal oscillator sensor, and the conventional crystal oscillator sensor will be described with reference thereto.

[0006] As shown in FIG. 1, a conventional crystal oscillator sensor comprises a crystal plate (10), a first electrode (20), and a second electrode (30).

[0007] At this time, the electrode is often made of gold (Au) in terms of chemical stability or electrical conductivity, but light metals such as magnesium (Mg) or lithium (Li) have a significantly low deposition rate on the surface of the gold electrode, and also have the disadvantage that cracks easily occur as stress is applied as the deposition material is deposited on the surface.

[0008] Korean Patent Publication No. 10-2014-0146827 discloses a crystal sensor that improves deposition power on a magnesium electrode by including a crystal plate; a gold electrode disposed on the crystal plate and coated with gold, and a tin (Sn) buffer layer deposited on one side of the gold electrode.

[0009] However, when lithium is used as the deposition material, the above sensor has a problem in that the initial stabilization time of deposition is long and the dispersion of the deposition rate is large, resulting in reduced productivity and difficulty in precise monitoring of the deposition. Prior art literature

[0010] Republic of Korea Published Patent No. 10-2014-0146827 The problem to be solved

[0011] One objective of the present invention is to provide a crystal oscillator sensor capable of improving the deposition power of light metals such as lithium, shortening the initial stabilization time of deposition, and reducing deposition rate variation. means of solving the problem

[0012] On the other hand, the present invention provides a quartz oscillator sensor comprising: a quartz plate; a first electrode formed on one side of the quartz plate; a second electrode formed on the other side of the quartz plate; and a first surface modification layer formed on the first electrode, wherein the first electrode and the second electrode comprise aluminum (Al) and the first surface modification layer comprises chromium (Cr).

[0013] In one embodiment of the present invention, the crystal oscillator sensor may detect the deposition of lithium.

[0014] In one embodiment of the present invention, the thickness of the first electrode and the second electrode may each independently be 8,000 to 15,000 Å.

[0015] In one embodiment of the present invention, the first electrode and the second electrode may have a double-layer structure comprising an aluminum layer containing aluminum and a chromium layer formed below the aluminum layer.

[0016] In one embodiment of the present invention, the thickness of the first surface modification layer may be 50 to 1,500 Å.

[0017] In one embodiment of the present invention, the crystal oscillator sensor may further include a second surface modification layer formed on the second electrode.

[0018] In one embodiment of the present invention, the thickness of the second surface modification layer may be 50 to 1,500 Å. Effects of the invention

[0019] The quartz oscillator sensor according to the present invention can improve the deposition power of light metals such as lithium and shorten the initial stabilization time of deposition, as well as reduce deposition rate variation, so it can be effectively used in a thin film deposition monitoring device. Brief explanation of the drawing

[0020] Figure 1 is a cross-sectional view of a conventional crystal oscillator sensor. FIG. 2 is a cross-sectional view of a crystal oscillator sensor according to one embodiment of the present invention. FIG. 3 is a cross-sectional view of a crystal oscillator sensor according to another embodiment of the present invention. Specific details for implementing the invention

[0021] The present invention will be described in more detail below with reference to the attached drawings.

[0023] FIG. 2 is a cross-sectional view of a crystal oscillator sensor according to one embodiment of the present invention.

[0024] Referring to FIG. 2, a crystal oscillator sensor according to one embodiment of the present invention comprises a crystal plate (100), a first electrode (200) formed on one side of the crystal plate (100), a second electrode (300) formed on the other side of the crystal plate, and a first surface modification layer (400) formed on the first electrode (200).

[0026] In addition, the first electrode and the second electrode contain aluminum (Al), and the first surface modification layer contains chromium (Cr).

[0028] A quartz crystal oscillator sensor according to one embodiment of the present invention can improve the deposition rate of light metals such as lithium and shorten the initial stabilization time of deposition, as well as reduce the dispersion of the deposition rate, by forming a surface modification layer containing chromium on an electrode containing aluminum.

[0030] Since the vibration frequency of the above-mentioned modified plate (100) changes before and after the deposition of the material, the deposition thickness and deposition rate of the material can be calculated through the amount of change in the vibration frequency of the modified crystal.

[0032] The first electrode (200) is formed on one side of the modification plate (100), and the second electrode (300) is formed on the other side of the modification plate (100), and the first electrode (200) and the second electrode (300) can be formed to be in direct contact with the modification plate (100).

[0034] The first electrode (200) and the second electrode (300) may include aluminum (Al) to prevent cracks from occurring in the electrode or crystal plate during the deposition process, and the electrode thickness may be formed thickly to 8,000 to 15,000 Å, preferably 8,000 to 13,000 Å to improve the durability of the crystal oscillator.

[0036] The first electrode (200) and the second electrode (300) may have a double-layer structure comprising an aluminum layer containing aluminum and a chromium layer formed below the aluminum layer.

[0037] The above chrome layer can act as a bonding layer between the modification plate and the aluminum layer.

[0039] The first surface modification layer (400) is formed on the first electrode (200) and can be formed to be in direct contact with the first electrode (200).

[0040] The first surface modification layer (400) can improve the deposition power of light metals such as lithium, including chromium (Cr), and can shorten the initial stabilization time of deposition as well as reduce the dispersion of the deposition rate.

[0042] In one embodiment of the present invention, the thickness of the first surface modification layer (400) may be 50 to 1,500 Å. If the thickness of the first surface modification layer (400) is less than 50 Å, the effect of improving the deposition power of light metals such as lithium is negligible, and if it exceeds 1,500 Å, the lifespan of the sensor is reduced and it may be difficult to maintain stable performance for a long period of time.

[0044] A crystal oscillator sensor according to one embodiment of the present invention may further include a second surface modification layer (500) formed on the second electrode (300), as shown in FIG. 3.

[0045] The second surface modification layer (500) can be formed to be in direct contact with the second electrode (300).

[0046] When a second surface modification layer (500) is formed on the second electrode (300), double-sided deposition is performed, thereby maintaining the physical and chemical balance of the electrode and stably maintaining the frequency change characteristics.

[0047] The thickness of the second surface modification layer (500) may be the same as or different from the thickness of the first surface modification layer (400).

[0049] A quartz crystal oscillator sensor according to one embodiment of the present invention can accurately measure the deposition amount of a light metal such as lithium, and thereby calculate the deposition thickness and deposition rate. Accordingly, it can be used in thin film deposition equipment for manufacturing organic light emitting display devices (OLEDs) to improve productivity and improve the quality of the thin film.

[0051] The present invention will be explained more specifically below through examples, comparative examples, and experimental examples. These examples, comparative examples, and experimental examples are intended solely to illustrate the present invention, and it is obvious to those skilled in the art that the scope of the present invention is not limited thereto.

[0053] Example 1: Fabrication of a Crystal Oscillator Sensor

[0054] A first electrode with a thickness of 11,000 Å was formed on one side of a quartz plate with a thickness of 0.28 mm using aluminum (Al), and a second electrode with the same thickness as the first electrode was formed on the other side using aluminum. Subsequently, a first surface modification layer with a thickness of 200 Å was formed on the first electrode using chromium to fabricate a quartz oscillator sensor.

[0056] Example 2: Fabrication of a Crystal Oscillator Sensor

[0057] A quartz oscillator sensor was fabricated in the same manner as in Example 1, except that a second surface modification layer with a thickness of 500 Å was further formed using chromium on the second electrode.

[0059] Comparative Example 1: Fabrication of a Crystal Oscillator Sensor

[0060] A quartz crystal oscillator sensor was fabricated in the same manner as in Example 1, except that a surface modification layer was not formed.

[0062] Comparative Example 2: Fabrication of a Crystal Oscillator Sensor

[0063] A quartz crystal oscillator sensor was fabricated in the same manner as in Example 1, except that a first surface modification layer was formed on the first electrode using tin (Sn) instead of chromium.

[0065] Comparative Example 3: Fabrication of a Crystal Oscillator Sensor

[0066] A first electrode with a thickness of 2,000 Å was formed using gold (Au) on one side of a quartz plate with a thickness of 0.28 mm, and a second electrode with a thickness of 2,000 Å was formed using gold (Au) on the other side. Subsequently, a first surface modification layer with a thickness of 200 Å was formed using chromium on the first electrode to fabricate a quartz oscillator sensor.

[0068] Experimental Example 1:

[0069] A deposition process was performed to deposit lithium (Li) using the crystal oscillator sensors fabricated in the above examples and comparative examples, and the time required until the deposition rate reached 1 Å / s was measured as the initial stabilization time (T). The deposition process was then carried out for 30 minutes after the initial stabilization time (T) to measure the dispersion of the deposition rate.

[0071] Initial stabilization time (T) Deposition rate dispersion Example 1 20 minutes 2 % Example 2 15 minutes 3 % Comparative Example 1 45 minutes 6.5 % Comparative Example 2 35 minutes 9 % Comparative Example 3 1 hour 11 %

[0073] As shown in Table 1 above, it can be confirmed that the crystal oscillator sensors of Examples 1 and 2, which include an aluminum electrode and a chrome surface modification layer, not only have a short initial stabilization time but also a reduced deposition rate dispersion value.

[0074] On the other hand, it can be seen that the crystal oscillator sensors of Comparative Examples 1 to 3, which do not include a chrome surface modification layer or an aluminum electrode, take a long time to stabilize initially or have large dispersion values ​​of deposition rates.

[0076] As specific parts of the present invention have been described in detail above, it is evident to those skilled in the art that such specific descriptions are merely preferred embodiments and do not limit the scope of the present invention. Those skilled in the art will be able to make various applications and modifications within the scope of the present invention based on the above description.

[0077] Accordingly, the substantial scope of the present invention shall be defined by the appended claims and their equivalents. Explanation of the symbols

[0078] 10, 100: Modification Plate 20, 200: First electrode 30, 300: Second electrode 400: First surface modification layer 500: Second surface modification layer

Claims

Claim 1 A quartz oscillator sensor comprising: a quartz plate; a first electrode formed on one side of the quartz plate; a second electrode formed on the other side of the quartz plate; and a first surface modification layer formed on the first electrode, wherein the first electrode and the second electrode comprise aluminum (Al) and the first surface modification layer comprises chromium (Cr). Claim 2 In claim 1, a crystal oscillator sensor for detecting lithium deposition. Claim 3 A crystal oscillator sensor according to claim 1, wherein the thickness of the first electrode and the second electrode are each independently 8,000 to 15,000 Å. Claim 4 In claim 1, the first electrode and the second electrode are a double-layer structure comprising an aluminum layer containing aluminum and a chromium layer formed below the aluminum layer, a crystal oscillator sensor. Claim 5 A crystal oscillator sensor according to claim 1, wherein the thickness of the first surface modification layer is 50 to 1,500 Å. Claim 6 A crystal oscillator sensor according to claim 1, further comprising a second surface modification layer formed on the second electrode. Claim 7 A crystal oscillator sensor according to claim 6, wherein the thickness of the second surface modification layer is 50 to 1,500 Å.