Near-infrared cut filter and use thereof

A near-infrared cut filter with a resin layer of specific pigments and a dielectric multilayer film addresses fluorescence and flare issues, ensuring high-quality camera images by enhancing absorption and reducing angle dependence.

KR1020260164489APending Publication Date: 2026-11-17제이에스알 가부시키가이샤
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
KR1020260080877
Authority / Receiving Office
KR · KR
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-05-06
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing near-infrared cut filters generate fluorescence and flare when using π-electron conjugated dyes, particularly in high-sensitivity camera sensors, leading to image defects.

Method used

A near-infrared cut filter with a resin layer containing two or more types of pigments with specific absorption characteristics and low luminescence quantum yields, combined with a dielectric multilayer film, to enhance absorption and reduce fluorescence.

Benefits of technology

The filter provides excellent near-infrared absorption and suppresses fluorescence, resulting in high-quality camera images with reduced flare and improved color reproduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PAT00016_ABST
    Figure PAT00016_ABST
Patent Text Reader

Abstract

Providing a near-infrared cut filter that has excellent near-infrared absorption characteristics and can also suppress fluorescence to a low level even when absorbing light. A near-infrared cut filter having a substrate including a resin layer, wherein the resin layer comprises a resin and two or more pigments (A), and each of the two or more pigments (A) independently has an absorption maximum wavelength at 650 to 820 nm and has a luminescence quantum yield of less than 22%, and the resin layer substantially does not contain a pigment (B) having an absorption maximum wavelength at 650 to 820 nm and has a luminescence quantum yield of 22% or more, and wherein the maximum value of the transmittance when measured from the vertical direction of the substrate in a region of 700 to 750 nm is 2.0% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a near-infrared cut filter and its uses. Background Technology

[0002] Solid-state imaging devices, such as smartphone cameras, use CCD or CMOS image sensors, which are solid-state imaging elements for color images. In these solid-state imaging elements, silicon photodiodes that are sensitive to near-infrared rays, which cannot be detected by the human eye, are used in the light-receiving part.

[0003] For example, in solid-state image sensors, it is necessary to perform visual sensitivity correction to create colors that look natural to the human eye, and optical components that selectively transmit or cut light in a specific wavelength range, particularly near-infrared cut filters, are often used.

[0004] As such near-infrared cut filters, those manufactured by various methods have been used in the past. For example, Patent Documents 1 to 4 disclose a near-infrared cut filter having a superior viewing angle compared to that which uses only a conventional near-infrared reflective film by having a resin layer comprising a resin and a plurality of near-infrared absorbing agents. Prior art literature

[0005] International Publication No. 2013 / 054864, International Publication No. 2015 / 025779, Japanese Patent Publication No. 2019-164269, Japanese Patent Publication No. 2021-134350 The problem to be solved

[0006] However, while the near-infrared cut filters described in Patent Documents 1 to 4 were able to achieve an excellent viewing angle by using a near-infrared absorber, there were cases where fine fluorescence generated when the near-infrared absorber, particularly a π-electron conjugated dye such as a squaryllium-based compound, absorbed light entered the solid-state image sensor, causing image defects such as flare. In particular, this problem tended to become more pronounced when using high-sensitivity camera sensors of recent years, and rapid improvement was required to obtain excellent camera images.

[0007] The present invention has been made in consideration of the above and aims to provide a near-infrared cut filter having excellent near-infrared absorption characteristics and capable of suppressing the emission of pigments, particularly fluorescence, to a low level even when light is absorbed. means of solving the problem

[0008] As a result of careful consideration to solve the above problem, the inventor discovered that the above problem can be solved according to the following configuration example, and thus completed the present invention.

[0009] Examples of the configuration of the present invention are as follows.

[0010] In addition, in the present invention, the notation “A to B,” etc., indicating a numerical range is synonymous with “A or more, B or less,” and includes A and B within that numerical range. Furthermore, in the present invention, wavelength A to B nm indicates a characteristic at a wavelength resolution of 1 nm in a wavelength range of wavelength A nm or more and wavelength B nm or less.

[0011] [1] A substrate having a resin layer,

[0012] The above resin layer comprises a resin and two or more types of pigments (A), and

[0013] The above two or more types of pigments (A) each independently have an absorption maximum wavelength at a wavelength of 650 to 820 nm and are pigments with a luminescence quantum yield of less than 22%,

[0014] The above resin layer has an absorption maximum wavelength at 650 to 820 nm and also substantially does not contain a pigment (B) having a luminescence quantum yield of 22% or more, and

[0015] In the region where the above-mentioned material has a wavelength of 700 to 750 nm, the maximum transmittance when measured from the vertical direction of the material is 2.0% or less,

[0016] Near-infrared cut filter.

[0017] [2] Among the above two or more types of pigments (A), let pigment (A) with the shortest wavelength of maximum absorption be pigment (A1) and pigment (A) with the longest wavelength of maximum absorption be pigment (A2).

[0018] The dye (A1) has an absorption maximum wavelength (λ1) (nm) at a wavelength of 650 to 760 nm, and

[0019] The dye (A2) has an absorption maximum wavelength (λ2) (nm) at a wavelength of 730 to 820 nm, and

[0020] A near-infrared cut filter described in claim [1], having a difference in absorption maximum wavelength (|λ2-λ1|) of 10 to 110 nm.

[0021] [3] A near-infrared cut filter having a dielectric multilayer film as described in [1] or [2].

[0022] [4] An optical element having a near-infrared cut filter as described in any one of claims [1] to [3].

[0023] [5] A camera module having a near-infrared cut filter as described in any one of claims [1] to [3]. Effects of the invention

[0024] According to the present invention, a near-infrared cut filter having excellent near-infrared absorption characteristics and capable of suppressing fluorescence to a low level even when absorbing light can be provided.

[0025] As described above, according to the present invention, a near-infrared cut filter having the above characteristics can be provided, thereby obtaining a good image with less flare. In addition, when the filter is a filter having a dielectric multilayer film, the dependence on the angle of incidence by the dielectric multilayer film can be reduced, thereby obtaining a good image. Brief explanation of the drawing

[0026] Figure 1 is an explanatory diagram of the captured images in the flare evaluation of the examples and comparative examples. Figure 2 is a spectral transmittance curve of the substrate obtained in Examples 1 and 2. Figure 3 is the spectral transmittance curve of the near-infrared cut filter obtained in Example 1. Figure 4 is the spectral transmittance curve of the substrate obtained in Example 3. Figure 5 is the spectral transmittance curve of the substrate obtained in Example 4. Figure 6 is the spectral transmittance curve of the substrate obtained in Example 6. Figure 7 is the spectral transmittance curve of the substrate obtained in Comparative Example 1. Figure 8 is the spectral transmittance curve of the substrate obtained in Comparative Example 2. Figure 9 is the spectral transmittance curve of the substrate obtained in Comparative Example 3. Figure 10 is the spectral transmittance curve of the substrate obtained in Comparative Example 4. Figure 11 is the spectral transmittance curve of the substrate obtained in Comparative Example 5. Figure 12 is the spectral transmittance curve of the substrate obtained in Comparative Example 6. Specific details for implementing the invention

[0027] The present invention will be described in detail below.

[0028] ≪Near-infrared cut filter, material≫

[0029] The near-infrared cut filter of the present invention (hereinafter also referred to as "the filter") has a substrate comprising a resin layer (hereinafter also referred to as "the resin layer"). Furthermore, in this specification, the term "substrate" refers to an embodiment prior to the formation of a dielectric multilayer film, and the dielectric multilayer film is not included in the substrate. Additionally, other layers, etc., stacked after the formation of the dielectric multilayer film are not included in the substrate.

[0030] The above-described material has a maximum transmittance of 2.0% or less when measured from the vertical direction of the material in the wavelength range of 700 to 750 nm, preferably 1.5% or less, and more preferably 1.2% or less. Using a near-infrared cut filter having such a material is desirable because it has excellent near-infrared absorption characteristics and can suppress fluorescence to a low level even when light is absorbed, thereby enabling the acquisition of camera images with high reproducibility of black (where black does not appear reddish) even in environments where the influence of near-infrared is strong, such as outdoors. The maximum transmittance of the above-described material can be set to a desired range, for example, depending on the type and amount of pigment added.

[0031] The above-mentioned material preferably has a high transmittance in the visible wavelength range, and specifically, in the region of wavelengths from 430 to 560 nm, the average value of the transmittance measured from the vertical direction of the material is preferably 84% or higher, and more preferably 85% or higher. If a near-infrared cut filter having a material satisfying this condition is used, it is possible to sufficiently cut light of wavelengths in the near-infrared region to be cut while further suppressing the decrease in visible light transmittance, so it can be used more suitably as a near-infrared cut filter with high visible light transmittance.

[0032] The shortest wavelength value (Xa) at which the transmittance is 50% when measured from the vertical direction of the above-described material in the region of wavelengths 580 to 900 nm is preferably 600 to 700 nm, more preferably 610 to 680 nm, and particularly preferably 615 to 650 nm.

[0033] When the longest wavelength value at which the transmittance is 50% when measured from the vertical direction of the above-described material in the region of wavelengths 580 to 900 nm is denoted as Xb, the difference between Xb and Xa (Xb-Xa) is preferably 130 nm or more, more preferably 140 nm or more, and even more preferably 150 nm or more. The upper limit of Xb-Xa is not particularly limited, but is, for example, 280 nm.

[0034] If the above description satisfies this requirement, it is possible to suppress reflected light in a wide absorption band of the near-infrared region, thereby easily obtaining a near-infrared cut filter that can provide a good image with little flare.

[0035] The filter may have one or more layers of the resin layer in the substrate, may include the resin layer and a glass support (functional film), or may include the resin layer and another resin layer (functional film) other than the resin layer.

[0036] Specific examples of the configuration of the present filter include, for instance, a configuration having a substrate comprising only the present resin layer; a configuration having a substrate having a resin layer (functional film), such as an overcoat layer containing a curable resin, laminated thereon using the present resin layer as a substrate; and a configuration having a substrate having the present resin layer laminated thereon on a support (functional film), such as a glass support or a resin support serving as a base.

[0037] Except for having the above-mentioned material, the filter may be configured in a conventionally known manner, and the material alone may be the filter; however, it is preferable to have a material and a dielectric multilayer film, and particularly preferable to have a dielectric multilayer film on at least one side of the material. Furthermore, "at least one side of the material" refers to one side of the material having the largest surface area (main surface).

[0038] As for the present filter having such a dielectric multilayer film, a filter having a dielectric multilayer film on one side of the main surface of a substrate, or a filter having a dielectric multilayer film on both sides of the main surface of a substrate is preferred. When the dielectric multilayer film is provided on one side of the substrate, manufacturing costs and ease of manufacturing are excellent, and when provided on both sides, the present filter having high strength and being resistant to bending or twisting can be easily obtained. When the present filter is used for a solid-state imaging device, etc., it is more preferable to provide the dielectric multilayer film on both sides of the substrate, as it is desirable for the bending or twisting of the filter to be small.

[0039] In a range that does not impair the effects of the present invention, the filter may appropriately provide a functional film, such as a support, an anti-reflective film, a hard coat film, or an anti-static film, between the substrate and the dielectric multilayer film, on the side opposite to the surface on which the dielectric multilayer film of the substrate is provided, or on the side opposite to the surface on which the dielectric multilayer film of the substrate is provided, for purposes such as improving the surface hardness of the substrate or the dielectric multilayer film, improving chemical resistance, preventing static electricity, and removing scratches.

[0040] The filter may include one layer of the functional film or two or more layers. If the filter includes two or more layers of the functional film, it may include two or more layers of the same film or two or more different films.

[0041] The thickness of the filter can be appropriately selected according to the desired application, but according to recent trends such as thinning and lightweighting of solid-state imaging devices, it is desirable for the thickness of the filter to be thin. Since the filter includes the resin layer, it is possible to make it thin.

[0042] The thickness of the filter is preferably 300 μm or less, more preferably 280 μm or less, even more preferably 250 μm or less, particularly preferably 240 μm or less, and the lower limit is not particularly limited, but is preferably 20 μm, for example.

[0043] It is preferable that this filter be an optical filter having excellent cutting performance in the wavelength range of 800 to 1200 nm and excellent transmittance in the visible light wavelength range.

[0044] The dielectric multilayer film used in this filter is preferably a near-infrared reflective film.

[0045] In the filter, it is preferable that the transmittance in the near-infrared wavelength range be low. In particular, it is known that the light reception sensitivity of a solid-state imaging element is relatively high in the wavelength range of 850 to 1200 nm, and by reducing the transmittance in the above wavelength range, the visual sensitivity of the camera image and the human eye can be effectively corrected, thereby achieving excellent color reproduction.

[0046] In the filter, the average value of the transmittance measured from the vertical direction of the filter in the wavelength range of 800 to 1200 nm is preferably 5% or less, more preferably 4% or less, even more preferably 3% or less, and particularly preferably 2% or less.

[0047] If the average value of the transmittance of a wavelength of 800 to 1200 nm is within the above range, it is desirable because near-infrared rays can be sufficiently cut, thereby achieving excellent color reproduction.

[0048] This filter has excellent cutting ability for wavelengths of a region to be cut and excellent transmission ability for wavelengths to be transmitted. Therefore, it is useful for correcting the visual sensitivity of solid-state imaging elements, such as CCDs or CMOS image sensors in camera modules. In particular, it is useful for smartphone cameras, digital still cameras, mobile phone cameras, digital video cameras, cameras for wearable devices, PC cameras, surveillance cameras, automotive cameras, optical sensors (e.g., ambient light sensors), etc.

[0049] ≪Resinus≫

[0050] The resin layer contains resin and two or more types of pigments (A), and substantially does not contain pigment (B).

[0051] T (㎛) is the thickness of the resin layer containing pigment (A) when the length is 60 mm and the width is 60 mm, and C is the content of one type of pigment (A) per 100 parts by mass of resin containing pigment (A) in the resin layer. a When referred to as (part of mass), T×C a It is preferable that the value of (㎛·parts by mass) is 2 to 25㎛·parts by mass. For example, when the thickness of the resin layer is 80㎛ and the content of pigment (A) per 100 parts by mass of resin is 0.12 parts by mass, T×C a The value of (㎛·parts by mass) is 9.6㎛·parts by mass. When the present resin layer is prepared by polymerizing a composition comprising monomers constituting the resin and a pigment (A), the content of one type of pigment (A) per 100 parts by mass of the total content of monomers constituting the resin is C a It can be called (mass part).

[0052] T×C a The value of (㎛·parts by mass) is more preferably 3 to 22㎛·parts by mass, and even more preferably 4 to 20㎛·parts by mass. In this case, sufficient near-infrared absorption performance can be exhibited to realize a near-infrared cut filter with a wide viewing angle. All dyes (A) are T×C aIt is preferable that (㎛·mass part) is within the above range.

[0053] The phrase “substantially does not contain pigment (B)” in the resin layer refers to the thickness T (㎛) of the resin layer containing pigment (A) when the length is 60 mm and the width is 60 mm, and the content of one type of pigment (B) per 100 parts by mass of resin contained together with pigment (A) in the resin layer is C. b When referred to as (part of mass), T×C b This means that the value of (㎛·parts by mass) is 0 to 2.0㎛·parts by mass. When the present resin layer is prepared by polymerizing a composition comprising monomers constituting the resin and a pigment (A), the content of one type of pigment (B) relative to 100 parts by mass of the total content of monomers constituting the resin is C b It can be called (mass part).

[0054] T×C b The value of (㎛·parts by mass) is preferably 0 to 1.8㎛·parts by mass, more preferably 0 to 1.5㎛·parts by mass, and even more preferably 0 to 1.2㎛·parts by mass. In this case, the resin layer as a whole can sufficiently suppress fluorescence even when absorbing light. All pigments (B) are T×C b It is preferable that (㎛·mass part) is within the above range.

[0055] The resin layer may be single-layer or multi-layer. In this case, two or more resin layers may be identical or different.

[0056] The thickness of the resin layer can be appropriately selected according to the desired application and is not particularly limited, but is typically 0.5 to 300 μm, preferably 1 to 250 μm, more preferably 2 to 230 μm, and particularly preferably 3 to 150 μm.

[0057] If the thickness of the resin layer is within the above range, the substrate and filter using the resin layer can be made thinner and lighter, and can be used for various applications such as solid-state imaging devices. In particular, when the single layer of the resin layer is used in a lens unit such as a camera module, it is desirable because it enables the reduction of the lens unit's magnification and weight.

[0058] ≪Pigment (A)≫

[0059] Two or more pigments (A) are not particularly limited as long as they are compounds that each independently have an absorption maximum wavelength of 650 to 820 nm and satisfy the condition that the emission quantum yield is less than 22%. The emission quantum yield is defined as the ratio of the number of emitted photons to the number of photons absorbed by the compound, and can be obtained by irradiating a solution or resin film containing the compound with light of a wavelength absorbed by the compound (typically light near the absorption maximum wavelength) and measuring the intensity of the generated light. The near-infrared cut filter of the present invention can suppress the generation of fluorescence that causes flare because the emission quantum yield of the pigment (A) is low. The emission quantum yield of the pigment (A) is more preferably less than 20%, and even more preferably less than 18%.

[0060] Among the two or more pigments (A) included in the resin layer, the pigment (A) having the shortest wavelength of maximum absorption is designated as pigment (A1), and the pigment (A) having the longest wavelength of maximum absorption is designated as pigment (A2). The maximum wavelength of absorption (λ1) of pigment (A1) is preferably 650 to 760 nm, more preferably 680 to 755 nm, and even more preferably 700 to 750 nm, and the maximum wavelength of absorption (λ2) of pigment (A2) is preferably 730 to 820 nm, more preferably 740 to 810 nm, and even more preferably 750 to 800 nm. In addition, the difference in maximum wavelength of absorption (|λ2-λ1|) is preferably 10 to 110 nm, more preferably 15 to 105 nm, even more preferably 20 to 100 nm, and particularly preferably 25 to 95 nm. When λ1 and λ2 are in this range, the width of the absorption band required to obtain a near-infrared cut filter with a wide viewing angle and excellent color reproduction can be secured.

[0061] Examples of the above pigment (A) include phthalocyanine compounds, naphthalocyanine compounds, polymethine compounds (wherein the above polymethine compounds are compounds other than squarylium compounds, croconium compounds, and cyanine compounds), and pyrrolopyrrole compounds.

[0062] Among these, phthalocyanine-based compounds and polymethine-based compounds are preferred in terms of the ability to select molecular structures with low emission quantum yields, and polymethine-based compounds are particularly preferred in terms of having spectral characteristics that exhibit high transmittance in the visible light region, as they can easily reduce shoulder peaks in the red to near-infrared region based on near-infrared absorbers.

[0063] Phthalocyanine compounds

[0064] The above phthalocyanine compounds are not particularly limited as long as they do not impair the effects of the present invention, but examples include compounds described in Japanese Patent Publication No. 2005-220060, Japanese Patent Publication No. 2007-169343, Japanese Patent Publication No. 2013-195480, International Publication No. 2015 / 025779, and International Publication No. 2017 / 164024, and can be synthesized by a generally known method.

[0065] When using phthalocyanine compounds, it is preferable to use them in combination with at least one other near-infrared absorber.

[0066] Naphthalocyanine compounds

[0067] The above-mentioned naphthalocyanine compounds are not particularly limited as long as they do not impair the effects of the present invention, but examples include compounds described in Japanese Patent Publication No. 2015-225290, Japanese Patent Publication No. 2017-142332, and International Publication No. 2018 / 186490, and can be synthesized by a generally known method.

[0068] Polymethicone compounds

[0069] The above-mentioned polymethine-based compound is a compound having a π-conjugated methine chain other than a squaryllium-based compound, a croconium-based compound, and a cyanine-based compound, and is not particularly limited as long as it does not impair the effect of the present invention, but, for the reason that a near-infrared cut filter in which the above effect is more exhibited can be easily obtained, compounds described in, for example, Japanese Patent Publication No. 2021-134350, International Publication No. 2021 / 085372, Japanese Patent Publication No. 2019-164269, Japanese Patent Publication No. 2022-025669, etc. are preferred.

[0070] The above-mentioned polymethine compound can be synthesized using a generally known method.

[0071] Pyrrolopyrole compounds

[0072] The above-mentioned pyrrolopyrrole compounds are not particularly limited as long as they do not impair the effects of the present invention, but examples include compounds described in Japanese Patent Publication No. 2018-119077 and International Publication No. 2018 / 020861, and can be synthesized by a generally known method.

[0073] The colorant (A) is preferably a compound soluble in organic solvents, and particularly preferably a compound soluble in dichloromethane.

[0074] Here, organic solvent solubility means that 0.1g or more of the pigment (A) dissolves in 100g of organic solvent at 25℃.

[0075] ≪Pigment (B)≫

[0076] The pigment (B) is not particularly limited as long as it is a compound that satisfies having an absorption maximum wavelength of 650 to 820 nm and an emission quantum yield of 22% or more. The near-infrared cut filter of the present invention does not substantially contain the pigment (B) in the resin layer, but if it contains a trace amount, it is preferable that the emission quantum yield of the pigment (B) be 50% or less, and more preferable that it be 45% or less, in order to keep the flare at an acceptable level.

[0077] Examples of the above pigment (B) include phthalocyanine compounds, naphthalocyanine compounds, squaryllium compounds, croconium compounds, cyanine compounds, polymethine compounds (wherein the above polymethine compounds are compounds other than squaryllium compounds, croconium compounds, and cyanine compounds), and pyrrolopyrrol compounds.

[0078] Squaryllium Compounds

[0079] The above squaryllium-based compounds are not particularly limited as long as they do not impair the effects of the present invention, but examples include compounds described in Japanese Patent Publication No. 2014-074002, Japanese Patent Publication No. 2014-052431, and International Publication No. 2017 / 164024, and can be synthesized by a generally known method.

[0080] Croconium Compounds

[0081] The above croconium-based compounds are not particularly limited as long as they do not impair the effects of the present invention, but examples include compounds described in Japanese Patent Publication No. 2007-31644, Japanese Patent Publication No. 2007-169315, and International Publication No. 2019 / 021767, and can be synthesized by a generally known method.

[0082] Cyanine compounds

[0083] The above cyanine-based compounds are not particularly limited as long as they do not impair the effects of the present invention, but examples include compounds described in Japanese Patent Publication No. 2009-108267, Japanese Patent Publication No. 2010-072575, and Japanese Patent Publication No. 2016-060774, and can be synthesized by a generally known method.

[0084] The pigment (B) is not substantially contained in the resin layer, but if it is contained in trace amounts, the absorption maximum wavelength (λ) of the pigment (B) B It is preferable that ) is on the shorter wavelength side than the absorption maximum wavelength (λ2) of the pigment (A2) included in the resin layer. Since the pigment (B) has a relatively high emission quantum yield, it can cause flare, but if it is contained in a trace amount in the resin layer, λ B When the wavelength is shorter than λ2, the fluorescence generated from the dye (B) can be reabsorbed by the dye (A2), so it tends to be easy to obtain an excellent camera image.

[0085] It is preferable that the pigment (B) is not substantially contained in the layer other than the resin layer included in the filter. In other words, it is preferable that the pigment (B) is not substantially contained in the filter. "Not substantially contained in the layer other than the resin layer" means that the content of the pigment (B) relative to 100 mass% of the layer other than the resin layer is less than 0.01 mass%, and it is most preferable that it be 0 mass%.

[0086] 〔profit〕

[0087] The resin used in the resin layer is not particularly limited, and conventionally known resins may be used. The resin used in the resin layer may be of one type alone or two or more types.

[0088] The resin mentioned above is not particularly limited as long as it does not impair the effects of the present invention, but, for example, a resin having a glass transition temperature (Tg) of preferably 110 to 380°C, more preferably 110 to 370°C, and particularly preferably 120 to 360°C may be cited, in that it has excellent thermal stability and moldability into a film (plate) shape, and can easily obtain a film capable of forming a dielectric multilayer film by high-temperature deposition performed at a deposition temperature of about 100°C or higher. In addition, if the Tg of the resin is 140°C or higher, it is particularly preferred because a film capable of forming a dielectric multilayer film by deposition at a higher temperature can be obtained.

[0089] As the resin, a resin having a thickness of 0.1 mm containing the resin may be used such that the total light transmittance (JIS K7375:2008) of the resin plate is preferably 75 to 95%, more preferably 78 to 95%, and particularly preferably 80 to 95%.

[0090] By using a resin with an overall light transmittance within the above range, a substrate with excellent transparency and a near-infrared cut filter can be easily obtained.

[0091] The weight average molecular weight (Mw) of the above resin, measured by gel permeation chromatography (GPC), is typically 15,000 to 350,000, preferably 30,000 to 250,000, and the number average molecular weight (Mn) is typically 10,000 to 150,000, preferably 20,000 to 100,000.

[0092] Examples of the above resins include cyclic (poly)olefin resins, aromatic polyether resins, polyimide resins, polyester resins, polycarbonate resins, polyamide (aramid) resins, polyarylate resins, polysulfone resins, polyethersulfone resins, polyparaphenylene resins, polyamideimide resins, polyethylene naphthalate (PEN) resins, fluorinated aromatic polymer resins, (modified) acrylic resins, epoxy resins, allyl ester-based curable resins, silsesquioxane-based UV-curable resins, acrylic-based UV-curable resins, and vinyl-based UV-curable resins.

[0093] Specific examples of these resins include the resin described in International Publication No. 2019 / 168090.

[0094] [Other ingredients]

[0095] The resin layer may additionally contain other components other than pigments (A) and (B), such as an absorbent (hereinafter also referred to as “compound (X)”), an antioxidant, a fluorescent quencher, a metal complex compound, and an antistatic agent, to the extent that the effects of the present invention are not impaired.

[0096] Each of the other ingredients may be used as a single type or as two or more types.

[0097] Other components may be mixed with the resin, etc., when forming the resin layer, or added when synthesizing the resin. In addition, the amount added may be appropriately selected according to desired characteristics, but is typically 0.01 to 5.0 parts by mass, preferably 0.05 to 2.0 parts by mass, per 100 parts by mass of the resin.

[0098] [Compound (X)]

[0099] The resin layer may contain one or more types of compound (X).

[0100] As for the above compound (X), a compound with an absorption maximum wavelength greater than 820 nm or less than or equal to 420 nm is preferred, and examples include near-infrared absorbers such as phthalocyanine compounds, naphthalocyanine compounds, squaryllium compounds, croconium compounds, polymethine compounds (provided that the above polymethine compounds are compounds other than squaryllium compounds and croconium compounds), diimonium compounds, perylene compounds, and dithiol metal complex compounds, or ultraviolet absorbers such as azomethine compounds, indole compounds, benzotriazole compounds, triazine compounds, anthracene compounds, cyanoacrylate compounds, and compounds described in Japanese Patent Publication No. 2019-014707, etc.

[0101] By including an ultraviolet absorber in the resin layer, a substrate and a near-infrared cut filter with low dependence on the angle of incidence can be easily obtained even in the near-ultraviolet wavelength region, and when the said substrate or near-infrared cut filter is used in an imaging device, the resulting camera image quality becomes better.

[0102] [Antioxidant]

[0103] Examples of the above antioxidants include 2,6-di-tert-butyl-4-methylphenol, 2,2'-deoxy-3,3'-di-tert-butyl-5,5'-dimethyldiphenylmethane, and tetrakis[methylene-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]methane.

[0104] [Method for Forming the Resin Layer]

[0105] The resin layer may be formed by a solution prepared by adding a pigment (A) to a previously synthesized resin, or by polymerizing a composition containing monomers constituting the resin and a pigment (A).

[0106] The resin layer can be formed, for example, by melt molding or cast molding, and, if necessary, a coating agent such as an anti-reflective agent, a hard coating agent and / or an antistatic agent may be coated after molding.

[0107] A laminate having the present resin layer laminated on the above-mentioned support (functional film) can be manufactured by, for example, melt-molding or cast-molding the present resin layer forming material on the support, preferably by a spin coat, slit coat, inkjet, etc., and then, if necessary, drying and removing the solvent or performing light irradiation or heating.

[0108] Examples of the above supports include glass plates (including absorbing glass such as near-infrared absorbing glass), steel belts, steel drums, and supports made of resin (e.g., polyester film, cyclic olefin resin film).

[0109] In addition, the resin layer may be formed on an optical component by a method such as coating a liquid resin layer forming material onto an optical component, such as a glass plate, quartz, or plastic, and drying the solvent, or by coating a curable resin layer forming material and curing and drying it.

[0110] The amount of residual solvent in the resin layer or in the resin layer is preferably as small as possible. Specifically, the amount of residual solvent is preferably 3 mass% or less, more preferably 1 mass% or less, and even more preferably 0.5 mass% or less with respect to 100 mass% of the resin layer. In addition, it is desirable to suppress the solvent content in the resin layer or in the resin layer to 100 mass ppm or less.

[0111] If the amount of residual solvent is within the above range, a resin layer is obtained that is resistant to deformation or changes in properties and can easily exhibit the desired function.

[0112] Genome Multilayer

[0113] Examples of the above-mentioned dielectric multilayer films include a laminate in which a high-refractive-index material layer and a low-refractive-index material layer are alternately stacked.

[0114] As a material constituting the high refractive index material layer, a material with a refractive index of 1.7 or higher may be cited, and typically, a material with a refractive index of 1.7 to 2.5 is selected. Examples of such materials include those having titanium oxide (titania), zirconium oxide, tantalum pentoxide, niobium pentoxide, lanthanum oxide, yttrium oxide, zinc oxide, zinc sulfide, or indium oxide as main components, and containing a small amount of titanium oxide, tin oxide, and / or cerium oxide (e.g., 0 to 10 mass% relative to the main components).

[0115] As a material constituting the low refractive index material layer above, a material with a refractive index of 1.6 or less may be used, and typically, a material with a refractive index of 1.2 to 1.6 is selected. Examples of such materials include silica, alumina, lanthanum fluoride, magnesium fluoride, and sodium aluminum hexafluoride.

[0116] Regarding the method of stacking the high-refractive-index material layer and the low-refractive-index material layer, there are no particular limitations as long as a dielectric multilayer film is formed by stacking these material layers. For example, a dielectric multilayer film in which the high-refractive-index material layer and the low-refractive-index material layer are alternately stacked can be formed on the substrate directly by a CVD method, a sputtering method, a vacuum deposition method, an ion-assisted deposition method, or an ion plating method.

[0117] The thickness of each layer of the high refractive index material layer and the low refractive index material layer is preferably 0.1λ to 0.5λ, where λ (nm) is the near-infrared wavelength to be blocked. Additionally, for the high refractive index material layer and the low refractive index material layer, layers with a thickness outside the range of 0.1λ to 0.5λ may be used depending on the purpose, such as reducing reflection in the visible light region or improving shielding performance in a specific wavelength region. As for the value of λ (nm), in the case of NIR-CF, for example, it is 700 to 1400 nm, preferably 750 to 1300 nm. When the thickness of each layer of the high refractive index material layer and the low refractive index material layer is within this range, the optical film thickness (n×d), which is the product of the refractive index (n) and the film thickness (d), becomes almost equal to λ / 4, and there is a tendency to easily control the blocking and transmission of a specific wavelength based on the relationship between the optical properties of reflection and refraction.

[0118] In the dielectric multilayer film, the total number of layers of high-refractive-index material layers and low-refractive-index material layers is preferably 16 to 70 layers as a whole filter, for example in the case of NIR-CF, and more preferably 20 to 60 layers. If the thickness of each layer, the thickness of the dielectric multilayer film as a whole filter, or the total number of layers is within the above range, sufficient manufacturing margin can be secured, and warping of the filter or cracking of the dielectric multilayer film can be reduced.

[0119] With this filter, by appropriately selecting the material type constituting the high-refractive-index material layer and the low-refractive-index material layer, the thickness of each layer of the high-refractive-index material layer and the low-refractive-index material layer, the stacking order, and the number of stacking layers according to the absorption characteristics of the pigments (A) and (B), sufficient transmittance can be secured in the wavelength range to be transmitted (e.g., visible light region), sufficient light cutting characteristics can be secured in the near-infrared wavelength range to be cut, and the reflectance can be reduced when near-infrared rays are incident from an oblique direction.

[0120] Here, in order to optimize the conditions of the dielectric multilayer film, parameters can be set using, for example, optical thin film design software (e.g., EssentialMacroD, ThinFilmCenter) to achieve a combination of an anti-reflection effect in the wavelength range to be transmitted (e.g., visible light region) and a light cutting effect in the near-infrared region to be cut. In the case of the software, for example, when forming a dielectric multilayer film of NIR-CF, parameter setting methods may include setting the target transmittance for a wavelength of 400 to 700 nm to 100% and the target tolerance value to 1, and then setting the target transmittance for a wavelength of 705 to 950 nm to 0% and the target tolerance value to 0.5.

[0121] These parameters can be adjusted to further finely subdivide the wavelength range to match various characteristics of the resin layer, thereby changing the value of the target tolerance.

[0122] <Functional Membrane>

[0123] The method of laminating the above functional film is not particularly limited, but may include methods such as melt molding or cast molding, in the same manner as above, on the resin layer or dielectric multilayer film, such as coating agents including anti-reflective agents, hard coat agents and / or antistatic agents.

[0124] In addition, the curable composition containing the above coating agent, etc., can also be manufactured by applying it onto the resin layer or dielectric multilayer film using a bar coater, etc., and then curing it by ultraviolet irradiation, etc.

[0125] Examples of the above coating agents include ultraviolet (UV) / electron beam (EB) curing type resins or thermosetting type resins, and specifically, vinyl compounds, urethane-based, urethane acrylate-based, acrylate-based, epoxy-based, and epoxy acrylate-based resins.

[0126] The coating agent may be used as a single type or as two or more types.

[0127] Examples of the above-mentioned curable compositions containing these coating agents include vinyl-based, urethane-based, urethane acrylate-based, acrylate-based, epoxy-based, and epoxy acrylate-based curable compositions.

[0128] The above-mentioned curable composition may include a polymerization initiator. As the polymerization initiator, a known photopolymerization initiator or a thermal polymerization initiator may be used, and a photopolymerization initiator and a thermal polymerization initiator may be used in combination. The polymerization initiator may be used as a single type or two or more types may be used.

[0129] Among the above curable compositions, the mixing ratio of the polymerization initiator is preferably 0.1 to 10 mass%, more preferably 0.5 to 10 mass%, and even more preferably 1 to 5 mass% when the total amount of the curable composition is 100 mass%. When the mixing ratio of the polymerization initiator is within the above range, a curable composition with excellent curing characteristics and handling properties can be easily obtained, and functional films such as anti-reflective films, hard coat films, or anti-static films having a desired hardness can be easily obtained.

[0130] In addition, an organic solvent may be added to the above-mentioned curable composition as a solvent, and known solvents may be used as organic solvents. Specific examples of organic solvents include alcohols such as methanol, ethanol, isopropanol, butanol, and octanol; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; esters such as ethyl acetate, butyl acetate, ethyl lactate, γ-butyrolactone, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate; ethers such as ethylene glycol monomethyl ether and diethylene glycol monobutyl ether; aromatic hydrocarbons such as benzene, toluene, and xylene; and amides such as dimethylformamide, dimethylacetamide, and N-methylpyrrolidone.

[0131] These solvents may be used as a single type or two or more types may be used.

[0132] The thickness of the above functional film is preferably 0.1 to 20 μm, more preferably 0.5 to 10 μm, and particularly preferably 0.7 to 5 μm.

[0133] In addition, for the purpose of improving the adhesion between the resin layer and the functional film and / or dielectric multilayer film, or the adhesion between the functional film and the dielectric multilayer film, surface treatments such as corona treatment or plasma treatment may be performed on the surface of the resin layer, the functional film, or the dielectric multilayer film.

[0134] ≪Optical Elements and Camera Modules≫

[0135] The optical element and camera module according to the present invention are not particularly limited as long as they are equipped with the filter, and may be configured in a conventionally known configuration. Here, a camera module is a device equipped with a solid-state imaging element such as a CCD or CMOS image sensor, and specifically, examples include a digital still camera, a camera for a smartphone, a camera for a mobile phone, a camera for a wearable device, a digital video camera, etc.

[0136] Examples

[0137] The present invention will be described more specifically below based on examples, but the present invention is not limited to these examples at all.

[0138] <Molecular weight>

[0139] The molecular weight of the resin was measured by the following method (a) or (b), taking into account the solubility of each resin in a solvent.

[0140] (a) Using a gel permeation chromatography (GPC) apparatus manufactured by Waters (Type 150C, column: H-type column manufactured by Toso Co., Ltd., developing solvent: o-dichlorobenzene), the weight average molecular weight (Mw) and number average molecular weight (Mn) of standard polystyrene were measured.

[0141] (b) The weight-average molecular weight (Mw) and number-average molecular weight (Mn) equivalent to standard polystyrene were measured using a GPC device manufactured by Doso Co., Ltd. (HLC-8220 type, column: TSKgelα-M, developing solvent: THF).

[0142] Glass Transition Temperature (Tg)

[0143] The glass transition temperature of the resin was measured using a differential scanning calorimeter (DSC6200) manufactured by Hitachi High-Tech Analysis Corp., under a nitrogen air stream with a heating rate of 20°C per minute.

[0144] <Absorption Maximum Wavelengths of Pigment (A), Pigment (B), and Compound (X)>

[0145] The compound described below was dissolved in dichloromethane, and the absorption maximum wavelength was determined from the absorption spectrum measured using a spectrophotometer (V-7200) manufactured by Nihon Bunko Co., Ltd.

[0146] <Emission quantum yield of pigment (A) and pigment (B)>

[0147] The compound described below was dissolved in dichloromethane, and the emission quantum yield was measured using an absolute PL quantum yield measuring device (C11347) manufactured by Hamamatsu Photonics Co., Ltd. In addition, when performing the measurement, the concentration was adjusted so that the absorbance of the dye at the maximum absorption wavelength was 0.05 or less, and the excitation wavelength was set to the wavelength of the value rounded to the last digit of the maximum absorption wavelength of the dye, for example, a dye with a maximum absorption wavelength of 717 nm was measured using excitation light of a wavelength of 720 nm.

[0148] Spectral transmittance

[0149] The spectral transmittance of the substrate and the filter in each wavelength range was measured using a spectrophotometer (U-4100) manufactured by Hitachi High-Tech Corporation.

[0150] <Flare evaluation around light source, Red flare evaluation on black background>

[0151] Flare evaluation and red flare evaluation on a black background when this filter is embedded in a camera module were performed using the following method.

[0152] A camera module was manufactured in the same manner as described in Japanese Patent Publication No. 2016-110067. A halogen lamp light source (Lumina Ace LA-150TX) manufactured by Hayashi Refic Co., Ltd. was installed in front of a black blackout curtain inside a dark room, and a camera image was captured using the obtained camera module. On this occasion, as illustrated in FIG. 1, when taking the picture, the light source was adjusted so that it was located at the upper right corner of the camera image.

[0153] Flare around the light source in camera images was evaluated according to the following criteria.

[0154] A level where there is no flare and there are no problems at all as a high-definition camera module was judged as “◎”, a level where slight flare is acknowledged but is sufficiently acceptable as a high-definition camera module was judged as “○”, a level where slight flare is occurring and is on the borderline between applicable and unapplicable as a high-definition camera module was judged as “△”, and a level where flare is occurring and is unacceptable as a high-definition camera module was judged as “×”.

[0155] The red flare of the black background around the light source in the camera image was evaluated according to the following criteria.

[0156] A level where no reddish tint is felt even on the black background around the light source, and there is no problem at all as a high-definition camera module, was judged as “○”; a level where a slight reddish tint is felt on the black background around the light source, and is acceptable as a high-definition camera module, was judged as “△”; and a level where a reddish tint is felt on the black background around the light source, and is unacceptable as a high-definition camera module, was judged as “×”.

[0157] [Resin Synthesis Example 1]

[0158] 8-methyl-8-methoxycarbonyltetracyclo[4.4.0.1 represented by the following formula (a) 2,5 .1 7,10 100 parts by mass of dodeca-3-ene (hereinafter also referred to as "DNM"), 18 parts by mass of 1-hexene (molecular weight regulator), and 300 parts by mass of toluene (solvent for ring-opening polymerization reaction) were added to a nitrogen-substituted reaction vessel, and the solution was heated to 80°C. Next, 0.2 parts by mass of a toluene solution of triethylaluminum (0.6 mol / L) and 0.9 parts by mass of a toluene solution of methanol-modified tungsten hexachloride (concentration 0.025 mol / L) were added to the solution in the reaction vessel as polymerization catalysts, and the ring-opening polymerization reaction was carried out by heating and stirring the solution at 80°C for 3 hours to obtain a ring-opening polymer solution. The polymerization conversion rate in this polymerization reaction was 97%.

[0159]

[0160] 1,000 parts by mass of the ring-opening polymer solution obtained above were placed into an autoclave, and 0.12 parts by mass of RuHCl(CO)[P(C6H5)3]3 were added to the ring-opening polymer solution. A hydrogenation reaction was carried out by heating and stirring for 3 hours under conditions of a hydrogen gas pressure of 100 kg / ㎠ and a reaction temperature of 165°C. After cooling the obtained reaction solution (hydrogenated polymer solution), the hydrogen gas was released. The obtained reaction solution was injected into a large amount of methanol to separate and recover the coagulated material, which was then dried to obtain a hydrogenated polymer (hereinafter also referred to as "Resin A"). The obtained Resin A had a number average molecular weight (Mn) of 32,000, a weight average molecular weight (Mw) of 137,000, and a glass transition temperature (Tg) of 165°C.

[0161] [Resin Synthesis Example 2]

[0162] 35.12 g (0.253 mol) of 2,6-difluorobenzonitrile, 87.60 g (0.250 mol) of 9,9-bis(4-hydroxyphenyl)fluorene, 41.46 g (0.300 mol) of potassium carbonate, 443 g of N,N-dimethylacetamide, and 111 g of toluene were added to a 3 L four-necked flask. Subsequently, a thermometer, a stirrer, a three-way stopcock equipped with a nitrogen inlet tube, a Dean-Stark tube, and a condenser were installed in the four-necked flask.

[0163] Next, after purging the flask with nitrogen, the resulting solution was reacted at 140°C for 3 hours, and the water produced was removed periodically from the Dean-Stark tube. At the point when no water was produced, the temperature was gradually raised to 160°C and the reaction was carried out at that temperature for 6 hours. Afterward, it was cooled to room temperature (25°C), the resulting salt was removed with filter paper, and the filtrate was added to methanol to re-precipitate, and the filtrate (residue) was isolated by filtration. The obtained filtrate was vacuum dried overnight at 60°C to obtain a white powder (hereinafter also referred to as "Resin B") (yield 95%). The obtained Resin B had a number average molecular weight (Mn) of 75,000, a weight average molecular weight (Mw) of 188,000, and a glass transition temperature (Tg) of 285°C.

[0164] [Synthesis of Pigment (A), Pigment (B), and Compound (X)]

[0165] The pigment (A), pigment (B), and compound (X) used in the following examples were synthesized based on a generally known synthesis method.

[0166] These compounds are, for example, Japanese Patent Publication No. 2009-108267, Japanese Patent Publication No. Hei 5-59291, Japanese Patent Publication No. 2014-95007, Japanese Patent Publication No. 2011-52218, Japanese Patent Publication No. 2021-134350, International Publication No. 2007 / 114398, Japanese Patent Publication No. 2003-246940, Chemistry of Heterocyclic Compounds: The Cyanine Dyes and Related Compounds, Volume 18 (Wiley, 1964), Near-Infrared Dyes for High Technology Applications (Springer, 1997), Japanese Patent No. 3366697, Japanese Patent No. 2846091, Japanese Patent No. 2864475, Japanese Patent It can be synthesized by referring to the methods described in Japanese Patent Publication No. 3703869, Japanese Patent Publication No. Sho 60-228448, Japanese Patent Publication No. Hei 1-146846, Japanese Patent Publication No. Hei 1-228960, Japanese Patent Publication No. 4081149, Japanese Patent Publication No. Sho 63-124054, “Phthalocyanine - Chemistry and Function -” (IPC, 1997), Japanese Patent Publication No. 2007-169315, Japanese Patent Publication No. 2009-108267, Japanese Patent Publication No. 2010-241873, Japanese Patent Publication No. 3699464, and Japanese Patent Publication No. 4740631.

[0167] ≪Pigment (A)≫

[0168] As a pigment (A), the following compound was used.

[0169] · Compound (a-1): Polymethine-based compound represented by the following formula (a-1) (absorption maximum wavelength in dichloromethane 717 nm, emission quantum yield 20%)

[0170] · Compound (a-2): Polymethine-based compound represented by the following formula (a-2) (absorption maximum wavelength in dichloromethane 770 nm, emission quantum yield 6%)

[0171] · Compound (a-3): Polymethine-based compound represented by the following formula (a-3) (absorption maximum wavelength in dichloromethane 739 nm, emission quantum yield 3%)

[0172] · Compound (a-4): Polymethine-based compound represented by the following formula (a-4) (absorption maximum wavelength in dichloromethane 720 nm, emission quantum yield 20%)

[0173] · Compound (a-5): A phthalocyanine compound represented by the following formula (a-5) (absorption maximum wavelength in dichloromethane 738 nm, emission quantum yield 4%)

[0174] · Compound (a-6): Polymethine-based compound represented by the following formula (a-6) (absorption maximum wavelength in dichloromethane 772 nm, emission quantum yield 5%)

[0175]

[0176]

[0177]

[0178]

[0179]

[0180]

[0181] ≪Pigment (B)≫

[0182] As a pigment (B), the following compound was used.

[0183] · Compound (b-1): A squaryllium-based compound represented by the following formula (b-1) (absorption maximum wavelength in dichloromethane 704 nm, emission quantum yield 38%)

[0184] · Compound (b-2): A squaryllium-based compound represented by the following formula (b-2) (maximum absorption wavelength in dichloromethane 704 nm, emission quantum yield 36%)

[0185] · Compound (b-3): A cyanine compound represented by the following formula (b-3) (absorption maximum wavelength in dichloromethane 740 nm, emission quantum yield 38%)

[0186]

[0187]

[0188]

[0189] ≪Compound (X)≫

[0190] As compound (X), the following compounds were used.

[0191] · Compound (x-1): A diimonium compound represented by the following formula (x-1) (maximum absorption wavelength in dichloromethane 1094 nm)

[0192] · Compound (x-2): Indole compound represented by the following formula (x-2) (maximum absorption wavelength in dichloromethane 388 nm)

[0193]

[0194]

[0195] The composition of the substrates and various compounds applied in the examples and comparative examples are as follows.

[0196] <Form of Recording>

[0197] ·Form (1): Transparent resin substrate containing pigment (A)

[0198] ·Form (2): A transparent resin substrate containing a pigment (A) has resin layers on both sides.

[0199] ·Form (3): One side of a glass support has a resin layer containing a pigment (A).

[0200] ·Form (4): One side of a resin support has a resin layer containing a pigment (A).

[0201] ·Form (5): A transparent resin substrate containing a pigment (A) and / or a pigment (B) has resin layers on both sides.

[0202] Transparent Resin

[0203] · Resin A: Cyclic olefin resin (Resin Synthesis Example 1)

[0204] · Resin B: Aromatic polyether-based resin (Resin Synthesis Example 2)

[0205] <Guitar Suzy>

[0206] A monomer contained in the composition (1) and composition (2) described below, which polymerizes by light.

[0207] · Monomer A: Tricyclodecanedimethanol acrylate

[0208] · Monomer B: Dipentaerythritol hexaacrylate

[0209] Support structure

[0210] · Support (1): Transparent glass support “OA-10G (thickness 200㎛)” cut to a size of 60 mm in length and 60 mm in width (manufactured by Nippon Denki Glass Co., Ltd.)

[0211] · Support (2): A resin support with a thickness of 0.1 mm, a length of 60 mm, and a width of 60 mm, made using resin A. The method of manufacturing the support (2) is as described in Example 5.

[0212] <Solvent>

[0213] · Solvent (1): Methylene chloride

[0214] · Solvent (2): N,N-dimethylacetamide

[0215] <Drying Conditions for Transparent Resin Substrates and Resin Supports>

[0216] The drying conditions of the transparent resin substrate and resin support of the examples and comparative examples in Table 3 are as follows. In addition, the coating film was peeled off from the glass plate before vacuum drying.

[0217] · Drying conditions (1): 20℃ / 8hr → 100℃ / 8hr under reduced pressure

[0218] · Drying conditions (2): 60℃ / 8hr → 80℃ / 8hr → 140℃ / 8hr under reduced pressure

[0219] <Composition for forming a resin layer>

[0220] The composition forming the resin layer in the example of Table 3 is as follows.

[0221] · Composition (1): A composition comprising 60 parts by mass of monomer A, 40 parts by mass of monomer B, 5 parts by mass of 1-hydroxycyclohexylphenyl ketone, and methyl ethyl ketone (solvent, used so that the solid content concentration in the resulting composition is 30% by mass).

[0222] · Composition (2): A composition comprising 20 parts by mass of monomer A, 80 parts by mass of monomer B, 4 parts by mass of 1-hydroxycyclohexylphenyl ketone, 1.00 parts by mass of compound (a-1), 3.60 parts by mass of compound (a-2), 1.00 parts by mass of compound (a-4), and methyl ethyl ketone (solvent, used so that the solid content concentration in the resulting composition is 30% by mass).

[0223] [Example 1]

[0224] In a container, 100 parts by mass of resin A obtained in Synthesis Example 1, 0.08 parts by mass of compound (a-1) and 0.20 parts by mass of compound (a-2) as pigment (A), and methylene chloride (solvent (1)) were added to obtain a solution with a resin concentration of 20 mass%. Next, the obtained solution was cast onto a smooth glass plate, dried at 20°C for 8 hours, and then peeled off from the glass plate. The peeled film was further dried at 100°C under reduced pressure for 8 hours to obtain a single-layer substrate (substrate shape (1)) including a transparent resin substrate with a thickness of 0.1 mm, a length of 60 mm, and a width of 60 mm.

[0225] The spectral transmittance of light incident from a direction perpendicular to the plane direction of the substrate was measured, and the shortest wavelength value (Xa) at which the transmittance measured from the perpendicular direction of the substrate in the wavelength range of 580 to 900 nm is 50%, the longest wavelength value (Xb) at which the transmittance measured from the perpendicular direction of the substrate in the wavelength range of 580 to 900 nm is 50%, the average transmittance value at wavelengths of 430 to 560 nm, and the maximum transmittance value at wavelengths of 700 to 750 nm were determined. The results are shown in FIG. 2 and Table 3.

[0226] Next, a dielectric multilayer film (I) is formed on one side of the obtained monolayer substrate, and a dielectric multilayer film (II) is formed on the other side of the substrate, and a near-infrared cut filter with a thickness of about 0.105 mm is obtained.

[0227] The dielectric multilayer film (I) is a laminate in which silica (SiO2) layers and titania (TiO2) layers are alternately stacked at a deposition temperature of 100°C (total of 26 layers). The dielectric multilayer film (II) is a laminate in which silica (SiO2) layers and titania (TiO2) layers are alternately stacked at a deposition temperature of 100°C (total of 22 layers). In either dielectric multilayer film (I) or (II), the silica layer and titania layer are alternately stacked in the order of titania layer, silica layer, titania layer, … silica layer, titania layer, silica layer from the substrate side, and the outermost layer of the filter is made to be a silica layer.

[0228] Regarding the thickness and number of layers of each layer, optimization was performed using optical thin film design software (EssentialMacroD, ThinFilmCenter) in accordance with the wavelength-dependent characteristics of the refractive index of the resin layer (1) and the absorption characteristics of the pigment (A) used, so as to achieve good transmittance in the visible light region and reflection performance in the near-infrared region. When performing optimization, the input parameters (target values) to the software in this embodiment were set as shown in Table 1 below.

[0229]

[0230] As a result of optimizing the film composition, the dielectric multilayer film (I) was made into a multilayer deposition film with 26 layers, in which a silica layer with a physical film thickness of about 31 to 157 nm and a titania layer with a physical film thickness of about 10 to 95 nm were alternately stacked, and the dielectric multilayer film (II) was made into a multilayer deposition film with 20 layers, in which a silica layer with a physical film thickness of about 37 to 194 nm and a titania layer with a physical film thickness of about 10 to 110 nm were alternately stacked. An example of the optimized film composition is shown in Table 2 below.

[0231]

[0232] For the obtained near-infrared cut filter, the spectral transmittance of light incident from a direction perpendicular to the plane direction of the filter was measured, and the average transmittance value at wavelengths of 430 to 560 nm and the average transmittance value at wavelengths of 800 to 1200 nm were calculated. The results are shown in Figure 3 and Table 3.

[0233] [Example 2]

[0234] In Example 2, a single-layer substrate including a transparent resin substrate and a near-infrared cut filter using the same were obtained in the same procedure as in Example 1, except that the amounts of compound (a-1) and compound (a-2) added were the amounts listed in Table 3 and the thickness was 0.2 mm. The results are shown in Table 3.

[0235] [Example 3]

[0236] A transparent resin substrate was prepared in the same procedure as in Example 1, except that 0.13 parts by mass of compound (a-1) and 0.08 parts by mass of compound (a-3) were used as pigment (A), and 0.10 parts by mass of compound (x-1) were also used.

[0237] On one side of the obtained transparent resin substrate, the composition (1) was applied using a bar coater so that the thickness of the resulting resin layer was 3 μm, and the solvent was evaporated by heating in an oven at 70°C for 2 minutes. Next, exposure (exposure amount 500 mJ / cm², illuminance: 200 mW / cm²) was performed using a UV conveyor-type exposure machine (manufactured by Eye Graphics Co., Ltd., Eye UV curing device, model US2-X0405, 60 Hz) to cure the composition (1) and form a resin layer on the transparent resin substrate. In the same way, a resin layer containing the composition (1) was formed on the other side of the transparent resin substrate. By doing so, a substrate (form of substrate (2)) having resin layers on both sides of a transparent resin substrate containing pigment (A) was obtained.

[0238] The spectral transmittance of light incident from a direction perpendicular to the plane direction of this substrate was measured, and (Xa), (Xb), the average value of transmittance at wavelengths of 430 to 560 nm, and the maximum value of transmittance at wavelengths of 700 to 750 nm were calculated. The results are shown in Fig. 4 and Table 3.

[0239] Next, dielectric multilayer films were formed on both sides of the obtained substrate in the same procedure as in Example 1, and a near-infrared cut filter with a thickness of about 0.111 mm was obtained. The results are shown in Table 3.

[0240] [Example 4]

[0241] Composition (2) was applied to a glass support (1) using a spin coater, heated at 80°C for 2 minutes on a hot plate, and the solvent was evaporated. At this time, the application conditions of the spin coater were adjusted so that the thickness after drying was 5 μm. Next, the applied composition was exposed (exposure amount: 500 mJ / ㎠, illuminance: 200 mW / ㎠) using a conveyor-type exposure machine to cure the composition (2), thereby producing a substrate (form of substrate (3)) having a resin layer containing pigment (A) on one side of the glass support (1).

[0242] The spectral transmittance of light incident from a direction perpendicular to the plane direction of this substrate was measured, and (Xa), (Xb), the average value of transmittance at wavelengths of 430 to 560 nm, and the maximum value of transmittance at wavelengths of 700 to 750 nm were calculated. The results are shown in Fig. 5 and Table 3.

[0243] Next, dielectric multilayer films were formed on both sides of the obtained substrate in the same procedure as in Example 1, and a near-infrared cut filter with a thickness of about 0.210 mm was obtained. The results are shown in Table 3.

[0244] [Example 5]

[0245] 100 parts by mass of resin A obtained in Synthesis Example 1 and methylene chloride (solvent (1)) were added to a container to obtain a solution with a resin concentration of 20 mass%. Next, the obtained solution was cast onto a smooth glass plate, dried at 20°C for 8 hours, and then peeled off from the glass plate. The peeled film was further dried at 100°C under reduced pressure for 8 hours to obtain a resin support (2) with a thickness of 0.1 mm, a length of 60 mm, and a width of 60 mm. Except for using the obtained resin support (2) instead of the glass support (1), a cured layer of composition (2) was formed on one side of the resin support in the same procedure as in Example 4, and a substrate (substrate shape (4)) having a resin layer containing pigment (A) on one side of the resin support was obtained.

[0246] The spectral transmittance of light incident from a direction perpendicular to the plane direction of this substrate was measured, and (Xa), (Xb), the average value of transmittance at wavelengths from 430 to 560 nm, and the maximum value of transmittance at wavelengths from 700 to 750 nm were calculated. The results are shown in Table 3.

[0247] Next, dielectric multilayer films were formed on both sides of the obtained substrate in the same procedure as in Example 1, and a near-infrared cut filter with a thickness of about 0.110 mm was obtained. The results are shown in Table 3.

[0248] [Example 6]

[0249] A substrate (form of substrate (2)) having resin layers on both sides of a transparent resin substrate containing pigment (A) was obtained in the same procedure as in Example 3, except that 0.10 parts by mass of compound (a-1), 0.05 parts by mass of compound (a-5), and 0.15 parts by mass of compound (a-6) were used as pigment (A).

[0250] The spectral transmittance of light incident from a direction perpendicular to the plane direction of this substrate was measured, and (Xa), (Xb), the average value of transmittance at wavelengths of 430 to 560 nm, and the maximum value of transmittance at wavelengths of 700 to 750 nm were calculated. The results are shown in Fig. 6 and Table 3.

[0251] Next, dielectric multilayer films were formed on both sides of the obtained substrate in the same procedure as in Example 1, and a near-infrared cut filter with a thickness of about 0.111 mm was obtained. The results are shown in Table 3.

[0252] [Examples 7 to 9]

[0253] A substrate having resin layers on both sides of a transparent resin substrate and a near-infrared cut filter using the same were obtained in the same procedure as in Example 3, except that the thickness of the transparent resin substrate and the amount of pigment (A) and compound (X) added were changed as shown in Table 3. The results are shown in Table 3.

[0254] [Example 10]

[0255] A substrate and a near-infrared cut filter were fabricated and evaluated in the same manner as in Example 1, except that the drying conditions of the resin, pigment (A), solvent, and resin substrate were changed as shown in Table 3. The results are shown in Table 3.

[0256] [Example 11]

[0257] A substrate and a near-infrared cut filter were prepared and evaluated in the same manner as in Example 3, except that the type and amount of pigment (A) were changed as shown in Table 3 and 0.01 parts by mass of pigment (B) were used. The results are shown in Table 3.

[0258] [Example 12]

[0259] A substrate and a near-infrared cut filter were prepared and evaluated in the same manner as in Example 3, except that the type and amount of pigment (A) added were changed as shown in Table 3. The results are shown in Table 3.

[0260] [Comparative Example 1]

[0261] A substrate (form of substrate (5)) having resin layers on both sides of a transparent resin substrate containing pigment (A) and pigment (B) was obtained in the same procedure as in Example 3, except that 0.10 parts by mass of compound (a-5) as pigment (A) and 0.04 parts by mass of compound (b-1) as pigment (B) were used.

[0262] The spectral transmittance of light incident from a direction perpendicular to the plane direction of this substrate was measured, and (Xa), (Xb), the average value of transmittance at wavelengths from 430 to 560 nm, and the maximum value of transmittance at wavelengths from 700 to 750 nm were calculated. The results are shown in Fig. 7 and Table 3.

[0263] Next, dielectric multilayer films were formed on both sides of the obtained substrate in the same procedure as in Example 1, and a near-infrared cut filter with a thickness of about 0.111 mm was obtained. The results are shown in Table 3.

[0264] As a result of evaluating camera image capture using the near-infrared cut filter obtained in Comparative Example 1, in addition to showing significant flare around the light source, red excitation on a black background was also confirmed. It is considered that the former is due to the large amount of pigment containing a high emission quantum yield, and the latter is due to the high maximum transmittance of the substrate at a wavelength of 700 to 750 nm being 9.9%.

[0265] [Comparative Example 2]

[0266] A substrate (form of the substrate (5)) having resin layers on both sides of a transparent resin substrate containing pigment (A) and pigment (B) was obtained in the same procedure as in Example 3, except that 0.10 parts by mass of compound (a-1) and 0.04 parts by mass of compound (a-3) were used as pigment (A), 0.04 parts by mass of compound (b-1) as pigment (B), and 0.10 parts by mass of compound (x-1) as compound (X).

[0267] The spectral transmittance of light incident from a direction perpendicular to the plane direction of this substrate was measured, and (Xa), (Xb), the average value of transmittance at wavelengths of 430 to 560 nm, and the maximum value of transmittance at wavelengths of 700 to 750 nm were calculated. The results are shown in Fig. 8 and Table 3.

[0268] Next, dielectric multilayer films were formed on both sides of the obtained substrate in the same procedure as in Example 1, and a near-infrared cut filter with a thickness of about 0.111 mm was obtained. The results are shown in Table 3.

[0269] As a result of evaluating camera image capture using the near-infrared cut filter obtained in Comparative Example 2, in addition to showing significant flare around the light source, red excitation on a black background was also confirmed. The former is attributed to the large amount of pigment containing a high emission quantum yield, and the latter is attributed to the fact that the maximum transmittance of the substrate at a wavelength of 700 to 750 nm is 5.5%, which is high and does not possess sufficient absorption characteristics to suppress red excitation.

[0270] [Comparative Example 3]

[0271] A substrate having resin layers on both sides of a transparent resin substrate containing pigment (A) and pigment (B) was obtained in the same procedure as in Example 3, except that 0.20 parts by mass of compound (a-2) and 0.10 parts by mass of compound (a-5) and 0.04 parts by mass of compound (b-1) were used as pigment (A), and pigment (B) was used.

[0272] The spectral transmittance of light incident from a direction perpendicular to the plane direction of this substrate was measured, and (Xa), (Xb), the average value of transmittance at wavelengths of 430 to 560 nm, and the maximum value of transmittance at wavelengths of 700 to 750 nm were calculated. The results are shown in Fig. 9 and Table 3.

[0273] Next, dielectric multilayer films were formed on both sides of the obtained substrate in the same procedure as in Example 1, and a near-infrared cut filter with a thickness of about 0.111 mm was obtained. The results are shown in Table 3.

[0274] As a result of evaluating camera image capture using the near-infrared cut filter obtained in Comparative Example 3, a slight flare was observed around the light source. It is considered that this is because it contains a large amount of pigment with a high emission quantum yield.

[0275] [Comparative Example 4]

[0276] A substrate (form of the substrate (5)) having resin layers on both sides of a transparent resin substrate containing pigment (A) and pigment (B) was obtained in the same procedure as in Example 3, except that 0.08 parts by mass of compound (a-4) and 0.15 parts by mass of compound (a-6) and 0.04 parts by mass of compound (b-2) were used as pigment (A).

[0277] The spectral transmittance of light incident from a direction perpendicular to the plane direction of this substrate was measured, and (Xa), (Xb), the average value of transmittance at wavelengths of 430 to 560 nm, and the maximum value of transmittance at wavelengths of 700 to 750 nm were calculated. The results are shown in FIG. 10 and Table 3.

[0278] Next, dielectric multilayer films were formed on both sides of the obtained substrate in the same procedure as in Example 1, and a near-infrared cut filter with a thickness of about 0.111 mm was obtained. The results are shown in Table 3.

[0279] As a result of evaluating camera image capture using the near-infrared cut filter obtained in Comparative Example 4, a slight flare was observed around the light source. It is considered that this is due to the large amount of pigment containing a high emission quantum yield.

[0280] [Comparative Example 5]

[0281] A substrate (form of substrate (2)) having resin layers on both sides of a transparent resin substrate containing pigment (A) was obtained in the same procedure as in Example 3, except that 0.15 parts by mass of compound (a-2) and 0.15 parts by mass of compound (a-3) were used as pigment (A).

[0282] The spectral transmittance of light incident from a direction perpendicular to the plane direction of this substrate was measured, and (Xa), (Xb), the average value of transmittance at wavelengths of 430 to 560 nm, and the maximum value of transmittance at wavelengths of 700 to 750 nm were calculated. The results are shown in FIG. 11 and Table 3.

[0283] Next, dielectric multilayer films were formed on both sides of the obtained substrate in the same procedure as in Example 1, and a near-infrared cut filter with a thickness of about 0.111 mm was obtained. The results are shown in Table 3.

[0284] As a result of evaluating camera image capture using the near-infrared cut filter obtained in Comparative Example 5, red excitation on a black background was confirmed. It is considered that this is because the maximum transmittance of the substrate at a wavelength of 700 to 750 nm was high at 4.1%, and it did not have sufficient absorption characteristics to suppress red excitation.

[0285] [Comparative Example 6]

[0286] A substrate (form of the substrate (5)) having resin layers on both sides of a transparent resin substrate containing pigments (A) and pigments (B) was obtained in the same procedure as in Example 3, except that 0.04 parts by mass of compound (a-1) and 0.15 parts by mass of compound (a-2) and 0.04 parts by mass of compound (b-3) were used as pigments (A).

[0287] The spectral transmittance of light incident from a direction perpendicular to the plane direction of this substrate was measured, and (Xa), (Xb), the average value of transmittance at wavelengths of 430 to 560 nm, and the maximum value of transmittance at wavelengths of 700 to 750 nm were calculated. The results are shown in FIG. 12 and Table 3.

[0288] Next, dielectric multilayer films were formed on both sides of the obtained substrate in the same procedure as in Example 1, and a near-infrared cut filter with a thickness of about 0.111 mm was obtained. The results are shown in Table 3.

[0289] As a result of evaluating camera image capture using the near-infrared cut filter obtained in Comparative Example 6, significant flare was observed around the light source. It is considered that this is due to the large amount of pigment containing a high emission quantum yield.

[0290] [Comparative Example 7]

[0291] A substrate having resin layers on both sides of a transparent resin substrate containing only pigment (A) and a near-infrared cut filter were fabricated and evaluated in the same manner as Comparative Example 6, except that the type and amount of pigment (A) added were changed as shown in Table 3. The results are shown in Table 3.

[0292] As a result of evaluating camera image capture using the near-infrared cut filter obtained in Comparative Example 7, red excitation on a black background was confirmed. It is considered that this is because the maximum transmittance of the substrate at a wavelength of 700 to 750 nm is high at 12.3%, and it does not have sufficient absorption characteristics to suppress red excitation.

[0293] [Comparative Example 8]

[0294] A substrate having resin layers on both sides of a transparent resin substrate containing only pigment (A) and a near-infrared cut filter were fabricated and evaluated in the same manner as Comparative Example 6, except that the type and amount of pigment (A) added were changed as shown in Table 3. The results are shown in Table 3.

[0295] As a result of evaluating camera image capture using the near-infrared cut filter obtained in Comparative Example 8, red excitation on a black background was confirmed. It is considered that this is because the maximum transmittance of the substrate at a wavelength of 700 to 750 nm is high at 5.5%, and it does not have sufficient absorption characteristics to suppress red excitation.

[0296]

Claims

Claim 1 A near-infrared cut filter having a substrate including a resin layer, wherein the resin layer comprises a resin and two or more pigments (A), wherein each of the two or more pigments (A) independently has an absorption maximum wavelength at 650 to 820 nm and has a luminescence quantum yield of less than 22%, and the resin layer substantially does not contain a pigment (B) having an absorption maximum wavelength at 650 to 820 nm and has a luminescence quantum yield of 22% or more, and wherein the maximum value of the transmittance when measured from the vertical direction of the substrate in a region of 700 to 750 nm is 2.0% or less. Claim 2 A near-infrared cut filter according to claim 1, wherein among the two or more types of pigments (A), the pigment (A) having the shortest wavelength at maximum absorption is denoted as pigment (A1) and the pigment (A) having the longest wavelength at maximum absorption is denoted as pigment (A2), wherein pigment (A1) has a maximum absorption wavelength (λ1) (nm) at a wavelength of 650 to 760 nm, pigment (A2) has a maximum absorption wavelength (λ2) (nm) at a wavelength of 730 to 820 nm, and the difference in maximum absorption wavelengths (|λ2-λ1|) is 10 to 110 nm. Claim 3 A near-infrared cut filter having a dielectric multilayer film in claim 1. Claim 4 An optical element having a near-infrared cut filter as described in any one of claims 1 to 3. Claim 5 A camera module having a near-infrared cut filter as described in any one of claims 1 to 3.