Glass thread, glass cloth, prepreg, and printed circuit boards

The glass cloth with controlled silicon content and snarl index, treated with specific silane coupling agents, addresses the issues of flatness and dielectric loss in printed circuit boards, enhancing their performance and reliability.

KR1020260164604APending Publication Date: 2026-11-17ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
KR1020267034192
Authority / Receiving Office
KR · KR
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-05-09
Filing Date
2024-12-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing glass cloths used in printed circuit boards face issues with reduced yield due to cylindrical grinding requirements for improved flatness and increased dielectric loss tangent due to residual silane coupling agents, leading to fluffing and poor signal transmission.

Method used

A glass cloth composed of glass threads with a silicon content of 95.0 to 100 mass% in terms of silicon dioxide (SiO2) and a snarl index of 400 mm or less, treated with a silane coupling agent that does not form salts, and woven with controlled twist differences, to enhance flatness and reduce lint generation.

Benefits of technology

The solution provides glass cloths with improved flatness, reduced lint frequency, and enhanced dielectric properties, suitable for high-performance printed circuit boards and electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCT00007_ABST
    Figure PCT00007_ABST
Patent Text Reader

Abstract

The problem that the invention aims to solve is to provide a glass cloth having excellent flatness and a reduced frequency of lint generation. The glass cloth of the present invention is a glass cloth composed of glass threads, wherein the silicon (Si) content in the glass threads is 95.0 to 100 mass% in terms of silicon dioxide (SiO2), and furthermore, the snarl index of the glass threads is 400 mm or less. Alternatively, the glass cloth of the present invention is a glass cloth composed of glass threads, wherein the bulk dielectric loss tangent of the glass constituting the glass threads at 10 GHz is in the range of 0.001 or less, and furthermore, the snarl index of the glass threads is 400 mm or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present disclosure relates to glass threads, glass cloths, prepregs, and printed circuit boards, etc. Background Technology

[0002] Currently, there is a growing demand for high-performance information terminals such as smartphones and high-speed communication represented by 5G. Against this backdrop, there is a demand for printed circuit boards for high-speed communication not only for the improvement of heat resistance that has been conventionally required, but also for further improvement in the dielectric properties of their insulating materials (e.g., low dielectric loss tangent). Similarly, there is a demand for improved dielectric properties for prepregs used as insulating materials for printed circuit boards, as well as for glass threads and glass cloths included in said prepregs.

[0003] In order to achieve low dielectric properties in insulating materials, a method of constructing an insulating material using a prepreg in which a low dielectric resin (hereinafter referred to as "matrix resin") is impregnated into a glass cloth is known (e.g., Patent Documents 1 and 2). Patent Documents 1 and 2 describe the purpose that polyphenylene ethers terminally modified with vinyl groups or methacrylate oxy groups are advantageous for low dielectric properties and heat resistance, and that these modified polyphenylene ethers are used as matrix resins.

[0004] In addition, for the purpose of improving flatness and stabilizing signal transmission speed in glass cloths, it has been reported that a glass yarn is used having a bending point with a radius of curvature of 5 mm or less and a bending angle of 120 degrees or less, and a yarn bending density of 0.10 pieces / cm or less (see, for example, Patent Document 3). Patent Document 3 describes a method in which a silica glass ingot having a desired roundness is obtained by cylindrically grinding a silica glass ingot using a cylindrical grinding machine, and a glass filament, which is a raw material for glass yarn, is obtained by using such a silica glass ingot having the desired roundness.

[0005] He is explaining.

[0006] In addition, an invention has been reported that includes the requirements of surface treating the glass cloth with a silane coupling agent and adjusting the loss on ignition value of the glass cloth to 0.13 to 0.40 mass% (see, for example, Patent Document 4). Patent Document 4 explains that for a glass cloth made by weaving a glass yarn containing a glass filament with a silicon dioxide (SiO2) composition of 98 to 100 mass%, by adjusting the loss on ignition value of the glass cloth to the above range, it is possible to improve insulation reliability and also suppress the occurrence of fluff on the glass cloth.

[0007] In addition, as an invention in the same technical field, the invention described in Patent Document 5 has been reported. Prior art literature

[0008] International Publication No. 2019 / 065940 International Publication No. 2019 / 065941 Japanese Patent Publication No. 2020-90432 Japanese Patent Publication No. 2018-127747 International Publication No. 2022 / 215288 The problem to be solved

[0009] However, in the invention described in Patent Document 3, there was a problem that the yield was reduced because cylindrical grinding of the silica glass ingot was required. Therefore, there was a strong demand for a technology that improves the flatness of the glass cloth without requiring special processing such as cylindrical grinding.

[0010] In addition, as described in Patent Document 4, in an invention that includes the requirement of surface-treating a glass cloth with a silane coupling agent, there was a problem that if the silane coupling agent remained unintended on the glass surface, the dielectric loss tangent of the glass cloth would increase (see, for example, the above Patent Document 5). Therefore, there was a strong demand for the creation of a technology to suppress fluffing of the glass cloth as a means other than the means of adjusting the loss on ignition value.

[0011] The object of the present disclosure is to provide a glass cloth having excellent flatness and a reduced frequency of lint generation. Another object of the present disclosure is to provide a method for manufacturing a glass cloth, a glass cloth package, and a glass cloth capable of providing such a glass cloth. Another object of the present disclosure is to provide prepregs, printed circuit boards, integrated circuits, and electronic devices using such a glass cloth. means of solving the problem

[0012] Examples of embodiments of the present disclosure are as follows.

[0013] [1]

[0014] It is a glass cloth composed of glass threads,

[0015] A glass cloth having a silicon (Si) content of 95.0 to 100 mass% in terms of silicon dioxide (SiO2) in the above glass thread, and also having a snarl index of 400 mm or less.

[0016] [2]

[0017] It is a glass cloth composed of glass threads,

[0018] A glass cloth in which the bulk dielectric loss tangent of the glass constituting the glass thread at 10 GHz is in the range of 0.001 or less, and the snar index of the glass thread is 400 mm or less.

[0019] [3]

[0020] A glass cloth as described in Item 1 or 2, having a snail index of the glass thread of the above glass of 70 mm or more.

[0021] [4]

[0022] The above glass seal is within the range described in the following formulas (A), (B), and (C);

[0023] (A) x+y+z=100 mass%

[0024] (B) x≥99.5 mass%

[0025] (C) 0.0003ppm≤y≤0.50ppm

[0026] x: Silicon content converted to silicon dioxide (SiO2)

[0027] y: Total content of uranium and thorium

[0028] z: Total content of elements other than silicon, uranium, and thorium

[0029] A glass cloth as described in Item 1 or 2, comprising a glass thread satisfying [ ].

[0030] [5]

[0031] A glass cloth as described in Item 4, wherein the range of x above is 99.6 mass% or more.

[0032] [6]

[0033] A glass cloth as described in Item 4, wherein the range of x above is 99.9 mass% or more.

[0034] [7]

[0035] A glass cloth described in any one of items 1 to 6, wherein the glass thread is treated with a surface treatment agent comprising a silane coupling agent.

[0036] [8]

[0037] The above surface treatment agent is the following formula (1):

[0038] X(R) 3-n SiY n ···(1)

[0039] (In formula (1), X is an organic functional group having at least one of an amino group and an unsaturated double bond group having radical reactivity, Y is each independently an alkoxy group, n is an integer from 1 to 3, and R is each independently a group selected from the group consisting of a methyl group, an ethyl group, and a phenyl group)

[0040] A glass cloth described in Item 7 comprising the above-mentioned silane coupling agent represented by .

[0041] [9]

[0042] The glass cloth described in item 8, wherein X in the above formula (1) is an organic functional group that does not form a salt with an ionic compound.

[0043]

[10]

[0044] Glass cloth as described in item 8 or 9, wherein X in the above formula (1) does not contain an amine and / or ammonium cation.

[0045]

[11]

[0046] A glass cloth described in any one of items 8 to 10, wherein X in the above formula (1) is an organic functional group having a methacryloxy group and / or an acryloxy group.

[0047]

[12]

[0048] A glass cloth described in any one of items 1 to 11, wherein the absolute value of the number of twists of the glass thread is in the range of 0.5 to 1.5 twists / 25 mm.

[0049]

[13]

[0050] The above glass cloth is formed by having the above glass threads as warp and weft threads, and

[0051] A glass cloth described in any one of items 1 to 12, wherein the absolute value of the difference in the number of twists of the warp and weft yarns is in the range of 0.01 to 0.70 twists / 25 mm.

[0052]

[14]

[0053] A glass cloth described in any one of items 1 to 13, having a thickness of 60 μm or less.

[0054]

[15]

[0055] A glass cloth for printed circuit boards, as described in any one of items 1 to 14.

[0056]

[16]

[0057] A prepreg containing a glass cloth as described in any one of items 1 to 15 and a thermosetting resin.

[0058]

[17]

[0059] A printed circuit board comprising the prepreg described in Item 16.

[0060]

[18]

[0061] An integrated circuit comprising a printed circuit board as described in Item 17.

[0062]

[19]

[0063] An electronic device comprising a printed circuit board as described in Item 17.

[0064]

[20]

[0065] This is a method for manufacturing glass cloth, and

[0066] The silicon (Si) content in the glass wire is in the range of 95.0 to 100 mass% in terms of silicon dioxide (SiO2), and

[0067] A method for manufacturing a glass cloth, comprising a process of obtaining a glass cloth using a glass thread having a snarl index of 400 mm or less.

[0068]

[21]

[0069] This is a method for manufacturing glass cloth, and

[0070] The bulk dielectric loss tangent of the glass constituting the glass chamber at 10 GHz is in the range of 0.001 or less, and

[0071] A method for manufacturing a glass cloth, comprising a process of obtaining a glass cloth using a glass thread having a snarl index of 400 mm or less.

[0072]

[22]

[0073] A method for manufacturing a glass cloth as described in item 20 or 21, wherein the snarl index of the glass thread is 70 mm or more.

[0074]

[23]

[0075] The above glass seal is within the range described in the following formulas (A), (B), and (C);

[0076] (A) x+y+z=100 mass%

[0077] (B) x≥99.5 mass%

[0078] (C) 0.0003ppm≤y≤0.50ppm

[0079] x: Silicon content converted to silicon dioxide (SiO2)

[0080] y: Total content of uranium and thorium

[0081] z: Total content of elements other than silicon, uranium, and thorium

[0082] A method for manufacturing a glass cloth as described in Item 20 or 21, comprising a process of obtaining a glass cloth using a glass thread that satisfies the above.

[0083]

[24]

[0084] A process for shaping the glass thread used as a warp (warp shaping process), and

[0085] A process of weaving using the above glass yarn (weaving process)

[0086] Includes,

[0087] A method for manufacturing a glass cloth as described in any one of items 20 to 23, wherein, in the warp warping process and / or the weaving process, the absolute value of the number of twists of the glass yarn is adjusted to a range of 0.5 to 1.5 times / 25 mm.

[0088]

[25]

[0089] The above glass cloth has the above glass threads as warp and weft,

[0090] A method for manufacturing a glass cloth as described in Item 24, comprising a process of adjusting the twist count of the weft yarn so that the absolute value of the difference between the twist count of the warp yarn and the twist count of the weft yarn is in the range of 0.01 to 0.70 twists / 25 mm.

[0091]

[26]

[0092] A method for manufacturing a glass cloth as described in Item 24 or 25, using a glass yarn in which the value obtained by dividing the yarn width of the glass yarn by TEX is in the range of 10 to 30, and performing the warp warping process and / or the weaving process.

[0093]

[27]

[0094] A glass yarn package having a core material and a glass yarn wound on the core material, and

[0095] A glass thread package wherein the silicon (Si) content in the glass thread is 95.0 to 100 mass% in terms of silicon dioxide (SiO2), and the snar index of the glass thread is 400 mm or less.

[0096]

[28]

[0097] A glass thread package as described in Item 27, having a snarl index of 70 mm or more of the glass thread.

[0098]

[29]

[0099] The above glass seal is within the range described in the following formulas (A), (B), and (C);

[0100] (A) x+y+z=100 mass%

[0101] (B) x≥99.5 mass%

[0102] (C) 0.0003ppm≤y≤0.50ppm

[0103] x: Silicon content converted to silicon dioxide (SiO2)

[0104] y: Total content of uranium and thorium

[0105] z: Total content of elements other than silicon, uranium, and thorium

[0106] Glass seal package as listed in item 27 or 28, satisfying [the condition].

[0107]

[30]

[0108] A glass thread package described in any one of items 27 to 29, wherein the absolute value of the number of twists of the glass thread is in the range of 0.5 to 1.5 twists / 25 mm.

[0109]

[31]

[0110] A glass thread package described in item 27 or 28, wherein the value obtained by dividing the thread width of the glass thread by TEX is in the range of 10 to 30.

[0111]

[32]

[0112] It is a glass thread used in the weaving of glass cloth,

[0113] A glass thread having a silicon (Si) content of 95.0 to 100 mass% in terms of silicon dioxide (SiO2) in the above glass thread, and also having a snarl index of 400 mm or less.

[0114]

[33]

[0115] A glass thread as described in Item 32, having a snarl index of 70 mm or more.

[0116]

[34]

[0117] The above glass seal is within the range described in the following formulas (A), (B), and (C);

[0118] (A) x+y+z=100 mass%

[0119] (B) x≥99.5 mass%

[0120] (C) 0.0003ppm≤y≤0.50ppm

[0121] x: Silicon content converted to silicon dioxide (SiO2)

[0122] y: Total content of uranium and thorium

[0123] z: Total content of elements other than silicon, uranium, and thorium

[0124] A glass thread as described in item 32 or 33 that satisfies

[0125]

[35]

[0126] A glass chamber described in Item 34, wherein y, representing the total content of the above uranium and thorium, is in the range of 0.0003 to 0.0010 ppm.

[0127]

[36]

[0128] A glass chamber described in Item 34, wherein y, representing the total content of the above uranium and thorium, is in the range of greater than 0.0010 and less than or equal to 0.0015 ppm.

[0129]

[37]

[0130] A glass chamber described in Item 34, wherein y, representing the total content of the above uranium and thorium, is in the range of greater than 0.0015 and less than or equal to 0.0018 ppm.

[0131]

[38]

[0132] A glass chamber described in Item 34, wherein y, representing the total content of the above uranium and thorium, is in the range of greater than 0.0018 and less than or equal to 0.0035 ppm.

[0133]

[39]

[0134] A glass chamber described in Item 34, wherein y, representing the total content of the above uranium and thorium, is in the range of greater than 0.0035 and less than or equal to 0.0040 ppm.

[0135]

[40]

[0136] A glass chamber described in Item 34, wherein y, representing the total content of the above uranium and thorium, is in the range of greater than 0.0040 and less than or equal to 0.09 ppm.

[0137]

[41]

[0138] A glass chamber described in Item 34, wherein y, representing the total content of the above uranium and thorium, is in the range of greater than 0.09 and less than or equal to 0.12 ppm.

[0139]

[42]

[0140] A glass chamber described in Item 34, wherein y, representing the total content of the above uranium and thorium, is in the range of greater than 0.12 and less than or equal to 0.50 ppm.

[0141]

[43]

[0142] A glass thread described in any one of items 32 to 42, wherein the snar index of the glass thread is in the range of 330 to 400 mm.

[0143]

[44]

[0144] A glass thread described in any one of items 32 to 42, wherein the snar index of the glass thread is in the range of 300 to 329 mm.

[0145]

[45]

[0146] A glass thread described in any one of items 32 to 42, wherein the snar index of the glass thread is in the range of 220 to 299 mm.

[0147]

[46]

[0148] A glass thread described in any one of items 32 to 42, wherein the snar index of the glass thread is in the range of 200 to 219 mm.

[0149]

[47]

[0150] A glass thread described in any one of items 32 to 42, wherein the snar index of the glass thread is in the range of 125 to 199 mm.

[0151]

[48]

[0152] A glass thread described in any one of items 32 to 42, wherein the snar index of the glass thread is in the range of 110 to 124 mm.

[0153]

[49]

[0154] A glass thread described in any one of items 32 to 42, wherein the snarl index of the glass thread is 110 mm or less. Effects of the invention

[0155] According to the present disclosure, a glass cloth having excellent flatness and a reduced frequency of lint generation can be provided. Furthermore, according to the present disclosure, a method for manufacturing such a glass cloth, a glass cloth package, and a glass cloth can be provided. Furthermore, according to the present disclosure, prepregs, printed circuit boards, integrated circuits, and electronic devices using such a glass cloth can be provided. Brief explanation of the drawing

[0156] FIG. 1 is a schematic diagram illustrating a method for measuring the amount of bending in the present disclosure. FIG. 2 is a schematic diagram illustrating a method for measuring the amount of bending in the present disclosure. Specific details for implementing the invention

[0157] Hereinafter, examples of embodiments of the present disclosure will be described. However, the present disclosure is not limited to the embodiments described below, and therefore various modifications are possible within the scope of not departing from the gist thereof.

[0158] In this specification, if multiple structures represented by the same reference numeral exist within the same formula, unless otherwise specified, said structures may be selected independently and may be identical or different from one another. In the case where multiple structures represented by the same reference numeral exist within different formulas, unless otherwise specified, said structures may be selected independently and may be identical or different from one another. Furthermore, in this specification, upper or lower limits in numerical ranges described in steps may be substituted with upper or lower limits in corresponding numerical ranges described in other steps, or may be substituted with corresponding values ​​described in the embodiments. Additionally, regarding the term "process" in this specification, it is included in this term not only when it is an independent process, but also when it cannot be clearly distinguished from other processes, provided that the function of the process is achieved. In the contents illustrated in the drawings, scales, shapes, and lengths may be exaggerated to enhance clarity.

[0159] Glass Cloth

[0160] <Overall Composition>

[0161] The glass cloth of the present disclosure is a glass cloth composed of glass threads, wherein the silicon (Si) content in the glass threads is 95.0 to 100 mass% in terms of silicon dioxide (SiO2), and furthermore, the snarl index of the glass threads is in the range of 400 mm or less.

[0162] In addition, the glass cloth of the present disclosure is a glass cloth composed of glass threads, wherein the bulk dielectric loss tangent of the glass constituting the glass threads at 10 GHz is in the range of 0.001 or less, and furthermore, the snarl index of the glass threads is in the range of 400 mm or less.

[0163] The inventors have provided a glass thread advantageous for improving the dielectric properties of a glass cloth, for example, (1), and / or (2);

[0164] (1) A glass wire having a silicon (Si) content of 95.0 to 100 mass% in terms of silicon dioxide (SiO2),

[0165] (2) A glass silt in which the bulk dielectric loss tangent at 10 GHz of the glass constituting the glass silt is in the range of 0.001 or less.

[0166] In this regard, it was discovered that residual stress is prone to occur in glass cloths obtained using this method, and that such glass threads tend to have a high snarl index. The inventors also discovered that glass cloths made using glass threads with a high snarl index have an adverse effect on the flatness (bending state) of the glass cloth.

[0167] Here, snarl refers to the twisting that occurs in a twisted yarn to reverse its twist, and in this specification, a higher snarl index means that snarl is more likely to occur. Furthermore, in JIS-L-0210:1981, Section 3.1, Item 1113, snarl is defined as "the entanglement of yarn caused by twisting when a twisted yarn is unraveled." In this regard, conventionally, how the snarl index affects the quality of glass cloth has not been examined.

[0168] Furthermore, the inventors have discovered that with respect to a glass yarn (referred to as a "glass yarn package" in this disclosure) wound on a core material (in one embodiment, a bobbin), the higher the snar index of the glass yarn, the more likely the glass yarn is to rub against the surface of the bobbin and be loosened when the glass yarn is released from the bobbin; as a result, lint is more likely to form on the surface of the glass cloth obtained using the glass yarn. In particular, the inventors have also discovered that in the process of warping the glass yarn used as the warp of the glass cloth (warp warping process), the speed of loosening the glass yarn is slower than in the process of weaving using the glass yarn (weaving process), and therefore the glass yarn tends to rub against the surface of the bobbin.

[0169] Therefore, the inventors, having conducted an investigation from the perspective of reducing the snarl index, discovered that the snarl index can be adjusted by the spinning conditions of the glass yarn. In one preferred embodiment, a glass yarn is produced from a glass rod having a silicon content of 99.5 mass% or more. At this time, after heating and stretching the glass rod, an annealing treatment can be performed to reduce the residual stress occurring in the glass yarn (in one embodiment, to relieve the residual stress). According to the present disclosure, a glass cloth can be provided that uses a glass yarn with a controlled snarl index, thereby improving flatness and also reducing the frequency of lint generation.

[0170] The weight per unit area of ​​the glass cloth (mass of the glass cloth) is preferably 8 to 250 g / m², more preferably 8 to 100 g / m², even more preferably 8 to 80 g / m², and particularly preferably 8 to 50 g / m². If the weight per unit area of ​​the glass cloth is within the above range, the effects of the present disclosure are easily obtained.

[0171] The thickness of the glass cloth is preferably 60 μm or less, more preferably 55 μm or less, and even more preferably 50 μm or less. If the thickness of the glass cloth is within the above range, the effects of the present disclosure are easily obtained. The thickness of the glass cloth may be greater than 0 μm and greater than 5 μm, or greater than 5 μm.

[0172] Glass Thread

[0173] The snar index of the glass thread is in the range of 400 mm or less. When a twist is applied to the thread, a twisting torque is generated to reverse the twist, and at this time, twisting may occur in the thread. In this specification, such twisting is referred to as "snaring," and as an indicator of the ease with which this snaring occurs, it is possible to use a snaring index such as that described in JIS L1095, for example.

[0174] It is known that glass yarn (glass thread) suitable for use in printed circuit boards, such as glass yarn, is obtained by melting glass in a melting furnace, extruding it from a nozzle to obtain a glass filament with a diameter of several μm, and then processing this filament.

[0175] Meanwhile, quartz glass with a silicon (Si) content of 95.0 to 100 mass% in terms of silicon dioxide (SiO2) has a much higher melting point than other glasses. For this reason, it differs from the aforementioned E glass yarn, etc., in that the glass filament, which serves as its raw material, is obtained by heating and stretching a quartz glass rod (quartz glass ingot). When a quartz glass rod is heated and stretched, the siloxane bonds constituting the glass are oriented in the stretching direction, and in this case, residual stress is likely to occur in the obtained glass filament.

[0176] The inventors have discovered that due to this residual stress, "snarl," which was not recognized as a problem in conventional glass yarns, adversely affects the fluff quality and flatness of glass cloths. Specifically, the higher the snarl index of the glass yarn, the more likely the glass yarn is to come into contact with the surface of the bobbin when the glass yarn is released from the bobbin during the warp warping of the glass cloth; as a result, fluff is more likely to occur on the surface of the glass cloth. Furthermore, glass yarns with a high snarl index are prone to adversely affecting the flatness (bending) of the glass cloth because the bending of the yarn becomes stronger in the state of the glass cloth.

[0177] Regarding "snarl," which is not recognized as a problem in conventional glass yarns, a method of annealing the glass filament or glass yarn immediately after heating and stretching is preferred in order to reduce the snarl index of the quartz glass yarn beyond the conventional level. This method is relatively simple and is also advantageous in providing a glass cloth with excellent fluff quality and flatness.

[0178] As a result of the inventors' investigation, it was found that by setting the snarl index of the glass thread to 400 mm or less, it is possible to perform warp warping while reducing the frequency of lint generation on the surface of the glass cloth. From the perspective of obtaining the effects of the present disclosure, the snarl index of the glass thread is preferably 70 to 400 mm. From the perspective of lint suppression on the glass surface, the upper limit of the snarl index is preferably 380 mm or less, more preferably 370 mm or less, even more preferably 350 mm or less, even more preferably 330 mm or less, particularly preferably 310 mm or less, for example 300 mm or less, 250 mm or less, 200 mm or less, 150 mm or less, or 100 mm or less. The lower limit of the Snall index that can be arbitrarily combined with the upper limit of these may be 70 mm or more, 100 mm or more, 150 mm or more, 200 mm or more, 250 mm or more, 300 mm or more, or 330 mm or more. For example, from the viewpoint of being able to obtain the effects of the present disclosure, the snarl index of the glass thread is preferably in the range of 330 to 400 mm, 300 to 329 mm, or 220 to 299 mm; from the viewpoint of slightly emphasizing the fluff on the surface of the glass cloth in addition to the productivity of the glass thread, the range of 200 to 219 mm is preferably; from the viewpoint of more emphasizing the fluff on the surface of the glass cloth in addition to the productivity of the glass thread, the range of 125 to 199 mm is preferably; from the viewpoint of even more emphasizing the fluff on the surface of the glass cloth in addition to the productivity of the glass thread, the range of 110 to 124 mm is more preferably; and from the viewpoint of particularly emphasizing the fluff on the surface of the glass cloth in addition to the productivity of the glass thread, the range of 110 mm or less, for example, 70 to 110 mm or less is particularly preferably.

[0179] From the perspective of easily obtaining the effect of reducing the snar index by annealing treatment, it is preferable that the silicon (Si) content in the glass shard be 99.5 mass% or more in terms of silicon dioxide (SiO2), a range of 99.6 mass% or more is more preferable, a range of 99.7 mass% or more is even more preferable, a range of 99.8 mass% or more is even more preferable, a range of 99.9 mass% or more, and a range of 99.95 mass% or more is particularly preferable.

[0180] Glass cloth is obtained by weaving glass yarn (e.g., glass yarn containing multiple glass filaments) as warp and weft. The weaving structure of the glass cloth can be, for example, plain weave, lion weave, satin weave, and twill weave, among which a plain weave structure is preferred.

[0181] The type density of the warp and weft threads is preferably 10 to 120 threads / inch (= 10 to 120 threads / 25 mm), and more preferably 40 to 100 threads / inch. If the type density is within the above range, the effects of the present disclosure are easily obtained. The type densities of the warp and weft threads may be different from each other.

[0182] The glass fibers constituting the glass cloth can be obtained by including so-called "low dielectric glass" in the raw materials. The said glass fibers are

[0183] The ranges described in (A), (B), and (C);

[0184] (A) x+y+z=100 mass%

[0185] (B) x≥99.5 mass%

[0186] (C) 0.0003ppm≤y≤0.50ppm

[0187] x: Silicon content converted to silicon dioxide (SiO2)

[0188] y: Total content of uranium and thorium

[0189] z: Total content of elements other than silicon, uranium, and thorium

[0190] It is preferable to include a glass yarn that satisfies the ranges described in (A), (B), and (C), and it is more preferable that the glass yarn satisfies the ranges described in (A), (B), and (C). By using a glass yarn that satisfies the ranges described in (A), (B), and (C), it is easy to improve the dielectric properties of the glass cloth obtained, for example.

[0191] In terms of improving the dielectric properties of the glass cloth obtained, the range of x is preferably 99.6 mass% or more, more preferably 99.7 mass% or more, even more preferably 99.8 mass% or more, even more preferably 99.9 mass% or more, and particularly preferably 99.95 mass% or more.

[0192] It is preferable that the range of y be the range described in (C) above, namely 0.0003 ppm ≤ y ≤ 0.50 ppm. Since uranium (U) and thorium (Th) in glass threads can cause memory malfunction in electronic devices, it is desirable that their total content be as low as possible. As a result of the inventors' investigation, although the mechanism of action is not necessarily obvious, it was found that the total content of uranium and thorium influences the control of residual stress in glass threads and the adjustment of the snarl index. Specifically, the inventors found that, as a characteristic of glass threads made from glass rods with a silicon content of 99.5 mass% or more, if the total content of uranium and thorium is 0.0003 ppm or higher, it becomes easier to reduce residual stress in the glass threads. The inventors have also discovered that glass yarns with high residual stress tend to have a high snarl index due to their strong snarl force, and that glass cloths produced using such glass yarns are prone to bending and also tend to have poor flatness.

[0193] From the above perspective, it has been a general technical understanding that the total content of uranium (U) and thorium (Th) should be kept as low as possible. In contrast, from the perspective of increasing the flatness of the glass cloth, adjusting the total content of uranium and thorium to be included within an appropriate range has not been done until now. As a result of careful consideration, the inventors have found that the higher the total content of uranium and thorium in the glass cloth, the easier it is to exhibit the effect of annealing treatment to reduce the snarl index in the glass cloth. From the perspective of obtaining the effect of the above-described disclosure, the range of y may be in the range of 0.0003 ppm ≤ y ≤ 0.50 ppm, and the lower limit is preferably 0.001 ppm or higher, more preferably 0.003 ppm or higher, even more preferably 0.005 ppm or higher, even more preferably 0.007 ppm or higher, and particularly preferably 0.01 ppm or higher. The upper limit of y, which can be arbitrarily combined with these lower limits, is preferably in the range of 0.45 ppm or less, more preferably 0.40 ppm or less, even more preferably 0.35 ppm or less, even more preferably 0.30 ppm or less, and particularly preferably 0.25 ppm or less. If the range of y is 0.0003 ppm or more, it is easy to avoid a situation where residual stress generated during heat stretching increases because the purity of the silicon content in the glass is too high, and as a result, it becomes easy to control the snarl index of the glass thread to a range of 400 mm or less. On the other hand, if the range of y is 0.50 ppm or less, it becomes easy to avoid being affected by uranium and thorium, for example, memory malfunction in electronic devices containing glass threads as components, which becomes a usage problem. Furthermore, from the perspective of easily improving memory malfunction performance, a range of y of 0.0003 to 0.0010 ppm is preferred. In addition to memory malfunction performance, from the perspective of making it easy to lower the glass thread slash, y is greater than 0.0010 and 0.A range of 0.015 ppm or less is more preferable, and in addition to memory malfunction performance, a range of y greater than 0.0015 and less than or equal to 0.0018 ppm is more preferable, and in addition to memory malfunction performance, a range of y greater than 0.0018 and less than or equal to 0.0035 ppm is more preferable, and in addition to memory malfunction performance, a range of y greater than 0.0035 and less than or equal to 0.0040 ppm is more preferable, and in addition to memory malfunction performance, a range of y greater than 0.0040 and less than or equal to 0.0040 ppm is particularly preferable, in addition to memory malfunction performance, a range of y greater than 0.0040 and less than or equal to 0.09 ppm is particularly preferable, in addition to memory malfunction performance, a range of y greater than 0.0040 and less than or equal to 0.09 ppm is more preferable.

[0194] Bulk oil field loss

[0195] In this specification, the bulk dielectric loss tangent refers to the dielectric loss tangent measured at 10 GHz using a split cylinder resonator with respect to the raw material of the glass cloth. The raw material of the glass cloth may be, for example, glass bell, glass filament, glass thread, etc. The bulk dielectric loss tangent of the glass raw material constituting the glass cloth can be measured by a glass plate with a thickness of 300 μm or less having the same type and composition as the glass raw material, in the same way as the method for measuring the dielectric loss tangent of the glass cloth.

[0196] From the perspective of facilitating the effect of the present disclosure, the bulk dielectric loss tangent at 10 GHz is preferably 0.0009 or less, more preferably 0.0008 or less, even more preferably 0.0007 or less, even more preferably 0.0005 or less, even more preferably 0.0004 or less, particularly preferably 0.0003 or less, and most preferably 0.0002 or less. The bulk dielectric loss tangent may exceed 0.

[0197] <Average Openness of Glass Cloth>

[0198] The average openness of the glass cloth is preferably 38% or more or exceeding 40%, more preferably exceeding 43%, even more preferably exceeding 46%, exceeding 50%, exceeding 53%, exceeding 56%, or exceeding 60%, and particularly preferably exceeding 65%. If the average openness of the glass cloth is 38% or more, it is easy to suppress the presence of bubbles called voids within the bundles of glass threads when manufacturing prepreg or printed circuit boards containing it, and thereby, adverse effects on solder heat resistance and insulation reliability are unlikely to occur. Furthermore, if the average openness of the glass cloth is 38% or more, it is difficult to be affected by snarling of the glass threads; thus, even if glass threads with a relatively high snarling index are used, it is easy to ensure the flatness of the glass cloth.

[0199] Silane coupling agents

[0200] The glass threads (including glass filaments) constituting the glass cloth are preferably surface-treated with a silane coupling agent. That is, in one embodiment, the surface treatment agent for the glass threads includes a silane coupling agent. As a silane coupling agent, for example, the following formula (1):

[0201] X(R) 3-n SiY n ···(1)

[0202] {In Formula (1), X is an organic functional group having at least one of an amino group and an unsaturated double bond group having radical reactivity, Y is independently an alkoxy group, n is an integer from 1 to 3, and R is a group selected from the group consisting of methyl, ethyl, and phenyl groups}

[0203] It is desirable to include a silane coupling agent represented by .

[0204] Conventionally, the causes of the increase in dielectric loss tangent of glass cloth are thought to be (i) extremely small amounts of thermal oxidation deterioration products of the binder remaining in a state of being physically attached to the surface of the glass yarn, and (ii) residues or modified products thereof of the surface treatment agent that are physically attached without forming a chemical bond with the glass surface and cannot be reduced by washing with water. In order to suppress the occurrence of (i) thermal oxidation deterioration products and / or (ii) residues or modified products, it is preferable that X in Formula (1) is an organic functional group that does not form salts with ionic compounds. Furthermore, in terms of reactivity with the matrix resin, it is more preferable that X in Formula (1) is an organic functional group having a methacryloxy group and / or an acryloxy group. In terms of ease of obtaining the effects of the present disclosure, it is preferable that X in Formula (1) does not contain amines such as primary amines, secondary amines, and tertiary amines, and it is also preferable that it does not contain ammonium cations such as quaternary ammonium cations.

[0205] For Y in the above formula (1), as an alkoxy group, an alkoxy group having 1 to 5 carbon atoms (1, 2, 3, 4 or 5 carbon atoms) is preferred from the perspective of stabilizing treatment into glass cloth.

[0206] As a surface treatment agent, the silane coupling agent shown in Formula (1) may be used as a single agent, or X in Formula (1) may be used mixed with two or more other silane coupling agents. In addition, as the silane coupling agent shown in Formula (1), for example, vinyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, acryloxypropyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, 5-hexenyltrimethoxysilane, etc., may be used as a single agent or a mixture thereof.

[0207] The molecular weight of the silane coupling agent is preferably 100 to 600, more preferably 150 to 500, and even more preferably 200 to 450. Among these, it is particularly preferable to use two or more types of silane coupling agents with different molecular weights. By treating the glass sill using two or more types of silane coupling agents with different molecular weights, the density of the treatment agent on the glass surface increases, and thereby, the reactivity with the matrix resin tends to be further improved.

[0208] From the perspective that it is difficult to impede reactivity with the resin, it is preferable that the silane coupling agent be nonionic. Among nonionic silane coupling agents, a silane coupling agent having at least one group selected from the group consisting of vinyl groups, methacryloxy groups, and acryloxy groups is preferred, and among these, a silane coupling agent having a methacryloxy group and / or an acryloxy group is particularly preferred. By ensuring reactivity with the resin, it is easy to increase the heat resistance and reliability of the printed circuit board.

[0209] In one embodiment, in Formula (1), X is an organic functional group having at least one of the unsaturated double bond and the amino group. Accordingly, the scope of Formula (1) includes not only the embodiment in which X has both the unsaturated double bond and the amino group, but also the embodiment in which X has the unsaturated double bond but not the amino group, and the embodiment in which X does not have the unsaturated double bond but has the amino group. However, in Formula (1), X is preferably the unsaturated double bond and preferably does not include the amino group.

[0210] <Loss on Ignition of Glass Cloth>

[0211] From the perspective of promoting a reduction in the dielectric loss tangent of the glass cloth, the loss on ignition of the glass cloth is preferably 0.010 mass% or more and less than 0.180 mass%, preferably 0.010 mass% or more and less than 0.174 mass%, more preferably 0.010 mass% or more and less than 0.150 mass%, and even more preferably 0.010 mass% or more and less than 0.130 mass%. If the loss on ignition is less than 0.180 mass%, it is easy to avoid a situation where a large amount of residues of a surface treatment agent and / or modified products thereof, which cannot be reduced by water washing, exist on the surface of the glass cloth because they do not form a chemical bond with the glass surface and instead physically adhere to it, and as a result, it is easy to promote a reduction in the dielectric loss tangent of the glass cloth. If the loss on ignition value is 0.010 mass% or more, it is easy to achieve sufficient adhesion between the matrix resin and the glass cloth, and therefore, it is easy to ensure the heat resistance and insulation reliability of the printed circuit board when it is manufactured.

[0212] <Actual Width / TEX Value>

[0213] The "thread width / TEX" value, calculated by dividing the thread width of a glass thread by its TEX, is preferably in the range of 10 to 30. This value is preferably in the range of 11 to 29, more preferably in the range of 12 to 28, even more preferably in the range of 13 to 27, and particularly preferably in the range of 14 to 26. Here, the "thread width / TEX" value corresponds to a parameter representing the cohesiveness of the glass thread. In the warp warping process of a glass cloth, if the cohesiveness of the warp is insufficient, the warp is prone to fraying, making thread breakage likely to occur. Therefore, if the "thread width / TEX" value is 30 or less, it is easy to ensure the cohesiveness of the glass thread, and thus, it is easy to prevent the cutting of the glass thread during the warp warping process. If the "thread width / TEX" value is 10 or higher, it is easier to open the glass threads in the next process, and therefore, it is easier to prevent impregnation defects of the matrix resin during prepreg production.

[0214] <Average filament diameter>

[0215] The average filament diameter of the glass filaments constituting the glass thread is preferably in the range of 2.5 to 10.0 μm, more preferably in the range of 2.5 to 9.0 μm, even more preferably in the range of 3.5 to 8.5 μm, even more preferably in the range of 3.5 to 8.0 μm, and particularly preferably in the range of 3.5 to 7.5 μm. If the filament diameter is 2.5 μm or more, it is easy to secure the breaking strength of the filament, and therefore, it is easy to prevent the generation of lint in the resulting glass cloth. If the filament diameter is 10.0 μm or less, it is easy to avoid the mass of the glass cloth increasing, and therefore, it is easy to transport or process.

[0216] Twist

[0217] The absolute value of the twist count of the glass yarn is preferably in the range of 0.5 to 1.5 twists / 25 mm. More preferably, it is in the range of 0.55 to 1.45 twists / 25 mm, even more preferably in the range of 0.57 to 1.4 twists / 25 mm, even more preferably in the range of 0.59 to 1.3 twists / 25 mm, and particularly preferably in the range of 0.60 to 1.2 twists / 25 mm. By configuring the twist count of the glass yarn, it is possible to control the snarl index of the glass yarn. The higher the absolute value of the twist count, the stronger the unraveling force of the glass yarn tends to become, and therefore, it tends to exhibit a high snarl index. If the absolute value of the twist count of the glass yarn is 0.5 twists / 25 mm or higher, it is easy to ensure the cohesiveness of the glass yarn; therefore, it is easy to prevent the cutting of the glass yarn during the warp warping process and also easy to prevent the generation of lint on the surface of the glass cloth. If the absolute value of the twist count of the glass thread is 1.5 times / 25 mm or less, it is easy to prevent the snar index of the glass thread from becoming too large, and in this case, it is easy to avoid the situation where lint is easily generated on the surface of the glass cloth as the glass thread rubs against the surface of the bobbin when the glass thread is being processed.

[0218] It is preferable that the absolute value of the difference in the twist count between the warp and weft yarns be in the range of 0.01 to 0.70 twists / 25 mm. If the difference in the absolute value is 0.01 twists / 25 mm or greater, it is easy to increase the flatness of the glass cloth and also easy to open the glass yarn during the manufacture of the glass cloth. If the difference in the absolute value exceeds 0.7 twists / 25 mm, the glass cloth tends to bend significantly because the direction of the unwinding force of the warp and weft yarns is different (e.g., the warp is in the z-direction and the weft is in the s-direction). Furthermore, even if the unwinding force direction is the same, if the difference in the absolute value is large, the difference in unwinding force also tends to increase, making it easy for the glass cloth to bend. Therefore, if the difference in the absolute value is 0.7 twists / 25 mm or less, it is easy to suppress the occurrence of lint in the resulting glass cloth. It is more preferable that the absolute value of the difference in the number of twists between the warp and weft yarns of the glass cloth be in the range of 0.05 to 0.65 twists / 25 mm, and even more preferable that it be in the range of 0.07 to 0.55 twists / 25 mm. In addition, it is more preferable that the absolute value of the difference in the number of twists between the warp and weft yarns of the glass cloth be in the range of 0.10 to 0.50 twists / 25 mm, and even more preferable that it be in the range of 0.15 to 0.45 twists / 25 mm.

[0219] The twist of a glass thread is classified into the z-direction or the s-direction depending on the direction in which the twist is performed. In this disclosure, the twist in the z-direction is defined as "positive" and the twist in the s-direction is defined as "negative." For example, in this specification, "1.00z twist number" is indicated as a twist number of 1.00, and "1.00s twist number" is indicated as a twist number of -1.00.

[0220] The number of twists in the glass yarn can be adjusted, for example, during the process of twisting the glass yarn (twisting process). In one embodiment, it is easy to increase the number of twists in the glass yarn by bundling the glass filaments. Increasing the number of twists in the glass yarn makes it easier to suppress the generation of lint caused by the breakage of the glass filaments, and also makes it easier to suppress yarn breakage during the warping process of the glass cloth. On the other hand, the width expansion of the glass yarn is easily hindered by the twisting of the glass yarn, and uneven thickness of the glass cloth is likely to occur at the twisted portions. Therefore, determining an appropriate number of twists and using glass yarn adjusted to such a number is advantageous for manufacturing glass cloth of high quality.

[0221] Glass Thread Package

[0222] The present disclosure provides, in a preferred embodiment, a glass yarn package formed in a state where the glass yarn is wound onto a core material. The glass yarn package has a silicon (Si) content in the glass yarn of 95.0 to 100 mass% in terms of silicon dioxide (SiO2), and the snarl index of the glass yarn is 400 mm or less. By using such a glass yarn package, it is possible to improve flatness and also reduce the frequency of lint generation, thereby providing a glass cloth.

[0223] As a preferred requirement for the glass thread constituting the glass thread package, the preferred requirement for the glass thread constituting the glass cloth may be referenced. For example, the glass thread constituting the glass thread package is within the range described in the following formulas (A), (B), and (C);

[0224] (A) x+y+z=100 mass%

[0225] (B) x≥99.5 mass%

[0226] (C) 0.0003ppm≤y≤0.50ppm

[0227] x: Silicon content converted to silicon dioxide (SiO2)

[0228] y: Total content of uranium and thorium

[0229] z: Total content of elements other than silicon, uranium, and thorium

[0230] It is desirable to satisfy the above. In addition, regarding the glass thread constituting the glass thread package, it is desirable that the absolute value of its twist count be in the range of 0.5 to 1.5 twists / 25 mm, and also desirable that the value of "thread width / TEX" be in the range of 10 to 30. In addition, regarding the desirable numerical range of the glass thread constituting the glass thread package, the desirable numerical range of the glass thread constituting the glass cloth may likewise be referenced.

[0231] The core material for winding glass yarn is sufficient if it can suitably produce glass yarn from said core material, and in one embodiment, is a bobbin. However, the core material is not limited to a bobbin, but may be any material capable of having a function or configuration equivalent to a bobbin.

[0232] Methods for manufacturing glass thread, glass thread package, and glass cloth respectively

[0233] The present disclosure provides, in preferred embodiments, a method for manufacturing each of a glass skein, a glass skein package, and a glass cloth. One embodiment of such a method for manufacturing a glass skein is a method for manufacturing said glass skein in which the silicon (Si) content in the glass skein is 95.0 to 100 mass% in terms of silicon dioxide (SiO2), and the skein index of said glass skein is 400 mm or less.

[0234] In addition, one aspect of such a manufacturing method is a method for manufacturing a glass yarn package having the process of winding the glass yarn onto a core material and forming a package.

[0235] In addition, one embodiment of such a manufacturing method is a method for manufacturing a glass cloth, comprising a process of obtaining a glass cloth using a glass yarn in which the silicon (Si) content in the glass yarn is in the range of 95.0 to 100 mass% in terms of silicon dioxide (SiO2) and the snar index of the glass yarn is in the range of 400 mm or less.

[0236] In addition, one embodiment of such a manufacturing method is a method for manufacturing a glass cloth, comprising a process of obtaining a glass cloth using a glass thread in which the bulk dielectric loss tangent at 10 GHz of the glass constituting the glass thread is in the range of 0.001 or less, and the snar index of the glass thread is in the range of 400 mm or less.

[0237] In the present disclosure, each of the above manufacturing methods may include a process for manufacturing a glass filament by heating and stretching a glass rod (a process for manufacturing a glass filament) and a process for bundling a plurality of glass filaments (a process for bundling glass filaments).

[0238] <Manufacturing Process of Glass Rods>

[0239] Known techniques may be used as a method for manufacturing a glass rod for producing the glass cloth of the present disclosure. As the glass rod, fused quartz glass produced by the electric melting method or flame melting method may be used, and synthetic quartz rod produced by the sol-gel method may also be used. In either manufacturing method, it is preferable to perform a purification treatment on the glass rod, which is the raw material, in order to adjust the silicon content in the glass thread. In addition, in order to make it easier to control the snarl index of the glass thread, it is preferable to perform a purification treatment on the glass rod so that the total content of uranium and thorium in the glass thread is in the range of 0.0003 to 0.50 ppm. For example, in the case of fused quartz glass, it is advantageous to use raw material powder with a low content of uranium and thorium. By using a glass rod in which the total content of uranium and thorium is within the above range, it is easy to reduce the elongation stress when processing the glass filament, and as a result, it is easy to reduce the residual stress in the glass yarn, and furthermore, it is easy to lower the snarl index of the glass yarn.

[0240] Glass Filament Manufacturing Process

[0241] In this process, a glass filament is manufactured by heating and stretching a glass rod. Known techniques may be used as a method for manufacturing and further processing the glass filament. For example, a method of heating and stretching a glass rod may be used. In one embodiment, a glass rod with a diameter of 1 to 50 mm may be heated and stretched in an electric furnace under an inert atmosphere at a temperature of 2000°C to manufacture a glass filament with a diameter of 3 to 10 μm. At this time, the diameter of the glass filament can be controlled by adjusting the ratio of the transfer speed of the glass rod into the electric furnace to the stretching speed of the glass filament. From the perspective of reducing stress when stretching the glass rod, the temperature during heating and stretching is preferably in the range of 1700 to 2500°C, more preferably in the range of 1800 to 2400°C, and even more preferably in the range of 1900 to 2300°C.

[0242] The inventors have discovered that stress generated when heating and stretching a glass rod may remain in the resulting glass filament, and that the higher this residual stress, the greater the tendency for the snarl index of the glass filament to increase. Furthermore, the inventors have also discovered that, in order to adjust the snarl index of the glass filament, it is effective to reduce the residual stress in the glass filament after stretching, for example, by annealing treatment. By making the microcrystalline structure oriented by stretching into an unoriented structure through annealing treatment, it is easy to reduce the snarl index of the glass filament.

[0243] It is preferable to perform the annealing treatment between the process of heating and stretching the glass rod and the process of applying a gathering agent to the glass filament. Furthermore, from the perspective of easily reducing residual stress in the glass filament, the temperature during the annealing treatment is preferably in the range of 1000 to 1900°C, more preferably in the range of 1100 to 1800°C, even more preferably in the range of 1200 to 1700°C, even more preferably in the range of 1300 to 1650°C, and particularly preferably in the range of 1400 to 1600°C. If the temperature during the annealing treatment is 1900°C or lower, it tends to be easy to prevent the glass filament from breaking after heating and stretching, and additionally, if the temperature during the annealing treatment is 1100°C or higher, it is easy to obtain an effect of reducing residual stress in the glass filament. In addition, the time during the annealing treatment is preferably in the range of 0.1 to 30 seconds, more preferably in the range of 0.2 to 20 seconds, even more preferably in the range of 0.3 to 5 seconds, and particularly preferably in the range of 0.4 to 3 seconds.

[0244] Glass Filament Convergence Process

[0245] In this process, multiple glass filaments are bundled together. Since a bundled glass filament is generally referred to as a "strand," this process is also interpreted as a "method for manufacturing glass strands." Known techniques may be used as the method for manufacturing glass strands.

[0246] When producing glass strands, it is desirable to apply a cohesive agent to increase the cohesion of glass filaments and to protect the surface of the glass filaments. Methods for applying the cohesive agent include, for example, using a roller-type applicator.

[0247] As for the binder, resin-based binders such as PVA, polyurethane, and epoxy resins, as well as starch-based binders, are known. Starch-based binders are preferred from the perspective of the non-greater nature of the glass yarn during the weaving process and the ease of removing the binder from the glass yarn. To improve the functionality of the glass yarn, additives such as lubricants and antistatic agents may be added to the binder. From the perspective of easily suppressing snarling of the glass yarn, it is desirable to adjust the yarn length and the shape of the heat stretching furnace, etc., so that tension is applied as uniformly as possible to each glass filament when binding the glass filaments.

[0248] In order to adjust the "thread width / TEX" value, which is calculated by dividing the thread width of the glass thread by the TEX of the glass thread, to a range of 10 to 30, it is possible to adjust the amount of adhesive applied during the glass filament bundling process. Here, from the perspective of easily obtaining the effects of the present disclosure, the loss on ignition value (LOI) of the glass thread is preferably in the range of 1.0 to 2.5 mass%, more preferably in the range of 1.1 to 2.4 mass%, even more preferably in the range of 1.2 to 2.3 mass%, and particularly preferably in the range of 1.3 to 2.2 mass%. If the loss on ignition value of the glass thread is 1.0 mass% or higher, it is easy to secure the bundling properties of the glass filament, and in this case, it is easy to adjust the "thread width / TEX" value to a range of 10 to 30. If the loss on ignition of the glass yarn is 2.5 mass% or less, it is easy to prevent poor oil removal and insufficient fiber opening during the oil removal processing and fiber opening processes of the glass yarn.

[0249] <Threading Process>

[0250] The method may include a process (twisting process) for applying a predetermined twist to a glass strand. For the glass strand, a predetermined twist may be applied, for example, using a twisting machine. Known devices or methods may be used as the twisting machine or the twisting method. For example, a method may be used in which a winding of glass strand coated with a gluing agent (for example, referred to as a "collet") is drawn out, and a twist is applied to it while winding it onto a core material (in one embodiment, a bobbin). At this time, the bobbin is mounted on the twisting machine using a fixed jig called a spindle. The twisting machine generally has a member called a traveler around the spindle, and the number of twists added to the glass strand can be adjusted by the ratio of the operating speeds of these various members.

[0251] The twisting process may also include the process of winding a twisted glass strand onto a core material. By doing so, a glass yarn package can be produced.

[0252] Method for manufacturing glass cloth

[0253] A method for manufacturing glass cloth comprises a process (weaving process) of weaving the glass yarn as warp and weft threads and obtaining glass cloth.

[0254] In addition, the method for manufacturing a glass cloth may further include a warping process in which, prior to the weaving process, a glass yarn having a value in which the yarn width is divided by the TEX of the glass yarn is in the range of 10 to 30 is used to align the warp of the glass cloth and then apply a binding agent; a process of heating and degreasing the glass yarn (heating and degreasing process) to remove the binding agent attached to the glass yarn after the warping process, and also before, during, or after the weaving process, a process of applying a surface treatment agent to the glass yarn (surface treatment process); and a process of opening the glass yarn (opening process). By having these processes, it is easy to provide a glass cloth with excellent flatness and fluff quality.

[0255] The above-described glass processing method (heating degreasing process, surface treatment process, and fiber opening process) can be applied to glass yarn before weaving and also to woven glass cloth. In other words, the process of weaving glass yarn to obtain glass cloth may be provided before, during, or after the said glass processing method. Furthermore, in the glass processing method, "reduction" means, for example, removing at least a portion of a binding agent or silane coupling agent, and residual material that could not be completely removed may remain. Below, an embodiment including the warping process, weaving process, heating degreasing process, surface treatment process, and fiber opening process in this order is described by way of example. However, the present disclosure is not limited to the following examples.

[0256] Political and Economic Fairness

[0257] In the warping process, a glass yarn with a Si content in the range of 95.0 to 100 mass% in terms of SiO2 is used, and after aligning the warp threads, a sizing agent can be applied to the glass yarn. By providing a sizing agent to the glass yarn, it is easy to suppress the occurrence of lint in the glass cloth. As a sizing agent, it is preferable to use a material with relatively high sizing properties, such as starch and PVA. In order to uniformly apply the sizing agent to the glass yarn, it is preferable to immerse the glass yarn in the sizing agent, remove excess sizing agent with a squeeze roller, and then dry the sizing agent.

[0258] Weaving Process

[0259] In the weaving process, weaving can be performed by using a loom to drive the weft yarn onto the warp yarn prepared in the warping process. While air jet, rapier, and shuttle looms are known to be used, it is preferable to use an air jet loom to suppress lint on the glass cloth.

[0260] In the warp warping and weaving process, it is preferable that the absolute value of the twist count of the glass yarn be in the range of 0.5 to 1.5 twists / 25 mm. In addition, in this process, it is preferable to adjust the twist count of the weft yarn so that the absolute value of the difference in the twist count between the warp and weft yarns is in the range of 0.01 to 0.70 twists / 25 mm.

[0261] <Heating Deoiling Process>

[0262] In the heating and degreasing process of glass cloth, by heating the glass filament, sizing agents (gluing agents) and their residues, as well as their modified products, arbitrarily attached to the glass filament can be reduced, and preferably removed. Since it is possible to form a surface treatment layer on the surface of the glass filament (glass filament) after reducing organic substances capable of increasing the dielectric loss tangent by performing the heating and degreasing process, it is easy to produce glass cloth with excellent dielectric properties.

[0263] As a means for heating and de-oiling, known means (heating means, heating medium, heating mechanism, heating device and heating component, etc.) may be used.

[0264] As one embodiment of the heating degreasing process, for example, a method of heating glass cloth at a temperature of 600 to 1600°C is known.

[0265] In the heat treatment process, by heating a glass cloth, in which the softening point of the glass fiber is 900°C or higher, within a temperature range of 600 to 1600°C, it is easy to suppress damage to the glass cloth and also easy to lower the dielectric loss tangent of the glass cloth. From the view of suitably obtaining the effects of the present disclosure, the temperature of the heating and degreasing is preferably 700 to 1500°C, more preferably 800 to 1400°C, more preferably 900 to 1300°C, and particularly preferably 1000 to 1200°C. If the heating and degreasing temperature is 600°C or higher, it is easy to effectively remove binders and the like attached to the cloth, making it easy to produce a glass cloth with excellent dielectric properties. If the heating and degreasing temperature is 1600°C or lower, it is easy to suppress the devitrification phenomenon of the glass, and as a result, it is easy to prevent a decrease in the strength of the glass cloth.

[0266] The heating time is preferably 30 minutes or less, more preferably 15 minutes or less, even more preferably 5 minutes or less, and particularly preferably 90 seconds or less. Since the heating treatment is performed at a high temperature, if the heating time is 30 minutes or less, the damage imparted to the glass cloth is likely to be reduced, and in this case, it is easy to avoid problems such as the glass cloth being partially punctured or the glass cloth being cut during processing. From the perspective of effectively removing the binder, the heating time may be, for example, 1 second or more, 5 seconds or more, 10 seconds or more, or 15 seconds or more.

[0267] When heating and degreasing glass cloth in a closed system, it is preferable to place the glass cloth inside a heating furnace from the perspective of appropriate heating by a heating means. Furthermore, from the perspective of optimizing storage space and heating range, it is preferable to heat the glass cloth while storing it in a wound state. Additionally, from the perspective of increasing the efficiency of organic matter removal and shortening the organic matter removal time, it is preferable to heat the glass cloth while conveying it inside the heating furnace. The conveying of the glass cloth can be performed, for example, by a combination of an unwinding mechanism and a winding mechanism.

[0268] When heating and degreasing a glass cloth in an open system, it is desirable to heat the glass cloth while conveying it in order to secure the surface area to be heated. The conveying of the glass cloth can be performed, for example, by a combination of a winding mechanism and a winding mechanism.

[0269] The embodiments of the heating de-oiling process are not limited to the above. As an additional embodiment of the heating de-oiling process, for example, a method of heating in a vacuum or a gas with a dew point of 15°C or lower under conditions where the amount of heating, expressed as heating temperature (°C) × heating time (h) of 100°C or higher is 450 (°C·h) or higher (provided that the maximum heating temperature is 100 to 600°C) is also known.

[0270] Heating means

[0271] As heating means, for example, a furnace, an electric heater, a burner, etc., are considered, and among these, a gas single radiant tube burner or an electric heater is preferred. Multiple other heating means may be combined.

[0272] From the perspective of efficiently removing organic matter attached to the surface of a glass cloth, a continuous method of heating the glass cloth while passing it through a heating furnace is preferred over a batch method of heating the glass cloth wound on a coil core at a predetermined atmosphere temperature. A method in which the cleaning of the glass cloth can also be performed continuously using a cleaning water having a low metal ion content, such as reverse osmosis (RO) water or ion exchange water, is even more preferable.

[0273] In addition, as a heating means, from the perspective of low running costs, the glass cloth may be heated by bringing the glass cloth into contact with a member (contact member) heated to a predetermined temperature.

[0274] The contact member is preferably capable of heating the glass cloth at a high temperature. The shape of the contact member is preferably a roll shape due to the ease of conveying the glass cloth. Specifically, as the contact member, a roll heated by an induction heating method is preferred, for example, which can be used in a high-temperature region and has relatively small temperature fluctuations in the width direction. When heating the glass cloth with the contact member, the temperature of the contact member and the surface temperature of the glass cloth are considered to be approximately equal.

[0275] When continuously heating a glass cloth, in order to remove carbonized material attached to the roll, it is preferable that the method of using the roll be equipped with a mechanism for removing attached foreign matter, such as a blade.

[0276] <Means of Steam Application>

[0277] The means for applying the above to the glass cloth (steam application means) may be spray, shower diffusion, jet nozzle, etc. Generally, the gas discharged from the heating furnace can be reused as high-temperature steam.

[0278] The steam applied to the glass cloth may include, for example, volatile solvents, water vapor, or gases other than water vapor; however, water vapor is preferred from the perspective of suppressing toxicity to the human body and from the perspective of easily promoting the decomposition of the binder used in the glass fiber. The temperature of the high-temperature steam should be such that the surface temperature of the glass cloth is higher than 650°C, and in this case, if necessary, a method of supplying high-temperature steam and heated air in any ratio may be employed. The temperature of the high-temperature steam may be 400°C or higher, 450°C or higher, 550°C or higher, 600°C or higher, or 650°C or higher.

[0279] Surface Treatment Process

[0280] The surface treatment process can be applied to glass yarn and also to glass cloth. In other words, the process of weaving glass yarn to obtain glass cloth may be provided before, during, or after the glass treatment method according to the present disclosure.

[0281] The process of attaching a surface treatment agent may include, for example, a coating process in which a silane coupling agent is attached to the surface of the glass by a treatment solution having a concentration of 0.1 to 0.5 mass%, and at least one fixation process in which the silane coupling agent is fixed to the surface of the glass by heat drying. By doing so, it becomes easier to suitably surface treat the glass.

[0282] As a method for applying the treatment solution to the glass in the coating process, the following methods are possible: (a) a method of immersing or passing the glass in a treatment solution stored in a bath (hereinafter referred to as the "immersion method"), (b) a method of applying the treatment solution to the glass using a roll coater, die coater, or gravure coater. When the immersion method is adopted, it is preferable to select the immersion time of the glass in the treatment solution to be 0.5 seconds or more and 1 minute or less. In addition, when the immersion method is adopted, the glass may be passed through the treatment solution at a conveying speed of 10 to 50 m / min while applying a predetermined tension (e.g., 100 to 250 N) to the glass. In addition, after applying the treatment solution to the glass, the solvent contained in the treatment solution may be heated and dried by a method such as hot air or electromagnetic waves.

[0283] The concentration of the treatment solution is preferably 0.1 to 0.5 mass%, more preferably 0.1 to 0.45 mass%, and even more preferably 0.1 to 0.4 mass%. According to this, it becomes easier to surface treat the glass more suitably.

[0284] In the fixation process, the heating and drying temperature is preferably 80°C or higher, and more preferably 90°C or higher, so that the reaction between the silane coupling agent and the glass is sufficiently carried out. In addition, the heating and drying temperature is preferably 300°C or lower, and more preferably 180°C or lower, in order to prevent deterioration of the organic functional groups of the silane coupling agent.

[0285] The process for reducing silane coupling agents may include, for example, a cleaning process for cleaning silane coupling agents that have not formed chemical bonds with the surface of the glass, a drying process for heating and drying the glass after cleaning, and at least one finishing cleaning process for reducing unnecessary components that have not formed chemical bonds with the surface of the glass and could not be completely cleaned. This makes it easier to control the loss on ignition value. Additionally, the process for reducing silane coupling agents may include, for example, a finishing drying process after the finishing cleaning process.

[0286] Among these, in the final cleaning process, unnecessary components that do not form chemical bonds with the surface of the glass and could not be completely washed with water in the cleaning process can be reduced. In this final cleaning process, for example, an organic solvent may be used as the cleaning solution. By having a final cleaning process, even if low dielectric glass such as that disclosed in the present disclosure is used, it becomes easier to adjust the difference between the dielectric loss tangent of the resulting glass cloth and the bulk dielectric loss tangent to within the numerical range described above. As for the organic solvent here, an organic solvent with high hydrophobicity is preferred, and an organic solvent with high affinity for residues and modified products of silane coupling agents having hydroxyl groups is also preferred. The cleaning method may employ an immersion method, shower spray, etc., and heating or cooling may be performed as necessary. It is desirable to reduce excess solvent from the glass after cleaning using an aperture roller, etc., so as to suppress the re-attachment of glass dissolved in the cleaning solution.

[0287] Organic solvents usable as cleaning solutions in the final cleaning process may be used, for example, the following solvents alone or in combination. As highly hydrophobic organic solvents, examples include saturated chain-type aliphatic hydrocarbons such as n-pentane, i-pentane, n-hexane, i-hexane, n-heptane, i-heptane, n-octane, i-octane, 2,2,4-trimethylpentane (isooctane), n-nonane, i-nonane, n-decane, i-decane, and 2,2,4,6,6-pentamethylheptane (isododecane); saturated cyclic aliphatic hydrocarbons such as cyclopentane, cyclohexane, methylcyclohexane, dimethylcyclohexane, and ethylcyclohexane; aromatic hydrocarbons such as benzene, toluene, xylene, ethylbenzene, diethylbenzene, trimethylbenzene, and triethylbenzene; Examples include halogen-containing solvents such as chloroform, dichloromethane, and dichloroethane. Organic solvents with high affinity for residues or modified products of silane coupling agents include alcohols such as methanol, ethanol, and butanol; ketones such as acetone and methyl ethyl ketone; ethers such as methyl ethyl ether and diethyl ether; amides such as N,N-dimethylformamide and N,N-dimethylacetamide; and dimethyl sulfoxide. Among these, aromatic hydrocarbons, alcohols, or ketones are preferred, and methanol is more preferred, from the perspective that it is easy to efficiently reduce the silane coupling agent physically attached to the glass. Therefore, as a cleaning solution in the final cleaning process, it is preferable to use a cleaning solution in which methanol is the main component (50 mass% or more, or 60 mass% or more, of methanol relative to 100 mass% of the cleaning solution).

[0288] In the final drying process, the cleaning solution used in the final cleaning process can be reduced. Due to the ease of reducing the cleaning solution through drying, it is preferable that the cleaning solution used in the final cleaning process has a boiling point of 120°C or lower. For drying, a method of heat drying or air drying may be employed. Furthermore, when an organic solvent is used as the cleaning solution, from a safety perspective, it is preferable to perform heat drying by hot air drying using low-pressure steam or a heat medium oil as a heat source. The drying temperature is preferably above the boiling point of the cleaning solution, and from the perspective of suppressing the deterioration of the silane coupling agent, it is preferable to be 180°C or lower.

[0289] <Island Development Project>

[0290] As a fiber opening method in the fiber opening process, methods such as opening the glass cloth using spray water (high-pressure water opening), a vibro washer, ultrasonic water, or a mangle may be adopted. During this fiber opening process, reducing the tension applied to the glass cloth tends to result in a smaller air permeability. Furthermore, to suppress the reduction in tensile strength of the glass cloth caused by the fiber opening process, it is desirable to implement measures such as reducing friction with contact members during glass yarn weaving, optimizing the binding agent, and increasing the adhesion amount. Dry ice blasting is preferred as a fiber opening method for glass cloth composed of glass yarn with high glass hardness.

[0291] The above process does not necessarily need to be performed in a separate process, and multiple processes may be integrated into a single process. For example, if the cleaning process is performed after the weaving process, the opening process can be combined with the cleaning process by using a high-pressure water spray, etc. The composition of the glass cloth usually does not change before and after opening. In addition, the method for manufacturing the glass cloth may include any process other than the above process. For example, a slit processing process may be included after the opening process. Furthermore, if possible, the order of the above processes may be changed.

[0292] Prepreg

[0293] The prepreg according to the present disclosure comprises the glass cloth and a matrix resin impregnated in the glass cloth. By doing so, a prepreg with low voids can be provided.

[0294] As the matrix resin, a thermosetting resin or a thermoplastic resin may be used. If possible, both may be used in combination, or other resins may be included.

[0295] As for thermosetting resins, for example

[0296] (a) an epoxy resin formed by reacting and curing a compound having an epoxy group with a compound having at least one group selected from the group consisting of an amino group, a phenol group, an acid anhydride group, a hydrazide group, an isocyanate group, a cyanate group, and a hydroxyl group that reacts with the epoxy group;

[0297] (b) a radical polymerization type curing resin formed by curing a compound having at least one group selected from the group consisting of allyl groups, methacrylic groups and acrylic groups;

[0298] (c) Maleimide triazine resin formed by reacting a compound having a cyanate group with a compound having a maleimide group and curing the result;

[0299] (d) a thermosetting polyimide resin formed by reacting a maleimide compound with an amine compound and curing it;

[0300] (e) Benzooxazine resin formed by cross-linking and curing a compound having a benzoxazine ring by heat polymerization;

[0301] Examples are given. In addition, (a) in obtaining an epoxy resin, the compound may be reacted without a catalyst, or the compound may be reacted by adding a catalyst having reaction catalytic ability, such as an imidazole compound, a tertiary amine compound, a urea compound, and a phosphorus compound. In addition, (b) in obtaining a radical polymerization type cured resin, a pyrolysis type catalyst or a photolysis type catalyst may be used as a reaction initiator.

[0302] Examples of thermoplastic resins include polyphenylene ether, modified polyphenylene ether, polyphenylene sulfide, polysulfone, polyethersulfone, polyarylate, aromatic polyamide, polyetheretherketone, thermoplastic polyimide, insoluble polyimide, polyamideimide, and fluoropolymer. As an insulating material for printed circuit boards for high-speed communication, polyphenylene ether or modified polyphenylene ether, which is rich in radical reactivity, is preferred.

[0303] When a matrix resin used in printed circuit boards for high-speed communication has vinyl or methacrylate groups, it has relatively high hydrophobicity, and a silane coupling agent having functional groups involved in radical reactions, such as methacrylate groups, has good compatibility with the said matrix resin.

[0304] As mentioned above, thermosetting resins and thermoplastic resins may be used in combination. Additionally, prepregs may further contain inorganic fillers. It is preferable for the inorganic filler to be used in combination with the thermosetting resin, and examples include aluminum hydroxide, zirconium oxide, calcium carbonate, alumina, mica, aluminum carbonate, magnesium silicate, aluminum silicate, silica, talc, glass staple fibers, aluminum borate, and silicon carbide. The inorganic filler may be used alone or two or more types may be used in combination.

[0305] Printed Wiring Board

[0306] The printed circuit board according to the present disclosure contains the prepreg. By doing so, a printed circuit board with excellent insulation reliability can be provided.

[0307] Integrated Circuits and Electronic Devices

[0308] In addition, an integrated circuit and an electronic device including the above-described printed circuit board are also an aspect of the present disclosure. An integrated circuit and an electronic device obtained using the printed circuit board according to the present disclosure have excellent various characteristics.

[0309] Examples

[0310] Examples of embodiments of the present disclosure are described below through examples and comparative examples. However, the present disclosure is not limited to the following examples. For the examples and comparative examples, various manufacturing, measurement, and evaluation, etc. were performed by the following methods. Furthermore, unless specifically stated otherwise, various manufacturing, measurement, and evaluation, etc. were performed at room temperature (25°C) and under atmospheric pressure.

[0311] "measurement"

[0312] <Thickness of glass cloth (㎛)>

[0313] The thickness of the glass cloth was determined in accordance with Section 7.10 of JIS R 3420. Specifically, using a micrometer, the spindle was slightly rotated and lightly contacted parallel to the measurement surface of the sample. Then, the scale was read after the ratchet clicked three times. In addition, Section 7.10 of JIS R 3420 specifies general test methods for cloth products such as glass cloth.

[0314] <Snarl Index of Glass Thread (mm)>

[0315] The snar index of the glass thread was calculated in accordance with Section 9.17 of JIS L 1095. Specifically, first, with the initial load described in Method A of Section 9.17.1 of JIS L 1095 applied to the glass thread (sample), the glass thread was stretched and flattened so that it became straight between the grippers, and then 1.1 × 10⁻⁶ at the center thereof -6 A load of N / tex was applied. At a speed of 0.5 m / min, one gripping part B was brought close to the other gripping part A to loosen the sample. The number on the scale at the position of gripping part B was read when snaring occurred at the load point. The test was performed 30 times, and the snaring index was calculated by determining the average value.

[0316] Glass Thread TEX (g / 1000m)

[0317] The TEX of the glass yarn was determined in accordance with JIS R3420 2012. Specifically, a glass yarn sampled to a length of 1000 m was subjected to a heat degreasing treatment for 30 minutes in a muffle furnace set to 625 ± 20°C, thereby removing the binder attached to the glass yarn. At this time, whether the binder was removed was determined by whether the weight loss of the glass yarn before and after the heat degreasing was less than 0.1 mass%. That is, it was determined that the binder was removed if the weight loss of the glass yarn before and after the heat degreasing was less than 0.1 mass%. The TEX of the glass yarn was determined by measuring the weight of the 1000 m portion of glass yarn after the heat degreasing treatment was completed.

[0318] Content of each element in the glass thread

[0319] The content of silicon, uranium, and thorium constituting the glass thread was determined by the absolute calibration curve method using an ICP mass spectrometer.

[0320] <Silicon Content (Mass%)>

[0321] In order to reduce impurities (e.g., sizing agents, etc.) attached to the glass thread or its raw material, the solution was adjusted by the following method. That is, the glass thread (sample) was weighed, hydrolyzed with sodium hydroxide, and then dissolved in dilute nitric acid to adjust the solution.

[0322] For the obtained solution, the silicon content was measured using an ICP emission spectroscopic analyzer (PS3520VDDII manufactured by Hitachi High-Tech Science Co., Ltd.), and then the silicon content in the sample was determined by converting it into an oxide value.

[0323] Uranium and Thorium Content (ppm)

[0324] A weighed glass thread (sample) was heated and washed with aqua regia, and then washed with ultrapure water. This sample was decomposed with nitric acid, hydrofluoric acid, and sulfuric acid, and then heated and concentrated until white sulfuric acid fumes were produced, and then the solution was adjusted using dilute nitric acid.

[0325] For the obtained solution, uranium and thorium were measured using an ICP mass spectrometer (SPQ9400 manufactured by SII Nanotechnologies), and the content of uranium and thorium contained in the sample was determined.

[0326] <Content of other ingredients (mass%)>

[0327] The content of other components (elements other than silicon, uranium, and thorium) in the glass seal (sample) was determined by subtracting the values ​​of the content of silicon, uranium, and thorium, respectively, from 100 mass%. The other components are indicated as "impurities" in the table below.

[0328] Here, regarding the unit “ppm” representing the content of uranium and thorium, it was converted as 1 ppm = 0.0001 mass%.

[0329] <Number of twists of glass thread, and the difference in its absolute value (twists / 25 mm)>

[0330] Measurements were performed in accordance with JIS R3420, and the twist count (twists / 25 mm) of the glass yarn was obtained. When measuring the twist count, in order to accurately measure the twist count of the glass yarn in the glass cloth, the glass yarn (warp or weft) was drawn from the glass cloth, and the measurement was performed on the corresponding glass yarn (corresponding warp or corresponding weft). For the obtained values, the twist in the z-direction was treated as positive and the twist in the s-direction as negative. For example, a twist of 1.00z (1.00 twist in the z-direction (twist / 25 mm)) was treated as +1.00, and a twist of 1.00s (1.00 twist in the s-direction (twist / 25 mm)) was treated as -1.00. Then, the following formula:

[0331] Absolute difference in twist count = |Warp twist count - Weft twist count|

[0332] By this, the absolute difference in the number of twists of the warp and weft yarns (twists / 25 mm) was calculated.

[0333] <Width of glass thread (㎛)>

[0334] While conveying the glass filament at a speed of 1 m / min, a transmissive measuring instrument with an LED projection method (HIGH ACCURACY CMOS MICROMETER LS-9006MR / manufactured by Keyence) was used to measure the width of the glass filament bundle over a length of 50 m. From the obtained data on the width of the glass filament bundle over a length of 50 m, the proportion of the width of the bundle that was less than or equal to a specific value and the average value of the glass filament bundle width were calculated. The measurement of the glass filament bundle width using the transmissive measuring instrument with an LED projection method was performed under the condition that 1,934 measurement points were obtained per m. In cases where an error occurred due to the LED being out of focus or other reasons (where a value of -9999 was displayed), the corresponding measurement value was deleted to calculate the average value of the glass filament width. In addition, measurement values ​​that caused errors were appropriately omitted to perform the calculation. In addition, the tension acting on the glass thread when the glass thread is being conveyed was 0.12 to 0.18 N when measured with a tension meter (SCHMIDT Conrol Instruments ETPB-100-C0585).

[0335] <Actual Width / TEX(㎛ / (g / 1000m))>

[0336] The value of thread width / TEX was calculated by dividing the thread width obtained above by the TEX obtained above.

[0337] Bulk dielectric loss tangent at 10GHz

[0338] In accordance with IEC 62562, the bulk dielectric loss tangent at 10 GHz was determined for each glass rod (bulk), which is the raw material for each glass chamber. Specifically, glass plate samples of 300 μm or less, sampled to a size required for measurement in a split cylinder resonator, were stored in a constant temperature and humidity oven at 23°C and 50% RH for 8 hours. After storage, dielectric properties were measured for the samples using a split cylinder resonator (manufactured by EM Labo) and an impedance analyzer (manufactured by Agilent Technologies). Measurements were performed five times on each sample, and the average value was calculated. Furthermore, IEC 62562 specifies the method for measuring dielectric properties in the microwave range for fine ceramic materials primarily used in microwave circuits.

[0339] <Number of each filament and filament diameter (㎛) of warp and weft>

[0340] In calculating the average fiber opening, the number of filaments and the diameter of each warp and weft were determined by observing a cross-sectional image of the glass yarn. Specifically, a cross-sectional image of the glass yarn as the warp (or weft) was acquired, and the number of filaments and the diameter of the corresponding warp (or weft) were measured in the cross-sectional image. Likewise, the acquisition of the glass yarn image and the measurement of the number of filaments were repeated, and the average of the five obtained measurements was treated as the number of filaments and the diameter of the warp (or weft).

[0341] Warp Width and Weft Width

[0342] In calculating the average openness, the warp width and weft width were determined by the following method. First, five glass cloth samples were cut from a glass cloth with dimensions of 70 mm in the warp direction and 70 mm in the weft direction. Each cut sample was observed from the vertical direction at a magnification of 100x using a macroscope. For each sample, the thread widths of 250 warp (or weft) threads were randomly measured, and the average value of the 250 warp (or weft) thread widths obtained was calculated. The calculated average value was treated as the warp width (or weft width).

[0343] <Warp and Weft Openness (%), and Glass Cloth Average Openness (%)>

[0344] The angle of opening of the glass cloth is given by the following formula:

[0345] Slant Fineness (%) = [Slant Width (㎛) / {Number of Slant Filaments × Slant Filament Diameter (㎛)}] × 100

[0346] It was calculated by.

[0347] In addition, the weft fiber of the glass cloth is as follows:

[0348] Weft fineness (%) = [Weft width (㎛) / {Number of weft filaments × Weft filament diameter (㎛)}] × 100

[0349] It was calculated by.

[0350] Using the calculated warp openness (%) and weft openness (%), the following formula:

[0351] Average openness (%) = {Warp openness (%) + Weft openness (%)} / 2

[0352] The average island opening was calculated by...

[0353] Lint quality

[0354] Glass cloths obtained in the examples and comparative examples were tested using a roll-to-roll inspection table while applying a tension of 100 N / 1000 mm and irradiating with a halogen lamp. The number of lint, particularly the number of lints with protrusions of 1 mm or more, was determined by visual inspection. The number of lints per 1 m² was treated as the frequency of lint, and this was used to evaluate the lint quality according to the following criteria.

[0355] (measurement standard)

[0356] Lint quality A: Lint frequency is 10 pieces / ㎡ or less.

[0357] Lint quality B: Lint frequency is 11 to 20 pieces / m².

[0358] Lint quality C: Lint frequency of 21 pieces / ㎡ or more.

[0359] The bending of the glass cloth

[0360] A sample was obtained by cutting the glass cloth obtained in the example and comparative example into a size of 200 mm × 200 mm. This sample was loaded onto a measuring stand with a flat surface, and the amount of bending in the glass cloth was measured.

[0361] FIGS. 1(a) and (b) are schematic diagrams for explaining a method for measuring the amount of bending in a glass cloth. Among these, FIG. 1(a) schematically illustrates a plan view of the glass cloth and the stacking table viewed from above, and FIG. 1(b) schematically illustrates a cross-sectional view of the left end portion of the glass cloth in FIG. 1(a) (the portion enclosed by dotted line A) when viewed with the left end facing forward and inward. In FIG. 1(a) and (b), the x direction, y direction, and z direction correspond to each other.

[0362] As shown in the illustration, a sample (2) of glass cloth is loaded onto a measuring table (1) with a flat surface. The sample (2) is curved so as to rise above the measuring table (1) at its left end, thereby floating by a height T1. At this time, the height T1 is treated as the amount of bending at the left end portion of the glass cloth.

[0363] And, as with the examples illustrated in FIG. 1 (a) and (b),

[0364] Height T2 at the top part of the glass cloth,

[0365] Height T3 at the right end portion of the glass cloth, and

[0366] Height T4 at the bottom part of the glass cloth

[0367] a, respectively, are treated as the amount of bending in the upper, right end, and lower parts of the glass cloth.

[0368] Among the four bending amounts in the glass cloth, the maximum bending amount Tmax is indicated as "bending amount" in the table below.

[0369] FIGS. 2 (a) and (b) are schematic diagrams for further explaining the method of measuring the amount of bending. FIGS. 2 (a) and (b) correspond to the cross-section of the part enclosed by the dotted line A in FIG. 1 (a).

[0370] Among these, Figure 2(a) shows the sample curling at the left end. In this case, the height Ta of the peak of the curl is treated as the amount of bending at the left end of the glass cloth.

[0371] In addition, Figure 2(b) shows that the sample is curved into an arch at the left end. In this case as well, the height Tb of the apex of the arch is treated as the amount of bending at the left end of the glass cloth.

[0372] <Production of Prepreg Samples>

[0373] A varnish was prepared by adding 45 parts by mass of polyphenylene ether (SABIC, Noryl SA9000), 10 parts by mass of triallyl isocyanurate, 45 parts by mass of toluene, and 0.6 parts by mass of 1,3-di(tert-butylisopropylbenzene) to a stainless steel container and stirring at room temperature for 1 hour.

[0374] Glass cloths obtained from the examples and comparative examples, respectively, were impregnated into the prepared varnish and then dried at 115°C for 1 minute. By doing so, a sample of prepreg was obtained.

[0375] <Malfunction Performance Test>

[0376] Two copper foils with a thickness of 18 μm were placed on both sides of the two prepregs obtained above. Then, a substrate was fabricated by heating at 200°C and 40 kg / cm² for 2 hours and applying pressure to cure it. Afterward, a copper wiring pattern with an L / S (line and space) of 10 μm was fabricated on the substrate, and 30 DRAMs were mounted so as to be electrically connected to this wiring pattern. The substrate with the DRAMs mounted on it was operated continuously for 1000 hours under conditions of a temperature of 150°C and a frequency of 10 GHz. Based on these results, the malfunction performance caused by uranium and thorium contained in the glass wire was evaluated.

[0377] (metewand)

[0378] A: 0 DRAM malfunctions.

[0379] B: 1 to 2 DRAM malfunctions.

[0380] C: 3 to 4 DRAM malfunctions.

[0381] D: 5 to 6 DRAM malfunctions.

[0382] E: 7 to 8 DRAM malfunctions.

[0383] F: 9 DRAM malfunctions.

[0384] G: More than 10 DRAM malfunctions.

[0385] Examples and Comparative Examples

[0386] <Manufacture of Glass Thread 1 and Its Package>

[0387] Glass filaments were manufactured using a quartz glass rod (diameter = 1 mm) having a silicon content of 99.92 mass% and a total uranium and thorium content of 0.103 ppm. The quartz glass rod was fed into a furnace filled with a sufficient amount of argon gas and set at a temperature of 1970°C, and by heating and stretching, glass filaments with a diameter of 5.0 μm and filament count of 50 were manufactured. Additionally, for each heated and stretched glass filament, a treatment to reduce residual stress present in the glass filament (annealing treatment) was performed by passing it through a furnace set at a temperature of 1500°C for 1 second. The annealed glass filaments were aligned, and then bundled using an applicator with a binding agent using starch as the main component, and wound onto a collet to obtain a bundle of glass filaments (glass strands). The obtained filament bundle was twisted in the z-direction at a pitch of 0.8 times / 25 mm using a twisting machine, and wound onto a bobbin to obtain glass thread 1 and its package, respectively.

[0388] <Manufacture of Glass Thread 2 and Its Package>

[0389] Glass thread 2 and its package were obtained in the same manner as glass thread 1, except that a quartz glass rod (diameter = 1 mm) with a silicon content of 99.98 mass% and a total content of uranium and thorium of 0.0036 ppm was used.

[0390] <Manufacture of Glass Thread 3 and Its Package>

[0391] Glass thread 3 and its package were obtained in the same manner as glass thread 1, except that a quartz glass rod (diameter = 1 mm) with a silicon content of 99.90 mass% and a total content of uranium and thorium of 0.204 ppm was used.

[0392] <Manufacture of Glass Thread 4 and its Package>

[0393] Glass thread 4 and its package were obtained in the same manner as glass thread 1, except that a quartz glass rod (diameter = 1 mm) with a silicon content of 99.85 mass% and a total content of uranium and thorium of 0.389 ppm was used.

[0394] <Manufacture of Glass Thread 5 and its Package>

[0395] Glass thread 5 and its package were each obtained in the same manner as in Example 1, except that the glass rod was heated and stretched to have 200 filaments.

[0396] <Manufacture of Glass Thread 6 and its Package>

[0397] Glass thread 6 and its package were each obtained in the same manner as in Example 2, except that the glass rod was heated and stretched to have 200 filaments.

[0398] <Manufacture of Glass Thread 7 and its Package>

[0399] Glass thread 7 and its package were each obtained in the same manner as in Example 1, except that twisting was applied at a pitch of 0.4 times / 25 mm in the z direction.

[0400] <Manufacture of Glass Thread 8 and its Package>

[0401] Glass thread 8 and its package were each obtained in the same manner as in Example 1, except that the annealing temperature of the glass filament was 1200°C.

[0402] <Manufacture of Glass Thread 9 and its Package>

[0403] Glass thread 9 and its package were each obtained in the same manner as in Example 2, except that the annealing temperature of the glass filament was 1200°C.

[0404] <Manufacture of Glass Thread 10 and its Package>

[0405] Except for the fact that the glass filament was not annealed, a glass thread 10 and its package were obtained in the same manner as in Example 1.

[0406] <Manufacture of Glass Thread 11 and its Package>

[0407] Glass thread 11 and its package were obtained in the same manner as glass thread 1, except that a quartz glass rod (diameter = 1 mm) with a silicon content of 99.70 mass% and a total content of uranium and thorium of 0.561 ppm was used.

[0408] <Manufacture of Glass Thread 12>

[0409] The glass was processed in the same manner as in Example 1, except that the annealing temperature of the glass filament was set to 2000°C. However, multiple glass filaments were cut during the annealing process, and therefore, the glass wire and its package could not be obtained.

[0410] <Manufacture of Glass Thread 13 and its Package>

[0411] Glass thread 13 and its package were obtained in the same manner as glass thread 1, except that a quartz glass rod (diameter = 1 mm) with a silicon content of 99.99 mass% and a total content of uranium and thorium of 0.0017 ppm was used.

[0412] <Manufacture of Glass Thread 14 and its Package>

[0413] Glass thread 14 and its package were obtained in the same manner as glass thread 1, except that a quartz glass rod (diameter = 1 mm) with a silicon content of 99.91 mass% and a total content of uranium and thorium of 0.09 ppm was used.

[0414] <Manufacture of Glass Thread 15 and its Package>

[0415] Glass thread 15 and its package were obtained in the same manner as glass thread 1, except that a quartz glass rod (diameter = 1 mm) with a silicon content of 99.99 mass% and a total content of uranium and thorium of 0.0006 ppm was used.

[0416] <Manufacture of Glass Thread 16 and its Package>

[0417] Glass thread 16 and its package were obtained in the same manner as glass thread 1, except that a quartz glass rod (diameter = 1 mm) with a silicon content of 99.99 mass% and a total content of uranium and thorium of 0.0010 ppm was used.

[0418] <Manufacture of Glass Thread 17 and its Package>

[0419] Glass thread 17 and its package were obtained in the same manner as glass thread 1, except that a quartz glass rod (diameter = 1 mm) with a silicon content of 99.98 mass% and a total content of uranium and thorium of 0.0022 ppm was used.

[0420] <Manufacture of Glass Thread 18 and its Package>

[0421] Glass thread 18 and its package were obtained in the same manner as glass thread 1, except that a quartz glass rod (diameter = 1 mm) with a silicon content of 99.93 mass% and a total content of uranium and thorium of 0.03 ppm was used.

[0422] <Example 1>

[0423] Glass yarn 1 was used as the warp and weft yarns. In the warp warping process, a room beam was produced by aligning the warp yarns at a line speed of 60 m / min and performing a secondary sizing treatment using a PVA gluing agent. Subsequently, using an air jet room, 2000 m of glass cloth with a plain weave structure was woven, with a weft density of 66 warp yarns / 25 mm and 68 weft yarns / 25 mm, and a cloth width of 1300 mm. In addition, during the weaving process, since it is possible to adjust the twist count of the weft yarns by the loom conditions, the main nozzle pressure and sub-nozzle angle of the loom were adjusted so that the twist count of the weft yarns was 0.6 twists / 25 mm in the z-direction.

[0424] The obtained glass cloth was washed with ion-exchanged water and then dried. This removed alkali metal ions and the like attached to the surface of the cloth. Afterward, it was heated and degreased at 1000°C for 15 seconds (heating and degreased process).

[0425] Next, a treatment solution was prepared by dispersing 0.3 mass% of 3-methacryloxypropyltrimethoxysilane (silane coupling agent A); Z6030 (manufactured by Dow Toray) in pure water adjusted to pH=3 with acetic acid. A cloth was immersed in the treatment solution at a line tension of 100 N and a line speed of 15 m / min (surface treatment process). After squeezing the treatment solution out of the cloth, it was heated and dried at 130°C for 60 seconds to fix the silane coupling agent (fixation process).

[0426] The dried cloth was irradiated with ultrasound in water at a frequency of 25 kHz and an output of 0.50 W / ㎠. Subsequently, the cloth was subjected to fiber opening treatment in a main stream discharged from a 1.4 MPa high-pressure water spray while reducing excess silane coupling agent physically attached to the cloth (fiber opening process). Afterward, the cloth was dried at 130°C for 1 minute (drying process).

[0427] By the above, the glass cloth of Example 1 was obtained.

[0428] <Examples 2 to 16 and Comparative Example 1>

[0429] A glass cloth was obtained in the same manner as in Example 1, except that the items listed in the table below were changed according to the table below.

[0430] For the examples and comparative examples, the manufacturing conditions and evaluation results are shown in the table below. In addition, using the glass cloth of the examples, prepregs, printed circuit boards, integrated circuits, and electronic devices could be fabricated by conventional methods.

[0431]

[0432]

[0433]

[0434]

[0435]

[0436]

[0437] According to the above table and the examples, it was confirmed that a glass cloth can be provided that can improve flatness and also reduce the frequency of lint generation. Furthermore, according to the above table, it was also confirmed that appropriately controlling the total content of uranium and thorium in the glass yarn is advantageous for the <malfunction performance test> evaluation. Industrial applicability

[0438] The present disclosure can be suitably used in the field of glass threads, glass cloths, prepregs and printed circuit boards, and methods for manufacturing glass cloths. Explanation of the symbols

[0439] 1: Measuring stand 2: Glass cloth sample

Claims

Claim 1 A glass cloth composed of glass threads, wherein the silicon (Si) content in the glass threads is 95.0 to 100 mass% in terms of silicon dioxide (SiO2), and furthermore, the snarl index of the glass threads is 400 mm or less. Claim 2 A glass cloth composed of glass threads, wherein the bulk dielectric loss tangent of the glass constituting the glass threads at 10 GHz is in the range of 0.001 or less, and furthermore, the snarl index of the glass threads is 400 mm or less. Claim 3 A glass cloth according to claim 1 or 2, wherein the snarl index of the glass thread is 70 mm or more. Claim 4 A glass cloth comprising, in accordance with claim 1 or 2, a glass thread satisfying the ranges described in the following formulas (A), (B), and (C); (A) x+y+z=100 mass% (B) x≥99.5 mass% (C) 0.0003 ppm≤y≤0.50 ppm, where x: silicon content when converted to silicon dioxide (SiO2), y: sum of uranium and thorium contents, and z: sum of elements other than silicon, uranium, and thorium. Claim 5 A glass cloth according to paragraph 4, wherein the range of x is 99.6 mass% or more. Claim 6 A glass cloth according to paragraph 4, wherein the range of x is 99.9 mass% or more. Claim 7 A glass cloth according to claim 1 or 2, wherein the glass thread is treated with a surface treatment agent comprising a silane coupling agent. Claim 8 In claim 7, the surface treatment agent is the following formula (1):X(R) 3-n SiY n A glass cloth comprising the silane coupling agent represented by ···(1)(wherein X is an organic functional group having at least one of an amino group and an unsaturated double bond group having radical reactivity, Y is each independently an alkoxy group, n is an integer from 1 to 3, and R is each independently a group selected from the group consisting of a methyl group, an ethyl group and a phenyl group). Claim 9 In claim 8, X in the above formula (1) is an organic functional group that does not form a salt with an ionic compound, and is a glass cloth. Claim 10 In claim 8, X in the above formula (1) does not contain an amine and / or ammonium cation, a glass cloth. Claim 11 In claim 8, a glass cloth in which X in the above formula (1) is an organic functional group having a methacryloxy group and / or an acryloxy group. Claim 12 A glass cloth according to claim 1 or 2, wherein the absolute value of the number of twists of the glass thread is in the range of 0.5 to 1.5 twists / 25 mm. Claim 13 A glass cloth according to claim 1 or 2, wherein the glass cloth comprises the glass yarn as warp and weft, and the absolute value of the difference in the number of twists of the warp and weft is in the range of 0.01 to 0.70 twists / 25 mm. Claim 14 A glass cloth according to claim 1 or 2, wherein the thickness of the glass cloth is 60 μm or less. Claim 15 A glass cloth for a printed circuit board, according to paragraph 1 or 2. Claim 16 A prepreg containing a glass cloth as described in paragraph 1 or 2 and a thermosetting resin. Claim 17 A printed circuit board comprising the prepreg described in paragraph 16. Claim 18 An integrated circuit comprising a printed circuit board as described in paragraph 17. Claim 19 An electronic device comprising a printed circuit board as described in paragraph 17. Claim 20 A method for manufacturing a glass cloth, comprising a process of obtaining a glass cloth using a glass yarn in which the silicon (Si) content in the glass yarn is in the range of 95.0 to 100 mass% in terms of silicon dioxide (SiO2) and the snar index of the glass yarn is 400 mm or less. Claim 21 A method for manufacturing a glass cloth, comprising a process of obtaining a glass cloth using a glass thread in which the bulk dielectric loss tangent at 10 GHz of the glass constituting the glass thread is in the range of 0.001 or less, and the snar index of the glass thread is 400 mm or less. Claim 22 A method for manufacturing a glass cloth according to claim 20 or 21, wherein the snarl index of the glass thread is 70 mm or more. Claim 23 A method for manufacturing a glass cloth according to claim 20 or 21, comprising a process of obtaining a glass cloth using a glass thread satisfying the ranges described in the following formulas (A), (B), and (C); (A) x+y+z=100 mass% (B) x≥99.5 mass% (C) 0.0003 ppm≤y≤0.50 ppm, x: silicon content when converted to silicon dioxide (SiO2), y: sum of uranium and thorium contents, z: sum of elements other than silicon, uranium, and thorium. Claim 24 A method for manufacturing a glass cloth according to claim 20 or 21, comprising a process of warping the glass yarn used as a warp (warp warping process) and a process of weaving using the glass yarn (weaving process), wherein in the warp warping process and / or the weaving process, the absolute value of the twist count of the glass yarn is adjusted to a range of 0.5 to 1.5 times / 25 mm. Claim 25 A method for manufacturing a glass cloth according to claim 24, wherein the glass cloth comprises the glass yarn as warp and weft, and the process of adjusting the twist count of the weft yarn such that the absolute value of the difference in the twist count of the warp yarn and the weft yarn is in the range of 0.01 to 0.70 twists / 25 mm. Claim 26 A method for manufacturing a glass cloth according to claim 24 or 25, wherein the value obtained by dividing the width of the glass yarn by TEX is in the range of 10 to 30, and the warp warping process and / or the weaving process are performed. Claim 27 A glass yarn package having a core material and a glass yarn wound on the core material, wherein the silicon (Si) content in the glass yarn is 95.0 to 100 mass% in terms of silicon dioxide (SiO2), and furthermore, the snar index of the glass yarn is 400 mm or less. Claim 28 In claim 27, a glass seal package having a snarl index of 70 mm or more of the glass seal. Claim 29 A glass seal package according to claim 27 or 28, wherein the glass seal satisfies the ranges described in the following formulas (A), (B), and (C); (A) x+y+z=100 mass% (B) x≥99.5 mass% (C) 0.0003 ppm≤y≤0.50 ppm x: silicon content when converted to silicon dioxide (SiO2) y: sum of uranium and thorium contents z: sum of elements other than silicon, uranium, and thorium. Claim 30 A glass thread package according to claim 27 or 28, wherein the absolute value of the number of twists of the glass thread is in the range of 0.5 to 1.5 twists / 25 mm. Claim 31 A glass thread package according to claim 27 or 28, wherein the value obtained by dividing the thread width of the glass thread by TEX is in the range of 10 to 30. Claim 32 A glass yarn used for weaving glass cloth, wherein the silicon (Si) content of the glass yarn is 95.0 to 100 mass% in terms of silicon dioxide (SiO2), and furthermore, the snarl index of the glass yarn is 400 mm or less. Claim 33 In Clause 32, a glass thread having a snarl index of 70 mm or more. Claim 34 A glass thread according to claim 32 or 33, wherein the glass thread satisfies the ranges described in the following formulas (A), (B), and (C): (A) x+y+z=100 mass% (B) x≥99.5 mass% (C) 0.0003 ppm≤y≤0.50 ppm, x: silicon content when converted to silicon dioxide (SiO2), y: sum of uranium and thorium contents, z: sum of elements other than silicon, uranium, and thorium. Claim 35 A glass chamber according to claim 34, wherein y, representing the total content of the uranium and thorium, is in the range of 0.0003 to 0.0010 ppm. Claim 36 A glass chamber according to claim 34, wherein y, representing the total content of the uranium and thorium, is in the range of greater than 0.0010 and less than or equal to 0.0015 ppm. Claim 37 A glass chamber according to claim 34, wherein y, representing the total content of the uranium and thorium, is in the range of greater than 0.0015 and less than or equal to 0.0018 ppm. Claim 38 A glass chamber according to claim 34, wherein y, representing the total content of the uranium and thorium, is in the range of greater than 0.0018 and less than or equal to 0.0035 ppm. Claim 39 A glass chamber according to claim 34, wherein y, representing the total content of the uranium and thorium, is in the range of greater than 0.0035 and less than or equal to 0.0040 ppm. Claim 40 A glass chamber according to claim 34, wherein y, representing the total content of the uranium and thorium, is in the range of greater than 0.0040 and less than or equal to 0.09 ppm. Claim 41 A glass chamber according to claim 34, wherein y, representing the total content of the uranium and thorium, is in the range of greater than 0.09 and less than or equal to 0.12 ppm. Claim 42 A glass chamber according to claim 34, wherein y, representing the total content of the uranium and thorium, is in the range of greater than 0.12 and less than or equal to 0.50 ppm. Claim 43 A glass thread according to claim 32 or 33, wherein the snar index of the glass thread is in the range of 330 to 400 mm. Claim 44 A glass thread according to claim 32 or 33, wherein the snar index of the glass thread is in the range of 300 to 329 mm. Claim 45 A glass thread according to claim 32 or 33, wherein the snar index of the glass thread is in the range of 220 to 299 mm. Claim 46 A glass thread according to claim 32 or 33, wherein the snar index of the glass thread is in the range of 200 to 219 mm. Claim 47 A glass thread according to claim 32 or 33, wherein the snar index of the glass thread is in the range of 125 to 199 mm. Claim 48 A glass thread according to claim 32 or 33, wherein the snar index of the glass thread is in the range of 110 to 124 mm. Claim 49 A glass thread according to Article 32 or 33, wherein the snarl index of the glass thread is 110 mm or less.