An additive composition for modified asphalt, a method for preparing the same and a modified asphalt composition comprising the same

A copolymer composition with aromatic vinyl and conjugated diene monomers addresses asphalt's temperature resistance and viscosity issues, enhancing processability and stability for road paving and waterproofing.

KR103045481B1Active Publication Date: 2026-11-10KOREA KUMHO PETROCHEMICAL CO LTD
-1 Cites 0 Cited by

Patent Information

Application Number
KR1020230131545
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-10-04
Publication Date
2026-11-10
Estimated Expiration
2043-10-04

AI Technical Summary

Technical Problem

Existing asphalt compositions face issues with high and low temperature resistance, increased viscosity when modified with polymers, and difficulty in processing due to rapid viscosity rise, necessitating an additive that improves temperature resistance while maintaining low viscosity for improved processability.

Method used

A copolymer composition for modified asphalt, comprising aromatic vinyl and conjugated diene monomers with specific coupling agents, including a non-aromatic compound with epoxy groups, is used to enhance temperature resistance and reduce viscosity, allowing for better processability and storage stability.

Benefits of technology

The copolymer composition improves high and low temperature resistance, maintains low viscosity for easier processing, and ensures excellent storage stability, with a softening point equivalent to conventional compositions, suitable for road paving and waterproofing applications.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

One embodiment of the present specification provides an additive composition for modified asphalt comprising a copolymer represented by the following chemical formula 1: (ACB)nX In the above chemical formula 1, A is a block composed of aromatic vinyl monomers, B is a block composed of conjugated diene monomers, C is a first coupling agent, X is a second coupling agent, n is an integer from 2 to 4, and the second coupling agent is a non-aromatic compound having two or more epoxy groups.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] This specification relates to an additive composition for modified asphalt, a method for manufacturing the same, and a modified asphalt composition containing the same. Background Technology

[0002] Asphalt, used in applications such as road paving and the manufacture of waterproofing sheets, is significantly affected by temperature due to its inherent properties. It easily softens and deforms at high temperatures, while conversely, it cracks and is prone to damage at low temperatures. These issues frequently occur when asphalt is paved on roads. Over time, continuous exposure to high and low temperatures, along with constant impact from heavy objects such as passing vehicles, exacerbates the cracking and failure of the asphalt pavement.

[0003] As part of countermeasures for these problems, a method of adding asphalt modifiers to asphalt is known, and polymers such as polybutadiene, ethylene propylene rubber (EPDM, EPR), and styrene block copolymer (SBS, SIS) are used as asphalt modifiers. When asphalt modifiers are mixed into asphalt, the resistance of the asphalt to high and low temperatures is improved, thereby suppressing cracking and failure phenomena in asphalt pavements. Due to this effect, the use of modified asphalt with added modifiers in road pavements is increasing in industrial sites.

[0004] Meanwhile, styrene block copolymers used as asphalt modifiers can show improved effects as the input amount increases, but there is a problem in that increasing the input amount causes the viscosity of the asphalt to rise rapidly, making processing difficult. Therefore, there is a need to develop an additive for modified asphalt that can improve the resistance of asphalt at high and low temperatures, while simultaneously exhibiting low viscosity when mixed with asphalt so that a large amount can be input and the processability of the asphalt composition can be improved. The problem to be solved

[0005] The provisions of this specification are intended to solve the problems of the aforementioned prior art. One objective of this specification is to provide an additive composition for modified asphalt and a method for manufacturing the same, which improves the resistance of asphalt at high and low temperatures, exhibits low viscosity when mixed with asphalt so that a large amount can be added, and improves the processability of the asphalt composition.

[0006] Another objective of this specification is to provide a modified asphalt composition that has a softening point equivalent to or higher than that of conventional modified asphalt compositions, while simultaneously achieving excellent low-temperature properties and storage stability, and has excellent processability due to its low viscosity. means of solving the problem

[0007] According to one aspect, an additive composition for modified asphalt is provided, comprising a copolymer represented by the following chemical formula 1.

[0008] <Chemical Formula 1>

[0009] (ACB) n -X

[0010] In the above chemical formula 1, A is a block composed of aromatic vinyl monomers, B is a block composed of conjugated diene monomers, C is a first coupling agent, X is a second coupling agent, n is an integer from 2 to 4, and the second coupling agent is a non-aromatic compound having two or more epoxy groups.

[0011] In one embodiment, the aromatic vinyl monomer is styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 4-propylstyrene, 4-cyclohexylstyrene, 4-(p-methylphenyl)styrene, 5-tert-butyl-2-methylstyrene, tert-butoxystyrene, 2-tert-butylstyrene, 3-tert-butylstyrene, 4-tert-butylstyrene, N,N-dimethylaminoethylstyrene, 1-vinyl-5-hexylnaphthalene, 1-vinylnaphthalene, vinylbenzyldimethylamine, (4-vinylbenzyl)dimethylaminoethyl ether, vinylpyridine, vinylxylene, diphenylethylene, diphenylethylene including tertiary amines, primary, secondary, or It may be one selected from the group consisting of styrene containing a tertiary amine and combinations of two or more of these.

[0012] In one embodiment, the conjugated diene monomer may be one selected from the group consisting of 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 2-phenyl-1,3-butadiene, 3-methyl-1,3-pentadiene, 2-chloro-1,3-butadiene, 3-butyl-1,3-octadiene, octadiene, and combinations of two or more of these.

[0013] In one embodiment, the first coupling agent may be a compound having two or more vinyl groups.

[0014] In one embodiment, the first coupling agent may be one selected from the group consisting of divinylnaphthalene, divinylbenzene, 2,5-divinylthiophene, trivinylbenzene, 1,4-divinyloxybenzene, methoxy-substituted divinylbenzene, diisopropenbenzene, 4-(4-(2-isopropenphenoxy)butyl)styrene and combinations of two or more of these.

[0015] In one embodiment, the second coupling agent may be a non-aromatic compound having two or more epoxy groups and one or more alkyl halides.

[0016] In one embodiment, the content of the aromatic vinyl monomer in the copolymer may be 10 to 60 weight percent.

[0017] In one embodiment, the vinyl content of the block composed of the conjugated diene monomer may be 10 to 80 mol%.

[0018] In one embodiment, the weight-average molecular weight (Mw) of the copolymer may be 20,000 to 1,000,000 g / mol.

[0019] According to another aspect, a method for preparing an additive composition for modified asphalt is provided, comprising: (a) polymerizing an aromatic vinyl monomer in the presence of an initiator; (b) reacting the product of step (a) by introducing a first coupling agent; (c) polymerizing the product of step (b) by introducing a conjugated diene monomer; and (d) reacting the product of step (c) by introducing a second coupling agent, wherein the second coupling agent comprises a non-aromatic compound having two or more epoxy groups.

[0020] In one embodiment, the second coupling agent may be a hydrogenated bisphenol A type epoxy resin.

[0021] According to another aspect, a modified asphalt composition is provided, comprising asphalt; and an additive composition for the modified asphalt.

[0022] In one embodiment, based on 100 parts by weight of the asphalt, the content of the additive composition for the modified asphalt may be 0.5 to 40 parts by weight. Effects of the invention

[0023] An additive composition for modified asphalt according to one aspect of the present specification can improve the resistance of asphalt at high and low temperatures, while exhibiting low viscosity when mixed with asphalt, allowing a large amount to be added, and can improve the processability of the modified asphalt composition.

[0024] In addition, a modified asphalt composition according to another aspect of the present specification can have a softening point equivalent to or higher than that of a conventional modified asphalt composition, while simultaneously achieving excellent low-temperature characteristics and storage stability, and can exhibit excellent processability due to its low viscosity.

[0025] The effects of one aspect of this specification are not limited to the effects described above, and should be understood to include all effects that can be inferred from the configurations described in the detailed description or claims of this specification. Specific details for implementing the invention

[0026] Hereinafter, one aspect of this specification will be described based on specific examples. However, the details described in this specification may be implemented in various different forms and are therefore not limited to the embodiments described herein.

[0027] Throughout the specification, when it is stated that a part is "connected" to another part, this includes not only cases where they are "directly connected," but also cases where they are "indirectly connected" with other members interposed between them. Furthermore, when it is stated that a part "includes" a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but rather allows for the inclusion of additional components.

[0028] When a range of numerical values ​​is described in this specification, unless a specific range is otherwise described, the value has the precision of significant figures provided according to the standard rules in chemistry for significant figures. For example, 10 includes a range of 5.0 to 14.9, and the number 10.0 includes a range of 9.50 to 10.49.

[0029] Additive composition for modified asphalt

[0030] An additive composition for modified asphalt according to one aspect of the present specification comprises a copolymer represented by the following chemical formula 1.

[0031] <Chemical Formula 1>

[0032] (ACB) n -X

[0033] In the above chemical formula 1, A is a block composed of aromatic vinyl monomers, B is a block composed of conjugated diene monomers, C is a first coupling agent, X is a second coupling agent, n is an integer from 2 to 4, and the second coupling agent is a non-aromatic compound having two or more epoxy groups.

[0034] The above aromatic vinyl monomer is styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 4-propylstyrene, 4-cyclohexylstyrene, 4-(p-methylphenyl)styrene, 5-tert-butyl-2-methylstyrene, tert-butoxystyrene, 2-tert-butylstyrene, 3-tert-butylstyrene, 4-tert-butylstyrene, N,N-dimethylaminoethylstyrene, 1-vinyl-5-hexylnaphthalene, 1-vinylnaphthalene, vinylbenzyldimethylamine, (4-vinylbenzyl)dimethylaminoethyl ether, vinylpyridine, vinylxylene, diphenylethylene, diphenylethylene including tertiary amines, primary, secondary, or tertiary amines It may be one selected from the group consisting of styrene containing and combinations of two or more of these, but is not limited thereto.

[0035] The above conjugated diene monomer may be one selected from the group consisting of 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 2-phenyl-1,3-butadiene, 3-methyl-1,3-pentadiene, 2-chloro-1,3-butadiene, 3-butyl-1,3-octadiene, octadiene, and combinations of two or more of these, but is not limited thereto.

[0036] The first coupling agent and the second coupling agent may be of the same or different types. The additive composition for modified asphalt may be prepared by reacting two or more coupling agents simultaneously or sequentially, and accordingly, compared to a copolymer prepared using one type of coupling agent, it may have a higher coupling number or, even if the coupling number is the same, may exhibit a lower solution viscosity due to higher solubility in asphalt, and accordingly, may exhibit excellent processability, workability, and storage stability.

[0037] The first coupling agent may be a compound having two or more vinyl groups. When the first coupling agent is a compound having two or more vinyl groups and the second coupling agent is a non-aromatic compound having two or more epoxy groups, the number of couplings increases compared to a conventional additive composition for modified asphalt, thereby reducing the viscosity of the modified asphalt composition. Even if the number of couplings is the same, high-temperature characteristics such as the softening point, low-temperature characteristics such as the plastic embrittlement point, and storage stability of the modified asphalt composition can be improved in a balanced manner.

[0038] The first coupling agent is divinylnaphthalene (e.g., 1,4-divinylnaphthalene, 1,6-divinylnaphthalene, 1,8-divinylnaphthalene, 2,7-divinylnaphthalene), divinylbenzene (e.g., 1,2-divinylbenzene, 1,3-divinylbenzene, 1,4-divinylbenzene), 2,5-divinylthiophene (e.g., 3-hexyl-2,5-divinylthiophene, 3-methyl-2,5-divinylthiophene), trivinylbenzene (e.g., 1,2,3-trivinylbenzene, 1,2,4-trivinylbenzene, 1,3,5-trivinylbenzene), 1,4-divinyloxybenzene, methoxy-substituted divinylbenzene (e.g., It may be one selected from the group consisting of 2-methoxy-1,4-divinylbenzene, 4-methoxy-1,2-divinylbenzene, 4-methoxy-1,3-divinylbenzene, 2-methoxy-1,3-divinylbenzene, 5-methoxy-1,3-divinylbenzene), diisopropenbenzene (e.g., 1,4-diisopropenbenzene, 1,2-diisopropenbenzene, 1,3-diisopropenbenzene), 4-(4-(2-isopropenphenylphenoxy)butyl)styrene and combinations of two or more of these, and may be, for example, divinylbenzene, but is not limited thereto.

[0039] The second coupling agent may be a non-aromatic compound having two or more epoxy groups and one or more alkyl halide groups. That is, the second coupling agent may be a non-aromatic compound having two or more epoxy groups and not including an alkyl halide group, or a non-aromatic compound having both two or more epoxy groups and one or more alkyl halide groups. For example, the second coupling agent may be a non-aromatic compound having two epoxy groups and not including an alkyl halide group, a non-aromatic compound having two epoxy groups and one alkyl halide group, or a non-aromatic compound having two epoxy groups and two alkyl halide groups, but is not limited thereto.

[0040] The above alkyl halide group may be one selected from the group consisting of alkyl chloride, alkyl fluoride, alkyl bromide, alkyl iodide, and combinations of two or more of these.

[0041] The above additive composition for modified asphalt includes the second coupling agent, thereby exhibiting a higher coupling number compared to conventional additive compositions for modified asphalt, and accordingly exhibiting low viscosity when mixed with asphalt, allowing a larger amount of the additive composition to be added to the asphalt compared to conventional methods.

[0042] The content of the aromatic vinyl monomer in the copolymer may be 10 to 60 wt%, preferably 15 to 40 wt%, but is not limited thereto. For example, it may be 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, 60 wt%, or a range between two of these values. If the content of the aromatic vinyl monomer is less than the above range, the softening point of the modified asphalt composition may be lowered, and if it exceeds the above range, the low-temperature properties may be lowered.

[0043] The vinyl content of the block composed of the above conjugated diene monomer may be 10 to 80 mol%, preferably 50 to 70 mol%, but is not limited thereto. For example, it may be 10 mol%, 15 mol%, 20 mol%, 25 mol%, 30 mol%, 35 mol%, 40 mol%, 45 mol%, 50 mol%, 55 mol%, 60 mol%, 65 mol%, 70 mol%, 75 mol%, 80 mol%, or a range between two of these values. If the vinyl content of the block composed of the conjugated diene monomer satisfies the above range, it may exhibit excellent solubility with respect to asphalt. If the vinyl content is below the above range, the high-temperature properties of the modified asphalt composition may be degraded, and if it exceeds the above range, storage stability may be reduced or viscosity may increase.

[0044] The weight-average molecular weight (Mw) of the copolymer may be 20,000 to 1,000,000 g / mol, preferably 20,000 to 300,000 g / mol, and more preferably 20,000 to 150,000 g / mol, but is not limited thereto. For example, 20,000 g / mol, 40,000 g / mol, 60,000 g / mol, 80,000 g / mol, 100,000 g / mol, 110,000 g / mol, 120,000 g / mol, 130,000 g / mol, 140,000 g / mol, 150,000 g / mol, 160,000 g / mol, 170,000 g / mol, 180,000 g / mol, 190,000 g / mol, 200,000 g / mol, 300,000 g / mol, 400,000 g / mol, 500,000 g / mol, 600,000 g / mol, 700,000 g / mol, It may be 800,000 g / mol, 900,000 g / mol, 1,000,000 g / mol, or a range between two of these values. If the weight-average molecular weight of the copolymer is below the above range, high-temperature properties such as the softening point of the modified asphalt composition may be reduced, or the expression of mechanical application properties may not be easy, and if it exceeds the above range, storage stability may be reduced, or processability may be reduced due to increased viscosity.

[0045] In addition to the copolymer represented by Chemical Formula 1, the above additive composition for modified asphalt may further include a block copolymer in which a block composed of aromatic vinyl monomers and a block composed of conjugated diene monomers are directly bonded without a coupling agent, a copolymer in which the block copolymers are bonded to one another or bonded through a coupling agent, but is not limited thereto.

[0046] Method for preparing an additive composition for modified asphalt

[0047] A method for preparing an additive composition for modified asphalt according to another aspect of the present specification comprises: (a) polymerizing an aromatic vinyl monomer in the presence of an initiator; (b) reacting the product of step (a) by introducing a first coupling agent; (c) polymerizing the product of step (b) by introducing a conjugated diene monomer; and (d) reacting the product of step (c) by introducing a second coupling agent; wherein the second coupling agent comprises a non-aromatic compound having two or more epoxy groups.

[0048] The types of monomer and first coupling agent used in the above manufacturing method are the same as those described above.

[0049] Step (a) above is a step of polymerizing an aromatic vinyl monomer in the presence of an initiator to form a block composed of the aromatic vinyl monomer. In Step (a), the polymerization reaction of the aromatic vinyl monomer is initiated to produce a living polymer.

[0050] The above initiator may be an organic lithium compound such as n-butyllithium, but is not limited thereto, and a conventional anionic initiator may be used.

[0051] The above step (a) may include the step of introducing an aromatic vinyl monomer and an initiator into a reactor.

[0052] The above step (a) may further include the step of introducing a polar modifier into the reactor. When the polar modifier is introduced, the vinyl content of the block composed of conjugated diene monomers can be controlled.

[0053] The above polar modifier may be one selected from the group consisting of ditetrahydrofurylpropane (DTHFP), tetramethylethylenediamine (TMEDA), tetrahydrofuran (THF), and combinations of two or more of these, but is not limited thereto.

[0054] In step (b) above, some of the living polymer may be coupled with the residue of the first coupling agent.

[0055] Step (c) above is a step of polymerizing conjugated diene monomers to form a block composed of conjugated diene monomers. In Step (c), the living polymer coupled with the first coupling agent may react with the polymer of conjugated diene monomers to form a block copolymer represented by the following chemical formula 2.

[0056] <Chemical Formula 2>

[0057] ACB

[0058] In the above chemical formula 2, A is a block composed of aromatic vinyl monomers, B is a block composed of conjugated diene monomers, and C is a first coupling agent.

[0059] The weight-average molecular weight (Mw) of the block copolymer represented by the above chemical formula 2 may be 5,000 to 500,000 g / mol. For example, 5,000 g / mol, 10,000 g / mol, 15,000 g / mol, 20,000 g / mol, 25,000 g / mol, 30,000 g / mol, 35,000 g / mol, 40,000 g / mol, 45,000 g / mol, 50,000 g / mol, 55,000 g / mol, 60,000 g / mol, 65,000 g / mol, 70,000 g / mol, 75,000 g / mol, 80,000 g / mol, 85,000 g / mol, 90,000 g / mol, 95,000 g / mol, 100,000 g / mol, 150,000 g / mol, 200,000 It may be g / mol, 250,000 g / mol, 300,000 g / mol, 350,000 g / mol, 400,000 g / mol, 450,000 g / mol, 500,000 g / mol, or a range between two of these values. If the weight-average molecular weight of the block copolymer represented by Chemical Formula 2 is less than the above range, the high-temperature properties of the modified asphalt composition may be reduced, and if it exceeds the above range, the viscosity may increase, thereby reducing processability or storage stability.

[0060] In step (d) above, some of the block copolymer represented by the chemical formula 2 may be coupled with the residue of the second coupling agent.

[0061] The second coupling agent comprises a non-aromatic compound having two or more epoxy groups, and accordingly, the additive composition for modified asphalt prepared by the above method has a higher number of couplings compared to conventional additive compositions for modified asphalt, or even if the number of couplings is the same, it has a higher solubility in asphalt and exhibits low solution viscosity, and accordingly can exhibit excellent processability, workability, and storage stability.

[0062] The second coupling agent may include a non-aromatic compound having two or more epoxy groups and one or more alkyl halides. When the second coupling agent includes a non-aromatic compound having two or more epoxy groups and one or more alkyl halides, the additive composition for modified asphalt prepared by the above method may exhibit a higher coupling number compared to conventional additive compositions for modified asphalt, and accordingly exhibit low viscosity when mixed with asphalt, allowing a larger amount of the additive composition to be added to the asphalt compared to conventional methods.

[0063] The second coupling agent may be a mixture of a non-aromatic compound having two or more epoxy groups and not including an alkyl halide group, and a non-aromatic compound having both two or more epoxy groups and one or more alkyl halide groups. For example, the second coupling agent may be a mixture comprising 40 to 60 weight% of a non-aromatic compound having two or more epoxy groups and not including an alkyl halide group, and 40 to 60 weight% of a non-aromatic compound having both two or more epoxy groups and one or more alkyl halide groups, but is not limited thereto.

[0064] The second coupling agent may be a mixture of a non-aromatic compound having two epoxy groups and not including an alkyl halide group, a non-aromatic compound having two epoxy groups and one alkyl halide group, and a non-aromatic compound having two epoxy groups and two alkyl halide groups, but is not limited thereto.

[0065] The second coupling agent may be a hydrogenated bisphenol A type epoxy resin. Compared to a bisphenol A type epoxy resin containing aromatic compounds, the hydrogenated bisphenol A type epoxy resin has less yellowing and excellent weather resistance, and has low viscosity, which can exhibit excellent workability and reduce the viscosity of the modified asphalt composition.

[0066] The second coupling agent may be the reaction product of hydrogenated bisphenol A and epichlorohydrin (CAS No. 30583-72-3), but is not limited thereto.

[0067] The total weight-average molecular weight (Mw) of the additive composition for modified asphalt prepared by the above method may be 5,000 to 500,000 g / mol. For example, 5,000 g / mol, 10,000 g / mol, 15,000 g / mol, 20,000 g / mol, 25,000 g / mol, 30,000 g / mol, 35,000 g / mol, 40,000 g / mol, 45,000 g / mol, 50,000 g / mol, 55,000 g / mol, 60,000 g / mol, 65,000 g / mol, 70,000 g / mol, 75,000 g / mol, 80,000 g / mol, 85,000 g / mol, 90,000 g / mol, 95,000 g / mol, 100,000 g / mol, 150,000 g / mol, 200,000 It may be g / mol, 250,000 g / mol, 300,000 g / mol, 350,000 g / mol, 400,000 g / mol, 450,000 g / mol, 500,000 g / mol, or a range between two of these values. If the total weight-average molecular weight is below the above range, the high-temperature properties of the modified asphalt composition may be degraded, and if it exceeds the above range, the viscosity may increase, resulting in reduced processability, reduced storage stability, or a decrease in the amount of additives that can be added to the asphalt.

[0068] The coupling efficiency of the additive composition for modified asphalt prepared by the above method may be 15 to 96%, preferably 15 to 40%, but is not limited thereto. For example, it may be 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, or a range between two of these values. If the coupling efficiency is below the above range, high-temperature characteristics such as the softening point of the modified asphalt composition may be reduced, and if it exceeds the above range, storage stability may be reduced or processability may be reduced due to increased viscosity.

[0069] Modified asphalt composition

[0070] A modified asphalt composition according to another aspect of the present specification comprises asphalt; and an additive composition for modified asphalt.

[0071] The additive composition for modified asphalt may include a copolymer represented by Chemical Formula 1. In another example, the additive composition for modified asphalt may be prepared by the above manufacturing method, but is not limited thereto.

[0072] Based on 100 parts by weight of the asphalt, the content of the additive composition for the modified asphalt may be 0.5 to 40 parts by weight. For example, it may be 0.5 parts by weight, 1 part by weight, 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, 3 parts by weight, 3.5 parts by weight, 4 parts by weight, 4.5 parts by weight, 5 parts by weight, 5.5 parts by weight, 6 parts by weight, 6.5 parts by weight, 7 parts by weight, 7.5 parts by weight, 8 parts by weight, 8.5 parts by weight, 9 parts by weight, 9.5 parts by weight, 10 parts by weight, 15 parts by weight, 20 parts by weight, 25 parts by weight, 30 parts by weight, 35 parts by weight, 40 parts by weight, or a range between two of these values. If the content of the additive composition for modified asphalt is below the above range, the concentration of the polymer is too low, making it difficult to exhibit performance as a modifier; if it exceeds the above range, the viscosity increases, which reduces the dispersibility between the asphalt and the additive composition for modified asphalt and the flowability of the modified asphalt composition, thereby delaying the dispersion time.

[0073] The above modified asphalt composition can have a softening point equivalent to or higher than that of conventional modified asphalt compositions, while simultaneously achieving excellent low-temperature characteristics and storage stability, and can exhibit excellent processability due to its low viscosity. Due to these excellent characteristics, the above modified asphalt composition may not contain sulfur-based crosslinking agents, and accordingly, can exhibit environmentally friendly characteristics.

[0074] The above modified asphalt composition may be used for road paving, waterproofing sheets, or sealants, but is not limited thereto.

[0075] The embodiments of this specification will be described in more detail below. However, the following experimental results represent only representative results among the above embodiments, and the scope and content of this specification should not be interpreted as being narrowed or limited by the embodiments. The respective effects of various embodiments of this specification not explicitly presented below will be described in detail in the relevant sections.

[0076] Example 1

[0077] The interior of a 5L internal pressure reactor was sufficiently replaced with nitrogen gas. 2.4 kg of purified cyclohexane, 400 ppm of polar modifier, and 132 g of styrene were injected into the reactor, and after maintaining the temperature at 50 ℃, 0.21 phm of n-butyllithium, an initiator, was introduced into the reactor to start the polymerization reaction. When the polymerization temperature reached its maximum, 0.0132 phm of divinylbenzene (DVB) was injected, and after 10 minutes, 268 g of butadiene was introduced to proceed with polymerization. 5 minutes after the polymerization temperature reached its maximum, 0.10 phm of KER-950 (Kumho P&B Chemical, CAS No. 30583-72-3), a coupling agent, was introduced to proceed with coupling. After 15 minutes, caprylic acid, a polymerization terminator, was added to the polymerization solution to completely remove the activity of the living polymer. An antioxidant was added to the terminated polymerization solution, and cyclohexane was removed using a roll mill to prepare a copolymer.

[0078] Example 2

[0079] A copolymer was prepared in the same manner as in Example 1, except that 0.15 phm of n-butyllithium was added.

[0080] Example 3

[0081] A copolymer was prepared in the same manner as in Example 1, except that 0.19 phm of n-butyllithium was added and 0.0264 phm of divinylbenzene was added.

[0082] Example 4

[0083] A copolymer was prepared in the same manner as in Example 3 above, except that 0.17 phm of n-butyllithium was added.

[0084] Example 5

[0085] A copolymer was prepared in the same manner as in Example 3 above, except that 0.17 phm of n-butyllithium was added and 0.09 phm of KER-950 was added.

[0086] Comparative Example 1

[0087] The interior of a 5L internal pressure reactor was sufficiently purged with nitrogen gas. 2.4 kg of purified cyclohexane, 400 ppm of polar modifier, and 132 g of styrene were injected into the reactor, and after maintaining the temperature at 50 ℃, 0.21 phm of n-butyllithium, an initiator, was introduced into the reactor to initiate the polymerization reaction. 10 minutes after the polymerization temperature reached its maximum, 268 g of butadiene was introduced to proceed with polymerization. 5 minutes after the polymerization temperature reached its maximum, 0.04 phm of dichlorodimethylsilane was introduced as a coupling agent to proceed with coupling. After 15 minutes, caprylic acid, a polymerization terminator, was added to the polymerization solution to completely eliminate the activity of the living polymer. An antioxidant was added to the terminated polymerization solution, and the cyclohexane was removed using a roll mill to produce a copolymer.

[0088] Experimental Example 1

[0089] The molecular weight, coupling efficiency, and composition of each copolymer prepared in Examples 1 to 5 and Comparative Example 1 were analyzed in the following manner, and the results are shown in Table 1 below.

[0090] 1) Molecular weight analysis

[0091] In the above Examples 1 to 5, the weight-average molecular weight before coupling using KER-950 (Mw before coupling), the weight-average molecular weight of the coupled structure formed after coupling (Mw after coupling), and the weight-average molecular weight of the entire product (total Mw) were each measured.

[0092] The weight-average molecular weight of each sample was analyzed using high-performance liquid chromatography (separation's module Waters 2690). The analysis was performed under conditions of a column temperature of 40°C, THF solvent, and a flow rate of 1.0 mL / min. Divinylbenzene Styragel HR 5E, HR 4, and HR 2 columns were connected in series, and the difference in refractive index was detected by a refractive index detector relative to a polystyrene standard sample.

[0093] 2) Coupling efficiency analysis

[0094] The coupling efficiency was analyzed according to Equation 1 below using the area of ​​the polymer peaks observed in GPC (gel permeation chromatography).

[0095] <Equation 1>

[0096] Coupling efficiency (%) = {(Area of ​​coupled polymer) / (Total area of ​​polymer)} × 100

[0097] 3) Composition Analysis

[0098] The styrene content in the copolymer and the vinyl content of the butadiene block were analyzed.

[0099] Styrene and vinyl content analysis was performed using a nuclear magnetic resonance analyzer (Bruker NMR-400), and the samples were analyzed using chloroform-d as a solvent.

[0100] division Mw (g / mol) before coupling Mw (g / mol) after coupling Total Mw(g / mol) Coupling efficiency (%) Styrene content (weight%) Vinyl content (mol%) Example 1 47,300 119,700 61,300 21.7 32.5 59.4 Example 2 51,700 126,400 67,900 23.9 32.5 59.9 Example 3 49,500 126,000 65,400 22.6 32.4 58.2 Example 4 45,500 113,500 59,200 21.9 32.4 56.7 Example 5 45,300 111,200 57,800 20.4 32.3 56.7 Comparative Example 1 54,300 119,400 68,900 23.9 32.1 63.5

[0101] Preparation Example

[0102] A modified asphalt composition was prepared by mixing the copolymer prepared in the above examples and comparative examples and molten pure asphalt with a high-speed shear mixer at 180°C for 2 hours. The composition ratio of the modified asphalt composition is shown in Table 2 below.

[0103] division Pure asphalt copolymer Content (parts by weight) type Content (parts by weight) Preparation Example 1 100 Example 1 7.5 Preparation Example 2 100 Example 2 7.5 Preparation Example 3 100 Example 3 7.5 Preparation Example 4 100 Example 4 7.5 Preparation Example 5 100 Example 5 7.5 Comparative Manufacturing Example 1 100 Comparative Example 1 7.5

[0104] Experimental Example 2

[0105] The physical properties of each modified asphalt composition prepared in Manufacturing Examples 1 to 5 and Comparative Manufacturing Example 1 were measured in the following manner, and the results are shown in Table 3 below.

[0106] 1) Softening point: Measured according to ASTM D36.

[0107] 2) Fraass breaking point: Measured according to EN 12593.

[0108] 3) Difference in softening point between phases: To evaluate storage stability, the difference in softening point between the top and bottom of the separated composition was measured according to ASTM D7173.

[0109] 4) Rotational viscosity @135 ℃: Measured according to ASTM D4402.

[0110] division Softening point (°C) Plasma embrittlement point (°C) Difference in softening point between phases (°C) Rotational viscosity (cps) Preparation Example 1 86.6 -18.7 17.8 2300 Preparation Example 2 90 -24.3 32 2775 Preparation Example 3 88.5 -20.7 19.6 2475 Preparation Example 4 87.5 -22.3 19.6 2150 Preparation Example 5 87.2 -22.0 15.3 2100 Comparative Manufacturing Example 1 82.2 -19.1 23.3 2725

[0111] Referring to Table 3 above, it was confirmed that the modified asphalt composition of Manufacturing Example 1 has excellent storage stability with a small difference in phase separation softening point compared to the modified asphalt composition of Comparative Example 1, excellent high-temperature characteristics with a high softening point, and low viscosity.

[0112] The modified asphalt composition of Preparation Example 2, prepared using the copolymer of Example 2 which had a higher weight-average molecular weight before coupling compared to Example 1, had excellent high and low temperature properties due to its high softening point and low plastic embrittlement point, but it was confirmed that the difference in phase separation softening point and viscosity were somewhat high.

[0113] The modified asphalt composition of Preparation Example 3, prepared using the copolymer of Example 3 in which the amount of divinylbenzene added was doubled compared to Example 1, exhibited excellent high and low temperature characteristics, excellent storage stability with a small difference in phase separation softening point, and also showed a low viscosity value.

[0114] It was confirmed that the modified asphalt composition of Preparation Example 4, prepared using the copolymer of Example 4 which has a lower weight-average molecular weight before coupling and a lower total weight-average molecular weight compared to Example 3, has excellent high and low temperature characteristics, excellent storage stability with a small difference in phase separation softening point, and low viscosity.

[0115] It was confirmed that the modified asphalt composition of Preparation Example 5, prepared using the copolymer of Example 5 with reduced coupling efficiency compared to Example 3 by reducing the amount of KER-950 input, has excellent high and low temperature characteristics, excellent storage stability with a small difference in phase separation softening point, and low viscosity.

[0116] The foregoing description of this specification is for illustrative purposes only, and those skilled in the art to which one aspect of this specification pertains will understand that other specific forms can be easily modified without altering the technical concept or essential features described in this specification. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. For example, each component described as a single unit may be implemented in a distributed manner, and components described as distributed may likewise be implemented in a combined form.

[0117] The scope of this specification is defined by the claims set forth below, and all modifications or variations derived from the meaning and scope of the claims and equivalent concepts thereof should be interpreted as being included within the scope of this specification.

Claims

Claim 1 Additive composition for modified asphalt comprising a copolymer represented by the following chemical formula 1, having a coupling efficiency of 40% or less: <Chemical Formula 1> (ACB) n - In the above chemical formula 1, A is a block composed of aromatic vinyl monomers, B is a block composed of conjugated diene monomers, C is a first coupling agent, X is a second coupling agent, n is an integer from 2 to 4, and the second coupling agent is a hydrogenated bisphenol A type epoxy resin having two or more epoxy groups. Claim 2 In claim 1, the aromatic vinyl monomer is styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 4-propylstyrene, 4-cyclohexylstyrene, 4-(p-methylphenyl)styrene, 5-tert-butyl-2-methylstyrene, tert-butoxystyrene, 2-tert-butylstyrene, 3-tert-butylstyrene, 4-tert-butylstyrene, N,N-dimethylaminoethylstyrene, 1-vinyl-5-hexylnaphthalene, 1-vinylnaphthalene, vinylbenzyldimethylamine, (4-vinylbenzyl)dimethylaminoethyl ether, vinylpyridine, vinylxylene, diphenylethylene, diphenylethylene including tertiary amines, primary, secondary, or An additive composition for modified asphalt, comprising styrene containing a tertiary amine and one selected from the group consisting of a combination of two or more of these. Claim 3 The additive composition for modified asphalt according to claim 1, wherein the conjugated diene monomer is one selected from the group consisting of 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 2-phenyl-1,3-butadiene, 3-methyl-1,3-pentadiene, 2-chloro-1,3-butadiene, 3-butyl-1,3-octadiene, octadiene, and combinations of two or more of these. Claim 4 An additive composition for modified asphalt according to claim 1, wherein the first coupling agent is a compound having two or more vinyl groups. Claim 5 An additive composition for modified asphalt according to claim 1, wherein the first coupling agent is one selected from the group consisting of divinylnaphthalene, divinylbenzene, 2,5-divinylthiophene, trivinylbenzene, 1,4-divinyloxybenzene, methoxy-substituted divinylbenzene, diisopropenylbenzene, 4-(4-(2-isopropenylphenoxy)butyl)styrene and combinations of two or more of these. Claim 6 delete Claim 7 An additive composition for modified asphalt according to claim 1, wherein the content of the aromatic vinyl monomer in the copolymer is 10 to 60 weight%. Claim 8 An additive composition for modified asphalt according to claim 1, wherein the vinyl content of the block composed of the conjugated diene monomer is 10 to 80 mol%. Claim 9 An additive composition for modified asphalt according to claim 1, wherein the weight-average molecular weight (Mw) of the copolymer is 20,000 to 1,000,000 g / mol. Claim 10 A method for preparing an additive composition for modified asphalt, comprising: (a) a step of polymerizing an aromatic vinyl monomer in the presence of an initiator; (b) a step of reacting the product of step (a) by introducing a first coupling agent; (c) a step of polymerizing the product of step (b) by introducing a conjugated diene monomer; and (d) a step of reacting the product of step (c) by introducing a second coupling agent; wherein the second coupling agent is a hydrogenated bisphenol A type epoxy resin having two or more epoxy groups. Claim 11 delete Claim 12 A modified asphalt composition comprising asphalt; and the additive composition for modified asphalt of claim 1. Claim 13 A modified asphalt composition according to claim 12, wherein, based on 100 parts by weight of the asphalt, the content of the additive composition for the modified asphalt is 0.5 to 40 parts by weight.