Encapsulant for Organic EL Display Devices
The use of cycloaliphatic epoxy compounds and flexible epoxy compounds with photocatalytic and thermal cationic initiators addresses the curing and adhesion issues in light-shielding areas, improving the durability and stability of organic EL display devices.
Patent Information
- Application Number
- KR1020227028289
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-07-27
- Filing Date
- 2021-07-19
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2041-07-19
AI Technical Summary
Existing encapsulants for organic EL display devices fail to achieve sufficient curing and adhesion when placed in light-shielding areas, leading to reduced durability and lifespan due to insufficient photocuring and inferior thermal curing properties.
A curable resin composition comprising cycloaliphatic epoxy compounds and epoxy compounds with flexible backbones, combined with photocatalytic and thermal cationic polymerization initiators, ensures adequate curing and adhesion even in light-shielding conditions.
The encapsulant provides excellent adhesion and sufficient curing in light-shielding areas, enhancing the durability and stability of organic EL display devices by preventing moisture and oxygen ingress.
Smart Images

Figure 112022085420175-PCT00001 
Figure 112022085420175-PCT00002 
Figure 112022085420175-PCT00003
Abstract
Description
Technology Field
[0001] The present invention relates to an encapsulant for an organic EL display element that has excellent adhesion and can be sufficiently cured even when placed in a light-shielding area. Background Technology
[0002] An organic electroluminescent display device (organic EL display device) has a thin film structure in which an organic light-emitting material layer is sandwiched between a pair of electrodes facing each other. Electrons are injected into the organic light-emitting material layer from one electrode and holes are injected from the other electrode, causing the electrons and holes to combine within the organic light-emitting material layer to perform self-luminescence. Compared to liquid crystal display devices that require a backlight, it has the advantages of good visibility, the ability to be made thinner, and the ability to drive at low DC voltage.
[0003] However, such organic EL display devices have a problem in that their light-emitting properties deteriorate rapidly and their lifespan is shortened when the organic light-emitting material layer or electrodes are exposed to the outside air. Therefore, in order to increase the stability and durability of organic EL display devices, encapsulation technology that blocks the organic light-emitting material layer or electrodes from moisture or oxygen in the atmosphere has become indispensable for organic EL display devices.
[0004] Patent Document 1 discloses a method for encapsulating an organic EL display element by a configuration comprising an organic filler layer that encapsulates a laminate having an organic light-emitting material layer, and a moisture-absorbing seal layer (encapsulation wall) that covers the side of the organic filler layer. Typically, as an encapsulator for an organic EL display element, an in-plane encapsulator is used in the organic filler layer, and an outer encapsulator with a different composition from the in-plane encapsulator is used in the encapsulation wall. Prior art literature
[0005] Japanese Patent Publication No. 2014-67598 The problem to be solved
[0006] The present invention aims to provide an encapsulant for an organic EL display element that has excellent adhesion and can be sufficiently cured even when placed in a light-shielding area. means of solving the problem
[0007] The present invention is an encapsulant for an organic EL display device comprising a curable resin, a photocatalytic polymerization initiator, a thermal cationic polymerization initiator, and a filler, wherein the curable resin comprises a cycloaliphatic epoxy compound and an epoxy compound having a flexible backbone.
[0008] The present invention is described in detail below.
[0009] Recently, in organic EL display devices, the frame of the display portion has been narrowing, and the encapsulant for the organic EL display device is placed directly below the electrode, etc., and when the encapsulant is photocured, the light irradiated is blocked, so the light does not reach the interior of the encapsulant, resulting in insufficient curing. The inventors considered using a thermal cation polymerization initiator to heat-cur the parts where photocuring was insufficient, in addition to the photocation polymerization initiator for photocuring the cation polymerization compound, for an encapsulant for an organic EL display device containing a cation polymerizable compound. However, when heat-curing was performed using a thermal cation polymerization initiator, the resulting encapsulant had inferior adhesive properties, or conversely, the curability in the light-blocking portion decreased. Therefore, the inventors considered using a combination of a cycloaliphatic epoxy compound and an epoxy compound having a flexible framework as a curable resin in an encapsulant for an organic EL display device containing a photocation polymerization initiator and a thermal cation polymerization initiator. As a result, it was discovered that an encapsulant for an organic EL display element with excellent adhesion and capable of sufficient curing even when placed in a light-shielding area can be obtained, and thus the present invention was completed.
[0010] The encapsulant for organic EL display elements of the present invention contains a curable resin.
[0011] The above-mentioned curable resin comprises a cycloaliphatic epoxy compound and an epoxy compound having a flexible backbone. By including the photocatalytic polymerization initiator described below and the thermal cationic polymerization initiator described below, and by including the cycloaliphatic epoxy compound and the epoxy compound having a flexible backbone as the curable resin, the encapsulant for an organic EL display device according to the present invention has excellent adhesion and can be sufficiently cured even when placed in a light-shielding area.
[0012] The above-mentioned alicyclic epoxy compounds include, for example, 3',4'-epoxycyclohexylmethyl(3,4-epoxy)cyclohexanecarboxylate, 1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol, 3',4'-epoxycyclohexylmethyl(meth)acrylate, 1,2:8,9-diepoxylimonene, 4-vinylcyclohexenediooxide, vinylcyclohexenediooxide, methylated vinylcyclohexenediooxide, bis(3,4-epoxycyclohexylmethyl)ether, 3,4,3',4'-diepoxybicyclohexyl, bis(3,4-epoxycyclohexyl)adipate, bis(2,3-epoxycyclopentyl)ether, Examples include bis(3,4-epoxy-6-methylcyclohexylmethyl)adipate and dicyclopentadiene dioxide. Among these, 3',4'-epoxycyclohexylmethyl(3,4-epoxy)cyclohexanecarboxylate is preferred.
[0013] Examples of flexible frameworks for the epoxy compound having the above-mentioned flexible framework include a ring-opening structure of a lactone, a polyalkylene oxide structure, a rubber structure derived from a conjugated diene, a polysiloxane structure, etc. Among these, at least one structure selected from the group consisting of a ring-opening structure of a lactone, a polyalkylene oxide structure, a rubber structure derived from a conjugated diene, and a polysiloxane structure is preferred, and a polyalkylene oxide structure is more preferred.
[0014] As for the epoxy compound having the above flexible framework, specifically, a compound represented by the following formula (1) is preferred.
[0015] [Chemical Formula 1]
[0016]
[0017] In formula (1), X represents an ethyleneoxyethyl group, a di(ethyleneoxy)ethyl group, a tri(ethyleneoxy)ethyl group, a tetra(ethyleneoxy)ethyl group, a propyleneoxypropyl group, a di(propyleneoxy)propyl group, a tri(propyleneoxy)propyl group, a tetra(propyleneoxy)propyl group, a butyleneoxybutyl group, a di(butyleneoxy)butyl group, a tri(butyleneoxy)butyl group, a tetra(butyleneoxy)butyl group, or an alkylene group having 2 or more carbon atoms and 15 or fewer carbon atoms, and n is 1 to 10.
[0018] Among the compounds represented by the above formula (1) that are commercially available, examples include EPICLON EXA-4850-150 and EPICLON EXA-4850-1000 (both manufactured by DIC).
[0019] The content ratio of the alicyclic epoxy compound and the epoxy compound having a flexible framework (alicyclic epoxy compound: epoxy compound having a flexible framework) is preferably 2:1 to 1:3 by weight. By having the content ratio of the alicyclic epoxy compound and the epoxy compound having a flexible framework within this range, the encapsulant for organic EL display devices obtained has superior adhesion and superior curability in the light-shielding portion. It is more preferable that the content ratio of the alicyclic epoxy compound and the epoxy compound having a flexible framework (alicyclic epoxy compound: epoxy compound having a flexible framework) is 1:1 to 1:2 by weight.
[0020] The above-mentioned curable resin may contain other curable resins in addition to the above-mentioned cycloaliphatic epoxy compound and the above-mentioned epoxy compound having a flexible framework.
[0021] When containing the above other curable resin, the preferred lower limit of the total content of the alicyclic epoxy compound and the epoxy compound having a flexible framework in 100 parts by weight of the curable resin is 60 parts by weight. By having a total content of the alicyclic epoxy compound and the epoxy compound having a flexible framework of 60 parts by weight or more, the encapsulant for organic EL display devices obtained has superior adhesion and light-shielding curability. A more preferred lower limit of the total content of the alicyclic epoxy compound and the epoxy compound having a flexible framework is 70 parts by weight.
[0022] Examples of the above other curable resins include, for instance, other epoxy compounds other than the above-mentioned alicyclic epoxy compound and the above-mentioned epoxy compound having a flexible backbone, oxetane compounds, (meth)acrylic compounds, urethane compounds, etc.
[0023] Additionally, in this specification, "(meth)acryl" means acrylic or methacryl, "(meth)acryl compound" means a compound having a (meth)acryloyl group, and "(meth)acryloyl" means acryloyl or methacryloyl.
[0024] Examples of the above other epoxy compounds include, for instance, bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, diethylene glycol diglycidyl ether, polyethylene glycol glycidyl ether, polytetramethylene glycol glycidyl ether, 2-(2-butyl)phenylglycidyl ether, neopentyl glycol diglycidyl ether, O-phenylphenol glycidyl ether, 1,7-octadiene diepoxide, hydrogenated bisphenol A type epoxy resin, hydrogenated bisphenol F type epoxy resin, dicyclopentadiene type epoxy compounds, phenol novolak type epoxy compounds, cresol novolak type epoxy compounds, etc.
[0025] Examples of the above oxetane compounds include 1,4-bis{[(3-ethyl-3-oxetanyl)methoxy]methyl}benzene, di[2-(3-oxetanyl)butyl]ether, 3-ethyl-3-hydroxymethyloxetane, etc.
[0026] Examples of the above (meth)acrylate compounds include, for instance, resorcinol-type epoxy(meth)acrylate, isobornyl(meth)acrylate, adamantyl(meth)acrylate, methylcyclohexyl(meth)acrylate, norbornylmethyl(meth)acrylate, dicyclofentanyl(meth)acrylate, dicyclopentenyl(meth)acrylate, dicyclopentenyloxyethyl(meth)acrylate, cyclodecyl(meth)acrylate, 4-t-butylcyclohexyl(meth)acrylate, trimethylcyclohexyl(meth)acrylate, tricyclodecanedimethylethanoldi(meth)acrylate, 2-hydroxybutyl(meth)acrylate, etc.
[0027] In addition, in this specification, the term "(meth)acrylate" means acrylate or methacrylate, and the term "epoxy(meth)acrylate" means a compound in which all epoxy groups in an epoxy compound are reacted with (meth)acrylic acid.
[0028] Examples of the above urethane compounds include, for instance, a reaction product of an isocyanate compound and any polyol compound.
[0029] Examples of the above isocyanate compounds include toluene diisocyanate compounds, diphenylmethane diisocyanate compounds, etc.
[0030] Examples of the above toluene diisocyanate compounds include 2,4-tolylene diisocyanate (2,4-TDI), 2,6-tolylene diisocyanate, or mixtures thereof.
[0031] Examples of the above diphenylmethane diisocyanate compounds include 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, or mixtures thereof.
[0032] The encapsulating agent for an organic EL display device according to the present invention contains a photocatalytic polymerization initiator and a thermal cationic polymerization initiator.
[0033] By using the above photocatalytic polymerization initiator and the above thermal catalytic polymerization initiator in combination, the encapsulant for organic EL display elements of the present invention can be sufficiently cured even when placed in a light-shielding portion.
[0034] The above photocatalytic polymerization initiator is not particularly limited as long as it generates a proton acid or a Lewis acid upon light irradiation, and may be an ionic photogenerative type or a non-ionic photogenerative type.
[0035] The anionic portion of the above-mentioned ionic photogenic photocatalytic polymerization initiator is, for example, BF4 - , PF6 -, SbF6 - , or, (BX4) - (wherein X represents a phenyl group substituted with at least two fluorine or trifluoromethyl groups) etc.
[0036] Examples of the above-mentioned ionic photogenic photocatalytic polymerization initiators include aromatic sulfonium salts, aromatic iodonium salts, aromatic diazonium salts, aromatic ammonium salts, (2,4-cyclopentadiene-1-yl)((1-methylethyl)benzene)-Fe salts, etc., which have the above-mentioned anionic portion.
[0037] The above aromatic sulfonium salts include, for example, bis(4-(diphenylsulfonio)phenyl)sulfide bishexafluorophosphate, bis(4-(diphenylsulfonio)phenyl)sulfide bishexafluoroantimonate, bis(4-(diphenylsulfonio)phenyl)sulfide bistetrafluoroborate, bis(4-(diphenylsulfonio)phenyl)sulfide tetrakis(pentafluorophenyl)borate, diphenyl-4-(phenylthio)phenylsulfonium hexafluorophosphate, diphenyl-4-(phenylthio)phenylsulfonium hexafluoroantimonate, diphenyl-4-(phenylthio)phenylsulfonium tetrafluoroborate, diphenyl-4-(phenylthio)phenylsulfonium tetrakis(pentafluorophenyl)borate, triphenylsulfonium hexafluorophosphate, triphenylsulfonium hexafluoroantimonate, triphenylsulfonium tetrafluoroborate, Examples include triphenylsulfonium tetrakis(pentafluorophenyl)borate, triarylsulfonium tetrakis(pentafluorophenyl)borate, bis(4-(di(4-(2-hydroxyethoxy))phenylsulfonio)phenyl)sulfide bishexafluorophosphate, bis(4-(di(4-(2-hydroxyethoxy))phenylsulfonio)phenyl)sulfide bishexafluoroantimonate, bis(4-(di(4-(2-hydroxyethoxy))phenylsulfonio)phenyl)sulfide bistetrafluoroborate, bis(4-(di(4-(2-hydroxyethoxy))phenylsulfonio)phenyl)sulfide tetrakis(pentafluorophenyl)borate, tris(4-(4-acetylphenyl)thiophenyl)sulfonium tetrakis(pentafluorophenyl)borate, etc.
[0038] The above aromatic iodine salts include, for example, diphenyliodonium hexafluorophosphate, diphenyliodonium hexafluoroantimonate, diphenyliodonium tetrafluoroborate, diphenyliodonium tetrakis(pentafluorophenyl)borate, bis(dodecylphenyl)iodonium hexafluorophosphate, bis(dodecylphenyl)iodonium hexafluoroantimonate, bis(dodecylphenyl)iodonium tetrafluoroborate, bis(dodecylphenyl)iodonium tetrakis(pentafluorophenyl)borate, 4-methylphenyl-4-(1-methylethyl)phenyliodonium hexafluorophosphate, 4-methylphenyl-4-(1-methylethyl)phenyliodonium hexafluoroantimonate, 4-methylphenyl-4-(1-methylethyl)phenyliodonium tetrafluoroborate, Examples include 4-methylphenyl-4-(1-methylethyl)phenyliodonium tetrakis(pentafluorophenyl)borate.
[0039] Examples of the above aromatic diazonium salts include phenyldiazonium hexafluorophosphate, phenyldiazonium hexafluoroantimonate, phenyldiazonium tetrafluoroborate, phenyldiazonium tetrakis(pentafluorophenyl)borate, etc.
[0040] Examples of the above aromatic ammonium salts include, for instance, 1-benzyl-2-cyanopyridinium hexafluorophosphate, 1-benzyl-2-cyanopyridinium hexafluoroantimonate, 1-benzyl-2-cyanopyridinium tetrafluoroborate, 1-benzyl-2-cyanopyridinium tetrakis(pentafluorophenyl)borate, 1-(naphthylmethyl)-2-cyanopyridinium hexafluorophosphate, 1-(naphthylmethyl)-2-cyanopyridinium hexafluoroantimonate, 1-(naphthylmethyl)-2-cyanopyridinium tetrafluoroborate, and 1-(naphthylmethyl)-2-cyanopyridinium tetrakis(pentafluorophenyl)borate.
[0041] Examples of the above (2,4-cyclopentadiene-1-yl)((1-methylethyl)benzene)-Fe salts include, for instance, (2,4-cyclopentadiene-1-yl)((1-methylethyl)benzene)-Fe(II)hexafluorophosphate, (2,4-cyclopentadiene-1-yl)((1-methylethyl)benzene)-Fe(II)hexafluoroantimonate, (2,4-cyclopentadiene-1-yl)((1-methylethyl)benzene)-Fe(II)tetrafluoroborate, (2,4-cyclopentadiene-1-yl)((1-methylethyl)benzene)-Fe(II)tetrakis(pentafluorophenyl)borate, etc.
[0042] Examples of the above nonionic photogenic photocatalytic polymerization initiators include nitrobenzyl esters, sulfonic acid derivatives, phosphate esters, phenolsulfonic acid esters, diazonaphthoquinone, N-hydroxyimidesulfonate, etc.
[0043] Among them, in terms of the strength of the acid generated, a salt in which the counter anion is tetrakis(pentafluorophenyl)borate is preferred as the photocatalytic polymerization initiator.
[0044] Among the above photocatalytic polymerization initiators that are commercially available, examples include the photocatalytic polymerization initiator manufactured by Midori Chemical Co., Ltd., the photocatalytic polymerization initiator manufactured by Union Carbide Co., Ltd., the photocatalytic polymerization initiator manufactured by ADEKA Co., Ltd., the photocatalytic polymerization initiator manufactured by 3M Co., Ltd., the photocatalytic polymerization initiator manufactured by BASF Co., Ltd., and the photocatalytic polymerization initiator manufactured by Rhodia Co., Ltd.
[0045] Examples of photocatalytic polymerization initiators manufactured by Midori Chemical Co., Ltd. include, for instance, DTS-200.
[0046] Examples of photocatalytic polymerization initiators manufactured by Union Carbide Co., Ltd. include UVI6990, UVI6974, etc.
[0047] Examples of the photocatalytic polymerization initiators manufactured by ADEKA, such as SP-150 and SP-170, are available.
[0048] Examples of the photocatalytic polymerization initiators manufactured by 3M include FC-508, FC-512, etc.
[0049] Examples of the photocatalytic polymerization initiators manufactured by BASF include IRGACURE261, IRGACURE290, etc.
[0050] Examples of photocatalytic polymerization initiators manufactured by Rhodia Co., Ltd. include PI2074, etc.
[0051] The content of the above photocatalytic polymerization initiator is preferably 0.1 parts by weight and 2.5 parts by weight per 100 parts by weight of the above curable resin (in cases containing the polyolefin described below, the sum of the above curable resin and the polyolefin described below). By having a content of 0.1 parts by weight or more of the above photocatalytic polymerization initiator, the encapsulant for organic EL display devices obtained has superior photocurability. By having a content of 2.5 parts by weight or less of the above photocatalytic polymerization initiator, the curing reaction of the encapsulant for organic EL display devices obtained is not excessively fast, thereby allowing for stable adhesion. A more preferred lower limit of the content of the above photocatalytic polymerization initiator is 0.5 parts by weight, and a more preferred upper limit is 1.5 parts by weight.
[0052] As for the above thermal cationic polymerization initiator, the anionic portion is BF4 - , PF6 - , SbF6 - , or, (BX4) - Examples include sulfonium salts, phosphonium salts, ammonium salts, etc., composed of (wherein X represents a phenyl group substituted with at least two fluorine or trifluoromethyl groups). Among these, sulfonium salts and ammonium salts are preferred.
[0053] Examples of the above sulfonium salts include benzyl(4-hydroxyphenyl)methylsulfonium tris(pentafluoroethyl)trifluorophosphate, triphenylsulfonium tetrafluoroborate, and triphenylsulfonium hexafluoroantimonate.
[0054] Examples of the above phosphonium salts include ethyltriphenylphosphonium hexafluoroantimonate and tetrabutylphosphonium hexafluoroantimonate.
[0055] The above ammonium salts include, for example, dimethylphenyl(4-methoxybenzyl)ammonium hexafluorophosphate, dimethylphenyl(4-methoxybenzyl)ammonium hexafluoroantimonate, dimethylphenyl(4-methoxybenzyl)ammonium tetrakis(pentafluorophenyl)borate, dimethylphenyl(4-methylbenzyl)ammonium hexafluorophosphate, dimethylphenyl(4-methylbenzyl)ammonium hexafluoroantimonate, dimethylphenyl(4-methylbenzyl)ammonium hexafluoroantimonate, methylphenyldibenzylammonium hexafluorophosphate, methylphenyldibenzylammonium hexafluoroantimonate, methylphenyldibenzylammonium tetrakis(pentafluorophenyl)borate, phenyltribenzylammonium tetrakis(pentafluorophenyl)borate, Examples include dimethylphenyl(3,4-dimethylbenzyl)ammonium tetrakis(pentafluorophenyl)borate, N,N-dimethyl-N-benzylanilinium hexafluoroantimonate, N,N-diethyl-N-benzylanilinium tetrafluoroborate, N,N-dimethyl-N-benzylpyridinium hexafluoroantimonate, and N,N-diethyl-N-benzylpyridinium trifluoromethanesulfonic acid.
[0056] Among them, in terms of the strength of the acid generated, a salt in which the counter anion is tetrakis(pentafluorophenyl)borate is preferred as the thermal cationic polymerization initiator.
[0057] Among the above-mentioned thermal cation polymerization initiators that are commercially available, examples include the thermal cation polymerization initiator manufactured by Sanshin Chemical Industry Co., Ltd., the thermal cation polymerization initiator manufactured by King Industries Co., Ltd., and the thermal cation polymerization initiator manufactured by San Apro Co., Ltd.
[0058] Examples of the thermal cation polymerization initiators manufactured by Sanshin Chemical Industry Co., Ltd. include San-Aid SI-60, San-Aid SI-80, San-Aid SI-B3, San-Aid SI-B3A, San-Aid SI-B4, etc.
[0059] Examples of the thermal cation polymerization initiators manufactured by King Industries, etc. include CXC-1612, CXC-1821, etc.
[0060] Examples of the thermal cationic polymerization initiators for the above San Aprosa production include TA-100, TA-100FG, etc.
[0061] The content of the above-mentioned thermal cation polymerization initiator is preferably 0.5 parts by weight and 3.0 parts by weight per 100 parts by weight of the above-mentioned curable resin (in cases containing the polyolefin described later, the sum of the above-mentioned curable resin and the polyolefin described later). By having a content of 0.5 parts by weight or more of the above-mentioned thermal cation polymerization initiator, the encapsulant for organic EL display devices obtained has superior thermal curing properties. By having a content of 3.0 parts by weight or less of the above-mentioned thermal cation polymerization initiator, the curing reaction of the encapsulant for organic EL display devices obtained is not excessively fast, resulting in superior workability and making the cured product more uniform. A more preferred lower limit for the content of the above-mentioned thermal cation polymerization initiator is 1.0 parts by weight and a more preferred upper limit is 2.0 parts by weight.
[0062] The encapsulating agent for the organic EL display device of the present invention may contain a radical polymerization initiator.
[0063] Examples of the above radical polymerization initiators include photo-radical polymerization initiators or thermal-radical polymerization initiators.
[0064] Examples of the above-mentioned photoradical polymerization initiators include benzophenone compounds, acetophenone compounds, acylphosphine oxide compounds, titanocene compounds, oxime ester compounds, benzoin ether compounds, thioxanthone compounds, etc.
[0065] The above photoradical polymerization initiator is, specifically, for example, 1-hydroxycyclohexylphenylketone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone, 1,2-(dimethylamino)-2-((4-methylphenyl)methyl)-1-(4-(4-morpholinyl)phenyl)-1-butanone, 2,2-dimethoxy-2-phenylacetophenone, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 1-(4-(2-hydroxyethoxy)-phenyl)-2-hydroxy-2-methyl-1-propan-1-one, 1-(4-(phenylthio)phenyl)-1,2-octanedione 2-(O-benzoyloxime), Examples include 2,4,6-trimethylbenzoyldiphenylphosphine oxide, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, etc.
[0066] Examples of the above thermal radical polymerization initiators include azo compounds, organic peroxides, etc.
[0067] Examples of the above azo compounds include 2,2'-azobis(2,4-dimethylvaleronitrile), azobisisobutyronitrile, etc.
[0068] Examples of the above organic peroxides include, for instance, benzoyl peroxide, ketone peroxide, peroxyketal, hydroperoxide, dialkyl peroxide, peroxyester, diacyl peroxide, peroxydicarbonate, etc.
[0069] Among the above-mentioned thermal radical polymerization initiators that are commercially available, examples include VPE-0201, VPE-0401, VPE-0601, VPS-0501, VPS-1001, V-501 (all manufactured by Fujifilm Wako Junpaku Co., Ltd.).
[0070] The content of the radical polymerization initiator is preferably 0.05 parts by weight and 5 parts by weight per 100 parts by weight of the curable resin (in cases containing the polyolefin described below, the sum of the curable resin and the polyolefin described below). By having a content of 0.05 parts by weight or more of the radical polymerization initiator, the encapsulant for an organic EL display device obtained has superior curability. By having a content of 5 parts by weight or less of the radical polymerization initiator, the curing reaction of the encapsulant for an organic EL display device obtained is not excessively fast, resulting in superior workability and making the cured product more uniform. A more preferred lower limit for the content of the radical polymerization initiator is 0.5 parts by weight and a more preferred upper limit is 2 parts by weight.
[0071] The encapsulant for an organic EL display device of the present invention may contain a sensitizer. The sensitizer has the role of further improving the polymerization initiation efficiency of the polymerization initiator and further promoting the curing reaction of the encapsulant for an organic EL display device of the present invention.
[0072] Examples of the above-mentioned sensitizers include anthracene compounds, thioxanthone compounds, 2,2-dimethoxy-1,2-diphenylethane-1-one, benzophenone, 2,4-dichlorobenzophenone, o-methyl benzoylbenzoate, 4,4'-bis(dimethylamino)benzophenone, 4-benzoyl-4'-methyldiphenylsulfide, etc.
[0073] Examples of the above anthracene compounds include 9,10-dibutoxycyanthracene.
[0074] Examples of the above thioxanthon-based compounds include 2,4-diethylthioxanthon.
[0075] These sensitizers may be used alone or in combination of two or more types.
[0076] The content of the sensitizer is preferably 0.05 parts by weight and 3 parts by weight per 100 parts by weight of the curable resin (in cases containing the polyolefin described below, the sum of the curable resin and the polyolefin described below). The sensitizing effect is further exhibited when the content of the sensitizer is 0.05 parts by weight or more. When the content of the sensitizer is 3 parts by weight or less, absorption does not become excessively large, allowing light to be transmitted to the deep tissue. A more preferred lower limit for the content of the sensitizer is 0.1 parts by weight and a more preferred upper limit is 1 part by weight.
[0077] The encapsulant for the organic EL display element of the present invention may contain a thermal curing agent.
[0078] Examples of the above-mentioned heat-curing agents include hydrazide compounds, imidazole derivatives, acid anhydrides, dicyandiamides, guanidine derivatives, modified aliphatic polyamines, various amines, and addition products of epoxy resins.
[0079] Examples of the above hydrazide compounds include 1,3-bis(hydrazinocarboethyl)-5-isopropylhydantoin, sebacic acid dihydrazide, isophthalic acid dihydrazide, adipic acid dihydrazide, malonic acid dihydrazide, etc.
[0080] Examples of the above imidazole derivatives include 1-cyanoethyl-2-phenylimidazole, N-(2-(2-methyl-1-imidazolyl)ethyl)urea, 2,4-diamino-6-(2'-methylimidazolyl-(1'))-ethyl-s-triazine, N,N'-bis(2-methyl-1-imidazolylethyl)urea, N,N'-(2-methyl-1-imidazolylethyl)-adipamide, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, etc.
[0081] Examples of the above acid anhydrides include tetrahydrophthalic anhydride, ethylene glycolbis(anhydrotrimellitate), etc.
[0082] These thermosetting agents may be used alone or in combination of two or more types.
[0083] Among the above-mentioned heat-curing agents that are commercially available, examples include SDH (manufactured by Nippon Finechem Co.), ADH (manufactured by Otsuka Chemical Co.), Amicure VDH, Amicure VDH-J, and Amicure UDH (all manufactured by Ajinomoto Fine Techno Co.).
[0084] The content of the above-mentioned thermal curing agent is preferably 0.01 parts by weight and preferably 10 parts by weight per 100 parts by weight of the above-mentioned curable resin (in cases containing the polyolefin described later, the sum of the above-mentioned curable resin and the polyolefin described later). By having a content of 0.01 parts by weight or more of the above-mentioned thermal curing agent, the encapsulant for an organic EL display device obtained has superior thermal curing properties. By having a content of 10 parts by weight or less of the above-mentioned thermal curing agent, the encapsulant for an organic EL display device obtained has superior storage stability. A more preferred lower limit of the content of the above-mentioned thermal curing agent is 0.5 parts by weight, a more preferred upper limit is 5 parts by weight, an even more preferred lower limit is 1 part by weight, and an even more preferred upper limit is 3 parts by weight.
[0085] The encapsulating agent for an organic EL display device according to the present invention contains a filler.
[0086] As the above filler, inorganic fillers or organic fillers may be used.
[0087] Examples of the above-mentioned inorganic fillers include silica, talc, alumina, etc.
[0088] Examples of the above organic fillers include polyester microparticles, polyurethane microparticles, vinyl polymer microparticles, acrylic polymer microparticles, etc.
[0089] Among them, talc is preferred as the above-mentioned filler.
[0090] In addition, the encapsulant for an organic EL display device of the present invention may contain an absorbent filler as the filler. By containing the absorbent filler, the encapsulant for an organic EL display device of the present invention has excellent moisture-proof properties.
[0091] Examples of the above-mentioned absorbent fillers include oxides of alkaline earth metals, magnesium oxide, molecular sieves, etc.
[0092] Examples of oxides of the above alkaline earth metals include calcium oxide, strontium oxide, barium oxide, etc.
[0093] Among them, in terms of absorbency, oxides of alkaline earth metals are preferred, and calcium oxide is more preferred.
[0094] These absorbable fillers may be used alone or in combination of two or more types.
[0095] The above filler has a preferred lower limit of average particle size of 0.5 μm and a preferred upper limit of 10 μm. Since the average particle size of the above filler is within this range, the encapsulant for organic EL display devices obtained has superior coatability, adhesion, and moisture barrier properties. A more preferred lower limit of the average particle size of the above filler is 1.0 μm and a more preferred upper limit is 5.0 μm.
[0096] In addition, the average particle size of the above filler can be measured by dispersing the filler in a solvent (water, organic solvent, etc.) using a particle size distribution measuring device such as NICOMP 380ZLS (manufactured by PARTICLE SIZING SYSTEMS).
[0097] The content of the above filler is preferably 10 parts by weight and preferably 50 parts by weight per 100 parts by weight of the above curable resin (in cases containing the polyolefin described below, the sum of the above curable resin and the polyolefin described below). By having the content of the above filler within this range, the encapsulant for organic EL display elements obtained has superior coatability, adhesion, and moisture permeability. A more preferred lower limit for the content of the above filler is 20 parts by weight and a more preferred upper limit is 30 parts by weight.
[0098] The encapsulant for the organic EL display element of the present invention preferably contains a polyolefin.
[0099] By containing the above polyolefin, the encapsulant for organic EL display elements of the present invention has superior moisture-proof properties.
[0100] As for the above polyolefin, it is preferable to include at least one selected from the group consisting of polyisobutylene, polybutene, and polybutadiene in order to further improve moisture permeability, and it is more preferable to include polyisobutylene.
[0101] The above polyolefin may be used alone or in combination of two or more types.
[0102] The preferred lower limit of the weight-average molecular weight of the above polyolefin is 10,000, and the preferred upper limit is 400,000. Since the weight-average molecular weight of the above polyolefin is within this range, the encapsulant for organic EL display devices obtained has superior coatability, adhesion, and moisture-permeability. A more preferred lower limit of the weight-average molecular weight of the above polyolefin is 20,000, and a more preferred upper limit is 70,000.
[0103] In addition, the "weight average molecular weight" in this specification is a value obtained by measuring using tetrahydrofuran as a solvent in gel permeation chromatography (GPC) and converting to polystyrene. Examples of columns used when measuring the weight average molecular weight by converting to polystyrene in GPC include Shodex LF-804 (manufactured by Showa Denko).
[0104] In the total of 100 parts by weight of the curable resin and the polyolefin, the preferred lower limit of the polyolefin content is 10 parts by weight, and the preferred upper limit is 80 parts by weight. When the polyolefin content is 10 parts by weight or more, the encapsulant for organic EL display devices obtained has superior moisture-permeability. When the polyolefin content is 80 parts by weight or less, the encapsulant for organic EL display devices obtained has superior coatability or adhesion. A more preferred lower limit of the polyolefin content is 20 parts by weight, and a more preferred upper limit is 60 parts by weight.
[0105] The encapsulant for organic EL display devices of the present invention may contain a tackifying resin for the purpose of further improving adhesion.
[0106] Examples of the above adhesive resins include terpene resin, modified terpene resin, coumarone resin, indene resin, petroleum resin, etc.
[0107] Examples of the above modified terpene resins include hydrogenated terpene resins, terpenephenol copolymer resins, aromatic modified terpene resins, etc.
[0108] Examples of the above petroleum resins include, for instance, aliphatic petroleum resins, hydrogenated alicyclic petroleum resins, aromatic petroleum resins, aliphatic aromatic copolymer petroleum resins, alicyclic petroleum resins, dicyclopentadiene-based petroleum resins, and their hydrides.
[0109] Among these, regarding the adhesive properties, moisture resistance, and compatibility of encapsulant for organic EL display elements, terpene resin, aromatic modified terpene resin, terpenephenol copolymer resin, hydrogenated alicyclic petroleum resin, aromatic petroleum resin, aliphatic aromatic copolymer petroleum resin, and alicyclic petroleum resin are preferred, alicyclic petroleum resin is more preferred, alicyclic saturated hydrocarbon resin and alicyclic unsaturated hydrocarbon resin are even more preferred, and cyclohexyl ring-containing saturated hydrocarbon resin and dicyclopentadiene-modified hydrocarbon resin are particularly preferred.
[0110] These tackifying resins may be used alone or in combination of two or more types.
[0111] The content of the tackifying resin is preferably 0.01 parts by weight and preferably 100 parts by weight per 100 parts by weight of the curable resin (in the case where the polyolefin is included, the sum of the curable resin and the polyolefin). By having the content of the tackifying resin within this range, the effect of improving adhesion while maintaining moisture barrier properties can be further exhibited. A more preferred lower limit for the content of the tackifying resin is 0.2 parts by weight and a more preferred upper limit is 20 parts by weight.
[0112] The encapsulant for an organic EL display device of the present invention may contain a stabilizer. By containing the stabilizer, the encapsulant for an organic EL display device of the present invention has superior storage stability.
[0113] Examples of the above stabilizers include aromatic amine compounds, 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxyl, etc.
[0114] Examples of the above aromatic amine compounds include benzylamine, aminophenol-type epoxy resin, etc.
[0115] Among them, aromatic amine compounds are preferred, and benzylamine is more preferred.
[0116] These stabilizers may be used alone or in combination of two or more types.
[0117] The content of the above stabilizer is preferably 0.001 parts by weight and preferably 2 parts by weight per 100 parts by weight of the above curable resin (in the case where the above polyolefin is included, the sum of the above curable resin and the above polyolefin). By having the content of the above stabilizer within this range, the encapsulant for organic EL display devices obtained has better storage stability while maintaining excellent curability. A more preferred lower limit for the content of the above stabilizer is 0.005 parts by weight and a more preferred upper limit is 1 part by weight.
[0118] The encapsulant for an organic EL display device of the present invention may contain a silane coupling agent. The silane coupling agent has the role of improving the adhesion between the encapsulant for an organic EL display device of the present invention and a substrate, etc.
[0119] Examples of the above silane coupling agents include 3-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-isocyanatepropyltrimethoxysilane, etc.
[0120] These silane coupling agents may be used alone or in combination of two or more types.
[0121] The content of the above silane coupling agent is preferably 0.1 parts by weight and preferably 10 parts by weight per 100 parts by weight of the above curable resin (in the case where the above polyolefin is contained, the sum of the above curable resin and the above polyolefin). By having the content of the above silane coupling agent within this range, the effect of improving the adhesion of the encapsulant for organic EL display devices obtained while preventing bleed-out of excess silane coupling agent becomes superior. A more preferred lower limit for the content of the above silane coupling agent is 0.5 parts by weight and a more preferred upper limit is 5 parts by weight.
[0122] The encapsulant for an organic EL display device of the present invention may contain a surface modifier to the extent that it does not impede the purpose of the present invention. By containing the surface modifier, the flatness of the coating film of the encapsulant for an organic EL display device of the present invention can be improved.
[0123] Examples of the above surface modifiers include surfactants or leveling agents.
[0124] Examples of the above surface modifiers include silicone-based, acrylic-based, and fluorine-based materials.
[0125] Among the above-mentioned surface modifiers that are commercially available, examples include the surface modifier manufactured by Big Chem Japan, the surface modifier manufactured by Kusumoto Kasei, and the surface modifier manufactured by AGC Seimi Chemical.
[0126] Examples of surface modifiers manufactured by Big Chemie Japan include BYK-300, BYK-302, BYK-331, etc.
[0127] Examples of surface modifiers manufactured by Kusumoto Chemical Co., Ltd. include UVX-272, etc.
[0128] Examples of surface modifiers manufactured by AGC Seimi Chemical Co., Ltd. include Surflon S-611.
[0129] The encapsulant for an organic EL display device of the present invention may contain a compound that reacts with an acid generated in the encapsulant for an organic EL display device and / or an ion exchange resin, to the extent that it does not impede the purpose of the present invention.
[0130] Compounds that react with the acid generated above may include substances that neutralize the acid, such as carbonates or bicarbonates of alkali metals, or carbonates or bicarbonates of alkaline earth metals. Specifically, examples used include calcium carbonate, calcium bicarbonate, sodium carbonate, and sodium bicarbonate.
[0131] As for the above ion exchange resin, any of the cation exchange type, anion exchange type, or both ion exchange type can be used, but a cation exchange type or both ion exchange type capable of adsorbing chloride ions is particularly preferred.
[0132] The encapsulating agent for an organic EL display device of the present invention may contain various known additives, such as curing retardants, reinforcing agents, softeners, plasticizers, viscosity modifiers, ultraviolet absorbers, and antioxidants, as needed, within a range that does not impede the purpose of the present invention.
[0133] The encapsulant for an organic EL display device of the present invention preferably does not contain a solvent in order to further suppress the generation of outgas. The encapsulant for an organic EL display device of the present invention can be made to have excellent coating properties even without containing a solvent.
[0134] In addition, in this specification, "does not contain solvent" means that the solvent content is less than 1000 ppm.
[0135] A method for manufacturing an encapsulant for an organic EL display device according to the present invention may include, for example, a method of mixing a curable resin, a photocatalytic polymerization initiator, a thermal cationic polymerization initiator, a filler, and an additive such as a silane coupling agent added as needed using a mixer.
[0136] Examples of the above-mentioned mixers include, for instance, a homodisperser, a homomixer, a universal mixer, a planetary mixer, a kneader, a three-roll kneader, etc.
[0137] The cured product of the encapsulation agent for an organic EL display device according to the present invention is preferably used as an encapsulation wall surrounding the periphery of an organic EL display device. That is, the encapsulation agent for an organic EL display device according to the present invention is preferably used as a peripheral encapsulation agent for an organic EL display device to form an encapsulation wall around a laminate having an organic light-emitting material layer. The peripheral encapsulation agent for an organic EL display device is typically used in combination with an in-plane encapsulation agent for an organic EL display device that covers the laminate.
[0138] The encapsulation wall formed using the cured product of the encapsulation agent for the organic EL display element of the present invention preferably has a thickness of 5 mm or less, from the perspective of securing a wide display area of the organic EL display element obtained. Effects of the invention
[0139] According to the present invention, it is possible to provide an encapsulant for an organic EL display element that has excellent adhesion and can be sufficiently cured even when placed in a light-shielding area. Specific details for implementing the invention
[0140] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples.
[0141] (Examples 1 to 11, Comparative Examples 1 to 3)
[0142] Encapsulating agents for organic EL display devices of Examples 1 to 9 and Comparative Examples 1 to 3 were prepared by mixing each material according to the mixing ratios listed in Tables 1 and 2 using a stirring mixer at a stirring speed of 2000 rpm for 3 minutes. The AR-310 (manufactured by Sinkie) was used as the stirring mixer.
[0143] <Evaluation>
[0144] For each encapsulator for organic EL display devices obtained in the examples and comparative examples, the following evaluation was performed. The results are shown in Tables 1 and 2.
[0145] (viscosity)
[0146] For each encapsulating agent for organic EL display devices obtained in the examples and comparative examples, an E-type viscometer was used to measure the initial viscosity immediately after preparation at 25°C.
[0147] For the above E-type viscometer, the VISCOMETER TV-22 (manufactured by Toki Sangyo Co., Ltd.) was used.
[0148] (Adhesion)
[0149] For every 10 g of encapsulant for organic EL display devices obtained in the examples and comparative examples, 0.03 g of spacer particles with a diameter of 10 μm was added and uniformly dispersed using a stirring mixer. Micropearl SP-210 (manufactured by Sekisui Chemical Industry Co., Ltd.) was used as the spacer particles, and ARV-310 (manufactured by Shinki Co., Ltd.) was used as the stirring mixer. After applying the encapsulant for organic EL display devices with dispersed spacer particles to the center of glass substrate A, glass substrate B was attached by crossing it in a cross shape, and the thickness was made uniform by applying pressure. The amount of the encapsulant for organic EL display devices applied was adjusted so that the encapsulant for organic EL display devices, after the thickness was made uniform by applying pressure, became a circle with a diameter of 5.0 to 7.0 mm. The above glass substrates A and B were obtained by cleaning the surface of glass with a length of 60 mm, a width of 30 mm, and a thickness of 5 mm with acetone and then drying it. Subsequently, the encapsulant for organic EL display devices was cured by irradiating ultraviolet rays with a wavelength of 365 nm at a rate of 3000 mJ / ㎠ using a UV-LED irradiation device and heating at 100 ℃ for 30 minutes, and glass substrate A and glass substrate B were bonded to obtain a test specimen for evaluating adhesion.
[0150] For the obtained test specimen, glass substrate B was positioned so that it was facing downward, and both ends of glass substrate A were fixed from below. The adhesion strength between glass substrate A and glass substrate B was measured by compressing both ends of glass substrate B from above using a precision universal testing machine at 23°C and a speed of 5 mm / min. The compression point was set to a range of 20 mm in length and 5 mm in width, centered at a position 7.25 mm from both ends of glass substrate B. An Autograph AG-Xplus (manufactured by Shimadzu Corporation) was used as the precision universal testing machine.
[0151] (Curing rate)
[0152] For each encapsulant for organic EL display devices obtained in the examples and comparative examples, the encapsulant for organic EL display devices was cured by heat alone by heating at 100°C for 30 minutes.
[0153] FT-IR analysis was performed on the encapsulant for organic EL display devices before curing and the cured product using a Fourier transform infrared spectrophotometer. 915 cm⁻¹ -1 The reduction rate of the peak after curing (reaction rate of the epoxy group) was calculated as the curing rate. An iS-5 (manufactured by Nicole) was used as the Fourier transform infrared spectrophotometer.
[0154] (Curing distance of the light-blocking section)
[0155] Each encapsulating agent for organic EL display devices obtained in the examples and comparative examples was applied to the center of the release surface of a release PET film, the release surface of the release PET film was attached from above, and a glass substrate was placed between the top and bottom, and then pressure was applied to make the thickness uniform. As the release PET film, PET50×1-C (manufactured by NIPPA, thickness 50 μm) was used. After applying pressure, the glass substrate was removed, and a black vinyl tape was attached to one side of the non-release surface of the release PET film with each encapsulating agent for organic EL display devices in between. A metal plate (made of SUS304) having a hole with a thickness of 1.0 mm and a diameter of 1.0 mm formed on one side of the non-release surface of a release PET film opposite to the side with black vinyl tape attached was placed so that the position of the hole was on top of the encapsulant for an organic EL display element, and ultraviolet light with a wavelength of 365 nm was irradiated vertically at a rate of 3000 mJ / cm² from above the metal plate using a UV-LED irradiation device. A surface irradiation type UV-LED irradiation device was used.
[0156] Test specimens were obtained by leaving the specimens for 5 minutes after UV irradiation, removing the metal plate and the release PET film on the UV irradiation side, and washing off the uncured portions of the encapsulant for each organic EL display element with ethanol.
[0157] For the obtained test specimen, the diameter of each encapsulant for organic EL display elements that remained as a circle on the release PET film without being washed off was measured, and the value obtained by subtracting 1.0 mm from the measured value and multiplying it by half was taken as the curing distance of the light-blocking part.
[0158]
[0159]
[0160] Industrial applicability
[0161] According to the present invention, it is possible to provide an encapsulant for an organic EL display element that has excellent adhesion and can be sufficiently cured even when placed in a light-shielding area.
Claims
Claim 1 An encapsulator for an organic EL display device comprising a curable resin, a photocatalytic polymerization initiator, a thermal cationic polymerization initiator, and a filler, wherein the curable resin comprises an alicyclic epoxy compound and an epoxy compound having a flexible backbone, wherein the epoxy compound having a flexible backbone is an epoxy compound having at least one structure selected from the group consisting of a ring-opening structure of a lactone, a polyalkylene oxide structure, a rubber structure derived from a conjugated diene, and a polysiloxane structure, wherein the content ratio of the alicyclic epoxy compound and the epoxy compound having a flexible backbone (alicyclic epoxy compound : epoxy compound having a flexible backbone) is 1:1 to 1:2 by weight, and the total content of the alicyclic epoxy compound and the epoxy compound having a flexible backbone in 100 parts by weight of the curable resin is 60 parts by weight or more. Claim 2 In claim 1, the epoxy compound having the flexible framework is an encapsulator for an organic EL display device, which is an epoxy compound having a polyalkylene oxide structure. Claim 3 In claim 2, the epoxy compound having the flexible framework is an encapsulant for an organic EL display device, which is a compound represented by the following formula (1). In formula (1), X represents an ethyleneoxyethyl group, a di(ethyleneoxy)ethyl group, a tri(ethyleneoxy)ethyl group, a tetra(ethyleneoxy)ethyl group, a propyleneoxypropyl group, a di(propyleneoxy)propyl group, a tri(propyleneoxy)propyl group, a tetra(propyleneoxy)propyl group, a butyleneoxybutyl group, a di(butyleneoxy)butyl group, a tri(butyleneoxy)butyl group, a tetra(butyleneoxy)butyl group, or an alkylene group having 2 or more carbon atoms and 15 or fewer carbon atoms, and n is 1 to 10. Claim 4 In claim 1, 2, or 3, the photocation polymerization initiator is an encapsulating agent for an organic EL display device, wherein tetrakis(pentafluorophenyl)borate is a salt with tetrakis(pentafluorophenyl)borate as the counter anone. Claim 5 In claim 1, 2, or 3, the thermal cationic polymerization initiator is a salt having tetrakis(pentafluorophenyl)borate as the counter anone, an encapsulating agent for an organic EL display device. Claim 6 delete