Cathode active material for lithium secondary battery and lithium secondary battery comprising the same
A single-particle lithium metal oxide with a yttrium concentration gradient and nickel content addresses structural instability in NCM-based batteries, enhancing lifespan and energy density by stabilizing the battery structure.
Patent Information
- Application Number
- KR1020240085235
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-06-28
AI Technical Summary
Conventional NCM-based lithium composite transition metal oxides used in lithium secondary batteries have structural instability and low particle strength, leading to reduced lifespan and stability due to high specific surface area and lithium byproduct content, which is exacerbated in high-nickel compositions.
A single-particle lithium metal oxide positive electrode active material with a concentration gradient of yttrium (Y) higher at the surface than the center, combined with a nickel content of 80 mol% and a coating layer, enhances structural stability and improves high-temperature life characteristics.
The Y concentration gradient and nickel content improve structural stability, reducing gas generation and particle breakage, resulting in superior lifespan, safety, and energy density of the battery.
Smart Images

Figure 112024070341274-PAT00001_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a positive electrode active material for a lithium secondary battery and a lithium secondary battery including the same, and more specifically, to a positive electrode active material for a lithium secondary battery in the form of a single particle and a lithium secondary battery including the same. Background Technology
[0003] In a lithium secondary battery, electrical energy is produced by oxidation and reduction reactions when lithium ions are inserted into or removed from the positive and negative electrodes, which are composed of active materials capable of lithium ion intercalation and deintercalation, with an organic or polymer electrolyte charged between them.
[0004] Lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2 or LiMn2O4, etc.), and lithium iron phosphate compounds (LiFePO4) have been used as cathode active materials for lithium-ion batteries. Among these, lithium cobalt oxide (LiCoO2) is widely used and applied as a cathode active material for high-voltage applications due to its advantages of high operating voltage and excellent capacity characteristics. However, due to the rising price and supply instability of cobalt (Co), there are limitations to its mass use as a power source in fields such as electric vehicles, leading to the emergence of a need for the development of cathode active materials that can replace it.
[0005] Accordingly, a nickel-cobalt-manganese-based lithium composite transition metal oxide (hereinafter simply referred to as 'NCM-based lithium composite transition metal oxide') was developed in which a portion of the cobalt (Co) was replaced with nickel (Ni) and manganese (Mn). However, the conventionally developed NCM-based lithium composite transition metal oxide generally has a secondary particle form in which primary particles are aggregated, and has a large specific surface area, low particle strength, and high lithium byproduct content, resulting in a large amount of gas generated during cell operation and consequently a decrease in lifespan and stability.
[0006] Accordingly, development of cathode active materials in the form of single particles, rather than the existing secondary particle form, is underway. The problem to be solved
[0008] One objective of the present invention is to provide a single-particle type positive electrode active material for a lithium secondary battery that can improve high-temperature life characteristics by improving structural stability, and a lithium secondary battery including the same. means of solving the problem
[0010] One embodiment of the present invention provides a positive electrode active material for a lithium secondary battery comprising a lithium metal oxide particle having a single particle form and containing nickel, wherein the lithium metal oxide particle comprises Y (yttrium), and the concentration gradient of Y is higher at the outermost surface of the lithium metal oxide particle than at the center of the lithium metal oxide particle.
[0011] The above positive active material can satisfy the following Equation 1.
[0012] [Equation 1]
[0013] 0 < DI Y-out - DI Y-cen ≤ 200 (au)
[0014] In Equation 1 above, DI Y-out Y is the X-ray count rate (CPS) intensity value of Y at the outermost surface of the particle during Energy-Dispersive Spectroscopy (EDS) line scan analysis of the lithium metal oxide particle, and DIY-cen is the X-ray count rate (CPS) intensity value of Y at the center of the particle during Energy-Dispersive Spectroscopy (EDS) line scan analysis of the lithium metal oxide particle.
[0015] The above positive active material can satisfy the following Equation 2.
[0016] [Equation 2]
[0017] 450 ≤ DI Y-out ≤ 600 (au)
[0018] In Equation 2 above, DI Y-out Y is the X-ray count rate (CPS) intensity value of Y at the outermost surface of the particle during Energy-Dispersive Spectroscopy (EDS) line scan analysis of lithium metal oxide particles.
[0019] The above positive active material can satisfy the following Equation 3.
[0020] [Equation 3]
[0021] 350 ≤ DI Y-cen ≤ 550 (au)
[0022] In Equation 3 above, DI Y-cen is the X-ray count rate (CPS) intensity value of Y at the center of the particle during Energy-Dispersive Spectroscopy (EDS) line scan analysis of lithium metal oxide particles.
[0023] The content of Y in the above lithium metal oxide particles may be 0.05 to 0.1 mol% based on the total molar amount of metal excluding lithium.
[0024] The above positive active material may have an average particle size (D50) of 3.0 to 4.0 μm.
[0025] The nickel content in the above lithium metal oxide particles may be 80 mol% or more based on the total molar amount of metal excluding lithium.
[0026] It may further include a coating layer containing Co located on the surface of the lithium metal oxide particles.
[0027] The content of Co in the above positive active material may be 0.3 to 4 mol% based on the total molar amount of lithium metal oxide.
[0028] The above lithium metal oxide may have an a-axis lattice constant of 2.8772 Å or more.
[0029] The above lithium metal oxide may have a c-axis lattice constant of 14.1965 Å or more.
[0030] The above lithium metal oxide may have a cation mixing ratio of 1.5% or less in the lithium layer.
[0031] The above lithium metal oxide particles can be represented by the following chemical formula 1.
[0032] [Chemical Formula 1]
[0033] Li a [Ni x Co y Mn z Y w1 M W2 ]O2
[0034] In the above chemical formula 1, 0.8≤a≤1.2, 0.8≤x<1, 0≤y≤0.2, 0≤z≤0.2, 0.0005≤w1≤0.001, 0≤w2≤0.1, x+y+z+w1+w2=1, and M is an other doping element such as Zr, Al, B, Mg, Ti, Nb, W, Sc, Si, V, Fe, Mo, Ce, Hf, Ta, La, Sr, Sn, Sb, Zn, Cu, Ge, Mo, Ru, Ir, Ca, K, Ga, or a combination thereof.
[0036] Another embodiment of the present invention provides a positive electrode for a lithium secondary battery comprising the aforementioned positive electrode active material.
[0037] Another embodiment of the present invention provides a lithium secondary battery comprising a positive electrode for the lithium secondary battery. Effects of the invention
[0039] A positive electrode active material for a lithium secondary battery according to one embodiment of the present invention is a lithium metal oxide in the form of a single particle, comprising Y, wherein structural stability is improved as Y has a predetermined concentration gradient pattern, thereby improving the high-temperature life characteristics of the battery. Brief explanation of the drawing
[0041] Figure 1 is a graph showing the results of EDS line scanning analysis for element Y after CP (Cross section Polisher) of the cathode active materials prepared according to Examples 1 to 3 and Comparative Examples 3 to 4. Figure 2 is an SEM image of the positive electrode active material prepared according to Example 1. Figure 3 is an SEM image of the positive electrode active material prepared according to Example 2. Figure 4 is an SEM image of the positive electrode active material prepared according to Comparative Example 1. Figure 5 is an SEM image of the positive electrode active material prepared according to Comparative Example 2. Figure 6 is an SEM image of the positive electrode active material prepared according to Comparative Example 3. Specific details for implementing the invention
[0042] Terms such as first, second, and third are used to describe various parts, components, regions, layers, and / or sections, but are not limited thereto. These terms are used solely to distinguish one part, component, region, layer, or section from another part, component, region, layer, or section. Accordingly, the first part, component, region, layer, or section described below may be referred to as the second part, component, region, layer, or section without departing from the scope of the present invention.
[0043] The technical terms used herein are for the reference of specific embodiments only and are not intended to limit the invention. The singular forms used herein include plural forms unless phrases clearly indicate otherwise. As used in the specification, the meaning of "comprising" specifies certain characteristics, areas, integers, steps, actions, elements, and / or components, and does not exclude the presence or addition of other characteristics, areas, integers, steps, actions, elements, and / or components.
[0044] When it is stated that one part is "above" or "on" another part, it may be directly above or on the other part, or other parts may be involved in between. In contrast, when it is stated that one part is "directly above" another part, no other parts are interposed in between.
[0045] Unless otherwise defined, all terms used herein, including technical and scientific terms, have the same meaning as generally understood by those skilled in the art to which this invention pertains. Terms defined in commonly used dictionaries are further interpreted to have meanings consistent with relevant technical literature and the present disclosure, and are not interpreted in an ideal or highly formal sense unless otherwise defined.
[0046] Also, unless otherwise specified, % means weight %, and 1 ppm is 0.0001 weight %.
[0047] In this specification, the term “combination(s) of these” described in the Markush-type expression means one or more mixtures or combinations selected from the group consisting of the components described in the Markush-type expression, and means including any one or more selected from the group consisting of said components.
[0048] Hereinafter, embodiments of the present invention are described in detail so that those skilled in the art can easily implement the invention. However, the present invention may be embodied in various different forms and is not limited to the embodiments described herein.
[0050] 1. Cathode active material
[0051] A positive electrode active material for a lithium secondary battery according to one embodiment of the present invention comprises a lithium metal oxide in the form of a single particle. The lithium metal oxide in the form of a single particle has a smaller specific surface area compared to conventional secondary particles, which reduces the amount of gas generated due to side reactions with the electrolyte, and has a higher particle strength, which can suppress particle breakage during rolling and reduce the occurrence of cracks due to repeated charging and discharging. Accordingly, it has the advantage of having superior lifespan and safety compared to secondary particles, and can achieve high energy density of the electrode.
[0052] In this specification, “single particle” is a term used to distinguish from a positive active material particle in the form of a secondary particle formed by the aggregation of tens to hundreds of primary particles that were conventionally used, and is a concept that includes a single particle consisting of one primary particle and an aggregate particle of 30 or fewer primary particles.
[0053] In addition, “secondary particles” refers to aggregates formed by the aggregation of tens to hundreds of primary particles through physical or chemical bonding between primary particles without any intentional aggregation or assembly process of the primary particles, i.e., secondary structures.
[0054] In addition, “primary particle” refers to the smallest particle unit that is distinguished as a single mass when the cross-section of the positive active material is observed through a scanning electron microscope (SEM), and it may consist of a single crystal grain or multiple crystal grains.
[0055] Meanwhile, the nickel content in the lithium metal oxide particles according to the present invention may be 80 mol% or more based on the total molar amount of metal excluding lithium. By containing such a high nickel content, capacity and output characteristics can be improved.
[0056] However, compared to conventional secondary-particle type cathode active material particles, the primary particles are relatively larger and there are fewer interfaces between the primary particles that serve as diffusion pathways for lithium ions, resulting in reduced lithium mobility. Additionally, because they are manufactured at relatively high calcination temperatures, a rock salt phase is formed on the particle surface, leading to high surface resistance. This reduction in lithium mobility causes an imbalance in lithium ion movement, which in turn causes deformation of the active material crystal structure and leads to a problem of reduced lifespan characteristics, such as significant deterioration in capacity characteristics as cycles progress.
[0057] The above problem is particularly pronounced in so-called high-nickel lithium metal oxides containing a high nickel content.
[0058] Accordingly, the inventors have completed the present invention as a result of repeated research on a method to improve the structural stability of lithium metal oxide in the form of single particles, and furthermore, high-nickel lithium metal oxide in the form of single particles containing a high nickel content.
[0060] Specifically, the lithium metal oxide according to the present invention includes Y (yttrium) as a doping element. Since Y has a relatively higher bonding affinity with oxygen in the transition metal layer compared to Ni, Co, or Mn, it can improve the structural stability of the active material layered structure and enhance the high-temperature life characteristics of the battery.
[0061] In particular, the lithium metal oxide according to the present invention has a concentration gradient in which the concentration of the doping element Y at the outermost surface of the particle is higher than the concentration at the center of the particle. That is, the doping element Y can be doped at a relatively high concentration at the surface of the lithium metal oxide particle. Accordingly, Y, which has a relatively strong bonding affinity with oxygen, is doped into the particle surface that primarily participates in electrochemical reactions, thereby enabling structural stabilization and long lifespan characteristics of the cathode material.
[0063] More specifically, the above positive active material can satisfy the following Equation 1.
[0064] [Equation 1]
[0065] 0 < DI Y-out - DI Y-cen ≤ 200 (au)
[0066] In Equation 1 above, DI Y-out ≠ is the X-ray counting rate (CPS) intensity value of Y at the outermost surface of the particle during Energy-Dispersive Spectroscopy (EDS) line scan analysis of lithium metal oxide particles, and DI Y-cen is the X-ray count rate (CPS) intensity value of Y at the center of the particle during Energy-Dispersive Spectroscopy (EDS) line scan analysis of lithium metal oxide particles.
[0067] The above DI Y-out - DI Y-cen More specifically, the value may be 20 to 200 or 20 to 140.
[0068] DI Y-out - DI Y-cen If the value is too small, the aforementioned concentration gradient is not present, and the effect of improving lifespan characteristics due to enhanced structural stability may be negligible. DI Y-out - DI Y-cen If the value is too large, an excessive concentration gradient is formed, which may actually reduce structural stability and result in minimal improvement in lifespan characteristics.
[0070] In addition, the above positive active material can satisfy the following Equation 2.
[0071] [Equation 2]
[0072] 450 ≤ DI Y-out ≤ 600 (au)
[0073] In Equation 2 above, DI Y-outY is the X-ray count rate (CPS) intensity value of Y at the outermost surface of the particle during Energy-Dispersive Spectroscopy (EDS) line scan analysis of lithium metal oxide particles.
[0074] The above DI Y-out More specifically, the value may be 470 to 570 or 470 to 550.
[0075] DI Y-out When the value satisfies the above range, the effect of improving lifespan characteristics due to the improvement in the structural stability of the active material can be more preferably realized.
[0077] In addition, the above positive active material can satisfy the following Equation 3.
[0078] [Equation 3]
[0079] 350 ≤ DI Y-cen ≤ 550 (au)
[0080] In Equation 3 above, DI Y-cen is the X-ray count rate (CPS) intensity value of Y at the center of the particle during Energy-Dispersive Spectroscopy (EDS) line scan analysis of lithium metal oxide particles.
[0081] The above DI Y-cen More specifically, the value may be 400 to 540 or 430 to 520.
[0082] DI Y-cen When the value satisfies the above range, the effect of improving lifespan characteristics due to the improvement in the structural stability of the active material can be more preferably realized.
[0084] DI in Equations 1 to 3 above Y-out and DI Y-cenMore specifically, it can be measured by analyzing the X-ray count rate (CPS) intensity value of Y detected through Energy-Dispersive Spectroscopy (EDS) line scan analysis from the center of the particle to the surface of the particle cross-section after processing the positive active material particles with a Cross Section Polisher (CP).
[0085] At this time, the EDS (Energy-Dispersive Spectroscopy) line scan analysis can be performed by adjusting the Z-axis so that the working distance corresponds to 8.5 mm, focusing appropriately, and then increasing the voltage to 10 kV.
[0087] The concentration gradient trend of Y according to the present invention, represented by Equations 1 to 3, can be obtained by dividing and doping the Y raw material during the calcination process in the manufacturing method, and this will be explained in more detail in the manufacturing method described below.
[0089] Meanwhile, the content of Y in the lithium metal oxide particles according to the present invention may be 0.05 to 0.1 mol% based on the total molar amount of metal excluding lithium. If the Y doping content is too low, the effect of improving lifespan characteristics due to improved structural stability of the active material may be negligible. If the Y doping content is too high, the capacity characteristics of the active material may be degraded.
[0090] In addition, the positive active material according to the present invention may have an average particle size (D50) of 3.0 to 4.0 μm, and more specifically, 3.3 to 3.8 μm. If the average particle size (D50) of the positive active material is too small, the electrode density may decrease. If the average particle size (D50) of the positive active material is too large, the lithium ion migration distance may increase as the particle size becomes too large, which may lead to a decrease in capacity characteristics. Therefore, when the average particle size (D50) of the positive active material satisfies the above range, the electrode density and capacity characteristics are evenly and excellently improved, and the energy density characteristics of the battery can be maximized.
[0091] In this specification, the average particle size (D50) may be defined as the particle size corresponding to 50% of the volume accumulation in the particle size distribution curve. The average particle size (D50) may be measured, for example, using a laser diffraction method.
[0092] Meanwhile, the positive electrode active material according to the present invention may further include a coating layer containing Co located on the surface of lithium metal oxide particles. Accordingly, residual lithium on the surface of the lithium metal oxide is reduced, and the cation mixing phenomenon resulting from the recrystallization process is suppressed, thereby enabling more desirable realization of the capacity, output, and lifespan characteristics of the battery.
[0093] At this time, the content of Co in the positive electrode active material may be 0.3 to 4 mol% based on the total molar amount of lithium metal oxide, and more specifically, 0.8 to 3 mol%. When the content of Co in the positive electrode active material satisfies the above range, the effect of improving electrochemical properties due to the aforementioned Co coating can be more preferably realized.
[0094] In addition, the lithium metal oxide according to the present invention may have an a-axis lattice constant of 2.8772 Å or more. The a-axis lattice constant of the above range may be a value obtained when the concentration gradient pattern of Y satisfies the range according to the present invention, and in this case, the effect of improving battery life characteristics due to improved structural stability of the active material can be more preferably realized.
[0095] The above lithium metal oxide may have a c-axis lattice constant of 14.1965 Å or more. The c-axis lattice constant of the above range may be a value obtained when the concentration gradient pattern of Y satisfies the range according to the present invention, and in this case, the effect of improving battery life characteristics due to improved structural stability of the active material can be more preferably realized.
[0096] In this specification, the a-axis lattice constant and the c-axis lattice constant of lithium metal oxide can be estimated using peak broadening of XRD data and can be quantitatively calculated through the Scherrer equation.
[0097] The above lithium metal oxide may have a cation mixing ratio of 1.5% or less in the lithium layer. The cation mixing ratio in the lithium layer refers to the ratio in which other cations, represented by nickel cations, are substituted in addition to lithium ions within the lithium layer. If the cation mixing ratio is too high, it may hinder the movement of lithium ions or cause structural instability of the layered structure, thereby degrading the capacity or lifespan characteristics of the battery. As the cation mixing ratio of the lithium metal oxide according to the present invention satisfies the above range, the capacity and lifespan characteristics can be preferably realized.
[0098] In the present specification, the cation mixing ratio of the lithium metal oxide can be measured by dividing the intensity of the (003) peak of the positive active material XRD (X-ray Diffraction) data by the intensity of the (104) peak.
[0100] The above lithium metal oxide particles can be represented by the following chemical formula 1.
[0101] [Chemical Formula 1]
[0102] Li a [Ni x Co y Mn z Y w1 M W2 ]O2
[0103] In the above chemical formula 1, 0.8≤a≤1.2, 0.8≤x<1, 0≤y≤0.2, 0≤z≤0.2, 0.0005≤w1≤0.001, 0≤w2≤0.1, x+y+z+w1+w2=1, and M is an other doping element such as Zr, Al, B, Mg, Ti, Nb, W, Sc, Si, V, Fe, Mo, Ce, Hf, Ta, La, Sr, Sn, Sb, Zn, Cu, Ge, Mo, Ru, Ir, Ca, K, Ga, or a combination thereof.
[0104] In the lithium metal oxide of Chemical Formula 1 above, lithium may be included in an amount corresponding to a, i.e., 0.8 ≤ a ≤ 1.2. If a is too small, the capacity may decrease, and if a is too large, the strength of the calcined cathode active material may increase, making it difficult to grind, and the amount of gas generated may increase due to an increase in lithium by-products. Considering the effect of improving the capacity characteristics of the cathode active material by controlling the lithium content and the balance of sinterability during the manufacture of the active material, the lithium may more preferably be included in an amount of 0.9 ≤ a ≤ 1.1.
[0105] In the lithium metal oxide of Chemical Formula 1 above, nickel may be included in an amount corresponding to x, i.e., 0.8≤x<1 or 0.85≤x≤0.97. If the nickel content is too low, the capacity and output characteristics may deteriorate. If the nickel content is too high, the lifespan and thermal safety may decrease due to reduced structural stability of the active material, and manufacturing costs may increase.
[0106] In the lithium metal oxide of Chemical Formula 1 above, cobalt may be included in an amount corresponding to y, i.e., 0≤y≤0.2 or 0.01≤y≤0.15. If the cobalt content is too low, grain size growth may be inhibited and output characteristics may be degraded. If the cobalt content is too high, manufacturing costs may increase and reversible capacity may decrease.
[0107] In the lithium metal oxide of Chemical Formula 1 above, manganese may be included in an amount corresponding to z, i.e., 0≤z≤0.2 or 0.01≤z≤0.15. If the manganese content is too low, the production cost may increase and the stability of the active material may decrease. If the manganese content is too high, the capacity and output characteristics of the battery may decrease.
[0108] In the lithium metal oxide of Chemical Formula 1 above, the doping element Y may be included in an amount corresponding to w1, i.e., 0.0005 ≤ w1 ≤ 0.001. If the Y doping content is too low, the effect of improving lifespan characteristics due to improved structural stability of the active material may be negligible. If the Y doping content is too high, the capacity characteristics of the active material may be degraded.
[0109] In the lithium metal oxide of the above chemical formula 1, other doping element M may be included in an amount corresponding to w2, i.e., 0≤w2≤0.1, and may be appropriately added and used within a range that does not degrade battery performance.
[0111] 2. Method for manufacturing positive electrode active material
[0112] Other physical properties, including the concentration gradient trend of Y according to the present invention represented by Equations 1 to 3, can be obtained by dividing and doping the Y raw material during the calcination process in the manufacturing method.
[0113] Specifically, another embodiment of the present invention provides a method for manufacturing a positive electrode active material for a lithium secondary battery, comprising the steps of: preparing a metal precursor containing nickel; mixing the metal precursor, a lithium raw material, and a first Y raw material, and then performing a first calcination to form a first calcined product; mixing the first calcined product and a second Y raw material, and then performing a second calcination to form a lithium metal oxide; and breaking down the lithium metal oxide to form a lithium metal oxide in the form of a single particle, wherein the ratio of the input amounts of the first Y raw material and the second Y raw material (first Y raw material: second Y raw material) is 60:40 to 0:100.
[0114] Hereinafter, a method for manufacturing a positive electrode active material for a lithium secondary battery according to another embodiment of the present invention will be described in detail step by step.
[0116] First, prepare a metal precursor containing nickel.
[0117] The nickel content in the above metal precursor may be 80 mol% or more based on the total molar amount of the metal. Accordingly, the capacity and output characteristics of the battery can be more preferably realized.
[0118] The above metal precursor may be, more specifically, a metal hydroxide.
[0119] The above metal hydroxide may be prepared by co-precipitating a metal-containing solution containing a complexing agent and a pH adjuster by adding them to a metal-containing solution containing a nickel raw material and optionally a cobalt raw material or a manganese raw material.
[0120] The above nickel raw material is not particularly limited as long as it is used in the industry for manufacturing a cathode active material precursor. For example, the above nickel raw material may be a nickel-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, or oxyhydroxide, and specifically, it may be NiSO4, NiSO4·6H2O, Ni(OH)2, NiO, NiOOH, NiCO3·2Ni(OH)2·4H2O, NiC2O2·2H2O, Ni(NO3)2·6H2O, nickel fatty acid salt, nickel halide, or a combination thereof, but is not limited thereto.
[0121] The above-mentioned cobalt raw material is not particularly limited as long as it is used in the industry for the manufacture of cathode active material precursors. For example, the above-mentioned cobalt raw material may be a cobalt-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, or oxyhydroxide, and specifically, CoSO₄ 4, It may be CoSO4·7H2O, Co(OH)2, CoOOH, Co(OCOCH3)2·4H2O, Co(NO3)2·6H2O, or a combination thereof, but is not limited thereto.
[0122] The above manganese raw material is not particularly limited as long as it is used in the industry for the manufacture of cathode active material precursors. For example, the above manganese raw material may be a manganese-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, oxyhydroxide, or a combination thereof. Specifically, it may be a manganese salt such as MnSO4, MnCO3, Mn(NO3)2, manganese acetate, manganese dicarboxylate, manganese citrate, and manganese fatty acid, manganese oxide such as Mn2O3, MnO2, and Mn3O4, oxyhydroxide, manganese chloride, or a combination thereof, but is not limited thereto.
[0123] The above metal-containing solution may be prepared by adding a nickel raw material and optionally a cobalt raw material or a manganese raw material to a solvent, specifically water, or a mixture of water and an organic solvent that can be uniformly mixed with water (e.g., alcohol).
[0124] The above-mentioned complexing agent-containing solution performs the role of forming a complex, and may include, for example, NH3, NH4OH, (NH4)2SO4, NH4NO3, NH4Cl, CH3COONH4, NH4CO3, or a combination thereof as the complexing agent, but is not limited thereto. Meanwhile, the above-mentioned complexing agent-containing solution may be used in the form of an aqueous solution, and in this case, water or a mixture of water and an organic solvent that is uniformly miscible with water (e.g., alcohol, etc.) may be used as the solvent.
[0125] The above pH-adjusting solution acts as a precipitating agent or a pH adjuster and may include alkali compounds such as hydroxides of alkali metals or alkaline earth metals like NaOH, KOH, or Ca(OH)2, their hydrates, or combinations thereof. Meanwhile, the above pH-adjusting solution may also be used in the form of an aqueous solution, in which case water or a mixture of water and an organic solvent that is uniformly miscible with water (e.g., alcohol) may be used as the solvent. In this case, the above pH-adjusting solution may be added in an amount such that the pH of the reaction solution becomes 11 to 13.
[0126] The above co-precipitation reaction can be carried out under an inert atmosphere such as nitrogen or argon, at a temperature of 30 to 70°C, and at a pH of 11 to 13.
[0127] By the above process, particles of nickel (-cobalt-manganese-doping element) hydroxide are generated and precipitated in the reaction solution. The precipitated precursor particles can be separated by conventional methods, washed, and dried to obtain a precursor. The precursor may be a secondary particle formed by the aggregation of primary particles.
[0128] At this time, the molar ratio of nickel, cobalt, and manganese in the precursor can be controlled by adjusting the concentrations of the nickel raw material, cobalt raw material, and manganese raw material.
[0129] Accordingly, the nickel content in the metal precursor can be controlled to 80 mol% or more based on the total molar amount of the transition metal. The technical significance of controlling the nickel content in the transition metal precursor is as described above and is therefore omitted.
[0131] Next, the metal precursor, lithium raw material, and first Y raw material are mixed and then calcined to form a first calcined product.
[0132] Next, the above first calcined product and the second Y raw material are mixed, and then second calcined to form a lithium metal oxide.
[0133] In this way, the calcination process for doping with Y is divided into a second calcination, and by doping by adding the Y raw material in a divided manner, a positive electrode active material particle having a Y concentration gradient tendency according to the present invention can be obtained.
[0134] At this time, the ratio of the input amounts of the first Y raw material and the second Y raw material (first Y raw material: second Y raw material) may be 60:40 to 0:100, and more specifically, 60:40 to 20:80. When the ratio of the input amounts of the first Y raw material and the second Y raw material satisfies the above range, the Y concentration gradient trend within the cathode active material can be more appropriately controlled to the range according to the present invention, and as a result, the effect of improving lifespan characteristics due to improved structural stability of the active material can be preferably realized.
[0135] In addition, the sum of the input amounts of the first Y raw material and the second Y raw material can be controlled so that the Y content in the lithium metal oxide is 0.05 to 0.1 mol% based on the total molar amount of metal excluding lithium. As the sum of the input amounts of the first Y raw material and the second Y raw material is adjusted to the above range, the Y content doped in the lithium metal oxide can be appropriately controlled to the range according to the present invention.
[0136] Meanwhile, the above-mentioned first Y raw material and second Y raw material are each independently Y2O3, Y(NO3)3·4H2O, (CH3CO2)3Y·4H2O, YCl 3, It may be YF3, (CF3SO3)3Y or a combination thereof, but is not necessarily limited thereto.
[0139] The above first firing and second firing can each be performed independently at a temperature of 600 to 900°C.
[0140] At this time, the first firing temperature may be higher than the second firing temperature. In this way, there may be an advantage in improving the lifespan characteristics of a single-particle cathode active material through a firing profile that controls the degree of particle growth in the first firing and then increases the structural stability of the material by performing a second firing at a temperature lower than the first firing temperature.
[0141] More specifically, the first firing temperature may be 800 to 850℃.
[0142] More specifically, the secondary firing temperature may be 680 to 800°C.
[0143] More specifically, the difference between the first firing and second firing temperatures may be 40 to 120°C or 60 to 100°C.
[0144] When the first firing temperature, the second firing temperature, and the difference between the first and second firing temperatures satisfy the above range, the effect of improving lifespan characteristics due to the improvement in structural stability of the aforementioned single-particle cathode active material can be more preferably realized.
[0145] In addition, the first firing time may be shorter than the second firing time. Accordingly, there may be an advantage in improving the performance of the material by controlling the degree of single particle growth of the precursor by controlling the firing time while carrying out the first firing at a high temperature, and then carrying out the second firing at a temperature lower than the first firing temperature while making the firing time longer than the first firing time to increase the crystal structure stability of the single particles.
[0146] At this time, the first firing time may be performed for 2 to 5 hours. If the first firing time is too short, the crystal structure is not formed properly and the formation of single particles is not achieved, which may lead to a decrease in lifespan characteristics. If the first firing time is too long, structural degradation of the material may occur due to over-firing, which may result in a decrease in electrochemical properties such as the discharge capacity and output characteristics of the material.
[0147] In addition, the second sintering time may be performed for 6 to 10 hours. If the second sintering time is too short, lithium metal oxide in the form of single particles may not be formed, and the crystal structure may be under-formed, which may lead to reduced structural stability and consequently deterioration of electrochemical properties. If the second sintering time is too long, lithium may be lost within the material due to over-sintering, which may result in crystal structure collapse and capacity degradation.
[0148] In addition, the first and second calcinations can be performed in an oxygen (O2) atmosphere. As the first and second calcinations are performed in an oxygen atmosphere, the layered structure of the lithium metal oxide can be better realized, and the electrochemical properties can be more preferably realized.
[0150] Next, the lithium metal oxide is broken down to form a single-particle form of lithium metal oxide.
[0151] The above disintegration method is not particularly limited and can be applied without restriction using general methods in the industry.
[0153] 3. Anodes and Lithium Secondary Batteries
[0154] Another embodiment of the present invention provides a positive electrode for a lithium secondary battery comprising the aforementioned positive electrode active material.
[0155] More specifically, the anode may include an anode current collector and an anode active material layer disposed on the anode current collector and comprising the aforementioned anode active material.
[0156] The above positive current collector is not particularly limited as long as it is conductive without causing chemical changes in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the above positive current collector may typically have a thickness of 3 to 500 μm, and fine irregularities may be formed on the surface of the positive current collector to increase the adhesion of the positive active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0157] The above positive active material layer may include a binder and / or a conductive material together with the aforementioned positive active material.
[0158] At this time, the binder serves to improve adhesion between positive active material particles and adhesion between the positive active material and the positive current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof. One of these alone or a mixture of two or more may be used, but is not limited thereto. The binder may be included in an amount of 1 to 30 weight% based on the total weight of the positive active material layer.
[0159] In addition, the conductive material is used to impart conductivity to the electrode, and in the battery being constructed, any material that possesses electronic conductivity without causing chemical changes may be used without any particular limitations. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives. One of these alone or a mixture of two or more may be used, but is not limited thereto. The conductive material may typically be included in an amount of 1 to 30 weight percent relative to the total weight of the positive electrode active material layer.
[0160] The above-mentioned anode can be manufactured according to a conventional anode manufacturing method, except for using the above-mentioned anode active material.
[0161] Specifically, the anode can be manufactured by applying a composition for forming an anode active material layer, comprising the aforementioned anode active material and optionally a binder, conductive material, or solvent as needed, onto an anode current collector, followed by drying and rolling. At this time, the types and contents of the anode active material, binder, and conductive material are as described above.
[0162] The above solvent may be a solvent commonly used in the relevant technical field, such as dimethylsulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, and one of these alone or a mixture of two or more may be used. The amount of the above solvent used is sufficient if it has a viscosity that allows for the dissolution or dispersion of the anode active material, conductive material, and binder, taking into account the coating thickness of the slurry and the manufacturing yield, and subsequently provides excellent thickness uniformity when coated for anode manufacturing.
[0163] Alternatively, the anode may be manufactured by casting the composition for forming the anode active material layer onto a separate support, and then laminating the film obtained by peeling off from the support onto an anode current collector.
[0165] Another embodiment of the present invention provides a lithium secondary battery comprising a positive electrode for a lithium secondary battery as described above.
[0166] More specifically, the above lithium secondary battery may include a positive electrode; a negative electrode; a separator; and an electrolyte.
[0167] The above lithium secondary battery may optionally further include a battery container that accommodates the electrode assembly of the positive electrode, negative electrode, and separator, and a sealing member that seals the battery container.
[0168] The above cathode may include a cathode current collector and a cathode active material layer located on the cathode current collector.
[0169] The above-mentioned negative current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., and aluminum-cadmium alloy may be used. In addition, the above-mentioned negative current collector may typically have a thickness of 3 to 500 μm, and, similar to the positive current collector, fine irregularities may be formed on the surface of the current collector to strengthen the bonding strength of the negative active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0170] The above-mentioned cathode active material layer may optionally include a binder and a conductive material together with the cathode active material. The above-mentioned cathode active material layer may be manufactured, as an example, by applying a composition for forming a cathode active material layer, comprising a cathode active material and optionally a binder and a conductive material, onto a cathode current collector and drying it, or by casting the composition for forming a cathode onto a separate support and then laminating the film obtained by peeling it off from the support onto a cathode current collector.
[0171] As the above-mentioned negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, or Al alloys; metal oxides capable of doping and dedoping lithium, such as SiOβ (0 < β < 2), SnO2, vanadium oxide, and lithium vanadium oxide; or composites comprising the above-mentioned metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or more of these may be used. Additionally, a metallic lithium thin film may be used as the above-mentioned negative electrode active material. Furthermore, the carbon material may include both low-crystallinity carbon and high-crystallinity carbon. Representative examples of low-crystallinity carbon include soft carbon and hard carbon, while representative examples of high-crystallinity carbon include amorphous, plate-like, flake-like, spherical, or fibrous natural or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch-derived cokes.
[0172] The binder and conductive material mentioned above may be the same as those previously described in the anode.
[0174] The above separator separates the negative electrode and the positive electrode and provides a pathway for the movement of lithium ions. It can be used without special restrictions as long as it is typically used as a separator in a lithium secondary battery, and it is particularly desirable that it has low resistance to the movement of electrolyte ions and excellent electrolyte wettability. Specifically, a porous polymer film, such as a porous polymer film made of a polyolefin-based polymer like ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, such as a nonwoven fabric made of high-melting-point glass fiber or polyethylene terephthalate fiber, may be used. Furthermore, a coated separator containing ceramic components or polymer materials may be used to ensure heat resistance or mechanical strength, and it may optionally be used in a single-layer or multi-layer structure.
[0176] The above electrolytes include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, molten inorganic electrolytes, etc., which can be used in the manufacture of lithium secondary batteries, but are not limited to these.
[0177] Specifically, the organic liquid electrolyte may include an organic solvent and a lithium salt.
[0178] The above organic solvent may be used without special restrictions as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the above organic solvent may include ester-based solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether-based solvents such as dibutyl ether or tetrahydrofuran; ketone-based solvents such as cyclohexanone; and aromatic hydrocarbon-based solvents such as benzene and fluorobenzene. Carbonate-based solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (where R is a straight-chain, branched, or cyclic hydrocarbon group having C2 to C20 structures and may include a double bond, a directional ring, or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes may be used. Among these, a carbonate-based solvent is preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery, and a low-viscosity linear carbonate-based compound (e.g., ethylmethyl carbonate, dimethyl carbonate or diethyl carbonate, etc.) is more preferred.In this case, using a mixture of cyclic carbonate and chain carbonate in a volume ratio of about 1:1 to about 1:9 can result in excellent performance of the electrolyte.
[0179] The above lithium salt can be used without special restrictions as long as it is a compound capable of providing lithium ions used in lithium secondary batteries. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably used within the range of 0.1 to 2.0 M. When the concentration of the lithium salt falls within the above range, the electrolyte has appropriate conductivity and viscosity, so it can exhibit excellent electrolyte performance and allow lithium ions to move effectively.
[0180] In addition to the above electrolyte components, the above electrolyte may further include one or more additives for the purpose of improving the lifespan characteristics of the battery, suppressing the decrease in battery capacity, and improving the discharge capacity of the battery, such as, for example, haloalkylene carbonate-based compounds like difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ether, ethylene diamine, n-glyme, hexamethylphosphate triamide, nitrobenzene derivative, sulfur, quinone imine dye, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, or aluminum trichloride. In this case, the additive may be included in an amount of 0.1 to 5 weight% based on the total weight of the electrolyte.
[0181] As described above, since the lithium secondary battery containing the positive electrode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics, and capacity retention rate, it is useful in portable devices such as mobile phones, laptop computers, and digital cameras, as well as in the field of electric vehicles such as hybrid electric vehicles (HEVs).
[0182] Accordingly, another embodiment of the present invention provides a battery module comprising the lithium secondary battery as a unit cell and a battery pack comprising the same.
[0183] The above battery module or battery pack can be used as a power source for one or more medium-to-large devices, including a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.
[0185] The embodiments of the present invention will be described in more detail below through examples. However, the following examples are merely preferred embodiments of the present invention, and the present invention is not limited by the following examples.
[0187] Example 1
[0188] (1) Manufacturing of positive electrode active material
[0189] (1st firing) Ni 0.96 Co 0.02 Mn 0.02 After mixing a metal precursor of (OH)2 composition, a lithium raw material of LiOH·H2O, and a first Y raw material of Y2O3, the mixture was first calcined at a temperature of 820°C for 4 hours under an oxygen atmosphere to form a first calcined product, and then naturally cooled.
[0190] (Second calcination) After mixing the first calcined product with the second Y raw material of Y2O3, a second calcination was performed at a temperature of 740°C for 9 hours under an oxygen atmosphere to form a lithium metal oxide. At this time, the ratio of the input amounts of the first Y raw material and the second Y raw material was set to 50:50, and the total input amounts of the first Y raw material and the second Y raw material were set so that the doping content of Y was 0.0752 mol% based on the total molar amount of metal excluding lithium in the lithium metal oxide.
[0191] After (disintegration), the lithium metal oxide was first disintegrated using a rotor mill and secondarily disintegrated using a jet mill to form a lithium transition metal oxide in the form of a single particle.
[0192] After (coating), the lithium metal oxide and Co(OH)2 as a Co raw material were mixed, and a coating heat treatment was performed at a temperature of 680°C for 6 hours to form a Co coating layer, thereby producing a final cathode active material. At this time, the amount of Co(OH)2 added was controlled so that the Co content was 2 mol% based on the total molar amount of the lithium metal oxide.
[0193] (2) Lithium secondary battery manufacturing
[0194] The slurry for electrode manufacturing was prepared by mixing the above-prepared cathode active material, conductive material (carbon black, Denka black), and binder (PVDF, KF9700) in a ratio of 95.0 : 2.0 : 3.0 wt%, and adding NMP (N-Methyl-2-pyrrolidone) to adjust the viscosity so that the solid content was approximately 60%. The prepared slurry was coated onto a 20 µm thick Al foil using a doctor blade and then dry-rolled. The electrode loading amount was 16.0 mg / cm². 2 It was, and the rolled density (25 ℃, 20 kN) was 3.5 g / cm³ 3 It was.
[0195] A coin cell was manufactured using an electrolyte of 1M LiPF6 in EC:DMC:DEC=1:2:1 (vol%) with 2.0 vol% of VC added relative to the total amount of the electrolyte, a PP separator, and a lithium anode (400 μm, Niba metal).
[0197] Example 2
[0198] A positive electrode active material and a lithium secondary battery were manufactured in the same manner as in Example 1, except that in the first and second calcination steps, the ratio of the input amounts of the first Y raw material and the second Y raw material was set to 30:70.
[0200] Example 3
[0201] A positive electrode active material and a lithium secondary battery were manufactured in the same manner as in Example 1, except that in the first and second calcination steps, the ratio of the input amounts of the first Y raw material and the second Y raw material was set to 0:100.
[0203] Comparative Example 1 (Continuous firing without Y doping)
[0204] Ni 0.96 Co 0.02 Mn 0.02 A positive electrode active material and a lithium secondary battery were prepared in the same manner as in Example 1, except that a metal precursor of (OH)2 composition and LiOH·H2O were mixed without adding Y raw material, then calcined at a temperature of 820°C for 4 hours under an oxygen atmosphere, followed by calcination at a temperature of 740°C for 9 hours to form a lithium metal oxide.
[0206] Comparative Example 2 (Secondary firing without Y doping)
[0207] A positive electrode active material and a lithium secondary battery were manufactured by performing a first firing and a second firing in the same manner as in Example 1, except that no Y raw material was added.
[0209] Comparative Example 3
[0210] A positive electrode active material and a lithium secondary battery were manufactured in the same manner as in Example 1, except that in the first and second firing steps, the ratio of the input amounts of the first Y raw material and the second Y raw material was set to 100:0.
[0212] Comparative Example 4
[0213] A positive electrode active material and a lithium secondary battery were manufactured in the same manner as in Example 1, except that in the first and second calcination steps, the ratio of the input amounts of the first Y raw material and the second Y raw material was set to 70:30.
[0215] Table 1 below summarizes the process conditions of the examples and comparative examples, and Tables 2 and 3 below summarize the evaluation results of the positive electrode active material properties and high-temperature life characteristics of the lithium secondary battery according to Experimental Examples 3 and 4 described later.
[0216] (In Table 1 below, the Y raw material input amount during continuous calcination, the first Y raw material input amount during secondary calcination, and the second Y raw material input amount are relative amounts assuming that the Y raw material input amount at which the Y doping content becomes 0.0752 mol% based on the total molar amount of metal excluding lithium in the lithium metal oxide is 100.)
[0217] Process conditions Continuous firing Secondary firing Y amount of raw material input Input amount of 1st Y raw material Input amount of 2 Y raw materials Comparative Example 1 0 - - Comparative Example 2 - 0 0 Comparative Example 3 - 100 0 Comparative Example 4 - 70 30 Example 1 - 50 50 Example 2 - 30 70 Example 3 - 0 100
[0218] Physical properties of active material OF Y-out (to the) OF Y-cen (to the) OF Y-out - OF Y-cen (to the) Average particle size (D50, μm) a-axis lattice constant (Å) c-axis lattice constant (Å) Cation mixing ratio (%) Comparative Example 1 - - - 4 2.8769 14.1961 0.9 Comparative Example 2 - - - 3.3 2.8768 14.1945 1.2 Comparative Example 3 392.2 604.3 -212.1 3.4 2.877 14.1952 1.1 Comparative Example 4 412.2 564.3 -152.1 3.5 2.8771 14.1964 0.9 Example 1 523.7 491.9 31.8 3.4 2.8773 14.1966 1 Example 2 546.5 451.9 94.6 3.6 2.8777 14.1989 1.2 Example 3 554.2 372.9 181.3 3.7 2.8775 14.1985 1.2
[0219] High-temperature life characteristics 30th discharge capacity (mAh / g) 30th retention (%) 50th discharge capacity (mAh / g) 50th retention(%) Comparative Example 1 170.2 84.5 152.3 75.7 Comparative Example 2 175 91.7 164.7 86.3 Comparative Example 3 181.2 89.8 168.1 83.1 Comparative Example 4 179.7 90.6 167.4 84.4 Example 1 184.8 90.8 173.5 85.2 Example 2 184.5 91.2 173.4 85.8 Example 3 182.3 91.5 169.3 85.5
[0221] Experimental Example 1: SEM image of cathode active material
[0222] Scanning electron microscope (SEM) images of the positive electrode active materials prepared according to Examples 1 and 2 and Comparative Examples 1, 2, and 3 were observed and are shown in order in Figures 2 to 6, respectively.
[0223] Referring to FIGS. 2 to 6, it was confirmed that the positive electrode active materials of the examples and comparative examples have a single particle form, and that there is no significant difference in morphology or degree of particle growth between the examples and comparative examples.
[0225] Experimental Example 2: Evaluation of Physical Properties of Anode Active Material
[0226] (1) Evaluation of Y element concentration gradient within active material particles
[0227] Energy-Dispersive Spectroscopy (EDS) line scan analysis was performed on the element Y after Cross-section Polishing (CP) of the cathode active materials prepared according to Examples 1 to 3 and Comparative Examples 4 to 5, and the X-ray Count Rate (CPS) intensity values of Y were analyzed and are shown in Fig. 1. In Fig. 1, the horizontal axis, Distance, represents the distance from the center of the particle to the concentration measurement point. At this time, the X-ray Count Rate (CPS) intensity values of Y were measured at the center of the particle and at the outermost surface, and these were respectively DI Y-cen and DI Y-out It was written as.
[0228] EDS line scan analysis measurements were performed by adjusting the Z-axis to a working distance of 8.5 mm, focusing appropriately, and increasing the voltage to 10 kV.
[0229] (2) Evaluation of average particle size (D50)
[0230] For the cathode active materials prepared according to the examples and comparative examples, the particle size corresponding to 50% of the volume accumulation was measured using the laser diffraction method.
[0231] (3) Evaluation of a-axis lattice constant and c-axis lattice constant
[0232] For the cathode active materials prepared according to the examples and comparative examples, the a-axis lattice constant and the c-axis lattice constant were evaluated by quantitatively calculating them using the Scherrer equation based on the peak broadening of the XRD data.
[0233] (4) Evaluation of cation mixing ratio
[0234] For the positive electrode active materials prepared according to the examples and comparative examples, the cation mixing ratio was measured by dividing the intensity of the (003) peak of the positive electrode active material XRD data by the intensity of the (104) peak.
[0236] Experimental Example 3: Evaluation of High-Temperature Life Characteristics of Lithium Secondary Battery (45℃, 30 cycles / 50 cycles)
[0237] After fabricating a lithium secondary battery half cell, it was charged to 4.3V at 45°C with a constant current of 0.5C, then switched to a constant voltage and charged until the termination current reached 0.05C. After a 10-minute rest time following charging, it was discharged with a constant current of 1.0C until it reached 3.0V. Under these charge-discharge cycle conditions, 30 and 50 charge-discharge cycles were performed, and the capacity retention rate of the 30th and 50th cycles was calculated relative to the first cycle.
[0239] Referring to FIG. 1 and Tables 1 to 3, in the case of Examples 1 to 3, where Y is doped in divided doses and the ratio of the divided doping amounts during the first and second firing is appropriately controlled, the particle has a surface-concentrated doping gradient in which the Y concentration at the outermost surface is greater than the Y concentration at the center of the particle, and DI Y-out - DI Y-cen It was confirmed that all physical properties, including the value, a-axis lattice constant, and c-axis lattice constant, were controlled within the range according to the present invention. As a result, it was confirmed that the discharge capacity at 30 cycles, the capacity retention rate at 30 cycles, the discharge capacity at 50 cycles, and the capacity retention rate at 50 cycles were all excellent, and thus it was confirmed that the high-temperature life characteristics were significantly improved.
[0240] On the other hand, in the case of Comparative Example 1, as a result of manufacturing the active material by continuous calcination without Y doping, it was confirmed that the lifespan characteristics were significantly degraded, with the discharge capacity at 30 cycles, the capacity retention rate at 30 cycles, the discharge capacity at 50 cycles, and the capacity retention rate at 50 cycles being significantly smaller than those of the example.
[0241] In the case of Comparative Example 2, as a result of manufacturing the active material by secondary calcination without Y doping, the capacity retention rate at 30 cycles and the capacity retention rate at 50 cycles were similar to those of the example, but since the discharge capacity at 30 cycles and the discharge capacity at 50 cycles themselves were smaller than those of the example, it was confirmed that the lifespan characteristics were deteriorated.
[0242] In the case of Comparative Examples 3 and 4, an active material is prepared by doping with Y and secondary calcination; however, as a result of the divided Y doping amount during the primary and secondary calcination deviating from the range according to the present invention, the Y concentration at the outermost surface of the particle is lower than the Y concentration at the center of the particle, and DI Y-out - DI Y-cen It was confirmed that various physical properties, including the value, a-axis lattice constant, and c-axis lattice constant, fell outside the range according to the present invention. In addition, it was confirmed that the lifespan characteristics deteriorated, as the discharge capacity at 30 cycles, the capacity retention rate at 30 cycles, the discharge capacity at 50 cycles, and the capacity retention rate at 50 cycles were smaller than those of the examples.
[0243] Meanwhile, when comparing Examples 1 to 3, in the case of Examples 1 and 2, where the divided Y doping amount during the first and second firing was more appropriately controlled, DI Y-out - DI Y-cen It was confirmed that the values, etc. were controlled within a more appropriate range. As a result, compared to Example 3 (although the capacity retention rate at 30 cycles and the capacity retention rate at 50 cycles were similar), it was confirmed that the 30-cycle discharge capacity and the 50-cycle discharge capacity themselves were larger, and accordingly, it was confirmed that the life characteristics were implemented more desirablely overall.
[0245] Although preferred embodiments of the present invention have been described above, the present invention is not limited thereto and can be implemented with various modifications within the scope of the claims, the detailed description of the invention, and the attached drawings, and it is obvious that such modifications also fall within the scope of the present invention.
[0246] Therefore, the substantive scope of the present invention shall be defined by the appended claims and their equivalents.
Claims
Claim 1 A positive electrode active material for a lithium secondary battery having a single particle form and comprising a lithium metal oxide particle containing nickel, wherein the lithium metal oxide particle contains Y (yttrium), and Y within the lithium metal oxide particle is present at both the center of the particle and the outermost surface of the particle, and wherein the concentration of Y at the outermost surface of the lithium metal oxide particle is higher than the concentration at the center of the lithium metal oxide particle, the positive electrode active material. Claim 2 In claim 1, a positive electrode active material for a lithium secondary battery satisfying the following Formula 1: [Formula 1]0 < DI Y-out - DI Y-cen ≤ 200 (au) In Equation 1 above, DI Y-out ≠ is the X-ray counting rate (CPS) intensity value of Y at the outermost surface of the particle during Energy-Dispersive Spectroscopy (EDS) line scan analysis of lithium metal oxide particles, and DI Y-cen is the X-ray count rate (CPS) intensity value of Y at the center of the particle during Energy-Dispersive Spectroscopy (EDS) line scan analysis of lithium metal oxide particles. Claim 3 In claim 1, a positive electrode active material for a lithium secondary battery satisfying the following Equation 2: [Equation 2] 450 ≤ DI Y-out ≤ 600 (au) In Equation 2 above, DI Y-out Y is the X-ray count rate (CPS) intensity value of Y at the outermost surface of the particle during Energy-Dispersive Spectroscopy (EDS) line scan analysis of lithium metal oxide particles. Claim 4 In claim 1, a positive electrode active material for a lithium secondary battery satisfying the following Equation 3: [Equation 3] 350 ≤ DI Y-cen ≤ 550 (au) In Equation 3 above, DI Y-cen is the X-ray count rate (CPS) intensity value of Y at the center of the particle during Energy-Dispersive Spectroscopy (EDS) line scan analysis of lithium metal oxide particles. Claim 5 A positive electrode active material for a lithium secondary battery according to claim 1, wherein the content of Y in the lithium metal oxide particles is 0.05 to 0.1 mol% based on the total molar amount of metal excluding lithium. Claim 6 A positive electrode active material for a lithium secondary battery according to claim 1, wherein the average particle size (D50) is 3.0 to 4.0 μm. Claim 7 A positive electrode active material for a lithium secondary battery according to claim 1, wherein the nickel content in the lithium metal oxide particles is 80 mol% or more based on the total molar amount of metal excluding lithium. Claim 8 A positive electrode active material for a lithium secondary battery according to claim 1, further comprising a coating layer containing Co located on the surface of the lithium metal oxide particles. Claim 9 A positive electrode active material for a lithium secondary battery according to claim 8, wherein the content of Co in the positive electrode active material is 0.3 to 4 mol% based on the total molar amount of lithium metal oxide. Claim 10 In claim 1, the lithium metal oxide is a positive electrode active material for a lithium secondary battery having an a-axis lattice constant of 2.8772 Å or more. Claim 11 In claim 1, the lithium metal oxide is a positive electrode active material for a lithium secondary battery having a c-axis lattice constant of 14.1965 Å or more. Claim 12 In claim 1, the lithium metal oxide is a positive electrode active material for a lithium secondary battery having a cation mixing ratio of 1.5% or less in the lithium layer. Claim 13 In claim 1, the lithium metal oxide particles are a positive electrode active material for a lithium secondary battery represented by the following chemical formula 1: [Chemical Formula 1]Li a [Ni x Co y Mn z Y w1 M W2 ]O2 In the above chemical formula 1, 0.8≤a≤1.2, 0.8≤x<1, 0≤y≤0.2, 0≤z≤0.2, 0.0005≤w1≤0.001, 0≤w2≤0.1, x+y+z+w1+w2=1, and M is an other doping element such as Zr, Al, B, Mg, Ti, Nb, W, Sc, Si, V, Fe, Mo, Ce, Hf, Ta, La, Sr, Sn, Sb, Zn, Cu, Ge, Mo, Ru, Ir, Ca, K, Ga, or a combination thereof. Claim 14 A positive electrode for a lithium secondary battery comprising the positive electrode active material of claim 1. Claim 15 A lithium secondary battery comprising a positive electrode for a lithium secondary battery according to claim 14.