Cathode material for sodium metal halide battery and sodium metal halide battery using the same

The use of ferronickel alloy in sodium metal halide batteries addresses high manufacturing costs by complementing nickel and iron components, enhancing battery performance and reducing overvoltage, thus optimizing cathode materials.

KR103046672B1Active Publication Date: 2026-11-10RES INST OF IND SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020210184796
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-12-22
Publication Date
2026-11-10
Estimated Expiration
2041-12-22

Smart Images

  • Figure 112021148569875-PAT00003_ABST
    Figure 112021148569875-PAT00003_ABST
Patent Text Reader

Abstract

The cathode material for a sodium metal halide battery of the present embodiment comprises alloy particles, a sodium source, and an additive, and the alloy particles may include one or more elements selected from nickel (Ni), iron (Fe), zinc (Zn), and copper (Cu).
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present embodiments relate to a cathode material for a high-temperature sodium metal halide battery and a sodium metal halide battery manufactured using the same. Background Technology

[0003] Sodium metal halide batteries are attracting attention as secondary batteries for electric vehicles and large-capacity energy storage (ESS) devices due to their advantages such as high safety, long lifespan, and high energy density.

[0004] The above sodium metal halide battery generally uses a liquid secondary electrolyte (NaAlCl4, etc.) impregnated with metal powder (Ni, Fe, Zn, Cu, etc.) and sodium chloride (NaCl) powder in a discharged state as a positive active material. If necessary, it may include additives such as sodium iodide (NaI), sodium fluoride (NaF), sodium bromide (NaBr), sulfur (S), sodium sulfide (Na2S), and iron sulfide (FeS).

[0005] Recently, research has been conducted to replace the high-cost sealing process with polymer sealing by lowering the operating temperature to reduce battery manufacturing costs. In addition, studies are underway to use iron (Fe) powder to replace expensive nickel (Ni) powder. However, even when iron powder is used, it is currently manufactured through a high-cost carbonyl process to achieve the quality required for battery use. Furthermore, other high-purity metals also face the problem of increased costs when used as cathode active materials due to the complex refining processes involved; therefore, to reduce raw material costs, it is necessary to discover affordable metal raw materials for active applications.

[0006] For example, the ferronickel alloy (Fe-Ni alloy) used to adjust the nickel content when manufacturing nickel-containing stainless steel, such as 300-series stainless steel (Fe-Ni-Cr alloy), is inexpensive because it reduces the cost of refining into a single metal element, and it satisfies the required characteristics as a transition metal material for sodium metal halide batteries as it is composed of nickel and iron, which are transition metals used as conventional cathode active materials. The problem to be solved

[0008] The present embodiments are intended to solve the aforementioned problems and aim to improve battery performance by using an inexpensive alloy as a cathode material and mutually complementing the characteristics of two or more elemental components. means of solving the problem

[0010] A positive electrode active material for a sodium metal halide battery according to one embodiment comprises alloy particles, a sodium source, and an additive, and the alloy particles may include one or more elements selected from nickel, iron, zinc, and copper.

[0011] In addition, the alloy particles may include a ferronickel (Fe-Ni) alloy.

[0012] In addition, the anode material may further include one or more single metal particles selected from nickel, iron, zinc, and copper, and may be a mixture with the alloy particles.

[0013] The alloy particles may have an average particle size (D50) in the range of 1 μm to 150 μm.

[0014] The sodium source is sodium chloride, and the weight ratio of the alloy particles to the sodium source may be in the range of 1:1 to 3:1.

[0015] The above additive may include one or more sulfide additives, sodium halide additives, or a combination thereof. The above additive may be included in a range of 0.05 wt.% to 20 wt.% of the total mass of the alloy particles and the sodium source.

[0016] The above sulfide additive may include one or more types of sulfur (S), sodium sulfide (Na2S), iron sulfide (FeS), or a combination thereof, and may be included in a range of 0.05 wt.% to 20 wt.% of the total mass of the alloy particles and sodium source.

[0017] The sodium halide additive may include one or more sodium fluoride (NaF), sodium iodide (NaI), sodium bromide (NaBr), or a combination thereof, and may be included in a range of 0.05 wt.% to 20 wt.% of the total mass of the alloy particles and the sodium source.

[0018] The above-mentioned anode material may include one or more primary particles, secondary particles formed by aggregating multiple primary particles, or a combination thereof, and the secondary particles of the above-mentioned anode material may have an average particle size (D50) in the range of 0.1 mm to 2 mm.

[0019] A sodium metal halide battery according to one embodiment of the present invention comprises a positive electrode, an electrolyte, and a negative electrode, and the positive electrode may comprise a positive electrode material according to the present invention. Effects of the invention

[0021] According to the present embodiment, by using a ferronickel alloy as the cathode material, the nickel component and the iron component complement each other to prevent rapid overvoltage of the battery due to the high energy density characteristics of nickel and the relatively lower OCV of iron compared to nickel, thereby maximizing the performance of the sodium metal halide battery.

[0022] In addition, by using a ferronickel alloy as an anode material, the problem of increased costs associated with the use of conventional high-purity metals or the pretreatment of single metals can be resolved. Brief explanation of the drawing

[0024] FIG. 1 is a schematic diagram illustrating a sodium metal halide battery according to the present embodiment. Figure 2 is the XRD analysis result of the sodium metal halide battery cathode material according to the present embodiment. Figure 3 shows the voltage-SOC curves of batteries using nickel, iron, and ferronickel alloys as the positive electrode material. Specific details for implementing the invention

[0025] Terms such as first, second, and third are used to describe various parts, components, regions, layers, and / or sections, but are not limited thereto. These terms are used solely to distinguish one part, component, region, layer, or section from another part, component, region, layer, or section. Accordingly, the first part, component, region, layer, or section described below may be referred to as the second part, component, region, layer, or section without departing from the scope of the present invention.

[0026] The technical terms used herein are for the reference of specific embodiments only and are not intended to limit the invention. The singular forms used herein include plural forms unless phrases clearly indicate otherwise. As used in the specification, the meaning of "comprising" specifies certain characteristics, areas, integers, steps, actions, elements, and / or components, and does not exclude the presence or addition of other characteristics, areas, integers, steps, actions, elements, and / or components.

[0027] When it is stated that one part is "above" or "on" another part, it may be directly above or on the other part, or other parts may be involved in between. In contrast, when it is stated that one part is "directly above" another part, no other parts are interposed in between.

[0028] Unless otherwise defined, all terms used herein, including technical and scientific terms, have the same meaning as generally understood by those skilled in the art to which this invention pertains. Terms defined in commonly used dictionaries are further interpreted to have meanings consistent with relevant technical literature and the present disclosure, and are not interpreted in an ideal or highly formal sense unless otherwise defined.

[0029] Hereinafter, embodiments of the present invention will be described in detail. However, these are presented as examples and are not intended to limit the present invention, and the present invention is defined only by the scope of the claims set forth below.

[0031] FIG. 1 is a schematic diagram illustrating a planar sodium metal halide battery according to the present embodiment.

[0032] Referring to FIG. 1, a sodium metal halide battery (100) (hereinafter referred to as the battery) according to one embodiment may include an upper case (10), a lower case (20), a positive electrode (30) located between the upper case (10) and the lower case (20), a solid electrolyte (40), and a negative electrode (50). FIG. 1 is illustrated in the form of a coin battery, but this is merely an example and is not limited thereto.

[0033] The upper case (10) may be made of a metal material such as aluminum and aluminum alloy, carbon steel, stainless steel, nickel and nickel-based alloy. The surface of the upper case (10) may be coated with a corrosion-resistant layer having chromium (Cr), nickel (Ni), molybdenum (Mo), etc. as its main components.

[0034] Additionally, the lower case (20) may be made of a metal material such as aluminum and aluminum alloy, carbon steel, stainless steel, nickel, or nickel-based alloy. A corrosion-resistant layer having chromium (Cr), nickel (Ni), molybdenum (Mo), etc. as main components may be coated on the surface of the lower case (20).

[0035] The above solid electrolyte (40) may include a sodium ion-conducting solid electrolyte, such as a beta-alumina ceramic, which can pass sodium ions.

[0036] Additionally, the above cathode (50) may include a sodium cathode member.

[0037] A sodium metal halide battery according to one embodiment of the present invention is a liquid sodium (mp=98 o It may be a high-temperature battery utilizing C), and specifically, it may be a battery that operates in a temperature range of 100°C to 400°C.

[0038] The anode (30) comprises an anode material, and the anode material may include alloy powder particles and a sodium source such as sodium chloride (NaCl), and may have the form of granules in which the two materials are mixed. If necessary, additives such as sodium fluoride (NaF), sodium iodide (NaI), sodium bromide (NaBr), sulfur (S), sodium sulfide (Na2S), and iron sulfide (FeS) may be included.

[0039] The alloy particles may include one or more elements selected from nickel (Ni), iron (Fe), zinc (Zn), and copper (Cu), and may include a ferronickel (Fe-Ni) alloy. The ferronickel alloy may contain nickel (Ni) in the range of 15 wt.% to 65 wt.% and may additionally include one or more elements selected from cobalt (Co), carbon (C), silicon (Si), zinc (Zn), and chromium (Cr). Specifically, the ferronickel may be a ferronickel alloy composition containing about 20 wt.% Ni. The ferronickel may be a composite phase of a β-Fe phase and intermetallic compounds such as Ni3Fe, Fe3Ni, and FeNi, or it may be a single phase having an average composition.

[0040] In addition, the alloy particles may further include one or more single metal particles selected from nickel (Ni), iron (Fe), zinc (Zn), and copper (Cu) in addition to the alloy particles.

[0041] The above alloy particles may be binary alloys or ternary alloys.

[0042] Meanwhile, the average particle size (D50) of the alloy particles may be in the range of 1 μm to 150 μm, specifically in the range of 1 μm to 100 μm. However, it is not limited thereto. When the average particle size (D50) of the alloy particles is in the above range, there is an advantage in that it can be mixed with a sodium source, such as sodium chloride (NaCl), to secure optimal battery performance.

[0043] In addition, the alloy particles may be primary particles, secondary particles formed by the aggregation of two or more primary particles, or a mixture of the primary particles and the secondary particles.

[0044] The above-mentioned anode material includes a sodium source. The sodium source may be a sodium compound containing sodium cations, specifically a sodium halide, and more specifically, sodium chloride (NaCl).

[0045] In addition, the weight ratio of the alloy particles to the sodium source may be in the range of 1:1 to 3:1, and specifically in the range of 1.2:1 to 2:1. When the alloy particles and the sodium source are mixed within the above range, the interconnectivity between the alloy particles is maintained, thereby maintaining high electron conductivity in the anode portion to lower cell resistance and maximizing the theoretical capacity of the active material.

[0046] Meanwhile, the above-mentioned cathode material may additionally include an additive. The additive may include a sulfide-based compound or a sodium halide. The additive may be included in a range of 0.05 wt.% to 20 wt.% of the total mass of the alloy particles and the sodium source, and specifically in a range of 0.1 wt.% to 10 wt.%.

[0047] In addition, the sulfide-based compound may be one or more selected from sulfur (S), sodium sulfide (Na2S), and iron sulfide (FeS). The sulfide-based compound additive may be included in a range of 0.05 wt.% to 20 wt.% of the total mass of the alloy particles and the sodium source, and specifically in a range of 0.1 wt.% to 10 wt.%. When the sulfide-based compound is included in the above range, the oxide layer formed on the surface of the anode metal material can be efficiently removed, and thus the surface of the anode metal material can be maximally activated, thereby having the effect of reducing resistance.

[0048] In addition, the sodium halide additive may be one or more selected from sodium fluoride (NaF), sodium iodide (NaI), and sodium bromide (NaBr). The sodium halide additive may be included in a range of 0.05 wt.% to 20 wt.% of the total mass of the alloy particles and the sodium source, and specifically in a range of 0.1 wt.% to 10 wt.%. When the sodium halide is included in the above range, it has the effect of effectively improving the capacity of the battery by causing defects in the metal halide formed on the surface of the alloy particles during charging, and has the effect of slightly improving the theoretical capacity.

[0049] Meanwhile, the above-mentioned cathode material may be a primary particle, a secondary particle formed by the aggregation of multiple primary particles, or a mixture of primary particles and secondary particles. Additionally, the average particle size (D50) of the cathode material secondary particles may be in the range of 0.1 mm to 2 mm, specifically in the range of 0.4 mm to 1.2 mm. However, it is not limited thereto. When the average particle size (D50) of the above-mentioned cathode material is within the above range, improved charge / discharge characteristics of the battery can be provided, and the filling density of the cathode portion can be improved.

[0051] Hereinafter, embodiments and comparative examples of the present invention will be described in detail. However, these are presented as examples and are not intended to limit the present invention, and the present invention is defined only by the scope of the claims set forth below.

[0052] Example 1

[0053] 60 wt.% of ferronickel alloy (20 wt.% Ni-Fe) powder, 35 wt.% of salt (NaCl), 3 wt.% of sodium sulfide (Na2S) additive, and 1.3 wt.% of sodium fluoride (NaF) additive are mixed using a ball mill for 24 hours. Afterward, the mixture is used to produce a cathode material in the form of granules with a size of approximately 1 mm using a roll compactor.

[0054] The XRD analysis results of the cathode material prepared according to Example 1 are shown in Figure 2.

[0055] Referring to Figure 2, the XRD analysis results of the cathode material prepared according to Example 1 showed that two phases, including α-Fe and FeNi3, were observed.

[0057] Comparative Example 1

[0058] The anode material was prepared in the same manner as in Example 1, except that iron powder was used instead of ferronickel alloy powder.

[0060] Comparative Example 2

[0061] A cathode material was prepared in the same manner as in Example 1, except that nickel powder was used instead of ferronickel alloy powder.

[0063] Manufacturing of sodium metal halide batteries for evaluation

[0064] As shown in FIG. 1, a positive electrode (30) having the positive electrode material prepared in Example 1 and Comparative Examples 1 and 2 was positioned between the upper case (10) and the lower case (20), and a sodium metal halide battery including a solid electrolyte (40) and a negative electrode (50) was manufactured.

[0066] Evaluation of charge and discharge characteristics of evaluation sodium metal halide batteries

[0067] The voltage-SOC curves of sodium metal halide batteries including anodes to which the anode materials prepared in Example 1 and Comparative Examples 1 and 2 are applied are shown in FIG. 3. The voltage-SOC curves were drawn based on the point when the SOC of the sodium metal halide batteries reached 100%.

[0068] Referring to Fig. 3, in the case of Comparative Example 1 using iron powder and Comparative Example 2 using nickel powder, one flat section appeared and it was confirmed that the capacity was expressed up to SOC 100%.

[0069] On the other hand, in the case of Example 1 using ferronickel alloy powder, two flat regions appeared, confirming that both components contained in the ferronickel were involved in charging and discharging, and that the capacity was developed up to 100% SOC. The characteristics of the two involved components complement each other, providing advantages such as preventing sudden overvoltage. Furthermore, it was shown that the SOC was developed up to 100% even in the case of the alloy, confirming the possibility of replacing expensive anode metal powder with low-cost ferronickel alloy powder.

[0071] The present invention is not limited to the above embodiments and can be manufactured in various different forms, and those skilled in the art will understand that the invention can be implemented in other specific forms without changing the technical concept or essential features of the invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive.

Claims

Claim 1 A cathode material for a sodium metal halide battery comprising alloy particles, a sodium source, and an additive, wherein the alloy particles comprise one or more elements selected from nickel (Ni), iron (Fe), zinc (Zn), and copper (Cu), wherein the alloy particles comprise a ferronickel (Fe-Ni) alloy, and wherein the additive comprises one or more sulfide additives, sodium halide additives, or a combination thereof. Claim 2 delete Claim 3 A cathode material for a sodium metal halide battery according to claim 1, wherein the cathode material further comprises one or more single metal particles selected from nickel (Ni), iron (Fe), zinc (Zn), and copper (Cu). Claim 4 A cathode material for a sodium metal halide battery according to claim 1, wherein the alloy particles have an average particle size (D50) in the range of 1 μm to 150 μm. Claim 5 A positive electrode material for a sodium metal halide battery according to claim 1, wherein the sodium source is a sodium halide such as sodium chloride (NaCl). Claim 6 A cathode material for a sodium metal halide battery according to claim 1, wherein the weight ratio of the alloy particles to the sodium source is in the range of 1:1 to 3:

1. Claim 7 delete Claim 8 A cathode material for a sodium metal halide battery according to claim 1, wherein the sulfide additive comprises one or more types of sulfur (S), sodium sulfide (Na2S), iron sulfide (FeS), or a combination thereof. Claim 9 A cathode material for a sodium metal halide battery according to claim 1, wherein the sulfide additive is included in a range of 0.05 wt.% to 20 wt.% of the total mass of the alloy particles and the sodium source. Claim 10 A cathode material for a sodium metal halide battery according to claim 1, wherein the sodium halide additive comprises one or more sodium fluoride (NaF), sodium iodide (NaI), sodium bromide (NaBr), or a combination thereof. Claim 11 A cathode material for a sodium metal halide battery according to claim 1, wherein the sodium halide additive is included in a range of 0.05 wt.% to 20 wt.% of the total mass of the alloy particles and the sodium source. Claim 12 A cathode material for a sodium metal halide battery according to claim 1, wherein the cathode material comprises one or more primary particles, secondary particles formed by aggregating multiple primary particles, or a combination thereof. Claim 13 A cathode material for a sodium metal halide battery according to claim 1, wherein the secondary particles of the cathode material have an average particle size (D50) in the range of 0.1 mm to 2 mm. Claim 14 A sodium metal halide battery comprising a positive electrode, an electrolyte, and a negative electrode, wherein the positive electrode comprises a positive electrode material according to any one of claims 1, 3 to 6, and 8 to 13.

Citation Information

Patent Citations

  • Na based Secondary Battery

    KR1020160028748A

  • Sodium-base battery operated at intermediate temperature and method for preparing the same